tire

A three-layer tire design with asymmetrically positioned layers addresses the issue of reduced wet grip after wear by optimizing complex modulus and loss tangent, enhancing both new and worn performance.

JP7559412B2Active Publication Date: 2024-10-02SUMITOMO RUBBER INDUSTRIES LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020132684
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-04
Publication Date
2024-10-02
Estimated Expiration
2040-08-04

AI Technical Summary

Technical Problem

Tires with a high loss tangent in the cap rubber layer exhibit excellent wet grip performance initially but suffer from hydroplaning and reduced grip performance after wear due to reduced groove volume, with the base rubber layer's exposure leading to heat generation issues.

Method used

A tire design with three rubber layers, where the complex modulus and loss tangent are set in a predetermined relationship, and the third layer is asymmetrically positioned in the tire width direction, minimizing the complex elastic modulus and biasing hardness distribution to enhance wet grip performance.

Benefits of technology

The tire achieves improved overall performance by maintaining wet grip and fuel efficiency both new and after wear, with the asymmetric design reducing the difference in grip performance between new and worn states.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559412000008
    Figure 0007559412000008
  • Figure 0007559412000009
    Figure 0007559412000009
  • Figure 0007559412000001
    Figure 0007559412000001
Patent Text Reader

Abstract

To provide a tire improved in combined performance of low fuel consumption performance, wet-grip performance at the time when the tire is new tire and wet-grip performance at the time when the tire is abraded.SOLUTION: The tire comprises a tread comprising a first rubber layer 6 constituting a tread surface 3, a second rubber layer 7 arranged adjacent to an inner side in a radial direction of the first rubber layer, and a third rubber layer 8 arranged adjacent to an inner side in a radial direction of the second rubber layer. A complex elastic modulus at 30°C of the third rubber layer is lower than complex elastic moduluses at 30°C of the first rubber layer and the second rubber layer, and tanδ at 30°C of the first rubber layer is higher than tanδ at 30°C of the second rubber layer and the third rubber layer. The tread has land parts 2 partitioned by a plurality of circumferential grooves 1 extending continuously in a tire circumferential direction. In a tire meridian cross section including a tire rotation shaft, at least one of the land parts has the third rubber layer formed in a bilaterally-asymmetric shape with respect to a normal line passing through a center in a tire width direction thereof.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a tire. [Background technology]

[0002] Patent Document 1 describes that the tread portion has a two-layer structure (so-called cap / base structure) of a base rubber located on the radially inner side of the tire and a cap rubber located on the radially outer side of the base rubber, and that the handling stability and fuel efficiency of the tire are improved by using a rubber composition with a small loss tangent tan δ for the base rubber. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 3213127 Summary of the Invention [Problem to be solved by the invention]

[0004] In the case of the above-mentioned tire, the loss tangent tanδ of the cap rubber layer is high, so that the wet grip performance is high when new. However, when the cap rubber layer wears, the groove volume of the circumferential groove decreases, making the hydroplaning phenomenon more likely to occur, and coupled with the exposure of the low heat generating base rubber layer, the wet grip performance may be rapidly degraded.

[0005] An object of the present invention is to provide a tire which has improved overall performance including fuel economy, wet grip performance when new, and wet grip performance after wear. [Means for solving the problem]

[0006] As a result of extensive research, the inventors have found that the above-mentioned problems can be solved by providing three or more rubber layers in the tread portion, setting the complex elastic modulus E* and loss tangent tanδ of the rubber layers to a predetermined relationship, and forming the inner base rubber layer corresponding to the bottom of the land portion asymmetrically in the tire width direction, thereby completing the present invention.

[0007] That is, the present invention provides [1] A tire having a tread including at least a first rubber layer constituting a tread surface, a second rubber layer adjacent to the radially inner side of the first rubber layer, and a third rubber layer adjacent to the radially inner side of the second rubber layer, wherein the complex modulus of the third rubber layer at 30°C is lower than the complex modulus of the first rubber layer and the second rubber layer at 30°C, and the tan δ of the first rubber layer at 30°C is higher than the tan δ of the second rubber layer and the third rubber layer at 30°C, the tread has land portions partitioned by a plurality of circumferential grooves extending continuously in the tire circumferential direction, and at least one of the land portions is formed asymmetrically with respect to a normal line passing through the center in the tire width direction in a tire meridian cross section including the tire rotation axis. [2] The tire according to [1], wherein a ratio of a thickness of the third rubber layer to a total thickness of the first rubber layer, the second rubber layer, and the third rubber layer is 0.30 or more. [3] The tire according to [1] or [2], wherein the complex modulus of the second rubber layer at 30° C. is lower than the complex modulus of the first rubber layer at 30° C. [4] The tire according to any one of [1] to [3], wherein the second rubber layer has a complex modulus of 8 MPa or more at 30° C.; [5] The tire according to any one of [1] to [4], wherein the second rubber layer has a tan δ of 0.25 or more at 30° C.; [6] The tire according to any one of [1] to [5], wherein the first rubber layer has a glass transition temperature of -15°C or higher. [7] The tire according to any one of [1] to [6], wherein the second rubber layer has a glass transition temperature of -20°C or higher. [8] The tire according to any one of [1] to [7], wherein the first rubber layer has a breaking elongation of 500% or more as measured in accordance with JIS K 6251. [9] The tire according to any one of [1] to [8], wherein the second rubber layer has a breaking elongation of 450% or more as measured in accordance with JIS K 6251.

[10] The tire according to any one of [1] to [9], wherein the modulus of the second rubber layer at 100% elongation is greater than the modulus of the first rubber layer at 100% elongation.

[11] The tire according to any one of [1] to

[10] , wherein the deepest portion of the groove bottom of any one of the circumferential grooves is formed to be located radially inward of an outermost portion of the second rubber layer in a land portion adjacent to the circumferential groove.

[12] The tire according to any one of [1] to

[11] , wherein the land portion has a sipe the both ends of which do not open into the circumferential groove. Effect of the Invention

[0008] According to the present invention, there is provided a tire which has improved overall performance including fuel economy performance, wet grip performance when new, and wet grip performance after wear. [Brief description of the drawings]

[0009] [Figure 1] 1 is an enlarged cross-sectional view of a portion of a tread of a tire according to an embodiment of the present disclosure. [Diagram 2] FIG. 2 is an enlarged cross-sectional view showing a portion of the tread of a tire according to a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] A tire according to one embodiment of the present disclosure has a tread including at least a first rubber layer constituting a tread surface, a second rubber layer adjacent to the radially inner side of the first rubber layer, and a third rubber layer adjacent to the radially inner side of the second rubber layer, wherein the complex modulus of the third rubber layer at 30°C is lower than the complex modulus of the first rubber layer and the second rubber layer at 30°C, the tan δ of the first rubber layer at 30°C is higher than the tan δ of the second rubber layer and the third rubber layer at 30°C, the tread has land portions separated by a plurality of circumferential grooves extending continuously in the tire circumferential direction, and at least one of the land portions has the third rubber layer formed asymmetrically with respect to a normal line passing through the center in the tire width direction in a tire meridian cross section including the tire rotation axis.

[0011] Although it is not intended to be bound by theory, the following mechanism is considered to suppress the deterioration of wet grip performance after tire wear in this disclosure. That is, by minimizing the complex modulus E* of the third rubber layer and forming the third rubber layer asymmetrically in the land portion, the hardness distribution of the land portion is biased, which affects the ground pressure. In the part with high ground pressure, there are places where the water film does not run up and touches the ground, improving the wet grip performance, and therefore the difference in wet grip performance between when new and when worn can be reduced.

[0012] It is preferable that a ratio of a thickness of the third rubber layer to a total thickness of the first rubber layer, the second rubber layer, and the third rubber layer is 0.30 or more.

[0013] The complex modulus of elasticity at 30°C of the second rubber layer is preferably lower than the complex modulus of elasticity at 30°C of the first rubber layer.

[0014] The second rubber layer preferably has a complex modulus at 30° C. of 8 MPa or more.

[0015] The second rubber layer preferably has a tan δ at 30° C. of 0.25 or more.

[0016] The first rubber layer preferably has a glass transition temperature of -15°C or higher.

[0017] The second rubber layer preferably has a glass transition temperature of -20°C or higher.

[0018] The first rubber layer preferably has an elongation at break measured in accordance with JIS K 6251 of 500% or more.

[0019] The second rubber layer preferably has an elongation at break measured in accordance with JIS K 6251 of 450% or more.

[0020] The modulus of the second rubber layer when stretched 100% is preferably greater than the modulus of the first rubber layer when stretched 100%.

[0021] It is preferable that the deepest portion of the groove bottom of any one of the circumferential grooves is formed so as to be located radially inward of the tire than an outermost portion of the second rubber layer in a land portion adjacent to that circumferential groove, and it is more preferable that the deepest portion of the groove bottom of any one of the circumferential grooves is formed so as to be located radially inward of the tire than an outermost portion of the second rubber layer and the third rubber layer in a land portion adjacent to that circumferential groove.

[0022] It is preferable that a recess is provided in a land portion adjacent to any one of the circumferential grooves, the recess being recessed radially inward relative to an outermost portion of the second rubber layer in the land portion adjacent to the circumferential groove, and a portion of the first rubber layer is formed in the recess of the second rubber layer with a predetermined thickness. It is more preferable that a recess is provided in a land portion adjacent to the circumferential groove, the recess being recessed radially inward relative to an outermost portion of the second rubber layer and the third rubber layer in the land portion adjacent to the circumferential groove, and a portion of the first rubber layer and the second rubber layer is formed in the recess of the third rubber layer with a predetermined thickness.

[0023] It is preferable that the land portion has a sipe having both ends not opening into the circumferential groove.

[0024] A tire according to an embodiment of the present disclosure will be described in detail below. However, the following description is merely an example for explaining the present invention, and is not intended to limit the technical scope of the present invention to the described range. In this specification, when a numerical range is indicated using "to" it is intended to include both ends of the numerical range.

[0025] Fig. 1 is an enlarged cross-sectional view showing a portion of a tire tread. In Fig. 2, the up-down direction is the tire radial direction, the left-right direction is the tire width direction, and the direction perpendicular to the paper surface is the tire circumferential direction.

[0026] As shown in the figure, the tread portion of the tire of the present disclosure includes a first rubber layer 6, a second rubber layer 7, and a third rubber layer 8 (hereinafter, sometimes simply referred to as the "first layer 6", the "second layer 7", and the "third layer 8"). The outer surface of the first layer 6 constitutes the tread surface 3, the second layer 7 is adjacent to the radially inner side of the first layer 6, and the third layer 8 is adjacent to the radially inner side of the second layer 7. The first layer 6 typically corresponds to a cap tread. The second layer 7 and the third layer 8 typically correspond to a base tread or an under tread. In addition, as long as the object of the present invention is achieved, one or more rubber layers may be further provided between the third layer 8 and the belt layer.

[0027] In Fig. 1, double arrow t1 indicates the thickness of the first layer 6, double arrow t2 indicates the thickness of the second layer 7, and double arrow t3 indicates the thickness of the third layer 8. In Fig. 1, the midpoint of the land portion 2 in the tire width direction is indicated by the symbol P. The straight line indicated by the symbol N is a straight line (normal line) that passes through point P and is perpendicular to the tangent plane at point P. In this specification, thicknesses t1, t2, and t3 are measured along the normal line N drawn from point P on the tread surface at a position where no groove exists in the cross section of Fig. 1.

[0028] In the present disclosure, the thickness t1 of the first layer 6 is not particularly limited, but from the viewpoint of wet grip performance, it is preferably 1.0 mm or more, more preferably 1.5 mm or more, and even more preferably 2.0 mm or more. On the other hand, from the viewpoint of heat generation, the thickness t1 of the first layer 6 is preferably 6.0 mm or less, more preferably 5.5 mm or less, and even more preferably 5.0 mm or less.

[0029] In the present disclosure, the thickness t2 of the second layer 7 is not particularly limited, but is preferably 1.0 mm or more, more preferably 2.0 mm or more, and even more preferably 3.0 mm or more. The thickness t2 of the second layer 7 is preferably 10.0 mm or less, more preferably 9.0 mm or less, and even more preferably 8.0 mm or less.

[0030] In the present disclosure, the thickness t3 of the third layer 8 is not particularly limited, but is preferably 1.0 mm or more, more preferably 2.0 mm or more, and even more preferably 3.0 mm or more. The thickness t3 of the third layer 8 is preferably 10.0 mm or less, more preferably 9.0 mm or less, and even more preferably 8.0 mm or less.

[0031] In view of the effects of the present disclosure, the ratio of the thickness of the third layer to the total thickness of the first layer 6, the second layer 7, and the third layer 8 (t3 / (t1+t2+t3)) is preferably 0.25 or more, more preferably 0.28 or more, even more preferably 0.30 or more, still more preferably 0.32 or more, and particularly preferably 0.35 or more.

[0032] The thickness of the first layer 6 is preferably less than the thickness of the second layer 7 .

[0033] The groove depth H1 of the circumferential groove 1 is determined by the distance between the extension line 4 of the land portion 2 and the extension line 5 of the deepest part of the groove bottom of the circumferential groove 1. Note that, for example, when there are multiple circumferential grooves 1, the groove depth H1 can be the distance between the extension line 4 of the land portion 2 and the extension line 5 of the deepest part of the groove bottom of the circumferential groove 1 having the deepest groove depth among the multiple circumferential grooves 1.

[0034] In the present disclosure, the deepest part of the groove bottom of the circumferential groove 1 having the deepest groove depth among the multiple circumferential grooves 1 (the left circumferential groove 1 in FIG. 1 ) is formed to be located radially inward of the outermost part of the second layer 7 and the outermost part of the third layer 8 in the land portion 2 adjacent to that circumferential groove. In other words, the extension line 5 of the deepest part of the groove bottom of the circumferential groove 1 having the deepest groove depth among the multiple circumferential grooves 1 (the left circumferential groove 1 in FIG. 1 ) is located radially inward of the outermost extension line 9 of the second layer 7 and the outermost extension line 10 of the third layer 7 in the land portion 2 adjacent to that circumferential groove.

[0035] In the present disclosure, immediately below (radially inward in the tire direction) the circumferential groove 1 having the deepest groove depth among the multiple circumferential grooves 1 (the circumferential groove 1 on the left side in FIG. 1 ), there is a recess that is recessed radially inward in the tire direction relative to the outermost parts of the second layer 7 and the third layer 8 in the land portion 2 adjacent to that circumferential groove, and a portion of the first layer 6 and the second layer 7 is formed in the recess of the third layer 8 with a predetermined thickness.

[0036] In the tire of the present disclosure, at least one of the land portions 2 has a third layer 8 formed asymmetrically with respect to a normal line N passing through the center in the tire width direction in a tire meridian cross section including the tire rotation axis. The land portion 2 having such an asymmetric third layer 8 may be a land portion 2 located on the outer side of the vehicle with respect to the tire equator when mounted on the vehicle, or may be a land portion 2 located on the inner side of the vehicle with respect to the tire equator when mounted on the vehicle. In addition, the land portion 2 having the asymmetric third layer 8 may be a land portion sandwiched between a plurality of circumferential grooves 1, or may be a shoulder land portion sandwiched between the circumferential groove 1 and the tread ground contact edge, but is preferably a land portion sandwiched between a plurality of circumferential grooves 1.

[0037] In this disclosure, unless otherwise specified, the dimensions and angles of each component of the tire are measured when the tire is mounted on a standard rim and inflated to a standard internal pressure. No load is applied to the tire during measurement. In this specification, the term "standard rim" refers to a rim that is determined for each tire by a standard system that includes the standard on which the tire is based, such as a standard rim for JATMA, a "Design Rim" for TRA, and a "Measuring Rim" for ETRTO. In this specification, the term "standard internal pressure" refers to the air pressure determined for each tire by the standard, such as the maximum air pressure for JATMA, the maximum value listed in the table "TIRE LOAD LIMITS AT VARIOUS COLD INFLATION PRESSURES" for TRA, and "INFLATION PRESSURE" for ETRTO.

[0038] In the present disclosure, "30°C E*" refers to the complex modulus E* under conditions of a temperature of 30°C, an initial strain of 10%, a dynamic strain of 1%, and a frequency of 10 Hz. From the viewpoint of handling stability, the 30°C E* of the first layer 6 is preferably 9 MPa or more, more preferably 10 MPa or more, even more preferably 11 MPa or more, and particularly preferably 12 MPa or more. From the viewpoint of handling stability, the 30°C E* of the second layer 7 is preferably 7 MPa or more, more preferably 8 MPa or more, and even more preferably 9 MPa or more. The 30°C E* of the third layer 8 is preferably 5 MPa or more, more preferably 6 MPa or more, and even more preferably 7 MPa or more. On the other hand, the 30°C E* of the first layer 6, the second layer 7, and the third layer 8 30 From the viewpoint of wet grip performance, ℃E* is preferably 25 MPa or less, more preferably 20 MPa or less, and even more preferably 18 MPa or less. In the present disclosure, 30°CE* of the third layer 8 is lower than 30°CE* of the first layer 6 and the second layer 7. Moreover, 30°CE* of the second layer 7 is preferably lower than 30°CE* of the first layer 6. The 30°CE* of each rubber layer can be appropriately adjusted by the type and amount of the rubber component, filler, softener, etc.

[0039] In the present disclosure, "30°C tan δ" refers to the loss tangent tan δ under the conditions of a temperature of 30°C, an initial strain of 10%, a dynamic strain of 1%, and a frequency of 10 Hz. From the viewpoint of wet grip performance, the 30°C tan δ of the first layer 6 is preferably 0.30 or more, more preferably 0.35 or more, and even more preferably 0.40 or more. The 30°C tan δ of the second layer 7 is preferably 0.20 or more, more preferably 0.25 or more, and even more preferably 0.30 or more. The 30°C tan δ of the third layer 8 is preferably 0.10 or more, more preferably 0.15 or more, and even more preferably 0.20 or more. On the other hand, the 30°C tan δ of the rubber composition constituting the first layer 6, the second layer 7, and the third layer 8 is preferably 0.65 or less, more preferably 0.60 or less, and even more preferably 0.55 or less, from the viewpoint of fuel efficiency performance. In the present disclosure, the 30°C tan δ of the first layer 6 is higher than the 30°C tan δ of the second layer 7 and the third layer 8. The 30° C. tan δ of the second layer 7 is preferably higher than the 30° C. tan δ of the third layer 8. The 30° C. tan δ of each rubber layer can be appropriately adjusted by the types and amounts of the rubber components, fillers, softeners, etc.

[0040] In the present disclosure, the term "elongation at break (EB)" refers to the elongation at break (elongation at break) measured in accordance with JIS K 6251 at a tensile speed of 3.3 mm / sec in an atmosphere of 23°C. From the viewpoint of maintaining the smoothness of the surface, the EB of the first layer 6 is preferably 500% or more, more preferably 510% or more, and even more preferably 520% ​​or more. The EB of the second layer 7 is preferably 450% or more, more preferably 460% or more, and even more preferably 470% or more. The upper limit of the EB of the rubber composition constituting the first layer 6, the second layer 7, and the third layer 8 is not particularly limited.

[0041] The modulus at 100% stretch in the present disclosure refers to the tensile stress at 100% elongation in the grain direction measured in accordance with JIS K 6251 at a tensile speed of 3.3 mm / sec in an atmosphere of 23°C. The modulus at 100% stretch of the first layer 6 is preferably 1.0 MPa or more, more preferably 1.1 MPa or more, even more preferably 1.2 MPa or more, and particularly preferably 1.3 MPa or more. The modulus at 100% stretch of the second layer 7 is preferably 1.0 MPa or more, more preferably 1.1 MPa or more, even more preferably 1.3 MPa or more, and particularly preferably 1.5 MPa or more. The upper limit of the modulus at 100% stretch of the first layer 6, the second layer 7, and the third layer 8 is not particularly limited. In the present disclosure, the modulus at 100% stretch of the second layer 7 is preferably greater than the modulus at 100% stretch of the first layer 6. The difference between the modulus of the second layer 7 at 100% stretch and the modulus of the first layer 6 at 100% stretch is preferably 0.1 MPa or more, more preferably 0.2 MPa or more, and even more preferably 0.3 MPa or more. In this specification, the term "grain direction" refers to the rolling direction when a rubber sheet is formed by extrusion or shearing treatment.

[0042] The EB and modulus at 100% stretching of each rubber layer can be appropriately adjusted by the types and amounts of the rubber components, fillers, softeners, etc., mentioned above.

[0043] The glass transition temperature (Tg) in the present disclosure refers to the tan δ peak temperature measured by the following method. That is, for a rubber test piece (e.g., 20 mm long x 4 mm wide x 1 mm thick) cut out from the inside of the rubber layer of the tread portion of each test tire so that the long side is in the tire circumferential direction, a temperature distribution curve of tan δ is measured under conditions of an initial strain of 10%, a dynamic strain of 1%, and a frequency of 10 Hz using a dynamic viscoelasticity evaluation device (e.g., an Iplexer series manufactured by GABO Corporation), and the temperature corresponding to the largest tan δ value in the obtained temperature distribution curve (tan δ peak temperature) is defined as the glass transition temperature (Tg) in the present disclosure. The Tg of the rubber composition constituting the first layer 6 is preferably -15°C or higher, more preferably -12°C or higher, from the viewpoint of wet grip performance. -10°C or higher is even more preferable. The Tg of the rubber composition constituting the second layer 7 is preferably -20°C or higher, more preferably -15°C or higher, and even more preferably -12°C or higher, from the viewpoint of wet grip performance. The upper limit of the Tg of the rubber compositions constituting the first layer 6, the second layer 7, and the third layer 8 is not particularly limited, but is preferably not higher than 20° C., more preferably not higher than 15° C., and even more preferably not higher than 10° C. The Tg of each rubber layer can be appropriately adjusted by the type and amount of the rubber component, etc.

[0044] [Rubber composition] The tire of the present disclosure can more effectively suppress deterioration of wet grip performance after tire wear by combining the above-described tire structure, particularly the tread shape, with the above-described physical properties of the rubber composition constituting each layer of the tread.

[0045] <Rubber component> The rubber composition according to the present disclosure preferably contains at least one rubber component selected from the group consisting of isoprene-based rubber, styrene butadiene rubber (SBR), and butadiene rubber (BR). The rubber components constituting the first layer 6 and the second layer 7 preferably contain SBR, more preferably contain SBR and BR, and may be rubber components consisting of only SBR and BR. The rubber component constituting the third layer 8 preferably contains isoprene-based rubber, more preferably contains isoprene-based rubber and BR, and may be rubber components consisting of only isoprene-based rubber and BR.

[0046] (Isoprene rubber) As the isoprene-based rubber, for example, isoprene rubber (IR) and natural rubber, which are common in the tire industry, can be used. In addition to unmodified natural rubber (NR), natural rubber also includes modified natural rubber such as epoxidized natural rubber (ENR), hydrogenated natural rubber (HNR), deproteinized natural rubber (DPNR), high-purity natural rubber, and grafted natural rubber. These isoprene-based rubbers may be used alone or in combination of two or more.

[0047] The NR is not particularly limited, and any NR commonly used in the tire industry can be used, such as SIR20, RSS#3, and TSR20.

[0048] In the rubber components constituting the first layer 6 and the second layer 7, when an isoprene-based rubber (preferably natural rubber, more preferably unmodified natural rubber (NR)) is contained, the content in 100% by mass of the rubber component is preferably 50% by mass or less, more preferably 40% by mass or less, even more preferably 30% by mass or less, and particularly preferably 20% by mass or less, from the viewpoint of wet grip performance. In addition, when an isoprene-based rubber is contained, the lower limit of the content is not particularly limited, and can be, for example, 1% by mass or more, 3% by mass or more, 5% by mass or more, 10% by mass or more, or 15% by mass or more.

[0049] When the rubber component constituting the third layer 8 contains an isoprene-based rubber (preferably natural rubber, more preferably unmodified natural rubber (NR)), the content of the isoprene-based rubber in 100% by mass of the rubber component is preferably 20% by mass or more, more preferably 30% by mass or more, and even more preferably 40% by mass or more. The upper limit of the content of the isoprene-based rubber in the rubber component is not particularly limited, and may be 100% by mass.

[0050] (SBR) There is no particular limitation on the SBR, and examples thereof include solution-polymerized SBR (S-SBR), emulsion-polymerized SBR (E-SBR), and modified SBRs thereof (modified S-SBR, modified E-SBR). Modified SBRs include SBRs whose ends and / or main chains are modified, and modified SBRs (condensates, those having a branched structure, etc.) coupled with tin, silicon compounds, etc. Among these, S-SBR and modified SBR are preferred. Furthermore, hydrogenated products of these SBRs (hydrogenated SBR), etc. can also be used. These SBRs may be used alone or in combination of two or more.

[0051] Examples of S-SBR that can be used in the present disclosure include S-SBR manufactured and sold by JSR Corporation, Sumitomo Chemical Co., Ltd., Ube Industries, Ltd., Asahi Kasei Corporation, ZS Elastomers Co., Ltd., and the like.

[0052] From the viewpoints of wet grip performance and abrasion resistance, the styrene content of SBR is preferably 10% by mass or more, more preferably 15% by mass or more, and even more preferably 20% by mass or more. From the viewpoints of temperature dependency of grip performance and blow resistance, the styrene content is preferably 60% by mass or less, more preferably 55% by mass or less, and even more preferably 50% by mass or less. In this specification, the styrene content of SBR is 1 It is calculated by H-NMR measurement.

[0053] The vinyl content of SBR is preferably 10 mol% or more, more preferably 15 mol% or more, and even more preferably 20 mol% or more, from the viewpoints of ensuring reactivity with silica, wet grip performance, rubber strength, and abrasion resistance. Also, the vinyl content of SBR is preferably 70 mol% or less, more preferably 65 mol% or less, and even more preferably 60 mol% or less, from the viewpoints of preventing an increase in temperature dependency, breaking elongation, and abrasion resistance. In this specification, the vinyl content of SBR (amount of 1,2-bonded butadiene units) is measured by infrared absorption spectroscopy.

[0054] From the viewpoint of wet grip performance, the weight average molecular weight (Mw) of SBR is preferably 200,000 or more, more preferably 250,000 or more, and even more preferably 300,000 or more. From the viewpoint of crosslinking uniformity, the weight average molecular weight is preferably 2,000,000 or less, more preferably 1,800,000 or less, and even more preferably 1,500,000 or less. In this specification, the weight average molecular weight of SBR can be calculated in terms of standard polystyrene based on the measured value by gel permeation chromatography (GPC) (for example, GPC-8000 series manufactured by Tosoh Corporation, detector: differential refractometer, column: TSKGEL SUPERMALTIPORE HZ-M manufactured by Tosoh Corporation).

[0055] In the rubber components constituting the first layer 6 and the second layer 7, when SBR is contained, the content in 100% by mass of the rubber component is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 65% ​​by mass or more, and particularly preferably 70% by mass or more, from the viewpoint of wet grip performance. The upper limit of the content of SBR in the rubber component is not particularly limited, and may be 100% by mass. In the rubber component constituting the third layer 8, when SBR is contained, the content in 100% by mass of the rubber component is not particularly limited.

[0056] (BR) The BR is not particularly limited, and can be one that is commonly used in the tire industry, such as BR with a cis content of less than 50% by mass (low cis BR), BR with a cis content of 90% by mass or more (high cis BR), rare earth butadiene rubber (rare earth BR) synthesized using a rare earth catalyst, BR containing syndiotactic polybutadiene crystals (SPB-containing BR), and modified BR (high cis modified BR, low cis modified BR). Modified BR can be BR modified with the same functional groups as those described above for SBR. These BRs can be used alone or in combination of two or more.

[0057] As the high cis BR, for example, those commercially available from Zeon Corporation, Ube Industries, Ltd., JSR Corporation, etc. can be used. By containing high cis BR, low temperature properties and wear resistance can be improved. The cis content is preferably 95 mass% or more, more preferably 96 mass% or more, further preferably 97 mass% or more, and particularly preferably 98 mass% or more. In this specification, the cis content (cis-1,4-bonded butadiene unit amount) is a value calculated by infrared absorption spectrum analysis.

[0058] The rare earth BR is synthesized using a rare earth catalyst, and has a vinyl content of preferably 1.8 mol% or less, more preferably 1.0 mol% or less, and even more preferably 0.8 mol% or less, and a cis content of preferably 95 mass% or more, more preferably 96 mass% or more, even more preferably 97 mass% or more, and particularly preferably 98 mass% or more. As the rare earth BR, for example, commercially available products from LANXESS Co., Ltd. can be used.

[0059] The SPB-containing BR is not one in which 1,2-syndiotactic polybutadiene crystals are simply dispersed in the BR, but one in which the 1,2-syndiotactic polybutadiene crystals are dispersed after being chemically bonded to the BR. As such an SPB-containing BR, commercially available products from Ube Industries, Ltd. can be used.

[0060] As the modified BR, a modified butadiene rubber (modified BR) in which the terminals and / or the main chain are modified with a functional group containing at least one element selected from the group consisting of silicon, nitrogen and oxygen is preferably used.

[0061] Other modified BRs include those obtained by polymerizing 1,3-butadiene with a lithium initiator and then adding a tin compound, and further having the terminals of the modified BR molecule bonded with tin-carbon bonds (tin-modified BR), etc. The modified BR may be either non-hydrogenated or hydrogenated.

[0062] The BRs listed above may be used alone or in combination of two or more.

[0063] The weight average molecular weight (Mw) of BR is preferably 300,000 or more, more preferably 350,000 or more, and even more preferably 400,000 or more from the viewpoint of abrasion resistance. From the viewpoint of crosslinking uniformity, etc., it is preferably 2,000,000 or less, and more preferably 1,000,000 or less. Mw can be determined by standard polystyrene conversion based on the measured value obtained by gel permeation chromatography (GPC) (for example, GPC-8000 series manufactured by Tosoh Corporation, detector: differential refractometer, column: TSKGEL SUPERMALTIPORE HZ-M manufactured by Tosoh Corporation).

[0064] In the rubber components constituting the first layer 6 and the second layer 7, when BR is contained, the content in 100% by mass of the rubber component is preferably 50% by mass or less, more preferably 40% by mass or less, even more preferably 30% by mass or less, and particularly preferably 20% by mass or less, from the viewpoint of wet grip performance. In addition, when BR is contained, the lower limit of the content is not particularly limited, and can be, for example, 1% by mass or more, 3% by mass or more, 5% by mass or more, 10% by mass or more, or 15% by mass or more.

[0065] When the rubber component constituting the third layer 8 contains BR, the content thereof in 100% by mass of the rubber component is preferably 80% by mass or less, more preferably 70% by mass or less, even more preferably 65% ​​by mass or less, and particularly preferably 60% by mass or less. When BR is contained, the lower limit of the content is not particularly limited, and can be, for example, 1% by mass or more, 3% by mass or more, 5% by mass or more, 10% by mass or more, or 15% by mass or more.

[0066] (Other rubber components) The rubber component according to the present disclosure may contain rubber components other than the isoprene-based rubber, SBR, and BR. As the other rubber components, crosslinkable rubber components generally used in the tire industry can be used, such as styrene-isoprene-butadiene copolymer rubber (SIBR), styrene-isobutylene-styrene block copolymer (SIBS), chloroprene rubber (CR), acrylonitrile-butadiene rubber (NBR), hydrogenated nitrile rubber (HNBR), butyl rubber (IIR), ethylene propylene rubber, polynorbornene rubber, silicone rubber, chlorinated polyethylene rubber, fluororubber (FKM), acrylic rubber (ACM), hydrin rubber, etc. These other rubber components may be used alone or in combination of two or more.

[0067] <Filler> The rubber composition according to the present disclosure preferably uses a filler containing carbon black and / or silica. The rubber compositions constituting the first layer 6 and the second layer 7 more preferably contain silica as a filler, and more preferably contain carbon black and silica. The rubber composition constituting the third layer 8 preferably contains carbon black as a filler.

[0068] (Carbon Black) The rubber composition according to the present disclosure preferably contains carbon black. By containing carbon black, weather resistance, antistatic properties, and rubber strength can be improved. As the carbon black, those commonly used in the tire industry can be appropriately used, for example, GPF, FEF, HAF, ISAF, SAF, etc. These carbon blacks may be used alone or in combination of two or more kinds.

[0069] From the perspective of reinforcement, the nitrogen adsorption specific surface area (N2SA) of carbon black is 10m 2 / g or more is preferable, and 20m 2 From the viewpoints of fuel economy and processability, it is more preferable that the tensile strength is 200 m 2 / g or less is preferable, and 150m 2 / g or less is more preferable, and 100m 2 / g or less is more preferable, and 80m 2 / g or less is more preferable, and 50m 2 The N2SA of carbon black is a value measured in accordance with JIS K 6217-2 "Basic properties of carbon black for rubber - Part 2: Determination of specific surface area - Nitrogen adsorption method - Single point method".

[0070] When carbon black is contained, the content per 100 parts by mass of the rubber component is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more from the viewpoint of abrasion resistance and wet grip performance, and is preferably 50 parts by mass or less, more preferably 35 parts by mass or less, even more preferably 20 parts by mass or less, and particularly preferably 10 parts by mass or less from the viewpoint of fuel economy.

[0071] (silica) The silica is not particularly limited, and can be, for example, silica prepared by a dry method (anhydrous silica), silica prepared by a wet method (hydrated silica), or other silica commonly used in the tire industry. Among them, hydrated silica prepared by a wet method is preferred because it contains a large number of silanol groups. These silicas can be used alone or in combination of two or more.

[0072] The nitrogen adsorption specific surface area (N2SA) of silica is set at 140m from the viewpoints of fuel efficiency and wear resistance. 2 / g or more is preferable, and 170m 2 / g or more is more preferable, and 200m 2 From the viewpoints of fuel efficiency and processability, it is more preferable that the tensile strength is 350 m 2 / g or less is preferable, and 300m 2 / g or less is more preferable, and 250m 2 / g or less is more preferable. In this specification, the N2SA of silica is a value measured by the BET method in accordance with ASTM D3037-93.

[0073] When silica is contained, the content per 100 parts by mass of the rubber component is preferably 20 parts by mass or more, more preferably 40 parts by mass or more, even more preferably 50 parts by mass or more, and particularly preferably 60 parts by mass or more, from the viewpoint of wet grip performance, and is preferably 130 parts by mass or less, more preferably 120 parts by mass or less, and even more preferably 110 parts by mass or less, from the viewpoint of abrasion resistance.

[0074] The total content of silica and carbon black per 100 parts by mass of the rubber component is preferably 40 parts by mass or more, more preferably 50 parts by mass or more, and even more preferably 60 parts by mass or more from the viewpoint of abrasion resistance, and is preferably 160 parts by mass or less, more preferably 140 parts by mass or less, and even more preferably 120 parts by mass or less from the viewpoint of fuel economy and elongation at break.

[0075] From the viewpoint of a balance between fuel economy performance, wet grip performance, and abrasion resistance, the rubber composition constituting the first layer 6 and the second layer 7 preferably has a silica content greater than the carbon black content per 100 parts by mass of the rubber component. The ratio of silica to the total content of silica and carbon black in the first layer 6 and the second layer 7 is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 85% by mass or more. The content ratio of silica and carbon black in the rubber composition constituting the third layer 8 is not particularly limited.

[0076] (Other fillers) As fillers other than silica and carbon black, those which have been generally used in the tire industry, such as aluminum hydroxide, calcium carbonate, alumina, clay, and talc, can be used.

[0077] (Silane coupling agent) Silica is preferably used in combination with a silane coupling agent. The silane coupling agent is not particularly limited, and any silane coupling agent conventionally used in combination with silica in the tire industry can be used. Examples of the silane coupling agent include the following mercapto-based silane coupling agents; sulfide-based silane coupling agents such as bis(3-triethoxysilylpropyl) disulfide and bis(3-triethoxysilylpropyl) tetrasulfide; vinyl-based silane coupling agents such as vinyl triethoxysilane and vinyl trimethoxysilane; amino-based silane coupling agents such as 3-aminopropyl triethoxysilane, 3-aminopropyl trimethoxysilane and 3-(2-aminoethyl) aminopropyl triethoxysilane; glycidoxy-based silane coupling agents such as γ-glycidoxypropyl triethoxysilane and γ-glycidoxypropyl trimethoxysilane; nitro-based silane coupling agents such as 3-nitropropyl trimethoxysilane and 3-nitropropyl triethoxysilane; and chloro-based silane coupling agents such as 3-chloropropyl trimethoxysilane and 3-chloropropyl triethoxysilane. Among them, sulfide-based silane coupling agents and / or mercapto-based silane coupling agents are preferred, and mercapto-based silane coupling agents are more preferred. These silane coupling agents may be used alone or in combination of two or more.

[0078] The mercapto-based silane coupling agent is preferably a compound represented by the following formula (1) and / or a compound containing a bonding unit A represented by the following formula (2) and a bonding unit B represented by the following formula (3). [ka] (In the formula, R 101 , R 102 , and R 103 are each independently an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, or -O-(R 111 -O) z -R 112 (z R 111 each independently represents a divalent hydrocarbon group having 1 to 30 carbon atoms; R112 represents an alkyl group having 1 to 30 carbon atoms, an alkenyl group having 2 to 30 carbon atoms, an aryl group having 6 to 30 carbon atoms, or an aralkyl group having 7 to 30 carbon atoms; z represents an integer of 1 to 30; 104 represents an alkylene having 1 to 6 carbon atoms. [ka] [ka] (wherein x represents an integer of 0 or more; y represents an integer of 1 or more; R 201 represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 30 carbon atoms, an alkenyl group having 2 to 30 carbon atoms, or an alkynyl group having 2 to 30 carbon atoms, which may be substituted by a hydroxyl or carboxyl group; R 202 represents an alkylene having 1 to 30 carbon atoms, an alkenylene having 2 to 30 carbon atoms, or an alkynylene having 2 to 30 carbon atoms; 201 and R 202 may form a ring structure.)

[0079] Examples of the compound represented by formula (1) include 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 2-mercaptoethyltrimethoxysilane, 2-mercaptoethyltriethoxysilane, and the compound represented by the following formula (4) (Si363 manufactured by Evonik Degussa), and the compound represented by the following formula (4) can be preferably used. These may be used alone or in combination of two or more kinds. [ka]

[0080] Examples of compounds containing a bond unit A represented by formula (2) and a bond unit B represented by formula (3) include those manufactured and sold by Momentive, Inc. These may be used alone or in combination of two or more.

[0081] When a silane coupling agent is contained, the total content per 100 parts by mass of the rubber component is preferably 0.5 parts by mass or more, more preferably 1.0 parts by mass or more, even more preferably 2.0 parts by mass or more, and particularly preferably 4.0 parts by mass or more, from the viewpoint of improving the dispersibility of silica, and is preferably 20 parts by mass or less, more preferably 12 parts by mass or less, even more preferably 10 parts by mass or less, and particularly preferably 9.0 parts by mass or less, from the viewpoint of preventing a decrease in abrasion resistance.

[0082] The content of silane coupling agent with respect to 100 parts by mass of silica (when multiple silane coupling agents are used, the total amount of all of them) is preferably 1.0 parts by mass or more, more preferably 3.0 parts by mass or more, and even more preferably 5.0 parts by mass or more, from the viewpoint of increasing the dispersibility of silica.Furthermore, from the viewpoint of cost and processability, it is preferably 20 parts by mass or less, more preferably 15 parts by mass or less, and even more preferably 12 parts by mass or less.

[0083] As the filler, in addition to carbon black and silica, other fillers may be used. Such fillers are not particularly limited, and any fillers generally used in this field, such as aluminum hydroxide, alumina (aluminum oxide), calcium carbonate, magnesium sulfate, talc, clay, etc., may be used. These fillers may be used alone or in combination of two or more.

[0084] <Plasticizer> The rubber composition according to the present disclosure preferably contains a plasticizer, such as a resin component, oil, liquid rubber, or an ester-based plasticizer.

[0085] The resin component is not particularly limited, but examples thereof include petroleum resins, terpene resins, rosin resins, phenol resins, etc. These resin components may be used alone or in combination of two or more.

[0086] In this specification, the term "C5 petroleum resin" refers to a resin obtained by polymerizing a C5 fraction. Examples of C5 fractions include petroleum fractions having 4 to 5 carbon atoms, such as cyclopentadiene, pentene, pentadiene, and isoprene. As the C5 petroleum resin, dicyclopentadiene resin (DCPD resin) is preferably used.

[0087] In this specification, the term "aromatic petroleum resin" refers to a resin obtained by polymerizing a C9 fraction, and may be a hydrogenated or modified resin. Examples of the C9 fraction include petroleum fractions having 8 to 10 carbon atoms, such as vinyltoluene, alkylstyrene, indene, and methylindene. Specific examples of aromatic petroleum resins that can be suitably used include coumarone-indene resins, coumarone resins, indene resins, and aromatic vinyl resins. As aromatic vinyl resins, homopolymers of α-methylstyrene or styrene or copolymers of α-methylstyrene and styrene are preferred, and copolymers of α-methylstyrene and styrene are more preferred, because they are economical, easy to process, and have excellent heat generation properties. As aromatic vinyl resins, for example, those commercially available from Kraton, Eastman Chemical, etc. can be used.

[0088] In this specification, the term "C5C9 petroleum resin" refers to a resin obtained by copolymerizing the C5 fraction and the C9 fraction, and may be a hydrogenated or modified resin. Examples of the C5 fraction and the C9 fraction include the petroleum fractions described above. As the C5C9 petroleum resin, for example, those commercially available from Tosoh Corporation, LUHUA, etc. can be used.

[0089] Examples of the terpene resin include polyterpene resins consisting of at least one selected from terpene compounds such as α-pinene, β-pinene, limonene, and dipentene; aromatic modified terpene resins made from the terpene compounds and aromatic compounds; terpene phenolic resins made from terpene compounds and phenolic compounds; and terpene resins obtained by subjecting these terpene resins to hydrogenation treatment (hydrogenated terpene resins). Examples of aromatic compounds that are raw materials for aromatic modified terpene resins include styrene, α-methylstyrene, vinyltoluene, and divinyltoluene. Examples of phenolic compounds that are raw materials for terpene phenolic resins include phenol, bisphenol A, cresol, and xylenol.

[0090] The rosin-based resin is not particularly limited, but examples thereof include natural resin rosin and rosin-modified resins obtained by modifying rosin by hydrogenation, disproportionation, dimerization, esterification, or the like.

[0091] The phenol-based resin is not particularly limited, but examples thereof include phenol formaldehyde resin, alkylphenol formaldehyde resin, alkylphenol acetylene resin, and oil-modified phenol formaldehyde resin.

[0092] From the viewpoint of wet grip performance, the softening point of the resin component is preferably 60° C. or higher, and more preferably 65° C. or higher. From the viewpoint of processability and improving the dispersibility of the rubber component and the filler, the softening point is preferably 150° C. or lower, more preferably 140° C. or lower, and even more preferably 130° C. or lower. In this specification, the softening point may be defined as the temperature at which the ball drops when the softening point specified in JIS K 6220-1:2001 is measured using a ring and ball softening point tester.

[0093] When a resin component is contained, the content per 100 parts by mass of the rubber component is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more from the viewpoint of wet grip performance, and is preferably 60 parts by mass or less, more preferably 50 parts by mass or less, even more preferably 40 parts by mass or less, and particularly preferably 30 parts by mass or less from the viewpoint of suppressing heat buildup.

[0094] Examples of the oil include process oil, vegetable oil, and animal oil. Examples of the process oil include paraffin-based process oil, naphthenic process oil, and aromatic process oil. In addition, as an environmental measure, process oil with a low content of polycyclic aromatic compound (PCA) compounds can be used. Examples of the low PCA content process oil include light extract solvate (MES), treated distillate aromatic extract (TDAE), and heavy naphthenic oil.

[0095] When oil is contained, the content per 100 parts by mass of the rubber component is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more from the viewpoint of processability. Also, from the viewpoint of abrasion resistance, the content is preferably 120 parts by mass or less, more preferably 100 parts by mass or less, and even more preferably 90 parts by mass or less. In this specification, the content of oil includes the amount of oil contained in the oil-extended rubber.

[0096] The liquid rubber is not particularly limited as long as it is a polymer that is in a liquid state at room temperature (25° C.), and examples thereof include liquid butadiene rubber (liquid BR), liquid styrene butadiene rubber (liquid SBR), liquid isoprene rubber (liquid IR), liquid styrene isoprene rubber (liquid SIR), liquid farnesene rubber, etc. These liquid rubbers may be used alone or in combination of two or more kinds.

[0097] When the liquid rubber is contained, the content per 100 parts by mass of the rubber component is preferably 1 part by mass or more, more preferably 2 parts by mass or more, even more preferably 3 parts by mass or more, and particularly preferably 5 parts by mass or more. The content of the liquid rubber is preferably 50 parts by mass or less, more preferably 40 parts by mass or less, and even more preferably 20 parts by mass or less.

[0098] Examples of ester-based plasticizers include dibutyl adipate (DBA), diisobutyl adipate (DIBA), dioctyl adipate (DOA), di-2-ethylhexyl azelate (DOZ), dibutyl sebacate (DBS), diisononyl adipate (DINA), diethyl phthalate (DEP), dioctyl phthalate (DOP), diundecyl phthalate (DUP), dibutyl phthalate (DBP), dioctyl sebacate (DOS), tributyl phosphate (TBP), trioctyl phosphate (TOP), triethyl phosphate (TEP), trimethyl phosphate (TMP), thymidine triphosphate (TTP), tricresyl phosphate (TCP), trixylenyl phosphate (TXP), etc. These ester-based plasticizers may be used alone or in combination of two or more.

[0099] The content of the plasticizer per 100 parts by mass of the rubber component (the total amount when multiple plasticizers are used in combination) is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more from the viewpoint of wet grip performance, and is preferably 120 parts by mass or less, more preferably 100 parts by mass or less, even more preferably 90 parts by mass or less, and particularly preferably 80 parts by mass or less from the viewpoint of processability.

[0100] <Other compounding agents> In addition to the above-mentioned components, the rubber composition according to the present disclosure may appropriately contain compounding agents commonly used in the tire industry, such as wax, processing aids, stearic acid, zinc oxide, antioxidants, vulcanizing agents, and vulcanization accelerators.

[0101] When the wax is contained, the content thereof per 100 parts by mass of the rubber component is preferably 0.5 parts by mass or more, and more preferably 1 part by mass or more, from the viewpoint of weather resistance of the rubber, and is preferably 10 parts by mass or less, and more preferably 5 parts by mass or less, from the viewpoint of preventing whitening of the tire due to bloom.

[0102] Examples of the processing aid include fatty acid metal salts, fatty acid amides, amide esters, silica surfactants, fatty acid esters, mixtures of fatty acid metal salts and amide esters, mixtures of fatty acid metal salts and fatty acid amides, etc. These processing aids may be used alone or in combination of two or more. Examples of the processing aids that can be used include those commercially available from Schill & Seilacher, Performance Additives, etc.

[0103] When a processing aid is contained, the content thereof per 100 parts by mass of the rubber component is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, from the viewpoint of improving processability, and is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, from the viewpoints of abrasion resistance and breaking strength.

[0104] The antiaging agent is not particularly limited, but examples thereof include amine-based, quinoline-based, quinone-based, phenol-based, and imidazole-based compounds, and carbamic acid metal salts, and the like. Phenylenediamine-based antiaging agents such as N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, N-isopropyl-N'-phenyl-p-phenylenediamine, N,N'-diphenyl-p-phenylenediamine, N,N'-di-2-naphthyl-p-phenylenediamine, and N-cyclohexyl-N'-phenyl-p-phenylenediamine, and quinoline-based antiaging agents such as 2,2,4-trimethyl-1,2-dihydroquinoline polymer and 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline are preferred. These antiaging agents may be used alone or in combination of two or more.

[0105] When an antioxidant is contained, the content per 100 parts by mass of the rubber component is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, from the viewpoint of ozone crack resistance of the rubber, and is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, from the viewpoint of abrasion resistance and wet grip performance.

[0106] When stearic acid is contained, the content thereof per 100 parts by mass of the rubber component is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, from the viewpoint of processability, and is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, from the viewpoint of vulcanization speed.

[0107] When zinc oxide is contained, the content per 100 parts by mass of the rubber component is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, from the viewpoint of processability, and is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, from the viewpoint of abrasion resistance.

[0108] As the vulcanizing agent, sulfur is preferably used, and examples of the sulfur that can be used include powdered sulfur, oil-treated sulfur, precipitated sulfur, colloidal sulfur, insoluble sulfur, and highly dispersible sulfur.

[0109] When sulfur is contained as a vulcanizing agent, the content per 100 parts by mass of the rubber component is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, and even more preferably 0.5 parts by mass or more, from the viewpoint of ensuring sufficient vulcanization reaction. Also, from the viewpoint of preventing deterioration, the content is preferably 5.0 parts by mass or less, more preferably 4.0 parts by mass or less, and even more preferably 3.0 parts by mass or less. Note that, when oil-containing sulfur is used as a vulcanizing agent, the content of the vulcanizing agent is the total content of the pure sulfur contained in the oil-containing sulfur.

[0110] Examples of vulcanizing agents other than sulfur include alkylphenol-sulfur chloride condensate, sodium 1,6-hexamethylene-dithiosulfate dihydrate, 1,6-bis(N,N'-dibenzylthiocarbamoyldithio)hexane, etc. As these vulcanizing agents other than sulfur, commercially available products from Taoka Chemical Co., Ltd., Lanxess Co., Ltd., Flexsys, etc. can be used.

[0111] Examples of the vulcanization accelerator include sulfenamide-based, thiazole-based, thiuram-based, thiourea-based, guanidine-based, dithiocarbamic acid-based, aldehyde-amine-based or aldehyde-ammonia-based, imidazoline-based, and xanthate-based vulcanization accelerators. These vulcanization accelerators may be used alone or in combination of two or more. Among them, one or more vulcanization accelerators selected from the group consisting of sulfenamide-based, guanidine-based, and thiazole-based vulcanization accelerators are preferred, and sulfenamide-based vulcanization accelerators are more preferred.

[0112] Examples of sulfenamide vulcanization accelerators include N-tert-butyl-2-benzothiazolylsulfenamide (TBBS), N-cyclohexyl-2-benzothiazolylsulfenamide (CBS), N,N-dicyclohexyl-2-benzothiazolylsulfenamide (DCBS), etc. Among them, N-tert-butyl-2-benzothiazolylsulfenamide (TBBS) is preferred.

[0113] Examples of the guanidine vulcanization accelerator include 1,3-diphenylguanidine (DPG), 1,3-di-o-tolylguanidine, 1-o-tolylbiguanide, di-o-tolylguanidine salt of dicatechol borate, 1,3-di-o-cumenylguanidine, 1,3-di-o-biphenylguanidine, 1,3-di-o-cumenyl-2-propionylguanidine, etc. Among them, 1,3-diphenylguanidine (DPG) is preferable.

[0114] Examples of the thiazole-based vulcanization accelerator include 2-mercaptobenzothiazole, cyclohexylamine salt of 2-mercaptobenzothiazole, di-2-benzothiazolyl disulfide, etc. Among these, 2-mercaptobenzothiazole is preferred.

[0115] When a vulcanization accelerator is contained, the content per 100 parts by mass of the rubber component is preferably 1 part by mass or more, more preferably 2 parts by mass or more. The content per 100 parts by mass of the rubber component is preferably 8 parts by mass or less, more preferably 7 parts by mass or less, and even more preferably 6 parts by mass or less. By setting the content of the vulcanization accelerator within the above range, breaking strength and elongation tend to be secured.

[0116] The rubber composition according to the present disclosure can be produced by a known method, for example, by kneading the above-mentioned components using a rubber kneading device such as an open roll or an internal kneader (such as a Banbury mixer or kneader).

[0117] The kneading step includes, for example, a base kneading step in which compounding ingredients and additives other than the vulcanizing agent and the vulcanization accelerator are kneaded, and a final kneading (F kneading) step in which the vulcanizing agent and the vulcanization accelerator are added to the kneaded product obtained in the base kneading step and kneaded. Furthermore, the base kneading step can be divided into a plurality of steps as desired.

[0118] The kneading conditions are not particularly limited, but examples thereof include a method in which in the base kneading step, kneading is performed for 3 to 10 minutes at a discharge temperature of 150 to 170° C., and in the final kneading step, kneading is performed for 1 to 5 minutes at 70 to 110° C. The vulcanization conditions are not particularly limited, but examples thereof include a method in which vulcanization is performed for 10 to 30 minutes at 150 to 200° C.

[0119] [tire] The tire according to the present disclosure has a tread including a first layer 6, a second layer 7, and a third layer 8, and may be a pneumatic tire or a non-pneumatic tire. The tire is suitable for use as a racing tire, a passenger car tire, a large passenger car tire, a large SUV tire, or a motorcycle tire, and can be used as a summer tire, a winter tire, or a studless tire for each of these.

[0120] A tire having a tread including the first layer 6, the second layer 7, and the third layer 8 can be manufactured by a normal method using the above rubber composition. That is, an unvulcanized rubber composition in which the above components are blended with the rubber component as necessary is extruded into the shapes of the first layer 6, the second layer 7, and the third layer 8 using an extruder equipped with a die of a predetermined shape, and then laminated together with other tire components on a tire building machine and molded by a normal method to form an unvulcanized tire, and the unvulcanized tire is heated and pressurized in a vulcanizer to manufacture a tire. EXAMPLES

[0121] The present disclosure will be described based on examples, but the present disclosure is not limited to only the examples.

[0122] The various chemicals used in the examples and comparative examples are listed below. NR:TSR20 SBR: Tufuden 4850 manufactured by Asahi Kasei Corporation (unmodified S-SBR, styrene content: 40% by mass, vinyl content: 46 mol%, Mw: 350,000, contains 50 parts by mass of oil per 100 parts by mass of rubber solids) BR: UBEPOL BR (registered trademark) 150B manufactured by Ube Industries, Ltd. (vinyl content: 1.5 mol%, cis content: 97 mass%, Mw: 440,000) Carbon black: Show Black N330 (N2SA: 75m) manufactured by Cabot Japan Co., Ltd. 2 / g) Silica: Ultrasil VN3 (N2SA: 175m) manufactured by Evonik Degussa 2 / g) Silane coupling agent: Momentive's NXT-Z45 (mercapto-based silane coupling agent) Oil: VivaTec500 (TDAE oil) manufactured by H&R Corporation Anti-aging agent: Antigen 6C (N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine) manufactured by Sumitomo Chemical Co., Ltd. Wax: Sannock N manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Stearic acid: Beads of stearic acid camellia manufactured by NOF Corporation Zinc oxide: Two types of zinc oxide manufactured by Mitsui Mining & Smelting Co., Ltd. Sulfur: Powdered sulfur manufactured by Karuizawa Sulfur Co., Ltd. Vulcanization accelerator: Noccela CZ (N-cyclohexyl-2-benzothiazolyl sulfenamide) manufactured by Ouchi Shinko Chemical Industry Co., Ltd.

[0123] Examples and Comparative Examples According to the compounding recipes shown in Tables 1 and 2, chemicals other than sulfur and vulcanization accelerator were kneaded for 1 to 10 minutes using a 1.7 L closed type Banbury mixer until the discharge temperature reached 150 to 160 ° C., and a kneaded product was obtained. Next, sulfur and vulcanization accelerator were added to the kneaded product obtained using a two-axis open roll, and the mixture was kneaded for 4 minutes until the temperature reached 105 ° C., and an unvulcanized rubber composition was obtained. The unvulcanized rubber composition obtained was molded according to the shape of the first layer, second layer, and third layer of the tread, and laminated together with other tire components to prepare an unvulcanized tire, which was vulcanized at 170 ° C. to obtain each test tire (size: 195 / 65R15 91V, rim: 15 × 6.0J, internal pressure: 240kPa) shown in Table 3.

[0124] In the tires of Examples 1 to 9 and Comparative Examples 1 and 5, the tread has a first rubber layer constituting the tread surface, a second rubber layer adjacent to the radially inner side of the first rubber layer, and a third rubber layer adjacent to the radially inner side of the second rubber layer, as shown in Fig. 1, and in a tire meridian cross section including the tire rotation axis, the third rubber layer is formed asymmetrically with respect to a normal line passing through the center in the tire width direction of the land portion sandwiched between the circumferential grooves. In the tires of Comparative Examples 2 to 4, the tread has a first rubber layer constituting the tread surface, a second rubber layer adjacent to the radially inner side of the first rubber layer, and a third rubber layer adjacent to the radially inner side of the second rubber layer, as shown in Fig. 2, and in a tire meridian cross section including the tire rotation axis, the third rubber layer is formed symmetrically with respect to a normal line passing through the center in the tire width direction of the land portion sandwiched between the circumferential grooves.

[0125] <Measurement of loss tangent tanδ, complex modulus of elasticity E*, and glass transition temperature (Tg)> For each rubber test piece cut from the inside of the rubber layer of the tread portion of each test tire with a length of 20 mm, width of 4 mm, and thickness of 1 mm, with the tire circumferential direction being the long side, a dynamic viscoelasticity measuring device Iplexer (registered trademark) series manufactured by GABO was used to measure the loss tangent tanδ and the complex modulus of elasticity E* under the conditions of a temperature of 30°C, an initial strain of 10%, a dynamic strain of 1%, and a frequency of 10 Hz. In addition, a temperature distribution curve of the loss tangent tanδ was measured under the conditions of an initial strain of 10%, a dynamic strain of 1%, and a frequency of 10 Hz, and the temperature (tanδ peak temperature) corresponding to the largest tanδ value in the obtained temperature distribution curve was taken as the glass transition temperature (Tg). The thickness direction of the sample was the tire radial direction.

[0126] <Tensile test> A 1 mm thick dumbbell-shaped No. 7 test piece was cut from inside the rubber layer of the tread of each test tire so that the tensile direction was the tire circumferential direction, and a tensile test was carried out in accordance with JIS K 6251:2017 "Vulcanized rubber and thermoplastic rubber - Determination of tensile test properties" at a 23°C atmosphere and a tensile speed of 3.3 mm / sec to measure the elongation at break EB (%) and the modulus at 100% elongation (MPa). The thickness direction of the sample was the tire radial direction.

[0127] <Low fuel consumption performance> Using a rolling resistance tester, the rolling resistance was measured when each new test tire was run under the conditions of rim 15×6.0J, internal pressure 230 kPa, load 4.24 kN, and speed 80 km / h, and the reciprocal was expressed as an index with Comparative Example 1 set at 100. A larger value indicates a smaller rolling resistance and better fuel economy performance.

[0128] <Wet grip performance of new and worn tires> Each test tire (size: 195 / 65R15, rim: 15×6.0J, internal pressure: 230kPa) was attached to all wheels of a vehicle (domestic FF2000cc) and the braking distance from the point where the brakes were applied at a speed of 100km / h was measured on a wet asphalt road surface. Furthermore, after the above tires were thermally aged at 80°C for 7 days, the tread portion was worn along the tread radius so that the thickness of the tread portion was 50% of that of a new tire, and each test tire was attached to all wheels of the vehicle and the braking distance from the point where the brakes were applied at a speed of 100km / h was measured on a wet asphalt road surface. The braking distances of the test tire of Comparative Example 1 when it was new and after it was worn were each set to 100, and the wet grip performance of each tire when it was new and after it was worn was expressed as an index according to the following calculation formula. The larger the index, the better the wet grip performance. (Wet grip performance index when new) = (Braking distance of the tire of Comparative Example 1 when it was new) / (Braking distance of each test tire when it was new)×100 (Wet grip performance index after wear) = (braking distance after wear of the tire of Comparative Example 1) / (braking distance after wear of each test tire)×100

[0129] The target performance value for the overall performance of fuel economy performance, wet grip performance when new, and wet grip performance after wear (the sum of the fuel economy performance index, the wet grip performance index when new, and the wet grip performance index after wear) is more than 300.

[0130] [Table 1]

[0131] [Table 2]

[0132] [Table 3]

[0133] The results in Tables 1 to 3 show that the tire of the present disclosure, which has three or more rubber layers in the tread portion, the complex modulus E* and loss tangent tan δ of the rubber layers being in a predetermined relationship, and the third layer at the bottom of the land portion being formed asymmetrically in the tire width direction, has improved overall performance in terms of fuel efficiency, wet grip performance when new, and wet grip performance after wear. [Explanation of symbols]

[0134] 1...Circumferential groove 2... land department 3. Tread surface 4. Land extension 5. Extension line of the deepest part of the bottom of the circumferential groove 6...First layer 7...Second layer 8...Third layer 9. The outermost extension of the second layer 10. The outermost extension of the third layer

Claims

1. A tire having a tread including at least a first rubber layer constituting a tread surface, a second rubber layer adjacent to the radially inner side of the first rubber layer, and a third rubber layer adjacent to the radially inner side of the second rubber layer, a ratio of a thickness of the third rubber layer to a total thickness of the first rubber layer, the second rubber layer, and the third rubber layer is 0.25 or more; a complex modulus of the third rubber layer at 30° C. is lower than the complex modulus of the first rubber layer and the complex modulus of the second rubber layer at 30° C.; The first rubber layer has a tan δ at 30° C. higher than the tan δ at 30° C. of the second rubber layer and the third rubber layer, The tread has land portions partitioned by a plurality of circumferential grooves extending continuously in a tire circumferential direction, In a tire meridian cross section including the tire rotation axis, at least one of the land portions has the third rubber layer formed asymmetrically with respect to a normal line passing through the center in the tire width direction.

2. A tire having a tread including at least a first rubber layer constituting a tread surface, a second rubber layer adjacent to the radially inward side of the first rubber layer, and a third rubber layer adjacent to the radially inward side of the second rubber layer, a complex modulus of the third rubber layer at 30° C. is lower than the complex modulus of the first rubber layer and the complex modulus of the second rubber layer at 30° C.; The second rubber layer has a complex modulus of elasticity at 30° C. of 7 MPa or more, The first rubber layer has a tan δ at 30° C. higher than the tan δ at 30° C. of the second rubber layer and the third rubber layer, The tread has land portions partitioned by a plurality of circumferential grooves extending continuously in a tire circumferential direction, In a tire meridian cross section including the tire rotation axis, at least one of the land portions has the third rubber layer formed asymmetrically with respect to a normal line passing through the center in the tire width direction.

3. A tire having a tread including at least a first rubber layer constituting a tread surface, a second rubber layer adjacent to the radially inward side of the first rubber layer, and a third rubber layer adjacent to the radially inward side of the second rubber layer, a complex modulus of the third rubber layer at 30° C. is lower than the complex modulus of the first rubber layer and the complex modulus of the second rubber layer at 30° C.; The first rubber layer has a tan δ at 30° C. higher than the tan δ at 30° C. of the second rubber layer and the third rubber layer, the second rubber layer has a tan δ of 0.20 or more at 30° C., The tread has land portions partitioned by a plurality of circumferential grooves extending continuously in a tire circumferential direction, In a tire meridian cross section including the tire rotation axis, at least one of the land portions has the third rubber layer formed asymmetrically with respect to a normal line passing through the center in the tire width direction.

4. A tire having a tread including at least a first rubber layer constituting a tread surface, a second rubber layer adjacent to the radially inward side of the first rubber layer, and a third rubber layer adjacent to the radially inward side of the second rubber layer, a complex modulus of the third rubber layer at 30° C. is lower than the complex modulus of the first rubber layer and the complex modulus of the second rubber layer at 30° C.; The first rubber layer has a tan δ at 30° C. higher than the tan δ at 30° C. of the second rubber layer and the third rubber layer, The glass transition temperature of the first rubber layer is −15° C. or higher, The tread has land portions partitioned by a plurality of circumferential grooves extending continuously in a tire circumferential direction, In a tire meridian cross section including the tire rotation axis, at least one of the land portions has the third rubber layer formed asymmetrically with respect to a normal line passing through the center in the tire width direction.

5. A tire having a tread including at least a first rubber layer constituting a tread surface, a second rubber layer adjacent to the radially inward side of the first rubber layer, and a third rubber layer adjacent to the radially inward side of the second rubber layer, a complex modulus of the third rubber layer at 30° C. is lower than the complex modulus of the first rubber layer and the complex modulus of the second rubber layer at 30° C.; The first rubber layer has a tan δ at 30° C. higher than the tan δ at 30° C. of the second rubber layer and the third rubber layer, The second rubber layer has a glass transition temperature of −20° C. or higher, The tread has land portions partitioned by a plurality of circumferential grooves extending continuously in a tire circumferential direction, In a tire meridian cross section including the tire rotation axis, at least one of the land portions has the third rubber layer formed asymmetrically with respect to a normal line passing through the center in the tire width direction.

6. A tire having a tread including at least a first rubber layer constituting a tread surface, a second rubber layer adjacent to the radially inward side of the first rubber layer, and a third rubber layer adjacent to the radially inward side of the second rubber layer, a complex modulus of the third rubber layer at 30° C. is lower than the complex modulus of the first rubber layer and the complex modulus of the second rubber layer at 30° C.; The first rubber layer has a tan δ at 30° C. higher than the tan δ at 30° C. of the second rubber layer and the third rubber layer, The first rubber layer has an elongation at break of 500% or more as measured in accordance with JIS K 6251, The tread has land portions partitioned by a plurality of circumferential grooves extending continuously in a tire circumferential direction, In a tire meridian cross section including the tire rotation axis, at least one of the land portions has the third rubber layer formed asymmetrically with respect to a normal line passing through the center in the tire width direction.

7. A tire having a tread including at least a first rubber layer constituting a tread surface, a second rubber layer adjacent to the radially inward side of the first rubber layer, and a third rubber layer adjacent to the radially inward side of the second rubber layer, a complex modulus of the third rubber layer at 30° C. is lower than the complex modulus of the first rubber layer and the complex modulus of the second rubber layer at 30° C.; The first rubber layer has a tan δ at 30° C. higher than the tan δ at 30° C. of the second rubber layer and the third rubber layer, The second rubber layer has an elongation at break of 450% or more as measured in accordance with JIS K 6251, The tread has land portions partitioned by a plurality of circumferential grooves extending continuously in a tire circumferential direction, In a tire meridian cross section including the tire rotation axis, at least one of the land portions has the third rubber layer formed asymmetrically with respect to a normal line passing through the center in the tire width direction.

8. A tire having a tread including at least a first rubber layer constituting a tread surface, a second rubber layer adjacent to the radially inward side of the first rubber layer, and a third rubber layer adjacent to the radially inward side of the second rubber layer, a complex modulus of the third rubber layer at 30° C. is lower than the complex modulus of the first rubber layer and the complex modulus of the second rubber layer at 30° C.; The first rubber layer has a tan δ at 30° C. higher than the tan δ at 30° C. of the second rubber layer and the third rubber layer, a modulus of the second rubber layer at 100% elongation is greater than a modulus of the first rubber layer at 100% elongation, The tread has land portions partitioned by a plurality of circumferential grooves extending continuously in a tire circumferential direction, In a tire meridian cross section including the tire rotation axis, at least one of the land portions has the third rubber layer formed asymmetrically with respect to a normal line passing through the center in the tire width direction.

9. A tire having a tread including at least a first rubber layer constituting a tread surface, a second rubber layer adjacent to the radially inward side of the first rubber layer, and a third rubber layer adjacent to the radially inward side of the second rubber layer, The rubber component constituting the first rubber layer contains 50% by mass or more of styrene-butadiene rubber, a complex modulus of the third rubber layer at 30° C. is lower than the complex modulus of the first rubber layer and the complex modulus of the second rubber layer at 30° C.; The first rubber layer has a tan δ at 30° C. higher than the tan δ at 30° C. of the second rubber layer and the third rubber layer, The tread has land portions partitioned by a plurality of circumferential grooves extending continuously in a tire circumferential direction, In a tire meridian cross section including the tire rotation axis, at least one of the land portions has the third rubber layer formed asymmetrically with respect to a normal line passing through the center in the tire width direction.

10. A tire having a tread including at least a first rubber layer constituting a tread surface, a second rubber layer adjacent to the radially inward side of the first rubber layer, and a third rubber layer adjacent to the radially inward side of the second rubber layer, The rubber component constituting the second rubber layer contains 10% by mass or more of butadiene rubber, a complex modulus of the third rubber layer at 30° C. is lower than the complex modulus of the first rubber layer and the complex modulus of the second rubber layer at 30° C.; The first rubber layer has a tan δ at 30° C. higher than the tan δ at 30° C. of the second rubber layer and the third rubber layer, The tread has land portions partitioned by a plurality of circumferential grooves extending continuously in a tire circumferential direction, In a tire meridian cross section including the tire rotation axis, at least one of the land portions has the third rubber layer formed asymmetrically with respect to a normal line passing through the center in the tire width direction.

11. A tire having a tread including at least a first rubber layer constituting a tread surface, a second rubber layer adjacent to the radially inward side of the first rubber layer, and a third rubber layer adjacent to the radially inward side of the second rubber layer, the rubber composition constituting the first rubber layer and / or the second rubber layer has a silica content greater than a carbon black content per 100 parts by mass of the rubber component, a complex modulus of the third rubber layer at 30° C. is lower than the complex modulus of the first rubber layer and the complex modulus of the second rubber layer at 30° C.; The first rubber layer has a tan δ at 30° C. higher than the tan δ at 30° C. of the second rubber layer and the third rubber layer, The tread has land portions partitioned by a plurality of circumferential grooves extending continuously in a tire circumferential direction, In a tire meridian cross section including the tire rotation axis, at least one of the land portions has the third rubber layer formed asymmetrically with respect to a normal line passing through the center in the tire width direction.

12. A tire having a tread including at least a first rubber layer constituting a tread surface, a second rubber layer adjacent to the radially inward side of the first rubber layer, and a third rubber layer adjacent to the radially inward side of the second rubber layer, The tire is a passenger vehicle tire, a complex modulus of the third rubber layer at 30° C. is lower than the complex modulus of the first rubber layer and the complex modulus of the second rubber layer at 30° C.; The first rubber layer has a tan δ at 30° C. higher than the tan δ at 30° C. of the second rubber layer and the third rubber layer, The tread has land portions partitioned by a plurality of circumferential grooves extending continuously in a tire circumferential direction, In a tire meridian cross section including the tire rotation axis, at least one of the land portions has the third rubber layer formed asymmetrically with respect to a normal line passing through the center in the tire width direction.

13. The tire according to any one of claims 1 to 12, wherein a complex modulus of elasticity at 30°C of the second rubber layer is lower than a complex modulus of elasticity at 30°C of the first rubber layer.

14. The tire according to any one of claims 1 to 13, wherein a deepest portion of a groove bottom of any one of the circumferential grooves is formed to be located radially inward of an outermost portion of the second rubber layer in a land portion adjacent to the circumferential groove.

15. The tire according to any one of claims 1 to 14, wherein the land portion has a sipe, both ends of which are not open to the circumferential groove.

Citation Information

Patent Citations

  • Pneumatic tire for heavy load

    JP2005035404A

  • Pneumatic tire for heavy load and its manufacturing method

    JP2006062518A

  • Pneumatic tire

    JP2015131599A

  • Pneumatic tire

    JP2018002008A

  • Pneumatic radial tire with excellent fuel efficiency

    JP3213127B2