Guidewires

The guidewire's solid-phase bonding of Ni-Ti alloy wires with a controlled grain size distribution and protrusion design addresses the issue of joint weakness, ensuring robust navigation through complex vessels.

JP7557528B2Active Publication Date: 2024-09-27TERUMO KK
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022511673
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-03-30
Filing Date
2021-03-01
Publication Date
2024-09-27
Estimated Expiration
2041-03-01

AI Technical Summary

Technical Problem

Existing guidewires face issues with insufficient bonding strength at the joint, leading to potential bending during use in complex blood vessels, compromising navigation and safety.

Method used

A guidewire design where a first wire and a second wire made of Ni-Ti alloy are solid-phase bonded, with a specific grain size distribution and joint structure to enhance bonding strength, including a protrusion to increase the joint area and reduce stress concentration.

Benefits of technology

The improved bonding strength reduces the risk of guidewire bending within blood vessels, enhancing navigation and safety by maintaining structural integrity under stress.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007557528000007
    Figure 0007557528000007
  • Figure 0007557528000005
    Figure 0007557528000005
  • Figure 0007557528000006
    Figure 0007557528000006
Patent Text Reader

Abstract

The present invention provides a guide wire, bonding strength of which is increased. Provided is a guide wire in which a first wire and a second wire are subjected to solid phase bonding. The first wire and the second wire are made of a Ni-Ti-based alloy. In a count-reference grain size distribution of a crystal grain of a metallic structure of a bonding surface of the first wire and the second wire, when a section of a crystal grain size is set to 1 μm, a frequency of the crystal grain having a mode grain size is 25% or more, and a frequency of the crystal grain having a crystal grain size, a representative diameter of which is (mode grain size (μm) - 1 μm) or more and (mode grain size (μm) + 1 μm) or less is 60% or more.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a guidewire. [Background technology]

[0002] A guidewire is a long medical device that is inserted into a blood vessel to guide a catheter or a stent for intravascular treatment to a target location.

[0003] A guidewire needs to travel through complex curves and branches in blood vessels and pass through stenosis. Therefore, the guidewire needs to have low bending rigidity at the side inserted into the blood vessel (distal end) to improve blood vessel selectivity and safety, and high bending rigidity at the side operated by the surgeon (base end) to ensure pushability and torque transmission. Thus, a guidewire is known in which wires made of metals with different thicknesses and material properties are joined together to form a single core wire so that the distal end and proximal end have different properties (for example, Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2013 / 100045 Summary of the Invention

[0005] When a guidewire advances through a blood vessel, it curves to match the shape of the blood vessel, and when passing through a stenosis, it is pushed, pulled, and rotated by the surgeon. Therefore, a guidewire joined with a metal wire needs to have sufficient joint strength at the joint. If the joint strength is insufficient, there is a risk that the guidewire will bend at the joint while being used in the blood vessel.

[0006] The present invention has been made to solve the above-mentioned problems, and an object of the present invention is to provide a guidewire with improved bonding strength.

[0007] The present invention is a guidewire formed by solid-state bonding of a first wire and a second wire, the first wire and the second wire being made of a Ni-Ti alloy, and in the number-based grain size distribution of crystal grains in the metal structure of the bonding surface between the first wire and the second wire, when the grain size section is set to 1 μm, the frequency of the mode grain size is 25% or more, and the frequency of the representative diameter being equal to or greater than (mode grain size (μm) - 1 μm) and equal to or less than (mode grain size (μm) + 1 μm) is 60% or more.

[0008] According to the present invention, in a guidewire having a joint where a first wire and a second wire are joined, the joint strength of the joint is improved, which can reduce the risk of the guidewire bending inside a blood vessel. [Brief description of the drawings]

[0009] [Figure 1] 1 is a partial longitudinal cross-sectional view showing a guidewire 10 (a cross-sectional view taken along the longitudinal direction of the guidewire 10). [Diagram 2] FIG. 2 is a graph showing particle size distribution in Example 1. [Diagram 3] FIG. 1 shows the particle size distribution of Example 2. [Figure 4] FIG. 2 is a graph showing the particle size distribution of Comparative Example 1. [Diagram 5] FIG. 13 is a graph showing the particle size distribution of Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment of the present invention will be described with reference to the attached drawings. Note that the present invention is not limited to the following embodiment. Note that in the description of the drawings, the same elements are given the same reference numerals, and duplicated description will be omitted. Also, the dimensional ratios in the drawings are exaggerated for the convenience of description, and may differ from the actual ratios.

[0011] In the description of this specification, the direction in which the guidewire extends in its natural state (straight state without application of external force) is defined as the "longitudinal direction". In a cross section (cross section perpendicular to the axis) of the guidewire with the longitudinal direction of the guidewire as the reference axis, the direction moving away from or approaching the guidewire is defined as the "radial direction". The direction of rotation with the longitudinal direction of the guidewire as the reference axis is defined as the "circumferential direction". In addition, the side of the guidewire that is inserted into a blood vessel is defined as the distal end, and the end side opposite to the distal end is defined as the proximal end. In addition, a portion including a certain range from the distal end (top end) in the longitudinal direction is defined as the "tip portion", and a portion including a certain range from the proximal end (most proximal end) in the longitudinal direction is defined as the "proximal portion".

[0012] In this specification, the term "X to Y" indicating a range includes X and Y, and means "at least X and at most Y."

[0013] <Guidewire> FIG. 1 is a longitudinal cross-sectional view of a guidewire 10.

[0014] The guidewire 10 is inserted into a blood vessel and, in a state where it is inserted into the inner cavity (guidewire lumen) of a therapeutic or diagnostic catheter, is used to guide the catheter to a target site in the blood vessel. As shown in Fig. 1, the guidewire 10 according to the first embodiment includes a core wire 20 extending in the axial direction, a coil 30 and a tip-side coating layer (corresponding to a resin coating layer) 41 disposed at the tip portion of the core wire 20, a tubular member 50 disposed on the base end side of the tip-side coating layer 41, and a base-side coating layer 60 disposed at the base end portion of the core wire 20.

[0015] The length of the guidewire 10 along the longitudinal direction is not particularly limited, but may be, for example, 200 to 5000 mm.

[0016] (Core Wire) 1, the core wire 20 has a first wire 21 disposed on the distal side in the longitudinal direction, and a second wire 22 disposed on the proximal side of the first wire 21. The first wire 21 and the second wire 22 are solid-state joined via a joining surface d1 at a joint 37. The joint 37 has a protruding portion 70 protruding from the outer surface of the core wire 20 toward the radially outward side.

[0017] The first wire 21 has a distal end portion 36 disposed on the distal end side of the first wire 21, a first constant outer diameter portion 34 disposed on the proximal end side of the distal end portion 36, and a first tapered portion 35 disposed between the distal end portion 36 and the first constant outer diameter portion 34. The distal end portion 36 extends from the distal end of the first wire 21 to the distal end of the first tapered portion 35, and has a substantially constant outer diameter along the longitudinal direction. The first tapered portion 35 extends from the proximal end of the distal end portion 36 to the distal end of the first constant outer diameter portion 34, and the outer diameter gradually increases along the longitudinal direction. The first constant outer diameter portion 34 extends from the proximal end of the first tapered portion 35 to the distal end of the protruding portion 70, and has a substantially constant outer diameter along the longitudinal direction. The outer diameter of the first constant outer diameter portion 34 is 0.6 mm to 0.8 mm.

[0018] The second wire 22 has a second constant outer diameter portion 38 disposed on the distal end side of the second wire 22, a third constant outer diameter portion 40 disposed on the proximal end side of the second constant outer diameter portion 38, and a second tapered portion 39 disposed between the second constant outer diameter portion 38 and the third constant outer diameter portion 40. The second constant outer diameter portion 38 extends from the proximal end of the protruding portion 70 to the distal end of the second tapered portion 39, and has a substantially constant outer diameter along the longitudinal direction. The outer diameter of the second constant outer diameter portion 38 is substantially equal to the outer diameter of the first constant outer diameter portion 34 of the first wire 21, and is 0.6 mm to 0.8 mm. The second tapered portion 39 extends from the proximal end of the second constant outer diameter portion 38 to the distal end of the third constant outer diameter portion 40, and the outer diameter gradually increases along the longitudinal direction. The third constant outer diameter portion 40 extends from the proximal end of the second tapered portion 39 to the proximal end of the second wire 22, and has a substantially constant outer diameter along the longitudinal direction.

[0019] The core wire 20 is formed by solid-state bonding of the first wire 21 and the second wire 22. The first wire 21 and the second wire 22 can be formed by grinding metal wires having a certain outer diameter. The outer diameter of the second wire 22 before grinding is larger than the outer diameter of the first wire 21 before grinding. The core wire 20 is formed by grinding and then joining two wires having different outer diameters, so that the length that needs to be ground is shorter than when a single wire is ground. Therefore, by joining two wires having different outer diameters, the core wire 20 having a portion with low bending rigidity on the tip side and a portion with high bending rigidity on the base side can be easily manufactured. In the core wire 20, the outer diameter (mm) at a position 150 mm from the joining surface d1 to the base end side is, for example, 115% or more of the outer diameter (mm) at a position 150 mm from the joining surface d1 to the tip side.

[0020] The first wire 21 and the second wire 22 each have a substantially circular cross-sectional shape. However, the shapes of the first wire 21 and the second wire 22 are not limited to this. For example, the first wire 21 and the second wire 22 may have other tapered portions or constant outer diameter portions between the tip portion 36 and the first constant outer diameter portion 34 of the first wire 21, and between the second constant outer diameter portion 38 and the third constant outer diameter portion 40 of the second wire 22. The cross-sectional shape of the tip portion 36 of the first wire may be rectangular.

[0021] The first wire 21 and the second wire 22 are made of a Ni-Ti alloy. Since the Ni-Ti alloy has superelasticity, even if stress is applied and the Ni-Ti alloy is deformed to the plastic deformation region, the Ni-Ti alloy is likely to restore its original shape after the stress is removed. This prevents the guide wire 10 from being plastically deformed and bent during use, resulting in a decrease in operability. In addition, if the first wire 21 and the second wire 22 are made of the same material, the core wire 20 has a gradual change in physical properties from the first wire 21 including the joint 37 to the second wire 22, so that the joint strength of the joint 37 is easily obtained. In addition, since the physical properties of the first wire 21 and the second wire 22 are similar, the plastic deformation during solid-state joining is similar between the first wire 21 and the second wire 22, and the shape of the joint 37 is approximately symmetrical with the joint surface as the symmetry plane. As a result, when guidewire 10 is subjected to strong bending deformation, stress concentration on either first wire 21 or second wire 22 is alleviated, and thus the bonding strength against bending deformation is improved.

[0022] As the Ni-Ti based alloy, for example, the following formula (1):

[0023] [ka]

[0024] In the formula (1), A is an inevitable impurity, The alloy represented by the formula (1) is more preferably such that in the formula (1), 40≦x≦60, 40≦y≦60, and 0≦a≦1, and x+y+a=100, where x, y, and a represent values ​​in weight percent, and 30≦x≦70, 30≦y≦70, and 0≦a≦1, and x+y+a=100.

[0025] The joint 37 is a portion of the core wire 20 including a joint surface d1 between the first wire 21 and the second wire 22 and the vicinity of the joint surface d1. The joint 37 is formed by solid-state joining a base end surface of the wire forming the first wire 21 and a tip end surface of the wire forming the second wire 22.

[0026] Solid-state welding is one of the methods for directly joining two metal materials. In solid-state welding, the base metal is joined by plastic flow without melting. Solid-state welding is performed at a temperature below the melting point, and a molten part called a nugget is not formed on the joining surface. Therefore, it is possible to suppress the material properties near the joining surface from being significantly different from the material properties of the base material. That is, the core wire 20 solid-state bonds the first wire 21 and the second wire 22, so that the change in material properties near the joining portion 37 when viewed along the longitudinal direction is small. Another method for directly joining two metals is fusion welding. In fusion welding, a plurality of base metals are joined by heating, melting, and solidifying the base metal, so that a nugget is formed on the joining surface. The nugget and the metal near the joining surface are degenerated from the base material by the melting heat. For this reason, the material properties near the joining surface may be significantly different from the material properties of the base material. Solid-state welding and fusion welding can be distinguished by checking the presence or absence of a nugget on the joining surface of two metals with a scanning electron microscope.

[0027] The method of solid-phase joining the first wire 21 and the second wire 22 is not particularly limited, but examples thereof include friction joining, room temperature pressure joining, high temperature pressure joining, explosive joining, and electromagnetic pulse joining. In particular, as a method for joining metal wires having a small outer diameter, such as the first wire 21 and the second wire 22, it is preferable to use friction joining or high temperature pressure joining. In these joining methods, the base end surface of the first wire 21 and the tip end surface of the second wire 22 are brought into pressurized contact while being butted against each other in the axial direction, and heat is input to the contact portion of both wires. As a result, the first wire 21 and the second wire 22 are softened by an increase in temperature near the contact portion, and are compressed in the longitudinal direction and plastically deformed. At this time, the metal material near the contact portion between the first wire 21 and the second wire 22 is pushed outward in the radial direction by compression, and a burr is formed on the joining surface d1 in an amount corresponding to the amount of deformation during plastic deformation. When the heat input is stopped after the contact portion has risen to an appropriate temperature, the temperature of the first wire 21 and the second wire 22 in the vicinity of the contact portion drops, and solid-phase bonding is achieved. As a method of inputting heat to the contact portion of the first wire 21 and the second wire 22, for example, there is a method of rotating one of the first wire 21 and the second wire 22 so that the central axis becomes the rotation axis to generate frictional heat. Alternatively, there is a method of passing electricity through the contact portion of the first wire 21 and the second wire 22 to generate Joule heat. The amount of heat input can be controlled by adjusting the bonding conditions such as pressure, rotation speed, current, and the time for which they are applied. In general, in order to improve the bonding strength, a sufficient amount of heat input is required in the initial stage of bonding. However, if the amount of heat input becomes too large, the strength of the contact portion of the first wire 21 and the second wire 22 may decrease or melt due to the thermal effect. If the amount of heat input becomes too small, the contact portion between first wire 21 and second wire 22 will not be softened sufficiently and will not undergo sufficient plastic deformation, resulting in a decrease in joint strength.

[0028] The base end of the first wire 21 and the tip end of the second wire 22 to be used in the joining step are preferably made to have approximately the same outer diameter by processing such as grinding. When the first wire 21 and the second wire 22 are butted together, the positions of both wires are unlikely to shift at the joining surface d1, so that the central axis of the core wire 20 (the axis passing through approximately the center of the cross section of the core wire 20 and extending in the longitudinal direction) becomes approximately straight. The central axis of the core wire 20 approximately coincides with the central axis of the guide wire 10.

[0029] The base end surface of the first wire 21 used in the joining process is approximately perpendicular to the central axis of the first wire 21. The tip surface of the second wire 22 used in the joining process is approximately perpendicular to the central axis of the second wire 22. This makes it easy to form the base end surface of the first wire 21 and the tip surface of the second wire 22. Note that the base end surface of the first wire 21 and the tip surface of the second wire 22 used in the joining process may be inclined with respect to a plane perpendicular to the central axis of each wire, and may be a concave or convex surface.

[0030] Before the joining step, the base end surface of the first wire 21 and the tip end surface of the second wire 22 are preferably treated to remove any deposits or oxide film present on the end surfaces. Examples of the treatment method include polishing and acid treatment.

[0031] The joint 37 has a metal structure different from the first constant outer diameter portion 34 of the first wire 21 and the second constant outer diameter portion 38 of the second wire 22 adjacent to the joint 37 due to solid-state welding. In general, the metal structure observed in the first wire 21 and the second wire 22 before welding is fibrous (elliptical shape with the major axis in the major axis direction of each wire) parallel to the longitudinal direction of each wire. When the first wire 21 and the second wire 22 are solid-state welded, the metal structure in the vicinity of the joint surface d1 is significantly refined by the heat and pressure applied during welding, and a heat-affected zone is observed around it. The fibrous metal structure changes to a direction along the extrusion direction of the burr (diametrically outward) in the vicinity of the joint surface d1, or disappears. In this specification, when a longitudinal section including the central axis of core wire 20 is macroscopically observed with a scanning electron microscope (magnification of about 1000 times), a portion where the orientation of the fibrous metal structure changes from a direction parallel to the longitudinal direction of first wire 21 or second wire 22 is defined as joint 37. The length of joint 37 along the longitudinal direction is equal to the length of the heat-affected zone along the longitudinal direction.

[0032] The joint surface d1 is the surface where the base end surface of the first wire 21 and the tip surface of the second wire 22 come into contact. In this specification, when the position where the first wire 21 and the second wire 22 come into contact is clearly identifiable in observing the metal structure of the longitudinal section of the core wire 20 with a scanning electron microscope, the position is defined as the joint surface d1. When the fibrous metal structure disappears due to solid-state bonding and the joint surface d1 cannot be clearly identified, the center position of the joint 37 in the longitudinal direction of the core wire 20 is defined as the joint surface d1.

[0033] The bonding surface d1 formed by solid-state bonding is approximately perpendicular to the central axis of the core wire 20. Furthermore, at the bonding surface d1 of the guide wire 10, it is preferable that the central axis of the first wire 21 and the central axis of the second wire 22 approximately coincide with each other. Note that the bonding surface d1 may be inclined with respect to a plane perpendicular to the central axis of the core wire 20, and may be a concave or convex surface.

[0034] The metal structure of the joint surface d1 and its vicinity greatly affects the joint strength between the first wire 21 and the second wire 22. In order to improve the joint strength between the first wire 21 and the second wire 22, it is preferable that the metal structure near the joint surface d1 is uniform. The size of the crystal grains in the metal structure is correlated with the hardness of the metal, and the smaller the crystal grains, the higher the hardness. Therefore, if the uniformity of the metal structure is low, the joint surface d1 is prone to local stress concentration due to differences in hardness, and the joint strength decreases. In addition, the height of the burrs generated at the joint 37 of the solid-phase bonded core wire 20 may be adjusted by mechanical polishing. At this time, the core wire 20 with low uniformity of the metal structure near the joint surface d1 has an uneven hardness distribution at the joint surface d1, so that unintended unevenness is likely to occur on the outer surface after mechanical polishing. Such unevenness on the outer surface leads to local stress concentration, which is a factor in reducing the joint strength of the joint surface d1. In particular, in the case of the joint surface d1 between metal wires having a small outer diameter, such as the guide wire 10, the unevenness of the outer surface has a large effect on the joint strength.

[0035] The uniformity of the metal structure can be evaluated by the grain size distribution of the crystal grains in the metal structure. The grain size distribution of the crystal grains in the metal structure can be obtained by dividing the grains present in an arbitrary area (measurement target area) into several sections between the maximum diameter and the minimum diameter, and measuring the number and area of ​​the crystal grains in each section. In this specification, the grain size distribution in the vicinity of the joint surface d1 is expressed as a frequency distribution based on the number of grains of the crystal grains present in the measurement target area of ​​the obtained image by microscopically observing (at a magnification of about 5000 times) the longitudinal section including the intersection of the central axis of the core wire 20 and the joint surface d1 using a scanning electron microscope. The grain size is calculated as the diameter of each crystal grain when each crystal grain is assumed to be a perfect sphere, that is, a perfect circle in a two-dimensional plane, by calculating the area of ​​each crystal grain from an image showing the grain boundaries of the crystal grains using a crystal orientation / grain boundary microstructure automatic analyzer (OIM). The measurement target area of ​​the grain size distribution is 0.075 mm x 0.075 mm, centered on the intersection of the central axis of the core wire 20 and the joint surface d1. The intervals of the grain size in the grain size distribution are 1.00 μm. The grain size corresponding to the median of each interval is the representative diameter of the interval. In other words, the frequency of grains with a representative diameter of 0.05 μm in the grain size distribution indicates the ratio of the number of grains with a grain size measurement value of more than 0 μm and 1.00 μm or less to the total number of grains in the measurement target area.

[0036] The size of the crystal grains in the metal structure is correlated with the hardness. Therefore, the uniformity of the metal structure can also be evaluated by the hardness distribution. In order to increase the joint strength, it is preferable that the hardness of the metal near the joint surface d1 is uniform. In this specification, the hardness is a value obtained by measuring the test force and the indentation depth when the indenter is indented, and converting the indentation hardness obtained from the load-unload curve into a Vickers hardness equivalent value. The hardness at the joint surface d1 is the average value of five points measured on a vertical cross section including the intersection point between the central axis of the core wire 20 and the joint surface d1, two points at the intersection point, and two points at the positions 0.0625 mm and 0.125 mm outward in the radial direction from the intersection point along the joint surface d1. The hardness is measured to two decimal places.

[0037] In order to improve the joining strength between the first wire 21 and the second wire 22, it is preferable that the core wire 20 has a small change in hardness along the longitudinal direction from the first constant outer diameter portion 34 of the first wire 21 to the second constant outer diameter portion 38 of the second wire 22. Therefore, it is preferable that the metal structure near the joining surface d1 has a moderately large crystal grain size. The metal structure near the joining surface d1 is recrystallized and refined by the heat and pressure during solid-state joining. At the same time, the hardness of the joining portion 37 located around the joining surface d1 becomes lower than the hardness of the first wire 21 and the second wire 22 before solid-state joining due to the influence of heat. Therefore, if the proportion of fine crystal grains contained in the joining surface d1 is large, the joining portion 37 has a large change in hardness near the joining surface d1, and local stress concentration is likely to occur at the joining surface d1 and the boundary point of the hardness change. As a result, the core wire 20 experiences a large change in hardness along the longitudinal direction from the first constant outer diameter portion 34 of the first wire 21 to the second constant outer diameter portion 38 of the second wire 22, making it difficult to improve the bonding strength in a tensile test.

[0038] In the number-based grain size distribution of the crystal grains in the metal structure of the joining surface d1, the frequency of the mode grain size when the grain size section is 1 μm is 25% or more, and more preferably 28% or more. The mode grain size is the representative diameter (mode diameter) of the section with the highest frequency in the grain size distribution. By including 25% or more of crystal grains having the mode grain size, the joining surface d1 has a high uniformity of the metal structure. As a result, the joining surface d1 is less likely to experience local stress concentration due to differences in physical properties, and the joining strength is improved. In addition, in the number-based grain size distribution of the crystal grains in the metal structure of the joining surface d1, the upper limit of the frequency of the mode grain size is 100% or less, but is usually 40% or less.

[0039] In the number-based grain size distribution of the crystal grains in the metal structure of the joint surface d1, when the grain size section is 1 μm, the frequency of the representative diameter being (mode grain size (μm)-1 μm) or more and (mode grain size (μm)+1 μm) or less is preferably 60% or more, more preferably 62% or more. In other words, the total frequency of the frequency of the mode grain size section and the frequency of the two sections adjacent to the mode grain size section is preferably 60% or more, more preferably 62% or more. The joint surface d1 having such a grain size distribution has a higher uniformity of the metal structure. Therefore, the joint surface d1 is more unlikely to cause local stress concentration due to differences in physical properties, and the effect of improving the joint strength is greater. In addition, in the number-based grain size distribution of the crystal grains in the metal structure near the joint surface d1, the upper limit of the frequency of the mode grain size is 100% or less, but is usually 75% or less.

[0040] In the number-based grain size distribution of the crystal grains in the metal structure of the joint surface d1, the most frequent grain size when the grain size interval is 1 μm is preferably 2.50 μm or more. By reducing the ratio of fine crystal grains contained in the joint surface d1, the joint 37 can reduce the change in hardness near the joint surface d1. As a result, the core wire 20 has a smaller change in hardness along the long axis direction from the first constant outer diameter portion 34 of the first wire 21 to the second constant outer diameter portion 38 of the second wire 22, and the joint strength is further improved in the tensile test. In addition, the upper limit of the most frequent grain size is preferably 5.50 μm or less, and more preferably 3.50 μm or less. By reducing the ratio of coarse crystal grains contained in the joint surface d1, the hardness of the joint surface d1 does not decrease significantly, so that the joint surface d1 can obtain a high joint strength.

[0041] The standard deviation of hardness at the joining surface d1 is preferably 10.00 or less, and more preferably 9.00 or less. The standard deviation of hardness is an unbiased standard deviation measured at five points on the joining surface d1, and is calculated to two decimal places. When the standard deviation of hardness is 10.00 or less, the joining surface d1 has a high uniformity of metal structure. As a result, the joining surface d1 is less susceptible to local stress concentration due to differences in physical properties, and the joining strength is improved. In addition, the joining surface d1 has improved workability during mechanical polishing. The lower limit of the standard deviation of hardness at the joining surface d1 is 0, but it is usually 4.00 or more.

[0042] The metal structure of the joining surface d1 as described above can be obtained by appropriately controlling the amount of heat input, amount of heat dissipation, and amount of deformation at the contact portion between the first wire 21 and the second wire 22 during solid-state welding. The amount of heat input and amount of heat dissipation affect the degree of recrystallization and growth of crystal grains near the joining surface d1. The amount of deformation during plastic deformation affects the degree to which the refined crystal grains generated by solid-state welding remain near the joining surface d1. The amount of heat input, amount of heat dissipation, and amount of deformation can be controlled by adjusting various conditions of solid-state welding.

[0043] In solid-state welding, when Joule heat is used to input heat to the contact portion between the first wire 21 and the second wire 22, the amount of heat input, the amount of heat dissipation, and the amount of deformation can be controlled by the current value and the current flow time, since Joule heat is a function of resistance, current value, and current flow time. In particular, in solid-state welding of metal wires with small outer diameters, such as the first wire 21 and the second wire 22, in order to obtain a metal structure with high joint strength at the joint surface d1, it is important to control the current value for a certain period of time from the start of current flow to the start of deformation. When current flow starts, Joule heat is generated at the contact portion due to high contact resistance caused by fine irregularities present on the base end surface of the first wire 21 and the tip surface of the second wire 22. When the first wire 21 and the second wire 22 start to deform due to the generated Joule heat, the fine irregularities are crushed, the contact area between the first wire 21 and the second wire 22 increases, and the contact resistance decreases, so the amount of Joule heat generated decreases. At the same time, the deformation increases the contact area between the joining device and the first wire 21 or the second wire 22, so that the amount of heat dissipation from the contact portion increases. When a high current is applied in a short time in the initial stage of joining, the amount of heat input increases rapidly immediately after the start of current flow, but then decreases rapidly because the deformation proceeds at a high speed. At the same time, a rapid increase in the amount of heat dissipation due to deformation also occurs. As a result, the temperature rise at the contact portion stops in a short time, so the amount of deformation becomes small. On the other hand, when a low current is applied for a long time, the amount of heat input due to current flow is small, so the amount of deformation becomes small. In this way, the current value during a certain period of time from the start of current flow to the start of deformation affects both the amount of heat input and the amount of heat dissipation, and as a result, affects the amount of deformation. From the transition of the amount of deformation, it was possible to estimate that the time to reach the maximum temperature was 5 ms from the start of current flow. The specific current value is appropriately set in consideration of the outer diameter, composition, etc. of the first wire and the second wire, but the current value 5 ms from the start of current flow is preferably 10 A to 1000 A, and preferably more than 75 A and less than 300 A. This allows the core wire 20 to have a metal structure in which the joint surface d1 between the first wire 21 and the second wire 22 has high joint strength.

[0044] When Joule heat is used as a method for inputting heat to the contact portion between the first wire 21 and the second wire 22, the pressure when the base end surface of the first wire 21 and the tip surface of the second wire 22 are brought into pressurized contact is, for example, 50 MPa to 1000 MPa. Note that the pressure may be increased or decreased during the joining process as necessary.

[0045] In obtaining the metal structure of the joint surface d1 as described above, the deformation amount is preferably 0.80 mm or more, more preferably 1.00 mm or more. The upper limit of the deformation amount is not particularly limited, but is, for example, 1.50 mm or less. The deformation amount is the amount of displacement of the length in the major axis direction of the first wire 21 and the second wire 22 before and after solid-state bonding. If the deformation amount is small, the joint surface d1 is likely to have a local increase in hardness due to the extremely fine crystal grains generated by solid-state bonding remaining on the joint surface d1. On the other hand, if the amount of heat is increased to increase the deformation amount, the joint 37 is likely to have a decrease in hardness due to the heat effect.

[0046] (protrusion) In the embodiment of FIG. 1, the core wire 20 has a protrusion 70 at the joint 37, which is formed by mechanically polishing burrs generated on the joint surface d1. The protrusion 70 protrudes radially outward from the outer surface of the core wire 20. That is, the outer diameter of the protrusion 70 is larger than the outer diameter of the first constant outer diameter portion 34 of the first wire 21 and the outer diameter of the second constant outer diameter portion 38 of the second wire 22, which are disposed near the joint 37. The first wire 21 and the second wire 22 have an increased area of ​​the joint surface d1 due to the formation of the protrusion 70 at the joint 37 of both wires, thereby improving the joint strength. In addition, the increased outer diameter of the protrusion 70 can prevent the guide wire 10 from locally bending at the joint 37 when it receives forces from both the distal end and the proximal end simultaneously. The bending rigidity of the guide wire 10 can be expressed by Young's modulus and the second moment of area. The joint 37 has a lower hardness than the first constant outer diameter portion of the first wire 21 and the second constant outer diameter portion of the second wire 22, which are disposed near the joint 37, due to solid-state bonding. Assuming that the hardness and Young's modulus are in a directly proportional relationship, when the outer diameter of the joint 37 is substantially equal to the first constant outer diameter portion 34 and the second constant outer diameter portion 38 of the second wire 22, the bending rigidity of the guidewire 10 decreases at the joint 37. Therefore, when the guidewire 10 receives a compressive force in the longitudinal direction, only the joint 37 is likely to deform. By providing the protrusion 70, the joint 37 has a larger outer diameter than the first constant outer diameter portion 34 and the second constant outer diameter portion 38 of the second wire 22, and the moment of inertia of area is increased. As a result, the guidewire 10 having the protrusion 70 can suppress a decrease in bending rigidity at the joint 37 and prevent only the joint 37 from deforming. This allows the guidewire 10 to efficiently transmit to the first wire 21 the torque or pushing force applied to the proximal end of the second wire 22 by the surgeon.

[0047] The outer shape of the protrusion 70 is approximately trapezoidal in the longitudinal cross-sectional view of the guidewire 10. The joint surface d1 between the first wire 21 and the second wire 22 is located approximately at the center of the upper base of the trapezoid. In other words, the joint surface d1 between the first wire 21 and the second wire 22 is located at the maximum outer diameter portion of the protrusion 70. The outer shape of the protrusion 70 in the longitudinal cross-sectional view of the guidewire 10 is not limited to a trapezoid, and may be an arc or a polygon. The upper base of the trapezoid of the protrusion 70 observed in the longitudinal cross-sectional view of the guidewire 10 is not limited to a straight line, and may be a curved line.

[0048] The height of protrusion 70 is the distance between the maximum outer diameter part of the protrusion and the outer surface of first constant outer diameter part 34 of first wire 21 or second constant outer diameter part 38 of second wire 22. When the outer shape of protrusion 70 in longitudinal cross section of guidewire 10 is trapezoidal, the height of protrusion 70 is the distance between the upper base of the trapezoid and the outer surface of first wire 21 or second wire 22 that is parallel to the upper base of the trapezoid, and is preferably 0.001 mm to 0.200 mm, and more preferably 0.020 mm to 0.100 mm.

[0049] The maximum outer diameter (mm) of the first wire 21 excluding the protrusion 70 is 90% to 100% of the maximum outer diameter (mm) of the protrusion 70, and the maximum outer diameter (mm) of the second wire 22 excluding the protrusion 70 is 100% to 120% of the maximum outer diameter (mm) of the protrusion 70.

[0050] (coil) The coil 30 is disposed so as to cover a certain range of the tip of the first wire 21. The coil 30 is formed by spirally winding the wire around the first wire 21 in the circumferential direction of the first wire 21. It is preferable that the coil 30 and the outer surface of the first wire 21 are in close contact with each other. It is also preferable that the coil 30 is formed so as to have a gap between adjacent turns when no external force is applied. Note that the coil 30 may be formed so as not to have a gap between adjacent turns when no external force is applied.

[0051] The wire forming the coil 30 is preferably made of a material that is opaque to radiography, such as precious metals such as gold, platinum, and tungsten, or alloys containing these metals.

[0052] A tip end of the coil 30 is fixed to a tip portion of the first wire 21 by a fixing member 31. A base end of the coil 30 is fixed to a first tapered portion 35 of the first wire 21 by a fixing member 32. Examples of materials that form the fixing member include an adhesive, a brazing material, and a solder.

[0053] (Tip side coating layer) The distal covering layer 41 is made of a resin material and is formed so as to cover the distal end of the core wire 20 including the coil 30. The distal end of the distal covering layer 41 preferably has a rounded shape so as not to damage the blood vessel wall. The proximal end of the distal covering layer 41 is located at the first constant outer diameter portion 34 of the core wire 20 (first wire 21).

[0054] The distal covering layer 41 is preferably made of a highly flexible resin material. This makes the distal end of the guidewire 10 flexible, preventing damage to the inner wall of the blood vessel. Examples of resin materials for forming the distal covering layer 41 include polyolefins such as polyethylene and polypropylene, polyvinyl chloride, polyesters (PET, PBT, etc.), polyamides, polyimides, polystyrene, polycarbonates, silicone resins, fluorine-based resins (PTFE, ETFE, PFA, etc.), urethane-based resins, composite materials thereof, various rubber materials such as latex rubber and silicone rubber, and composite materials combining two or more of these materials. Of the above materials, it is more preferable to use urethane-based resins.

[0055] The thickness of the distal covering layer 41 is not particularly limited, but is preferably, for example, 5 μm to 500 μm. The distal covering layer 41 is not limited to a single-layer structure, and may be configured by laminating a plurality of layers.

[0056] The distal coating layer 41 is preferably covered with a hydrophilic coating layer (not shown), which reduces frictional resistance between the guidewire 10 and the blood vessel wall or the inner wall of the catheter into which the guidewire 10 is inserted, thereby improving operability.

[0057] The material for forming the hydrophilic coating layer is not particularly limited, but examples thereof include known hydrophilic substances such as cellulose-based polymer substances, polyethylene oxide-based polymer substances, maleic anhydride-based polymer substances (e.g., maleic anhydride copolymers such as methyl vinyl ether-maleic anhydride copolymer), acrylamide-based polymer substances (e.g., polyacrylamide, polyglycidyl methacrylate-dimethylacrylamide (PGMA-DMAA) block copolymers), water-soluble nylon, polyvinyl alcohol, and polyvinylpyrrolidone.

[0058] The thickness of the hydrophilic coating layer is not particularly limited, but is preferably, for example, 0.1 μm to 100 μm.

[0059] (Cylindrical member) The cylindrical member 50 is a tubular member disposed in the first constant outer diameter portion 34 of the first wire 21. The distal end of the cylindrical member is in contact with the proximal end of the distal coating layer 41, and the proximal end of the distal coating layer 41 enters the lumen of the cylindrical member 50. The proximal end of the cylindrical member 50 is fixed to the first wire 21 by a fixing member 51. The proximal end of the cylindrical member 50 has a tapered portion 52 whose outer diameter gradually decreases toward the proximal end. The fixing member 51, which is located closer to the proximal end than the proximal end of the cylindrical member 50, is tapered so as to be continuous with the tapered portion 52 of the cylindrical member 50.

[0060] The cylindrical member 50 is preferably made of a metal. Examples of metals that can be used to form the cylindrical member 50 include stainless steel, superelastic alloys, cobalt-based alloys, precious metals such as gold, platinum, and tungsten, and alloys containing these metals (platinum-iridium alloys).

[0061] (Proximal coating layer) 1, the base end covering layer 60 is formed so as to cover at least a portion of the outer surface of the second wire 22. The base end covering layer 60 has an inner layer 61 covering the outer surface of the second wire 22, an outer layer 62 covering the outer surface of the inner layer, and a filament 63 wound helically around the outer surface of the outer layer 62.

[0062] Examples of materials forming the inner layer 61 and the outer layer 62 include fluorine-based resins such as polytetrafluoroethylene (PTFE) and tetrafluoroethylene-ethylene copolymer (ETFE). The inner layer 61 and the outer layer 62 may also contain a pigment.

[0063] The proximal covering layer 60 is not limited to the above-mentioned configuration, and may be composed of, for example, one layer.

[0064] The filament 63 is a member that is wound in a spiral shape along the circumferential direction of the second wire 22 and has a convex shape extending radially outward from the outer surface of the outer layer 62. The filament 63 is formed such that adjacent windings are spaced apart. Due to this filament 63, the outer surface of the second wire 22 has a plurality of convex portions and concave portions formed between adjacent convex portions.

[0065] The filament 63 is preferably made of resin. The resin for forming the filament 63 may be a fluorine-based resin such as polytetrafluoroethylene (PTFE) or tetrafluoroethylene-hexafluoropropylene copolymer (FEP). The filament 63 may also contain a pigment.

[0066] The method of winding the filament 63 in a spiral shape on the outer surface of the outer layer 62 includes dipping and spotting. The dipping method is a method in which the second wire 22, in which a masking tape is spirally wound around a portion on the outer layer 62 where a recess is to be formed, is immersed in a solution containing a resin for forming the filament 63, dried, and then the masking tape is removed. The spotting method is a method in which the resin for forming the filament 63, which is dissolved in a solvent or in a molten state, is extruded linearly onto the outer surface of the outer layer 62 of the second wire 22, which moves in the longitudinal direction while rotating. The filament 63 may be fixed to the outer surface of the outer layer 62 by heating it to a temperature close to the melting point of the filament 63 after being wound around the outer surface of the outer layer 62. By these methods, the resin is applied in a spiral shape to the outer surface of the outer layer 62 of the second wire 22, and a linear body 63, which is a convex portion extending radially outward from the outer surface of the outer layer 62, is formed. In the vertical cross-sectional view of the second wire 22, each protrusion has an apex which is the most radially outwardly protruding position of the protrusion, a tip end located on the tip side of the apex, and a base end located on the base side of the apex, and the contour of the outer surface of the protrusion is a smooth arc connecting the tip end, the apex, and the base end. Note that the contour of the outer surface of the protrusion in the vertical cross-sectional view of the second wire 22 is not limited to an arc, and may be an elliptical arc, a triangle, or a rectangle.

[0067] The height of the protrusions is preferably 0.001 mm to 0.100 mm. Note that the height of the protrusions refers to the length of a perpendicular line drawn from the top of the protrusion to the outer surface of the outer layer 62 when the second wire 22 is viewed in vertical cross section. EXAMPLES

[0068] The effects of the present invention will be described with reference to the following examples and comparative examples. Unless otherwise specified, all operations were carried out at room temperature (15 to 29° C.).

[0069] Example 1 (Preparation of test specimens) Two wires made of Ni-Ti alloy with an outer diameter of 0.68 to 0.72 mm were prepared, and the ends of the wires were solid-phase bonded to each other. The composition of the Ni-Ti alloy was 55 to 56 wt % Ni and the remainder Ti. The two wires were arranged in an axially aligned state in a bonding device, and each wire was clamped and fixed. Then, the end faces of the two wires were pressed and contacted to each other, and electricity was passed through the bonding device. The two wires were softened and plastically deformed by heat generated at the contact point of the two wires, thereby being solid-phase bonded. The bonded wires had burrs protruding radially outward at the position where the two wires contacted due to plastic deformation caused by compression. The burrs were mechanically polished to obtain a wire with an outer diameter of 0.62 mm to 0.72 mm at the protruding part. The outer diameter was measured using a thickness gauge. The obtained wire was used as a test piece for the following evaluation. In Example 1, the current value at 5 ms from the start of current flow was 200 A.

[0070] In this embodiment and the comparative example, the current value 5 ms after the start of current flow was 75 to 300A.

[0071] Example 2 Two wires made of Ni-Ti alloy with an outer diameter of 0.68 to 0.72 mm were prepared, and the ends of the wires were solid-phase bonded to each other. The composition of the Ni-Ti alloy was 55 to 56 wt % Ni and the remainder Ti. The two wires were arranged in an axially aligned state in a bonding device, and each wire was clamped and fixed. Then, the end faces of the two wires were pressed and contacted to each other, and electricity was passed through the bonding device. The two wires were softened and plastically deformed by heat generated at the contact point of the two wires, thereby being solid-phase bonded. The bonded wires had burrs protruding radially outward at the position where the two wires contacted due to plastic deformation caused by compression. The burrs were mechanically polished to obtain a wire with an outer diameter of 0.62 mm to 0.72 mm at the protruding part. The outer diameter was measured using a thickness gauge. The obtained wire was used as a test piece for the following evaluation. In Example 2, the current value at 5 ms from the start of current flow was 100 A.

[0072] Comparative Example 1 Two wires made of Ni-Ti alloy with an outer diameter of 0.68 to 0.72 mm were prepared, and the ends of the wires were solid-phase bonded to each other. The composition of the Ni-Ti alloy was 55 to 56 wt % Ni and the remainder Ti. The two wires were arranged in an axially aligned state in a bonding device, and each wire was clamped and fixed. Then, the end faces of the two wires were pressed and contacted to each other, and electricity was passed through the bonding device. The two wires were softened and plastically deformed by heat generated at the contact point of the two wires, thereby being solid-phase bonded. The bonded wires had burrs protruding radially outward at the position where the two wires contacted due to plastic deformation caused by compression. The burrs were mechanically polished to obtain a wire with an outer diameter of the protruding part of 0.62 mm to 0.72 mm. The outer diameter was measured using a thickness gauge. The obtained wire was used as a test piece for the following evaluation. In Comparative Example 1, the current value at 5 ms from the start of current flow was 300 A.

[0073] Comparative Example 2 Two wires made of Ni-Ti alloy with an outer diameter of 0.68 to 0.72 mm were prepared, and the ends of the wires were solid-phase welded together. The composition of the Ni-Ti alloy was 55 to 56 wt % Ni and the remainder Ti. The two wires were arranged in an axially aligned state in a joining device, and each wire was clamped and fixed. Next, the end faces of the two wires were pressed together and electricity was passed through the joining device. The two wires were softened and plastically deformed by heat generated at the contact point of the two wires, thereby being solid-phase welded. The joined wires had burrs protruding radially outward at the position where the two wires contacted due to plastic deformation caused by compression. The burrs were mechanically polished to obtain a wire with an outer diameter of 0.62 mm to 0.72 mm at the protruding part. The outer diameter was measured using a thickness gauge. The obtained wire was used as a test piece for the following evaluation. In Comparative Example 2, the current value at 5 ms from the start of current flow was 75 A.

[0074] [Test example] (Deformation amount) The longitudinal distance between the two clamps that fixed the wire was recorded before and after solid-state bonding. The difference in the distance between the clamps before and after solid-state bonding was taken as the amount of deformation.

[0075] (Measuring the bonding strength) The bond strength of the test pieces, including the joint, was determined by a tensile test using an autograph (Shimadzu Corporation). The test pieces were fixed to the chucks at the top and bottom so that the joint was located in the center between the chucks. The upper part of the test piece was pulled, and the maximum test force until the test piece broke was taken as the bond strength of the test piece. The chuck distance (original gauge length) was 8 mm, and the test speed was 5 mm / min.

[0076] (Hardness measurement) The hardness of the test specimen was determined by a microindentation test specified in the international standard ISO14577-1. The test specimen, including the joint surface and its vicinity, was embedded in resin, then cut and polished to expose the longitudinal section including the central axis or the vicinity of the central axis of the test specimen. Using a dynamic ultra-microhardness tester (Shimadzu Corporation, DUH-211S), an indenter was pressed into a specified position on the longitudinal section according to ISO14577-1 (instrumented indentation hardness test) until the test force reached 65 μN, and the displacement-test force was recorded when the indenter was pulled up after holding the indenter for 5 seconds, and the indentation hardness (N / mm) obtained from the load-unload curve was used. 2 ) was multiplied by 0.0924 to calculate the value converted into a Vickers hardness equivalent value (HV*). A triangular pyramid indenter (edge ​​angle 115 degrees, Berkovich type) was used for the measurement. The hardness at the joint surface was measured on a vertical cross section including the intersection point between the central axis of the test piece and the joint surface, and the average value and unbiased standard deviation were calculated to two decimal places for five points measured at the intersection point, two points 0.0625 mm away from the intersection point along the joint surface d1, and two points 0.125 mm away from the intersection point in the radial direction.

[0077] (Measurement of particle size distribution) After embedding the test specimen in resin, it was cut and polished to expose the longitudinal section including the central axis or the vicinity of the central axis of the test specimen. In the longitudinal section of the test specimen, a measurement area of ​​0.075 mm × 0.075 mm was observed at a magnification of 5000 times using a scanning electron microscope, centered on the intersection of the central axis of the test specimen and the joint surface, and an image showing the grain boundaries of the crystal grains was obtained using an automatic crystal orientation and grain boundary microstructure analyzer (OIM). The area of ​​the crystal grains present in the measurement area was calculated, and the crystal grain size was calculated assuming that each crystal grain was a perfect sphere. Note that the calculation included crystal grains that exist across the boundaries of the measurement area. Based on the obtained crystal grain size, a number-based grain size distribution was created with a grain size interval of 1 μm.

[0078] Table 1 shows the deformation amount, bonding strength, mode grain size, frequency of crystal grains having the mode grain size, frequency of crystal grains having a representative diameter of (mode grain size (μm)-1 μm) or more and (mode grain size (μm)+1 μm) or less, hardness, and standard deviation of hardness for Examples 1 and 2 and Comparative Examples 1 and 2. Figures 2 to 5 show the number-based grain size distributions for Examples 1 and 2 and Comparative Examples 1 and 2, respectively. The grain size intervals in the grain size distribution are 1 μm, and the representative grain size diameter equivalent to the median value of each interval is plotted on the horizontal axis.

[0079] [Table 1]

[0080] As shown in Table 1, in Examples 1 and 2, the bonding strength was significantly improved compared to Comparative Examples 1 and 2. Moreover, in Example 1, in which the mode particle size was 2.50 μm or more and the standard deviation of the hardness at the bonding surface was 10.00 or less, the bonding strength was further improved.

[0081] As described above, the guide wire of the present invention has high joining strength. It is also expected that the torque transmission property will be improved and the fatigue strength will be improved by mitigating stress concentration.

[0082] This application is based on Japanese Patent Application No. 2020-061404 filed on March 30, 2020, the disclosure of which is hereby incorporated by reference in its entirety. [Explanation of symbols]

[0083] 10 Guidewire, 20 core wire, 21 first wire, 22 second wire, 30 coils, 31, 32, 51 Fixing member, 34 1st constant outer diameter part, 35 first taper section, 36 tip, 37 joint, 38 2nd constant outer diameter part, 39 Second taper section, 40 3rd constant outer diameter part, 41 tip side coating layer, 50 tubular member, 52 Tapered section, 60 base end coating layer, 61 inner layer, 62 outer layer, 63 Striatum 70 Protrusion.

Claims

1. A guide wire in which a first wire and a second wire are solid-state bonded, the first wire and the second wire are made of a Ni-Ti based alloy; A guide wire in which, in a number-based grain size distribution of crystal grains in the metal structure of the joint surface between a first wire and a second wire, when the grain size interval is 1 μm, the frequency of the mode grain size is 25% or more, and the frequency of the representative diameter being equal to or greater than (mode grain size (μm) - 1 μm) and equal to or less than (mode grain size (μm) + 1 μm) is 60% or more.

2. The guidewire according to claim 1 , wherein the modal particle size is 2.50 μm or more.

3. The guide wire according to claim 1 or 2, wherein a standard deviation of hardness at the joint surface is 10.00 or less.

Citation Information

Patent Citations

  • Method for preventing oxidation of stainless steel pipe due to steam

    JP1984085849A

  • Diffusion joined sputtering target assembly and its production

    JP1999350120A

  • Discharge lamp

    JP2011249027A

  • Medical guide wire

    JP2017113267A

  • JPP4734029B