Annealing method for hot rolled steel strip
By using a continuous annealing furnace with a rapid heating device to adjust heating temperature based on LSD, the method addresses the challenge of controlling hot-rolled steel strip annealing precision, improving magnetic properties and reducing defects.
Patent Information
- Application Number
- JP2023513752
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-10-27
- Filing Date
- 2022-10-18
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-10-18
AI Technical Summary
Existing annealing methods for hot-rolled steel strips used in electrical steel sheets struggle to control the heating temperature with high precision due to fluctuations in thickness and threading speed, leading to inconsistent magnetic properties and defects.
Implementing a continuous annealing furnace with a heating zone, soaking zone, and cooling zone, and installing a rapid heating device upstream, adjusting the heating temperature based on the LSD (thickness x threading speed) to maintain precise control over the steel strip temperature, using methods like induction heating or electrical heating.
Achieves high-precision temperature control of the steel strip, reducing defects and enhancing magnetic properties by uniformly heating the strip to a target temperature despite thickness and speed variations.
Smart Images

Figure 0007558476000003 
Figure 0007558476000004 
Figure 0007558476000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for annealing a hot-rolled steel strip (hot-rolled steel strip) used in the manufacture of electrical steel sheets. [Background technology]
[0002] It is known that annealing (hot-rolled sheet annealing) of a hot-rolled steel strip for electrical steel sheet containing 1.6 to 5.0 mass% Si before cold rolling improves the magnetic properties of the product sheet, that is, the Goss orientation can be highly developed. The above-mentioned hot-rolled sheet annealing is usually performed using a continuous annealing facility equipped with a heating zone, a soaking zone, and a cooling zone.
[0003] It is known that the annealing temperature in hot-rolled steel strip annealing has a large effect on the magnetic properties of the product steel strip, and it is necessary to control the steel strip temperature to be constant and uniform over the entire length and width of the hot-rolled steel strip. Therefore, in the above-mentioned continuous annealing equipment, the furnace temperature of the soaking zone is controlled to be constant in order to control the heating temperature of the hot-rolled steel strip to be annealed within a suitable range.
[0004] However, in the above-mentioned annealing method in which only the furnace temperature of the conventional soaking zone is controlled, it is difficult to suppress the fluctuation of the heating temperature of the steel strip due to the fluctuation of the thickness in the longitudinal direction of the steel strip and the fluctuation of the sheet passing speed, and to control it within a suitable range. The reason is that the hot-rolled steel strip is thick because it is before cold rolling, and has a large heat capacity per unit length (amount of heat required to raise the temperature of an object by 1°C), so it requires a larger amount of heat for heating than the cold-rolled steel strip. In addition, since the hot-rolled steel strip is thick, the thickness fluctuation is large compared to the rolled thickness, especially at the leading end of the steel strip, so that the heat capacity varies greatly even within the same steel strip. Therefore, the hot-rolled steel strip has a large effect on the furnace temperature of the annealing furnace compared to the cold-rolled steel strip, and it is difficult to maintain the furnace temperature of the heating zone and the soaking zone at a specified temperature and heat the hot-rolled steel strip to a specified soaking temperature.
[0005] However, there are few techniques disclosed for controlling the heating temperature in hot-rolled sheet annealing with high precision.For example, Patent Document 1 discloses a technique for reducing the aging index of a steel sheet before final cold rolling in the manufacture of grain-oriented electrical steel sheets by controlling the cooling rate in hot-rolled sheet annealing. Furthermore, Patent Document 2 discloses a hot-rolled sheet annealing technique for a Si-containing steel sheet, in which a steel strip is rapidly heated during hot-rolled sheet annealing. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2016-000856 A [Patent Document 2] JP 2018-066040 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, although the technology disclosed in the above Patent Document 1 discloses improving the hot-rolled sheet structure of grain-oriented electrical steel sheet by performing hot-rolled sheet annealing, it makes no mention of the need to control the heating temperature of hot-rolled sheet annealing with high precision or of the means for achieving this. Furthermore, the technology disclosed in Patent Document 2 describes rapid heating in hot-rolled sheet annealing as a means for improving descaling properties after annealing, but makes no mention of increasing the precision of the heating temperature after rapid heating.
[0008] As described above, in the manufacture of electrical steel sheets, highly accurate control of the heating temperature of hot-rolled sheet annealing is extremely important from the viewpoint of improving magnetic properties. However, hot-rolled steel strips are characterized by a large thickness, poor thickness accuracy, and large thickness variation, which causes fluctuations in the furnace temperature of the annealing furnace, and therefore there is a limit to the highly accurate control of the heating temperature of the steel strip.
[0009] The present invention aims to solve the above-mentioned problems of the conventional technology and to provide a method for annealing a hot-rolled steel strip that can control the steel strip temperature at the exit of the heating zone and therefore the steel strip temperature at the exit of the soaking furnace with high precision in hot-rolled sheet annealing. Here, the temperature of the steel strip at the exit side of the heating zone refers to the temperature of the steel strip at the exit of the heating zone. [Means for solving the problem]
[0010] As a result of intensive research by the inventors to solve the above problems, they discovered that in order to control the heating temperature with high precision in hot-rolled strip annealing, a thickness gauge and a rapid heating device are provided upstream of the soaking zone in a continuous annealing furnace having a heating zone, a soaking zone, and a cooling zone, and that it is effective to change the heating temperature of the steel strip in the rapid heating device according to the fluctuation of the LSD (strip thickness x strip running speed) of the steel strip, which led to the development of the present invention.
[0011] That is, the method for annealing a hot-rolled steel strip for electrical steel sheet according to the present invention is configured as follows. [1] In a method for annealing a hot-rolled steel strip for electrical steel sheet containing 1.6 to 5.0 mass% Si using annealing equipment having a heating zone, a soaking zone, and a cooling zone arranged in this order from the upstream side, a thickness gauge and a rapid heating device are arranged upstream of the soaking zone, and the heating temperature of the steel strip by the rapid heating device is determined from the LSD value defined by the following formula (1) based on the thickness of the steel strip measured by the thickness gauge and the passing speed of the steel strip during annealing. Note LSD = t × LS (1) Here, t is the thickness of the steel strip (mm) and LS is the threading speed of the steel strip (m / min). [2] In the above [1], the heating temperature of the steel strip by the rapid heating device can be determined from at least one of the following information in addition to the LSD: the width of the steel strip, the furnace temperature of the heating zone after the rapid heating device, the steel strip temperature at the exit of the heating zone, the furnace temperature in the soaking zone, and the steel strip temperature at the exit of the soaking zone. [3] In the above [1] or [2], the rapid heating device can be installed upstream of the heating zone or in the front or middle stage within the heating zone. [4] In any of the above [1] to [3], the heating temperature of the steel strip by the rapid heating device can be determined by feeding back the furnace temperature of the heating zone subsequent to the rapid heating device. [5] In any of the above [1] to [4], the heating temperature of the steel strip by the rapid heating device can be determined so that the temperature of the steel strip at the exit side of the heating zone is constant. [6] In any one of the above [1] to [5], the heating means of the rapid heating device may be one or more of induction heating, electric current heating, and infrared heating. Effect of the Invention
[0012] According to the present invention, the heating temperature of the steel strip by the rapid heating device is set higher as the LSD value, defined as the steel strip thickness x the threading speed, is larger, and set lower as the LSD is smaller, so that the steel strip temperature on the exit side of the heating zone, and in turn the steel strip temperature on the exit side of the soaking zone, can be controlled to a predetermined target temperature with high precision. As a result, the magnetic properties of the product strip are improved, which greatly contributes to reducing the occurrence of defects. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a schematic diagram showing an example of a hot-rolled sheet annealing facility used in an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing an example of hot-rolled sheet annealing equipment used in another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The present invention will now be described with reference to the drawings. 1 is a schematic diagram showing the first half of a continuous annealing facility used for annealing hot-rolled steel strips for electrical steel sheets (hot-rolled sheet annealing), which has a heating zone, a soaking zone, and a cooling zone arranged from the upstream side, and the hot-rolled sheet annealing is usually performed by heating the steel strip S in the heating zone 3 so that the steel strip temperature at the outlet side of the heating zone reaches a target soaking temperature, then holding the steel strip S at the soaking temperature in the soaking zone 4 for a predetermined time, and then cooling the steel strip S in a cooling zone (not shown). At this time, the furnace temperatures of the heating zone 3 and the soaking zone 4 and the passing speed of the steel strip S are held under certain conditions from the viewpoint of holding the steel strip at the predetermined soaking temperature for a predetermined time.
[0015] However, there is a certain amount of thickness variation in the steel strip, especially at the leading and trailing ends. In addition, the threading speed may be changed suddenly during annealing of the steel strip. When such a large thickness variation or a sudden change in the threading speed occurs, the heating temperature of the steel strip cannot be heated to the target temperature by simply controlling the furnace temperature of the heating zone and the soaking zone to be constant, so the set temperature of the furnace must be changed. However, a sudden change in the set temperature of the furnace causes overshooting and hunting of not only the furnace temperature but also the steel strip temperature. In addition, it takes time for the furnace temperature to change, and an instantaneous change in the furnace temperature cannot be expected. Therefore, it is desirable to keep the furnace temperature of the annealing furnace 1 as constant as possible, or to change it gradually.
[0016] Furthermore, as described above, a hot-rolled steel strip is thicker and has a larger heat capacity than a cold-rolled steel strip, so that it is difficult to follow the change in furnace temperature of the heating zone and also affects the furnace temperature of heating zone 3, making it difficult to heat the steel strip to a target temperature. Therefore, in heating zone 3, it is desired to heat the steel strip so that the temperature of the steel strip on the exit side of the heating zone always becomes a predetermined target temperature regardless of the fluctuation in the thickness of the steel strip and the threading speed.
[0017] Furthermore, the ultimate objective of hot-rolled steel strip annealing is to perform heat treatment in the soaking zone 4 by holding the steel strip S at a target soaking temperature for a predetermined time, but in the case of a hot-rolled steel strip which is thicker than a cold-rolled steel strip, if the steel strip temperature on the exit side of the heating zone is different, the heat amount of the steel strip also differs, so the amount of heat brought into the soaking zone 4 changes, and ultimately the furnace temperature also changes, making it difficult to heat the hot-rolled steel strip to the target soaking temperature. In this sense, too, it is preferable to set the steel strip temperature on the exit side of the rapid heating device 2 so that the steel strip temperature on the exit side of the heating zone 3 is constant.
[0018] In the present invention, when hot-rolled steel strip for electrical steel sheet is annealed using the continuous annealing equipment shown in Fig. 1, a thickness gauge 5 and a rapid heating device 2 are arranged upstream of the heating zone 3, and the heating temperature of the steel strip S by the rapid heating device 2 is changed according to the value of LSD defined by the following formula (1) based on the thickness of the steel strip measured by the thickness gauge 5 and the passing speed of the steel strip during annealing, thereby heating the steel strip temperature on the exit side of the heating zone to a predetermined target temperature. The LSD is an index proportional to the heat capacity of the steel strip. LSD = t × LS (1) Here, t is the thickness of the steel strip (mm) and LS is the threading speed of the steel strip (m / min).
[0019] In the present invention, the larger the LSD value of the hot rolled steel strip, the higher the heating temperature of the steel strip by the rapid heating device 2 is set, and conversely, the smaller the LSD value of the hot rolled steel strip, the lower the heating temperature by the rapid heating device 2 is set. More specifically, the thicker the steel strip is, including minute thickness variations of the steel strip, the higher the steel strip temperature at the exit side of the rapid heating device, i.e., the heating temperature by the rapid heating device 2, is set than the conventional heating temperature that does not take LSD into consideration, and conversely, the thinner the strip is, the lower the steel strip temperature at the exit side of the rapid heating device, i.e., the heating temperature by the rapid heating device 2, is set than the conventional heating temperature that does not take LSD into consideration. Similarly, when the line speed increases, the steel strip temperature at the exit of the rapid heating device, i.e., the heating temperature by the rapid heating device 2, is set higher than the conventional heating temperature that does not take LSD into account, and conversely, when the line speed decreases, the steel strip temperature at the exit of the rapid heating device 2, i.e., the heating temperature by the rapid heating device 2, is set lower than the conventional heating temperature that does not take LSD into account, and heating is performed.
[0020] By taking the LSD value into consideration in this manner, even if the thickness t or the strip passing speed LS of the hot rolled strip S suddenly changes, it is possible to suppress fluctuations in the strip temperature at the exit side of the heating zone without changing the furnace temperature setting of the heating zone 3, and ultimately to suppress furnace temperature fluctuations in the soaking zone, thereby making it possible to control the temperature of the hot rolled strip to the target soaking temperature with high precision.
[0021] Any type of rapid heating device 2 may be used as long as it can heat and change the temperature of the steel strip with good responsiveness. Any method of heating the steel strip, such as induction heating (solenoid type or transverse type), electric current heating, or near-infrared heating, which have a long track record, can be suitably used.
[0022] The rapid heating device 2 is installed upstream of the soaking zone because its purpose is to control the steel strip temperature at the exit of the heating zone, and therefore the steel strip temperature at the exit of the soaking furnace, with high accuracy. It may be installed upstream of the heating zone as shown in Figure 1, or it may be installed inside the heating zone 3 (including the case where it is located between the divided heating zones 3) as shown in Figure 2. However, when an induction heating device, particularly a solenoid type device, is used as the rapid heating device 2, it is difficult to heat to a temperature higher than the Curie point, so it is preferable to install it in the front or middle section when the heating zone is divided into three sections from the upstream to the front, middle and rear sections, avoiding the rear section.
[0023] Furthermore, the greater the heating capacity of the rapid heating device 2, the more preferable it is to accommodate large thicknesses of hot-rolled steel strips and fluctuations in the strip passing speed. As a guideline, although it depends on the temperature range (position) where the rapid heating device is installed and the "temperature-specific heat" relationship of the steel strip, if it is desired to change the heating temperature of a steel strip with a thickness of about 2 mm at the exit side of the heating zone by about ±20°C, a heating capacity (amount of temperature rise) of the rapid heating device 2 of about 50 to 100°C will be sufficient to suppress the variation.
[0024] As explained above, changing the setting of the heating temperature of the steel strip by the rapid heating device 2 according to the fluctuation of the LSD value, i.e., (strip thickness x strip passing speed), can contribute sufficiently to improving the accuracy of the heating temperature of the steel strip. However, in order to control the steel strip temperature at the exit side of the heating zone 3 with even higher accuracy, it is preferable to consider the width of the hot-rolled steel strip S in addition to the above-mentioned LSD value. This is because the heat capacity of the steel strip changes in proportion to the width of the steel strip, so that the amount of heat required to heat the steel strip and the amount of heat removed from the furnace body also change, which in turn affects the steel strip temperature at the exit side of the heating zone and the furnace temperatures of the heating zone and soaking zone. In particular, when using an annealing facility having a heating zone or soaking zone with a small heat capacity of the furnace body and a furnace temperature that is easily changed, it is preferable to set the heating temperature of the rapid heating device taking into account the width of the steel strip.
[0025] Furthermore, in order to control the steel strip temperature on the exit side of the heating zone with greater precision, it is preferable to take into account furnace temperature information of the heating zone subsequent to the rapid heating device when setting the heating temperature of the rapid heating device 2. For example, if the heating capacity of the rapid heating device 2 is small and a large change in the heat capacity of the steel strip occurs due to a change in the thickness or threading speed of the hot rolled steel strip or a change in the LSD, it may not be possible for the rapid heating device alone to handle the change, so it may be possible to deliberately change the furnace temperature setting of the heating zone. Therefore, by feeding back the constantly changing furnace temperature information from the rapid heating device 2 onwards and reflecting it in the setting of the heating temperature of the rapid heating device 2, it is possible to control the steel strip temperature at the exit of the heating zone 3 with greater precision.
[0026] When the furnace temperature information is fed back, the increase in the steel strip temperature at the exit side of the heating zone can be calculated using the following formula (2). TIFF0007558476000001.tif20166 Where, ΔT: temperature rise [℃] σ: Stefan-Boltzmann constant (4.88×10 -8 [kcal / m 2 h K 4 ]) φ CG : Overall heat absorption rate L: Heating length [m] C p :Specific heat [kcal / kg℃] ρ: Density 7850[kg / m 3 ] V: Line speed [m / min] t: Plate thickness [mm] T f :Furnace temperature [℃] T s :Inlet steel plate temperature [℃] By using the above formula (2), the furnace temperature T f Considering the fluctuation of the inlet steel plate temperature T s In other words, by adjusting the heating temperature of the steel sheet in the rapid heating device, it is possible to adjust the temperature rise ΔT and control the steel strip temperature at the inlet side of the soaking zone. CG is an index showing the efficiency of heat flow throughout the furnace, and is determined based on the furnace temperature and strip temperature records.
[0027] In order to control the steel strip temperature at the exit of the heating zone with even greater accuracy, it is preferable to use information on the steel strip temperature at the exit of the heating zone, the furnace temperature in the soaking zone, and the steel strip temperature at the exit of the soaking zone in addition to the above-mentioned LSD, steel strip width, and furnace temperature of the heating zone after the rapid heating device, in determining the heating temperature of the steel strip in the rapid heating device 2.
[0028] Here, the hot-rolled steel strip for electrical steel sheet that is the subject of the present invention contains Si in the range of 1.6 to 5.0 mass%. Since Si is an effective element for increasing the resistivity of steel and reducing iron loss, it is preferable to contain 1.6 mass% or more. However, if the Si content exceeds 5.0 mass%, not only does the magnetic flux density decrease, but the steel becomes embrittled, cracks are generated during cold rolling, and the manufacturability is greatly reduced. The preferred range is 2.0 to 3.8 mass%.
[0029] In addition to Si, the hot-rolled steel strip may further contain known inhibitor-forming components for inducing secondary recrystallization, or may contain known additive elements for improving magnetic properties and mechanical properties.
[0030] According to the hot-rolled sheet annealing of the present invention described above, heat treatment can be performed uniformly and at an appropriate temperature over the entire length of the hot-rolled steel strip in the longitudinal direction (rolling direction), so that the final product sheet can be given excellent magnetic properties without secondary recrystallization defects or crystal orientation defects over the entire length of the coil in the longitudinal direction. EXAMPLES
[0031] A hot-rolled steel strip having a thickness of 1.4 to 2.8 mm and a width of 1200 mm was subjected to hot-rolled sheet annealing under the conditions shown in Table 1, with a target soaking temperature of 1050°C, using an annealing furnace 1 having a rapid heating device 2, heating zone 3, and soaking zone 4 as shown in Fig. 1. During this process, the threading speed of the steel strip was changed at points 1 / 3 and 2 / 3 of the way along the length of the hot-rolled steel strip, and the steel strip temperature at the exit side of the heating zone 3 and the steel strip temperature at the exit side of the soaking zone 4 were measured. The rapid heating device 2 is a solenoid type induction heating device, and the change in the heating temperature of the steel strip by the rapid heating device is calculated by multiplying the difference between the set thickness (rolling set thickness) of the hot rolled steel strip and the threading speed (LSDs) and the steel strip thickness actually measured by a thickness gauge 5 installed upstream of the rapid heating device and the threading speed (LSDt) by a proportionality coefficient K. The value of K is not a fixed value, but a value that changes depending on the heating characteristics such as the thickness and specific heat of the steel strip, the installation position of the rapid heating device, the furnace temperature and heating length of the annealing furnace, etc., and the K value used in this embodiment is shown in Table 1. In addition, for some hot-rolled steel strips, the effect of the furnace temperature FT of the heating zone after the rapid heating device was calculated from the above-mentioned formula (2), and this was taken into consideration when setting the heating temperature on the outlet side of the rapid heating device. The furnace temperature of the annealing furnace 1 (the heating zone 3 or the soaking zone 4) was adjusted to a range of 800 to 1100°C.
[0032] [Table 1]
[0033] The heating accuracy of each of the above annealing conditions was evaluated by dividing the hot rolled steel strip into 20 sections in the longitudinal direction, calculating the difference between the average steel strip temperature in each section and the target soaking temperature (1050°C), and evaluating the maximum value among them. The weight of the hot rolled steel strip (coil) used in this example was about 20 tons, and the difference between the set thickness (rolling set thickness) of the hot rolled steel strip and the actually measured thickness was a maximum of 200 μm at the front and rear ends of the hot rolled steel strip, and a maximum of about 50 μm at the middle part.
[0034] The above results are shown in Table 1. In Table 1, the line speed for the first 1 / 3 of the length of the hot rolled steel strip is indicated as line speed 1, the LSD is indicated as LSD1, the line speed for the next 1 / 3 is indicated as line speed 2, the LSD is indicated as LSD2, and the line speed for the last 1 / 3 is indicated as line speed 3, the LSD is indicated as LSD3.
[0035] As can be seen from Table 1 above, in the comparative examples of the conventional technology that do not use a rapid heating device (Test Nos. 18-22, 27), the steel strip temperature at the exit of the heating zone and the soaking zone varies greatly due to the influence of fluctuations in the plate thickness and the plate threading speed. Even when a rapid heating device is used (Test Nos. 23-26, 28), the steel strip temperature at the exit of the heating zone and the soaking zone varies greatly under conditions where the heating temperature of the rapid heating device is constant without taking into account the influence of LSDt. In contrast, in the examples of the present invention (Tests No. 1 to 16) in which the steel strip heating temperature at the exit of the rapid heating device was changed in accordance with the fluctuations in LSDt obtained from the actual measured plate thickness, it was found that the variation in the steel strip temperature at the exit of the heating zone and the exit of the soaking zone could be reduced to a small value even if there were fluctuations in the plate thickness or the plate passing speed. In particular, in an example of the invention (Test No. 17) in which the influence of the furnace temperature FT downstream of the heating zone was taken into account when setting the steel strip heating temperature at the exit of the rapid heating device, it was found that the difference between the steel strip temperatures at the exit of the heating zone and the exit of the soaking zone and the target heating temperature could be further reduced. The derivation of FT is as follows. (Target annealing strip temperature) - (sum of ΔT1+ΔT2+ΔT3...ΔTn in each section of the annealing furnace) - (K*(LSDt-LSDs)+250) = FT By solving the above equation, which changes from moment to moment, and fine-tuning FT (the temperature at the exit of the rapid heating device), it was possible to approach the target strip temperature. In the above embodiment, the thickness and width of the steel strip, the threading speed, the annealing temperature, etc. were set under certain specific conditions, but the present invention is also effective and applicable under other conditions. [Industrial Applicability]
[0036] The technology of the present invention is a technology that aims to minimize variation in the quality of product sheets by suppressing fluctuations in the steel strip temperature at the exit of the heating zone and controlling the annealing temperature (soaking temperature) of the steel strip to a predetermined temperature with high precision, and can be applied not only to hot-rolled steel strips for electrical steel sheets, but also to all metal strips that require control of the annealing temperature. [Explanation of symbols]
[0037] S: Steel strip 1: Annealing furnace 2: Rapid heating device 3: Heating zone 4:Solid temperature 5: Plate thickness gauge
Claims
1. A method for annealing a hot-rolled steel strip for electrical steel sheet containing 1.6 to 5.0 mass% Si using annealing equipment having a heating zone, a soaking zone, and a cooling zone arranged in this order from the upstream side, the method comprising: arranging a thickness gauge and a rapid heating device on the upstream side of the heating zone or in a front or middle section within the heating zone; and determining the steel strip temperature at the outlet side of the rapid heating device by the rapid heating device based on the LSD value defined by the following formula (1) based on the thickness of the steel strip measured by the thickness gauge and the passing speed of the steel strip during annealing, so that the steel strip temperature at the outlet side of the heating zone and the steel strip temperature at the outlet side of the soaking zone become target temperatures: Note LSD=t×LS...(1) Here, t is the thickness of the steel strip (mm), and LS is the threading speed of the steel strip (m / min).
2. 2. The method for annealing a hot-rolled steel strip according to claim 1, characterized in that the heating temperature of the steel strip by the rapid heating device is determined from at least one of the following information in addition to the LSD: the width of the steel strip, the furnace temperature of the heating zone subsequent to the rapid heating device, the steel strip temperature at the exit of the heating zone, the furnace temperature in the soaking zone, and the steel strip temperature at the exit of the soaking zone.
3. 2. The method for annealing a hot-rolled steel strip according to claim 1, wherein the heating temperature of the steel strip by the rapid heating device is determined by feeding back the furnace temperature of the heating zone subsequent to the rapid heating device.
4. A method for annealing a hot-rolled steel strip as described in claim 2, characterized in that the heating temperature of the steel strip by the rapid heating device is determined by feeding back the furnace temperature of the heating zone subsequent to the rapid heating device.
5. 5. The method for annealing a hot-rolled steel strip according to claim 1, wherein the heating temperature of the steel strip by the rapid heating device is determined so that the temperature of the steel strip on the exit side of the heating zone is constant.
6. 5. The method for annealing a hot-rolled steel strip according to claim 1, wherein the heating means of the rapid heating device is at least one of induction heating, electric current heating, and infrared heating.
7. 6. The method for annealing a hot-rolled steel strip according to claim 5, wherein the heating means of the rapid heating device is at least one of induction heating, electric current heating and infrared heating.
Citation Information
Patent Citations
Method for manufacturing a highly effective cold rolling electrical steel product
CN101684514A
Direct switch-on heating annealing apparatus of hot rolled plate
CN201265027Y
Method and apparatus for annealing steel strip continuously
JP1986201735A
Method for controlling temperature of continuous normalized sheet
JP2004197144A
Method for controlling sheet temperature in continuous annealing furnace, and continuous annealing furnace