Photosensitive resin composition

By integrating an alkylene oxide chain into the resin components of photosensitive resin compositions, the trade-off between flexibility and insulation is resolved, resulting in a cured product with enhanced properties for printed wiring boards and semiconductor devices.

JP7557262B2Active Publication Date: 2024-09-27AJINOMOTO CO INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2019159653
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-09-02
Publication Date
2024-09-27
Estimated Expiration
2039-09-02

AI Technical Summary

Technical Problem

Photosensitive resin compositions for solder resists face a trade-off between flexibility and insulation properties, making it difficult to achieve both high flexibility and good insulation in printed wiring boards as they miniaturize.

Method used

Incorporating an alkylene oxide chain into the resin components of the photosensitive resin composition, specifically in components (A), (B), and (C), with a parameter X represented by a specific formula ranging from 4 to 25, to balance flexibility and insulation properties.

Benefits of technology

The composition yields a cured product with excellent flexibility, insulation properties, and resolution, suitable for applications in printed wiring boards and semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007557262000007
    Figure 0007557262000007
  • Figure 0007557262000002
    Figure 0007557262000002
  • Figure 0007557262000015
    Figure 0007557262000015
Patent Text Reader

Abstract

To provide a photosensitive resin composition or the like which can give a cured product excellent in flexibility and insulating properties and is excellent in resolution.SOLUTION: The photosensitive resin composition contains (A) a resin containing an ethylenically unsaturated group and a carboxyl group, (B) an epoxy resin, (C) a photopolymerizable monomer, and (D) a photopolymerization initiator. Any of the component (A), the component (B) and the component (C) contains an alkylene oxide chain. A parameter X represented by the following formula (1) is 4 or more and 25 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a photosensitive resin composition, and further to a photosensitive film, a photosensitive film with a support, a printed wiring board, and a semiconductor device obtained by using the photosensitive resin composition. [Background technology]

[0002] In printed wiring boards, solder resist is sometimes provided as a permanent protective film for preventing solder from adhering to areas where solder is not required and for preventing the circuit board from corroding. As the solder resist, a photosensitive resin composition such as that described in Patent Document 1 is generally used. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2014-115672 A Summary of the Invention [Problem to be solved by the invention]

[0004] Photosensitive resin compositions for solder resists are generally required to have resolution, insulating properties, etc. In recent years, the miniaturization of electronic devices has led to the need for space saving, and therefore printed wiring boards are required to have flexibility (bendability). The solder resists used in such printed wiring boards are also required to have flexibility.

[0005] However, as a result of extensive research, the present inventors have found that attempts to improve flexibility can result in a deterioration in the insulating properties of the solder resist, and that there is a trade-off between flexibility and insulating properties in photosensitive resin compositions for solder resists.

[0006] An object of the present invention is to provide a photosensitive resin composition which can give a cured product having excellent flexibility and insulating properties and excellent resolution; and to provide a photosensitive film, a photosensitive film with a support, a printed wiring board, and a semiconductor device which are obtained using the photosensitive resin composition. [Means for solving the problem]

[0007] As a result of intensive research, the present inventors have found that both flexibility and insulating properties are improved when any one of the resin containing an ethylenically unsaturated group and a carboxyl group, the epoxy resin, and the photopolymerizable monomer contained in the photosensitive resin composition contains an alkylene oxide chain, and the alkylene oxide chain satisfies a specific relationship, thereby completing the present invention.

[0008] That is, the present invention includes the following. [1] (A) a resin containing an ethylenically unsaturated group and a carboxyl group, (B) epoxy resin, (C) a photopolymerizable monomer, and (D) a photopolymerization initiator, A photosensitive resin composition, wherein any one of the components (A), (B), and (C) contains an alkylene oxide chain, and a parameter X represented by the following formula (1) is 4 or more and 25 or less:

number

number

[10] A photosensitive film comprising the photosensitive resin composition according to any one of [1] to [9].

[11] A support-attached photosensitive film comprising: a support; and a photosensitive resin composition layer provided on the support, the photosensitive resin composition layer comprising the photosensitive resin composition according to any one of [1] to [9].

[12] A printed wiring board comprising an insulating layer formed from a cured product of the photosensitive resin composition according to any one of [1] to [9].

[13] The printed wiring board according to

[12] , wherein the insulating layer is a solder resist.

[14] A semiconductor device comprising the printed wiring board according to

[12] or

[13] . Effect of the Invention

[0009] According to the present invention, it is possible to provide a photosensitive resin composition which can give a cured product having excellent flexibility and insulating properties and excellent resolution; and a photosensitive film, a photosensitive film with a support, a printed wiring board, and a semiconductor device which are obtained using the photosensitive resin composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The photosensitive resin composition, photosensitive film, photosensitive film with a support, printed wiring board, and semiconductor device of the present invention will be described in detail below.

[0011] [Photosensitive resin composition] The photosensitive resin composition of the present invention is a photosensitive resin composition containing (A) a resin containing an ethylenically unsaturated group and a carboxyl group, (B) an epoxy resin, (C) a photopolymerizable monomer, and (D) a photopolymerization initiator, wherein any one of the components (A), (B), and (C) contains an alkylene oxide chain, and a parameter X represented by the following formula (1) is 4 or more and 25 or less.

number

number

[0012] In the present invention, by adjusting the content of the alkylene oxide chain contained in any one of the (A), (B), and (C) components relative to the entire components (A) to (C) that are curable resins, a cured product having excellent flexibility and insulation can be obtained, and a photosensitive resin composition having excellent resolution can be provided. In addition, a cured product having excellent adhesion can also be obtained. The present inventors have found that when a photosensitive resin composition is hydrophilic, it has excellent flexibility but poor insulation. For this reason, they have focused on the content of the alkylene oxide chain that is involved in polymerization and has a hydrophobic structure in the (A) to (C) components. As a result, when the content of the alkylene oxide chain contained in any one of the (A), (B), and (C) components relative to the entire components (A) to (C) is adjusted so as to satisfy the above formula (1), the flexibility of the photosensitive resin composition is increased, and both the flexibility and insulation can be improved. In addition, it is considered that the hydrophobic structure of the alkylene oxide chain also improves adhesion.

[0013] The alkylene oxide chain has a structure represented by the following formula (a). [ka] In formula (a), each R independently represents an alkylene group which may have a substituent; q represents an integer of 1-100.

[0014] R represents an alkylene group which may have a substituent. The alkylene group is preferably an alkylene group having 1 to 10 carbon atoms, more preferably an alkylene group having 1 to 6 carbon atoms, and further preferably an alkylene group having 1 to 5, 1 to 4, or 1 to 3 carbon atoms. Specific examples of the alkylene group include a methylene group, an ethylene group, a propylene group, an isopropylene group, an n-butylene group, a pentylene group, and a hexylene group.

[0015] The alkylene group may have a substituent. Examples of the substituent include an alkyl group having 1 to 3 carbon atoms, a halogen atom, etc. The substituent may be contained alone or in combination of two or more kinds.

[0016] q represents an integer of 1 to 100, preferably an integer of 1 to 50, more preferably an integer of 1 to 10, and further preferably an integer of 1 to 5.

[0017] Examples of the alkylene oxide chain include methylene oxide, ethylene oxide (EO), propylene oxide (PO), isopropylene oxide, and butylene oxide (BO).

[0018] The alkylene oxide chain is preferably contained in the (A) component, more preferably in the (B) component, and more preferably in the (C) component. The alkylene oxide chain is preferably contained in the (A) component and the (B) component, more preferably in the (A) component and the (C) component, more preferably in the (B) component and the (C) component, and more preferably in the (A) to (C) components. Among them, the alkylene oxide chain is more preferably contained in the (B) component and the (C) component.

[0019] The components (A) to (C) may each have one type of alkylene oxide chain in one molecule, or may have multiple types of alkylene oxide chains.

[0020] The photosensitive resin composition may further contain optional components in combination with the components (A) to (D). Examples of the optional components include an inorganic filler (E), a solvent (F), and other additives (G). Each component contained in the photosensitive resin composition will be described in detail below.

[0021] <(A) Resin containing an ethylenically unsaturated group and a carboxyl group> The photosensitive resin composition contains a resin containing an ethylenically unsaturated group and a carboxyl group as component (A). By including component (A) in the photosensitive resin composition, the developability can be improved.

[0022] Examples of the ethylenically unsaturated group include a vinyl group, an allyl group, a propargyl group, a butenyl group, an ethynyl group, a phenylethynyl group, a maleimide group, a nadimide group, and a (meth)acryloyl group. From the viewpoint of reactivity in photoradical polymerization, a (meth)acryloyl group is preferable. The term "(meth)acryloyl group" refers to a methacryloyl group and an acryloyl group.

[0023] The component (A) has an ethylenically unsaturated group and a carboxyl group. Because of this structure, the component (A) can be photoradical polymerized and can be developed in an alkali. As the component (A), for example, a resin having both a carboxyl group and two or more ethylenically unsaturated groups in one molecule is preferable.

[0024] An embodiment of the resin containing an ethylenically unsaturated group and a carboxyl group includes an acid-modified unsaturated epoxy ester resin obtained by reacting an epoxy compound with an unsaturated carboxylic acid and then with an acid anhydride. In detail, an unsaturated epoxy ester resin is obtained by reacting an epoxy compound with an unsaturated carboxylic acid, and an acid-modified unsaturated epoxy ester resin is obtained by reacting the unsaturated epoxy ester resin with an acid anhydride. Any of the epoxy compound, the unsaturated carboxylic acid, and the acid anhydride may have an alkylene oxide chain.

[0025] As the epoxy compound, any compound having an epoxy group in the molecule can be used, and examples thereof include bisphenol-type epoxy resins such as epoxy group-containing copolymers, bisphenol A-type epoxy resins, hydrogenated bisphenol A-type epoxy resins, bisphenol F-type epoxy resins, hydrogenated bisphenol F-type epoxy resins, bisphenol S-type epoxy resins, and modified bisphenol F-type epoxy resins obtained by reacting bisphenol F-type epoxy resins with epichlorohydrin to modify them to have three or more functional groups; biphenol-type epoxy resins, such as biphenol-type epoxy resins and tetramethylbiphenol-type epoxy resins; novolac-type epoxy resins, such as phenol novolac-type epoxy resins, cresol novolac-type epoxy resins, bisphenol A-type novolac-type epoxy resins, and alkylphenol novolac-type epoxy resins; fluorine-containing epoxy resins, such as bisphenol AF-type epoxy resins and perfluoroalkyl-type epoxy resins; naphthalene-type epoxy resins, dihydroxynaphthalene-type epoxy resins, polyhydroxybinaphthalene-type epoxy resins, naphthol-type epoxy resins, and binaphthol-type epoxy resins. epoxy resins having a naphthalene skeleton, such as naphthylene ether type epoxy resins, naphthol novolac type epoxy resins, and naphthalene type epoxy resins obtained by a condensation reaction between polyhydroxynaphthalene and aldehydes (naphthalene skeleton-containing epoxy resins); bixylenol type epoxy resins; dicyclopentadiene type epoxy resins; trisphenol type epoxy resins; tert-butyl-catechol type epoxy resins; epoxy resins containing a condensed ring skeleton, such as anthracene type epoxy resins; glycidylamine type epoxy resins; glycidyl ester type epoxy resins; biphenyl type epoxy resins; linear aliphatic epoxy resins; epoxy resins having a butadiene structure; alicyclic epoxy resins; heterocyclic epoxy resins; spiro ring-containing epoxy resins; cyclohexanedimethanol type epoxy resins; trimethylol type epoxy resins; tetraphenylethane type epoxy resins; glycidyl group-containing acrylic resins, such as polyglycidyl (meth)acrylate and copolymers of glycidyl methacrylate and acrylic acid esters; fluorene type epoxy resins; and halogenated epoxy resins.

[0026] From the viewpoint of reducing the average linear thermal expansion coefficient, the epoxy compound is preferably an epoxy group-containing copolymer or an epoxy resin containing an aromatic skeleton. Here, the aromatic skeleton is a concept including polycyclic aromatics and aromatic heterocycles. The epoxy compound is preferably a naphthalene skeleton-containing epoxy resin; an epoxy resin containing a condensed ring skeleton; a biphenyl type epoxy resin; a bisphenol type epoxy resin such as a bisphenol F type epoxy resin or a bisphenol A type epoxy resin; a cresol novolac type epoxy resin; or a glycidyl ester type epoxy resin.

[0027] The epoxy group-containing copolymer can be obtained by polymerizing an epoxy group-containing monomer and, if necessary, any other monomer. Examples of the epoxy group-containing monomer include epoxy group-containing (meth)acrylate monomers such as glycidyl (meth)acrylate, 3,4-epoxybutyl (meth)acrylate, 2-methyl-3,4-epoxycyclohexyl (meth)acrylate, and allyl glycidyl ether, and glycidyl (meth)acrylate is preferred. The epoxy group-containing monomer may be used alone or in combination of two or more.

[0028] Examples of the optional monomer include styrene, (meth)acrylic acid, methyl (meth)acrylate, ethyl methacrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl methacrylate, and nonyl (meth)acrylate. , decyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, behenyl (meth)acrylate, cyclohexyl (meth)acrylate, 4-tert-butylcyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, benzyl (meth)acrylate, acrylamide, N,N-dimethyl (meth)acrylamide, (meth)acrylonitrile, 3-(meth)acrylate, p) Acryloylpropyltrimethoxysilane, N,N-dimethylaminoethyl (meth)acrylate, glycidyl (meth)acrylate, styrene, α-methylstyrene, p-methylstyrene, p-methoxystyrene, 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxy-n-butyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxy-n-butyl (meth)acrylate, 3-hydroxy-n-butyl (meth)acrylate , 1,4-cyclohexanedimethanol mono(meth)acrylate, glycerin mono(meth)acrylate, polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, 2-hydroxy-3-phenoxypropyl(meth)acrylate, 2-(meth)acryloyloxyethyl-2-hydroxyethyl phthalate, lactone-modified (meth)acrylate having a hydroxyl group at the end, 1-adamantyl(meth)acrylate, etc., are included, and n-butyl(meth)acrylate is preferred. Any monomer may be used alone or in a mixture of two or more kinds."(Meth)acrylic acid" refers to acrylic acid and methacrylic acid. "(Meth)acrylate" refers to acrylate and methacrylate.

[0029] As the epoxy resin containing a naphthalene skeleton, dihydroxynaphthalene type epoxy resin, polyhydroxybinaphthalene type epoxy resin, and naphthalene type epoxy resin obtained by condensation reaction of polyhydroxynaphthalene and aldehydes are preferable. As the dihydroxynaphthalene type epoxy resin, for example, 1,3-diglycidyloxynaphthalene, 1,4-diglycidyloxynaphthalene, 1,5-diglycidyloxynaphthalene, 1,6-diglycidyloxynaphthalene, 2,3-diglycidyloxynaphthalene, 2,6-diglycidyloxynaphthalene, 2,7-diglycidyloxynaphthalene, etc. are mentioned. As the polyhydroxybinaphthalene type epoxy resin, for example, 1,1'-bi-(2-glycidyloxy)naphthyl, 1-(2,7-diglycidyloxy)-1'-(2'-glycidyloxy)binaphthyl, 1,1'-bi-(2,7-diglycidyloxy)naphthyl, etc. are mentioned. Examples of naphthalene-type epoxy resins obtained by the condensation reaction of polyhydroxynaphthalene with aldehydes include 1,1'-bis(2,7-diglycidyloxynaphthyl)methane, 1-(2,7-diglycidyloxynaphthyl)-1'-(2'-glycidyloxynaphthyl)methane, and 1,1'-bis(2-glycidyloxynaphthyl)methane.

[0030] Examples of unsaturated carboxylic acids include acrylic acid, methacrylic acid, cinnamic acid, crotonic acid, glycidyl methacrylate, and glycidyl acrylate, and these may be used alone or in combination of two or more. Among them, acrylic acid and methacrylic acid are preferred from the viewpoint of improving the photocurability of the photosensitive resin composition. In this specification, the epoxy ester resin, which is a reaction product of the above-mentioned epoxy compound and (meth)acrylic acid, may be referred to as "epoxy (meth)acrylate", and here the epoxy group of the epoxy compound is substantially eliminated by the reaction with (meth)acrylic acid.

[0031] Examples of the acid anhydride include maleic anhydride, succinic anhydride, itaconic anhydride, phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, trimellitic anhydride, pyromellitic anhydride, and benzophenonetetracarboxylic dianhydride, and these may be used alone or in combination of two or more. Among these, succinic anhydride and tetrahydrophthalic anhydride are preferred from the viewpoint of improving the resolution and insulation reliability of the cured product.

[0032] In obtaining the acid-modified unsaturated epoxy ester resin, a catalyst, a solvent, a polymerization inhibitor, and the like may be used, if necessary.

[0033] The acid-modified unsaturated epoxy ester resin is preferably an acid-modified epoxy (meth)acrylate, and more preferably contains either an acid-modified naphthalene skeleton-containing epoxy (meth)acrylate or an acid-modified bisphenol skeleton-containing epoxy (meth)acrylate. The "epoxy" in the acid-modified unsaturated epoxy ester resin represents the structure derived from the above-mentioned epoxy compound. For example, "acid-modified bisphenol type epoxy (meth)acrylate" refers to an acid-modified unsaturated epoxy ester resin obtained by using a bisphenol type epoxy resin as an epoxy compound and (meth)acrylic acid as an unsaturated carboxylic acid.

[0034] The acid-modified unsaturated epoxy ester resin is preferably a (meth)acrylic polymer having a glass transition temperature of -20°C or less. A (meth)acrylic polymer is a polymer containing a structural unit having a structure formed by polymerizing a (meth)acrylic monomer. Examples of such a (meth)acrylic polymer include a polymer obtained by polymerizing a (meth)acrylic monomer, or a polymer obtained by copolymerizing a (meth)acrylic monomer and a monomer copolymerizable with the (meth)acrylic monomer.

[0035] Examples of (meth)acrylic polymers having a glass transition temperature of -20°C or less include acid-modified unsaturated epoxy (meth)acrylic copolymers obtained by reacting an epoxy group-containing copolymer with (meth)acrylic acid and further reacting with an acid anhydride. In more detail, an acid-modified unsaturated epoxy (meth)acrylic copolymer can be obtained by reacting an epoxy group-containing copolymer with (meth)acrylic acid to obtain an unsaturated epoxy (meth)acrylic copolymer, and then reacting the unsaturated epoxy (meth)acrylic copolymer with an acid anhydride to obtain an acid-modified unsaturated epoxy (meth)acrylic copolymer.

[0036] Preferred embodiments of the (meth)acrylic polymer having a glass transition temperature of -20°C or less include an epoxy group-containing copolymer obtained by polymerizing an epoxy group-containing monomer and an arbitrary monomer, and a compound obtained by reacting (meth)acrylic acid and an acid anhydride, in which the epoxy group-containing monomer is glycidyl methacrylate, the arbitrary monomer is butyl acrylate, and the acid anhydride is tetrahydrophthalic anhydride.

[0037] Such acid-modified unsaturated epoxy ester resins can be commercially available products, and specific examples include "ZAR-2000" (a reaction product of bisphenol A type epoxy resin, acrylic acid, and succinic anhydride), "ZFR-1491H", and "ZFR-1533H" (a reaction product of bisphenol F type epoxy resin, acrylic acid, and tetrahydrophthalic anhydride (a bisphenol F type skeleton-containing acid-modified epoxy acrylate)) manufactured by Nippon Kayaku Co., Ltd., and "PR-300CP" (a reaction product of cresol novolac type epoxy resin, acrylic acid, and acid anhydride) manufactured by Showa Denko KK. These may be used alone or in combination of two or more.

[0038] Another embodiment of the resin containing an ethylenically unsaturated group and a carboxyl group is an unsaturated modified (meth)acrylic resin obtained by reacting an ethylenically unsaturated group-containing epoxy compound with a (meth)acrylic resin having a structural unit obtained by polymerizing (meth)acrylic acid to introduce an ethylenically unsaturated group. Examples of the ethylenically unsaturated group-containing epoxy compound include glycidyl methacrylate, 4-hydroxybutyl (meth)acrylate glycidyl ether, and 3,4-epoxycyclohexylmethyl (meth)acrylate. It is also possible to react an acid anhydride with the hydroxyl group generated during the introduction of the unsaturated group. The acid anhydride can be the same as the above-mentioned acid anhydride, and the preferred range is also the same.

[0039] Such unsaturated modified (meth)acrylic resins can be commercially available products, and specific examples include "SPC-1000" and "SPC-3000" manufactured by Showa Denko K.K., and "Cyclomer P(ACA)Z-250", "Cyclomer P(ACA)Z-251", "Cyclomer P(ACA)Z-254", "Cyclomer P(ACA)Z-300", and "Cyclomer P(ACA)Z-320" manufactured by Daicel-Allnex Corporation.

[0040] The weight average molecular weight of the component (A) is preferably 1000 or more, more preferably 1500 or more, and even more preferably 2000 or more, from the viewpoint of film-forming properties. The upper limit is preferably 50000 or less, more preferably 30000 or less, and even more preferably 25000 or less, from the viewpoint of developability. The weight average molecular weight is a polystyrene-equivalent weight average molecular weight measured by gel permeation chromatography (GPC).

[0041] The acid value of the (A) component is preferably 0.1 mgKOH / g or more, more preferably 0.5 mgKOH / g or more, and even more preferably 1 mgKOH / g or more, from the viewpoint of improving the alkaline developability of the photosensitive resin composition. On the other hand, from the viewpoint of suppressing the fine pattern of the cured product from dissolving due to development and improving the insulation reliability, the acid value is preferably 150 mgKOH / g or less, more preferably 120 mgKOH / g or less, and even more preferably 100 mgKOH / g or less. Here, the acid value refers to the residual acid value of the carboxyl group present in the (A) component, and the acid value can be measured by the following method. First, after weighing out about 1 g of the resin solution to be measured, 30 g of acetone is added to the resin solution to dissolve the resin solution uniformly. Next, an appropriate amount of phenolphthalein as an indicator is added to the solution, and titration is performed using a 0.1 N KOH aqueous solution. Then, the acid value is calculated by the following formula. Formula: A(b)=10×Vf×56.1 / (Wp×I)

[0042] In the above formula, A(b) represents the acid value (mgKOH / g), Vf represents the titration amount of KOH (mL), Wp represents the mass of the measured resin solution (g), and I represents the proportion of non-volatile content of the measured resin solution (mass%).

[0043] In producing the component (A), from the viewpoint of improving storage stability, the ratio of the number of moles of epoxy groups in the epoxy resin to the total number of moles of carboxyl groups in the unsaturated carboxylic acid and the acid anhydride is preferably in the range of 1:0.8 to 1.3, and more preferably in the range of 1:0.9 to 1.2.

[0044] From the viewpoint of improving flexibility, the glass transition temperature (Tg) of the component (A) is preferably −300° C. or higher, more preferably −200° C. or higher, and even more preferably −80° C. or higher, and is preferably −20° C. or lower, more preferably −23° C. or lower, and even more preferably −25° C. or lower. Here, the glass transition temperature of the component (A) refers to the theoretical glass transition temperature of the main chain of the component (A), and this theoretical glass transition temperature can be calculated by the FOX formula shown below. The glass transition temperature calculated by the FOX formula is almost the same as the glass transition temperature measured by differential scanning calorimetry (TMA, DSC, DTA), so the glass transition temperature of the main chain of the component (A) may be measured by differential scanning calorimetry. 1 / Tg=(W1 / Tg1)+(W2 / Tg2)+...+(Wm / Tgm) W1+W2+···+Wm=1 Wm represents the content (mass %) of each monomer constituting the component (A), and Tgm represents the glass transition temperature (K) of each monomer constituting the component (A).

[0045] From the viewpoint of improving alkaline developability, the (A) component is preferably 3% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more, when the non-volatile components in the photosensitive resin composition are taken as 100% by mass. From the viewpoint of improving heat resistance and average linear expansion coefficient, the upper limit is preferably 30% by mass or less, more preferably 25% by mass or less, and even more preferably 20% by mass or less. In the present invention, the content of each component in the photosensitive resin composition is a value when the non-volatile components in the photosensitive resin composition are taken as 100% by mass, unless otherwise specified.

[0046] <(B) Epoxy resin> The photosensitive resin composition contains an epoxy resin as component (B). By containing component (B), the insulation reliability can be improved. However, component (B) does not include epoxy resins containing ethylenically unsaturated groups and carboxyl groups.

[0047] Examples of the component (B) include bixylenol type epoxy resins, bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bisphenol AF type epoxy resins, dicyclopentadiene type epoxy resins, trisphenol type epoxy resins, naphthol novolac type epoxy resins, phenol novolac type epoxy resins, tert-butyl-catechol type epoxy resins, naphthalene type epoxy resins, naphthol type epoxy resins, anthracene type epoxy resins, glycidylamine type epoxy resins, glycidyl ester type epoxy resins, cresol novolac type epoxy resins, biphenyl type epoxy resins, linear aliphatic epoxy resins, alkylene oxide chain-containing aliphatic epoxy resins, epoxy resins having a butadiene structure, alicyclic epoxy resins, heterocyclic epoxy resins, spiro ring-containing epoxy resins, cyclohexane type epoxy resins, cyclohexane dimethanol type epoxy resins, naphthylene ether type epoxy resins, trimethylol type epoxy resins, and tetraphenylethane type epoxy resins. Among them, the (B) epoxy resin is preferably a biphenyl type epoxy resin or a linear aliphatic epoxy resin, and more preferably a biphenyl type epoxy resin. The (B) epoxy resin may be used alone or in combination of two or more. Examples of the alkylene oxide chain-containing aliphatic epoxy resin include an alkylene oxide chain-containing linear aliphatic epoxy resin, an alkylene oxide chain-containing branched aliphatic epoxy resin, and an alkylene oxide chain-containing cyclic aliphatic epoxy resin.

[0048] The photosensitive resin composition preferably contains, as component (B), an epoxy resin having two or more epoxy groups in one molecule. From the viewpoint of significantly obtaining the desired effects of the present invention, the ratio of the epoxy resin having two or more epoxy groups in one molecule to 100% by mass of the non-volatile components of component (B) is preferably 50% by mass or more, more preferably 60% by mass or more, and particularly preferably 70% by mass or more.

[0049] Component (B) includes epoxy resins that are liquid at a temperature of 20° C. (hereinafter sometimes referred to as “liquid epoxy resins”) and epoxy resins that are solid at a temperature of 20° C. (hereinafter sometimes referred to as “solid epoxy resins”). The resin composition may contain only a liquid epoxy resin as component (B), may contain only a solid epoxy resin, or may contain a combination of a liquid epoxy resin and a solid epoxy resin.

[0050] As the solid epoxy resin, a solid epoxy resin having three or more epoxy groups in one molecule is preferable, and an aromatic solid epoxy resin having three or more epoxy groups in one molecule is more preferable.

[0051] As the solid epoxy resin, bixylenol type epoxy resin, naphthalene type epoxy resin, naphthalene type tetrafunctional epoxy resin, cresol novolac type epoxy resin, dicyclopentadiene type epoxy resin, trisphenol type epoxy resin, naphthol type epoxy resin, biphenyl type epoxy resin, naphthylene ether type epoxy resin, anthracene type epoxy resin, bisphenol A type epoxy resin, bisphenol AF type epoxy resin, and tetraphenylethane type epoxy resin are preferred, and naphthalene type epoxy resin is more preferred.

[0052] Specific examples of solid epoxy resins include "HP4032H" (naphthalene type epoxy resin) manufactured by DIC Corporation; "HP-4700" and "HP-4710" (naphthalene type tetrafunctional epoxy resins) manufactured by DIC Corporation; "N-690" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "N-695" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "HP-7200", "HP-7200HH", and "HP-7200H" (dicyclopentadiene epoxy resin) manufactured by DIC Corporation. diene type epoxy resins); "EXA-7311", "EXA-7311-G3", "EXA-7311-G4", "EXA-7311-G4S", and "HP6000" (naphthylene ether type epoxy resins) manufactured by DIC; "EPPN-502H" (trisphenol type epoxy resins) manufactured by Nippon Kayaku; "NC7000L" (naphthol novolac type epoxy resins) manufactured by Nippon Kayaku; "NC3000H", "NC3000", and "NC3000" manufactured by Nippon Kayaku L, "NC3100" (biphenyl type epoxy resin); "ESN475V" (naphthol type epoxy resin) manufactured by Nippon Steel & Sumitomo Metal Chemical Co., Ltd.; "ESN485" (naphthol novolac type epoxy resin) manufactured by Nippon Steel & Sumitomo Metal Chemical Co., Ltd.; "YX4000H", "YX4000", "YL6121" (biphenyl type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "YX4000HK" (bixylenol type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "YX8800" ( anthracene type epoxy resin); "PG-100" and "CG-500" manufactured by Osaka Gas Chemicals; "YL7760" (bisphenol AF type epoxy resin) manufactured by Mitsubishi Chemical; "YL7800" (fluorene type epoxy resin) manufactured by Mitsubishi Chemical; "jER1010" (solid bisphenol A type epoxy resin) manufactured by Mitsubishi Chemical; "jER1031S" (tetrakishydroxyphenylethane type epoxy resin) manufactured by Mitsubishi Chemical. These may be used alone or in combination of two or more.

[0053] The liquid epoxy resin is preferably a liquid epoxy resin having two or more epoxy groups in one molecule.

[0054] As the liquid epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AF type epoxy resin, naphthalene type epoxy resin, glycidyl ester type epoxy resin, glycidyl amine type epoxy resin, phenol novolac type epoxy resin, alicyclic epoxy resin having an ester skeleton, cyclohexane type epoxy resin, cyclohexane dimethanol type epoxy resin, glycidyl amine type epoxy resin, and epoxy resin having a butadiene structure are preferred, and bisphenol A type epoxy resin and bisphenol F type epoxy resin are more preferred.

[0055] Specific examples of liquid epoxy resins include "HP4032", "HP4032D", and "HP4032SS" (naphthalene type epoxy resins) manufactured by DIC Corporation; "828US", "jER828EL", "825", and "Epikote 828EL" (bisphenol A type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER807" and "1750" (bisphenol F type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER152" (phenol novolac type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "630" and "630LSD" (glycidylamine type epoxy resins) manufactured by Mitsubishi Chemical Corporation; and "ZX1059" (bisphenol A type epoxy resin) manufactured by Nippon Steel & Sumitomo Metal Chemical Co., Ltd. Examples of such epoxy resins include mixtures of bisphenol A type epoxy resins and bisphenol F type epoxy resins; Nagase ChemteX's "EX-721" (glycidyl ester type epoxy resin); Nagase ChemteX's "EX-821" and "EX-920" (linear aliphatic epoxy resins containing alkylene oxide chains); Daicel's "Celloxide 2021P" (alicyclic epoxy resin having an ester skeleton); Daicel's "PB-3600" (epoxy resin having a butadiene structure); Nippon Steel & Sumikin Chemical's "ZX1658" and "ZX1658GS" (liquid 1,4-glycidylcyclohexane type epoxy resins). These may be used alone or in combination of two or more.

[0056] When a liquid epoxy resin and a solid epoxy resin are used in combination as component (B), the ratio by mass (liquid epoxy resin:solid epoxy resin) is preferably 1:1 to 1:20, more preferably 1:1.5 to 1:15, and particularly preferably 1:2 to 1:10. When the ratio by mass of the liquid epoxy resin and the solid epoxy resin is within this range, the desired effects of the present invention can be significantly obtained.

[0057] The epoxy equivalent of the (B) component is preferably 50 g / eq. to 5000 g / eq., more preferably 50 g / eq. to 3000 g / eq., even more preferably 80 g / eq. to 2000 g / eq., and even more preferably 110 g / eq. to 1000 g / eq. When it is in this range, the crosslink density of the cured product of the resin composition layer becomes sufficient, and an insulating layer with small surface roughness can be obtained. The epoxy equivalent is the mass of an epoxy resin containing one equivalent of epoxy groups. This epoxy equivalent can be measured according to JIS K7236.

[0058] The weight average molecular weight (Mw) of the component (B) is preferably 100 to 5,000, more preferably 250 to 3,000, and even more preferably 400 to 1,500, from the viewpoint of significantly achieving the desired effects of the present invention. The weight average molecular weight of the resin can be measured by gel permeation chromatography (GPC) as a polystyrene-equivalent value.

[0059] From the viewpoint of obtaining an insulating layer exhibiting good tensile mechanical strength and insulating reliability, the content of the (B) component is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more, when the non-volatile components in the resin composition are taken as 100% by mass. From the viewpoint of obtaining the desired effects of the present invention significantly, the upper limit of the content of the (C) component is preferably 20% by mass or less, more preferably 15% by mass or less, and particularly preferably 10% by mass or less.

[0060] <(C) Photopolymerizable monomer> The photosensitive resin composition contains a photopolymerizable monomer as component (C). However, component (C) does not include components (A) and (B). By including photopolymerizable monomer (C) in the photosensitive resin composition, photoreactivity can be improved. As component (C), for example, a photosensitive (meth)acrylate compound that has one or more (meth)acryloyl groups in one molecule and is liquid, solid or semi-solid at room temperature can be used. Room temperature refers to about 25°C.

[0061] Examples of the photosensitive (meth)acrylate compound include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl acrylate and 2-hydroxybutyl acrylate; mono- or di(meth)acrylates of glycols such as ethylene glycol, methoxytetraethylene glycol, polyethylene glycol, and propylene glycol; acrylamides such as N,N-dimethylacrylamide and N-methylolacrylamide; aminoalkyl (meth)acrylates such as N,N-dimethylaminoethyl acrylate; trimethylolpropane, pentaerythritol, dipentaerythritol, and the like. Examples of the polyhydric (meth)acrylates include polyhydric alcohols such as taerythritol or their adducts with ethylene oxide, propylene oxide or ε-caprolactone; (meth)acrylates of phenols such as phenoxy acrylate and phenoxyethyl acrylate or their ethylene oxide or propylene oxide adducts; epoxy acrylates derived from glycidyl ethers such as trimethylolpropane triglycidyl ether, modified epoxy acrylates, melamine acrylates, and / or methacrylates corresponding to the above acrylates. (Meth)acrylate refers to acrylate and methacrylate.

[0062] Among these, (meth)acrylates and polyhydric (meth)acrylates such as mono- or di(meth)acrylates of glycols, phenols such as phenoxy acrylate and phenoxyethyl acrylate, and their ethylene oxide or propylene oxide adducts are preferred.

[0063] Examples of glycol mono- or di(meth)acrylates include polytetramethylene glycol diacrylate.

[0064] Examples of phenols such as phenoxy acrylate and phenoxyethyl acrylate, or (meth)acrylates such as their ethylene oxide or propylene oxide adducts include EO-modified bisphenol A-type acrylate.

[0065] As the polyvalent (meth)acrylates, for example, trivalent acrylates or methacrylates are preferable. Examples of the trivalent acrylates or methacrylates include 1,9-nonanediol diacrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, trimethylolpropane EO-added tri(meth)acrylate, glycerin PO-added tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, tetrafurfuryl alcohol oligo(meth)acrylate, ethyl carbitol oligo(meth)acrylate, 1,4-butanediol oligo(meth)acrylate, 1,6-hexanediol oligo(meth)acrylate, trimethylolpropane oligo(meth)acrylate, pentaerythritol oligo(meth)acrylate, and tetramethylolmethane tetra(meth)acrylate. Examples of the trivalent or higher acrylates or methacrylates include phosphate triester (meth)acrylates such as tri(2-(meth)acryloyloxyethyl)phosphate, tri(2-(meth)acryloyloxypropyl)phosphate, tri(3-(meth)acryloyloxypropyl)phosphate, tri(3-(meth)acryloyl-2-hydroxyloxypropyl)phosphate, di(3-(meth)acryloyl-2-hydroxyloxypropyl)(2-(meth)acryloyloxyethyl)phosphate, and (3-(meth)acryloyl-2-hydroxyloxypropyl)di(2-(meth)acryloyloxyethyl)phosphate. These photosensitive (meth)acrylate compounds may be used alone or in combination of two or more.

[0066] (C) The photopolymerizable monomer may be a commercially available product, such as "DPHA" manufactured by Nippon Kayaku Co., Ltd., "EBECRYL3708" manufactured by Daicel Allnex Co., Ltd., "R-551" manufactured by Nippon Kayaku Co., Ltd., "A-PTMG-65" manufactured by Shin-Nakamura Chemical Co., Ltd., or "1.9ND" manufactured by Kyoeisha Chemical Co., Ltd.

[0067] From the viewpoint of promoting photocuring, the content of the (C) photopolymerizable monomer is preferably 0.5% by mass or more, more preferably 1% by mass or more, and even more preferably 1.5% by mass or more, when the total solid content of the photosensitive resin composition is taken as 100% by mass, and is preferably 20% by mass or less, more preferably 15% by mass or less, and even more preferably 10% by mass or less.

[0068] <(D) Photopolymerization initiator> The photosensitive resin composition contains a photopolymerization initiator as component (D). By including the photopolymerization initiator (D) in the photosensitive resin composition, the photosensitive resin composition can be efficiently photocured. These may be used alone or in combination of two or more.

[0069] (D) The photopolymerization initiator may be any compound, and examples of such photopolymerization initiators include acylphosphine oxide-based photopolymerization initiators such as bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide) and 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide; oxime ester-based photopolymerization initiators such as 1,2-octanedione, 1-4-(phenylthio)-2-(O-benzoyloxime), ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, and 1-(O-acetyloxime); 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-1-butanone, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-[4-(4-morpholinyl)phenyl]-1-butanone, and 2-methyl-1-[4-(methylthio)phenyl]-2-mol Examples of the photopolymerization initiator include α-aminoalkylphenone-based photopolymerization initiators such as holinopropan-1-one; benzophenone, methylbenzophenone, o-benzoylbenzoic acid, benzoyl ethyl ether, 2,2-diethoxyacetophenone, 2,4-diethylthioxanthone, diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide, ethyl-(2,4,6-trimethylbenzoyl)phenylphosphinate, 4,4'-bis(diethylamino)benzophenone, 1-hydroxy-cyclohexyl-phenyl ketone, 2,2-dimethoxy-1,2-diphenylethan-1-one, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxand; and sulfonium salt-based photopolymerization initiators. These may be used alone or in combination of two or more. Among these, from the viewpoint of more efficiently photocuring the photosensitive resin composition, either an acylphosphine oxide-based photopolymerization initiator or an oxime ester-based photopolymerization initiator is preferred, and an oxime ester-based photopolymerization initiator is more preferred.

[0070] Specific examples of the (D) photopolymerization initiator include "Omnirad907", "Omnirad369", "Omnirad379", "Omnirad819", and "OmniradTPO" manufactured by IGM; "IrgacureOXE-01", "IrgacureOXE-02", "IrgacureTPO", and "Irgacure819" manufactured by BASF; and "N-1919" and "NCI-831" manufactured by ADEKA.

[0071] Furthermore, the photosensitive resin composition may contain, in combination with the (D) photopolymerization initiator, tertiary amines such as N,N-dimethylaminobenzoic acid ethyl ester, N,N-dimethylaminobenzoic acid isoamyl ester, pentyl-4-dimethylaminobenzoate, triethylamine, triethanolamine, etc. as a photopolymerization initiation assistant, or may contain photosensitizers such as pyrarizones, anthracenes, coumarins, xanthones, thioxanthones, etc. Any of these may be used alone or in combination of two or more.

[0072] The content of the (D) photopolymerization initiator is preferably 0.001% by mass or more, more preferably 0.005% by mass or more, and even more preferably 0.01% by mass or more, when the non-volatile components of the photosensitive resin composition are taken as 100% by mass, from the viewpoint of sufficiently photocuring the photosensitive resin composition and improving insulation reliability. On the other hand, from the viewpoint of suppressing a decrease in resolution due to excessive sensitivity, the upper limit is preferably 3% by mass or less, more preferably 1% by mass or less, and even more preferably 0.5% by mass or less. In addition, when the photosensitive resin composition contains a photopolymerization initiation assistant, it is preferable that the total content of the (D) photopolymerization initiator and the photopolymerization initiation assistant is within the above range.

[0073] <(E) Inorganic filler> In addition to the above-mentioned components, the photosensitive resin composition may further contain an inorganic filler as an optional component (E).

[0074] (E) An inorganic compound is used as the material of the inorganic filler. Examples of the material of the inorganic filler include silica, alumina, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium zirconate titanate, barium zirconate, calcium zirconate, zirconium phosphate, and zirconium tungstate phosphate. Among these, silica and magnesium hydroxide are preferred, and magnesium hydroxide is particularly preferred. Examples of silica include amorphous silica, fused silica, crystalline silica, synthetic silica, and hollow silica. In addition, spherical silica is preferred as the silica. The (F) inorganic filler may be used alone or in combination of two or more kinds.

[0075] Examples of commercially available products of component (E) include "UFP-20" and "UFP-30" manufactured by Denka Company; "SP60-05" and "SP507-05" manufactured by Nippon Steel & Sumikin Materials Co., Ltd.; "SC2050", "YC100C", "YA050C", "YA050C-MJE", "YA010C", "SC2500SQ", "SO-C4", "SO-C2", and "SO-C1" manufactured by Admatechs Co., Ltd.; "Silfil NSS-3N", "Silfil NSS-4N", and "Silfil NSS-5N" manufactured by Tokuyama Corporation; and "EP4-A" manufactured by Konoshima Chemical Co., Ltd.

[0076] The specific surface area of ​​component (E) is preferably 1 m 2 / g or more, more preferably 2m 2 / g or more, particularly preferably 3m 2 / g or more. There is no particular upper limit, but it is preferably 60m 2 / g or less, 50m 2 / g or less or 40m 2The specific surface area is determined by adsorbing nitrogen gas onto the surface of a sample using a specific surface area measuring device (Macsorb HM-1210 manufactured by Mountec Co., Ltd.) according to the BET method, and calculating the specific surface area using the BET multipoint method.

[0077] From the viewpoint of significantly obtaining the desired effects of the present invention, the average particle size of component (E) is preferably 0.01 μm or more, more preferably 0.05 μm or more, and particularly preferably 0.1 μm or more, and is preferably 5 μm or less, more preferably 2 μm or less, and even more preferably 1 μm or less.

[0078] The average particle size of component (E) can be measured by a laser diffraction / scattering method based on the Mie scattering theory. Specifically, the particle size distribution of the inorganic filler is created on a volume basis using a laser diffraction / scattering particle size distribution measuring device, and the median diameter is used as the average particle size. The measurement sample can be prepared by weighing 100 mg of inorganic filler and 10 g of methyl ethyl ketone into a vial and dispersing the mixture by ultrasonic waves for 10 minutes. The measurement sample is measured using a laser diffraction particle size distribution measuring device with blue and red light wavelengths as the light source, and the particle size distribution of component (E) on a volume basis is measured using a flow cell method, and the average particle size can be calculated as the median diameter from the particle size distribution obtained. An example of a laser diffraction particle size distribution measuring device is the "LA-960" manufactured by Horiba, Ltd.

[0079] From the viewpoint of improving moisture resistance and dispersibility, it is preferable that the (E) component is treated with a surface treatment agent. Examples of the surface treatment agent include vinylsilane coupling agents, (meth)acrylic coupling agents, fluorine-containing silane coupling agents, aminosilane coupling agents, epoxysilane coupling agents, mercaptosilane coupling agents, silane coupling agents, alkoxysilanes, organosilazane compounds, and titanate coupling agents. Among them, from the viewpoint of obtaining the effects of the present invention remarkably, vinylsilane coupling agents, (meth)acrylic coupling agents, and aminosilane coupling agents are preferred. Moreover, the surface treatment agent may be used alone or in any combination of two or more types.

[0080] Commercially available surface treatment agents include, for example, Shin-Etsu Chemical Co., Ltd.'s "KBM1003" (vinyltriethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM503" (3-methacryloxypropyltriethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM403" (3-glycidoxypropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM803" (3-mercaptopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBE903" (3-aminopropyltriethoxysilane), ... Examples of such silane coupling agents include Shin-Etsu Chemical Co., Ltd.'s "KBM573" (N-phenyl-3-aminopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "SZ-31" (hexamethyldisilazane), Shin-Etsu Chemical Co., Ltd.'s "KBM103" (phenyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM-4803" (long-chain epoxy-type silane coupling agent), and Shin-Etsu Chemical Co., Ltd.'s "KBM-7103" (3,3,3-trifluoropropyltrimethoxysilane).

[0081] The degree of surface treatment with the surface treatment agent is preferably within a predetermined range from the viewpoint of improving the dispersibility of the inorganic filler. Specifically, 100 parts by mass of the inorganic filler is preferably surface-treated with 0.2 parts by mass to 5 parts by mass of the surface treatment agent, more preferably 0.2 parts by mass to 3 parts by mass, and even more preferably 0.3 parts by mass to 2 parts by mass.

[0082] The degree of surface treatment with the surface treatment agent can be evaluated by the amount of carbon per unit surface area of ​​the inorganic filler. From the viewpoint of improving the dispersibility of the inorganic filler, the amount of carbon per unit surface area of ​​the inorganic filler is set to 0.02 mg / m 2 More than 0.1 mg / m is preferable. 2 More preferably, 0.2 mg / m or more 2 On the other hand, from the viewpoint of suppressing an increase in the melt viscosity of the resin varnish and the melt viscosity in the form of a film, it is more preferable that the content is 1 mg / m 2 Less than 0.8 mg / m is preferred. 2 Less than 0.5 mg / m is more preferable. 2 The following is even more preferred:

[0083] The amount of carbon per unit surface area of ​​the inorganic filler can be measured after the surface-treated inorganic filler is washed with a solvent (e.g., methyl ethyl ketone (MEK)). Specifically, a sufficient amount of MEK as a solvent is added to the inorganic filler that has been surface-treated with a surface treatment agent, and ultrasonic cleaning is performed at 25°C for 5 minutes. After removing the supernatant and drying the solid content, the amount of carbon per unit surface area of ​​the inorganic filler can be measured using a carbon analyzer. The carbon analyzer that can be used is the "EMIA-320V" manufactured by Horiba, Ltd.

[0084] From the viewpoint of significantly obtaining the effects of the present invention, the content of the component (E) is preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 25% by mass or more, 30% by mass or more, 40% by mass or more, or 50% by mass or more, and is preferably 90% by mass or less, more preferably 80% by mass or less, even more preferably 70% by mass or less, 60% by mass or less, 50% by mass or less, or 40% by mass or less, based on 100% by mass of non-volatile components in the photosensitive resin composition.

[0085] <(F) Solvent> The photosensitive resin composition may further contain a solvent (F) as an optional component in addition to the above-mentioned components. The viscosity of the varnish can be adjusted by adding the solvent (F). Examples of the solvent (F) include organic solvents.

[0086] Examples of the (F) solvent include ketones such as ethyl methyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as methyl cellosolve, butyl cellosolve, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; esters such as ethyl acetate, butyl acetate, butyl cellosolve acetate, carbitol acetate, and ethyl diglycol acetate; aliphatic hydrocarbons such as octane and decane; and petroleum solvents such as petroleum ether, petroleum naphtha, hydrogenated petroleum naphtha, and solvent naphtha. These are used alone or in combination of two or more. The content of the solvent when used can be appropriately adjusted from the viewpoint of the coating property of the resin composition.

[0087] <(G) Other Additives> The photosensitive resin composition may further contain (G) other additives to the extent that the object of the present invention is not impaired. Examples of (G) other additives include thermoplastic resins, organic fillers, fine particles such as melamine and organic bentonite, colorants such as phthalocyanine blue, phthalocyanine green, iodine green, diazo yellow, crystal violet, titanium oxide, carbon black, and naphthalene black, polymerization inhibitors such as hydroquinone, phenothiazine, methylhydroquinone, hydroquinone monomethyl ether, catechol, and pyrogallol, thickeners such as bentone and montmorillonite, silicone-based, fluorine-based, and vinyl resin-based defoamers, flame retardants such as brominated epoxy compounds, acid-modified brominated epoxy compounds, antimony compounds, phosphorus-based compounds, aromatic condensed phosphate esters, and halogen-containing condensed phosphate esters, and thermosetting resins such as phenol-based curing agents and cyanate ester-based curing agents.

[0088] The photosensitive resin composition can be produced by mixing the above-mentioned components (A) to (D) as essential components, appropriately mixing the above-mentioned components (E) to (G) as optional components, and kneading or stirring, as necessary, with kneading means such as a triple roll mill, a ball mill, a bead mill, or a sand mill, or with stirring means such as a super mixer or a planetary mixer.

[0089] <Properties and applications of photosensitive resin compositions> The photosensitive resin composition contains an alkylene oxide chain in any one of the components (A), (B), and (C), in which the parameter X shown in the following formula (1) is 4 or more and 25 or less. By satisfying formula (1), it is possible to obtain a cured product with excellent flexibility and insulating properties.

number

number

[0090] The term "copolymer" refers to a polymer obtained by polymerization of two or more monomers and having a weight average molecular weight of at least 10000. The copolymer may be any of random copolymers, block copolymers, alternating copolymers, and graft copolymers.

[0091] As described above, the copolymer may be a random copolymer, and the molecular weight of the copolymer may be M AO It can be difficult to calculate the value of M for copolymers. AO If it is difficult to calculate the value of M, use formula (2) to calculate AO It is possible to calculate A in Equation (2). AO The molecular weight per unit of the alkylene oxide chain is calculated by / A, and further, B in formula (2) AO By multiplying the molar ratio of the monomer containing the alkylene oxide chain represented by / B, the M AO The value of can be calculated. The "monomer" in the definition of formula (2) represents a compound corresponding to a monomer unit contained in a copolymer. The "monomer unit" represents a partial structure in a copolymer formed by polymerizing a certain compound.

[0092] In order to obtain a cured product having excellent flexibility and insulating properties and to improve resolution, X in formula (1) is 25 or less, preferably 23 or less, more preferably 20 or less, and even more preferably 18 or less. In order to obtain the effects of the present invention significantly, the lower limit of X in formula (1) is 4 or more, preferably 5 or more, and more preferably 6 or more.

[0093] The cured product obtained by photocuring the photosensitive resin composition of the present invention exhibits excellent resolution. Therefore, when a round hole (via) with an opening diameter of 100 μm is formed using the cured product, the formation of residue at the bottom of the round hole can be suppressed. The via bottom residue can be evaluated according to the method described below in <Evaluation of via bottom residue>.

[0094] The cured product obtained by photocuring the photosensitive resin composition of the present invention exhibits excellent flexibility. A specific example of the measurement of flexibility is to use a photosensitive film in which the photosensitive resin composition layer is exposed to light over the entire surface, developed, and heat-treated, and evaluate the flexibility according to JIS P8115 using an MIT folding fatigue tester. At this time, the average number of flexing is usually 100 times or more, preferably 300 times or more. The details of the evaluation of flexibility can be measured according to the method described in the examples below.

[0095] The photocured product obtained by photocuring the photosensitive resin composition of the present invention exhibits excellent insulating properties. In a specific example of evaluation of insulating properties, the photosensitive resin film is exposed to light from above the comb-shaped wiring pattern, developed, and heat-treated. Copper wires are soldered to both sides of the comb-shaped pattern as electrodes, a predetermined voltage is applied, and the resistance values ​​at seven points after 500 hours are measured. At this time, the resistance value is preferably 10 8 The insulation property can be evaluated in detail according to the method described in the examples below.

[0096] The cured product obtained by photocuring the photosensitive resin composition of the present invention usually exhibits excellent adhesive strength with copper foil. A specific example of the evaluation of adhesive strength is to laminate a photosensitive resin composition layer with a glass epoxy substrate laminated to rolled copper foil, and then perform full-surface exposure, development, and heat treatment. The copper foil is peeled off using a tensile tester ("AC-50C-SL" manufactured by TSE) conforming to the Japanese Industrial Standards (JIS C6481). At this time, the adhesive strength with the copper foil is usually 0.5 kgf or more. Details of the evaluation of adhesive strength can be measured according to the method described in the examples below.

[0097] The use of the photosensitive resin composition of the present invention is not particularly limited, but it can be used in a wide range of applications requiring a photosensitive resin composition, such as photosensitive films, photosensitive films with supports, insulating resin films such as prepregs, circuit boards (for laminates, multilayer printed wiring boards, etc.), solder resists, underfill materials, die bonding materials, semiconductor encapsulants, hole filling resins, component embedding resins, etc. In particular, it can be suitably used as a photosensitive resin composition for insulating layers of printed wiring boards (printed wiring boards in which a cured product of a photosensitive resin composition is used as an insulating layer), a photosensitive resin composition for interlayer insulating layers (printed wiring boards in which a cured product of a photosensitive resin composition is used as an interlayer insulating layer), a photosensitive resin composition for plating (printed wiring boards in which plating is formed on a cured product of a photosensitive resin composition), and a photosensitive resin composition for solder resist (printed wiring boards in which a cured product of a photosensitive resin composition is used as a solder resist).

[0098] [Photosensitive film] The photosensitive resin composition of the present invention can be applied in a resin varnish state onto a supporting substrate, and the organic solvent can be dried to form a photosensitive resin composition layer, which can be used as a photosensitive film. Also, a photosensitive film formed in advance on a support can be laminated onto the supporting substrate. The photosensitive film can be laminated onto various supporting substrates. Examples of the supporting substrate include glass epoxy substrates, metal substrates, polyester substrates, polyimide substrates, BT resin substrates, and thermosetting polyphenylene ether substrates.

[0099] [Photosensitive film with support] The photosensitive resin composition of the present invention can be suitably used in the form of a supported photosensitive film in which a photosensitive resin composition layer is formed on a support. That is, the supported photosensitive film includes a support and a photosensitive resin composition layer formed of the photosensitive resin composition of the present invention provided on the support.

[0100] Examples of the support include a polyethylene terephthalate film, a polyethylene naphthalate film, a polypropylene film, a polyethylene film, a polyvinyl alcohol film, a triacetyl acetate film, and the like, with a polyethylene terephthalate film being particularly preferred.

[0101] Examples of commercially available supports include, but are not limited to, polyethylene terephthalate films such as "Alphan MA-410" and "E-200C" manufactured by Oji Paper Co., Ltd., polypropylene films manufactured by Shin-Etsu Film Co., Ltd., and PS series films such as "PS-25" manufactured by Teijin Co., Ltd. These supports are preferably coated with a release agent such as a silicone coating agent on the surface in order to facilitate removal of the photosensitive resin composition layer. The thickness of the support is preferably in the range of 5 μm to 50 μm, and more preferably in the range of 10 μm to 25 μm. By making the thickness 5 μm or more, it is possible to prevent the support from being torn when peeling off the support before development, and by making the thickness 50 μm or less, it is possible to improve the resolution when exposing from above the support. In addition, a support with low fisheyes is preferable. Here, fisheyes are foreign matter, undissolved matter, oxidized deterioration products, etc. of the material that are taken into the film when the material is thermally melted and then kneaded, extruded, biaxially stretched, cast, etc. to produce a film.

[0102] In addition, in order to reduce scattering of light during exposure to active energy rays such as ultraviolet rays, the support is preferably one having excellent transparency. Specifically, the support is preferably one having a turbidity (haze standardized by JIS-K6714) as an index of transparency of 0.1 to 5. Furthermore, the photosensitive resin composition layer may be protected with a protective film.

[0103] By protecting the photosensitive resin composition layer side of the support-attached photosensitive film with a protective film, it is possible to prevent the adhesion of dirt and the like to the surface of the photosensitive resin composition layer and scratches. As the protective film, a film made of the same material as the support can be used. The thickness of the protective film is not particularly limited, but is preferably in the range of 1 μm to 40 μm, more preferably in the range of 5 μm to 30 μm, and even more preferably in the range of 10 μm to 30 μm. By making the thickness 1 μm or more, the handleability of the protective film can be improved, and by making the thickness 40 μm or less, the cost tends to be improved. In addition, it is preferable that the adhesive strength between the photosensitive resin composition layer and the protective film is smaller than the adhesive strength between the photosensitive resin composition layer and the support.

[0104] The photosensitive film with a support of the present invention can be produced according to a method known to those skilled in the art, for example, by preparing a resin varnish by dissolving the photosensitive resin composition of the present invention in an organic solvent, applying the resin varnish on a support, and drying the organic solvent by heating or blowing hot air to form a photosensitive resin composition layer. Specifically, first, bubbles in the photosensitive resin composition are completely removed by a vacuum degassing method or the like, and then the photosensitive resin composition is applied on a support, the solvent is removed by a hot air oven or a far-infrared oven, the support is dried, and then a protective film is laminated on the obtained photosensitive resin composition layer as necessary to produce a photosensitive film with a support. Specific drying conditions vary depending on the curability of the photosensitive resin composition and the amount of organic solvent in the resin varnish, but in a resin varnish containing 30% by mass to 60% by mass of organic solvent, drying can be performed at 80°C to 120°C for 3 minutes to 13 minutes. The amount of the remaining organic solvent in the photosensitive resin composition layer is preferably 5% by mass or less, more preferably 2% by mass or less, based on the total amount of the photosensitive resin composition layer, from the viewpoint of preventing the diffusion of the organic solvent in the subsequent process. Those skilled in the art can appropriately set suitable drying conditions through simple experiments. The thickness of the photosensitive resin composition layer is preferably in the range of 5 μm to 500 μm, more preferably in the range of 10 μm to 200 μm, even more preferably in the range of 15 μm to 150 μm, even more preferably in the range of 20 μm to 100 μm, and especially preferably in the range of 20 μm to 60 μm, from the viewpoint of improving the handleability and suppressing the decrease in the sensitivity and resolution inside the photosensitive resin composition layer.

[0105] Examples of methods for applying the photosensitive resin composition include gravure coating, microgravure coating, reverse coating, kiss reverse coating, die coating, slot die, lip coating, comma coating, blade coating, roll coating, knife coating, curtain coating, chamber gravure coating, slot orifice coating, spray coating, and dip coating. The photosensitive resin composition may be applied in several portions, may be applied in one portion, or may be applied by combining a plurality of different methods. Among them, the die coating method is preferable because of its excellent uniformity of application. In addition, in order to avoid contamination by foreign matter, it is preferable to carry out the application process in an environment where foreign matter is unlikely to be generated, such as a clean room.

[0106] [Printed wiring board] The printed wiring board of the present invention includes an insulating layer formed from a cured product of the photosensitive resin composition of the present invention. The insulating layer is preferably used as a solder resist.

[0107] In particular, the printed wiring board of the present invention can be produced by using the above-mentioned photosensitive film or the photosensitive film with a support. Hereinafter, the case where the insulating layer is a solder resist will be described.

[0108] <Coating and drying process> The photosensitive resin composition is applied directly onto the circuit board in the form of a resin varnish, and the organic solvent is dried to form a photosensitive film on the circuit board.

[0109] Examples of the circuit board include a glass epoxy board, a metal board, a polyester board, a polyimide board, a BT resin board, and a thermosetting polyphenylene ether board. The circuit board here refers to a board having a patterned conductor layer (circuit) on one or both sides of the board as described above. In addition, in a multilayer printed wiring board formed by alternately laminating a conductor layer and an insulating layer, a board in which one or both sides of the outermost layer of the multilayer printed wiring board are patterned conductor layers (circuits) is also included in the circuit board here. The surface of the conductor layer may be previously roughened by blackening, copper etching, or the like.

[0110] As a coating method, full-surface printing by screen printing is generally used, but any other coating method that can apply uniformly may be used. For example, spray coating, hot melt coating, bar coating, applicator, blade coating, knife coating, air knife coating, curtain flow coating, roll coating, gravure coating, offset printing, dip coating, brush coating, and other normal coating methods can all be used. After coating, drying is performed in a hot air oven or far-infrared oven, etc., as necessary. Drying conditions are preferably 80°C to 120°C for 3 to 13 minutes. In this way, a photosensitive film is formed on the circuit board.

[0111] <Lamination process> When a photosensitive film with a support is used, the photosensitive resin composition layer side is laminated on one or both sides of a circuit board using a vacuum laminator. In the lamination step, if the photosensitive film with a support has a protective film, the protective film is removed, and then the photosensitive film with a support and the circuit board are preheated as necessary, and the photosensitive resin composition layer is pressure-bonded to the circuit board while being pressurized and heated. For a photosensitive film with a support, a method of laminating the film to the circuit board under reduced pressure by a vacuum lamination method is preferably used.

[0112] The conditions for the lamination step are not particularly limited, but for example, the pressure bonding temperature (lamination temperature) is preferably 70° C. to 140° C., and the pressure bonding pressure is preferably 1 kgf / cm. 2 ~11kgf / cm 2 (9.8×10 4 N / m 2 ~107.9×10 4 N / m 2), the pressure bonding time is preferably 5 seconds to 300 seconds, and lamination is preferably performed under reduced pressure with an air pressure of 20 mmHg (26.7 hPa) or less. The lamination process may be a batch type or a continuous type using a roll. The vacuum lamination method can be performed using a commercially available vacuum laminator. Examples of commercially available vacuum laminators include a vacuum applicator manufactured by Nikko Materials Co., Ltd., a vacuum pressure laminator manufactured by Meiki Seisakusho Co., Ltd., a roll type dry coater manufactured by Hitachi Industries Co., Ltd., and a vacuum laminator manufactured by Hitachi AIC Co., Ltd. In this way, a photosensitive film is formed on the circuit board.

[0113] <Exposure process> After the photosensitive film is provided on the circuit board by the coating and drying process or the lamination process, an exposure process is then performed in which a predetermined portion of the photosensitive resin composition layer is irradiated with active light through a mask pattern to photocure the photosensitive resin composition layer in the irradiated portion. Examples of active light include ultraviolet light, visible light, electron beams, and X-rays, and ultraviolet light is particularly preferred. The irradiation dose of ultraviolet light is about 10 mJ / cm. 2 ~1000mJ / cm 2 The exposure method includes a contact exposure method in which a mask pattern is closely attached to a printed wiring board, and a non-contact exposure method in which exposure is performed using parallel light without closely attaching the mask pattern to the printed wiring board, and either method may be used. In addition, when a support is present on the photosensitive resin composition layer, exposure may be performed from above the support, or after peeling off the support.

[0114] The solder resist has excellent resolution because it uses the photosensitive resin composition of the present invention. Therefore, as the exposure pattern in the mask pattern, for example, a pattern in which the ratio (L / S) of the circuit width (line; L) to the width between circuits (space; S) is 100 μm / 100 μm or less (i.e., wiring pitch is 200 μm or less), L / S=80 μm / 80 μm or less (wiring pitch is 160 μm or less), L / S=70 μm / 70 μm or less (wiring pitch is 140 μm or less), or L / S=60 μm / 60 μm or less (wiring pitch is 120 μm or less) can be used. Note that the pitch does not need to be the same over the entire circuit board.

[0115] <Developing process> After the exposure step, if a support is present on the photosensitive resin composition layer, the support is removed, and then the non-photocured portion (unexposed portion) is removed and developed by wet development or dry development, whereby a pattern can be formed.

[0116] In the case of the wet development, a developer that is safe, stable, and easy to operate, such as an alkaline aqueous solution, a water-based developer, or an organic solvent, is used, and among them, a development process using an alkaline aqueous solution is preferred. As a development method, a known method such as spraying, rocking immersion, brushing, or scraping is appropriately adopted.

[0117] Examples of alkaline aqueous solutions used as the developer include aqueous solutions of alkali metal hydroxides such as lithium hydroxide, sodium hydroxide, and potassium hydroxide; carbonates or bicarbonates such as sodium carbonate and sodium bicarbonate; alkali metal phosphates such as sodium phosphate and potassium phosphate; and alkali metal pyrophosphates such as sodium pyrophosphate and potassium pyrophosphate; and aqueous solutions of organic bases that do not contain metal ions, such as tetraalkylammonium hydroxide. An aqueous solution of tetramethylammonium hydroxide (TMAH) is preferred because it does not contain metal ions and does not affect the semiconductor chip.

[0118] To improve the development effect, surfactants, antifoaming agents, etc. may be added to these alkaline aqueous solutions. The pH of the alkaline aqueous solution is, for example, preferably in the range of 8 to 12, more preferably in the range of 9 to 11. The base concentration of the alkaline aqueous solution is preferably 0.1% by mass to 10% by mass. The temperature of the alkaline aqueous solution can be appropriately selected according to the developability of the photosensitive resin composition layer, but is preferably 20°C to 50°C.

[0119] Examples of organic solvents used as developers include acetone, ethyl acetate, alkoxyethanol having an alkoxy group having 1 to 4 carbon atoms, ethyl alcohol, isopropyl alcohol, butyl alcohol, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, and diethylene glycol monobutyl ether.

[0120] The concentration of such an organic solvent is preferably 2% by mass to 90% by mass based on the total amount of the developer. The temperature of such an organic solvent can be adjusted according to the developability. Furthermore, such an organic solvent can be used alone or in combination of two or more kinds. Examples of organic solvent-based developers used alone include 1,1,1-trichloroethane, N-methylpyrrolidone, N,N-dimethylformamide, cyclohexanone, methyl isobutyl ketone, and γ-butyrolactone.

[0121] In forming a pattern, two or more of the above-mentioned developing methods may be used in combination as necessary. The developing methods include a dip method, a bath method, a spray method, a high-pressure spray method, brushing, slapping, etc., and the high-pressure spray method is suitable for improving resolution. When adopting a spray method, the spray pressure is preferably 0.05 MPa to 0.3 MPa.

[0122] <Thermal curing (post-bake) process> After the development step, a thermal curing (post-baking) step is performed to form a solder resist. Examples of the post-baking step include an ultraviolet ray irradiation step using a high-pressure mercury lamp and a heating step using a clean oven. When ultraviolet rays are irradiated, the amount of irradiation can be adjusted as necessary, for example, 0.05 J / cm. 2 ~10J / cm 2 The heating conditions may be appropriately selected depending on the type and content of the resin component in the photosensitive resin composition, but are preferably selected within the range of 150°C to 220°C for 20 minutes to 180 minutes, and more preferably 160°C to 200°C for 30 minutes to 120 minutes.

[0123] <Other processes> After the solder resist is formed, the printed wiring board may further include a drilling step and a desmearing step, which may be carried out according to various methods used in the manufacture of printed wiring boards and known to those skilled in the art.

[0124] After the solder resist is formed, via holes and through holes are formed in the solder resist formed on the circuit board by a drilling process, if desired. The drilling process can be performed by a known method such as a drill, a laser, or plasma, or by a combination of these methods if necessary, but a drilling process using a laser such as a carbon dioxide laser or a YAG laser is preferred.

[0125] The desmear process is a process of performing a desmear treatment. Generally, resin residue (smear) adheres to the inside of the opening formed in the hole drilling process. Since such smear can cause poor electrical connection, a process of removing the smear (desmear treatment) is performed in this process.

[0126] The desmear treatment may be performed by a dry desmear treatment, a wet desmear treatment, or a combination thereof.

[0127] The dry desmear treatment may be, for example, a desmear treatment using plasma. The desmear treatment using plasma may be performed using a commercially available plasma desmear treatment device. Among the commercially available plasma desmear treatment devices, examples suitable for use in the manufacture of printed wiring boards include a microwave plasma device manufactured by Nissin Co., Ltd. and an atmospheric pressure plasma etching device manufactured by Sekisui Chemical Co., Ltd.

[0128] The wet desmear treatment may be, for example, a desmear treatment using an oxidizing agent solution. When the desmear treatment is performed using an oxidizing agent solution, it is preferable to perform a swelling treatment using a swelling liquid, an oxidation treatment using an oxidizing agent solution, and a neutralization treatment using a neutralizing liquid in this order. Examples of the swelling liquid include "Swelling Dip Securigance P" and "Swelling Dip Securigance SBU" manufactured by Atotech Japan. The swelling treatment is preferably performed by immersing a substrate on which via holes or the like are formed in a swelling liquid heated to 60°C to 80°C for 5 to 10 minutes. The oxidizing agent solution is preferably an alkaline permanganate solution, and examples of the solution include a solution in which potassium permanganate or sodium permanganate is dissolved in an aqueous solution of sodium hydroxide. The oxidation treatment using an oxidizing agent solution is preferably performed by immersing a substrate after the swelling treatment in an oxidizing agent solution heated to 60°C to 80°C for 10 to 30 minutes. Commercially available alkaline permanganate aqueous solutions include, for example, "Concentrate Compact CP" and "Dosing Solution Securiganth P" manufactured by Atotech Japan. The neutralization treatment using a neutralizing solution is preferably carried out by immersing the substrate after the oxidation treatment in the neutralizing solution at 30°C to 50°C for 3 to 10 minutes. The neutralizing solution is preferably an acidic aqueous solution, and a commercially available product thereof is, for example, "Reduction Solution Securiganth P" manufactured by Atotech Japan.

[0129] When the dry desmear treatment and the wet desmear treatment are performed in combination, the dry desmear treatment may be performed first, or the wet desmear treatment may be performed first.

[0130] When the insulating layer is used as an interlayer insulating layer, it can be carried out in the same manner as in the case of a solder resist, and after the thermal curing step, a hole drilling step, a desmearing step, and a plating step may be carried out.

[0131] The plating process is a process of forming a conductor layer on an insulating layer. The conductor layer may be formed by a combination of electroless plating and electrolytic plating, or a plating resist having a reverse pattern to the conductor layer may be formed and the conductor layer may be formed only by electroless plating. Subsequent pattern formation methods may include, for example, subtractive methods and semi-additive methods known to those skilled in the art.

[0132] [Semiconductor Devices] The semiconductor device of the present invention includes a printed wiring board. The semiconductor device of the present invention can be manufactured using the printed wiring board of the present invention.

[0133] Examples of the semiconductor device include various semiconductor devices used in electric appliances (for example, computers, mobile phones, digital cameras, and televisions) and vehicles (for example, motorcycles, automobiles, trains, ships, and aircraft).

[0134] The semiconductor device of the present invention can be manufactured by mounting a component (semiconductor chip) on a conductive portion of a printed wiring board. The "conductive portion" refers to a portion of a printed wiring board that transmits an electric signal, and the portion may be either on the surface or embedded. The semiconductor chip is not particularly limited as long as it is an electric circuit element made of semiconductor material.

[0135] The method of mounting the semiconductor chip when manufacturing the semiconductor device of the present invention is not particularly limited as long as the semiconductor chip functions effectively, but specific examples include a wire bonding mounting method, a flip chip mounting method, a mounting method using a bumpless buildup layer (BBUL), a mounting method using an anisotropic conductive film (ACF), a mounting method using a non-conductive film (NCF), etc. Here, the "mounting method using a bumpless buildup layer (BBUL)" refers to "a mounting method in which a semiconductor chip is directly embedded in a recess in a printed wiring board and the semiconductor chip is connected to the wiring on the printed wiring board." EXAMPLES

[0136] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the following description, the terms "parts" and "%" used to express amounts refer to "parts by mass" and "% by mass", respectively, unless otherwise specified.

[0137] (Synthesis Example 1: Synthesis of Resin (A-1)) In a four-neck flask, 60.8 parts (0.26 mol) of bisphenol A, 43.4 parts (0.11 mol) of bisphenol A type epoxy compound (YD8125, manufactured by Nippon Steel Chemical Co., Ltd.), 145.8 parts (0.13 mol) of polyethylene glycol diglycidyl ether (EX861, manufactured by Nagase ChemteX Corporation), 1.25 parts of triphenylphosphine as a catalyst, 1.25 parts of N,N-dimethylbenzylamine, and 250 parts of toluene as a solvent were charged, and the mixture was heated to 110 ° C. while stirring under a nitrogen stream and reacted for 8 hours to obtain a hydroxyl group-containing resin. Next, 49.8 parts (0.48 mol) of succinic anhydride (Rikacid SA, manufactured by New Japan Chemical Co., Ltd.) was charged as an acid anhydride and reacted for 4 hours at 110 ° C. After confirming the absorption and disappearance of the acid anhydride group by FT-IR measurement, it was cooled to room temperature. Next, 41.1 parts (0.29 mol) of glycidyl methacrylate (GMA, manufactured by NOF Corp.) and 0.17 parts of hydroquinone as a polymerization inhibitor were added while stirring, and the mixture was reacted at 80°C for 8 hours. After the reaction was completed, 26.0 parts (0.25 mol) of Rikacid SA (manufactured by New Japan Chemical Co., Ltd.: succinic anhydride) were added as an acid anhydride, and the mixture was reacted at 80°C for 4 hours. After confirming that the absorption of the acid anhydride group had disappeared by FT-IR measurement, the mixture was cooled to room temperature. Methyl ethyl ketone was added to this solution to adjust the solid content to 50%. The weight average molecular weight of the obtained resin (A-1) was 20000, and the acid value of the resin solid content was 70 mgKOH / g.

[0138] Resin (A-1) is a copolymer. Therefore, M in formula (1) is AO Specifically, it was calculated as follows. The monomer having an alkylene oxide chain is polyethylene glycol diglycidyl ether (EX861). Since the molecular weight of EX861 is 1098, A in formula (2) is 1098. In addition, since the molecular weight of the alkylene oxide chain is 968, A in formula (2) is AO is 968. Resin (A-1) is a copolymer of bisphenol A, a bisphenol A type epoxy compound, polyethylene glycol diglycidyl ether, succinic anhydride, and glycidyl methacrylate. Since the monomer containing an alkylene oxide chain is polyethylene glycol diglycidyl ether, B in formula (2) AO is 0.13. Also, B in formula (2) is 0.26 + 0.11 + 0.13 + 0.48 + 0.29 + 0.25 = 1.52. Therefore, equation (2) becomes (968 / 1098) × (0.13 / 1.52) ≒ 0.08.

[0139] (Synthesis Example 2: Synthesis of Polymer 1) 510 g of propylene glycol monomethyl ether acetate, 50 g of methyl methacrylate, 90 g of butyl methacrylate, 60 g of hydroxyethyl methacrylate, and 2 g of azobisisobutyronyl were added to a four-neck flask, and the mixture was heated at 80° C. for 6 hours while blowing in nitrogen gas. The weight average molecular weight of the obtained polymer 1 was 40,000.

[0140] (Preparation of Resin Varnish) The resin materials were mixed as shown in the following recipe, and a resin varnish was obtained using a high-speed rotating mixer. [Table 1]

[0141] The abbreviations in the table are as follows: (A-1): Resin (A-1) synthesized in Synthesis Example 1, methyl ethyl ketone solution with a solid content of 50%, M AO ×100=8 ZFR-1491H: bis-F skeleton-containing acid-modified epoxy acrylate, manufactured by Nippon Kayaku Co., Ltd., EDGAc (ethyl diglycol acetate) cut, solid content 70%, M AO ×100=0 ZAR-2000: bis-A skeleton-containing acid-modified epoxy acrylate, manufactured by Nippon Kayaku Co., Ltd., EDGAc cut, solid content 70%, M AO ×100=0 EX-821: Polyethylene glycol diglycidyl ether, n=4, epoxy equivalent 185, Nagase ChemteX Corporation, M AO ×100=58 EX-920: Polypropylene glycol diglycidyl ether, n=3, epoxy equivalent 176, Nagase Chemtex Corporation) AO ×100=57 NC3000H: Biphenyl type epoxy resin (manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent: approx. 272), M AO ×100=0 R-551: EO modified bisphenol A type acrylate, manufactured by Nippon Kayaku Co., Ltd., M AO ×100=34 A-PTMG-65: Polytetramethylene glycol #650 diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd., M AO ×100=83 1.9ND-A: 1.9-nonanediol diacrylate, manufactured by Kyoeisha Chemical Co., Ltd., M AO ×100=0 NCI-831: Oxime ester photoinitiator, manufactured by ADEKA Corporation. EP4-A: Aminosilane-treated magnesium hydroxide (manufactured by Konoshima Chemical Co., Ltd.) MEK: Methyl ethyl ketone, manufactured by Junsei Chemical Co., Ltd. Polymer 1: Polymer 1 synthesized in Synthesis Example 2, propylene glycol monomethyl ether acetate solution with a solid content of 25%, M AO ×100=8

[0142] Shin-Nakamura Chemical's "A-PTMG-65" has the following structural formula: A-PTMG-65 is not a copolymer, so according to formula (1), M AO asked for. [ka] The molecular weight of A-PTMG-65 is 774. The molecular weight of the alkylene oxide chain is 648 (72×9=648). Therefore, M AO is 648 / 774 ≒ 0.83.

[0143] X in the formula (1) of Example 1 was determined as follows. X={(2.5÷55)×58}+{(7÷55)×34}+{(3÷55)×83}≒11.5

[0144] (Preparation of a photosensitive film with a support) A PET film (Toray Industries, Inc., "Lumirror T6AM", thickness 38 μm, softening point 130° C., "release PET") that had been release-treated with an alkyd resin-based release agent (Lintec Corporation, "AL-5") was prepared as a support. The prepared resin varnish was uniformly applied to the release PET with a die coater so that the thickness of the photosensitive resin composition layer after drying was 25 μm, and the film was dried at 80° C. to 120° C. to obtain a photosensitive film with a support.

[0145] (Formation of Laminate for Evaluation) The copper layer of a glass epoxy board (copper-clad laminate) on which a circuit patterned with a copper layer having a thickness of 18 μm was formed was roughened by treatment with a surface treatment agent containing an organic acid (CZ8100, manufactured by MEC Co., Ltd.). Next, the photosensitive resin composition layer of the photosensitive film with the support obtained in the examples and comparative examples was arranged so as to be in contact with the surface of the copper layer, and laminated using a vacuum laminator (manufactured by Nikko Materials Co., Ltd., VP160) to form a laminate in which the copper-clad laminate, the photosensitive resin composition layer, and the support were laminated in this order. The pressure bonding conditions were a vacuum drawing time of 30 seconds, a pressure bonding temperature of 80° C., a pressure bonding pressure of 0.7 MPa, and a pressure application time of 30 seconds. The laminate was left at room temperature for 30 minutes or more, and exposed to ultraviolet light from above the support of the laminate using a pattern forming device using a round hole pattern. The exposure pattern used was a quartz glass mask that drew an opening: 50μm / 60μm / 70μm / 80μm / 90μm / 100μm round hole (via), L / S (line / space): 50μm / 50μm, 60μm / 60μm, 70μm / 70μm, 80μm / 80μm, 90μm / 90μm, 100μm / 100μm line and space, and a 1cm×2cm square. After leaving it at room temperature for 30 minutes, the support was peeled off from the laminate. A 1% by mass aqueous solution of sodium carbonate at 30°C was used as a developer on the entire surface of the insulating layer on the laminate for 2 minutes for spray development at a spray pressure of 0.2MPa. After spray development, 1J / cm 2 The laminate was then subjected to ultraviolet irradiation for 100 s, and then to a heat treatment at 180° C. for 30 minutes to form an insulating layer having an opening on the laminate. This was used as a laminate for evaluation.

[0146] <Evaluation of via bottom residue> The evaluation was performed according to the following criteria for a 100 μm round hole formed in the evaluation laminate. ○: No residue. ×: Residue is observed, or the film is peeled off or the resin is partially dissolved.

[0147] <Evaluation of flexibility> The photosensitive resin composition layer of the photosensitive film with the support obtained in the examples and comparative examples was exposed to light, developed, and heated. The conditions of exposure, development, and heat treatment were the same as those for forming the laminate for evaluation. The support was peeled off to obtain a cured film. This cured film was cut to 15 mm x 110 mm, and its bending property was evaluated using an MIT folding fatigue tester (manufactured by Toyo Seiki Co., Ltd.). The test was performed in accordance with JIS P8115, with tension: 500 g, test speed: 175 times / min, folding angle: 135°, and bending clamp R: 0.38 mm. The number of foldings until breakage was counted, and the average of the three folding times was evaluated according to the following criteria. ◎: 300 times or more ○: 100 to less than 300 times ×: Less than 100 times

[0148] <Evaluation of copper adhesion> A rolled copper foil (JX Nippon Mining & Metals, BHY-22B-T, thickness 18 μm) was prepared by washing with 10% sulfuric acid and drying. A photosensitive film with a support was attached to the shiny side of the rolled copper foil, and the entire surface was exposed to light, developed, and heated to obtain a substrate. The conditions for exposure, development, and heat treatment were the same as those for the evaluation of flexibility. The insulating layer side of the obtained substrate was joined to a glass epoxy substrate, and the peel strength of the copper foil was measured using a tensile tester (TSE, "AC-50C-SL") conforming to the Japanese Industrial Standards (JIS C6481), and evaluated according to the following criteria. ○: Adhesion strength is 0.5kgf or more ×: Adhesion strength is less than 0.5kgf

[0149] <Evaluation of insulation (HHBT)> A comb-shaped wiring pattern with L (wiring width) / S (spacing) = 20 μm / 20 μm was used on the support of the photosensitive film with a support, and the entire surface was exposed to ultraviolet light, developed, and heated. The conditions for the entire surface exposure, development, and heat treatment were the same as those for forming the laminate for evaluation. Copper wires were soldered as electrodes on both sides of the comb-shaped wiring pattern, and a voltage of 50 V was applied at 85°C and 85% RH. The resistance value (Ω) was measured after 500 hours, and the average value was calculated from the resistance values ​​at seven points and evaluated according to the following criteria. ○: The average resistance value is 10 8 Ω or more ×: The average resistance value is 10 8 Less than Ω

[0150] From the results in the above table, it was found that the use of the photosensitive resin composition of the present invention results in good developability, flexibility, adhesion, and insulation. In Comparative Example 3, an acrylic polymer having an alkylene oxide chain (Polymer 1) is used, but since Polymer 1 is a thermoplastic resin, it is not incorporated into the curing system, and therefore it is believed that the desired results were not obtained.

[0151] In each example, it has been confirmed that even when components (E) and (F) are not contained, the results are similar to those of the above examples, although to different degrees.

Claims

1. (A) a resin containing an ethylenically unsaturated group and a carboxyl group, (B) an epoxy resin, (C) a photopolymerizable monomer, and (D) a photopolymerization initiator; The weight average molecular weight of the component (A) is 2,000 or more and 50,000 or less, The component (A) contains an acid-modified unsaturated epoxy ester resin, A photosensitive resin composition, wherein any one of the components (A), (B), and (C) contains an alkylene oxide chain represented by the following formula (a), and a parameter X represented by the following formula (1) is 4 or more and 25 or less. 【number】 In formula (a), each R independently represents an alkylene group having 1 to 6 carbon atoms, and q represents an integer of 2 to 100. [0010] In formula (1), M AO represents the value shown by the following formula (2) when the component containing an alkylene oxide chain is a copolymer, or represents (the molecular weight of the alkylene oxide chain of each compound contained in components (A) to (C)) / (the molecular weight of each compound contained in components (A) to (C)) when the component containing an alkylene oxide chain is not a copolymer. N represents the solids content (parts by mass) of all compounds contained in components (A) to (C), and n represents the solids content (parts by mass) of each compound contained in components (A) to (C). [0025] In formula (2), A AO represents the molecular weight of the alkylene oxide chain of each monomer containing an alkylene oxide chain, A represents the molecular weight of each monomer containing an alkylene oxide chain, B AO represents the number of moles of each monomer containing an alkylene oxide chain, and B represents the total number of moles of all monomers contained in the copolymer.

2. (A) a resin containing an ethylenically unsaturated group and a carboxyl group, (B) an epoxy resin, (C) a photopolymerizable monomer, and (D) a photopolymerization initiator; The weight average molecular weight of the component (A) is 2,000 or more and 50,000 or less, The component (B) contains an epoxy resin having a biphenyl skeleton, Any one of the components (A), (B), and (C) contains an alkylene oxide chain represented by the following formula (a), and a parameter X represented by the following formula (1) is 4 or more and 25 or less. 【number】 In formula (a), each R independently represents an alkylene group having 1 to 6 carbon atoms, and q represents an integer of 2 to 100. [0030] In formula (1), M AO represents the value shown by the following formula (2) when the component containing an alkylene oxide chain is a copolymer, or represents (the molecular weight of the alkylene oxide chain of each compound contained in components (A) to (C)) / (the molecular weight of each compound contained in components (A) to (C)) when the component containing an alkylene oxide chain is not a copolymer. N represents the solids content (parts by mass) of all compounds contained in components (A) to (C), and n represents the solids content (parts by mass) of each compound contained in components (A) to (C). [0045] In formula (2), A AO represents the molecular weight of the alkylene oxide chain of each monomer containing an alkylene oxide chain, A represents the molecular weight of each monomer containing an alkylene oxide chain, B AO represents the number of moles of each monomer containing an alkylene oxide chain, and B represents the total number of moles of all monomers contained in the copolymer.

3. The photosensitive resin composition according to claim 2 , wherein the component (A) comprises an acid-modified unsaturated epoxy ester resin.

4. The photosensitive resin composition according to any one of claims 1 to 3, wherein the component (A) comprises an acid-modified epoxy (meth)acrylate.

5. The photosensitive resin composition according to any one of claims 1 to 4, wherein the component (A) comprises any one of an acid-modified naphthalene skeleton-containing epoxy (meth)acrylate and an acid-modified bisphenol skeleton-containing epoxy (meth)acrylate.

6. The photosensitive resin composition according to claim 5 , wherein the acid-modified bisphenol skeleton-containing epoxy (meth)acrylate has either a bisphenol A skeleton or a bisphenol F skeleton.

7. The photosensitive resin composition according to any one of claims 1 to 6, further comprising (E) an inorganic filler.

8. 8. The photosensitive resin composition according to claim 1, wherein the alkylene oxide chain is contained in either the component (B) or the component (C).

9. The photosensitive resin composition according to any one of claims 1 to 8, wherein the component (D) comprises an oxime ester-based photopolymerization initiator.

10. The photosensitive resin composition according to any one of claims 1 to 9, wherein the content of the component (C) is 0.5 mass% to 10 mass% when the total solid content of the photosensitive resin composition is 100 mass%.

11. A photosensitive film comprising the photosensitive resin composition according to any one of claims 1 to 10.

12. A supported photosensitive film comprising a support and a photosensitive resin composition layer provided on the support, the photosensitive resin composition layer comprising the photosensitive resin composition according to any one of claims 1 to 10.

13. A printed wiring board comprising an insulating layer formed from a cured product of the photosensitive resin composition according to any one of claims 1 to 10.

14. The printed wiring board according to claim 13 , wherein the insulating layer is a solder resist.

15. A semiconductor device comprising the printed wiring board according to claim 13 or 14.

Citation Information

Patent Citations

  • Colored curable composition, color filter, and method for producing color filter

    JP2010244028A

  • Photosensitive adhesive composition, method for manufacturing laminated body or solid-state imaging element using the composition, and solid-state imaging element

    JP2012042601A

  • Flattening film and electronic component including the same

    JP2013187279A

  • Photosensitive element, solder resist and printed wiring board using photosensitive resin composition

    JP2014115672A