Adhesive sheet

The adhesive sheet addresses noise and slipping issues during laser processing by incorporating a slip-resistant release surface and high peel strength, ensuring stable adhesion and efficient laser processing.

JP7558661B2Active Publication Date: 2024-10-01NITTO DENKO CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020020903
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-02-10
Publication Date
2024-10-01
Estimated Expiration
2040-02-10

AI Technical Summary

Technical Problem

Adhesive sheets used in laser processing with short wavelength lasers experience high-speed peeling noise and slipping issues due to high assist gas pressure, leading to inefficiencies and environmental disturbances.

Method used

A pressure-sensitive adhesive sheet with a resin film base material and adhesive layer, featuring a slip-resistant release surface, high-speed peel strength, and controlled self-back adhesive force to minimize noise and slipping, while maintaining adherence during laser processing.

Benefits of technology

The adhesive sheet effectively suppresses peeling noise and slipping, ensuring stable adhesion and efficient laser processing without environmental disturbances, even under high assist gas pressure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007558661000002
    Figure 0007558661000002
  • Figure 0007558661000003
    Figure 0007558661000003
  • Figure 0007558661000004
    Figure 0007558661000004
Patent Text Reader

Abstract

To provide an adhesive sheet which has high speed peeling strength applicable to processing by a laser beam, suppresses peeling sound when being peeled from a back face at high speed, and prevents excessive slippage even when stackedly placed in a state of being stuck to a metal plate.SOLUTION: An adhesive sheet includes a resin film 10 as a base material, and an adhesive layer 20 provided on a first surface 10A of the base material, in which a second surface 10B of the base material is a peeled surface, a sliding resistance value of the second surface is 3.5 N or more, high speed peeling strength measured on the condition of tensile speed of 30 m / min after 30 minutes after being stuck to a stainless steel plate is 4.5 N / 20 mm or more, and a difference between a maximum value and a minimum value of a self-back side adhesive force measured on the condition of tensile speed of 30 m / min is 1.5 N / 20 mm or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pressure-sensitive adhesive sheet. [Background technology]

[0002] Generally, adhesives (also called pressure-sensitive adhesives; the same applies below) are in a soft solid (viscoelastic) state at temperatures around room temperature and have the property of easily adhering to an adherend when pressure is applied. Taking advantage of such properties, adhesives are widely used in various fields for purposes such as joining, fixing, surface protection, masking, and marking, typically in the form of an adhesive sheet having an adhesive layer on a substrate. For example, Patent Documents 1 and 2 are technical documents related to adhesive films that can be used for surface protection during laser processing. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-59879 A [Patent Document 2] International Publication No. 2018 / 159591 Summary of the Invention [Problem to be solved by the invention]

[0004] In recent years, interest in processing techniques using laser light has been increasing. Processing techniques using laser light are widely used for cutting and drilling various materials. Representative examples of lasers used in such processing include carbon dioxide gas lasers with a dominant wavelength of about 9.3 μm to 10.6 μm and short-wavelength lasers with a dominant wavelength of about 0.9 μm to 1.1 μm. One embodiment of laser processing is a mode in which an adhesive sheet as an auxiliary material is attached to an object to be processed (a workpiece, hereinafter also referred to as a "work") as an adherend, and the workpiece is laser-processed together with the adhesive sheet by irradiating the adhesive sheet with laser light. The adhesive sheet that can be used in such an embodiment preferably has a high-speed peel strength suitable for suppressing lifting and peeling caused by an assist gas supplied during laser processing.

[0005] In particular, by using a short-wavelength laser beam with a main wavelength of about 0.9 μm to 1.1 μm, the energy required for processing can be efficiently applied to the workpiece. This can be advantageous in terms of speeding up processing and fine processing. On the other hand, in processing with a short-wavelength laser, the assist gas pressure tends to be high in order to speed up processing. For this reason, it is particularly desirable that the adhesive sheet expected to be used in processing with a short-wavelength laser has a certain level of high-speed peel strength in order to prevent the occurrence of an event in which such a high-pressure assist gas gets between the workpiece and the workpiece and the workpiece is lifted off.

[0006] By the way, from the viewpoint of saving resources and reducing waste generated at the work site, the adhesive sheet before use (before being attached to the adherend) may be provided in the form of a roll or laminate in which the second surface (back surface) of the substrate is a release surface that has been subjected to a release treatment such as coating with a release agent, and the surface of the adhesive layer is abutted against the back surface. The attachment of such an adhesive sheet to the workpiece involves an operation of peeling the adhesive sheet from the back surface to expose the surface (adhesive surface) of the adhesive layer. In order to improve the efficiency of the process involving laser processing, it is desirable to speed up the operation of attaching the adhesive sheet to the workpiece prior to the laser processing, and it is also preferable to speed up the operation of peeling the adhesive sheet from the back surface.

[0007] However, it has been found that an adhesive sheet configured to exhibit high-speed peel strength sufficient to withstand assist gas pressure during laser processing is prone to generate loud peeling noise when the operation of peeling the adhesive sheet from the back surface is accelerated. In order to improve the working environment in terms of noise, it is desirable to suppress the above-mentioned peeling noise. However, if a peeling treatment is performed on the back surface of a substrate using a release treatment agent with a higher slippage imparting effect in an attempt to suppress the peeling noise by increasing the peelability of the adhesive sheet from the back surface, there is a concern that when multiple sheets of the adhesive sheet are stacked flat on a workpiece (e.g., a metal plate) with the adhesive sheet attached thereto, the sheets may easily slip sideways, causing the load to collapse.

[0008] In view of these circumstances, the present invention aims to provide an adhesive sheet that has high-speed peel strength that is also applicable to processing using laser light, suppresses the peeling noise when peeled off from the back at high speed, and does not slip excessively even when stacked while attached to a metal plate or the like. [Means for solving the problem]

[0009] According to this specification, there is provided a pressure-sensitive adhesive sheet comprising a resin film as a substrate and a pressure-sensitive adhesive layer provided on a first surface of the substrate. In the pressure-sensitive adhesive sheet, the second surface of the substrate is a release surface, and the slip resistance value of the second surface is 3.5 N or more. The pressure-sensitive adhesive sheet has a high-speed peel strength (hereinafter also simply referred to as "high-speed peel strength") of 4.5 N / 20 mm or more when measured 30 minutes after attachment to a stainless steel plate at a tensile speed of 30 m / min, and the difference between the maximum and minimum values ​​(hereinafter also referred to as "variation range") of the self-backside adhesive strength (hereinafter also simply referred to as "self-backside adhesive strength") measured at a tensile speed of 30 m / min is 1.5 N / 20 mm or less.

[0010] The adhesive sheet thus constructed can be favorably maintained attached to the adherend without floating or peeling even when subjected to impacts such as assist gas pressure during laser processing, etc. Also, the peeling noise when the adhesive sheet is peeled off from its back surface at high speed during use can be reduced, and side slippage can be suppressed when the adherends to which the adhesive sheet is attached are stacked.

[0011] In some preferred embodiments of the pressure-sensitive adhesive sheet, the second surface of the substrate is made of a resin composition containing a release agent. The pressure-sensitive adhesive sheet disclosed herein can be preferably implemented in a configuration including such a substrate. As the release agent, for example, a silicone-based release agent can be preferably used. One preferred example of the silicone-based release agent is silylated polyolefin.

[0012] In some embodiments, a natural rubber-based adhesive can be preferably used as the adhesive constituting the adhesive layer. An adhesive sheet having such an adhesive layer can be suitably used in applications requiring high high-speed peel strength.

[0013] In some preferred embodiments, the PSA sheet disclosed herein has an average backside adhesive strength of 1 N / 20 mm or more and 5 N / 20 mm or less. Such PSA sheets are preferred from the viewpoints of facilitating compatibility with an appropriate slip resistance value and improving workability when peeling from the backside.

[0014] In some embodiments of the pressure-sensitive adhesive sheet disclosed herein, the pressure-sensitive adhesive sheet has a low-speed peel strength (hereinafter, simply referred to as "low-speed peel strength") measured 30 minutes after attachment to a stainless steel plate at a tensile speed of 0.3 m / min, of preferably 5 N / 20 mm or less. Such a pressure-sensitive adhesive sheet can be easily peeled off from an adherend after use, and tends to better suppress adhesive residue after peeling.

[0015] In some embodiments, the substrate is a polyolefin resin film or a polyester resin film. A pressure-sensitive adhesive sheet having such a substrate is preferable because, for example, when cut with a laser beam, the cutting width is easily controlled and a cut end surface having good shape accuracy is easily formed.

[0016] The adhesive sheet disclosed herein can contain a laser beam absorbent as necessary. By containing a laser absorbent in the adhesive sheet, the laser beam absorption rate can be increased, and the laser processability of the adherend to which the adhesive sheet is attached can be improved. From the viewpoint of easily achieving both good laser beam absorbency and desired adhesive properties, it is preferable that at least the substrate contains a laser beam absorbent.

[0017] In some embodiments, the laser beam absorbent may be, for example, at least one selected from the group consisting of carbon black, titanium oxide, titanium black, iron oxides, and manganese oxides. From the viewpoint of stable availability of materials, preferred laser beam absorbents include carbon black and iron oxides.

[0018] The adhesive sheet disclosed herein is unlikely to lift off or peel off from the adherend due to assist gas pressure, even when it is attached to an object to be processed (adherend) and cut together with the object to be processed with laser light. Therefore, as another aspect of the adhesive sheet, there is provided an adhesive sheet for laser cutting, which is made of any of the adhesive sheets disclosed herein and is used by cutting with laser light (e.g., laser light such as a carbon dioxide laser or a short-wavelength laser). As yet another aspect of the adhesive sheet, there is provided an adhesive sheet for laser cutting, which is used by cutting with a short-wavelength laser light (hereinafter also referred to as a "specific laser light") having a dominant wavelength in the range of 900 nm to 1100 nm.

[0019] According to this specification, a roll body is provided that includes the pressure-sensitive adhesive sheet in a wound state such that the pressure-sensitive adhesive layer is in contact with the second surface (back surface) of the substrate. With such a roll body, the back surface peeling noise generated when the pressure-sensitive adhesive sheet is unwound from the roll body is suppressed, and therefore the working environment for workers can be improved. [Brief description of the drawings]

[0020] [Figure 1] FIG. 1 is a cross-sectional view illustrating a schematic diagram of a pressure-sensitive adhesive sheet according to an embodiment. [Diagram 2] 1 is a cross-sectional view illustrating a schematic diagram of a roll around which a pressure-sensitive adhesive sheet according to one embodiment is wound. [Diagram 3] FIG. 4 is a cross-sectional view illustrating a schematic diagram of a pressure-sensitive adhesive sheet according to another embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] A preferred embodiment of the present invention will be described below. Note that matters other than those specifically mentioned in this specification and necessary for carrying out the present invention can be understood by a person skilled in the art based on the teachings on carrying out the invention described in this specification and the common general knowledge at the time of filing. The present invention can be carried out based on the contents disclosed in this specification and the common general knowledge in the field. In addition, in the following drawings, components and parts having the same function may be described by using the same reference numerals, and duplicated descriptions may be omitted or simplified. In addition, the embodiments described in the drawings are schematic in order to clearly explain the present invention, and do not necessarily accurately represent the size or scale of the product actually provided.

[0022] The adhesive sheet disclosed herein has an adhesive layer on one surface (first surface) of a resin film as a substrate. The configuration of an adhesive sheet according to an embodiment is shown in FIG. 1. The adhesive sheet 1 includes a resin film 10 as a substrate and an adhesive layer 20 provided on one surface (first surface) 10A of the resin film 10, and the adhesive layer 20 is attached to an adherend for use. In the adhesive sheet 1, the other surface (back surface, second surface) 10B of the resin film 10 is a surface (release surface) having releasability. The adhesive sheet 1 before use (i.e., before attachment to an adherend) may be in the form of a roll 50 in which the surface (adhesive surface) 20A of the adhesive layer 20 is wound around a core (roll core) 52 in a roll shape so that the surface 20A is in contact with the back surface 10B of the resin film 10, as shown in FIG. 2, for example, and thus the surface 20A is protected. The adhesive sheet 1 may also be in the form of a roll without a core 52, that is, a so-called coreless type roll in which the adhesive sheet 1 is wound alone. Alternatively, the adhesive sheet 1 before use may be in the form of a roll, or may be in the form of a laminate in which the adhesive layer surface of one adhesive sheet is abutted against the back surface of another adhesive sheet to form a laminate in which the adhesive surface 20A is protected. Alternatively, the surface 20A of the adhesive sheet 1 before use may be protected by a release liner, rather than by the back surface of the substrate constituting the adhesive sheet.

[0023] In a preferred aspect of the pressure-sensitive adhesive sheet 1 of this embodiment, the resin film 10 includes a back layer 11 constituting the other surface (second surface) 10B of the resin film 10, and a support layer 12 arranged on the inside of the back layer 11 (the side on which the pressure-sensitive adhesive layer 20 is provided), as shown in FIG. 3, for example. The back layer 11 is composed of a resin composition containing a release agent, and thus the surface of the back layer 11 (which also serves as the second surface 10B of the resin film 10) is a release surface. The support layer 12 may be a layer made of a resin composition that does not contain a release agent, or may be a layer made of a resin composition that contains a release agent. In an aspect in which one surface 10A of the resin film 10 is composed of the support layer 12 as in the example shown in FIG. 3, from the viewpoint of the anchoring property of the pressure-sensitive adhesive layer 20 to the resin film 10, it is preferable that the support layer 12 is a layer made of a resin composition that does not contain a release agent. In the adhesive sheet 2 shown in FIG. 3, the resin film 10 has a two-layer structure made up of the back layer 11 and the support layer 12, but the structure of the resin film 10 is not limited to a two-layer structure.

[0024] <Adhesive sheet> The adhesive sheet disclosed herein is an adhesive sheet comprising a resin film as a substrate and an adhesive layer provided on a first surface of the substrate, and the second surface of the substrate is a peeling surface. The adhesive sheet preferably has a high-speed peel strength of 4.5 N / 20 mm or more when measured at a tensile speed of 30 m / min 30 minutes after being attached to a stainless steel (SUS) plate. Here, the tensile speed of 30 m / min is a measurement condition set assuming a situation in which an assist gas is blown onto the adhesive sheet attached to the workpiece when the workpiece is processed with a short-wavelength laser beam. If the adhesive sheet is lifted by the assist gas supplied during laser processing (typically, partial peeling occurs due to the assist gas entering the adhesive interface between the workpiece and the adhesive sheet due to the wind pressure from the cut portion by the laser beam), the adhesive sheet is exposed to heat in a state in which the adhesive sheet is released from its fixation to the workpiece (bonding by the adhesive), and this may cause inconveniences such as increased thermal contraction, which makes it easier for the surface of the workpiece to be exposed on both sides of the cut portion. A pressure-sensitive adhesive sheet having a high-speed peel strength of 4.5 N / 20 mm or more can effectively prevent the pressure-sensitive adhesive sheet from lifting when cut.

[0025] From the viewpoint of obtaining a higher effect, in some embodiments, the high-speed peel strength of the adhesive sheet may be, for example, 5.0 N / 20 mm or more, 5.5 N / 20 mm or more, or 6.0 N / 20 mm or more. The upper limit of the high-speed peel strength is not particularly limited, but from the viewpoint of reducing the work load when peeling the adhesive sheet from the workpiece and preventing the adhesive sheet from tearing, in some embodiments, the high-speed peel strength of the adhesive sheet may be, for example, 20 N / 20 mm or less, 15 N / 20 mm or less, 10 N / 20 mm or less, or 8 N / 20 mm or less. Specifically, the high-speed peel strength is measured by the method described in the examples below. The high-speed peel strength can be adjusted, for example, by selecting the type and thickness of the adhesive layer, selecting the type and amount of the crosslinking agent, selecting the type and amount of the release agent, using optional components such as tackifier resin, etc.

[0026] The pressure-sensitive adhesive sheet disclosed herein preferably has a fluctuation range of its own backside adhesive strength of 1.5 N / 20 mm or less. A pressure-sensitive adhesive sheet having a fluctuation range of its own backside adhesive strength of 1.5 N / 20 mm or less can reduce the peeling noise when peeling the pressure-sensitive adhesive sheet from the surface of a protective material (typically the backside of a substrate) that protects the surface of the pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet before use, thereby suppressing noise and improving the working environment. The noise level due to the peeling sound of the pressure-sensitive adhesive sheet can be evaluated, for example, by the method described in the Examples.

[0027] In carrying out the technology disclosed in this specification, it is not necessary to clarify the mechanism by which the difference between the maximum and minimum values ​​of the backside adhesive strength (fluctuation range) contributes to the volume of the peeling sound, but in the case of a pressure-sensitive adhesive sheet with a large fluctuation range of the backside adhesive strength, stick-slip failure occurs between the release surface (back side) and the adhesive surface, in which peeling progresses and stops repeatedly, and it is thought that this is the source of the "beep" sound. However, this is not intended to be interpreted as being limited to this mechanism alone.

[0028] From the viewpoint of obtaining a higher effect, in some embodiments, the fluctuation range of the adhesive force on the back side of the pressure-sensitive adhesive sheet may be, for example, less than 1.5 N / 20 mm, may be 1.4 N / 20 mm or less, or may be 1.0 N / 20 mm or less. The lower limit of the fluctuation range of the adhesive force on the back side is, in principle, 0 N / 20 mm, and from the viewpoint of reducing the peeling sound, the smaller the fluctuation range, the more preferable. In some embodiments, from the viewpoint of practicality such as balance with other properties and ease of manufacture, the fluctuation range of the adhesive force on the back side may be, for example, 0.01 N / 20 mm or more, 0.05 N / 20 mm or more, or 0.1 N / 20 mm or more. The fluctuation range of the adhesive force on the back side is measured by the method described in the examples below. The fluctuation range of the adhesive force on the back side can be adjusted, for example, by selecting the constituent material (for example, the type and amount of release agent) and surface treatment of the second surface of the substrate, selecting the type of adhesive constituting the adhesive layer, whether or not optional components such as a crosslinking agent and a tackifier resin are used, and selecting the type and amount of the optional components when used.

[0029] In the PSA sheet disclosed herein, the average value of the adhesive force on the back side is preferably, for example, 5 N / 20 mm or less, more preferably 4.5 N / 20 mm or less, and may be 4 N / 20 mm or less, from the viewpoint of easily reducing the fluctuation range of the adhesive force on the back side. A low average value of the adhesive force on the back side can be advantageous, for example, in a PSA sheet constituting a roll body, from the viewpoint of reducing the labor required for rewinding and improving workability, and from the viewpoint of preventing the PSA sheet stretched during rewinding from shrinking after being applied to the adherend and floating from the adherend. There is no particular lower limit for the average value of the adhesive force on the back side, but from the viewpoint of easily achieving a balance with other properties, it is preferably, for example, 0.5 N / 20 mm or more, more preferably 1 N / 20 mm or more, and may be 1.5 N / 20 mm or more. For example, in the case of a PSA sheet constituting a roll body, it is preferable that the average value of the adhesive force on the back side is not too low, from the viewpoint of preventing inconveniences such as being easily unwound from the roll form. The average value of the adhesive force on the back side is measured by the method described in the Examples described below.

[0030] The adhesive sheet disclosed herein preferably has a slip resistance value of 3.5N or more on the second surface of the substrate. In this specification, the slip resistance value of the second surface of the substrate refers to the dynamic friction force between the back surface of the adhesive sheet and a SUS plate, and is specifically measured by the method described in the Examples below. If the slip resistance value is too small, there is a concern that when the adhesive sheet is attached to a workpiece (adherend) such as a SUS plate or other metal plate and multiple sheets are stacked flat, the load may easily collapse due to lateral slippage. An adhesive sheet having a slip resistance value of 3.5N or more on the second surface of the substrate can effectively suppress the slipperiness of the adherend.

[0031] From the viewpoint of obtaining a higher effect, in some embodiments, the slip resistance value of the second surface of the substrate of the pressure-sensitive adhesive sheet may be, for example, 4N or more, 4.5N or more, or 5N or more. The upper limit of the slip resistance value of the second surface of the substrate of the pressure-sensitive adhesive sheet is not particularly limited. From the viewpoint of easily suppressing the fluctuation range of the back adhesive force, in some embodiments, the slip resistance value may be, for example, 10N or less, 15N or less, or 20N or less.

[0032] In some embodiments, the adhesive sheet disclosed herein preferably has a low-speed peel strength of 10 N / 20 mm or less, more preferably 8 N / 20 mm or less, particularly preferably 5 N / 20 mm or less, and may be 4.5 N / 20 mm or less, measured 30 minutes after application to a stainless steel plate at a tensile speed of 0.3 m / min. Here, the tensile speed of 0.3 m / min is a measurement condition set on the assumption that, for example, after a processing step of an object to be processed (adherend), an adhesive sheet applied to the object to be processed is peeled off and removed. From the viewpoint of reducing the effort required to peel off an unnecessary adhesive sheet and improving workability, and from the viewpoint of suppressing the occurrence of a state in which the adhesive remains on the surface of the adherend after the adhesive sheet is peeled off (so-called "glue residue"), the lower the low-speed peel strength, the more preferable it is. There is no particular lower limit on the low-speed peel strength. From the viewpoint of facilitating compatibility with other properties (e.g., a high-speed peel strength of a predetermined level or higher), in some embodiments, the low-speed peel strength may be 0.5 N / 20 mm or more, 0.8 N / 20 mm or more, or 1.0 N / 20 mm or more. The low-speed peel strength is measured by the method described in the Examples below. The low-speed peel strength can be adjusted, for example, by selecting the type and thickness of the pressure-sensitive adhesive layer, the type and amount of the crosslinking agent, the type and amount of the release agent, the use of optional components such as a tackifier resin, etc.

[0033] The adhesive sheet disclosed in this specification includes embodiments in which there are no restrictions on one or more of the above-mentioned high-speed peel strength, the fluctuation range of the backside adhesive strength, and the slip resistance value of the second surface of the substrate, and in such embodiments, the adhesive sheet is not limited to those that satisfy the above-mentioned characteristics.

[0034] In some embodiments of the pressure-sensitive adhesive sheet disclosed herein, the pressure-sensitive adhesive sheet preferably has a laser light absorptance in the wavelength range of the laser light used for processing (typically, the laser light absorptance at the main wavelength of the laser light) of 20% or more. This laser light absorptance means the proportion of the laser light that is actually absorbed by the pressure-sensitive adhesive sheet out of the laser light irradiated onto the pressure-sensitive adhesive sheet. A pressure-sensitive adhesive sheet with a laser light absorptance of 20% or more can efficiently absorb laser light.

[0035] In some embodiments, the laser light absorptivity of the pressure-sensitive adhesive sheet may be, for example, 25% or more, 30% or more, 45% or more, 60% or more, or 75% or more. The laser light absorptivity of the pressure-sensitive adhesive sheet may be 100%, but in practice, it is preferably 95% or less, and may be 90% or less.

[0036] In this specification, the term "laser light absorptance" refers to a value calculated from the transmittance T (%) and reflectance R (%) of a sample measured using a spectrophotometer (e.g., a spectrophotometer manufactured by Hitachi High-Technologies Corporation, model "U-4100" or an equivalent product) using the following formula (I). Absorption rate A(%)=100(%)-T(%)-R(%) (I)

[0037] In this specification, for example, "laser light absorptance in the wavelength range of 900 nm to 1100 nm" refers to the minimum laser light absorptance in the wavelength range. Furthermore, unless otherwise specified, the laser light absorptance in this specification refers to the laser light absorptance of the back surface of the adhesive sheet or substrate (the surface on the side irradiated with the laser light, i.e., the surface opposite to the surface attached to the workpiece).

[0038] The transmittance and reflectance of the adhesive sheet are not particularly limited. In some embodiments, the adhesive sheet may have a laser light transmittance of less than 70% at a wavelength where the laser light absorptance is the minimum within the wavelength range of the laser light used for processing, for example, less than 50%. In some embodiments, the adhesive sheet may have a laser light reflectance of less than 50% at a wavelength where the laser light absorptance is the minimum, for example, less than 40%, less than 20%, or less than 10%. An adhesive sheet that satisfies at least one of the transmittance and the reflectance (preferably both) is likely to have the preferred laser light absorptance disclosed herein.

[0039] In order to adjust the laser light absorption rate, a laser light absorbent can be used as necessary. As the laser light absorbent, various materials that can increase the absorption rate of the laser light used in processing (typically, the absorption rate at least at the main wavelength) can be preferably used. The type of laser light absorbent contained in the adhesive sheet may be one type, or two or more types. In an adhesive sheet containing two or more types of laser light absorbents, the laser light absorbents may be used in a blend, or may be contained in different layers in the adhesive sheet.

[0040] In this specification, the term "laser beam absorbent" refers to a material that can increase the laser beam absorption rate compared to when the laser beam absorbent is not used. In addition, in this specification, the term "specific absorbing agent" refers to the above-mentioned laser beam absorbents that have as a constituent element a metal with a specific heat of less than 900 J / kg·K and a thermal conductivity of less than 200 W / m·K. In this specification, a layer containing a laser beam absorbent (which may be a specific absorbing agent) may be referred to as a "laser beam absorbing layer."

[0041] Examples of the laser light absorbent that can be used in the adhesive sheet disclosed herein include metals such as aluminum, stainless steel, titanium, nickel, zirconium, tungsten, copper, silver, gold, zinc, molybdenum, chromium, and alloys mainly composed of these metals; metal compounds such as oxides (e.g., titanium oxide, aluminum oxide, etc.), nitrides, and carbides of the above metals; carbon materials such as carbon black and carbon fiber; organic compounds such as phthalocyanine compounds, cyanine compounds, aminium compounds, naphthalocyanine compounds, naphthoquinone compounds, diimonium compounds, anthraquinone compounds, and aromatic dithiol metal complexes (e.g., nickel complexes); and the like. In the laser light absorbing layer containing a laser light absorbent in the resin composition, it is preferable to use a material having a higher thermal decomposition temperature than the resin components constituting the laser light absorbing layer as the laser light absorbent.

[0042] When a powdered laser beam absorbent is used, the shape of the particles constituting the powder is not particularly limited, and may be, for example, flaky, spherical, needle-like, polyhedral, irregular, etc. Usually, a flaky, spherical, or needle-like laser beam absorbent may be preferably used. The average particle size of the laser beam absorbent is not particularly limited, and may be, for example, 0.005 μm or more and 20 μm or less. From the viewpoint of dispersibility, usually, a laser beam absorbent having an average particle size of 10 μm or less or 5 μm or less may be preferably used. From the viewpoint of efficiently increasing the laser beam absorption rate with a small amount of laser beam absorbent, in some embodiments, the average particle size of the laser beam absorbent may be, for example, 3 μm or less, 1 μm or less, 0.6 μm or less, 0.4 μm or less, or 0.3 μm or less. From the viewpoint of powder handling and ease of uniform dispersion, in some embodiments, the average particle size of the laser beam absorbent may be, for example, 0.008 μm or more, 0.01 μm or more, 0.05 μm or more, 0.1 μm or more, 0.15 μm or more, or 0.2 μm or more. In this specification, the term "average particle size" refers to the particle size at an integrated value of 50% in a particle size distribution measured with a particle size distribution measuring device based on a laser scattering / diffraction method (50% volume average particle size), unless otherwise specified.

[0043] In some embodiments, the laser light absorbing layer may contain carbon black as the laser light absorbing agent. For example, carbon black having an average particle size of 10 nm to 500 nm (more preferably 10 nm to 120 nm) may be used. Carbon black may be used alone or in combination with other laser light absorbing agents.

[0044] In some embodiments, the laser light absorbing layer may contain at least one of a metal powder and a metal compound powder as a laser light absorbent. Such a laser light absorbent is preferable because it can withstand heat generation accompanying absorption of a specific laser light and appropriately maintain the property of absorbing the specific laser light. Suitable examples of this type of laser light absorbent include titanium oxide powder, aluminum oxide powder, and metallic aluminum powder.

[0045] The laser light absorbing layer is typically a layer containing a laser light absorbing agent in a resin component. Non-limiting examples of materials that can be used as such a resin component include polyester resins such as polyethylene terephthalate (PET) and polybutylene terephthalate (PBT); polyolefin resins such as polyethylene, polypropylene, ethylene-propylene copolymers, and polypropylene-polyethylene blend resins; and other vinyl chloride resins, vinyl acetate resins, and polyamide resins. The laser light absorbing layer can be formed by molding a resin composition obtained by blending a laser light absorbing agent with such a resin material into a typically film-like shape.

[0046] When using a laser beam absorbent, its amount is not particularly limited.In some embodiments, the amount of the laser beam absorbent may be, for example, 0.01% by weight or more of the laser beam absorption layer containing the laser beam absorbent, 0.05% by weight or more, or 0.1% by weight or more.In addition, from the viewpoint of reducing laser cutting residue and suppressing reflectance, in some embodiments, the content of the laser beam absorbent may be, for example, 10% by weight or less of the laser beam absorption layer containing the laser beam absorbent, 5% by weight or less, 3% by weight or less, or 2% by weight or less.

[0047] In some embodiments, the pressure-sensitive adhesive sheet disclosed herein may preferably use, as the laser beam absorbent, a specific absorbent, i.e., a laser beam absorbent having as a constituent element a metal with a specific heat of less than 900 J / kg·K and a thermal conductivity of less than 200 W / m·K. The specific absorbent may be selected from the group consisting of any one of a single metal satisfying the above specific heat and thermal conductivity; an alloy containing any one of a single metal satisfying the above specific heat and thermal conductivity at a ratio of more than 50 wt%, more than 70 wt%, or more than 90 wt%; an alloy containing two or more metals satisfying the above specific heat and thermal conductivity at a ratio of more than 50 wt%, more than 70 wt%, or more than 90 wt% in total; a metal compound containing a metal corresponding to such a single metal or alloy as a constituent element; and the like. The specific absorbent referred to here includes, for example, iron, iron alloys (for example, iron alloys containing at least one element selected from the group consisting of Cr, Ni, Si, W, Mn, Si, and C), and metal compounds (iron-based compounds) containing a metal (iron-based metal) corresponding to the iron or iron alloy as a constituent element. As the iron-based compound, for example, an oxide of the iron-based metal (iron-based oxide) can be preferably used. Other examples of the specific absorbent include Mn-based compounds containing a metal (Mn-based metal) corresponding to Mn or an Mn alloy as a constituent element, and among them, Mn-based oxides are preferred. The specific absorbent can be used alone or in combination of two or more. In a pressure-sensitive adhesive sheet containing two or more types of specific absorbents, the specific absorbents may be used in a blend, or may be contained in different layers within the pressure-sensitive adhesive sheet.

[0048] In general, the specific heat and thermal conductivity of a metal compound containing a metal as a constituent element tend to be smaller than those of a metal alone. Therefore, in some embodiments of the pressure-sensitive adhesive sheet disclosed herein, a metal compound containing a metal as a constituent element that satisfies the preferred specific heat and thermal conductivity disclosed herein can be preferably used as a specific absorbent. The metal compound that can be used as a specific absorbent can be, for example, an oxide, sulfide, carbide, nitride, hydroxide, oxyhydroxide, etc. of a metal that satisfies the preferred specific heat and thermal conductivity disclosed herein. Other examples of metal compounds that can be used as specific absorbents include metal organic compounds (complexes, etc.) that contain ions of the metal. From the viewpoint of enduring the heat generation accompanying the absorption of specific laser light and appropriately maintaining the property of absorbing the specific laser light, the oxide, sulfide, carbide, and nitride of the above metal are preferred, and oxides are particularly preferred. Examples of the oxides include iron oxide (FeO, Fe3O4, Fe2O3, etc.), manganese dioxide, titanium black, chromium oxide (CrO, Cr2O3, etc.), ferrite, etc., and examples of the sulfides include iron sulfide, molybdenum sulfide, etc., but are not limited to these.

[0049] In the case where the pressure-sensitive adhesive sheet disclosed herein contains a specific absorbent, the content of the specific absorbent is not particularly limited, and may be appropriately selected, for example, from the range of 0.01% by weight or more and 20% by weight or less of the pressure-sensitive adhesive sheet. In some embodiments, the content of the specific absorbent may be, for example, 0.05% by weight or more, 0.1% by weight or more, 0.3% by weight or more, 0.5% by weight or more, or 0.8% by weight or more. When the content of the specific absorbent is high, the absorption rate of the specific laser light tends to be high. On the other hand, when the content of the specific absorbent is too high, the energy of the absorbed specific laser light tends to diffuse in the surface direction, and energy loss may increase. From this viewpoint, the content of the specific absorbent is usually appropriate to be 15% by weight or less of the pressure-sensitive adhesive sheet, preferably 10% by weight or less, more preferably 7% by weight or less, and may be 5% by weight or less or less than 5% by weight.

[0050] The adhesive sheet disclosed herein may contain, in addition to the specific absorbent, a laser light absorbent other than the specific absorbent as needed. Hereinafter, the laser light absorbent other than the specific absorbent used as an auxiliary in this way is also referred to as an "auxiliary absorbent". The auxiliary absorbent may be used for the purpose of, for example, improving the absorption rate of the adhesive sheet, adjusting the transmittance or reflectance, adjusting the appearance, etc. Examples of the auxiliary absorbent include metals such as aluminum, copper, silver, and gold; metal compounds such as oxides, nitrides, and carbides of the above metals; carbon black; organic compounds such as phthalocyanine compounds, cyanine compounds, aminium compounds, naphthalocyanine compounds, naphthoquinone compounds, diimonium compounds, and anthraquinone compounds; and the like.

[0051] The amount of auxiliary absorbent used is preferably less than 50% by weight of the total amount of laser light absorbent contained in the adhesive sheet (i.e., the total amount of the specific absorbent and the auxiliary absorbent), and may be less than 25%, less than 10%, or less than 5%. The adhesive sheet may be substantially free of auxiliary absorbent. Here, substantially free of auxiliary absorbent means that the auxiliary absorbent is not used at least intentionally. The total amount of laser light absorbent contained in the adhesive sheet is suitably 25% by weight or less of the adhesive sheet, and more preferably 20% by weight or less, 15% by weight or less, or 10% by weight or less.

[0052] When the adhesive sheet disclosed herein contains a specific absorbent, the carbon black (CB) content of the adhesive sheet is preferably less than 0.3% by weight of the adhesive sheet, more preferably less than 0.1% by weight, even more preferably less than 0.05% by weight, and particularly preferably 0.02% by weight or less. The reduction in the CB content tends to improve the non-contamination properties of the adhesive sheet. The adhesive sheet may be substantially free of CB, that is, an adhesive sheet in which CB is not used at least intentionally. The adhesive sheet disclosed herein contains a specific absorbent, so that the workpiece can be efficiently processed even if no CB is used or the amount of CB used is limited as described above. With such an adhesive sheet, the improvement in the processing efficiency of the workpiece and the non-contamination properties can be suitably achieved at the same time.

[0053] In some embodiments, a black metal compound may be preferably used as the specific absorbent. The use of a black metal compound can efficiently increase the laser light absorptivity of the adhesive sheet. This makes it possible to preferably realize an adhesive sheet having the above-mentioned preferred laser light absorptivity even if CB is not used or the amount of CB used is limited. The inventors' study has revealed that, unexpectedly, unlike CB, such black metal compounds are less likely to produce black residues. Therefore, the use of a black metal compound can preferably achieve both improved processing efficiency and non-contamination of the workpiece.

[0054] Examples of black metal compounds include, but are not limited to, iron oxide, manganese dioxide, titanium black, chromium oxide, iron sulfide, molybdenum sulfide, etc. In terms of availability, preferred black metal compounds include iron oxide (e.g., FeO, Fe3O4, etc.), titanium black, manganese dioxide, etc. The titanium black is black particles having titanium atoms, and is preferably black particles such as titanium oxynitride and low-order titanium oxide. Among these, preferred black metal compounds include iron oxide and titanium black.

[0055] The content of the black metal compound in the adhesive sheet can be, for example, 0.05% by weight or more of the adhesive sheet, and from the viewpoint of improving the laser light absorption rate, it may be 0.1% by weight or more, 0.3% by weight or more, 0.5% by weight or more, or 0.8% by weight or more. In addition, from the viewpoint of reducing the energy loss due to diffusion in the surface direction of the adhesive sheet, the content of the black metal compound is usually appropriate to be 15% by weight or less of the adhesive sheet, preferably 10% by weight or less, more preferably 7% by weight or less, and may be 5% by weight or less or less than 5% by weight. The proportion of the black metal compound in the specific absorbent may be, for example, more than 50% by weight, may be 70% by weight or more, may be 90% by weight or more, or may be substantially 100% by weight.

[0056] Lightness L of the back of the adhesive sheet * Preferably, the lightness L of the back surface of the pressure-sensitive adhesive sheet is less than 95. * For example, the lightness L of the back surface may be less than 90, less than 70, less than 60, less than 50, less than 45, or less than 40. * By setting the lightness L low, it becomes easier to increase the laser light absorption rate of the adhesive sheet. * The lower limit of the lightness L of the back surface of the PSA sheet is not particularly limited, but from the viewpoint of the design, surface printability, weather resistance, and distinguishability of the PSA sheet, it is usually appropriate to set the lightness L to 20 or more, and may be set to 30 or more. * may be, for example, 40 or more, or 50 or more.

[0057] Chromaticity a of the back of the adhesive sheet * is not particularly limited. In some embodiments, the lightness L * From the same viewpoint, the chromaticity a of the back of the adhesive sheet * The chromaticity b of the back surface of the pressure-sensitive adhesive sheet may be, for example, in the range of -15 to +15, in the range of -10 to +10, in the range of -5 to +7, in the range of -3 to +5, in the range of -1.5 to +3, or in the range of 0 to +2. *is not particularly limited, and may be, for example, in the range of -15 to +15, in the range of -10 to +10, in the range of -5 to +5, in the range of -3 to +2, or in the range of -1.5 to +1.

[0058] Lightness L of the front surface of the adhesive sheet * , chromaticity a * , chromaticity b * is the lightness L of the back surface of the adhesive sheet mentioned above. * , chromaticity a * , chromaticity b * The lightness can be appropriately selected from the same range as above. * , chromaticity a * , chromaticity b * Each of the above may be the same on the front and back surfaces of the pressure-sensitive adhesive sheet, or may be different.

[0059] In this specification, the lightness L * , chromaticity a * and chromaticity b * , L * a * b * Lightness L defined in the color system * , chromaticity a * , chromaticity b * This refers to the brightness L, which is based on the standard recommended by the International Commission on Illumination in 1976 or the standard specified in JIS Z 8729. * , chromaticity a * , chromaticity b * is measured using a color difference meter (for example, a color difference meter under the trade name "CR-400" manufactured by Minolta Co., Ltd.). * , chromaticity a * , chromaticity b * can be adjusted by selecting the type of laser beam absorbent, selecting the amount of laser beam absorbent used, whether or not a colorant other than the laser beam absorbent is used, and selecting the type and amount of the colorant when a colorant is used, etc.

[0060] The thickness of the adhesive sheet is not particularly limited, but is usually about 10 μm to 200 μm. From the viewpoint of the handleability of the adhesive sheet, in some embodiments, the thickness of the adhesive sheet may be, for example, 20 μm or more, 25 μm or more, 40 μm or more, 55 μm or more, or 80 μm or more. Also, from the viewpoint of the speed and precision of laser processing, for example, the thickness of the adhesive sheet may be, for example, 150 μm or less, 120 μm or less, or 100 μm or less. In some cases, the thickness of the adhesive sheet may be 80 μm or less, 60 μm or less, or 50 μm or less.

[0061] <Base material> The adhesive sheet disclosed herein includes a resin film as a substrate. Examples of the resin material constituting the resin film include, but are not limited to, polyester resins such as polyethylene terephthalate (PET) and polybutylene terephthalate (PBT); polyolefin resins such as polyethylene, polypropylene, ethylene-propylene copolymers, and polypropylene-polyethylene blend resins; and other vinyl chloride resins (typically soft vinyl chloride resins), vinyl acetate resins, and polyamide resins.

[0062] From the viewpoint of various processability due to the flexibility of the substrate, or, for example, from the viewpoint of the cuttability and non-contamination of the adhesive sheet by specific laser light, in some embodiments, a polyolefin-based resin film or a polyester-based resin film can be preferably used as the resin film.

[0063] Here, the polyolefin resin film refers to a resin film whose main component is a polyolefin resin. In this specification, the main component refers to a component contained in an amount of more than 50% by weight, unless otherwise specified. For example, when the main component of a resin film is a polyolefin resin, the resin film contains a polyolefin resin in an amount of more than 50% by weight of its total weight. A suitable example of a polyolefin resin film is a resin film whose main component is a polyethylene (PE) resin and / or a polypropylene (PP) resin. A polyolefin resin film may contain a PE resin and / or a PP resin, and the total amount of the PE resin and the PP resin may be more than 50% by weight of the polyolefin resin film, preferably 70% by weight or more, for example 85% by weight or more. The above total amount corresponds to the content of the PE resin in a resin film containing a PE resin and not containing a PP resin.

[0064] The PE resin may be mainly composed of various polymers (ethylene-based polymers) having ethylene as the main constituent monomer unit. The PE resin may be substantially composed of one or more ethylene-based polymers. The ethylene-based polymer may be a homopolymer of ethylene, or may be a copolymer of ethylene as the main monomer with another α-olefin as a secondary monomer (random copolymerization, block copolymerization, etc.). Suitable examples of the α-olefin include α-olefins having 3 to 10 carbon atoms, such as propylene, 1-butene (which may be branched 1-butene), 1-hexene, 4-methyl-1-pentene, and 1-octene. For example, a PE resin mainly composed of an ethylene-based polymer copolymerized with the α-olefin as a secondary monomer at a ratio of 10% by weight or less (typically 5% by weight or less) may be preferably used.

[0065] The PE resin may also be a PE resin containing a copolymer of ethylene and a monomer (functional group-containing monomer) having another functional group in addition to the polymerizable functional group, or a PE resin in which such a functional group-containing monomer is copolymerized with an ethylene-based polymer, etc. Examples of copolymers of ethylene and functional group-containing monomers include ethylene-vinyl acetate copolymer (EVA), ethylene-acrylic acid copolymer (EAA), ethylene-methacrylic acid copolymer (EMAA), ethylene-methyl acrylate copolymer (EMA), ethylene-ethyl acrylate copolymer (EEA), ethylene-methyl methacrylate copolymer (EMMA), and ethylene-(meth)acrylic acid (i.e., acrylic acid and / or methacrylic acid) copolymers crosslinked with metal ions.

[0066] The density of the PE resin is not particularly limited. The concept of PE resin here includes high density polyethylene (HDPE), medium density polyethylene (MDPE), low density polyethylene (LDPE) and linear low density polyethylene (LLDPE). In one embodiment, the density of the PE resin is, for example, 0.90 to 0.94 g / cm 3 Preferred PE resins include LDPE and LLDPE.

[0067] The PP resin may be a polymer (propylene-based polymer) having propylene as the main constituent monomer unit, i.e., a polymer having more than 50% by weight of all constituent monomer units being propylene as the main component. The PP resin may be substantially composed of one or more propylene-based polymers. The concept of propylene-based polymer here includes homopolypropylene, as well as random copolymers (random polypropylenes) and block copolymers (block polypropylenes) of propylene and other monomers.

[0068] The first surface of the substrate (i.e., the surface on which the adhesive layer is provided) may be subjected to an appropriate surface treatment to enhance adhesion to the adhesive layer, as necessary. Examples of surface treatments to enhance adhesion include corona discharge treatment, acid treatment, ultraviolet irradiation treatment, plasma treatment, and application of a primer.

[0069] In the pressure-sensitive adhesive sheet disclosed herein, the second surface of the substrate serves as a release surface. The term "the second surface of the substrate serves as a release surface" typically means that a pressure-sensitive adhesive sheet in which the surface (adhesive surface) of the pressure-sensitive adhesive layer provided on the first surface of the substrate is in contact with the release surface can be peeled off without leaving any adhesive residue (residual adhesive) on the release surface.

[0070] In some embodiments, the resin composition constituting the second surface (hereinafter also referred to as "second surface forming material") preferably contains a release agent. A substrate having such a second surface can be understood as a substrate having the release agent kneaded into at least the second surface. According to such an embodiment, a pressure-sensitive adhesive sheet can be preferably realized in which the slip resistance value of the second surface is 3.5 N or more and the fluctuation range of the adhesive strength of the back surface is 1.5 N / 20 mm or less. The second surface forming material needs only to constitute at least the second surface of the substrate, and may, for example, constitute only the second surface side of the substrate, or may constitute the entire substrate.

[0071] As the second surface forming material, a resin composition containing at least a release agent and a resin material can be preferably used.The above-mentioned resin material includes, but is not limited to, various materials exemplified as the resin material constituting the resin film as the substrate, such as polyester resins such as polyethylene terephthalate (PET) and polybutylene terephthalate (PBT); polyolefin resins such as polyethylene, polypropylene, ethylene-propylene copolymer and polypropylene-polyethylene blend resin; and other vinyl chloride resins (typically soft vinyl chloride resins), vinyl acetate resins, polyamide resins; etc.

[0072] Examples of release agents that can be used as a component of the second surface forming material (i.e., release agents for kneading into the second surface) include ethylene-vinyl alcohol copolymers, fatty acid amide-based additives, low molecular weight polyolefin waxes, long chain alkyl-based additives, silicone-based release agents, etc. The release agents can be used alone or in appropriate combination of two or more. It is preferable to select a release agent that has good mixability with the resin component contained in the second surface forming material.

[0073] As the ethylene-vinyl alcohol copolymer, for example, an ethylene-vinyl alcohol copolymer obtained by saponifying a copolymer of ethylene with vinyl acetate, vinyl formate, vinyl propionate, or vinyl acetate can be used. Examples of fatty acid amide additives include saturated fatty acid bisamides, unsaturated fatty acid bisamides, aromatic bisamides, and substituted ureas. Examples of fatty acid amide additives include methylene bisstearic acid amide, ethylene bisstearic acid amide, ethylene bisoleic acid amide, N,N-dioleyl adipic acid amide, N-stearyl-N'-stearyl urea, and other N-stearyl-N'-stearyl acid amides. These fatty acid amide additives may be used alone or in combination of two or more. As the low molecular weight polyolefin wax, for example, low molecular weight waxes such as polyethylene wax and polypropylene wax can be appropriately used. As the long-chain alkyl additive, low molecular weight additives having an alkyl chain, such as Peloil (registered trademark) 1010 and Peloil (registered trademark) 1010S (both manufactured by Ipposha Yushi Kogyo Co., Ltd.), can be appropriately used. Examples of silicone-based release agents include silylated polyolefins, silicone resins, silicone alkoxy oligomers, silicone oligomers, silicone master pellets, silicone rubber powders, silicone emulsions, etc. As the silylated polyolefins, for example, silylated polyolefins prepared by the method shown in the examples of JP-A-2011-26448 can be used.

[0074] The above-mentioned long-chain alkyl additive and silicone-based release agent are suitable examples of the release agent for kneading the second surface, because they can easily realize appropriate slip resistance and can easily suppress the fluctuation range of the adhesive force of the back surface.Among them, silicone-based release agent is particularly preferred.As the silicone-based release agent, silylated polyolefin is particularly preferred.

[0075] The content of the release agent in the second surface forming material is not particularly limited, and may be, for example, about 0.01 to 80% by weight of the entire second surface forming material. From the viewpoint of setting the fluctuation range of the self back adhesion and the slip resistance value in the desired range, in some embodiments, the content of the release agent in the second surface forming material may be, for example, 0.1% by weight or more, 0.3% by weight or more, 0.5% by weight or more, 0.7% by weight or more, or 1% by weight or more. From the viewpoint of compatibility with the resin material, etc., the content of the release agent in the second surface forming material may be, for example, 70% by weight or less, 50% by weight or less, 30% by weight or less, or 10% by weight or less.

[0076] The substrate may be a single-layer structure or a multi-layer structure of two or more layers. In some embodiments, a substrate with a multi-layer structure may be preferably adopted. A substrate with a multi-layer structure has an advantage that the function and appearance of the first surface and the second surface of the substrate can be easily made different. In a substrate with a multi-layer structure, the type of resin material constituting each layer may be the same or different. The substrate with a multi-layer structure may be, for example, a two-layer to five-layer structure, or may be a two-layer or three-layer structure. In some other embodiments, the substrate may be a single-layer structure. A substrate with a single-layer structure may be advantageous in terms of the productivity and quality stability of the substrate.

[0077] The method of forming the substrate is not particularly limited, and a conventionally known extrusion molding method, such as an inflation extrusion molding method or a cast molding method, can be appropriately adopted. The substrate may be unstretched or may be stretched uniaxially or biaxially. A multi-layer substrate can be obtained by simultaneously molding resin compositions corresponding to each layer (for example, by a multi-layer inflation molding method), laminating each layer after molding, casting another layer on a layer previously molded, or the like, either alone or in combination.

[0078] In some embodiments, the substrate may be a substrate having a multi-layer structure of two or more layers, including a back layer formed from the second surface forming material as described above and a support layer disposed inside the back layer (i.e., on the side closer to the first surface). Hereinafter, the resin composition (i.e., the second surface forming material) forming the back layer in the substrate having such a configuration may be particularly referred to as a "back layer forming material". As the back layer forming material, a resin composition containing a release agent can be preferably used, as in the second surface forming material described above. The back layer forming material may be, for example, a resin composition containing at least a release agent and a resin material. The release agent that can be used as a component of the back layer forming material, the content of the release agent in the back layer forming material, and examples of resin materials that can be used as a component of the back layer forming material are the same as those of the second surface forming material described above, so that repeated explanations will be omitted.

[0079] The support layer may be a layer formed from a resin composition. Hereinafter, the resin composition forming the support layer may be referred to as a "support layer forming material". Resin components that can be used as components of the support layer forming material include, but are not limited to, polyester resins, polyolefin resins, vinyl chloride resins, vinyl acetate resins, polyamide resins, etc., similar to the resin materials constituting the above-mentioned resin film. The support layer forming material may contain one type selected from such resin materials alone, or two or more types in appropriate combination. The support layer forming material may not contain a release agent similar to the release agent that can be used in the second surface forming material, or may contain a release agent. In an embodiment in which one surface of the support layer also serves as the first surface of the substrate, it is preferable that the support layer forming material does not contain a release agent from the viewpoint of improving the anchoring property of the pressure-sensitive adhesive layer to the support layer. The resin material constituting the back layer forming material and the resin material constituting the support layer forming material may be the same or different. From the viewpoint of adhesion between the back layer and the support layer, in some embodiments, the resin material constituting the back layer forming material may preferably be the same type of resin as the resin material constituting the support layer forming material.

[0080] The substrate including the back layer and the support layer disposed inside thereof can be obtained, for example, by laminating the support layer forming material and the back layer forming material by co-extrusion molding. The support layer forming material may be co-extrusion molded with the back layer forming material in the form of a preformed base resin film. The number of layers to be laminated in each of the above layers is not particularly limited, and the back layer and the support layer may each be a single layer, or may be a laminate structure of multiple layers as necessary.

[0081] The co-extrusion molding may be a method generally used for the production of films, sheets, etc., and is not particularly limited. Specifically, a two-layer, three-layer, four-layer or more multilayer structure may be formed, for example, by an inflation method, a co-extrusion T-die method, etc. The use of these co-extrusion molding methods is preferable in terms of cost and productivity.

[0082] In the pressure-sensitive adhesive sheet disclosed herein, the method of forming the second surface as a release surface may preferably be a method of forming the second surface of the substrate with a second surface forming material containing a release agent in a resin composition as described above, but is not limited thereto. As a method of forming the second surface of the substrate as a release surface, various methods that can realize a pressure-sensitive adhesive sheet showing an appropriate slip resistance value and a fluctuation range of the self-backside adhesive force can be applied alone or in combination of two or more. The second surface of the substrate may be a release surface obtained by performing a surface treatment in which a release agent is applied to a surface formed from a resin composition that does not contain a release agent. Such a surface treatment may be performed, for example, using a general silicone-based, long-chain alkyl-based, fluorine-based, or other release agent. A surface formed from a resin composition containing a release agent (i.e., a surface into which the release agent is kneaded) may be further subjected to a surface treatment in which a release agent is applied.

[0083] The substrate may contain a laser beam absorbent as necessary. In some embodiments, the laser beam absorbent preferably contains a specific absorbent. A suitable example of the substrate containing a laser beam absorbent is a substrate containing a laser beam absorbing layer (which may be a specific absorbent). In a substrate having a multi-layer structure, at least one layer is preferably a laser beam absorbing layer containing a laser beam absorbent. The laser beam absorptivity of the substrate containing a laser beam absorbing layer can be set so that the laser beam absorptivity of the adhesive sheet is 20% or more. In some embodiments, the laser beam absorptivity of the substrate may be, for example, 15% or more, usually 20% or more is appropriate, and may be 25% or more, 30% or more, 45% or more, 60% or more, or 75% or more. The laser beam absorptivity of the substrate may be 100%, but in practical terms, it is preferably 95% or less, and may be 90% or less. The transmittance and reflectance of the substrate may be appropriately selected from the same range as the transmittance and reflectance of the adhesive sheet described above.

[0084] The laser beam absorbent contained in the substrate may be one of the above-mentioned examples of the laser beam absorbent usable in the pressure-sensitive adhesive sheet, or two or more of them may be used in combination. In the embodiment in which the laser beam absorbent contains a specific absorbent, the specific absorbent may be one of the above-mentioned examples of the specific absorbent usable in the pressure-sensitive adhesive sheet, or two or more of them may be used in combination. The content of the laser beam absorbent and the content of the specific absorbent in the substrate may be the same as those in the above-mentioned examples of the laser beam absorbent and the content of the specific absorbent in the pressure-sensitive adhesive sheet, respectively.

[0085] Back surface brightness L of the substrate * , chromaticity a * , chromaticity b * is the lightness L of the back surface of the adhesive sheet mentioned above. * , chromaticity a * , chromaticity b * Similarly, the lightness L of the front surface of the substrate can be appropriately selected from the same range. * , chromaticity a * , chromaticity b * is the brightness L of the front surface of the adhesive sheet mentioned above. * , chromaticity a * , chromaticity b * It can be appropriately selected from the same range.

[0086] The substrate may contain any additives as necessary, such as flame retardants, antistatic agents, light stabilizers (radical scavengers, ultraviolet absorbers, etc.), and antioxidants.

[0087] The thickness of the substrate is not particularly limited, and may be, for example, about 5 μm to 150 μm. From the viewpoint of the handleability of the substrate or the adhesive sheet having the substrate, in some embodiments, the thickness of the substrate may be, for example, 15 μm or more, 20 μm or more, 35 μm or more, 50 μm or more, or 75 μm or more. Also, from the viewpoint of the speed and precision of the laser processing, in some embodiments, the thickness of the substrate may be, for example, 130 μm or less, 110 μm or less, or 90 μm or less. In some cases, the thickness of the substrate may be 70 μm or less, 50 μm or less, or 40 μm or less.

[0088] In a substrate including a back layer (preferably a back layer made of a resin composition containing a release agent) and a support layer, the thickness of the back layer (when the back layer has a laminated structure, the total thickness of those layers) is not particularly limited. From the viewpoint of easily forming a back layer with little thickness unevenness, the thickness of the back layer is advantageously, for example, 1 μm or more, and may be 3 μm or more, or 5 μm or more. The technology disclosed herein can also be suitably implemented in the form of a pressure-sensitive adhesive sheet including a substrate having a back layer with a thickness of more than 7 μm, more than 10 μm, more than 15 μm, more than 20 μm, or more than 25 μm. The upper limit of the thickness of the back layer is not particularly limited, and may be less than the thickness of the entire substrate including the back layer. The thickness of the back layer of the entire substrate thickness can be, for example, 1% or more, 3% or more, 5% or more, or 8% or more, or, for example, 95% or less, 70% or less, 50% or less, 20% or less, or 15% or less. The thickness of the back layer can be, for example, 60 μm or less, 40 μm or less, 30 μm or less, 20 μm or less, 10 μm or less, etc., depending on the thickness of the entire substrate. Reducing the thickness of the back layer can be advantageous from the viewpoint of making the pressure-sensitive adhesive sheet thinner.

[0089] From the viewpoints of suppressing unevenness in the thickness of the support layer and handling of the resin film when a preformed resin film is used as the support layer, the thickness of the support layer is usually 5 μm or more, preferably 10 μm or more, may be 25 μm or more, may be 40 μm or more, or may be 60 μm or more. The upper limit of the thickness of the support layer is not particularly limited, and it is sufficient that it is less than the thickness of the entire substrate including the back layer.

[0090] In a substrate including a laser light absorbing layer, the thickness of the laser light absorbing layer (in a substrate including a plurality of laser light absorbing layers, the total thickness of those layers) may be, for example, 3 μm or more, 5 μm or more, or 10 μm or more. From the viewpoint of rapidity and precision of laser processing, in some embodiments, the thickness of the laser light absorbing layer (in other words, the portion where the laser light absorbent is disposed) of the entire thickness of the substrate may be, for example, 20% or more, 50% or more, 70% or more, or 90% or more. Note that, in a substrate including a single layer of a laser light absorbing layer or a substrate including a plurality of laser light absorbent layers, the thickness of the laser light absorbing layer is 100% of the entire thickness of the substrate.

[0091] <Adhesive layer> The adhesive constituting the adhesive layer in the technology disclosed herein is not particularly limited, and for example, known rubber-based adhesives, acrylic-based adhesives, polyester-based adhesives, polyurethane-based adhesives, silicone-based adhesives, etc. can be used. From the viewpoint of adhesive performance and cost, rubber-based adhesives or acrylic-based adhesives can be preferably adopted. Here, the rubber-based adhesive refers to an adhesive in which the main component of the polymer component contained in the adhesive (typically a component contained in more than 50 wt%) is a rubber-based polymer, and the acrylic-based adhesive refers to an adhesive in which the main component of the polymer component contained in the adhesive is an acrylic polymer. The same applies to polyester-based adhesives, polyurethane-based adhesives, silicone-based adhesives, etc. The pressure-sensitive adhesive layer may be a single layer structure or a laminate structure having two or more layers having the same or different compositions. From the viewpoint of increasing the uniformity of the pressure-sensitive adhesive layer and reducing the fluctuation range of the adhesive strength of the back side, a pressure-sensitive adhesive layer having a single layer structure is preferred.

[0092] As the adhesive constituting the adhesive layer of the adhesive sheet disclosed herein, a rubber-based adhesive is particularly preferably used from the viewpoint of exhibiting better high-speed peel strength. Examples of the rubber-based adhesive include natural rubber-based adhesives and synthetic rubber-based adhesives.

[0093] The concept of the natural rubber-based adhesive includes those in which the base polymer is natural rubber and those in which the base polymer is modified natural rubber. The natural rubber is not particularly limited, and for example, standard Malaysian rubber (SMR), standard Vietnamese rubber (SVR), ribbed smoked sheet (RSS), pale crepe, etc. can be used. The modified natural rubber can preferably be one in which 50% by weight or more (for example, 60% by weight or more) of the modified natural rubber is a structural part derived from natural rubber. A specific example of the modified natural rubber is acrylic modified natural rubber, but is not limited thereto.

[0094] Specific examples of rubber-based polymers that serve as the base polymer of the synthetic rubber-based adhesives include polybutadiene, polyisoprene, butyl rubber, polyisobutylene, styrene-butadiene rubber (SBR), styrene-butadiene-styrene block copolymer (SBS), styrene-ethylene / butylene-styrene block copolymer (SEBS), styrene-isoprene-styrene block copolymer (SIS), and the like.

[0095] In a preferred embodiment, the base polymer of the rubber-based adhesive layer is natural rubber. For example, natural rubber having a Mooney viscosity of about 10 to 60 under the measurement conditions of MS(1+4)100°C (using an L-type rotor, preheating for 1 minute, viscosity measurement time for 4 minutes, test temperature of 100°C) is preferred. Adhesive sheets having a natural rubber-based adhesive layer tend to have a quicker increase in adhesion to an adherend than adhesive sheets having a synthetic rubber-based adhesive layer. This can suitably suppress lifting or peeling of the adhesive sheet due to assist gas pressure, even if the time between attaching the adhesive sheet to an object to be processed (adherend) and subjecting the object to laser processing is shortened.

[0096] The rubber-based adhesive layer in the technology disclosed herein may have a composition in which a base polymer is blended with another polymer (hereinafter also referred to as a secondary polymer). Such secondary polymers may be, for example, acrylic polymers, polyester polymers, polyurethane polymers, silicone polymers, etc., which can serve as base polymers for acrylic adhesives, polyester adhesives, polyurethane adhesives, silicone adhesives, etc. Alternatively, the secondary polymers may be any of the above-mentioned rubber-based polymers other than the base polymers. Such secondary polymers may be used alone or in combination of two or more kinds.

[0097] Such a secondary polymer is used in an amount of 100 parts by weight or less (when two or more secondary polymers are used, the total amount of the secondary polymers) relative to 100 parts by weight of the base polymer. Usually, it is appropriate to use 70 parts by weight or less of the secondary polymer relative to 100 parts by weight of the base polymer, and it is preferable to use 50 parts by weight or less. The rubber-based pressure-sensitive adhesive layer may be substantially free of secondary polymers (i.e., substantially 100% by weight of the polymer components is the base polymer). The rubber-based pressure-sensitive adhesive layer may also be substantially free of polymer components other than rubber-based polymers (for example, a rubber-based pressure-sensitive adhesive layer substantially free of polymer components other than natural rubber and modified natural rubber).

[0098] The adhesive sheet disclosed herein may have an acrylic adhesive layer composed of an acrylic adhesive. As the acrylic adhesive, for example, an acrylic polymer having a monomer composition mainly composed of an alkyl (meth)acrylate such as butyl (meth)acrylate or 2-ethylhexyl (meth)acrylate, and optionally a modifying monomer copolymerizable with the alkyl (meth)acrylate, as a base polymer (main component of the polymer components) can be preferably used. Examples of the modifying monomer include hydroxyl group-containing monomers such as 2-hydroxyethyl (meth)acrylate; carboxyl group-containing monomers such as (meth)acrylic acid; styrene-based monomers such as styrene; vinyl esters such as vinyl acetate; and the like. Such an acrylic adhesive can be obtained by a conventional polymerization method such as a solution polymerization method, an emulsion polymerization method, or an ultraviolet (UV) polymerization method.

[0099] The adhesive layer (e.g., rubber-based adhesive layer) may contain a laser beam absorbent as necessary. That is, the adhesive layer may be a laser beam absorbing layer. In an adhesive layer consisting of a plurality of layers, at least one of the layers may contain a laser beam absorbent. As the laser beam absorbent to be contained in the adhesive layer, one or more of the laser beam absorbents exemplified above may be appropriately selected and used. The content of the laser beam absorbent in the adhesive layer is usually 5% by weight or less of the adhesive layer, and from the viewpoint of adhesive performance, it is preferably 3% by weight or less, and may be 1% by weight or less. The technology disclosed herein may also be preferably implemented in an embodiment in which the adhesive layer does not substantially contain a laser beam absorbent.

[0100] The adhesive layer may contain a tackifier as necessary. As the tackifier, one or more selected from various tackifier resins such as known rosin resins, rosin derivative resins, petroleum resins (C5-based, C9-based, etc.), terpene resins, and ketone resins may be used. Examples of the rosin resins include rosins such as gum rosin, wood rosin, and tall oil rosin, as well as stabilized rosin, polymerized rosin, and modified rosin. Examples of the rosin derivative resins include esters of the rosin resins, phenol-modified products, and esters thereof. Examples of the petroleum resins include aliphatic petroleum resins, aromatic petroleum resins, copolymerized petroleum resins, alicyclic petroleum resins, and hydrogenated products thereof. Examples of the terpene resins include α-pinene resins, β-pinene resins, aromatic modified terpene resins, and terpene phenol resins. Examples of the ketone resins include ketone resins obtained by condensation of ketones and formaldehyde. Such tackifiers may be used alone or in combination of two or more. Among them, preferred tackifiers include rosin resins, rosin derivative resins, aliphatic (C5) petroleum resins, and terpene resins. These tackifier resins can be suitably used in, for example, a rubber-based adhesive layer, an acrylic-based adhesive layer, and the like.

[0101] The amount of the tackifier used (when two or more kinds are used, the total amount thereof) is usually about 20 to 150 parts by weight (preferably about 30 to 100 parts by weight) relative to 100 parts by weight of the base polymer. From the viewpoint of improving the high-speed peel strength, in some embodiments, the amount of the tackifier used may be, for example, 30 parts by weight or more, 40 parts by weight or more, or 45 parts by weight or more relative to 100 parts by weight of the base polymer. Also, from the viewpoint of avoiding the occurrence of adhesive residue due to a decrease in cohesive force, in some embodiments, the amount of the tackifier used relative to 100 parts by weight of the base polymer may be, for example, 85 parts by weight or less, or 75 parts by weight or less. In some embodiments, the amount of the tackifier used relative to 100 parts by weight of the base polymer may be, for example, less than 70 parts by weight, 65 parts by weight or less, 55 parts by weight or less, or 50 parts by weight or less. Reducing the amount of the tackifier used can be advantageous, for example, from the viewpoint of reducing the workload when peeling off the pressure-sensitive adhesive sheet from the adherend and preventing the pressure-sensitive adhesive sheet from tearing.

[0102] The pressure-sensitive adhesive layer can contain a crosslinking agent. The use of the crosslinking agent can impart an appropriate cohesive force to the pressure-sensitive adhesive layer. The pressure-sensitive adhesive layer containing the crosslinking agent can be obtained, for example, by forming the pressure-sensitive adhesive layer using a pressure-sensitive adhesive composition containing the crosslinking agent. The crosslinking agent can be contained in the pressure-sensitive adhesive layer in a form after crosslinking reaction, a form before crosslinking reaction, a form partially crosslinked, an intermediate or composite form thereof, or the like. The crosslinking agent is typically contained in the pressure-sensitive adhesive layer exclusively in a form after crosslinking reaction.

[0103] When a crosslinking agent is used, the amount of the crosslinking agent used can be, for example, in the range of 0.005 parts by weight or more and 10 parts by weight or less relative to 100 parts by weight of the base polymer. The amount of the crosslinking agent used relative to 100 parts by weight of the base polymer may be, for example, 0.01 parts by weight or more, 0.1 parts by weight or more, or 0.5 parts by weight or more. In addition, from the viewpoint of improving adhesion to the surface of the adherend (object to be processed), the amount of the crosslinking agent used relative to 100 parts by weight of the base polymer may be, for example, less than 5.0 parts by weight, less than 4.0 parts by weight, 3.5 parts by weight or less, or 2.5 parts by weight or less. The technology disclosed herein can also be suitably implemented in an embodiment in which the amount of the crosslinking agent used relative to 100 parts by weight of the base polymer is less than 2.0 parts by weight or 1.5 parts by weight or less.

[0104] Examples of crosslinking agents that can be used include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, silicone-based crosslinking agents, oxazoline-based crosslinking agents, aziridine-based crosslinking agents, silane-based crosslinking agents, alkyl etherified melamine-based crosslinking agents, metal chelate-based crosslinking agents, peroxides, and the like. Suitable examples of the crosslinking agents include isocyanate-based crosslinking agents and epoxy-based crosslinking agents. The crosslinking agents can be used alone or in combination of two or more. In some embodiments, isocyanate-based crosslinking agents can be preferably used. The isocyanate-based crosslinking agents can be used alone or in combination of two or more. The isocyanate-based crosslinking agents may be used in combination with other crosslinking agents, such as epoxy-based crosslinking agents.

[0105] As the isocyanate-based crosslinking agent, a compound having two or more isocyanate groups (including isocyanate regenerating functional groups in which the isocyanate group is temporarily protected by a blocking agent or oligomerization, etc.) in one molecule can be used. Examples of the isocyanate-based crosslinking agent include aromatic isocyanates such as tolylene diisocyanate and xylylene diisocyanate, alicyclic isocyanates such as isophorone diisocyanate, and aliphatic isocyanates such as hexamethylene diisocyanate.

[0106] More specifically, examples of the isocyanate-based crosslinking agent include lower aliphatic polyisocyanates such as butylene diisocyanate and hexamethylene diisocyanate, alicyclic isocyanates such as cyclopentylene diisocyanate, cyclohexylene diisocyanate and isophorone diisocyanate, aromatic diisocyanates such as 2,4-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, xylylene diisocyanate and polymethylene polyphenyl isocyanate, trimethylolpropane / tolylene diisocyanate trimer adduct (manufactured by Tosoh Corporation, product name: Coronate L), trimethylolpropane / hexamethylene diisocyanate trimer adduct (manufactured by Tosoh Corporation, product name: Coronate HL), and isocyanurate of hexamethylene diisocyanate (manufactured by Tosoh Corporation, product name: Coronate HL). Examples of the isocyanate adducts include isocyanate adducts such as (manufactured by Saw Co., Ltd., trade name: Coronate HX), trimethylolpropane adduct of xylylene diisocyanate (manufactured by Mitsui Chemicals, Inc., trade name: Takenate D110N), trimethylolpropane adduct of xylylene diisocyanate (manufactured by Mitsui Chemicals, Inc., trade name: Takenate D120N), trimethylolpropane adduct of isophorone diisocyanate (manufactured by Mitsui Chemicals, Inc., trade name: Takenate D140N), trimethylolpropane adduct of hexamethylene diisocyanate (manufactured by Mitsui Chemicals, Inc., trade name: Takenate D160N); polyether polyisocyanate, polyester polyisocyanate, and adducts of these with various polyols, polyisocyanates multifunctionalized with isocyanurate bonds, biuret bonds, allophanate bonds, etc. Among these, aromatic isocyanates and alicyclic isocyanates are preferably used.

[0107] The amount of the isocyanate crosslinking agent used may be, for example, about 0.1 parts by weight or more, about 0.5 parts by weight or more, about 1.0 parts by weight or more, or more than 1.5 parts by weight, relative to 100 parts by weight of the base polymer. From the viewpoint of obtaining a higher usage effect, in the pressure-sensitive adhesive layer according to some preferred embodiments, the amount of the isocyanate crosslinking agent used relative to 100 parts by weight of the base polymer may be, for example, more than 2.0 parts by weight, about 2.5 parts by weight or more, more than 2.5 parts by weight, or about 2.7 parts by weight or more. In addition, the amount of the isocyanate crosslinking agent used relative to 100 parts by weight of the base polymer may be, for example, 10 parts by weight or less, 7 parts by weight or less, or 5 parts by weight or less.

[0108] As the epoxy crosslinking agent, a polyfunctional epoxy compound having two or more epoxy groups in one molecule can be used. Examples of the epoxy crosslinking agent include N,N,N',N'-tetraglycidyl-m-xylylenediamine, diglycidylaniline, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, 1,6-hexanediol diglycidyl ether, neopentyl glycol diglycidyl ether, ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, sorbitol polyglycidyl ether, and the like. Examples of the epoxy crosslinking agent include glycerol polyglycidyl ether, pentaerythritol polyglycidyl ether, polyglycerol polyglycidyl ether, sorbitan polyglycidyl ether, trimethylolpropane polyglycidyl ether, adipic acid diglycidyl ester, o-phthalic acid diglycidyl ester, triglycidyl-tris(2-hydroxyethyl)isocyanurate, resorcinol diglycidyl ether, bisphenol-S-diglycidyl ether, and epoxy resins having two or more epoxy groups in the molecule. Examples of commercially available products of the epoxy crosslinking agent include "Tetrad C" and "Tetrad X" manufactured by Mitsubishi Gas Chemical Company, Inc.

[0109] The epoxy crosslinking agent may be used alone or in combination with two or more kinds. The epoxy crosslinking agent may be used alone or in combination with another crosslinking agent, for example, an isocyanate crosslinking agent. The amount of the epoxy crosslinking agent used may be, for example, about 0.005 to 5 parts by weight, may be 0.01 to 5 parts by weight, or may be 0.1 to 3 parts by weight, based on 100 parts by weight of the base polymer.

[0110] In addition, the pressure-sensitive adhesive layer may contain various additives, as necessary, that are common in the field of pressure-sensitive adhesives, such as crosslinking assistants, plasticizers, softeners, fillers, antistatic agents, antiaging agents, UV absorbers, antioxidants, light stabilizers, etc. As such additives, conventionally known ones can be used in the usual manner, and they do not particularly characterize the present invention, so detailed explanations will be omitted.

[0111] The method of providing such a pressure-sensitive adhesive layer on the first surface of the substrate is not particularly limited. For example, a method of forming a pressure-sensitive adhesive layer directly on a substrate by applying a pressure-sensitive adhesive composition (for example, a solution in which the pressure-sensitive adhesive layer-forming components are dissolved in an organic solvent, or a dispersion in which the components are dispersed in an aqueous solvent) containing a pressure-sensitive adhesive layer-forming component in a suitable medium to the substrate and drying or curing the composition, a method of transferring a pressure-sensitive adhesive layer formed on a surface having peelability to a substrate, a method of melting and heating the pressure-sensitive adhesive layer-forming components together with the substrate-forming components and laminating them by co-extrusion molding, and other known methods can be appropriately adopted. In order to form a pressure-sensitive adhesive layer constituting a pressure-sensitive adhesive sheet having a higher high-speed peel strength, a method of applying a pressure-sensitive adhesive composition can be preferably adopted from the viewpoint of ease of handling of the pressure-sensitive adhesive layer-forming components. The pressure-sensitive adhesive composition can be prepared, for example, by mixing a polymer component, typically a tackifier, other components used as necessary, and the medium by a conventional method. As a method of applying the pressure-sensitive adhesive composition, various conventionally known methods can be used. Specific examples of the coating method include roll coating, kiss roll coating, gravure coating, reverse coating, roll brushing, spray coating, dip roll coating, bar coating, knife coating, air knife coating, curtain coating, lip coating, and extrusion coating using a die coater or the like.

[0112] The thickness of the adhesive layer can be appropriately set so that appropriate adhesive performance is obtained depending on the application of the adhesive sheet. The thickness of the adhesive layer is usually appropriate to be 0.5 μm to 50 μm. From the viewpoint of improving adhesion to the adherend, in some embodiments, the thickness of the adhesive layer may be, for example, 1.5 μm or more, 3 μm or more, 5 μm or more, or 7 μm or more. The thickness of the adhesive layer may be, for example, 30 μm or less, 20 μm or less, 15 μm or less, or 10 μm or less. For example, in an adhesive sheet that can be used in an embodiment in which it is laser cut together with the adherend (work), a small thickness of the adhesive layer can be advantageous from the viewpoint of rapidity and precision of laser processing. The technology disclosed herein can also be preferably implemented in an embodiment of an adhesive sheet having an adhesive layer having a thickness of less than 10 μm or 8 μm or less.

[0113] <Roll body> According to this specification, a roll body including the adhesive sheet disclosed herein in a wound form can be provided. Such a roll body typically includes a core (winding core) and an adhesive sheet wound around the core. The shape of the core is not particularly limited, and may be, for example, a solid columnar shape, a hollow columnar shape (i.e., a cylindrical shape), a hollow or solid polygonal columnar shape, etc. From the viewpoint of improving the handleability of the roll body, a hollow columnar or hollow polygonal columnar core can be preferably adopted. A cylindrical core is particularly preferred.

[0114] The material constituting the core is not particularly limited, and known materials can be used. For example, paper such as cardboard, plastic materials such as PE resin, PP resin, vinyl chloride resin, polyester, epoxy resin, phenol resin, melamine resin, silicon resin, polyurethane, polycarbonate, acrylonitrile-butadiene-styrene copolymer resin (ABS resin), composite materials such as fiber reinforced plastic (FRP), metal materials such as iron, stainless steel (SUS), and aluminum, etc. can be mentioned.

[0115] The outer diameter of the core is not particularly limited. In some embodiments, the outer diameter of the core may be, for example, 30 mm or more, 50 mm or more, 70 mm or more, 80 mm or more, or 85 mm or more. For the purpose of improving productivity, etc., there is a demand to reduce the frequency of roll replacement by lengthening the laminated sheet contained in the roll body. In order to lengthen the laminated sheet contained in the roll body, it is advantageous to have a smaller outer diameter of the core. From this viewpoint, the outer diameter of the core is preferably, for example, 300 mm or less, may be 250 mm or less, 200 mm or less, or may be 180 mm or less. The technology disclosed herein can be suitably implemented in the embodiment of a roll body in which the outer diameter of the core is 150 mm or less, 100 mm or less, or even 95 mm or less. In addition, the diameter of the core refers to the diameter of the cross-sectional shape of a non-circular winding core, which is approximated by a circle.

[0116] In the case of a hollow core, the thickness of the core (i.e., the thickness of the outer wall) is not particularly limited and can be appropriately set so as to obtain a desired strength, taking into consideration the material and outer diameter of the core, etc. From the viewpoint of reducing the weight of the roll body, the thickness of the core is usually appropriate to be about 2 mm to 15 mm, and preferably about 3 mm to 10 mm.

[0117] The width of the adhesive sheet constituting the roll body disclosed herein is typically 5 mm or more, for example, 10 mm or more, preferably 20 mm or more, more preferably 30 mm or more, 50 mm or more, 150 mm or more, 300 mm or more, or 500 mm or more. When the width of the adhesive sheet is large, the peeling sound when the roll body of the adhesive sheet is unwound generally tends to be large. Therefore, it is particularly meaningful to suppress the generation of the peeling sound by applying the technology disclosed herein. In addition, from the viewpoint of handleability, etc., the width of the above-mentioned adhesive sheet is usually about 5 m or less, for example, about 4 m or less, about 3 m or less, about 2 m or less, or about 1 m or less.

[0118] In the pressure-sensitive adhesive sheet constituting the roll body disclosed herein, the high-speed unwinding force measured at a speed of 30 m / min is, for example, preferably 5 N / 20 mm or less, more preferably 4.5 N / 20 mm or less, and may be 4 N / 20 mm or less, from the viewpoint of easily reducing the fluctuation range of the back adhesive force. A small high-speed unwinding force can be advantageous from the viewpoint of reducing the labor required for unwinding and improving workability, and from the viewpoint of suppressing the pressure-sensitive adhesive sheet stretched during unwinding from shrinking after being attached to the adherend and causing lifting from the adherend. There is no particular limit to the lower limit of the high-speed unwinding force, but from the viewpoint of easily achieving a balance with other properties, it is, for example, preferably 0.5 N / 20 mm or more, more preferably 1 N / 20 mm or more, and may be 1.5 N / 20 mm or more. From the viewpoint of suppressing inconveniences such as being easily unwound excessively from the roll form, it is preferable that the high-speed unwinding force is not too small. The high-speed unwinding force can be measured in accordance with JIS Z0237:2009. The high-speed unwinding force can be adjusted, for example, by selecting the type of adhesive in the adhesive layer, the type and amount of crosslinking agent used, the type and treatment method of release agent, and the use of optional components such as tackifier resins.

[0119] <Application> The adhesive sheet disclosed herein has high high-speed peel strength, suppresses the peeling sound when the surface of the adhesive layer is exposed prior to application to an adherend, and does not slip too much even when it is applied to a metal plate or the like and stacked on top of it, and can be suitably used, for example, as a surface protection material (which can also be understood as an adhesive sheet for surface protection). The adhesive sheet disclosed herein can be used, for example, for applications such as attaching to the surface of a metal plate, a painted plate, an aluminum sash, a resin plate, a decorative steel plate, a vinyl chloride laminated steel plate, a glass plate, an optical film for liquid crystal such as a polarizing film, an optical member such as a liquid crystal panel, an electronic member, etc., when transporting, processing, or curing these members.

[0120] The adhesive sheet disclosed herein can be preferably used as one aspect of surface protection in a state where it is attached to a workpiece to be processed by various lasers and is laser cut in association with the laser processing of the workpiece. The laser light used in the above-mentioned laser processing is not particularly limited, and various conventionally known lasers can be adopted. For example, excimer lasers such as ArF excimer laser, KrF excimer laser, and XeCl excimer laser, solid-state lasers such as YAG laser, YLF laser, YVO4 laser, and titanium sapphire laser, semiconductor laser (sometimes called diode laser), fiber laser, carbon dioxide laser, etc. can be used. The type of laser processing performed on the workpiece with the adhesive sheet disclosed herein attached is not particularly limited, and can be, for example, cutting, drilling, cutting, engraving, etc.

[0121] The material of the workpiece is not particularly limited as long as it can be cut by laser light (for example, laser light of a carbon dioxide gas laser or a fiber laser), and may be, for example, metal or semimetal materials such as iron, iron alloys (carbon steel, stainless steel, chromium steel, nickel steel, etc.), aluminum, aluminum alloys, nickel, tungsten, copper, copper alloys, titanium, titanium alloys, silicon, etc.; resin materials such as polyolefin resins, polycarbonate resins, acrylic resins, etc.; ceramic materials such as alumina, silica, sapphire, silicon nitride, tantalum nitride, titanium carbide, silicon carbide, gallium nitride, gypsum, etc.; glass materials such as aluminosilicate glass, soda lime glass, soda aluminosilicate glass, quartz glass, etc.; cellulose-based materials such as paper, cardboard, wood, plywood, etc.; laminates or composites thereof; etc. Suitable examples of the workpiece include metal materials such as iron, aluminum, copper, titanium, and alloys (stainless steel, etc.) mainly composed of each of these metals. The shape of the workpiece is not particularly limited, and may be plate-shaped, cylindrical, block-shaped, etc. The adhesive sheet disclosed herein is preferable because it suppresses lateral slippage even when attached to a metal plate as a workpiece and then stacked.

[0122] The adhesive sheet disclosed herein can be preferably used in such laser processing in a state where it is attached to the surface of the workpiece on the laser light irradiation side. In addition, for the purpose of protecting the surface of the workpiece before and after laser processing or during laser processing, the adhesive sheet may be attached to the surface (back side) of the workpiece opposite to the laser light irradiation side. The adhesive sheet disclosed herein can be preferably used in such laser processing by a short-wavelength laser having a main wavelength of 900 to 1100 nm. As the short-wavelength laser, for example, a fiber laser having a main wavelength of about 1050 nm, a diode laser having a main wavelength of about 950 nm, etc. can be used.

[0123] The matters disclosed in this specification include the following. (1) A pressure-sensitive adhesive sheet comprising a resin film as a substrate and a pressure-sensitive adhesive layer provided on a first surface of the substrate, a second surface of the substrate is a release surface; The slip resistance value of the second surface is 3.5N or more, The high-speed peel strength measured at a tensile speed of 30 m / min after 30 minutes of application to a stainless steel plate is 4.5 N / 20 mm or more. An adhesive sheet in which the difference between the maximum and minimum adhesive strength of its own back surface measured at a tensile speed of 30 m / min is 1.5 N / 20 mm or less. (2) The pressure-sensitive adhesive sheet according to (1) above, wherein the second surface of the substrate is made of a resin composition containing a release agent. (3) The pressure-sensitive adhesive sheet according to (2) above, wherein the release agent comprises a silicone-based release agent. (4) The pressure-sensitive adhesive sheet according to (3) above, wherein the silicone-based release agent contains a silylated polyolefin. (5) The pressure-sensitive adhesive sheet according to any one of (2) to (4) above, wherein the substrate and a resin composition containing the release agent are integrally formed by coextrusion molding. (6) The pressure-sensitive adhesive sheet according to any one of (1) to (5) above, wherein the pressure-sensitive adhesive layer is made of a natural rubber-based pressure-sensitive adhesive. (7) The pressure-sensitive adhesive sheet according to any one of (1) to (6) above, wherein the average adhesive strength to the back surface of the sheet is 1 N / 20 mm or more and 5 N / 20 mm or less. (8) The pressure-sensitive adhesive sheet according to any one of (1) to (7) above, which has a low-speed peel strength of 5 N / 20 mm or less when measured 30 minutes after attachment to a stainless steel plate at a tensile speed of 0.3 m / min. (9) The pressure-sensitive adhesive sheet according to any one of (1) to (8) above, wherein the substrate is a polyolefin resin film or a polyester resin film. (10) The pressure-sensitive adhesive sheet according to any one of (1) to (9), wherein the substrate includes a back layer made of a resin composition containing the release agent, and a support layer disposed on the inner side of the back layer. (11) The pressure-sensitive adhesive sheet according to (10) above, wherein the support layer is a polyolefin resin layer or a polyester resin layer.

[0124] (12) A pressure-sensitive adhesive sheet comprising a resin film as a substrate and a pressure-sensitive adhesive layer provided on a first surface of the substrate, the second surface of the substrate is a release surface constituted by a resin composition containing a release agent; The substrate includes a back surface layer made of a resin composition containing the release agent, and a support layer disposed on the inner side of the back surface layer, The release agent comprises a silylated polyolefin; The support layer is a polyolefin resin layer or a polyester resin layer, The pressure-sensitive adhesive sheet, wherein the pressure-sensitive adhesive layer is made of a natural rubber-based pressure-sensitive adhesive. (13) The pressure-sensitive adhesive sheet according to (12) above, wherein the substrate and a resin composition containing the release agent are integrally formed by coextrusion molding. (14) The pressure-sensitive adhesive sheet according to (12) or (13) above, wherein the substrate comprises a back layer made of a resin composition containing the release agent, and a support layer disposed on the inside of the back layer. (15) The pressure-sensitive adhesive sheet according to any one of (12) to (14) above, which has a high-speed peel strength of 4.5 N / 20 mm or more when measured 30 minutes after attachment to a stainless steel plate at a tensile speed of 30 m / min. (16) The pressure-sensitive adhesive sheet according to any one of (12) to (15) above, in which the difference between the maximum and minimum values ​​of the adhesive strength on its back surface measured at a tensile speed of 30 m / min is 1.5 N / 20 mm or less. (17) The pressure-sensitive adhesive sheet according to any one of (12) to (16) above, wherein the second surface has a slip resistance value of 3.5 N or more.

[0125] (18) A pressure-sensitive adhesive sheet comprising the pressure-sensitive adhesive sheet according to any one of (1) to (17) above, which is used as a surface protective material. (19) The pressure-sensitive adhesive sheet according to any one of (1) to (18) above, which is used by being cut with laser light. (20) The pressure-sensitive adhesive sheet according to any one of (1) to (19) above, wherein the substrate contains a laser beam absorbent. (21) The pressure-sensitive adhesive sheet according to (20) above, wherein the laser beam absorbent comprises at least one selected from the group consisting of carbon black, titanium oxide, iron-based oxides, titanium black and manganese-based oxides. (22) The pressure-sensitive adhesive sheet according to any one of (1) to (21) above, which is used by being cut with a laser beam having a dominant wavelength of 900 nm to 1100 nm. (23) The pressure-sensitive adhesive sheet according to any one of (1) to (22) above, wherein the pressure-sensitive adhesive layer contains a tackifier. (24) The pressure-sensitive adhesive sheet according to (23) above, wherein the tackifier comprises at least one selected from the group consisting of rosin-based resins, rosin derivative resins, aliphatic (C5-based) petroleum resins, and terpene resins. (25) The pressure-sensitive adhesive sheet according to (23) or (24) above, wherein the pressure-sensitive adhesive layer contains less than 70 parts by weight of a tackifier per 100 parts by weight of the base polymer. (26) The pressure-sensitive adhesive sheet according to any one of (1) to (25) above, wherein the pressure-sensitive adhesive layer has a thickness of less than 10 μm.

[0126] (27) Preparing an object to be processed to which the pressure-sensitive adhesive sheet according to any one of (1) to (26) above is attached; and Irradiating the object to be processed with a laser beam having a dominant wavelength of 900 nm to 1100 nm to cut the adhesive sheet with the laser beam, thereby laser processing the object to be processed and cutting the adhesive sheet with the laser beam; A method for producing a laser processed article, comprising: (28) The method according to (27) above, wherein the workpiece to be irradiated with the laser light has the adhesive sheet affixed to at least one of the surface of the workpiece to be irradiated with the laser light and the opposite surface of the workpiece. (29) further post-processing the object after the laser processing; and Peeling and removing the adhesive sheet from the object to be processed; The method according to (27) or (28) above, comprising, in this order: (30) The method according to any one of (27) to (29) above, wherein the object is a metal plate. (31) A roll comprising the pressure-sensitive adhesive sheet according to any one of (1) to (26) above, wound so that the pressure-sensitive adhesive layer is in contact with the second surface of the substrate. (32) The roll body according to (31) above, wherein a high-speed unwinding force is 1 N / 20 mm or more and 5 N / 20 mm or less. EXAMPLES

[0127] Several examples of the present invention will be described below, but it is not intended that the present invention be limited to those specific examples. In the following description, "parts" and "%" are based on weight unless otherwise specified. In addition, unless otherwise specified, the amount of each material used is based on the amount of active ingredient.

[0128] In each of the following examples, the raw materials used to prepare the pressure-sensitive adhesive sheets are as follows. Adhesive composition P1: 100 parts of natural rubber was mixed with 45 parts of a tackifier (manufactured by Zeon Corporation, product name "Quintone A100"), 2 parts of an antioxidant (manufactured by Ouchi Shinko Chemical Industry Co., Ltd., product name "Nocrac NS-5"), 3 parts of an isocyanate-based crosslinking agent (manufactured by Tosoh Corporation, product name "Coronate L"), and toluene. Adhesive composition P2: 100 parts of natural rubber was mixed with 70 parts of a tackifier (manufactured by Zeon Corporation, product name "Quintone A100"), 2 parts of an antioxidant (manufactured by Ouchi Shinko Chemical Industry Co., Ltd., product name "Nocrac NS-5"), 3 parts of an isocyanate-based crosslinking agent (manufactured by Tosoh Corporation, product name "Coronate L"), and toluene.

[0129] <Preparation of adhesive sheet> Example 1 A support layer forming material consisting of 3 parts of a black master batch (hereinafter also referred to as Fe3O4 master batch) containing 40% Fe3O4 (iron tetraoxide powder with an average particle size of 250 nm) in polyolefin and 97 parts of LDPE (low-density polyethylene, manufactured by Tosoh Corporation, product name "Petrothene 186R"), and a back layer forming material consisting of 96 parts of the support layer forming material and 4 parts of a silylated polyolefin master batch containing about 30% of a silylated polyolefin (prepared by the method shown in the example of JP 2011-26448 A) as a silicone-based release agent and about 70% of PE resin (the content of the silicone-based release agent in the back layer forming material is 1.2%) were co-extruded by an inflation molding method at a die temperature of 180°C to form a film, thereby obtaining a two-layered resin film F1 consisting of a support layer and a back layer. The total thickness of this resin film F1 was 80 μm, of which the thickness of the back layer was 8 μm. The first surface (non-release surface) of the resin film F1 was subjected to a corona discharge treatment, and the corona discharge treated surface was coated with the pressure-sensitive adhesive composition P1 and dried to form a 5 μm thick pressure-sensitive adhesive layer. In this way, a pressure-sensitive adhesive sheet was obtained having a pressure-sensitive adhesive layer on the first surface of the substrate and a second surface of the substrate serving as a release surface.

[0130] (Examples 2 to 5) Resin films F2 to F5 were obtained in the same manner as for resin film F1, except that the content of the silylated polyolefin master batch in the back layer forming material was changed as shown in Table 1. Pressure-sensitive adhesive sheets according to Examples 2 to 5 were obtained in the same manner as for example 1, except that resin films F2 to F5 were used instead of resin film F1, respectively.

[0131] Example 6 An adhesive sheet according to this example was obtained in the same manner as in Example 1, except that adhesive composition P2 was used instead of adhesive composition P1 and the thickness of the adhesive layer was set to 10 μm.

[0132] (Examples 7 and 8) Pressure-sensitive adhesive sheets according to Examples 7 and 8 were obtained in the same manner as in Example 6, except that resin film F1 was replaced by resin films F2 and F3, respectively.

[0133] Comparative Example 1 The first surface (the surface other than the release surface) of the resin film F2 obtained in the same manner as in Example 2 was subjected to a corona discharge treatment, and a 10 μm-thick rubber-based adhesive layer having a styrene-ethylene / butylene-styrene block copolymer (SEBS) as the base polymer was formed on the corona discharge-treated surface to obtain an adhesive sheet according to this example.

[0134] Comparative Example 2 The first surface (the surface other than the release surface) of the resin film F2 obtained in the same manner as in Example 2 was subjected to a corona discharge treatment, and the following acrylic adhesive composition was applied to the corona discharge treated surface and dried to form an acrylic adhesive layer having a thickness of 10 μm, thereby obtaining the adhesive sheet of this example. Acrylic adhesive composition: Ethyl acetate as a polymerization solvent, 96 parts of 2-ethylhexyl acrylate (2EHA) and 4 parts of acrylic acid (AA) as monomer raw materials, and 0.2 parts of AIBN as a polymerization initiator were added and subjected to a polymerization reaction under a nitrogen gas flow. The resulting ethyl acetate solution of the acrylic polymer (concentration 40%, Mw of the acrylic polymer = 50 × 10 4) and 1 part of an isocyanate-based crosslinking agent (manufactured by Tosoh Corporation, product name "Coronate L") was added for every 100 parts of non-volatile matter contained in the solution and mixed.

[0135] Comparative Example 3 The base layer forming material obtained in the same manner as in Example 1 was formed into a film by inflation molding at a die temperature of 180°C to obtain a resin film F6 having a single layer structure and a thickness of 90 μm. One side (first side) of the resin film F6 was subjected to a corona discharge treatment, and the pressure-sensitive adhesive composition P1 was applied to the corona discharge treated side and dried to form a pressure-sensitive adhesive layer having a thickness of 5 μm. A UV-curable solventless silicone-based release agent was applied to the other side (second side) of the resin film F6. The application amount of the release agent was 1.3 g / m 2 After applying the above-mentioned release agent, the illuminance was 2W / cm 2 The release agent was cured by irradiating it with ultraviolet light from a high pressure mercury lamp as a light source under the conditions of a line speed of 70 m / min, thereby forming a back surface treatment layer. In this manner, a pressure-sensitive adhesive sheet according to this example was obtained.

[0136] Comparative Example 4 Resin film F6 was obtained in the same manner as in Comparative Example 3. One side (first side) of resin film F6 was subjected to corona discharge treatment, and pressure-sensitive adhesive composition P2 was applied to the corona discharge-treated side and dried to form a pressure-sensitive adhesive layer having a thickness of 10 μm. A reaction product of polyvinyl alcohol and octadecyl isocyanate as an alkyl-based release agent was applied to the other side (second side) of resin film F6 so that the film thickness after drying was 0.05 μm to form a back treatment layer. In this manner, a pressure-sensitive adhesive sheet according to this example was obtained.

[0137] In addition, the pressure-sensitive adhesive sheets according to the examples and comparative examples all had a specific laser light transmittance in the range of 20 to 40% at wavelengths where the laser light absorptance was minimum in the wavelength range of 900 nm to 1100 nm. Also, the specific laser light reflectance in the wavelength where the laser light absorptance was minimum was in the range of 3 to 10%. The minimum laser light absorptance in the wavelength range of 900 nm to 1100 nm was in the range of 60 to 70%. The lightness L of the back surface of the pressure-sensitive adhesive sheet *The chromaticity of the back of the adhesive sheet is in the range of 20 to 35. * are all in the range of 0 to +1, and the chromaticity b * were all in the range of 0 to +1.

[0138] <Performance evaluation> A sample of an appropriate size was cut from the pressure-sensitive adhesive sheet prepared above, and the following items were evaluated. The results are shown in Table 1.

[0139] (1) High-speed peel strength The adhesive sheet according to each example was cut into a strip of 20 mm width and 100 mm length to prepare a test piece. The adhesive surface of the test piece was pressed against a stainless steel plate (SUS430BA) as an adherend by rolling it back and forth once with a 2 kg rubber roller as specified in JIS Z0237. The sample was left in a standard environment of 23°C x 50% RH for 30 minutes, and then the high-speed peel strength (N / 20 mm) was measured under the standard environment at a tensile speed of 30 m / min and a peel angle of 180° using a universal tensile tester.

[0140] (2) Low-speed peel strength The adhesive sheet according to each example was cut into a strip of 20 mm wide and 100 mm long to prepare a test piece. The adhesive surface of the test piece was pressed against a stainless steel plate (SUS430BA) as an adherend by rolling it back and forth once with a 2 kg rubber roller as specified in JIS Z0237. The sample was left in a standard environment of 23°C x 50% RH for 30 minutes, and then the low-speed peel strength (N / 20 mm) was measured under the standard environment with a universal tensile tester at a tensile speed of 0.3 m / min and a peel angle of 180 degrees.

[0141] (3) Self-back adhesive strength A long resin film with a width of 1000 mm was used as the substrate in each example, and the adhesive composition according to each example was applied to the center of the width of the substrate in a width of about 930 mm and dried to prepare a long adhesive sheet. Both ends of the adhesive sheet were cut inside the width of the adhesive layer (having a thickness corresponding to each example) formed from the adhesive composition to prepare a sample for making a roll body with a width of 300 mm and a length of about 1000 m. A cylindrical core having an outer diameter of 90.2 mm and an axial length of 305 mm was prepared. One end of the sample in the longitudinal direction (the winding start end) was fixed to the outer peripheral surface of the core with a commercially available adhesive tape so that the adhesive layer side of the sample for preparing a roll was on the inner peripheral side, and the remaining part of the sample was wound around the core with a winding tension of about 200 N / m to prepare a roll. The roll body prepared above was stored for 28 days in a room at 30° C., and then about 50 cm of the adhesive sheet was unwound and removed from the end of the roll. Next, two slits were made at 20 mm intervals along the outer periphery of the remaining roll body, extending along the axial direction of the roll, and about three adhesive sheets (i.e., about three laps) located between the slits were laminated, and the innermost adhesive sheet was peeled off from its back surface to obtain an adhesive sheet laminate (sample for self-back surface peeling test) having a width of 20 mm and a length of 300 mm. The adhesive surface exposed on the inner circumference side of the above-mentioned adhesive sheet laminate was backed by attaching a SUS304 plate (BA finish), and left for 30 minutes under a standard environment of 23°C x 50% RH. Then, under the standard environment, a universal tensile tester was used to peel the first adhesive sheet from the outer circumference side of the above-mentioned adhesive sheet laminate from the back surface of the second adhesive sheet from the outer circumference side at a tensile speed of 30 m / min and a peel angle of 180 degrees. At this time, adhesive strength data was obtained every 0.25 mm of peel distance. For the adhesive strength data obtained within the peel distance range of 20 mm to 70 mm, the difference between the maximum and minimum values ​​of the adhesive strength on the back surface and the average value of the adhesive strength on the back surface were obtained, and the obtained results are shown in the "adhesive strength on the back surface fluctuation range" and "average adhesive strength on the back surface" columns of Table 1, respectively.

[0142] (4) Processability A 3.0 mm thick SUS304 plate (2B finish) was used as the workpiece, and the adhesive sheet according to each example was attached to the top surface of the workpiece. A cutting test was performed by irradiating a laser beam from the top side of this workpiece. Specifically, a fiber laser processing machine (Trumpf, Trulaser 5030, main wavelength 1050 nm) was used to perform straight line cutting under the following conditions. [Laser processing conditions] Cutting speed: 5.0m / min Output: 3000W Supply gas and gas pressure: Nitrogen gas, pressure 18 bar Nozzle diameter: 2.0mm Nozzle height: 2mm Laser beam focus: 1.5 mm below the top surface of the workpiece

[0143] The edges of the workpiece that had been laser processed (laser cut in this case) were then visually inspected. If the workpiece could be cut under the above conditions without any lifting or peeling of the adhesive sheet, it was rated as having good processability (G); if the workpiece could be cut but any lifting or peeling of the adhesive sheet was observed, it was rated as having poor processability (NG).

[0144] (5) Noise A roll body was obtained in which a long adhesive sheet having a width of 200 mm according to each example was wound in the same manner as in the preparation of a roll body for obtaining a sample for the self-backside peeling test, except that the width of the adhesive sheet to be cut was 200 mm. The sound volume when the adhesive sheet was unwound from this roll body at a pulling speed of about 30 m / min and a peeling angle of about 90° was measured using a sound level meter (manufactured by Rion Co., Ltd., SOUND LEVEL METER NL-27) installed at a position about 10 cm horizontally away from the unwound roll body, and a sound level of less than 100 dB was evaluated as good (G) in noise quality, and a sound level of 100 dB or more was evaluated as poor (NG) in noise quality. It is generally known that a sound level of 100 dB or more is a level that causes abnormalities in the hearing function.

[0145] (6)Slip resistance value A sample plate was prepared by attaching the adhesive sheet according to each example to the upper surface of a SUS304 plate (2B finish) having a thickness of 3.0 mm, a length of 300 mm, and a width of 200 mm, while being careful not to trap air bubbles. The adhesive sheet was attached so that the longitudinal direction (MD) of the resin film used as the substrate was parallel to the length direction of the sample plate. Made of SUS304 plate (BA finish) with a contact area of ​​25cm 2 A load was placed on a square slider (50 mm on each side), and the total load including the weight of the slider was 1.0 kg. The slider was placed on the sample plate (i.e., on the back surface of the adhesive sheet), and the kinetic friction force (N) was measured using an autograph (AG-ISD, manufactured by Shimadzu Corporation) when the slider was slid in the length direction of the sample plate at a pulling speed of 300 mm / min under a standard environment of 23°C x 50% RH. The average value obtained for the sliding resistance value data obtained in the sliding distance range of 100 mm to 200 mm is shown in the "Sliding resistance value" column of Table 1.

[0146] (7) Slipperiness A number of sample plates were prepared by attaching the adhesive sheet according to each example to the top surface of a SUS304 plate (2B finish) with a thickness of 3.0 mm, length of 300 mm, and width of 200 mm. Ten sample plates were stacked horizontally so that the top surface (the surface with the adhesive sheet attached) and the back surface (the SUS plate surface) of the sample plates were in contact with each other, and the state of the topmost sample plate was visually observed when it was lightly pressed horizontally by hand. When the sample plate was pressed, if no lateral shifting of the stacked sample plates was observed, it was rated as good (G), and when the sample plate slid sideways with almost no resistance when pressed and lateral shifting of the stacked sample plates was observed, it was rated as poor (NG).

[0147] (8) Adhesive residue (adhesive residue test after bending) The surface of a 0.6 mm thick SUS304 plate (2B finish) used as the adherend was wiped with a rag soaked in toluene, and then the adhesive sheet of each example was bonded to it using a laminator (linear pressure 40 N / cm, speed 3 m / min). The plate was left at room temperature for at least 30 minutes, and then bent 90° so that the adhesive sheet side was convex. The adhesive sheet was then peeled off at a pulling speed of approximately 0.3 m / min and a peel angle of approximately 180 degrees, and the surface condition of the adherend was visually observed. If no adhesive residue was observed on the adherend's surface, it was rated as good (G), and if adhesive residue was observed, it was rated as poor (NG).

[0148] [Table 1]

[0149] As shown in Table 1, the adhesive sheets of Examples 1 to 8 could be cut without lifting or peeling when the adhesive sheet was used to process a workpiece with a fiber laser. These adhesive sheets also had good noise characteristics when peeled off from their own back surfaces, and side slippage was suppressed when the SUS plates to which the adhesive sheets were attached were placed on top of each other. On the other hand, in the adhesive sheets of Comparative Examples 1 and 2, which had a high-speed peel strength of 4.5 N / 20 mm or less, lifting and peeling of the adhesive sheet was observed during fiber laser processing. In addition, in the adhesive sheet of Comparative Example 3, which had a slip resistance value of less than 3.5 N, side slippage was likely to occur when the SUS plates to which the adhesive sheets were attached were placed on top of each other. The adhesive sheet of Comparative Example 4, in which the difference between the maximum and minimum values ​​of the adhesive strength of the own back surface exceeded 1.5 N / 20 mm, made a large noise when peeling off the adhesive sheet from its own back surface, and there was concern that the working environment would deteriorate in terms of noise when used.

[0150] Although specific examples of the present invention have been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and changes of the specific examples exemplified above. [Explanation of symbols]

[0151] 1,2 Adhesive sheet 10 Resin film (base material) 10A front page 10B Second surface (back, peeling surface) 11 Back layer 12 Support layer 20 Adhesive layer 20A surface (adhesive surface) 50 roll 52 cores

Claims

1. A pressure-sensitive adhesive sheet comprising a resin film as a substrate and a pressure-sensitive adhesive layer provided on a first surface of the substrate, a second surface of the substrate is a release surface; The second surface has a slip resistance value of 3.5 N or more; The adhesive constituting the adhesive layer is a natural rubber-based adhesive, The pressure-sensitive adhesive layer contains less than 70 parts by weight of a tackifier relative to 100 parts by weight of a base polymer, The substrate includes a back layer constituting the second surface and a support layer constituting the first surface, The back layer is made of a resin composition containing a release agent, The release agent comprises a silicone-based release agent, The silicone-based release agent comprises a silylated polyolefin, The high-speed peel strength measured 30 minutes after application to a stainless steel plate at a tensile speed of 30 m / min is 4.5 N / 20 mm or more, A pressure-sensitive adhesive sheet, the difference between the maximum and minimum values ​​of its own backside adhesive strength measured under the condition of a tensile speed of 30 m / min, being 1.5 N / 20 mm or less.

2. The pressure-sensitive adhesive sheet according to claim 1 , wherein the average adhesive strength of the back surface is 1 N / 20 mm or more and 5 N / 20 mm or less.

3. 3. The pressure-sensitive adhesive sheet according to claim 1, which has a low-speed peel strength of 5 N / 20 mm or less when measured 30 minutes after application to a stainless steel plate at a tensile speed of 0.3 m / min.

4. The pressure-sensitive adhesive sheet according to claim 1 , wherein the substrate is a polyolefin resin film or a polyester resin film.

5. The pressure-sensitive adhesive sheet according to claim 1 , which is used by being cut with laser light.

6. The pressure-sensitive adhesive sheet according to claim 1 , wherein the substrate contains a laser beam absorbent.

7. The pressure-sensitive adhesive sheet according to claim 6 , wherein the laser beam absorbent comprises at least one selected from the group consisting of carbon black, titanium oxide, iron-based oxides, titanium black, and manganese-based oxides.

8. The pressure-sensitive adhesive sheet according to any one of claims 1 to 7, which is used by being cut with a laser beam having a dominant wavelength of 900 nm to 1100 nm.

9. A roll comprising the pressure-sensitive adhesive sheet according to claim 1 in a rolled form such that the pressure-sensitive adhesive layer is in contact with the second surface of the substrate.

Citation Information

Patent Citations

  • Surface protective film

    JP2008080626A

  • Rubber-based adhesive tape

    JP2017200977A

  • Self-adhesive film

    JP2019059879A

  • Adhesive film

    WO2018159591A1