Sulfur-Curable Rubber Mixtures, Vulcanizates, and Vehicle Tires

A rubber mixture with polyisoprene, silica, and silane B addresses high heat and poor tearing issues in vehicle tires, enhancing durability and processability, resulting in improved tire performance and service life.

JP7559242B2Active Publication Date: 2024-10-01CONTINENTAL REIFEN DEUTSCHLAND GMBH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023532131
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-12-08
Filing Date
2021-11-08
Publication Date
2024-10-01
Estimated Expiration
2041-11-08

AI Technical Summary

Technical Problem

Existing rubber mixtures for vehicle tires, particularly those used in internal components, suffer from high heat build-up and poor tearing performance, which affect durability and service life, while also being difficult to process effectively.

Method used

A rubber mixture comprising 50 to 100 phr of polyisoprene, 5 to 500 phr of silica, and a specific silane B with a defined empirical formula, which improves heat generation and friction properties, enhancing processability and tear resistance.

Benefits of technology

The rubber mixture achieves reduced heat build-up, improved durability, and enhanced tearing performance, with better processability and adhesion to strength members, leading to improved tire service life and rolling resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559242000001
    Figure 0007559242000001
  • Figure 0007559242000002
    Figure 0007559242000002
  • Figure 0007559242000003
    Figure 0007559242000003
Patent Text Reader

Abstract

The present invention relates to a sulfur-crosslinkable rubber mixture, a vulcanizate, and a vehicle tire, the sulfur-crosslinkable rubber mixture comprising at least the following components: 50 to 100 phr of at least one polyisoprene selected from the group consisting of natural and synthetic polyisoprenes; and 5 to 500 phr of at least one silicic acid; and at least one silicic acid represented by general empirical formula I, (R 1 ) o Si-R 2 -S n -R 2 -Si(R 1 ) o Silane B having the formula 2 may be the same or different and are each independently an unbranched alkylene group having 6 to 20 carbon atoms, preferably 6 to 10 carbon atoms, where n is an integer of 2 to 10.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to sulfur-crosslinkable rubber mixtures, vulcanizates thereof, and vehicle tires. [Background technology]

[0002] The rubber mixture of the various components greatly influences the driving performance and the service life of a vehicle tire. At the same time, the components of the internal tire or their mixture (also called body mixture) as well as the tread that is in contact with the road influence the durability and the service life of the tire. As is known, the components of the internal tire also include strength members for reinforcement, such as belt plies. These strength members are ensheathed by one or more rubber mixtures, and are therefore rubber-coated. The corresponding rubber mixtures are also called rubber-coated mixtures.

[0003] Such rubber coating mixtures are also described, for example, in EP 2 746 327 B1.

[0004] In the rubber coating mixture, as is generally the case for internal tire components, the crucial factors are heat build-up due to the stresses encountered during driving operations and durability. Summary of the Invention [Problem to be solved by the invention]

[0005] The object of the present invention is to provide a rubber mixture, in particular for the internal tire components and in particular for encasing strength members, which is characterized by a lower and therefore improved heat build-up and improved tear performance, while at the same time the rubber mixture must have better processability. [Means for solving the problem]

[0006] The object is achieved by a rubber mixture comprising: - from 50 to 100 phr of at least one polyisoprene selected from the group consisting of natural and synthetic polyisoprenes, and - from 5 to 500 phr of at least one silica, and at least one silane B having the general empirical formula I), [ka] [wherein, two o's may be independently the same or different and may each take the value of 1, 2, or 3; R 1 The groups may be independently the same or different, and are each an alkoxy group having 1 to 10 carbon atoms, a cycloalkoxy group having 4 to 10 carbon atoms, a phenoxy group having 6 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, an alkyl group having 1 to 10 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a halide, or an alkyl polyether group -O-(R 6 -O) r -R 5 (where R 6 are the same or different, branched or unbranched, saturated or unsaturated, aliphatic, aromatic, or mixed aliphatic / aromatic bridges C 1 ~C 30 Hydrocarbon groups, preferably -CH 2 -CH 2 -, r is an integer from 1 to 30, preferably from 3 to 10, R 5 is an unsubstituted or substituted, branched or unbranched, terminal alkyl, alkenyl, aryl or aralkyl group, preferably -C 13 H 27 alkyl group; Or, 2 R's 1 forms a cyclic dialkoxy group having 2 to 10 carbon atoms (in which case o is less than 3); Or, two or more silanes of formula I) are R 1 In formula I), each (R 1 ) o Among the Si-groups, at least one R 1 is selected from the above options, this R 1 is i) bonded to the silicon atom through an oxygen atom or ii) is a halide; R 2 groups may be independently the same or different and are unbranched alkylene groups having 6 to 20 carbon atoms, preferably 6 to 10 carbon atoms, and n is an integer from 2 to 10.

[0007] Surprisingly, it has been found that by combining the above-mentioned components, improvements in heat buildup and friction can be achieved.

[0008] The present invention further provides a vulcanizate of at least one rubber mixture according to the invention.

[0009] The invention further provides a vehicle tire comprising, at least one component thereof, at least one inventive vulcanizate of the inventive rubber mixture. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The vehicle tyre according to the invention preferably comprises the vulcanizate according to the invention, in particular as a rubber coating mixture, in particular as a steel cord rubber coating and / or as a belt rubber coating, and / or in the sidewall, and / or in the tread and / or in further tyre components, such as in particular the belt cushion.

[0011] In an advantageous embodiment of the invention, the vehicle tire comprises at least one vulcanizate according to the invention at least in its internal components, for example, in particular as a rubber coating mixture, for example, in particular as a rubber coating of the belt and / or as a belt cushion.

[0012] However, the rubber mixtures according to the invention are in principle equally suitable for the sidewalls and / or treads.

[0013] The vulcanizates according to the invention and the vehicle tires according to the invention are distinguished in particular by improved durability and service life.

[0014] Vehicle tyres are to be understood in the context of the present invention to mean pneumatic vehicle tyres and all-rubber tyres, such as tyres for vehicles on factories and construction sites, truck tyres, passenger car tyres and bicycle tyres.

[0015] The rubber mixtures of the invention are also suitable for other industrial rubber articles, such as, for example, bellows, conveyor belts, air springs, belts, power transmission belts or hoses, and shoe soles.

[0016] In the following, the constituents of the sulfur-crosslinkable rubber mixture of the invention are explained in detail. All the statements furthermore relate to the vulcanizate of the invention and to the vehicle tire of the invention, which comprises, in at least one component thereof, the vulcanizate of the invention of at least one rubber mixture of the invention.

[0017] The present invention includes all advantageous configurations, as reflected in the patent claims or otherwise. More specifically, the present invention also includes configurations resulting from combinations of various features of the components in the rubber mixture, various levels of suitability of these features, such as, for example: a combination of a first feature described as "preferred" or a feature described in the context of an advantageous embodiment with a feature described as, for example, "particularly preferred" is included in the present invention, unless it is clear from the technical reasons or context that this is not the case.

[0018] As used herein, the unit "phr (parts per hundred parts of rubber by weight)" is a unit of quantity commonly used in the rubber industry for compounding mixtures. The dosage of each substance in this specification is determined by the weight of the molecular weight M of the rubber by GPC greater than 20,000 g / mol. w The total weight of all rubbers present in the mixture is based on 100 parts by weight.

[0019] As used herein, the unit "phf (parts per hundred parts of filler by weight)" is a unit of quantity commonly used in the rubber industry for coupling agents for fillers.

[0020] In the context of this application, phf refers to the silica present, which means that any other fillers present, such as carbon black, are not included in calculating the amount of silane.

[0021] The rubber mixture of the present invention contains from 50 to 100 phr, preferably from 70 to 100 phr, more preferably from 75 to 100 phr, of at least one polyisoprene selected from natural polyisoprene (NR) and synthetic polyisoprene (IR).

[0022] The polyisoprene(s) has a weight average molecular weight M by GPC of 250,000 to 5,000,000 g / mol. w It is preferred that the ion exchange resin has the following structure:

[0023] The natural and / or synthetic polyisoprene in all embodiments may be either cis-1,4-polyisoprene or 3,4-polyisoprene. However, it is preferred to use cis-1,4-polyisoprene with a cis-1,4 content of more than 90% by weight. In the first place, such polyisoprene can be obtained by stereospecific polymerization in solution using Ziegler-Natta catalysts or by using finely dispersed lithium alkyls. In the second place, natural rubber (NR) is cis-1,4-polyisoprene, and the cis-1,4 content in natural rubber is greater than 99% by weight.

[0024] Additionally, mixtures of one or more natural polyisoprenes with one or more synthetic polyisoprenes are also contemplated.

[0025] In the context of the present invention, "natural rubber" is understood to mean the naturally occurring rubber obtainable from the Hevea rubber tree and from "non-Hevea" starting sources, such as the guayule bush and dandelions, such as TKS (Taraxacum kok-saghyz; Russian dandelion).

[0026] If the rubber mixture contains less than 100 phr of NR and / or IR, it contains at least one further diene rubber.

[0027] Diene rubber refers to rubbers formed by polymerizing or copolymerizing dienes and / or cycloalkenes and therefore having C=C double bonds in either the backbone or in side groups.

[0028] In this case, the further diene rubber is preferably selected from the group consisting of epoxidized polyisoprene, butadiene rubber (BR), butadiene-isoprene rubber, solution-polymerized styrene-butadiene rubber (SSBR), emulsion-polymerized styrene-butadiene rubber (ESBR), styrene-isoprene rubber, and polyisoprene rubbers with a molecular weight M of more than 20,000 g / mol. w rubber, halobutyl rubber, polynorbornene, isoprene-isobutylene copolymer, ethylene-propylene-diene rubber, nitrile rubber, chloroprene rubber, acrylate rubber, fluororubber, silicone rubber, polysulfide rubber, epichlorohydrin rubber, styrene-isoprene-butadiene terpolymer, hydrogenated acrylonitrile-butadiene rubber, and hydrogenated styrene-butadiene rubber.

[0029] In particular, nitrile rubber, hydrogenated acrylonitrile-butadiene rubber, chloroprene rubber, butyl rubber, halobutyl rubber or ethylene-propylene-diene rubber are used in the manufacture of industrial rubber articles, such as belts, transmission belts and hoses, and / or shoe soles. The mixture compositions preferably employed here are those known to those skilled in the art for these rubbers, in particular fillers, plasticizers, vulcanization systems and additives.

[0030] In an advantageous embodiment, the further diene rubber, in particular in the case of the use of the rubber mixture in vehicle tires, is selected from the group consisting of butadiene rubber (BR), solution-polymerized styrene-butadiene rubber (SSBR), emulsion-polymerized styrene-butadiene rubber (ESBR), butyl rubber (IIR) and halobutyl rubber.

[0031] In an advantageous embodiment of the invention, the rubber mixture comprises 75 to 99 phr NR and 1 to 25 phr BR, preferably 75 to 85 phr NR and 15 to 25 phr BR, for example and in particular 80 phr NR and 20 phr BR.

[0032] Such rubber mixtures are particularly well suited as rubber coating mixtures, in particular as rubber coatings for belts, in which the objectives on which the invention is based are achieved particularly well.

[0033] According to the invention, the rubber mixture contains from 5 to 500 phr of at least one silica.

[0034] The silica may be of the type known to those skilled in the art to be suitable as a filler for tire rubber compounds. 2 / g, preferably 35 to 350m 2 / g, more preferably 85 to 320 m 2 / g, most preferably 120 to 235 m 2 / g nitrogen surface area (BET surface area) (according to DIN ISO 9277 and DIN 66132) and 30 to 400 m 2 / g, preferably 30 to 330m 2 / g, more preferably 80 to 300m 2 / g, most preferably 110 to 230m 2 It is particularly preferred to use fine precipitated silicas having a CTAB surface area (according to ASTM D 3765) of 10 ...

[0035] In a preferred embodiment of the invention, the rubber mixture of the invention comprises from 20 to 300 phr, preferably from 20 to 250 phr, more preferably from 40 to 150 phr, even more preferably from 40 to 100 phr, more preferably still from 50 to 70 phr of at least one silica.

[0036] If at least two different silicas, differing, for example, in terms of their BET surface area, are present in the rubber mixtures according to the invention, the above amounts are in each case based on the total amount of all silicas present.

[0037] The rubber mixtures of the invention may further comprise at least one carbon black, in particular industrial carbon black.

[0038] Useful carbon blacks include all types of carbon black known to those skilled in the art.

[0039] In one embodiment, the carbon black has an iodine number (also called iodine adsorption number) according to ASTM D 1510 of between 30 and 250 g / kg, preferably between 30 and 180 g / kg, more preferably between 40 and 180 g / kg, and most preferably between 40 and 130 g / kg, and a DBP number according to ASTM D 2414 of between 30 and 200 mL / 100 g, preferably between 70 and 200 mL / 100 g, and more preferably between 90 and 200 mL / 100 g.

[0040] The DBP number according to ASTM D 2414 defines the specific absorption volume of a carbon black or light colored filler by means of dibutyl phthalate.

[0041] The use of such types of carbon black in rubber mixtures, especially for vehicle tires, ensures the best possible compromise between wear resistance and heat build-up, which therefore also influences the environmentally important rolling resistance. In this case, it is preferred to use only one type of carbon black in each rubber mixture, but it is also possible to mix different types of carbon black in a rubber mixture. The total amount of carbon black present is preferably between 0 and 250 phr.

[0042] In an advantageous embodiment of the invention, the rubber mixture comprises from 0 to 20 phr, preferably from 0 to 10 phr, of at least one carbon black and from 40 to 500 phr, preferably from 40 to 100 phr, of at least one silica.

[0043] The rubber mixtures of the invention may preferably contain a minimum amount, i.e. preferably between 0 and 20 phr, more preferably between 0 and 10 phr, of further (non-reinforcing) fillers, which in the context of the present invention include aluminosilicates, kaolin, chalk, starch, magnesium oxide, titanium dioxide or rubber gels, and fibres (for example aramid fibres, glass fibres, carbon fibres, cellulose fibres).

[0044] Further reinforcing and non-reinforcing fillers are, for example, carbon nanotubes (CNTs) (including discrete CNTs, also called hollow carbon fibers (HCFs), and modified CNTs that contain one or more functional groups, such as hydroxy, carboxy, and carbonyl groups), graphite, and graphene, as well as what are referred to as "carbon-silica dual-phase fillers."

[0045] In the context of the present invention, zinc oxide is not included among the fillers.

[0046] According to the invention, the rubber mixture contains at least one silane B having the general empirical formula I). [ka] (Definition above)

[0047] At least one silane B present in the present invention is S n Because of the presence of the sulfur group S and because n is at least 2, n The silanes are capable of bonding to the polymer by means of the above formula (1), where n is an integer from 2 to 10, preferably from 2 to 8, more preferably from 2 to 6, and may be a mixture of different molecules with different values ​​of n.

[0048] Most preferably, n is an integer of 2 to 4.

[0049] In a particularly advantageous embodiment of the invention, n is 2.

[0050] In a further particularly advantageous embodiment of the invention, n is 4.

[0051] Furthermore, R 2 It is essential to the present invention that the groups, which may be independently the same or different, are unbranched alkylene groups having from 6 to 20 carbon atoms, preferably from 6 to 10 carbon atoms.

[0052] Surprisingly, it is possible to obtain a silane having 6 to 20 carbon atoms, in particular a propyl having 3 carbon atoms in the silane, for example TESPD (3,3'-bis(triethoxysilylpropyl) disulfide) or TESPT (3,3'-bis(triethoxysilylpropyl) tetrasulfide), R 2 It has been found that by extending the group the basic objective of the present invention is achieved.

[0053] R 2 is the same on both sides, and therefore is preferably -(CH 2 ) 8 It is more preferred that it is a - group.

[0054] R 1 The R 1 One or more silane bridges via groups may all be bonded to each other within the silyl group.

[0055] 2 R's 1 corresponds to a dialkoxy group having 2 to 10 carbon atoms, and if o<3 (o is less than 3), then the silicon atom is part of a ring structure.

[0056] If two silanes of formula I) are bridged to each other, they may be linked by the formula R 1 Either share a group or two Si-R 1 - groups are combined to be bonded to each other via an oxygen atom. In this way, it is also possible that more than two silanes are bonded to each other. Thus, after synthesis of the silane of formula I), it is possible to combine the oxygen atom or the R 1 It is also possible that three or more silanes are linked together, for example via dialkoxy groups.

[0057] The rubber mixtures according to the invention therefore further comprise silanes B, which are reacted with silanes R 1 The copolymer may include oligomers formed by means of dialkoxy groups as alkyl groups.

[0058] The silanes of formula I are each 1 ) o In the Si-group, at least one R 1 However, among them, this R 1 is selected from the above options of i) bonded to the silicon atom through an oxygen atom, or ii) a halide, each (R 1 ) o At least one R 1 Contains a group.

[0059] More specifically, they are thus alkoxy groups, phenoxy groups, or various other groups mentioned above that are bonded to the silicon atom by an oxygen atom or a halide.

[0060] R 1 Preferably the group comprises an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms, or a halide, with alkoxy groups having 1 to 6 carbon atoms being particularly preferred.

[0061] Preferably, each (R 1 ) o In the Si-group, at least one R 1 However, it is preferable that the alkoxy group has 1 to 10 carbon atoms, and more preferably has 1 to 6 carbon atoms.

[0062] It is preferred that the o's on both sides of the molecule are 3.

[0063] In a particularly advantageous embodiment of the present invention, the silyl group (R 1 ) o R in Si- 1 The groups are the same and are alkoxy groups having 1 to 3 carbon atoms, preferably even having 1 or 2 carbon atoms, i.e. methoxy or ethoxy groups, most preferably ethoxy groups, where o is 3.

[0064] It can further be used in the case of oligomers or two R 1 This also applies to dialkoxy groups, and other R 1 The group is preferably an alkyl group or halide having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms, preferably 1 or 2 carbon atoms, i.e., a methoxy group or an ethoxy group, most preferably an ethoxy group.

[0065] In the context of the present invention, in the formula of the silane, the ethoxy group is represented in the abbreviated form as "EtO" or "OEt". These two notations indicate that an alkoxy group, such as an ethoxy group, is bonded to a silicon atom, Si, through an oxygen atom, O.

[0066] In principle, however, the abbreviations "OEt" or "EtO" can also be used synonymously in the context of the present invention.

[0067] In a preferred embodiment of the invention, the silane B has the following formula II: [ka] [wherein EtO represents an ethoxy group] It has the following structure.

[0068] In a further preferred embodiment of the present invention, the silane B has the following formula III: [ka] [wherein EtO represents an ethoxy group] It has the following structure.

[0069] In particular with the silanes of the formulae II) and / or III), the objective underlying the present invention is achieved in a particularly efficient manner.

[0070] The silane of formula III) is disclosed, for example, in EP 3567078A1 or EP 3312232A1. It is prepared in particular according to the method of EP 3567078A1, paragraph

[0097] combined with paragraph

[0095] , using 1 mole of sulfur.

[0071] Silanes of formula II) are prepared in a similar manner, in particular according to EP 3567078 A1, para. 0095, by using sulphur in an amount of 3 moles instead of 1.2 moles.

[0072] It is also conceivable that the rubber mixtures of the invention contain mixtures of two silanes of formula I), for example a mixture of a silane of formula II) with a silane of formula III).

[0073] The total amount of silane B represented by formula I) present is preferably 0.1 to 30 phf, preferably 0.5 to 20 phf, more preferably 0.5 to 15 phf.

[0074] In particular, preferred and especially preferred amounts and developments or embodiments result in improved processability and improved properties related to heat build-up and tear performance.

[0075] The silane B(s) present in the present invention may be applied to a support, such as wax, polymer or carbon black, and in that form applied to the rubber mixture. The silane B(s) present in the present invention may also be applied to silica, in which case the bonding may be by physical or chemical means.

[0076] By applying the silane B present in the present invention to silica, for example, volatile by-products such as ethoxy-substituted silanes (R 1 In the case of the use of ethylene glycol (ethylene glycol ethoxylate), the emission of ethanol is reduced.

[0077] It is further conceivable that the rubber mixture of the present invention comprises at least one further silane coupling agent which is not Silane B.

[0078] In addition, the rubber mixture may contain further activators and / or reactants for binding the fillers, especially the carbon black, which may be, for example, S-(3-aminopropyl)thiosulfate, the compounds disclosed in EP 2 589 619 A1, and / or their metal salts, which result in very good physical properties of the rubber mixture, especially in combination with at least one carbon black as filler.

[0079] The rubber mixture of the invention is in a preferred embodiment designed to encase (rubber coat) strength members, and for this purpose it preferably contains a bonding system for bonding the rubber mixture to textile or metal strength members.

[0080] Depending on whether the mixture is to be used for textile or metal strength members, either rubber-textile or rubber-metal bonding systems are employed.

[0081] Preferably, the bonding system is a steel cord bonding system based on cobalt compounds, especially selected from organic cobalt salts, as well as reinforcing resins and more than 2.5 phr of sulfur. Such mixtures, when in contact with metal strength members, have a particularly positive effect on the improvement of adhesion and cracking properties, since the latter lose adhesion and become subject to cracking, which would significantly impair the life of the elastomeric products, especially pneumatic vehicle tires.

[0082] The organic cobalt salt is typically used in an amount of 0.1 to 3 phr. The cobalt salt used may be, for example, cobalt stearate, cobalt borate, cobalt alkanoate borate, cobalt naphthenate, cobalt rosinate, cobalt octanoate, cobalt adipate, and the like.

[0083] The reinforcing resins used may be resorcinol-formaldehyde resins, such as resorcinol-hexamethoxymethylmelamine resins (HMMM) or resorcinol-hexamethylenetetramine resins (HEXA), or modified phenolic resins, such as the grades of Alnovol®. It is also possible to use precondensates of resorcinol resins.

[0084] The rubber mixtures according to the invention preferably contain from 2.5 to 8 phr of sulfur, more preferably from 3 to 8 phr of sulfur.

[0085] In an advantageous embodiment of the invention, the rubber mixture contains between 3.5 and 5 phr of sulphur.

[0086] In an advantageous embodiment of the invention, the rubber mixture comprises an organic cobalt salt and a reinforcing resin and more than 2.5 phr, in particular 3 to 6 phr, of a sulphur-based steel cord bonding system, the above remarks being also applicable to the cobalt salt and the reinforcing resin.

[0087] In addition, the rubber mixtures may contain conventional additives in conventional weight ratios, which are preferably added during at least one basic mixing stage of their preparation, such as: a) Aging stabilizers, such as N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (6PPD), N,N'-diphenyl-p-phenylenediamine (DPPD), N,N'-ditolyl-p-phenylenediamine (DTPD), N-isopropyl-N'-phenyl-p-phenylenediamine (IPPD), 2,2,4-trimethyl-1,2-dihydroquinoline (TMQ), b) activators such as zinc oxide and fatty acids (e.g., stearic acid) and / or other activators such as zinc complexes, e.g., zinc ethylhexanoate; c) wax, d) hydrocarbon resins, such as, if appropriate, in particular tackifying resins, e) Mastication aids such as 2,2'-dibenzamidodiphenyl disulfide (DBD), and f) processing aids, such as, in particular, fatty acid esters and metal soaps, such as zinc soaps and / or calcium soaps; g) Plasticizers.

[0088] Plasticizers to be used in the context of the present invention include all plasticizers known to the person skilled in the art, such as aromatic, naphthenic or paraffinic mineral oil plasticizers, such as MES (mild extraction solvate), or RAE (residual aromatic extract), or TDAE (treated distillate aromatic extract), or RTL (rubber-to-liquid oil), or BTL (biomass-to-liquid oil), preferably having a polyaromatic content of less than 3% by weight, as determined by the IP346 method, or triglycerides, such as rapeseed oil, or vulcanized oil, or hydrocarbon resins or liquid polymers having an average molecular weight between 500 and 20,000 g / mol (measured by GPC (=gel permeation chromatography) according to BS ISO 11344:2004). If additional liquid polymers are used as plasticizers in the rubber mixtures of the present invention, they are not included in the rubber in calculating the composition of the polymer matrix.

[0089] The plasticizer is preferably selected from the group consisting of those plasticizers mentioned above.

[0090] More preferably, the plasticizer is selected from the group consisting of hydrocarbon resins, liquid polymers, and mineral oils.

[0091] If mineral oils are used, they are preferably selected from the group consisting of: DAE (distillate aromatic extracts) and / or RAE and / or TDAE and / or MES and / or naphthenic oils.

[0092] In a preferred embodiment of the invention, the rubber mixture contains as plasticizer at least one mineral oil plasticizer, preferably at least TDAE and / or RAE, which gives the rubber mixture a particularly good processability, in particular a good compatibility.

[0093] In a preferred embodiment of the invention, the rubber mixture contains at least one liquid polymer as plasticizer.

[0094] In a preferred embodiment of the invention, the rubber mixture contains at least one hydrocarbon resin as plasticizer.

[0095] As will be appreciated by those skilled in the art, a hydrocarbon resin is a polymer formed from monomers, where the hydrocarbon resin is formally composed of the derivatives of the monomers by bonding them together. However, in the context of the present invention, such hydrocarbon resins are not counted as rubbers. The term "hydrocarbon resin" means, in the context of the present application, a resin having carbon and hydrogen atoms, and optionally containing heteroatoms, such as, in particular, oxygen atoms. The hydrocarbon resin may be a homopolymer or a copolymer.

[0096] The proportion of the further additives in the total amount is between 3 and 150 phr, preferably between 3 and 100 phr, more preferably between 5 and 80 phr.

[0097] The total proportion of further additives may include zinc oxide (ZnO).

[0098] It may be any type of zinc oxide known to those skilled in the art, for example ZnO granules or powder. Conventional zinc oxides are generally available in the form of 10 ml 2 / g. Alternatively, it has a BET surface area of ​​10 to 100 m 2 It is also possible to use zinc oxide having a BET surface area of ​​100 nm / g, such as that referred to as "nano zinc oxide".

[0099] In an advantageous embodiment of the invention, the rubber mixture contains from 1 to 10 phr, preferably from 3 to 10 phr, more preferably from 7 to 9 phr, of zinc oxide.

[0100] The vulcanization is preferably carried out in the presence of sulfur and / or sulfur donors, also with the aid of vulcanization accelerators, although some vulcanization accelerators can also simultaneously act as sulfur donors.

[0101] Sulfur and / or further sulfur donors and one or more vulcanization accelerators are added to the rubber mixture in the final mixing step, where the vulcanization accelerators are selected from the group consisting of thiazole vulcanization accelerators and / or mercapto vulcanization accelerators and / or sulfenamide vulcanization accelerators and / or thiocarbamate vulcanization accelerators and / or thiuram vulcanization accelerators and / or thiophosphate vulcanization accelerators and / or thiourea vulcanization accelerators and / or xanthogenate vulcanization accelerators and / or guanidine vulcanization accelerators.

[0102] It is preferred to use at least one sulfenamide vulcanization accelerator selected from the group consisting of N-cyclohexyl-2-benzothiazole sulfenamide (CBS) and / or N,N-dicyclohexylbenzothiazole-2-sulfenamide (DCBS) and / or benzothiazyl-2-sulfene morpholide (MBS) and / or N-tert-butyl-2-benzothiazyl sulfenamide (TBBS).

[0103] In a preferred embodiment of the invention, the rubber mixture contains DCBS as a vulcanization accelerator, which has been found to be particularly advantageous for the adhesion of steel cords to the rubber mixture due to its relatively slow reaction kinetics.

[0104] The sulfur donors used here may be any of the various sulfur donors known to those skilled in the art. If sulfur donors are present in the rubber mixture, they are preferably selected, for example, from the group comprising: thiuram disulfides, such as tetrabenzylthiuram disulfide (TBzTD) and / or tetramethylthiuram disulfide (TMTD) and / or tetraethylthiuram disulfide (TETD), and / or thiuram tetrasulfides, such as dipentamethylenethiuram tetrasulfide (DPTT), and / or dithiophosphates, such as DipDis (bis(diisopropyl)thiophosphoryl disulfide) and / or bis(O,O-2-ethylhexyl-thiophosphoryl) polysulfide (for example Rhenocure SDT 50®, from Rheinchemie GmbH) and / or zinc dichloryl dithiophosphate (for example Rhenocure ZDT / S®, from Rheinchemie GmbH). GmbH) and / or zinc alkyldithiophosphate, and / or 1,6-bis(N,N-dibenzylthiocarbamoyldithio)hexane, and / or diaryl polysulfides, and / or dialkyl polysulfides.

[0105] In the rubber mixtures it is also possible to use further network-forming systems, such as those available, for example, under the trade names Vulkuren®, Duralink® or Perkalink® or as described in WO 2010 / 049216 A2, which comprise a vulcanizing agent crosslinking with a functionality of 5 or more and at least one vulcanization accelerator.

[0106] The rubber mixtures according to the invention are used for producing vehicle tyres, and for producing power transmission belts, belts and hoses.

[0107] More specifically, the rubber mixture serves to manufacture at least one internal component of a vehicle tire, which may be any conceivable type of tire in which a strength member is used.

[0108] A further aspect of the present invention are strength members encased with the rubber mixture of the present invention.

[0109] All the above remarks are applicable to the constituents of the rubber mixture according to the invention.

[0110] The strength members of the present invention are preferably constructed from at least one steel.

[0111] The rubber mixtures according to the invention are in particular coating mixtures for steel cord rubber, which offer the advantages associated with the invention in terms of the good adhesion of the rubber mixture to steel.

[0112] The steel strength members may in principle be any type of steel strength member known to the person skilled in the art, who in this context is able to select the configuration of the strength members and in particular their strength class.

[0113] The rubber mixture is prepared by the methods conventional in the rubber industry, in which a base mixture containing all the components except the vulcanization system (sulphur and substances influencing the vulcanization) is first prepared in one or more mixing stages, with the vulcanization system being added in the last mixing stage, thereby obtaining a mixture ready for use.

[0114] In the case of rubber coating mixtures, the strength members are partially or completely covered with the rubber mixture of the invention. This is achieved by calendaring the rubber mixture, in which thin sheets are produced from the rubber mixture and placed above and below the strength members. The rubber mixture penetrates the exterior and interior of the strength members. After cutting to size, the strength members are equipped with the rubber mixture and are further used to produce the required end product, as known to those skilled in the art.

[0115] The rubber mixtures of the invention for use as tread, sidewall or other body mix in vehicle tires are produced as described above. The difference is the shaping of the mixture in an extrusion operation or in calendaring. The shaping of the still unvulcanized rubber mixtures thus obtained for one or more different body mixes, sidewalls or treads then serves for the construction of tire blanks.

[0116] The invention will now be illustrated in more detail by comparative examples and working examples, summarized in Table 1.

[0117] The rubber mixture according to the invention (E1) and the comparative mixture (V1) are each rubber coating mixtures for steel cords.

[0118] The amount of silane in phf is based on 60 phr of silica.

[0119] In the case of E1 vs. V1, there was an equimolar displacement of silane, resulting in a difference in the amount in the phf.

[0120] The mixes were alternatively prepared in three stages under standard conditions in laboratory mixers of 300 ml to 3 liters capacity, as is customary in the rubber industry, except that in the first mixing stage (base mix stage), all the components except the vulcanization system (sulfur and vulcanization-influencing substances) were first mixed at 145-165°C (target temperature 152-157°C) for 200-600 seconds. In the second stage, the mix from stage 1 was mixed once more, performing what is called a "remill". In the third stage (ready-mix stage), the vulcanization system was added and mixed at 90-120°C for 180-300 seconds to produce the finished mix.

[0121] Using all mixtures, t 95 ~t 100 After the rheological properties (measured using a moving die rheometer in accordance with ASTM D 5289-12 / ISO 6502), test specimens were prepared by vulcanization at 160°C to 170°C under pressure, and the typical physical properties in the rubber industry were confirmed using the test methods specified below. - Mooney Viscosity (ML1+4), 100°C, conforms to ASTM D 1646 (2004) - Resilience, at room temperature (RT), according to DIN 53 512 and ISO 4662 - Tensile strength and elongation at break at 100°C according to DIN 53 504 - maximum loss factor tan d (= tan δ max.) and dynamic storage modulus E' at 55°C and 100°C (by dynamic mechanical measurement according to DIN 53 513 (strain sweep of 0.15% and elongation of 8%) - Adhesion (rubber coating, room temperature RT, average value) and pull-out force (average value) (according to ASTM D2229-10), code used: 1+5 * 0.4HT (high tension)

[0122] The figures for tensile strength at 100°C, elongation at break at 100°C, pull-out force and coverage are each given as a percentage of performance when the performance of V1 is normalized to 100% in each case.

[0123] The substances used were as follows: a) Silica: Hi-Sil EZ160G (PPG) b) Processing aids and plasticizers: oils and hydrocarbon resins (plasticizer resins) c) [ka] (Prepared according to

[0095] of EP 3567078 A1, the amount of sulfur was 3 moles instead of 1.2 moles) d) Cobalt salt: Co alkanoate borate, 22.5% by weight cobalt

[0124] As can be seen from table 1, with the rubber mixtures E1 according to the invention containing silane B) a lower heat build-up is achieved, as can be seen from the lower hysteresis loss at 55° C., the lower values ​​at tan d max., and the increased resilience, as compared to V1 containing TESPT, while at the same time the tear properties at 100° C., especially the tensile strength and the elongation at break, are improved.

[0125] One reason for this could be the improved filler dispersion in E1, which can be confirmed by the reduced Payne effect (see E'(0.15%)-(E'(8%)DKF55°C)).

[0126] The above-mentioned properties at elevated temperatures are particularly relevant and significant in terms of enduring the stresses of driving operations, since internal tire components may heat up, especially during driving operations, proceeding from ambient temperatures.

[0127] Furthermore, E1 has a reduced Mooney viscosity and therefore better processability, while at the same time the adhesion of the steel cord is not adversely affected, as evidenced by the pull-out force and coverage.

[0128] Vehicle tyres which contain at least one rubber mixture according to the invention in at least one component, in particular the inner component, for example and in particular as a rubber coating of the belt, are characterised by an improved service life and durability, and also by a lower and therefore improved rolling resistance.

[0129] [Table 1] While this application is directed to the invention set forth in the claims, the disclosure of this application also includes: 1. A sulfur-crosslinkable rubber mixture comprising at least the following components: - from 50 to 100 phr of at least one polyisoprene selected from the group consisting of natural and synthetic polyisoprenes, and - from 5 to 500 phr of at least one silica, and at least one silane B having the general empirical formula I), [ka] [wherein, two o's may be independently the same or different and may each take the value of 1, 2, or 3; R 1 The groups may be independently the same or different, and are each an alkoxy group having 1 to 10 carbon atoms, a cycloalkoxy group having 4 to 10 carbon atoms, a phenoxy group having 6 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, an alkyl group having 1 to 10 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a halide, or an alkyl polyether group -O-(R 6 -O) r -R 5 (where R 6 are the same or different, branched or unbranched, saturated or unsaturated, aliphatic, aromatic, or mixed aliphatic / aromatic bridges C 1 ~C 30 Hydrocarbon groups, preferably -CH 2 -CH 2 -, r is an integer from 1 to 30, preferably from 3 to 10, R 5 is an unsubstituted or substituted, branched or unbranched, terminal alkyl, alkenyl, aryl or aralkyl group, preferably -C 13 H 27 alkyl group; Or, 2 R's 1 forms a cyclic dialkoxy group having 2 to 10 carbon atoms (in which case o is less than 3); Or, two or more silanes of formula I) are R 1 may be bridged via a group, In formula I, each (R 1 ) o Among the Si-groups, at least one R 1 is selected from the above options, this R 1 is i) bonded to the silicon atom through an oxygen atom or ii) is a halide; R 2 groups, which may be independently the same or different, are unbranched alkylene groups having 6 to 20 carbon atoms, preferably 6 to 10 carbon atoms; n is an integer from 2 to 10; A mixture comprising: 2. R 2 is the same on both sides, -(CH 2 ) 8 3. The rubber mixture according to claim 1, wherein the 3. Each (R 1 ) o In the Si-group, at least one R 1 3. The rubber mixture according to claim 1, wherein R is an alkoxy group having 1 to 10 carbon atoms. 4. A rubber mixture described in any one of 1. to 3., wherein o on both sides of the molecule is 3. 5. Both sides of the molecule and (R 1 ) o Within the Si-group, all R 1 The rubber mixture according to 4 above, wherein 6. Both sides of the molecule and (R 1 ) o Within the Si-group, all R 1 The rubber mixture according to claim 5, wherein R is the same and is an ethoxy group. 7. A rubber mixture according to any one of the above items 1 to 6, wherein n is an integer from 2 to 8, preferably from 2 to 6. 8. The silane B has the following formula II:

change

change

Claims

1. A sulfur-crosslinkable rubber mixture comprising at least the following components: from 50 to 100 phr of at least one polyisoprene selected from the group consisting of natural and synthetic polyisoprenes, and - 5 to 500 phr of at least one silica, and - 2.5 to 8 phr sulfur, and at least one silane B having the general empirical formula I), 【Chemistry 1】 [wherein the two o's may be independently the same or different and may each take the value of 1, 2, or 3; R 1 The groups may be independently the same or different and are selected from the group consisting of an alkoxy group having 1 to 10 carbon atoms, a cycloalkoxy group having 4 to 10 carbon atoms, a phenoxy group having 6 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, an alkyl group having 1 to 10 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a halide, or an alkyl polyether group -O-(R 6 -O) r -R 5 (Here, R 6 are the same or different, branched or unbranched, saturated or unsaturated, aliphatic, aromatic, or mixed aliphatic / aromatic bridges C 1 ~C 30 is a hydrocarbon group, r is an integer from 1 to 30, R 5 is an unsubstituted or substituted, branched or unbranched, terminal alkyl, alkenyl, aryl or aralkyl group; Or, Two R's 1 forms a cyclic dialkoxy group having 2 to 10 carbon atoms (in which case o is less than 3); Or, two or more silanes of formula I) are R 1 may be bridged via a group, In formula I, each (R 1 ) o Among the Si-groups, at least one R 1 is selected from the above options, this R 1 is i) bonded to the silicon atom through an oxygen atom or ii) is a halide; R 2 groups, which may be independently the same or different, are unbranched alkylene groups having 6 to 20 carbon atoms; n is an integer from 2 to 10; A mixture comprising:

2. R 2 is the same on both sides, and -(CH 2 ) 8 2. The rubber mixture according to claim 1, wherein the aryl group is .alpha.-.

3. Each (R 1 ) o In the Si-group, at least one R 1 3. A rubber mixture according to claim 1, wherein is an alkoxy group having 1 to 10 carbon atoms.

4. A rubber mixture according to any one of claims 1 to 3, in which o on both sides of the molecule is 3.

5. Both sides of the molecule and (R 1 ) o Within the Si-group, all R 1 5. The rubber mixture according to claim 4, wherein:

6. Both sides of the molecule and (R 1 ) o Within the Si-group, all R 1 6. The rubber mixture according to claim 5, wherein:

7. A rubber mixture according to any one of the preceding claims, wherein n is an integer from 2 to 8.

8. Said silane B is represented by the following formula II: 【Chemistry 2】 [wherein EtO represents an ethoxy group] 8. The rubber mixture according to claim 1, having the structure

9. Said silane B has the following formula III: 【Chemistry 3】 [wherein EtO represents an ethoxy group] 8. The rubber mixture according to claim 1, having the structure

10. 10. A rubber mixture according to claim 1, comprising from 0.1 to 30 phf of Silane B.

11. A rubber mixture according to any one of the preceding claims, which is designed to encase strength members and for that purpose comprises a bonding system for bonding the rubber mixture to textile or metal strength members.

12. A vulcanizate obtainable by sulfur vulcanization of at least one rubber mixture according to any one of claims 1 to 11.

13. A vehicle tire comprising, in at least one component, at least one vulcanizate according to claim 12.

14. 14. Vehicle tyre according to claim 13, comprising at least one vulcanizate according to claim 12 at least as a rubber coating mixture and / or in the sidewall and / or in the tread and / or in other tyre components.

15. Use of a rubber mixture according to any one of claims 1 to 11 for producing air springs, sets of bellows, conveyor belts, belts, power transmission belts, hoses, rubber bands, profiles, seals, membranes, tactile sensors for medical or robotic applications, or shoe soles or parts thereof.

Citation Information

Patent Citations

  • Inorganic filler and silane polysulfide-based tire belt

    JP2006502270A

  • Tire rubber composition and pneumatic tire

    JP2018065954A

  • Rubber composition for tires, and pneumatic tires

    WO2018143111A1

  • Propylene-ethylene-diene terpolymer polyolefin additives for improved tire tread performance

    WO2019226843A1