Molded product, welding method, and manufacturing method of molded product

By controlling the molten pool area and composition in laser welding polyamide resin components, the method enhances bonding strength and appearance, addressing reliability issues in complex-shaped parts like battery cases and camera modules.

JP7557643B2Active Publication Date: 2024-09-27ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024028548
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-04-22
Filing Date
2024-02-28
Publication Date
2024-09-27
Estimated Expiration
2043-01-23

AI Technical Summary

Technical Problem

Existing laser welding methods for polyamide resin components, such as those used in battery cases and electronic equipment, face challenges in achieving high bonding strength, reliability, and maintaining good appearance characteristics, with issues like interfacial peeling and base material failure, while also requiring complex molds and processes.

Method used

The method involves laser welding a transparent resin member and an absorbent resin member, with specific control over the molten pool area in the joint, using a resin composition that includes polyamide resin, fillers, and flame retardants, and optimizing the thickness and light transmittance of the transparent resin member to enhance bonding strength and appearance.

Benefits of technology

This approach results in molded products with improved joint strength, reliability, and appearance characteristics, suitable for applications like lithium secondary battery housings and camera modules, by ensuring efficient energy transfer and minimizing surface defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007557643000012
    Figure 0007557643000012
  • Figure 0007557643000009
    Figure 0007557643000009
  • Figure 0007557643000013
    Figure 0007557643000013
Patent Text Reader

Abstract

To provide a molded article excellent in joint strength, reliability of the joint and appearance characteristics of the joint, a manufacturing method of the molded article, and a laser welding method.SOLUTION: A molded article according to the present disclosure is a molded article obtained by laser welding of a transmission resin member and an absorption resin member. The molded article comprises a joint in which the transmission resin member and the absorption resin member are joined by laser welding. A molten pool is observed in the joint in cross-sectional section that includes a normal of the transmission resin member or the absorption resin member and is perpendicular to the scanning direction of a laser beam. The area of the molten pool is 0.210 mm2 to 1.00 mm2. The transmission resin member and the absorption resin member are each molded from a resin composition. The resin composition contains a thermoplastic resin, the thermoplastic resin contains at least a polyamide-based resin (A1), and the resin composition has a glass transition temperature of 85°C or higher.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a molded article, a welding method, and a method for manufacturing a molded article. [Background technology]

[0002] Polyamide resin, a representative engineering plastic, is easy to process and has excellent mechanical properties, electrical properties, heat resistance, and other physical and chemical properties, which is why it is widely used in vehicle parts, electrical and electronic equipment parts, and other precision equipment parts.

[0003] Recently, parts with complex shapes have also come to be manufactured from polyamide resins. For example, in order to make the battery cases of lithium secondary batteries into sealed structures, various joining techniques, such as adhesives, vibration welding, ultrasonic welding, hot plate welding, injection welding, and laser welding, are used.

[0004] However, welding with an adhesive not only requires time to harden, but also poses problems such as environmental pollution. Problems have been pointed out with ultrasonic welding and hot plate welding, including damage to the product due to vibration and heat, and the generation of wear powder and burrs that require post-processing. Furthermore, injection welding often requires special molds and molding machines, and furthermore, it cannot be used if the material has low fluidity.

[0005] On the other hand, laser welding is a method in which a resin material that is transparent (also called non-absorbent or weakly absorbent) to laser light (hereinafter sometimes referred to as a "transmissive resin material") and a resin material that is absorbent to laser light (hereinafter sometimes referred to as an "absorbent resin material") are brought into contact with each other and welded together to join the two resin materials.

[0006] Specifically, this method irradiates the joining surface with laser light from the side of the transparent resin member, and melts the absorptive resin member that forms the joining surface with the energy of the laser light to join them. Laser welding does not generate abrasion powder or burrs, and causes little damage to precision parts and products such as circuit boards inside housings. Furthermore, polyamide resin itself is a material with a relatively high laser transmittance, so processing polyamide resin products using laser welding technology has recently attracted attention.

[0007] The above-mentioned transparent resin member is usually obtained by molding a light-transmitting resin composition. As such a light-transmitting resin composition, in the examples of Patent Document 1, the laser welding strength of a resin composition consisting of polyamide 66, polyamide 6I, glass fiber, and a flame retardant is disclosed. In Patent Document 2, the laser welding strength of a resin composition consisting of polyamide 66, glass fiber, and a flame retardant is disclosed. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2020-193333 A [Patent Document 2] JP 2019-25673 A Summary of the Invention [Problem to be solved by the invention]

[0009] In recent years, laser welding processing has been increasing, and there is a tendency for high bonding strength to be required from the viewpoint of ensuring product reliability and safety. The bonding strength of the examples disclosed in Patent Documents 1 and 2 is not sufficient in practical terms, and higher bonding strength is required. Not only the bonding strength but also the destruction mode is important. The destruction mode is preferably not interfacial peeling at the bonding surface, but rather base material destruction in which the bonded resin composition breaks or the resin around the bonding part is torn off together to include the bonding part. The reason for this is that base material destruction means that the bonding part has sufficient bonding strength and there is no defect in the bonding process, and that the reliability of the bonding part is high. In addition, molded products manufactured by laser welding require design in addition to joint strength, so the appearance characteristics of the joints are also required. The present invention has been made in consideration of the above circumstances, and has an object to provide a molded product having excellent bonding strength, reliability of the bonded portion, and appearance characteristics of the bonded portion, a method for manufacturing a molded product, and a laser welding method. [Means for solving the problem]

[0010] As a result of extensive research into achieving the above object, the present inventors have found that the above problems can be solved by setting the area of ​​the molten joint portion of the laser welded portion to a specific range. The present invention includes the following aspects. [1] A molded product in which a transparent resin member and an absorptive resin member are laser-welded, the molded product having a joint where the transparent resin member and the absorptive resin member are joined by laser welding, a molten pool is observed at the joint in a cross section that includes a normal to the transparent resin member or the absorptive resin member and is perpendicular to the scanning direction of the laser beam, and the area of ​​the molten pool is 0.210 mm 2 Over 1.00mm 2 The molded product according to claim 1, wherein the transparent resin member and the absorptive resin member are each molded from a resin composition, the resin composition contains a thermoplastic resin, the thermoplastic resin contains at least a polyamide-based resin (A1), and the resin composition has a glass transition temperature of 85°C or higher. [2] The molded article according to [1], wherein the resin composition contains a filler (B). [3] The molded product according to [1] or [2], wherein the light transmittance of the transparent resin member for a light wavelength of 940 nm is 30% or more. [4] The molded product according to any one of [1] to [3], wherein the transparent resin member has a thickness of 0.3 mm or more and 5 mm or less. [5] The molded article according to any one of [1] to [4], wherein the resin composition contains 0 parts by mass or more and 150 parts by mass or less of a filler (B) per 100 parts by mass of the thermoplastic resin. [6] The molded article according to any one of [2] to [5], wherein the filler (B) is one or more of glass fiber, calcium carbonate, talc, mica, wollastonite, and milled fiber. [7] The molded article according to any one of [1] to [6], wherein the polyamide resin (A1) is a semi-aromatic polyamide (A1-2) containing an aromatic ring in the skeleton, or an alloy of the semi-aromatic polyamide (A1-2) and an aliphatic polyamide (A1-1). [8] The molded article according to [7], wherein the content of the semi-aromatic polyamide (A1-2) is 5.0 parts by mass or more and 100.0 parts by mass or less relative to 100.0 parts by mass in total of the aliphatic polyamide (A1-1) and the semi-aromatic polyamide (A1-2). [9] The molded article according to [7] or [8], wherein the content of an isophthalic acid component in 100 mol % of dicarboxylic acid components constituting the semi-aromatic polyamide (A1-2) is 10 mol % or more.

[10] The molded article according to any one of [1] to [9], wherein the resin composition contains a flame retardant (C).

[11] The molded article according to

[10] , wherein the flame retardant (C) is either or both of a phosphinate and a diphosphinate.

[12] The molded article according to

[11] , wherein the phosphinate is a compound represented by the following general formula (I) and the diphosphinate is a compound represented by the following general formula (II):

[0011] [ka] (In general formula (I), R 11 and R 12 Each of M is independently an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 10 carbon atoms. n11+ is a metal ion having a valence of n11. M is an element belonging to Group 2 or Group 15 of the periodic table, a transition element, zinc, or aluminum. n11 is 2 or 3. When n11 is 2 or 3, multiple R 11 and R 12may be the same or different. In general formula (II), R 21 and R 22 Each of Y is independently an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 10 carbon atoms. 21 M' is an alkylene group having 1 to 10 carbon atoms or an arylene group having 6 to 10 carbon atoms. m21+ is a metal ion having a valence of m21. M' is an element belonging to Group 2 or Group 15 of the periodic table, a transition element, zinc, or aluminum. n21 is an integer of 1 to 3. When n21 is 2 or 3, multiple R 21 , R 22 and Y 21 may be the same or different. m21 is 2 or 3. x is 1 or 2. When x is 2, multiple M' may be the same or different. n21, x, and m21 are integers that satisfy the relational formula 2×n21=m21×x.

[13] The molded article according to any one of [1] to

[12] , wherein the resin composition further contains (D) a colorant.

[14] The molded article according to any one of [1] to

[13] , wherein the resin composition forming the absorbing resin member contains a colorant (D1) for absorbing a laser.

[15] The molded product according to any one of [1] to

[13] , wherein the resin composition forming the transmissive resin member contains a colorant (D2) that transmits a laser.

[16] The molded article according to any one of [1] to

[15] , having a sealed structure joined by laser welding.

[17] The molded article according to any one of [1] to

[16] , which is for use in a battery case for a lithium secondary battery, a sensor case, a camera case, a housing for an image or video shooting part, a magnet switch housing, a breaker housing, a connector, a housing for a secondary battery, a current sensor case, a camera module housing, a camera module, or a lens barrel.

[18] A method for laser welding a transmissive resin member and an absorptive resin member, the transmissive resin member and the absorptive resin member being molded from a resin composition, the resin composition containing a thermoplastic resin, and by laser welding the transmissive resin member and the absorptive resin member, in a cross section including a normal to the transmissive resin member or the absorptive resin member and perpendicular to the scanning direction of a laser beam, the area of ​​a molten pool observed at the laser-welded joint is 0.210 mm 2 Over 1.00mm 2 A welding method which produces a molded product as follows:

[19] A method for producing a molded article using the welding method described in

[18] . Effect of the Invention

[0012] According to the present invention, it is possible to provide a molded article having excellent joint strength, reliability of the joint, and appearance characteristics of the joint, a method for manufacturing a molded article, and a laser welding method. [Brief description of the drawings]

[0013] [Figure 1] FIG. 2 is a cross-sectional photograph of an example of a molded product of the present embodiment. [Diagram 2] FIG. 2 is a cross-sectional photograph of an example of a molded product of the present embodiment. [Diagram 3] FIG. 2 is a schematic diagram for explaining laser welding. [Figure 4] FIG. 4 is a schematic diagram for explaining a method for measuring a bonding strength. [Diagram 5] FIG. 13 is a schematic diagram for explaining a method for obtaining a cross section of a molded product. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, an embodiment for carrying out the present invention (hereinafter, simply referred to as "the present embodiment") will be described in detail. The present embodiment is an example for explaining the present invention, and is not intended to limit the present invention to the following content. The present invention can be carried out by appropriately modifying it within the scope of its gist.

[0015] In this specification, the term "polyamide" refers to a polymer having an amide (-NHCO-) ​​group in the main chain.

[0016] <Molded products> This embodiment is a molded product in which a transmissive resin member and an absorptive resin member are laser welded together. The molded product of this embodiment has joints formed by laser welding. In this specification, the "joint portion" refers to the portion where the transmissive resin member and the absorbing resin member are joined by laser welding, whereby the absorbing resin member melts, the transmissive resin member melts as it receives heat from the molten portion, and these molten areas solidify in a contacting state.

[0017] The molded product may have one or more "joints" in the molded product. By having joints, it is expected that the molded product can have effects such as joining parts together to form a composite body or forming a sealed structure.

[0018] The laser irradiation path is not particularly limited, but for example, when joining parts, it can be an open path with a start point and an end point separated from each other, and when producing a molded product having a sealed structure, it can be a closed path with an end point overlapping any point on the path (including the start point). The shape of the open path is not particularly limited, and may be a straight line, a curve, or a combination of these. The shape of the closed path is not particularly limited, and can be appropriately adjusted depending on the shape of the molded product having a sealed structure.

[0019] The molded product of this embodiment only needs to have at least a permeable resin member and an absorptive resin member joined together, and the permeable resin member and the absorptive resin member may be joined at two or more points each.

[0020] The transmissive resin member is a member through which the laser light passes. The absorptive resin material is a material that absorbs laser light, generates heat, and melts.

[0021] In the molded article of this embodiment, a molten pool is observed at the joint in a cross section that includes the normal to the transmitting resin member or the absorbing resin member and is perpendicular to the scanning direction of the laser beam. As shown in Fig. 5, a normal line N of the transmissible resin member 1 or the absorptive resin member 2 is defined. The normal line N is a line perpendicular to the tangent plane. If the transmissible resin member 1 or the absorptive resin member 2 is a curved surface, the normal line N is a line perpendicular to the tangent line of the curved surface. In this specification, the optical axis of a laser beam means an axis that coincides with the traveling direction of the laser beam. In the flood head type, in which the laser irradiation port itself moves, the direction of movement of the laser irradiation port is the scanning direction of the laser beam. In a galvanometer type laser, which is operated by the angle of a mirror installed at a fixed irradiation port, the direction of travel of the laser beam reflected by the mirror is set as the scanning direction of the laser beam. In FIG. 5, La1 and La2 are the optical axes of the laser beams, and La is the scanning direction of the laser beam. In the molded product of this embodiment, a molten pool is observed in a cross section S that includes a normal N of the transmitting resin member or the absorbing resin member and is perpendicular to the scanning direction La of the laser beam. The molten pool refers to a region where the absorbing resin member has melted and the adjacent transmitting resin member has also melted and then resolidified.

[0022] An example of a cross section of a molded product of this embodiment is shown in Figure 1. Figure 1 is an optical microscope photograph of a cross section including a joint portion of a molded product of this embodiment, exposed on a cross section that includes a normal line of the transmitting resin member or the absorbing resin member and is perpendicular to the scanning direction of the laser beam. The observation magnification is appropriately selected so that the entire molten pool fits within the field of view. As an example, the magnification of Figure 1 is 50 times.

[0023] In the cross section of the molded product shown in FIG. 1, a molten pool 3 is observed between the permeable resin member 1 and the absorbing resin member 2.

[0024] Similarly, an example of a cross section of a molded product of this embodiment is shown in Figure 2. The width of the molten pool is the length x of the longest diameter, and the height of the molten pool is the maximum diameter y perpendicular to x.

[0025] The area of ​​the molten pool is 0.21 mm 2 Over 1.00mm 2 Less than 0.22mm 2 More than 0.85mm 2 Less than 0.23mm is preferable 2 More than 0.65mm 2 The following is more preferred: When the molten pool area is equal to or greater than the lower limit, the bonding strength is improved, whereas when the molten pool area is equal to or less than the upper limit, a molded product having a good appearance and no processing marks on the surface of the molded product can be obtained.

[0026] [Method of measuring the area of ​​the molten pool] The area of ​​the molten pool of the molded product is determined by obtaining a cross section of the molded product by the following method, and then calculating the area of ​​the molten pool by the following method.

[0027] How to obtain a cross section First, the molded product is cut to expose a cross section including the joint portion. At this time, the molded product is cut in a direction that includes the normal line of the transmitting resin member or the absorbing resin member and is perpendicular to the scanning direction of the laser beam. The exposed cross section is observed with an optical microscope to obtain an optical microscope image. For example, a VHX6000 manufactured by Keyence Corporation can be used as the optical microscope. The magnification at this time is 50 times.

[0028] How to calculate the area of ​​the molten pool The optical microscope image of the cross section of the molded product obtained by the above-mentioned method can be measured using the function of calculating the area of ​​a specified area of ​​the device. The area designation for measuring the area of ​​the molten pool is performed by designating the outer periphery of the molten pool so that it passes through both ends of the maximum diameter length x and both ends of the maximum diameter y perpendicular to x as shown in Figure 2. An example of the area designation is shown by the dashed line in Figure 2.

[0029] In order to clearly observe the molten pool, the laser welded portion may be cut with a band saw or saw and then polished before observation.

[0030] The method of polishing is not particularly limited, but a rotary polishing machine is preferred as the polishing method because it can polish the observation area uniformly.

[0031] In order to observe the molten pool more clearly, the observation portion may be subjected to an etching process.

[0032] The etching method is not particularly limited, but chemical etching that attacks the target material is preferred.

[0033] For example, in the case of polyamide, inorganic acids, particularly hydrochloric acid, sulfuric acid, and formic acid, are suitable as etching agents.

[0034] The molded article of the present embodiment has the above-described configuration, and thus can have sufficient bonding strength by laser welding and a good appearance.

[0035] In the molded product of this embodiment, by setting the light transmittance of the transmissive resin member to 30% or more for a light wavelength of 940 nm, sufficient energy is transmitted to the absorptive resin member, allowing efficient processing.

[0036] The thickness of the transparent resin member is not particularly limited as long as the light transmittance for a light wavelength of 940 nm is 30% or more, but the thickness is preferably 0.3 mm or more and 5 mm or less, more preferably 0.5 mm or more and 4 mm or less, even more preferably 0.7 mm or more and 3 mm or less, and most preferably 0.9 mm or more and 2 mm or less. If the thickness of the transmissive resin member is smaller than the above-mentioned lower limit, when a load is applied to the joint, the member itself will be damaged. On the other hand, if the thickness is equal to or greater than the above-mentioned lower limit and equal to or less than the above-mentioned upper limit, the light transmittance is increased and energy can be efficiently transmitted to the absorbing resin member.

[0037] [Method of measuring light transmittance] The light transmittance of the transparent resin member is measured by the following method after a molded article is obtained by the following method.

[0038] Acquisition of transparent resin components Permeable resin parts can be obtained by various processing techniques such as injection molding, extrusion molding, heat pressing, etc. Among them, injection molding has small compositional variation inside the molded product, and is suitable for creating reproducible test pieces (permeable resin parts).

[0039] How to measure light transmittance The light transmittance of the transparent resin member obtained by the above-mentioned method can be measured using a spectrophotometer. For example, the spectrophotometer can be a combination of a JASCO Corporation (V670) and an integrating sphere "ILN-725". Since the light transmitted through the resin is scattered, it is preferable to use an integrating sphere to collect the scattered light.

[0040] The molded article of this embodiment preferably has a sealed structure joined by laser welding. More specifically, the molded article of this embodiment is preferably a housing for a lithium ion secondary battery, a current sensor, a camera module housing, a camera module, or a lens barrel.

[0041] Next, the resin composition constituting the molded article of this embodiment will be described below.

[0042] ≪Resin composition≫ The transmissive resin member and the absorptive resin member are each formed from a resin composition containing a thermoplastic resin.

[0043] [Thermoplastic resin] Examples of thermoplastic resins include polyamide-based resins, polyester-based resins, polyacetal-based resins, polycarbonate-based resins, polyacrylic-based resins, polyphenylene ether-based resins (including modified polyphenylene ethers obtained by blending or graft polymerizing polyphenylene ethers with other resins), polyarylate-based resins, polysulfone-based resins, polyphenylene sulfide-based resins, polyethersulfone-based resins, polyketone-based resins, polyphenylene ether ketone-based resins, polyimide-based resins, polyamideimide-based resins, polyetherimide-based resins, polyurethane-based resins, polyolefin-based resins (e.g., α-olefin (co)polymers), and various ionomers.

[0044] The thermoplastic resin is preferably a crystalline resin having a melting point in the range of 100° C. to 350° C., an amorphous resin having a glass transition temperature in the range of 50° C. to 250° C., or a combination thereof. The melting point of the crystalline resin referred to here is the peak top temperature of the endothermic peak that appears when the temperature is increased from 23°C at a rate of 10°C / min using a differential scanning calorimeter (DSC). When two or more endothermic peaks appear, it refers to the peak top temperature of the endothermic peak on the highest temperature side. The enthalpy of the endothermic peak at this time is preferably 10 J / g or more, and more preferably 20 J / g or more. In addition, when measuring, it is desirable to use a sample that is heated once to a temperature condition of the melting point + 20°C or more to melt the resin, and then cooled to 23°C at a rate of 10°C / min.

[0045] The glass transition temperature Tg of the amorphous resin referred to here means the peak top temperature at which the storage modulus is greatly reduced and the loss modulus is maximized when measured using a dynamic viscoelasticity measuring device at an applied frequency of 8 Hz while heating from 23 ° C. at a heating rate of 2 ° C. / min. When two or more peaks of the loss modulus appear, it refers to the peak top temperature of the peak on the highest temperature side. In this case, the measurement frequency is at least once every 20 seconds to improve the measurement accuracy. There is no particular restriction on the method of preparing the measurement sample, but from the viewpoint of eliminating the influence of molding distortion, it is desirable to use a cut piece of a hot press molded product, and from the viewpoint of heat conduction, it is desirable that the size (width and thickness) of the cut piece is as small as possible.

[0046] The thermoplastic resin may be a homopolymer or a copolymer.

[0047] The thermoplastic resin may be any one of the above resins or a combination of two or more of them. The thermoplastic resin may be any one of the above resins modified with at least one compound selected from unsaturated carboxylic acids, their acid anhydrides, and their derivatives.

[0048] As the thermoplastic resin, from the viewpoints of heat resistance, moldability, designability, and mechanical properties, one or more resins selected from the group consisting of polyolefin-based resins, polyamide-based resins, polyester-based resins, polyacetal-based resins, polyacrylic-based resins, polyphenylene ether-based resins, and polyphenylene sulfide-based resins are preferable.

[0049] In this embodiment, the thermoplastic resin contains at least a polyamide resin (A1). This improves the joining strength by laser welding and improves the appearance of the joining portion. The polyamide resin (A1) may be used alone or in combination with other thermoplastic resins.

[0050] (Polyamide resin (A1)) The polyamide resin (A1) is preferably a semi-aromatic polyamide (A1-2) having an aromatic ring in the skeleton, or an alloy of an aliphatic polyamide (A1-1) and a semi-aromatic polyamide (A1-2). This improves the joining strength during laser welding and improves the appearance of the joining portion. When the polyamide resin (A1) is an alloy, the thermoplastic resin may be an alloy of three or more kinds in which other thermoplastic resins are further used in combination.

[0051] When the polyamide-based resin (A1) is the above-mentioned alloy, the contents of the aliphatic polyamide (A1-1) and the semi-aromatic polyamide (A1-2) in the polyamide-based resin (A1) are not particularly limited. In particular, the content of the semi-aromatic polyamide (A1-2) relative to a total of 100.0 parts by mass of the aliphatic polyamide (A1-1) and the semi-aromatic polyamide (A1-2) is preferably 5.0 parts by mass or more and 100.0 parts by mass or less, more preferably 5.0 parts by mass or more and 95.0 parts by mass or less, even more preferably 10.0 parts by mass or more and 80.0 parts by mass or less, and even more preferably 15.0 parts by mass or more and 70.0 parts by mass or less.

[0052] Furthermore, relative to 100.0 parts by mass in total of the aliphatic polyamide (A1-1) and the semi-aromatic polyamide (A1-2), the content of the aliphatic polyamide (A1-1) is preferably from 0.0 to 95.0 parts by mass, more preferably from 5.0 to 95.0 parts by mass, even more preferably from 7.0 to 80.0 parts by mass, and even more preferably from 9.0 to 70.0 parts by mass.

[0053] When the content of each of the aliphatic polyamide (A1-1) and the semi-aromatic polyamide (A1-2) is within the above-mentioned numerical range relative to 100 parts by mass in total of the aliphatic polyamide (A1-1) and the semi-aromatic polyamide (A1-2), the joining strength during laser welding can be improved and the appearance of the joined portion can be improved.

[0054] (1) Aliphatic polyamide (A1-1) The constituent units of the aliphatic polyamide (A1-1) preferably satisfy at least one of the following conditions (1) and (2). (1) It contains an aliphatic dicarboxylic acid unit (A1-1a) and an aliphatic diamine unit (A1-1b). (2) It contains at least one structural unit (A1-1c) selected from the group consisting of lactam units and aminocarboxylic acid units.

[0055] The constituent units of the aliphatic polyamide (A1-1) may contain one or more polyamides that satisfy at least one of the above conditions (1) and (2). In particular, the constituent units of the aliphatic polyamide (A1-1) preferably satisfy the above condition (1).

[0056] (1-1) Aliphatic dicarboxylic acid unit (A1-1a) Examples of the aliphatic dicarboxylic acid constituting the aliphatic dicarboxylic acid unit (A1-1a) include linear or branched saturated aliphatic dicarboxylic acids having 3 to 20 carbon atoms.

[0057] Examples of linear saturated aliphatic dicarboxylic acids having 3 to 20 carbon atoms include, but are not limited to, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, tetradecanedioic acid, hexadecanedioic acid, octadecanedioic acid, eicosane dioic acid, and diglycolic acid.

[0058] Examples of branched saturated aliphatic dicarboxylic acids having 3 to 20 carbon atoms include, but are not limited to, dimethylmalonic acid, 2,2-dimethylsuccinic acid, 2,3-dimethylglutaric acid, 2,2-diethylsuccinic acid, 2,3-diethylglutaric acid, 2,2-dimethylglutaric acid, 2-methyladipic acid, and trimethyladipic acid.

[0059] The aliphatic dicarboxylic acids constituting the aliphatic dicarboxylic acid unit (A1-1a) may be used alone or in combination of two or more.

[0060] Among these, the aliphatic dicarboxylic acid constituting the aliphatic dicarboxylic acid unit (A1-1a) is preferably a linear saturated aliphatic dicarboxylic acid having 6 or more carbon atoms, since the resin composition tends to have better heat resistance, fluidity, toughness, low water absorption, rigidity, and the like.

[0061] Specific examples of preferred linear saturated aliphatic dicarboxylic acids having 6 or more carbon atoms include adipic acid, sebacic acid, dodecanedioic acid, tetradecanedioic acid, hexadecanedioic acid, octadecanedioic acid, and eicosane dioic acid. Among these, from the viewpoint of the heat resistance of the resin composition, adipic acid, sebacic acid, or dodecanedioic acid is preferred as the linear saturated aliphatic dicarboxylic acid having 6 or more carbon atoms.

[0062] In addition, the aliphatic polyamide (A1-1) may further contain a unit derived from a trivalent or higher polycarboxylic acid, if necessary, within a range that does not impair the effects of the molded article of this embodiment. Examples of trivalent or higher polycarboxylic acids include trimellitic acid, trimesic acid, and pyromellitic acid. These trivalent or higher polycarboxylic acids may be used alone or in combination of two or more.

[0063] (1-2) Aliphatic diamine unit (A1-1b) Examples of the aliphatic diamine constituting the aliphatic diamine unit (A1-1b) include linear saturated aliphatic diamines having 2 to 20 carbon atoms, and branched saturated aliphatic diamines having 3 to 20 carbon atoms.

[0064] Examples of linear saturated aliphatic diamines having 2 to 20 carbon atoms include, but are not limited to, ethylenediamine, propylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, undecamethylenediamine, dodecamethylenediamine, tridecamethylenediamine, and the like.

[0065] Examples of branched saturated aliphatic diamines having 3 to 20 carbon atoms include, but are not limited to, 2-methylpentamethylenediamine (also referred to as 2-methyl-1,5-diaminopentane), 2,2,4-trimethylhexamethylenediamine, 2,4,4-trimethylhexamethylenediamine, 2-methyl-1,8-octanediamine (also referred to as 2-methyloctamethylenediamine), 2,4-dimethyloctamethylenediamine, and the like.

[0066] The aliphatic diamines constituting the aliphatic diamine unit (A1-1b) may be used alone or in combination of two or more.

[0067] Among them, the carbon number of the aliphatic diamine constituting the aliphatic diamine unit (A1-1b) is preferably 6 to 12, more preferably 6 to 10. When the carbon number of the aliphatic diamine constituting the aliphatic diamine unit (A1-1b) is equal to or more than the lower limit, the heat resistance of the molded article is more excellent. On the other hand, when the carbon number is equal to or less than the upper limit, the crystallinity and releasability of the molded article are more excellent.

[0068] Specific examples of preferred linear or branched saturated aliphatic diamines having 6 to 12 carbon atoms include hexamethylenediamine, 2-methylpentamethylenediamine, and 2-methyl-1,8-octanediamine.

[0069] Among these, hexamethylenediamine or 2-methylpentamethylenediamine is preferred as the linear or branched saturated aliphatic diamine having from 6 to 12 carbon atoms. By including such an aliphatic diamine unit (A1-1b), the heat resistance, rigidity, etc. of the molded article are more excellent.

[0070] In addition, the aliphatic polyamide (A1-1) may further contain a unit derived from a trivalent or higher polyvalent aliphatic amine, if necessary, within a range that does not impair the effects of the molded article of this embodiment. Examples of trivalent or higher polyvalent aliphatic amines include bishexamethylenetriamine.

[0071] (1-3) At least one structural unit (A1-1c) selected from the group consisting of lactam units and aminocarboxylic acid units The aliphatic polyamide (A1-1) may contain at least one structural unit (A1-1c) selected from the group consisting of lactam units and aminocarboxylic acid units. By containing such units, the resulting polyamide tends to have excellent toughness. The terms "lactam unit" and "aminocarboxylic acid unit" used herein refer to poly(condensed) lactam and aminocarboxylic acid.

[0072] Examples of lactams constituting the lactam unit include, but are not limited to, butyrolactam, pivalolactam, ε-caprolactam, caprylolactam, enantholactam, undecanolactam, laurolactam (dodecanolactam), and the like. Among them, the lactam constituting the lactam unit is preferably ε-caprolactam or laurolactam, and more preferably ε-caprolactam. By including such a lactam, the toughness of the molded article tends to be superior.

[0073] Examples of aminocarboxylic acids constituting the aminocarboxylic acid unit include, but are not limited to, ω-aminocarboxylic acids, which are compounds formed by ring-opening of lactams, and α,ω-amino acids.

[0074] The amino carboxylic acid constituting the amino carboxylic acid unit is preferably a linear or branched saturated aliphatic carboxylic acid having 4 to 14 carbon atoms and substituted with an amino group at the ω position. Examples of such amino carboxylic acids include, but are not limited to, 6-aminocaproic acid, 11-aminoundecanoic acid, and 12-aminododecanoic acid. Other examples of amino carboxylic acids include paraaminomethylbenzoic acid.

[0075] The lactam and aminocarboxylic acid constituting the structural unit (A1-1c) may each be used alone or in combination of two or more types.

[0076] The weight average molecular weight can be used as an index of the molecular weight of the aliphatic polyamide (A1-1). The weight average molecular weight of the aliphatic polyamide is preferably 10,000 to 50,000, more preferably 17,000 to 45,000, even more preferably 20,000 to 45,000, even more preferably 25,000 to 45,000, particularly preferably 30,000 to 45,000, and most preferably 35,000 to 40,000.

[0077] When the weight average molecular weight is within the above range, the joining strength during laser welding can be improved and the appearance of the joined portion can be improved. The weight average molecular weight of the aliphatic polyamide (A1-1) can be measured, for example, by using gel permeation chromatography (GPC).

[0078] (2) Semi-aromatic polyamide (A1-2) The semi-aromatic polyamide (A1-2) is a polyamide having an aromatic ring in the skeleton, and containing a diamine unit and a dicarboxylic acid unit.

[0079] The semi-aromatic polyamide (A1-2) preferably contains 10 mol % to 95 mol % of aromatic structural units, more preferably 20 mol % to 90 mol %, and even more preferably 30 mol % to 85 mol % of aromatic structural units, based on the total structural units of the semi-aromatic polyamide (A1-2). The term "aromatic structural units" as used herein means aromatic diamine units and aromatic dicarboxylic acid units.

[0080] Furthermore, the semi-aromatic polyamide (A1-2) preferably contains 10 mol % or more of aromatic dicarboxylic acid units, more preferably 30 mol % or more of aromatic dicarboxylic acid units, even more preferably 50 mol % or more of aromatic dicarboxylic acid units, and particularly preferably 70 mol % or more of aromatic dicarboxylic acid units, relative to 100 mol % of all dicarboxylic acid units in the semi-aromatic polyamide (A1-2).

[0081] When the content of the aromatic dicarboxylic acid unit is equal to or more than the above lower limit, the joining strength during laser welding can be improved and the appearance of the joined portion can be improved.

[0082] The aromatic dicarboxylic acid unit in the semi-aromatic polyamide (A1-2) is not particularly limited, but is preferably a terephthalic acid unit or an isophthalic acid unit, and more preferably an isophthalic acid unit.

[0083] The ratio of the predetermined monomer units constituting the semi-aromatic polyamide (A1-2) can be determined by nuclear magnetic resonance spectroscopy ( 1 H-NMR) or the like.

[0084] Specifically, for example, the semi-aromatic polyamide (A1-2) is dissolved in heavy hexafluoroisopropanol by heating to a concentration of about 5% by mass, and the resulting solution is analyzed using a nuclear magnetic resonance analyzer JNM ECA-500 manufactured by JEOL Ltd. 1By performing H-NMR analysis and calculating the integral ratio, the amounts of units composed of aromatic dicarboxylic acids, units composed of dicarboxylic acids other than aromatic dicarboxylic acids, units composed of aromatic diamines, and units composed of amines other than aromatic diamines that constitute the semi-aromatic polyamide (A1-2) can be calculated.

[0085] (2-1) Dicarboxylic acid unit (A1-2a) The dicarboxylic acid unit (A1-2a) is not particularly limited, and examples thereof include an aromatic dicarboxylic acid unit, an aliphatic dicarboxylic acid unit, and an alicyclic dicarboxylic acid unit.

[0086] (2-2-1) Aromatic dicarboxylic acid unit Examples of aromatic dicarboxylic acids constituting aromatic dicarboxylic acid units other than isophthalic acid units include, but are not limited to, dicarboxylic acids having an aromatic group such as a phenyl group, a naphthyl group, etc. The aromatic group of the aromatic dicarboxylic acid may be unsubstituted or may have a substituent.

[0087] The substituent is not particularly limited, but examples thereof include alkyl groups having 1 to 4 carbon atoms, aryl groups having 6 to 10 carbon atoms, arylalkyl groups having 7 to 10 carbon atoms, alkylaryl groups having 7 to 10 carbon atoms, halogen groups, silyl groups having 1 to 6 carbon atoms, sulfonic acid groups and salts thereof (such as sodium salts). Examples of the alkyl group having 1 to 4 carbon atoms include, but are not limited to, a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, and a tert-butyl group.

[0088] Examples of the aryl group having 6 to 10 carbon atoms include, but are not limited to, a phenyl group, a naphthyl group, and the like.

[0089] Examples of the arylalkyl group having 7 to 10 carbon atoms include, but are not limited to, a benzyl group.

[0090] Examples of the alkylaryl group having 7 to 10 carbon atoms include, but are not limited to, a tolyl group, a xylyl group, and the like.

[0091] Examples of the halogen group include, but are not limited to, a fluoro group, a chloro group, a bromo group, and an iodo group.

[0092] Examples of the silyl group having 1 to 6 carbon atoms include, but are not limited to, a trimethylsilyl group, a tert-butyldimethylsilyl group, and the like.

[0093] Among these, the aromatic dicarboxylic acid constituting the aromatic dicarboxylic acid unit other than the isophthalic acid unit is preferably an aromatic dicarboxylic acid having 8 to 20 carbon atoms which is unsubstituted or substituted with a specific substituent.

[0094] Specific examples of unsubstituted or predetermined substituent-substituted aromatic dicarboxylic acids having 8 to 20 carbon atoms include, but are not limited to, terephthalic acid, naphthalenedicarboxylic acid, 2-chloroterephthalic acid, 2-methylterephthalic acid, 5-methylisophthalic acid, and 5-sodium sulfoisophthalic acid.

[0095] The aromatic dicarboxylic acid constituting the aromatic dicarboxylic acid unit may be used alone or in combination of two or more kinds.

[0096] (2-1-2) Aliphatic dicarboxylic acid unit Examples of the aliphatic dicarboxylic acid constituting the aliphatic dicarboxylic acid unit include linear or branched saturated aliphatic dicarboxylic acids having 3 to 20 carbon atoms.

[0097] Examples of linear saturated aliphatic dicarboxylic acids having 3 to 20 carbon atoms include, but are not limited to, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, tetradecanedioic acid, hexadecanedioic acid, octadecanedioic acid, eicosane dioic acid, and diglycolic acid.

[0098] Examples of branched saturated aliphatic dicarboxylic acids having 3 to 20 carbon atoms include, but are not limited to, dimethylmalonic acid, 2,2-dimethylsuccinic acid, 2,3-dimethylglutaric acid, 2,2-diethylsuccinic acid, 2,3-diethylglutaric acid, 2,2-dimethylglutaric acid, 2-methyladipic acid, and trimethyladipic acid.

[0099] (2-1-3) Alicyclic dicarboxylic acid unit Examples of alicyclic dicarboxylic acids constituting an alicyclic dicarboxylic acid unit (hereinafter sometimes referred to as an "alicyclic dicarboxylic acid unit") include, but are not limited to, alicyclic dicarboxylic acids having an alicyclic structure with 3 to 10 carbon atoms. Among these, alicyclic dicarboxylic acids are preferably alicyclic dicarboxylic acids having an alicyclic structure with 5 to 10 carbon atoms.

[0100] Examples of such alicyclic dicarboxylic acids include, but are not limited to, 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,3-cyclopentanedicarboxylic acid, etc. Among them, 1,4-cyclohexanedicarboxylic acid is preferred as the alicyclic dicarboxylic acid.

[0101] The alicyclic dicarboxylic acid constituting the alicyclic dicarboxylic acid unit may be used alone or in combination of two or more kinds.

[0102] The alicyclic group of the alicyclic dicarboxylic acid may be unsubstituted or may have a substituent. Examples of the substituent include an alkyl group having 1 to 4 carbon atoms. Examples of the alkyl group having 1 to 4 carbon atoms include the same as those exemplified in the above "aromatic dicarboxylic acid unit".

[0103] The dicarboxylic acid units other than the isophthalic acid units preferably contain aromatic dicarboxylic acid units, and more preferably contain aromatic dicarboxylic acids having 6 or more carbon atoms. By using such a dicarboxylic acid, a resin composition having superior mechanical properties tends to be obtained, and the joining strength during laser welding can be improved, and the appearance of the joined portion can be improved.

[0104] In the semi-aromatic polyamide (A1-2), the dicarboxylic acid constituting the dicarboxylic acid unit (A1-2a) is not limited to the compounds described above as the dicarboxylic acid, and may be a compound equivalent to the above dicarboxylic acid. The term "compound equivalent to a dicarboxylic acid" used herein means a compound that can have a dicarboxylic acid structure similar to the dicarboxylic acid structure derived from the above dicarboxylic acid. Examples of such compounds include, but are not limited to, anhydrides of dicarboxylic acids and halides of dicarboxylic acids.

[0105] Furthermore, the semi-aromatic polyamide (A1-2) may further contain units derived from a trivalent or higher polyvalent carboxylic acid, if necessary, within the range that does not impair the effects of the molded article of this embodiment. Examples of the trivalent or higher polyvalent carboxylic acid include trimellitic acid, trimesic acid, pyromellitic acid, etc. These trivalent or higher polyvalent carboxylic acids may be used alone or in combination of two or more.

[0106] (2-2) Diamine unit (A1-2b) The diamine unit (A1-2b) constituting the semi-aromatic polyamide (A1-2) is not particularly limited and may be, for example, an aromatic diamine unit, an aliphatic diamine unit, an alicyclic diamine unit, etc. Among them, the diamine unit (A1-2b) constituting the semi-aromatic polyamide (A1-2) preferably contains a diamine unit having 4 to 10 carbon atoms, more preferably contains a diamine unit having 6 to 10 carbon atoms.

[0107] (2-2-1) Aliphatic diamine unit Examples of the aliphatic diamine constituting the aliphatic diamine unit include linear saturated aliphatic diamines having 4 to 20 carbon atoms. Examples of linear saturated aliphatic diamines having 4 to 20 carbon atoms include, but are not limited to, ethylenediamine, propylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, undecamethylenediamine, dodecamethylenediamine, tridecamethylenediamine, and the like.

[0108] (2-2-2) Alicyclic diamine unit Examples of alicyclic diamines constituting the alicyclic diamine unit (hereinafter, also referred to as "alicyclic diamines") include, but are not limited to, 1,4-cyclohexanediamine, 1,3-cyclohexanediamine, 1,3-cyclopentanediamine, and the like.

[0109] (2-2-3) Aromatic diamine unit The aromatic diamine constituting the aromatic diamine unit is not limited to the following as long as it is a diamine containing an aromatic group. Specific examples of the aromatic diamine include metaxylylenediamine.

[0110] The diamines constituting the diamine units may be used alone or in combination of two or more. Among these, the diamine unit (A1-2b) is preferably an aliphatic diamine unit, more preferably a linear saturated aliphatic diamine unit having 4 to 10 carbon atoms, still more preferably a linear saturated aliphatic diamine unit having 6 to 10 carbon atoms, and particularly preferably a hexamethylenediamine unit. Use of such a diamine tends to provide a resin composition having superior mechanical properties, and can improve the bonding strength during laser welding and improve the appearance of the bonded portion.

[0111] The weight average molecular weight can be used as an index of the molecular weight of the semi-aromatic polyamide (A1-2). The weight average molecular weight of the semi-aromatic polyamide is preferably 10,000 to 50,000, more preferably 15,000 to 45,000, even more preferably 15,000 to 40,000, even more preferably 17,000 to 35,000, particularly preferably 17,000 to 30,000, and most preferably 18,000 to 28,000. When the weight average molecular weight is within the above range, the joining strength during laser welding can be improved and the appearance of the joined portion can be improved. The weight average molecular weight of the semi-aromatic polyamide (A1-2) can be measured, for example, by using GPC.

[0112] (3) End-capping agent The terminals of the polyamide resin (A1) may be capped with a known terminal capping agent. Such an end-capping agent can also be added as a molecular weight regulator when producing a polyamide from the above dicarboxylic acid and the above diamine, or from at least one member selected from the group consisting of the above lactam and the above aminocarboxylic acid.

[0113] Examples of the terminal blocking agent include, but are not limited to, monocarboxylic acid, monoamine, acid anhydride (phthalic anhydride, etc.), monoisocyanate, monoester, monoalcohol, etc. Only one type of terminal blocking agent may be used alone, or two or more types may be used in combination. Among these, the terminal blocking agent is preferably a monocarboxylic acid or a monoamine. By blocking the terminals of the polyamide with the terminal blocking agent, the thermal stability of the molded product tends to be more excellent.

[0114] The monocarboxylic acid that can be used as the end-capping agent may be any one that is reactive with amino groups that may be present at the terminals of the polyamide. Examples of the monocarboxylic acid include, but are not limited to, aliphatic monocarboxylic acids, alicyclic monocarboxylic acids, and aromatic monocarboxylic acids.

[0115] Examples of the aliphatic monocarboxylic acid include formic acid, acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, tridecylic acid, myristic acid, palmitic acid, stearic acid, pivalic acid, and isobutyric acid.

[0116] An example of the alicyclic monocarboxylic acid is cyclohexanecarboxylic acid. Examples of aromatic monocarboxylic acids include benzoic acid, toluic acid, α-naphthalenecarboxylic acid, β-naphthalenecarboxylic acid, methylnaphthalenecarboxylic acid, and phenylacetic acid.

[0117] These monocarboxylic acids may be used alone or in combination of two or more. In particular, from the viewpoints of fluidity and mechanical strength, it is preferable that the terminals of the semi-aromatic polyamide (A1-2) are blocked with acetic acid.

[0118] The monoamine usable as the end-capping agent may be any monoamine that is reactive with a carboxyl group that may be present at the end of the polyamide, and may include, but is not limited to, aliphatic monoamines, alicyclic monoamines, aromatic monoamines, etc.

[0119] Examples of the aliphatic monoamine include methylamine, ethylamine, propylamine, butylamine, hexylamine, octylamine, decylamine, stearylamine, dimethylamine, diethylamine, dipropylamine, and dibutylamine.

[0120] Examples of the alicyclic monoamine include cyclohexylamine and dicyclohexylamine. Examples of aromatic monoamines include aniline, toluidine, diphenylamine, and naphthylamine. These monoamines may be used alone or in combination of two or more.

[0121] A resin composition containing a polyamide end-capped with an end-capping agent tends to have better heat resistance, flowability, toughness, low water absorbency, and rigidity.

[0122] (4) Preferred polyamide resin (A1) Preferred polyamide-based resins (A1) are not particularly limited, and examples thereof include polyamides obtained by polycondensation reaction of lactams, such as polyamide 6, polyamide 11, and polyamide 12; and polyamides obtained as copolymers of diamines and dicarboxylic acids, such as polyamide 6,6, polyamide 6,10, polyamide 6,11, polyamide 6,12, polyamide 6,6 / 6,I, polyamide 6,T, polyamide 6,I, polyamide 6,I / 6,T, polyamide 9,T, polyamide 10,T, polyamide 2M5,T, polyamide MXD,6, polyamide 6,C, and polyamide 2M5,C.

[0123] Among these, one or more aliphatic polyamides selected from the group consisting of polyamide 6, polyamide 11, polyamide 12, polyamide 6,6, polyamide 6,10, polyamide 6,11, and polyamide 6,12, or one or more semi-aromatic polyamides selected from the group consisting of polyamide 6,6 / 6,I, polyamide 6,T, polyamide 6,I, polyamide 6,I / 6,T, polyamide 9,T, and polyamide MXD,6 are more preferred.

[0124] (Production method of polyamide resin (A1)) When producing the polyamide resin (A1) (aliphatic polyamide (A1-1) and semi-aromatic polyamide (a1-2)), the amount of dicarboxylic acid added and the amount of diamine added are preferably approximately the same molar amount. Taking into consideration the amount of diamine that escapes to the outside of the reaction system during the polymerization reaction, the molar amount of the total diamine per molar amount of the total dicarboxylic acids is preferably 0.9 to 1.2, more preferably 0.95 to 1.1, and even more preferably 0.98 to 1.05.

[0125] A method for producing a polyamide includes, but is not limited to, the following polymerization step (1) or (2). (1) A step of polymerizing a combination of a dicarboxylic acid constituting a dicarboxylic acid unit and a diamine constituting a diamine unit to obtain a polymer. (2) A step of polymerizing one or more members selected from the group consisting of lactam constituting the lactam unit and aminocarboxylic acid constituting the aminocarboxylic acid unit to obtain a polymer.

[0126] The method for producing a polyamide preferably further comprises, after the polymerization step, an increasing step of increasing the degree of polymerization of the polyamide. If necessary, the method may comprise, after the polymerization step and the increasing step, a capping step of capping the ends of the resulting polymer with a terminal capping agent.

[0127] Specific examples of the method for producing polyamide include the following various methods 1) to 4). 1) A method in which an aqueous solution or suspension of one or more selected from the group consisting of a dicarboxylic acid-diamine salt, a mixture of a dicarboxylic acid and a diamine, a lactam, and an aminocarboxylic acid is heated and polymerized while maintaining the molten state (hereinafter, sometimes referred to as a "thermal melt polymerization method"). 2) A method in which the degree of polymerization of polyamide obtained by hot melt polymerization is increased while maintaining the polyamide in a solid state at a temperature below the melting point (hereinafter sometimes referred to as "hot melt polymerization / solid-state polymerization method"). 3) A method of polymerizing one or more members selected from the group consisting of dicarboxylic acid-diamine salts, mixtures of dicarboxylic acids and diamines, lactams, and aminocarboxylic acids while maintaining the solid state (hereinafter, sometimes referred to as the "solid-state polymerization method"). 4) A method of polymerization using a dicarboxylic acid halide component equivalent to a dicarboxylic acid and a diamine component (hereinafter, sometimes referred to as a "solution method").

[0128] Among them, as a specific method for producing polyamide, a production method including a hot melt polymerization method is preferable. When producing polyamide by the hot melt polymerization method, it is preferable to maintain the molten state until the polymerization is completed. In order to maintain the molten state, it is necessary to produce the polyamide composition under polymerization conditions suitable for the composition. Examples of the polymerization conditions include the following conditions. First, the polymerization pressure in the hot melt polymerization method is set to 14 kg / cm. 2 More than 25kg / cm 2 Heating is continued while controlling the pressure in the vessel to below atmospheric pressure (gauge pressure is 0 kg / cm 2 ) over 30 minutes or more until the blood pressure drops to 0.

[0129] In the method for producing a polyamide, the polymerization form is not particularly limited, and may be a batch type or a continuous type. The polymerization apparatus used for producing polyamide is not particularly limited, and known apparatuses can be used. Specific examples of the polymerization apparatus include an autoclave type reactor, a tumbler type reactor, and an extruder type reactor (such as a kneader).

[0130] Hereinafter, as a method for producing polyamide, a method for producing polyamide by a batch-type hot melt polymerization method will be specifically described, but the method for producing polyamide is not limited thereto.

[0131] First, an aqueous solution containing about 40% to 60% by mass of raw material components for polyamide (a combination of dicarboxylic acid and diamine, and, if necessary, at least one selected from the group consisting of lactam and aminocarboxylic acid) is prepared. The aqueous solution is then concentrated to about 65% to 90% by mass in a concentration tank operated at a temperature of 110°C to 180°C and a pressure of about 0.035 MPa to 0.6 MPa (gauge pressure) to obtain a concentrated solution.

[0132] The concentrated solution obtained is then transferred to an autoclave, and heating is continued until the pressure in the autoclave reaches about 1.2 MPa or more and 2.2 MPa or less (gauge pressure).

[0133] Next, in the autoclave, the pressure is maintained at about 1.2 MPa to 2.2 MPa (gauge pressure) while removing at least one of water and gas components. Next, when the temperature reaches about 220° C. to 260° C., the pressure is reduced to atmospheric pressure (gauge pressure: 0 MPa). After the pressure in the autoclave is reduced to atmospheric pressure, the pressure can be reduced as necessary to effectively remove the by-product water.

[0134] The autoclave is then pressurized with an inert gas such as nitrogen, and the polyamide melt is extruded from the autoclave as a strand. The extruded strand is cooled and cut to obtain polyamide pellets.

[0135] Filler In addition to the thermoplastic resin, the resin composition preferably further contains a filler (B). By containing the filler (B), the resin composition can have more excellent mechanical properties such as toughness and rigidity.

[0136] The filler (B) is not particularly limited, and examples thereof include glass fibers, carbon fibers, calcium silicate fibers, potassium titanate fibers, aluminum borate fibers, glass flakes, calcium carbonate, talc, kaolin, mica, hydrotalcite, zinc carbonate, calcium hydrogen phosphate, wollastonite, zeolite, boehmite, magnesium oxide, calcium silicate, sodium aluminosilicate, magnesium silicate, ketjen black, acetylene black, furnace black, carbon nanotubes, graphite, brass, copper, silver, aluminum, nickel, iron, calcium fluoride, montmorillonite, swellable fluoromica, apatite, and milled fibers.

[0137] These fillers (B) may be used alone or in combination of two or more. Among these, from the viewpoints of rigidity, strength, and the like, the filler (B) is preferably glass fiber, carbon fiber, glass flake, talc, kaolin, mica, calcium hydrogen phosphate, wollastonite, carbon nanotubes, graphite, calcium fluoride, montmorillonite, swellable fluoromica, or apatite.

[0138] The filler (B) is more preferably one or more selected from the group consisting of glass fiber, calcium carbonate, talc, mica, wollastonite, and milled fiber, further preferably glass fiber or carbon fiber, and particularly preferably glass fiber.

[0139] When the filler (B) is a glass fiber or a carbon fiber, the number average fiber diameter (d1) is preferably 3 μm or more and 30 μm or less. The weight average fiber length (L) is preferably 100 μm or more and 5 mm or less. Furthermore, the aspect ratio ((L) / (d1)) of the number average fiber diameter (D1) to the weight average fiber length (L) is preferably 10 or more and 100 or less. By using the glass fiber or carbon fiber having the above configuration, higher properties can be exhibited.

[0140] When the filler (B) is a glass fiber, the number average fiber diameter (d1) is preferably 3 μm or more and 30 μm or less, the weight average fiber length (L) is preferably 103 μm or more and 5 mm or less, and the aspect ratio ((L) / (d1)) is preferably 3 or more and 100 or less.

[0141] The number average fiber diameter and weight average fiber length of the filler (B) can be measured by the following method. First, the molded product is dissolved in a solvent such as formic acid that dissolves the thermoplastic resin (A). Next, from the resulting insoluble components, fillers (B) having, for example, 100 or more particles are arbitrarily selected.

[0142] Next, the filler (B) is observed with an optical microscope, a scanning electron microscope, or the like, and the number average fiber diameter can be obtained by dividing the total measured fiber diameter by the number of measured fillers (B). Alternatively, the weight average fiber length can be obtained by dividing the total measured fiber length by the total weight of the measured filler (B).

[0143] The resin composition preferably contains 0.0 parts by mass or more and 150.0 parts by mass or less of filler (B) per 100 parts by mass of thermoplastic resin (A), more preferably contains 10.0 parts by mass or more and 140.0 parts by mass or less of filler (B), even more preferably contains 20.0 parts by mass or more and 135.0 parts by mass or less of filler (B), particularly preferably contains 25.0 parts by mass or more and 130.0 parts by mass or less of filler (B), and most preferably contains 30.0 parts by mass or more and 100 parts by mass or less of filler (B).

[0144] When the content of the filler (B) is equal to or more than the lower limit, the mechanical properties such as strength and rigidity of the molded article tend to be improved. On the other hand, when the content of the filler (B) is equal to or less than the upper limit, the molded article tends to have better surface appearance and laser welding strength. In particular, when the filler (B) is glass fiber and the content of the filler (B) is within the above range per 100 parts by mass of the thermoplastic resin (A), the mechanical properties such as strength and rigidity of the molded article tend to be further improved.

[0145] [Flame retardant (C)] The resin composition preferably further contains a flame retardant (C) in addition to the above thermoplastic resin.

[0146] The flame retardant (C) is not particularly limited, and examples thereof include halogen-based flame retardants containing a halogen element, such as chlorine-based flame retardants and bromine-based flame retardants, and phosphorus-based flame retardants not containing a halogen element. These flame retardants (C) may be used alone or in combination of two or more thereof. The flame retardancy can be further improved by using them in combination with a flame retardant assistant.

[0147] As the halogen-based flame retardant, from the viewpoint of suppressing the amount of corrosive gas generated during melt processing such as extrusion or molding, and further from the viewpoint of the expression of flame retardancy and mechanical properties such as toughness and rigidity, brominated polyphenylene ether (including poly(di)bromophenylene ether, etc.) or brominated polystyrene (including polydibromostyrene, polytribromostyrene, crosslinked brominated polystyrene, etc.) is preferred, and brominated polystyrene is more preferred.

[0148] The bromine content in the brominated polystyrene is preferably 5% by mass or more and 75% by mass or less based on the total mass of the brominated polystyrene. By having the bromine content be equal to or more than the above lower limit, the amount of bromine required for flame retardancy can be satisfied with a smaller amount of brominated polystyrene blended, and a molded article having excellent heat resistance, flowability, toughness, low water absorption, and rigidity and excellent flame retardancy can be obtained without impairing the properties of the polyamide copolymer. In addition, by having the bromine content be equal to or less than the above upper limit, thermal decomposition is less likely to occur during melt processing such as extrusion and molding, gas generation can be more suppressed, and a molded article having excellent heat discoloration resistance can be obtained.

[0149] The phosphorus-based flame retardant is not particularly limited as long as it does not contain a halogen element and contains a phosphorus element. Examples of the phosphorus-based flame retardant include a phosphate ester flame retardant, a melamine polyphosphate flame retardant, a phosphazene flame retardant, a phosphinic acid flame retardant, and a red phosphorus flame retardant.

[0150] Among these, the flame retardant (C) is preferably a phosphate-based flame retardant, a melamine polyphosphate-based flame retardant, a phosphazene-based flame retardant or a phosphinic acid-based flame retardant, and more preferably a phosphinic acid-based flame retardant. Specific examples of the phosphinic acid flame retardant include phosphinates and diphosphinates. Examples of phosphinates include compounds represented by the following general formula (I) (hereinafter sometimes abbreviated as "phosphinate (I)"). Examples of the diphosphinate include diphosphinates represented by the following general formula (II) (hereinafter sometimes abbreviated as "diphosphinate (II)").

[0151] [ka]

[0152] (In general formula (1), R 11 and R 12 Each of M is independently an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 10 carbon atoms. n11+ is a metal ion having a valence of n11. M is an element belonging to Group 2 or Group 15 of the periodic table, a transition element, zinc, or aluminum. n11 is 2 or 3. When n11 is 2 or 3, multiple R 11 and R 12 may be the same or different.

[0153] In general formula (2), R 21 and R 22 Each of Y is independently an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 10 carbon atoms.21 M' is an alkylene group having 1 to 10 carbon atoms or an arylene group having 6 to 10 carbon atoms. m21+ is a metal ion having a valence of m21. M' is an element belonging to Group 2 or Group 15 of the periodic table, a transition element, zinc, or aluminum. n21 is an integer of 1 to 3. When n21 is 2 or 3, multiple R 21 , R 22 and Y 21 may be the same or different. m21 is 2 or 3. x is 1 or 2. When x is 2, multiple M' may be the same or different. n21, x, and m21 are integers that satisfy the relational formula 2×n21=m21×x.

[0154] (R 11 , R 12 , R 21 and R 22 ) R 11 , R 12 , R 21 and R 22 are each independently an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 10 carbon atoms. When n11 is 2 or 3, a plurality of R 11 and R 12 may be the same or different, but are preferably the same in terms of ease of production. 21 and R 22 may be the same or different, but is preferably the same in terms of ease of production.

[0155] The alkyl group may be chain-like or cyclic, but is preferably chain-like. The chain-like alkyl group may be linear or branched. Examples of the linear alkyl group include methyl, ethyl, n-propyl, n-butyl, n-pentyl, and n-hexyl groups. Examples of branched alkyl groups include a 1-methylethyl group, a 1-methylpropyl group, a 2-methylpropyl group, a 1,1-dimethylethyl group, a 1-methylbutyl group, a 2-methylbutyl group, a 3-methylbutyl group, a 1,1-dimethylpropyl group, a 1,2-dimethylpropyl group, a 2,2-dimethylpropyl group, a 1-methylpentyl group, a 2-methylpentyl group, a 3-methylpentyl group, a 4-methylpentyl group, a 1,1-dimethylbutyl group, a 1,2-dimethylbutyl group, a 1,3-dimethylbutyl group, a 2,2-dimethylbutyl group, a 2,3-dimethylbutyl group, a 3,3-dimethylbutyl group, a 1-ethylbutyl group, a 2-ethylbutyl group, and a 1,1,2-trimethylpropyl group.

[0156] Examples of the aryl group include a phenyl group and a naphthyl group.

[0157] The alkyl group and the aryl group may have a substituent. Examples of the substituent in the alkyl group include an aryl group having 6 to 10 carbon atoms. Examples of the substituent in the aryl group include an alkyl group having 1 to 6 carbon atoms.

[0158] Specific examples of the alkyl group having a substituent include a benzyl group. Specific examples of the aryl group having a substituent include a tolyl group and a xylyl group. Among them, R 11 , R 12 , R 21 and R 22 As the alkyl group, an alkyl group having 1 to 6 carbon atoms is preferable, and a methyl group or an ethyl group is more preferable.

[0159] (Y 21 ) Y 21is an alkylene group having 1 to 10 carbon atoms or an arylene group having 6 to 10 carbon atoms. 21 may be the same or different, but is preferably the same in terms of ease of production.

[0160] The alkylene group may be either chain-like or cyclic, but is preferably chain-like. The chain-like alkylene group may be either linear or branched. Examples of linear alkylene groups include methylene, ethylene, trimethylene, tetramethylene, pentamethylene, and hexamethylene. Examples of branched alkylene groups include 1-methylethylene and 1-methylpropylene.

[0161] Examples of the arylene group include a phenylene group and a naphthylene group. The alkylene group and the arylene group may have a substituent. Examples of the substituent in the alkylene group include an aryl group having 6 to 10 carbon atoms. Examples of the substituent in the arylene group include an alkyl group having 1 to 6 carbon atoms.

[0162] Specific examples of the alkylene group having a substituent include a phenylmethylene group, a phenylethylene group, a phenyltrimethylene group, and a phenyltetramethylene group. Specific examples of the substituted arylene group include a methylphenylene group, an ethylphenylene group, a tert-butylphenylene group, a methylnaphthylene group, an ethylnaphthylene group, and a tert-butylnaphthylene group. Among them, Y 21 As the alkyl group, an alkylene group having 1 to 10 carbon atoms is preferable, and a methylene group or an ethylene group is more preferable.

[0163] (M and M') M and M' are each independently an ion of an element belonging to Group 2 or Group 15 of the periodic table, an ion of a transition element, a zinc ion, or an aluminum ion. Examples of the ion of an element belonging to Group 2 of the periodic table include a calcium ion and a magnesium ion. Examples of the ion of an element belonging to Group 15 of the periodic table include a bismuth ion.

[0164] Furthermore, when x is 2, a plurality of M' may be the same or different, but it is preferable that they are the same in terms of ease of production. Among these, M and M' are preferably calcium, zinc or aluminum, and more preferably calcium or aluminum.

[0165] (x) x represents the number of M' and is 1 or 2. x can be appropriately selected depending on the type of M' and the number of diphosphinic acids.

[0166] (n11 and n21) n11 represents the number of phosphinic acids and the valence of M, and is 2 or 3. n11 can be appropriately selected depending on the type and valence of M. n21 represents the number of diphosphinic acids and is an integer of 1 to 3. n21 can be appropriately selected depending on the type and number of M'.

[0167] (m21) m21 represents the valence of M' and is 2 or 3. n21, x, and m21 are integers that satisfy the relational expression 2×n21=m21×x.

[0168] Specific examples of preferred phosphinates (1) include calcium dimethylphosphinate, magnesium dimethylphosphinate, aluminum dimethylphosphinate, zinc dimethylphosphinate, calcium ethylmethylphosphinate, magnesium ethylmethylphosphinate, aluminum ethylmethylphosphinate, zinc ethylmethylphosphinate, calcium diethylphosphinate, magnesium diethylphosphinate, aluminum diethylphosphinate, zinc diethylphosphinate, calcium methyl-n-propylphosphinate, magnesium methyl-n-propylphosphinate, aluminum methyl-n-propylphosphinate, zinc methyl-n-propylphosphinate, methane di(methylphosphinate), ) calcium, methane di(methylphosphinate) magnesium, methane di(methylphosphinate) aluminum, methane di(methylphosphinate) zinc, benzene-1,4-(dimethylphosphinate) calcium, benzene-1,4-(dimethylphosphinate) magnesium, benzene-1,4-(dimethylphosphinate) aluminum, benzene-1,4-(dimethylphosphinate) zinc, methylphenylphosphinate calcium, methylphenylphosphinate magnesium, methylphenylphosphinate aluminum, methylphenylphosphinate zinc, diphenylphosphinate calcium, diphenylphosphinate magnesium, diphenylphosphinate aluminum, diphenylphosphinate zinc, etc. Among them, as the phosphinate (I), dimethylphosphinate calcium or dimethylphosphinate aluminum is particularly preferred because of its excellent flame retardancy.

[0169] Specific examples of preferred diphosphinates (II) include calcium methane di(methylphosphinate), magnesium methane di(methylphosphinate), aluminum methane di(methylphosphinate), zinc methane di(methylphosphinate), calcium benzene-1,4-di(methylphosphinate), magnesium benzene-1,4-di(methylphosphinate), aluminum benzene-1,4-di(methylphosphinate), and zinc benzene-1,4-di(methylphosphinate).

[0170] The content of the flame retardant (C) is preferably 5.0 parts by mass or more and 90.0 parts by mass or less, more preferably 10.0 parts by mass or more and 80.0 parts by mass or less, still more preferably 15.0 parts by mass or more and 70.0 parts by mass or less, and particularly preferably 20.0 parts by mass or more and 60.0 parts by mass or less, relative to 100 parts by mass of the thermoplastic resin.

[0171] By setting the content of the phosphorus-based flame retardant to the above lower limit or more, a resin composition having superior flame retardancy can be obtained. On the other hand, by setting the content of the phosphorus-based flame retardant to the above upper limit or less, a resin composition having superior flame retardancy can be obtained without impairing the properties of the resin composition.

[0172] [Colorant (D)] The resin composition may further contain (D) a colorant in addition to the above-mentioned thermoplastic resin.

[0173] As the colorant (D), a commonly used colorant can be blended, and the resin composition can be colored in any color tone from black to pale colors.

[0174] When using colorant (D), it has two roles. The first role is to absorb the laser and melt the resin by generating heat. The colorant (D1) for absorbing the laser is added to the resin that absorbs the laser, that is, the resin composition that forms the absorbing resin member.

[0175] Another role is to transmit the laser, allowing the light to pass through to the resin on the side that will absorb the laser and give the desired color. This laser-transmitting colorant (D2) is added to the resin on the side that transmits the laser, i.e., the resin composition that forms the transmitting resin member.

[0176] The colorant (D1) for absorbing the laser in laser welding can be either an inorganic material or an organic material as long as it is a colorant that absorbs the laser. Examples of such colorants include carbon black (acetylene black, lamp black, thermal black, furnace black, channel black, ketjen black, gas black, oil black, etc.), graphite, titanium black, black iron oxide, etc. Among these, carbon black (D1-1) is preferred in terms of dispersibility, color development, cost, etc. These colorants can be used alone or in combination of two or more kinds.

[0177] Examples of the non-black pigment include various inorganic pigments and organic pigments described below. These non-black pigments can be used alone or in combination of two or more kinds.

[0178] Examples of inorganic pigments include white pigments such as calcium carbonate, titanium oxide, zinc oxide, and zinc sulfide; yellow pigments such as cadmium yellow, yellow lead, titanium yellow, zinc chromate, yellow ocher, and yellow iron oxide; red pigments such as red pigments, umber, red iron oxide, and cadmium red; blue pigments such as iron blue, ultramarine, and cobalt blue; and green pigments such as chrome green.

[0179] Examples of organic pigments include azo pigments, azomethine pigments, methine pigments, indanthrone pigments, anthraquinone pigments, pyranthrone pigments, flavanthrone pigments, benzenethrone pigments, phthalocyanine pigments, quinophthalone pigments, perylene pigments, perinone pigments, dioxazine pigments, thioindigo pigments, isoindolinone pigments, isoindoline pigments, pyrrulepyrrole pigments, and quinacridone pigments.

[0180] Any organic material that transmits the laser in laser welding can be used as the colorant (D2). An example of such a colorant is eBIND ACW-9871 (hereinafter simply referred to as ACW) by Orient Chemical Industries.

[0181] The content of the colorant (D1) is preferably 0.001 to 5.00 parts by mass, more preferably 0.005 to 2.5 parts by mass, and even more preferably 0.01 to 1.00 parts by mass, relative to 100 parts by mass of the thermoplastic resin. By having the content of the colorant (D1) be equal to or more than the lower limit, the efficiency of heating by the laser is improved, the effect of thermally deteriorating the resin is suppressed, and melting can be achieved in a short time. On the other hand, by having the content of the colorant (D1) be equal to or less than the upper limit, carbonization of the resin by heating can be more effectively prevented.

[0182] The content of the colorant (D2) is preferably 0.001 to 5.00 parts by mass, more preferably 0.005 to 2.5 parts by mass, and even more preferably 0.01 to 1.00 parts by mass, relative to 100 parts by mass of the thermoplastic resin. When the content of the colorant (D2) is equal to or greater than the lower limit, it is possible to develop a desired color by coloring. On the other hand, when the content of the colorant (D2) is equal to or less than the upper limit, the laser transmission inhibition is suppressed, and energy is efficiently transferred to the material on the absorbing side, thereby effectively preventing thermal deterioration of the resin on the transmitting side.

[0183] [Other additives (E)] In addition to the thermoplastic resin, the resin composition may contain other additives (E) commonly used in resin compositions, as long as the effect of the molded article of the present embodiment is not impaired. Examples of the other additives (E) include moldability improvers, deterioration inhibitors, nucleating agents, and heat stabilizers.

[0184] The content of the other additives (E) in the resin composition varies depending on the type and use of the composition, and is not particularly limited as long as it is within a range that does not impair the effects of the molded article of this embodiment.

[0185] (Moldability improver) The moldability improver is not particularly limited, but examples thereof include higher fatty acids, higher fatty acid metal salts, higher fatty acid esters, higher fatty acid amides, etc. The moldability improver is also used as a "lubricant".

[0186] (1) Higher fatty acids Examples of higher fatty acids include linear or branched, saturated or unsaturated aliphatic monocarboxylic acids having 8 to 40 carbon atoms. Examples of the linear saturated aliphatic monocarboxylic acid having 8 to 40 carbon atoms include lauric acid, palmitic acid, stearic acid, behenic acid, and montanic acid. Examples of branched saturated aliphatic monocarboxylic acids having 8 to 40 carbon atoms include isopalmitic acid and isostearic acid. Examples of the linear unsaturated aliphatic monocarboxylic acid having 8 to 40 carbon atoms include oleic acid and erucic acid. Examples of the branched unsaturated aliphatic monocarboxylic acid having 8 to 40 carbon atoms include isooleic acid. Among these, stearic acid or montanic acid is preferred as the higher fatty acid.

[0187] (2) Metal salts of higher fatty acids The higher fatty acid metal salt is a metal salt of a higher fatty acid. Examples of the metal element of the metal salt include Group 1, Group 2 and Group 3 elements of the periodic table, zinc, aluminum, and the like. Examples of Group 1 elements in the periodic table include sodium and potassium. Examples of Group 2 elements in the periodic table include calcium and magnesium. Examples of Group 3 elements in the periodic table include scandium and yttrium. Among these, elements of Groups 1 and 2 of the Periodic Table or aluminum are preferred, and sodium, potassium, calcium, magnesium or aluminum is more preferred.

[0188] Specific examples of higher fatty acid metal salts include calcium stearate, aluminum stearate, zinc stearate, magnesium stearate, calcium montanate, sodium montanate, calcium palmitate, and the like. Among these, as the higher fatty acid metal salt, a metal salt of montanic acid or a metal salt of stearic acid is preferred.

[0189] (3) Higher fatty acid esters The higher fatty acid ester is an ester of a higher fatty acid and an alcohol. As the higher fatty acid ester, an ester of an aliphatic carboxylic acid having 8 to 40 carbon atoms and an aliphatic alcohol having 8 to 40 carbon atoms is preferred. Examples of the aliphatic alcohol having 8 to 40 carbon atoms include stearyl alcohol, behenyl alcohol, and lauryl alcohol. Specific examples of higher fatty acid esters include stearyl stearate and behenyl behenate.

[0190] (4) Higher fatty acid amide Higher fatty acid amides are amide compounds of higher fatty acids. Examples of higher fatty acid amides include stearic acid amide, oleic acid amide, erucic acid amide, ethylene bisstearylamide, ethylene bisoleylamide, N-stearyl stearic acid amide, and N-stearyl erucic acid amide. These higher fatty acids, higher fatty acid metal salts, higher fatty acid esters and higher fatty acid amides may each be used alone or in combination of two or more.

[0191] (deterioration inhibitor) The deterioration inhibitor is used for the purpose of preventing thermal deterioration and discoloration when heated, and improving heat aging resistance. The deterioration inhibitor is not particularly limited, but examples thereof include copper compounds, phenol-based stabilizers, phosphite-based stabilizers, hindered amine-based stabilizers, triazine-based stabilizers, benzotriazole-based stabilizers, benzophenone-based stabilizers, cyanoacrylate-based stabilizers, salicylate-based stabilizers, and sulfur-based stabilizers. Examples of the copper compound include copper acetate and copper iodide. Examples of the phenol-based stabilizer include hindered phenol compounds. These deterioration inhibitors may be used alone or in combination of two or more kinds.

[0192] (Nucleating agent) The nucleating agent refers to a substance that, when added, provides at least one of the following effects (1) to (3). (1) The effect of increasing the crystallization peak temperature of the resin composition. (2) The effect of reducing the difference between the extrapolated onset temperature and the extrapolated end temperature of the crystallization peak. (3) The effect of making the spherulites in the resulting molded product finer or more uniform in size.

[0193] Examples of the nucleating agent include, but are not limited to, talc, boron nitride, mica, kaolin, silicon nitride, carbon black, potassium titanate, and molybdenum disulfide. The nucleating agents may be used alone or in combination of two or more kinds. Among these, talc or boron nitride is preferred as the nucleating agent from the viewpoint of nucleating agent effect.

[0194] In addition, since the effect of the nucleating agent is high, the number average particle size of the nucleating agent is preferably 0.01 μm or more and 10 μm or less. The number average particle size of the nucleating agent can be measured by the following method. First, the molded product is dissolved in a solvent in which the resin composition is soluble, such as formic acid. Next, from the insoluble components obtained, for example, 100 or more nucleating agents are arbitrarily selected. Then, the particle size can be determined by observing with an optical microscope, a scanning electron microscope, or the like and measuring the particle size.

[0195] The content of the nucleating agent in the resin composition is preferably 0.001 parts by mass or more and 1 part by mass or less, more preferably 0.001 parts by mass or more and 0.5 parts by mass or less, and even more preferably 0.001 parts by mass or more and 0.09 parts by mass or less, per 100 parts by mass of the thermoplastic resin. When the content of the nucleating agent is equal to or more than the above lower limit, the heat resistance of the molded article tends to be improved, whereas when the content of the nucleating agent is equal to or less than the above upper limit, a molded article having superior toughness can be obtained.

[0196] (Heat stabilizer) Examples of the heat stabilizer include, but are not limited to, phenol-based heat stabilizers, phosphorus-based heat stabilizers, amine-based heat stabilizers, and metal salts of elements in groups 3, 4, and 11 to 14 of the periodic table.

[0197] (1) Phenol-based heat stabilizers Examples of the phenol-based heat stabilizer include, but are not limited to, hindered phenol compounds, etc. Hindered phenol compounds have the property of imparting excellent heat resistance and light resistance to resins such as polyamides and fibers.

[0198] Examples of the hindered phenol compound include, but are not limited to, N,N'-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenylpropionamide), pentaerythrityl-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], N,N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxy-hydrocinnamamide), triethylene glycol-bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl)propionate], and the like. onate], 3,9-bis{2-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propynyloxy]-1,1-dimethylethyl}-2,4,8,10-tetraoxaspiro[5,5]undecane, 3,5-di-tert-butyl-4-hydroxybenzylphosphonate-diethyl ester, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)isocyanuric acid, and the like. These hindered phenol compounds may be used alone or in combination of two or more.

[0199] When a phenol-based heat stabilizer is used, the content of the phenol-based heat stabilizer in the resin composition is preferably 0.01 mass % or more and 1 mass % or less, and more preferably 0.05 mass % or more and 1 mass % or less, relative to the total mass of the resin composition. By setting the content of the phenol-based heat stabilizer within the above range, it is possible to further improve the heat aging resistance of the molded article and further reduce the amount of gas generation.

[0200] (2) Phosphorus-based heat stabilizers Examples of phosphorus-based heat stabilizers include, but are not limited to, pentaerythritol-type phosphite compounds, trioctyl phosphite, trilauryl phosphite, tridecyl phosphite, octyl diphenyl phosphite, trisisodecyl phosphite, phenyl diisodecyl phosphite, phenyl di(tridecyl) phosphite, diphenyl isooctyl phosphite, diphenyl isodecyl phosphite, diphenyl (tridecyl) phosphite, triphenyl phosphite, tris( nonylphenyl) phosphite, tris(2,4-di-tert-butylphenyl) phosphite, tris(2,4-di-tert-butyl-5-methylphenyl) phosphite, tris(butoxyethyl) phosphite, 4,4'-butylidene-bis(3-methyl-6-tert-butylphenyl-tetra-tridecyl) diphosphite, tetra(C12-C15 mixed alkyl)-4,4'-isopropylidene diphenyl diphosphite, 4,4'-isopropylidenebis(2-tert-butylphenyl)- Di(nonylphenyl)phosphite, tris(biphenyl)phosphite, tetra(tridecyl)-1,1,3-tris(2-methyl-5-tert-butyl-4-hydroxyphenyl)butane diphosphite, tetra(tridecyl)-4,4'-butylidenebis(3-methyl-6-tert-butylphenyl)diphosphite, tetra(C1-C15 mixed alkyl)-4,4'-isopropylidene diphenyl diphosphite, tris(mono,dimixed nonylphenyl)phosphite, 4,4'-isopropylidene Bis(2-tert-butylphenyl)-di(nonylphenyl)phosphite, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, tris(3,5-di-tert-butyl-4-hydroxyphenyl)phosphite, hydrogenated-4,4'-isopropylidenediphenyl polyphosphite, bis(octylphenyl)-bis(4,4'-butylidenebis(3-methyl-6-tert-butylphenyl))-1,6-hexanol diphosphite, hexatridecyl-1,1,Examples of the phosphite include 3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)diphosphite, tris(4,4'-isopropylidenebis(2-tert-butylphenyl))phosphite, tris(1,3-stearoyloxyisopropyl)phosphite, 2,2-methylenebis(4,6-di-tert-butylphenyl)octylphosphite, 2,2-methylenebis(3-methyl-4,6-di-tert-butylphenyl)2-ethylhexylphosphite, tetrakis(2,4-di-tert-butyl-5-methylphenyl)-4,4'-biphenylene diphosphite, and tetrakis(2,4-di-tert-butylphenyl)-4,4'-biphenylene diphosphite. These phosphorus-based heat stabilizers may be used alone or in combination of two or more.

[0201] Examples of the pentaerythritol type phosphite compound include, but are not limited to, 2,6-di-tert-butyl-4-methylphenyl-phenyl-pentaerythritol diphosphite, 2,6-di-tert-butyl-4-methylphenyl-methyl-pentaerythritol diphosphite, 2,6-di-tert-butyl-4-methylphenyl-2-ethylhexyl-pentaerythritol diphosphite, 2,6-di-tert-butyl-4-methylphenyl-isodecyl-pentaerythritol diphosphite, 2, 6-di-tert-butyl-4-methylphenyl-lauryl-pentaerythritol diphosphite, 2,6-di-tert-butyl-4-methylphenyl-isotridecyl-pentaerythritol diphosphite, 2,6-di-tert-butyl-4-methylphenyl-stearyl-pentaerythritol diphosphite, 2,6-di-tert-butyl-4-methylphenyl-cyclohexyl-pentaerythritol diphosphite, 2,6-di-tert-butyl-4-methylphenyl-benzyl-pentaerythritol diphosphite, 2,6-di-tert-butyl-4-methylphenyl ethyl cellosolve-pentaerythritol diphosphite, 2,6-di-tert-butyl-4-methylphenyl-butylcarbitol-pentaerythritol diphosphite, 2,6-di-tert-butyl-4-methylphenyl-octylphenyl-pentaerythritol diphosphite, 2,6-di-tert-butyl-4-methylphenyl-nonylphenyl-pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-ethylphenyl)pentaerythritol diphosphite, 2,6-di-tert-butyl-4-methylphenyl-2,6-di-tert-butylphenyl-pentaerythritol diphosphite, 2,6-di-tert-butyl-4-methylphenyl-2,4-di-tert-butylphenyl-pentaerythritol diphosphite, 2,6-di-tert-butyl-4-methylphenyl-2,4-di-tert-octylphenyl-pentaerythritol diphosphite, 2,Examples of the diphosphite include 6-di-tert-butyl-4-methylphenyl-2-cyclohexylphenyl-pentaerythritol diphosphite, 2,6-di-tert-amyl-4-methylphenyl-phenyl pentaerythritol diphosphite, bis(2,6-di-tert-amyl-4-methylphenyl)pentaerythritol diphosphite, and bis(2,6-di-tert-octyl-4-methylphenyl)pentaerythritol diphosphite. These pentaerythritol type phosphite compounds may be used alone or in combination of two or more kinds.

[0202] When a phosphorus-based heat stabilizer is used, the content of the phosphorus-based heat stabilizer in the resin composition is preferably 0.01 mass % or more and 1 mass % or less, and more preferably 0.05 mass % or more and 1 mass % or less, relative to the total mass of the resin composition. By setting the content of the phosphorus-based heat stabilizer within the above range, it is possible to further improve the heat aging resistance of the molded article and further reduce the amount of gas generation.

[0203] (3) Amine-based heat stabilizers Examples of the amine-based heat stabilizer include, but are not limited to, 4-acetoxy-2,2,6,6-tetramethylpiperidine, 4-stearoyloxy-2,2,6,6-tetramethylpiperidine, 4-acryloyloxy-2,2,6,6-tetramethylpiperidine, 4-(phenylacetoxy)-2,2,6,6-tetramethylpiperidine, 4-benzoyloxy-2,2,6,6-tetramethylpiperidine, 4-methoxy-2,2,6,6-tetramethylpiperidine, and 4-stearyloxy-2,2,6,6-tetramethylpiperidine. , 4-cyclohexyloxy-2,2,6,6-tetramethylpiperidine, 4-benzyloxy-2,2,6,6-tetramethylpiperidine, 4-phenoxy-2,2,6,6-tetramethylpiperidine, 4-(ethylcarbamoyloxy)-2,2,6,6-tetramethylpiperidine, 4-(cyclohexylcarbamoyloxy)-2,2,6,6-tetramethylpiperidine, 4-(phenylcarbamoyloxy)-2,2,6,6-tetramethylpiperidine, bis(2,2,6,6-tetramethyl-4-piperidyl)-carbonate, bis( 2,2,6,6-tetramethyl-4-piperidyl)-oxalate, bis(2,2,6,6-tetramethyl-4-piperidyl)-malonate, bis(2,2,6,6-tetramethyl-4-piperidyl)-sebacate, bis(2,2,6,6-tetramethyl-4-piperidyl)-adipate, bis(2,2,6,6-tetramethyl-4-piperidyl)-terephthalate, 1,2-bis(2,2,6,6-tetramethyl-4-piperidyloxy)-ethane, α,α'-bis(2,2,6,6-tetramethyl-4-piperidyloxy)-p-xylene, biphenyl Bis(2,2,6,6-tetramethyl-4-piperidyl)tolylene-2,4-dicarbamate, bis(2,2,6,6-tetramethyl-4-piperidyl)-hexamethylene-1,6-dicarbamate, tris(2,2,6,6-tetramethyl-4-piperidyl)-benzene-1,3,5-tricarboxylate, tris(2,2,6,6-tetramethyl-4-piperidyl)-benzene-1,3,4-tricarboxylate, 1-[2-{3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyloxy}butyl]-4-[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyloxy]2,2,6,6-tetramethylpiperidine, a condensate of 1,2,3,4-butanetetracarboxylic acid, 1,2,2,6,6-pentamethyl-4-piperidinol, and β,β,β',β'-tetramethyl-3,9-[2,4,8,10-tetraoxaspiro(5,5)undecane]diethanol, and the like. These amine-based heat stabilizers may be used alone or in combination of two or more kinds.

[0204] When an amine-based heat stabilizer is used, the content of the amine-based heat stabilizer in the resin composition is preferably 0.01 mass % or more and 1 mass % or less, and more preferably 0.05 mass % or more and 1 mass % or less, relative to the total mass of the resin composition. By setting the content of the amine-based heat stabilizer within the above range, the heat aging resistance of the molded article can be further improved, and the amount of gas generation can be further reduced.

[0205] (4) Metal salts of elements in groups 3, 4, and 11 to 14 of the periodic table There are no particular limitations on the metal salts of elements in Groups 3, 4, and 11 to 14 of the periodic table, so long as they are salts of metals belonging to these groups.

[0206] Among these, copper salts are preferred from the viewpoint of further improving the heat aging resistance of the molded article. Examples of such copper salts include, but are not limited to, copper acetate, copper propionate, copper benzoate, copper adipate, copper terephthalate, copper isophthalate, copper salicylate, copper nicotinate, copper stearate, and copper complex salts in which copper is coordinated with a chelating agent.

[0207] Examples of the chelating agent include ethylenediamine and ethylenediaminetetraacetic acid. These copper salts may be used alone or in combination of two or more. Among them, copper acetate is preferable as the copper salt. When copper acetate is used, a resin composition having excellent heat aging resistance and capable of more effectively suppressing metal corrosion of the screw and cylinder part during extrusion (hereinafter, may be simply referred to as "metal corrosion") can be obtained.

[0208] When a copper salt is used as a heat stabilizer, the content of the copper salt in the resin composition is preferably 0.01 parts by mass or more and 0.60 parts by mass or less, and more preferably 0.02 parts by mass or more and 0.40 parts by mass or less, per 100 parts by mass of the thermoplastic resin (A). By ensuring that the copper salt content is within the above range, the heat aging resistance of the molded article can be further improved, and copper precipitation and metal corrosion can be more effectively suppressed.

[0209] In addition, the content of copper element derived from the above copper salt is set to 10% by mass of the thermoplastic resin (A) from the viewpoint of improving the heat aging resistance of the molded product. 6 The amount is preferably from 10 to 2000 parts by mass, more preferably from 30 to 1500 parts by mass, and even more preferably from 50 to 500 parts by mass, based on parts by mass (1 million parts by mass).

[0210] The heat stabilizer components explained above may be used alone or in combination of two or more kinds.

[0211] [Method of producing resin composition] The method for producing the resin composition is not particularly limited as long as it is a method of mixing a thermoplastic resin with a polyamide (A1), and, if necessary, each of the components of a filler (B), a flame retardant (C), a colorant (D) and other additives (E). Hereinafter, the polyamide (A1), the filler (B), the flame retardant (C), the colorant (D) and other additives (E) are also referred to as component (A1), component (B), component (C), component (D) and component (E), respectively.

[0212] Examples of a method for mixing the component (A) and, if necessary, the components (B) to (E) include the following methods (1) to (3). (1) The above-mentioned component (A) and, if necessary, components (B) to (E) are mixed using a Henschel mixer or the like, and the mixture is fed to a melt kneader and kneaded. (2) A method in which the above-mentioned thermoplastic resin, component (A1), and, if necessary, components (C) to (E) are mixed in advance using a Henschel mixer or the like in a single-screw or twin-screw extruder to prepare a mixture, and the mixture is fed to a melt kneader and kneaded, and then, optionally, component (B) is blended in through a side feeder. (3) A method in which the above methods (1) and (2) are used in combination, and component (B) is supplied together with other raw materials at the initial stage and also supplied again from a feeder.

[0213] The components constituting the resin composition may be supplied to the melt kneader in such a manner that all the components are supplied to the same supply port at once, or each component may be supplied from a different supply port.

[0214] When the polyamide (A1) contains an aliphatic polyamide (A1-1), the melt-kneading temperature is preferably about 1°C to 100°C higher than the melting point of the aliphatic polyamide (A1-1), and more preferably about 10°C to 50°C higher than the melting point of the aliphatic polyamide (A1-1). The shear rate in the mixer is 100 sec -1 The average residence time during kneading is preferably about 0.5 minutes or more and 5 minutes or less. The melt-kneading apparatus may be any known apparatus, and for example, a single-screw or twin-screw extruder, a Banbury mixer, a melt-kneader (mixing roll, etc.), etc. are preferably used. The amount of each component blended when producing the resin composition is the same as the content of each component in the resin composition described above.

[0215] [Physical properties of resin composition] The glass transition temperature Tg of the resin composition is preferably 75°C or higher, more preferably 75°C or higher and 220°C or lower, even more preferably 80°C or higher and 210°C or lower, particularly preferably 85°C or higher and 200°C or lower, and most preferably 90°C or higher and 150°C or lower. When the glass transition temperature Tg of the resin composition is within the above range, the gloss of the molded article and the clarity of the marking by laser marking are excellent.

[0216] The glass transition temperature Tg of the resin composition can be measured, for example, by a dynamic viscoelasticity measuring device. Specifically, when the temperature is increased from 23° C. at a rate of 2° C. / min and the applied frequency is 8 Hz, the glass transition temperature Tg is determined as the peak top temperature at which the storage modulus is significantly decreased and the loss modulus is maximized. When two or more loss modulus peaks appear, the peak top temperature of the highest temperature peak is determined as the glass transition temperature Tg. In this case, the measurement frequency is at least once every 20 seconds to improve the measurement accuracy.

[0217] There is no particular restriction on the method for preparing the measurement sample, but from the viewpoint of eliminating the influence of molding distortion, it is preferable to use a cut-out piece of a hot press molded product, and from the viewpoint of thermal conduction, it is preferable that the size (width and thickness) of the cut-out piece be as small as possible.

[0218] The crystallization temperature of the resin composition is preferably 240°C or lower, more preferably 120°C or higher and 235°C or lower, further preferably 130°C or higher and 230°C or lower, and particularly preferably 140°C or higher and 225°C or lower. When the crystallization temperature of the resin composition is within the above range, the joining strength of the molded article by laser welding can be improved, and the appearance of the joined portion can be improved.

[0219] The crystallization temperature of the resin composition can be measured, for example, by DSC. Specifically, in the measurement by DSC, for example, the crystallization temperature is determined as the peak top temperature of the endothermic peak that appears when the temperature is increased from 23° C. at a rate of 10° C. / min. When two or more endothermic peaks appear, the peak top temperature of the endothermic peak on the highest temperature side is determined as the crystallization temperature.

[0220] The enthalpy of the endothermic peak at this time is preferably 10 J / g or more, more preferably 20 J / g or more. In addition, when measuring, it is desirable to heat the sample once to a temperature condition of melting point + 20°C or more to melt the resin, and then cool the sample to 23°C at a temperature decreasing rate of 10°C / min.

[0221] <Welding method and manufacturing method of molded products> The above-mentioned molded article can be produced, for example, by the method described below. That is, the manufacturing method for a laser welded molded article of the present embodiment (hereinafter sometimes abbreviated as "the manufacturing method of the present embodiment") includes a welding method (hereinafter referred to as "welding method" or "laser welding method") in which a molded article obtained by molding a resin composition containing a thermoplastic resin is laser welded.

[0222] In the welding method, the laser welded portion of the obtained molded article is cut along a cross section that includes the normal to the transmitting resin member or the absorbing resin member and is perpendicular to the scanning direction of the laser beam, and the melt pool area is 0.210 mm 2 Above 1.00mm 2 Laser welding is performed as follows.

[0223] The manufacturing method of this embodiment, by having the above-mentioned configuration, can improve the joint strength by laser welding and obtain a molded product having a good appearance at the joints. In other words, the manufacturing method of this embodiment can also be said to be a laser welding method for performing laser welding processing on a molded product with high bonding strength and with a good appearance of the bonded portion.

[0224] [Laser welding method] Examples of lasers used in the laser welding method include carbon dioxide laser, Nd-YAG laser, YAG laser, ruby ​​laser, semiconductor laser, argon laser, excimer laser, etc. Among these, Nd-YAG laser, YAG laser, and semiconductor laser are preferred from the viewpoint of welding processing.

[0225] The wavelength of the laser used is usually 193 nm or more and 1100 nm or less, preferably three wavelength bands of 220 nm or more and 250 nm or less, 520 nm or more and 550 nm or less, or 850 nm or more and 1100 nm or less, more preferably two wavelength bands of 520 nm or more and 550 nm or less, or 850 nm or more and 1050 nm or less, and even more preferably a wavelength band of 900 nm or more and 1000 nm or less. By processing with the laser in these wavelength ranges, the laser is efficiently absorbed by the colorant and resin, suppressing the thermal load on the resin on the transmitting side and improving the appearance of the joint.

[0226] From the viewpoint of shortening the tact time, the scanning speed of laser welding is usually 0.1 mm / sec or more and 3000 mm / sec or less, preferably 1 mm / sec or more and 2000 mm / sec or less, more preferably 5 mm / sec or more and 1000 mm / sec or less, and even more preferably 10 mm / sec or more and 500 mm / sec or less.

[0227] By setting the scanning speed to the above lower limit, it is possible to prevent the laser absorption from becoming excessive and suppress deterioration of the appearance of the laser welded portion due to heating, whereas by setting the scanning speed to the above upper limit, it is possible to absorb a sufficient amount of laser energy and melt uniformly, thereby improving and stabilizing the joining strength.

[0228] The processing output of the laser welding is usually 1.0 W or more and 1000.0 W or less, preferably 5.0 W or more and 800.0 W or less, and more preferably 10.0 W or more and 500.0 W or less. By setting the processing output to the above lower limit, sufficient energy is absorbed from the laser to melt uniformly, improving and stabilizing the joining strength. On the other hand, by setting the scanning speed to the above upper limit or less, the amount of laser absorption is prevented from becoming too large, and deterioration of the appearance of the laser welded portion due to heating can be suppressed.

[0229] The frequency of the laser welding is usually 1 kHz to 1000 kHz or continuous wave, preferably 5 kHz to 750 kHz or continuous wave, and more preferably 10 kHz to 500 kHz or continuous wave. By setting the frequency to the lower limit or more, it is possible to improve the joining strength and the airtightness by welding without gaps. On the other hand, by setting the frequency to the upper limit or less, it is possible to prevent the peak power of the laser from becoming too low and suppress the decrease in strength of the welded portion. In addition, if the frequency is a continuous wave, it is possible to weld without gaps, so this is also a preferred form.

[0230] The diameter of the laser spot for laser welding is usually 0.1 mm or more and 10 mm or less, preferably 0.5 mm or more and 6 mm or less, and more preferably 1 mm or more and 4 mm or less.

[0231] By setting the spot diameter to be equal to or greater than the lower limit, it is possible to prevent excessive energy from being applied and to suppress deterioration of the appearance of the welded portion due to burning, whereas by setting the spot diameter to be equal to or less than the upper limit, it is possible to prevent a situation in which sufficient energy required for melting is not applied due to energy dispersion, resulting in failure to weld the portion, and suppress a decrease in the strength of the welded portion.

[0232] The pitch interval of the laser welding is usually 0.1 μm or more and 500 μm or less, preferably 1 μm or more and 250 μm or less, and more preferably 5 μm or more and 250 μm or less. By setting the pitch interval to the above lower limit, it is possible to prevent the laser absorption amount from becoming too large and suppress deterioration of the appearance of the laser welded portion due to heating, while by setting the scanning speed to the above upper limit or less, it is possible to absorb sufficient energy from the laser and melt uniformly, thereby improving and stabilizing the joining strength.

[0233] [Molding process] The manufacturing method of this embodiment may further include a molding step prior to the laser welding step by the welding method. In the molding step, the above-mentioned resin composition is molded to obtain an intermediate molded product that does not have any joints formed by laser welding. The method for obtaining the intermediate molded product is not particularly limited, and any known molding method can be used.

[0234] Examples of known molding methods include extrusion molding, injection molding, vacuum molding, blow molding, injection compression molding, decorative molding, other material molding, gas-assisted injection molding, foam injection molding, low-pressure molding, ultra-thin-wall injection molding (ultra-high-speed injection molding), and in-mold composite molding (insert molding, outsert molding).

[0235] <Applications of molded products> The molded article of this embodiment can be used for a variety of purposes because of the high bonding strength achieved by laser welding and the good appearance of the bonded parts.

[0236] The molded article of the present embodiment can be suitably used in, for example, the automotive field, the electrical and electronic field, the mechanical and industrial field, parts for transporting fluids such as air and liquid, the office equipment field, and the aviation and space fields.

[0237] The molded article of the present embodiment can be particularly suitably used as an electric / electronic component in applications in the electric / electronic field, such as battery housings for lithium secondary batteries, current measuring components, magnet switch housings, breaker housings, various switch components, camera module housings, camera modules, lens barrels (lens barrels), and molded articles for connectors, and can be more suitably used as battery housings for lithium secondary batteries, magnet switch housings, breaker housings, camera module housings, camera modules, lens barrels (lens barrels), or molded articles for connectors. EXAMPLES

[0238] The present invention will be described in detail below with reference to specific examples and comparative examples, but the present invention is not limited to the following examples.

[0239] Each of the components of the resin compositions used in the molded articles of the Examples and Comparative Examples will be described below.

[0240] <Components> [Aliphatic polyamide (A1-1)] A1-1-1: Polyamide 66

[0241] [Semi-aromatic polyamide (A1-2)] A1-2-1: Polyamide 6I A1-2-2: Polyamide 66 / 6I (copolymer)

[0242] Filler B-1: Glass fiber (GF) (manufactured by Nippon Electric Glass, product name "ECS03T275H", average fiber diameter 10 μmφ, cut length 3 mm)

[0243] [Flame retardant (C)] C-1: Phosphinic acid flame retardant Aluminum diethylphosphinate (manufactured by Clariant, product name: "Exolit OP1230")

[0244] [Colorant (D)] D1: Carbon black (primary particle size 27 nm)

[0245] <Production of polyamide> The manufacturing methods of the aliphatic polyamide A1-1-1, the semi-aromatic polyamide A1-2-1, and the semi-aromatic polyamide A1-2-2 are described in detail below. The aliphatic polyamide A1-1-1, the semi-aromatic polyamide A1-2-1, and the semi-aromatic polyamide A1-2-2 obtained by the manufacturing methods below are dried in a nitrogen stream to adjust the moisture content to about 0.2 mass%, and then used as the raw material of the resin composition used in the molded products of the examples and comparative examples described later.

[0246] [Synthesis Example 1] (Synthesis of Aliphatic Polyamide A1-1-1 (Polyamide 66)) The polymerization reaction of polyamide was carried out by the "thermal melt polymerization method" as follows. First, 1500 g of an equimolar salt of adipic acid and hexamethylenediamine was dissolved in 1500 g of distilled water to prepare a homogeneous aqueous solution of 50% by mass of the raw material monomers. This aqueous solution was charged into an autoclave with an internal volume of 5.4 L and substituted with nitrogen. Next, the solution was concentrated by gradually removing steam to a solution concentration of 70% by mass while stirring at a temperature of about 110°C to 150°C. Next, the internal temperature was raised to 220°C. At this time, the autoclave was pressurized to 1.8 MPa. The reaction was continued for 1 hour while gradually removing steam and maintaining the pressure at 1.8 MPa until the internal temperature reached 245°C. Next, the pressure was lowered over 1 hour. Next, the inside of the autoclave was maintained under a reduced pressure of 650 torr (86.66 kPa) for 10 minutes using a vacuum device. At this time, the final internal temperature of the polymerization was 265°C. The mixture was then pressurized with nitrogen to form a strand from the lower spinneret (nozzle), cooled with water, cut, and discharged in pellet form. The pellets were then dried at 100°C under a nitrogen atmosphere for 12 hours to obtain aliphatic polyamide A1-1-1 (polyamide 66).

[0247] [Synthesis Example 2] (Synthesis of semi-aromatic polyamide A1-2-1 (polyamide 6I)) The polymerization reaction of polyamide was carried out by the "thermal melt polymerization method" as follows. First, 1500 g of an equimolar salt of isophthalic acid and hexamethylenediamine, 1.5 mol % excess adipic acid relative to the total equimolar salt components, and 0.5 mol % acetic acid were dissolved in 1500 g of distilled water to prepare a 50 mass % equimolar homogeneous aqueous solution of raw material monomers. Next, the solution was concentrated by gradually removing steam to a solution concentration of 70 mass % while stirring at a temperature of about 110 ° C. to 150 ° C. Next, the internal temperature was raised to 220 ° C. At this time, the autoclave was pressurized to 1.8 MPa. The reaction was continued for 1 hour while gradually removing steam and maintaining the pressure at 1.8 MPa until the internal temperature reached 245 ° C. Next, the pressure was reduced over 30 minutes. Next, the inside of the autoclave was maintained at a reduced pressure of 650 torr (86.66 kPa) for 10 minutes using a vacuum device. At this time, the final internal temperature of the polymerization was 265 ° C. The mixture was then pressurized with nitrogen to form a strand from the lower spinneret (nozzle), cooled with water, cut, and discharged in pellet form. The pellets were then dried at 100°C under a nitrogen atmosphere for 12 hours to obtain semi-aromatic polyamide A1-2-1 (polyamide 6I).

[0248] [Synthesis Example 3] (Synthesis of semi-aromatic polyamide A1-2-2 (polyamide 66 / 6I (copolymer))) 2.00 kg of an equimolar salt of adipic acid and hexamethylenediamine, 0.50 kg of an equimolar salt of isophthalic acid and hexamethylenediamine, and 2.5 kg of pure water were charged into a 5 L autoclave and thoroughly stirred. After sufficient nitrogen replacement, the temperature was raised from room temperature to 220°C over about 1 hour while stirring. During this time, the internal pressure was 18 kg / cm due to the natural pressure of water vapor inside the autoclave. 2 G, but 18kg / cm 2Heating was continued while removing water from the reaction system so that the pressure did not exceed G. After another 2 hours, when the internal temperature reached 260°C, heating was stopped, the exhaust valve of the autoclave was closed, and the autoclave was cooled to room temperature over about 8 hours. After cooling, the autoclave was opened, and about 2 kg of polymer was taken out and pulverized. The pulverized polymer obtained was placed in a 10L evaporator and solid-phase polymerized at 200°C for 10 hours under a nitrogen stream. Next, the mixture was pressurized with nitrogen and made into a strand shape from the lower spinneret (nozzle), water-cooled, cut, and discharged in pellet form. The pellets were then dried at 100°C under a nitrogen atmosphere for 12 hours to obtain semi-aromatic polyamide A1-2-2 (polyamide 66 / 6I).

[0249] <Production of Resin Composition> [Production Example 1] Using a TEM 35mm twin-screw extruder (set temperature: 280°C, screw speed: 300 rpm) manufactured by Toshiba Machine Co., Ltd., a pre-blended aliphatic polyamide A1-1-1 and semi-aromatic polyamide A1-2-1 were fed from the top feed port provided at the most upstream part of the extruder. The molten mixture extruded from the die head was cooled in a strand shape and pelletized to obtain pellets of the resin composition. The blending amounts were as shown in Table 1.

[0250] [Manufacturing Examples 2 to 7] Each resin composition was produced in the same manner as in Production Example 1, except that the amounts of components (A) to (C) were as shown in Table 1 and filler B-1 was fed from a side feed port downstream of the extruder (when the resin fed from the top feed port was fully molten).

[0251] [Table 1]

[0252] <Physical properties and evaluation> First, the pellets of each resin composition obtained in Production Examples 1 to 7 were dried in a nitrogen stream to reduce the moisture content in the resin composition to 500 ppm or less. Next, the pellets of each resin composition with the adjusted moisture content were measured for various physical properties using the following method. In addition, the molded products described below were measured for various physical properties and evaluated.

[0253] [Physical Properties 1] (glass transition temperature Tg) The pellets of each resin composition obtained in Production Examples 1 to 7 were molded into molded articles conforming to JIS-K7139 using a PS40E injection molding machine manufactured by Nissei Kogyo Co., Ltd., with the following conditions: cooling time 15 seconds, screw rotation speed 100 rpm, cylinder temperature 290°C, mold temperature 80°C, and filling time in the range of 1.5 seconds ± 0.1 seconds. The injection pressure and injection speed were appropriately adjusted. The molded articles were measured under the following conditions using a dynamic viscoelasticity evaluation device (EPLEXOR500N manufactured by GABO Co., Ltd.).

[0254] (Measurement conditions) Measurement mode: Tensile Measurement frequency: 8Hz Heating rate: 3℃ / min Temperature range: -100℃ to 250℃

[0255] The ratio of the loss modulus E2 to the storage modulus E1 (E2 / E1) was defined as tan δ, and the temperature at which tan δ was maximum was defined as the glass transition temperature Tg.

[0256] [Physical Properties 2] (Crystallization peak temperature) The crystallization peak temperature was measured in accordance with JIS-K7121 using a Diamond-DSC manufactured by PERKINELMER as follows. The measurement was carried out under a nitrogen atmosphere. First, about 10 mg of the resin composition was heated from 50°C to 350°C at a heating rate of 20°C / min. Then, after keeping at 350°C for 3 minutes, it was cooled from 350°C to 50°C at a cooling rate of 20°C / min. After keeping at 50°C for 3 minutes, it was heated again from 50°C to 350°C at a heating rate of 20°C / min. After keeping at 350°C for 3 minutes, it was cooled from 350°C to 50°C at a cooling rate of 20°C / min. The crystallization peak temperature that appeared at this time was measured.

[0257] The measurement results of physical property 1 (glass transition temperature Tg) and physical property 2 (crystallization peak temperature) are shown in Table 2. [Table 2]

[0258] (Laser welding test piece 1 created) For the pellets of each resin composition obtained in Production Examples 1 to 7, an injection molding machine [IS150E: manufactured by Toshiba Machine Co., Ltd.] was used to prepare laser welding test piece 1 (6 cm x 2.5 cm, thickness 2 mm) by setting the cooling time to 15 seconds, the screw rotation speed to 100 rpm, the cylinder temperature to 290°C, and the mold temperature to 80°C, and adjusting the injection pressure and injection speed appropriately so that the filling time was in the range of 0.4±0.1 seconds.

[0259] (Laser welding test piece 2 created) The resin composition pellets obtained in Production Example 1 were dry-blended with a colored masterbatch for laser welding (Orient Chemical Industry: eBIND ACW-9871, hereinafter simply referred to as ACW) at a dilution ratio of 60 times, and using an injection molding machine [IS150E: manufactured by Toshiba Machine Co., Ltd.], the cooling time was set to 15 seconds, the screw rotation speed to 100 rpm, the cylinder temperature to 290°C, and the mold temperature to 80°C, and the injection pressure and injection speed were appropriately adjusted so that the filling time was in the range of 0.4±0.1 seconds, to produce a laser welding test piece 2 (60 mm, 25 mm, thickness 2 mm).

[0260] (Laser welding test piece 3 created) For the pellets of each resin composition obtained in Production Examples 1 to 7, 1500 ppm of colorant D1 was dry blended with 100 parts by mass of the resin composition, and using an injection molding machine [IS150E: manufactured by Toshiba Machine Co., Ltd.], the cooling time was set to 15 seconds, the screw rotation speed to 100 rpm, the cylinder temperature to 290°C, and the mold temperature to 80°C. The injection pressure and injection speed were appropriately adjusted so that the filling time was in the range of 0.4±0.1 seconds, and laser welding test piece 3 (60 mm, 25 mm, thickness 2 mm) was produced.

[0261] (Laser welding test piece 4 created) For the pellets of each resin composition obtained in Production Examples 1 to 7, an injection molding machine [IS150E: manufactured by Toshiba Machine Co., Ltd.] was used to prepare laser welding test piece 4 (6 cm x 2.5 cm, thickness 2 mm) by setting the cooling time to 15 seconds, the screw rotation speed to 100 rpm, the cylinder temperature to 290°C, and the mold temperature to 30°C, and adjusting the injection pressure and injection speed appropriately so that the filling time was in the range of 0.4±0.1 seconds.

[0262] (Laser welding and joint strength measurement) The laser welding process will be described with reference to FIG. 3. The laser welding test pieces 1 to 4 were combined as shown in Tables 3 to 5, and the transmissive resin member 1 and the absorptive resin member 2 were overlapped and fixed so that L3 was 20 mm in the long direction. In FIG. 3, L1 is 25 mm and L2 is 60 mm. Furthermore, the top surface of the transmissive resin member 1 was pressed down with a glass plate (a square with a length and width of 15 cm and a thickness of 10 mm) to fix the position of each resin member and to increase the cooling efficiency of the resin heated during laser irradiation. In this state, the laser was irradiated parallel to L1 from 3a to 3b in FIG. 3, and a linear laser irradiation was performed once to create a test piece. In addition, the test piece was created while simultaneously blowing air to cool it. 3a and 3b in FIG. 3 show the end located at the center 10 mm part of L3. In addition, the laser wavelength and frequency were as follows. Laser wavelength: 940nm Laser frequency: Continuous wave (CW)

[0263] The absorption side in Tables 3 to 5 is the side on which the light that has passed through the transmission side is incident. The laser output and scanning speed are shown in Tables 3 to 5. The laser spot diameter was 2.4 mm.

[0264] The welded parts of the laser welded test pieces prepared by the above method were visually inspected and their appearance was judged. The judging criteria were classified into the following three categories. Good: Appearance is good, and the laser welded areas are not noticeable. △: The laser welded area has a different luster from the surrounding area, making it clear that it is a welded area. ×: The laser welded area is burned.

[0265] The test pieces laser welded by the above method were subjected to a tensile test using an Instron universal testing machine, with both ends of the absorption side and the transmission side clamped in chucks using a 30kN load cell, with a chuck distance of 55mm and a tensile test speed of 5.0mm / min, to measure the maximum point load. Tensile tests were performed at five points for each sample. In the tensile test, the permeable resin member 1 and the absorptive resin member 2 were pulled in the directions shown by the arrows in Figure 4. Plates 3 and 4 are spacers installed to attach the permeable resin member 1 and the absorptive resin member 2 to the measuring device. Plates 3 and 4 have the same thickness as the permeable resin member 1 and the absorptive resin member 2, respectively.

[0266] The fracture mode after the tensile test was also confirmed. A fracture of the base material was counted when the base material broke at the joint, or when a part of the base material on the permeation side or the base material on the absorption side was welded to the other. The destruction of the base material means that the bonding by laser welding is sufficient, whereas the separation at the interface without destruction of the base material means that the absorbing resin member is not melted or the transmitting resin member has not sufficiently absorbed the heat of the absorbing resin member, resulting in an unstable bond. Therefore, the higher the rate of base material destruction, the more stable the bonded state is, which is desirable for laser welding.

[0267] (Observation of the molten pool) How to obtain a cross section The test pieces laser welded by the above method were cut vertically through the center of the short side including the joint, to create a cross section perpendicular to the scanning direction of the laser light and expose the molten pool. That is, the molded product was cut in a direction including the normal line of the transmitting resin member or the absorbing resin member and perpendicular to the scanning direction of the laser beam.

[0268] Unnecessary parts not related to the observation of the molten pool were cut off, and the observation piece including the molten pool was embedded in Epomount manufactured by Refine Tech Co., Ltd. The hardening conditions were that it was left to stand in a 40°C environment for 12 hours.

[0269] After the embedding agent hardened, the observation surface was polished using a rotary polishing machine (MA-600e, manufactured by Musashino Electronics Co., Ltd.) The abrasive grain sizes during polishing were 20 μm, 13 μm, 9 μm, 2 μm, and 0.5 μm in this order.

[0270] Next, an etching operation was performed. The test pieces using the resin compositions of Production Examples 1 and 3 to 6 were immersed in a 15 mol / L formic acid solution for 30 seconds before observation. The test piece using the resin composition of Production Example 2 was immersed in a 15 mol / L formic acid solution for 300 seconds before observation. The test piece using the resin composition of Production Example 7 was immersed in a 15 mol / L calcium chloride solution (solvent: ethanol) for 30 seconds before observation.

[0271] The molten pool was observed using an optical microscope, VHX6000, manufactured by Keyence Corp. The observation magnification was 50x, which is a magnification at which the entire molten pool fits within the field of view.

[0272] How to calculate the area of ​​the molten pool The area of ​​the molten pool was measured using the specified area measurement function of the device for the optical microscope image of the cross section of the molded product obtained by the above-mentioned method. The area specified for measuring the area of ​​the molten pool was the outer periphery of the molten pool that passed both ends of the length x of the maximum diameter and both ends of the maximum diameter y perpendicular to x as shown in Figure 2.

[0273] (Gloss measurement) The 60 degree gloss (%) was measured in accordance with JIS-K7150 using a glossmeter (HORIBA IG320) for the center of the laser welding test piece 3. The larger the measured value, the better the gloss, and a gloss of 60% or more was determined to be good.

[0274] (Light transmittance measurement) The light transmittance at a wavelength of 940 nm of the laser welding test pieces 1, 2, or 4 prepared as the transparent resin members was measured using an apparatus consisting of a JASCO Corporation (V670) combined with an integrating sphere "ILN-725". The higher the transmittance, the better the light transmittance, and a value of 30% or more was evaluated as good.

[0275] According to the above-described method for preparing the laser welding test piece, a test piece was prepared from each resin composition, and laser welding and evaluation were performed. The combinations of the resin composition and the type of test piece used in each example and each comparative example, and the evaluation results are summarized in Tables 3 to 5.

[0276] [Table 3]

[0277] [Table 4]

[0278] [Table 5]

[0279] From Tables 3 to 5, the molten pool area is 0.21 mm 2 Over 1.00mm 2 In the following Examples 1 to 12, the weld strength and the appearance of the welded portion were good. On the other hand, the molten pool area is 0.21 mm 2In the comparative examples 1, 2, and 7 to 10, the bonding strength was low, and the molten pool area was less than 1.00 mm 2 The appearance of the laser welded parts was poor in the above Comparative Examples 3, 4, and 5. Furthermore, Comparative Examples 11 to 13, which used the resin composition of Production Example 7, which had a Tg of 80° C., showed poor results in at least two of the evaluations of bonding strength, appearance of the laser welded parts, and gloss.

[0280] From the above, it became clear that molded products with a molten pool area within a specific numerical range have excellent joint strength by laser welding and excellent appearance of the welded parts. [Industrial Applicability]

[0281] According to the molded article and manufacturing method of the present embodiment, a molded article having excellent joint strength, reliability of the joint, and appearance characteristics of the joint can be obtained by laser welding. The molded article of the present embodiment can be suitably used in, for example, the automotive field, the electrical and electronic field, the mechanical and industrial field, the office equipment field, and the aviation and space field.

Claims

1. A molded product in which a transparent resin member and an absorptive resin member are laser welded together, a joint portion where the transmissible resin member and the absorbing resin member are joined by laser welding; a molten pool is observed at the joint in a cross section including a normal to the transmissive resin member or the absorbing resin member and perpendicular to the scanning direction of the laser beam; The area of ​​the molten pool is 0.210 mm 2 More than 1.00 mm 2 is as follows: The transmissive resin member and the absorptive resin member are each molded from a resin composition, The resin composition contains a thermoplastic resin, The thermoplastic resin contains at least a polyamide-based resin (A1), The resin composition has a glass transition temperature of 85° C. or higher.

2. The molded article according to claim 1 , wherein the resin composition contains a filler (B).

3. 3. The molded product according to claim 1, wherein the light transmitting resin member has a light transmittance of 30% or more for a light wavelength of 940 nm.

4. The molded product according to claim 1 or 2, wherein the transparent resin member has a thickness of 0.3 mm or more and 5 mm or less.

5. The molded article according to claim 1 or 2, wherein the resin composition contains 0 parts by mass or more and 150 parts by mass or less of a filler (B) relative to 100 parts by mass of the thermoplastic resin.

6. The molded article according to claim 2, wherein the filler (B) is one or more of glass fiber, calcium carbonate, talc, mica, wollastonite, and milled fiber.

7. The molded article according to claim 1 or 2, wherein the polyamide resin (A1) is a semi-aromatic polyamide (A1-2) containing an aromatic ring in the skeleton, or an alloy of the semi-aromatic polyamide (A1-2) and the aliphatic polyamide (A1-1).

8. The content of the semi-aromatic polyamide (A1-2) is 5.0 parts by mass or more and 100.0 parts by mass or less relative to a total of 100.0 parts by mass of the aliphatic polyamide (A1-1) and the semi-aromatic polyamide (A1-2). The molded article according to claim 7.

9. The molded article according to claim 7, wherein the content of an isophthalic acid component in 100 mol % of a dicarboxylic acid component constituting the semi-aromatic polyamide (A1-2) is 10 mol % or more.

10. The molded article according to claim 1 or 2, wherein the resin composition contains a flame retardant (C).

11. The molded article according to claim 10, wherein the flame retardant (C) is either or both of a phosphinate and a diphosphinate.

12. The phosphinate is a compound represented by the following general formula (I): The molded article according to claim 11, wherein the diphosphinic acid salt is a compound represented by the following general formula (II): 【Chemistry 1】 (In general formula (I), R 11 and R 12 Each of M is independently an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 10 carbon atoms. n11+ is a metal ion having a valence of n11. M is an element belonging to Group 2 or Group 15 of the Periodic Table, a transition element, zinc, or aluminum. n11 is 2 or 3. When n11 is 2 or 3, a plurality of R 11 and R 12 may be the same or different. In general formula (II), R 21 and R 22 Each of Y is independently an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 10 carbon atoms. 21 M' is an alkylene group having 1 to 10 carbon atoms or an arylene group having 6 to 10 carbon atoms. m21+ is a metal ion having a valence of m21. M' is an element belonging to Group 2 or Group 15 of the Periodic Table, a transition element, zinc, or aluminum. n21 is an integer of 1 to 3. When n21 is 2 or 3, a plurality of R 21 , R 22 and Y 21 may be the same or different. m21 is 2 or 3. x is 1 or 2. When x is 2, multiple M' may be the same or different. n21, x, and m21 are integers that satisfy the relational expression 2×n21=m21×x.

13. The molded article according to claim 1 or 2, wherein the resin composition further contains a colorant (D).

14. The molded article according to claim 13, wherein the resin composition forming the absorbing resin member contains a colorant (D1) for absorbing a laser.

15. The molded product according to claim 13 , wherein the resin composition forming the transmissive resin member contains a colorant (D2) that transmits a laser.

16. The molded article according to claim 1 or 2, which has a sealed structure joined by laser welding.

17. The molded article according to claim 1 or 2, which is used for a battery case for a lithium secondary battery, a sensor case, a camera case, a housing for an image or video shooting part, a magnet switch housing, a breaker housing, a connector, a housing for a secondary battery, a current sensor case, a camera module housing, a camera module, or a lens barrel.

18. A method for laser welding a transmissive resin member and an absorptive resin member, comprising the steps of: The transparent resin member and the absorbing resin member are molded from a resin composition, The resin composition contains a thermoplastic resin, The transparent resin member and the absorbing resin member are laser-welded to each other, In a cross section including a normal line of the transmissive resin member or the absorptive resin member and perpendicular to the scanning direction of the laser beam, the area of ​​the molten pool observed at the laser welded joint is 0.210 mm 2 More than 1.00 mm 2 A welding method which produces a molded product as follows:

19. A method for producing a molded product using the welding method according to claim 18.

Citation Information

Patent Citations

  • Flame resistant resin molded article and method of producing the same

    JP2019025673A

  • Polyamide composition, method for producing the same, and molded article

    JP2020193333A

  • JPP6937531B

  • Polyamide resin composition, molded body thereof, and method for manufacturing laser-welded body

    WO2019160117A1