Rubber composition for tires and tires
The rubber composition for tires, using silica and a specific silane coupling agent with a high EB/E* ratio, addresses the issue of chipping resistance at high speeds by improving the flexibility and durability of the tire components.
Patent Information
- Application Number
- JP2020119399
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-10
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2040-07-10
AI Technical Summary
Automobile tires face challenges in chipping resistance, particularly at high speeds, due to the rapid deformation and separation of the rubber components under continuous high-speed travel.
A rubber composition for tires incorporating silica and a silane coupling agent with an alkoxysilyl group and sulfur atom, where the organosilicon compound has 6 or more carbon atoms connecting these groups, and a specific ratio of elongation at break (EB) to complex modulus of elasticity (E*) (EB/E*) of 70 or more, enhancing the chipping resistance.
The composition improves chipping resistance at high speeds by reducing deformation and increasing the flexibility of the silica-polymer bond, thereby enhancing durability and resistance to sudden impacts.
Smart Images

Figure 0007559388000001 
Figure 0007559388000002 
Figure 0007559388000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a rubber composition for a tire and a tire. [Background technology]
[0002] Automobile tires are required to have various performance characteristics, and techniques for improving rubber performance using silane coupling agents have been proposed. For example, Patent Document 1 discloses that fuel economy and wear resistance are improved by using silica and a silane coupling agent and optimizing the method of adding them. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2019-156930 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, as the speed of transportation increases, it is not uncommon for tires to travel continuously at high speeds, and there is room for improvement in the chipping resistance of the tread portion under such conditions.
[0005] An object of the present invention is to solve the above problems and to provide a rubber composition for tires and a tire that have improved chipping resistance at high speeds. [Means for solving the problem]
[0006] The present invention includes a filler containing silica and a silane coupling agent, the silane coupling agent including an organosilicon compound containing an alkoxysilyl group and a sulfur atom, and the number of carbon atoms connecting the alkoxysilyl group and the sulfur atom is 6 or more; The rubber composition for tires has a ratio (EB / E*) of elongation at break EB [%] at 23°C to complex modulus of elasticity E* [MPa] at 30°C that satisfies the following formula (1). (Formula 1) EB / E*≧70
[0007] It is preferable that the content of silica is 5 to 120 parts by mass per 100 parts by mass of the rubber component, and the content of the organosilicon compound is 5 to 15 parts by mass per 100 parts by mass of silica.
[0008] It is preferable that the rubber composition contains a butadiene rubber, a styrene-butadiene rubber and / or an isoprene-based rubber.
[0009] It is preferable that the content of the butadiene rubber is 15 to 40 mass % and the content of the styrene-butadiene rubber is 35 to 85 mass % in 100 mass % of the rubber component.
[0010] It is preferable that the content of the butadiene rubber is 10 to 45 mass % and the content of the isoprene-based rubber is 40 to 85 mass % in 100 mass % of the rubber component.
[0011] The amount of carbon black per 100 parts by mass of the rubber component is preferably 5 to 80 parts by mass.
[0012] It is preferable that the content (mass %) of butadiene rubber in 100% by mass of the rubber component and the content (parts by mass) of silica relative to 100 parts by mass of the rubber component satisfy the following (Formula 2). (Formula 2) Butadiene rubber content < Silica content ≦ 50
[0013] It is preferable that the content (mass %) of butadiene rubber in 100% by mass of the rubber component and the content (parts by mass) of silica relative to 100 parts by mass of the rubber component satisfy the following formula: Silica content-butadiene rubber content≧20
[0014] It is preferable that the content (parts by mass) of carbon black per 100 parts by mass of the rubber component and the content (parts by mass) of silica per 100 parts by mass of the rubber component satisfy the following (Equation 3). (Formula 3) Carbon black content > Silica content
[0015] It is preferable that the content (parts by mass) of carbon black per 100 parts by mass of the rubber component and the content (parts by mass) of silica per 100 parts by mass of the rubber component satisfy the following formula: Carbon black content - silica content ≥ 20
[0016] The amount of sulfur per 100 parts by mass of the rubber component is preferably 5.0 parts by mass or less.
[0017] The present invention also relates to a tire having a tire component made of the rubber composition.
[0018] Preferably, the tire component is a cap tread.
[0019] Preferably, the tire component is a base tread. Effect of the Invention
[0020] According to the present invention, the rubber composition for tires contains a filler containing silica and a silane coupling agent, and the silane coupling agent contains an organosilicon compound containing an alkoxysilyl group and a sulfur atom, and the number of carbon atoms connecting the alkoxysilyl group and the sulfur atom is 6 or more, and the ratio (EB / E*) of the breaking elongation EB [%] at 23°C to the complex modulus E* [MPa] at 30°C satisfies the above (Formula 1), thereby improving chipping resistance at high speeds. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] The present invention relates to a rubber composition for tires (rubber composition after vulcanization) having EB / E*≧70, containing a filler containing silica, and a silane coupling agent containing an alkoxysilyl group and an organosilicon compound having 6 or more carbon atoms connecting a sulfur atom. The rubber composition can improve chipping resistance at high speeds.
[0022] The reason why the above-mentioned effects are obtained is not entirely clear, but it is presumed that they are due to the following mechanism. By adjusting EB / E* to 70 or more, it is possible to reduce the deformation of the entire rubber and increase the amount of deformation that can be followed, so that good chipping resistance and peeling resistance can be imparted when a sudden impact is applied. Furthermore, by using an organic silicon compound containing an alkoxysilyl group and a sulfur atom as a silane coupling agent and having 6 or more carbon atoms connecting the alkoxysilyl group and the sulfur atom, that is, a long-chain silane coupling agent, the bond between the silica and the polymer becomes flexible, and input can be further alleviated. Therefore, it is presumed that the chipping resistance at high speeds is improved by using the rubber composition (rubber composition after vulcanization).
[0023] In this way, the rubber composition has "EB / E*≧70" and is configured to contain a filler containing silica and a silane coupling agent containing an organosilicon compound containing an alkoxysilyl group and a sulfur atom, and the number of carbon atoms connecting the alkoxysilyl group and the sulfur atom is 6 or more, thereby solving the problem (objective) of improving chipping resistance at high speeds. In other words, the configuration of "EB / E*≧70" does not define the problem (objective), and the problem of the present application is to improve chipping resistance at high speeds, and a configuration that satisfies the parameter is used as a means to achieve this.
[0024] The rubber composition (rubber composition after vulcanization) has a ratio (EB / E*) of the breaking elongation EB [%] at 23° C. to the complex modulus E* [MPa] at 30° C. that satisfies the following (formula 1). (Formula 1) EB / E*≧70 From the viewpoint of chipping resistance at high speed, EB / E* is preferably 80 or more, more preferably 90 or more, and even more preferably 100 or more. There is no particular upper limit, but it is preferably 200 or less, more preferably 150 or less, and even more preferably 130 or less.
[0025] The rubber composition (rubber composition after vulcanization) preferably has a breaking elongation EB [%] at 23°C of 150% or more, more preferably 300% or more, even more preferably 400% or more, and particularly preferably 500% or more. The upper limit is preferably 900% or less, more preferably 850% or less, even more preferably 800% or less, and particularly preferably 750% or less. By keeping it within the above range, chipping resistance at high speeds tends to be improved.
[0026] The rubber composition (rubber composition after vulcanization) has a complex modulus E* at 30°C of preferably 4.0 MPa or more, more preferably 5.0 MPa or more, even more preferably 7.0 MPa or more, and particularly preferably 8.0 MPa or more. The upper limit is preferably 15.0 MPa or less, more preferably 12.0 MPa or less, even more preferably 10.0 MPa or less, and particularly preferably 9.0 MPa or less. By keeping it within the above range, there is a tendency that chipping resistance at high speeds can be improved.
[0027] The breaking elongation EB and complex modulus E* of the rubber composition (rubber composition after vulcanization) can be adjusted by the type and amount of chemicals (particularly rubber components, fillers, softeners, sulfur, vulcanization accelerators, and silane coupling agents) compounded in the rubber composition. For example, the complex modulus E* tends to increase with a decrease in the amount of softener, an increase in the amount of fillers, and an increase in the amount of sulfur. The breaking elongation EB tends to increase with an increase in the amount of softener, a decrease in the amount of fillers, and the use of an organosilicon compound that contains an alkoxysilyl group and a sulfur atom and has 6 or more carbon atoms connecting the alkoxysilyl group and the sulfur atom.
[0028] A method for achieving EB / E* of a rubber composition (rubber composition after vulcanization) of ≥ 70 includes, for example, the use of an organosilicon compound that contains an alkoxysilyl group and a sulfur atom and in which the number of carbon atoms connecting the alkoxysilyl group and the sulfur atom is 6 or more.
[0029] In this specification, the breaking elongation EB of the rubber composition (rubber composition after vulcanization) is measured in accordance with JIS K 6251:2017 by carrying out a tensile test at 23°C using a No. 7 dumbbell-shaped test piece. The complex modulus E* of the rubber composition (rubber composition after vulcanization) is measured using an Eplexer manufactured by GABO under the conditions of a frequency of 10 Hz, an initial strain of 5%, a dynamic strain of 1%, and a temperature of 30°C.
[0030] (Rubber component) As the rubber component usable in the rubber composition, for example, diene rubber can be used. Examples of diene rubber include isoprene rubber, butadiene rubber (BR), styrene butadiene rubber (SBR), styrene isoprene butadiene rubber (SIBR), ethylene propylene diene rubber (EPDM), chloroprene rubber (CR), and acrylonitrile butadiene rubber (NBR). Examples also include butyl rubber and fluororubber. These may be used alone or in combination of two or more. Among them, BR, SBR, and isoprene rubber are preferred from the viewpoint of improving chipping resistance at high speeds. In particular, in the case of a cap tread, a combination of BR and SBR is preferred, and in the case of a base tread, a combination of BR and isoprene rubber is preferred.
[0031] The reason why such an effect is obtained is not entirely clear, but it is presumed that the effect is due to the following mechanism. Silica is used as a reinforcing agent for rubber components to reduce heat generation in tires, but since silica is bonded to polymers via silane coupling agents, the polymer-silica interface does not have the same stickiness as carbon black. Therefore, when high-speed input is applied, the bond is suddenly cut, and there is a concern that the rubber phase will peel off. Therefore, for example, if butadiene rubber, styrene-butadiene rubber, and / or isoprene-based rubber are introduced as rubber components, a sea-island structure of styrene parts and butadiene (parts / rubber) is formed when styrene-butadiene rubber is contained, and a sea-island structure of isoprene-based rubber and butadiene rubber is formed when isoprene-based rubber is contained, making it possible to mitigate input. Therefore, it is presumed that chipping resistance at high speeds will be significantly improved.
[0032] The diene rubber may be a non-modified diene rubber or a modified diene rubber. The modified diene rubber may be any diene rubber having a functional group that interacts with a filler such as silica. Examples of the modified diene rubber include terminal-modified diene rubber (terminal-modified diene rubber having the functional group at the terminal) in which at least one terminal of the diene rubber has been modified with a compound (modifier) having the functional group, main-chain modified diene rubber having the functional group in the main chain, main-chain terminal-modified diene rubber having the functional group in the main chain and at least one terminal (for example, main-chain terminal-modified diene rubber having the functional group in the main chain and at least one terminal modified with the modifier), and terminal-modified diene rubber modified (coupled) with a polyfunctional compound having two or more epoxy groups in the molecule and having a hydroxyl group or epoxy group introduced therein.
[0033] Examples of the functional group include an amino group, an amide group, a silyl group, an alkoxysilyl group, an isocyanate group, an imino group, an imidazole group, a urea group, an ether group, a carbonyl group, an oxycarbonyl group, a mercapto group, a sulfide group, a disulfide group, a sulfonyl group, a sulfinyl group, a thiocarbonyl group, an ammonium group, an imide group, a hydrazo group, an azo group, a diazo group, a carboxyl group, a nitrile group, a pyridyl group, an alkoxy group, a hydroxyl group, an oxy group, and an epoxy group. These functional groups may have a substituent. Among them, an amino group (preferably an amino group in which a hydrogen atom of an amino group is substituted with an alkyl group having 1 to 6 carbon atoms), an alkoxy group (preferably an alkoxy group having 1 to 6 carbon atoms), and an alkoxysilyl group (preferably an alkoxysilyl group having 1 to 6 carbon atoms) are preferred.
[0034] The BR is not particularly limited, and for example, high cis BR with a high cis content, BR containing syndiotactic polybutadiene crystals, BR synthesized using a rare earth catalyst (rare earth BR), etc. can be used. These may be used alone or in combination of two or more. In particular, the BR preferably contains high cis BR with a cis content of 90% by mass or more. The cis content is more preferably 95% by mass or more. The cis content can be measured by infrared absorption spectroscopy.
[0035] The BR may be unmodified or modified. The modified BR may be modified BR having the same functional group as the modified diene rubber. The BR may be a hydrogenated butadiene polymer (hydrogenated BR).
[0036] As the BR, for example, products from Ube Industries, Ltd., JSR Corporation, Asahi Kasei Corporation, Zeon Corporation, etc. can be used.
[0037] The BR content in 100% by mass of the rubber component is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 15% by mass or more, and particularly preferably 20% by mass or more. The upper limit is preferably 60% by mass or less, more preferably 45% by mass or less, even more preferably 40% by mass or less, and particularly preferably 35% by mass or less. By keeping it within the above range, chipping resistance at high speeds tends to be improved.
[0038] When the rubber composition is used for a cap tread, the BR content in 100% by mass of the rubber component is preferably 10% by mass or more, more preferably 15% by mass or more, even more preferably 20% by mass or more, and particularly preferably 25% by mass or more. The upper limit is preferably 60% by mass or less, more preferably 45% by mass or less, even more preferably 40% by mass or less, and particularly preferably 35% by mass or less. By keeping it within the above range, chipping resistance at high speeds tends to be improved.
[0039] When the rubber composition is used for a base tread, the BR content in 100% by mass of the rubber component is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 15% by mass or more, and particularly preferably 20% by mass or more. The upper limit is preferably 60% by mass or less, more preferably 50% by mass or less, even more preferably 45% by mass or less, and particularly preferably 40% by mass or less. By keeping it within the above range, chipping resistance at high speeds tends to be improved.
[0040] There are no particular limitations on the SBR, and examples of the SBR that can be used include emulsion-polymerized styrene-butadiene rubber (E-SBR), solution-polymerized styrene-butadiene rubber (S-SBR), etc. These may be used alone or in combination of two or more kinds.
[0041] The styrene content of the SBR is preferably 5% by mass or more, more preferably 20% by mass or more, and even more preferably 25% by mass or more. The styrene content is preferably 45% by mass or less, more preferably 40% by mass or less, and even more preferably 35% by mass or less. By keeping the styrene content within the above range, chipping resistance at high speeds tends to be improved. In this specification, the styrene content is 1 It can be measured by H-NMR measurement.
[0042] The vinyl bond content of SBR is preferably 3% by mass or more, more preferably 5% by mass or more, and even more preferably 7% by mass or more. The vinyl bond content is preferably 25% by mass or less, more preferably 15% by mass or less, and even more preferably 13% by mass or less. By keeping it within the above range, chipping resistance at high speeds tends to be improved. In this specification, the vinyl bond amount (1,2-bonded butadiene unit amount) can be measured by infrared absorption spectroscopy.
[0043] The SBR may be unmodified or modified. Modified SBR includes modified SBR into which functional groups similar to those of modified diene rubbers have been introduced. Hydrogenated styrene-butadiene copolymers (hydrogenated SBR) can also be used as SBR.
[0044] As the SBR, for example, SBR manufactured and sold by Sumitomo Chemical Co., Ltd., JSR Corporation, Asahi Kasei Corporation, Zeon Corporation, and the like can be used.
[0045] The content of SBR in 100% by mass of the rubber component is preferably 5% by mass or more, more preferably 20% by mass or more, even more preferably 30% by mass or more, and particularly preferably 35% by mass or more. The upper limit is preferably 90% by mass or less, more preferably 85% by mass or less, even more preferably 80% by mass or less, and particularly preferably 75% by mass or less. By keeping it within the above range, chipping resistance at high speeds tends to be improved.
[0046] When the rubber composition is used for a cap tread, the content of SBR in 100% by mass of the rubber component is preferably 35% by mass or more, more preferably 50% by mass or more, even more preferably 60% by mass or more, and particularly preferably 65% by mass or more. The upper limit is preferably 90% by mass or less, more preferably 85% by mass or less, even more preferably 80% by mass or less, and particularly preferably 75% by mass or less. By keeping it within the above range, chipping resistance at high speeds tends to be improved.
[0047] Examples of isoprene-based rubber include natural rubber (NR), isoprene rubber (IR), modified NR, modified NR, and modified IR. Examples of NR include SIR20, RSS♯3, TSR20, and other rubber industry-standard rubbers. Examples of IR include IR2200 and other rubber industry-standard rubbers. Examples of modified NR include deproteinized natural rubber (DPNR), high-purity natural rubber (UPNR), and other rubbers. Examples of modified NR include epoxidized natural rubber (ENR), hydrogenated natural rubber (HNR), and grafted natural rubber. Examples of modified IR include epoxidized isoprene rubber, hydrogenated isoprene rubber, and grafted isoprene rubber. These may be used alone or in combination of two or more.
[0048] The content of the isoprene-based rubber in 100% by mass of the rubber component is preferably 5% by mass or more, more preferably 20% by mass or more, even more preferably 30% by mass or more, and particularly preferably 40% by mass or more. The upper limit is preferably 90% by mass or less, more preferably 85% by mass or less, and even more preferably 80% by mass or less. By keeping it within the above range, chipping resistance at high speeds tends to be improved.
[0049] When the rubber composition is used in a base tread, the content is preferably 30% by mass or more, more preferably 40% by mass or more, even more preferably 50% by mass or more, and particularly preferably 60% by mass or more. The upper limit is preferably 90% by mass or less, more preferably 85% by mass or less, and even more preferably 80% by mass or less. By keeping the content within the above range, chipping resistance at high speeds tends to be improved.
[0050] (silica) Silica is compounded as a filler in the rubber composition. Usable silica includes dry process silica (anhydrous silica) and wet process silica (hydrated silica). Among them, wet process silica is preferred because it has a large number of silanol groups. Commercially available products include those from Degussa, Rhodia, Tosoh Silica, Solvay Japan, and Tokuyama. These may be used alone or in combination of two or more.
[0051] The nitrogen adsorption specific surface area (N2SA) of the silica is preferably 50 m 2 / g or more, more preferably 100m 2 / g or more, more preferably 150m 2 The upper limit of the N2SA of silica is not particularly limited, but is preferably 350 m 2 / g or less, more preferably 250m 2 / g or less, more preferably 200m 2 By keeping it within the above range, there is a tendency that chipping resistance at high speeds can be improved. The N2SA of silica is a value measured by the BET method in accordance with ASTM D3037-93.
[0052] In the rubber composition, the content of silica is preferably 5 parts by mass or more, more preferably 15 parts by mass or more, and even more preferably 20 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 150 parts by mass or less, more preferably 100 parts by mass or less, even more preferably 80 parts by mass or less, and particularly preferably 50 parts by mass or less. By keeping the content within the above range, there is a tendency that chipping resistance at high speeds can be improved. In particular, when the content of silica is 50 parts by mass or less, it is possible to block the propagation of input between silica particles in the sea-island structure, so that it is presumed that the chipping resistance at high speeds is significantly improved.
[0053] When the rubber composition is used for a cap tread, the content of silica is preferably 5 parts by mass or more, more preferably 15 parts by mass or more, and even more preferably 20 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 150 parts by mass or less, more preferably 120 parts by mass or less, even more preferably 80 parts by mass or less, and particularly preferably 50 parts by mass or less. By keeping the content within the above range, there is a tendency that chipping resistance at high speeds can be improved.
[0054] When the rubber composition is used for a base tread, the content of silica is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, even more preferably 15 parts by mass or more, and particularly preferably 20 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 120 parts by mass or less, more preferably 80 parts by mass or less, even more preferably 60 parts by mass or less, and particularly preferably 40 parts by mass or less. By keeping the content within the above range, chipping resistance at high speeds tends to be improved.
[0055] From the viewpoint of chipping resistance at high speeds, it is preferable that the content (mass %) of butadiene rubber in 100 mass % of the rubber component and the content (parts by mass) of silica per 100 parts by mass of the rubber component satisfy the following (Equation 2). (Formula 2) Butadiene rubber content < Silica content ≦ 50
[0056] From the viewpoint of chipping resistance at high speeds, it is preferable that the content (mass %) of butadiene rubber in 100 mass % of the rubber component and the content (parts by mass) of silica per 100 parts by mass of the rubber component satisfy the following formula: Silica content-butadiene rubber content≧5 The ratio of the silica content to the butadiene rubber content is preferably 5 or more, more preferably 10 or more, and even more preferably 20 or more. The upper limit is preferably 100 or less, more preferably 60 or less, even more preferably 50 or less, and particularly preferably 40 or less. By keeping it within the above range, good durability of the tire after aging tends to be obtained.
[0057] (Silane coupling agent) The silane coupling agent used in the rubber composition contains an organosilicon compound that contains an alkoxysilyl group and a sulfur atom, and the number of carbon atoms connecting the alkoxysilyl group and the sulfur atom is 6 or more. Such organosilicon compounds may be used alone or in combination of two or more. Among the organosilicon compounds, an organosilicon compound represented by the following average composition formula (I) is preferred. [ka] (In the formula, x represents the average number of sulfur atoms and is 3.5 or more. m represents an integer of 6 or more. 1 ~R 6 are the same or different and each represents an alkyl group or an alkoxy group having 1 to 6 carbon atoms; R 1 ~R 3 At least one of and R 4 ~R 6 At least one of R is the alkoxy group. 1 ~R 6 may be a ring structure formed by bonding the alkyl group or the alkoxy group.
[0058] x represents the average number of sulfur atoms in the organosilicon compound, and is preferably 3.5 or more and 12 or less. Here, the average number of sulfur atoms and the number of silicon atoms are values calculated from the molecular weights of the sulfur and silicon atoms in the composition measured by fluorescent X-rays.
[0059] m represents an integer of 6 or more, and preferably 6 or more and 14 or less.
[0060] Alkyl group (R 1 ~R 6 The number of carbon atoms in the alkyl group is preferably 1 to 5. The alkyl group may be linear, branched, or cyclic. Specific examples include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, and a tert-butyl group.
[0061] Alkoxy group (R1 ~R 6 ) preferably has 1 to 5 carbon atoms. The hydrocarbon group in the alkoxy group may be linear, branched, or cyclic. Specific examples include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, and an n-butoxy group.
[0062] R 1 ~R 3 At least one of and R 4 ~R 6 At least one of R is an alkoxy group having 1 to 6 carbon atoms, and preferably R 1 ~R 3 , R 4 ~R 6 At least two of each of these are alkoxy groups having 1 to 6 carbon atoms.
[0063] In addition, R 1 ~R 6 may be a ring structure formed by bonding an alkyl group or an alkoxy group having 1 to 6 carbon atoms. For example, (i) R 1 is an ethoxy group, R 2 (ii) R 1 is an ethyl group, R 2 When R forms a ring structure with a methyl group bonded thereto, 1 and R 2 Examples of structures in which divalent groups such as "-O-C2H4-CH2-" and "-C2H4-CH2-" are formed and bonded to Si include
[0064] The organosilicon compound can be prepared, for example, by the manufacturing method described in JP 2018-65954 A. Specifically, the organosilicon compound can be produced by reacting a halogen-containing organosilicon compound of formula (I-1) described in JP 2018-65954 A, anhydrous sodium sulfide represented by Na2S, and sulfur as necessary. When carrying out the above reaction, the addition of sulfur is optional for adjusting the sulfide chain, and may be determined from the blending amount of the compound of the average composition formula (I-1), anhydrous sodium sulfide, and sulfur as necessary, so as to obtain a compound of the desired average composition formula (I). For example, if you want to make the x of the compound of the average composition formula (I) 3.5, you can react 1.0 mol of anhydrous sodium sulfide, 2.5 mol of sulfur, and 2.0 mol of the compound of formula (I-1).
[0065] And, when using an organic silicon compound that contains an alkoxysilyl group and a sulfur atom, and the number of carbon atoms that connects the alkoxysilyl group and the sulfur atom is 6 or more as a silane coupling agent, that is, a long-chain silane coupling agent, the alkoxy group in the compound reacts with the hydroxyl group on the silica surface, making the silica surface hydrophobic, and the effect of hydrophobization is greater than that of conventional silane coupling agents due to the long carbon chain of the compound, so the dispersibility of silica is significantly improved.In addition, the long-chain structure makes the bond between silica and polymer flexible, and input can be alleviated.Therefore, by using such a long-chain silane coupling agent, it is possible to improve chipping resistance at high speeds.
[0066] In the rubber composition, the content of the organosilicon compound is preferably 0.1 parts by mass or more, more preferably 3 parts by mass or more, even more preferably 5 parts by mass or more, and particularly preferably 7 parts by mass or more, based on 100 parts by mass of silica. The upper limit of the content is preferably 50 parts by mass, more preferably 20 parts by mass or less, even more preferably 15 parts by mass or less, and particularly preferably 10 parts by mass or less. By keeping it within the above range, there is a tendency that chipping resistance at high speeds can be improved. The content of the organosilicon compound represented by the average composition formula (I) is also preferably within the same range.
[0067] The rubber composition may contain a silane coupling agent other than the organosilicon compound that contains an alkoxysilyl group and a sulfur atom and in which the number of carbon atoms connecting the alkoxysilyl group and the sulfur atom is 6 or more. The other silane coupling agent is not particularly limited, and examples thereof include bis(3-triethoxysilylpropyl)tetrasulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(4-triethoxysilylbutyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, bis(2-triethoxysilylethyl)trisulfide, bis(4-trimethoxysilylbutyl)trisulfide, bis(3-triethoxysilylpropyl)disulfide, bis(2-triethoxysilylethyl)disulfide, bis(4-triethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, 3-trimethoxysilylpropyl-N,N-dimethylthiocarbamate, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide ...3-trimethoxysilylpropyl-N,N-dimethylthiocarbamate, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, bis(2-trimethoxysilylpropyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-trimethoxysil Examples of such silanes include sulfide-based silanes such as rubamoyl tetrasulfide, 2-triethoxysilylethyl-N,N-dimethylthiocarbamoyl tetrasulfide, and 3-triethoxysilylpropyl methacrylate monosulfide; mercapto-based silanes such as 3-mercaptopropyltrimethoxysilane, 2-mercaptoethyltriethoxysilane, and Momentive's NXT and NXT-Z; vinyl-based silanes such as vinyltriethoxysilane and vinyltrimethoxysilane; amino-based silanes such as 3-aminopropyltriethoxysilane and 3-aminopropyltrimethoxysilane; glycidoxy-based silanes such as γ-glycidoxypropyltriethoxysilane and γ-glycidoxypropyltrimethoxysilane; nitro-based silanes such as 3-nitropropyltrimethoxysilane and 3-nitropropyltriethoxysilane; and chloro-based silanes such as 3-chloropropyltrimethoxysilane and 3-chloropropyltriethoxysilane. Commercially available products include those manufactured by Degussa, Momentive, Shin-Etsu Silicones, Tokyo Chemical Industry, Azumax, and Dow Corning Toray Co., Ltd. These may be used alone or in combination of two or more.
[0068] In the rubber composition, the content of the silane coupling agent (the total amount of the organosilicon compound and other silane coupling agents) is preferably 0.1 parts by mass or more, more preferably 3 parts by mass or more, even more preferably 5 parts by mass or more, and particularly preferably 7 parts by mass or more, based on 100 parts by mass of silica. The upper limit of the content is preferably 50 parts by mass, more preferably 20 parts by mass or less, even more preferably 15 parts by mass or less, and particularly preferably 10 parts by mass or less. By keeping it within the above range, chipping resistance at high speeds tends to be improved.
[0069] (Other filling materials) The filler other than silica is not particularly limited, and materials known in the rubber field can be used, such as inorganic fillers such as carbon black, calcium carbonate, talc, alumina, clay, aluminum hydroxide, aluminum oxide, and mica. Of these, carbon black is preferred.
[0070] In the rubber composition, the content of the filler (total content of the fillers) is preferably 5 parts by mass or more, more preferably 15 parts by mass or more, even more preferably 20 parts by mass or more, and particularly preferably 25 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 200 parts by mass or less, more preferably 130 parts by mass or less, even more preferably 120 parts by mass or less, and particularly preferably 100 parts by mass or less. By keeping the content within the above range, chipping resistance at high speeds tends to be improved.
[0071] When the rubber composition is used for a cap tread, the content of the filler (total content of the filler) is preferably 20 parts by mass or more, more preferably 40 parts by mass or more, even more preferably 50 parts by mass or more, and particularly preferably 60 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 200 parts by mass or less, more preferably 130 parts by mass or less, even more preferably 100 parts by mass or less, and particularly preferably 80 parts by mass or less. By keeping the content within the above range, there is a tendency that chipping resistance at high speeds can be improved.
[0072] When the rubber composition is used for the base tread, the content of the filler (total content of the filler) is preferably 5 parts by mass or more, more preferably 15 parts by mass or more, even more preferably 20 parts by mass or more, and particularly preferably 25 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 100 parts by mass or less, more preferably 80 parts by mass or less, even more preferably 60 parts by mass or less, and particularly preferably 50 parts by mass or less. By keeping the content within the above range, chipping resistance at high speeds tends to be improved.
[0073] Carbon black that can be used in the rubber composition is not particularly limited, and examples thereof include N134, N110, N220, N234, N219, N339, N330, N326, N351, N550, and N762. Commercially available products include those from Asahi Carbon Co., Ltd., Cabot Japan Co., Ltd., Tokai Carbon Co., Ltd., Mitsubishi Chemical Co., Ltd., Lion Co., Ltd., Shinnikka Carbon Co., Ltd., Columbia Carbon Co., Ltd., and the like. These may be used alone or in combination of two or more kinds.
[0074] The nitrogen adsorption specific surface area (N2SA) of carbon black is 30m 2 / g or more is preferable, and 50m 2 / g or more is more preferable, and 70m 2 / g or more is more preferable. 2 / g or less is preferable, and 200m 2 / g or less is more preferable, and 180m 2 / g or less is more preferable, and 160m 2 By keeping it within the above range, there is a tendency that chipping resistance at high speeds can be improved.
[0075] When the rubber composition is used for a cap tread, the nitrogen adsorption specific surface area (N2SA) of the carbon black is 50 m 2 / g or more is preferable, and 100m 2 / g or more is more preferable, and 120m 2 / g or more is more preferable, and 130m 2 / g or more is particularly preferable. 2 / g or less is preferable, and 200m 2 / g or less is more preferable, and 180m 2 / g or less is more preferable, and 160m 2 By keeping it within the above range, there is a tendency that chipping resistance at high speeds can be improved.
[0076] When the rubber composition is used for a base tread, the nitrogen adsorption specific surface area (N2SA) of the carbon black is 30m 2 / g or more is preferable, and 50m 2 / g or more is more preferable, and 70m 2 / g or more is more preferable. 2 / g or less is preferable, and 90m 2 / g or less is more preferable, and 80m 2 By keeping it within the above range, there is a tendency that chipping resistance at high speeds can be improved. The nitrogen adsorption specific surface area of carbon black is determined in accordance with JIS K6217-2:2001.
[0077] In the rubber composition, the content of carbon black is preferably 5 parts by mass or more, more preferably 15 parts by mass or more, and even more preferably 20 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 200 parts by mass or less, more preferably 150 parts by mass or less, even more preferably 100 parts by mass or less, and particularly preferably 80 parts by mass or less. By keeping the content within the above range, chipping resistance at high speeds tends to be improved.
[0078] When the rubber composition is used for a cap tread, the carbon black content is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, even more preferably 20 parts by mass or more, and particularly preferably 30 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 150 parts by mass or less, more preferably 100 parts by mass or less, even more preferably 80 parts by mass or less, and particularly preferably 60 parts by mass or less. By keeping the content within the above range, there is a tendency that chipping resistance at high speeds can be improved.
[0079] When the rubber composition is used for a base tread, the carbon black content is preferably 5 parts by mass or more, more preferably 15 parts by mass or more, and even more preferably 20 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 100 parts by mass or less, more preferably 80 parts by mass or less, even more preferably 50 parts by mass or less, and particularly preferably 40 parts by mass or less. By keeping the content within the above range, chipping resistance at high speeds tends to be improved.
[0080] From the viewpoint of chipping resistance at high speeds, it is preferable that the carbon black content (parts by mass) per 100 parts by mass of the rubber component and the silica content (parts by mass) per 100 parts by mass of the rubber component satisfy the following (Equation 3). (Formula 3) Carbon black content > Silica content
[0081] In the rubber composition, it is preferable that the content (parts by mass) of carbon black per 100 parts by mass of the rubber component and the content (parts by mass) of silica per 100 parts by mass of the rubber component satisfy the following formula: Carbon black content - silica content ≥ 10 The carbon black content minus the silica content is more preferably 20 parts by mass or more, and even more preferably 25 parts by mass or more. The upper limit is preferably 100 parts by mass or less, more preferably 80 parts by mass or less, even more preferably 60 parts by mass or less, and particularly preferably 50 parts by mass or less. By keeping it within the above range, there is a tendency that good durability of the tire after deterioration can be obtained.
[0082] (Plasticizer) The rubber composition may contain a plasticizer. A plasticizer is a material that imparts plasticity to a rubber component, and examples of the plasticizer include liquid plasticizers (plasticizers that are in a liquid state at room temperature (25° C.)) and resins (resins that are in a solid state at room temperature (25° C.)).
[0083] In the rubber composition, the content of the plasticizer (total amount of the plasticizer) is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and even more preferably 5 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 100 parts by mass or less, more preferably 70 parts by mass or less, even more preferably 50 parts by mass or less, and particularly preferably 30 parts by mass or less. By keeping the content within the above range, chipping resistance at high speeds tends to be improved.
[0084] When the rubber composition is used for a cap tread, the content of the plasticizer (total amount of the plasticizer) is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 100 parts by mass or less, more preferably 70 parts by mass or less, even more preferably 50 parts by mass or less, and particularly preferably 30 parts by mass or less. By keeping the content within the above range, there is a tendency that chipping resistance at high speeds can be improved.
[0085] When the rubber composition is used for a base tread, the content of the plasticizer (total amount of the plasticizer) in the rubber composition is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and even more preferably 5 parts by mass or more, per 100 parts by mass of the rubber component. The upper limit of the content is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, even more preferably 20 parts by mass or less, and particularly preferably 10 parts by mass or less. By keeping it within the above range, it tends to be possible to improve chipping resistance at high speeds. By keeping it within the above range, it tends to be possible to improve chipping resistance at high speeds.
[0086] Liquid plasticizers (plasticizers that are in a liquid state at room temperature (25° C.)) that can be used in the rubber composition are not particularly limited, and examples thereof include oils, liquid polymers (liquid resins, liquid diene-based polymers, etc.), etc. These may be used alone or in combination of two or more kinds.
[0087] In the rubber composition, the content of the liquid plasticizer is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and even more preferably 5 parts by mass or more. The upper limit of the content is preferably 100 parts by mass or less, more preferably 70 parts by mass or less, even more preferably 50 parts by mass or less, and particularly preferably 30 parts by mass or less. By keeping the content within the above range, chipping resistance at high speeds tends to be improved.
[0088] When the rubber composition is used for a cap tread, the content of the liquid plasticizer is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 100 parts by mass or less, more preferably 70 parts by mass or less, even more preferably 50 parts by mass or less, and particularly preferably 30 parts by mass or less. By keeping the content within the above range, there is a tendency that chipping resistance at high speeds can be improved.
[0089] When the rubber composition is used for the base tread, the content of the liquid plasticizer is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and even more preferably 5 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, even more preferably 20 parts by mass or less, and particularly preferably 10 parts by mass or less. By keeping it within the above range, it tends to be possible to improve chipping resistance at high speeds. By keeping it within the above range, it tends to be possible to improve chipping resistance at high speeds.
[0090] Examples of the oil include process oil, vegetable oil, or a mixture thereof. Examples of the process oil include paraffin-based process oil, aromatic process oil, and naphthenic process oil. Examples of the vegetable oil include castor oil, cottonseed oil, linseed oil, rapeseed oil, soybean oil, palm oil, coconut oil, peanut oil, rosin, pine oil, pine tar, tall oil, corn oil, rice oil, safflower oil, sesame oil, olive oil, sunflower oil, palm kernel oil, camellia oil, jojoba oil, macadamia nut oil, and tung oil. Examples of commercially available products include products from Idemitsu Kosan Co., Ltd., Sankyo Yuka Kogyo Co., Ltd., Japan Energy Co., Ltd., Orisoi Co., Ltd., H&R Co., Ltd., Toyokuni Oil Mill Co., Ltd., Showa Shell Sekiyu K.K., Fuji Kosan Co., Ltd., and Nisshin Oillio Group Co., Ltd. Among these, process oils (paraffin-based process oils, aromatic process oils, naphthenic process oils, etc.) and vegetable oils are preferred.
[0091] In the rubber composition, the oil content is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and even more preferably 5 parts by mass or more. The upper limit of the content is preferably 100 parts by mass or less, more preferably 70 parts by mass or less, even more preferably 50 parts by mass or less, and particularly preferably 30 parts by mass or less. By keeping it within the above range, there is a tendency that chipping resistance at high speeds can be improved. The oil content also includes the oil contained in the oil extension oil.
[0092] When the rubber composition is used for a cap tread, the oil content is preferably 5 parts by mass or more, more preferably 7 parts by mass or more, and even more preferably 10 parts by mass or more. The upper limit of the content is preferably 100 parts by mass or less, more preferably 70 parts by mass or less, even more preferably 50 parts by mass or less, and particularly preferably 30 parts by mass or less. By keeping the content within the above range, there is a tendency that chipping resistance at high speeds can be improved. The oil content includes the oil contained in the oil extension oil.
[0093] When the rubber composition is used for a base tread, the oil content is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and even more preferably 5 parts by mass or more. The upper limit of the content is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, even more preferably 20 parts by mass or less, and particularly preferably 10 parts by mass or less. By keeping the content within the above range, there is a tendency that chipping resistance at high speeds can be improved. The oil content includes the oil contained in the oil extension oil.
[0094] Examples of liquid resins include terpene resins (including terpene phenol resins and aromatic modified terpene resins), rosin resins, styrene resins, C5 resins, C9 resins, C5 / C9 resins, dicyclopentadiene (DCPD) resins, coumarone-indene resins (including coumarone and indene simple resins), phenol resins, olefin resins, polyurethane resins, acrylic resins, etc. Hydrogenated products of these resins can also be used.
[0095] Examples of liquid diene polymers include liquid styrene butadiene copolymers (liquid SBR), liquid butadiene polymers (liquid BR), liquid isoprene polymers (liquid IR), liquid styrene isoprene copolymers (liquid SIR), liquid styrene butadiene styrene block copolymers (liquid SBS block polymers), liquid styrene isoprene styrene block copolymers (liquid SIS block polymers), liquid farnesene polymers, and liquid farnesene butadiene copolymers that are in a liquid state at 25°C. The ends or main chains of these may be modified with polar groups. Hydrogenated versions of these may also be used.
[0096] Examples of the resins (resins in a solid state at room temperature (25°C)) that can be used in the rubber composition include aromatic vinyl polymers, coumarone-indene resins, coumarone resins, indene resins, phenolic resins, rosin resins, petroleum resins, terpene resins, and acrylic resins that are in a solid state at room temperature (25°C). The resins may be hydrogenated. These may be used alone or in combination of two or more. Of these, aromatic vinyl polymers, petroleum resins, and terpene resins are preferred.
[0097] When the rubber composition contains the resin, the content of the resin is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 200 parts by mass or less, more preferably 100 parts by mass or less, even more preferably 50 parts by mass or less, and particularly preferably 20 parts by mass or less. By keeping the content within the above range, chipping resistance at high speeds tends to be improved.
[0098] The softening point of the resin is preferably 60° C. or higher, more preferably 70° C. or higher, and even more preferably 80° C. or higher. The upper limit is preferably 160° C. or lower, more preferably 130° C. or lower, and even more preferably 115° C. or lower. By keeping the softening point within the above range, chipping resistance at high speeds tends to be improved. The softening point of the resin is the temperature at which the ball drops when the softening point specified in JIS K6220-1:2001 is measured using a ring and ball softening point tester.
[0099] The aromatic vinyl polymer is a polymer containing an aromatic vinyl monomer as a structural unit. For example, it can be a resin obtained by polymerizing α-methylstyrene and / or styrene, and specifically, it can be a homopolymer of styrene (styrene resin), a homopolymer of α-methylstyrene (α-methylstyrene resin), a copolymer of α-methylstyrene and styrene, a copolymer of styrene and another monomer, etc.
[0100] The coumarone-indene resin is a resin containing coumarone and indene as main monomer components constituting the resin skeleton (main chain). Other monomer components contained in the skeleton besides coumarone and indene include styrene, α-methylstyrene, methylindene, vinyltoluene, etc.
[0101] The coumarone resin is a resin containing coumarone as a main monomer component constituting the skeleton (main chain) of the resin.
[0102] The indene resin is a resin containing indene as a main monomer component constituting the skeleton (main chain) of the resin.
[0103] The phenolic resin may be a known polymer obtained by reacting phenol with an aldehyde such as formaldehyde, acetaldehyde, or furfural in the presence of an acid or alkali catalyst. Among these, those obtained by reacting with an acid catalyst (such as novolac-type phenolic resin) are preferred.
[0104] Examples of the rosin resin include rosin-based resins such as natural rosin, polymerized rosin, modified rosin, ester compounds thereof, and hydrogenated products thereof.
[0105] Examples of the petroleum resin include C5 resin, C9 resin, C5 / C9 resin, dicyclopentadiene (DCPD) resin, and hydrogenated versions of these resins. Of these, DCPD resin and hydrogenated DCPD resin are preferred.
[0106] The terpene resin is a polymer containing terpene as a structural unit. For example, polyterpene resin obtained by polymerizing a terpene compound, aromatic modified terpene resin obtained by polymerizing a terpene compound and an aromatic compound, etc. can be mentioned. Hydrogenated products of these can also be used.
[0107] The polyterpene resin is a resin obtained by polymerizing a terpene compound. The terpene compound is (C5H8) n The hydrocarbons and their oxygen-containing derivatives represented by the composition 10 H 16 ), sesquiterpenes (C 15 H 24 ), diterpenes (C 20 H 32), and examples thereof include α-pinene, β-pinene, dipentene, limonene, myrcene, alloocimene, ocimene, α-phellandrene, α-terpinene, γ-terpinene, terpinolene, 1,8-cineole, 1,4-cineole, α-terpineol, β-terpineol, and γ-terpineol.
[0108] Examples of the polyterpene resin include pinene resin, limonene resin, dipentene resin, pinene / limonene resin, etc., which are made from the above-mentioned terpene compounds. Among them, pinene resin is preferable. Pinene resin usually contains both α-pinene and β-pinene, which are isomers, but depending on the components contained, it is classified into β-pinene resin mainly composed of β-pinene and α-pinene resin mainly composed of α-pinene.
[0109] Examples of the aromatic modified terpene resin include terpene phenol resins made from the above terpene compounds and phenolic compounds, and terpene styrene resins made from the above terpene compounds and styrene compounds. Terpene phenol styrene resins made from the above terpene compounds, phenolic compounds, and styrene compounds can also be used. Examples of the phenolic compounds include phenol, bisphenol A, cresol, and xylenol. Examples of the styrene compounds include styrene and α-methylstyrene.
[0110] The acrylic resin is a polymer containing an acrylic monomer as a constituent unit. For example, a styrene-acrylic resin having a carboxyl group and obtained by copolymerizing an aromatic vinyl monomer component and an acrylic monomer component, such as a styrene-acrylic resin, can be used. Among them, a solventless carboxyl group-containing styrene-acrylic resin can be preferably used.
[0111] The solvent-free carboxyl group-containing styrene-acrylic resin is a (meth)acrylic resin (polymer) synthesized by a high-temperature continuous polymerization method (high-temperature continuous bulk polymerization method) (methods described in U.S. Pat. No. 4,414,370, JP-A-59-6207, JP-B-5-58005, JP-A-1-313522, U.S. Pat. No. 5,010,166, Toa Gosei Kenkyuu Nenpo TREND 2000 Vol. 3, p. 42-45, etc.) with minimal use of auxiliary raw materials such as polymerization initiators, chain transfer agents, and organic solvents. In this specification, (meth)acrylic means methacryl and acrylic.
[0112] Examples of the acrylic monomer components constituting the acrylic resin include (meth)acrylic acid, (meth)acrylic acid esters (alkyl esters such as 2-ethylhexyl acrylate, aryl esters, aralkyl esters, etc.), (meth)acrylamide, (meth)acrylic acid derivatives such as (meth)acrylamide derivatives, etc. (Meth)acrylic acid is a general term for acrylic acid and methacrylic acid.
[0113] Examples of the aromatic vinyl monomer component constituting the acrylic resin include aromatic vinyls such as styrene, α-methylstyrene, vinyltoluene, vinylnaphthalene, divinylbenzene, trivinylbenzene, and divinylnaphthalene.
[0114] As the monomer components constituting the acrylic resin, other monomer components may be used in addition to the (meth)acrylic acid, (meth)acrylic acid derivatives, and aromatic vinyl.
[0115] Examples of the plasticizer that can be used include products from Maruzen Petrochemical Co., Ltd., Sumitomo Bakelite Co., Ltd., Yasuhara Chemical Co., Ltd., Tosoh Corporation, Rutgers Chemicals, BASF, Arizona Chemical Company, Nippon Paint Chemical Co., Ltd., Nippon Shokubai Co., Ltd., ENEOS Corporation, Arakawa Chemical Industries, Ltd., and Taoka Chemical Co., Ltd.
[0116] (Other materials) From the viewpoints of crack resistance, ozone resistance, and the like, the rubber composition preferably contains an antioxidant.
[0117] The antiaging agent is not particularly limited, and examples thereof include naphthylamine-based antiaging agents such as phenyl-α-naphthylamine; diphenylamine-based antiaging agents such as octylated diphenylamine and 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine; N-isopropyl-N'-phenyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, N,N'-di-2-naphthyl-p-phenylenediamine, Examples of the antioxidant include p-phenylenediamine antioxidants such as amines; quinoline antioxidants such as polymerized 2,2,4-trimethyl-1,2-dihydroquinoline; monophenol antioxidants such as 2,6-di-t-butyl-4-methylphenol and styrenated phenol; and bis, tris, and polyphenol antioxidants such as tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane. Among these, p-phenylenediamine antioxidants and quinoline antioxidants are preferred, and N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine and polymerized 2,2,4-trimethyl-1,2-dihydroquinoline are more preferred. Commercially available products include those from Seiko Chemical Co., Ltd., Sumitomo Chemical Co., Ltd., Ouchi Shinko Chemical Co., Ltd., and Flexis Co., Ltd.
[0118] In the rubber composition, the content of the antioxidant is preferably 0.2 parts by mass or more, more preferably 0.5 parts by mass or more, based on 100 parts by mass of the rubber component. The content is preferably 7.0 parts by mass or less, more preferably 4.0 parts by mass or less.
[0119] The rubber composition preferably contains stearic acid. The content of stearic acid in the rubber composition is preferably 0.5 to 10 parts by mass, and more preferably 0.5 to 5 parts by mass, based on 100 parts by mass of the rubber component.
[0120] As the stearic acid, any known stearic acid can be used, for example, products available from NOF Corporation, NOF Corporation, Kao Corporation, Fujifilm Wako Pure Chemical Industries, Ltd., Chiba Fatty Acid Co., Ltd., and the like.
[0121] The rubber composition preferably contains zinc oxide. The content of zinc oxide in the rubber composition is preferably 0.5 to 10 parts by mass, and more preferably 1 to 5 parts by mass, based on 100 parts by mass of the rubber component.
[0122] As the zinc oxide, any known zinc oxide can be used, for example, products available from Mitsui Mining & Smelting Co., Ltd., Toho Zinc Co., Ltd., Hakusui Tech Co., Ltd., Seido Chemical Industry Co., Ltd., Sakai Chemical Industry Co., Ltd., etc.
[0123] The rubber composition may contain wax. The content of the wax in the rubber composition is preferably 0.5 to 10 parts by mass, and more preferably 1 to 5 parts by mass, based on 100 parts by mass of the rubber component.
[0124] The wax is not particularly limited, and examples thereof include petroleum waxes, natural waxes, etc. Also, synthetic waxes obtained by refining or chemically treating multiple waxes can be used. These waxes may be used alone or in combination of two or more kinds.
[0125] Examples of petroleum waxes include paraffin wax and microcrystalline wax. Examples of natural waxes are not particularly limited as long as they are derived from resources other than petroleum, and include, for example, vegetable waxes such as candelilla wax, carnauba wax, Japan wax, rice wax, and jojoba wax; animal waxes such as beeswax, lanolin, and spermaceti; mineral waxes such as ozokerite, ceresin, and petrolactam; and refined products thereof. Examples of commercially available products include products from Ouchi Shinko Chemical Industry Co., Ltd., Nippon Seiro Co., Ltd., and Seiko Chemical Co., Ltd.
[0126] It is preferable to compound sulfur into the rubber composition in that it forms an appropriate amount of crosslinked chains in the polymer chains and imparts good performance.
[0127] In the rubber composition, the amount of sulfur is preferably 0.1 part by mass or more, more preferably 0.3 part by mass or more, and even more preferably 0.5 part by mass or more, based on 100 parts by mass of the rubber component. The amount is preferably 5.0 parts by mass or less, more preferably 3.0 parts by mass or less, and even more preferably 2.0 parts by mass or less.
[0128] Examples of sulfur include powdered sulfur, precipitated sulfur, colloidal sulfur, insoluble sulfur, highly dispersible sulfur, soluble sulfur, etc., which are commonly used in the rubber industry. Commercially available products include those from Tsurumi Chemical Industry Co., Ltd., Karuizawa Sulfur Co., Ltd., Shikoku Chemical Industry Co., Ltd., Flexis Corporation, Nippon Kanzuri Kogyo Co., Ltd., Hosoi Chemical Industry Co., Ltd., etc. These may be used alone or in combination of two or more kinds.
[0129] The rubber composition preferably contains a vulcanization accelerator. In the rubber composition, the content of the vulcanization accelerator is not particularly limited and may be freely determined according to the desired vulcanization speed and crosslink density, but is preferably 0.5 parts by mass or more, more preferably 1.0 parts by mass or more, and even more preferably 1.5 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit is preferably 8.0 parts by mass or less, more preferably 6.0 parts by mass or less, and even more preferably 5.0 parts by mass or less.
[0130] The type of vulcanization accelerator is not particularly limited, and any commonly used accelerator can be used. Examples of the vulcanization accelerator include thiazole-based vulcanization accelerators such as 2-mercaptobenzothiazole, di-2-benzothiazolyl disulfide, and N-cyclohexyl-2-benzothiazyl sulfenamide; thiuram-based vulcanization accelerators such as tetramethylthiuram disulfide (TMTD), tetrabenzylthiuram disulfide (TBzTD), and tetrakis(2-ethylhexyl)thiuram disulfide (TOT-N); sulfenamide-based vulcanization accelerators such as N-cyclohexyl-2-benzothiazole sulfenamide, Nt-butyl-2-benzothiazolyl sulfenamide, N-oxyethylene-2-benzothiazole sulfenamide, N-oxyethylene-2-benzothiazole sulfenamide, and N,N'-diisopropyl-2-benzothiazole sulfenamide; and guanidine-based vulcanization accelerators such as diphenyl guanidine, di-orthotolyl guanidine, and orthotolyl biguanidine. These may be used alone or in combination of two or more. Among them, sulfenamide-based, guanidine-based and benzothiazole-based vulcanization accelerators are preferred.
[0131] In addition to the above components, the rubber composition may contain compounding agents generally used in the tire industry, such as materials such as a mold release agent, as appropriate.
[0132] The rubber composition can be produced by a known method, for example, by kneading the components using a rubber kneading device such as an open roll or a Banbury mixer, followed by vulcanization.
[0133] As for the kneading conditions, in the base kneading step in which additives other than the vulcanizing agent and the vulcanization accelerator are kneaded, the kneading temperature is usually 50 to 200°C, preferably 80 to 190°C, and the kneading time is usually 30 seconds to 30 minutes, preferably 1 minute to 30 minutes. In the finish kneading step in which the vulcanizing agent and the vulcanization accelerator are kneaded, the kneading temperature is usually 100°C or lower, preferably room temperature to 80°C. Furthermore, the composition kneaded with the vulcanizing agent and the vulcanization accelerator is usually subjected to a vulcanization treatment such as press vulcanization. The vulcanization temperature is usually 120 to 200°C, preferably 140 to 180°C.
[0134] The rubber composition can be preferably used for each component of a pneumatic tire such as a cap tread, a base tread, a sidewall, a bead apex, a clinch apex, an inner liner, an undertread, a breaker topping, a ply topping, an insert (sidewall reinforcing layer), etc. Among them, the rubber composition can be preferably used for a cap tread and a base tread.
[0135] A tire is manufactured by a conventional method using a rubber composition. That is, the rubber composition containing the above-mentioned components is extruded in an unvulcanized state to match the shape of a cap tread, a base tread, etc., and molded together with other tire components in a conventional manner on a tire building machine to form an unvulcanized tire. The unvulcanized tire is heated and pressurized in the vulcanizer to obtain a tire.
[0136] Examples of the tire include pneumatic tires and non-pneumatic tires. Among them, pneumatic tires are preferred. The tire can be used as a passenger car tire, a large passenger car tire, a large SUV tire, a heavy load tire such as a truck or a bus tire, a light truck tire, a two-wheeled vehicle tire, a racing tire (high performance tire), a run-flat tire, etc. Among them, it can be preferably used as a passenger car tire. EXAMPLES
[0137] The present invention will be specifically described based on examples, but the present invention is not limited to these examples.
[0138] Various chemicals used in the examples and comparative examples will be collectively described below. SBR3830: Tufuden 3830 manufactured by Asahi Kasei Corporation (styrene content 33% by mass, contains 37.5 parts by mass of oil per 100 parts by mass of rubber solids) BR: Ubepol BR150B (cis content 97% by mass) manufactured by Ube Industries, Ltd. NR:TSR20 Carbon black 1: Show Black N134 (N2SA148m) manufactured by Cabot Japan Co., Ltd. 2 / g) Carbon black 2: Show Black N330 (N2SA75m) manufactured by Cabot Japan Co., Ltd. 2 / g) Silica: Ultrasil VN3 (N2SA175m) manufactured by Evonik Degussa 2 / g) Organosilicon compound 1: Silane coupling agent synthesized in Production Example 1 below Organosilicon compound 2: Si266 (bis(3-triethoxysilylpropyl) disulfide) manufactured by Evonik Degussa Wax: Ozoace wax made by Nippon Seiro Co., Ltd. Anti-aging agent: Nocrac 6C (N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine) (6PPD) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Oil: Diana Process NH-70S (aromatic process oil) manufactured by Idemitsu Kosan Co., Ltd. Stearic acid: Paulownia wood produced by NOF Corporation Zinc oxide: Two types of zinc oxide manufactured by Mitsui Mining & Smelting Co., Ltd. Sulfur: Powdered sulfur manufactured by Tsurumi Chemical Industry Co., Ltd. Vulcanization accelerator CBS: Noccela CZ (N-cyclohexyl-2-benzothiazolyl sulfenamide) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Vulcanization accelerator TBBS: Noccela NS (N-tert-butyl-2-benzothiazylsulfenamide (TBBS)) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Vulcanization accelerator DPG: Noccelaer D (1,3-diphenylguanidine) manufactured by Ouchi Shinko Chemical Industry Co., Ltd.
[0139] (Production Example: Synthesis of Organosilicon Compound 1) A 2L separable flask equipped with a stirrer, reflux condenser, dropping funnel and thermometer was charged with 78.0g (1.0 mol) of anhydrous sodium sulfide, 80.3g (2.5 mol) of sulfur and 480g of ethanol, and heated to 80°C. 566g (2.0 mol) of 6-chlorohexyltriethoxysilane was added dropwise thereto, and the mixture was heated and stirred at 80°C for 10 hours. The reaction liquid was filtered under pressure using a filter plate to obtain a filtrate from which the salt generated as the reaction proceeded was removed. The obtained filtrate was heated to 100°C, and ethanol was distilled off under a reduced pressure of 10mmHg or less to obtain an organosilicon compound 1 (silane coupling agent) as a reaction product. The obtained organosilicon compound 1 had a sulfur content of 18.5% by mass, the average number of sulfur atoms X contained in one molecule of the organosilicon compound was 3.5, and the value of m was 6.
[0140] <Examples and Comparative Examples> (Production of Cap Tread Rubber Composition) According to the composition shown in Table 1, materials other than sulfur and vulcanization accelerator were kneaded for 5 minutes under the condition of 150°C using a 1.7L Banbury mixer manufactured by Kobe Steel, Ltd. to obtain a kneaded product. Next, sulfur and vulcanization accelerator were added to the kneaded product obtained, and the mixture was kneaded for 5 minutes under the condition of 80°C using an open roll to obtain an unvulcanized cap tread rubber composition. The obtained unvulcanized cap tread rubber composition was press-vulcanized in a 0.5 mm thick mold at 170° C. for 20 minutes to obtain a cap tread rubber composition (rubber composition after vulcanization).
[0141] (Manufacturing of test tires (cap tread)) The unvulcanized cap tread rubber composition obtained above was molded into the shape of a cap tread, and was laminated together with other tire components on a tire building machine to form an unvulcanized tire. The tire was then vulcanized at 170°C for 10 minutes to obtain a test tire (cap tread) of size 215 / 55R17.
[0142] (Production of base tread rubber composition) According to the composition shown in Table 2, materials other than sulfur and vulcanization accelerator were kneaded for 5 minutes at 150°C using a 1.7L Banbury mixer manufactured by Kobe Steel, Ltd. to obtain a kneaded product. Next, sulfur and vulcanization accelerator were added to the kneaded product obtained, and the mixture was kneaded for 5 minutes at 80°C using an open roll to obtain an unvulcanized base tread rubber composition. The unvulcanized base red rubber composition obtained was press-vulcanized in a 0.5 mm-thick mold at 170° C. for 20 minutes to obtain a base red rubber composition (rubber composition after vulcanization).
[0143] (Production of test tires (base tread)) The unvulcanized base tread rubber composition obtained above was molded into the shape of a base tread, and was laminated together with other tire components on a tire building machine to form an unvulcanized tire. The tire was then vulcanized at 170°C for 10 minutes to obtain a test tire (base tread) of size 215 / 55R17.
[0144] The following physical property measurements and evaluations were performed using the obtained cap tread rubber composition and test tire (cap tread), and the results are shown in Table 1. Similarly, the following physical property measurements and evaluations were performed using the obtained base tread rubber composition and test tire (base tread), and the results are shown in Table 2. The reference comparative examples in Tables 1 and 2 were Comparative Examples 1-1 and 2-1, respectively.
[0145] [Elongation at break] In accordance with JIS K 6251:2017, a tensile test was carried out at 23°C using No. 7 dumbbell-shaped test pieces made of the above-mentioned cap tread rubber composition and base tread rubber composition, and the breaking elongation EB (%) was measured.
[0146] [Viscoelasticity measurement] The complex elastic modulus E* of the cap tread rubber composition and base tread rubber composition was measured using an Iplexer manufactured by GABO under conditions of a frequency of 10 Hz, an initial strain of 5%, a dynamic strain of 1% and a temperature of 30°C.
[0147] [Chipping resistance at high speeds] Test tires were fitted to all wheels of a domestically produced 2000cc car, and the car was driven at 100km / h on rough roads (unpaved roads with sand and stones scattered around and large unevenness on the road surface), and the sum of chipping and peeling in the tread at the end of the drive was calculated and indexed as the reciprocal (reference comparison example: 100). The higher the index, the better the chipping resistance at high speeds.
[0148] [Table 1]
[0149] [Table 2]
[0150] From each table, it can be seen that the tires of the examples, which had EB / E* of 70 or more and contained a filler containing silica and a silane coupling agent containing an alkoxysilyl group and an organosilicon compound having 6 or more carbon atoms linking sulfur atoms, had excellent chipping resistance at high speeds.
Claims
1. A rubber composition comprising a rubber component, a filler containing silica, and a silane coupling agent, The silane coupling agent includes an organosilicon compound that contains an alkoxysilyl group and a sulfur atom, and the number of carbon atoms connecting the alkoxysilyl group and the sulfur atom is 6 or more, The ratio (EB / E*) of the breaking elongation EB [%] at 23°C to the complex modulus E* [MPa] at 30°C satisfies the following (Formula 1), (Formula 1) EB / E*≧70 the content (mass%) of the butadiene rubber in 100% by mass of the rubber component and the content (parts by mass) of the silica relative to 100 parts by mass of the rubber component satisfy the following (Formula 2), (Formula 2) Butadiene rubber content < Silica content ≦ 50 A rubber composition for tires, in which a carbon black content (parts by mass) per 100 parts by mass of a rubber component and a silica content (parts by mass) per 100 parts by mass of the rubber component satisfy the following formulas: Carbon black content - silica content ≧10
2. A rubber composition comprising a rubber component, a filler containing silica, and a silane coupling agent, The silane coupling agent includes an organosilicon compound that contains an alkoxysilyl group and a sulfur atom, and the number of carbon atoms connecting the alkoxysilyl group and the sulfur atom is 6 or more, The ratio (EB / E*) of the breaking elongation EB [%] at 23°C to the complex modulus E* [MPa] at 30°C satisfies the following (Formula 1), (Formula 1) EB / E*≧70 the content (parts by mass) of carbon black per 100 parts by mass of the rubber component and the content (parts by mass) of silica per 100 parts by mass of the rubber component satisfy the following formulae, Carbon black content - silica content ≧10 A rubber composition for tires, in which a content (mass %) of butadiene rubber in 100 mass % of a rubber component and a content (parts by mass) of silica per 100 parts by mass of the rubber component satisfy the following formulas: 5≦Silica content−butadiene rubber content≦30
3. A rubber composition for tires according to claim 1 or 2, wherein the silica content per 100 parts by mass of the rubber component is 5 parts by mass or more and 150 parts by mass or less.
4. A rubber composition for tires according to claim 1, wherein the content of the organosilicon compound is 0.1 parts by mass or more and 50 parts by mass or less per 100 parts by mass of silica.
5. A rubber composition for tires according to any one of claims 1 to 4, wherein the carbon black content per 100 parts by mass of the rubber component is 5 parts by mass or more and 200 parts by mass or less.
6. A silica content of 5 to 120 parts by mass per 100 parts by mass of the rubber component; 6. The rubber composition for tires according to claim 1, wherein the content of said organosilicon compound is 5 to 15 parts by mass based on 100 parts by mass of silica.
7. 7. The rubber composition for tires according to claim 1, comprising a butadiene rubber, and a styrene-butadiene rubber and / or an isoprene-based rubber.
8. The rubber composition for tires according to claim 1, comprising a butadiene rubber and an isoprene-based rubber.
9. 9. The rubber composition for tires according to claim 1, wherein the content of the butadiene rubber is 15 to 40 mass % and the content of the styrene-butadiene rubber is 35 to 85 mass % based on 100 mass % of the rubber component.
10. 9. The rubber composition for tires according to claim 1, wherein the content of the butadiene rubber is 10 to 45% by mass and the content of the isoprene-based rubber is 40 to 85% by mass, based on 100% by mass of the rubber component.
11. 11. The rubber composition for tires according to claim 1, wherein the content of the carbon black is 5 to 80 parts by mass based on 100 parts by mass of the rubber component.
12. The rubber composition for tires according to claim 2, wherein the content (mass%) of the butadiene rubber in 100 mass% of the rubber component and the content (parts by mass) of the silica per 100 parts by mass of the rubber component satisfy the following (Equation 2): (Formula 2) Butadiene rubber content < Silica content ≦ 50
13. The rubber composition for tires according to any one of claims 1 to 12, wherein the content (mass%) of the butadiene rubber in 100 mass% of the rubber component and the content (parts by mass) of the silica per 100 parts by mass of the rubber component satisfy the following formulas: Silica content-butadiene rubber content≧20
14. The rubber composition for tires according to any one of claims 1 to 13, wherein a content (parts by mass) of carbon black per 100 parts by mass of the rubber component and a content (parts by mass) of silica per 100 parts by mass of the rubber component satisfy the following formulas: Carbon black content - silica content ≧20
15. The rubber composition for tires according to any one of claims 1 to 14, wherein the amount of sulfur per 100 parts by mass of the rubber component is 5.0 parts by mass or less.
16. A tire having a tire member made of the rubber composition according to any one of claims 1 to 15.
17. 17. The tire of claim 16, wherein the tire component is a cap tread.
18. 17. The tire of claim 16, wherein the tire component is a base tread.
Citation Information
Patent Citations
Rubber composition for tire
JP2010095705A
Tire rubber composition and pneumatic tire
JP2018065954A
Rubber composition for tire, and pneumatic tire
JP2018123260A
Rubber composition for tire, and pneumatic tire
JP2018150420A
Method of producing rubber composition for tires
JP2019156930A