Rubber composition, laminate, and marine hose
A rubber composition with acrylonitrile butadiene and styrene butadiene copolymers, silica, and melamine compounds improves adhesion and strength in marine hoses, addressing low adhesion and strength issues in existing compositions.
Patent Information
- Application Number
- JP2020103940
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-06-16
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2040-06-16
AI Technical Summary
Existing rubber compositions for marine hoses exhibit low adhesion and strength when used with acrylonitrile butadiene rubber or styrene butadiene rubber layers, particularly in the innermost and carcass layers.
A rubber composition containing 30 to 80% acrylonitrile butadiene copolymer and 20 to 70% styrene butadiene copolymer, silica, resorcinol resin, and at least one melamine compound, along with a sulfenamide vulcanization accelerator, to enhance adhesion and strength.
The composition achieves excellent adhesion and strength in the cured product, particularly with acrylonitrile butadiene rubber and styrene butadiene rubber layers, suitable for marine hoses.
Smart Images

Figure 0007557124000012 
Figure 0007557124000001 
Figure 0007557124000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a rubber composition, a laminate, and a marine hose. [Background technology]
[0002] Rubber products have been used in various technical fields. Among the rubber products, there are large products such as marine hoses. Marine hoses are used on the sea for transporting oil, for example. As described above, marine hoses are used to transport petroleum and the like, and therefore generally have, as the innermost layer, a tube rubber made of acrylonitrile butadiene rubber or the like having excellent oil resistance, and a carcass layer or the like in which reinforcing cords such as fiber cords or steel cords are covered with rubber (for example, Patent Document 1).
[0003] On the other hand, Patent Document 2, which aims to improve the adhesion between canvas and the coating rubber covering it, describes a coating rubber composition for conveyor belts, which contains a diene rubber component, di-2-benzothiazolyl disulfide, silica, cresol formaldehyde resin, and modified etherified methylol melamine, and the content of the di-2-benzothiazolyl disulfide is 0.25 parts by mass or more and 3.0 parts by mass or less per 100 parts by mass of the diene rubber component, the content of the silica is 5.0 parts by mass or more and 15.0 parts by mass or less per 100 parts by mass of the diene rubber component, the content of the cresol formaldehyde resin is 1 part by mass or more and 5 parts by mass or less per 100 parts by mass of the diene rubber component, and the content of the modified etherified methylol melamine is 1 part by mass or more and 4 parts by mass or less per 100 parts by mass of the diene rubber component. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 7-63288 [Patent Document 2] International Publication No. 2018 / 179629 Summary of the Invention [Problem to be solved by the invention]
[0005] Under these circumstances, in order to improve the adhesion between the innermost layer (tube rubber) of a marine hose and a carcass layer in which reinforcing cords such as fiber cords are covered with rubber, the present inventors prepared a rubber composition with reference to Patent Document 2 and evaluated the rubber composition as a rubber composition for an interlayer adhesive layer to be applied between the innermost layer and carcass layer of a marine hose. As a result, it became clear that the adhesion to a rubber layer containing acrylonitrile butadiene rubber or styrene butadiene rubber was sometimes low, and the strength of the obtained cured product was sometimes low (Comparative Examples 1, 10, and 11).
[0006] Therefore, an object of the present invention is to provide a rubber composition which provides excellent adhesion between the resulting cured product and a rubber layer containing acrylonitrile butadiene rubber or styrene butadiene rubber, and which provides the cured product with excellent strength. Another object of the present invention is to provide a laminate and a marine hose. [Means for solving the problem]
[0007] As a result of intensive research by the present inventors to solve the above problems, it has been found that when a rubber composition contains a rubber component containing 30-80 mass% of an acrylonitrile-butadiene copolymer and 20-70 mass% of a styrene-butadiene copolymer, silica, a resorcinol resin, and at least one melamine compound selected from the group consisting of methylol melamines, methylol melamine alkyl ethers, and condensates thereof, the obtained cured product has excellent adhesion to a rubber layer containing acrylonitrile-butadiene rubber or styrene-butadiene rubber, and the strength of the cured product is excellent, and the present invention has been completed. The present invention is based on the above findings and has the following specific configuration to solve the above problems.
[0008] [1] A rubber component containing 30 to 80% by mass of an acrylonitrile butadiene copolymer and 20 to 70% by mass of a styrene butadiene copolymer; Silica and Resorcinol resin, A rubber composition comprising at least one melamine compound selected from the group consisting of methylol melamines, methylol melamine alkyl ethers, and condensates thereof. [2] The rubber composition according to [1], wherein the content of the melamine compound is 30 to 250 mass % of the content of the resorcinol resin. [3] Also contains a sulfenamide vulcanization accelerator, The rubber composition according to [1] or [2], wherein the content of the sulfenamide vulcanization accelerator is 0.7 to 1.2 parts by mass per 100 parts by mass of the rubber component. [4] The rubber composition according to any one of [1] to [3], wherein the content of the silica is 10 to 40 parts by mass per 100 parts by mass of the rubber component. [5] The rubber composition according to any one of [1] to [4], wherein the content of the resorcinol resin is 0.3 to 8.0 parts by mass based on 100 parts by mass of the acrylonitrile butadiene copolymer. [6] The rubber composition according to any one of [1] to [5], which is used for forming a marine hose.
[0009] [7] A vulcanized rubber layer A formed using the rubber composition according to any one of [1] to [5]; a vulcanized rubber layer B containing acrylonitrile butadiene rubber or styrene butadiene rubber; The reinforcing layer has polyester fibers, The vulcanized rubber layer A is adjacent to the vulcanized rubber layer B, forming a laminate. [8] The vulcanized rubber layer B includes a vulcanized rubber layer B-1 containing the acrylonitrile butadiene rubber and a vulcanized rubber layer B-2 containing the styrene butadiene rubber, The laminate according to [7], wherein the vulcanized rubber layer B-1, the vulcanized rubber layer A, and the vulcanized rubber layer B-2 are laminated in this order.
[0010] [9] A marine hose formed using the rubber composition according to any one of [1] to [5].
[10] An innermost layer, an interlayer adhesive layer, and a carcass layer are laminated in this order; the innermost layer is a vulcanized rubber layer containing acrylonitrile butadiene rubber, the interlayer adhesive layer is a vulcanized rubber layer formed using the rubber composition, The marine hose according to [9], wherein the carcass layer has a vulcanized rubber layer containing styrene-butadiene rubber and polyester fibers.
[11] The marine hose according to
[10] , wherein the innermost layer is adjacent to the interlayer adhesive layer, and the interlayer adhesive layer is adjacent to the vulcanized rubber layer containing the styrene-butadiene rubber possessed by the carcass layer. Effect of the Invention
[0011] The rubber composition of the present invention provides excellent adhesion between the resulting cured product and a rubber layer containing acrylonitrile butadiene rubber or styrene butadiene rubber, and the cured product has excellent strength. The present invention can also provide a laminate and a marine hose. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will be described in detail below. In this specification, a numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the lower and upper limits. In this specification, unless otherwise specified, each component may be used alone or in combination of two or more substances corresponding to that component. When a component contains two or more substances, the content of the component means the total content of the two or more substances. In the present specification, unless otherwise specified, the method for producing each component is not particularly limited, and may be, for example, a conventionally known method.
[0013] In the present invention, one of the effects of the present invention, "the obtained cured product has excellent adhesion to a rubber layer containing acrylonitrile butadiene rubber or styrene butadiene rubber", means that the obtained cured product has excellent adhesion to a rubber layer containing acrylonitrile butadiene rubber and to a rubber layer containing styrene butadiene rubber. In this specification, the effect of the present invention may be said to be superior when at least one of the adhesion between the obtained cured product and a rubber layer containing acrylonitrile butadiene rubber or styrene butadiene rubber, and the strength of the cured product is superior.
[0014] [Rubber composition] The rubber composition of the present invention comprises: A rubber component containing 30 to 80% by mass of an acrylonitrile butadiene copolymer and 20 to 70% by mass of a styrene butadiene copolymer; Silica and Resorcinol resin, The rubber composition contains at least one melamine compound selected from the group consisting of methylol melamines, methylol melamine alkyl ethers, and condensates thereof.
[0015] Since the rubber composition of the present invention has the above-mentioned structure, it is believed that the desired effects can be obtained. Although the reason is not clear, it is speculated to be as follows. First, the rubber composition of the present invention contains a rubber component including 30 to 80 mass% of an acrylonitrile-butadiene copolymer and 20 to 70 mass% of a styrene-butadiene copolymer, and therefore a cured product obtained from the rubber composition of the present invention has excellent adhesion to a rubber layer including an acrylonitrile-butadiene rubber or a styrene-butadiene rubber. Generally, it is often difficult to vulcanize and bond a rubber composition containing an acrylonitrile-butadiene rubber and a rubber composition containing an acrylonitrile-butadiene rubber having a larger acrylonitrile content than the acrylonitrile-butadiene rubber (for example, an acrylonitrile-butadiene rubber called a very high nitrile rubber) only by sulfur crosslinking. However, the rubber composition of the present invention contains a resorcinol resin and the melamine compound in addition to the rubber component. Therefore, when the rubber composition of the present invention is adjacent to a rubber composition containing acrylonitrile butadiene rubber or styrene butadiene rubber (excluding the rubber composition of the present invention) and vulcanized, it is considered that the cured product obtained from the rubber composition of the present invention has excellent adhesion not only to a rubber layer containing styrene butadiene rubber but also to a rubber layer containing acrylonitrile butadiene rubber (other than the rubber layer containing styrene butadiene rubber) due to the reaction between the resorcinol resin and the formaldehyde generated from the melamine compound. The acrylonitrile content of the acrylonitrile butadiene rubber contained in the rubber layer containing acrylonitrile butadiene rubber is not particularly limited, and includes the case where the acrylonitrile content is large. In addition, the rubber layer containing the acrylonitrile butadiene rubber is different from the cured product obtained from the rubber composition of the present invention. The rubber layer containing styrene butadiene rubber is different from the cured product obtained from the rubber composition of the present invention. The rubber composition of the present invention will now be described.
[0016] <<Rubber component>> In the rubber composition of the present invention, the rubber component contains an acrylonitrile butadiene copolymer and a styrene butadiene copolymer.
[0017] <Acrylonitrile butadiene copolymer> In the present invention, the acrylonitrile butadiene copolymer (NBR) is a copolymer of acrylonitrile and butadiene. The acrylonitrile butadiene copolymer may be a hydrogenated product of the copolymer of acrylonitrile and butadiene. The NBR is preferably a copolymer of acrylonitrile and butadiene (not a hydrogenated product) because it provides better effects for the present invention.
[0018] (Acrylonitrile content) The acrylonitrile content of the NBR (the content of repeating units due to acrylonitrile in the NBR. Hereinafter, also referred to as "AN content") is preferably 10 to 40 mass % of the NBR, and more preferably 15 to 25 mass %, because the effects of the present invention are superior. The acrylonitrile content (bound acrylonitrile content) of an acrylonitrile butadiene copolymer can be measured in accordance with JIS K6451-2:2016 (Kjeldahl method).
[0019] (Mooney viscosity) The Mooney viscosity of the NBR is preferably from 45 to 85, and more preferably from 60 to 80, because the effects of the present invention are more excellent. In the present invention, the Mooney viscosity of the acrylonitrile butadiene copolymer can be measured under the condition of 100°C in accordance with JIS K6300-1:2013.
[0020] <Styrene butadiene copolymer> In the present invention, the styrene-butadiene copolymer (SBR) is a copolymer of a styrene-based monomer and butadiene. Examples of the styrene monomer include styrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, α-methylstyrene, 2,4-dimethylstyrene, 2,4-diisopropylstyrene, 4-tert-butylstyrene, tert-butoxystyrene, N,N-dimethylaminoethylstyrene, etc. Among these, styrene is preferable.
[0021] Weight average molecular weight (Mw) of styrene butadiene copolymer The weight average molecular weight of the styrene-butadiene copolymer is preferably from 300,000 to 2,000,000 because the effects of the present invention are more excellent. The weight average molecular weight of the styrene-butadiene copolymer can be determined in terms of standard polystyrene by gel permeation chromatography (GPC) using tetrahydrofuran as a solvent.
[0022] Styrene content of styrene butadiene copolymer The styrene content of the styrene-butadiene copolymer (the content of repeating units of styrene-based monomers in the styrene-butadiene copolymer) is preferably 15 to 40% by mass, more preferably 20 to 35% by mass, because the effects of the present invention are superior. The styrene content of the styrene-butadiene copolymer can be measured by infrared spectroscopy (Hampton method).
[0023] Other rubber The rubber component may contain, in addition to the NBR and SBR, rubber components other than the NBR and SBR (other rubbers). Examples of other rubbers include diene rubbers such as natural rubber (NR), isoprene rubber (IR), butadiene rubber (BR), chloroprene rubber (CR), butyl rubber (IIR), and ethylene-propylene-diene rubber (EPDM).
[0024] The rubber component preferably contains only the NBR and the SBR because this provides better effects for the present invention.
[0025] <Acrylonitrile butadiene copolymer content> In the present invention, the content of the acrylonitrile butadiene copolymer is 30 to 80% by mass in the total amount of the rubber component. The content of the NBR is preferably 50 to 80 mass % of the total rubber component, and more preferably 60 to 80 mass %, because this leads to superior effects of the present invention and excellent tensile strength of the resulting cured product.
[0026] <Content of styrene butadiene copolymer> In the present invention, the content of the styrene-butadiene copolymer is 20 to 70% by mass in the total amount of the rubber component. The content of the SBR is preferably 20 to 50 mass % and more preferably 20 to 40 mass % of the total rubber component, because the effects of the present invention are excellent and the tensile strength of the resulting cured product is excellent.
[0027] <Silica> The rubber composition of the present invention contains silica. By containing silica, the rubber composition of the present invention provides the resulting cured product with excellent strength and tensile properties.
[0028] The silica contained in the rubber composition of the present invention is not particularly limited, and examples thereof include conventionally known silica. Among these, from the viewpoint of achieving superior effects of the present invention (particularly strength of the resulting cured product), acidic silica having a pH of less than 7 is preferred. In the present invention, the pH of silica can be measured in accordance with JIS K5101-17-2:2004.
[0029] (Silica content) From the viewpoint of obtaining superior effects of the present invention (particularly strength of the resulting cured product), the content of the silica is preferably 10 to 40 parts by mass, and more preferably 15 to 30 parts by mass, per 100 parts by mass of the rubber component.
[0030] <Resorcinol resin> The rubber composition of the present invention contains a resorcinol resin. In the present invention, the resorcinol resin can function as a methylene acceptor. In the rubber composition of the present invention, the resorcinol resin reacts with formaldehyde or the like generated from the melamine compound described below, thereby imparting adhesiveness to the rubber composition of the present invention, and the rubber composition of the present invention has excellent adhesiveness to a rubber layer containing an acrylonitrile butadiene rubber or a styrene butadiene rubber.
[0031] The resorcinol resin contained in the rubber composition of the present invention is a condensation product of resorcin (1,3-benzenediol) and formaldehyde. The resorcinol resin may further contain unreacted resorcin and / or formaldehyde. The resorcinol resin may be a modified resorcinol resin, for example, a resorcinol resin in which a part of the repeating units of the resorcinol resin is alkylated (specifically, for example, a resorcinol resin in which a part of the resorcin constituting the resorcinol resin is alkylated).
[0032] (Resorcinol resin content in rubber component) The content of the resorcinol resin is preferably 1 to 10 parts by mass, and more preferably 2.0 to 5.0 parts by mass, per 100 parts by mass of the rubber component, from the viewpoint of obtaining superior effects of the present invention.
[0033] (Resorcinol resin content relative to NBR) From the viewpoint of obtaining superior effects of the present invention, the content of the resorcinol resin is preferably 0.3 to 8.0 parts by mass, and more preferably 0.5 to 4.0 parts by mass, based on 100 parts by mass of the acrylonitrile butadiene copolymer.
[0034] <<Melamine compounds>> The rubber composition of the present invention contains at least one melamine compound selected from the group consisting of methylol melamines, methylol melamine alkyl ethers, and condensates thereof. In the present invention, the melamine compound can function as a methylene donor. The melamine compound can be decomposed into formaldehyde and the like, for example, by heat during vulcanization.
[0035] <Methylol melamines> Methylolmelamines, which are melamine compounds, are compounds in which 1 to 6 formaldehyde groups are added to the three amino groups (-NH2) that melamine has. In the present invention, the methylol melamines do not include methylol melamine alkyl ethers, which will be described later. Examples of methylol melamines include monomethylol melamine and hexamethylol melamine.
[0036] <Methylol melamine alkyl ethers> Methylol melamine alkyl ethers as melamine compounds are compounds in which at least a part or all of the methylol groups (hydroxymethyl groups) of the above-mentioned methylol melamines are alkyl-etherified. Examples of methylolmelamine alkyl ethers include hexamethylolmelamine pentamethyl ether (structure shown below). [ka]
[0037] An example is hexamethylolmelamine hexamethyl ether (structure shown below). [ka]
[0038] <Condensation product> In the present invention, the condensation product as the melamine compound is a condensation product of the above-mentioned methylol melamines and / or the above-mentioned methylol melamine alkyl ethers. Examples of the condensates of the methylolmelamine alkyl ethers include a condensate of hexamethylolmelamine pentamethyl ether and a condensate of hexamethylolmelamine hexamethyl ether. The condensate may be a partial condensate of the methylol melamines and / or the methylol melamine alkyl ethers.
[0039] Examples of the condensation products of hexamethylolmelamine pentamethyl ether include compounds represented by the following formula (n in the following formula is 2 to 3). [ka]
[0040] Examples of the condensation products of hexamethylolmelamine hexamethyl ether include compounds represented by the following formula (n in the following formula is 2 to 3). [ka]
[0041] The melamine compound preferably contains the above-mentioned methylol melamine alkyl ethers and / or condensates thereof, more preferably contains a mixture of hexamethylol melamine pentamethyl ether and a condensate thereof, or hexamethylol melamine hexamethyl ether and / or a condensate thereof, and even more preferably contains hexamethylol melamine hexamethyl ether and / or a condensate thereof, because this provides superior effects of the present invention.
[0042] (Melamine compound content in rubber component) The content of the melamine compound is preferably 1 to 10 parts by mass, and more preferably 2.0 to 7.0 parts by mass, per 100 parts by mass of the total content of the rubber components, because this provides better effects for the present invention.
[0043] (Melamine compound content relative to acrylonitrile butadiene copolymer) The content of the melamine compound is preferably 0.3 to 8.0 parts by mass, more preferably 0.5 to 5.0 parts by mass, based on 100 parts by mass of the acrylonitrile butadiene copolymer, because this provides better effects for the present invention.
[0044] (Content of melamine compounds relative to resorcinol resin) The content of the melamine compound is preferably 30 to 250 mass %, more preferably 80 to 150 mass %, of the content of the resorcinol resin, because this provides better effects for the present invention.
[0045] The rubber composition of the present invention uses the above-mentioned melamine compound as a methylene donor. It is preferable to use the above-mentioned melamine compound as a methylene donor because the nitrogen-containing compound generated (other than formaldehyde) after the decomposition of the above-mentioned melamine compound does not hydrolyze polyester or is difficult to hydrolyze polyester. Examples of the nitrogen-containing compound generated after the decomposition of the melamine compound include, when the melamine compound is a methylol melamine alkyl ether, a compound in which the ether in the methylol melamine alkyl ether is partially decomposed, methylol melamines, or melamine. When the melamine compound is a methylol melamine, examples of the nitrogen-containing compound include, when the melamine compound is a methylol melamine, a compound in which the methylol in the methylol melamine is partially decomposed, or melamine. Therefore, for example, in a rubber product having a reinforcing layer made of polyester, a rubber layer adjacent to the reinforcing layer, and a rubber layer made of the rubber composition of the present invention adjacent to the reinforcing layer, even if the nitrogen-containing compound migrates to the rubber layer, the polyester is not hydrolyzed or is hardly hydrolyzed. Therefore, it is considered that the rubber composition of the present invention is unlikely to reduce the reinforcing property and adhesiveness of the polyester reinforcing layer.
[0046] One of the preferred embodiments of the rubber composition of the present invention is one that is substantially free of hexamethylenetetramine. In the present invention, "substantially free of hexamethylenetetramine" means that the content of hexamethylenetetramine is 0 to 0.1% by mass in the entire rubber composition of the present invention.
[0047] (Vulcanization accelerator) The composition of the present invention may further contain a vulcanization accelerator.
[0048] (Sulfenamide vulcanization accelerator) The composition of the present invention preferably further contains a sulfenamide vulcanization accelerator as a vulcanization accelerator, because this provides superior effects of the present invention and the resulting cured product has superior tensile strength. Examples of the sulfenamide vulcanization accelerator include N-cyclohexylbenzothiazole sulfenamide, N-tert-butylbenzothiazole sulfenamide, N-oxydiethylenebenzothiazole sulfenamide, and N,N-dicyclohexylbenzothiazole sulfenamide. Among these, N-alkyl-2-benzothiazolylsulfenamide is preferred, and N-tert-butyl-2-benzothiazolylsulfenamide is more preferred, because they provide superior effects in the present invention.
[0049] (Sulfenamide vulcanization accelerator content) The content of the sulfenamide vulcanization accelerator is preferably 0.7 to 1.2 parts by mass, and more preferably 0.8 to 0.9 parts by mass, per 100 parts by mass of the rubber component, because the effects of the present invention are excellent and the reinforcing property of the polyester reinforcing layer and / or the adhesiveness of the polyester reinforcing layer are excellent.
[0050] (Carbon Black) The rubber composition of the present invention preferably further contains carbon black because the effect of the present invention is more excellent. The carbon black is not particularly limited. For example, conventionally known carbon black can be used. Among these, the carbon black preferably contains FT (Fine Thermal) grade, GPF (General Purpose Furnace) grade, SRF (Semi-Reinforcing Furnace) grade or other carbon black, more preferably FT grade or SRF grade carbon black, and even more preferably FT grade carbon black, because these carbon blacks have better effects than the carbon black of the present invention.
[0051] Nitrogen adsorption specific surface area of carbon black The nitrogen adsorption specific surface area (N2SA) of the carbon black is preferably 20 to 40 m because this provides a superior effect of the present invention. 2 / g is preferable, and 20 to 30m 2 / g is more preferred. The nitrogen adsorption specific surface area of carbon black can be measured in accordance with JIS K6217-2:2017 "Carbon black for rubber - Basic characteristics - Part 2: Determination of specific surface area - Nitrogen adsorption method - Single point method."
[0052] Dibutyl phthalate oil absorption of carbon black The dibutyl phthalate oil absorption (DBP oil absorption) of the carbon black is preferably from 20 to 80 ml / 100 g, and more preferably from 20 to 50 ml / 100 g, because this provides better effects for the present invention. The dibutyl phthalate oil absorption (DBP oil absorption) of carbon black can be measured in accordance with JIS K6217-4:2017 "Carbon black for rubber - Basic properties - Part 4: Determination of oil absorption (including compressed samples)".
[0053] Carbon black content The content of the carbon black is preferably 40 to 100 parts by mass, and more preferably 50 to 80 parts by mass, per 100 parts by mass of the rubber component, because this provides better effects for the present invention.
[0054] (sulfur) From the viewpoint of obtaining superior effects of the present invention and excellent oil resistance, the rubber composition of the present invention preferably further contains sulfur. The sulfur is not particularly limited. For example, conventionally known sulfur may be used.
[0055] Sulfur content The content of the sulfur is preferably 1 to 4 parts by mass, and more preferably 2 to 3 parts by mass, per 100 parts by mass of the rubber component, from the viewpoints of achieving a superior effect of the present invention and excellent oil resistance.
[0056] (tackifier) From the viewpoint of achieving superior effects of the present invention (particularly strength of the cured product), the rubber composition of the present invention preferably further contains a tackifier. Examples of tackifiers include rosin-based resins, terpene-based resins, petroleum resins, coumarone resins, and phenolic resins (excluding the above-mentioned resorcinol resins). In particular, from the viewpoint of achieving superior effects of the present invention, the tackifier preferably contains a coumarone resin and / or an alkylphenol resin, and more preferably contains a coumarone resin and an alkylphenol resin.
[0057] Examples of coumarone resins include polymers of coumarone (1-benzofuran), polymers of coumarone derivatives, coumarone-indene resins (copolymers of coumarone and indene), and hydrogenated coumarone-indene resins.
[0058] Examples of alkylphenol resins include condensates of alkylphenol components and aldehydes. Examples of the alkylphenol component include phenols having an alkyl group having 1 to 18 carbon atoms, such as cresol, isopropylphenol, t-butylphenol, amylphenol, octylphenol (e.g., p-octylphenol), nonylphenol, dodecylphenol, allylphenol, and cyclohexylphenol, as well as various derivatives thereof, such as methylol derivatives and halogenated derivatives. Of these, octylphenol is preferred, and p-octylphenol is more preferred.
[0059] Examples of the aldehydes include formaldehyde, paraformaldehyde, trioxane, polyoxymethylene, acetaldehyde, propionaldehyde, polyoxymethylene, chloral, hexamethylenetetramine, furfural, glyoxal, n-butylaldehyde, caproaldehyde, allylaldehyde, benzaldehyde, crotonaldehyde, acrolein, tetraoxymethylene, phenylacetaldehyde, o-tolualdehyde, salicylaldehyde, and paraxylene dimethyl ether.
[0060] Tackifier content The content of the tackifier (the total amount of the tackifiers when two or more types of tackifiers are used) is preferably 3 to 30 parts by mass, and more preferably 10 to 20 parts by mass, per 100 parts by mass of the rubber component, from the viewpoint of obtaining superior effects of the present invention.
[0061] When a coumarone resin and an alkylphenol resin are used in combination as a tackifier, the content of the coumarone resin is preferably 1.5 to 3 times the content of the alkylphenol resin in parts by mass.
[0062] (Additives) The rubber composition of the present invention may further contain additives such as vinyl chloride resin, plasticizer (including aromatic oil, etc.), zinc oxide, stearic acid, antioxidant, antioxidant, antistatic agent, flame retardant, vulcanizing agent other than sulfur, vulcanization retarder, filler other than carbon black and silica, etc., within the scope not impairing the object of the present invention.
[0063] The method for producing the rubber composition of the present invention is not particularly limited, and examples thereof include a method in which components other than a melamine compound, sulfur, and a vulcanization accelerator are mixed under conditions of 80 to 140°C to obtain a mixture, and then the melamine compound, sulfur, and vulcanization accelerator are added to the obtained mixture, and these are mixed under conditions of 40 to 100°C. Examples of the device used for mixing include a Banbury mixer, a kneader, and a roll.
[0064] The rubber composition of the present invention can be vulcanized under conventionally known vulcanization conditions.
[0065] The rubber composition of the present invention can be used, for example, to form a marine hose. There is no particular limitation as to which component of a marine hose the rubber composition of the present invention is used. Among them, from the viewpoint of excellent adhesion between the obtained cured product and a rubber layer containing acrylonitrile butadiene rubber or styrene butadiene rubber, and excellent strength of the cured product, the rubber composition of the present invention is one of the preferred embodiments for forming an interlayer adhesive layer that bonds an innermost layer containing acrylonitrile butadiene rubber and a carcass layer containing styrene butadiene rubber in a marine hose.
[0066] [Laminate] The laminate of the present invention comprises a vulcanized rubber layer A formed using the rubber composition of the present invention, a vulcanized rubber layer B containing acrylonitrile butadiene rubber or styrene butadiene rubber; The reinforcing layer has polyester fibers, The vulcanized rubber layer A is adjacent to the vulcanized rubber layer B, and is a laminate.
[0067] <Vulcanized rubber layer A> In the laminate of the present invention, the vulcanized rubber layer A is a vulcanized rubber layer formed using the rubber composition of the present invention. The rubber composition used in the vulcanized rubber layer A is not particularly limited as long as it is the rubber composition of the present invention.
[0068] <Vulcanized rubber layer B> In the laminate of the present invention, the vulcanized rubber layer B is a vulcanized rubber layer containing acrylonitrile butadiene rubber or styrene butadiene rubber. The rubber composition used to form the vulcanized rubber layer B excludes the rubber composition of the present invention. The vulcanized rubber layer B may have one or both of a vulcanized rubber layer B-1 containing an acrylonitrile butadiene rubber and a vulcanized rubber layer B-2 containing a styrene butadiene rubber. A preferred embodiment of the vulcanized rubber layer B includes both a vulcanized rubber layer B-1 containing an acrylonitrile butadiene rubber and a vulcanized rubber layer B-2 containing a styrene butadiene rubber. In this case, it is preferred that the vulcanized rubber layer A is disposed between the vulcanized rubber layer B-1 and the vulcanized rubber layer B-2, the vulcanized rubber layer B-1 is adjacent to the vulcanized rubber layer A, and the vulcanized rubber layer A is adjacent to the vulcanized rubber layer B-2.
[0069] (Vulcanized rubber layer B-1 containing acrylonitrile butadiene rubber) The rubber composition BB-1 used in the vulcanized rubber layer B-1 containing acrylonitrile butadiene rubber is not particularly limited as long as it is a rubber composition containing acrylonitrile butadiene rubber, however, the rubber composition of the present invention is excluded from the rubber composition BB-1.
[0070] The rubber composition BB-1 is not particularly limited except that it contains acrylonitrile butadiene rubber. The acrylonitrile butadiene rubber contained in the rubber composition BB-1 is not particularly limited, and examples thereof include those conventionally known.
[0071] Acrylonitrile content of acrylonitrile butadiene rubber The amount of acrylonitrile in the acrylonitrile-butadiene rubber contained in the rubber composition BB-1 (the amount of repeating units due to acrylonitrile in the acrylonitrile-butadiene rubber) is not particularly limited. In order to obtain a better effect of the present invention, the amount of acrylonitrile is preferably 10 to 50 mass% in the acrylonitrile-butadiene rubber. The cured product obtained from the rubber composition of the present invention has excellent adhesion to a rubber layer containing an acrylonitrile-butadiene rubber, so that the amount of acrylonitrile may be large regardless of the amount of acrylonitrile of the acrylonitrile-butadiene rubber contained in the rubber composition BB-1. Therefore, even when the amount of acrylonitrile in the acrylonitrile-butadiene rubber contained in the rubber composition BB-1 exceeds 40% by mass in the acrylonitrile-butadiene rubber, the adhesion between the vulcanized rubber layer A and the vulcanized rubber layer B can be excellent. The acrylonitrile content (bound acrylonitrile content) of acrylonitrile butadiene rubber can be measured in accordance with JIS K6451-2:2016 (Kjeldahl method).
[0072] In the rubber composition BB-1, the content of the acrylonitrile butadiene rubber is preferably 50 to 100 mass %, and more preferably 100 mass %, of the total amount of the rubber components in the rubber composition BB-1. In the rubber composition BB-1, the content of the acrylonitrile butadiene rubber is preferably 20 to 80 mass % in the rubber composition BB-1.
[0073] The rubber composition BB-1 may further contain, in addition to the acrylonitrile-butadiene rubber, for example, a rubber other than the acrylonitrile-butadiene rubber, a filler such as carbon black or silica, a plasticizer, zinc oxide, stearic acid, a vulcanization accelerator, a vulcanizing agent such as sulfur, a phenolic resin such as resorcin, a methylene donor such as hexamethylenetetramine, and the like. The type and content of each of the above components can be appropriately selected. The rubber composition BB-1 may be free of styrene-butadiene rubber.
[0074] (Vulcanized rubber layer B-2 containing styrene butadiene rubber) The rubber composition BB-2 used in the vulcanized rubber layer B-2 containing styrene-butadiene rubber is not particularly limited as long as it is a rubber composition containing styrene-butadiene rubber. Note that the rubber composition BB-2 does not include the rubber composition of the present invention.
[0075] Rubber composition containing styrene butadiene rubber BB-2 The rubber composition BB-2 is not particularly limited except that it contains a styrene-butadiene rubber. Styrene butadiene rubber The styrene-butadiene rubber contained in the rubber composition BB-2 is not particularly limited, and may be, for example, a conventionally known rubber. Natural rubber, butadiene rubber The rubber composition BB-2 may further contain a rubber other than the styrene-butadiene rubber as a rubber component. The rubber composition BB-2 preferably further contains a natural rubber and / or a butadiene rubber as a rubber component. The rubber composition BB-2 may contain, as the rubber component, for example, a styrene-butadiene rubber and a natural rubber, or a styrene-butadiene rubber, a natural rubber, and a butadiene rubber.
[0076] In the rubber composition BB-2, the content of the styrene-butadiene rubber is preferably from 10 to 100 mass %, and more preferably from 15 to 40 mass %, of the rubber component in the rubber composition BB-2. When the rubber composition BB-2 further contains a natural rubber and a butadiene rubber as the rubber component, the content of the styrene-butadiene rubber in the rubber component is preferably 15 to 40 parts by mass. When the rubber composition BB-2 further contains a natural rubber and a butadiene rubber as rubber components, the content of the natural rubber in the rubber components is preferably 40 to 70 parts by mass. When the rubber composition BB-2 further contains a natural rubber and a butadiene rubber as the rubber component, the content of the butadiene rubber in the rubber component is preferably 15 to 45 parts by mass.
[0077] In the rubber composition BB-2, the content of the rubber component containing the styrene-butadiene rubber is preferably 50 to 80 mass % in the rubber composition BB-2.
[0078] The rubber composition BB-2 may further contain, for example, a filler such as carbon black or silica, a plasticizer (including aromatic oil), a tackifier such as a C5-based resin, zinc oxide, stearic acid, a vulcanization accelerator, a vulcanizing agent such as sulfur, and the like. The type and content of each of the above components can be appropriately selected. The rubber composition BB-2 may be free of acrylonitrile butadiene rubber.
[0079] <Polyester fiber> The laminate of the present invention has polyester fibers as a reinforcing layer. The polyester fiber is not particularly limited, and examples thereof include those conventionally known. Examples of polyester fiber materials include polyethylene terephthalate (PET) and polyethylene naphthalate (PEN).
[0080] Examples of polyester fibers include continuous fiber reinforcement (i.e., fiber reinforcement having sufficient length) and discontinuous fiber reinforcement (i.e., short fiber, usually fiber having a length of 1 cm or less). The above-mentioned fiber reinforcement is preferably a continuous fiber reinforcement from the viewpoint of excellent reinforcing properties of the obtained rubber product. The continuous fiber reinforcing material is not particularly limited in terms of fiber diameter, fiber length, shape, etc., so long as it is a continuous fiber reinforcing material that can be generally used in rubber products (for example, marine hoses, etc.).
[0081] The continuous fiber reinforcement may have, for example, a blind shape. The blind-shaped fiber reinforcement may have, for example, a plurality of warp threads arranged in parallel. The plurality of warp threads may be bundled (cords), and the plurality of bundles may be arranged in parallel. In the plurality of bundles, adjacent bundles may be in contact with each other, or adjacent bundles may be separated from each other. A plurality of weft threads may be incorporated so as to cross the plurality of warp threads (or the plurality of bundles).
[0082] The polyester fiber may be surface-treated. The surface treatment is not particularly limited. For example, a conventionally known surface treatment may be used.
[0083] In the laminate of the present invention, so long as the vulcanized rubber layer A is adjacent to the vulcanized rubber layer B, the arrangement of the polyester fiber as the reinforcing layer in the laminate of the present invention is not particularly limited. The polyester fiber reinforcing layer is preferably laminated on the vulcanized rubber layer B on the side opposite to the side on which the vulcanized rubber layer A is laminated. The polyester fiber reinforcing layer is preferably laminated with the vulcanized rubber layer B-2.
[0084] When the polyester fiber is laminated with the vulcanized rubber layer B-2, for example, the polyester fiber may be disposed on top of the vulcanized rubber layer B-2 (vulcanized rubber layer B-2 / polyester fiber) or between adjacent vulcanized rubber layers B-2 (vulcanized rubber layer B-2 / polyester fiber / vulcanized rubber layer B-2). When polyester fibers are disposed between adjacent vulcanized rubber layers B-2, the polyester fibers may be integrated with the adjacent vulcanized rubber layers B-2 and embedded (covered) in the vulcanized rubber layers B-2.
[0085] Each of the vulcanized rubber layer A, the vulcanized rubber layers B-1 and B-2, and the reinforcing layer may be a single layer or multiple layers.
[0086] In the laminate of the present invention, the vulcanized rubber layer B has a vulcanized rubber layer B-1 containing the above-mentioned acrylonitrile butadiene rubber and a vulcanized rubber layer B-2 containing the above-mentioned styrene butadiene rubber, It is preferable that the vulcanized rubber layer B-1, the vulcanized rubber layer A, and the vulcanized rubber layer B-2 are laminated in this order. In the above embodiment, it is preferable that the vulcanized rubber layer B-1 is adjacent to the vulcanized rubber layer A, and the vulcanized rubber layer A is adjacent to the vulcanized rubber layer B-2. In the above embodiment, the polyester fiber as the reinforcing layer may be the same as that described above. In particular, the polyester fiber is preferably laminated with the vulcanized rubber layer B-2, and more preferably disposed between adjacent vulcanized rubber layers B-2.
[0087] The laminate of the present invention can be produced, for example, by layering the rubber composition of the present invention on a rubber composition BB-1 containing acrylonitrile butadiene rubber, layering a rubber composition BB-2 containing styrene butadiene rubber on the above-mentioned rubber composition of the present invention, layering polyester fiber thereon, and further layering another rubber composition BB-2 on the above to obtain an unvulcanized laminate, and vulcanizing the unvulcanized laminate under conditions of, for example, 50 to 150° C. After vulcanization, the rubber composition BB-1 becomes the vulcanized rubber layer B-1, the rubber composition of the present invention becomes the vulcanized rubber layer A, and the rubber composition BB-2 becomes the vulcanized rubber layer B-2. In the above case, the vulcanized rubber layer B-1 can be adjacent to the vulcanized rubber layer A, and the vulcanized rubber layer A can be adjacent to the vulcanized rubber layer B-2. In the above case, the rubber composition BB-2 on the rubber composition of the present invention, the polyester fiber on that, and the rubber composition BB-2 on that are integrated after vulcanization, and the polyester fiber can be embedded (covered) in the vulcanized rubber layer B-2.
[0088] [Marine hose] The marine hose of the present invention is a marine hose formed using the rubber composition of the present invention. The rubber composition used in the marine hose of the present invention is not particularly limited as long as it is the rubber composition of the present invention.
[0089] There is no particular limitation as to which component of a marine hose the rubber composition of the present invention is used.
[0090] The marine hose of the present invention comprises an innermost layer, an interlayer adhesive layer, and a carcass layer laminated in this order, the innermost layer is a vulcanized rubber layer containing acrylonitrile butadiene rubber, the interlayer adhesive layer is a vulcanized rubber layer formed using the rubber composition of the present invention, One of the preferred embodiments of the marine hose is one in which the carcass layer has a vulcanized rubber layer containing styrene-butadiene rubber and polyester fibers. The innermost layer, the interlayer adhesive layer, and the carcass layer may each independently be a single layer or multiple layers.
[0091] (Innermost layer) In the marine hose of the present invention, the innermost layer is a vulcanized rubber layer containing acrylonitrile butadiene rubber. The vulcanized rubber layer containing acrylonitrile-butadiene rubber as the innermost layer is the same as the vulcanized rubber layer B-1 containing acrylonitrile-butadiene rubber in the laminate of the present invention. The thickness of the innermost layer (as a whole) can usually be set to 1.5 to 8.0 mm.
[0092] (Interlayer adhesive layer) In the marine hose of the present invention, the interlayer adhesive layer is a vulcanized rubber layer formed using the rubber composition of the present invention. The interlayer adhesive layer is the same as the vulcanized rubber layer A in the laminate of the present invention. The thickness of the interlayer adhesive layer (as a whole) can usually be set to 0.5 to 2.0 mm.
[0093] (Carcass layer) In the marine hose of the present invention, the carcass layer has a vulcanized rubber layer containing styrene-butadiene rubber and polyester fibers. The vulcanized rubber layer containing styrene-butadiene rubber in the carcass layer is the same as the vulcanized rubber layer B-2 containing styrene-butadiene rubber in the laminate of the present invention. The polyester fiber contained in the carcass layer is the same as the polyester fiber contained in the reinforcing layer in the laminate of the present invention. The thickness of the carcass layer (single layer) can usually be set to 1.0 to 3.0 mm.
[0094] In one preferred embodiment of the marine hose of the present invention, for example, the innermost layer is adjacent to the interlayer adhesive layer, and the interlayer adhesive layer is adjacent to the vulcanized rubber layer containing styrene-butadiene rubber contained in the carcass layer.
[0095] (outer layer) The marine hose of the present invention may further have an outer layer on the above-mentioned carcass layer. The outer layer is not particularly limited. For example, the outer layer may be a rubber layer. Examples of the rubber contained in the outer layer include natural rubber and / or synthetic rubber. The thickness of the outer layer can be, for example, 2.0 to 10.0 mm.
[0096] The marine hose of the present invention may have a further layer between the carcass layer and the outer layer. The further layer is not particularly limited as long as it is a layer that a marine hose can normally have between the carcass layer and the outer layer. Examples include a metal layer (e.g., a layer in which wire-shaped metal is wound in a spiral shape) and a rubber layer for maintaining the shape of the marine hose. The metal layer is not particularly limited. Examples include conventionally known metal layers. The same applies to the rubber layer for maintaining the shape of the marine hose.
[0097] (Marine hose size) The inner diameter of the marine hose of the present invention is not particularly limited and can be, for example, 10 to 30 inches. The length of the marine hose of the present invention is not particularly limited and can be, for example, 5 to 20 meters.
[0098] (Marine hose manufacturing method)
[0099] In the method for producing the marine hose of the present invention, for example, a sheet of a rubber composition containing acrylonitrile butadiene rubber for the innermost layer is first wound around a mandrel, and a sheet of the composition of the present invention is then wound thereon. The method for winding the sheet of the composition of the present invention around the mandrel is not particularly limited, but examples include a method of winding the sheets while partially overlapping each other (for example, spirally). Next, a sheet for the carcass layer, in which polyester fibers are coated with a rubber composition containing styrene butadiene rubber, is wound on the sheet of the composition of the present invention. Next, a metal wire is wound spirally on the sheet for the carcass, and a rubber layer composition for maintaining the shape of the marine hose is layered on top of the metal wire, and finally a sheet of the rubber composition for the outer layer is layered on top of the metal wire. By subjecting the laminate obtained as described above to vulcanization or the like, a marine hose having an interlayer adhesive layer formed from the composition of the present invention can be produced.
[0100] Since marine hoses are generally large, one preferred embodiment of vulcanizing the laminate is to heat the laminate at an initial stage, for example, at a temperature in the range of 100 to 110°C for 1 to 1.5 hours, and then heat the laminate at a temperature in the range of 130 to 147°C to complete the vulcanization.
[0101] As described above, in a marine hose manufactured by laminating the rubber composition of the present invention on a rubber composition containing acrylonitrile-butadiene rubber for the innermost layer, laminating a rubber composition containing styrene-butadiene rubber coated with polyester fiber for the carcass layer on the rubber composition of the present invention, laminating other layers as necessary, and vulcanizing the above laminate, the interlayer adhesive layer formed from the composition of the present invention can bond the innermost layer and the carcass layer. Furthermore, since the rubber composition of the present invention provides a cured product with excellent strength, when the rubber composition of the present invention is used as the rubber constituting the interlayer adhesive layer of a marine hose, a marine hose with excellent durability can be produced. EXAMPLES
[0102] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these.
[0103] <Production of Rubber Composition> Each component in Table 1 below was used in the composition (parts by mass) shown in the table. First, the components shown in Table 1 below, except for sulfur, vulcanization accelerators such as sulfenamide-based vulcanization accelerators, hexamine, and melamine compounds, were mixed in a 1.5-liter sealed mixer at 100°C for 5 minutes to obtain a master batch. Next, sulfur, vulcanization accelerators such as sulfenamide-based vulcanization accelerators, hexamine, and melamine compounds were added to the obtained master batch in the amounts (parts by mass) shown in Table 1 below, and these were mixed in an open roll at 50°C to obtain a rubber composition.
[0104] (Preparation of Rubber Sheet X) Using each of the rubber compositions produced as described above, a rubber sheet X having a thickness of 3.0 mm in an unvulcanized state was obtained.
[0105] [Table 1]
[0106] [Table 2]
[0107] [Table 3]
[0108] Details of each component shown in Table 1 are as follows. SBR: Styrene butadiene copolymer. Tufden 2000R (Asahi Kasei Corporation). Weight average molecular weight 320,000, styrene content 25% by mass.
[0109] NBR: Acrylonitrile butadiene copolymer. Nipol DN 401 (Zeon Corporation). AN content 18.0 mass%. Mooney viscosity 78. Not hydrogenated.
[0110] NR: Natural rubber. STR-20 (TECK BEE HANG CO., LTD.) Mixture of polyvinyl chloride resin and plasticizer: Popiron R♯0715-1 (Popiron Chemical Co., Ltd.) Carbon black: Asahi Thermal (Asahi Carbon Co., Ltd.), nitrogen adsorption specific surface area 24 m 2 / g, dibutyl phthalate oil absorption 28ml / 100g. FT class carbon black
[0111] Silica: Nipsil AQ (Tosoh Silica Corporation) pH 6.4
[0112] Zinc oxide: Three types of zinc oxide (Seido Chemical Industry Co., Ltd.) Stearic acid: Stearic acid YR (NOF CORPORATION)
[0113] Resorcinol resin: Resorcinol (Sumitomo Chemical Co., Ltd.). Condensation product of resorcin (1,3-benzenediol) and formaldehyde.
[0114] Aroma oil: A-OMIX (Sankyo Yuka Kogyo Co., Ltd.) Sulfur: Oil treatment sulfur (Hosoi Chemical Co., Ltd.) Sulfenamide vulcanization accelerator: Noccela NS-P (Ouchi Shinko Chemical Industry Co., Ltd.). N-tert-butyl-2-benzothiazolyl sulfenamide
[0115] Hexamine: Hexamethylenetetramine (structure below). Suncerer HT-PO (Sanshin Chemical Industry Co., Ltd.) [ka]
[0116] Melamine compound 1: Sumikanol 507AP (BARA CHEMICAL CO., LTD.). A mixture of the compound with the following structure (hexamethylolmelamine pentamethyl ether), its dimer and oligomer, silica, and plasticizer. [ka]
[0117] In the melamine compound 1, the content of the net melamine compounds (hexamethylolmelamine pentamethyl ether, its dimer and oligomer) was 65 mass%. The values shown in the "Melamine Compound 1" column are the amounts of the above mixture. When the amount of melamine compound 1 (amount as the above mixture) is 2.74 parts by mass (Example 12), the total amount of silica and plasticizer in the used melamine compound 1 is about 1.0 part by mass. Therefore, Example 12 contains silica in a total amount of more than 20 parts by mass and less than 21.0 parts by mass.
[0118] Melamine compound 2: Cyrez 964RPC (ALLnex USA Inc.). A compound having the following structure (hexamethylolmelamine hexamethyl ether) and / or its condensate. [ka]
[0119] Coumarone resin: Soft Coumarone 25B (Kobe Oil Chemical Industry Co., Ltd.) Phenolic resin (alkylphenol resin): Condensation product of alkylphenol and formaldehyde. PP 5121 (Gunei Chemical Industry Co., Ltd.)
[0120] (Preparation of Rubber Composition for Vulcanized Rubber Layer B-1 Containing NBR) Each component in Table 2 below was used in the composition (parts by mass) shown in the table. First, the components shown in Table 2 below, except for sulfur, vulcanization accelerator, and hexamine, were mixed in a 1.5-liter closed mixer at 100°C for 5 minutes to obtain a master batch. Next, sulfur, vulcanization accelerator, and hexamine were added to the obtained master batch in the amounts (parts by mass) shown in Table 2 below, and these were mixed in an open roll at 50°C to obtain a rubber composition for vulcanized rubber layer B-1 containing NBR.
[0121] [Table 4]
[0122] (Preparation of Rubber Sheet Y) Using the rubber composition for the vulcanized rubber layer B-1 prepared as described above, a rubber sheet Y having a thickness of 3.0 mm in an unvulcanized state was obtained.
[0123] (Preparation of Rubber Composition for Vulcanized Rubber Layer B-2 Containing SBR) Each component in Table 3 below was used in the composition (parts by mass) shown in the same table. First, among the components shown in Table 3 below, the components excluding sulfur and vulcanization accelerator DM were mixed in a 1.5-liter sealed mixer at 100 °C for 5 minutes to obtain a masterbatch. Next, sulfur and vulcanization accelerator DM were added to the obtained masterbatch in the amounts (parts by mass) shown in Table 3 below, and these were mixed on an open roll at 50 °C to obtain a rubber composition for vulcanized rubber layer B-2 containing SBR.
[0124]
Table 5
[0125] (Preparation of Rubber Sheet Z) Using the rubber composition for vulcanized rubber layer B-2 prepared as described above and a polyester cord (a cord of 3-ply polyester fibers (polyethylene terephthalate fibers) of 1670 dtex, a reed-like fabric. Manufactured by HYOSUNG ADVANCED MATERIALS CORPORATION. Thickness 1.0 mm), an unvulcanized rubber sheet Z (thickness of one sheet is 1.5 mm) in which the polyester cords were aligned (reed-like state) and embedded (coated) in the rubber composition for vulcanized rubber layer B-2 was obtained.
[0126] <<Evaluation of Adhesion>> In the present invention, the following evaluation of adhesion was carried out. The results are shown in Table 1. <Adhesion with Vulcanized Rubber Layer B-1 Containing NBR> (Preparation of Laminated Body XY) Each rubber sheet X manufactured as described above and the rubber sheet Y prepared as described above (the vulcanized rubber layer B-1 containing NBR formed into a sheet as described above) were stacked together to form a two-layer rubber sheet, and the two-layer rubber sheet was steam vulcanized for 60 minutes under conditions of 148°C and a surface pressure of 4.0 MPa to obtain a laminate XY (width 25 mm, thickness 6 mm, length 100 mm, thickness of rubber sheet X after vulcanization 3 mm, thickness of rubber sheet Y after vulcanization 3 mm). When the rubber sheets X and Y were stacked together, a small amount of cellophane was sandwiched between the rubber sheets X and Y from one end of the 25 mm width. After the vulcanization, the cellophane was removed from the laminate XY, and a gripping portion was made to attach the laminate XY to a gripping tool for a peel test described later.
[0127] (Peel test) In accordance with JIS K6256-1:2013, a peel test was performed using the laminate XY described above, in which the gripping portions of the laminate XY were each held by a tensile tester, and the vulcanized rubber sheet Y was peeled off from the vulcanized rubber sheet X at a peel angle of 180° at a speed of 50 mm / min.
[0128] (Evaluation Criteria) In the present invention, when the laminate XY does not progress in peeling from the state at the start of the peel test and the vulcanized rubber sheet X or the vulcanized rubber sheet Y held by the gripping tool breaks, the adhesion between the cured product obtained from the rubber composition and the vulcanized rubber layer B-1 containing NBR is evaluated as excellent, and this is indicated by "O". In the above peel test, if the laminate XY further peeled off from the state at the start of the peel test, the adhesion between the cured product obtained from the rubber composition and the vulcanized rubber layer B-1 containing NBR was evaluated as poor, and this was indicated by "X". The NBR-containing vulcanized rubber layer B-1 corresponds to the innermost layer in the marine hose, and the cured product obtained from the rubber composition corresponds to the interlayer adhesive layer in the marine hose. Therefore, the adhesion between the innermost layer and the interlayer adhesive layer in the marine hose can be evaluated based on the adhesion between the cured product obtained from the rubber composition and the NBR-containing vulcanized rubber layer B-1.
[0129] <Adhesion to the vulcanized rubber layer B-2 containing SBR> (Preparation of laminate XZ) One rubber sheet X manufactured as described above and two rubber sheets Z prepared as described above (the vulcanized rubber layer B-2 containing SBR formed into a sheet as described above) were stacked in the order of rubber sheet X, the first rubber sheet Z, and the second rubber sheet Z to form a three-layer rubber sheet (rubber sheet X / the first rubber sheet Z / the second rubber sheet Z). The three-layer rubber sheet was steam vulcanized at 148 °C and a surface pressure of 4.0 MPa for 200 minutes to obtain a laminate XZ (the width of the laminate XZ was 25 mm, the thickness was 6 mm, and the length was 100 mm. The thickness of the rubber sheet X after vulcanization was 3 mm, and the total thickness of the two rubber sheets Z after vulcanization was 3 mm). In the above laminate XZ, the two rubber sheets Z were arranged in the laminate XZ so that the polyester cords (bundles of warp threads) of the rubber sheet Z constituting the laminate XZ were parallel to the longitudinal direction of the laminate XZ. Also, when stacking each rubber sheet X and the rubber sheet Z, cellophane was slightly sandwiched between the rubber sheet X and the first rubber sheet Z from one end with a width of 25 mm. After the above vulcanization, the cellophane was removed from the laminate XZ, and a gripping portion for attaching the laminate XZ to the gripping tool for the peel test described later was made. In the obtained laminate XZ, there is a vulcanizate of the rubber composition for the vulcanized rubber layer B-2 between the rubber sheet X and the polyester cord of the first rubber sheet Z (the one in which the polyester cord is embedded (coated) in the rubber composition for the vulcanized rubber layer B-2), and the rubber sheet X and the polyester cord do not contact directly.
[0130] (Peel test) In accordance with JIS K6256-1:2013, using the above laminate XZ, a peel test was conducted in which the gripping portions of the laminate XZ were respectively gripped by a tensile testing machine, and the vulcanized rubber sheet Z was peeled from the vulcanized rubber sheet X at a peeling angle of 180° at a speed of 50 mm / min, and the peel strength (N / mm) was measured.
[0131] (Evaluation criteria) In the present invention, when the peel strength measured as described above was 6.2 N / mm or more, the adhesion between the cured product obtained from the rubber composition and the vulcanized rubber layer B-2 containing SBR was evaluated to be excellent. The higher the peel strength, the better the adhesiveness was evaluated to be. On the other hand, when the peel strength was less than 6.2 N / mm, the adhesion between the cured product obtained from the rubber composition and the vulcanized rubber layer B-2 containing SBR was evaluated as being poor. The layer formed of the vulcanized rubber layer containing SBR and the polyester fiber corresponds to the carcass layer in the marine hose, so the adhesion between the interlayer adhesive layer and the carcass layer in the marine hose can be evaluated based on the adhesion between the cured product obtained from the rubber composition and the vulcanized rubber layer B-2 containing SBR.
[0132] <<Evaluation of tensile properties>> The following tensile properties were evaluated using each of the rubber compositions produced as described above and shown in Table 1. The results are shown in Table 1. (Preparation of initial test specimen) Each of the rubber compositions produced as described above was vulcanized for 60 minutes using a press molding machine at 148° C. under a surface pressure of 3.0 MPa to prepare a vulcanized sheet having a thickness of 2 mm. The above vulcanized sheet was punched into JIS No. 3 dumbbells to prepare initial test specimens.
[0133] (Tensile test) Using each of the initial test pieces prepared as described above, a tensile test was performed at a tensile speed of 500 mm / min at 23°C in accordance with JIS K6251:2017, and the tensile strength (TB, unit: MPa) and elongation at break (EB, unit: %) were measured.
[0134] (Evaluation criteria: strength of cured product) In the present invention, the strength of the cured product was evaluated by the elongation at break measured as described above. In the present invention, when the above-mentioned elongation at break was 400% or more, the strength of the cured product was evaluated as excellent. Moreover, it was evaluated that the greater the elongation at break, the better the strength of the cured product. On the other hand, when the elongation at break was less than 400%, the strength of the cured product was evaluated as poor. The above cured product corresponds to the cured product of the rubber composition of the present invention, the vulcanized rubber layer A in the laminate of the present invention, and the interlayer adhesive layer that the marine hose of the present invention may have, and therefore the strength of the vulcanized rubber layer A in the laminate of the present invention and the strength of the interlayer adhesive layer in the marine hose can be evaluated based on the strength of the above cured product.
[0135] As is clear from the results shown in Table 1, Comparative Example 1, which did not contain an acrylonitrile-butadiene copolymer but contained natural rubber instead, and did not contain a specific melamine compound but contained hexamine instead, had poor adhesion to the vulcanized rubber layer B-1 containing NBR and poor adhesion to the vulcanized rubber layer B-2 containing SBR. Comparative Example 2, which did not contain the specified melamine compound but contained hexamine instead, had poor adhesion to the vulcanized rubber layer B-2 containing SBR, and poor strength of the cured product. Comparative Example 3, which did not contain the specified melamine compound, had poor adhesion to the vulcanized rubber layer B-1 containing NBR and poor adhesion to the vulcanized rubber layer B-2 containing SBR. Comparative Examples 4 and 7 to 8, which did not contain the specified melamine compound but contained hexamine instead, had poor adhesion to the vulcanized rubber layer B-2 containing SBR. Comparative Example 5, in which the amount of the acrylonitrile butadiene copolymer was less than the predetermined amount, had poor adhesion to the vulcanized rubber layer B-1 containing NBR. Comparative Example 6, in which the amount of styrene-butadiene copolymer was less than the prescribed amount, had poor adhesion to the vulcanized rubber layer B-2 containing SBR. Comparative Example 9, which did not contain silica, had poor strength in the cured product. Comparative Examples 10 and 13, which did not contain an acrylonitrile butadiene copolymer but contained natural rubber instead, had poor adhesion to the vulcanized rubber layer B-1 containing NBR. Comparative Example 11, which did not contain an acrylonitrile butadiene copolymer but contained natural rubber instead, and did not contain a resorcinol resin but contained a cresol resin instead, had poor adhesion to the vulcanized rubber layer B-1 containing NBR. Comparative Example 12, which did not contain an acrylonitrile butadiene copolymer but contained natural rubber instead and did not contain the specified melamine compound, had poor adhesion to the vulcanized rubber layer B-1 containing NBR.
[0136] In contrast, the rubber composition of the present invention has excellent adhesion between a cured product obtained from the rubber composition of the present invention and a rubber layer containing acrylonitrile butadiene rubber or styrene butadiene rubber (i.e., the cured product obtained from the rubber composition of the present invention has excellent adhesion to a rubber layer containing acrylonitrile butadiene rubber, and to a rubber layer containing styrene butadiene rubber), and the strength of the cured product is excellent.
Claims
1. A rubber component containing 30 to 80% by mass of an acrylonitrile butadiene copolymer and 20 to 70% by mass of a styrene butadiene copolymer; Silica and Resorcinol resin, A rubber composition comprising at least one melamine compound selected from the group consisting of methylol melamines, methylol melamine alkyl ethers, and condensates thereof.
2. The rubber composition according to claim 1, wherein the content of the melamine compound is 30 to 250 mass % of the content of the resorcinol resin.
3. Furthermore, it contains a sulfenamide vulcanization accelerator, The rubber composition according to claim 1 or 2, wherein the content of the sulfenamide vulcanization accelerator is 0.7 to 1.2 parts by mass based on 100 parts by mass of the rubber component.
4. The rubber composition according to any one of claims 1 to 3, wherein the content of the silica is 10 to 40 parts by mass based on 100 parts by mass of the rubber component.
5. The rubber composition according to any one of claims 1 to 4, wherein the content of the resorcinol resin is 0.3 to 8.0 parts by mass based on 100 parts by mass of the acrylonitrile butadiene copolymer.
6. The rubber composition according to any one of claims 1 to 5, which is used to form a marine hose.
7. A vulcanized rubber layer A formed using the rubber composition according to any one of claims 1 to 5; A vulcanized rubber layer B having one or both of a vulcanized rubber layer B-1 containing an acrylonitrile butadiene rubber and a vulcanized rubber layer B-2 containing a styrene butadiene rubber; The reinforcing layer has polyester fibers, The vulcanized rubber layer A is adjacent to the vulcanized rubber layer B, forming a laminate.
8. The vulcanized rubber layer B includes a vulcanized rubber layer B-1 containing the acrylonitrile butadiene rubber and a vulcanized rubber layer B-2 containing the styrene butadiene rubber, The laminate according to claim 7, wherein the vulcanized rubber layer B-1, the vulcanized rubber layer A, and the vulcanized rubber layer B-2 are laminated in this order.
9. A marine hose formed using the rubber composition according to any one of claims 1 to 5.
10. The innermost layer, the interlayer adhesive layer, and the carcass layer are laminated in this order, the innermost layer is a vulcanized rubber layer containing acrylonitrile butadiene rubber, the interlayer adhesive layer is a vulcanized rubber layer formed using the rubber composition, The marine hose according to claim 9 , wherein the carcass layer has a vulcanized rubber layer containing styrene-butadiene rubber and polyester fibers.
11. The marine hose according to claim 10 , wherein the innermost layer is adjacent to the interlayer adhesive layer, and the interlayer adhesive layer is adjacent to the vulcanized rubber layer containing the styrene-butadiene rubber contained in the carcass layer.
Citation Information
Patent Citations
Adhesive composition
JP1984159872A
Hose
JP1995063288A
Rubber composition for rubber between layers of hose, and hose
JP2004250696A
Rubber composition and pneumatic tire
JP2014095020A
Hose rubber composition and hose
JP2017019984A