Tread rubber with five-composite-tread different-rubber structure and tire made of tread rubber with five-composite-tread different-rubber structure

Through the five-composite tread dissimilar structure, combined with a low rolling resistance and good wear rubber composition, the tire's balance problem between rolling resistance, grip and wear resistance is solved, achieving low rolling resistance, high wet grip and Good handling tires.

CN118769767AActive Publication Date: 2024-10-15ZHONGCE RUBBER GRP CO LTD +1

Patent Information

Application Number
CN202410841258.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-15
Estimated Expiration
2044-06-27

AI Technical Summary

Technical Problem

It is difficult for existing tires to strike a balance between rolling resistance, grip and wear resistance, breaking the devil's triangle. Traditional tread rubber has the problem of balancing rolling resistance and wear resistance.

Method used

It adopts a five-compound tread rubber structure, including a middle tread rubber and a shoulder tread rubber. The middle tread rubber uses a low rolling resistance rubber composition, and the shoulder tread rubber uses a rubber composition with good wear and strong grip. The conductive glue is located in the center, and the rolling resistance and handling performance are controlled through the combination of different rubber materials and molding methods.

Benefits of technology

It achieves low rolling resistance, high wet grip, and good handling performance of the tire, while reducing tire shoulder hysteresis loss and taking into account wet grip performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118769767A_ABST
    Figure CN118769767A_ABST
Patent Text Reader

Abstract

The invention relates to the application field of production and manufacturing industries of tires, automobiles and the like, and discloses tread rubber of a five-composite-tread different-rubber structure and a tire of the tread rubber. The tread rubber comprises tread rubber, base rubber, conductive rubber and tire shoulder rubber, and the tread rubber and the base rubber are sequentially arranged from outside to inside to form a tread layer; the tread rubber comprises middle tread rubber and shoulder tread rubber, the shoulder tread rubber is arranged on the two transverse sides of the middle tread rubber, the middle tread rubber is made of a low-rolling-resistance rubber composition, the shoulder tread rubber is arranged on the two transverse sides of the tread layer, and the conductive rubber is located in the center of the tread layer and penetrates through the middle tread rubber and the base rubber from outside to inside. Rolling resistance, wear resistance, braking and control are controlled through two different tread rubber combination modes on the inner side and the outer side, the tire which is low in rolling resistance, high in wear resistance and good in braking performance and control performance can be provided after vulcanization, the lagging loss of the shoulder of the tire can be effectively reduced, and meanwhile the wet land grabbing performance of the tire is considered.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the application field of manufacturing industries such as tires and automobiles, and in particular to a tread rubber profile with a five-composite tread different rubber structure and a tire thereof. Background Art

[0002] The tread rubber structure corresponding to the traditional asymmetric pattern ( Figure 1 ) is mainly composed of four compounds, tread rubber, base rubber, shoulder rubber and conductive rubber. The outer and inner tread rubbers are the same rubber. The tread is responsible for braking and wear resistance, handling comfort, and drainage performance; the base rubber is responsible for modulus transition and molding viscosity, reducing heat generation; the shoulder rubber is responsible for flexibility at the shoulder; and the conductive rubber is responsible for releasing static electricity.

[0003] The Chinese invention patent applied by the applicant (publication number: CN114874510A, publication date: 2022-08-09) is a tread rubber with a five-composite rubber structure, which includes an upper tread rubber, a lower tread rubber, a base rubber, a shoulder rubber and a conductive rubber. The upper tread rubber, the lower tread rubber and the base rubber are arranged from the outside to the inside in sequence to form a tread layer. The upper tread rubber adopts a low rolling resistance and low heat generation rubber composition, and the lower tread rubber adopts a low rolling resistance, good handling, low wear and tear resistance rubber composition; the shoulder rubber is arranged on both sides of the tread layer, and the conductive rubber is located on one side of the center of the tread layer. The conductive rubber runs through the upper tread rubber, the lower tread rubber and the base rubber from the outside to the inside. The tread rubber controls rolling resistance and handling through two different tread rubber combinations in the upper and lower layers, and can provide a tire with low rolling resistance, high wet grip and good handling performance after vulcanization.

[0004] With the rapid development of economy, the automobile production is increasing. As the only part of the car in contact with the ground when driving, the tire is closely related to life safety. With the mandatory implementation of European regulatory labels, the rolling resistance and wet grip performance of tires are increasingly concerned by developers and consumers. It is difficult for tires to achieve a good balance between rolling resistance, grip and wear resistance. To break this devil's triangle, the tread rubber needs to take into account rolling resistance, wear and grip performance. Summary of the invention

[0005] In view of the deficiencies of the prior art, the present invention provides a tread rubber profile with a five-composite tread different rubber structure and a tire thereof, which can ensure both the rolling resistance performance of the tire and the grip and wear performance of the tire.

[0006] In order to achieve the above-mentioned purpose, the present invention adopts the following technical solutions: A tread rubber with a five-composite tread different rubber structure, the tread rubber comprises a tread rubber, a base rubber, a conductive rubber and a shoulder rubber, the tread rubber and the base rubber are sequentially arranged from outside to inside to form a tread layer, the tread rubber comprises an intermediate tread rubber and a shoulder tread rubber, the shoulder tread rubber is arranged on both lateral sides of the intermediate tread rubber, the intermediate tread rubber adopts a low rolling resistance rubber composition, the laboratory room temperature Shore A hardness is 62-68, 300% elongation stress is 8.0-10.0MPa, tanD ≥0.30 at 0°C, tanD ≥0.17 at 20°C, composite modulus E* ≥13.0MPa at 20°C, and tanD ≤0.13 at 60°C; the shoulder tread rubber adopts a rubber composition with good wear and strong grip, the laboratory room temperature Shore A hardness is 66-72, 300% elongation stress is 10.0-13.0MPa, tanD≥0.40 at 0℃, tanD≥0.20 at 20℃, composite modulus E*≥20MPa at 20℃, and tanD is 0.12-0.20 at 60℃; the shoulder rubber is arranged on both sides of the tread layer, the conductive rubber is located in the center of the tread layer, and the conductive rubber runs through the middle tread rubber and the base rubber from the outside to the inside; The intermediate tread rubber composition is prepared by mixing the following raw materials based on 100 parts by weight of raw rubber: 70-90 parts of low Tg soluble styrene butadiene rubber, Neodymium-based butadiene rubber 10-30 parts, 60-90 parts of white carbon black, Super wear-resistant carbon black 10-40 parts, Silane coupling agent 4.8-7.2 parts, Vulcanization accelerator DPG 1-2 parts, Super wear-resistant carbon black 10-40 parts, Sulfur 1.0-2.0 parts, and appropriate amounts of vulcanization accelerator, zinc oxide, stearic acid, microcrystalline wax and antioxidant, wherein the amount of the silane coupling agent is 8% of the amount of white carbon black; the glass transition temperature of the low Tg solution polymerized styrene-butadiene rubber is -30 to -50°C; the particle size of the carbon black is 20-30nm; The shoulder tread rubber composition is prepared by mixing the following raw materials based on 100 parts by weight of raw rubber: Solution polymerized styrene butadiene rubber A 30-45 parts, Solution polymerized styrene butadiene rubber B 30-45 parts, Natural rubber 10-40 parts, 90-120 parts of white carbon black, 3-10 parts of super wear-resistant carbon black, Silane coupling agent 7.2-12 parts, Vulcanization accelerator DPG 1-2 parts, 10-40 parts of poly-α-methylstyrene resin, Sulfur 1.0-2.0 parts, and appropriate amounts of vulcanization accelerator, zinc oxide, stearic acid, environmentally friendly oil, microcrystalline wax and antioxidant, the amount of the silane coupling agent is 8-10% of the amount of white carbon black; in the solution polymerized styrene-butadiene rubber A, styrene accounts for 20-30% of the total weight of the solution polymerized styrene-butadiene rubber A, and the mass of vinyl accounts for 50-60% of the total weight of butadiene; in the solution polymerized styrene-butadiene rubber B, styrene accounts for 40-50% of the total weight of the solution polymerized styrene-butadiene rubber A, and the mass of vinyl accounts for 25-35% of the total weight of butadiene; the nitrogen adsorption specific surface area (BET) of white carbon black is 160-210m2 / g; and the particle size of carbon black is 20-30nm.

[0007] Preferably, the intermediate tread rubber composition is prepared by mixing the following raw materials based on 100 parts by weight of raw rubber: 75-85 parts of low Tg soluble styrene butadiene rubber, 15-25 parts of neodymium-based butadiene rubber, 70-80 parts of white carbon black, 15-25 parts of super wear-resistant carbon black, Silane coupling agent 5.6-6.4 parts, Vulcanization accelerator DPG 1-2 parts, Super wear-resistant carbon black 10-40 parts, Sulfur 1.0-2.0 parts, 2.5-3.5 parts of zinc oxide, 1.5-2.5 parts of stearic acid, Antioxidant 6PPD 1.0-2.0 parts, 1.5-2.5 parts of microcrystalline wax, Vulcanization accelerator NS 1.5-2.5 parts.

[0008] Preferably, the shoulder tread rubber composition is prepared by mixing the following raw materials based on 100 parts by weight of raw rubber: Solution polymerized styrene butadiene rubber A 30-45 parts, Solution polymerized styrene butadiene rubber B 30-45 parts, Natural rubber 15-25 parts, 90-120 parts of white carbon black, 5-7 parts of super wear-resistant carbon black, Silane coupling agent 7.2-12 parts, Vulcanization accelerator DPG 1-2 parts, 10-40 parts of poly-α-methylstyrene resin, Sulfur 1.0-2.0 parts, Zinc oxide 1.5-2.5 parts, 1.5-2.5 parts of stearic acid, Antioxidant 6PPD 1.5-2.5 parts, 1.5-2.5 parts of microcrystalline wax, Vulcanization accelerator CZ 1.0-2.0 parts, Vulcanization accelerator TBzTD 0.2-0.5 parts.

[0009] Preferably, in the raw materials of the intermediate tread rubber and / or shoulder tread rubber rubber composition: super wear-resistant carbon black is N220 or N234, and silane coupling agent is SI69 or SI75.

[0010] Preferably, the intermediate tread rubber has a room temperature Shore A hardness of 64-66, and tanD≤0.10 at 60°C; the shoulder tread rubber has a room temperature Shore A hardness of 68-70, tanD>0.50 at 0°C, tanD>0.22 at 20°C, and tanD is 0.15-0.18 at 60°C.

[0011] Preferably, the middle tread rubber is flat, the tread rubbers on both sides are raised upward, and the thickness of the shoulder tread rubber is 1.1-1.5 times the thickness of the middle tread rubber. Preferably, the thickness of the middle tread rubber is 5.5 mm, and the thickness of the shoulder tread rubber is 7 mm.

[0012] Preferably, the shoulder rubber is a rubber strip with an obtuse triangle cross section, which is spliced ​​on both lateral sides of the tread layer, and the height of the shoulder rubber is 0.6-0.8 times the center height of the tread layer.

[0013] Preferably, the conductive adhesive is a columnar adhesive strip.

[0014] Furthermore, the present invention provides an asymmetric tire with heterogeneous tread rubber, the tire comprising a tread, a sidewall and a shoulder, the shoulder connecting the tread and the sidewall, that is, the shoulder is arranged on both lateral sides of the tread; wherein the tread adopts the tire tread, and the shoulder is composed of shoulder rubber.

[0015] The tread rubber molding method of the above tire is as follows: the outer tread rubber, inner tread rubber, base rubber, shoulder rubber, and conductive rubber are respectively fed into the rubber inlet of each screw extruder, and then extruded through their respective screw extruders and runners, pressed out through a pre-die component and arranged into a preset shape, and finally passed through an extrusion die component together to compositely extrude the tread.

[0016] The beneficial effects of the present invention are as follows: the tread rubber provided by the present invention controls rolling resistance, wear resistance, braking and handling by combining two tread rubbers with different inner and outer sides. After vulcanization, a tire with low rolling resistance, high wear resistance, good braking performance and good handling performance can be provided. The tire shoulder hysteresis loss can be effectively reduced while taking into account the tire wet grip performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is a diagram of the structure of a traditional four-composite tread rubber.

[0018] Figure 2 It is a structural diagram of the five-composite tread rubber of the present invention.

[0019] Figure 3 It is a cross-sectional view of the tire of the present invention.

[0020] Figure 4 The tread pattern of the tire of the present invention.

[0021] Reference numerals: 1 - tread rubber, 11 - middle tread rubber, 12 - shoulder tread rubber, 2 - conductive rubber, 3 - base rubber, 4 - shoulder rubber. DETAILED DESCRIPTION

[0022] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] Example 1 like Figure 2 The tread rubber profile of the five-composite tread different rubber structure shown in the figure comprises a tread rubber 1, a base rubber 3, a conductive rubber 2 and a shoulder rubber 4. The tread rubber 1 and the base rubber 3 are arranged in sequence from the outside to the inside to constitute a tread layer. The tread rubber 1 comprises an intermediate tread rubber 11 and a shoulder tread rubber 12. The shoulder tread rubber 12 is arranged on both lateral sides of the intermediate tread rubber 11. The intermediate tread rubber 11 adopts a low rolling resistance rubber composition, and the shoulder tread rubber 12 adopts a rubber composition with good wear and strong grip. The shoulder rubber 4 is arranged on both lateral sides of the tread layer. The conductive rubber 2 is located at the center of the tread layer. The conductive rubber 2 penetrates the intermediate tread rubber 11 and the base rubber 3 from the outside to the inside. The conductive rubber 2 is a cylindrical rubber strip.

[0024] The intermediate tread rubber 11 rubber composition is prepared by mixing the raw materials of the following components based on 100 parts by weight of raw rubber: 80 parts of low Tg solution-polymerized styrene-butadiene rubber, 20 parts of neodymium-based butadiene rubber, 75 parts of white carbon black, 20 parts of super wear-resistant carbon black, 6.0 parts of silane coupling agent SI69, 1.5 parts of vulcanization accelerator DPG, 25 parts of super wear-resistant carbon black N220, 1.5 parts of sulfur, 3.0 parts of zinc oxide, 2.0 parts of stearic acid, 1.5 parts of antioxidant 6PPD, 2.0 parts of microcrystalline wax, and 2.0 parts of vulcanization accelerator NS.

[0025] Among them, the glass transition temperature of low Tg solution-polymerized styrene-butadiene rubber is -30 to -50°C, and the carbon black particle size is 20-30nm.

[0026] The shoulder tread rubber composition is prepared by mixing the following raw materials based on 100 parts by weight of raw rubber: 40 parts of solution polymerized styrene butadiene rubber A, 40 parts of solution polymerized styrene butadiene rubber B, 20 parts of natural rubber, 105 parts of white carbon black, 6 parts of super wear-resistant carbon black N220, 8.4 parts of silane coupling agent SI69, 1.5 parts of vulcanization accelerator DPG, 25 parts of poly-α-methylstyrene resin, 1.5 parts of sulfur, 2.0 parts of zinc oxide, 2.0 parts of stearic acid, 2.0 parts of antioxidant 6PPD, 2.0 parts of microcrystalline wax, 1.5 parts of vulcanization accelerator CZ, and 0.35 parts of vulcanization accelerator TBzTD.

[0027] Among them, the styrene in solution polymerized styrene butadiene rubber A accounts for 20-30% of the total weight of solution polymerized styrene butadiene rubber A, and the weight of vinyl accounts for 50-60% of the total weight of butadiene; the styrene in solution polymerized styrene butadiene rubber B accounts for 40-50% of the total weight of solution polymerized styrene butadiene rubber A, and the weight of vinyl accounts for 25-35% of the total weight of butadiene; the nitrogen adsorption specific surface area (BET) of white carbon black is 160-210m 2 / g; carbon black particle size is 20-30nm.

[0028] Example 2 Provided is an asymmetric tire with different tread rubber, the tire cross-section diagram is as follows Figure 3 As shown, the tread pattern structure is as follows Figure 4 The tire comprises a tread, a sidewall and a shoulder, wherein the shoulder connects the tread and the sidewall, that is, the shoulder is arranged on both lateral sides of the tread; wherein the tread is made of Figure 2 The tread profile structure shown.

[0029] The tire tread rubber molding method is as follows: the intermediate tread rubber 11, the shoulder tread rubber 12, the base rubber 3, the shoulder rubber 4, and the conductive rubber 2 are fed through the rubber inlet of the respective screw extruders, and then extruded through the respective screw extruders and runners, and then pressed out through the pre-die parts and arranged into a preset shape, and finally passed through the extrusion die parts together to compositely extrude the five composite treads and integrally molded. The thickness of the intermediate tread rubber 11 is 5.5 mm, and the thickness of the shoulder tread rubber 12 is 7 mm.

[0030] This patent can compound five kinds of rubber materials into tread parts by compound extrusion, only by adjusting the extrusion flow channel, and the process is simple. The five rubber compositions provided by this patent have their own characteristics and take into account the mutual coordination of the five kinds of rubber materials. After the five kinds of rubber materials are compound extruded, they are subjected to the molding and vulcanization processes, and the interfaces between the five kinds of rubber materials are cross-linked with each other, so there will be no problem of separation of different rubber materials in actual use.

[0031] The intermediate tread rubber 11 and the shoulder tread rubber 12 adopt the rubber compound formula of Example 1.

[0032] Table 1 Comparison of rheological and physical properties of rubber compositions 11 and 12 In the above Table 1, tensile strength & elongation at break: the larger the value, the better the reinforcement of the rubber compound; hardness: the larger the value, the higher the hardness; tanD at 0℃: characterizes the wet braking performance of the tire, the higher the value, the better; tanD at 20℃: characterizes the dry braking performance of the tire, the higher the value, the better; 20℃ composite modulus E*: characterizes the stiffness of the rubber compound, the larger the value, the stronger the stiffness of the middle tread rubber, and the stronger the cornering control performance of the shoulder tread rubber; tanD at 60℃: characterizes the rolling resistance performance of the tread, the lower the value, the lower the rolling resistance performance.

[0033] Dynamic Mechanical Analyzer (DMA) test conditions (tensile mode): pre-strain 7%, dynamic strain 0.25%, 12HZ.

[0034] Comparative Example 1 A conventional asymmetric pattern tire, which is different from the embodiment 2 in that the tread of the tire is Figure 1 The conventional tread rubber structure shown; the tread rubber adopts the rubber compound formula of the intermediate tread rubber 11 of Example 1.

[0035] Performance Testing According to the relevant national standard test method, the tires of Example 2 and Comparative Example 1 were subjected to indoor performance tests. All test results were calculated based on the comparative example as 100. Test value (relative value) = test value of the embodiment / test value of the comparative example × 100. The specific measurement results are shown in Table 2. The tires with a trial production specification of 245 / 45R18 were used.

[0036] Table 2 Comparison of indoor test performance between comparative example 1 and embodiment 2 Physical properties Comparative Example 1 Example 2 Dry braking 100 105 Dry handling 100 107 Wet braking 100 103 Wet handling 100 105 wear and tear 100 102 Rolling resistance 100 102 In the above Table 2, it can be seen from the comparison between the examples and the embodiments that the tires of the embodiments have better dry and wet braking and tire handling performance, while the tire rolling resistance and wear are slightly improved.

[0037] The above is a description of the embodiments of the present invention. Through the above description of the disclosed embodiments, professionals and technicians in the field can implement or use the present invention. Various modifications to these embodiments will be apparent to professionals and technicians in the field. The general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to these embodiments shown in this article, but will conform to the widest range consistent with the principles and novelties disclosed herein.

Claims

1. A tread rubber with a five-composite tread rubber structure. It is characterized in that The tread rubber comprises a tread rubber, a base rubber, a conductive rubber and a shoulder rubber. The tread rubber and the base rubber are sequentially arranged from the outside to the inside to form a tread layer. The tread rubber comprises an intermediate tread rubber and a shoulder tread rubber. The shoulder tread rubber is arranged on both lateral sides of the intermediate tread rubber. The intermediate tread rubber adopts a low rolling resistance rubber composition, with a laboratory room temperature Shore A hardness of 62-68, a 300% elongation stress of 8.0-10.0 MPa, tanD ≥0.30 at 0°C, tanD ≥0.17 at 20°C, a composite modulus E* ≥13.0 MPa at 20°C, and tanD ≤0.13 at 60°C. The shoulder tread rubber adopts a rubber composition with good wear resistance and strong grip, with a laboratory room temperature Shore A hardness of 66-72, 300% elongation stress is 10.0-13.0MPa, tanD≥0.40 at 0℃, tanD≥0.20 at 20℃, composite modulus E*≥20MPa at 20℃, and tanD is 0.12-0.20 at 60℃; the shoulder rubber is arranged on both sides of the tread layer, the conductive rubber is located in the center of the tread layer, and the conductive rubber runs through the middle tread rubber and the base rubber from the outside to the inside; The intermediate tread rubber composition is prepared by mixing the following raw materials based on 100 parts by weight of raw rubber: 70-90 parts of low Tg soluble styrene butadiene rubber, Neodymium-based butadiene rubber 10-30 parts, 60-90 parts of white carbon black, Super wear-resistant carbon black 10-40 parts, Silane coupling agent 4.8-7.2 parts, Vulcanization accelerator DPG 1-2 parts, Super wear-resistant carbon black 10-40 parts, Sulfur 1.0-2.0 parts, and appropriate amounts of vulcanization accelerator, zinc oxide, stearic acid, microcrystalline wax and antioxidant, wherein the amount of the silane coupling agent is 8% of the amount of white carbon black; the glass transition temperature of the low Tg solution polymerized styrene-butadiene rubber is -30 to -50°C; the particle size of the carbon black is 20-30nm; The shoulder tread rubber composition is prepared by mixing the following raw materials based on 100 parts by weight of raw rubber: Solution polymerized styrene butadiene rubber A 30-45 parts, Solution polymerized styrene butadiene rubber B 30-45 parts, Natural rubber 10-40 parts, 90-120 parts of white carbon black, 3-10 parts of super wear-resistant carbon black, Silane coupling agent 7.2-12 parts, Vulcanization accelerator DPG 1-2 parts, 10-40 parts of poly-α-methylstyrene resin, Sulfur 1.0-2.0 parts, and appropriate amounts of vulcanization accelerator, zinc oxide, stearic acid, environmentally friendly oil, microcrystalline wax and antioxidant, wherein the amount of the silane coupling agent is 8-10% of the amount of the white carbon black; in the solution polymerized styrene-butadiene rubber A, styrene accounts for 20-30% of the total weight of the solution polymerized styrene-butadiene rubber A, and the weight of the vinyl accounts for 50-60% of the total weight of butadiene; in the solution polymerized styrene-butadiene rubber B, styrene accounts for 40-50% of the total weight of the solution polymerized styrene-butadiene rubber A, and the weight of the vinyl accounts for 25-35% of the total weight of butadiene; the nitrogen adsorption specific surface area (BET) of the white carbon black is 160-210 m 2 / g; carbon black particle size is 20-30nm.

2. The tread rubber according to claim 1, It is characterized in that The intermediate tread rubber composition is prepared by mixing the following raw materials based on 100 parts by weight of raw rubber: 75-85 parts of low Tg soluble styrene butadiene rubber, 15-25 parts of neodymium-based butadiene rubber, 70-80 parts of white carbon black, 15-25 parts of super wear-resistant carbon black, Silane coupling agent 5.6-6.4 parts, Vulcanization accelerator DPG 1-2 parts, Super wear-resistant carbon black 10-40 parts, Sulfur 1.0-2.0 parts, 2.5-3.5 parts of zinc oxide, 1.5-2.5 parts of stearic acid, Antioxidant 6PPD 1.0-2.0 parts, 1.5-2.5 parts of microcrystalline wax, Vulcanization accelerator NS 1.5-2.5 parts.

3. The tread rubber according to claim 1, It is characterized in that The shoulder tread rubber composition is prepared by mixing the following raw materials based on 100 parts by weight of raw rubber: Solution polymerized styrene butadiene rubber A 30-45 parts, Solution polymerized styrene butadiene rubber B 30-45 parts, Natural rubber 15-25 parts, 90-120 parts of white carbon black, 5-7 parts of super wear-resistant carbon black, Silane coupling agent 7.2-12 parts, Vulcanization accelerator DPG 1-2 parts, 10-40 parts of poly-α-methylstyrene resin, Sulfur 1.0-2.0 parts, Zinc oxide 1.5-2.5 parts, 1.5-2.5 parts of stearic acid, Antioxidant 6PPD 1.5-2.5 parts, 1.5-2.5 parts of microcrystalline wax, Vulcanization accelerator CZ 1.0-2.0 parts, Vulcanization accelerator TBzTD 0.2-0.5 parts.

4. The tread rubber according to any one of claims 1 to 3, It is characterized in that In the raw materials of the intermediate tread rubber and / or shoulder tread rubber rubber composition: the super wear-resistant carbon black is N220 or N234, and the silane coupling agent is SI69 or SI75.

5. The tread rubber according to claim 1, It is characterized in that The laboratory room temperature Shore A hardness of the intermediate tread rubber is 64-66, and tanD≤0.10 at 60°C; the laboratory room temperature Shore A hardness of the shoulder tread rubber is 68-70, tanD>0.50 at 0°C, tanD>0.22 at 20°C, and tanD is 0.15-0.18 at 60°C.

6. The tread rubber according to claim 1, It is characterized in that The middle tread rubber is flat, the tread rubbers on both sides are raised upward, and the thickness of the shoulder tread rubber is 1.1-1.5 times the thickness of the middle tread rubber.

7. The tread rubber according to claim 1 or 6, It is characterized in that The thickness of the middle tread rubber is 5.5 mm, and the thickness of the shoulder tread rubber is 7 mm.

8. The tread rubber according to claim 1, It is characterized in that The shoulder rubber (4) is a rubber strip with an obtuse triangle cross section, which is spliced ​​and arranged on both lateral sides of the tread layer. The height of the shoulder rubber (4) is 0.6-0.8 times the center height of the tread layer.

9. The tread rubber according to claim 1, It is characterized in that The conductive adhesive (2) is a columnar adhesive strip.

10. An asymmetric tire with different tread rubber, It is characterized in that The tire comprises a tread, a sidewall and a shoulder, wherein the shoulder connects the tread and the sidewall, that is, the shoulder is arranged on both lateral sides of the tread; wherein the tread adopts the tire tread described in any one of claims 1 to 9, and the shoulder is composed of shoulder rubber.

Citation Information

Patent Citations

  • Pneumatic tire

    CN103826878A

  • Tread for an aircraft tire

    CN113165427A

  • Low-rolling-resistance wet-skid-resistance four-season tire capable of preventing groove bottom cracks in winter

    CN114163702A

  • Tread rubber with five-compound rubber material structure, preparation method and tire adopting tread rubber

    CN114874510A

  • Tire for two-wheel vehicle

    US20210213784A1

Cited By

  • Tread rubber with asymmetric rubber material structure, preparation method and tire adopting tread rubber

    CN119898140A

  • Tread rubber with staggered rubber material structure, preparation method and tire adopting tread rubber

    CN119898141A

  • Sidewall rubber with four-composite rubber material structure

    CN120116660A