Method for producing conjugated diene rubber
By reacting a conjugated diene polymer chain with a polyorganosiloxane modifier and a nitrogen-containing compound, the affinity between rubber and silica is improved, addressing processing difficulties and enhancing the low heat generation and wet grip properties of crosslinked rubber products.
Patent Information
- Application Number
- JP2018551614
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2016-11-16
- Filing Date
- 2017-11-13
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2037-11-13
AI Technical Summary
Conventional rubber compositions containing silica face issues with insufficient affinity between rubber and silica, leading to separation and processing difficulties, as well as inadequate low heat generation and wet grip properties, which are exacerbated by the use of silane coupling agents that increase manufacturing costs.
A method involving the reaction of a conjugated diene polymer chain with a specific polyorganosiloxane modifier, followed by a compound capable of reacting with the reaction residue, to enhance the affinity between rubber and silica, resulting in a crosslinked rubber product with improved hot flow, low heat build-up, and excellent wet grip properties.
The method produces a crosslinked rubber product with enhanced hot flow properties, preventing coagulated crumbs from sticking together, and exhibits low heat build-up and superior wet grip characteristics, suitable for applications in tires and other rubber products.
Smart Images

Figure 0007557258000015 
Figure 0007557258000010 
Figure 0007557258000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a conjugated diene rubber, more specifically, to a method for producing a conjugated diene rubber capable of giving a cross-linked rubber product having excellent hot flow properties (resistance to adhesion of solidified crumbs to each other) and excellent low heat build-up and wet grip properties. The present invention also relates to a conjugated diene rubber obtained by the production method, a rubber composition containing the conjugated diene rubber, and a cross-linked rubber product thereof. [Background technology]
[0002] In recent years, automobile tires are required to have low fuel consumption due to environmental and resource issues, while excellent wet grip is required from the safety standpoint. A crosslinked product of a rubber composition containing silica as a filler has excellent low heat generation properties compared to a crosslinked product of a rubber composition containing carbon black, so that the rolling resistance is small when a tire is formed. Therefore, a tire with excellent fuel consumption can be obtained by forming a tire using a crosslinked product of a rubber composition containing silica.
[0003] However, even if silica is blended with conventional rubber, the affinity between the rubber and silica is insufficient, and therefore they are prone to separation. As a result, the processability of the rubber composition before crosslinking is poor, and the low heat build-up property of the crosslinked rubber obtained by crosslinking this is insufficient.
[0004] Therefore, in order to improve the affinity between rubber and silica, it has been proposed to add various silane coupling agents to the rubber composition, as disclosed in, for example, Patent Document 1 and Patent Document 2. However, handling of the silane coupling agent requires advanced processing technology, and since the silane coupling agent is expensive, there is a problem that the manufacturing cost of the tire increases when the compounded amount is increased.
[0005] In order to solve such problems, a technique has been studied in which a modifier is reacted with the active end of a polymer chain when a rubber polymer is obtained by a solution polymerization method, thereby giving the rubber itself affinity with silica, as disclosed in, for example, Patent Document 3. For example, Patent Document 3 discloses a technique in which a modifier made of a cyclic compound containing at least three siloxane units in a ring structure is reacted with the active end of a rubber polymer, and then an amine having an active hydrogen atom bonded to the amino nitrogen atom is reacted with the resulting reaction product to obtain a rubber polymer functionalized with an amine.
[0006] According to the technology of Patent Document 3, the affinity between rubber and silica is improved to some extent, and the low heat generation property and wet grip property of the obtained cross-linked rubber are improved to a certain extent, but in recent years, the demand for low fuel consumption and wet grip property for automobile tires has increased, and further improvement in low heat generation property and wet grip property is desired. Also, the rubber polymer obtained by the technology of Patent Document 1 does not have sufficient hot flow property, and therefore, when the rubber polymer is recovered from the polymer solution by steam stripping or the like during its production, the solidified crumbs of the rubber polymer adhere to each other, which causes them to swell and adhere to the wall surface or stirring blade of the coagulation tank, causes clogging of the solidified crumb transport pipe, and causes problems such as unstable operation during solidification. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2011-46640 A [Patent Document 2] JP 2012-17291 A [Patent Document 3] Special Publication No. 2008-518086 Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention has been made in view of the above circumstances, and has an object to provide a method for producing a conjugated diene rubber, which can give a cross-linked rubber product having excellent hot flow properties (resistance to adhesion of solidified crumbs to each other), low heat build-up properties and excellent wet grip properties. [Means for solving the problem]
[0009] As a result of intensive research by the present inventors to achieve the above object, it was found that a conjugated diene rubber obtained by reacting a specific amount of a specific polyorganosiloxane as a modifier with a conjugated diene polymer chain having an active terminal, and then reacting the conjugated diene polymer chain having the polyorganosiloxane reacted with a compound having a group capable of reacting with a reaction residue formed by the reaction of the conjugated diene polymer chain having an active terminal with the polyorganosiloxane and a group containing a nitrogen atom, has excellent hot flow properties, and can effectively prevent the occurrence of mutual adhesion of solidified crumbs, and can provide a cross-linked rubber product having excellent low heat build-up and wet grip properties, thereby completing the present invention.
[0010] That is, according to the present invention, there is provided a method for producing a conjugated diene rubber, comprising: a first step of polymerizing a monomer containing a conjugated diene compound in an inert solvent using a polymerization initiator to obtain a conjugated diene polymer chain having an active end; a second step of adding a polyorganosiloxane represented by the following general formula (1) to the conjugated diene polymer chain having an active end in a ratio of 1 mol or more calculated in terms of the number of repeating units of the siloxane structure (-Si-O-) in the polyorganosiloxane per 1 mol of the polymerization initiator used in the first step, and reacting the polyorganosiloxane obtained in the second step with a compound represented by the following general formula (2). [ka] (In general formula (1), R 1 ~R 8is an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 12 carbon atoms, which may be the same or different. X 1 and X 4 is any group selected from the group consisting of an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, and an epoxy group-containing group having 4 to 12 carbon atoms, which may be the same or different. X 2 is an alkoxy group having 1 to 5 carbon atoms or a group having 4 to 12 carbon atoms containing an epoxy group, 2 They may be the same or different. X 3 is a group containing 2 to 20 repeating alkylene glycol units, X 3 When there are a plurality of, they may be the same or different. m is an integer of 3 to 200, n is an integer of 0 to 200, k is an integer of 0 to 200, and m+n+k is 3 or more. [ka] (In general formula (2), R 9 is a hydrocarbyl group, A 1 is a group capable of reacting with a reaction residue formed by the reaction of a conjugated diene polymer chain having an active terminal with a polyorganosiloxane, and A 2 is a group containing a nitrogen atom, p is an integer of 0 to 2, q is an integer of 1 to 3, r is an integer of 1 to 3, and p+q+r=4.
[0011] In the production method of the present invention, A in the general formula (2) 1 But -OR 10 (R 10 is preferably a hydrogen atom or a hydrocarbyl group. In the production method of the present invention, A in the general formula (2) 2 is preferably a group containing a primary amino group having an active hydrogen atom and / or a secondary amino group having an active hydrogen atom. In the production method of the present invention, it is preferable to use an organic alkali metal amide compound as the polymerization initiator, and it is more preferable that the organic alkali metal amide compound is a compound represented by the following general formula (3). [ka] (In general formula (3), M 1 represents an alkali metal atom, and R 11 , R 12 each independently represents an alkyl group, a cycloalkyl group, an aryl group, an aralkyl group, a protecting group for an amino group, or a group capable of generating a hydroxyl group upon hydrolysis; R 11 and R 12 may be bonded to each other to form a ring structure together with the nitrogen atom to which they are bonded, and when forming such a ring structure, they may form a ring structure together with the nitrogen atom to which they are bonded and a heteroatom other than the nitrogen atom to which they are bonded.
[0012] In the production method of the present invention, the first step preferably comprises a step of polymerizing isoprene or a monomer containing isoprene and an aromatic vinyl compound in an inert solvent using a polymerization initiator to form a polymer block (A) having an active end containing 80 to 100% by weight of isoprene monomer units and 0 to 20% by weight of aromatic vinyl monomer units, and a step of mixing the polymer block (A) having an active end with 1,3-butadiene or a monomer containing 1,3-butadiene and an aromatic vinyl compound to continue the polymerization reaction to form a polymer block (B) having an active end containing 50 to 100% by weight of 1,3-butadiene monomer units and 0 to 50% by weight of aromatic vinyl monomer units in a continuous manner with the polymer block (A), thereby obtaining a conjugated diene-based polymer chain having an active end.
[0013] According to the present invention, there is also provided a conjugated diene rubber obtained by the above production method. Furthermore, according to the present invention, there is provided a rubber composition containing 10 to 200 parts by weight of silica per 100 parts by weight of the rubber component containing the conjugated diene rubber. The rubber composition of the present invention preferably further contains a crosslinking agent.
[0014] Furthermore, according to the present invention, there are provided a cross-linked rubber product obtained by cross-linking the above rubber composition, and a tire comprising the cross-linked rubber product. Effect of the Invention
[0015] According to the present invention, it is possible to provide a conjugated diene rubber which has excellent hot flow properties and can effectively prevent adhesion of solidified crumbs to each other, and which can give a cross-linked rubber product which has excellent low heat build-up properties and wet grip properties, a rubber composition containing the conjugated diene rubber, a cross-linked rubber product which is obtained by cross-linking the rubber composition and has excellent low heat build-up properties and wet grip properties, and a tire which includes the cross-linked rubber product. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] <Method of producing conjugated diene rubber> The method for producing a conjugated diene rubber of the present invention comprises the steps of: A first step of polymerizing a monomer including a conjugated diene compound in an inert solvent using a polymerization initiator to obtain a conjugated diene polymer chain having an active terminal; a second step of adding a polyorganosiloxane represented by general formula (1) described later to the conjugated diene polymer chain having an active terminal in an amount of 1 mole or more calculated in terms of the number of repeating units of the siloxane structure (-Si-O-) in the polyorganosiloxane per mole of the polymerization initiator used in the first step, and reacting the polyorganosiloxane with the conjugated diene polymer chain having an active terminal; The method further comprises a third step of reacting the conjugated diene polymer chain obtained in the second step with a compound represented by general formula (2) described below.
[0017] <1st process> The first step of the production method of the present invention is a step of polymerizing a monomer containing a conjugated diene compound in an inert solvent using a polymerization initiator to obtain a conjugated diene polymer chain having an active end.
[0018] In the first step of the production method of the present invention, the conjugated diene compound used as a monomer to obtain a conjugated diene polymer chain having an active terminal is not particularly limited, but examples thereof include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 2-phenyl-1,3-butadiene, 1,3-pentadiene, 2-methyl-1,3-pentadiene, 1,3-hexadiene, 4,5-diethyl-1,3-octadiene, and 3-butyl-1,3-octadiene. Among these, 1,3-butadiene and isoprene are preferred. These conjugated diene compounds may be used alone or in combination of two or more.
[0019] In addition, in the first step of the production method of the present invention, an aromatic vinyl compound may be used together with the conjugated diene compound as a monomer used for polymerization. Examples of aromatic vinyl compounds used as monomers include styrene, methylstyrene, ethylstyrene, t-butylstyrene, α-methylstyrene, α-methyl-p-methylstyrene, chlorostyrene, bromostyrene, methoxystyrene, dimethylaminomethylstyrene, dimethylaminoethylstyrene, diethylaminomethylstyrene, diethylaminoethylstyrene, cyanoethylstyrene, and vinylnaphthalene. Among these, styrene is preferred. The conjugated diene polymer chain having an active end obtained in the first step of the production method of the present invention preferably contains 50 to 100% by weight of conjugated diene monomer units, more preferably 52 to 95% by weight, and more preferably 0 to 50% by weight of aromatic vinyl monomer units, more preferably 5 to 48% by weight.
[0020] Furthermore, in the first step of the production method of the present invention, a compound copolymerizable with the conjugated diene compound other than the aromatic vinyl compound may be used together with the conjugated diene compound. Examples of such compounds copolymerizable with the conjugated diene compound include linear olefin compounds such as ethylene, propylene, and 1-butene; cyclic olefin compounds such as cyclopentene and 2-norbornene; non-conjugated diene compounds such as 1,5-hexadiene, 1,6-heptadiene, 1,7-octadiene, dicyclopentadiene, and 5-ethylidene-2-norbornene; (meth)acrylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, and butyl (meth)acrylate; other (meth)acrylic acid derivatives such as (meth)acrylonitrile and (meth)acrylamide; and the like. The compounds copolymerizable with these conjugated diene compounds are preferably 10% by weight or less, more preferably 5% by weight or less, as monomer units, in the conjugated diene polymer chain having an active end obtained in the first step of the production method of the present invention.
[0021] The inert solvent used in the polymerization is not particularly limited as long as it is one that is usually used in solution polymerization and does not inhibit the polymerization reaction. Specific examples of the inert solvent include chain aliphatic hydrocarbons such as butane, pentane, hexane, and heptane; alicyclic hydrocarbons such as cyclopentane and cyclohexane; and aromatic hydrocarbons such as benzene, toluene, and xylene. These inert solvents may be used alone or in combination of two or more. The amount of the inert solvent used is not particularly limited, but is an amount that provides a monomer concentration of, for example, 1 to 50% by weight, and preferably 10 to 40% by weight.
[0022] The polymerization initiator used in the polymerization is not particularly limited as long as it can polymerize a monomer containing a conjugated diene compound to give a conjugated diene polymer chain having an active end. Specific examples of the polymerization initiator include polymerization initiators using an organic alkali metal compound, an organic alkaline earth metal compound, and a lanthanum series metal compound as a main catalyst. Examples of the organic alkali metal compound include organic monolithium compounds such as n-butyl lithium, sec-butyl lithium, t-butyl lithium, hexyl lithium, phenyl lithium, and stilbene lithium; organic polyvalent lithium compounds such as dilithiomethane, 1,4-dilithiobutane, 1,4-dilithio-2-ethylcyclohexane, 1,3,5-trilithiobenzene, and 1,3,5-tris(lithiomethyl)benzene; organic sodium compounds such as sodium naphthalene; and organic potassium compounds such as potassium naphthalene. Examples of organic alkaline earth metal compounds include di-n-butyl magnesium, di-n-hexyl magnesium, diethoxy calcium, calcium distearate, di-t-butoxy strontium, diethoxy barium, diisopropoxy barium, diethylmercapto barium, di-t-butoxy barium, diphenoxy barium, diethylamino barium, barium distearate, diketyl barium, etc. Examples of polymerization initiators using a lanthanum series metal compound as a main catalyst include polymerization initiators using a lanthanum series metal salt consisting of a lanthanum series metal such as lanthanum, cerium, praseodymium, neodymium, samarium, gadolinium, etc., a carboxylic acid, and a phosphorus-containing organic acid, etc., as a main catalyst, and a co-catalyst such as an alkyl aluminum compound, an organoaluminum hydride compound, an organoaluminum halide compound, etc. Among these polymerization initiators, the organic monolithium compounds and the organic polyvalent lithium compounds are preferably used, the organic monolithium compounds are more preferably used, and n-butyllithium is particularly preferably used. The organic alkali metal compound may be used as an organic alkali metal amide compound by reacting it in advance with a secondary amine compound such as dibutylamine, dihexylamine, dibenzylamine, pyrrolidine, piperidine, hexamethyleneimine, and heptamethyleneimine. By using the organic alkali metal amide compound as a polymerization initiator, the obtained cross-linked rubber product can have excellent low heat generation properties and wet grip properties. These polymerization initiators may be used alone or in combination of two or more.
[0023] Examples of the organic alkali metal amide compound include those obtained by reacting an organic alkali metal compound with a secondary amine compound. Among them, in the production method of the present invention, a compound represented by the following general formula (3) can be preferably used. [ka]
[0024] In general formula (3), M 1 represents an alkali metal atom, and R 11 , R 12 each independently represents an alkyl group, a cycloalkyl group, an aryl group, an aralkyl group, a protecting group for an amino group, or a group capable of generating a hydroxyl group upon hydrolysis; R 11 and R 12 may be bonded to each other to form a ring structure together with the nitrogen atom to which they are bonded, and when forming such a ring structure, they may form a ring structure together with, in addition to the nitrogen atom to which they are bonded, a heteroatom other than the nitrogen atom to which they are bonded.
[0025] The alkyl group is not particularly limited, but is preferably an alkyl group having 1 to 20 carbon atoms, and more preferably an alkyl group having 1 to 10 carbon atoms. Examples of such an alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, and an n-decyl group.
[0026] The cycloalkyl group is not particularly limited, but is preferably a cycloalkyl group having 3 to 20 carbon atoms, and more preferably a cycloalkyl group having 3 to 12 carbon atoms. Examples of such cycloalkyl groups include a cyclopropyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, a cyclooctyl group, and a cyclododecyl group.
[0027] The aryl group is not particularly limited, but is preferably an aryl group having 6 to 12 carbon atoms, and more preferably an aryl group having 6 to 10 carbon atoms. Examples of such aryl groups include a phenyl group, a 1-naphthyl group, and a 2-naphthyl group.
[0028] The aralkyl group is not particularly limited, but is preferably an aralkyl group having 7 to 13 carbon atoms, and more preferably an aralkyl group having 7 to 9 carbon atoms. Examples of such aralkyl groups include a benzyl group and a phenethyl group.
[0029] The protecting group for the amino group is not particularly limited as long as it acts as a protecting group for the amino group, and examples thereof include alkylsilyl groups, etc. Examples of such alkylsilyl groups include trimethylsilyl groups, triethylsilyl groups, triphenylsilyl groups, methyldiphenylsilyl groups, ethylmethylphenylsilyl groups, and tert-butyldimethylsilyl groups. In addition, R 11 , and / or R 12 is a protecting group for an amino group, the protecting group for the amino group is removed, and the R 13 , and / or R 14 It is possible to introduce a structure in which is a hydrogen atom.
[0030] The group that can be hydrolyzed to generate a hydroxyl group is not particularly limited as long as it is a group that generates a hydroxyl group by hydrolysis in the presence of an acid or the like, and examples of the group include an alkoxyalkyl group and a group containing an epoxy group. Examples of the alkoxyalkyl group include a methoxymethyl group, an ethoxymethyl group, an ethoxyethyl group, a propoxymethyl group, a butoxymethyl group, a butoxyethyl group, and a propoxyethyl group. Examples of the group containing an epoxy group include a group represented by the following general formula (4). -Z 1 -Z 2 -E 1 (4) In general formula (4), Z 1 is an alkylene group or an alkylarylene group having 1 to 10 carbon atoms, Z 2 is a methylene group, a sulfur atom or an oxygen atom, and E 1 is a glycidyl group.
[0031] Also, R 11 and R 12 may be bonded to each other to form a ring structure together with the nitrogen atom to which they are bonded, in which case, R 11 and R 12 A specific example of the structure formed by the nitrogen atom bonded to the ring is an azetidine ring (R 11 and R 12 propylene group), pyrrolidine ring (R 11 and R 12 butylene group), piperidine ring (R 11 and R 12 pentylene group), hexamethyleneimine ring (R 11 and R 12 However, hexylene groups are also included. R 11 and R 12 When they are bonded to each other to form a ring structure together with the nitrogen atom to which they are bonded, the ring structure is preferably a 4- to 8-membered ring structure.
[0032] In addition, in the general formula (3), M1 is an alkali metal atom. Examples of such an alkali metal atom include a lithium atom, a sodium atom, and a potassium atom. Among these, a lithium atom is preferred from the viewpoint of polymerization activity.
[0033] In the first step of the production method of the present invention, when a compound represented by general formula (3) is used as a polymerization initiator, the amine structure forming the organic alkali metal amide compound remains in a state of being bonded to the polymerization initiation terminal of the polymer chain. Therefore, when a compound represented by general formula (3) is used as a polymerization initiator, a structure represented by the following general formula (5) is introduced to one terminal of the polymer chain forming the obtained conjugated diene rubber. [ka]
[0034] In general formula (5), R 13 , R 14 each independently represents a hydrogen atom, an alkyl group, a cycloalkyl group, an aryl group, an aralkyl group, a protecting group for an amino group, or a group which can be hydrolyzed to produce a hydroxyl group; R 13 and R 14 may be bonded to each other to form a ring structure together with the nitrogen atom to which they are bonded, and when forming such a ring structure, they may form a ring structure together with, in addition to the nitrogen atom to which they are bonded, a heteroatom other than the nitrogen atom to which they are bonded.
[0035] R 13 , R 14 Examples of the alkyl group, cycloalkyl group, aryl group, aralkyl group, protecting group for amino group, or group capable of generating a hydroxyl group upon hydrolysis include R 11 , R 12 The same can be mentioned as R 13 and R 14 In the case where R is bonded to each other to form a ring structure together with the nitrogen atom to which they are bonded, 11 , R 12 can be the same as In addition, R 13 , R 14 The hydrogen atom capable of being introduced is introduced by removing the protecting group of the amino group.
[0036] In the production method of the present invention, when an organic alkali metal amide compound is used as a polymerization initiator, the resulting conjugated diene rubber can have an amine structure at one end and a specific structure derived from a modifier at the other end. As a result, due to the effect of such an amine structure, the cross-linked rubber using the resulting conjugated diene rubber has excellent low heat build-up properties and wet grip properties.
[0037] The method of adding the organic alkali metal amide compound as a polymerization initiator to the polymerization system is not particularly limited, and a method of reacting an organic alkali metal compound with a secondary amine compound in advance to obtain an organic alkali metal amide compound, which is then mixed with a monomer containing a conjugated diene compound to proceed with the polymerization reaction can be adopted. Alternatively, a method of separately adding an organic alkali metal compound and a secondary amine compound to the polymerization system, mixing them with a monomer containing a conjugated diene compound to generate an organic alkali metal amide compound in the polymerization system, and proceeding with the polymerization reaction can be adopted. The reaction conditions such as the reaction temperature are not particularly limited, and may be, for example, in accordance with the desired polymerization reaction conditions.
[0038] The amount of the secondary amine compound used may be determined depending on the amount of the polymerization initiator to be added, but is usually in the range of 0.01 to 1.5 mmol, preferably 0.1 to 1.2 mmol, and more preferably 0.5 to 1.0 mmol, per 1 mmol of the organic alkali metal compound.
[0039] The amount of the polymerization initiator used may be determined depending on the molecular weight of the desired conjugated diene polymer chain, but is usually in the range of 1 to 50 mmol, preferably 1.5 to 20 mmol, and more preferably 2 to 15 mmol per 1000 g of monomer.
[0040] The polymerization temperature is usually in the range of −80 to +150° C., preferably 0 to 100° C., and more preferably 30 to 90° C. As the polymerization mode, any mode such as a batch mode or a continuous mode can be adopted, but when a conjugated diene compound and an aromatic vinyl compound are copolymerized, the batch mode is preferred in that it is easy to control the randomness of the bonds between the conjugated diene monomer units and the aromatic vinyl monomer units.
[0041] In addition, when polymerizing a monomer containing a conjugated diene compound, it is preferable to add a polar compound to an inert organic solvent in order to adjust the vinyl bond content in the conjugated diene monomer unit in the resulting conjugated diene polymer chain. Examples of polar compounds include ether compounds such as dibutyl ether, tetrahydrofuran, and 2,2-di(tetrahydrofuryl)propane; tertiary amines such as tetramethylethylenediamine; alkali metal alkoxides; and phosphine compounds. Among these, ether compounds and tertiary amines are preferred, tertiary amines are more preferred, and tetramethylethylenediamine is particularly preferred. These polar compounds may be used alone or in combination of two or more. The amount of the polar compound used may be determined according to the desired vinyl bond content, and is preferably 0.001 to 100 mol, more preferably 0.01 to 10 mol, relative to 1 mol of the polymerization initiator. When the amount of the polar compound used is within this range, it is easy to adjust the vinyl bond content in the conjugated diene monomer unit, and problems due to deactivation of the polymerization initiator are unlikely to occur.
[0042] The vinyl bond content in the conjugated diene monomer units in the conjugated diene polymer chain having an active terminal obtained in the first step of the production method of the present invention is preferably 1 to 90% by weight, more preferably 3 to 80% by weight, and particularly preferably 5 to 70% by weight. By setting the vinyl bond content in the conjugated diene monomer units within the above range, the obtained cross-linked rubber product can be made to have excellent low heat build-up properties.
[0043] The weight average molecular weight (Mw) of the conjugated diene polymer chain having an active end obtained in the first step of the production method of the present invention is not particularly limited, but is preferably 100,000 to 1,000,000, more preferably 150,000 to 700,000, and particularly preferably 150,000 to 500,000, as a value measured by gel permeation chromatography in terms of polystyrene. By setting the weight average molecular weight (Mw) of the conjugated diene polymer chain having an active end within the above range, the obtained cross-linked rubber product can have a good balance between wet grip properties and low heat build-up.
[0044] In addition, the molecular weight distribution represented by the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the conjugated diene polymer chain having an active end obtained in the first step of the production method of the present invention is not particularly limited, but is preferably 1.0 to 3.0, and more preferably 1.0 to 2.5. When the molecular weight distribution (Mw / Mn) of the conjugated diene polymer chain having an active end is within the above range, the production of the conjugated diene rubber becomes easy.
[0045] In the production method of the present invention, in order to obtain a cross-linked rubber product with even better low heat build-up properties, it is preferable that the first step is the following step. That is, a step of polymerizing isoprene or a monomer containing isoprene and an aromatic vinyl compound in an inert solvent using a polymerization initiator to form a polymer block (A) having an active terminal containing 80 to 100% by weight of isoprene monomer units and 0 to 20% by weight of aromatic vinyl monomer units; and mixing the polymer block (A) having an active end with a monomer containing 1,3-butadiene or 1,3-butadiene and an aromatic vinyl compound to continue the polymerization reaction, thereby forming a polymer block (B) having an active end containing 50 to 100% by weight of 1,3-butadiene monomer units and 0 to 50% by weight of aromatic vinyl monomer units in a continuous manner with the polymer block (A), thereby obtaining a conjugated diene-based polymer chain having an active end.
[0046] By employing such a process, the conjugated diene polymer chain having an active end obtained in the first process can be one which comprises a polymer block (A) containing 80 to 100% by weight of isoprene monomer units and 0 to 20% by weight of aromatic vinyl monomer units and a polymer block (B) containing 50 to 100% by weight of 1,3-butadiene monomer units and 0 to 50% by weight of aromatic vinyl monomer units, which are formed in a continuous manner. Such an embodiment will be described below.
[0047] [Polymer block (A)] The polymer block (A) in the conjugated diene polymer chain according to one embodiment of the present invention may contain 80-100% by weight of isoprene monomer units and 0-20% by weight of aromatic vinyl monomer units in the polymer block (A), preferably 85-95% by weight of isoprene monomer units and 5-15% by weight of aromatic vinyl monomer units, and more preferably 89-95% by weight of isoprene monomer units and 5-11% by weight of aromatic vinyl monomer units. When the content ratio of isoprene monomer units and aromatic vinyl monomer units is within the above range, when silica is blended with the conjugated diene rubber, the affinity between the conjugated diene rubber and silica is good, and the low heat build-up property of the cross-linked rubber obtained by using this can be further improved.
[0048] The aromatic vinyl compound used to constitute the aromatic vinyl monomer unit contained in the polymer block (A) may be the same as the aromatic vinyl compound described above, and among these, styrene is preferred. These aromatic vinyl compounds may be used alone or in combination of two or more.
[0049] The polymer block (A) preferably consists of only isoprene monomer units, or isoprene monomer units and aromatic vinyl monomer units, but may contain other monomer units in addition to the isoprene monomer units, or isoprene monomer units and aromatic vinyl monomer units, if desired. Other compounds used to form the other monomer units include conjugated diene compounds other than isoprene, such as 1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, 1,3-pentadiene, and 1,3-hexadiene; α,β-unsaturated nitriles, such as acrylonitrile and methacrylonitrile; unsaturated carboxylic acids or acid anhydrides, such as acrylic acid, methacrylic acid, and maleic anhydride; unsaturated carboxylic acid esters, such as methyl methacrylate, ethyl acrylate, and butyl acrylate; non-conjugated dienes, such as 1,5-hexadiene, 1,6-heptadiene, 1,7-octadiene, dicyclopentadiene, and 5-ethylidene-2-norbornene; and the like. Among these, 1,3-butadiene is preferred. These other monomers can be used alone or in combination of two or more. The content of other monomer units in the polymer block (A) is preferably 20% by weight or less, more preferably 10% by weight or less, and even more preferably 6% by weight or less.
[0050] In the present invention, the polymer block (A) in the conjugated diene polymer chain is formed by polymerizing a monomer containing isoprene or a monomer containing isoprene and an aromatic vinyl compound with a polymerization initiator in an inert solvent. The formed polymer block (A) has an active terminal.
[0051] The inert solvent used in the polymerization of isoprene or a monomer containing isoprene and an aromatic vinyl compound to form the polymer block (A) may be the same as the inert solvent described above. The amount of the inert solvent used is preferably an amount that results in a monomer concentration of 1 to 80% by weight, more preferably an amount that results in a monomer concentration of 10 to 50% by weight.
[0052] The polymerization initiator used to form the polymer block (A) is not particularly limited as long as it can polymerize isoprene or a monomer containing isoprene and an aromatic vinyl compound to give a polymer chain having an active terminal. Specific examples of the polymerization initiator include the same as those described above.
[0053] The amount of the polymerization initiator used may be determined depending on the target molecular weight, but is preferably in the range of 4 to 250 mmol, more preferably 6 to 200 mmol, and particularly preferably 10 to 70 mmol, per 100 g of isoprene or a monomer containing isoprene and an aromatic vinyl compound.
[0054] The polymerization temperature when polymerizing isoprene or a monomer containing isoprene and an aromatic vinyl compound is preferably in the range of -80 to +150°C, more preferably 0 to 100°C, and further preferably 20 to 90°C. Any polymerization mode, such as a batch mode or a continuous mode, can be adopted. In addition, various bonding modes, such as a block mode, a tapered mode, and a random mode, can be adopted.
[0055] In the production method according to one aspect of the present invention, it is preferable to add a polar compound to the inert solvent during polymerization in order to adjust the vinyl bond content in the isoprene monomer unit in the polymer block (A). The polar compound may be the same as the polar compound described above. The amount of the polar compound used may be determined according to the desired vinyl bond content, and is preferably 0.01 to 30 moles, more preferably 0.05 to 10 moles, per mole of the polymerization initiator. When the amount of the polar compound used is within the above range, it is easy to adjust the vinyl bond content in the isoprene monomer unit, and furthermore, problems due to deactivation of the polymerization initiator are unlikely to occur. In addition, by increasing the amount of the polar compound used within the above range, the vinyl bond content in the isoprene monomer unit can be increased.
[0056] The vinyl bond content in the isoprene monomer unit in the polymer block (A) is preferably 5 to 90% by weight, more preferably 5 to 80% by weight. By setting the vinyl bond content in the isoprene monomer unit within the above range, the low heat build-up property of the obtained cross-linked rubber product can be further improved. In this specification, the vinyl bond content in the isoprene monomer unit refers to the ratio of the total amount of the isoprene monomer unit having a 1,2-structure and the isoprene monomer unit having a 3,4-structure in the isoprene monomer unit.
[0057] The weight average molecular weight (Mw) of the polymer block (A), expressed as a polystyrene equivalent value measured by gel permeation chromatography, is preferably 500 to 15,000, more preferably 1,000 to 12,000, and particularly preferably 1,500 to 10,000. When the weight average molecular weight of the polymer block (A) is within the above range, the low heat build-up property of the obtained cross-linked rubber can be further improved.
[0058] The molecular weight distribution of the polymer block (A), which is expressed by the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn), is preferably 1.0 to 1.5, and more preferably 1.0 to 1.3. When the molecular weight distribution value (Mw / Mn) of the polymer block (A) is within the above range, the production of the conjugated diene rubber becomes easier.
[0059] [Polymer block (B)] The polymer block (B) in the conjugated diene polymer chain according to one embodiment of the present invention may contain 50-100% by weight of 1,3-butadiene monomer units and 0-50% by weight of aromatic vinyl monomer units, but preferably contains 52-95% by weight of 1,3-butadiene monomer units and 5-48% by weight of aromatic vinyl monomer units. When the content ratio of the 1,3-butadiene monomer units and the aromatic vinyl monomer units is within the above range, the production of the conjugated diene rubber becomes easier.
[0060] As the aromatic vinyl compound used to constitute the aromatic vinyl monomer unit contained in the polymer block (B), the same aromatic vinyl compounds as those mentioned above can be used, and among these, styrene is preferred.
[0061] The polymer block (B) is preferably composed of only 1,3-butadiene monomer units, or 1,3-butadiene monomer units and aromatic vinyl monomer units, but may contain other monomer units in addition to 1,3-butadiene monomer units, or 1,3-butadiene monomer units and aromatic vinyl monomer units, as desired, within the range that does not impair the essential characteristics of the present invention. As other monomers used to constitute the other monomer units, the same compounds exemplified in the above-mentioned polymer block (A) (excluding 1,3-butadiene) can be used. In addition, isoprene can also be used as the other monomer in the polymer block (B). The content ratio of other monomer units in the polymer block (B) is preferably 50% by weight or less, more preferably 40% by weight or less, and even more preferably 35% by weight or less.
[0062] In one embodiment of the present invention, the polymer block (B) in the conjugated diene polymer chain is formed in a continuous manner with the polymer block (A) by mixing the polymer block (A) having the above-mentioned active terminal with a monomer containing 1,3-butadiene or 1,3-butadiene and an aromatic vinyl compound and continuing the polymerization reaction. The formed polymer block (B) has an active terminal. On the other hand, the active terminal disappears from the polymer block (A).
[0063] The inert solvent used in the polymerization of the polymer block (A) with a monomer containing 1,3-butadiene or 1,3-butadiene and an aromatic vinyl compound to form the polymer block (B) is not particularly limited, and the same inert solvents as those described above can be used.
[0064] The amount of the polymer block (A) having an active end used in forming the polymer block (B) may be determined depending on the target molecular weight, but is preferably in the range of 0.1 to 5 mmol, more preferably 0.15 to 2 mmol, and even more preferably 0.2 to 1.5 mmol, per 100 g of 1,3-butadiene or a monomer containing 1,3-butadiene and an aromatic vinyl compound.
[0065] The method of mixing the polymer block (A) with 1,3-butadiene or a monomer containing 1,3-butadiene and an aromatic vinyl compound is not particularly limited, and the polymer block (A) having an active end may be added to a solution of 1,3-butadiene or a monomer containing 1,3-butadiene and an aromatic vinyl compound, or 1,3-butadiene or a monomer containing 1,3-butadiene and an aromatic vinyl compound may be added to a solution of the polymer block (A) having an active end. From the viewpoint of controlling the polymerization, the method of adding the polymer block (A) having an active end to a solution of 1,3-butadiene or a monomer containing 1,3-butadiene and an aromatic vinyl compound is preferred.
[0066] The polymerization temperature when polymerizing 1,3-butadiene or a monomer containing 1,3-butadiene and an aromatic vinyl compound is preferably in the range of -80 to +150°C, more preferably 0 to 100°C, and further preferably 20 to 90°C. As the polymerization mode, any mode such as a batch system or a continuous system can be adopted. When the polymer block (B) is a copolymer chain, the batch system is preferred in that it is easy to control the randomness of the bonds.
[0067] When the polymer block (B) is a copolymer chain, the bonding pattern of each monomer can be various bonding patterns such as block, tapered, and random. Among these, the random bonding pattern is preferable. By making the bonding pattern random, the low heat generation property of the obtained cross-linked rubber product can be further improved. When making the bonding pattern of 1,3-butadiene and the aromatic vinyl compound random, it is preferable to polymerize 1,3-butadiene or 1,3-butadiene and the aromatic vinyl compound by continuously or intermittently supplying them to the polymerization system so that the ratio of the aromatic vinyl compound to the total amount of 1,3-butadiene and the aromatic vinyl compound in the polymerization system does not become too high.
[0068] In one embodiment of the present invention, in order to adjust the vinyl bond content in the 1,3-butadiene monomer unit in the polymer block (B), it is preferable to add a polar compound to the inert solvent during polymerization, as in the case of adjusting the vinyl bond content in the isoprene monomer unit in the polymer block (A). However, when a polar compound is added to the inert solvent in an amount sufficient to adjust the vinyl bond content in the 1,3-butadiene monomer unit in the polymer block (B) during preparation of the polymer block (A), it is not necessary to add a new polar compound. The polar compound used to adjust the vinyl bond content can be the same as the polar compound described above. The amount of the polar compound used may be determined according to the desired vinyl bond content, and may be adjusted within a range of preferably 0.01 to 100 mol, more preferably 0.1 to 30 mol, relative to 1 mol of the polymerization initiator used in the first polymerization reaction (polymerization reaction for forming the first polymer block (A)). When the amount of the polar compound used is within this range, the vinyl bond content in the 1,3-butadiene monomer unit can be easily adjusted, and problems due to deactivation of the polymerization initiator are unlikely to occur.
[0069] The vinyl bond content in the 1,3-butadiene monomer unit in the polymer block (B) is preferably 1 to 90% by weight, more preferably 3 to 80% by weight, and particularly preferably 5 to 70% by weight. By setting the vinyl bond content in the 1,3-butadiene monomer unit in the polymer block (B) within the above range, the obtained cross-linked rubber product can be made to have excellent low heat build-up properties.
[0070] In this way, a conjugated diene polymer chain having an active end, which has a polymer block (A) and a polymer block (B), can be obtained. In one aspect of the present invention, the conjugated diene polymer chain having an active end is preferably composed of a polymer block (A)-polymer block (B) from the viewpoint of productivity, and the end of the polymer block (B) is preferably an active end, but may have a plurality of polymer blocks (A) or may have other polymer blocks. For example, a conjugated diene polymer chain having an active end, such as polymer block (A)-polymer block (B)-polymer block (A), may be mentioned. In this case, an active end is formed at the end of the polymer block (A) formed following the polymer block (B). When forming the polymer block (A) on the active end side of the conjugated diene polymer chain, the amount of isoprene used is preferably 10 to 100 mol, more preferably 15 to 70 mol, and particularly preferably 20 to 35 mol, relative to 1 mol of the polymerization initiator used in the initial polymerization reaction (polymerization reaction for forming the first polymer block (A)).
[0071] The weight ratio of polymer block (A) to polymer block (B) in the conjugated diene polymer chain having an active end obtained in one embodiment of the present invention (when a plurality of polymer blocks (A) and polymer blocks (B) are present, the weight ratio is based on the total weight of each) (weight of polymer block (A)) / (weight of polymer block (B)) is preferably 0.001 to 0.1, more preferably 0.003 to 0.07, and particularly preferably 0.005 to 0.05. By setting the weight ratio of polymer block (A) to polymer block (B) within the above range, the obtained cross-linked rubber product can have a good balance between wet grip properties and low heat build-up.
[0072] The content ratio of the total monomer units of isoprene monomer units and 1,3-butadiene monomer units and aromatic vinyl monomer units in the conjugated diene polymer chain having an active end, which has polymer block (A) and polymer block (B), is preferably 50 to 100% by weight of the total monomer units of isoprene monomer units and 1,3-butadiene monomer units and 0 to 50% by weight of aromatic vinyl monomer units, and more preferably 52 to 95% by weight of the total monomer units of isoprene monomer units and 1,3-butadiene monomer units and 5 to 48% by weight of aromatic vinyl monomer units. In addition, the vinyl bond contents in the isoprene monomer units and the 1,3-butadiene monomer units in the conjugated diene polymer chain having an active end, which has the polymer block (A) and the polymer block (B), are preferably in the same range as the vinyl bond content in the 1,3-butadiene monomer units in the above-mentioned polymer block (B).
[0073] <Second process> The second step of the production method of the present invention is a step of adding and reacting a polyorganosiloxane represented by the following general formula (1) to the conjugated diene polymer chain having an active end obtained in the first step in a ratio of 1 mol or more calculated as the number of repeating units of the siloxane structure (-Si-O-) in the polyorganosiloxane per 1 mol of the polymerization initiator used in the first step. [ka] In general formula (1), R 1 ~R 8 is an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 12 carbon atoms, which may be the same or different. X 1 and X 4 is any group selected from the group consisting of an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, and an epoxy group-containing group having 4 to 12 carbon atoms, which may be the same or different. 2 is an alkoxy group having 1 to 5 carbon atoms or a group having 4 to 12 carbon atoms containing an epoxy group, 2 They may be the same or different. X 3 is a group containing 2 to 20 repeating alkylene glycol units, X 3 When there are a plurality of m, they may be the same or different. m is an integer of 3 to 200, n is an integer of 0 to 200, k is an integer of 0 to 200, and m+n+k is 3 or more.
[0074] In the polyorganosiloxane represented by the general formula (1), R 1 ~R 8 , X 1 and X 4 Examples of the alkyl group having 1 to 6 carbon atoms that can constitute the above include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, a butyl group, a pentyl group, a hexyl group, and a cyclohexyl group. Examples of the aryl group having 6 to 12 carbon atoms include a phenyl group and a methylphenyl group. Among these, from the viewpoint of ease of production of the polyorganosiloxane itself, a methyl group and an ethyl group are preferred.
[0075] In addition, in the polyorganosiloxane represented by the general formula (1), X 1 , X 2 and X 4Examples of the alkoxy group having 1 to 5 carbon atoms that can constitute the above include a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, and a butoxy group. Among these, from the viewpoint of ease of production of the polyorganosiloxane itself, a methoxy group and an ethoxy group are preferred.
[0076] Furthermore, in the polyorganosiloxane represented by the general formula (1), X 1 , X 2 and X 4 Examples of the epoxy group-containing group having 4 to 12 carbon atoms that can constitute the above formula include groups represented by the following general formula (6). -Z 3 -Z 4 -E 2 (6) In general formula (6), Z 3 is an alkylene group or an alkylarylene group having 1 to 10 carbon atoms; Z 4 is a methylene group, a sulfur atom, or an oxygen atom, and E 2 is a hydrocarbon group having 2 to 10 carbon atoms and having an epoxy group.
[0077] The group represented by formula (6) is Z 4 is preferably an oxygen atom, and Z 4 is an oxygen atom, and E 2 is more preferably a glycidyl group, and Z 3 is an alkylene group having 1 to 3 carbon atoms, and Z 4 is an oxygen atom, and E 2 is particularly preferably a glycidyl group.
[0078] In addition, in the polyorganosiloxane represented by the general formula (1), X 1 and X 4 Among the above, X is preferably a group containing an epoxy group and having 4 to 12 carbon atoms, or an alkyl group having 1 to 6 carbon atoms. 2 Among the above, an epoxy group-containing group having 4 to 12 carbon atoms is preferable. 1 and X 4is an alkyl group having 1 to 6 carbon atoms, and X 2 It is more preferable that the group is an epoxy group-containing group having 4 to 12 carbon atoms.
[0079] In addition, in the polyorganosiloxane represented by the general formula (1), X 3 That is, as a group containing 2 to 20 repeating units of alkylene glycol, a group represented by the following general formula (7) is preferred. [ka] In the general formula (7), t is an integer of 2 to 20, and X 5 is an alkylene group or alkylarylene group having 2 to 10 carbon atoms, R 15 is a hydrogen atom or a methyl group, and X 6 is an alkoxy group or an aryloxy group having 1 to 10 carbon atoms. Among these, t is an integer of 2 to 8, and X 5 is an alkylene group having 3 carbon atoms, and R 15 is a hydrogen atom and X 6 is preferably a methoxy group.
[0080] In the polyorganosiloxane represented by the general formula (1), m is an integer of 3 to 200, preferably an integer of 20 to 150, and more preferably an integer of 30 to 120. When m is 3 or more, the coupling ratio of the resulting conjugated diene rubber is high, resulting in excellent hot flow properties. When m is 200 or less, the polyorganosiloxane represented by the general formula (1) itself is easier to produce, and the viscosity does not become too high, making it easier to handle.
[0081] In the polyorganosiloxane represented by the general formula (1), n is an integer of 0 to 200, preferably an integer of 0 to 150, more preferably an integer of 0 to 120. k is an integer of 0 to 200, preferably an integer of 0 to 150, more preferably an integer of 0 to 130. The total number of m, n, and k is 3 or more, preferably 3 to 400, more preferably 20 to 300, and particularly preferably 30 to 250. When the total number of m, n, and k is 3 or more, the reaction between the polyorganosiloxane represented by the general formula (1) and the conjugated diene polymer chain having an active terminal easily proceeds, and when the total number of m, n, and k is 400 or less, the polyorganosiloxane represented by the general formula (1) itself is easily produced, and the viscosity does not become too high, making it easy to handle.
[0082] The amount of polyorganosiloxane used in the second step of the production method of the present invention is 1 mole or more, preferably 1 to 2.5 moles, and more preferably 1.1 to 2 moles, calculated as the number of repeating units of the siloxane structure (-Si-O-) in the polyorganosiloxane, per mole of the polymerization initiator used for polymerization in the above-mentioned first step.
[0083] By setting the amount of polyorganosiloxane to 1 mole or more in terms of the number of repeating units of the siloxane structure (-Si-O-) per mole of the polymerization initiator, it is possible to react substantially all of the active ends of the conjugated diene polymer chain having an active end obtained in the first step with the polyorganosiloxane, which is preferable. That is, the alkyl metal group, i.e., -R - M + (R is a hydrocarbon group forming a polymer chain end, and M is an alkali metal atom, an alkaline earth metal atom, or a lanthanide series metal atom) can be made to substantially not remain.
[0084] This can substantially prevent the compound represented by the general formula (2) from directly reacting with the active end of the conjugated diene polymer chain having the active end obtained in the first step when the compound represented by the general formula (2) is reacted in the third step described later. As a result, the compound represented by the general formula (2) can be appropriately reacted with the reaction residue generated by the reaction of the conjugated diene polymer chain with the polyorganosiloxane represented by the general formula (1). This allows the modified structure of the compound represented by the general formula (2) to be appropriately introduced into the conjugated diene polymer chain via the structure derived from the polyorganosiloxane represented by the general formula (1), and the effects of introducing such a modified structure, that is, excellent hot flow properties (difficulty in mutual adhesion of solidified crumbs), low heat generation properties, and wet grip properties, can be realized.
[0085] The method of reacting the polyorganosiloxane with the conjugated diene polymer chain having an active terminal is not particularly limited, but includes a method of mixing them in a solvent in which each of them can be dissolved. The solvent used in this case can be any of those exemplified as the inert solvent used in the first step described above. In this case, a method of adding the polyorganosiloxane to the polymerization solution used in the polymerization to obtain the conjugated diene polymer chain having an active terminal is simple and preferable. In this case, the polyorganosiloxane is preferably dissolved in an inert solvent and added to the polymerization system, and the solution concentration is preferably in the range of 1 to 50% by weight. The reaction temperature is not particularly limited, but is usually 0 to 120°C, and the reaction time is not particularly limited, but is usually 1 minute to 1 hour.
[0086] The time when polyorganosiloxane is added to the solution containing the conjugated diene polymer chain having an active terminal is not particularly limited, but it is preferable to add polyorganosiloxane to the solution when the polymerization reaction is not completed and the solution containing the conjugated diene polymer chain having an active terminal also contains a monomer, more specifically, when the solution containing the conjugated diene polymer chain having an active terminal contains 100 ppm or more, more preferably 300 to 50,000 ppm of monomer.By adding polyorganosiloxane in this way, it is possible to suppress the side reaction between the conjugated diene polymer chain having an active terminal and impurities contained in the polymerization system, and to control the reaction well.
[0087] In the second step of the production method of the present invention, the active terminal of the conjugated diene polymer chain having an active terminal obtained in the above-mentioned first step is reacted with polyorganosiloxane as a modifier, and the active terminal of the conjugated diene polymer chain reacts with a silicon atom in the siloxane structure. Alternatively, a part of the active terminal of the conjugated diene polymer chain is reacted with an alkoxy group or epoxy group (X which is essential in the general formula (1)) in the side chain of the polyorganosiloxane. 2 According to the second step of the production method of the present invention, a modified structure by siloxane is introduced into the conjugated diene polymer chain by such a reaction.
[0088] Specifically, the active end of the conjugated diene polymer chain reacts with the silicon atom in the siloxane structure, and the conjugated diene polymer chain forms a new bond between the silicon atom in the siloxane structure and the active end of the conjugated diene polymer chain, and a modified structure by siloxane is introduced at the end of the conjugated diene polymer chain. At the same time, a reaction residue between the oxygen atom in the siloxane structure and the metal atom that formed the active end of the conjugated diene polymer chain, such as -O - M + (M is an alkali metal atom, an alkaline earth metal atom, or a lanthanide series metal atom) is thought to be formed.
[0089] Alternatively, the active end of the conjugated diene polymer chain reacts with the epoxy group on the side chain of the polyorganosiloxane, opening the epoxy group and forming a new bond between the carbon atom at the portion where the epoxy group is opened and the active end of the conjugated diene polymer chain, introducing a siloxane structure to the end of the conjugated diene polymer chain, and forming a reaction residue between the oxygen atom in the epoxy group and the metal atom that formed the active end of the conjugated diene polymer chain, such as -O - M + Alternatively, the active end of the conjugated diene polymer chain reacts with an alkoxy group on the side chain of the polyorganosiloxane, resulting in the elimination of the alkoxy group, and the conjugated diene polymer chain forms a new bond between the silicon atom in the siloxane structure and the active end of the conjugated diene polymer chain, thereby introducing a siloxane structure into the end of the conjugated diene polymer chain.
[0090] In particular, in the second step of the production method of the present invention, the amount of polyorganosiloxane used is 1 mole or more per mole of polymerization initiator in terms of the number of repeating units of the siloxane structure (-Si-O-), so that a modified structure by siloxane can be introduced into almost all of the conjugated diene polymer chains having active ends obtained in the first step. Therefore, the alkyl metal group, i.e., -R - M + It is possible to make almost all of the -O as a reactive residue disappear. - M + However, in the present invention, a very small amount (for example, 5% by weight or less) of a conjugated diene polymer chain having an active end that is not modified with siloxane may be included (that is, a very small amount of an alkyl metal group, i.e., -R - M +The above does not exclude cases where the above-mentioned substances remain.
[0091] In the second step of the production method of the present invention, before reacting the conjugated diene polymer chain having an active end with the polyorganosiloxane represented by general formula (1), a part of the active end of the conjugated diene polymer chain having an active end may be coupled or modified by adding a coupling agent or modifying agent that has been conventionally used to the polymerization system, within a range that does not impair the effects of the present invention.
[0092] <3rd process> The third step of the production method of the present invention is a step of reacting the conjugated diene polymer chain reacted with the polyorganosiloxane obtained in the second step with a compound represented by the following general formula (2). [ka] In general formula (2), R 9 is a hydrocarbyl group, A 1 is a group capable of reacting with a reaction residue formed by the reaction of a conjugated diene polymer chain having an active terminal with a polyorganosiloxane, and A 2 is a group containing a nitrogen atom, p is an integer of 0 to 2, q is an integer of 1 to 3, r is an integer of 1 to 3, and p+q+r=4.
[0093] According to the present invention, in the above-mentioned second step, an alkyl metal group, i.e., -R - M + In place of these, -O as a reaction residue by the reaction with the polyorganosiloxane represented by the general formula (1) is - M + According to the third step of the present invention, the compound represented by the general formula (2) has a group represented by the following formula: - M + A group represented by (-O - M +and (including those in which a group represented by the formula:
[0094] That is, according to the present invention, the compound represented by the general formula (2) is -R - M + This can appropriately prevent the modified structure of the compound represented by general formula (2) from being directly introduced into the conjugated diene polymer chain by reacting with the group represented by general formula (1), and thus the modified structure of the compound represented by general formula (2) can be appropriately introduced into the conjugated diene polymer chain via the structure derived from the polyorganosiloxane represented by general formula (1). As a result, the conjugated diene rubber obtained by the production method of the present invention can give a cross-linked rubber product that is excellent in hot flow properties (difficulty in adhesion of solidified crumbs to each other) and has excellent low heat generation properties and wet grip properties.
[0095] However, the conjugated diene polymer chain reacted with polyorganosiloxane, which is used in the third step of the production method of the present invention, may be one that has been subjected to the above-mentioned second step, and in addition to the conjugated diene polymer chain having a siloxane-modified structure introduced therein, a very small amount (for example, 5% by weight or less) of a conjugated diene polymer chain having an unmodified active end to which a siloxane-modified structure has not been introduced may remain (i.e., a very small amount of an alkyl metal group, i.e., -R - M + may remain), and further, -O may be included as a reactive residue formed as a result of the introduction of a modified structure by siloxane. - M + may include those in which a part of the formula is hydrolyzed and converted into a hydroxyl group.
[0096] In the compound represented by the general formula (2), R 9is a hydrocarbyl group, and examples of such groups include an alkyl group, a cycloalkyl group, an alkenyl group, an aryl group, and an aralkyl group, with an alkyl group having 1 to 6 carbon atoms being preferred. Examples of the alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, a butyl group, a pentyl group, and a hexyl group, with a methyl group and an ethyl group being more preferred among these.
[0097] In the compound represented by the general formula (2), A in the general formula (2) 1 is a reaction residue (typically, -O) formed by the reaction of a conjugated diene polymer chain having an active terminal with a polyorganosiloxane. - M + is a group capable of reacting with a group represented by -OR 10 (R 10 R is preferably a hydrogen atom or a hydrocarbyl group. 10 Examples of hydrocarbyl groups that can constitute the above include alkyl groups, cycloalkyl groups, alkenyl groups, aryl groups, and aralkyl groups, and from the viewpoint of reactivity with the above-mentioned reaction residues, alkyl groups having 1 to 6 carbon atoms are preferred. Examples of alkyl groups having 1 to 6 carbon atoms include methyl groups, ethyl groups, n-propyl groups, isopropyl groups, butyl groups, pentyl groups, and hexyl groups, and among these, methyl groups and ethyl groups are more preferred.
[0098] In the compound represented by the general formula (2), A in the general formula (2) 2is a group containing a nitrogen atom, and is not particularly limited as long as it is a group containing a nitrogen atom, but is preferably an organic group having a nitrogen atom, and examples thereof include a 3-aminopropyl group, a 4-aminobutyl group, a 3-(2-aminoethylamino)propyl group, a 2-dimethylaminoethyl group, a 3-dimethylaminopropyl group, a 3-diethylaminopropyl group, a 3-dipropylaminopropyl group, a 3-dibutylaminopropyl group, a 3-phenylmethylaminopropyl group, a 3-(4-methylpiperazinyl)propyl group, an N,N-bis(trimethylsilyl)aminopropyl group, an N,N-bis(triethylsilyl)aminopropyl group, and an N,N',N'-tris(trimethylsilyl)-N-(2-aminoethyl)-3-aminopropyl group. Among these, from the viewpoint of further improving the low heat build-up and wet grip properties of the obtained cross-linked rubber product, groups containing a primary amino group having an active hydrogen atom and / or a secondary amino group having an active hydrogen atom, such as a 3-aminopropyl group, a 4-aminobutyl group, a 3-(2-aminoethylamino)propyl group, etc. Here, the term "active hydrogen atom" refers to a hydrogen atom bonded to an atom other than a carbon atom, and preferably has a bond energy lower than that of the carbon-hydrogen bond of a polymethylene chain.
[0099] In the compound represented by the general formula (2), p is an integer of 0 to 2, q is an integer of 1 to 3, r is an integer of 1 to 3, and p+q+r=4. From the viewpoint of reactivity with the reaction residue generated by the reaction of the conjugated diene polymer chain having an active end with the polyorganosiloxane, p is preferably an integer of 0 to 1, q is an integer of 2 to 3, and r is an integer of 1 to 2, and more preferably p=0, q=3, and r=1. When p is 2, two R groups are contained in one molecule of the compound represented by the general formula (2). 9 The groups represented by may be the same or different from each other. Similarly, when q is 2 or 3, the groups represented by A are contained in one molecule of the compound represented by the general formula (2). 1The groups represented by the formula (2) may be the same or different from each other. When r is 2 or 3, a plurality of A 2 The groups represented by the following formula (I) may be the same or different from each other.
[0100] Specific examples of the compound represented by formula (2) are not particularly limited, but include, for example, A 2 is a group containing a primary amino group having an active hydrogen atom and / or a secondary amino group having an active hydrogen atom, such as 3-aminopropyldimethylmethoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyldimethylethoxysilane, 3-aminopropylmethyldiethoxysilane, and 3-aminopropyltriethoxysilane. 2 Compounds having a 3-aminopropyl group; 4-aminobutyldimethylmethoxysilane, 4-aminobutylmethyldimethoxysilane, 4-aminobutyltrimethoxysilane, 4-aminobutyldimethylethoxysilane, 4-aminobutylmethyldiethoxysilane, 4-aminobutyltriethoxysilane, etc. 2 Compounds having a 4-aminobutyl group; 3-(2-aminoethylamino)propyldimethylmethoxysilane, 3-(2-aminoethylamino)propylmethyldimethoxysilane, 3-(2-aminoethylamino)propyltrimethoxysilane, 3-(2-aminoethylamino)propyldimethylethoxysilane, 3-(2-aminoethylamino)propylmethyldiethoxysilane, 3-(2-aminoethylamino)propyltriethoxysilane, etc. 2 Examples of the aryl group include compounds having a 3-(2-aminoethylamino)propyl group.
[0101] In addition, A in the general formula (2) 2is a group other than a group containing a primary amino group having an active hydrogen atom and / or a secondary amino group having an active hydrogen atom, such as 3-dimethylaminopropyltrimethoxysilane, 3-dimethylaminopropylmethyldimethoxysilane, 3-dimethylaminopropyldimethylmethoxysilane, 3-dimethylaminopropyltriethoxysilane, 3-dimethylaminopropylmethyldiethoxysilane, and 3-dimethylaminopropyldimethylethoxysilane. 2 Compounds having a 3-dimethylaminopropyl group; 3-diethylaminopropyl trimethoxysilane, 3-diethylaminopropyl methyl dimethoxysilane, 3-diethylaminopropyl dimethyl methoxysilane, 3-diethylaminopropyl triethoxysilane, 3-diethylaminopropyl methyl diethoxysilane, 3-diethylaminopropyl dimethyl ethoxysilane, etc. 2 Compounds having a 3-diethylaminopropyl group; such as 3-dipropylaminopropyltrimethoxysilane, 3-dipropylaminopropylmethyldimethoxysilane, 3-dipropylaminopropyldimethylmethoxysilane, 3-dipropylaminopropyltriethoxysilane, 3-dipropylaminopropylmethyldiethoxysilane, and 3-dipropylaminopropyldimethylethoxysilane. 2 Compounds having a 3-dipropylaminopropyl group; such as 3-dibutylaminopropyltrimethoxysilane, 3-dibutylaminopropylmethyldimethoxysilane, 3-dibutylaminopropyldimethylmethoxysilane, 3-dibutylaminopropyltriethoxysilane, 3-dibutylaminopropylmethyldiethoxysilane, and 3-dibutylaminopropyldimethylethoxysilane. 2 Compounds having a 3-dibutylaminopropyl group; 3-phenylmethylaminopropyl trimethoxysilane, 3-phenylmethylaminopropyl methyl dimethoxysilane, 3-phenylmethylaminopropyl dimethyl methoxysilane, 3-phenylmethylaminopropyl triethoxysilane, 3-phenylmethylaminopropyl methyl diethoxysilane, 3-phenylmethylaminopropyl dimethyl ethoxysilane, etc. 2Compounds having a 3-phenylmethylaminopropyl group; 3-(4-methylpiperazinyl)propyltrimethoxysilane, 3-(4-methylpiperazinyl)propylmethyldimethoxysilane, 3-(4-methylpiperazinyl)propyldimethylmethoxysilane, 3-(4-methylpiperazinyl)propyltriethoxysilane, 3-(4-methylpiperazinyl)propylmethyldiethoxysilane, 3-(4-methylpiperazinyl)propyldimethylethoxysilane, etc. 2 as a compound having a 3-(4-methylpiperazinyl)propyl group;
[0102] A such as N,N-bis(trimethylsilyl)aminopropyltrimethoxysilane, N,N-bis(trimethylsilyl)aminopropyltriethoxysilane, N,N-bis(trimethylsilyl)aminopropylmethyldimethoxysilane, and N,N-bis(trimethylsilyl)aminopropylmethyldiethoxysilane 2 Compounds having an N,N-bis(trimethylsilyl)aminopropyl group; N,N-bis(triethylsilyl)aminopropyltrimethoxysilane, N,N-bis(trimethylsilyl)aminopropyltriethoxysilane, N,N-bis(triethylsilyl)aminopropylmethyldimethoxysilane, N,N-bis(triethylsilyl)aminopropylmethyldiethoxysilane, etc. 2 Compounds having an N,N-bis(triethylsilyl)aminopropyl group; N,N',N'-tris(trimethylsilyl)-N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N,N',N'-tris(trimethylsilyl)-N-(2-aminoethyl)-3-aminopropyltriethoxysilane, N,N',N'-tris(trimethylsilyl)-N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N,N',N'-tris(trimethylsilyl)-N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane, etc. 2 Examples of the compound include a compound having an N,N',N'-tris(trimethylsilyl)-N-(2-aminoethyl)-3-aminopropyl group.
[0103] The amount of the compound represented by formula (2) used is not particularly limited, but is preferably 0.1 to 5 mol, more preferably 0.2 to 2 mol, and even more preferably 0.4 to 1.5 mol, relative to 1 mol of the polymerization initiator used in step 1. By setting the amount of the compound represented by formula (2) used within the above range, the obtained cross-linked rubber product can have excellent low heat build-up and wet grip properties.
[0104] The timing of adding the compound represented by the general formula (2) to the solution containing the conjugated diene polymer chain is not particularly limited as long as it is after the polyorganosiloxane represented by the general formula (1) is added in the second step described above. For example, as in the second step described above, the compound represented by the general formula (2) can be added to the solution in a state where the polymerization reaction is not completed and the solution containing the conjugated diene polymer chain also contains a monomer, more specifically, in a state where the solution containing the conjugated diene polymer chain contains 100 ppm or more, more preferably 300 to 50,000 ppm of a monomer. By adding the compound represented by the general formula (2) in this manner, it is possible to suppress side reactions between the conjugated diene polymer chain and impurities contained in the polymerization system, and to control the reaction well. Alternatively, before or after adding the compound represented by the general formula (2) to a solution containing a conjugated diene polymer chain, water or an alcohol such as methanol is added to the solution, and the -O group as a reaction residue formed by the reaction with the polyorganosiloxane represented by the general formula (1) is formed. - M + The modification reaction may be carried out in a state where the group represented by is hydrolyzed and converted to a hydroxyl group. When the compound represented by the general formula (2) is added to a solution containing a conjugated diene polymer chain, the compound represented by the general formula (2) may be added after being dissolved in an inert solvent, or may be added directly without being dissolved in an inert solvent. The reaction temperature and reaction time are the same as those in the first step.
[0105] After reacting the compound represented by general formula (2), if necessary, a known polymerization terminator or the like is added to inactivate the reaction system, and then, if desired, an antiaging agent such as a phenol-based stabilizer, a phosphorus-based stabilizer, or a sulfur-based stabilizer, a crumbing agent, and a scale inhibitor are added to the reaction solution, and then the polymerization solvent is separated from the reaction solution by direct drying or steam stripping, etc., to recover the conjugated diene rubber. Note that, before separating the polymerization solvent from the reaction solution, an extender oil may be mixed with the polymerization solution, and the conjugated diene rubber may be recovered as an oil-extended rubber.
[0106] Examples of extender oils used when recovering conjugated diene rubber as oil-extended rubber include paraffinic, aromatic and naphthenic petroleum-based softeners, vegetable-based softeners, and fatty acids. When using a petroleum-based softener, it is preferable that the content of polycyclic aromatics extracted by the IP346 method (testing method of THE INSTITUTE PETROLEUM in the UK) is less than 3%. When using an extender oil, the amount used is preferably 5 to 100 parts by weight, more preferably 10 to 60 parts by weight, and even more preferably 20 to 50 parts by weight, based on 100 parts by weight of the conjugated diene rubber.
[0107] The conjugated diene rubber obtained by the manufacturing method of the present invention in this way is obtained by adding a polyorganosiloxane represented by general formula (1) as a modifier in a ratio of 1 mole or more in terms of the number of repeating units of the siloxane structure (-Si-O-) in the polyorganosiloxane to 1 mole of the polymerization initiator used in the first step, and then, in the above-mentioned third step, reacting using a compound represented by general formula (2) as a modifier. Therefore, the conjugated diene rubber obtained by the manufacturing method of the present invention includes those in which a modified structure by siloxane and a modified structure by the compound represented by general formula (2) are introduced at the polymer chain end, but in addition to these, it may also include those in which only a modified structure by siloxane is introduced at the polymer chain end. Furthermore, it may also include those in which only a modified structure by the compound represented by general formula (2) is introduced at the polymer chain end, or those in which no modified structure is introduced, for example, within a range that does not impair the effects of the present invention. In particular, in the present invention, from the viewpoint of appropriately achieving the effects of the present invention, i.e., excellent hot flow properties, low heat generation properties, and wet grip properties, the proportion of the modified structure by siloxane and the modified structure by the compound represented by general formula (2) introduced at the polymer chain end is preferably 10% by weight or more, more preferably 20% by weight or more. The upper limit is not particularly limited.
[0108] The coupling ratio of the conjugated diene rubber obtained by the manufacturing method of the present invention is not particularly limited, but is preferably 10% by weight or more, more preferably 20% by weight or more, particularly preferably 40% by weight or more, and is preferably 80% by weight or less, more preferably 75% by weight or less, particularly preferably 70% by weight or less. When the coupling ratio is within the above range, the obtained conjugated diene rubber has better hot flow properties. The coupling ratio is the weight fraction of the polymer molecule having a molecular weight of 1.8 times or more of the peak top molecular weight of the conjugated diene polymer chain having an active terminal before reacting with the polyorganosiloxane represented by general formula (1) and the compound represented by general formula (2), as well as the coupling agent and other modifiers used as necessary, relative to the total amount of the finally obtained conjugated diene rubber, and the molecular weight is measured as a polystyrene-equivalent molecular weight by gel permeation chromatography.
[0109] The weight average molecular weight (Mw) of the conjugated diene rubber obtained by the production method of the present invention is preferably 100,000 to 3,000,000, more preferably 150,000 to 2,000,000, and particularly preferably 200,000 to 1,500,000, as measured by gel permeation chromatography in terms of polystyrene. By making the weight average molecular weight of the conjugated diene rubber within the above range, it becomes easy to compound silica into the conjugated diene rubber, the processability of the rubber composition can be further improved, and further the low heat build-up and wet grip properties of the obtained cross-linked rubber can be further improved.
[0110] The molecular weight distribution of the conjugated diene rubber obtained by the production method of the present invention, represented by the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn), is preferably 1.1 to 3.0, more preferably 1.2 to 2.5, and particularly preferably 1.2 to 2.2. By setting the molecular weight distribution (Mw / Mn) of the conjugated diene rubber within the above range, the low heat build-up and wet grip properties of the obtained cross-linked rubber can be further improved.
[0111] The Mooney viscosity (ML 1+4 , 100° C.) is preferably 20 to 100, more preferably 30 to 90, and particularly preferably 35 to 80. When the conjugated diene rubber is used as the oil-extended rubber, it is preferable that the Mooney viscosity of the oil-extended rubber is within the above range.
[0112] The conjugated diene rubber thus obtained by the production method of the present invention can be suitably used for various applications after adding compounding agents such as a filler and a crosslinking agent. In particular, when silica is compounded as a filler, a rubber composition is obtained that can give a crosslinked rubber product having low heat buildup and excellent wet grip properties.
[0113] <Rubber composition> The rubber composition of the present invention is a composition containing 10 to 200 parts by weight of silica based on 100 parts by weight of a rubber component containing a conjugated diene rubber obtained by the above-mentioned production method of the present invention.
[0114] Examples of silica used in the present invention include dry white carbon, wet white carbon, colloidal silica, and precipitated silica. Among these, wet white carbon containing hydrated silicic acid as a main component is preferable. Carbon-silica dual phase filler in which silica is supported on the surface of carbon black may also be used. These silicas may be used alone or in combination of two or more. The nitrogen adsorption specific surface area of the silica used (measured by the BET method in accordance with ASTM D3037-81) is preferably 50 to 300 m. 2 / g, more preferably 80 to 220m 2 / g, particularly preferably 100 to 170m 2 The pH of the silica is preferably 5 to 10.
[0115] The amount of silica in the rubber composition of the present invention is 10 to 200 parts by weight, preferably 30 to 150 parts by weight, and more preferably 50 to 100 parts by weight, based on 100 parts by weight of the rubber component in the rubber composition. By setting the amount of silica in the above range, the processability of the rubber composition becomes excellent, and the wet grip property and low heat build-up property of the obtained cross-linked rubber can be further improved.
[0116] The rubber composition of the present invention may further contain a silane coupling agent from the viewpoint of further improving low heat generation. Examples of the silane coupling agent include vinyltriethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, 3-octanoylthio-1-propyl-triethoxysilane, bis(3-(triethoxysilyl)propyl)disulfide, bis(3-(triethoxysilyl)propyl)tetrasulfide, γ-trimethoxysilylpropyldimethylthiocarbamyltetrasulfide, and γ-trimethoxysilylpropylbenzothiazyltetrasulfide. These silane coupling agents may be used alone or in combination of two or more. The amount of the silane coupling agent is preferably 0.1 to 30 parts by weight, more preferably 1 to 15 parts by weight, based on 100 parts by weight of silica.
[0117] The rubber composition of the present invention may further contain carbon black such as furnace black, acetylene black, thermal black, channel black, and graphite. Among these, furnace black is preferred. These carbon blacks may be used alone or in combination of two or more. The amount of carbon black is usually 120 parts by weight or less per 100 parts by weight of the rubber component in the rubber composition.
[0118] The method for adding silica to the rubber component containing the conjugated diene rubber obtained by the production method of the present invention is not particularly limited, and may include a method of adding silica to a solid rubber component and kneading it (dry kneading method) or a method of adding silica to a solution containing the conjugated diene rubber and coagulating / drying it (wet kneading method).
[0119] In addition, the rubber composition of the present invention preferably further contains a crosslinking agent. Examples of crosslinking agents include sulfur, sulfur halides, organic peroxides, quinone dioximes, organic polyamine compounds, and alkylphenol resins having a methylol group. Among these, sulfur is preferably used. The amount of the crosslinking agent is preferably 0.1 to 15 parts by weight, more preferably 0.5 to 5 parts by weight, and particularly preferably 1 to 4 parts by weight, based on 100 parts by weight of the rubber component in the rubber composition.
[0120] Furthermore, in addition to the above-mentioned components, the rubber composition of the present invention may contain, in accordance with a conventional method, a required amount of each of compounding agents such as a crosslinking accelerator, a crosslinking activator, an antiaging agent, a filler (excluding the above-mentioned silica and carbon black), an activator, a process oil, a plasticizer, a lubricant, a tackifier, and a compatibilizer.
[0121] When sulfur or a sulfur-containing compound is used as the crosslinking agent, it is preferable to use a crosslinking accelerator and a crosslinking activator in combination. Examples of the crosslinking accelerator include sulfenamide crosslinking accelerators, guanidine crosslinking accelerators, thiourea crosslinking accelerators, thiazole crosslinking accelerators, thiuram crosslinking accelerators, dithiocarbamic acid crosslinking accelerators, and xanthogenic acid crosslinking accelerators. Among these, those containing sulfenamide crosslinking accelerators are preferable. These crosslinking accelerators are used alone or in combination of two or more. The amount of the crosslinking accelerator is preferably 0.1 to 15 parts by weight, more preferably 0.5 to 5 parts by weight, and particularly preferably 1 to 4 parts by weight, based on 100 parts by weight of the rubber component in the rubber composition.
[0122] Examples of the crosslinking activator include higher fatty acids such as stearic acid, zinc oxide, etc. These crosslinking activators may be used alone or in combination of two or more. The amount of the crosslinking activator is preferably 0.05 to 20 parts by weight, particularly preferably 0.5 to 15 parts by weight, based on 100 parts by weight of the rubber component in the rubber composition.
[0123] The rubber composition of the present invention may contain rubbers other than the conjugated diene rubber obtained by the above-mentioned manufacturing method of the present invention. Examples of the other rubbers include natural rubber, polyisoprene rubber, emulsion-polymerized styrene-butadiene copolymer rubber, solution-polymerized styrene-butadiene copolymer rubber, polybutadiene rubber (which may be high cis-BR or low cis-BR. Also, it may be polybutadiene rubber containing crystal fibers made of 1,2-polybutadiene polymer), styrene-isoprene copolymer rubber, butadiene-isoprene copolymer rubber, styrene-isoprene-butadiene copolymer rubber, acrylonitrile-butadiene copolymer rubber, and acrylonitrile-styrene-butadiene copolymer rubber, which are not conjugated diene rubbers obtained by the above-mentioned manufacturing method of the present invention. Among these, natural rubber, polyisoprene rubber, polybutadiene rubber, and solution-polymerized styrene-butadiene copolymer rubber are preferred. These rubbers may be used alone or in combination of two or more.
[0124] In the rubber composition of the present invention, the conjugated diene rubber obtained by the production method of the present invention preferably accounts for 10 to 100% by weight, and particularly preferably 50 to 100% by weight, of the rubber component in the rubber composition. By including the conjugated diene rubber of the present invention in the rubber component in such a ratio, a cross-linked rubber having improved low heat generation and wet grip properties can be obtained.
[0125] To obtain the rubber composition of the present invention, each component may be kneaded according to a conventional method. For example, the components other than the heat-unstable components such as the crosslinking agent and the crosslinking accelerator are kneaded with the conjugated diene rubber, and then the heat-unstable components such as the crosslinking agent and the crosslinking accelerator are mixed with the kneaded mixture to obtain the desired composition. The kneading temperature of the components other than the heat-unstable components and the conjugated diene rubber is preferably 80 to 200°C, more preferably 120 to 180°C, and the kneading time is preferably 30 seconds to 30 minutes. In addition, the kneaded mixture is usually mixed with the heat-unstable components after cooling to 100°C or less, preferably 80°C or less.
[0126] <Rubber cross-linked products> The cross-linked rubber product of the present invention is obtained by cross-linking the above-mentioned rubber composition of the present invention. The cross-linked rubber product of the present invention can be produced by using the rubber composition of the present invention, for example, molding the rubber composition into a desired shape using a molding machine such as an extruder, an injection molding machine, a compressor, or a roll, and then heating the composition to cause a cross-linking reaction and fix the shape as a cross-linked product. In this case, the cross-linking may be carried out after molding in advance or simultaneously with molding. The molding temperature is usually 10 to 200°C, preferably 25 to 120°C. The cross-linking temperature is usually 100 to 200°C, preferably 130 to 190°C, and the cross-linking time is usually 1 minute to 24 hours, preferably 2 minutes to 12 hours, and particularly preferably 3 minutes to 6 hours.
[0127] Depending on the shape, size, etc. of the cross-linked rubber product, even if the surface is cross-linked, the inside may not be sufficiently cross-linked, so secondary cross-linking may be performed by further heating.
[0128] The heating method may be appropriately selected from among methods commonly used for crosslinking rubber, such as press heating, steam heating, oven heating, and hot air heating.
[0129] The cross-linked rubber product of the present invention thus obtained is obtained using the conjugated diene rubber obtained by the above-mentioned production method of the present invention, and therefore has excellent low heat generation properties and wet grip properties. The cross-linked rubber product of the present invention can be used for various applications, such as materials for various tire parts such as cap tread, base tread, carcass, sidewall, and bead parts in tires, materials for hoses, belts, mats, anti-vibration rubber, and various other industrial products, impact resistance improvers for resins, resin film buffers, shoe soles, rubber shoes, golf balls, and toys, by making use of such properties. In particular, the cross-linked rubber product of the present invention can be suitably used for various tire parts such as tread, carcass, sidewall, and bead parts in various tires such as all-season tires, high-performance tires, and studless tires, and is particularly suitable for use in the tread of low fuel consumption tires, since it has excellent low heat generation properties. EXAMPLES
[0130] The present invention will be described below in more detail with reference to examples, but the present invention is not limited to these examples. In the following, "parts" are by weight unless otherwise specified. Tests and evaluations were performed according to the following.
[0131] [Weight average molecular weight, molecular weight distribution, coupling ratio] The weight average molecular weight (Mw), molecular weight distribution (Mw / Mn), and coupling ratio were determined based on a chart obtained by gel permeation chromatography (GPC) based on the molecular weight converted into polystyrene. The specific measurement conditions for gel permeation chromatography were as follows: Measuring instrument: High-performance liquid chromatograph (Tosoh Corporation, product name "HLC-8220") Column: Two polystyrene columns manufactured by Tosoh Corporation, trade name "GMH-HR-H", were connected in series. Detector: Differential refractometer Eluent: Tetrahydrofuran Column temperature: 40℃ The coupling rate of the conjugated diene polymer chain was determined as the area ratio of a peak portion having a peak top molecular weight 1.8 times or more the peak top molecular weight of the smallest peak relative to the total elution area in the elution curve obtained by gel permeation chromatography under the above conditions.
[0132] [Aromatic vinyl monomer unit content, vinyl bond content] The aromatic vinyl monomer unit content and the vinyl bond content are 1 Measurements were performed by H-NMR.
[0133] [Hot flow properties (adhesion of solidified crumbs)] The hot flow property was evaluated by measuring the shear modulus G' at 108 ° C. under conditions of dynamic strain of 10% and 0.1 Hz using a rubber process analyzer RPA-2000 (manufactured by Alpha Technologies) for about 7 g of conjugated diene rubber bales. The values of the shear modulus G' in Examples 1 to 8 and Comparative Examples 1 to 7 are shown as indexes with the measured value of Comparative Example 3 set to 100. The values of the shear modulus G' in Example 9 and Comparative Example 8 are shown as indexes with the measured value of Comparative Example 8 set to 100. The values of the shear modulus G' in Example 10 and Comparative Example 9 are shown as indexes with the measured value of Comparative Example 9 set to 100. The values of the shear modulus G' in Example 11 and Comparative Example 10 are shown as indexes with the measured value of Comparative Example 10 set to 100. The larger this index, the less likely the solidified crumbs are to adhere to each other, meaning that the operability during solidification is stable.
[0134] [Low heat build-up of cross-linked rubber] The low heat build-up properties of the cross-linked rubber were evaluated by measuring tan δ at 60°C using a test piece having a length of 50 mm, a width of 12.7 mm, and a thickness of 2 mm, under conditions of a dynamic strain of 2.5% and 10 Hz, using an ARES manufactured by Rheometrics. The values of tan δ in Examples 1 to 8 and Comparative Examples 1 to 7 are shown as indexes with the measured value of Comparative Example 3 set to 100. The values of tan δ in Example 9 and Comparative Example 8 are shown as indexes with the measured value of Comparative Example 8 set to 100. The values of tan δ in Example 10 and Comparative Example 9 are shown as indexes with the measured value of Comparative Example 9 set to 100. The values of tan δ in Example 11 and Comparative Example 10 are shown as indexes with the measured value of Comparative Example 10 set to 100. The smaller this index, the better the low heat build-up properties.
[0135] [Wet Grip Property of Cross-Linked Rubber] The wet grip properties of the cross-linked rubber were evaluated by measuring the tan δ value at 0°C using a test piece having a length of 50 mm, a width of 12.7 mm, and a thickness of 2 mm, using an ARES manufactured by Rheometrics, Inc., under conditions of a dynamic strain of 0.5% and 10 Hz. The tan δ values of Examples 1 to 8 and Comparative Examples 1 to 7 are shown as indexes with the measured value of Comparative Example 3 set to 100. The tan δ values of Example 9 and Comparative Example 8 are shown as indexes with the measured value of Comparative Example 8 set to 100. The tan δ values of Example 10 and Comparative Example 9 are shown as indexes with the measured value of Comparative Example 9 set to 100. The tan δ values of Example 11 and Comparative Example 10 are shown as indexes with the measured value of Comparative Example 10 set to 100. The larger this index, the better the wet grip properties.
[0136] Example 1 In an autoclave equipped with a stirrer, 800g of cyclohexane, 1.42mmol of tetramethylethylenediamine, 87.6g of 1,3-butadiene, and 32.4g of styrene were charged under a nitrogen atmosphere, and then 0.79mmol of n-butyllithium was added to initiate polymerization at 60°C. The polymerization reaction was continued for 60 minutes, and after it was confirmed that the polymerization conversion rate was in the range of 95% to 100%, 0.31g (equivalent to 1.3 times the molar amount of n-butyllithium used, calculated as the number of repeating units of the siloxane structure (-Si-O-) in the polyorganosiloxane) of 40% by weight concentration in xylene solution was added to the mixture, and the mixture was allowed to react for 30 minutes. Next, 0.79mmol of 3-aminopropyltrimethoxysilane (equivalent to 1.0 times the molar amount of n-butyllithium used) was added, and the mixture was stirred for 10 minutes. Thereafter, methanol was added as a polymerization terminator in an amount equivalent to twice the molar amount of n-butyl lithium used to obtain a solution containing a conjugated diene rubber. To this solution, 0.15 parts of Irganox 1520L (manufactured by Ciba Specialty Chemicals) was added as an anti-aging agent relative to 100 parts of the conjugated diene rubber, and the solvent was removed by steam stripping, and the mixture was vacuum dried at 60°C for 24 hours to obtain a solid conjugated diene rubber. The weight average molecular weight (Mw) of the obtained conjugated diene rubber of Example 1 was 482,000, the coupling ratio was 57.9%, the styrene monomer unit content was 27.3% by weight, and the vinyl bond content was 60.0% by weight. In addition, the hot flow property of the obtained conjugated diene rubber of Example 1 was measured according to the above method. The results are shown in Table 1. [ka]
[0137] Example 2 A solid conjugated diene rubber was obtained in the same manner as in Example 1, except that the amount of polyorganosiloxane represented by the above formula (8) was changed to 0.26 g (equivalent to 1.1 times the molar amount of n-butyllithium used, calculated as the number of repeating units of the siloxane structure (-Si-O-) in the polyorganosiloxane). The weight average molecular weight (Mw) of the obtained conjugated diene rubber of Example 2 was 469,000, the coupling ratio was 55.0%, the styrene monomer unit content was 27.2% by weight, and the vinyl bond content was 59.3% by weight. In addition, the hot flow property of the obtained conjugated diene rubber of Example 2 was measured according to the above method. The results are shown in Table 1.
[0138] Example 3 A solid conjugated diene rubber was obtained by the same operation as in Example 2, except that 0.79 mmol of 3-(2-aminoethylamino)propyltrimethoxysilane (amount equivalent to 1.0 times the molar amount of n-butyllithium used) was used instead of 0.79 mmol of 3-aminopropyltrimethoxysilane. The weight average molecular weight (Mw) of the obtained conjugated diene rubber of Example 3 was 467,000, the coupling ratio was 54.4%, the styrene monomer unit content was 26.9% by weight, and the vinyl bond content was 58.5% by weight. In addition, the hot flow property of the obtained conjugated diene rubber of Example 3 was measured according to the above method. The results are shown in Table 1.
[0139] Example 4 Into a nitrogen-purged 100-ml ampoule, 50.0 g of cyclohexane and 0.66 mmol of tetramethylethylenediamine were added, and further, 6.6 mmol of n-butyllithium was added. Next, 11.61 g of isoprene and 0.87 g of styrene were slowly added, and the mixture was reacted for 120 minutes in the ampoule at 50°C to obtain a polymer block (A) having an active terminal. The weight-average molecular weight (Mw) of this polymer block (A) was 3,500, the molecular weight distribution (Mw / Mn) was 1.10, the styrene monomer unit content was 7.0% by weight, the isoprene monomer unit content was 93.0% by weight, and the vinyl bond content was 7.7% by weight.
[0140] Next, 4000g of cyclohexane, 11.1mmol of tetramethylethylenediamine, 393.0g of 1,3-butadiene, and 207.0g of styrene were charged into an autoclave equipped with a stirrer under a nitrogen atmosphere, and then the entire amount of the polymer block (A) having active terminals obtained above was added and polymerization was initiated at 40°C. After 10 minutes had elapsed since the start of polymerization, 337.0g of 1,3-butadiene and 63.0g of styrene were continuously added over 40 minutes. The maximum temperature during the polymerization reaction was 60°C. After the continuous addition was completed, the polymerization reaction was continued for another 20 minutes, and after confirming that the polymerization conversion rate was in the range of 95% to 100%, 2.13 g (equivalent to 1.1 times the molar amount of n-butyl lithium used, calculated as the number of repeating units of the siloxane structure (-Si-O-) in the polyorganosiloxane) of 40% by weight concentration in xylene solution was added and reacted for 30 minutes. Next, 6.6 mmol of 3-aminopropyltrimethoxysilane (equivalent to 1.0 times the molar amount of n-butyl lithium used) was added and stirred for 10 minutes. Then, methanol was added as a polymerization terminator in an amount equivalent to 2 times the molar amount of n-butyl lithium used to obtain a solution containing a conjugated diene rubber. To this solution, 0.15 parts of Irganox 1520L (manufactured by Ciba Specialty Chemicals) was added as an anti-aging agent relative to 100 parts of conjugated diene rubber, and the solvent was removed by steam stripping. The mixture was vacuum dried at 60°C for 24 hours to obtain a solid conjugated diene rubber. The weight average molecular weight (Mw) of the obtained conjugated diene rubber of Example 4 was 494,000, the coupling ratio was 60.8%, the styrene monomer unit content was 26.5% by weight, and the vinyl bond content was 59.0% by weight. The hot flow property of the obtained conjugated diene rubber of Example 4 was measured according to the above method. The results are shown in Table 1.
[0141] Example 5 A solid conjugated diene rubber was obtained by the same operation as in Example 4, except that 6.6 mmol of 3-(2-aminoethylamino)propyltrimethoxysilane (amount equivalent to 1.0 times the molar amount of n-butyllithium used) was used instead of 6.6 mmol of 3-aminopropyltrimethoxysilane. The weight average molecular weight (Mw) of the obtained conjugated diene rubber of Example 5 was 488,000, the coupling ratio was 60.2%, the styrene monomer unit content was 26.6% by weight, and the vinyl bond content was 60.4% by weight. In addition, the hot flow property of the obtained conjugated diene rubber of Example 5 was measured according to the above method. The results are shown in Table 1.
[0142] Example 6 In an autoclave equipped with a stirrer, 800g of cyclohexane, 1.42mmol of tetramethylethylenediamine, 0.71mmol of di-N-hexylamine, 87.6g of 1,3-butadiene, and 32.4g of styrene were charged under a nitrogen atmosphere, and then 0.79mmol of n-butyllithium was added to initiate polymerization at 60°C. The polymerization reaction was continued for 60 minutes, and after it was confirmed that the polymerization conversion rate was in the range of 95% to 100%, 0.26g of polyorganosiloxane represented by the above formula (8) was added in a xylene solution having a concentration of 40% by weight (equivalent to 1.1 times the molar amount of n-butyllithium used, calculated as the number of repeating units of the siloxane structure (-Si-O-) in the polyorganosiloxane), and the reaction was allowed to proceed for 30 minutes. Next, 0.79 mmol of 3-aminopropyltrimethoxysilane (an amount equivalent to 1.0 times the molar amount of n-butyllithium (di-N-hexylaminolithium) used) was added, and the mixture was stirred for 10 minutes. Thereafter, as a polymerization terminator, methanol in an amount equivalent to 2 times the molar amount of n-butyllithium used was added to obtain a solution containing a conjugated diene rubber. To this solution, 0.15 parts of Irganox 1520L (manufactured by Ciba Specialty Chemicals) were added as an antiaging agent relative to 100 parts of the conjugated diene rubber, and the solvent was removed by steam stripping, and the mixture was vacuum dried at 60°C for 24 hours to obtain a solid conjugated diene rubber. The weight average molecular weight (Mw) of the obtained conjugated diene rubber of Example 6 was 484,000, the coupling ratio was 58.8%, the styrene monomer unit content was 27.1% by weight, and the vinyl bond content was 59.1% by weight. The hot flow property of the obtained conjugated diene rubber of Example 6 was measured according to the above-mentioned method. The results are shown in Table 1.
[0143] Example 7 A solid conjugated diene rubber was obtained in the same manner as in Example 2, except that 0.79 mmol of N,N-bis(triethylsilyl)aminopropyltrimethoxysilane (amount equivalent to 1.0 times the molar amount of n-butyllithium used) was used instead of 0.79 mmol of 3-aminopropyltrimethoxysilane. The weight average molecular weight (Mw) of the obtained conjugated diene rubber of Example 7 was 464,000, the coupling ratio was 53.8%, the styrene monomer unit content was 27.0% by weight, and the vinyl bond content was 59.5% by weight. In addition, the hot flow property of the obtained conjugated diene rubber of Example 7 was measured according to the above method. The results are shown in Table 1.
[0144] Example 8 A solid conjugated diene rubber was obtained by the same operation as in Example 2, except that 0.79 mmol of 3-diethylaminopropyltrimethoxysilane (amount equivalent to 1.0 times the molar amount of n-butyllithium used) was used instead of 0.79 mmol of 3-aminopropyltrimethoxysilane. The weight average molecular weight (Mw) of the obtained conjugated diene rubber of Example 8 was 465,000, the coupling ratio was 54.0%, the styrene monomer unit content was 27.5% by weight, and the vinyl bond content was 59.8% by weight. In addition, the hot flow property of the obtained conjugated diene rubber of Example 8 was measured according to the above method. The results are shown in Table 1.
[0145] Comparative Example 1 A solid conjugated diene rubber was obtained in the same manner as in Example 1, except that the amount of polyorganosiloxane represented by the above formula (8) was changed to 0.16 g (equivalent to 0.7 times the molar amount of n-butyllithium used, calculated as the number of repeating units of the siloxane structure (-Si-O-) in the polyorganosiloxane). The weight average molecular weight (Mw) of the obtained conjugated diene rubber of Comparative Example 1 was 383,000, the coupling ratio was 34.4%, the styrene monomer unit content was 26.6% by weight, and the vinyl bond content was 58.5% by weight. In addition, the hot flow property of the obtained conjugated diene rubber of Comparative Example 1 was measured according to the above method. The results are shown in Table 1.
[0146] Comparative Example 2 A solid conjugated diene rubber was obtained in the same manner as in Example 1, except that the amount of polyorganosiloxane represented by the above formula (8) was changed to 0.09 g (equivalent to 0.4 times the molar amount of n-butyllithium used, calculated as the number of repeating units of the siloxane structure (-Si-O-) in the polyorganosiloxane). The weight average molecular weight (Mw) of the obtained conjugated diene rubber of Comparative Example 2 was 286,000, the coupling ratio was 11.4%, the styrene monomer unit content was 26.9% by weight, and the vinyl bond content was 57.2% by weight. The hot flow property of the obtained conjugated diene rubber of Comparative Example 2 was measured according to the above method. The results are shown in Table 1.
[0147] Comparative Example 3 A solid conjugated diene rubber was obtained in the same manner as in Example 2, except that 3-aminopropyltrimethoxysilane was not added. The weight average molecular weight (Mw) of the obtained conjugated diene rubber of Comparative Example 3 was 460,000, the coupling ratio was 52.5%, the styrene monomer unit content was 27.6% by weight, and the vinyl bond content was 58.8% by weight. In addition, the hot flow property of the obtained conjugated diene rubber of Comparative Example 3 was measured according to the above-mentioned method. The results are shown in Table 1.
[0148] Comparative Example 4 A solid conjugated diene rubber was obtained in the same manner as in Example 2, except that 0.87 mmol of hexamethylcyclotrisiloxane (equivalent to 1.1 times the molar amount of n-butyllithium used) was used instead of the polyorganosiloxane represented by the above formula (8). The weight average molecular weight (Mw) of the obtained conjugated diene rubber of Comparative Example 4 was 323,000, the coupling ratio was 20.5%, the styrene monomer unit content was 27.0% by weight, and the vinyl bond content was 59.8% by weight. In addition, the hot flow property of the obtained conjugated diene rubber of Comparative Example 4 was measured according to the above method. The results are shown in Table 1.
[0149] Comparative Example 5 A solid conjugated diene rubber was obtained in the same manner as in Comparative Example 4, except that 3-aminopropyltrimethoxysilane was not added. The weight average molecular weight (Mw) of the obtained conjugated diene rubber of Comparative Example 5 was 265,000, the coupling ratio was 8.4%, the styrene monomer unit content was 27.3% by weight, and the vinyl bond content was 58.7% by weight. In addition, the hot flow property of the obtained conjugated diene rubber of Comparative Example 5 was measured according to the above-mentioned method. The results are shown in Table 1.
[0150] Comparative Example 6 A solid conjugated diene rubber was obtained in the same manner as in Example 2, except that 0.87 mmol of N,N-bis(triethylsilyl)aminopropyltrimethoxysilane (amount equivalent to 1.1 times the molar amount of n-butyllithium used) was used instead of the polyorganosiloxane represented by the above formula (8). The weight average molecular weight (Mw) of the obtained conjugated diene rubber of Comparative Example 6 was 383,000, the coupling ratio was 36.5%, the styrene monomer unit content was 26.7% by weight, and the vinyl bond content was 58.0% by weight. In addition, the hot flow property of the obtained conjugated diene rubber of Comparative Example 6 was measured according to the above method. The results are shown in Table 1.
[0151] Comparative Example 7 A solid conjugated diene rubber was obtained in the same manner as in Comparative Example 6, except that 3-aminopropyltrimethoxysilane was not added. The weight average molecular weight (Mw) of the obtained conjugated diene rubber of Comparative Example 7 was 377,000, the coupling ratio was 34.5%, the styrene monomer unit content was 27.5% by weight, and the vinyl bond content was 60.3% by weight. In addition, the hot flow property of the obtained conjugated diene rubber of Comparative Example 7 was measured according to the above-mentioned method. The results are shown in Table 1.
[0152] [Production and Evaluation of Rubber Composition and Cross-Linked Rubber Product] In a 250 ml Brabender type mixer, 100 parts of the conjugated diene rubber of Example 1 was masticated for 30 seconds, and then 50 parts of silica (manufactured by Rhodia, trade name "Zeosil1115MP"), 20 parts of process oil (manufactured by JX Nippon Oil & Energy Corporation, trade name "Aromax T-DAE"), and 6.0 parts of a silane coupling agent: bis(3-(triethoxysilyl)propyl)tetrasulfide (manufactured by Degussa, trade name "Si69") were added, and the mixture was kneaded for 1.5 minutes at a starting temperature of 110°C, after which 25 parts of silica (manufactured by Rhodia, trade name "Zeosil1115MP"), 3 parts of zinc oxide, 2 parts of stearic acid, and 2 parts of an antioxidant: N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (manufactured by Ouchi Shinko, trade name "Nocrac 6C") were added, and the mixture was kneaded for a further 2.5 minutes, and the kneaded product was discharged from the mixer. The temperature of the kneaded product at the end of kneading was 150°C. After cooling the kneaded product to room temperature, it was kneaded again in a Brabender type mixer with a starting temperature of 110°C for 2 minutes, and then the kneaded product was discharged from the mixer. Next, a mixture of 1.4 parts of sulfur, 1.2 parts of a crosslinking accelerator: N-tert-butyl-2-benzothiazolylsulfenamide (trade name "Noccela NS-P", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), and 1.2 parts of 1,3-diphenylguanidine (trade name "Noccela D", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) was added to the kneaded product obtained with an open roll at 50°C, and the mixture was kneaded, and then a sheet-shaped rubber composition was taken out. This rubber composition was press-crosslinked at 160°C for 20 minutes to prepare a test piece of the crosslinked rubber product, and the wet grip property and low heat generation property of this test piece were evaluated. Similarly, for the conjugated diene rubbers of Examples 2 to 8 and Comparative Examples 1 to 7, test pieces of the rubber compositions and cross-linked rubbers were prepared, and the low heat build-up and wet grip properties of these test pieces were evaluated according to the above-mentioned methods. The results are shown in Table 1.
[0153] [Table 1] In Table 1, the amount of each component added is shown as the amount when the amount of the polymerization initiator added is taken as 1 part by mole.
[0154] As can be seen from Table 1, the conjugated diene rubbers (Examples 1 to 8) obtained by the method for producing a conjugated diene rubber of the present invention were modified with polyorganosiloxane represented by general formula (1) while being excellent in hot flow properties (difficulty of solidified crumbs adhering to each other) compared with the conjugated diene rubber (Comparative Example 3) which was not further modified with a compound represented by general formula (2), and the obtained cross-linked rubber products were excellent in wet grip properties and low heat build-up properties. In particular, when a modifier containing a primary amino group having an active hydrogen atom and / or a secondary amino group having an active hydrogen atom was used as the second stage modifier, the effect was remarkable. On the other hand, all of the conjugated diene rubbers in which the amount of polyorganosiloxane represented by the general formula (1) was less than 1 mole were inferior in hot flow properties (difficulty of solidified crumbs adhering to each other), and the obtained cross-linked rubber products were inferior in wet grip properties and low heat generation properties (Comparative Examples 1 and 2). In addition, all of the conjugated diene rubbers using modifiers other than the polyorganosiloxane represented by the general formula (1) were poor in hot flow properties (difficulty in adhesion of solidified crumbs to each other) (Comparative Examples 4 to 7).
[0155] Example 9 Into a nitrogen-substituted 800-ml ampoule, 70.0 g of cyclohexane and 0.77 mmol of tetramethylethylenediamine were added, followed by 7.69 mmol of n-butyllithium (an amount such that the amount of tetramethylethylenediamine as a polar compound per mole of n-butyllithium was 0.10 moles). Then, 27.9 g of isoprene and 2.1 g of styrene were slowly added, and the mixture was reacted for 120 minutes in the ampoule at a temperature of 50° C. to obtain a polymer block (A) having an active terminal. The weight-average molecular weight (Mw) of this polymer block (A) was 6,500, the molecular weight distribution (Mw / Mn) was 1.10, the styrene monomer unit content was 7.0% by weight, the isoprene monomer unit content was 93.0% by weight, and the vinyl bond content was 7.7% by weight.
[0156] In a stirrer-equipped autoclave, 4000g of cyclohexane, 2.69mmol of tetramethylethylenediamine, 474g of 1,3-butadiene, and 126g of styrene were charged under a nitrogen atmosphere, and the entire amount of the polymer block (A) having active terminals obtained above was added, and polymerization was initiated at 50°C (the amount of tetramethylethylenediamine as a polar compound present in the reaction system per mole of n-butyllithium used was 0.45 moles). 10 minutes after the start of polymerization, 376g of 1,3-butadiene and 24g of styrene were continuously added over 60 minutes. The maximum temperature during the polymerization reaction was 75°C. After the continuous addition was completed, the polymerization reaction was continued for another 10 minutes, and after confirming that the polymerization conversion rate was in the range of 95% to 100%, 2.44 g (equivalent to 1.1 times the molar amount of n-butyl lithium used, calculated as the number of repeating units of the siloxane structure (-Si-O-) in the polyorganosiloxane) of the polyorganosiloxane represented by the above formula (8) was added in a state of a 40% by weight concentration xylene solution, and reacted for 30 minutes. Next, 7.69 mmol of 3-(2-aminoethylamino)propyltrimethoxysilane (equivalent to 1.0 times the molar amount of n-butyl lithium used) was added, and reacted for 10 minutes. After that, methanol was added in an amount equivalent to 2 times the molar amount of n-butyl lithium used as a polymerization terminator to obtain a solution containing a conjugated diene rubber. To this solution, 0.15 parts of Irganox 1520L (manufactured by BASF) was added as an anti-aging agent relative to 100 parts of conjugated diene rubber, and the solvent was removed by steam stripping, and the mixture was vacuum dried at 60°C for 24 hours to obtain a solid conjugated diene rubber. The weight average molecular weight (Mw) of the obtained conjugated diene rubber of Example 9 was 460,000, the coupling ratio was 58.0%, the styrene monomer unit content was 15.0% by weight, and the vinyl bond content was 30.5% by weight. In addition, the hot flow property of the obtained conjugated diene rubber of Example 9 was measured according to the above method. The results are shown in Table 2.
[0157] Comparative Example 8 A solid conjugated diene rubber was obtained in the same manner as in Example 9, except that 7.69 mmol of 3-(2-aminoethylamino)propyltrimethoxysilane was not added. The weight average molecular weight (Mw) of the obtained conjugated diene rubber of Comparative Example 8 was 450,000, the coupling ratio was 56.8%, the styrene monomer unit content was 15.0% by weight, and the vinyl bond content was 30.0% by weight. In addition, the hot flow property of the obtained conjugated diene rubber of Comparative Example 8 was measured according to the above-mentioned method. The results are shown in Table 2.
[0158] [Production and Evaluation of Rubber Composition and Cross-Linked Rubber Product] In a 250 ml Brabender type mixer, 70 parts of the conjugated diene rubber obtained in Example 9 and 30 parts of butadiene rubber (manufactured by Nippon Zeon Co., Ltd., product name "Nipol BR1220") were masticated for 30 seconds, and then 66.7 parts of silica (manufactured by Evonik Co., Ltd., product name "Ultrasil 7000GR"), 11.3 parts of process oil (manufactured by JX Nippon Oil & Energy Corporation, product name "Aromax T-DAE"), and 7.2 parts of a silane coupling agent: bis(3-(triethoxysilyl)propyl)tetrasulfide (manufactured by Evonik Co., Ltd., product name "Si69") were added, and the mixture was kneaded for 1.5 minutes at a starting temperature of 110°C, followed by addition of 23.3 parts of silica (manufactured by Evonik Co., Ltd., product name "Ultrasil 7000GR") and carbon black (manufactured by Tokai Carbon Co., Ltd., product name "Seastone The mixture was mixed with 10 parts of process oil (manufactured by JX Nippon Oil & Energy Corporation, trade name "Aromax T-DAE"), 3 parts of zinc oxide, 2 parts of stearic acid, and 2 parts of antioxidant: N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (manufactured by Ouchi Shinko Chemical Industry Co., Ltd., trade name "Nocrac 6C"), and further kneaded for 2.5 minutes, and the kneaded product was discharged from the mixer. The temperature of the kneaded product at the end of kneading was 150°C. After cooling to room temperature, the kneaded product was kneaded again for 2 minutes in a Brabender type mixer with a starting temperature of 110°C, and the kneaded product was discharged from the mixer. Next, a mixture of 1.7 parts of sulfur, 1.8 parts of a crosslinking accelerator: N-tert-butyl-2-benzothiazolylsulfenamide (manufactured by Ouchi Shinko Chemical Industry Co., Ltd., trade name "Noccela NS-P"), and 1.7 parts of a crosslinking accelerator: 1,3-diphenylguanidine (manufactured by Ouchi Shinko Chemical Industry Co., Ltd., trade name "Noccela D") was added to the obtained kneaded product with an open roll at 50 ° C., and then the mixture was kneaded, and a sheet-shaped rubber composition was taken out. This rubber composition was press-crosslinked at 160 ° C. for 20 minutes to prepare a test piece of a rubber crosslinked product, and the low heat generation property and wet grip property of this test piece were evaluated. The results are shown in Table 2. Similarly, for the conjugated diene rubber of Comparative Example 8, test pieces of the rubber composition and the cross-linked rubber were prepared, and the low heat build-up property and wet grip property of these test pieces were evaluated according to the above-mentioned methods. The results are shown in Table 2.
[0159] [Table 2] In Table 2, the amount of each component added is shown as the amount when the amount of the polymerization initiator added is taken as 1 part by mole.
[0160] Example 10 Into a nitrogen-substituted 800-ml ampoule, 74.3 g of cyclohexane and 0.48 mmol of tetramethylethylenediamine were added, followed by 4.76 mmol of n-butyllithium (an amount such that the amount of tetramethylethylenediamine as a polar compound per mole of n-butyllithium was 0.10 moles). Next, 17.3 g of isoprene and 1.3 g of styrene were slowly added, and the mixture was allowed to react for 120 minutes in the ampoule at 50°C to obtain a polymer block (A) having an active terminal. The weight-average molecular weight (Mw) of this polymer block (A) was 6,500, the molecular weight distribution (Mw / Mn) was 1.12, the styrene monomer unit content was 7.0%, the isoprene monomer unit content was 93.0% by weight, and the vinyl bond content was 7.5% by weight.
[0161] In a stirrer-equipped autoclave, 4000g of cyclohexane, 3.57mmol of tetramethylethylenediamine, 252g of 1,3-butadiene, and 348g of styrene were charged under a nitrogen atmosphere, and the entire amount of the polymer block (A) having active terminals obtained above was added, and polymerization was initiated at 50°C (the amount of tetramethylethylenediamine as a polar compound present in the reaction system per mole of n-butyllithium used was 0.85 moles). 15 minutes after the start of polymerization, 338g of 1,3-butadiene and 62g of styrene were continuously added over 60 minutes. The maximum temperature during the polymerization reaction was 70°C. After the continuous addition was completed, the polymerization reaction was continued for another 15 minutes, and after confirming that the polymerization conversion rate was in the range of 95% to 100%, 1.51 g (equivalent to 1.1 times the molar amount of n-butyl lithium used, calculated as the number of repeating units of the siloxane structure (-Si-O-) in the polyorganosiloxane) of 40% by weight concentration in xylene solution was added and reacted for 30 minutes. Next, 4.76 mmol of 3-(2-aminoethylamino)propyltrimethoxysilane (equivalent to 1.0 times the molar amount of n-butyl lithium used) was added and reacted for 10 minutes. Then, methanol was added as a polymerization terminator in an amount equivalent to 2 times the molar amount of n-butyl lithium used to obtain a solution containing a conjugated diene rubber. To this solution, 0.15 parts of Irganox 1520L (manufactured by BASF) was added as an anti-aging agent relative to 100 parts of conjugated diene rubber, and the solvent was removed by steam stripping, and the mixture was vacuum dried at 60°C for 24 hours to obtain a solid conjugated diene rubber. The weight average molecular weight (Mw) of the obtained conjugated diene rubber of Example 10 was 570,000, the coupling ratio was 45.0%, the styrene monomer unit content was 41.1% by weight, and the vinyl bond content was 33.5% by weight. In addition, the hot flow property of the obtained conjugated diene rubber of Example 10 was measured according to the above method. The results are shown in Table 3.
[0162] Comparative Example 9 A solid conjugated diene rubber was obtained in the same manner as in Example 10, except that 4.76 mmol of 3-(2-aminoethylamino)propyltrimethoxysilane was not added. The weight average molecular weight (Mw) of the obtained conjugated diene rubber of Comparative Example 9 was 552,000, the coupling ratio was 43.0%, the styrene monomer unit content was 41.0% by weight, and the vinyl bond content was 33.0% by weight. In addition, the hot flow property of the obtained conjugated diene rubber of Comparative Example 9 was measured according to the above-mentioned method. The results are shown in Table 3.
[0163] [Production and Evaluation of Rubber Composition and Cross-Linked Rubber Product] In a 250 ml Brabender type mixer, 70 parts of the conjugated diene rubber obtained in Example 10 and 30 parts of butadiene rubber (manufactured by Zeon Corporation, trade name "Nipol BR1220") were masticated for 30 seconds, and then 50.0 parts of silica (manufactured by Rhodia Corporation, trade name "Zeosil 1165MP"), 27.5 parts of process oil (manufactured by JX Nippon Oil & Energy Corporation, trade name "Aromax T-DAE"), and 6.0 parts of a silane coupling agent: bis(3-(triethoxysilyl)propyl)tetrasulfide (manufactured by Evonik Corporation, trade name "Si69") were added, and the mixture was kneaded for 1.5 minutes at a starting temperature of 110°C, and silica (manufactured by Rhodia Corporation, trade name "Zeosil 25.0 parts of "Nocrac 6C" (product name: N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine) (manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), 3 parts of zinc oxide, 2 parts of stearic acid, and 2 parts of an antioxidant, N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (manufactured by Ouchi Shinko Chemical Industry Co., Ltd., product name: "Nocrac 6C"), were added, and kneaded for a further 2.5 minutes, and the kneaded product was discharged from the mixer. The temperature of the kneaded product at the end of kneading was 150°C. After cooling to room temperature, the kneaded product was kneaded again for 2 minutes in the Brabender type mixer with an initial temperature of 110°C, and the kneaded product was discharged from the mixer. Next, a mixture of 1.5 parts of sulfur, 1.8 parts of a crosslinking accelerator: N-tert-butyl-2-benzothiazolylsulfenamide (manufactured by Ouchi Shinko Chemical Industry Co., Ltd., product name "Noccela NS-P"), and 1.5 parts of a crosslinking accelerator: 1,3-diphenylguanidine (manufactured by Ouchi Shinko Chemical Industry Co., Ltd., product name "Noccela D") was added to the obtained kneaded product with an open roll at 50 ° C., and then the mixture was kneaded, and a sheet-shaped rubber composition was taken out. This rubber composition was press-crosslinked at 160 ° C. for 20 minutes to prepare a test piece of a crosslinked rubber product, and the wet grip property and low heat generation property of this test piece were evaluated. The results are shown in Table 3. Similarly, for the conjugated diene rubber of Comparative Example 9, test pieces of the rubber composition and the cross-linked rubber were prepared, and the low heat build-up property and wet grip property of these test pieces were evaluated according to the above-mentioned methods. The results are shown in Table 3.
[0164] [Table 3] In Table 3, the amount of each component added is shown as the amount when the amount of the polymerization initiator added is taken as 1 part by mole.
[0165] Example 11 In a stirrer-equipped autoclave, 800 g of cyclohexane and 120 g of 1,3-butadiene were charged under a nitrogen atmosphere, and then 1.00 mmol of n-butyllithium was added to initiate polymerization at 80° C. The polymerization reaction was continued for 90 minutes, and after it was confirmed that the polymerization conversion rate was in the range of 95% to 100%, the polyorganosiloxane represented by the above formula (8) was added. In the state of a 40% by weight concentration xylene solution, 0.32 g (equivalent to 1.1 times the molar amount of n-butyllithium used, calculated as the number of repeating units of the siloxane structure (-Si-O-) in the polyorganosiloxane) ) attachment Then, 1.00 mmol of 3-(2-aminoethylamino)propyltrimethoxysilane (amount equivalent to 1.0 times the molar amount of n-butyllithium used) was added, and the mixture was allowed to react for 10 minutes. After that, as a polymerization terminator, methanol was added in an amount equivalent to 2 times the molar amount of n-butyllithium used, to obtain a solution containing a conjugated diene rubber. To this solution, 0.15 parts of Irganox 1520L (manufactured by BASF) was added as an antiaging agent relative to 100 parts of the conjugated diene rubber, and the solvent was removed by steam stripping, and the mixture was vacuum dried at 60°C for 24 hours to obtain a solid conjugated diene rubber. The weight average molecular weight (Mw) of the obtained conjugated diene rubber of Example 11 was 485,000, the coupling rate was 55.5%, and the vinyl bond content was 9.8% by weight. In addition, the hot flow property of the obtained conjugated diene rubber of Example 11 was measured according to the above method. The results are shown in Table 4.
[0166] Comparative Example 10 A solid conjugated diene rubber was obtained in the same manner as in Example 11, except that 1.00 mmol of 3-(2-aminoethylamino)propyltrimethoxysilane was not added. The weight average molecular weight (Mw) of the obtained conjugated diene rubber of Comparative Example 10 was 460,000, the coupling rate was 54.0%, and the vinyl bond content was 9.1% by weight. In addition, the hot flow property of the obtained conjugated diene rubber of Comparative Example 10 was measured according to the above-mentioned method. The results are shown in Table 4.
[0167] [Production and Evaluation of Rubber Composition and Cross-Linked Rubber Product] In a 250 ml Banbury mixer, 70 parts of the conjugated diene rubber of Example 11 and 30 parts of natural rubber were masticated for 30 seconds, and then 30 parts of silica (manufactured by Rhodia, trade name "Zeosil 1115MP") and 2.4 parts of a silane coupling agent: bis(3-(triethoxysilyl)propyl)tetrasulfide (manufactured by Evonik, trade name "Si69") were added, and the mixture was kneaded for 1.5 minutes at a starting temperature of 80°C., and then 10 parts of silica (manufactured by Rhodia, trade name "Zeosil 1115MP"), 10 parts of carbon black (manufactured by Tokai Carbon Co., Ltd., trade name "Seest SO"), 10 parts of process oil (manufactured by JX Nippon Oil & Energy Corporation, trade name "Aromax"), and 10 parts of silica (manufactured by Rhodia, trade name "Zeosil 1115MP") were added. The rubber mixture was mixed with 5 parts of N-tert-butyl-2-benzothiazolylsulfenamide (manufactured by Ouchi Shinko Chemical Industry Co., Ltd., product name "Noccela NS-P"), 2 parts of zinc oxide, 2 parts of stearic acid, 2 parts of an antioxidant (manufactured by Ouchi Shinko Chemical Industry Co., Ltd., product name "Noccela 6C"), and 1 part of paraffin wax, and mixed for 2.5 minutes, and then the rubber mixture was discharged from the Banbury mixer. The temperature of the rubber mixture at the end of mixing was 150°C. The rubber mixture was cooled to room temperature, and then mixed again in the Banbury mixer for 3 minutes, and then the rubber mixture was discharged from the Banbury mixer. Next, the obtained rubber mixture was mixed with 1.5 parts of sulfur and 1.3 parts of a crosslinking accelerator [a mixture of 0.9 parts of N-tert-butyl-2-benzothiazolylsulfenamide (manufactured by Ouchi Shinko Chemical Industry Co., Ltd., product name "Noccela NS-P") and 0.4 parts of 1,3-diphenylguanidine (manufactured by Ouchi Shinko Chemical Industry Co., Ltd., product name "Noccela D")] using an open roll at 50°C, and then a sheet-shaped rubber composition was taken out. This rubber composition was press-crosslinked at 150° C. for 20 minutes to prepare test pieces of the crosslinked rubber. The test pieces were evaluated for low heat build-up and wet grip properties according to the above-mentioned methods. Similarly, for the conjugated diene rubber of Comparative Example 10, test pieces of the rubber composition and the cross-linked rubber were prepared, and the low heat build-up and wet grip properties of these test pieces were evaluated according to the above-mentioned methods. The results are shown in Table 4.
[0168] [Table 4] In Table 4, the amount of each component added is shown as the amount when the amount of the polymerization initiator added is taken as 1 part by mole.
[0169] As can be seen from Tables 2 to 4, the conjugated diene rubbers (Examples 9 to 11) obtained by the method for producing a conjugated diene rubber of the present invention had excellent hot flow properties (resistance of solidified crumbs to each other) even when blended with other rubbers, and the obtained cross-linked rubber products had excellent wet grip properties and low heat build-up.
Claims
1. A first step of polymerizing a monomer including a conjugated diene compound in an inert solvent using a polymerization initiator to obtain a conjugated diene polymer chain having an active terminal; A second step of adding a polyorganosiloxane represented by the following general formula (1) to the conjugated diene polymer chain having an active terminal in a ratio of 1 mole or more calculated as the number of repeating units of the siloxane structure (-Si-O-) in the polyorganosiloxane per mole of the polymerization initiator used in the first step, and reacting the polyorganosiloxane with the conjugated diene polymer chain having an active terminal; and a third step of reacting a compound represented by the following general formula (2) with the conjugated diene polymer chain obtained by reacting the polyorganosiloxane obtained in the second step. [C10] (In general formula (1), R 1 ~R 8 is an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 12 carbon atoms, which may be the same or different. X 1 and X 4 is any group selected from the group consisting of an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, and an epoxy group-containing group having 4 to 12 carbon atoms, which may be the same or different. 2 is an alkoxy group having 1 to 5 carbon atoms or a group containing an epoxy group and having 4 to 12 carbon atoms, 2 They may be the same or different. X 3 is a group containing 2 to 20 repeating alkylene glycol units, X 3 When there are a plurality of, they may be the same or different. m is an integer of 3 to 200, n is an integer of 0 to 200, k is an integer of 0 to 200, and m+n+k is 3 or more. [C11] (In general formula (2), R 9 is a hydrocarbyl group, A 1is a group capable of reacting with a reaction residue formed by the reaction of a conjugated diene polymer chain having an active terminal with a polyorganosiloxane, and A 2 is a group containing a primary amino group having an active hydrogen atom, p is an integer of 0 to 2, q is an integer of 1 to 3, r is an integer of 1 to 3, and p+q+r=4.
2. A in the above general formula (2) 1 But, -OR 10 (R 10 The method for producing a conjugated diene rubber according to claim 1, wherein R is a hydrogen atom or a hydrocarbyl group.
3. The method for producing a conjugated diene rubber according to claim 1 or 2, wherein an organic alkali metal amide compound is used as the polymerization initiator.
4. The method for producing a conjugated diene rubber according to claim 3, wherein the organic alkali metal amide compound is a compound represented by the following general formula (3): [C12] (In general formula (3), M 1 represents an alkali metal atom, R 11 , R 12 each independently represents an alkyl group, a cycloalkyl group, an aryl group, an aralkyl group, a protecting group for an amino group, or a group capable of generating a hydroxyl group upon hydrolysis; R 11 and R 12 may be bonded to each other to form a ring structure together with the nitrogen atom to which they are bonded, and when forming such a ring structure, they may form a ring structure together with the nitrogen atom to which they are bonded and a heteroatom other than the nitrogen atom to which they are bonded.
5. The first step comprises: a step of polymerizing isoprene or a monomer containing isoprene and an aromatic vinyl compound in an inert solvent using a polymerization initiator to form a polymer block (A) having an active terminal containing 80 to 100% by weight of isoprene monomer units and 0 to 20% by weight of aromatic vinyl monomer units; and mixing the polymer block (A) having an active end with a monomer containing 1,3-butadiene or 1,3-butadiene and an aromatic vinyl compound to continue a polymerization reaction, thereby forming a polymer block (B) having an active end, which contains 50 to 100% by weight of 1,3-butadiene monomer units and 0 to 50% by weight of aromatic vinyl monomer units, in a continuous state with the polymer block (A), thereby obtaining a conjugated diene polymer chain having an active end.
6. A conjugated diene rubber obtained by the process according to any one of claims 1 to 5.
7. A rubber composition comprising 100 parts by weight of a rubber component containing the conjugated diene rubber according to claim 6 and 10 to 200 parts by weight of silica.
8. The rubber composition according to claim 7, further comprising a crosslinking agent.
9. A cross-linked rubber product obtained by cross-linking the rubber composition according to claim 8.
10. A tire comprising the cross-linked rubber product according to claim 9.
Citation Information
Patent Citations
Terminal-modified conjugated diene-vinyl aromatic hydrocarbon copolymer and method for synthesizing the same
CN103848940A
Functionalized polymer with linking groups
JP2008518086A
Method for producing silane coupling agent
JP2011046640A
Aqueous solution of piperazinyl-containing silanol compound and method for producing the same
JP2012017291A