Laminated glass, vehicle

The laminated glass design achieves balanced infrared transmittance and heat shielding by using a specific configuration of glass plates and interlayer film with infrared shielding layers, addressing the challenge of integrating information devices in vehicles.

JP7559525B2Active Publication Date: 2024-10-02AGC INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020196303
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-02-13
Filing Date
2020-11-26
Publication Date
2024-10-02
Estimated Expiration
2040-11-26

AI Technical Summary

Technical Problem

Existing laminated glass technologies struggle to balance heat shielding properties with sufficient infrared transmittance in areas where information devices, such as LiDAR, require infrared light transmission, often requiring complex process modifications to achieve this balance.

Method used

A laminated glass design with a specific configuration of glass plates and an interlayer film that includes a high infrared transmittance region and an infrared shielding layer, where the infrared shielding layer is sandwiched between non-shielding layers, ensuring high infrared transmittance in the required areas while maintaining heat shielding properties.

Benefits of technology

The design allows for both effective infrared light transmission for information devices and improved heat shielding, enhancing passenger comfort by reducing temperature rise in the vehicle.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559525000001
    Figure 0007559525000001
  • Figure 0007559525000002
    Figure 0007559525000002
  • Figure 0007559525000003
    Figure 0007559525000003
Patent Text Reader

Abstract

To provide a glass laminate capable of achieving both of heat shielding and infrared transparency in a region in which an information device transmits and / or receives infrared light.SOLUTION: A vehicle glass laminate including a pair of glass plates and an intermediate film positioned between the pair of glass plates includes a see-through region. In the condition that in the see-through region, a region satisfying at least one of T905≥90% and T1550≥80% is defined to be an infrared high transmissive region, the glass laminate is attached to a vehicle, the vehicle is arranged on a horizontal plane, and a straight line horizontal to the vehicle and passing through a point at a lower end in the infrared high transmission region in a plan view is defined to be a straight line P; the see-through region includes a first region existing on the glass laminate above a curve formed by projecting the straight line P onto the glass laminate in the normal direction of the glass laminate at the point of the lower end, and a second region existing below the curve. A proportion of the infrared high transmission region in the first region is 5% or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminated glass and a vehicle. [Background technology]

[0002] In recent years, vehicles are sometimes equipped with information devices that use infrared light to recognize the state of the outside world. In such cases, an information transmission / reception area for transmitting and / or receiving infrared light so that the information device can obtain information about the outside of the vehicle is provided in a part of the windshield, etc.

[0003] On the other hand, a technology is known in which laminated glass having infrared shielding properties imparted thereto by blending an infrared shielding material in the interlayer is used for windshields, etc. The use of this technology is preferable in terms of improving passenger comfort since it improves heat shielding properties, but it may prevent information devices from transmitting and / or receiving infrared light due to a decrease in infrared transmittance in the information transmitting / receiving region.

[0004] As a countermeasure to this problem, it is possible to coat the information transmitting / receiving area with an infrared-shielding material, avoiding the information transmitting / receiving area, or to hollow out the information transmitting / receiving area of ​​the interlayer film containing the infrared-shielding material and replace it with an interlayer film that does not substantially contain the infrared-shielding material, but either of these methods imposes a large process load.

[0005] For this reason, measures have been taken to suppress a decrease in infrared transmittance in the information transmitting and receiving area by partially providing the intermediate film with an area that does not contain an infrared shielding material (see, for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent No. 4876362 [Patent Document 2] International Publication No. 2015 / 019921 Summary of the Invention [Problem to be solved by the invention]

[0007] However, although the above-mentioned measures provide good heat shielding properties, the infrared transmittance of the information transmitting / receiving area is insufficient.

[0008] The present invention has been made in consideration of the above-mentioned points, and has an object to provide laminated glass that combines heat insulation and infrared transparency in the area where an information device transmits and / or receives infrared light. [Means for solving the problem]

[0009] The present laminated glass is a laminated glass for vehicles having a pair of glass sheets and an interlayer film located between the pair of glass sheets, and has a see-through area, and in the see-through area, 905 ≧90%, T 1550 and a high infrared transmission region is a region that satisfies at least one of the above conditions: ≧80%; and when the laminated glass is attached to a vehicle and the vehicle is placed on a horizontal plane, in a plan view, when a straight line that passes through a lower end point of the high infrared transmission region and is horizontal to the vehicle is defined as a line P, the see-through region includes a first region that is above the laminated glass relative to a curve obtained by projecting the line P onto the laminated glass in a normal direction of the laminated glass at the lower end point, and a second region that is below the curve, and a proportion of the high infrared transmission region in the first region is 5% or more. The intermediate film located in the second region has an infrared shielding layer in which infrared shielding fine particles are dispersed, and the infrared shielding layer is sandwiched between infrared non-shielding layers on both sides. Effect of the Invention

[0010] According to one embodiment of the disclosure, it is possible to provide a laminated glass that has both heat insulation properties and infrared transmittance in a region where an information device transmits and / or receives infrared light. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a diagram illustrating an example of laminated glass according to a first embodiment. [Diagram 2]4 is a diagram illustrating the relationship between a high infrared transmittance region and a first region and a second region. FIG. [Diagram 3] 1 is a schematic diagram showing a state in which the laminated glass according to the first embodiment is installed in an opening formed in the front of a vehicle. [Figure 4] FIG. 4 is an enlarged view of a portion S in FIG. [Diagram 5] FIG. 2 is a cross-sectional view illustrating a laminated glass according to a first modified example of the first embodiment. [Figure 6] FIG. 4 is a cross-sectional view illustrating a laminated glass according to a second embodiment. [Figure 7] FIG. 11 is a cross-sectional view illustrating a laminated glass according to Modification 1 of the second embodiment. [Figure 8] FIG. 11 is a cross-sectional view illustrating a laminated glass according to Modification 2 of the second embodiment. [Figure 9] FIG. 11 is a cross-sectional view illustrating a laminated glass according to Modification 3 of the second embodiment. [Figure 10] FIG. 2 is a cross-sectional view illustrating the laminated glass of Example 1. [Figure 11] FIG. 2 is a cross-sectional view illustrating the laminated glass of Example 2. [Figure 12] FIG. 1 is a diagram (part 1) for explaining an embodiment. [Figure 13] FIG. 2 is a diagram (part 2) for explaining the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, the embodiment of the present invention will be described with reference to the drawings. In each drawing, the same components are given the same reference numerals, and duplicated explanations may be omitted. In addition, in the drawings, the size and shape may be partially exaggerated to make the contents of the present invention easier to understand.

[0013] In the following, a vehicle windshield will be described as an example, but the present invention is not limited to this. The laminated glass according to this embodiment can also be applied to other applications besides vehicle windshields, such as side windows and rear windows.

[0014] In the following description, a plan view refers to viewing an object from a normal direction passing through the center of gravity of the main surface of the glass sheet on the vehicle exterior side, and a planar shape refers to the shape of an object viewed from a normal direction passing through the center of gravity of the main surface of the glass sheet on the vehicle exterior side.

[0015] First Embodiment FIG. 1 illustrates an example of laminated glass according to the first embodiment, where FIG. 1(a) is a plan view that shows a schematic view of a state in which a glass plate 11 is arranged facing the front side of the page, and FIG. 1(b) is a cross-sectional view taken along line AA in FIG. 1(a).

[0016] Referring to Fig. 1, the laminated glass 10 is a laminated glass for vehicles having a glass plate 11, a glass plate 12, an interlayer film 13, and a shielding layer 14. However, the shielding layer 14 is provided as necessary. The laminated glass 10 is used, for example, as a windshield for a vehicle. In Fig. 1, the laminated glass 10 is shown in a flat shape, but the laminated glass 10 may be a compound curved shape curved in both the longitudinal direction and the lateral direction. Alternatively, the laminated glass 10 may be a single curved shape curved only in the longitudinal direction or a single curved shape curved only in the lateral direction. When the laminated glass 10 is curved, it is preferable that the curve be convex toward the outside of the vehicle.

[0017] In addition, in FIG. 1(a), the laminated glass 10 has a trapezoidal shape, but the planar shape of the laminated glass 10 is not limited to a trapezoidal shape and may be any shape including a rectangular shape.

[0018] The glass sheet 11 is an interior glass sheet that faces the interior side of the vehicle when the laminated glass 10 is installed in the vehicle. The glass sheet 12 is an exterior glass sheet that faces the exterior side of the vehicle when the laminated glass 10 is installed in the vehicle.

[0019] When the laminated glass 10 is curved, the radius of curvature is preferably 1000 mm or more and 100000 mm or less. The radii of curvature of the glass plates 11 and 12 may be the same or different. When the radii of curvature of the glass plates 11 and 12 are different, the radius of curvature of the glass plate 11 is smaller than the radius of curvature of the glass plate 12.

[0020] The glass plate 11 and the glass plate 12 are a pair of glass plates facing each other, and the interlayer film 13 is located between the pair of glass plates. The glass plate 11 and the glass plate 12 are fixed together with the interlayer film 13 sandwiched therebetween.

[0021] The interlayer film 13 is a film that bonds the glass plate 11 and the glass plate 12. The interlayer film 13 may be composed of multiple layers.

[0022] The outer periphery of the interlayer film 13 is preferably edge-treated. That is, the ends (edges) of the interlayer film 13 are preferably treated so as not to protrude significantly from the ends (edges) of the glass sheets 11 and 12. If the amount of protrusion of the ends of the interlayer film 13 from the ends of the glass sheets 11 and 12 is 150 μm or less, this is preferable in terms of not impairing the appearance. However, when the laminated glass 10 is a side glass, the lower edge is hidden by the door panel, so edge treatment of the lower edge of the interlayer film 13 is not essential. Details of the glass sheets 11, 12, and the interlayer film 13 will be described later.

[0023] The shielding layer 14 is an opaque layer, and can be provided, for example, in a strip shape along the peripheral edge of the laminated glass 10. The shielding layer 14 is, for example, an opaque (for example, black) colored ceramic layer. The shielding layer 14 may be a colored interlayer or film having light-shielding properties, or a combination of a colored interlayer and a colored ceramic layer. The colored film may be integrated with an infrared reflective film or the like.

[0024] The presence of the opaque shielding layer 14 in the laminated glass 10 makes it possible to prevent the adhesive, made of a resin such as urethane, that holds the peripheral edge of the laminated glass 10 to the vehicle body from being deteriorated by ultraviolet rays.

[0025] The shielding layer 14 can be formed, for example, by applying a ceramic color paste containing a fusible glass frit containing a black pigment onto a glass plate by screen printing or the like, and then firing the paste, but is not limited thereto. The shielding layer 14 may also be formed, for example, by applying an organic ink containing a black or dark color pigment onto a glass plate by screen printing or the like, and then drying the ink.

[0026] The shielding layer 14 has an opening 16. That is, the opening 16 corresponds to a small region surrounded by the inner edge of the light-shielding layer 14 in a plan view, which is different from an opening region that surrounds the entire outer periphery of the laminated glass 10. However, when the light-shielding layer 14 is formed in a substantially U-shape, the opening 16 is not partially surrounded by the inner edge. In that case, a straight line virtually connecting one end of the inner edge of the light-shielding layer 14 to the other end may be regarded as part of the inner edge of the light-shielding layer 14.

[0027] The opening 16 is an information transmission / reception area where information devices such as LiDAR (Light Detection And Ranging), rain sensors, collision prevention sensors, white line detectors, night vision devices, etc. transmit and / or receive information. That is, when the laminated glass 10 is mounted on a vehicle, these information devices can be arranged on the vehicle interior side of the opening 16. The band of light used by these information devices is, for example, about 750 nm or more and 1650 nm or less. In particular, LiDAR uses infrared light (for example, wavelengths of 905 nm or 1550 nm).

[0028] The information transmitting / receiving area may be provided with a low reflection coating, an electric heat coating, an anti-fogging coating, etc. Also, a plate-like member or film may be provided in the information transmitting / receiving area.

[0029] The opening 16 is preferably arranged above the test area A defined in the annex of JIS R3212 (2015) "Test Area for Optical Properties and Light Resistance of Safety Glass" in order not to obstruct the driver's view when the laminated glass 10 is installed in a vehicle and to facilitate information acquisition. Unless otherwise specified, the upper side refers to the roof side when the laminated glass 10 is installed in a vehicle, and the lower side refers to the engine room side when the laminated glass 10 is installed in a vehicle. The upper side refers to the upper side of the laminated glass 10. The lower side refers to the lower side of the laminated glass 10. The side side refers to the side between the upper side and the lower side of the laminated glass 10. When the laminated glass 10 is trapezoidal or rectangular, the side side can also be said to be two sides extending in the vertical direction of the laminated glass 10.

[0030] In this embodiment, the shielding layer 14 is disposed between the end of the upper edge of the laminated glass 10 and near the center of the upper edge, and has a first shielding layer 14a which is a portion with a substantially constant width. In addition, at the upper edge of the laminated glass 10, the shielding layer 14 is disposed between the multiple first shielding layers 14a, and has a second shielding layer 14b which is a portion with a substantially constant width. However, the shielding layer 14 does not necessarily have to have the second shielding layer 14b. The substantially constant width allows for a change of up to ±20%.

[0031] In the laminated glass 10, the area where the shielding layer 14 is not formed is the see-through area 15. The inside of the opening 16 is also part of the see-through area 15. Here, the see-through area refers to an area having a visible light transmittance Tv of 70% or more.

[0032] The perspective region 15 includes a first region 151 and a second region 152. The first region 151 is T 905 ≧90%, T 1550≧80% is defined as the high infrared transmittance region 17, which, when viewed in plan, is a region of the laminated glass 10 above a curve obtained by projecting a straight line horizontal to the vehicle that passes through the lower end point of the high infrared transmittance region 17 onto the laminated glass 10 in the normal direction of the laminated glass 10 at the lower end point when the laminated glass 10 is attached to the vehicle and the vehicle is placed on a horizontal plane. The second region 152 is a region below this curve.

[0033] In other words, the high infrared transmittance region 17 is always included in the first region 151, and all or part of the first region 151 becomes the high infrared transmittance region 17. In each drawing, for convenience, the high infrared transmittance region 17 is shown with a matte pattern. In the example of FIG. 1, the entire first region 151 is the high infrared transmittance region 17. In other words, in FIG. 1, the first region 151 and the high infrared transmittance region 17 coincide with each other, and the proportion of the high infrared transmittance region 17 in the first region 151 is 100%.

[0034] In addition, T 905 is the infrared light transmittance of light with a wavelength of 905 nm, and T 1550 is the infrared light transmittance of light with a wavelength of 1550 nm. 905 and T 1550 can be measured according to the measurement method specified in JIS R3106 (1998).

[0035] Here, the relationship between the high infrared transmission region 17 and the first and second regions 151 and 152 will be described. For example, in Fig. 2(a) and Fig. 2(b), a substantially semi-elliptical high infrared transmission region 17 is provided in the see-through region 15. In this case, when the laminated glass 10 is attached to a vehicle and the vehicle is placed on a horizontal plane, a straight line that passes through the lower end point 17a of the high infrared transmission region 17 and is horizontal to the vehicle in a plan view is defined as a straight line P (virtual line). The region of the laminated glass 10 above a curve obtained by projecting the straight line P onto the laminated glass 10 with respect to the normal direction of the laminated glass 10 at the lower end point 17a is the first region 151, and the region below the curve obtained by projecting the straight line P is the second region 152.

[0036] Since the laminated glass 10 is curved, when the straight line P is projected onto the interior side of the glass sheet 11 with respect to the normal direction of the laminated glass 10 at the lower end 17a, the straight line P forms a curve on the interior side of the glass sheet 11.

[0037] Since the opening 16 is an information transmission / reception area where an information device that handles infrared light, such as LiDAR, transmits and / or receives information, the inside of the opening 16 is necessarily a high infrared transmittance area 17. On the other hand, in consideration of the temperature rise inside the vehicle and the heat generated by the occupants, it is preferable that the areas not used by the information device are shielded from infrared light as much as possible. Therefore, it is preferable that as many areas as possible of the see-through area 15 other than the opening 16 are not high infrared transmittance areas 17.

[0038] 2(a) and 2(b), in the first region 151, the high infrared transmission region 17 is provided in a substantially semi-elliptical shape, and the outside of the high infrared transmission region 17 is not the high infrared transmission region 17. Specifically, in the first region 151, an infrared shielding layer, which will be described later, contacts an edge of the outer edge of the first region 151 that extends in the vertical direction. This makes it possible to effectively shield infrared light in the portion corresponding to the arms of the occupant, where the stinging sensation is particularly felt. Also, in the first region 151, the infrared shielding layer may contact an upper edge of the outer edge of the first region 151 that extends in the horizontal direction.

[0039] In the case of Fig. 2(a), the proportion of the high infrared transmittance regions 17 in the first region 151 is about 50%. In the case of Fig. 2(b), the proportion of the high infrared transmittance regions 17 in the first region 151 is about 80%. In the case of Fig. 1, the proportion of the high infrared transmittance regions 17 in the first region 151 is 100%.

[0040] The proportion of the high infrared transmittance region 17 in the first region 151 may be 100% as shown in FIG. 1, but taking into consideration the temperature rise inside the vehicle and the heat-receiving sensation of the occupants as described above, it is preferable that it be 95% or less, and since the area causing the heat-receiving sensation to the arms and heads of the occupants will be reduced, it is more preferable that it be 90% or less, and even more preferable that it be 85% or less.

[0041] Note that, if the inside of the opening 16 is the high infrared transmittance region 17, the see-through region 15 other than the inside of the opening 16 does not need to be the high infrared transmittance region 17. That is, the proportion of the high infrared transmittance region 17 in the first region 151 may be even smaller than that in Fig. 2(a). However, considering the minimum area required by an information device that handles infrared light, such as LiDAR, the proportion of the high infrared transmittance region 17 in the first region 151 needs to be 5% or more.

[0042] The range of the high infrared transmittance region 17 is determined by the layer configuration of the intermediate film 13. That is, as shown in Fig. 1(b), the intermediate film 13 has an infrared shielding layer 135 and an infrared non-shielding layer 136. The infrared shielding layer 135 is a layer in which infrared shielding fine particles are dispersed in an organic resin film, and the infrared non-shielding layer 136 is a layer that does not contain any or almost no infrared shielding fine particles.

[0043] Therefore, in the see-through region 15 of the laminated glass 10, the infrared transmittance of the region where the infrared shielding layer 135 is not arranged in a plan view is higher than the infrared transmittance of the region where the infrared shielding layer 135 is arranged. On the other hand, in the see-through region 15 of the laminated glass 10, the heat shielding property of the region where the infrared shielding layer 135 is arranged in a plan view is higher than the heat shielding property of the region where the infrared shielding layer 135 is not arranged.

[0044] From the viewpoint of heat insulation, when the laminated glass 10 is viewed in a state installed in a vehicle, the vertical width of the first region 151 is preferably 400 mm or less, more preferably 300 mm or less, even more preferably 250 mm or less, and even more preferably 200 mm or less.

[0045] Since the infrared shielding layer 135 is necessarily disposed on the intermediate film 13 located in the second region 152, from the viewpoint of heat shielding properties, it is preferable that the area of ​​the second region 152 occupies a larger area of ​​the see-through region 15. The area of ​​the second region 152 is preferably 50% or more of the area of ​​the see-through region 15, more preferably 60% or more, and even more preferably 70% or more.

[0046] From the viewpoint of heat shielding properties, the minimum value of the total solar transmittance (Tts) of the second region 152 is preferably 75% or less, more preferably 70% or less, and even more preferably 65 or less. Note that the total solar transmittance of the second region 152 is not constant; for example, the total solar transmittance at the lower end of the laminated glass 10 is the minimum value, which effectively results in the highest heat shielding properties.

[0047] In the example of FIG. 1(b), when the laminated glass 10 is viewed in a state where it is attached to a vehicle, the infrared shielding layer 135 is provided in a cross-sectional wedge shape in which the thickness decreases from the lower end side of the laminated glass 10 toward the upper end, and is sandwiched from both sides by the infrared non-shielding layer 136. The infrared non-shielding layer 136 is integrally formed with the high infrared transmission region 17 and the other region. Therefore, a laminated glass having excellent impact resistance and penetration resistance can be provided. The other region is, for example, a region outside the high infrared transmission region 17. The wedge angle of the infrared shielding layer 135 is approximately constant at each position in the longitudinal direction of the infrared shielding layer 135. In the see-through region 15, the region where the infrared shielding layer 135 is not arranged in a plan view forms the high infrared transmission region 17.

[0048] In this way, by providing the infrared shielding layer 135 in a wedge-shaped cross section from the lower end side to the upper end side of the laminated glass 10, the color tone changes gradually from the region where the infrared shielding layer 135 is disposed to the region where the infrared shielding layer 135 is not disposed. In other words, a sudden change in color tone can be suppressed, and the color tone uniformity of the entire laminated glass 10 can be improved.

[0049] The change in transmitted color tone over a 10 mm width preferably satisfies ΔE≦4. If the change in transmitted color tone over a 10 mm width is ΔE≦4, the change in color tone in the laminated glass 10 is not noticeable, and the color uniformity of the entire laminated glass 10 can be improved.

[0050] Here, ΔE is the L standardized by CIE 1976. * a * b * The L of two colors expressed by the chromaticity coordinates in the color system* a * b * A value expressed using the difference between the values ​​of ΔE = ((ΔL * ) 2 +(Δa * ) 2 +(Δb * ) 2 ) 1 / 2 ΔE is the ratio of the tristimulus values ​​XYZ of the XYZ color system measured in accordance with JIS Z8722:2009 to the ΔE of JIS Z8781-4:2013. * ab This was calculated using the formula:

[0051] The infrared shielding fine particles mixed in the infrared shielding layer 135 preferably have a particle size of 0.2 μm or less, more preferably 0.001 μm to 0.15 μm or less. Examples of the material of the infrared shielding fine particles include fine particles made of metals, oxides, nitrides, and sulfides of Sn, Ti, Si, Zn, Zr, Fe, Al, Cr, Co, Ce, In, Ni, Ag, Cu, Pt, Mn, Ta, W, V, and Mo, or doped materials obtained by doping these with Sb or F. These fine particles can be used alone or as a composite. In particular, it is effective to use a mixture in which these alone or a composite is mixed with an organic resin, or a coating in which these alone or a composite is coated with an organic resin, in order to obtain various properties required for automobile window glass.

[0052] As the infrared shielding particles, it is preferable to use at least one of antimony-doped tin oxide (ATO) particles and tin-doped indium oxide (ITO) particles. Both ATO particles and ITO particles have excellent infrared shielding performance, and only a small amount of them is required to be mixed into the intermediate film. In addition, when comparing ATO particles with ITO particles, ITO particles have better infrared shielding performance, so it is particularly preferable to use ITO particles as the infrared shielding particles.

[0053] The infrared shielding layer 135 preferably has infrared shielding fine particles dispersed therein at a dispersion blending ratio of 0.1 to 0.5 parts by mass relative to 100 parts by mass of the total mass of the infrared shielding layer 135. An amount of 0.1 part by mass or more can provide the desired infrared shielding performance, while an amount of 0.5 part by mass or less can reduce the haze of the laminated glass 10 and improve the appearance of the laminated glass 10.

[0054] Fig. 3 is a schematic diagram showing a state in which the laminated glass according to the first embodiment is mounted in an opening formed in the front of a vehicle. As shown in Fig. 3, a laminated glass 10 is mounted in an opening 110 formed in the front of an automobile 100. A housing 120 containing an information device is attached to the surface of the laminated glass 10 on the inside of the vehicle. Here, a case in which a LiDAR 201 is mounted on the vehicle as the information device is illustrated.

[0055] Fig. 4 is an enlarged view of a portion S in Fig. 3, and is a perspective view showing a portion where the housing 120 is attached to the laminated glass 10. The housing 120 houses a LiDAR 201 as an information device.

[0056] As shown in FIG. 4, the high infrared transmission region 17 of the laminated glass 10 and the LiDAR 201 are positioned so that the infrared light 300 passing through the high infrared transmission region 17 of the laminated glass 10 reaches the LiDAR 201. 905 ≧90%, T 1550 ≧80%, the LiDAR 201 can suitably transmit and receive infrared light with a wavelength of 905 nm or infrared light with a wavelength of 1550 nm via the high infrared transmittance region 17.

[0057] Incidentally, the housing 120 is usually attached on the outer side of the vehicle than the rearview mirror 150, but may be attached to another part. Alternatively, the LiDAR 201 may be attached to the automobile 100 side, not to the laminated glass 10 side.

[0058] In this way, in the laminated glass 10, the information transmission and reception area used by an information device that handles infrared light, such as LiDAR, is T 905 ≧90%, T 1550 ≧80%, and in most of the regions other than the high infrared transmittance region 17, an infrared shielding layer 135 is provided.

[0059] As a result, the laminated glass 10 can improve the infrared transmittance of the information transmitting and receiving region while improving the heat shielding properties of many regions other than the high infrared transmittance region 17. In other words, by installing the laminated glass 10 in a vehicle, information devices that handle infrared light, such as LiDAR, can be used with high sensitivity, and the temperature rise inside the vehicle can be suppressed, improving the comfort of the occupants.

[0060] Here, the glass plate 11, the glass plate 12, and the interlayer film 13 will be described in detail.

[0061] [Glass plate] The glass plate 11 and the glass plate 12 may be inorganic glass or organic glass. Examples of inorganic glass that can be used include, without particular limitation, soda-lime glass, aluminosilicate glass, borosilicate glass, alkali-free glass, and quartz glass. The glass plate 12 located on the outer side of the laminated glass 10 is preferably inorganic glass from the viewpoint of scratch resistance, and is preferably soda-lime glass from the viewpoint of formability. When the glass plate 11 and the glass plate 12 are soda-lime glass, clear glass, green glass containing a predetermined amount or more of iron components, and UV-cut green glass can be suitably used.

[0062] The inorganic glass may be either unstrengthened glass or tempered glass. Unstrengthened glass is obtained by forming molten glass into a plate shape and slowly cooling it. Tempered glass is obtained by forming a compressive stress layer on the surface of unstrengthened glass.

[0063] The tempered glass may be either physically tempered glass such as air-cooled tempered glass or chemically tempered glass. In the case of physically tempered glass, the glass surface can be tempered by generating a compressive stress layer on the glass surface due to the temperature difference between the glass surface and the inside of the glass by an operation other than slow cooling, such as rapidly cooling a glass sheet uniformly heated in bending from a temperature near the softening point.

[0064] In the case of chemically strengthened glass, for example, after bending, the glass surface can be strengthened by generating a compressive stress on the glass surface by an ion exchange method or the like. Glass that absorbs ultraviolet or infrared rays may be used, and further, although it is preferable that the glass is transparent, a glass plate that is colored to the extent that the transparency is not impaired may be used.

[0065] On the other hand, examples of materials for organic glass include transparent resins such as polycarbonate, acrylic resins such as polymethyl methacrylate, polyvinyl chloride, and polystyrene.

[0066] The glass plates 11 and 12 are made of T 905 and T 1550 It is particularly preferable to select glass having a good value of . Specifically, it is preferable that at least one of the glass plates 11 and 12 contains, by weight ratio, the sum of the total iron content calculated as Fe2O3: 0.002% to 1%, Cr2O3: 0.0001% to 1%, and Co: 0.0001% to 0.5%.

[0067] At least one of the glass plates 11 and 12 may contain, by weight, the sum of all iron contents converted into Fe2O3: 0.002% to 0.06%, and Cr2O3: 0.0001% to 0.06%. At least one of the glass plates 11 and 12 may contain, by weight, the sum of all iron contents converted into Fe2O3: 0.002% to 0.06%, Cr2O3: 0.0015% to 1%, and Co: 0.0001% to 0.5%. At least one of the glass plates 11 and 12 may contain, by weight, the sum of all iron contents converted into Fe2O3: 0.02% to 1%, Cr2O3: 0.002% to 0.5%, and Co: 0.0001% to 0.5%. At least one of glass plate 11 and glass plate 12 may contain, by weight, the sum of all iron contents converted into Fe2O3: 0.002% or more and 1% or less, Cr2O3: 0.001% or more and 0.5% or less, Co: 0.0001% or more and 0.5% or less, and Se: 0.0003% or more and 0.5% or less.

[0068] The shapes of the glass plates 11 and 12 are not particularly limited to a rectangular shape, and may be processed into various shapes and curvatures. Gravity forming, press forming, roller forming, etc. are used for bending the glass plates 11 and 12. The forming method of the glass plates 11 and 12 is also not particularly limited, but for example, in the case of inorganic glass, glass plates formed by a float method or the like are preferable.

[0069] The thickness of the glass plate 12 at its thinnest portion is preferably 1.1 mm or more and 3 mm or less. When the thickness of the glass plate 12 is 1.1 mm or more, the strength such as resistance to flying stones is sufficient, and when the thickness is 3 mm or less, the mass of the laminated glass 10 does not become too large, which is preferable in terms of fuel efficiency of the vehicle. The thickness of the glass plate 12 at its thinnest portion is more preferably 1.8 mm or more and 2.8 mm or less, further preferably 1.8 mm or more and 2.6 mm or less, further preferably 1.8 mm or more and 2.2 mm or less, and further preferably 1.8 mm or more and 2.0 mm or less.

[0070] The thickness of the glass plate 11 is preferably 0.3 mm or more and 2.3 mm or less. When the thickness of the glass plate 11 is 0.3 mm or more, the glass plate 11 is easy to handle, and when the thickness is 2.3 mm or less, the weight does not become too large.

[0071] Furthermore, the glass plates 11 and 12 may be flat or curved. However, if the glass plates 11 and 12 are curved and the thickness of the glass plate 11 is not appropriate, when two pieces of glass having particularly deep curves are formed as the glass plates 11 and 12, a mismatch occurs between the shapes of the two pieces, which significantly affects the glass quality such as residual stress after pressure bonding.

[0072] However, by setting the thickness of the glass plate 11 to 0.3 mm or more and 2.3 mm or less, the glass quality such as residual stress can be maintained. Setting the thickness of the glass plate 11 to 0.3 mm or more and 2.3 mm or less is particularly effective in maintaining the glass quality of deeply curved glass. The thickness of the glass plate 11 is more preferably 0.5 mm or more and 2.1 mm or less, and further preferably 0.7 mm or more and 1.9 mm or less. Within this range, the above-mentioned effects become more remarkable.

[0073] When the laminated glass 10 is used in, for example, a head-up display, the glass sheets 11 and / or 12 may not have a constant thickness, but may have a thickness that varies from place to place as necessary. For example, when the laminated glass 10 is a windshield, one or both of the glass sheets 11 and 12 may have a wedge-shaped cross section whose thickness increases from the lower edge to the upper edge of the windshield when the windshield is attached to a vehicle. In this case, if the thickness of the interlayer film 13 is constant, the total wedge angle of the glass sheets 11 and 12 varies, for example, in the range of more than 0 mrad to 1.0 mrad or less.

[0074] A coating having a water repellent property and an ultraviolet or infrared ray blocking property, or a coating having low reflection property and low radiation property may be provided on the outer side of the glass plate 11 and / or the glass plate 12. In addition, a coating having an ultraviolet or infrared ray blocking property, low radiation property, visible light absorption property, coloring property, etc. may be provided on the side of the glass plate 11 and / or the glass plate 12 that contacts the interlayer film 13.

[0075] When the glass sheets 11 and 12 are curved inorganic glass, the glass sheets 11 and 12 are bent after being formed by a float method and before being bonded with the interlayer film 13. The bending is performed by softening the glass by heating. The heating temperature of the glass during bending is about 550°C to 700°C.

[0076] [Interlayer] Thermoplastic resins are often used for the intermediate film 13, and examples of such thermoplastic resins include those conventionally used for this type of application, such as plasticized polyvinyl acetal resins, plasticized polyvinyl chloride resins, saturated polyester resins, plasticized saturated polyester resins, polyurethane resins, plasticized polyurethane resins, ethylene-vinyl acetate copolymer resins, ethylene-ethyl acrylate copolymer resins, cycloolefin polymer resins, ionomer resins, etc. Also suitable for use is a resin composition containing a modified hydrogenated block copolymer, as described in Japanese Patent No. 6065221.

[0077] Among these, plasticized polyvinyl acetal resins are preferably used because they have an excellent balance of various properties such as transparency, weather resistance, strength, adhesive strength, penetration resistance, impact energy absorption, moisture resistance, heat insulation, and sound insulation. These thermoplastic resins may be used alone or in combination of two or more. The term "plasticized" in the plasticized polyvinyl acetal resin means that it is plasticized by adding a plasticizer. The same applies to other plasticized resins.

[0078] However, when a light emitting element or the like is enclosed in the intermediate film 13, deterioration may occur due to a specific plasticizer depending on the type of the enclosed object, and in such a case, it is preferable to use a resin that does not substantially contain the plasticizer. In other words, it may be preferable that the intermediate film 13 does not contain a plasticizer. Examples of resins that do not contain a plasticizer include ethylene-vinyl acetate copolymer resins.

[0079] Examples of the polyvinyl acetal resin include polyvinyl formal resin obtained by reacting polyvinyl alcohol (hereinafter, sometimes referred to as "PVA" as necessary) with formaldehyde, polyvinyl acetal resin in the narrow sense obtained by reacting PVA with acetaldehyde, and polyvinyl butyral resin (hereinafter, sometimes referred to as "PVB" as necessary) obtained by reacting PVA with n-butylaldehyde, and the like. In particular, PVB is preferred because it has an excellent balance of various properties such as transparency, weather resistance, strength, adhesive strength, penetration resistance, impact energy absorption, moisture resistance, heat insulation, and sound insulation. These polyvinyl acetal resins may be used alone or in combination of two or more kinds.

[0080] However, the material forming the intermediate film 13 is not limited to a thermoplastic resin. The intermediate film 13 may also contain functional particles such as an ultraviolet absorbing agent, a luminescent agent, etc. The intermediate film 13 may also have a colored portion called a shade band.

[0081] The thickness of the interlayer film 13 is preferably 0.5 mm or more at its thinnest part. When the interlayer film 13 is made up of multiple layers, the thickness of the interlayer film 13 is the total thickness of all layers. If the thickness of the interlayer film 13 at its thinnest part is 0.5 mm or more, the impact resistance required for laminated glass is sufficient. Furthermore, the thickness of the interlayer film 13 is preferably 3 mm or less at its thickest part. If the maximum thickness of the interlayer film 13 is 3 mm or less, the mass of the laminated glass does not become too large. The maximum thickness of the interlayer film 13 is more preferably 2.8 mm or less, and even more preferably 2.6 mm or less.

[0082] When the laminated glass 10 is used in, for example, a head-up display, the interlayer film 13 does not have to have a constant thickness, and the thickness may vary from place to place as necessary. For example, when the laminated glass 10 is a windshield, the interlayer film 13 may have a wedge-shaped cross section whose thickness increases from the lower edge to the upper edge of the windshield when the windshield is attached to a vehicle. In this case, if the thicknesses of the glass sheets 11 and 12 are constant, the wedge angle of the interlayer film 13 varies, for example, in the range of more than 0 mrad to 1.0 mrad or less.

[0083] The interlayer film 13 may have three or more layers. For example, the sound insulation of the laminated glass 10 can be improved by forming the interlayer film from three or more layers and making the shear modulus of any layer other than the layers on both sides smaller than the shear modulus of the layers on both sides by adjusting the plasticizer or the like. In this case, the shear modulus of the layers on both sides may be the same or different.

[0084] Furthermore, when the interlayer film 13 is made up of multiple layers, it is preferable that each layer in the interlayer film 13 is made of the same material, but each layer may be made of a different material. However, from the viewpoint of adhesion to the glass plates 11 and 12, or functional materials to be incorporated into the laminated glass 10, it is preferable that 50% or more of the thickness of the interlayer film 13 be made of the above-mentioned materials.

[0085] To produce the interlayer film 13, for example, the above-mentioned resin material that will become the interlayer film is appropriately selected and extruded in a heated and molten state using an extruder. The extrusion conditions, such as the extrusion speed of the extruder, are set so as to be uniform. Thereafter, the extruded resin film is stretched as necessary to give curvature to the upper and lower sides in accordance with the design of the laminated glass, thereby completing the interlayer film 13.

[0086] [Method of forming an infrared shielding layer on a part of an interlayer film] One embodiment of a method for forming an infrared shielding layer on a part of an interlayer film will be described. First, infrared shielding fine particles having a particle size of 0.2 μm or less are dispersed in a plasticizer, and the plasticizer is dispersed and added to a resin solution for the interlayer film, and mixed and kneaded to obtain a resin raw material containing infrared shielding fine particles. Next, this resin raw material and a resin raw material for the interlayer film that does not substantially contain infrared shielding fine particles are molded into a film shape by extrusion molding or the like to obtain the interlayer film 13 shown in FIG. 1(b). At this time, each resin raw material may be extruded simultaneously, or films extruded separately may be laminated together.

[0087] In order to simplify the manufacturing process, it is preferable to extrude each resin material at the same time. The infrared non-shielding layer 136 in the intermediate film 13 may be made of one organic resin film, or may be made by laminating a plurality of films made of the same material. When dispersing and adding the plasticizer, various additives can be added to the resin solution of the intermediate film. Examples of additives include various pigments, organic ultraviolet absorbers, and organic infrared absorbers. Known solvents can be used as the plasticizer and the resin solution of the intermediate film.

[0088] In addition, in view of the fact that it is preferable to simultaneously extrude the resin materials as described above and that it is easy to manage the materials during production, it is preferable that the infrared non-shielding layer 136 does not contain any infrared shielding fine particles.

[0089] 2(a) and 2(b), in order to make the proportion of the high infrared transmission region 17 in the first region 151 smaller than 100%, for example, the entire intermediate film 13 may be stretched. As a result, the infrared shielding layer 135 can be stretched upward from the straight line P shown in FIG. 2(a) and FIG. 2(b) as it approaches the left and right ends relative to the center. Note that in FIG. 2(a) and FIG. 2(b), the high infrared transmission region 17 is in contact with the first shielding layer 14a. By positioning the high infrared transmission region 17 in this way, even when the entire intermediate film 13 is stretched, it is easy to adjust the thickness of the intermediate film 13 to 0.5 mm or more at the thinnest part. In addition, in order to make it easier to adjust the thickness of the intermediate film 13 to 0.5 mm or more at the thinnest part, it is preferable that the high infrared transmission region 17 is in contact with a side extending in the vertical direction among the outer edges of the first region 151 as shown in FIG. 2(b).

[0090] [Laminated Glass] The total thickness of the laminated glass 10 is preferably 2.8 mm or more and 10 mm or less. If the total thickness of the laminated glass 10 is 2.8 mm or more, sufficient rigidity can be ensured. If the total thickness of the laminated glass 10 is 10 mm or less, sufficient transmittance can be obtained and haze can be reduced.

[0091] The plate misalignment between the glass plates 11 and 12 is preferably 1.5 mm or less, and more preferably 1 mm or less, on at least one side of the laminated glass 10. Here, the plate misalignment between the glass plates 11 and 12 refers to the amount of misalignment between the end of the glass plate 11 and the end of the glass plate 12 in a plan view.

[0092] It is preferable that the misalignment between the glass plates 11 and 12 be 1.5 mm or less along at least one side of the laminated glass 10 in order to avoid impairing the appearance. It is even more preferable that the misalignment between the glass plates 11 and 12 be 1.0 mm or less along at least one side of the laminated glass 10 in order to avoid impairing the appearance.

[0093] To manufacture the laminated glass 10, an interlayer film 13 is sandwiched between glass plates 11 and 12 to form a laminate. Then, for example, this laminate is placed in a rubber bag, a rubber chamber, a resin bag, or the like, and bonded at a temperature of about 70° C. to 110° C. in a vacuum with a gauge pressure of −65 kPa to −100 kPa.

[0094] Furthermore, by carrying out a pressure bonding treatment under conditions of heating and pressing at 100°C to 150°C and an absolute pressure of 0.6 MPa to 1.3 MPa, for example, it is possible to obtain a laminated glass 10 with even greater durability. However, in some cases, in order to simplify the process and in consideration of the properties of the material to be filled in the laminated glass 10, this heating and pressing step may not be used.

[0095] That is, a method called "cold bending" may be used in which either or both of the glass plates 11 and 12 are joined in a state of elastic deformation to each other. Cold bending can be achieved by using a laminate consisting of the glass plates 11, 12, and the interlayer film 13 fixed by a temporary fixing means such as tape, a conventionally known preliminary pressure bonding device such as a nip roller, a rubber bag, or a rubber chamber, and an autoclave.

[0096] In addition to the interlayer 13, a film or device having functions such as heating, light emission, power generation, light control, touch panel, visible light reflection, scattering, decoration, absorption, etc. may be provided between the glass plates 11 and 12, so long as the effects of the present application are not impaired. In addition, the surface of the laminated glass 10 may have a film having functions such as anti-fogging, water repellency, heat shielding, low reflection, etc. In addition, the surface of the glass plate 11 facing the vehicle exterior and the surface of the glass plate 12 facing the vehicle interior may have a film having functions such as heat shielding, heat generation, etc.

[0097] First Modification of the First Embodiment In Modification 1 of the first embodiment, an example is shown in which the arrangement of the infrared shielding layer and the infrared non-shielding layer in the intermediate film is different from that of the first embodiment. Note that in Modification 1 of the first embodiment, the description of the same components as those in the already-described embodiments may be omitted.

[0098] Fig. 5 is a cross-sectional view illustrating a laminated glass according to Modification 1 of the first embodiment. Referring to Fig. 5, the laminated glass 10A differs from the laminated glass 10 (see Fig. 1) in that the interlayer film 13 is replaced with an interlayer film 13A.

[0099] The intermediate film 13A includes an infrared shielding layer 135A and an infrared non-shielding layer 136A. The infrared shielding layer 135A is a layer in which infrared shielding particles are dispersed in an organic resin film, and the infrared non-shielding layer 136A is a layer that does not contain any or almost no infrared shielding particles. The infrared shielding particles are as described in the first embodiment.

[0100] Therefore, in the see-through region 15 of the laminated glass 10A, the infrared transmittance of the region where the infrared shielding layer 135A is not arranged in a plan view is higher than the infrared transmittance of the region where the infrared shielding layer 135A is arranged. On the other hand, in the see-through region 15 of the laminated glass 10A, the heat shielding property of the region where the infrared shielding layer 135A is arranged in a plan view is higher than the heat shielding property of the region where the infrared shielding layer 135A is not arranged.

[0101] The infrared shielding layer 135A is provided in a rectangular shape in cross section from the lower end side to the upper end side of the laminated glass 10A, and is sandwiched from both sides by the glass plate 11 and the glass plate 12. In the see-through region 15, a region where the infrared shielding layer 135A is not arranged in a plan view forms a high infrared transmittance region 17.

[0102] The proportion of the high infrared transmittance region 17 in the first region 151 may be 100% as in FIG. 1, or may be less than 100% as shown in FIGS. 2(a) and 2(b).

[0103] In the infrared shielding layer 135A, it is preferable to lower the blending ratio of infrared shielding fine particles on the boundary side with the infrared non-shielding layer 136A compared to other parts of the infrared shielding layer 135A in order to suppress color change at the boundary.

[0104] In this manner, in the second region 152, a portion of the intermediate film may be made into an infrared shielding layer, as in infrared shielding layer 135 (see FIG. 1(b)), or the entire intermediate film may be made into an infrared shielding layer, as in infrared shielding layer 135A.

[0105] Second Embodiment In the second embodiment, an example in which the intermediate film is made up of a plurality of layers will be described. Note that in the second embodiment, the description of the same components as those in the embodiments already described may be omitted.

[0106] Fig. 6 is a cross-sectional view illustrating a laminated glass according to embodiment 2. Referring to Fig. 6, the laminated glass 10B differs from the laminated glass 10 (Fig. 1) in that the interlayer film 13 is replaced with an interlayer film 13B.

[0107] The interlayer film 13B has a first layer 131, a second layer 132, and a third layer 133. The first layer 131 is in contact with the glass plate 11, and the third layer 133 is in contact with the glass plate 12. The second layer 132 is sandwiched between the first layer 131 and the third layer 133 on both sides.

[0108] The second layer 132 may have a lower (softer) Shore hardness than the first layer 131 and the third layer 133 by, for example, increasing the plasticizer content therein compared to the first layer 131 and the third layer 133. In such a configuration of the interlayer film 13B, the second layer 132, which is softer than the other layers, is disposed in the center, so that sound waves with frequencies within the audible range are more likely to be attenuated. Therefore, the laminated glass 10B having the interlayer film 13B can exhibit good sound insulation performance. In this case, the Shore hardness of the first layer 131 and the third layer 133 may be the same or different.

[0109] The first layer 131 and the second layer 132 of the intermediate film 13B are layers that contain no or almost no infrared shielding particles. The third layer 133 of the intermediate film 13B includes an infrared shielding layer 135B and an infrared non-shielding layer 136B. The infrared shielding layer 135B is a layer in which infrared shielding particles are dispersed in an organic resin film, and the infrared non-shielding layer 136B is a layer that contains no or almost no infrared shielding particles. The infrared shielding particles are as described in the first embodiment.

[0110] Therefore, in the see-through region 15 of the laminated glass 10B, the infrared transmittance of the region where the infrared shielding layer 135B is not arranged in a plan view is higher than the infrared transmittance of the region where the infrared shielding layer 135B is arranged. On the other hand, in the see-through region 15 of the laminated glass 10B, the heat shielding property of the region where the infrared shielding layer 135B is arranged in a plan view is higher than the heat shielding property of the region where the infrared shielding layer 135B is not arranged.

[0111] When the laminated glass 10B is viewed in a state where it is attached to a vehicle, the infrared shielding layer 135B is provided in a cross-sectional wedge shape that becomes thinner from the lower end side to the upper end of the laminated glass 10B, and is sandwiched from both sides by the infrared non-shielding layers 136B. The wedge angle of the infrared shielding layer 135B is approximately constant at each position in the longitudinal direction of the infrared shielding layer 135B. In the see-through region 15, the region where the infrared shielding layer 135B is not arranged in a plan view forms the high infrared transmittance region 17.

[0112] The proportion of the high infrared transmittance region 17 in the first region 151 may be 100% as in FIG. 1, or may be less than 100% as shown in FIGS. 2(a) and 2(b).

[0113] In this way, the intermediate film may be composed of a plurality of layers, and the infrared shielding layer may be provided on any one of the layers.

[0114] <Modification 1 of the second embodiment> In the first modification of the second embodiment, an example is shown in which the arrangement of the infrared shielding layer and the infrared non-shielding layer in the intermediate film is different from that of the second embodiment. Note that in the first modification of the second embodiment, the description of the same components as those in the already described embodiment may be omitted.

[0115] Fig. 7 is a cross-sectional view illustrating a laminated glass according to Modification 1 of Embodiment 2. Referring to Fig. 7, the laminated glass 10C differs from the laminated glass 10B (see Fig. 6) in that the interlayer film 13B is replaced with an interlayer film 13C.

[0116] The second layer 132 of the intermediate film 13C is a layer that does not contain any or almost no infrared shielding particles. The first layer 131 of the intermediate film 13C includes an infrared shielding layer 135C and an infrared non-shielding layer 136C. The infrared shielding layer 135C is a layer in which infrared shielding particles are dispersed in an organic resin film, and the infrared non-shielding layer 136C is a layer that does not contain any or almost no infrared shielding particles. The infrared shielding particles are as described in the first embodiment.

[0117] Therefore, in the see-through region 15 of the laminated glass 10C, the infrared transmittance of a region where neither the infrared shielding layer 135B nor the infrared shielding layer 135C is arranged in a plan view is higher than the infrared transmittance of a region where at least one of the infrared shielding layer 135B and the infrared shielding layer 135C is arranged. On the other hand, in the see-through region 15 of the laminated glass 10C, the heat shielding property of the region where at least one of the infrared shielding layer 135B and the infrared shielding layer 135C is arranged in a plan view is higher than the heat shielding property of a region where neither the infrared shielding layer 135B nor the infrared shielding layer 135C is arranged.

[0118] In the first layer 131 of the interlayer film 13C, the infrared shielding layer 135C is provided in a cross-sectional wedge shape that becomes thinner from the lower end side to the upper end of the laminated glass 10C when viewed in a state in which the laminated glass 10C is attached to a vehicle, and is sandwiched from both sides by the infrared non-shielding layers 136C. The wedge angle of the infrared shielding layer 135C is approximately constant at each position in the longitudinal direction of the infrared shielding layer 135C. In the see-through region 15, a region where neither the infrared shielding layer 135B nor the infrared shielding layer 135C is disposed in a plan view forms a high infrared transmittance region 17.

[0119] The proportion of the high infrared transmittance region 17 in the first region 151 may be 100% as in FIG. 1, or may be less than 100% as shown in FIGS. 2(a) and 2(b).

[0120] In this way, the intermediate film may be made up of a plurality of layers, and the infrared shielding layer may be provided on any two or more layers, which can improve the heat shielding property of the second region 152 compared to the case of FIG.

[0121] <Modification 2 of the second embodiment> In Modification 2 of the second embodiment, another example is shown in which the arrangement of the infrared shielding layer and the infrared non-shielding layer in the intermediate film is different from that of the second embodiment. Note that in Modification 2 of the second embodiment, the description of the same components as those in the already described embodiment may be omitted.

[0122] Fig. 8 is a cross-sectional view illustrating a laminated glass according to Modification 2 of the second embodiment. Referring to Fig. 8, the laminated glass 10D differs from the laminated glass 10B (see Fig. 6) in that the interlayer film 13B is replaced with an interlayer film 13D.

[0123] The first layer 131 and the second layer 132 of the intermediate film 13D are layers that contain no or almost no infrared shielding particles. The third layer 133 of the intermediate film 13D includes an infrared shielding layer 135D and an infrared non-shielding layer 136D. The infrared shielding layer 135D is a layer in which infrared shielding particles are dispersed in an organic resin film, and the infrared non-shielding layer 136D is a layer that contains no or almost no infrared shielding particles. The infrared shielding particles are as described in the first embodiment.

[0124] Therefore, in the see-through region 15 of the laminated glass 10D, the infrared transmittance of the region where the infrared shielding layer 135D is not arranged in a plan view is higher than the infrared transmittance of the region where the infrared shielding layer 135D is arranged. On the other hand, in the see-through region 15 of the laminated glass 10D, the heat shielding property of the region where the infrared shielding layer 135D is arranged in a plan view is higher than the heat shielding property of the region where the infrared shielding layer 135D is not arranged.

[0125] The infrared shielding layer 135D has a wedge-shaped cross section that becomes thinner from the lower end side of the laminated glass 10D toward the upper end when viewed in a state in which the laminated glass 10D is attached to a vehicle, and is sandwiched from both sides by the infrared non-shielding layers 136D. In the see-through region 15, a region where the infrared shielding layer 135D is not arranged in a plan view forms a high infrared transmittance region 17.

[0126] In the laminated glass 10D, the wedge angle of the infrared shielding layer 135D is smaller in most of the infrared shielding layer 135D than that of the infrared shielding layer 135B of the laminated glass 10B. Therefore, the proportion of the infrared shielding layer 135D in the third layer 133 can be made larger than the proportion of the infrared shielding layer 135B in the third layer 133 of the laminated glass 10B. As a result, the heat shielding property of the second region 152 can be improved. Moreover, by increasing the wedge angle of the tip of the infrared shielding layer 135D, the wedge angle of the infrared shielding layer 135D can be made smaller, and the heat shielding property of the second region 152 can be improved.

[0127] <Modification 3 of the second embodiment> Modification 3 of the second embodiment shows another example in which the arrangement of the infrared shielding layer and the infrared non-shielding layer in the intermediate film is different from that of the second embodiment. Note that in Modification 3 of the second embodiment, the description of the same components as those in the already described embodiments may be omitted.

[0128] Fig. 9 is a cross-sectional view illustrating a laminated glass according to Modification 3 of Embodiment 2. Referring to Fig. 9, the laminated glass 10E differs from the laminated glass 10B (see Fig. 6) in that the interlayer film 13B is replaced with an interlayer film 13E.

[0129] The second layer 132 of the intermediate film 13E is a layer that does not contain any or almost no infrared shielding particles. The first layer 131 of the intermediate film 13E includes an infrared shielding layer 135E and an infrared non-shielding layer 136E. The third layer 133 of the intermediate film 13E includes an infrared shielding layer 135F and an infrared non-shielding layer 136F. The infrared shielding layers 135E and 135F are layers in which infrared shielding particles are dispersed in an organic resin film, and the infrared non-shielding layers 136E and 136F are layers that do not contain any or almost no infrared shielding particles. The infrared shielding particles are as described in the first embodiment.

[0130] Therefore, in the see-through region 15 of the laminated glass 10E, the infrared transmittance of a region where neither the infrared shielding layer 135E nor the infrared shielding layer 135F is arranged in a plan view is higher than the infrared transmittance of a region where at least one of the infrared shielding layer 135E and the infrared shielding layer 135F is arranged. On the other hand, in the see-through region 15 of the laminated glass 10E, the heat shielding property of the region where at least one of the infrared shielding layer 135E and the infrared shielding layer 135F is arranged in a plan view is higher than the heat shielding property of a region where neither the infrared shielding layer 135E nor the infrared shielding layer 135F is arranged.

[0131] The infrared shielding layer 135E is provided from the lower end side to the upper end side of the laminated glass 10E in a rectangular shape in cross section, and is sandwiched from both sides by the glass plates 12 and the second layer 132. The infrared shielding layer 135F is provided from the lower end side to the upper end side of the laminated glass 10E in a rectangular shape in cross section, and is sandwiched from both sides by the glass plates 11 and the second layer 132. In the see-through region 15, a region where neither the infrared shielding layer 135E nor the infrared shielding layer 135F is disposed in a planar view forms a high infrared transmittance region 17.

[0132] In the infrared shielding layer 135E, the blending ratio of the infrared shielding fine particles is preferably lower on the boundary side with the infrared non-shielding layer 136E than in other parts of the infrared shielding layer 135E in order to suppress color change at the boundary. Also, in the infrared shielding layer 135F, the blending ratio of the infrared shielding fine particles is preferably lower on the boundary side with the infrared non-shielding layer 136F than in other parts of the infrared shielding layer 135F in order to suppress color change at the boundary.

[0133] In this way, by forming the intermediate film from a plurality of layers and providing an infrared shielding layer in any two or more layers, the heat shielding property of the second region 152 can be improved compared to a case where an infrared shielding layer is provided in only one layer. In this case, in the second region 152, the entire regions of the first layer 131 and the third layer 133 may be made into an infrared shielding layer.

[0134] Example Examples will be described below, but the present invention is not limited to these examples in any way.

[0135] (Example 1) A glass plate G1, which will be the inner plate (glass plate on the inside of the vehicle) when laminated, and a glass plate G2 (sum of total iron content converted to Fe2O3: 0.01%, Cr2O3: 0.0021%, Co: 0.0001%) with a thickness of 2.1 mm, which will be the outer plate (glass plate on the outside of the vehicle) were prepared (manufactured by AGC). The dimensions of the glass plates G1 and G2 were both 300 mm long x 300 mm wide x 2 mm thick. A black colored ceramic layer was formed as a shielding layer on the outer periphery of the glass plate G1 on the inside of the vehicle. The colored ceramic layer was formed by screen printing a black ceramic paste on the surface of the glass plate G1, drying it at 120°C for 15 minutes, and then firing it at 600°C for 5 minutes. At this time, an opening was formed in the colored ceramic layer to become an information transmission / reception area.

[0136] Next, a three-layer interlayer was prepared by integrating a PVB film having a thickness of 0.33 mm as a first layer, a PVB film having a thickness of 0.1 mm as a second layer, and a PVB film having a thickness of 0.33 mm as a third layer. The three-layer interlayer was then sandwiched between glass plate G1 and glass plate G2 to prepare a laminate, which was then placed in a rubber bag and bonded at a temperature of about 70°C to 110°C in a vacuum with a gauge pressure of -65 kPa to -100 kPa to prepare laminated glass 10X shown in Fig. 10.

[0137] Fig. 10 is a cross-sectional view illustrating the laminated glass of Example 1. The laminated glass 10X shown in Fig. 10 is obtained by replacing the interlayer film 13B in the laminated glass 10B shown in Fig. 6 with an interlayer film 13X. The infrared-shielding layer 135 is not formed on the third layer 133 of the interlayer film 13X, and the entire third layer 133 is formed only from a layer having the same specifications as the infrared non-shielding layer 136. In other words, the entire interlayer film 13X is an infrared non-shielding layer.

[0138] In the laminated glass 10X, the infrared transmittance is approximately constant throughout the entire see-through region 18, but for convenience, the same regions as those of the laminated glass 10Y described below are referred to as a first region 181, a second region 182, and a high infrared transmittance region 19.

[0139] (Example 2) Except for changing the specifications of the interlayer film, laminated glass 10Y shown in Fig. 11 was produced in the same manner as in Example 1. Fig. 11 is a cross-sectional view illustrating the laminated glass of Example 2. The laminated glass 10Y shown in Fig. 11 is obtained by replacing the interlayer film 13B in the laminated glass 10B shown in Fig. 6 with an interlayer film 13Y.

[0140] The intermediate film 13Y has a first layer 131Y, a second layer 132, and a third layer 133Y. The first layer 131Y is entirely formed only from layers having the same specifications as the infrared shielding layer 135. The second layer 132 is entirely formed only from layers having the same specifications as the infrared non-shielding layer 136. The third layer 133Y is mostly formed from an infrared shielding layer 135Y having the same specifications as the infrared shielding layer 135. However, an infrared non-shielding layer 136Y having the same specifications as the infrared non-shielding layer 136 is provided in a wedge-shaped cross section from the upper end side to the lower end side of the laminated glass 10Y. The infrared non-shielding layer 136Y is sandwiched from both sides by the infrared shielding layers 135Y.

[0141] In the see-through region 18 of the laminated glass 10Y, the region where the infrared non-shielding layer 136Y exists has a higher infrared transmittance in a plan view than the region where the infrared non-shielding layer 136Y does not exist. Therefore, in the see-through region 18 of the laminated glass 10Y, the region where the infrared non-shielding layer 136Y exists is defined as the high infrared transmission region 19. In addition, when the laminated glass 10Y is attached to a vehicle and the vehicle is placed on a horizontal plane, in a plan view, the region above the laminated glass 10Y is defined as the first region 181, and the region below is defined as the second region 182, relative to a curve obtained by projecting a straight line horizontal to the vehicle through the lower end point of the high infrared transmission region 17 onto the laminated glass 10Y in the normal direction of the laminated glass 10Y at the lower end point. In the laminated glass 10Y, the proportion of the high infrared transmission region 19 in the first region 181 is 100%.

[0142] The intermediate film 13Y was manufactured as follows. First, a resin material for the infrared shielding layer, which would become the first layer 131Y and the infrared shielding layer 135Y, was prepared. Specifically, infrared shielding fine particles having a particle size of 0.2 μm or less were dispersed in a plasticizer, and the plasticizer was dispersed and added to a resin solution for the intermediate film, and the mixture was kneaded to obtain a resin material for the infrared shielding layer, which contains infrared shielding fine particles and is mainly composed of PVB.

[0143] Next, a resin raw material for the infrared non-shielding layer, which was to become the second layer 132 and the infrared non-shielding layer 136Y and contained substantially no infrared shielding fine particles and was mainly composed of PVB, was obtained.

[0144] Next, the resin raw material for the infrared shielding layer and the resin raw material for the infrared non-shielding layer were molded into a film by extrusion molding, to obtain an interlayer film 13Y shown in FIG.

[0145] (Example 3) Except for changing the specifications of the interlayer film, the laminated glass 10B shown in Fig. 6 was produced in the same manner as in Example 1. In the laminated glass 10B, the proportion of the high infrared transmittance region 17 in the first region 151 was set to 100%. Moreover, the area of ​​the high infrared transmittance region 17 in a plan view was set to be the same as the area of ​​the high infrared transmittance region 19 of the laminated glass 10Y.

[0146] The intermediate film 13B was obtained by using the same resin raw material for the infrared shielding layer and the resin raw material for the infrared non-shielding layer as in Example 2, and molding the resin raw material for the infrared shielding layer and the resin raw material for the infrared non-shielding layer into a film by extrusion molding.

[0147] (Example 4) Except for changing the specifications of the interlayer film, the laminated glass 10C shown in Fig. 7 was produced in the same manner as in Example 1. In the laminated glass 10C, the proportion of the high infrared transmittance region 17 in the first region 151 was set to 100%. Furthermore, the area of ​​the high infrared transmittance region 17 in a plan view was set to be the same as the area of ​​the high infrared transmittance region 19 of the laminated glass 10Y.

[0148] The intermediate film 13C was obtained by using the same resin raw material for the infrared shielding layer and the resin raw material for the infrared non-shielding layer as in Example 2, and molding the resin raw material for the infrared shielding layer and the resin raw material for the infrared non-shielding layer into a film by extrusion molding.

[0149] (Example 5) Except for changing the specifications of the interlayer film, the laminated glass 10D shown in Fig. 8 was produced in the same manner as in Example 1. In the laminated glass 10D, the proportion of the high infrared transmittance region 17 in the first region 151 was set to 100%. Moreover, the area of ​​the high infrared transmittance region 17 in a plan view was set to be the same as the area of ​​the high infrared transmittance region 19 of the laminated glass 10Y.

[0150] Interlayer film 13D was obtained by using the same resin raw material for the infrared shielding layer and the resin raw material for the infrared non-shielding layer as in Example 2, and molding the resin raw material for the infrared shielding layer and the resin raw material for the infrared non-shielding layer into a film by extrusion molding.

[0151] (Example 6) Except for changing the specifications of the interlayer film, the laminated glass 10E shown in Fig. 9 was produced in the same manner as in Example 1. In the laminated glass 10E, the proportion of the high infrared transmittance region 17 in the first region 151 was set to 100%. Moreover, the area of ​​the high infrared transmittance region 17 in a plan view was set to be the same as the area of ​​the high infrared transmittance region 19 of the laminated glass 10Y.

[0152] The intermediate film 13E was obtained by using the same resin raw material for the infrared shielding layer and the resin raw material for the infrared non-shielding layer as in Example 2, and molding the resin raw material for the infrared shielding layer and the resin raw material for the infrared non-shielding layer into a film by extrusion molding.

[0153] (Example 7) A laminated glass of the type shown in Fig. 2(b) was produced in the same manner as in Example 3, except that the proportion of the high infrared transmittance region 17 in the first region 151 was 85%. The cross-sectional shape of the laminated glass was the same as in Fig. 6.

[0154] (Rating 1) For the laminated glass of Examples 1 to 6, the infrared transmittance (T 905, T 1550 ), the heat insulation of the second region, and the color uniformity of the entire laminated glass were evaluated.

[0155] First, the infrared transmittance was evaluated according to JIS R3106 (1998). 905 and T 1550 Considering the range in which information devices that use infrared light, such as LiDAR, operate satisfactorily, the T 905 If the T value was 90% or more, it was judged as ◯ (pass), and if it was less than 90%, it was judged as × (fail). 1550 If it was 80% or more, it was marked as ◯ (pass), and if it was less than 80%, it was marked as × (fail).

[0156] As shown in FIG. 12, the laminated glasses of Examples 1 and 3 to 6, in which the high infrared transmittance region does not include an infrared shielding layer, have a T 905 ≧90% and T 1550 In contrast, the laminated glass of Example 2, which includes an infrared shielding layer in a part of the high infrared transmittance region, satisfies T 905 ≧90% and T 1550 In other words, when an infrared shielding layer is included in a part of the high infrared transmittance region, good infrared transmittance cannot be obtained, and therefore it was found that it is preferable that the high infrared transmittance region does not include an infrared shielding layer.

[0157] Next, to evaluate the heat shielding properties of the second region, the total solar transmittance Tts (%) was measured in accordance with ISO 13837. Taking into consideration the temperature rise inside the vehicle cabin and the heat-shivering sensation of the occupants, if the minimum Tts value was 70% or less, it was rated as ◎ (pass), if it was between 70% and 75% or less, it was rated as ◯ (pass), and if it was greater than 75%, it was rated × (fail).

[0158] As shown in Fig. 12, the laminated glasses of Examples 2 to 6, which include an infrared shielding layer in at least a part of the second region, satisfy Tts≦75%. In particular, the laminated glasses of Examples 2, 4, and 6, which include an infrared shielding layer in two of the three-layer interlayer films, satisfy Tts≦70% because the proportion of the infrared shielding layer in the interlayer film located in the second region is high. In contrast, the laminated glass of Example 1, which does not include an infrared shielding layer in the second region, does not satisfy Tts≦75%. In other words, it was found that when the second region does not include an infrared shielding layer, good heat shielding properties cannot be obtained, so it is preferable that the second region includes an infrared shielding layer, and the higher the proportion of the infrared shielding layer in the interlayer film located in the second region, the better the heat shielding properties can be obtained.

[0159] Next, to evaluate the color uniformity of the entire laminated glass, the transmittance change ΔE (ΔE / 10mm) over a 10mm width was measured in accordance with JIS Z8722: 2009. Taking into consideration whether the passengers would feel uncomfortable, ΔE / 10mm was rated as ◎ (pass) if it was 2 or less, ◯ (pass) if it was greater than 2 and less than 4, and × (fail) if it was greater than 4.

[0160] As shown in Fig. 12, all of the laminated glasses of Examples 1 to 6 satisfied ΔE / 10mm≦4 and were pass. However, in the laminated glass of Example 6 in which the entire second region is an infrared-shielding layer, the color of the infrared-shielding layer suddenly switches to the color of the infrared non-shielding layer at the boundary between the second region and the first region, and so the value is larger than in Examples 1 to 5. Therefore, when importance is attached to the color tone uniformity of the entire laminated glass, it can be said that it is preferable not to make the entire second region an infrared-shielding layer.

[0161] The infrared transmittance (T 905 , T 1550 When the evaluation results of the heat shielding property of the second region and the color uniformity of the entire laminated glass are judged comprehensively, it can be said that the laminated glasses of Examples 3 to 6 have good overall performance.

[0162] In other words, the area used by information devices that handle infrared light, such as LiDAR, is T 905 ≧90%, T 1550It is preferable to have a high infrared transmittance region that satisfies at least one of the above criteria and to provide an infrared shielding layer in the region other than the region used by the information device to ensure the heat shielding properties of the second region and the uniformity of color tone of the entire laminated glass. In this case, a glass with even one evaluation item marked "x" was deemed to have failed.

[0163] (Rating 2) The heat shielding properties were compared between the laminated glass of Example 3 and Example 7. The laminated glass of Example 7, in which the proportion of high infrared transmittance regions in the first region was 85%, had better heat shielding properties than the laminated glass of Example 3, in which the proportion of high infrared transmittance regions in the first region was 100%.

[0164] In this way, the lower the proportion of the high infrared transmittance region in the first region, the better the heat shielding properties, so the lower the proportion of the high infrared transmittance region in the first region is, the more preferable. However, considering the minimum area required by an information device that handles infrared light, such as LiDAR, the proportion of the high infrared transmittance region in the first region needs to be 5% or more.

[0165] Although preferred embodiments have been described above in detail, the present invention is not limited to the above-described embodiments, and various modifications and substitutions can be made to the above-described embodiments without departing from the scope of the claims.

[0166] For example, although an automobile is used as an example of a vehicle in Fig. 3 and other figures, the vehicle according to the present invention is not limited to an automobile, and may be any moving body to which laminated glass can be attached. Examples of such moving bodies include trains, ships, and airplanes.

[0167] Furthermore, the entire periphery of the information transmission / reception area does not necessarily have to be surrounded by a shielding layer; it may be that only a portion of the periphery of the information transmission / reception area is in contact with the shielding layer, or that the information transmission / reception area is not in contact with the shielding layer at all. [Explanation of symbols]

[0168] 10, 10A, 10B, 10C, 10D, 10E Laminated Glass 11, 12 Glass plate 13, 13A, 13B, 13C, 13D, 13E Intermediate film 14 Shielding layer 14a 1st shielding layer 14b 2nd shielding layer 15 Transparent area 16 Opening 17 High infrared transmission area 17a Lower end of high infrared transmittance region 100 Automobiles 120 Housing 131 1st layer 132 2nd layer 133 3rd layer 135, 135A, 135B, 135C, 135D, 135E, 135F Infrared shielding layer 136, 136A, 136B, 136C, 136D, 136E, 136F Infrared non-shielding layer 150 Rearview Mirror 151 First area 152 Second area 201 LiDAR 300 Infrared

Claims

1. A laminated glass for a vehicle having a pair of glass sheets and an interlayer film located between the pair of glass sheets, A see-through area is provided, In the perspective region, T 905 ≧90%, T 1550 A region that satisfies at least one of the above conditions is defined as a high infrared transmittance region. When the laminated glass is attached to a vehicle and the vehicle is placed on a horizontal plane, a straight line that passes through the lower end point of the high infrared transmittance region and is horizontal to the vehicle in a plan view is defined as a straight line P. The see-through region includes a first region that is above a curve obtained by projecting the straight line P onto the laminated glass in a normal direction of the laminated glass at the lower end point, and a second region that is below the curve, The proportion of the high infrared transmittance region in the first region is 5% or more, the intermediate film located in the second region has an infrared shielding layer in which infrared shielding fine particles are dispersed, The laminated glass has an infrared shielding layer sandwiched between infrared non-shielding layers on both sides.

2. The laminated glass according to claim 1 , wherein the area of ​​the second region is 50% or more of the area of ​​the see-through region.

3. When the laminated glass is viewed in a state where it is installed in a vehicle, 3. The laminated glass according to claim 1, wherein the first region has a width in the vertical direction of 400 mm or less.

4. The laminated glass according to claim 1 , wherein a ratio of the high infrared transmittance region in the first region is 95% or less.

5. The laminated glass according to claim 1 , wherein the second region has a minimum total solar transmittance of 75% or less.

6. 6. The laminated glass according to claim 1, wherein a change in transmitted color tone in a width of 10 mm is ΔE≦4.

7. At least one of the pair of glass plates is made of Fe, 2 O 3 Sum of all iron content converted into Cr: 0.002% or more and 1% or less, Cr 2 O 3 The laminated glass according to claim 1 , further comprising: Mo: 0.0001% or more and 1% or less; and Co: 0.0001% or more and 0.5% or less.

8. A laminated glass as described in any one of claims 1 to 7, wherein in the transparent region, an area in which the infrared shielding layer is not arranged in a planar view forms the high infrared transmittance region.

9. The intermediate film located in the first region partially includes the infrared shielding layer, The laminated glass according to claim 1 , wherein the infrared shielding layer in the first region is in contact with a side of an outer edge of the first region that extends in a vertical direction.

10. The laminated glass described in Claim 9, wherein the infrared shielding layer in the first region further contacts an upper edge of the outer edge of the first region extending in the left-right direction.

11. The laminated glass described in any one of claims 1 to 10, wherein the infrared shielding microparticles include at least one of ITO microparticles or ATO microparticles.

12. 12. The laminated glass according to claim 1, wherein, when the laminated glass is viewed in a state where it is attached to a vehicle, the infrared shielding layer has a thickness that decreases from a lower end side of the laminated glass toward an upper end thereof.

13. The laminated glass according to claim 1 , wherein the interlayer film includes a portion that is integrally formed with the high infrared transmittance region and a region other than the high infrared transmittance region.

14. A band-shaped shielding layer is provided along the peripheral portions of the pair of glass plates in a plan view, The shielding layer includes a first shielding layer that is disposed between an upper edge end portion and an upper edge center portion of the laminated glass 10 and has a substantially constant width, The laminated glass according to claim 1 , wherein the high infrared transmittance region is in contact with the first shielding layer.

15. A vehicle having the laminated glass according to any one of claims 1 to 14 mounted as a windshield.

16. An information device is installed that transmits and / or receives information using a wavelength band of 750 nm or more and 1650 nm or less, The vehicle according to claim 15, wherein the information device transmits and / or receives the information through the high infrared transmittance area.

Citation Information

Patent Citations

  • JP1973076362A

  • Glass for autonomous vehicles

    JP2019527665A

  • Laminated glass for vehicle