Plating Method

The plating method addresses the issue of non-uniform bump heights by employing a forward current followed by a reverse current pulse, ensuring uniform deposition through controlled substrate rotation and solution stirring alignment.

JP7558461B1Active Publication Date: 2024-09-30EBARA CORP

Patent Information

Application Number
JP2024535244
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-03-06
Publication Date
2024-09-30
Estimated Expiration
2044-03-06

AI Technical Summary

Technical Problem

Conventional plating methods struggle to achieve uniform height of bumps formed on substrates, necessitating an improvement in the uniformity of the plating process.

Method used

A plating method involving a first plating process with a forward current followed by a second plating process with a reverse current pulse, where the substrate holder is rotated and the plating solution is stirred, with specific alignment of the aperture density change direction relative to the flow direction of the plating solution to enhance uniformity.

Benefits of technology

The method effectively achieves uniform heights of bumps by uniformly distributing the plating solution and promoting even deposition, reducing variations in bump height.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007558461000001
    Figure 0007558461000001
  • Figure 0007558461000002
    Figure 0007558461000002
  • Figure 0007558461000003
    Figure 0007558461000003
Patent Text Reader

Abstract

To provide a technique capable of making bump height uniform. The plating method includes acquiring an opening density change direction Dr2, holding the substrate Wf for which the opening density change direction has been acquired in a substrate holder 30, immersing the substrate held by the substrate holder in plating solution Ps so that it faces the anode, performing a first plating process in which a forward current is supplied to the power source 80 while rotating the substrate holder and stirring the plating solution with a stirring mechanism 60, performing a second plating process in which a reverse current pulse is supplied to the power source while stirring the plating solution with the stirring mechanism, with the rotation of the substrate holder stopped in a state in which the opening density change direction is non-parallel to the direction Dr1 of flow of the plating solution stirred by the stirring mechanism, and performing the first plating process again.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a plating method. [Background technology]

[0002] Conventionally, plating methods for plating a substrate are known (see, for example, Patent Documents 1, 2, and 3). A plating apparatus used in such a plating method includes, for example, a plating tank that stores a plating solution and in which an anode is disposed, a substrate holder that holds a substrate as a cathode facing the anode, a power source configured to supply a current between the substrate and the anode, and a stirring mechanism configured to stir the plating solution (see, for example, Patent Documents 1 and 2).

[0003] Patent Documents 2 and 3 also disclose a technique for forming bumps by depositing metal on a substrate by plating. Patent Documents 2 and 3 also disclose a technique for controlling a power supply so that a forward current and a reverse current pulse are supplied to a substrate and an anode in a plating method using a plating solution containing an accelerator for accelerating plating. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 7079388 [Patent Document 2] Patent No. 7357824 [Patent Document 3] JP 2006-131926 A Summary of the Invention [Problem to be solved by the invention]

[0005] In recent years, there has been a demand for uniform height of bumps formed on a substrate by plating. In this regard, there is room for improvement in conventional techniques.

[0006] The present invention has been made in view of the above, and has as its object to provide a technique capable of making the height of bumps uniform. [Means for solving the problem]

[0007] (Aspect 1) In order to achieve the above object, a plating method according to one aspect of the present invention includes: acquiring an opening density change direction, which is a direction in which an opening density of a photoresist layer provided on a substrate changes; holding the substrate for which the opening density change direction has been acquired in a substrate holder; immersing the substrate held by the substrate holder in a plating solution of a plating tank in which a plating solution containing an accelerator that accelerates plating is stored and in which an anode is disposed, so as to face the anode; rotating the substrate holder and stirring the plating solution with a stirring mechanism while rotating the substrate holder and stirring the plating solution with a stirring mechanism. The method includes performing a first plating process by causing a power source configured to supply a current between the anode and the plating solution to supply a forward current for depositing metal from the plating solution onto the substrate; performing a second plating process by causing the power source to supply a reverse current pulse, which is a current that flows in pulses in the opposite direction to the forward current, while stirring the plating solution with the stirring mechanism, while stopping rotation of the substrate holder in a state where the direction of change in opening density is non-parallel to the direction of flow of the plating solution stirred by the stirring mechanism; and performing the first plating process again.

[0008] According to this aspect, it is possible to make the height of the bumps formed by the metal deposited on the substrate uniform.

[0009] (Aspect 2) In the above first aspect, in the second plating process, the direction of change in the opening density may be perpendicular to a direction of flow of the plating solution stirred by the stirring mechanism.

[0010] (Aspect 3) In the above-mentioned embodiment 1 or embodiment 2, the stirring mechanism may include a paddle configured to stir the plating solution in the plating tank by reciprocating movement, and the direction in which the paddle reciprocates may be used as the direction of flow of the plating solution stirred by the stirring mechanism in the second plating process. [Brief description of the drawings]

[0011] [Figure 1] 1 is a perspective view showing an overall configuration of a plating apparatus according to an embodiment; [Diagram 2] 1 is a plan view showing an overall configuration of a plating apparatus according to an embodiment; [Diagram 3] FIG. 2 is a schematic diagram showing a configuration of a plating module according to an embodiment. [Figure 4] FIG. 2 is a schematic diagram showing a state in which a substrate according to an embodiment is immersed in a plating solution. [Diagram 5] FIG. 2 is a schematic plan view of a paddle according to an embodiment. [Figure 6] Fig. 6(A) is a schematic diagram for explaining the surface configuration of the substrate according to the embodiment, and Fig. 6(B) is a schematic diagram showing an example of an opening pattern of a photoresist layer according to the embodiment. [Figure 7] 7(A) and 7(B) are diagrams for explaining an example of a time waveform of a current supplied from a power supply to an anode and a substrate according to an embodiment. [Figure 8] 7 is a graph showing an example of measuring the height of a bump in each pattern region when a plurality of bumps are formed on a substrate having a photoresist layer as exemplified in FIG. 6(B). [Figure 9] 1 is an example of a flowchart for explaining a plating method according to an embodiment. [Figure 10] 5 is a schematic plan view for explaining a direction in which the opening density of the substrate according to the embodiment changes. FIG. [Figure 11] Figures 11(A) and 11(B) are diagrams for explaining how the degree of uniformity of bump height changes depending on the angle between the direction of change in opening density on the substrate and the direction of plating solution flow during stirring. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. The drawings are shown in a schematic manner to facilitate understanding of the characteristics of the components, and the dimensional ratios of the components are not necessarily the same as those in reality. In addition, some drawings show XYZ orthogonal coordinates for reference. In these orthogonal coordinates, the Z direction corresponds to the upward direction, and the -Z direction corresponds to the downward direction (the direction in which gravity acts).

[0013] Fig. 1 is a perspective view showing the overall configuration of a plating apparatus 1000 according to an embodiment. Fig. 2 is a plan view (top view) showing the overall configuration of the plating apparatus 1000 according to an embodiment. As shown in Figs. 1 and 2, the plating apparatus 1000 includes a load port 100, a transfer robot 110, an aligner 120, a pre-wet module 200, a pre-soak module 300, a plating module 400, a cleaning module 500, a spin rinse dryer 600, a transfer device 700, and a control module 800.

[0014] The load port 100 is a module for loading a substrate accommodated in a cassette such as a FOUP (not shown) into the plating apparatus 1000 and for unloading a substrate from the plating apparatus 1000 to the cassette. In this embodiment, four load ports 100 are arranged in a horizontal line, but the number and arrangement of the load ports 100 are arbitrary. The transfer robot 110 is a robot for transferring a substrate, and is configured to transfer a substrate between the load port 100, the aligner 120, the pre-wet module 200, and the spin rinse dryer 600. When transferring a substrate between the transfer robot 110 and the transfer apparatus 700, the transfer robot 110 and the transfer apparatus 700 can transfer the substrate via a temporary placement table (not shown).

[0015] The aligner 120 is a module for aligning the position of an orientation flat, a notch, etc. of a substrate to a predetermined direction. In this embodiment, two aligners 120 are arranged side by side in the horizontal direction, but the number and arrangement of the aligners 120 are arbitrary. The pre-wet module 200 wets the surface to be plated of the substrate before plating with a treatment liquid such as pure water or degassed water, thereby replacing air inside a pattern formed on the substrate surface with the treatment liquid. The pre-wet module 200 is configured to perform a pre-wet process that makes it easier to supply plating liquid to the inside of the pattern by replacing the treatment liquid inside the pattern with a plating liquid during plating. In this embodiment, two pre-wet modules 200 are arranged side by side in the vertical direction, but the number and arrangement of the pre-wet modules 200 are arbitrary.

[0016] The presoak module 300 is configured to perform a presoak process in which an oxide film with high electrical resistance present on the surface of a seed layer formed on the surface to be plated of a substrate before plating is etched away with a treatment liquid such as sulfuric acid or hydrochloric acid to clean or activate the surface of the substrate to be plated. In this embodiment, two presoak modules 300 are arranged vertically, but the number and arrangement of the presoak modules 300 are arbitrary. The plating module 400 applies plating to the substrate. In this embodiment, two sets of 12 plating modules 400 are arranged vertically, three modules, and horizontally, four modules, for a total of 24 plating modules 400, but the number and arrangement of the plating modules 400 are arbitrary.

[0017] The cleaning module 500 is configured to perform a cleaning process on the substrate to remove plating solution and the like remaining on the substrate after plating. In this embodiment, two cleaning modules 500 are arranged vertically, but the number and arrangement of the cleaning modules 500 are arbitrary. The spin rinse dryer 600 is a module for drying the substrate after cleaning by rotating it at high speed. In this embodiment, two spin rinse dryers 600 are arranged vertically, but the number and arrangement of the spin rinse dryers 600 are arbitrary. The transport device 700 is a device for transporting the substrate between multiple modules in the plating apparatus 1000. The control module 800 is configured to control multiple modules of the plating apparatus 1000, and can be configured from, for example, a general computer or a dedicated computer equipped with an input / output interface with an operator.

[0018] An example of a series of plating processes performed by the plating apparatus 1000 will be described. First, a substrate stored in a cassette is carried into the load port 100. Next, the transfer robot 110 removes the substrate from the cassette of the load port 100 and transfers the substrate to the aligner 120. The aligner 120 aligns the positions of the orientation flat, notch, etc. of the substrate to a predetermined direction. The transfer robot 110 delivers the substrate, whose direction has been aligned by the aligner 120, to the pre-wet module 200.

[0019] The pre-wet module 200 performs a pre-wet process on the substrate. The transport device 700 transports the substrate that has been subjected to the pre-wet process to the pre-soak module 300. The pre-soak module 300 performs a pre-soak process on the substrate. The transport device 700 transports the substrate that has been subjected to the pre-soak process to the plating module 400. The plating module 400 platings the substrate.

[0020] The transfer device 700 transfers the plated substrate to the cleaning module 500. The cleaning module 500 performs a cleaning process on the substrate. The transfer device 700 transfers the cleaned substrate to the spin rinse dryer 600. The spin rinse dryer 600 dries the substrate. The transfer robot 110 receives the substrate from the spin rinse dryer 600 and transfers the dried substrate to a cassette on the load port 100. Finally, the cassette containing the substrate is removed from the load port 100.

[0021] It should be noted that the configuration of the plating apparatus 1000 described in FIG. 1 and FIG. 2 is merely an example, and the configuration of the plating apparatus 1000 is not limited to the configuration in FIG.

[0022] Next, a description will be given of the plating module 400. Since the plating modules 400 included in the plating apparatus 1000 according to this embodiment have the same configuration, one plating module 400 will be described.

[0023] Fig. 3 is a schematic diagram showing the configuration of a plating module 400 in the plating apparatus 1000. Specifically, Fig. 3 is a schematic diagram showing the plating module 400 in a state before the substrate Wf is immersed in the plating solution Ps. Fig. 4 is a schematic diagram showing a state in which the substrate Wf is immersed in the plating solution Ps.

[0024] 3 and 4 is, for example, a plating apparatus (a so-called cup-type plating apparatus) in which the substrate Wf is immersed in the plating solution Ps with the surface direction of the substrate Wf in a horizontal direction. However, the configuration of the plating apparatus 1000 is not limited thereto, and may be, for example, a plating apparatus in which the substrate Wf is immersed in the plating solution Ps with the surface direction of the substrate Wf in a non-horizontal direction (for example, a direction perpendicular to the ground).

[0025] A plating module 400 of a plating apparatus 1000 illustrated in Figures 3 and 4 includes a plating tank 10, an overflow tank 20, a substrate holder 30, and a paddle 70 as an example of a stirring mechanism 60. As illustrated in Figure 3, the plating module 400 also includes a rotation mechanism 40, a tilt mechanism 45, and a lifting mechanism 50. As illustrated in Figure 3, the plating module 400 also includes sensors 130. As illustrated in Figure 4, the plating module 400 also includes a power source 80 and a plating solution flow mechanism 90.

[0026] The plating tank 10 according to this embodiment is configured as a bottomed container having an opening at the top. Specifically, the plating tank 10 has a bottom wall 10a and an outer peripheral wall 10b extending upward from the outer peripheral edge of the bottom wall 10a, and the upper part of the outer peripheral wall 10b is open. The shape of the outer peripheral wall 10b of the plating tank 10 is not particularly limited, but the outer peripheral wall 10b according to this embodiment has a cylindrical shape as an example. A plating solution Ps is stored inside the plating tank 10.

[0027] The plating solution Ps may be any solution containing ions of metal elements that constitute the plating film, and the specific example is not particularly limited. In this embodiment, a copper plating process is used as an example of a plating process, and a copper sulfate solution is used as an example of the plating solution Ps. The plating solution Ps may also contain a predetermined additive.

[0028] The plating solution Ps may contain, for example, an accelerator that accelerates plating (specifically, an accelerator that accelerates the formation of a plating film). For example, SPS (bis(3-sulfopropyl)disulfide) may be used as the accelerator.

[0029] An anode 11 is disposed inside the plating tank 10. The specific type of the anode 11 is not particularly limited, and may be an insoluble anode or a soluble anode. In the present embodiment, an insoluble anode is used as an example of the anode 11. The specific type of the insoluble anode is not particularly limited, and platinum, iridium oxide, or the like may be used.

[0030] As illustrated in Fig. 3 and Fig. 4, an ionic resistor 12 may be disposed above an anode 11 inside a plating tank 10. Specifically, as illustrated in a partially enlarged view of Fig. 4, the ionic resistor 12 is formed of a porous plate member having a plurality of holes 12a (pores). The holes 12a are provided so as to connect the lower surface and the upper surface of the ionic resistor 12 to each other.

[0031] The ionic resistor 12 is provided to homogenize the electric field formed between the anode 11 and the substrate Wf serving as the cathode. By disposing the ionic resistor 12 in the plating tank 10 as in this embodiment, it is possible to easily homogenize the thickness of the plating film (plating layer) formed on the substrate Wf.

[0032] As illustrated in Fig. 3 and Fig. 4, a membrane 16 may be disposed in the plating tank 10 at a position above the anode 11 and below the ionic resistor 12. In this case, the inside of the plating tank 10 is divided by the membrane 16 into an anode chamber 17a below the membrane 16 and a cathode chamber 17b above the membrane 16. The anode 11 is disposed in the anode chamber 17a, and the ionic resistor 12 and the substrate Wf are disposed in the cathode chamber 17b. The membrane 16 is configured to allow ionic species including metal ions contained in the plating solution Ps to pass through the membrane 16, while suppressing non-ionic plating additives contained in the plating solution Ps from passing through the membrane 16. For example, an ion exchange membrane can be used as such a membrane 16.

[0033] 4, the plating solution flow mechanism 90 is configured to flow the plating solution Ps in the plating tank 10. The plating solution flow mechanism 90 according to the present embodiment includes, for example, a first flow mechanism 91a and a second flow mechanism 91b.

[0034] The first flow mechanism 91a is a mechanism for causing the plating solution Ps in the anode chamber 17a to flow. The second flow mechanism 91b is a mechanism for causing the plating solution Ps in the cathode chamber 17b to flow. The first flow mechanism 91a is connected to the anode chamber 17a via a pipe 92a. The second flow mechanism 91b is connected to the cathode chamber 17b via a pipe 92b. Each of the first flow mechanism 91a and the second flow mechanism 91b includes a pump or the like for pressure-feeding the plating solution Ps.

[0035] 3 and 4, the plating tank 10 is provided with a supply port for supplying the plating solution Ps to the plating tank 10. Specifically, the outer peripheral wall 10b of the plating tank 10 according to this embodiment is provided with a first supply port 13a for supplying the plating solution Ps to the anode chamber 17a and a second supply port 13b for supplying the plating solution Ps to the cathode chamber 17b. The plating solution Ps discharged from the first discharge port 14a is pumped by the first flow mechanism 91a and is again supplied from the first supply port 13a to the anode chamber 17a.

[0036] The overflow tank 20 is composed of a bottomed container disposed outside the plating tank 10. The overflow tank 20 is provided to temporarily store the plating solution Ps that has exceeded the upper end of the outer peripheral wall 10b of the plating tank 10 (i.e., the plating solution Ps that has overflowed from the plating tank 10). The plating solution Ps stored in the overflow tank 20 is discharged from the second discharge port 14b, and then pressure-fed by the second flow mechanism 91b, and is again supplied to the cathode chamber 17b from the second supply port 13b.

[0037] The substrate holder 30 holds the substrate Wf as a cathode such that a surface Wfa to be plated of the substrate Wf faces the anode 11. In this embodiment, the surface Wfa to be plated of the substrate Wf is specifically provided on a surface (lower surface) facing downward of the substrate Wf.

[0038] The substrate holder 30 is connected to the rotation mechanism 40. The rotation mechanism 40 is a mechanism for rotating the substrate holder 30. "R1" illustrated in FIG. 3 is an example of a rotation direction of the substrate holder 30. A known rotation motor or the like can be used as the rotation mechanism 40. The tilt mechanism 45 is a mechanism for tilting the rotation mechanism 40 and the substrate holder 30. The lifting mechanism 50 is supported by a support shaft 51 extending in the vertical direction. The lifting mechanism 50 is a mechanism for raising and lowering the substrate holder 30, the rotation mechanism 40, and the tilt mechanism 45 in the vertical direction. A known lifting mechanism such as a linear actuator can be used as the lifting mechanism 50.

[0039] The control module 800 includes a microcomputer, which includes a processor 801, a storage device 802 as a non-transitory storage medium, etc. The control module 800 controls the operation of the plating module 400 by the processor 801 operating based on commands of a program stored in the storage device 802.

[0040] 3, the sensors 130 detect various information used for various controls of the control module 800 and transmit the detection results to the control module 800. The sensors 130 include, for example, a current sensor that detects a current value (A) between the anode 11 and the substrate Wf, and a voltage sensor that detects a voltage value (V) between the anode 11 and the substrate Wf.

[0041] The sensors 130 also include a speed sensor for detecting the moving speed (rpm or m / sec) of the paddle 70. The sensors 130 also include a rotation speed sensor for detecting the rotation speed (rpm) of the substrate holder 30. The sensors 130 also include a flow velocity sensor for detecting the flow velocity (m / sec) of the plating solution Ps in the plating tank 10. Specifically, the flow velocity sensor includes a flow velocity sensor for detecting the flow velocity of the plating solution Ps in the anode chamber 17a and a flow velocity sensor for detecting the flow velocity of the plating solution Ps in the cathode chamber 17b.

[0042] The sensors 130 also include an angle sensor for detecting the rotation angle of the substrate holder 30. The control module 800 can obtain the rotation angle (rotation position) of the substrate holder 30 by acquiring the detection result of this angle sensor, and can also obtain the rotation angle (rotation position) of the substrate Wf held by the substrate holder 30.

[0043] 4, the power supply 80 is electrically connected to the substrate Wf and the anode 11, and is configured to supply a current between the substrate Wf and the anode 11. The operation of the power supply 80 is controlled by a control module 800.

[0044] The control module 800 of this embodiment controls the power supply 80 so that, during the "plating process" in which plating is performed on the substrate Wf, a "forward current" for depositing metal from the plating solution Ps onto the substrate Wf and a "reverse current pulse", which is a current that flows in pulses in the opposite direction to the forward current, are supplied.

[0045] Fig. 5 is a schematic plan view of the paddle 70. With reference to Figs. 3, 4 and 5, the paddle 70 is disposed between the substrate Wf and the anode 11 (specifically, in the present embodiment, as an example, between the substrate Wf and the ion resistor 12). The paddle 70 is driven by a driving device 77 that receives an instruction from a control module 800. By driving the paddle 70, the plating solution Ps in the plating tank 10 is stirred.

[0046] The paddle 70 according to the present embodiment is, for example, alternately driven in a "first direction (in the present embodiment, the X direction as an example)" parallel to the substrate Wf and a "second direction (in the present embodiment, the -X direction as an example)" opposite to the first direction. That is, the paddle 70 according to the present embodiment reciprocates in the X-axis direction as an example.

[0047] 5, the paddle 70 according to the present embodiment has, as an example, a plurality of stirring members 71a extending in a direction (the direction of the Y axis) perpendicular to the first and second directions of the paddle 70. A gap is provided between adjacent stirring members 71a. One end of each of the stirring members 71a is connected to a connecting member 72a, and the other end is connected to a connecting member 72b.

[0048] However, the configuration of the paddle 70 is not limited to this, and various known paddles such as those exemplified in Patent Document 1 can be used.

[0049] The paddle 70 only needs to be disposed inside the plating tank 10 at least when the plating solution Ps is being stirred, and does not need to be disposed inside the plating tank 10 all the time. For example, when the driving of the paddle 70 is stopped and the plating solution Ps is not being stirred by the paddle 70, the paddle 70 may not be disposed inside the plating tank 10.

[0050] Note that "the moving speed of the paddle 70 is N (rpm)" specifically means that the paddle 70 makes one reciprocating motion (i.e., the paddle 70 starts from a predetermined position, moves, for example, in a first direction, then moves in a second direction, moves in the first direction again, and returns to the predetermined position) N times per minute. The faster the moving speed of the paddle 70, the stronger the stirring strength of the plating solution Ps by the paddle 70. In other words, the moving speed of the paddle 70 is an example of "the stirring strength of the plating solution Ps."

[0051] Fig. 6(A) is a schematic diagram for explaining the surface configuration of the substrate Wf. Specifically, Fig. 6(A) is a schematic cross-sectional view showing a state in which bumps 143 are formed on the substrate Wf by plating. Specifically, the bumps 143 are formed by a metal (e.g., Cu) deposited on the substrate Wf.

[0052] As illustrated in FIG. 6(A), a thin metal seed layer 140 is provided in advance on the entire surface of the substrate Wf according to this embodiment, for example. During plating, power is supplied to the surface of the substrate Wf via this seed layer 140. A photoresist layer 141 is provided on the surface of the seed layer 140 opposite the substrate Wf. The photoresist layer 141 has an opening 142 in a portion where a bump 143 is to be formed. Note that "φ" illustrated in FIG. 6(A) is the diameter (μm) of the opening 142 in the photoresist layer 141, and "BH" is the height (μm) of the bump 143.

[0053] Fig. 6(B) is a schematic diagram showing an example of an opening pattern of the photoresist layer 141. No1 and No2 in Fig. 6(B) show examples in which the diameter φ of the openings 142 is relatively small (30 μm, as an example), and No3 and No4 show examples in which the diameter φ of the openings 142 is relatively large (75 μm, as an example). Comparing No1 and No2, the openings 142 are arranged at a higher density in No1 than in No2. Comparing No3 and No4, the openings 142 are arranged at a higher density in No3 than in No4.

[0054] The substrate Wf provided with the photoresist layer 141 as described above is held by the substrate holder 30 and immersed in the plating solution Ps in the plating tank 10 to perform plating. During plating, the surface of the substrate Wf other than the openings 142 of the photoresist layer 141 is shielded from the plating solution Ps by the photoresist layer 141. As a result, a plating film grows only in the openings 142 of the photoresist layer 141, forming bumps 143 on the substrate Wf. The photoresist layer 141 may be removed after plating.

[0055] 7(A) and 7(B) are diagrams for explaining an example of a time waveform of a current output from the power supply 80 according to the present embodiment and supplied to the anode 11 and the substrate Wf. As illustrated in FIGS. 7(A) and 7(B), upon receiving an instruction from the control module 800, the power supply 80 supplies a forward current during a first period T1. The "forward direction" is the direction in which a current flows through the plating solution Ps from the anode 11 to the substrate Wf. Therefore, during the first period T1, metal ions in the plating solution Ps are reduced on the plated surface Wfa of the substrate Wf, so that a metal (bump 143) is precipitated on the plated surface Wfa, forming a plating film.

[0056] The length of the first period T1 may be a length that occupies the majority of the total time during which the plating process is performed so that the plating film is substantially grown. In other words, the sum of the lengths of the second period T2 and the third period T3 described below may be negligible compared to the length of the first period T1. The magnitude of the forward current may be, for example, a constant current value throughout the first period T1. Alternatively, the current value of the forward current may be controlled to change with time.

[0057] In a second period T2 provided in the middle of the first period T1, the power supply 80 receives an instruction from the control module 800 and supplies a current in the opposite direction to the above-mentioned forward current, i.e., a reverse current pulse. For example, the length of the second period T2, i.e., the pulse width of the reverse current pulse, may be about 0.1 seconds to several seconds. In the second period T2, contrary to the reduction reaction of metal ions in the first period T1, a part of the metal of the plating film formed on the substrate Wf in the first period T1 is redissolved in the plating solution Ps, and the accelerator (one of the additives contained in the plating solution Ps) that was attached to the outermost surface of the plating film during the reduction reaction is detached from the plating film surface. Note that the current value of the reverse current pulse is desirably set to a value that allows sufficient detachment of the accelerator.

[0058] As illustrated in Fig. 7(B), the power source 80 may stop supplying current during a third period T3 following the second period T2. That is, during the third period T3, current does not flow in either the forward or reverse direction through the plating solution Ps. As with the second period T2, the length of the third period T3 is an extremely short time compared to the first period T1, and may be, for example, about 0.1 seconds to several seconds. During the third period T3, the accelerator desorbed from the plating film surface diffuses within the plating solution Ps.

[0059] After the second period T2 or the third period T3, the power source 80 again supplies a forward current. The forward current is continued until a predetermined plating process time is completed, for example, until the thickness of the formed plating film reaches a predetermined target film thickness.

[0060] Fig. 8 is a graph showing an example of measuring the height (BH) of the bumps 143 in each pattern region when multiple bumps 143 are formed on a substrate Wf having a photoresist layer 141 as exemplified in Fig. 6(B). On the vertical axis of Fig. 8, the height (BH) of each bump 143 corresponding to each of the pattern regions P1, P2, P3, and P4 in Fig. 6(B) specifically indicates the average value of the heights of the multiple bumps 143 included in that pattern region.

[0061] The graph on the left of Figure 8 shows the measurement results when a forward current was supplied throughout the entire plating process to form bump 143, and the graph on the right of Figure 8 shows the measurement results when a reverse current pulse was supplied once during the plating process to form bump 143.

[0062] 8, among all the pattern regions, the height (BH) of the bump 143 in the pattern region P1 is the smallest, and the height (BH) of the bump 143 in the pattern region P4 is the largest. This is because the smaller the diameter φ of the opening 142 and the higher the arrangement density of the openings 142, the more difficult it becomes to sufficiently replenish metal ions into the openings 142, resulting in a lower formation rate of the plating film. Here, the difference between the maximum and minimum values ​​of the height (BH) of the bump 143 is defined as the "bump height variation (ΔBH)."

[0063] 8, it can be seen that when a reverse current pulse is supplied during plating (graph on the right side of FIG. 8), the bump height variation (ΔBH) is smaller than when a reverse current pulse is not supplied (graph on the left side of FIG. 8). In this way, by supplying a reverse current pulse, the height of the bumps 143 can be made uniform.

[0064] Fig. 10 is a schematic plan view for explaining an "opening density change direction (Dr2)" which is a direction in which the opening density of a photoresist layer 141 provided on a substrate Wf changes. As an example, in Fig. 10, the openings 142 of the photoresist layer 141 include a "region Ar1 (i.e., a region where the opening density is "sparse")" where the opening density is lower than a predetermined value, and a "region Ar2 (i.e., a region where the opening density is "dense")" where the opening density is higher than the opening density of the region Ar1. In this case, the opening density change direction (Dr2) is the direction from the region Ar1 toward the region Ar2 (or the direction from the region Ar2 toward the region Ar1).

[0065] Here, the inventor's research has revealed that when a reverse current pulse is supplied, the degree of uniformity of the height of the bumps 143 changes depending on the angle (α1) between the "opening density change direction (Dr2)" and the flow direction (Dr1) of the plating solution Ps during stirring (for details, see the description of the experimental results explained in FIG. 11 described later). Therefore, in this embodiment, in order to effectively uniform the height of the bumps 143, a plating method described in FIG. 9 below is executed.

[0066] 9 is an example of a flowchart for explaining the plating method according to the present embodiment. First, a user (operator) obtains an "opening density change direction (Dr2)" which is a direction in which the opening density of a photoresist layer 141 provided on a substrate Wf changes (step S10).

[0067] Note that, when obtaining the opening density change direction (Dr2), for example, if information regarding the opening density is described in a specification or the like for the substrate Wf, the user may obtain the opening density change direction (Dr2) based on the specification, etc. Alternatively, the user may obtain (i.e., measure) the opening density change direction (Dr2) by observing the substrate Wf visually or using a microscope, etc.

[0068] After step S10, the user or the control module 800 causes the substrate holder 30 to hold the substrate Wf for which the opening density change direction (Dr2) has been acquired (step S20).

[0069] The substrate Wf is held by the substrate holder 30 so that, for example, an orientation flat provided on the substrate Wf faces a predetermined direction of the substrate holder 30. That is, the substrate Wf is held by the substrate holder 30 in such a manner that the orientation of the substrate Wf (the direction of the orientation flat) can be grasped. Therefore, when the substrate Wf is held by the substrate holder 30, the control module 800 can grasp in which direction the opening density change direction (Dr2) of the substrate Wf faces.

[0070] Next, the control module 800 immerses the substrate Wf held by the substrate holder 30 in the plating solution Ps in the plating tank 10 so as to face the anode 11 (step S30).

[0071] Next, the control module 800 executes a first plating process (step S40). Specifically, in step S40, the control module 800 causes the stirring mechanism 60 (e.g., the paddle 70) to stir the plating solution Ps and the rotation mechanism 40 to rotate the substrate holder 30, while causing the power source 80 to supply a forward current for a predetermined time. As a result, a plating film (specifically, bumps 143) is formed on the substrate Wf.

[0072] Next, the control module 800 executes the second plating process (step S50). Specifically, in step S50, the control module 800 stops the rotation of the substrate holder 30 in a state where the opening density change direction (Dr2) is non-parallel to the flow direction (Dr1) of the plating solution Ps stirred by the stirring mechanism 60, and causes the power source 80 to supply a reverse current pulse while stirring the plating solution Ps by the stirring mechanism 60.

[0073] In addition, the "direction of opening density change (Dr2)" being non-parallel to the "direction of flow of plating solution Ps (Dr1)" means, in other words, that the "direction of opening density change (Dr2)" is neither the same direction as the "direction of flow of plating solution Ps (Dr1)" nor the opposite direction.

[0074] Specifically, referring to FIG. 10, the control module 800 according to this embodiment stops the rotation of the substrate holder 30 at an angle such that the angle (α1) between the opening density change direction (Dr2) and the flow direction (Dr1) of the plating solution Ps is greater than 0 degrees and less than 180 degrees.

[0075] 10, as an example, the rotation of the substrate holder 30 is stopped so that the opening density change direction (Dr2) and the flow direction (Dr1) of the plating solution Ps are perpendicular (α1 is 90 degrees). With the rotation of the substrate holder 30 stopped in this manner, the control module 800 causes the stirring mechanism 60 to stir the plating solution Ps while causing the power source 80 to supply a reverse current pulse.

[0076] In this embodiment, the "flow direction (Dr1) of the plating solution Ps stirred by the stirring mechanism 60" specifically coincides with the "direction (Dr1) in which the paddle 70 reciprocates." Therefore, the "direction (Dr1) in which the paddle 70 reciprocates" may be used as the "direction (Dr1) of the plating solution Ps stirred by the stirring mechanism 60."

[0077] That is, in this case, in step S50, the control module 800 stops the rotation of the substrate holder 30 in a state in which the opening density change direction (Dr2) is non-parallel to the direction (Dr1) in which the paddle 70 moves back and forth, and then causes the stirring mechanism 60 to stir the plating solution Ps while supplying a reverse current pulse to the power supply 80.

[0078] Referring to FIG. 9, after step S50, the control module 800 executes the first plating process again (step S60).

[0079] The control module 800 may repeatedly execute steps S40, S50, and S60 in FIG. 9 a number of times.

[0080] 11(A) and 11(B) are diagrams for explaining how the degree of uniformity of the height of the bumps 143 changes depending on the angle (α1) between the opening density change direction (Dr2) and the flow direction (Dr1) of the plating solution Ps during stirring. The vertical axis of FIG. 11(A) and FIG. 11(B) indicates the within-die uniformity (the difference between the maximum and minimum heights of the bumps 143).

[0081] 11A shows the results of an experiment using a substrate Wf with a relatively large degree of variation in the aperture ratio of the bumps 143 (substrate Wf with an 8-fold difference in the aperture ratio within the die), and FIG 11B shows the results of an experiment using a substrate Wf with a relatively small degree of variation in the aperture ratio of the bumps 143 (substrate Wf with a 3-fold difference in the aperture ratio within the die).

[0082] Sample No. 1 in FIG. 11(A) is an experimental result when only the first plating process was performed (i.e., when only a forward current was supplied). Sample No. 2 is an experimental result when the plating method according to this embodiment (FIG. 9) was performed. Specifically, in Sample No. 2, an angle (α1) of 90 degrees was used in the second plating process in step S50. Sample No. 3 is an experimental result when steps S10 to S60 of the flowchart in FIG. 9 were performed, but an angle (α1) of zero degrees (or 180 degrees) was used in the second plating process in step S50. That is, Sample No. 2 is an example, and Sample No. 1 and Sample No. 3 are comparative examples.

[0083] As can be seen by comparing Sample No. 1 with Sample No. 2 and Sample No. 3, it is possible to lower the intra-die uniformity value by supplying a reverse current pulse during plating (i.e., it is possible to make the heights of the bumps 143 uniform). Also, as can be seen by comparing Sample No. 2 with Sample No. 3, it is possible to change the intra-die uniformity value depending on the value of the angle (α1) when the second plating process is performed.

[0084] As can be seen by comparing sample No. 2 and sample No. 3, sample No. 2 has a lower intra-die uniformity value than sample No. 3. This shows that, as in sample No. 2, stopping the rotation of substrate holder 30 in a state in which the opening density change direction (Dr2) is non-parallel to the flow direction (Dr1) of plating solution Ps during stirring can reduce the intra-die uniformity value, compared to stopping the rotation of substrate holder 30 in a state in which the opening density change direction (Dr2) is parallel to the flow direction (Dr1) of plating solution Ps during stirring, as in sample No. 3.

[0085] This is thought to be because, during the second plating process, when the direction of change in opening density (Dr2) is non-parallel to the direction of flow of the plating solution Ps during stirring (Dr1), the plating solution Ps present on the surface of the substrate Wf (i.e., the surface of the plating film) can be stirred more uniformly over the entire surface of the substrate Wf than when the direction is not parallel to the direction of flow of the plating solution Ps during stirring. This allows the accelerator to be removed from the surface of the plating film uniformly and effectively, resulting in a smaller within-die uniformity value.

[0086] Sample No. 4 in FIG. 11(B) is an experimental result when only the first plating process was performed (i.e., when only a forward current was supplied). Sample No. 5 is an experimental result when the plating method according to this embodiment (FIG. 9) was performed. Specifically, in sample No. 5, an angle (α1) of 90 degrees was used in the second plating process in step S50. Sample No. 6 is an experimental result when steps S10 to S60 of the flowchart in FIG. 9 were performed, but an angle (α1) of zero degrees (or 180 degrees) was used in the second plating process in step S50. That is, sample No. 5 is an embodiment, and samples No. 4 and No. 6 are comparative examples.

[0087] As can be seen by comparing Sample No. 4 with Sample No. 5 and Sample No. 6, it is possible to reduce the within-die uniformity value by supplying a reverse current pulse during plating. Also, as can be seen by comparing Sample No. 5 with Sample No. 6, it is possible to change the within-die uniformity value depending on the value of the angle (α1) during the second plating process.

[0088] Furthermore, as can be seen by comparing sample No. 5 and sample No. 6, it can be seen that stopping the rotation of the substrate holder 30 during the second plating process when the direction of opening density change (Dr2) is non-parallel to the direction of flow of the plating solution Ps during stirring (Dr1), as in sample No. 5, can reduce the within-die uniformity value compared to stopping the rotation of the substrate holder 30 when the direction of opening density change (Dr2) is parallel to the direction of flow of the plating solution Ps during stirring (Dr1), as in sample No. 6.

[0089] As described above, it can be seen that the in-die uniformity, that is, the degree of uniformity of the heights of the bumps 143, changes depending on the value of the angle (α1) when the second plating process is performed.

[0090] In this embodiment, the angle (α1) when the second plating process is performed is 90 degrees, but is not limited to this. The angle (α1) is not particularly limited as long as it is greater than 0 degrees and less than 180 degrees. The angle (α1) can be determined in advance by experimentation to find a value that will best achieve uniformity in the height of the bumps 143, and the determined value can be set as the angle (α1).

[0091] When the relationship between the angle (α1) and the uniformity of the height of the bumps 143 was investigated, it was found that the closer the angle (α1) is to 90 degrees, the more uniform the height of the bumps 143 tends to be. Therefore, from the viewpoint of uniformity of the height of the bumps 143, the angle (α1) is preferably a value selected from the range of 40 degrees or more and 135 degrees or less, more preferably a value selected from the range of 80 degrees or more and 100 degrees or less, and even more preferably 90 degrees.

[0092] According to the present embodiment as described above, the height of the bumps 143 can be made uniform.

[0093] Although the embodiments and modifications of the present invention have been described in detail above, the present invention is not limited to such specific embodiments and modifications, and various further modifications and alterations are possible within the scope of the present invention described in the claims. [Explanation of symbols]

[0094] 10 Plating tank 11 Anode 30 Substrate holder 60 Mixing mechanism 70 Paddle 80 power supply 141 Photoresist layer 142 Aperture Ps plating solution Wf substrate Dr1 Flow direction of plating solution stirred by the stirring mechanism Dr2 Opening density change direction

Claims

1. acquiring an opening density change direction, which is a direction in which the opening density of a photoresist layer provided on a substrate changes; holding the substrate, for which the aperture density change direction has been acquired, on a substrate holder; A plating solution containing an accelerator for accelerating plating is stored in a plating tank in which an anode is disposed, and the substrate held by the substrate holder is immersed in the plating solution so as to face the anode; performing a first plating process by rotating the substrate holder and stirring the plating solution with a stirring mechanism, and causing a power source configured to supply a current between the substrate and the anode to supply a forward current for depositing metal from the plating solution onto the substrate; a second plating process is performed in which the rotation of the substrate holder is stopped in a state in which the opening density change direction is non-parallel to the flow direction of the plating solution stirred by the stirring mechanism, and a reverse current pulse, which is a current flowing in a pulsed manner in a direction opposite to the forward current, is supplied to the power source while stirring the plating solution by the stirring mechanism; and performing the first plating process again.

2. 2. The plating method according to claim 1, wherein in the second plating process, the direction of change in the opening density is perpendicular to a direction of flow of the plating solution stirred by the stirring mechanism.

3. the stirring mechanism includes a paddle configured to stir the plating solution in the plating tank by reciprocating; 2. The plating method according to claim 1, wherein a direction in which the paddle reciprocates is used as a flow direction of the plating solution stirred by the stirring mechanism in the second plating process.

Citation Information

Patent Citations

  • Plating apparatus

    JP2011026708A

  • Plating apparatus and plating method

    JP7357824B1

  • Plating method for micropore, method for forming gold bump using the same, method for producing semiconductor device, and semiconductor device

    JP2006131926A

  • Plating method and plating apparatus

    JP7079388B1

  • JPP7357824B

Cited By

  • Plating apparatus and plating method

    JP7718005B1

  • Plating device and plating method

    WO2026126339A1