Equipment and method for continuous casting of steel strip and subsequent flat rolling
The described installation and method for continuous casting and flat rolling of steel strips with austenitic and/or ferritic structures address production challenges by directly rolling thin strips, enhancing efficiency and reducing costs.
Patent Information
- Application Number
- JP2023514924
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-09-08
- Filing Date
- 2021-09-08
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-09-08
AI Technical Summary
Existing technologies face difficulties in producing thin steel strips with austenitic and/or ferritic microstructures, requiring multiple processing steps and lacking adequate production capabilities.
An installation and method for continuous casting and subsequent flat rolling of steel strips, utilizing a casting equipment connected to a hot rolling stand with cooling and heating devices, enabling direct hot pre-rolling and finish rolling into thin steel strips with austenitic and/or ferritic structures.
This approach reduces process steps, shortens delivery times, lowers investment costs, and achieves significant energy savings while producing ultra-thin steel strips with precise structural control.
Smart Images

Figure 0007559225000001 
Figure 0007559225000002
Abstract
Description
[Technical field]
[0001] The present invention relates to an installation and a method for the continuous casting and subsequent flat rolling of steel strip having an austenitic and / or ferritic microstructure and a thickness of less than 1.0 mm, preferably less than 0.80 mm, particularly preferably in the range from 0.40 mm to 0.60 mm. [Background technology]
[0002] Such steel strip is usually produced by cold rolling a hot strip in a separate cold rolling mill, so at least two or three processing steps are required to produce such thin steel strip with an austenitic and / or ferritic microstructure.
[0003] From the German publication DE 11 2013 000 841 T5 an installation for producing thin steel strip is known, in which a cast steel strip having a thickness of 1 mm to 5 mm is cast and can be hot rolled directly in a hot rolling line to a thin steel strip, however, in such an installation a suitable production of steel strip with an austenitic and / or ferritic microstructure is not realized. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] DE112013000841T5 Summary of the Invention [Problem to be solved by the invention]
[0005] Against this background, the problem underlying the present invention is to provide an improved installation compared to the prior art and an improved method compared to the prior art, in particular an installation or a method which allows the production of steel strip having an austenitic and / or ferritic microstructure and a thickness of less than 1.0 mm. [Means for solving the problem]
[0006] Description of the invention According to the invention, this problem is solved by an installation having the features of claim 1 and by a method having the features of claim 8.
[0007] The installation according to the invention is provided and / or suitable for the continuous casting and subsequent flat rolling of steel strip having an austenitic and / or ferritic structure and a thickness of less than 1.0 mm, comprising a casting device, by means of which blank steel strip having a thickness in the range of 1.50 mm to 4.0 mm can be continuously cast, and at least one hot rolling stand connected to the casting device, by means of which the blank steel strip, still in the austenitic and / or ferritic structure range, can be hot pre-rolled into a steel strip immediately after the casting process.
[0008] According to the invention, the installation comprises at least one rolling module arranged immediately downstream of a hot rolling stand connected to a casting device, the rolling module comprising, in this order, a cooling device, a heating device and a hot rolling stand, by means of which the pre-rolled steel strip can be hot-finished rolled into a steel strip in the austenitic and / or ferritic range.
[0009] Similarly, the present invention contemplates a method for producing a steel strip having an austenitic and / or ferritic structure and a thickness less than 1.0 mm, which comprises first continuously casting a steel strip having a thickness ranging from 1.50 mm to 4.0 mm in a casting apparatus and then hot pre-rolling the steel strip in the austenitic and / or ferritic range at a higher temperature, preferably at least 700° C., to a steel strip using at least one hot rolling stand directly connected to the casting apparatus.
[0010] According to the invention, the steel strip which has been hot pre-rolled in the austenitic and / or ferritic structure range is hot finish rolled into austenitic and / or ferritic steel strip via at least one rolling module which comprises a cooling device, a heating device and a hot rolling stand in this order and which is arranged immediately downstream of the hot rolling stand which is connected to a casting device.
[0011] The plant or the method on the one hand allows for improved economy in the production of hot steel strip, especially in the production of very thin hot steel strip, since delivery times can be significantly shortened due to the savings in process steps, investment costs can be reduced and significant energy savings can be achieved.
[0012] The combination of "and / or" in the term "austenitic and / or ferritic structure" is understood in the context of the present invention to mean that the steel strip to be produced has, at the end of the process, an austenitic or ferritic structure and can be rolled during production not only with austenite but also with ferrite, in other words the steel strip to be produced does not have, at the end of the process, substantially a mixed austenitic and ferritic structure.
[0013] The term "very thin hot steel strip" is understood in the sense of the present invention to mean a steel strip having a thickness of less than 1.0 mm, preferably less than 0.80 mm, particularly preferably in the range from 0.40 mm to 0.60 mm. More particularly preferably, the steel strip having an austenitic and / or ferritic structure has a thickness of 0.4 mm.
[0014] Furthermore, the austenite and / or ferrite microstructure of the steel strip can be precisely set via at least one rolling module. For example, in order to produce a ferrite microstructure in the steel strip, the steel strip hot pre-rolled with austenite or ferrite is cooled via a cooling device and then finish-rolled with ferrite in a rolling stand of a rolling module, preferably at a temperature range of 700° C. to 780° C. In contrast, if an austenite microstructure is to be set in the steel strip, the steel strip hot pre-rolled with austenite or ferrite is heated via a heating device and then finish-rolled with austenite in a rolling stand of a rolling module, preferably at a temperature above 850° C.
[0015] Further advantageous embodiments of the invention are defined in the dependent claims. The features individually defined in the dependent claims can be combined with one another in a technically meaningful manner to define further embodiments of the invention. Furthermore, the features defined in the claims are explicitly indicated and explained in the description, thereby forming further preferred embodiments of the invention.
[0016] In an advantageous embodiment, the plant can have at least two, more preferably at least three rolling modules arranged one after the other, each having a cooling device, a heating device and a hot rolling stand in this order, so that hot rolling in the austenitic and / or ferritic ranges is accordingly possible, as a result of which the total degree of change in the respective austenitic and / or ferritic ranges can be varied depending on the number of changes used, which can advantageously influence the quality parameters of the steel strip.
[0017] In another advantageous embodiment, the installation may further comprise a heating device arranged between the casting device and the hot rolling stand connected to the casting device, thereby allowing precise heating of the raw steel strip coming from the casting device before it is hot pre-rolled in austenite in the hot rolling stand.
[0018] Preferably, the installation comprises at least one cooling section downstream of at least one rolling module, particularly preferably downstream of the last rolling module, via which the steel strip is cooled to the coiling temperature. In this connection, it is advantageously provided for the installation to comprise at least one coiler device, more preferably at least two coiler devices, via which the finished steel strip is wound into a coil. Usually, the installation further comprises a separating device arranged upstream of the coiler device for separating the steel strip.
[0019] In another embodiment, the installation may further comprise a pickling unit for pickling the steel strip and / or a heat treatment unit for annealing the steel strip, the units being further preferably arranged between the last rolling module and the cooling section.
[0020] In another aspect, the present invention further relates to the use of the device according to the invention for the precise production of steel strip having an austenitic and / or ferritic microstructure and a thickness of less than 1.0 mm, preferably less than 0.80 mm, particularly preferably in the range of 0.40 mm to 0.60 mm.
[0021] The present invention and its technical environment will be described in detail below with reference to the drawings. Please note that the present invention should not be limited by the illustrated embodiments. In particular, unless otherwise specified, it is possible to extract partial aspects of the matters described in the drawings and combine them with other components and understandings understood from this specification and / or the drawings. In particular, please note that the relationships between the drawings and the values particularly indicated are merely schematic. Since the same reference numerals indicate the same objects, the description of other drawings may be used supplementarily as necessary. [Brief description of the drawings]
[0022] [Figure 1] 1 shows a first embodiment of the installation according to the invention. [Diagram 2] 2 shows a second embodiment of the installation according to the invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Figure 1 shows an embodiment of a plant 1 which makes it possible to produce, by continuous casting and subsequent flat rolling, a steel strip 2 having an austenitic and / or ferritic structure and a thickness of less than 1.0 mm.
[0024] In the embodiment shown here, the plant 1 comprises a casting device 3, which is continuously fed with molten steel. Via the casting device 3, a blank steel strip 4 having a thickness in the range of 1.50 mm to 4.0 mm is firstly continuously cast. A first heating device 5 is arranged downstream of the casting device 3 in the direction of strip travel, by means of which the blank steel strip 4 can be heated upstream of a first rolling stand, if the temperature falls below 700° C. and / or if the first transformation step is to be carried out in the austenitic range. The first heating device 5 can, for example, be configured in the form of an induction heating device. Furthermore, the plant 1 comprises a first hot rolling stand 6, which is directly connected to the casting device 3. The term "directly connected" is understood in the sense of the present invention to mean that the first hot rolling stand 6 is arranged immediately downstream of the casting device 3 in the direction of strip travel, so that the raw steel strip 4 produced by the casting device 3 can be hot pre-rolled directly, and therefore in the austenitic and / or ferritic structure range.
[0025] Furthermore, downstream of the first hot rolling stand 6 in the strip travel direction, the installation 1 comprises a first rolling module 7 which comprises in this order a first cooling device 8, a second heating device 9 and a second hot rolling stand 10 by means of which the austenitic and / or ferritic pre-rolled strip 2 is hot-finished into a strip 2 in the austenitic and / or ferritic structure range. The second heating device 9 may also be configured, for example, in the form of an induction heating device. The first cooling device 10 may be configured, for example, in the form of an intermediate stand cooling device.
[0026] Downstream of the first rolling module 7 in the strip travel direction, the installation 1 first has a cooling section 11, preferably configured in the form of a spray cooler, by means of which the strip 2 rolled to the desired final strip thickness, for example of 0.4 mm, can be cooled carefully on the basis of very small thicknesses. Following this, the strip 2 passes through a separator 12, which may for example consist of a cantilever shear, and is wound into a coil via a first and / or second coiler device 13, 14.
[0027] FIG. 2 shows a second embodiment of the plant 1 according to the invention, which differs from the first embodiment in that it has a second rolling module 15 which likewise has a second cooling device 16, a third heating device 17 and a third hot rolling stand 18, via which rolling in the austenitic and / or ferritic structure range is possible.
[0028] Working Example Example 1 To produce a steel strip 2 with a pure austenitic structure, a blank steel strip 4 with a thickness of 2.0 mm and a width of 1100 mm is first cast using the plant 1 shown in Fig. 1. The blank steel strip 4 has a temperature of 1250°C when it leaves the casting device 3 and is then heated via an induction heating device 5 from an inlet temperature of 1157°C to 1246°C. Following this, the blank steel strip 4 is hot pre-rolled in austenite with a reduction of 55% at a rolling speed of 2.52 m / s in a first hot rolling stand 6, the inlet temperature being 1130°C and the outlet temperature being 971°C. The resulting austenitically pre-rolled steel strip 2 with a thickness of 0.9 mm is subsequently finish-rolled through the first rolling module 7 by first being heated via an induction heater 9 to a temperature of 938°C to 1051°C and then finish-rolled in austenite in the second hot rolling stand 10 at a rolling speed of 3.78 m / s with a drop of 33%. The inlet temperature to the second hot rolling stand 10 is 992°C and the outlet temperature is 882°C. The steel strip 2 thus obtained with a final strip thickness of 0.6 mm is subsequently cooled and wound into a coil.
[0029] Example 2 To produce a steel strip 2 with a pure ferritic structure, a blank steel strip 4 having a thickness of 2.0 mm and a width of 1100 mm is first cast using the plant 1 shown in Fig. 1. The blank steel strip 4 has a temperature of 1250°C when it leaves the casting device 3 and, due to the sufficiently high temperature, is fed without heating to a hot rolling stand 6 where it is pre-rolled in austenite with a drop of 55% at a rolling speed of 2.22 m / s, the inlet temperature being 1020°C and the outlet temperature being 882°C. The austenitic pre-rolled strip 2 then obtained with a thickness of 0.9 mm is subsequently finish-rolled in ferritic via the first rolling module 7 by first cooling the strip 2 via a cooling device 8 to a temperature of 794°C to 785°C and then hot-finish rolling in the second hot rolling stand 10 at a rolling speed of 3.33 m / s with a drop of 33%. The inlet temperature to the second hot rolling stand 10 is 757°C and the outlet temperature is 705°C. The strip 2 thus obtained with a final strip thickness of 0.6 mm is subsequently cooled and wound into a coil. This application relates to the invention described in the claims, but also includes the following as other aspects. 1. An installation (1) for the continuous casting and subsequent flat rolling of steel strip (2) having an austenitic and / or ferritic microstructure and a thickness of less than 1.0 mm, a casting device (3) capable of continuously casting a blank steel strip (4) having a thickness in the range of 1.50 mm to 4.0 mm; at least one hot rolling stand (6) connected to the casting device (3), by means of which the blank steel strip (4), still in the austenitic and / or ferritic range, can be hot pre-rolled into the steel strip (2) immediately after the casting process; In the equipment (1), 1. An installation (1), comprising at least one rolling module (7) arranged immediately downstream of a hot rolling stand (6) connected to a casting device (3), the rolling module (7) comprising, in this order, a cooling device (8), a heating device (9) and a hot rolling stand (10), by means of which the pre-rolled steel strip (2) can be hot-finished into austenitic and / or ferritic steel strip (2). 2. The installation (1) according to claim 1, comprising at least two, preferably at least three rolling modules (7, 15) arranged one behind the other, each of the rolling modules (7, 15) comprising a cooling device (8, 16), a heating device (9, 17) and a hot rolling stand (10, 18) in this order. 3. 3. The installation (1) according to claim 1 or 2, further comprising at least one cooling section (11) provided downstream of at least one rolling module (7), preferably downstream of the last rolling module (15). 4. 4. The installation (1) according to any one of claims 1 to 3, further comprising at least one heating device (5) arranged upstream of a hot rolling stand (6) connected to the casting device (3). 5. 5. The installation (1) according to any one of claims 1 to 4, further comprising a pickling unit for pickling the metal strip (2) and / or a heat treatment unit for annealing the metal strip (2), arranged downstream of at least one rolling module (7), preferably downstream of the last rolling module (15). 6. 6. The installation (1) of any one of 1 to 5 above, further comprising at least one, preferably at least two coiler devices (13, 14) for winding the steel strip (2) to form a coil. 7. The installation (1) of claim 6, further comprising a separating device (12) for separating the steel strip (2), disposed upstream of the at least one coiler device (13, 14). 8. A method for producing a steel strip (2) having an austenitic and / or ferritic microstructure and a thickness of less than 1.0 mm, comprising the steps of: A method for producing a steel strip (4) having a thickness ranging from 1.50 mm to 4.0 mm, which is first continuously cast in a casting device (3) and then hot pre-rolled into a steel strip (2) in the austenitic and / or ferritic range at a higher temperature, preferably at least 700° C., using at least one hot rolling stand (6) directly connected to the casting device (3), 1. A method according to claim 1, characterized in that the hot pre-rolled steel strip (2) is hot finish rolled into austenitic and / or ferritic steel strip (2) through at least one rolling module (7) having a cooling device (8), a heating device (9) and a hot rolling stand (10) in that order and arranged immediately downstream of a hot rolling stand (6) connected to a casting device (3). 9. 8. Use of the installation (1) according to any one of claims 1 to 7 for producing a steel strip (2) having an austenitic and / or ferritic microstructure and a thickness of less than 1.0 mm. [Explanation of symbols]
[0030] 1 equipment 2. Steel strip 3 Casting Equipment 4. Steel strip material 5 First heating device / induction heating device 6. First hot rolling stand 7 (First) Rolling Module 8. First cooling device 9 Second heating device / induction heating device 10 No. 2 hot rolling stand 11 Cooling section / spray cooling device 12 Separation device 13 First coiler device 14 Second coiler device 15 Second rolling module 16 Second cooling device 17 Third heating device 18. 3rd hot rolling stand
Claims
1. A method for producing an extremely thin steel strip (2) having an austenitic and / or ferritic microstructure and a thickness of less than 0.8 mm, comprising the steps of: A method for producing a steel strip (4) having a thickness ranging from 1.50 mm to 4.0 mm, which is first continuously cast in a casting device (3) and then hot pre-rolled in the austenitic and / or ferritic range to a steel strip (2) by means of at least one hot rolling stand (6) directly connected to the casting device (3), 1. A method according to claim 1, further comprising the step of hot finish rolling the pre-hot rolled steel strip (2) into an extremely thin steel strip (2) in austenite and / or ferrite through at least one rolling module (7) having a cooling device (8), a heating device (9) and a hot rolling stand (10) in that order and arranged immediately downstream of a hot rolling stand (6) connected to a casting device (3).
2. A method as described in claim 1, in which the hot pre-rolled steel strip (2) is finish rolled via at least two rolling modules (7, 15) arranged one behind the other, each of the rolling modules (7, 15) having a cooling device (8, 16), a heating device (9, 17) and a hot rolling stand (10, 18) in that order.
3. A method according to claim 1 or 2, in which the extremely thin steel strip (2) is cooled to the coiling temperature via at least one cooling section (11) downstream of at least one rolling module (7) or downstream of the last rolling module (15).
4. An equipment (1) as described in any one of claims 1 to 3, in which a raw steel strip (4) is heated via at least one heating device (5) arranged upstream of a hot rolling stand (6) connected to a casting device (3).
Citation Information
Patent Citations
Method for producing a weather-resistant continuous thin-strip cast steel exhibiting high strength with a grade of 700 MPa
DE112013000841T5
Method and finish rolling line for hot rolling incoming material
JP2009513360A
Method of casting and rolling steel using twin-roll caster
WO1996001710A1
Thermomechanical treatment method
WO2011079341A2