Adhesive composition for organic fiber cord, rubber reinforcing material and its manufacturing method, and rubber article
A graft copolymer-based adhesive composition for organic fiber cords addresses the environmental concerns of resorcinol and formaldehyde by providing superior adhesion without these chemicals, enhancing safety and sustainability.
Patent Information
- Application Number
- JP2022532405
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-06-19
- Filing Date
- 2021-05-19
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-05-19
AI Technical Summary
Existing adhesive compositions for organic fiber cords, such as those used in tire cords, rely on resorcinol and formaldehyde, which are suspected carcinogens and endocrine disruptors, necessitating a shift towards environmentally friendly alternatives without compromising adhesive properties.
A graft copolymer derived from chloroprene polymer and ethylenically unsaturated carboxylic acid, combined with a surfactant, forms an adhesive composition with a specific molar ratio of oxygen to chlorine atoms and solid content concentration, eliminating the need for resorcinol and formaldehyde.
The adhesive composition achieves excellent adhesive properties while reducing environmental impact by eliminating resorcinol and formaldehyde, thereby minimizing health and environmental hazards.
Smart Images

Figure 0007559065000001 
Figure 0007559065000002
Abstract
Description
[Technical field]
[0001] The present invention relates to an adhesive composition for organic fiber cords, a rubber reinforcing material and a method for producing the same, and a rubber article. [Background technology]
[0002] Conventionally, a resorcinol-formaldehyde-latex (RFL) adhesive containing resorcinol, formaldehyde, and rubber latex has been used to bond a tire cord made of nylon fiber or the like to a rubber composition for tires, and a technique for ensuring adhesive strength by thermal curing of the adhesive is known (see, for example, Patent Documents 1 to 3 below). Also known is a technique using an initial condensation product of resorcinol and formaldehyde (see, for example, Patent Documents 4 and 5 below). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 58-2370 [Patent Document 2] Japanese Patent Application Publication No. 60-92371 [Patent Document 3] Japanese Patent Application Publication No. 60-96674 [Patent Document 4] Japanese Patent Application Publication No. 63-249784 [Patent Document 5] Special Publication No. 63-61433 Summary of the Invention [Problem to be solved by the invention]
[0004] Although formaldehyde is an important raw material for crosslinking resorcinol, it is suspected to be carcinogenic, and therefore in recent years, in consideration of the environmental load (especially the work environment load), there has been a demand to suppress its release into the atmosphere during use and to reduce its usage. In addition, resorcinol is suspected to be an environmental hormone, and there has been a demand to reduce its usage. Therefore, adhesive compositions used for organic fiber cords such as tire cords are required to have excellent adhesion without using resorcinol and formaldehyde.
[0005] An object of one aspect of the present invention is to provide an adhesive composition for organic fiber cords having excellent adhesion without using resorcinol and formaldehyde.Another object of the present invention is to provide a rubber reinforcing material using the adhesive composition and a method for producing the same.Another object of the present invention is to provide a rubber article including the rubber reinforcing material. [Means for solving the problem]
[0006] As a result of extensive investigations, the present inventors have found that an adhesive composition containing a graft copolymer in which an ethylenically unsaturated carboxylic acid is grafted onto a chloroprene polymer and a surfactant, wherein the molar ratio of the oxygen atom content to the chlorine atom content in the graft copolymer and the solids concentration are within specific ranges, can solve the above-mentioned problems when an organic fiber cord is used, and have completed the present invention.
[0007] One aspect of the present invention provides an adhesive composition for organic fiber cords, comprising a graft copolymer and a surfactant, wherein the graft copolymer has a chloroprene polymer chain and a graft chain that is bonded to the chloroprene polymer chain and contains a structural unit derived from an ethylenically unsaturated carboxylic acid, the molar ratio of the oxygen atom content to the chlorine atom content in the graft copolymer is 0.04 to 1, and the adhesive composition has a solids concentration of 10 to 50 mass %.
[0008] Another aspect of the present invention provides a rubber reinforcing material comprising: the adhesive composition described above; an organic fiber cord; and a rubber member adhered to the organic fiber cord via the adhesive composition.
[0009] Another aspect of the present invention provides a method for producing a rubber reinforcing material, comprising a step of adhering an organic fiber cord and a rubber member via the above-mentioned adhesive composition.
[0010] Another aspect of the present invention provides a rubber article comprising the rubber reinforcement described above. Effect of the Invention
[0011] According to one aspect of the present invention, an adhesive composition for organic fiber cords having excellent adhesion without using resorcin and formaldehyde can be provided. In this case, since resorcin and formaldehyde are not used, the environmental load (particularly the load on the working environment) can be reduced. According to another aspect of the present invention, a rubber reinforcing material using the adhesive composition and a method for producing the same can be provided. According to another aspect of the present invention, a rubber article including the rubber reinforcing material can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will be described in detail below. The embodiment described below is an example of a typical embodiment of the present invention, and the scope of the present invention is not to be construed as being narrow.
[0013] In this specification, the numerical range indicated by "~" indicates a range including the numerical values described before and after "~" as the minimum and maximum values, respectively. The numerical range "A or more" means a range exceeding A and A. The numerical range "A or less" means a range less than A and A. In the numerical ranges described in stages in this specification, the upper limit or lower limit of a numerical range of a certain stage can be arbitrarily combined with the upper limit or lower limit of a numerical range of another stage. In the numerical ranges described in this specification, the upper limit or lower limit of the numerical range may be replaced with a value shown in the examples. "A or B" may include either A or B, or may include both. Unless otherwise specified, the materials exemplified in this specification may be used alone or in combination of two or more types. When a plurality of substances corresponding to each component are present in the composition, the content of each component in the composition means the total amount of the plurality of substances present in the composition, unless otherwise specified. "(Meth)acrylic acid" means at least one of acrylic acid and the corresponding methacrylic acid. The same applies to other similar expressions such as "(meth)acrylate."
[0014] <Adhesive composition> The adhesive composition according to this embodiment is an adhesive composition for organic fiber cords (adhesive composition for organic fiber cords) containing a graft copolymer P and a surfactant. The graft copolymer P has a chloroprene polymer chain (polychloroprene chain) and a graft chain that is bonded to the chloroprene polymer chain and contains a structural unit derived from an ethylenically unsaturated carboxylic acid (ethylenically unsaturated carboxylic acid), the molar ratio of the oxygen atom content to the chlorine atom content in the graft copolymer P is 0.04 to 1, and the solid content concentration of the adhesive composition is 10 to 50 mass%.
[0015] According to the adhesive composition of this embodiment, when an organic fiber cord is used, excellent adhesion can be obtained without using resorcin and formaldehyde. According to the adhesive composition of this embodiment, since resorcin and formaldehyde are not used, the environmental load (particularly the load on the working environment) can be reduced. According to the adhesive composition of this embodiment, it is also possible to obtain superior adhesion to the case where resorcin and formaldehyde are used.
[0016] The adhesive composition according to the present embodiment may be an embodiment that does not contain resorcin and formaldehyde, and the content of each of resorcin and formaldehyde may be substantially 0 mass% based on the total amount of the adhesive composition (solid content equivalent). The adhesive composition according to the present embodiment may contain a liquid component such as water (for example, a component that is liquid at 23°C). The adhesive composition according to the present embodiment can be used as a water-based adhesive (water-based adhesive composition). The adhesive composition according to the present embodiment may be an embodiment that does not contain an organic solvent, and the content of the organic solvent may be substantially 0 mass% based on the total amount of the adhesive composition (solid content equivalent).
[0017] (Graft Copolymer P) The graft copolymer P has a chloroprene polymer chain (polychloroprene chain) and a graft chain that is bonded to the chloroprene polymer chain and contains a structural unit derived from an ethylenically unsaturated carboxylic acid. The chloroprene polymer chain is a backbone polymer for the graft chain and may be the main chain of the graft copolymer P.
[0018] The graft copolymer P can be obtained by grafting (graft polymerization) an ethylenically unsaturated carboxylic acid onto a chloroprene polymer (polychloroprene). That is, the method for producing the graft copolymer P includes a graft polymerization step of grafting (graft polymerization) an ethylenically unsaturated carboxylic acid onto a chloroprene polymer. The method for producing the graft copolymer P may include a chloroprene polymerization step of polymerizing chloroprene to obtain a chloroprene polymer, and in the chloroprene polymerization step, chloroprene may be polymerized (copolymerized) with another monomer copolymerizable with chloroprene.
[0019] The chloroprene polymer (polychloroprene) in the chloroprene polymer chain has structural units derived from chloroprene (2-chloro-1,3-butadiene). The chloroprene polymer may be a homopolymer of chloroprene, a copolymer of chloroprene and another monomer copolymerizable with chloroprene, or a mixture of these polymers.
[0020] From the viewpoint of easily obtaining excellent adhesiveness, the content of the structural units derived from chloroprene is preferably 50 mass% or more, more than 50 mass%, 70 mass% or more, 90 mass% or more, 95 mass% or more, 98 mass% or more, or 99 mass% or more based on the entire chloroprene polymer. The chloroprene polymer may be an embodiment consisting of structural units derived from chloroprene (an embodiment in which substantially 100 mass% of the chloroprene polymer is structural units derived from chloroprene).
[0021] Examples of monomers copolymerizable with chloroprene include (meth)acrylic acid esters (methyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, etc.), hydroxy(meth)acrylates (2-hydroxyethyl (meth)acrylate, 2-hydroxymethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, etc.), 2,3-dichloro-1,3-butadiene, 1-chloro-1,3-butadiene, butadiene, isoprene, ethylene, styrene, and acrylonitrile.
[0022] When a copolymer of chloroprene and another monomer copolymerizable with chloroprene is used as the chloroprene polymer, the copolymerization amount of the other monomer is preferably 50 parts by mass or less, and more preferably 30 parts by mass or less, per 100 parts by mass of chloroprene. By adjusting the copolymerization amount of the other monomer within this range, the effects of copolymerizing these monomers can be easily achieved without impairing the properties of the adhesive composition.
[0023] The other monomer copolymerizable with chloroprene is not limited to one type, and for example, three or more types of monomers including chloroprene may be copolymerized. The polymer structure of the chloroprene polymer is not particularly limited. The chloroprene polymer may be a mercaptan-modified chloroprene polymer, a xanthogen-modified chloroprene polymer, a sulfur-modified chloroprene polymer, a dithiocarbonate-based chloroprene polymer, a trithiocarbonate-based chloroprene polymer, a carbamate-based chloroprene polymer, or the like.
[0024] The chloroprene polymer can be obtained, for example, by emulsion polymerization of a raw material monomer containing chloroprene as a main component in the presence of a polymerization catalyst, a catalyst activator, a polymerization initiator, a chain transfer agent, etc. When obtaining the chloroprene polymer, rosin or the like may be used as an emulsifying dispersant.
[0025] Examples of catalysts for the polymerization reaction include organic peroxides such as ketone peroxides, peroxyketals, hydroperoxides (for example, t-butyl hydroperoxide), dialkyl peroxides, and diacyl peroxides.
[0026] Examples of catalyst activators include sodium sulfite, sodium hydrogen sulfite, potassium sulfite, iron (II) oxide, anthraquinone, sodium β-sulfonate, formamidinesulfinic acid, and L-ascorbic acid.
[0027] The polymerization initiator is not particularly limited, and any known polymerization initiator generally used in emulsion polymerization of chloroprene monomers can be used. Examples of the polymerization initiator include inorganic peroxides (potassium persulfate, ammonium persulfate, sodium persulfate, etc.), hydrogen peroxide, etc.
[0028] The chain transfer agent is not particularly limited, and a chain transfer agent used in normal emulsion polymerization of chloroprene can be used. Examples of the chain transfer agent include long-chain alkyl mercaptans such as n-dodecyl mercaptan (also known as 1-dodecanethiol), t-dodecyl mercaptan, and n-octyl mercaptan; xanthogen compounds such as diisopropyl xanthogen disulfide and diethyl xanthogen disulfide; iodoform; benzyl 1-pyrrole dithiocarbamate (also known as benzyl 1-pyrrole carbodithioate), benzyl phenyl carbodithioate, 1-benzyl-N,N-dimethyl-4-aminodithiobenzoate, 1-benzyl-4-methoxydithiobenzoate, 1-phenylethylimidazole dithiocarbamate (also known as 1-phenylethylimidazole carbodithioate), benzyl-1-(2-pyrrolidinone) dithiocarbamate (also known as benzyl-1-(2-pyrrolidinone) carbodithioate), benzyl phthalimidyl dithiocarbamate (also known as benzyl phthalimidyl carbodithioate), 2-cyanoprop-2-yl-1-pyrrole dithiocarbamate (also known as 2-cyanoprop-2-yl-1- pyrrole carbodithioate), 2-cyanobut-2-yl-1-pyrrole dithiocarbamate (also known as 2-cyanobut-2-yl-1-pyrrole carbodithioate), benzyl-1-imidazole dithiocarbamate (also known as benzyl-1-imidazole carbodithioate), 2-cyanoprop-2-yl-N,N-dimethyldithiocarbamate, benzyl-N,N-diethyldithiocarbamate, cyanomethyl-1-(2-pyrrolidone)dithiocarbamate, 2-(ethoxycarbonylbenzyl)propanol Prop-2-yl-N,N-diethyl dithiocarbamate, 1-phenylethyl dithiobenzoate, 2-phenylprop-2-yl dithiobenzoate, 1-acetate-1-yl-ethyl dithiobenzoate, 1-(4-methoxyphenyl)ethyl dithiobenzoate, benzyl dithioacetate, ethoxycarbonylmethyl dithioacetate, 2-(ethoxycarbonyl)prop-2-yl dithiobenzoate, 2-cyanoprop-2-yl dithiobenzoate, t-butyl dithiobenzoate, 2,4,4-Trimethylpent-2-yldithiobenzoate, 2-(4-chlorophenyl)-prop-2-yldithiobenzoate, 3-vinylbenzyldithiobenzoate, 4-vinylbenzyldithiobenzoate, benzyldiethoxyphosphinyldithioformate, t-butyltrithioperbenzoate, 2-phenylprop-2-yl-4-chlorodithiobenzoate, naphthalene-1-carboxylic acid-1-methyl-1-phenyl-ethyl ester, 4-cyano-4-methyl-4-thiobenzylsulfanylbutyric acid, dibenzyltetrathioterephthalate, carboxymethyldithiobenzoate, poly(ethylene oxide) with dithiobenzoate end groups, poly(ethylene oxide) with 4-cyano-4-methyl-4-thiobenzylsulfanylbutyric acid end groups, 2-[(2-phenylethanethioyl)sulfanyl]propanoic acid , 2-[(2-phenylethanethioyl)sulfanyl]succinic acid, potassium 3,5-dimethyl-1H-pyrazole-1-carbodithioate, cyanomethyl-3,5-dimethyl-1H-pyrazole-1-carbodithioate, cyanomethylmethyl-(phenyl)dithiocarbamate, benzyl-4-chlorodithiobenzoate, phenylmethyl-4-chlorodithiobenzoate, 4-nitrobenzyl-4-chlorodithiobenzoate, phenylprop-2-yl-4-chlorodithiobenzoate, 1-cyano-1-methylethyl-4-chlorodithiobenzoate, 3-chloro-2-butenyl-4-chlorodithiobenzoate, 2-chloro-2-butenyl dithiobenzoate, benzyl dithioacetate, 3-chloro-2-butenyl-1H-pyrrole-1-dithiocarboxylic acid, 2-cyanobutan-2-yl-4-chloro-3,5-Dimethyl-1H-pyrazole-1-carbodithioate, cyanomethylmethyl(phenyl)carbamodithioate, 2-cyano-2-propyldodecyltrithiocarbonate, dibenzyltrithiocarbonate, butylbenzyltrithiocarbonate, 2-[[(butylthio)thioxomethyl]thio]propionic acid, 2-[[(dodecylthio)thioxomethyl]thio]propionic acid, 2-[[(butylthio)thioxomethyl]thio]succinic acid, 2-[[(dodecylthio)thioxomethyl]thio]succinic acid, 2-[[(dodecylthio)thioxomethyl]thio] thiocarbonyl compounds such as 2-methylpropionic acid, 2,2'-[carbonothioylbis(thio)]bis[2-methylpropionic acid], 2-amino-1-methyl-2-oxoethylbutyl trithiocarbonate, benzyl-2-[(2-hydroxyethyl)amino]-1-methyl-2-oxoethyltrithiocarbonate, 3-[[[(t-butyl)thio]thioxomethyl]thio]propionic acid, cyanomethyldodecyltrithiocarbonate, diethylaminobenzyltrithiocarbonate, and dibutylaminobenzyltrithiocarbonate.
[0029] The polymerization temperature is not particularly limited and may be a temperature at which emulsion polymerization is generally performed, preferably in the range of 0 to 50°C, more preferably in the range of 10 to 50°C. The final polymerization rate of the chloroprene polymer obtained in the above-mentioned chloroprene polymerization step is not particularly limited, but is preferably adjusted arbitrarily within the range of 30 to 100%. In order to adjust the final conversion rate, a polymerization terminator that terminates the polymerization reaction may be added to terminate the polymerization when the desired conversion rate is reached.
[0030] The polymerization terminator is not particularly limited, and any commonly used polymerization terminator can be used. Examples of the polymerization terminator include thiodiphenylamine, 4-t-butylcatechol, and 2,2-methylenebis-4-methyl-6-t-butylphenol.
[0031] The graft copolymer P may be a graft copolymer in which a monomer mainly composed of an ethylenically unsaturated carboxylic acid is grafted to a chloroprene polymer. The graft copolymer P may have a graft chain in which the content of structural units derived from an ethylenically unsaturated carboxylic acid is in the following range. From the viewpoint of easily obtaining excellent adhesiveness, the content of structural units derived from an ethylenically unsaturated carboxylic acid is preferably 50% by mass or more, more than 50% by mass, 70% by mass or more, 90% by mass or more, 95% by mass or more, 98% by mass or more, or 99% by mass or more based on the entire graft chain. The graft chain may be an embodiment consisting of structural units derived from an ethylenically unsaturated carboxylic acid (an embodiment in which substantially 100% by mass of the graft chain is a structural unit derived from an ethylenically unsaturated carboxylic acid). The graft chain may not have structural units derived from chloroprene.
[0032] Examples of the ethylenically unsaturated carboxylic acid to be grafted to the chloroprene polymer include acrylic acid, methacrylic acid, maleic acid, itaconic acid, and crotonic acid. The ethylenically unsaturated carboxylic acid is not limited to one type, and two or more types can be used in combination. From the viewpoint of easily obtaining excellent adhesion, the ethylenically unsaturated carboxylic acid preferably contains at least one type selected from the group consisting of acrylic acid and methacrylic acid.
[0033] The graft chain may include a structural unit derived from polyvinyl alcohol, or may not include a structural unit derived from polyvinyl alcohol. The graft chain may include a structural unit derived from a styrene-based monomer (e.g., styrene), or may not include a structural unit derived from a styrene-based monomer (e.g., styrene). The graft chain may include a structural unit derived from a vinyl-based monomer other than (meth)acrylic acid, or may not include a structural unit derived from a vinyl-based monomer other than (meth)acrylic acid.
[0034] From the viewpoint of easily obtaining excellent adhesiveness, the content of the structural units derived from (meth)acrylic acid (the total amount of structural units derived from acrylic acid and structural units derived from methacrylic acid; the same applies below) is preferably 10 parts by mass or more, 20 parts by mass or more, more than 20 parts by mass, 30 parts by mass or more, 50 parts by mass or more, 80 parts by mass or more, 100 parts by mass or more, or more than 100 parts by mass, relative to 100 parts by mass of structural units derived from vinyl monomers other than (meth)acrylic acid.
[0035] From the viewpoint of easily obtaining excellent adhesiveness, the content of the structural unit derived from (meth)acrylic acid is preferably 30% by mass or more, more than 30% by mass, more than 50% by mass, more than 50% by mass, 70% by mass or more, 90% by mass or more, 95% by mass or more, 98% by mass or more, or 99% by mass or more based on the entire graft chain. The graft chain may be an embodiment consisting of a structural unit derived from (meth)acrylic acid (an embodiment in which substantially 100% by mass of the graft chain is a structural unit derived from (meth)acrylic acid).
[0036] As a method for grafting an ethylenically unsaturated carboxylic acid onto a chloroprene polymer, an emulsion polymerization method is generally used in which the chloroprene polymer obtained by the above-mentioned method is mixed with an ethylenically unsaturated carboxylic acid, and the ethylenically unsaturated carboxylic acid is grafted onto the chloroprene polymer in the presence of a radical polymerization initiator. Alternatively, a solution polymerization method can be used in which an ethylenically unsaturated carboxylic acid is added to a solution obtained by dissolving a chloroprene polymer rubber obtained by freeze-drying the chloroprene polymer in an organic solvent, and the ethylenically unsaturated carboxylic acid is grafted onto the chloroprene polymer in the presence of a radical polymerization initiator. For example, potassium persulfate can be used as the radical polymerization initiator.
[0037] The molar ratio of the oxygen atom content to the chlorine atom content in the graft copolymer P (oxygen atom content / chlorine atom content) is 0.04 to 1 (i.e., the molar ratio of chlorine atoms to oxygen atoms in the graft copolymer P is 1:0.04 to 1:1). The molar ratio of chlorine atoms to oxygen atoms represents the molar ratio of the amount of chlorine atoms contained in the chloroprene polymer to the amount of oxygen atoms contained in the ethylenically unsaturated carboxylic acid, and indicates the graft amount of the ethylenically unsaturated carboxylic acid in the graft copolymer P. For example, in order to increase the oxygen atom content, the amount of the ethylenically unsaturated carboxylic acid to be grafted or the polymerization time may be increased to increase the graft amount of the ethylenically unsaturated carboxylic acid to the chloroprene polymer.
[0038] The contents of chlorine atoms and oxygen atoms in the graft copolymer P can be measured by the following method. (1) The adhesive composition containing the graft copolymer P is frozen at −60° C. for 24 hours and then freeze-dried to obtain a dry product. (2) 1.00 g of the above-mentioned dried product is cut into 2 mm squares (cubes of 2 mm length × 2 mm width × 2 mm height), and the resulting pieces are immersed in 100 mL of acetone (23°C) to obtain an acetone solution. The acetone solution is then stirred at 23°C for 24 hours using a magnetic stirrer (e.g., CHPS-170DS, manufactured by AS ONE Corporation, dimensions: 175 mm × 178 mm). (3) The insoluble matter in the acetone solution is filtered and collected using a 200-mesh stainless steel mesh, and then dried (for example, the insoluble matter is left to stand in a vacuum dryer for 24 hours to dry). (4) The elements on the surface of the insoluble matter (polymer) are analyzed using a scanning electron microscope (e.g., Hitachi High-Technologies Corporation, SU6600) equipped with an energy dispersive X-ray analyzer (e.g., Oxford Instruments, INCAx-act). The contents of chlorine atoms and oxygen atoms are quantified from the peaks of the detected elements, and the molar ratio of the oxygen atom content / chlorine atom content in the polymer is calculated.
[0039] The molar ratio of the oxygen atom content to the chlorine atom content in the graft copolymer P is preferably 0.05 or more, 0.06 or more, 0.1 or more, 0.2 or more, 0.3 or more, 0.35 or more, 0.38 or more, 0.39 or more, or 0.4 or more, from the viewpoint of easily obtaining excellent adhesiveness. The molar ratio may be 0.41 or more, 0.42 or more, 0.45 or more, 0.48 or more, 0.5 or more, 0.6 or more, 0.7 or more, or 0.8 or more. The molar ratio of the oxygen atom content to the chlorine atom content in the graft copolymer P is preferably 0.9 or less, 0.8 or less, 0.7 or less, 0.6 or less, 0.5 or less, 0.48 or less, 0.45 or less, 0.42 or less, or 0.41 or less, from the viewpoint of easily obtaining excellent adhesiveness. The molar ratio may be 0.4 or less, 0.39 or less, 0.38 or less, 0.35 or less, 0.3 or less, 0.2 or less, 0.1 or less, or 0.06 or less.
[0040] The adhesive composition according to the present embodiment contains a graft copolymer P as a chloroprene polymer (a polymer having a structural unit derived from chloroprene). The adhesive composition according to the present embodiment may contain a chloroprene polymer other than the graft copolymer P. From the viewpoint of easily obtaining excellent adhesiveness, the content of the graft copolymer P is preferably 50% by mass or more, more than 50% by mass, 70% by mass or more, 90% by mass or more, 95% by mass or more, 98% by mass or more, or 99% by mass or more based on the total chloroprene polymer contained in the adhesive composition. The content of the chloroprene homopolymer may be 50% by mass or less, less than 50% by mass, 30% by mass or less, 10% by mass or less, 5% by mass or less, 2% by mass or less, 1% by mass or less, or substantially 0% by mass based on the total chloroprene polymer contained in the adhesive composition.
[0041] (Surfactant) The surfactant is not particularly limited, but includes polyvinyl alcohol; resin acid soaps such as rosin acid soap and disproportionated rosin soap; alkyl sulfates such as sodium lauryl sulfate; alkyl benzene sulfonates such as sodium dodecylbenzene sulfonate; alkyl naphthalene sulfonates; dialkyl sulfosuccinates; polyoxyethylene alkyl ether sulfates; salts of aryl sulfonic acid formalin condensates such as salts of β-naphthalene sulfonic acid formalin condensates; polyoxyethylene alkyl ethers such as polyoxyethylene lauryl ether; polyoxyethylene higher alcohol ethers; polyoxyethylene alkyl phenyl ethers such as polyoxyethylene nonyl phenyl ether. The surfactant contained in the adhesive composition may contain an anionic surfactant, or may not contain an anionic surfactant. The surfactant contained in the adhesive composition may contain a nonionic surfactant, or may not contain a nonionic surfactant.
[0042] The content of the surfactant (surfactant amount, solid content equivalent) is preferably in the following range based on the total amount of the adhesive composition (solid content equivalent) from the viewpoint of improving the stability of the adhesive composition. The content of the surfactant is preferably 0.5 mass% or more, 0.7 mass% or more, 0.8 mass% or more, 1 mass% or more, 1.2 mass% or more, or 1.4 mass% or more. The content of the surfactant is preferably 2.5 mass% or less, 2 mass% or less, 1.8 mass% or less, 1.6 mass% or less, 1.5 mass% or less, or 1.4 mass% or less. From these viewpoints, the content of the surfactant is preferably 0.5 to 2.5 mass%. The content of the surfactant may be 1.5 mass% or more, 1.6 mass% or more, 1.8 mass% or more, or 2 mass% or more. The content of the surfactant may be 1.2 mass% or less, 1 mass% or less, 0.8 mass% or less, or 0.7 mass% or less. The content of the surfactant can be measured by the method described in the examples.
[0043] From the viewpoint of improving the stability of the adhesive composition, the content of the surfactant (amount of surfactant, converted into solid content) is preferably 25 parts by mass or less, 20.5 parts by mass or less, less than 20.5 parts by mass, 20 parts by mass or less, 15 parts by mass or less, or 10 parts by mass or less per 100 parts by mass of chloroprene polymer (including graft copolymer P) or 100 parts by mass of graft copolymer P contained in the adhesive composition.
[0044] The content of the nonionic surfactant is preferably 1 part by mass or less, less than 1 part by mass, 0.5 parts by mass or less, less than 0.5 parts by mass, 0.1 parts by mass or less, 0.01 parts by mass or less, or substantially 0 parts by mass per 100 parts by mass of chloroprene polymer (including graft copolymer P) or 100 parts by mass of graft copolymer P contained in the adhesive composition.
[0045] The content of polyvinyl alcohol is preferably 1 part by mass or less, 0.5 parts by mass or less, 0.2 parts by mass or less, less than 0.2 parts by mass, 0.1 parts by mass or less, less than 0.1 parts by mass, 0.01 parts by mass or less, or substantially 0 parts by mass per 100 parts by mass of chloroprene polymer (including graft copolymer P) or 100 parts by mass of graft copolymer P contained in the adhesive composition.
[0046] The surfactant may be added after the graft copolymer P is obtained by the above-mentioned method, or may be added during polymerization of the chloroprene polymer (chloroprene polymerization step) or when the graft copolymer P is obtained (graft polymerization step).
[0047] (Other Ingredients) The adhesive composition according to the present embodiment may contain any of a tackifier resin, a thickener, an isocyanate, an ultraviolet absorber, an antioxidant, a plasticizer, a filler, a vulcanizing agent, a vulcanization accelerator, an antifoaming agent, an antirust agent, etc., depending on the required performance. The content of the crosslinking agent (vulcanization accelerator, etc.) is preferably 1 part by mass or less, 0.5 parts by mass or less, less than 0.5 parts by mass, 0.1 parts by mass or less, 0.01 parts by mass or less, or substantially 0 parts by mass, per 100 parts by mass of the polymer component (including the graft copolymer P) contained in the adhesive composition, or per 100 parts by mass of the graft copolymer P.
[0048] [Tackifier resin] A tackifier resin can be blended to further improve adhesion. The tackifier resin is not particularly limited, and examples thereof include rosin resin, polymerized rosin resin, α-pinene resin, β-pinene resin, terpene phenol resin, C5 fraction petroleum resin, C9 fraction petroleum resin, C5 / C9 fraction petroleum resin, DCPD petroleum resin, alkylphenol resin, xylene resin, coumarone resin, and coumarone-indene resin.
[0049] [Thickener] The thickener can be added to increase the viscosity of the adhesive to improve the application or workability of the adhesive. The tackifier resin is not particularly limited, and examples thereof include an aqueous solution of carboxymethyl cellulose (CMC), an aqueous solution of hydroxyethyl cellulose, polyvinyl alcohol, and a hydrophilic group-containing synthetic resin emulsion.
[0050] [Isocyanate] Isocyanate can be added to further improve adhesion. The isocyanate is not particularly limited, and examples thereof include methyl isocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, and the like.
[0051] The content (addition amount) of the isocyanate is preferably 3 to 10 parts by mass per 100 parts by mass of the adhesive composition (converted into solid content). By adjusting the content (addition amount) of the isocyanate within this range, it is easy to further improve the adhesiveness of the adhesive composition.
[0052] The solid content of the adhesive composition according to the present embodiment is 10 to 50% by mass based on the total amount of the adhesive composition (including the liquid component) from the viewpoint of obtaining excellent adhesion. If the solid content is 50% by mass or less, sufficient mechanical stability can be obtained. The solid content of the adhesive composition can be measured by the method described in the examples.
[0053] From the viewpoint of easily obtaining excellent adhesion, the solid content concentration of the adhesive composition is preferably more than 10% by mass, 12% by mass or more, 15% by mass or more, 18% by mass or more, or 20% by mass or more. From the viewpoint of easily obtaining excellent adhesion and easily obtaining sufficient mechanical stability, the solid content concentration of the adhesive composition is preferably less than 50% by mass, 40% by mass or less, 30% by mass or less, 25% by mass or less, or 20% by mass or less.
[0054] The content of the liquid component (including water) or the content of water in the adhesive composition according to this embodiment is preferably 10 parts by mass or more, 50 parts by mass or more, 100 parts by mass or more, 120 parts by mass or more, more than 120 parts by mass, 150 parts by mass or more, 180 parts by mass or more, 200 parts by mass or more, 240 parts by mass or more, more than 240 parts by mass, 250 parts by mass or more, 300 parts by mass or more, or 400 parts by mass or more, per 100 parts by mass of chloroprene polymer (including graft copolymer P) or 100 parts by mass of graft copolymer P contained in the adhesive composition.
[0055] In the adhesive composition according to this embodiment, the acetone soluble content measured in the following (1) to (4) is preferably 3 mass % or less, 2 mass % or less, 1 mass % or less, or less than 1 mass %, from the viewpoint of easily obtaining excellent adhesion. The acetone soluble content may be 0 mass % or more than 0 mass. The adhesive composition according to this embodiment may contain an acetone soluble content measured in the following (1) to (4) in the range of more than 0 mass % to 3 mass % or less. (1) The adhesive composition is frozen at −60° C. for 24 hours and then freeze-dried to obtain a dry product. (2) 1.00 g of the above-mentioned dried product is cut into 2 mm squares (cubes of 2 mm length × 2 mm width × 2 mm height), and the resulting pieces are immersed in 100 mL of acetone (23°C) to obtain an acetone solution. The acetone solution is then stirred at 23°C for 24 hours using a magnetic stirrer (e.g., CHPS-170DS, manufactured by AS ONE Corporation, dimensions: 175 mm × 178 mm). (3) After removing the insoluble matter in the acetone solution by filtration using a 200-mesh stainless steel mesh, the acetone solution is concentrated and dried using an evaporator, and the mass (A) of the residue is measured (precisely weighed). (4) Calculate the acetone soluble portion using the following formula. Acetone solubles = mass of residue (A) [g] / mass of dry matter 1.00 [g] x 100
[0056] The above-mentioned acetone soluble matter can be used as an indicator of the amount of a polymer (such as a homopolymer of methacrylic acid) obtained by polymerization of the ethylenically unsaturated carboxylic acids used in obtaining the graft copolymer P.
[0057] <Rubber articles, rubber reinforcing materials, and adhesive-coated organic fiber cords> The rubber article according to the present embodiment includes the rubber reinforcing material according to the present embodiment. Examples of the rubber article include tires and various belts.
[0058] The rubber reinforcing material according to the present embodiment includes the adhesive composition according to the present embodiment, an organic fiber cord, and a rubber member bonded to the organic fiber cord via the adhesive composition. The rubber member may cover the surface of the organic fiber cord. The organic fiber cord and the rubber member may be laminated via the adhesive composition. The rubber reinforcing material can be used as a carcass, a belt reinforcing material, etc.
[0059] The adhesive-attached organic fiber cord according to the present embodiment includes the adhesive composition according to the present embodiment and an organic fiber cord to which the adhesive composition is attached. The adhesive-attached organic fiber cord may be an adhesive-attached tire cord (an organic fiber cord for tire reinforcement). The rubber reinforcing material described above includes an adhesive-attached organic fiber cord and a rubber member adhered to the organic fiber cord via the adhesive composition.
[0060] (Organic fiber cord) The organic fiber cord can improve the strength of the rubber reinforcing material, and may be an organic fiber cord formed by twisting organic fibers. The organic fiber cord may be a tire cord. The material of the organic fiber cord is not particularly limited, but thermoplastics are preferable. Examples of thermoplastics include polyamide, polyester, polyolefin (polyethylene, polypropylene, etc.), polycarbonate, polyacrylate, styrene-based resin (ABS resin, etc.), and vinyl chloride resin. Among these, polyester or nylon is preferable. In the rubber reinforcing material according to this embodiment, polyester, which has high mechanical strength but is relatively difficult to bond to rubber members by conventional methods, can also be used as the material of the organic fiber cord.
[0061] (Rubber parts) The rubber member is preferably one in which a compounding agent commonly used in the rubber industry is compounded with the rubber component. The rubber component is not particularly limited, and examples thereof include natural rubber; conjugated diene synthetic rubber such as polyisoprene rubber (IR), polybutadiene rubber (BR), styrene-butadiene copolymer rubber (SBR), acrylonitrile butadiene rubber (NBR), chloroprene rubber (CR), and butyl rubber (IIR); ethylene-propylene copolymer rubber (EPM); ethylene-propylene-diene copolymer rubber (EPDM); and polysiloxane rubber. Among these, natural rubber or conjugated diene synthetic rubber is preferred.
[0062] <Method of manufacturing rubber reinforcing material> The method for producing a rubber reinforcing material according to the present embodiment includes a bonding step of bonding an organic fiber cord to a rubber member via the adhesive composition according to the present embodiment. The method for producing a rubber reinforcing material according to the present embodiment is a method for bonding an organic fiber cord to a rubber member.
[0063] The method for producing a rubber reinforcing material according to the present embodiment may include a step of covering the organic fiber cord with an adhesive layer containing the adhesive composition according to the present embodiment before the bonding step. In this case, in the bonding step, the organic fiber cord and the rubber member can be bonded via the adhesive layer.
[0064] Methods for forming the adhesive layer include dipping, impregnation, brush coating, casting, spraying, roll coating, knife coating, etc. Among these, it is preferable to form the adhesive layer by impregnating an organic fiber cord with the adhesive composition. After forming the adhesive layer, a drying treatment may be performed at 120 to 180°C for 5 to 10 minutes.
[0065] In the bonding step, the organic fiber cord and the rubber member can be bonded by vulcanization via the adhesive composition. In the bonding step, for example, the organic fiber cord covered with the adhesive layer can be embedded in unvulcanized rubber and vulcanized. EXAMPLES
[0066] The present invention will be described below with reference to examples, but the present invention is not limited to these examples.
[0067] <Preparation of Adhesive Composition> Example 1 [Production of Chloroprene Latex A] In a reactor having a capacity of 10 L, 150 parts by mass of water, 4.0 parts by mass of sodium dodecylbenzenesulfonate (Kao Corporation: Neopelex G-65 (purity: 65% by mass)), 0.7 parts by mass of sodium salt of naphthalenesulfonic acid formalin condensate (Kao Corporation: Demol N), and 0.5 parts by mass of sodium hydrogen sulfite were added under a nitrogen gas flow, and the solids were dissolved to obtain a solution. Then, while stirring the solution, 100 parts by mass of chloroprene and 0.55 parts by mass of 1-dodecanethiol were added to the solution. Polymerization was started at 10°C under a nitrogen atmosphere using potassium persulfate as a polymerization initiator. When the polymerization rate reached 75%, an emulsion containing 0.02 parts by mass of thiodiphenylamine was added to terminate the polymerization. Unreacted monomers were removed under reduced pressure to obtain chloroprene latex A (mercaptan modified).
[0068] [Production of adhesive composition a] While stirring 100 parts by mass of the above-mentioned chloroprene latex A, 0.5 parts by mass of methacrylic acid and 0.005 parts by mass of 1-dodecanethiol were added to the chloroprene latex A. Using 0.0005 parts by mass of potassium persulfate as a polymerization initiator, polymerization was initiated at 40°C under a nitrogen atmosphere. When the polymerization rate reached 100%, the polymerization was terminated. Water was added to adjust the solid content concentration to 20% by mass, thereby obtaining an adhesive composition a containing a graft copolymer.
[0069] Example 2 Adhesive composition b containing a graft copolymer was obtained in the same manner as in Example 1, except that the amount of methacrylic acid used in Example 1 was changed to 4 parts by mass, the amount of 1-dodecanethiol used was changed to 0.04 parts by mass, and the amount of potassium persulfate used was changed to 0.004 parts by mass.
[0070] Example 3 An adhesive composition c containing a graft copolymer was obtained in the same manner as in Example 1, except that the amount of methacrylic acid used in Example 1 was changed to 8 parts by mass, the amount of 1-dodecanethiol used was changed to 0.08 parts by mass, and the amount of potassium persulfate used was changed to 0.008 parts by mass.
[0071] Example 4 [Production of Chloroprene Latex B] Chloroprene latex B (xanthogen-modified) was obtained in the same manner as in Example 1, except that 0.55 parts by mass of 1-dodecanethiol in Example 1 was changed to 0.55 parts by mass of diethylxanthogen disulfide (manufactured by Ouchi Shinko Chemical Industry Co., Ltd.).
[0072] [Production of adhesive composition d] While stirring 100 parts by mass of the above-mentioned chloroprene latex B, 4 parts by mass of methacrylic acid and 0.04 parts by mass of 1-dodecanethiol were added to the chloroprene latex B. Using 0.004 parts by mass of potassium persulfate as a polymerization initiator, polymerization was initiated at 40°C under a nitrogen atmosphere. When the polymerization rate reached 100%, the polymerization was terminated. Thus, an adhesive composition d containing a graft copolymer was obtained.
[0073] Example 5 [Production of Chloroprene Latex C] Chloroprene latex C (sulfur-modified) was obtained in the same manner as in Example 1, except that 0.55 parts by mass of 1-dodecanethiol in Example 1 was changed to 0.55 parts by mass of sulfur.
[0074] [Production of adhesive composition e] While stirring 100 parts by mass of the above-mentioned chloroprene latex C, 4 parts by mass of methacrylic acid and 0.04 parts by mass of 1-dodecanethiol were added to the chloroprene latex C. Using 0.004 parts by mass of potassium persulfate as a polymerization initiator, polymerization was initiated at 40°C under a nitrogen atmosphere. When the polymerization rate reached 100%, the polymerization was terminated. As a result, an adhesive composition e containing a graft copolymer was obtained.
[0075] Example 6 An adhesive composition f containing a graft copolymer was obtained in the same manner as in Example 2, except that the methacrylic acid in Example 2 was changed to acrylic acid.
[0076] Example 7 [Production of Chloroprene Latex D] Chloroprene latex D (mercaptan modified) was obtained in the same manner as in Example 1, except that the amount of sodium dodecylbenzenesulfonate (Kao Corporation: Neopelex G-65 (purity: 65 mass%)) used in Example 1 was changed from 4.0 parts by mass to 2.0 parts by mass.
[0077] [Production of adhesive composition g] While stirring 100 parts by mass of the above-mentioned chloroprene latex D, 4 parts by mass of methacrylic acid and 0.04 parts by mass of 1-dodecanethiol were added to the chloroprene latex D. Using 0.004 parts by mass of potassium persulfate as a polymerization initiator, polymerization was initiated at 40°C under a nitrogen atmosphere. When the polymerization rate reached 100%, the polymerization was terminated. Thus, an adhesive composition g containing a graft copolymer was obtained.
[0078] Example 8 [Production of Chloroprene Latex E] Chloroprene latex E (mercaptan modified) was obtained in the same manner as in Example 1, except that the amount of sodium dodecylbenzenesulfonate (Kao Corporation: Neopelex G-65 (purity: 65 mass%)) used in Example 1 was changed from 4.0 parts by mass to 6.0 parts by mass.
[0079] [Production of adhesive composition h] While stirring 100 parts by mass of the above-mentioned chloroprene latex E, 4 parts by mass of methacrylic acid and 0.04 parts by mass of 1-dodecanethiol were added to the chloroprene latex E. Using 0.004 parts by mass of potassium persulfate as a polymerization initiator, polymerization was initiated at 40°C under a nitrogen atmosphere. When the polymerization rate reached 100%, the polymerization was terminated. Thus, an adhesive composition h containing a graft copolymer was obtained.
[0080] Example 9 [Production of Chloroprene Latex F] Chloroprene latex F was obtained in the same manner as in Example 1, except that 4.0 parts by mass of sodium dodecylbenzenesulfonate (manufactured by Kao Corporation: Neopelex G-65 (purity: 65% by mass)) in Example 1 was changed to 4.0 parts by mass of polyvinyl alcohol (manufactured by Denka Company Ltd.: B-05).
[0081] [Production of adhesive composition i] While stirring 100 parts by mass of the above-mentioned chloroprene latex F, 4 parts by mass of methacrylic acid and 0.04 parts by mass of 1-dodecanethiol were added to the chloroprene latex F. Using 0.004 parts by mass of potassium persulfate as a polymerization initiator, polymerization was initiated at 40°C under a nitrogen atmosphere. When the polymerization rate reached 100%, the polymerization was terminated. Thus, an adhesive composition i containing a graft copolymer was obtained.
[0082] Example 10 [Production of Chloroprene Latex G] Chloroprene latex G (mercaptan modified) was obtained in the same manner as in Example 1, except that the polymerization initiation temperature in obtaining chloroprene latex A in Example 1 was changed to 40°C.
[0083] [Production of adhesive composition j] While stirring 100 parts by mass of the above-mentioned chloroprene latex G, 4 parts by mass of methacrylic acid and 0.04 parts by mass of 1-dodecanethiol were added to the chloroprene latex G. Using 0.004 parts by mass of potassium persulfate as a polymerization initiator, polymerization was initiated at 40°C under a nitrogen atmosphere. When the polymerization rate reached 100%, the polymerization was terminated. Thus, an adhesive composition j containing a graft copolymer was obtained.
[0084] Comparative Example 1 An adhesive composition k containing a graft copolymer was obtained in the same manner as in Example 1, except that the amount of methacrylic acid used in Example 1 was changed to 0.3 parts by mass, the amount of 1-dodecanethiol used was changed to 0.003 parts by mass, and the amount of potassium persulfate used was changed to 0.0003 parts by mass.
[0085] Comparative Example 2 An adhesive composition l containing a graft copolymer was obtained in the same manner as in Example 1, except that the amount of methacrylic acid used in Example 1 was changed to 12 parts by mass, the amount of 1-dodecanethiol used was changed to 0.12 parts by mass, and the amount of potassium persulfate used was changed to 0.012 parts by mass.
[0086] Comparative Example 3 Water was added to a carboxyl group-modified chloroprene latex (manufactured by Denka Co., Ltd.: LC-501, random copolymer) to adjust the solid content concentration to 20 mass %, and the resulting mixture was used as adhesive composition m.
[0087] Comparative Example 4 Chloroprene latex A was produced in the same manner as in Example 1. 4.0 parts by mass of polymethacrylic acid (PMA, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added to 100 parts by mass of chloroprene latex A, and the mixture was stirred at 25° C. until the polymethacrylic acid was dissolved. Thus, an adhesive composition n was obtained.
[0088] Comparative Example 5 The adhesive composition a of Example 1 was diluted with pure water to adjust the solid content concentration to 5 mass %, thereby obtaining an adhesive composition o containing a graft copolymer.
[0089] Comparative Example 6 The adhesive composition a of Example 1 was concentrated to adjust the solid content concentration to 55 mass %, thereby obtaining an adhesive composition p containing a graft copolymer.
[0090] <Polymerization rate> The polymerization rate of the above-mentioned copolymer was calculated by the following formula, where the total amount of monomers charged was 100 parts by mass, and the evaporation residue indicates the non-volatile components excluding the copolymer contained in the adhesive composition. Copolymer polymerization rate [%] = (total amount of monomers charged [parts by mass] × solid concentration [% by mass] - evaporation residue [parts by mass]) / total amount of monomers charged [parts by mass] × 100
[0091] <Solid content concentration of adhesive composition> The solid content concentration of the adhesive composition was measured by the following procedure. First, the mass X [g] of the aluminum plate alone was obtained. Next, 2 g of the adhesive composition was placed in the aluminum plate, and the total mass Y [g] of the adhesive composition and the aluminum plate was obtained. Next, the aluminum plate containing the adhesive composition was dried in a hot air dryer at 125°C for 1 hour, and the mass Z [g] was obtained. The solid content concentration [mass%] was then calculated based on the following formula. Solid concentration={(ZX) / (YX)}×100
[0092] <Evaluation> (molar ratio of oxygen atom content to chlorine atom content in polymer) The adhesive composition was frozen at -60°C for 24 hours and then freeze-dried to obtain a dried product. 1.00 g of the dried product was cut into 2 mm squares (cubes measuring 2 mm long x 2 mm wide x 2 mm high) to obtain small pieces. At 23°C, the small pieces were immersed (dispersed) in 100 mL of acetone (23°C) to obtain an acetone solution, and the acetone solution was stirred for 24 hours using a magnetic stirrer (As One Corporation, CHPS-170DS, dimensions: 175 mm x 178 mm). The insoluble matter (polymer) in the acetone solution was filtered and collected using a 200-mesh stainless steel mesh, and then the insoluble matter was left to stand in a vacuum dryer for 24 hours to dry. The elements on the surface of the insoluble matter (polymer) were analyzed using a scanning electron microscope (Hitachi High-Technologies Corporation, SU6600) equipped with an energy dispersive X-ray analyzer (Oxford Instruments, INCAx-act). The content of chlorine atoms and oxygen atoms was quantified. Based on the measurement results, the molar ratio of the oxygen atom content / chlorine atom content in the polymer was calculated. The results are shown in Tables 1 and 2. In the tables, the molar ratio of oxygen atoms when the amount of chlorine atoms is taken as 1 is shown.
[0093] (amount of surfactant) The above adhesive composition was diluted 200 times with pure water, centrifuged, and 25 μL of the resulting supernatant was quantitatively analyzed by liquid chromatography. Using a calibration curve, the amount of surfactant in the adhesive composition was calculated based on the measured value. The results are shown in Tables 1 and 2.
[0094] (Acetone solubles) The adhesive composition was frozen at -60°C for 24 hours and then freeze-dried to obtain a dried product. 1.00 g of the dried product was cut into 2 mm squares (cubes measuring 2 mm long x 2 mm wide x 2 mm high) to obtain small pieces. At 23°C, the small pieces were immersed (dispersed) in 100 mL of acetone (23°C) to obtain an acetone solution, and then the acetone solution was stirred for 24 hours using a magnetic stirrer (manufactured by AS ONE Corporation, CHPS-170DS, dimensions: 175 mm x 178 mm). Insoluble matter (polymers, etc.) in the acetone solution was removed by filtration using a 200-mesh stainless steel mesh. The acetone solution was concentrated and dried using an evaporator, and the mass (A) of the residue was measured (precisely weighed). The acetone-soluble content was calculated by dividing the mass (A) of the residue by the mass of the dried product according to the following formula. The results are shown in Tables 1 and 2. Acetone solubles [mass%] = mass of residue (A) [g] / mass of dried material (1.00 [g]) × 100
[0095] (Adhesiveness) The adhesive strength of the adhesive composition was measured according to JIS K6301. As an adhesive composition using resorcin and formaldehyde, 16.7 parts by mass of chloroprene latex (manufactured by Denka Co., Ltd., product name: LM-61, solid content: 60.0 mass%, chloroprene latex containing no graft copolymer), 1.5 parts by mass of resorcin, 1.5 parts by mass of formaldehyde, 0.3 parts by mass of caustic soda, and 80 parts by mass of water were mixed to prepare an RFL-based adhesive composition, and the adhesive strength measured using the adhesive composition was set to 100, and the adhesive strength measured using each of the above-mentioned adhesive compositions was relatively evaluated. The results are shown in Tables 1 and 2. The larger the value, the better the result. For Comparative Example 6, the viscosity of the adhesive composition was high and a test specimen could not be prepared, so the adhesive strength could not be measured.
[0096] [Table 1]
[0097] [Table 2]
[0098] <Preparation of adhesive tire cord> The adhesive composition of each of the above-mentioned Examples was applied to a tire cord (made of nylon-6,6), and then dried for 1 minute at 180° C. Thereafter, a tension of 1 to 2 kg / cord (cord tension) was applied to the tire cord, and then the cord was heat-treated for 2 minutes at 240° C. using a heat treatment machine, thereby obtaining an adhesive-coated tire cord.
Claims
1. An adhesive composition comprising a graft copolymer and a surfactant, the graft copolymer has a chloroprene polymer chain and a graft chain bonded to the chloroprene polymer chain and containing a structural unit derived from an ethylenically unsaturated carboxylic acid, the content of the structural unit derived from the ethylenically unsaturated carboxylic acid is 50 mass% or more based on the entirety of the graft chain, the molar ratio of the content of oxygen atoms to the content of chlorine atoms in the graft copolymer is 0.04 to 1; The adhesive composition for organic fiber cords has a solids concentration of 10 to 50 mass %.
2. The adhesive composition according to claim 1 , wherein the ethylenically unsaturated carboxylic acid comprises at least one selected from the group consisting of acrylic acid and methacrylic acid.
3. The adhesive composition according to claim 2 , wherein the total amount of the structural units derived from acrylic acid and the structural units derived from methacrylic acid is 50 mass % or more based on the entirety of the graft chains.
4. The adhesive composition according to any one of claims 1 to 3, wherein the acetone soluble content measured by the following (1) to (4) is 3 mass% or less. (1) The adhesive composition is frozen at −60° C. for 24 hours and then freeze-dried to obtain a dry product. (2) 1.00 g of the dried product is cut into 2 mm square pieces, and the resulting pieces are immersed in 100 mL of acetone to obtain an acetone solution. The acetone solution is then stirred at 23° C. for 24 hours using a magnetic stirrer. (3) After removing insoluble matters in the acetone solution by filtration using a 200 mesh stainless steel mesh, the acetone solution is concentrated and dried using an evaporator, and the mass of the residue is measured. (4) Calculate the acetone soluble matter using the following formula. Acetone soluble matter=mass of the residue [g] / mass of the dried material 1.00 [g]×100
5. The adhesive composition according to any one of claims 1 to 4, wherein the content of the graft copolymer is more than 50 mass% based on the total amount of the chloroprene polymer contained in the adhesive composition.
6. The adhesive composition according to any one of claims 1 to 5, An organic fiber cord; a rubber member adhered to the organic fiber cord via the adhesive composition.
7. A method for producing a rubber reinforcing material, comprising a step of adhering an organic fiber cord and a rubber member via the adhesive composition according to any one of claims 1 to 5.
8. A rubber article comprising the rubber reinforcement of claim 6.
9. 9. The rubber article of claim 8 which is a tire.
Citation Information
Patent Citations
Adhesive for high-speed rail and automobile brake hoses and preparation method thereof
CN110128970A
Adhesive between rubber and fiber
JP1983002370A
Adhesive for reinforcing fiber contained in rubber
JP1985092371A
Rubber reinforcement adhesive
JP1985096674A
Optical information recording medium
JP1988061433A