Optical multilayers
The optical laminate addresses orange peel, local load resistance, and humidity-induced warping through precise adhesive layer thickness and reinforcing layer integration, enhancing display device stability.
Patent Information
- Application Number
- JP2023025744
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-02-22
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2041-07-29
AI Technical Summary
Image display devices face issues such as orange peel, damage from local loads, and warping in high humidity environments due to the configuration of optical laminates, which affect display performance and integrity.
An optical laminate design with specific thickness constraints for adhesive layers and inclusion of a reinforcing layer, along with balanced refractive index characteristics for retardation layers, to suppress orange peel, resist local loads, and prevent warping.
The design effectively balances suppression of orange peel, resistance to local loads, and prevention of warping in high humidity, ensuring stable display performance.
Smart Images

Figure 0007557561000003 
Figure 0007557561000002 
Figure 0007557561000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an optical laminate. [Background technology]
[0002] In recent years, image display devices, such as liquid crystal display devices and electroluminescence (EL) display devices (e.g., organic EL display devices, inorganic EL display devices), have rapidly become widespread. In image display devices, optical laminates including a polarizing plate and an optical functional layer (e.g., an anti-glare layer, an anti-reflection layer) are typically used. As such optical laminates, for example, anti-reflection layers and polarizing plates with anti-glare layers are known (e.g., Patent Document 1). In the anti-reflection layer and the polarizing plate with anti-glare layer, an anti-glare laminate including an anti-glare layer is bonded to the viewing side of a polarizing plate via an adhesive layer, and an anti-reflection laminate including an anti-reflection layer is bonded to the viewing side of the anti-glare laminate via an adhesive layer. However, in the anti-reflection layer and the polarizing plate with anti-glare layer, minute irregularities called orange peel may occur on the surface on the viewing side, which may adversely affect the display performance of the image display device.
[0003] In addition, a local load may be applied to the optical laminate used in the image display device. Depending on the configuration of the optical laminate, such a local load may damage the polarizing plate, resulting in light leakage or bright spots (so-called white dots) in the image display device. Furthermore, the optical laminate having a plurality of optical functional layers has a problem that it is prone to warping in a high humidity environment. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-155998 A Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention has been made to solve the above-mentioned problems of the conventional art, and a main object of the present invention is to provide an optical laminate that satisfies a good balance of orange peel suppression, resistance to localized load, and suppression of warping in a high-humidity environment. [Means for solving the problem]
[0006] An optical laminate according to an embodiment of the present invention comprises a polarizing plate, a first optical functional body bonded to the viewing side of the polarizing plate via a first adhesive layer, a reinforcing layer bonded to the viewing side of the first optical functional body via a second adhesive layer, and a second optical functional body bonded to the viewing side of the reinforcing layer via a third adhesive layer, wherein each of the first adhesive layer, the second adhesive layer and the third adhesive layer has a thickness of 17 μm or less, and the sum of the thickness of the first optical functional body, the thickness of the reinforcing layer and the thickness of the second optical functional body is 200 μm or less. In one embodiment, the first optical functional body is an anti-glare laminate comprising an anti-glare layer in contact with the first pressure-sensitive adhesive layer, and a first substrate arranged on the viewing side of the anti-glare layer and in contact with the second pressure-sensitive adhesive layer. In one embodiment, the second optical functional body is an antireflection laminate, which includes a second substrate in contact with the third pressure-sensitive adhesive layer, a hard coat layer arranged on the viewing side of the second substrate, and an antireflection layer arranged on the viewing side of the hard coat layer. In one embodiment, the antireflection layer is located on the outermost surface of the optical laminate, and the moisture permeability of the antireflection layer is 0.1 g / mm 2 The following is the result. In one embodiment, the polarizing plate includes a polarizer and a protective layer that is disposed on the viewing side of the polarizer and in contact with the first pressure-sensitive adhesive layer. In one embodiment, the polarizer has a thickness of 10 μm or less. In one embodiment, the optical laminate further includes a first retardation layer and a second retardation layer arranged in order from the polarizing plate side on the side opposite the viewing side of the polarizing plate, the first retardation layer exhibiting a refractive index characteristic of nx>ny>nz, and the second retardation layer exhibiting a refractive index characteristic of nz>nx>ny. Effect of the Invention
[0007] According to an embodiment of the present invention, by setting the thickness of each adhesive layer to less than the above-mentioned upper limit, providing a reinforcing layer between the first optical functional body and the second optical functional body, and setting the total thickness of the first optical functional body, the reinforcing layer and the second optical functional body to less than the above-mentioned upper limit, it is possible to realize an optical laminate that satisfies in a balanced manner the suppression of orange peel, resistance to localized loads, and suppression of warping in high humidity environments. [Brief description of the drawings]
[0008] [Figure 1] 1 is a schematic cross-sectional view of an optical laminate according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Representative embodiments of the present invention will be described below, but the present invention is not limited to these embodiments.
[0010] (Definition of terms and symbols) The definitions of terms and symbols used in this specification are as follows. (1) Refractive index (nx, ny, nz) "nx" is the refractive index in the direction in which the in-plane refractive index is maximum (i.e., the slow axis direction), "ny" is the refractive index in the direction perpendicular to the slow axis in the plane (i.e., the fast axis direction), and "nz" is the refractive index in the thickness direction. (2) In-plane phase difference (Re) "Re(λ)" is the in-plane retardation of a film measured with light of wavelength λ nm at 23° C. For example, "Re(450)" is the in-plane retardation of a film measured with light of wavelength 450 nm at 23° C. Re(λ) is calculated by the formula: Re=(nx-ny)×d, where d(nm) is the thickness of the film. (3) Retardation in the thickness direction (Rth) "Rth(λ)" is the retardation in the thickness direction of a film measured with light of wavelength λ nm at 23° C. For example, "Rth(450)" is the retardation in the thickness direction of a film measured with light of wavelength 450 nm at 23° C. Rth(λ) is calculated by the formula: Rth=(nx-nz)×d, where d(nm) is the thickness of the film. (4) Nz coefficient The Nz coefficient is calculated by Nz=Rth / Re. (5)Angle When angles are referred to herein, unless otherwise specified, the angles include angles in both clockwise and counterclockwise directions.
[0011] A. Overall configuration of optical laminate 1 is a schematic cross-sectional view of an optical laminate according to one embodiment of the present invention. The optical laminate 1 of the illustrated example includes a polarizing plate 2, a first optically functional body 3 bonded to the viewing side of the polarizing plate 2 via a first adhesive layer 61, a reinforcing layer 5 bonded to the viewing side of the first optically functional body 3 via a second adhesive layer 62, and a second optically functional body 4 bonded to the viewing side of the reinforcing layer 5 via a third adhesive layer 63. That is, the second optically functional body 4, the third adhesive layer 63, the reinforcing layer 5, the second adhesive layer 62, the first optically functional body 3, the first adhesive layer 61, and the polarizing plate 2 are laminated in this order from the viewing side of the optical laminate 1. The thickness of each of the first adhesive layer 61, the second adhesive layer 62, and the third adhesive layer 63 is 17 μm or less, preferably 15 μm or less, and typically 5 μm or more. The first adhesive layer 61, the second adhesive layer 62, and the third adhesive layer 63 may have the same thickness or different thicknesses. In one embodiment of the present invention, the first adhesive layer 61, the second adhesive layer 62, and the third adhesive layer 63 have the same thickness. The sum of the thickness of the first optical functional body 3, the thickness of the reinforcing layer 5 and the thickness of the second optical functional body 4 is 200 μm or less, preferably 180 μm or less, more preferably 170 μm or less, and typically 140 μm or more. The orange peel occurring on the surface of the visible side of the optical laminate may be caused by the unevenness of the adhesive layer. In contrast, with the above-mentioned configuration, the thickness of each adhesive layer is equal to or less than the upper limit, so that the unevenness of the adhesive layer can be prevented from affecting the surface of the visible side of the optical laminate, and the occurrence of orange peel can be prevented on the surface of the visible side of the optical laminate. However, if the thickness of each adhesive layer is equal to or less than the upper limit, the resistance of the optical laminate to local loads may be reduced. In this regard, with the above-mentioned configuration, since a reinforcing layer is provided between the first optical functional body and the second optical functional body, even if a load of a predetermined value or more is locally applied to the optical laminate, no cracks will occur, and as a result, an image display device in which light leakage and bright spots (white dots) are suppressed can be realized. Furthermore, since the sum of the thickness of the first optical functional body, the thickness of the reinforcing layer, and the thickness of the second optical functional body is equal to or less than the upper limit, even if a reinforcing layer is provided between the first optical functional body and the second optical functional body, warping of the optical laminate in a high humidity environment can be suppressed. Therefore, it is possible to realize an optical laminate that satisfies in a well-balanced manner the suppression of orange peel, resistance to localized load, and suppression of warping in a high-humidity environment.
[0012] In one embodiment of the present invention, the optical laminate 1 further includes a first retardation layer 7 and a second retardation layer 8 arranged in this order from the polarizing plate 2 side on the side opposite to the viewing side of the polarizing plate 2. The first retardation layer 7 preferably exhibits a refractive index characteristic of nx>ny>nz. The second retardation layer 8 preferably exhibits a refractive index characteristic of nz>nx>ny. With this configuration, it is possible to impart a desired optical compensation function to the optical laminate 1.
[0013] Moreover, in one embodiment of the present invention, the optical laminate 1 further includes a panel-side pressure-sensitive adhesive layer 9. The panel-side pressure-sensitive adhesive layer 9 is disposed on the opposite side of the first retardation layer 7 with respect to the second retardation layer 8. When the optical laminate 1 includes the panel-side pressure-sensitive adhesive layer 9, the panel-side pressure-sensitive adhesive layer 9 enables the optical laminate 1 to be attached to an image display cell.
[0014] In one embodiment of the present invention, the thickness of the optical laminate 1 is typically 330 μm or less, preferably 310 μm or less, more preferably 300 μm or less, and typically 250 μm or more, preferably 270 μm or more. According to this configuration, since the thickness of the optical laminate 1 is equal to or less than the upper limit, warping of the optical laminate in a high humidity environment can be stably suppressed. Also, since the thickness of the optical laminate 1 is equal to or more than the lower limit, cracking can be stably suppressed even when a load equal to or more than a predetermined value is locally applied to the optical laminate.
[0015] The components of the optical laminate will be described below.
[0016] B. Polarizing plate In one embodiment of the present invention, the polarizing plate 2 includes a polarizer 21 and a protective layer 22 disposed on the viewing side of the polarizer 21. The protective layer 22 is typically attached to the viewing side of the polarizer 21 via any appropriate adhesive layer (adhesive layer, pressure-sensitive adhesive layer: not shown). That is, the polarizing plate 2 may include the polarizer 21, an adhesive layer, and the protective layer 22. The protective layer 22 is located between the polarizer 21 and the first pressure-sensitive adhesive layer 61 and is in contact with the first pressure-sensitive adhesive layer 61. The protective layer 22 is pressure-sensitively bonded to the first pressure-sensitive adhesive layer 61. The polarizing plate 2 may further include a second protective layer on the side opposite to the viewing side of the polarizer 21.
[0017] B-1.Polarizer Any appropriate polarizer can be adopted as the polarizer 21. For example, the resin film forming the polarizing plate 2 may be a single-layer resin film or a laminate of two or more layers.
[0018] A specific example of a polarizer composed of a single-layer resin film is a PVA-based resin film that has been subjected to a dyeing treatment with iodine and a stretching treatment (typically, uniaxial stretching). The dyeing with iodine is performed, for example, by immersing the PVA-based film in an aqueous iodine solution. The stretching ratio of the uniaxial stretching is preferably 3 to 7 times. The stretching may be performed after the dyeing treatment or while dyeing. Alternatively, the film may be stretched and then dyed. If necessary, the PVA-based resin film is subjected to a swelling treatment, a crosslinking treatment, a washing treatment, a drying treatment, or the like. For example, by immersing the PVA-based resin film in water and washing it before dyeing, not only can dirt and antiblocking agents on the surface of the PVA-based film be washed off, but also the PVA-based resin film can be swelled to prevent uneven dyeing.
[0019] Specific examples of polarizers obtained using a laminate include a laminate of a resin substrate and a PVA-based resin layer (PVA-based resin film) laminated on the resin substrate, or a polarizer obtained using a laminate of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate. A polarizer obtained using a laminate of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate can be produced by, for example, applying a PVA-based resin solution to the resin substrate and drying the resin substrate to form a PVA-based resin layer on the resin substrate to obtain a laminate of the resin substrate and the PVA-based resin layer; stretching and dyeing the laminate to make the PVA-based resin layer into a polarizer. In one embodiment of the present invention, a polyvinyl alcohol-based resin layer containing a halide and a polyvinyl alcohol-based resin is preferably formed on one side of the resin substrate. The stretching typically includes immersing the laminate in an aqueous boric acid solution to stretch it. Furthermore, the stretching may further include, as necessary, stretching the laminate in air at a high temperature (for example, 95° C. or higher) before stretching in the aqueous boric acid solution. In addition, in one embodiment of the present invention, the laminate is preferably subjected to a drying shrinkage treatment in which the laminate is heated while being transported in the longitudinal direction to shrink the laminate by 2% or more in the width direction. Typically, the manufacturing method of this embodiment includes subjecting the laminate to an air-assisted stretching treatment, a dyeing treatment, an underwater stretching treatment, and a drying shrinkage treatment in this order. By introducing the auxiliary stretching, even when PVA is applied onto a thermoplastic resin, it is possible to increase the crystallinity of PVA, and to achieve high optical properties. At the same time, by increasing the orientation of PVA in advance, problems such as a decrease in the orientation of PVA or dissolution when immersed in water in the subsequent dyeing step or stretching step can be prevented, and high optical properties can be achieved. Furthermore, when the PVA-based resin layer is immersed in a liquid, the disorder of the orientation of polyvinyl alcohol molecules and the decrease in the orientation can be suppressed compared to when the PVA-based resin layer does not contain a halide. This can improve the optical properties of a polarizer obtained through a treatment step in which the laminate is immersed in a liquid, such as a dyeing treatment and an underwater stretching treatment. Furthermore, the optical properties can be improved by shrinking the laminate in the width direction through drying shrinkage treatment.The obtained laminate of resin substrate / polarizer may be used as it is (i.e., the resin substrate may be used as a protective layer for the polarizer), or the resin substrate may be peeled off from the laminate of resin substrate / polarizer, and any suitable protective layer may be laminated on the peeled surface depending on the purpose. Details of the method for producing such a polarizer are described in, for example, JP2012-73580A and JP6470455A. The entire disclosures of these publications are incorporated herein by reference.
[0020] The polarizer 21 is preferably made of a laminate of two or more layers, and more preferably made of a laminate of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate.
[0021] The thickness of the polarizer 21 is preferably 15 μm or less, more preferably 12 μm or less, further preferably 10 μm or less, particularly preferably 8 μm or less, and typically 1 μm or more, preferably 3 μm or more. When the thickness of the polarizer is in this range, the occurrence of warping of the optical laminate in a high-humidity environment can be more stably suppressed.
[0022] The polarizer 21 preferably exhibits absorptive dichroism at any wavelength of 380 nm to 780 nm. The single transmittance of the polarizer 21 is, for example, 41.5% to 46.0%, preferably 43.0% to 46.0%, and more preferably 44.5% to 46.0%. The degree of polarization of the polarizer 21 is preferably 97.0% or more, more preferably 99.0% or more, and even more preferably 99.9% or more.
[0023] B-2.Protective layer The protective layer 22 is formed of any suitable film that can be used as a protective layer for the polarizer 21. Specific examples of materials that are the main components of the film include cellulose-based resins such as triacetyl cellulose (TAC), and transparent resins such as polyesters, polyvinyl alcohols, polycarbonates, polyamides, polyimides, polyethersulfones, polysulfones, polystyrenes, polynorbornenes, polyolefins, (meth)acrylics, and acetates. Other examples include thermosetting resins or ultraviolet-curing resins such as (meth)acrylics, urethanes, (meth)acrylic urethanes, epoxys, and silicones. The term "(meth)acrylic resin" refers to acrylic resins and / or methacrylic resins. Other examples include glassy polymers such as siloxane polymers. Polymer films described in JP 2001-343529 A (WO01 / 37007) can also be used. The material for this film may be, for example, a resin composition containing a thermoplastic resin having a substituted or unsubstituted imide group in the side chain, and a thermoplastic resin having a substituted or unsubstituted phenyl group and a nitrile group in the side chain, such as a resin composition containing an alternating copolymer of isobutene and N-methylmaleimide, and an acrylonitrile-styrene copolymer. The polymer film may be, for example, an extrusion molded product of the above resin composition.
[0024] In one embodiment of the present invention, the protective layer 22 contains a (meth)acrylic resin. As the (meth)acrylic resin, for example, a (meth)acrylic resin having a glutarimide structure is used. (Meth)acrylic resins having a glutarimide structure are described, for example, in JP 2006-309033 A, JP 2006-317560 A, JP 2006-328329 A, JP 2006-328334 A, JP 2006-337491 A, JP 2006-337492 A, JP 2006-337493 A, JP 2006-337569 A, JP 2007-009182 A, JP 2009-161744 A, and JP 2010-284840 A. These descriptions are incorporated herein by reference.
[0025] The thickness of the protective layer 22 is typically 300 μm or less, preferably 100 μm or less, more preferably 5 μm to 80 μm, and further preferably 10 μm to 60 μm. When a surface treatment is applied, the thickness of the protective layer 22 includes the thickness of the surface treatment layer.
[0026] C. First optical function body The first optical function body 3 can impart a desired optical function to the optical laminate 1. Examples of the first optical function body 3 include an anti-glare laminate, an anti-sunglasses laminate, and the like. The thickness of the first optical function body 3 is typically 20 μm to 60 μm, and preferably 30 μm to 50 μm.
[0027] In one embodiment of the present invention, the first optical functional body 3 is an anti-glare laminate 3a. The anti-glare laminate 3a includes an anti-glare layer 32 and a first substrate 31 disposed on the viewing side of the anti-glare layer 32. The anti-glare layer 32 is supported by the first substrate 31. The anti-glare layer 32 is disposed on the viewing side of the protective layer 22 and is bonded to the protective layer 22 via a first adhesive layer 61. The anti-glare layer 32 is in contact with the first adhesive layer 61 and is pressure-sensitively bonded to the first adhesive layer 61. The first substrate 31 is located on the opposite side of the anti-glare layer 32 to the first adhesive layer 61. The first substrate 31 is in contact with the second adhesive layer 62 and is pressure-sensitively bonded to the second adhesive layer 62.
[0028] C-1. Anti-glare layer The anti-glare layer 32 is provided to prevent the reflection of the face of a user of the image display device, the keyboard of the image display device, external light (e.g., fluorescent light), etc. In one embodiment of the present invention, the anti-glare layer 32 is an oriented and solidified layer of a liquid crystal compound. In this specification, the term "oriented and solidified layer" refers to a layer in which the liquid crystal compound is oriented in a predetermined direction within the layer and the oriented state is fixed. The term "oriented and solidified layer" is a concept that includes an oriented and solidified layer obtained by hardening a liquid crystal monomer. The liquid crystal compound may be a rod-shaped liquid crystal compound, a discotic liquid crystal compound, or a combination thereof.
[0029] In one embodiment of the present invention, the anti-glare layer 32 contains a discotic liquid crystal compound. More specifically, the anti-glare layer 32 is a layer in which a discotic liquid crystal compound is fixed in a state of being aligned in a predetermined direction. A discotic liquid crystal compound generally refers to a liquid crystal compound having a disk-shaped molecular structure in which a cyclic mother nucleus such as benzene, 1,3,5-triazine, calixarene, etc. is arranged at the center of the molecule and linear alkyl groups, alkoxy groups, substituted benzoyloxy groups, etc. are substituted radially as side chains. Representative examples of discotic liquid crystals include benzene derivatives, triphenylene derivatives, truxene derivatives, and phthalocyanine derivatives described in the research report by C. Destrade et al., Mol. Cryst. Liq. Cryst., Vol. 71, p. 111 (1981); cyclohexane derivatives described in the research report by B. Kohne et al., Angew. Chem. Vol. 96, p. 70 (1984); and azacrown and phenylacetylene macrocycles described in the research report by JM Lehn et al., J. Chem. Soc. Chem. Commun., p. 1794 (1985) and the research report by J. Zhang et al., J. Am. Chem. Soc., Vol. 116, p. 2655 (1994). Further specific examples of discotic liquid crystal compounds include compounds described in, for example, JP 2006-133652 A, JP 2007-108732 A, JP 2010-244038 A, and JP 2014-214177 A. The descriptions in the above documents and publications are incorporated herein by reference. The anti-glare layer containing a discotic liquid crystal compound can be a so-called negative A plate having a refractive index characteristic of nx=nz>ny.
[0030] In another embodiment, the anti-glare layer 32 includes a rod-shaped liquid crystal compound. More specifically, the anti-glare layer is oriented (homogeneous orientation) in a state where the rod-shaped liquid crystal compounds are aligned in a predetermined direction (typically, the slow axis direction). As the rod-shaped liquid crystal compound, for example, a liquid crystal compound having a nematic liquid crystal phase (nematic liquid crystal) can be mentioned. As such a liquid crystal compound, for example, a liquid crystal polymer or a liquid crystal monomer can be used. The mechanism of liquid crystallinity of the liquid crystal compound may be either lyotropic or thermotropic. The liquid crystal polymer and the liquid crystal monomer may be used alone or in combination. As the liquid crystal monomer, any appropriate liquid crystal monomer may be adopted. For example, polymerizable mesogen compounds described in JP-A-2002-533742 (WO00 / 37585), EP358208 (US5211877), EP66137 (US4388453), WO93 / 22397, EP0261712, DE19504224, DE4408171, and GB2280445 can be used. Specific examples of such polymerizable mesogen compounds include BASF's product name LC242, Merck's product name E7, and Wacker-Chem's product name LC-Sillicon-CC3767. As the liquid crystal monomer, for example, a nematic liquid crystal monomer is preferable. Specific examples of liquid crystal compounds are described in JP-A-2006-163343, for example. The description of the publication is incorporated herein by reference. The anti-glare layer containing a rod-like liquid crystal compound can be typically a so-called positive A plate having a refractive index characteristic of nx>ny=nz.
[0031] The anti-glare layer 32 can typically function as a λ / 2 plate. When the anti-glare layer 32 functions as a λ / 2 plate, the anti-glare layer 32 can effectively prevent glare by controlling its orientation angle (or slow axis direction). The in-plane retardation Re(550) of the anti-glare layer 32 is 220 nm to 320 nm, more preferably 240 nm to 300 nm, and further preferably 250 nm to 280 nm.
[0032] The angle between the slow axis of the anti-glare layer 32 and the absorption axis of the polarizer 21 is preferably 35° to 55°, more preferably 40° to 50°, and even more preferably about 45°. By disposing the anti-glare layer 32 functioning as a λ / 2 plate at such an axial angle, it is possible to effectively prevent glare.
[0033] The thickness of the anti-glare layer 32 is preferably 1 μm to 5 μm, and more preferably 1 μm to 3 μm.
[0034] When an alignment film is used to align the liquid crystal compound, the anti-glare laminate 3a further includes an alignment film between the anti-glare layer 32 and the first substrate 31. That is, the anti-glare laminate 3a may be composed of the anti-glare layer 32, the alignment film, and the first substrate 31. The alignment film generally contains a polymer material as a main component. Representative examples of the polymer material include polyvinyl alcohol, polyimide, and derivatives thereof. In one embodiment of the present invention, modified or unmodified polyvinyl alcohol is preferred. For example, modified polyvinyl alcohol described in WO01 / 88574A1 and Japanese Patent No. 3907735 can be used as the alignment film. The alignment film is typically subjected to an alignment treatment. Representative examples of the alignment treatment include rubbing treatment and photoalignment treatment. Since the rubbing treatment is well known in the industry, a detailed description thereof will be omitted. As the alignment film subjected to photo-alignment treatment (photo-alignment film), for example, those described in WO2005 / 096041, product name LPP-JP265CP manufactured by Rolic Technologies, etc. can be used. The thickness of the alignment film is, for example, 0.01 μm to 10 μm, preferably 0.01 μm to 1 μm, and more preferably 0.01 μm to 0.5 μm.
[0035] The anti-glare layer 32 can be formed, for example, by the following procedure. First, a coating liquid for forming an alignment film is applied onto the first substrate 31, and dried to form a coating film. The coating film is rubbed in a predetermined direction to form an alignment film on the first substrate 31. The predetermined direction can correspond to the slow axis direction of the anti-glare layer 32 to be obtained. Next, a coating liquid for forming an anti-glare layer (for example, a solution containing a liquid crystal compound and, if necessary, a crosslinkable monomer) is applied onto the formed alignment film, and heated. By heating, the solvent of the coating liquid is removed and the alignment of the liquid crystal compound is promoted. Heating may be performed in one step, or may be performed in multiple steps at different temperatures. Next, the crosslinkable (or polymerizable) monomer is crosslinked (or polymerized) by ultraviolet irradiation to fix the alignment of the liquid crystal compound. In this way, the anti-glare layer 32 is formed on the first substrate 31 (substantially, on the alignment film). A method for aligning discotic liquid crystal compounds is described, for example, in JP 2014-214177 A, and a method for aligning rod-shaped liquid crystal compounds is described, for example, in JP 2006-163343 A. The descriptions in these publications are incorporated herein by reference. The alignment film may be omitted depending on the desired alignment state and the type of liquid crystal compound.
[0036] C-2. First substrate The first base material 31 is used to form the anti-glare layer 32 .
[0037] Any appropriate resin film is used as the first base material 31. Examples of materials for forming the resin film include polyester-based resins such as polyethylene terephthalate (PET), cycloolefin-based resins such as norbornene-based resins, resins (COC) obtained by addition polymerization of cycloolefins (e.g., norbornene) and α-olefins (e.g., ethylene), and cellulose-based resins such as triacetyl cellulose (TAC). In one embodiment of the present invention, the first base material 31 includes a TAC-based resin.
[0038] The thickness of the first base material 31 can be appropriately set depending on the purpose. The thickness of the first base material 31 is typically 20 μm to 200 μm, preferably 25 μm to 100 μm, and more preferably 30 μm to 50 μm.
[0039] D. Reinforcement layer The reinforcing layer 5 provides the optical laminate 1 with excellent resistance to localized loads. In one embodiment of the present invention, the reinforcing layer 5 is bonded to the first substrate 31 via the second pressure-sensitive adhesive layer 62. The reinforcing layer 5 is disposed between the second pressure-sensitive adhesive layer 62 and the third pressure-sensitive adhesive layer 63. The reinforcing layer 5 is in contact with the second pressure-sensitive adhesive layer 62 and the third pressure-sensitive adhesive layer 63, and is pressure-sensitively bonded to the second pressure-sensitive adhesive layer 62 and the third pressure-sensitive adhesive layer 63.
[0040] The reinforcing layer 5 is formed of any appropriate film. Specific examples of the main component of the reinforcing layer 5 include the same main component of the protective layer 22 described in the above section B-2 (the transparent resin, the thermosetting resin or the ultraviolet curing resin, the glassy polymer, and the resin composition). In one embodiment of the present invention, the reinforcing layer 5 contains a (meth)acrylic resin, and preferably contains a (meth)acrylic resin having a glutarimide structure. That is, each of the protective layer 22 and the reinforcing layer 5 contains a (meth)acrylic resin. By using a (meth)acrylic resin as the protective layer 22 and the reinforcing layer 5, light leakage can be stably suppressed when a load of a predetermined value or more is locally applied to the optical laminate 1.
[0041] Similarly to the protective layer 22, the reinforcing layer 5 may be subjected to the above-mentioned surface treatment and / or the above-mentioned treatment for improving visibility, if necessary.
[0042] The thickness of the reinforcing layer 5 is typically 20 μm to 70 μm, and preferably 30 μm to 50 μm. If the thickness of the reinforcing layer 5 is in this range, excellent resistance to localized loads can be imparted to the optical laminate 1, and warping of the optical laminate 1 in a high-humidity environment can be sufficiently suppressed.
[0043] E. Second Optical Function Body The second optical function body 4 can impart an optical function to the optical laminate 1 that is different from that of the first optical function body 3. Examples of the second optical function body 4 include an anti-reflection laminate and a laminate for sunglasses. The thickness of the second optical function body 4 is typically 40 μm to 120 μm, and preferably 70 μm to 100 μm or less.
[0044] In one embodiment of the present invention, the second optical functional body 4 is an antireflection laminate 4a. The antireflection laminate 4a includes a second substrate 41, a hard coat layer 42 disposed on the viewing side of the second substrate 41, and an antireflection layer 43 disposed on the viewing side of the hard coat layer 42. That is, the antireflection laminate 4a may be composed of the second substrate 41, the hard coat layer 42, and the antireflection layer 43. The second substrate 41 is disposed on the viewing side of the reinforcing layer 5, and is bonded to the reinforcing layer 5 via a third pressure-sensitive adhesive layer 63. The second substrate 41 is in contact with the third pressure-sensitive adhesive layer 63, and is pressure-sensitively bonded to the third pressure-sensitive adhesive layer 63. In one embodiment of the present invention, the hard coat layer 42 is formed directly on the viewing side surface of the second substrate 41. In this specification, "directly" means that no adhesive layer or pressure-sensitive adhesive layer is interposed. The anti-reflection layer 43 is formed directly on the viewing side surface of the hard coat layer 42 .
[0045] E-1. Second substrate The second substrate 41 is used to form the hard coat layer 42 and the anti-reflection layer 43. Any appropriate resin film is used as the second substrate 41. Examples of materials for forming the second substrate 41 include the same materials as those for forming the first substrate 31 described in Section C-2 above (the above-mentioned polyester-based resins, the above-mentioned cycloolefin-based resins, the above-mentioned resins obtained by addition polymerization of cycloolefins and α-olefins, and the above-mentioned cellulose-based resins). In one embodiment of the present invention, the second substrate 41 contains a TAC-based resin.
[0046] The thickness of the second base material 41 can be appropriately set depending on the purpose. The thickness of the second base material 41 is typically 20 μm to 200 μm, preferably 50 μm to 150 μm, and more preferably 70 μm to 90 μm.
[0047] E-2. Hard coat layer The hard coat layer 42 can impart excellent pencil hardness to the optical laminate 1. Furthermore, by appropriately adjusting the refractive index difference between the hard coat layer 42 and the antireflection layer 43, the reflectance of the optical laminate 1 can be further reduced.
[0048] The hard coat layer 42 preferably has sufficient surface hardness, excellent mechanical strength, and excellent light transmittance. The hard coat layer 42 may be formed from any appropriate resin as long as it has such desired properties. Specific examples of the resin include thermosetting resin, thermoplastic resin, ultraviolet curing resin, electron beam curing resin, and two-part mixture resin. Among the resins forming the hard coat layer 42, ultraviolet curing resin is preferred. When the resin is an ultraviolet curing resin, the hard coat layer 42 can be formed with simple operation and high efficiency.
[0049] Specific examples of ultraviolet curing resins include polyester-based, acrylic-based, urethane-based, amide-based, silicone-based, and epoxy-based ultraviolet curing resins. The ultraviolet curing resins include ultraviolet curing monomers, oligomers, and polymers. A preferred ultraviolet curing resin is a resin composition containing an acrylic monomer or oligomer component having preferably two or more, more preferably three to six, ultraviolet polymerizable functional groups. Typically, the ultraviolet curing resin contains a photopolymerization initiator.
[0050] The hard coat layer 42 can be formed by any appropriate method. For example, the hard coat layer 42 can be formed by coating a resin composition for forming a hard coat layer on the second substrate 41, drying the composition, and curing the dried coating film by irradiating it with ultraviolet light.
[0051] The thickness of the hard coat layer 42 is, for example, 0.5 μm to 20 μm, and preferably 1 μm to 15 μm.
[0052] Details of the hard coat layer and the adhesion structure between the hard coat layer and the antireflection layer are described in, for example, JP 2016-224443 A. The description of this publication is incorporated herein by reference.
[0053] E-3.Anti-reflection layer The antireflection layer 43 is provided to prevent reflection of external light (e.g., fluorescent light) and the like. Any appropriate configuration may be adopted as the configuration of the antireflection layer 43. Representative configurations of the antireflection layer 43 include (1) a single layer of a low refractive index layer having an optical thickness of 120 nm to 140 nm and a refractive index of about 1.35 to 1.55; (2) a laminate having a medium refractive index layer, a high refractive index layer, and a low refractive index layer in this order from the second substrate 41; and (3) an alternating multilayer laminate of a high refractive index layer and a low refractive index layer.
[0054] Examples of materials that can form a low refractive index layer include silicon oxide (SiO2) and magnesium fluoride (MgF2). The refractive index of the low refractive index layer is typically about 1.35 to 1.55. Examples of materials that can form a high refractive index layer include titanium oxide (TiO2), niobium oxide (Nb2O3 or Nb2O5), tin-doped indium oxide (ITO), antimony-doped tin oxide (ATO), and ZrO2-TiO2. The refractive index of the high refractive index layer is typically about 1.60 to 2.20. Examples of materials that can form a medium refractive index layer include titanium oxide (TiO2) and a mixture of a material that can form a low refractive index layer and a material that can form a high refractive index layer (for example, a mixture of titanium oxide and silicon oxide). The refractive index of the medium refractive index layer is typically about 1.50 to 1.85. The thicknesses of the low refractive index layer, the medium refractive index layer and the high refractive index layer can be set so as to realize an appropriate optical film thickness depending on the layer structure of the antireflection layer, the desired antireflection performance, and the like.
[0055] The anti-reflection layer 43 is typically formed by a dry process. Specific examples of the dry process include a PVD (Physical Vapor Deposition) method and a CVD (Chemical Vapor Deposition) method. Examples of the PVD method include a vacuum deposition method, a reactive deposition method, an ion beam assisted method, a sputtering method, and an ion plating method. Examples of the CVD method include a plasma CVD method. The dry process for forming the anti-reflection layer 43 is preferably a sputtering method.
[0056] The antireflection layer 43 has a thickness of, for example, about 20 nm to 300 nm.
[0057] The difference between the maximum reflectance and the minimum reflectance in the wavelength range of 400 nm to 700 nm of the antireflection layer 43 is preferably 2.0% or less, more preferably 1.9% or less, and further preferably 1.8% or less. If the difference between the maximum reflectance and the minimum reflectance is within such a range, coloring of the reflected light can be effectively prevented.
[0058] In one embodiment of the present invention, the antireflection layer 43 is located on the outermost surface on the viewing side of the optical laminate 1. The moisture permeability of the antireflection layer 43 is typically 1.0 g / mm 2 Less than 0.1 g / mm 2 A typical value is 0.01 g / mm 2 The moisture permeability was measured in accordance with the JIS Z0208 moisture permeability test (cup method) at a temperature of 40°C and a humidity of 92% RH in an atmosphere with an area of 1 m 2 When the moisture permeability of the antireflection layer 43 located on the outermost surface is equal to or lower than the upper limit, warping of the optical laminate 1 in a high-humidity environment can be more stably suppressed.
[0059] The antireflection layer 43 does not have to be located on the outermost surface of the optical laminate 1. The antireflection laminate 4a may have an outermost layer on the viewing side of the antireflection layer 43, if necessary. That is, the antireflection laminate 4a may be composed of a second substrate 41, a hard coat layer 42, an antireflection layer 43, and an outermost layer. The moisture permeability range of the outermost layer is the same as that of the antireflection layer 43 described above. The outermost layer may be, for example, an antifouling layer. The antifouling layer contains, for example, a fluorine group-containing silane-based compound (for example, an alkoxysilane compound having a perfluoropolyether group) or a fluorine group-containing organic compound. The antifouling layer preferably exhibits water repellency with a water contact angle of 110 degrees or more.
[0060] F. First Adhesive Layer, Second Adhesive Layer and Third Adhesive Layer Each of the first adhesive layer 61, the second adhesive layer 62, and the third adhesive layer 63 is formed from an adhesive (pressure-sensitive adhesive). More specifically, the first adhesive layer 61 is formed by coating an adhesive on the protective layer 22 of the polarizing plate 2 to the above-mentioned thickness. The second adhesive layer 62 is formed by coating an adhesive on the first base material 31 of the first optical function body 3 to the above-mentioned thickness. The third adhesive layer 63 is formed by coating an adhesive on the reinforcing layer 5 to the above-mentioned thickness. The first adhesive layer 61, the second adhesive layer 62, and the third adhesive layer 63 may be formed from the same adhesive or from different adhesives. In one embodiment of the present invention, the first adhesive layer 61, the second adhesive layer 62, and the third adhesive layer 63 are formed from the same adhesive. When the first pressure-sensitive adhesive layer 61, the second pressure-sensitive adhesive layer 62 and the third pressure-sensitive adhesive layer 63 are each formed from the same pressure-sensitive adhesive, the production costs of the optical laminate 1 can be reduced.
[0061] The pressure-sensitive adhesive typically contains a (meth)acrylic polymer, a urethane polymer, a silicone polymer, or a rubber polymer as a base polymer. When a (meth)acrylic polymer is used as the base polymer, the pressure-sensitive adhesive layer is formed from a pressure-sensitive adhesive containing, for example, a (meth)acrylic polymer.
[0062] F-1. (Meth)acrylic polymer The (meth)acrylic polymer contains a polymer of a monomer component (raw material monomer) mainly composed of an alkyl (meth)acrylate. In other words, the (meth)acrylic polymer contains a structural unit derived from an alkyl (meth)acrylate. The alkyl (meth)acrylate is preferably 50% by weight or more of the total monomer components that are the raw material of the (meth)acrylic polymer, and can be arbitrarily set as the remainder of the monomers other than the alkyl (meth)acrylate. Note that the (meth)acrylate refers to acrylate and / or methacrylate.
[0063] The alkyl (meth)acrylate constituting the main skeleton of the (meth)acrylic polymer may be a linear or branched alkyl group having 1 to 18 carbon atoms. Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, an amyl group, a hexyl group, a cyclohexyl group, a heptyl group, a 2-ethylhexyl group, an isooctyl group, a nonyl group, a decyl group, an isodecyl group, a dodecyl group, an isomyristyl group, a lauryl group, a tridecyl group, a pentadecyl group, a hexadecyl group, a heptadecyl group, and an octadecyl group. The alkyl (meth)acrylate may be used alone or in combination. The average carbon number of the alkyl group is preferably 3 to 10.
[0064] The (meth)acrylic polymer may contain a structural unit derived from a copolymerizable monomer polymerizable with the alkyl (meth)acrylate in addition to the structural unit derived from the alkyl (meth)acrylate. That is, the monomer component serving as the raw material of the (meth)acrylic polymer may further contain a copolymerizable monomer in addition to the alkyl (meth)acrylate.
[0065] Examples of copolymerizable monomers include carboxyl group-containing monomers, hydroxyl group-containing monomers, amino group-containing monomers, amide group-containing monomers, cyclopolymerizable monomers, epoxy group-containing monomers, sulfonic acid group-containing monomers, phosphoric acid group-containing monomers, polyfunctional acrylates, (meth)acrylic acid esters having an alicyclic hydrocarbon group, (meth)acrylic acid esters having an aromatic hydrocarbon group, vinyl esters, aromatic vinyl compounds, dienes, vinyl ethers, vinyl chloride, etc. The copolymerizable monomers can be used alone or in combination.
[0066] Among such copolymerization monomers, preferably, reactive group-containing monomers containing reactive groups capable of reacting with the crosslinking agent described later are used, and more preferably, carboxyl group-containing monomers and hydroxyl group-containing monomers are used. When the pressure-sensitive adhesive contains a crosslinking agent described later, the reactive group-containing monomers become reaction sites with the crosslinking agent. Carboxyl group-containing monomers and hydroxyl group-containing monomers are highly reactive with intermolecular crosslinking agents, and are preferably used to improve the cohesiveness and heat resistance of the resulting pressure-sensitive adhesive layer. In addition, carboxyl group-containing monomers are preferred in terms of achieving both durability and reworkability, and hydroxyl group-containing monomers are preferred in terms of improving reworkability. The copolymerization monomers can be used alone or in combination as raw material monomers for (meth)acrylic polymers.
[0067] The carboxyl group-containing monomer is a compound that contains a carboxyl group in its structure and a polymerizable unsaturated double bond such as a (meth)acryloyl group or a vinyl group. Examples of the carboxyl group-containing monomer include (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid. Among these, acrylic acid is preferred. The (meth)acrylic polymer may preferably contain a structural unit derived from a carboxyl group-containing monomer, more preferably a structural unit derived from (meth)acrylic acid. When the (meth)acrylic polymer contains a structural unit derived from a carboxyl group-containing monomer, the adhesive properties of the adhesive layer may be improved.
[0068] When a carboxyl group-containing monomer is used as the raw material monomer, the content of the carboxyl group-containing monomer is usually 0.01% by weight to 10% by weight in total monomer components serving as raw materials for the (meth)acrylic polymer.
[0069] The hydroxyl group-containing monomer is a compound that contains a hydroxyl group in its structure and a polymerizable unsaturated double bond such as a (meth)acryloyl group or a vinyl group. Examples of the hydroxyl group-containing monomer include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, and 12-hydroxylauryl (meth)acrylate; (4-hydroxymethylcyclohexyl)-methyl acrylate, etc. Among these, 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate are preferred, and 4-hydroxybutyl (meth)acrylate is more preferred. The (meth)acrylic polymer may preferably contain structural units derived from hydroxyl group-containing monomers, more preferably structural units derived from 2-hydroxyethyl (meth)acrylate and / or 4-hydroxybutyl (meth)acrylate. When the (meth)acrylic polymer contains structural units derived from hydroxyl group-containing monomers, the durability of the pressure-sensitive adhesive layer can be improved.
[0070] When a hydroxyl group-containing monomer is used as the raw material monomer, the content of the hydroxyl group-containing monomer is usually 0.01% by weight or more and 10% by weight or less in all monomer components serving as raw materials for the (meth)acrylic polymer.
[0071] The weight average molecular weight Mw of the (meth)acrylic polymer is, for example, 200,000 to 3,000,000, preferably 1,000,000 to 2,500,000, and more preferably 1,200,000 to 2,500,000. If the weight average molecular weight Mw is within this range, a pressure-sensitive adhesive layer having excellent durability (particularly, heat resistance) can be obtained. If the weight average molecular weight Mw exceeds 3,000,000, an increase in viscosity and / or gelation during polymer polymerization may occur.
[0072] F-2. Crosslinking agent The adhesive may contain a crosslinking agent. As the crosslinking agent, an organic crosslinking agent, a polyfunctional metal chelate, etc. may be used. As the organic crosslinking agent, for example, an isocyanate crosslinking agent, a peroxide crosslinking agent, an epoxy crosslinking agent, and an imine crosslinking agent may be mentioned. The polyfunctional metal chelate is a crosslinking agent in which a polyvalent metal is covalently bonded or coordinately bonded to an organic compound. When the adhesive is a radiation curing type, a polyfunctional monomer may be used as the crosslinking agent. The crosslinking agents may be used alone or in combination. The crosslinking agent preferably includes an isocyanate crosslinking agent and a peroxide crosslinking agent.
[0073] When a crosslinking agent is blended in the adhesive, the blending amount of the crosslinking agent is usually 0.01 to 15 parts by weight relative to 100 parts by weight of the (meth)acrylic polymer (base polymer). When an isocyanate-based crosslinking agent is blended in the adhesive, the blending amount of the isocyanate-based crosslinking agent is usually 0.01 to 15 parts by weight, preferably 1.0 to 10 parts by weight, more preferably 2.5 to 5 parts by weight, relative to 100 parts by weight of the (meth)acrylic polymer. When a peroxide-based crosslinking agent is blended in the adhesive, the blending amount of the peroxide-based crosslinking agent is usually 0.01 to 2 parts by weight, preferably 0.1 to 0.5 parts by weight, relative to 100 parts by weight of the (meth)acrylic polymer. When the blending ratio of the crosslinking agent (isocyanate-based crosslinking agent and peroxide-based crosslinking agent) is within the above range, when the raw material monomer component of the (meth)acrylic polymer contains a reactive group-containing monomer, the elastic modulus of the pressure-sensitive adhesive layer described below can be smoothly adjusted to the desired range.
[0074] F-3. Silane coupling agents containing reactive functional groups The adhesive can contain a reactive functional group-containing silane coupling agent. The reactive functional group of the reactive functional group-containing silane coupling agent is typically a functional group other than an acid anhydride group. Examples of functional groups other than an acid anhydride group include epoxy groups, mercapto groups, amino groups, isocyanate groups, isocyanurate groups, vinyl groups, styryl groups, acetoacetyl groups, ureido groups, thiourea groups, (meth)acrylic groups, heterocyclic groups, and combinations thereof. The reactive functional group-containing silane coupling agents can be used alone or in combination.
[0075] When a reactive functional group-containing silane coupling agent is blended with the pressure-sensitive adhesive, the blending amount of the reactive functional group-containing silane coupling agent is usually 0.001 to 5 parts by weight per 100 parts by weight of the (meth)acrylic polymer.
[0076] F-4. Additives The adhesive may contain a (meth)acrylic oligomer and / or an ionic compound. The adhesive may also contain an additive. Specific examples of additives include colorants, powders such as pigments, dyes, surfactants, plasticizers, tackifiers, surface lubricants, leveling agents, softeners, antioxidants, antiaging agents, light stabilizers, UV absorbers, polymerization inhibitors, inorganic or organic fillers, metal powders, particles, and foils. A redox system may also be used by adding a reducing agent within a controllable range. The adhesive may also contain a polyether compound having a reactive group (e.g., a reactive silyl group). The type, number, combination, and content of the additives may be appropriately set according to the purpose. The content of the additive is preferably 5 parts by weight or less, more preferably 3 parts by weight or less, and even more preferably 1 part by weight or less, relative to 100 parts by weight of the (meth)acrylic polymer.
[0077] F-5. Characteristics of adhesive The storage modulus of the pressure-sensitive adhesive at 23°C and 55% RH is typically 0.05 GPa or more, preferably 0.11 GPa or more, and typically 0.2 GPa or less, preferably 0.15 GPa or less. The storage modulus can be measured using a dynamic viscoelasticity measuring device "ARES" manufactured by Rheometrics Co., Ltd. in accordance with JIS K 7244. If the modulus of the pressure-sensitive adhesive is within this range, the resistance of the optical laminate 1 to local loads can be further improved.
[0078] G. First retardation layer The first retardation layer 7 may be composed of a retardation film having any suitable optical and / or mechanical properties depending on the purpose. The first retardation layer 7 is located on the opposite side to the viewing side of the polarizing plate 2. The first retardation layer 7 is typically attached to the opposite side to the viewing side of the polarizer 21 via any suitable adhesive layer. The first retardation layer 7 may also serve as a protective layer on the opposite side to the viewing side of the polarizer 21.
[0079] The thickness of the first retardation layer 7 is preferably 10 μm to 60 μm, and more preferably 30 μm to 50 μm.
[0080] The in-plane retardation Re(550) of the first retardation layer 7 is preferably 80 nm to 150 nm, more preferably 90 nm to 140 nm, and further preferably 100 nm to 130 nm.
[0081] As described above, the first retardation layer 7 preferably has refractive index characteristics that satisfy the relationship nx>ny>nz. The Nz coefficient of the first retardation layer 7 is preferably 1.1 to 3.0, and more preferably 1.3 to 2.7.
[0082] The first retardation layer 7 may be preferably arranged so that its slow axis is substantially parallel to the absorption axis of the polarizer 21. In this specification, the terms "substantially parallel" and "almost parallel" include the case where the angle between the two directions is 0°±7°, preferably 0°±5°, and more preferably 0°±3°. The terms "substantially orthogonal" and "almost orthogonal" include the case where the angle between the two directions is 90°±7°, preferably 90°±5°, and more preferably 90°±3°. Furthermore, when simply referring to "orthogonal" or "parallel" in this specification, it is understood that it may include a substantially orthogonal or substantially parallel state.
[0083] The absolute value of the photoelastic coefficient of the first retardation layer 7 is preferably 2×10 -11 m 2 / N or less, preferably 2.0×10 -13 m 2 / N~1.5×10 -11 m 2 / N, more preferably 1.0×10 -12 m 2 / N~1.2×10 -11 m 2 / N resin. If the absolute value of the photoelastic coefficient is in this range, the phase difference is unlikely to change when shrinkage stress occurs during heating. Therefore, by forming the first phase difference layer 7 using a resin having such an absolute value of the photoelastic coefficient, it is possible to effectively prevent thermal unevenness when the optical laminate 1 is applied to an image display device.
[0084] The first retardation layer 7 may exhibit a reverse wavelength dispersion characteristic in which the retardation value increases according to the wavelength of the measurement light, may exhibit a positive wavelength dispersion characteristic in which the retardation value decreases according to the wavelength of the measurement light, or may exhibit a flat wavelength dispersion characteristic in which the retardation value hardly changes according to the wavelength of the measurement light. The first retardation layer 7 preferably exhibits a flat wavelength dispersion characteristic. Specifically, Re(450) / Re(550) of the first retardation layer 7 is preferably 0.99 to 1.03, and Re(650) / Re(550) is preferably 0.98 to 1.02. By arranging a λ / 2 plate (first retardation layer) and a λ / 4 plate (second retardation layer) having flat wavelength dispersion characteristics at a predetermined axial angle, it is possible to obtain characteristics close to ideal reverse wavelength dispersion characteristics, and as a result, it is possible to realize very excellent antireflection characteristics.
[0085] The first retardation layer 7 may be made of any suitable resin film that satisfies the above-mentioned characteristics. Representative examples of such resins include cyclic olefin resins, polycarbonate resins, cellulose resins, polyester resins, polyvinyl alcohol resins, polyamide resins, polyimide resins, polyether resins, polystyrene resins, and acrylic resins. Among them, cyclic olefin resins may be preferably used. The first retardation layer 7 may be obtained, for example, by stretching a film formed from the above-mentioned resin. Details of the cyclic olefin resins and the stretching method of the resin film (method of forming the retardation film) are described, for example, in JP-A-2015-210459 and JP-A-2016-105166. The description of this publication is incorporated herein by reference.
[0086] H. Second retardation layer The second retardation layer 8 may be composed of a retardation film having any suitable optical and / or mechanical properties depending on the purpose. The second retardation layer 8 is located on the opposite side to the viewing side of the first retardation layer 7. The second retardation layer 8 is typically attached to the opposite side to the viewing side of the first retardation layer 7 via any suitable adhesive layer.
[0087] The thickness of the second retardation layer 8 is preferably 10 μm to 50 μm, and most preferably 20 μm to 40 μm.
[0088] The in-plane retardation Re(550) of the second retardation layer 8 is preferably from 10 nm to 60 nm, more preferably from 20 nm to 50 nm, and further preferably from 30 nm to 40 nm.
[0089] As described above, the second retardation layer 8 preferably has refractive index characteristics that satisfy the relationship nz>nx>ny. The Nz coefficient of the second retardation layer 8 is preferably -10 to -0.1, and more preferably -5 to -1.
[0090] The second retardation layer 8 can be preferably disposed so that its slow axis is substantially perpendicular to the absorption axis of the polarizer 21 .
[0091] The second retardation layer 8 may be composed of any appropriate resin film that can satisfy the above-mentioned characteristics. Such a resin may typically be a polymer having a negative intrinsic birefringence. A polymer having a negative intrinsic birefringence refers to a polymer whose refractive index in the orientation direction becomes relatively small when the polymer is oriented by stretching or the like. Examples of polymers having a negative intrinsic birefringence include those in which a chemical bond or functional group having a large polarization anisotropy, such as an aromatic or carbonyl group, is introduced into the side chain of the polymer. Specific examples include modified polyolefin resins (e.g., modified polyethylene resins), acrylic resins, styrene resins, maleimide resins, fumaric acid ester resins, and the like. The second retardation layer 8 may be obtained, for example, by appropriately stretching a film formed from the above-mentioned resin.
[0092] In one embodiment of the present invention, the optical laminate 1 includes a first retardation layer 7 and a second retardation layer 8, but the optical laminate does not necessarily include the first retardation layer and / or the second retardation layer.
[0093] I. Panel side adhesive layer The panel-side pressure-sensitive adhesive layer 9 is located on the side opposite to the viewing side of the second retardation layer 8. The panel-side pressure-sensitive adhesive layer 9 is typically formed by coating any appropriate pressure-sensitive adhesive on the second retardation layer 8. The thickness of the panel-side pressure-sensitive adhesive layer 9 is preferably 1 μm to 60 μm, and more preferably 5 μm to 30 μm. In one embodiment of the present invention, the optical laminate 1 includes the panel-side pressure-sensitive adhesive layer 9, but the optical laminate does not necessarily need to include a panel-side pressure-sensitive adhesive layer.
[0094] J. Image display device The optical laminate described in the above items A to I can be applied to an image display device. Therefore, one embodiment of the present invention also includes an image display device using such an optical laminate. Representative examples of image display devices include liquid crystal display devices and organic EL display devices. The image display device according to the embodiment of the present invention typically includes the optical laminate described in the above items A to I on the viewing side. The image display device includes an image display panel. The image display panel includes an image display cell. The image display device may be referred to as an optical display device, the image display panel may be referred to as an optical display panel, and the image display cell may be referred to as an optical display cell. EXAMPLES
[0095] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring the various properties are as follows.
[0096] (1) Orange peel The optical laminates obtained in the examples and comparative examples were cut into a size of 200 mm x 300 mm to prepare test samples. In the test samples, the absorption axis direction (MD direction) of the polarizer was parallel to the width direction (direction perpendicular to the longitudinal direction) of the test samples. Next, the test samples were attached to a black acrylic plate by the panel-side adhesive layer. Light was irradiated from a fluorescent lamp to the surface of the visible side of the test sample attached to the acrylic plate at a reflection angle of 45° to 70°, and the appearance of the test sample (surface of the visible side) was visually observed. The results were evaluated according to the following criteria. A: Inconspicuous unevenness B: Visible unevenness C: Significantly noticeable unevenness
[0097] (2)Puncture test The optical laminates obtained in the examples and comparative examples were cut into a size of 5 cm x 5 cm to prepare test samples. Next, the test samples were attached to a glass plate having a thickness of 1.2 mm by the panel-side adhesive layer. The test sample attached to the glass plate was placed on the stage of an Indenter CMS tester (manufactured by Instron, product name: 5581) equipped with a piercing jig. The radius of curvature R of the tip of the piercing jig was 500 μm. The piercing jig was pierced with a load of 9 kg into the test sample on the stage in a room temperature (23°C ± 3°C) environment. The optical laminate and the standard polarizing plate after the piercing test were arranged so that the polarizer of the optical laminate and the polarizer of the standard polarizing plate were in a cross-Nicol state, and the light leakage was visually observed and evaluated according to the following criteria. A: No light leakage is observed. B: Light leakage is observed to such an extent that it may affect practical use. C: Light leakage is significant and practically unacceptable.
[0098] (3) Warping in high humidity environments The optical laminate obtained in the examples and comparative examples was cut to a size of 200 mm x 300 mm to be used as a viewer-side sample. In the viewer-side sample, the absorption axis direction (MD direction) of the polarizer was parallel to the width direction (direction perpendicular to the longitudinal direction) of the viewer-side sample. Then, the viewer-side sample was attached to the surface of a glass plate by a panel-side adhesive layer. The glass plate had a size of 210 mm x 310 mm, and the thickness of the glass plate was 550 μm. In addition, the laminate obtained in the manufacturing example was cut to a size of 200 mm x 300 mm to be used as a light source-side sample. In the light source-side sample, the absorption axis direction (MD direction) of the polarizer was parallel to the longitudinal direction of the light source-side sample. Then, the light source-side sample was attached to the back side of the glass plate by an adhesive layer. In this way, a test sample in which the viewer-side sample, the glass plate, and the light source-side sample were laminated was obtained. The test sample was then autoclaved for 15 minutes under normal conditions (50°C, 5 atm), and then allowed to stand for 48 hours under conditions of 23°C and 55% RH, and then allowed to stand for 48 hours under conditions of 65°C and 90% RH. The shape of the test sample was then visually observed and evaluated according to the following criteria. A: A concave shape is observed when the backlight side polarizing plate (light source side sample) is placed downward. B: When the backlight side polarizing plate (light source side sample) was placed on the bottom and observed, the shape was a convex shape. Furthermore, if the test sample has a convex shape after the high humidity test, it is understood that the upper viewer side sample (the optical laminate of the examples and comparative examples) has expanded more than the lower light source side sample (the laminate of the manufacturing example), and warping has occurred in the viewer side sample. On the other hand, if the test sample has a concave shape after the high humidity test, it is understood that in a high humidity environment, the lower light source side sample (the laminate of the manufacturing example) expands more than the upper viewer side sample (the optical laminate of the examples and comparative examples), and warping of the viewer side sample is suppressed.
[0099] [Production Example 1] A polarizing plate was obtained in the same manner as in "1. Preparation of polarizing plate (polarizer laminate)" described later. An acrylic adhesive (adhesive PSA2 described later) was applied to the surface of the polarizer opposite to the protective layer to form an adhesive layer. The thickness of the adhesive layer was 20 μm. In addition, a reflective polarizer film (product name: APF-T35, thickness: 38 μm) manufactured by 3M was attached to the surface of the protective layer (acrylic resin film) opposite to the polarizer via an acrylic adhesive (adhesive PSA3 described below). This formed an adhesive layer between the acrylic resin film and the reflective polarizer film. The thickness of the adhesive layer was 12 μm. In this manner, a laminate having a structure of pressure-sensitive adhesive layer / polarizing plate / pressure-sensitive adhesive layer / reflective polarizer film was obtained. <Preparation of adhesive PSA2> In a reaction vessel equipped with a cooling tube, a nitrogen inlet tube, a thermometer and a stirrer, 99 parts of butyl acrylate, 1.0 part of 4-hydroxybutyl acrylate and 0.3 parts of 2,2'-azobisisobutyronitrile were added together with ethyl acetate, and the mixture was reacted at 60°C for 4 hours under a nitrogen gas stream. Ethyl acetate was then added to the reaction solution to obtain a solution (solids concentration 30% by weight) containing an acrylic polymer A2 having a weight average molecular weight of 1.65 million. 100 parts of the solid content of the obtained acrylic polymer A2 solution was mixed with 0.3 parts of dibenzoyl peroxide (Niper BMT, manufactured by Nippon Oil & Fats Co., Ltd.), 0.1 parts of trimethylolpropane xylene diisocyanate (Takenate D110N, manufactured by Mitsui Takeda Chemical Co., Ltd.), and 0.2 parts of a silane coupling agent (A-100, an acetoacetyl group-containing silane coupling agent, manufactured by Soken Chemical Industries, Ltd.) to obtain an acrylic adhesive PSA2. <Preparation of adhesive PSA3> Into a four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser, 100 parts of butyl acrylate, 5 parts of acrylic acid, 0.1 parts of 2-hydroxyethyl acrylate, and 0.1 parts of 2,2'-azobisisobutyronitrile as a polymerization initiator were charged together with 100 g of ethyl acetate, and nitrogen gas was introduced while gently stirring to replace the atmosphere with nitrogen. The liquid temperature in the flask was then kept at around 55°C and a polymerization reaction was carried out for 8 hours, yielding a solution containing an acrylic polymer A3 having a weight average molecular weight of 2.2 million. 0.60 parts of an isocyanate crosslinking agent (Coronate L, manufactured by Tosoh Corporation) and 0.20 parts of a silane coupling agent (KBM403, manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed with 100 parts of the solid content of the obtained acrylic polymer A3 solution to obtain acrylic adhesive PSA3, which is a solution of an acrylic adhesive composition (solid content 11 wt%).
[0100] [Examples 1 to 3] 1. Preparation of polarizing plate (polarizer laminate) As a thermoplastic resin substrate, a long amorphous isophthalic copolymerized polyethylene terephthalate film (thickness: 100 μm) having a Tg of about 75° C. was used, and one side of the resin substrate was subjected to a corona treatment. A PVA aqueous solution (coating solution) was prepared by adding 13 parts by weight of potassium iodide to 100 parts by weight of a PVA-based resin made by mixing polyvinyl alcohol (polymerization degree 4200, saponification degree 99.2 mol%) and acetoacetyl-modified PVA (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., product name "GOHSEFFIMER") in a ratio of 9:1, and dissolving the mixture in water. The above PVA aqueous solution was applied to the corona-treated surface of a resin substrate and dried at 60° C. to form a PVA-based resin layer with a thickness of 13 μm, thereby producing a laminate. The obtained laminate was uniaxially stretched 2.4 times in the machine direction (longitudinal direction) in an oven at 130° C. (auxiliary air stretching treatment). Next, the laminate was immersed in an insolubilizing bath (a boric acid aqueous solution obtained by mixing 4 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (insolubilizing treatment). Next, the film was immersed in a dye bath (an aqueous iodine solution obtained by mixing iodine and potassium iodide in a weight ratio of 1:7 with 100 parts by weight of water) at a liquid temperature of 30°C for 60 seconds while adjusting the concentration so that the single transmittance (Ts) of the finally obtained polarizer would be the desired value (dyeing treatment). Next, the piece was immersed in a crosslinking bath (a boric acid aqueous solution obtained by mixing 3 parts by weight of potassium iodide and 5 parts by weight of boric acid with respect to 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (crosslinking treatment). Thereafter, the laminate was immersed in an aqueous boric acid solution (boric acid concentration: 4% by weight, potassium iodide concentration: 5% by weight) at a liquid temperature of 70°C and uniaxially stretched in the longitudinal direction (longitudinal direction) between rolls with different peripheral speeds to a total stretch ratio of 5.5 times (underwater stretching treatment). Thereafter, the laminate was immersed in a cleaning bath (an aqueous solution obtained by mixing 4 parts by weight of potassium iodide with 100 parts by weight of water) at a liquid temperature of 20° C. (cleaning treatment). Thereafter, the film was dried in an oven maintained at about 90° C. while being brought into contact with a SUS heated roll whose surface temperature was maintained at about 75° C. (drying shrinkage treatment). In this manner, a polarizer having a thickness of about 5 μm was formed on the resin substrate. An acrylic resin film (thickness: 40 μm) having a glutarimide structure as a protective layer was attached to the surface of the obtained polarizer (the surface opposite to the resin substrate) via an ultraviolet-curing adhesive. Specifically, the curing adhesive was applied so that the total thickness was about 2.0 μm, and the layers were attached using a rolling machine. Thereafter, the adhesive was cured by irradiating it with UV light from the acrylic resin film side. Next, the resin substrate was peeled off to obtain a polarizing plate having an acrylic resin film (protective layer) / polarizer configuration.
[0101] 2. Anti-glare laminate As the anti-glare laminate, a TAC film with a retardation layer (product name: HL214, thickness: 42 μm) manufactured by Fujifilm Corporation was used.
[0102] 3. Fabrication of Antireflective Laminate As the antireflection laminate, an AR film (AR+HC thickness: 4 μm, substrate thickness: 80 μm) manufactured by Dexerials Corporation was used.
[0103] 4. Preparation of Adhesive 4-1. Preparation of adhesive PSA1 used for the first adhesive layer to the third adhesive layer and the panel side adhesive layer A monomer mixture containing 94.9 parts of butyl acrylate, 0.1 parts of 4-hydroxybutyl acrylate, and 5.0 parts of acrylic acid was charged into a four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser. Furthermore, 0.1 parts of 2,2'-azobisisobutyronitrile as a polymerization initiator was charged together with 100 parts of ethyl acetate for 100 parts of this monomer mixture, and nitrogen gas was introduced while gently stirring to replace the atmosphere with nitrogen. The liquid temperature in the flask was kept at about 55°C, and a polymerization reaction was carried out for 8 hours to prepare a solution of acrylic polymer A1 with a weight average molecular weight (Mw) of 2.2 million and Mw / Mn=3.0. To 100 parts of the solid content of the acrylic polymer A1 solution, 3 parts of trimethylolpropane / tolylene diisocyanate adduct (manufactured by Tosoh Corporation, product name "Coronate L"), 0.2 parts of peroxide crosslinking agent (benzoyl peroxide), 0.075 parts of epoxy group-containing silane coupling agent (manufactured by Shin-Etsu Chemical Co., Ltd., product name "KBM-403"), and 0.5 parts of a polyether compound having a reactive silyl group (manufactured by Kaneka Corporation, product name "Silyl SAT10") were mixed to obtain adhesive PSA1. The adhesive constituting the adhesive layer was measured for storage modulus based on JIS K 7244 using a dynamic viscoelasticity measuring device "ARES" manufactured by Rheometrics Co., Ltd. The storage modulus of adhesive PSA1 at 23°C 55% RH was 0.11 GPa.
[0104] 5. Fabrication of Optical Laminates The anti-glare laminate was attached to the protective layer of the polarizing plate via the adhesive PSA1. Specifically, the adhesive PSA1 was applied to the viewing side surface of the protective layer to form a first adhesive layer having a thickness shown in Table 1, and then the anti-glare layer of the anti-glare laminate was brought into contact with the first adhesive layer, and the anti-glare laminate was attached to the polarizing plate via the first adhesive layer. At this time, the slow axis of the anti-glare layer (the layer in which the liquid crystal compound is oriented and solidified) was adjusted to form an angle of 45° with respect to the absorption axis of the polarizer. Next, an acrylic resin film (thickness: 40 μm) having a glutarimide structure as a reinforcing layer was attached to the first substrate of the anti-glare laminate via the adhesive PSA 1. Specifically, the adhesive PSA 1 was applied to the viewing side surface of the first substrate to form a second adhesive layer having the thickness shown in Table 1, and the reinforcing layer was brought into contact with the second adhesive layer and attached to the anti-glare laminate. Next, the antireflection laminate was attached to the reinforcing layer via the adhesive PSA 1. Specifically, the adhesive PSA 1 was applied to the surface of the reinforcing layer on the viewing side to form a third adhesive layer having the thickness shown in Table 1, and then the second substrate of the antireflection laminate was brought into contact with the second adhesive layer to attach the antireflection laminate to the reinforcing layer via the third adhesive layer. In addition, a cyclic olefin film (refractive index characteristics: nx>ny>nz, in-plane phase difference: 116 nm) was attached as a first phase difference layer to the surface of the polarizer opposite to the protective layer via a UV-curable adhesive. At this time, the slow axis of the first phase difference layer was adjusted to form an angle of 0° with respect to the absorption axis of the polarizer. After that, a modified polyethylene film (refractive index characteristics: nz>nx>ny, in-plane phase difference: 35 nm) was attached as a second phase difference layer to the surface of the first phase difference layer opposite to the polarizer via a UV-curable adhesive. At this time, the slow axis of the second phase difference layer was adjusted to form an angle of 90° with respect to the absorption axis of the polarizer. Next, the pressure-sensitive adhesive PSA1 was applied to the surface of the second retardation layer opposite to the first retardation layer to form a panel-side pressure-sensitive adhesive layer having a thickness shown in Table 1. As a result, an optical laminate having a structure of antireflection laminate / third adhesive layer / reinforcing layer / second adhesive layer / antireflection laminate / first adhesive layer / polarizing plate / first retardation layer / second retardation layer / panel side adhesive layer was obtained. The thickness of each layer of the optical laminate, the total thickness of the optical laminate, and the total thickness of the antireflection laminate, the reinforcing layer, and the antireflection laminate are shown in Table 1. The optical laminate was also subjected to the above orange peel test, piercing test (light leakage), and evaluation of warping in a high humidity environment. The results are shown in Table 2 together with the total thickness of the antireflection laminate, the reinforcing layer, and the antireflection laminate, and the thickness of each adhesive layer.
[0105] [Comparative Example 1] An optical laminate having a configuration of first adhesive layer / polarizing plate / first retardation layer / second retardation layer / panel-side adhesive layer was obtained in the same manner as in Example 2, except that only the first adhesive layer was formed on the viewing side of the polarizing plate and the thickness of the panel-side adhesive layer was changed to the value shown in Table 1.
[0106] [Comparative Example 2] An optical laminate having a configuration of anti-glare laminate / first adhesive layer / polarizing plate / first retardation layer / second retardation layer / panel-side adhesive layer was obtained in the same manner as in Comparative Example 1, except that only the first adhesive layer and anti-glare laminate were formed on the viewing side of the polarizing plate.
[0107] [Comparative Example 3] An optical laminate having a configuration of antireflection laminate / second pressure-sensitive adhesive layer / antireflection laminate / first pressure-sensitive adhesive layer / polarizing plate / first retardation layer / second retardation layer / panel-side pressure-sensitive adhesive layer was obtained in the same manner as in Comparative Example 1, except that no reinforcing layer was provided between the antireflection laminate and the antireflection laminate, and the antireflection laminate was bonded to the antireflection laminate via the second pressure-sensitive adhesive layer.
[0108] [Comparative Example 4] Except for changing the thicknesses of the first adhesive layer, the second adhesive layer, the third adhesive layer and the panel-side adhesive layer to the values shown in Table 1, an optical laminate having a configuration of antireflection laminate / second adhesive layer / antiglare laminate / first adhesive layer / polarizing plate / first retardation layer / second retardation layer / panel-side adhesive layer was obtained in the same manner as in Comparative Example 3.
[0109] [Comparative Example 5] An optical laminate having a configuration of antireflection laminate / fourth adhesive layer / second reinforcing layer / third adhesive layer / reinforcing layer / second adhesive layer / anti-reflection laminate / first adhesive layer / polarizing plate / first retardation layer / second retardation layer / panel-side adhesive layer was obtained in the same manner as in Example 2, except that a second reinforcing layer and a fourth adhesive layer were provided between the third adhesive layer and the antireflection laminate, and the thickness of the panel-side adhesive layer was changed to the value shown in Table 1. The second reinforcing layer was an acrylic resin film (thickness: 40 μm) having a glutarimide structure. The fourth adhesive layer was formed by coating the adhesive PSA1 on the surface of the viewing side of the second reinforcing layer to a thickness shown in Table 1.
[0110] [Comparative Example 6] Except for changing the thickness of the reinforcing layer to 80 μm and the thickness of the panel-side adhesive layer to the values shown in Table 1, an optical laminate having a configuration of antireflection laminate / third adhesive layer / reinforcing layer / second adhesive layer / anti-glare laminate / first adhesive layer / polarizing plate / first retardation layer / second retardation layer / panel-side adhesive layer was obtained in the same manner as in Example 2.
[0111] [Comparative Example 7] Except for changing the anti-reflection laminate from a TAC film with a retardation layer manufactured by FUJIFILM Corporation (product name: HL214, thickness: 42 μm) to a polycarbonate-based anti-reflection film manufactured by Nitto Denko Corporation (thickness 82 μm) and changing the thickness of the panel-side adhesive layer to the value shown in Table 1, an optical laminate having a configuration of anti-reflection laminate / third adhesive layer / reinforcing layer / second adhesive layer / anti-reflection laminate / first adhesive layer / polarizing plate / first retardation layer / second retardation layer / panel-side adhesive layer was obtained in the same manner as in Example 2.
[0112] [Table 1]
[0113] [Table 2]
[0114] [evaluation] As is clear from Table 2, by making the thickness of each adhesive layer 17 μm or less, providing a reinforcing layer between the anti-glare laminate and the anti-reflection laminate, and making the total thickness of the anti-glare laminate, reinforcing layer and anti-reflection laminate 200 μm or less, it is possible to obtain an optical laminate that satisfies in a balanced manner the suppression of orange peel, resistance to localized loads, and suppression of warping in high humidity environments. [Industrial Applicability]
[0115] The optical laminate of the present invention can be suitably used in image display devices (typically, liquid crystal display devices and organic EL display devices). [Explanation of symbols]
[0116] 1 Optical laminate 2. Polarizing plate 21 Polarizer 22 Protective layer 3 Anti-glare laminate 31 First substrate 32 Anti-glare layer 4. Anti-reflective laminate 41 Second substrate 42 Hard coat layer 43 Anti-reflection layer 5 Reinforcement layer 61 First adhesive layer 62 Second adhesive layer 63 Third adhesive layer 7 First retardation layer 8 Second retardation layer
Claims
1. A polarizing plate; a first optical functional body attached to the viewing side of the polarizing plate via a first pressure-sensitive adhesive layer; a reinforcing layer bonded to the viewing side of the first optical function body via a second pressure-sensitive adhesive layer; a second optical functional body bonded to the visible side of the reinforcing layer via a third pressure-sensitive adhesive layer, each of the first pressure-sensitive adhesive layer, the second pressure-sensitive adhesive layer and the third pressure-sensitive adhesive layer has a thickness of 17 μm or less; the sum of the thickness of the first optical functional body, the thickness of the reinforcing layer, and the thickness of the second optical functional body is 200 μm or less; The thickness of the reinforcing layer is 50 μm or less, The thickness of the first optical functional body is 20 μm to 60 μm, The thickness of the second optical functional body is 40 μm to 100 μm, The thickness of the optical laminate is 310 μm or less, The polarizing plate is A polarizer; a protective layer attached to the viewing side of the polarizer and in contact with the first pressure-sensitive adhesive layer; The thickness of the protective layer is 60 μm or less, the first optical functional body is bonded to the protective layer via the first pressure-sensitive adhesive layer, the second optical functional body has an outermost layer located on the outermost surface of the optical laminate, The moisture permeability of the outermost layer was measured in accordance with the moisture permeability test (cup method) of JIS Z0208, in an atmosphere of 40° C. temperature and 92% RH, over an area of 1 m 2 It is measured as the amount of water vapor (g) passing through a sample of 0.1 g / mm 2 is as follows: The outermost layer of the optical laminate is an anti-reflection layer or an anti-fouling layer.
2. The first optical function body is an anti-glare laminate, The anti-glare laminate is an anti-glare layer in contact with the first pressure-sensitive adhesive layer; The optical laminate according to claim 1 , further comprising: a first substrate disposed on the viewing side of the anti-glare layer and in contact with the second pressure-sensitive adhesive layer.
3. The second optical functional body is an anti-reflection laminate, The antireflection laminate comprises: a second substrate in contact with the third pressure-sensitive adhesive layer; A hard coat layer disposed on the viewing side of the second substrate; The optical laminate according to claim 1 or 2, further comprising an antireflection layer disposed on a viewing side of the hard coat layer.
4. The optical laminate according to claim 3 , wherein the antireflection layer is the outermost layer.
5. The optical laminate according to claim 1 , wherein the polarizer has a thickness of 10 μm or less.
6. Further comprising a first retardation layer and a second retardation layer disposed in this order from the polarizing plate side on the side opposite to the viewing side of the polarizing plate, The first retardation layer exhibits a refractive index characteristic of nx>ny>nz, The optical laminate according to any one of claims 1 to 5, wherein the second retardation layer exhibits a refractive index characteristic of nz>nx>ny.
Citation Information
Patent Citations
JP155998A
Laminated optical film, elliptically polarizing plate and image display device
JP2008046147A
Polarizing plate with Anti-reflection layer and manufacturing method therefor
JP2019086605A
Retardation layer-laminated polarizing plate and image display device using the same
JP2020134678A
Image display device and method for manufacturing said image display device