Manufacturing method of grain-oriented electrical steel sheet

The method strengthens inhibitor heat resistance and increases Goss-oriented grains at the coil ends of grain-oriented electrical steel sheets, addressing non-uniform magnetic properties and iron loss issues, thereby enhancing transformer stability.

JP7557125B2Active Publication Date: 2024-09-27NIPPON STEEL CORPORATION
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2020108587
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-06-24
Publication Date
2024-09-27
Estimated Expiration
2040-06-24

AI Technical Summary

Technical Problem

Existing methods for manufacturing grain-oriented electrical steel sheets fail to ensure stable and uniform magnetic properties along the length of the coil, particularly at the longitudinal ends, due to inconsistent inhibitor strength and temperature fluctuations, which affect iron loss and magnetic flux density.

Method used

A manufacturing method involving controlled pre-pickling treatment, pickling treatment conditions, and atmospheric nitrogen partial pressure during final annealing, combined with rapid heating in the temperature rising process of primary recrystallization annealing, to strengthen inhibitor heat resistance and increase Goss-oriented grains at the coil ends.

Benefits of technology

This method enhances magnetic flux density and achieves uniform magnetic properties along the coil length, ensuring stable operation of transformers by reducing iron loss variations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007557125000001
    Figure 0007557125000001
  • Figure 0007557125000002
    Figure 0007557125000002
Patent Text Reader

Abstract

To provide a grain-oriented electromagnetic steel sheet that has a good appearance and magnetic property.SOLUTION: One aspect of the present invention provides a method for manufacturing grain-oriented electromagnetic steel sheet that comprises a hot rolling step, a pickling pretreatment-containing pickling step, a cold rolling step, a primary recrystallization annealing step, a finish annealing step and a flattening annealing step. A chelating agent is applied to at least 80% of the center part in the coil longitudinal direction prior to the pickling, the pickling solution contains one or two or more of Cu, Hg, Ag, Pb, Cd, Co, Zn and Ni in a predetermined amount, the pH is -1.5 or more and less than 7, the liquid temperature is 15°C or more and 100°C or less, and the time for the steel sheet to be immersed in pickling solution is 5 seconds or more and 200 seconds or less, the primary recrystallization annealing comprises a step of raising temperature, a step of intermediate treatment after raising temperature and before decarburization annealing, and a step of decarburization annealing, and the nitrogen partial pressure in the annealing atmosphere at 600°C to 1100°C in the finish annealing is set at 50 vol% or more and 90 vol% or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a grain-oriented electrical steel sheet. [Background technology]

[0002] Grain-oriented electrical steel sheets contain about 2% to 5% by mass of Si, and the grain orientation of the steel sheet is called the Goss orientation, {110} <001> Grain-oriented electrical steel has excellent magnetic properties and is used, for example, as the core material for static inductors in transformers and other equipment.

[0003] In order to improve the magnetic properties of such grain-oriented electrical steel sheets, various developments have been made. In particular, with the recent demand for energy saving, grain-oriented electrical steel sheets are required to have even lower iron loss. In order to reduce the iron loss of grain-oriented electrical steel sheets, it is effective to increase the concentration of the crystal grains in the Goss orientation of the steel sheet to improve the magnetic flux density and reduce the hysteresis loss.

[0004] In the manufacture of grain-oriented electrical steel sheets, the crystal orientation is controlled by utilizing a catastrophic grain growth phenomenon called secondary recrystallization. However, in order to appropriately control the crystal orientation in secondary recrystallization, it is important to improve the heat resistance of fine precipitates in the steel, called inhibitors.

[0005] For example, the inhibitor is completely dissolved when the slab is heated before hot rolling, and then finely precipitated during hot rolling and the subsequent annealing process. Specifically, the inhibitor is used as an inhibitor in a method in which MnS and AlN are used as inhibitors and rolling is performed at a reduction rate of more than 80% in the final cold rolling process, as exemplified in Patent Document 1 below, or the inhibitor is used as an inhibitor in a method in which MnS and MnSe are used as inhibitors and two cold rolling processes are performed, as exemplified in Patent Document 2 below.

[0006] Patent Document 3 discloses a technique for manufacturing grain-oriented electrical steel sheet with excellent coating properties by controlling the conditions for hot-rolled sheet annealing and the conditions for pickling treatment. Patent Document 4 discloses a method for manufacturing grain-oriented electrical steel sheet with less variation in magnetic properties at the edge by controlling the cooling rate of hot-rolled sheet annealing in the coil width direction. Furthermore, Patent Document 5 discloses a technique for manufacturing grain-oriented electrical steel sheet with excellent magnetic properties by controlling the temperature rise process of primary recrystallization annealing and introducing microstrain during the temperature rise process.

[0007] Also, the following Patent Document 6 discloses a technique for manufacturing grain-oriented electrical steel sheet with low iron loss over the entire coil length by controlling the heat pattern during the temperature increase process of primary recrystallization annealing.Furthermore, the following Patent Document 7 discloses a technique for reducing the iron loss value of grain-oriented electrical steel sheet by strictly controlling the average grain size of crystal grains after secondary recrystallization and the deviation angle from the ideal orientation. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Special Publication No. 40-15644 [Patent Document 2] Special Publication No. 51-13469 [Patent Document 3] JP 2019-99827 A [Patent Document 4] Japanese Patent Application Publication No. 9-137225 [Patent Document 5] Japanese Patent Application Publication No. 6-212274 [Patent Document 6] International Publication No. 2014 / 049770 [Patent Document 7] Japanese Patent Application Publication No. 7-268567 Summary of the Invention [Problem to be solved by the invention]

[0009] In recent years, with the progress of global transformer efficiency regulations, there is an increasing demand for reduced iron loss in grain-oriented electrical steel sheets. On the other hand, since transformers are important equipment that support social infrastructure over the long term, it is important that they continue to operate stably. For this reason, grain-oriented electrical steel sheets, which are a major component, are also required to have the reliability to contribute to the stable operation of transformers. In particular, it is important for grain-oriented electrical steel sheets to have no significant difference in iron loss between the longitudinal ends of the coil (top and / or end parts, in other words, the start and / or end of the coil winding) and the longitudinal center part (parts other than the ends) in order to gain the trust of customers.

[0010] The above-mentioned Patent Document 3 discloses a technique for improving coating adhesion by creating a difference in the concentration of Mn or Cu between the steel sheet surface and the center of the sheet thickness. However, the technique for concentrating a specific component on the steel sheet surface is aimed only at improving the coating properties, and no technique for obtaining stable and good magnetic properties in the coil longitudinal direction of the steel sheet, particularly in the top and / or end portions, has been considered.

[0011] Patent Document 4 discloses a technique for reducing the variation in magnetic properties of the edge portions by slowing the cooling rate of the edge portions in the width direction of the steel sheet compared to the center portion in the width direction of the steel sheet in the cooling process of hot-rolled sheet annealing. However, this technique focuses on the fact that the temperature fluctuations are larger in the edge portions than in the center portion, and the precipitation behavior (size, distribution density) of precipitates such as MnS is unstable, and does not consider strengthening the precipitates themselves.

[0012] Furthermore, Patent Document 5 considers controlling the temperature rise process of the primary recrystallization annealing, but does not consider strengthening the inhibitor in the coil longitudinal direction, particularly in the top and / or end portions.

[0013] In addition, as disclosed in the above Patent Document 6, it has been confirmed that the magnetic properties of grain-oriented electrical steel sheets can be significantly affected by rapidly increasing the temperature between 500°C and 600°C at 100°C / s or more during the temperature increase process of primary recrystallization annealing. The above Patent Document 7 discloses that the temperature increase rate up to 850°C is set to 300°C / s or 450°C / s during the temperature increase process of primary recrystallization annealing.

[0014] However, the above Patent Documents 6 and 7 did not examine in detail what effect would be caused on the magnetic properties of the grain-oriented electrical steel sheet when the inhibitor is changed in the longitudinal direction of the steel sheet coil.

[0015] Therefore, the present invention has been made in consideration of the above-mentioned problems, and an object of the present invention is to provide a new and improved method for producing grain-oriented electrical steel sheet, which makes it possible to produce grain-oriented electrical steel sheet having excellent magnetic properties along the longitudinal direction of the coil by controlling the pickling pretreatment and pickling treatment conditions to enhance the inhibitor heat resistance of the longitudinal ends of the coil (top and / or end portions), and by appropriately increasing the atmospheric nitrogen partial pressure in finish annealing to achieve high magnetic flux density. [Means for solving the problem]

[0016] In order to solve the above problems, according to one aspect of the present invention, a step of heating a slab containing, by mass%, C: 0.02% or more and 0.10% or less, Si: 2.5% or more and 4.5% or less, Mn: 0.01% or more and 0.50% or less, the total of one or more of S, Se and Te: 0.001% or more and 0.050% or less, acid-soluble Al: more than 0.05% or less, N: more than 0% and 0.015% or less, with the balance being Fe and impurities, and hot rolling the slab to obtain a hot-rolled steel sheet; A step of obtaining a pickled sheet by subjecting the hot-rolled steel sheet to pickling, or obtaining a hot-rolled annealed sheet by subjecting the hot-rolled steel sheet to hot-rolled sheet annealing, and then obtaining a pickled sheet by subjecting the hot-rolled annealed sheet to pickling; A step of obtaining a cold-rolled steel sheet by cold rolling the pickled sheet; A step of subjecting the cold-rolled steel sheet to primary recrystallization annealing; A step of applying an annealing separator containing MgO to the surface of the cold-rolled steel sheet after the primary recrystallization annealing, and then performing finish annealing; A step of applying an insulating coating to the steel sheet after the finish annealing and then performing planarization annealing, Prior to the pickling, a chelating agent is applied to at least 80% of the central portion of the coil in the longitudinal direction; In the pickling, the pickling solution contains one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn and Ni, the total concentration of each element is 0.0001% or more and 1.0000% or less, the pH is -1.5 or more and less than 7, the liquid temperature is 15°C or more and 100°C or less, and the steel sheet is immersed in the pickling solution for 5 seconds or more and 200 seconds or less, The present invention provides a method for producing a grain-oriented electrical steel sheet, characterized in that the nitrogen partial pressure in the annealing atmosphere at 600° C. to 1100° C. in the final annealing is set to 50 vol % or more and 90 vol % or less.

[0017] In addition, in the heating for the primary recrystallization, the average heating rate in the temperature range of 550° C. to 700° C. may be 100° C. / s or more and 3000° C. / s or less. Effect of the Invention

[0018] According to the present invention, a new and improved method for producing grain-oriented electrical steel sheet can be provided, which is capable of producing grain-oriented electrical steel sheet with excellent magnetic properties and high magnetic flux density by combining a technique for enhancing the inhibitor heat resistance of the longitudinal ends of the coil by controlling the conditions before pickling treatment and the conditions for pickling treatment, a technique for increasing the Goss-oriented grains at the longitudinal ends of the coil by optionally performing a rapid heat treatment in the temperature rising process of primary recrystallization annealing, and a technique for appropriately increasing the atmospheric nitrogen partial pressure in finish annealing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Preferred embodiments of the present invention will be described in detail below. Unless otherwise specified, the expression "A to B" for numerical values ​​A and B means "A or more and B or less." In such an expression, when a unit is added only to numerical value B, the unit is also applied to numerical value A.

[0020] [Method of manufacturing grain-oriented electrical steel sheets] Means for Solving the Problems The present inventors have conducted extensive research into methods for producing grain-oriented electrical steel sheets in order to improve the magnetic properties of the grain-oriented electrical steel sheets, and as a result have discovered the following.

[0021] Specifically, the inventors discovered that by optimizing the conditions before pickling, the pickling conditions, and the atmospheric nitrogen partial pressure conditions during finish annealing, it is possible to control the inhibitors at the coil longitudinal ends of the steel sheet and improve the magnetic properties.

[0022] The present inventors have taken the above findings into consideration and arrived at the present invention. One embodiment of the present invention is a method for producing a grain-oriented electrical steel sheet having the following configuration.

[0023] a step of heating a slab containing, by mass%, C: 0.02% or more and 0.10% or less, Si: 2.5% or more and 4.5% or less, Mn: 0.01% or more and 0.50% or less, the total of one or more of S, Se and Te: 0.001% or more and 0.050% or less, acid-soluble Al: more than 0.0% and 0.05% or less, N: more than 0% and 0.015% or less, with the balance being Fe and impurities, and hot rolling the slab to obtain a hot-rolled steel sheet; A step of obtaining a pickled sheet by subjecting the hot-rolled steel sheet to pickling, or obtaining a hot-rolled annealed sheet by subjecting the hot-rolled steel sheet to hot-rolled sheet annealing, and then obtaining a pickled sheet by subjecting the hot-rolled annealed sheet to pickling; A step of obtaining a cold-rolled steel sheet by cold rolling the pickled sheet; A step of subjecting the cold-rolled steel sheet to primary recrystallization annealing; A step of applying an annealing separator containing MgO to the surface of the cold-rolled steel sheet after the primary recrystallization annealing, and then performing finish annealing; A step of applying an insulating coating to the steel sheet after the finish annealing and then performing planarization annealing, Prior to the pickling, a chelating agent is applied to at least 80% of the central portion of the coil in the longitudinal direction; In the pickling, the pickling solution contains one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn and Ni, the total concentration of each element is 0.0001% or more and 1.0000% or less, the pH is -1.5 or more and less than 7, the liquid temperature is 15°C or more and 100°C or less, and the steel sheet is immersed in the pickling solution for 5 seconds or more and 200 seconds or less, The nitrogen partial pressure in the annealing atmosphere at 600° C. to 1100° C. in the finish annealing is set to 50 vol % or more and 90 vol % or less. In the heating for the primary recrystallization, the average heating rate in the temperature range of 550° C. to 700° C. may be 100° C. / s or more and 3000° C. / s or less.

[0024] The method for manufacturing the grain-oriented electrical steel sheet according to this embodiment will be specifically described below.

[0025] [Slab composition] First, the composition of the slab used in the grain-oriented electrical steel sheet according to this embodiment will be described. In the following, unless otherwise specified, the notation "%" will represent "mass %". The remainder of the slab other than the elements described below is Fe and impurities. Here, impurities refer to components contained in raw materials or components mixed in during the manufacturing process, and components that are not intentionally contained in the steel sheet. The chemical composition of the slab, which is the material for the grain-oriented electrical steel sheet, is basically similar to the composition of the grain-oriented electrical steel sheet. However, in the manufacture of general grain-oriented electrical steel sheets, some of the contained elements are discharged outside the system by decarburization annealing and purification annealing during the manufacturing process, so that the chemical composition of the slab, which is the material, and the grain-oriented electrical steel sheet, which is the final product, are different. The slab composition can be appropriately adjusted in consideration of the effects of decarburization annealing and purification annealing during the manufacturing process so that the grain-oriented electrical steel sheet has the desired characteristics.

[0026] The C (carbon) content is 0.02% or more and 0.10% or less. C has various roles, but if the C content is less than 0.02%, the grain size becomes excessively large when the slab is heated, which increases the iron loss value of the final grain-oriented electrical steel sheet, which is not preferable. If the C content exceeds 0.10%, the decarburization time becomes long during decarburization after cold rolling, which is not preferable, and the manufacturing cost increases. In addition, if the C content exceeds 0.10%, decarburization is likely to be incomplete, which is not preferable, as there is a possibility that magnetic aging will occur in the final grain-oriented electrical steel sheet. Therefore, the C content is 0.02% or more and 0.10% or less, and preferably 0.05% or more and 0.09% or less.

[0027] The content of Si (silicon) is 2.5% or more and 4.5% or less. Si increases the electrical resistance of the steel sheet, thereby reducing eddy current loss, which is one of the causes of iron loss. If the content of Si is less than 2.5%, it is not preferable because it becomes difficult to sufficiently suppress the eddy current loss of the final grain-oriented electrical steel sheet. If the content of Si is more than 4.5%, it is not preferable because the workability of the grain-oriented electrical steel sheet decreases. Therefore, the content of Si is 2.5% or more and 4.5% or less, and preferably 2.7% or more and 4.0% or less.

[0028] The content of Mn (manganese) is 0.01% or more and 0.50% or less. Mn forms MnS, MnSe, MnTe, etc., which are inhibitors that affect secondary recrystallization. If the content of Mn is less than 0.01%, the absolute amount of MnS, MnSe, and MnTe that cause secondary recrystallization is insufficient, which is not preferable. If the content of Mn is more than 0.15%, it is not preferable because it becomes difficult to dissolve Mn during slab heating. In addition, if the content of Mn is more than 0.15%, it is not preferable because the precipitate size of MnS, MnSe, and MnTe, which are inhibitors, tends to become coarse, and the optimal size distribution as an inhibitor is impaired. Therefore, the content of Mn is 0.01% or more and 0.50% or less, preferably 0.01% or more and 0.30% or less. More preferably, it is 0.03% or more and 0.15% or less.

[0029] The total content of S (sulfur), Se (selenium) and Te (tellurium) is 0.001% or more and 0.050% or less. S, Se and Te form an inhibitor together with the above-mentioned Mn. All three of S, Se and Te may be contained in the slab, but at least one of them should be contained in the slab. If the total content of S, Se and Te is outside the above range, it is not preferable because a sufficient inhibitor effect cannot be obtained. Therefore, the total content of S, Se and Te is 0.001% or more and 0.050% or less, preferably 0.001% or more and 0.040% or less.

[0030] The content of acid-soluble Al (acid-soluble aluminum) is more than 0% and not more than 0.05%. Acid-soluble Al constitutes an inhibitor necessary for producing a grain-oriented electrical steel sheet with high magnetic flux density. When the content of acid-soluble Al is 0, AlN does not exist, and the inhibitor strength is insufficient, so that good magnetic properties may not be obtained, which is not preferable. When the content of acid-soluble Al is more than 0.05%, AlN precipitated as an inhibitor becomes coarse, which reduces the inhibitor strength, which is not preferable. Therefore, the content of acid-soluble Al is more than 0% and not more than 0.05%, and preferably more than 0% and not more than 0.04%.

[0031] The N (nitrogen) content is more than 0% and not more than 0.015%. N forms AlN, which is an inhibitor, together with the above-mentioned acid-soluble Al. If the N content is outside the above range, it is not preferable because a sufficient inhibitor effect cannot be obtained. Therefore, the N content is more than 0% and not more than 0.015%, preferably more than 0% and not more than 0.012%.

[0032] P (phosphorus) may be contained in an amount of more than 0% and not more than 1.0%. P has the effect of increasing strength without decreasing magnetic flux density. However, excessive P content impairs the toughness of the steel, making the steel sheet more susceptible to fracture. Therefore, the upper limit of the P content is set to 1.0%, preferably 0.150% or less, and more preferably 0.120% or less. There is no particular lower limit for the P content, but taking into consideration the manufacturing cost, it is set to 0.001% or more.

[0033] Furthermore, the slab used in the manufacture of the grain-oriented electrical steel sheet according to this embodiment may contain, in addition to the above-mentioned elements, one or more of Cu, Sn, Ni, Cr, Sb, and Bi as elements that stabilize secondary recrystallization. When the slab contains the above-mentioned elements, the magnetic flux density of the grain-oriented electrical steel sheet to be manufactured can be further improved. In one embodiment, the slab may contain, in place of a portion of the Fe, one or more selected from the group consisting of Cu: 1.0% or less, Sn: 1.0% or less, Ni: 1.0% or less, Cr: 1.0% or less, Sb: 1.0% or less, and Bi: 1.0% or less.

[0034] A slab is formed by casting molten steel adjusted to the above-described composition. The method for casting the slab is not particularly limited. In research and development, even if a steel ingot is formed in a vacuum melting furnace or the like, the same effects as when a slab is formed can be confirmed for the above-described components.

[0035] [Process to make hot-rolled steel sheet] The slab is then heated and hot-rolled to be processed into a hot-rolled steel sheet. The slab heating temperature is not particularly limited. When the inhibitor components in the slab are completely dissolved, the slab may be heated to, for example, 1280°C or higher. The upper limit of the slab heating temperature is not particularly specified, but is preferably 1450°C from the viewpoint of equipment protection. For example, the slab heating temperature may be 1280°C or higher and 1450°C or lower. On the other hand, when the inhibitor components in the slab are not completely dissolved, the slab heating temperature may be less than 1280°C, for example. In this case, the steel sheet may be subjected to a nitriding treatment in any of the steps from the hot-rolled sheet annealing step to the finish annealing step.

[0036] Next, the heated slab is hot-rolled to be processed into a hot-rolled steel sheet. The thickness of the hot-rolled steel sheet after processing may be, for example, 1.8 mm or more and 3.5 mm or less. If the thickness of the hot-rolled steel sheet is less than 1.8 mm, the shape of the steel sheet after hot rolling may be inferior, which is not preferable. If the thickness of the hot-rolled steel sheet is more than 3.5 mm, the rolling load in the cold rolling process becomes large, which is not preferable. The hot-rolled steel sheet may be annealed to obtain a hot-rolled annealed sheet. When hot-rolled steel sheet annealing is performed, the shape of the steel sheet becomes better, so that the possibility of the steel sheet breaking during the subsequent cold rolling process can be reduced.

[0037] (Shot blasting) Subsequently, the hot-rolled steel sheet or the hot-rolled annealed sheet may be subjected to a shot blasting treatment before the pickling treatment, particularly to the ends in the longitudinal direction of the coil (top portion and / or end portion). The shot blasting treatment introduces defects such as cracks and voids into the surface of the hot-rolled steel sheet, and in the subsequent pickling treatment, the pickling solution penetrates into the steel sheet through these spaces, so that the pickling solution can reach not only the outermost surface of the steel sheet but also a certain depth range. The pickling, which will be described in detail later, replaces Mn on the surface of MnS, MnSe, and MnTe (which may be referred to as "MnS, etc." in this specification), which are precipitates and act as inhibitors, with Cu, thereby improving the heat resistance of the inhibitor. Therefore, the shot blasting allows the pickling solution to penetrate not only the outermost surface of the steel sheet but also to a certain depth of the steel sheet, thereby strengthening the strength of the inhibitors such as MnS present therein.

[0038] The strength of shot blasting is determined by the relative magnitude of the product of the projection velocity V and the projection amount M, and the projection velocity V and the projection amount M are not particularly limited and can be appropriately selected and adjusted according to the practical means for shot blasting. As an example, the projection velocity V may be 10 to 150 m / s, and the projection amount M may be 200 to 2000 kg / min.

[0039] The shot blasting conditions may be such that the average particle size of the shot material is 0.1 mm or more and 5.0 mm or less. This introduces fine cracks into the steel plate surface through which the pickling solution penetrates. As the blast material (shot material), a general one may be used, and iron balls with a hardness of about Hv500 may be used. The shape of the blast material may be either angular or round.

[0040] [Process for obtaining pickled board] In this process, a hot-rolled steel sheet or a hot-rolled annealed sheet that has been subjected to pickling pretreatment is immersed in a pickling solution to obtain a pickled sheet. (The pickling pretreatment will be described later.) Pickling is performed at least once after hot rolling and before primary recrystallization annealing in order to control inhibitors at the coil longitudinal ends (top and / or end portions) described later. In one embodiment, pickling is performed before the cold rolling step in order to reduce roll wear in cold rolling.

[0041] The pickling treatment conditions are as follows: the pickling solution contains one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn, and Ni, the total concentration of each element is 0.0001% or more and 1.0000% or less, the pH is -1.5 or more and less than 7, the liquid temperature is 15°C or more and 100°C or less, and the time for which the steel sheet is immersed in the pickling solution is 5 seconds or more and 200 seconds or less. If the total concentration of one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn and Ni in the pickling solution is less than 0.0001%, the inhibitor control effect at the coil width edge portion becomes insufficient, which is not preferable. If the total concentration of one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn and Ni in the pickling solution exceeds 1.0000%, the effect of improving the magnetic property becomes saturated and the cost of the pickling solution increases, which is not preferable. Therefore, the total concentration of one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn and Ni in the pickling solution is 0.0001% or more and 1.0000% or less. In addition, if the pH of the pickling solution is less than -1.5, the acidity becomes too strong and the handling of the pickling solution becomes difficult, which is not preferable. If the pH of the pickling solution is 7 or more, the inhibitor control effect in the thickness direction by the pickling process becomes insufficient, which is not preferable. Therefore, the pH of the pickling solution is -1.5 or more and less than 7. In addition, if the temperature of the pickling solution is less than 15°C, the inhibitor control effect in the thickness direction by the pickling treatment becomes insufficient, which is not preferable. If the temperature of the pickling solution is more than 100°C, the handling of the pickling solution becomes difficult, which is not preferable. Therefore, the temperature of the pickling solution is 15°C or more and 100°C or less. In addition, when the time for which the steel sheet is immersed in the pickling solution in the pickling treatment is less than 5 seconds, the effect of the pickling treatment in controlling inhibitors in the sheet thickness direction becomes insufficient, which is not preferable. When the time for which the steel sheet is immersed in the pickling solution in the pickling treatment exceeds 200 seconds, the equipment becomes long and large, which is not preferable. Therefore, the time for which the steel sheet is immersed in the pickling solution in the pickling treatment is 5 seconds or more and 200 seconds or less.

[0042] The mechanism by which pickling treatment enables inhibitor control at the longitudinal ends (top and / or end portions) of the coil is presumed to be as follows: When the pickling solution contains one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn, and Ni (these elements are sometimes referred to as "Cu, etc." in this specification), these elements have a very high affinity with S, Se, and Te in the solution, and therefore substitute for Mn in MnS, MnSe, and MnTe (these elements are sometimes referred to as "MnS, etc." in this specification) precipitates exposed on the steel sheet surface to form compounds. This reaction is likely to occur in the MnS, etc. precipitates, particularly on the surface side that comes into contact with the pickling solution. When Mn is replaced by other metal elements (Cu, etc.) on the surface side of MnS precipitates, the surface compounds act as a barrier to suppress the dissolution of Mn, S, Se, and Te in the center of MnS precipitates into the steel, which suppresses the Ostwald ripening of MnS during the final annealing process, and is thought to increase the heat resistance of MnS precipitates, i.e., the inhibitor strength. This reaction occurs when a pickling solution containing one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn, and Ni comes into contact with MnS, MnSe, or MnTe. In addition, shot blasting causes defects such as cracks and voids in the surface layer of the steel sheet, and the pickling solution penetrates into the steel sheet through the cracks, voids, and other spaces, and reacts not only with MnS exposed on the outermost surface of the steel sheet, but also with MnS within a certain depth range of the steel sheet surface, increasing the inhibitor strength. In particular, in areas that have been subjected to heavy shot blasting, defects such as cracks and voids increase, facilitating the penetration of the subsequent pickling solution and further increasing the inhibitor strength. For the purpose of increasing the inhibitor strength of MnS and the like in a certain range, particularly in the longitudinal ends of the coil (top and / or end portions), defects such as cracks may be introduced into the steel sheet surface by shot blasting or the like before pickling.

[0043] (Pre-pickling treatment) Prior to the pickling, a chelating agent (complex-forming agent) is applied to at least 80% of the central portion in the longitudinal direction of the coil. Coating the center of the coil with a chelating agent prior to the pickling is extremely effective as a means for suppressing the replacement of Mn such as MnS with Cu or the like on the steel sheet surface in the center of the coil during pickling. That is, the chelating agent captures Cu or the like in the pickling solution to form a stable complex of Cu or the like, thereby suppressing the replacement of Cu or the like on the steel sheet surface with Cu or the like. This leads to suppression of the strengthening of inhibitors in the center of the coil. Note that the end portions in the longitudinal direction of the coil refer to one or both longitudinal ends of the steel sheet (the start and / or end of the coil winding), and the central portion refers to the portion of the coil excluding both ends in the width direction of the steel sheet. Therefore, by applying a chelating agent to the longitudinal central portion of the steel sheet, that is, 80% or more of the total length excluding the ends, it is possible to suppress inhibitor strengthening in 80% or more of the longitudinal central portion of the coil. On the other hand, the chelating agent may not be applied to the range of 0.5% to 10% of the total length from the longitudinal ends of the coil (the start and end of the coil winding). This ensures that the inhibitor strengthening effect can be obtained in the range near the longitudinal ends of the coil where the chelating agent is not applied. Note that the range (length) where the chelating agent is not applied may differ at the longitudinal ends of the coil (the start and / or end of the coil winding). The chelating agent may be generally applied in the form of a water slurry to the steel sheet surface by a known application method such as a spray method or a calendar method, or the steel sheet surface may be immersed in a solution containing the chelating agent. After application of the chelating agent, a drying treatment may be performed to prevent the chelating agent from dripping.

[0044] A chelating agent (complex forming agent) is a drug containing a molecule or ion capable of forming a complex of Cu or the like. The chelating agent may be a molecule or ion that is understood by those skilled in the art as a ligand of a complex of Cu or the like (for example, a terminal ligand, a bridging ligand, a chelating ligand, a macrocyclic ligand, etc.). The chelating agent may be linear, branched, or cyclic, and specific examples thereof include anionic ligands such as carboxylate, oxalate, and oxo; amine-based ligands such as ammine, diamine, triamine, and tetramine; imine-based ligands such as pyridine, diimine, triimine, and porphyrin; Schiff bases; phosphine-based ligands having 1 to 3 phosphine moieties; crown ethers; and the like. The chelating agent may be a monodentate ligand or a multidentate ligand. From the viewpoint of the capture efficiency of Cu or the like in the pickling solution, a multidentate ligand is preferred. In a preferred embodiment, the chelating agent contains a nitrogen-containing ligand. Suitable examples of the nitrogen-containing ligand include ethyleneamine compounds (i.e., compounds having one or more ethylene groups and one or more amino groups) such as ethylenediamine (EDA), diethylenetriamine (DETA), triethylenetetramine (TETA), tetraethylenepentamine (TEPA), and pentaethylenehexamine (PEHA); aminocarboxylic acids such as ethylenediaminetetraacetic acid (EDTA) and cyclohexanediaminetetraacetic acid (CyDTA); and iminocarboxylic acids such as iminodiacetic acid. Particularly preferred examples are one or more selected from the group consisting of diethylenetriamine (DETA), triethylenetetramine (TETA), tetraethylenepentamine (TEPA), pentaethylenehexamine (PEHA), ethylenediaminetetraacetic acid (EDTA), and cyclohexanediaminetetraacetic acid (CyDTA).

[0045] The stability of the complex of Cu etc. formed by the chelating agent can be evaluated by the stability constant (LogKd) of the metal complex. The stability constant of the complex of Cu etc. formed by the chelating agent of this embodiment is preferably 4 or more, or 5 or more, or 10 or more, or 12 or more, or 14 or more, or 16 or more, or 18 or more, or 20 or more. The stability constant of the present disclosure means the total stability constant when multiple ligands form a complex of Cu etc. In one aspect, the stability constant is a value based on literature (specifically, IUPAC Stability Constants Database (SC-Database)). The larger the stability constant of the complex of Cu etc. formed by the chelating agent, the easier the chelating agent tends to capture Cu etc. and the harder it is to release it, which is preferable. A chelating agent with high basicity tends to form a Cu complex with a large stability constant. Examples of the relationship between the type of chelating agent and the stability constant of the complex formed by the chelating agent include the following (stability constants are in parentheses): ammonia (NH3) (4.2); iminodiacetic acid (IDA) (10.3); ethylenediaminetetraacetic acid (EDTA) (18.3); ethylenediamine (EDA) (10.7); diethylenetriamine (DETA) (16.1); triethylenetetramine (TETA) (20.4); tetraethylenepentamine (TEPA) (23.1); pentaethylenehexamine (PEHA) (26.2).

[0046] The amount of chelating agent applied to the center of the coil in the longitudinal direction may be appropriately selected depending on the concentration of Cu, etc. contained in the pickling solution, the pickling time, the composition ratio of Cu, etc.:complex-forming agent corresponding to the structure of the complex, etc. In one embodiment, when a complex with a composition ratio of Cu, etc.:complex-forming agent of 1:n (n is an integer of 1 or more) is to be formed, the amount of the chelating agent is preferably 1.1 or more, 1.2 or more, 1.5 or more, or 2.0 or more in terms of the efficiency of capturing Cu, etc., as a molar ratio to the value obtained by multiplying the amount of Cu, etc. in the pickling solution by the above n, and is preferably 5.0 or less, or 3.0 or less, from the viewpoint of avoiding an increase in cost due to the use of a complex-forming agent in excess of the required amount.

[0047] In one embodiment, the concentration of the chelating agent to be applied may be 0.0001% or more and 90.0000% or less by mass from the viewpoint of effectively capturing Cu and the like in the pickling solution. The solution may be aqueous or non-aqueous. Another advantage is that the chelating agent is applied to the central portion of the coil in the longitudinal direction, and does not substantially cause any inconvenience to the pickling solution itself.

[0048] [Process to make cold-rolled steel sheet] The obtained pickled sheet is then processed into a cold-rolled steel sheet by rolling it through one cold rolling or multiple cold rolling with intermediate annealing. When rolling it through multiple cold rolling with intermediate annealing and / or pickling, it is possible to omit the hot-rolled sheet annealing in the previous stage. In addition, both hot-rolled sheet annealing and intermediate annealing may be performed. In order to control the inhibitors at the coil longitudinal end (top portion and / or end portion) described above, pickling may be performed at least once after hot rolling and before primary recrystallization annealing. From the viewpoint of reducing roll wear in cold rolling, it is preferable to perform pickling before each cold rolling process.

[0049] In addition, the steel sheet may be heat-treated at about 300°C or less between passes of cold rolling, between rolling roll stands, or during rolling. In such a case, the magnetic properties of the final grain-oriented electrical steel sheet can be improved. The hot-rolled steel sheet may be rolled by three or more cold rolling passes, but since multiple cold rolling passes increase the manufacturing cost, it is preferable that the hot-rolled steel sheet is rolled by one or two cold rolling passes. When cold rolling is performed by reverse rolling such as a Sendzimir mill, the number of passes in each cold rolling pass is not particularly limited, but is preferably 9 passes or less from the viewpoint of manufacturing cost.

[0050] [Primary recrystallization annealing process] Next, the cold-rolled steel sheet is heated and then decarburized. These processes are also called primary recrystallization annealing, and are preferably performed continuously. By rapidly heating the temperature in the primary recrystallization annealing, it is possible to increase the number of Goss-oriented grains before secondary recrystallization in the cold-rolled steel sheet, and it is expected that grains with an orientation closer to the ideal Goss orientation will be secondary recrystallized in the secondary recrystallization process.

[0051] (Temperature rise process) In the present invention, the average heating rate between 550°C and 700°C during the heating process in the primary recrystallization annealing may be 100°C / s or more and 3000°C / s or less. This can increase the number of Goss-oriented grains before secondary recrystallization in the cold-rolled steel sheet, and improve the magnetic flux density of the final grain-oriented electrical steel sheet. The temperature range for rapid heating is 550°C to 700°C. If the start temperature of rapid heating is more than 550°C, dislocation recovery progresses significantly in the steel sheet, and primary recrystallization of grains other than the Goss-oriented grains begins, which is undesirable as it reduces the effect of increasing the Goss-oriented grains. If the end temperature of rapid heating is less than 700°C, the primary recrystallization of other grains is completed before the primary recrystallization of the Goss-oriented grains is completed, which is undesirable as it reduces the effect of increasing the Goss-oriented grains.

[0052] In addition, when the average heating rate between 550°C and 700°C is 400°C / s or more, the number of Goss-oriented grains before the secondary recrystallization can be further increased, and the magnetic flux density of the final grain-oriented electrical steel sheet can be further improved, which is more preferable, and when the average heating rate between 550°C and 700°C is 700°C / s or more, the magnetic flux density of the grain-oriented electrical steel sheet can be further improved, which is extremely preferable. When the average heating rate between 550°C and 700°C is less than 100°C / s, it is not preferable because sufficient Goss-oriented grains cannot be obtained to improve the magnetic properties by the secondary recrystallization. On the other hand, the upper limit of the average heating rate between 550°C and 700°C is not particularly limited, but may be, for example, 3000°C / s from the viewpoint of equipment and manufacturing costs. The heating start temperature of the primary recrystallization annealing, the heat pattern other than the rapid heating from 550°C to 700°C, and the final temperature are not particularly limited.

[0053] The increase in inhibitor strength at the surface layer side of the steel sheet by pickling, especially at the coil longitudinal end (top and / or end), and the increase in Goss oriented grains by the rapid temperature rise in primary recrystallization annealing bring about a synergistic effect on the improvement of magnetic properties. Although not necessarily bound by a specific theory, the following is considered as the mechanism of the synergistic effect. In the surface layer of the coil longitudinal end (top and / or end), the inhibitor constituents are reduced due to reaction with the atmosphere during finish annealing, and the inhibitor strength near the coil longitudinal end may be reduced. According to an embodiment of the present invention, the chelating agent is not applied to the coil longitudinal end (top and / or end), and the inhibitor strength is increased by the subsequent pickling. Therefore, it is considered that abnormal grain growth other than Goss oriented grains is suppressed at the coil longitudinal end (top and / or end) during the temperature rise process in finish annealing, and as a result, abnormal grain growth of many Goss oriented grains is promoted.

[0054] Such a rapid temperature rise can be achieved, for example, by using a current heating method or an induction heating method.

[0055] Here, the heating process may be performed by a plurality of devices. For example, holding or slow cooling at a temperature lower than 550°C at which recovery of the steel sheet occurs, i.e., a decrease in dislocation density in the steel sheet, may be performed because this can improve the temperature uniformity of the steel sheet before heating. Furthermore, the heating process including heating from 550°C to 700°C may also be performed by one or more devices.

[0056] The point at which heating starts is the point at which the temperature of the steel plate transitions from a decreasing state to an increasing state on the low-temperature side of 550°C or less (i.e., the point at which the temperature change is at a minimum value), while the point at which heating ends is the point at which the temperature of the steel plate transitions from an increasing state to a decreasing state on the high-temperature side of 700°C or more (i.e., the point at which the temperature change is at a maximum value).

[0057] However, depending on the arrangement of the multiple heating devices, there is a possibility that the temperature of the steel sheet may continue to rise at a temperature higher than the temperature of the heating process including 700° C. In such a case, for example, the end point of the rapid heating may be a point at or above 700° C. where the rate of change of the heating rate is a negative value and is minimal.

[0058] Here, the method of determining the temperature rise start point and the rapid temperature rise end point is not particularly limited, but for example, it is possible to determine by measuring the steel sheet temperature using a radiation thermometer or the like. The method of measuring the steel sheet temperature is not particularly limited. Furthermore, even if the temperature rise end temperature of the primary recrystallization is lower or higher than the subsequent decarburization annealing temperature, the effect of the present invention is not impaired. When the temperature rise end temperature of the primary recrystallization is lower than the decarburization annealing temperature, the steel sheet may be heated in the decarburization annealing process. When the temperature rise end temperature of the primary recrystallization is higher than the decarburization annealing temperature, the steel sheet may be cooled by performing a heat radiation treatment or a gas cooling treatment. Furthermore, after cooling to a temperature lower than the decarburization annealing temperature, the steel sheet may be reheated in the decarburization annealing process.

[0059] However, when it is difficult to measure the steel sheet temperature and difficult to estimate the exact positions of the temperature rise start point and the rapid temperature rise end point, these positions may be estimated by analogy with the heat patterns of the temperature rise process and the cooling process. Furthermore, the entry and exit temperatures of the steel sheet into the temperature rise device during the temperature rise process may be set as the temperature rise start point and the rapid temperature rise end point.

[0060] (Decarburization annealing) Next, the cold-rolled steel sheet is decarburized and annealed. From the viewpoint of decarburization, the decarburization may be performed at a temperature of 900° C. or less in a moist atmosphere containing hydrogen and nitrogen. In order not to inhibit the decarburization, the oxygen partial pressure ratio of the decarburization annealing atmosphere, i.e., the water vapor partial pressure P H2O and hydrogen partial pressure P H2 Compared to P H2O / P H2 may be set to 0.35 or more and 0.60 or less.

[0061] In the step of primary recrystallization annealing, the cold-rolled steel sheet may be subjected to reduction annealing following decarburization annealing in order to improve magnetic properties and coating properties.

[0062] [Finish annealing process] Thereafter, the cold-rolled steel sheet after the primary recrystallization annealing is subjected to a finish annealing. In this case, an annealing separator mainly composed of MgO may be applied before the finish annealing for the purpose of preventing seizure between steel sheets, forming a primary coating, controlling secondary recrystallization behavior, etc. The annealing separator is generally applied to the steel sheet surface in the form of a water slurry and dried, but an electrostatic application method or the like may also be used.

[0063] Then, the coiled steel sheet is subjected to a finish annealing for the purpose of forming a primary coating and secondary recrystallization. The finish annealing may be performed by heat treating the coiled steel sheet using, for example, a batch-type heating furnace. Furthermore, in order to further reduce the iron loss value of the final grain-oriented electrical steel sheet, the coiled steel sheet may be subjected to a purification treatment in which the temperature is raised to about 1200°C and then held at that temperature.

[0064] In general, the ends of the coil in the longitudinal direction are easily affected by the annealing atmosphere during final annealing, and MnS, an inhibitor, is easily reduced by desulfurization. Note that S, Se, and Te are elements of the same group in the periodic table, and their behaviors are similar in many ways. Therefore, not only MnS, but also MnSe and MnTe are easily affected by the annealing atmosphere during final annealing, and MnSe and MnTe as inhibitors are also easily reduced. However, in one embodiment of the present invention, the inhibitors at the longitudinal ends of the coil are strengthened, and the inhibitors such as MnS are not reduced during finish annealing, stabilizing the secondary recrystallization behavior at the longitudinal ends of the coil.

[0065] Finish annealing is generally performed by raising the temperature from about room temperature, and the temperature raising rate of finish annealing is various, but is not particularly limited in the present invention, and general finish annealing conditions can be used. For example, the rate may be 5°C / h to 100°C / h from the viewpoint of productivity and general equipment constraints. In addition, other known heat patterns may be used. The heat pattern in the cooling process is also not particularly limited.

[0066] The atmospheric gas composition in the final annealing is set to a nitrogen partial pressure of 50 vol% to 90 vol% in the annealing atmosphere at 600°C to 1100°C. By setting the nitrogen partial pressure in the above range, AlN is easily formed in the steel, and the effect of suppressing desulfurization is obtained. In other words, inhibitors such as MnS are less likely to decrease at the ends of the coil in the longitudinal direction, and the secondary recrystallization behavior at the ends of the coil in the longitudinal direction is stabilized. On the other hand, in the center of the coil in the longitudinal direction, the secondary recrystallization behavior becomes excessively stable due to this nitrogen partial pressure atmosphere, which may result in deterioration of the magnetic properties of the product sheet. However, in one embodiment of the present invention, the inhibitor strengthening can be suppressed by applying a chelating agent to the center of the coil in the longitudinal direction, so that excessive stabilization of the secondary recrystallization behavior does not occur, and good magnetic properties can be obtained even in the center of the coil in the longitudinal direction of the product sheet. If the nitrogen partial pressure is less than 50 vol%, the secondary recrystallization behavior at the longitudinal ends of the coil may be unstable, and if the nitrogen partial pressure exceeds 90 vol%, the magnetic properties at the longitudinal center of the coil may deteriorate. The atmosphere gas during the secondary recrystallization process may be a mixed gas of nitrogen and hydrogen, a dry atmosphere or a wet atmosphere. The purification annealing may be performed in dry hydrogen gas.

[0067] [Planarization annealing process] Next, after the finish annealing, an insulating coating mainly composed of, for example, aluminum phosphate or colloidal silica is applied to the surface of the steel sheet in order to provide the steel sheet with insulation and tension. Then, flattening annealing is performed in order to bake the insulating coating and flatten the shape of the steel sheet by the finish annealing. Note that the components of the insulating coating are not particularly limited as long as the steel sheet is provided with insulation and tension. Note that in this embodiment, it goes without saying that the grain-oriented electrical steel sheet may be subjected to a magnetic domain control treatment depending on the purpose of the customer.

[0068] The above steps allow the final grain-oriented electrical steel sheet to be manufactured. According to the manufacturing method of this embodiment, it is possible to manufacture a grain-oriented electrical steel sheet that is excellent in magnetic properties, particularly in the magnetic properties not only in the center portion of the coil in the longitudinal direction but also in the ends of the coil in the longitudinal direction.

[0069] In the grain-oriented electrical steel sheet according to the present embodiment, the magnetic flux density B8 value may be further controlled. Specifically, in the grain-oriented electrical steel sheet according to the present embodiment, the magnetic flux density B8 value may be 1.90 T or more, preferably 1.91 T or more, and more preferably 1.92 T or more. Here, the magnetic flux density B8 value is the magnetic flux density when a magnetic field of 800 A / m at 50 Hz is applied to the grain-oriented electrical steel sheet. If the magnetic flux density B8 value is less than 1.90 T, the iron loss value (particularly, hysteresis loss) of the grain-oriented electrical steel sheet becomes large, which is not preferable. The upper limit of the magnetic flux density B8 value is not particularly limited, but may be, for example, 2.0 T in reality. In addition, the difference in the B8 value between the longitudinal end portion and the center portion of the coil is 0.02 T or less. If the difference in the B8 value between the longitudinal end portion and the center portion of the coil exceeds 0.02 T, the magnetic properties in the longitudinal direction of the coil become non-uniform, which is not preferable. The magnetic properties of the grain-oriented electrical steel sheet, such as the magnetic flux density, can be measured by a known method. For example, the magnetic properties of grain-oriented electrical steel sheets can be measured by using a method based on the Epstein test specified in JIS C2550, or the Single Sheet Tester (SST) method specified in JIS C2556. In research and development, when steel ingots are formed in a vacuum melting furnace or the like, it is difficult to obtain test pieces of the same size as those produced by actual equipment. In this case, for example, a test piece with a width of 60 mm and a length of 300 mm may be obtained, and measurements may be performed in accordance with the Single Sheet Magnetic Property Test Method. Furthermore, the obtained results may be multiplied by a correction factor so that the same measured values ​​as those obtained by the method based on the Epstein test are obtained. In this embodiment, measurements are performed using a measurement method in accordance with the Single Sheet Magnetic Property Test Method.

[0070] The grain-oriented electrical steel sheet according to the present embodiment has been described above. The grain-oriented electrical steel sheet according to the present embodiment can be manufactured by the above-mentioned method for manufacturing the grain-oriented electrical steel sheet according to the present embodiment. However, the method is not limited to this method. EXAMPLES

[0071] The method for producing a grain-oriented electrical steel sheet according to an embodiment of the present invention and the grain-oriented electrical steel sheet will be described in more detail below with reference to examples. Note that the examples shown below are merely examples of the grain-oriented electrical steel sheet according to this embodiment, and the grain-oriented electrical steel sheet according to this embodiment is not limited to the examples shown below.

[0072] Example 1 <Manufacturing of grain-oriented electrical steel sheets> First, a slab containing 0.08% C, 3.2% Si, 0.08% Mn, 0.024% S, 0.03% acid-soluble Al, 0.008% N, and the balance being Fe and impurities was prepared. The slab was annealed at 1350°C for 1 hour, and then hot-rolled to obtain a hot-rolled steel sheet having a thickness of 2.3 mm. Samples were taken from the coil longitudinal end and coil longitudinal center from the obtained hot-rolled steel sheet. Here, the end samples were taken within a range of 5 m from the coil end, and the center samples were taken from a position 300 m from one end of the coil longitudinal direction. At this time, it was confirmed that the sample taking position was 300 m or more toward the center side from the other end. These hot-rolled sheets were annealed at a maximum temperature of 1100°C for 140 seconds, subjected to pickling pretreatment and pickling, and then cold-rolled to obtain cold-rolled steel sheets with a thickness of 0.23 mm. Here, the conditions shown in Table 1 were used for whether or not pickling pretreatment was performed, and the treatment liquid was methanol as a solvent and 5 mass% triethylenetetramine. The pickling conditions after the annealing of the hot-rolled sheets were also shown in Table 1.

[0073] The cold-rolled steel sheet thus obtained was then subjected to primary recrystallization annealing in a wet hydrogen atmosphere at 850°C for 180 seconds. Here, the heating rate was 20°C / s. Next, an annealing separator containing MgO was applied in the form of a water slurry to the surface of the steel sheet after the primary recrystallization annealing, and dried. Thereafter, the steel sheet after the primary annealing was subjected to finish annealing, and washed with water. Here, the nitrogen partial pressure of the finish annealing atmosphere was set to the conditions shown in Table 1. Thereafter, an insulating coating mainly composed of aluminum phosphate and colloidal silica was applied to the surface of the steel sheet, and then flattening annealing was performed for the purpose of baking the insulating coating and flattening the steel sheet.

[0074] The grain-oriented electrical steel sheet samples obtained above after the flattening annealing were sheared and stress relief annealed, and then the magnetic flux density B8 value of the grain-oriented electrical steel sheets according to each of the present invention examples and comparative examples was measured using a single sheet magnetic property measurement method (based on the method described in JIS C2556) with a sample size of 60 mm x 300 mm. Here, the B8 value is the magnetic flux density of the steel sheet when the grain-oriented electrical steel sheet is excited at 800 A / m at 50 Hz. In the present invention, the average value of five samples was used.

[0075] Here, the condition was judged as good (B) if the difference in B8 value between the longitudinal end and center of the coil was 0.020 T or less, and the magnetic flux density B8 value of the grain-oriented electrical steel sheet at the longitudinal end of the coil was 1.910 T or more. Any other condition was judged as unacceptable (C).

[0076] Table 1 shows the manufacturing conditions, measurement results, and evaluations of the above examples of the present invention and comparative examples.

[0077] [Table 1]

[0078] Referring to the results in Table 1, it was found that the grain-oriented electrical steel sheet satisfying the conditions of this embodiment was judged to be good.

[0079] Example 2 First, a slab containing 0.08% C, 3.2% Si, 0.08% Mn, 0.024% S, 0.03% acid-soluble Al, 0.008% N, and the remainder being Fe and impurities was prepared. The slab was annealed at 1350°C for 1 hour, and then hot-rolled to obtain a hot-rolled steel sheet having a thickness of 2.3 mm. Samples were taken from the end and center of the coil length from the obtained hot-rolled steel sheet. Here, the end samples were taken within a range of 5 m from the end of the coil, and the center samples were taken from a position 300 m from one end of the coil length. At this time, it was confirmed that the sample taking position was 300 m or more toward the center side from the other end. These hot-rolled sheets were annealed at a maximum temperature of 1100°C for 140 seconds, shot-blasted (projection speed V: 50 m / s, projection amount M: 500 kg / min), pickled, and then cold-rolled to obtain cold-rolled steel sheets with a thickness of 0.23 mm. Here, pickling pretreatment was performed only on the samples at the longitudinal ends of the coil, and the treatment solution was an aqueous solution containing 5 mass% ethylenediaminetetraacetic acid. The pickling conditions after the annealing of the hot-rolled sheets were as follows: Cu concentration in the pickling solution: 0.001%, pickling solution: hydrochloric acid, pickling solution pH: 3, pickling solution temperature: 70°C, and contact time between the pickling solution and the steel sheet: 30 seconds.

[0080] The cold-rolled steel sheet thus obtained was then subjected to primary recrystallization annealing in a wet hydrogen atmosphere at 850°C for 180 seconds. Here, the average heating rate in the temperature range of 550°C to 700°C was set to the conditions shown in Table 2. Next, an annealing separator containing MgO was applied in the form of a water slurry to the surface of the steel sheet after the primary recrystallization annealing, and dried. Thereafter, the steel sheet after the primary annealing was subjected to finish annealing, and washed with water. Here, the nitrogen partial pressure in the finish annealing atmosphere was set to 80 vol%. Thereafter, an insulating coating mainly composed of aluminum phosphate and colloidal silica was applied to the surface of the steel sheet, and then flattening annealing was performed for the purpose of baking the insulating coating and flattening the steel sheet.

[0081] The grain-oriented electrical steel sheet samples obtained above after the flattening annealing were sheared and stress relief annealed, and then the magnetic flux density B8 value of the grain-oriented electrical steel sheets according to each of the present invention examples and comparative examples was measured using a single sheet magnetic property measurement method (based on the method described in JIS C2556) with a sample size of 60 mm x 300 mm. Here, the B8 value is the magnetic flux density of the steel sheet when the grain-oriented electrical steel sheet is excited at 800 A / m at 50 Hz. In the present invention, the average value of five samples was used.

[0082] Here, the condition where the difference in B8 value between the longitudinal end and center of the coil is 0.020 T or less and the magnetic flux density B8 value of the grain-oriented electrical steel sheet at the longitudinal end of the coil is 1.910 T or more was judged as good (B), the condition where it is 1.920 T or more was judged as even better (A), and the condition where it is 1.930 T or more was judged as extremely good (S). Anything other than the above was judged as unacceptable (C).

[0083] Table 2 shows the manufacturing conditions, measurement results, and evaluations of the above-mentioned examples of the present invention and comparative examples.

[0084] [Table 2]

[0085] Referring to the results in Table 2, it was found that the grain-oriented electrical steel sheet satisfying the conditions of this embodiment was judged to be good.

Claims

1. a step of heating a slab containing, by mass%, C: 0.02% or more and 0.10% or less, Si: 2.5% or more and 4.5% or less, Mn: 0.01% or more and 0.50% or less, one or more of S, Se and Te in total: 0.001% or more and 0.050% or less, acid-soluble Al: more than 0% and 0.05% or less, N: more than 0% and 0.015% or less, with the balance being Fe and impurities, and hot rolling the slab to obtain a hot-rolled steel sheet; A step of obtaining a pickled sheet by subjecting the hot-rolled steel sheet to pickling, or obtaining a hot-rolled annealed sheet by subjecting the hot-rolled steel sheet to hot-rolled sheet annealing, and then obtaining a pickled sheet by subjecting the hot-rolled annealed sheet to pickling; A step of obtaining a cold-rolled steel sheet by cold rolling the pickled sheet; A step of subjecting the cold-rolled steel sheet to primary recrystallization annealing; A step of applying an annealing separator containing MgO to the surface of the cold-rolled steel sheet after the primary recrystallization annealing, and then performing finish annealing; A step of applying an insulating coating to the steel sheet after the finish annealing and then performing planarization annealing, Prior to the pickling, a chelating agent is applied to at least 80% of a central portion of the coil in the longitudinal direction; In the pickling, the pickling solution contains one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn and Ni, the total concentration of each element is 0.00010% or more and 1.0000% or less, the pH is -1.5 or more and less than 7, the solution temperature is 15°C or more and 100°C or less, and the steel sheet is immersed in the pickling solution for 5 seconds or more and 200 seconds or less, The method for producing a grain-oriented electrical steel sheet, characterized in that the nitrogen partial pressure in the annealing atmosphere at 600°C to 1100°C in the finish annealing is 50 vol% or more and 90 vol% or less.

2. 2. The method for producing a grain-oriented electrical steel sheet according to claim 1, wherein in the rapid heating in the primary recrystallization annealing, an average heating rate in a temperature range of 550° C. to 700° C. is 100° C. / s or more and 3000° C. / s or less.

Citation Information

Patent Citations

  • Method for producing high magnetic induction orientated silicon steel based on ESP endless rolling technology

    CN108546814A

  • JP1965-015644B

  • hifunsaibutsushitsuofunsaisurutamenoshindomiru

    JP1976013469A

  • Production of grain-oriented silicon steel sheet having extremely low iron loss