Rubber composition for tires and tires
The rubber composition with specific styrene-butadiene rubber and carbon black properties improves wear resistance and traction performance at high temperatures by promoting a regularly arranged crystal structure and enhanced interaction between components.
Patent Information
- Application Number
- JP2020136175
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-12
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2040-08-12
AI Technical Summary
Existing rubber compositions for tires fail to adequately improve wear resistance and traction performance at high temperatures.
A rubber composition containing styrene-butadiene rubber with a trans content/cis content ratio of 3.0 or more, carbon black with a specific surface area of 110 m²/g or more, and vulcanized rubber particles, along with other additives, to enhance interaction and reinforcing properties.
The composition achieves improved wear resistance and traction performance at high temperatures by promoting a regularly arranged crystal structure in the butadiene portion, enhancing rigidity and interaction between rubber components, resulting in better overall performance.
Smart Images

Figure 0007559419000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a rubber composition for a tire and a tire. [Background technology]
[0002] Conventionally, various methods for improving wear resistance and traction performance have been studied (for example, see Patent Documents 1 and 2). However, in recent years, there has been a demand for further improvement in the overall performance of wear resistance and traction performance at high temperatures. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-141405 A [Patent Document 2] JP 2003-25809 A Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present invention is to provide a rubber composition for tires and a tire that can solve the above problems and improve overall performance including wear resistance and traction performance at high temperatures. [Means for solving the problem]
[0005] The present invention relates to a rubber composition for tires, which contains a rubber component containing styrene-butadiene rubber, vulcanized rubber particles, and a filler component containing carbon black, wherein the trans content / cis content of the styrene-butadiene rubber is 3.0 or more, and the content of the vulcanized rubber particles is greater than or equal to the trans content / cis content of the styrene-butadiene rubber.
[0006] The content of the carbon black in 100% by mass of the filler component is preferably 50% by mass or more.
[0007] The rubber composition preferably contains a resin component.
[0008] The carbon black has a cetyltrimethylammonium bromide adsorption specific surface area of 110 m 2 It is preferable that the molecular weight is 1 / g or more.
[0009] The styrene-butadiene rubber preferably has a trans / cis ratio of 4.0 or more.
[0010] The filler component is cetyltrimethylammonium bromide with a specific surface area of 180 m 2 It is preferable that the silica content is at least 1 / g.
[0011] The rubber composition preferably contains a styrene-butadiene rubber that is soluble in acetone when immersed in acetone for 24 hours.
[0012] The rubber composition preferably contains a caprolactam compound.
[0013] The present invention also relates to a tire using the rubber composition. Effect of the Invention
[0014] The present invention relates to a rubber composition for tires which contains a rubber component containing styrene-butadiene rubber, vulcanized rubber particles, and a filler component containing carbon black, in which the trans content / cis content of the styrene-butadiene rubber is 3.0 or more, and the content of the vulcanized rubber particles is equal to or greater than the trans content / cis content of the styrene-butadiene rubber, and therefore the overall performance of the abrasion resistance at high temperatures and the traction performance is good. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The rubber composition for tires of the present invention contains a rubber component containing styrene-butadiene rubber, vulcanized rubber particles, and a filler component containing carbon black, wherein the trans content / cis content of the styrene-butadiene rubber is 3.0 or more, and the content of the vulcanized rubber particles ≧ the trans content / cis content of the styrene-butadiene rubber.
[0016] The reason why the above-mentioned effects are obtained with the above-mentioned rubber composition is presumed to be as follows. In the rubber composition, the trans / cis ratio of the styrene-butadiene rubber is 3.0 or more, so that a regularly arranged crystal structure is appropriately formed in the butadiene part of the styrene-butadiene rubber. As a result, the butadiene part is also likely to have good rigidity, which increases the reaction force against deformation and improves traction performance. In addition, since the trans structure portion tends to have dense molecules, it may be difficult to disperse other chemicals such as filler components, but in the above rubber composition, by making the amount of vulcanized rubber particles previously bonded with sulfur larger than the trans amount / cis amount of styrene-butadiene rubber, interaction between the rubber component of the vulcanized rubber particles and the trans portion of the styrene-butadiene rubber, and interaction between the vulcanized rubber particles and carbon black are likely to occur. As a result, it is believed that good reinforcement properties are obtained even at high temperatures, and wear resistance is improved. It is believed that these actions result in a marked improvement in overall performance, including wear resistance at high temperatures and traction performance.
[0017] The rubber composition contains a rubber component. Here, the rubber component is a component that contributes to crosslinking, and generally has a weight average molecular weight (Mw) of 10,000 or more.
[0018] The weight average molecular weight of the rubber component is preferably 50,000 or more, more preferably 150,000 or more, and even more preferably 200,000 or more, and is preferably 2,000,000 or less, more preferably 1,500,000 or less, and even more preferably 1,000,000 or less. Within the above ranges, the effect tends to be better obtained.
[0019] In this specification, the weight average molecular weight (Mw) can be determined by converting it into standard polystyrene based on the measured value obtained by gel permeation chromatography (GPC) (GPC-8000 series manufactured by Tosoh Corporation, detector: differential refractometer, column: TSKGEL SUPERMULTIPORE HZ-M manufactured by Tosoh Corporation).
[0020] The total styrene content in the rubber component is preferably 10% by mass or more, more preferably 25% by mass or more, and even more preferably 35% by mass or more, and is preferably 70% by mass or less, more preferably 55% by mass or less, and even more preferably 45% by mass or less. Within the above ranges, the effect tends to be better obtained.
[0021] Here, the total amount of styrene in the rubber component is the total content of styrene parts contained in the total amount of rubber component (unit: mass%), and can be calculated by Σ(content of each rubber component × amount of styrene in each rubber component / 100). For example, in a case where 100% by mass of rubber component contains 85% by mass of SBR with styrene content: 40% by mass, 5% by mass of SBR with styrene content: 25% by mass, and 10% by mass of BR with styrene content: 0% by mass, the total amount of styrene in the rubber component is 35.25% by mass (=85×40 / 100+5×25 / 100+10×0 / 100).
[0022] The amount of styrene in each rubber component can be measured by a nuclear magnetic resonance (NMR) method. In addition, the total styrene amount in the rubber component is calculated according to the above-mentioned formula in the examples of this specification, but it may be analyzed from the tire using, for example, a pyrolysis gas chromatograph mass spectrometer (Py-GC / MS) or the like.
[0023] The rubber composition contains styrene-butadiene rubber (SBR) as a rubber component. The SBR is not particularly limited, and for example, emulsion-polymerized styrene-butadiene rubber (E-SBR), solution-polymerized styrene-butadiene rubber (S-SBR), etc. Commercially available products include those from Sumitomo Chemical Co., Ltd., JSR Corporation, Asahi Kasei Corporation, Nippon Zeon Co., Ltd., etc.
[0024] The trans content of SBR is preferably 40% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more, and is preferably 95% by mass or less, more preferably 85% by mass or less, and even more preferably 80% by mass or less. When it is within the above range, the effect tends to be better obtained. In this specification, the trans content of SBR refers to the proportion of trans moieties in 100% by mass of butadiene moieties of SBR.
[0025] The cis content of SBR is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, and is preferably 30% by mass or less, more preferably 25% by mass or less, and even more preferably 20% by mass or less. When it is within the above range, the effect tends to be better obtained. In this specification, the cis content of SBR refers to the proportion of cis portions based on 100% by mass of the butadiene portion of SBR.
[0026] The trans / cis ratio of SBR may be 3.0 or more, but is preferably 4.0 or more, more preferably 4.5 or more, and is preferably 8.0 or less, more preferably 6.5 or less, and even more preferably 5.5 or less. When it is within the above range, the effect tends to be better.
[0027] The above-mentioned trans content and cis content of SBR mean the trans content and cis content of the SBR when there is one type of SBR, and mean the average trans content and average cis content when there are multiple types of SBR. The average trans amount of SBR can be calculated by {Σ(content of each SBR × trans amount of each SBR)} / total content of all SBRs. For example, when 100% by mass of the rubber component contains 85% by mass of SBR with a trans amount of 40% by mass and 5% by mass of SBR with a trans amount of 25% by mass, the average trans amount of the SBRs is 39.2% by mass (=(85×40+5×25) / (85+5)). Similarly, the average cis content of SBR can be calculated by {Σ(content of each SBR × cis content of each SBR)} / total content of all SBRs. For example, when 100% by mass of the rubber component contains 85% by mass of SBR with a cis content of 30% by mass and 5% by mass of SBR with a cis content of 20% by mass, the average cis content of SBR is 29.4% by mass (=(85×30+5×20) / (85+5)).
[0028] In 100% by mass of the rubber component, the content of SBR is preferably 60% by mass or more, more preferably 75% by mass or more, and further preferably 90% by mass or more, and may be 100% by mass. When it is within the above range, the effect tends to be better obtained.
[0029] Examples of rubber components that can be used other than SBR include diene rubbers such as isoprene rubber, butadiene rubber (BR), styrene butadiene rubber (SBR), acrylonitrile butadiene rubber (NBR), chloroprene rubber (CR), butyl rubber (IIR), and styrene-isoprene-butadiene copolymer rubber (SIBR). These may be used alone or in combination of two or more.
[0030] The rubber component may be modified to introduce a functional group that interacts with a filler such as silica. Examples of the functional group include an amino group, an amide group, a silyl group, an alkoxysilyl group, an isocyanate group, an imino group, an imidazole group, a urea group, an ether group, a carbonyl group, an oxycarbonyl group, a mercapto group, a sulfide group, a disulfide group, a sulfonyl group, a sulfinyl group, a thiocarbonyl group, an ammonium group, an imide group, a hydrazo group, an azo group, a diazo group, a carboxyl group, a nitrile group, a pyridyl group, an alkoxy group, a hydroxyl group, an oxy group, and an epoxy group. These functional groups may have a substituent. Among them, an amino group (preferably an amino group in which a hydrogen atom of an amino group is substituted with an alkyl group having 1 to 6 carbon atoms), an alkoxy group (preferably an alkoxy group having 1 to 6 carbon atoms), and an alkoxysilyl group (preferably an alkoxysilyl group having 1 to 6 carbon atoms) are preferred.
[0031] Specific examples of compounds (modifiers) having the above-mentioned functional groups include 2-dimethylaminoethyltrimethoxysilane, 3-dimethylaminopropyltrimethoxysilane, 2-dimethylaminoethyltriethoxysilane, 3-dimethylaminopropyltriethoxysilane, 2-diethylaminoethyltrimethoxysilane, 3-diethylaminopropyltrimethoxysilane, 2-diethylaminoethyltriethoxysilane, 3-diethylaminopropyltriethoxysilane, and the like.
[0032] The rubber composition contains vulcanized rubber particles. The vulcanized rubber particles are particles made of vulcanized rubber, and specifically, rubber powder or the like specified in JIS K 6316:2017 can be used. From the viewpoint of environmental consideration and cost, recycled rubber powder produced from crushed waste tires or the like is preferable. These may be used alone or in combination of two or more types.
[0033] As commercially available vulcanized rubber particles, products from Muraoka Rubber Industries Co., Ltd. and the like can be used.
[0034] The average particle size of the vulcanized rubber particles is preferably 100 μm or more, more preferably 300 μm or more, and even more preferably 400 μm or more, and is preferably 800 μm or less, more preferably 600 μm or less, and even more preferably 500 μm or less. The average particle size of the vulcanized rubber particles is a mass-based average particle size calculated from the particle size distribution measured in accordance with JIS Z 8815:1994.
[0035] The content of the vulcanized rubber particles is preferably 5 parts by mass or more, more preferably 7 parts by mass or more, and even more preferably 10 parts by mass or more, relative to 100 parts by mass of the rubber component, and is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 15 parts by mass or less. Within the above ranges, the effect tends to be better obtained.
[0036] In the above rubber composition, the content of vulcanized rubber particles≧trans content / cis content of SBR.
[0037] The content of vulcanized rubber particles / (trans content of SBR / cis content) is preferably 1.5 or more, more preferably 1.8 or more, and even more preferably 2.0 or more, and is preferably 3.5 or less, more preferably 2.6 or less, and even more preferably 2.4 or less. Within the above ranges, the effect tends to be better obtained.
[0038] The rubber composition contains carbon black as a filler component. The carbon black is not particularly limited, and examples thereof include N134, N110, N220, N234, N219, N339, N330, N326, N351, N550, and N762. Commercially available products include those from Asahi Carbon Co., Ltd., Cabot Japan Co., Ltd., Tokai Carbon Co., Ltd., Mitsubishi Chemical Corporation, Lion Corporation, Shin-Nichika Carbon Co., Ltd., Columbia Carbon Co., Ltd., and the like. These may be used alone or in combination of two or more kinds.
[0039] The cetyltrimethylammonium bromide (CTAB) specific surface area of the carbon black is preferably 110 m 2 / g or more, more preferably 120m 2 / g or more, more preferably 130m 2 / g or more, and preferably 180m 2 / g or less, more preferably 160m 2 / g or less, more preferably 150m 2 Within the above range, there is a tendency for the effect to be better obtained. The CTAB specific surface area of carbon black is a value measured in accordance with JIS K6217-3:2001.
[0040] The amount of carbon black is preferably 50 parts by mass or more, more preferably 60 parts by mass or more, and even more preferably 65 parts by mass or more, per 100 parts by mass of the rubber component, and is preferably 100 parts by mass or less, more preferably 85 parts by mass or less, and even more preferably 75 parts by mass or less. Within the above ranges, the effect tends to be better obtained.
[0041] The amount of carbon black in 100% by mass of the filler contained in the rubber composition is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 65% by mass or more, and is preferably 90% by mass or less, more preferably 80% by mass or less, and even more preferably 75% by mass or less. Within the above ranges, the effect tends to be better obtained.
[0042] The rubber composition preferably contains silica as a filler component. Examples of silica include dry silica (anhydrous silicic acid) and wet silica (hydrated silicic acid), but wet silica is preferred because it has a large number of silanol groups. Commercially available products include those from EVONIK, Tosoh Silica Co., Ltd., Solvay Japan Co., Ltd., Tokuyama Co., Ltd., etc. These may be used alone or in combination of two or more.
[0043] The cetyltrimethylammonium bromide (CTAB) specific surface area of the silica is preferably 160 m 2 / g or more, more preferably 180m 2 / g or more, more preferably 190m 2 / g or more, and preferably 250m 2 / g or less, more preferably 230m 2 / g or less, more preferably 210m 2 Within the above range, there is a tendency for the effect to be better obtained. The CTAB specific surface area of silica is measured in accordance with ASTM D3765-92.
[0044] The content of silica is preferably 10 parts by mass or more, more preferably 25 parts by mass or more, and even more preferably 35 parts by mass or more, and is preferably 60 parts by mass or less, more preferably 50 parts by mass or less, and even more preferably 40 parts by mass or less, based on 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better obtained.
[0045] From the viewpoint of overall performance such as abrasion resistance at high temperatures and traction performance, it is preferable that the carbon black content in the rubber composition is equal to or greater than the silica content.
[0046] The carbon black content / silica content is preferably 1.2 or more, more preferably 1.6 or more, and even more preferably 2.0 or more, and is preferably 4.0 or less, more preferably 3.0 or less, and even more preferably 2.5 or less. Within the above ranges, the effect tends to be better.
[0047] In these relationships, the carbon black content and the silica content are the contents (unit: parts by mass) relative to 100 parts by mass of the rubber component.
[0048] Filler components that can be used other than carbon black and silica include those commonly used in the tire industry, such as aluminum hydroxide, talc, mica, magnesium oxide, magnesium sulfate, etc. These may be used alone or in combination of two or more.
[0049] The content (total content) of the filler components is preferably 60 parts by mass or more, more preferably 80 parts by mass or more, and even more preferably 100 parts by mass or more, relative to 100 parts by mass of the rubber component, and is preferably 160 parts by mass or less, more preferably 140 parts by mass or less, even more preferably 120 parts by mass or less, and particularly preferably 110 parts by mass or less. Within the above ranges, the effect tends to be better obtained.
[0050] The rubber composition preferably contains a silane coupling agent. The silane coupling agent is not particularly limited, and examples thereof include bis(3-triethoxysilylpropyl)tetrasulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(4-triethoxysilylbutyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, bis(2-triethoxysilylethyl)trisulfide, bis(4-trimethoxysilylbutyl)trisulfide, bis(3-triethoxysilylpropyl)disulfide, bis(2-triethoxysilylethyl)disulfide, bis(4-triethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, 3-trimethoxysilylpropyl, mercapto-based compounds such as 3-mercaptopropyltrimethoxysilane and 2-mercaptoethyltriethoxysilane; vinyl-based compounds such as vinyltriethoxysilane and vinyltrimethoxysilane; amino-based compounds such as 3-aminopropyltriethoxysilane and 3-aminopropyltrimethoxysilane; glycidoxy-based compounds such as γ-glycidoxypropyltriethoxysilane and γ-glycidoxypropyltrimethoxysilane; nitro-based compounds such as 3-nitropropyltrimethoxysilane and 3-nitropropyltriethoxysilane; and chloro-based compounds such as 3-chloropropyltrimethoxysilane and 3-chloropropyltriethoxysilane. As commercially available products, for example, products from Degussa, Momentive, Shin-Etsu Silicone Co., Ltd., Tokyo Chemical Industry Co., Ltd., Azumax Co., Ltd., Toray Dow Corning Co., Ltd., etc. can be used. These may be used alone or in combination of two or more. Among them, sulfide-based products are preferred.
[0051] The content of silane coupling agent is preferably 3 parts by mass or more, more preferably 6 parts by mass or more, even more preferably 8 parts by mass or more, and is preferably 15 parts by mass or less, more preferably 12 parts by mass or less, even more preferably 10 parts by mass or less, based on 100 parts by mass of silica.When it is within the above range, the effect tends to be better obtained.
[0052] The rubber composition preferably contains a resin component. Examples of the resin component include aromatic resins, terpene resins, etc. These may be used alone or in combination of two or more. Among these, aromatic resins are preferred.
[0053] An aromatic resin is a polymer containing an aromatic monomer as a constituent monomer, and examples of such a resin include a homopolymer obtained by polymerizing one type of aromatic monomer alone, a copolymer obtained by copolymerizing two or more types of aromatic monomers, and a copolymer of an aromatic monomer and another monomer that can be copolymerized with the aromatic monomer.
[0054] Examples of aromatic monomers include styrene monomers such as styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, α-methylstyrene, p-methoxystyrene, p-tert-butylstyrene, p-phenylstyrene, o-chlorostyrene, m-chlorostyrene, and p-chlorostyrene; phenol monomers such as phenol, alkylphenol, and alkoxyphenol; naphthol monomers such as naphthol, alkylnaphthol, and alkoxynaphthol; coumarone, indene, and the like. These may be used alone or in combination of two or more. Among them, coumarone and indene are preferred.
[0055] The aromatic resin is preferably a polymer containing coumarone and indene as constituent monomers (coumarone-indene resin) because better effects tend to be obtained.
[0056] Examples of commercially available resins that can be used include products from Maruzen Petrochemical Co., Ltd., Sumitomo Bakelite Co., Ltd., Yasuhara Chemical Co., Ltd., Tosoh Corporation, Rutgers Chemicals, BASF, Arizona Chemical Company, Nippon Paint Chemical Co., Ltd., Nippon Shokubai Co., Ltd., JXTG Nippon Oil & Energy Corporation, Arakawa Chemical Industries, Ltd., and Taoka Chemical Co., Ltd.
[0057] The content of the resin component (when a plurality of resins are used in combination, the total content thereof) is preferably 5 parts by mass or more, more preferably 8 parts by mass or more, and even more preferably 10 parts by mass or more, relative to 100 parts by mass of the rubber component, and is preferably 40 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 20 parts by mass or less. Within the above range, the effect tends to be better obtained.
[0058] In the rubber composition, the resin component content / silica content is preferably 0.1 or more, more preferably 0.2 or more, and is preferably 0.8 or less, more preferably 0.6 or less, and even more preferably 0.5 or less. Within the above ranges, the effect tends to be better obtained. In this relationship, the resin component content and the silica content are the contents (unit: parts by mass) relative to 100 parts by mass of the rubber component.
[0059] In the rubber composition, the resin component content / carbon black content is preferably 0.1 or more, and is preferably 0.8 or less, more preferably 0.5 or less, and further preferably 0.3 or less. Within the above range, the effect tends to be better obtained. In this relationship, the resin component content and the carbon black content are the contents (unit: parts by mass) relative to 100 parts by mass of the rubber component.
[0060] The rubber composition preferably contains SBR that is soluble in acetone when immersed in acetone for 24 hours. In this specification, the SBR that is soluble in acetone when immersed in acetone for 24 hours is an SBR that at least a part of which dissolves in acetone when the rubber composition after vulcanization is subjected to acetone extraction for 24 hours according to a method in accordance with JIS K 6229: 2015. This SBR is not included in the rubber component.
[0061] As the SBR that is soluble in acetone when immersed in acetone for 24 hours, SBR that is liquid at room temperature (25°C) (hereinafter also referred to as liquid SBR) can be used, and commercially available products such as those from Cray Valley and Kuraray Co., Ltd. can be used.
[0062] The weight average molecular weight (Mw) of SBR that is soluble in acetone when immersed in acetone for 24 hours (liquid SBR) is preferably 9000 or less, more preferably 6000 or less, and even more preferably 4500 or less, and is preferably 100 or more, more preferably 1000 or more, and even more preferably 2000 or more. Within the above ranges, there is a tendency for better effects to be obtained.
[0063] The content of SBR soluble in acetone when immersed in acetone for 24 hours (liquid SBR) is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more, per 100 parts by mass of the rubber component, and is preferably 40 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 20 parts by mass or less. Within the above ranges, the effect tends to be better obtained.
[0064] The rubber composition preferably contains a caprolactam compound. The caprolactam compounds include N,N'-di(δ-caprolactam) disulfide, N,N'-di(ε-caprolactam) disulfide, N,N'-di(3-methyl-δ-caprolactam) disulfide, N,N'-di(3-ethyl-ε-caprolactam) disulfide, N,N'-di(3-isopropyl-ε-caprolactam) disulfide, and N,N'-di( Examples of the disulfide include N,N'-di(3-ethoxy-ε-caprolactam) disulfide, N,N'-di(3-chloro-ε-caprolactam) disulfide, N,N'-di(δ-nitro-ε-caprolactam) disulfide, N,N'-di(3-amino-ε-caprolactam) disulfide, and dithiodicarolactam. Commercially available products include those from Rhein Chemie. These may be used alone or in combination of two or more. Among these, N,N'-di(ε-caprolactam) disulfide is preferred.
[0065] The content of the caprolactam compound is preferably 0.5 parts by mass or more, more preferably 0.8 parts by mass or more, and even more preferably 1 part by mass or more, and is preferably 6 parts by mass or less, more preferably 4 parts by mass or less, and even more preferably 2 parts by mass or less, based on 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better obtained.
[0066] The rubber composition may contain oil. Examples of the oil include process oil, vegetable oil, and mixtures thereof. Examples of the process oil include paraffin-based process oil, aromatic process oil, and naphthenic process oil. Examples of the vegetable oil include castor oil, cottonseed oil, linseed oil, rapeseed oil, soybean oil, palm oil, coconut oil, peanut oil, rosin, pine oil, pine tar, tall oil, corn oil, rice oil, safflower oil, sesame oil, olive oil, sunflower oil, palm kernel oil, camellia oil, jojoba oil, macadamia nut oil, and tung oil. Examples of commercially available products include products from Idemitsu Kosan Co., Ltd., Sankyo Yuka Kogyo Co., Ltd., JXTG Nippon Oil & Energy Corporation, Orisoi Co., Ltd., H&R Co., Ltd., Toyokuni Oil Mill Co., Ltd., Showa Shell Sekiyu K.K., Fuji Kosan Co., Ltd., and the like. These may be used alone or in combination of two or more.
[0067] The content of the oil is preferably 10 parts by mass or more, more preferably 25 parts by mass or more, and even more preferably 35 parts by mass or more, and is preferably 65 parts by mass or less, more preferably 55 parts by mass or less, and even more preferably 45 parts by mass or less, based on 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better obtained.
[0068] The rubber composition may contain an antioxidant. Examples of the antioxidant include naphthylamine-based antioxidants such as phenyl-α-naphthylamine; diphenylamine-based antioxidants such as octylated diphenylamine and 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine; N-isopropyl-N'-phenyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, and N,N'-di-2-naphthyl-p-phenylenediamine. Examples of the antioxidant include p-phenylenediamine antioxidants such as quinolinone; quinoline antioxidants such as polymers of 2,2,4-trimethyl-1,2-dihydroquinoline; monophenol antioxidants such as 2,6-di-t-butyl-4-methylphenol and styrenated phenol; and bis, tris, and polyphenol antioxidants such as tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane. Commercially available products include those from Seiko Chemical Co., Ltd., Sumitomo Chemical Co., Ltd., Ouchi Shinko Chemical Co., Ltd., and Flexis Co., Ltd. These may be used alone or in combination of two or more.
[0069] The content of the antioxidant is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and even more preferably 3 parts by mass or more, and is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, and even more preferably 6 parts by mass or less, based on 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better.
[0070] The rubber composition may contain a wax. The wax is not particularly limited, and examples thereof include petroleum waxes such as paraffin wax and microcrystalline wax; natural waxes such as vegetable wax and animal wax; and synthetic waxes such as polymers of ethylene, propylene, etc. Commercially available products include those from Ouchi Shinko Chemical Industry Co., Ltd., Nippon Seiro Co., Ltd., Seiko Chemical Co., Ltd., etc. These may be used alone or in combination of two or more kinds.
[0071] The amount of the wax is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and is preferably 10 parts by mass or less, more preferably 6 parts by mass or less, based on 100 parts by mass of the rubber component. Within the above ranges, the effect tends to be better obtained.
[0072] The rubber composition may contain stearic acid. As the stearic acid, a conventionally known one can be used, and as a commercially available product, a product from NOF Corp., Kao Corp., Fujifilm Wako Pure Chemical Corp., Chiba Fatty Acid Corp., etc. can be used. These may be used alone or in combination of two or more kinds.
[0073] The content of stearic acid is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and is preferably 10 parts by mass or less, more preferably 6 parts by mass or less, based on 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better obtained.
[0074] The rubber composition may contain zinc oxide. As the zinc oxide, a conventionally known one can be used, and as a commercially available product, it is possible to use products from Mitsui Mining & Smelting Co., Ltd., Toho Zinc Co., Ltd., Hakusui Tech Co., Ltd., Seido Chemical Industry Co., Ltd., Sakai Chemical Industry Co., Ltd., etc. These may be used alone or in combination of two or more kinds.
[0075] The amount of zinc oxide is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and is preferably 10 parts by mass or less, more preferably 6 parts by mass or less, based on 100 parts by mass of the rubber component. Within the above ranges, the effect tends to be better obtained.
[0076] The rubber composition may contain sulfur. Examples of sulfur include powdered sulfur, precipitated sulfur, colloidal sulfur, insoluble sulfur, highly dispersible sulfur, soluble sulfur, etc., which are commonly used in the rubber industry. Commercially available products include those from Tsurumi Chemical Industry Co., Ltd., Karuizawa Sulfur Co., Ltd., Shikoku Chemical Industry Co., Ltd., Flexis Corporation, Nippon Kanzuri Kogyo Co., Ltd., Hosoi Chemical Industry Co., Ltd., etc. These may be used alone or in combination of two or more kinds.
[0077] The amount of sulfur is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and even more preferably 3 parts by mass or more, and is preferably 8 parts by mass or less, more preferably 6 parts by mass or less, and even more preferably 4 parts by mass or less, based on 100 parts by mass of the rubber component. When the amount is within the above range, the effect tends to be better obtained.
[0078] The rubber composition may contain a vulcanization accelerator. Examples of the vulcanization accelerator include thiazole-based vulcanization accelerators such as 2-mercaptobenzothiazole, di-2-benzothiazolyl disulfide, and dibenzothiazolyl disulfide (MBTS); thiuram-based vulcanization accelerators such as tetramethylthiuram disulfide (TMTD) and tetrakis(2-ethylhexyl)thiuram disulfide (TOT-N); sulfenamide-based vulcanization accelerators such as N-cyclohexyl-2-benzothiazylsulfenamide (CBS), N-tert-butyl-2-benzothiazolyl sulfenamide (TBBS), N-oxyethylene-2-benzothiazole sulfenamide, and N,N'-diisopropyl-2-benzothiazole sulfenamide; and guanidine-based vulcanization accelerators such as diphenylguanidine, di-orthotolylguanidine, and orthotolylbiguanidine. Commercially available products include products from Sumitomo Chemical Co., Ltd., Ouchi Shinko Chemical Co., Ltd., and the like. These may be used alone or in combination of two or more. Among them, thiazole-based vulcanization accelerators and thiuram-based vulcanization accelerators are preferred.
[0079] The content of the vulcanization accelerator is preferably 1 part by mass or more, more preferably 1.5 parts by mass or more, and is preferably 8 parts by mass or less, more preferably 5 parts by mass or less, and further preferably 3 parts by mass or less, based on 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better.
[0080] In addition to the above components, the rubber composition may further contain additives commonly used in the tire industry, such as organic peroxides, etc. The content of the additive is preferably 0.1 to 200 parts by mass per 100 parts by mass of the rubber component.
[0081] The rubber composition can be produced, for example, by kneading the above-mentioned components using a rubber kneading device such as an open roll or a Banbury mixer, and then vulcanizing the mixture.
[0082] As for the kneading conditions, in the base kneading step in which additives other than the vulcanizing agent and the vulcanization accelerator are kneaded, the kneading temperature is usually 100 to 180°C, preferably 120 to 170°C. In the finish kneading step in which the vulcanizing agent and the vulcanization accelerator are kneaded, the kneading temperature is usually 120°C or lower, preferably 85 to 110°C. Furthermore, the composition kneaded with the vulcanizing agent and the vulcanization accelerator is usually subjected to a vulcanization treatment such as press vulcanization. The vulcanization temperature is usually 140 to 190°C, preferably 150 to 185°C. The vulcanization time is usually 5 to 15 minutes.
[0083] The rubber composition can be used (as a rubber composition for tires) for tire components such as treads (cap treads), sidewalls, base treads, under treads, shoulders, clinches, bead apexes, breaker cushion rubbers, carcass cord covering rubbers, insulations, chafers, inner liners, and side reinforcing layers of run-flat tires. Among these, the rubber composition is particularly suitable for treads.
[0084] The tire of the present invention is produced by a conventional method using the above rubber composition. That is, the rubber composition is extruded in an unvulcanized state to match the shape of the tread, etc., and molded together with other tire components in a tire building machine by a normal method to form an unvulcanized tire. The unvulcanized tire is then heated and pressurized in a vulcanizer to obtain a tire.
[0085] The above tires (pneumatic tires, etc.) can be used for passenger car tires; truck and bus tires; motorcycle tires; high-performance tires; winter tires such as studless tires; run-flat tires with side reinforcing layers; tires with sound-absorbing material having a sound-absorbing material such as sponge in the tire cavity; tires with sealing material having a sealant inside or in the tire cavity that can seal in the event of a puncture; tires with electronic components having electronic components such as sensors and wireless tags inside or in the tire cavity, etc., and are suitable for passenger car tires.
[0086] The size of the tire is not particularly limited, and can be appropriately selected, for example, from a tire width in the range of 100 to 400 mm, an aspect ratio in the range of 25 to 85%, and a rim diameter in the range of 10 to 25 inches. Specific examples include 105 / 50R16, 115 / 50R17, 125 / 55R20, 135 / 45R21, 145 / 45R21, 155 / 45R18, 165 / 45R22, 175 / 45R23, 185 / 60R20, 195 / 55R14, 205 / 40R16, 215 / 40R16, 225 / 40R17, 235 / 40R17, 245 / 40R16, 255 / 40R17, 265 / 40R17, 275 / 35R18, 285 / 30R19, and 295 / 45R20. EXAMPLES
[0087] The present invention will be specifically described based on examples, but the present invention is not limited to these examples.
[0088] The various chemicals used in the examples and comparative examples will be described below.
[0089] (Rubber component) SBR1: Tufuden 3830 manufactured by Asahi Kasei Corporation (styrene content: 33% by mass, trans content: 44% by mass, cis content: 21% by mass, contains 37.5 parts by mass of oil per 100 parts by mass of rubber solids) SBR2: JSR0122 manufactured by JSR Corporation (styrene content: 37% by mass, trans content: 71% by mass, cis content: 15% by mass, contains 34 parts by mass of oil per 100 parts by mass of rubber solids) SBR3: JSR1502 manufactured by JSR Corporation (styrene content: 24.5% by mass, trans content: 70% by mass, cis content: 14% by mass)
[0090] (Chemicals other than rubber components) Vulcanized rubber particles: Muraoka Rubber Industries Co., Ltd. (rubber powder: 30 mesh, average particle size: 500 μm) Carbon black 1: N220 (CTAB: 111m 2 / g) Carbon black 2: N134 (CTAB: 135m 2 / g) Silica 1: Ultrasil VN3 (CTAB: 165 m) manufactured by Evonik Degussa 2 / g) Silica 2: Ultrasil 9100GR (CTAB: 200m) manufactured by Evonik Degussa 2 / g) Silane coupling agent: Si266 (bis(3-triethoxysilylpropyl) disulfide) manufactured by Evonik Degussa Resin: Nitto Chemical Co., Ltd. knit resin Kumarone V-120 (kumarone indene resin) Oil: H&R VIVATEC 500 (TDAE oil) Liquid SBR: Ricon 100 (liquid SBR, Mw: 4500) manufactured by Cray Valley Wax: Ozoace 0355 manufactured by Nippon Seiro Co., Ltd. Antioxidant 1: Nocrac 6C (N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Antioxidant 2: Nocrac RD (poly(2,2,4-trimethyl-1,2-dihydroquinoline)) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Stearic acid: NOF Corporation's "Tsubaki" stearic acid Zinc oxide: Zinc oxide No. 1 manufactured by Mitsui Mining & Smelting Co., Ltd. Sulfur: Powdered sulfur manufactured by Tsurumi Chemical Industry Co., Ltd. Vulcanization accelerator 1: Noccela CZ (N-cyclohexyl-2-benzothiazolyl sulfenamide) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Vulcanization accelerator 2: Noccelaer D (diphenyl guanidine) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Vulcanization accelerator 3: Noccela DM (dibenzothiazolyl disulfide) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Vulcanization accelerator 4: Noccela TOT-N (tetrakis(2-ethylhexyl)thiuram disulfide) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Caprolactam compound: Rhenogran CLD-80 (N,N'-di(ε-caprolactam) disulfide) manufactured by Rhein Chemie
[0091] Examples and Comparative Examples According to the composition shown in Table 1, materials other than the caprolactam compound, sulfur, and vulcanization accelerator were kneaded for 5 minutes under the condition of 150 ° C using a 1.7 L Banbury mixer manufactured by Kobe Steel, Ltd. to obtain a kneaded product. Next, the caprolactam compound, sulfur, and vulcanization accelerator were added to the kneaded product obtained, and the mixture was kneaded for 5 minutes under the condition of 80 ° C using an open roll to obtain an unvulcanized rubber composition. The obtained unvulcanized rubber composition was molded into a tread shape, and laminated together with other tire components to form an unvulcanized tire, which was press-vulcanized for 12 minutes under the condition of 150 ° C to produce a test tire (size: 175 / 60R18). The following evaluations were performed using the obtained test tire, and the results are shown in Table 1. In Table 1, the rubber content in oil-extended rubber is listed in the rubber column, and the oil content in oil-extended rubber is added to the oil column.
[0092] (Wear resistance (at high temperatures)) The above test tire, which had been pre-warmed to 70°C using a tire warmer, was mounted on a vehicle and driven at high speed on a test course at an average vehicle speed of 100km. The remaining groove depth of the tread after the drive was then measured and expressed as an index with Comparative Example 2 being set at 100. The larger the index, the larger the remaining groove depth and the better the wear resistance at high temperatures.
[0093] (Traction performance) A vehicle fitted with the above test tires on all wheels was driven on a test course at 80km / h, and the traction performance was evaluated based on the feeling when stepping on the accelerator at the corner exit. The sensory evaluation was carried out by 10 drivers on a 10-point scale, and the total score was expressed as an index, with Comparative Example 3 being 100. The higher the index, the better the traction performance.
[0094] [Table 1]
[0095] As can be seen from Table 1, the Examples were superior to the Comparative Examples in the overall performance (total of each index) of the intended wear resistance at high temperatures and traction performance.
Claims
1. The rubber composition includes a rubber component including styrene-butadiene rubber, vulcanized rubber particles, a filler component including carbon black, and a resin component, The styrene-butadiene rubber has a trans / cis ratio of 3.0 or more, the content of the vulcanized rubber particles is equal to or greater than the trans content / cis content of the styrene-butadiene rubber, The content of the vulcanized rubber particles is a content (unit: parts by mass) relative to 100 parts by mass of the rubber component, the ratio of the content of the resin component to the content of the carbon black is 0.1 or more and 0.8 or less, The content of the resin component is the content (unit: parts by mass) relative to 100 parts by mass of the rubber component, The content of the carbon black is the content (unit: parts by mass) based on 100 parts by mass of the rubber component of the rubber composition for tires.
2. A rubber composition comprising a rubber component including styrene-butadiene rubber, vulcanized rubber particles, and a filler component including carbon black, The styrene-butadiene rubber has a trans / cis ratio of 3.0 or more, the content of the vulcanized rubber particles is equal to or greater than the trans content / cis content of the styrene-butadiene rubber, The content of the vulcanized rubber particles is a content (unit: parts by mass) relative to 100 parts by mass of the rubber component, The rubber composition for tires, wherein the filler component contains silica having a cetyltrimethylammonium bromide adsorption specific surface area of 180 m 2 / g or more.
3. A rubber composition comprising a rubber component including styrene-butadiene rubber, vulcanized rubber particles, a filler component including carbon black, and a caprolactam compound, The styrene-butadiene rubber has a trans / cis ratio of 3.0 or more, the content of the vulcanized rubber particles is equal to or greater than the trans content / cis content of the styrene-butadiene rubber, The content of the vulcanized rubber particles is the content (unit: parts by mass) based on 100 parts by mass of the rubber component of the rubber composition for tires.
4. 4. The rubber composition for tires according to claim 1, wherein the content of the carbon black is 50% by mass or more based on 100% by mass of the filler component.
5. The rubber composition for tires according to any one of claims 1 to 4, which contains a resin component.
6. The carbon black has a cetyltrimethylammonium bromide adsorption specific surface area of 110 m 2 The rubber composition for tires according to any one of claims 1 to 5, wherein the viscosity is 100 / g or more.
7. 7. The rubber composition for tires according to claim 1, wherein the styrene-butadiene rubber has a trans / cis ratio of 4.0 or more.
8. The filler component has a cetyltrimethylammonium bromide adsorption specific surface area of 180 m 2 The rubber composition for tires according to any one of claims 1 to 7, further comprising at least one silica component.
9. 9. The rubber composition for tires according to claim 1, which contains a styrene-butadiene rubber that is soluble in acetone when immersed in acetone for 24 hours.
10. The rubber composition for a tire according to any one of claims 1 to 9, which contains a caprolactam compound.
11. A tire using the rubber composition according to any one of claims 1 to 10.
Citation Information
Patent Citations
Pneumatic tire
JP2003025809A
Tire rubber composition and pneumatic tire
JP2006089552A
Rubber composition for base tread, method for producing the same, and pneumatic tire
JP2010132772A
Rubber composition for canvas chafer and pneumatic tire