Semiconductor Device
By short-circuiting the source and OC pads in the current sensing section of silicon carbide semiconductor devices, the design addresses the sensitivity of the gate insulating film to electric charges, enhancing ESD resistance and preventing dielectric breakdown, thus ensuring reliable operation.
Patent Information
- Application Number
- JP2023104570
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-06-26
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2039-02-15
AI Technical Summary
The semiconductor devices using silicon carbide as a material face challenges with the gate insulating film being sensitive to electric charges, leading to increased leakage current and reduced Electro-Static Discharge (ESD) withstand capability due to plasma and static electricity during the manufacturing process, particularly in the current sensing section with a smaller active area.
A semiconductor device design that includes a short-circuiting electrode between the source pad and the OC pad of the current sensing section, stabilizing the source potential and increasing ESD resistance by short-circuiting these pads with a metal film, thereby reducing the impact of plasma and static electricity on the gate insulating film.
The design enhances the ESD resistance of the current sensing section, preventing dielectric breakdown and maintaining the integrity of the gate insulating film during manufacturing, ensuring the device's reliability and stability.
Smart Images

Figure 0007559879000001 
Figure 0007559879000002 
Figure 0007559879000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a semiconductor device. [Background technology]
[0002] Conventionally, silicon (Si) has been used as a constituent material of power semiconductor devices that control high voltages and large currents. There are several types of power semiconductor devices, such as bipolar transistors, IGBTs (Insulated Gate Bipolar Transistors), and MOSFETs (Metal Oxide Semiconductor Field Effect Transistors with an insulated gate made of a three-layer structure of metal-oxide film-semiconductor), and these are used according to the purpose.
[0003] For example, bipolar transistors and IGBTs have a higher current density and can handle larger currents than MOSFETs, but they cannot be switched at high speeds. Specifically, bipolar transistors can only be used at switching frequencies of a few kHz, while IGBTs can only be used at switching frequencies of a few tens of kHz. On the other hand, power MOSFETs have a lower current density and are more difficult to use at high currents than bipolar transistors and IGBTs, but they are capable of high-speed switching operations up to a few MHz.
[0004] Also, unlike IGBTs, MOSFETs have a p-type base region and an n - The parasitic diode formed by the pn junction with the MOSFET drift region can be used as a freewheeling diode to protect the MOSFET. Therefore, when the MOSFET is used as an inverter device, there is no need to add an external freewheeling diode to the MOSFET, and this is attracting attention from an economical point of view.
[0005] There is a strong demand in the market for power semiconductor devices that combine high current and high speed, and efforts have been made to improve IGBTs and power MOSFETs, with development currently approaching the material limit. For this reason, semiconductor materials to replace silicon are being considered from the perspective of power semiconductor devices, and silicon carbide (SiC) is attracting attention as a semiconductor material that can be used to fabricate (manufacture) next-generation power semiconductor devices with low on-voltage, high-speed characteristics, and excellent high-temperature characteristics.
[0006] Silicon carbide is also a chemically very stable semiconductor material with a wide band gap of 3 eV, allowing it to be used extremely stably as a semiconductor even at high temperatures. Silicon carbide also has a maximum electric field strength that is at least one order of magnitude greater than that of silicon, making it a promising semiconductor material that can sufficiently reduce on-resistance. One of the features of silicon carbide is that it also has a wider band gap than other types of silicon (hereafter referred to as a wide band gap semiconductor).
[0007] In addition, as currents increase, the trench gate structure, in which a channel (inversion layer) is formed along the sidewall of the trench in a direction perpendicular to the front surface of the semiconductor substrate, is more cost-effective than the planar gate structure, in which a channel is formed along the front surface of the semiconductor substrate. This is because the trench gate structure can increase the density of unit cells (element constituent units) per unit area, thereby increasing the current density per unit area.
[0008] Since the rate of temperature rise corresponding to the volume occupied by the unit cell increases as the current density of the device increases, a double-sided cooling structure is required to improve discharge efficiency and stabilize reliability. Furthermore, in consideration of reliability, it is necessary to have a highly functional structure in which highly functional parts such as a current sensor, temperature sensor, and overvoltage protection unit are arranged as circuit parts for protecting and controlling the main semiconductor element on the same semiconductor substrate as the vertical MOSFET, which is the main semiconductor element.
[0009] As a conventional semiconductor device equipped with a current sense section, a silicon carbide device has been proposed in which the thickness of the portion of the gate insulating film covering the base region of the current sense section is made thicker than the thickness of the portion covering the base region of the main semiconductor element (see, for example, Patent Document 1 below). In Patent Document 1 below, electrostatic breakdown resistance is reduced when the gate insulating film is made thinner than when silicon is used as the semiconductor material to achieve low on-resistance, but this is improved by thickening the gate insulating film of the current sense section. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] International Publication No. 2017 / 002255 Summary of the Invention [Problem to be solved by the invention]
[0011] However, the quality of the gate insulating film formed on the surface of a semiconductor substrate made of silicon carbide is vulnerable to electric charges, and in a current sensing section in which the surface area of the active region (hereinafter referred to as active area) of the semiconductor substrate is smaller than that of the main semiconductor element, the leakage current of the gate insulating film becomes high due to plasma and static electricity generated during chemical vapor deposition (CVD) and sputtering in the manufacturing process (wafer process). Therefore, the ESD (Electro-Static Discharge) tolerance of the current sensing section is lower than that of the main semiconductor element, making it more susceptible to dielectric breakdown.
[0012] The present invention provides a semiconductor device that is less susceptible to breakdown. [Means for solving the problem]
[0013] A semiconductor device according to the present invention includes a semiconductor chip having a surface, a first metal film disposed on the surface, and a first plating film disposed on the first metal film and having the same potential as the first metal film, the first plating film including portions spaced apart by a first gap portion in a cross-sectional view. the first metal film has a planar shape that partially protrudes into the first gap. It is characterized by: In addition, a semiconductor device according to the present invention comprises a semiconductor chip having a surface, a first metal film arranged on the surface, and a first plating film arranged on the first metal film and having the same potential as the first metal film, wherein the first plating film includes, in a cross-sectional view, a first plating portion and a second plating portion spaced apart by a first gap portion, and in the first gap portion, the first metal film is arranged so as to short-circuit the first plating portion and the second plating portion.
[0014] Another semiconductor device of the present invention comprises a semiconductor chip having a surface, a first metal film arranged on the surface, a second metal film arranged on the surface, a first plating film arranged on the first metal film and having the same potential as the first metal film, and a second plating film arranged on the second metal film and having the same potential as the second metal film, wherein the first plating film includes portions spaced apart by a first gap portion in a cross-sectional view. Effect of the Invention
[0015] According to the semiconductor device of the present invention, it is possible to provide a semiconductor device that is not easily broken. [Brief description of the drawings]
[0016] [Figure 1] 1 is a plan view showing an example of a layout, as viewed from the front surface side, of a semiconductor wafer on which a semiconductor device according to a first embodiment is fabricated (manufactured). [Diagram 2] 1 is a plan view showing an example of a layout of the semiconductor device according to the first embodiment as viewed from the front surface side of a semiconductor chip. [Diagram 3] 3A to 3C are cross-sectional views showing cross-sectional structures along the cutting lines X1-X2, X2-X3, and Y1-Y2 in FIG. 2. [Figure 4] 1 is a circuit diagram showing an equivalent circuit of a semiconductor device 20 according to a first embodiment. [Diagram 5] 1 is a cross-sectional view showing a state during the manufacture of the semiconductor device according to the first embodiment. [Figure 6] 1 is a cross-sectional view showing a state during the manufacture of the semiconductor device according to the first embodiment. [Figure 7] 1 is a cross-sectional view showing a state during the manufacture of the semiconductor device according to the first embodiment. [Figure 8] 1 is a cross-sectional view showing a state during the manufacture of the semiconductor device according to the first embodiment. [Figure 9] 1 is a cross-sectional view showing a state during the manufacture of the semiconductor device according to the first embodiment. [Figure 10] 1 is a cross-sectional view showing a state during the manufacture of the semiconductor device according to the first embodiment. [Figure 11] FIG. 2 is a plan view showing a state during the manufacture of the semiconductor device according to the first embodiment. [Figure 12] 1 is a cross-sectional view showing a state during the manufacture of the semiconductor device according to the first embodiment. [Figure 13] 5 is a cross-sectional view showing another example of a state during the manufacture of the semiconductor device according to the first embodiment. FIG. [Figure 14] FIG. 11 is a plan view showing a state during the manufacture of a semiconductor device according to a second embodiment. [Figure 15] FIG. 11 is a plan view showing a state during the manufacture of a semiconductor device according to a third embodiment. [Figure 16] FIG. 13 is a plan view showing a state during the manufacture of a semiconductor device according to a fourth embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] A preferred embodiment of the semiconductor device according to the present invention will be described in detail below with reference to the accompanying drawings. In this specification and the accompanying drawings, in a layer or region prefixed with n or p, electrons or holes are the majority carriers, respectively. In addition, + and - attached to n or p respectively mean that the impurity concentration is higher and lower than that of a layer or region not prefixed with n or p. Note that in the following description of the embodiment and the accompanying drawings, the same reference numerals are attached to similar configurations, and duplicated explanations are omitted. Note that in this specification, in the notation of Miller indices, "-" means a bar attached to the index immediately following it, and adding "-" before an index represents a negative index.
[0018] (Embodiment 1) The semiconductor device according to the first embodiment is configured by using a semiconductor (wide band gap semiconductor) having a wider band gap than silicon (Si) as a semiconductor material. The structure of the semiconductor device according to the first embodiment will be described by taking an example of using silicon carbide (SiC) as the wide band gap semiconductor. FIG. 1 is a plan view showing an example of a layout of a semiconductor wafer on which the semiconductor device according to the first embodiment is fabricated (manufactured), as viewed from the front surface side. FIG. 2 is a plan view showing an example of a layout of the semiconductor device according to the first embodiment, as viewed from the front surface side of a semiconductor chip.
[0019] 2 shows an example of the layout of electrode pads of each element arranged in a region (hereinafter referred to as chip region) 10' that will become semiconductor chips 70 after dicing (cutting) of semiconductor wafer 10 using silicon carbide as a semiconductor material. Chip region 10' has, for example, a substantially rectangular planar shape, and a plurality of chip regions 10' are arranged in a matrix on semiconductor wafer 10. Chip region 10' is surrounded by scribe lines 3 (FIG. 1). Scribe lines 3 are arranged in a lattice pattern on semiconductor wafer 10. Semiconductor devices 20 according to the first embodiment shown in FIG. 2 are formed in each of chip regions 10' of semiconductor wafer 10.
[0020] The semiconductor device 20 according to the first embodiment shown in Fig. 2 has a main semiconductor element 11 and one or more circuit units for protecting and controlling the main semiconductor element 11 in the active region 1 of the same chip region 10'. The main semiconductor element 11 is a vertical MOSFET in which drift current flows vertically (depth direction Z of the semiconductor chip 70) when on, and is composed of a plurality of unit cells (functional units of the element) arranged adjacent to each other to perform a main operation. Examples of the circuit units for protecting and controlling the main semiconductor element 11 include high-function units such as a current sensing unit 12, a temperature sensing unit 13, an overvoltage protection unit (not shown), and an arithmetic circuit unit (not shown).
[0021] The main semiconductor element 11 is disposed in an effective area 1a of the active region 1. The effective area 1a of the active region 1 is an area through which a main current of the main semiconductor element 11 flows when the main semiconductor element 11 is turned on. The effective area 1a of the active region 1 has, for example, a substantially rectangular planar shape. A circuit section for protecting and controlling the main semiconductor element 11 is disposed in an ineffective area 1b of the active region 1. The ineffective area 1b of the active region 1 is an area that does not operate as the main semiconductor element 11 when the main semiconductor element 11 is turned on. The ineffective area 1b of the active region 1 has, for example, a substantially rectangular planar shape, and is adjacent to one side of the effective area 1a of the active region 1.
[0022] The ineffective region 1b of the active region 1 is disposed, for example, between the effective region 1a of the active region 1 and an edge termination region 2 surrounding the periphery of the active region 1. The edge termination region 2 is a region between the active region 1 and the outer periphery of the chip region 10', and maintains a breakdown voltage by mitigating the electric field on the front surface side of the semiconductor chip 70. In the edge termination region 2, a breakdown voltage structure (not shown), such as a field limiting ring (FLR) or a junction termination extension (JTE) structure, is disposed. The breakdown voltage is the limit voltage at which an element does not malfunction or break down.
[0023] In the effective region 1a of the active region 1, a source pad (electrode pad: first metal film, first pad portion) 21a of the main semiconductor element 11 is arranged on the front surface of the semiconductor chip 70. In the ineffective region 1b of the active region 1, electrode pads of a circuit section for protecting and controlling the main semiconductor element 11 are arranged apart from each other on the front surface of the semiconductor chip 70. The main semiconductor element 11 has a larger current capacity than other circuit sections. For this reason, the source pad 21a of the main semiconductor element 11 has, for example, a substantially rectangular planar shape that covers almost the entire effective region 1a of the active region 1. The planar shape of the source pad 21a is determined according to the required specifications, such as the current capacity of the main semiconductor element 11.
[0024] The electrode pads other than the source pad 21a are arranged in the ineffective region 1b of the active region 1. The electrode pads other than the source pad 21a include the gate pad (second metal film) 21b of the main semiconductor element 11, the electrode pad (hereinafter referred to as the OC pad: first metal film, second pad portion) 22 of the current sensing section 12, the electrode pads (hereinafter referred to as the anode pad and cathode pad) 23a, 23b of the temperature sensing section 13, the electrode pad of the overvoltage protection section (hereinafter referred to as the OV pad: not shown), and the electrode pad of the arithmetic circuit section (hereinafter referred to as the arithmetic section pad: not shown). The electrode pads other than the source pad 21a have, for example, a substantially rectangular planar shape.
[0025] All the electrode pads are arranged apart from each other. At least the OC pad 22 among the electrode pads other than the source pad 21a faces the source pad 21a. The source pad 21a and the OC pad 22 are arranged between the source pad 21a and the OC pad 22 during the manufacturing process of the semiconductor device 20 according to the first embodiment, and are spaced apart by a length w1 (see FIGS. 11 and 12) of a short-circuit electrode 111 that connects the source pad 21a and the OC pad 22. Hereinafter, the portion between the source pad 21a and the OC pad 22 where the short-circuit electrode 111 is arranged is referred to as a short-circuit region 4 (part of the first gap).
[0026] The short-circuit region 4 may be located in either the effective region 1a or the ineffective region 1b of the active region 1, but is a region that does not function as the main semiconductor element 11 when the main semiconductor element 11 is turned on. In this short-circuit region 4, the front surface of the semiconductor chip 70 is covered with an insulating layer formed by laminating a field insulating film 80 and an interlayer insulating film 40 in this order. In the semiconductor device 20 according to the first embodiment as a product, The insulating layer A part of the cut short-circuit electrode 111 may remain on the cut short-circuit electrode 111. Reference numeral 110 denotes a cut portion of the short-circuit electrode 111 (second gap portion).
[0027] 2 illustrates the source pad 21a, the gate pad 21b, the OC pad 22, the anode pad 23a, and the cathode pad 23b in a rectangular planar shape labeled with S, G, OC, A, and K, respectively. Also, FIG. 2 illustrates a case in which the gate pad 21b, the anode pad 23a, the cathode pad 23b, and the OC pad 22 all face the source pad 21a. The electrode pads arranged in the invalid region 1b of the active region 1 may be arranged in a row along the boundary between the invalid region 1b of the active region 1 and the edge termination region 2, for example.
[0028] The current sense unit 12 has a function of detecting an overcurrent (OC) flowing through the main semiconductor element 11. The current sense unit 12 is a vertical MOSFET having a smaller number (e.g., about 10 to 20) of unit cells having the same configuration as the main semiconductor element 11 than the number of unit cells of the main semiconductor element 11 (e.g., about 10,000). The current sense unit 12 is disposed away from the main semiconductor element 11. The current sense unit 12 operates under the same conditions as the main semiconductor element 11. The current sense unit 12 may be configured using some of the unit cells of the main semiconductor element 11.
[0029] The temperature sensing unit 13 has a function of detecting the temperature of the main semiconductor element 11 by utilizing the temperature characteristics of a diode. The temperature sensing unit 13 is, for example, a polysilicon diode made of a polysilicon (poly-Si) layer provided on a field insulating film 80 (see FIG. 3) on the front surface of the semiconductor chip 70. The overvoltage protection unit (not shown) is a diode that protects the main semiconductor element 11 from overvoltage (OV) such as a surge. The current sensing unit 12, the temperature sensing unit 13 and the overvoltage protection unit are controlled by an arithmetic circuit unit, and the main semiconductor element 11 is controlled based on output signals from these units.
[0030] The arithmetic circuit section is composed of multiple semiconductor elements such as CMOS (Complementary MOS) circuits. For this reason, the arithmetic circuit section has arithmetic unit pads in addition to front surface electrodes (source electrodes, etc.: not shown) of the multiple semiconductor elements that constitute the arithmetic circuit section. When the arithmetic circuit section is arranged on the same semiconductor chip 70 as the main semiconductor element 11, it is sufficient that the element structures (including front surface electrodes) of the multiple semiconductor elements that constitute the arithmetic circuit section are arranged in the effective region 1a of the active region 1. The arithmetic unit pads may be arranged in either the effective region 1a or the ineffective region 1b of the active region 1, or may be arranged in the edge termination region 2.
[0031] Next, the cross-sectional structures of the main semiconductor element 11, the current sensing section 12, and the temperature sensing section 13 described above will be described. Fig. 3 is a cross-sectional view showing the cross-sectional structures along the cutting lines X1-X2, X2-X3, and Y1-Y2 in Fig. 2. Fig. 3 shows the cross-sectional structure along the cutting line X1-Y2 from the source pad 21a in the effective region 1a of the active region 1 in Fig. 1 through the OC pad 22 and the cathode pad 23b in the ineffective region 1b to the anode pad 23a. Fig. 3 shows the semiconductor device 20 according to the first embodiment in the state of a semiconductor chip 70 cut from the semiconductor wafer 10.
[0032] The main semiconductor element 11 and the circuit section that protects and controls the main semiconductor element 11 have the same wiring structure using pin-shaped wiring members (terminal pins 48a to 48d, described later). The main semiconductor element 11 is a vertical MOSFET having a MOS gate with a trench gate structure on the front surface side of a semiconductor chip 70. The semiconductor chip 70 is a n-type + On the starting substrate 31 - The semiconductor substrate 10 is formed by epitaxially growing silicon carbide layers 71, 72 which become the p-type drift region 32 and the p-type base region 34a in that order. The components constituting the MOS gate of the main semiconductor element 11 are provided in the effective region 1a of the active region 1.
[0033] The respective portions constituting the MOS gate of the main semiconductor element 11 are the p-type base region 34a, +Type source region 35a,p ++ The trench 37a is a n-type contact region 36a, a trench 37a, a gate insulating film 38a, and a gate electrode 39a. The trench 37a penetrates the p-type silicon carbide layer 72 in the depth direction Z from the front surface of the semiconductor chip 70 (the surface of the p-type silicon carbide layer 72). - The depth direction Z is the direction from the front surface to the back surface of the semiconductor chip 70. In the region where the main semiconductor element 11 is arranged, a p-type base region 34a is provided in the p-type silicon carbide layer 72 between adjacent trenches 37a (mesa region).
[0034] The trenches 37a may be arranged in stripes parallel to the front surface of the semiconductor chip 70 and extending in a direction X in which the electrode pads 21b, 23a, 23b, and 22 are arranged (see FIG. 2; hereinafter, referred to as a first direction) or in a direction Y perpendicular to the first direction X (hereinafter, referred to as a second direction), or may be arranged in a matrix when viewed from the front surface side of the semiconductor chip 70. FIGS. 2 and 3 show a case in which the trenches 37a are arranged in stripes extending in the first direction X. A gate electrode 39a is provided inside the trench 37a via a gate insulating film 38a. FIG. 3 shows a part of a unit cell of the main semiconductor element 11.
[0035] n - An n-type region (hereinafter referred to as n-type current diffusion region) 33a may be provided in the mesa region inside the silicon carbide layer 71 in contact with the p-type base region 34a. The n-type current diffusion region 33a is a so-called current spreading layer (CSL) that reduces the spreading resistance of carriers. The n-type current diffusion region 33a is located at a position closer to the n-type current diffusion region 33a than the bottom surface of the trench 37a from the interface with the p-type base region 34a. + Drain region (n + The starting substrate 31) is located close to the n - The first and second p-type silicon carbide layers 71 are formed in the silicon carbide layer 71. + The mold regions 61a and 62a may be selectively provided.
[0036] 1st p.+ The second p-type region 61a is provided apart from the p-type base region 34a and faces the bottom surface of the trench 37a in the depth direction Z. + The first p-type region 62a is disposed between adjacent trenches 37a (mesa region). + The first and second p-type regions 61a and 37a are spaced apart from each other, and are in contact with the p-type base region 34a. + The n-type regions 61a and 62a have a function of reducing the electric field applied to the gate insulating film 38a at the bottom of the trench 37a. + Type regions 61a, 62a and n + Between these regions, the n-type drain region is - A mold drift region 32 is provided.
[0037] Within the p-type silicon carbide layer 72, p-type base regions 34a, + type source region 35a and p ++ The contact regions 36a are selectively provided. + type source region 35a and p ++ The n-type contact region 36a is provided between the front surface of the semiconductor chip 70 and the p-type base region 34a. + The source region 35a contacts the gate insulating film 38a on the sidewall of the trench 37a and faces the gate electrode 39a via the gate insulating film 38a. The interlayer insulating film 40 is provided on the entire front surface of the semiconductor chip 70 so as to cover the gate electrode 39a.
[0038] All the gate electrodes 39a of the main semiconductor element 11 are electrically connected to the gate pad 21b (see FIG. 2) via a gate runner (not shown) made of, for example, polysilicon, in a portion not shown. The interlayer insulating film 40 is provided with a first contact hole 40a that penetrates the interlayer insulating film 40 in the depth direction Z and reaches the front surface of the semiconductor chip 70. The first contact hole 40a is electrically connected to the n-type gate electrode 39a of the main semiconductor element 11. + type source region 35a and p ++ The mold contact area 36a is exposed.
[0039] Inside the first contact hole 40a, a nickel silicide (NiSi, Ni2Si, or thermally stable NiSi2: hereinafter collectively referred to as NiSi) film 41a is provided on the front surface of the semiconductor chip 70. The NiSi film 41a is in ohmic contact with the semiconductor chip 70 inside the first contact hole 40a, and has an n + type source region 35a and p ++ The contact region 36a is electrically connected to the contact area 36b.
[0040] In the effective region 1a of the active region 1, a barrier metal (first metal film) 46a is provided on the entire surface of the interlayer insulating film 40 and the NiSi film 41a. The barrier metal 46a has a function of preventing mutual reaction between the metal films of the barrier metal or between regions facing each other across the barrier metal. The barrier metal 46a may have a layered structure in which, for example, a first titanium nitride (TiN) film 42a, a first titanium (Ti) film 43a, a second TiN film 44a, and a second Ti film 45a are layered in this order.
[0041] The first TiN film 42a is provided only on the surface of the interlayer insulating film 40, and covers the entire surface of the interlayer insulating film 40. The first Ti film 43a is provided on the surfaces of the first TiN film 42a and the NiSi film 41a. The second TiN film 44a is provided on the surface of the first Ti film 43a. The second Ti film 45a is provided on the surface of the second TiN film 44a. The barrier metal is not provided on, for example, the temperature sensing unit 13.
[0042] The source pad 21a is embedded in the first contact hole 40a and is provided on the entire surface of the second Ti film 45a. The source pad 21a is connected to the n-type semiconductor layer 41a via the barrier metal 46a and the NiSi film 41a. + type source region 35a and p ++ The source pad 21a is electrically connected to the type contact region 36a and functions as a source electrode of the main semiconductor element 11. The source pad 21a is, for example, an aluminum (Al) film or an Al alloy film.
[0043] Specifically, when the source pad 21a is an Al alloy film, the source pad 21a may be, for example, an aluminum-silicon (Al-Si) film containing silicon at about 5% or less of the total, an aluminum-silicon-copper (Al-Si-Cu) film containing silicon at about 5% or less of the total and copper (Cu) at about 5% or less of the total, or an aluminum-copper (Al-Cu) film containing copper at about 5% or less of the total.
[0044] One end of a terminal pin (first wiring) 48a is joined onto the source pad 21a via a plating film (first plating film, first plating portion) 47a and a solder layer (not shown). The other end of the terminal pin 48a is joined to a metal bar (not shown) arranged to face the front surface of the semiconductor chip 70. The other end of the terminal pin 48a is exposed to the outside of a case (not shown) in which the semiconductor chip 70 is mounted, and is electrically connected to an external device (not shown).
[0045] The terminal pin 48a is a wiring member in the shape of a round bar (cylinder) having a predetermined diameter. The terminal pin 48a is soldered to the plating film 47a in a state in which it stands approximately perpendicular to the front surface of the semiconductor chip 70. The terminal pin 48a serves as an external connection terminal for extracting the potential of the source pad 21a to the outside. The source pad 21a is connected to an external ground potential (minimum potential) via the terminal pin 48a.
[0046] The plating film 47a is formed of a material that has high adhesion to the source pad 21a even under high temperature conditions (e.g., 200°C to 300°C) and is less likely to peel off than wire bonding. The surface of the source pad 21a except for the plating film 47a is covered with a first protective film 49a. The boundary between the plating film 47a and the first protective film 49a is covered with a second protective film 50a. The first and second protective films 49a and 50a are, for example, polyimide films.
[0047] The drain electrode 51 is disposed on the back surface (n +The drain electrode 51 is in ohmic contact with the entire surface of the back surface of the starting mold substrate 31. A drain pad (electrode pad: not shown) is provided on the drain electrode 51. The drain pad has a layered structure in which, for example, a Ti film, a nickel (Ni) film, and a gold (Au) film are layered in this order. The Ni film and Au film constituting the drain pad may have thicknesses of, for example, 20 μm, 100 μm, and 2 μm, respectively.
[0048] The drain pad is soldered to a metal base plate (not shown), and at least a portion of the drain pad is in contact with a base portion of a cooling fin (not shown) via the metal base plate. The semiconductor chip 70 has a double-sided cooling structure. That is, heat generated in the semiconductor chip 70 is dissipated from the fin portion of the cooling fin that is in contact with the back surface of the semiconductor chip 70 via the metal base plate, and is also dissipated from a metal bar to which the terminal pin 48a on the front surface of the semiconductor chip 70 is joined.
[0049] A gate pad 21b of the main semiconductor element 11 is provided in the invalid region 1b of the active region 1. The gate pad 21b is electrically connected to a gate runner. The gate runner is disposed on a field oxide film (not shown) that is provided to cover the front surface of the semiconductor wafer 10 in the edge termination region 2. The gate runner is provided along the boundary between the active region 1 and the edge termination region 2, and surrounds the periphery of the active region 1.
[0050] In the ineffective region 1b of the active region 1, the p-type base region 34b of the current sense unit 12 is selectively provided in the surface region of the front surface of the semiconductor chip 70. The p-type base region 34b of the current sense unit 12 is formed by penetrating the p-type silicon carbide layer 72 in the depth direction Z and - The n-type silicon carbide layer 71 - The p-type region 32a separates the main semiconductor element 11 from the p-type base region 34a. That is, the main semiconductor element 11 and the current sensing unit 12 are - It is electrically isolated by mold region 32a.
[0051] The current sensing section 12 includes p-type base regions 34b and n-type + Type source region 35b, p ++ The current sensing section 12 includes an n-type contact region 36b, a trench 37b, a gate insulating film 38b, a gate electrode 39b, and an interlayer insulating film 40. Each portion of the MOS gate of the current sensing section 12 is provided in a region in which the current sensing section 12 is formed in the invalid region 1b of the active region 1. The current sensing section 12 includes an n-type current diffusion region 33b and first and second p-type current diffusion regions 34b and 35b of the active region 1. + It may have mold regions 61b and 62b.
[0052] All the gate electrodes 39b of the current sense section 12 are electrically connected to the gate pads 21b (see FIG. 2) of the main semiconductor element 11 via gate runners in a portion not shown. In the region where the current sense section 12 is formed, the interlayer insulating film 40 is provided with second contact holes 40b that penetrate the interlayer insulating film 40 in the depth direction Z and reach the front surface of the semiconductor chip 70. The second contact holes 40b are connected to n-type terminals of the current sense section 12. + Type source region 35b and p ++ The mold contact area 36b is exposed.
[0053] Inside the second contact hole 40b, a NiSi film 41b is provided on the front surface of the semiconductor chip 70. The NiSi film 41b is in ohmic contact with the semiconductor chip 70 inside the second contact hole 40b. In the ineffective region 1b of the active region 1, in the region where the current sense unit 12 is formed, a barrier metal (first metal film) 46b is provided on the entire surface of the interlayer insulating film 40 and the entire surface of the NiSi film 41b. The barrier metal 46b has, for example, the same layered structure and function as the barrier metal 46a of the main semiconductor element 11.
[0054] That is, the barrier metal 46b has a layered structure in which a first TiN film 42b, a first Ti film 43b, a second TiN film 44b, and a second Ti film 45b are layered in this order. The first TiN film 42b is provided only on the surface of the interlayer insulating film 40, and covers the entire surface of the interlayer insulating film 40. The first Ti film 43b covers the entire surface of the first TiN film 42b and the entire surface of the NiSi film 41b. The second TiN film 44b covers the entire surface of the first Ti film 43b. The second Ti film 45b covers the entire surface of the second TiN film 44b.
[0055] The OC pad 22 is embedded in the second contact hole 40b and is provided on the entire surface of the second Ti film 45b. The OC pad 22 is connected to the n-type semiconductor layer 41b via the barrier metal 46b and the NiSi film 41b. + Type source region 35b and p ++ The OC pad 22 is electrically connected to the type contact region 36b and functions as a source electrode of the current sense unit 12. The OC pad 22 is formed, for example, of the same material as the source pad 21a at the same time as the source pad 21a. The barrier metal 46b and the OC pad 22 have the same thickness as the barrier metal 46a of the main semiconductor element 11 and the source pad 21a.
[0056] On the OC pad 22, one end of a terminal pin (second wiring) 48b is joined via a plating film (first plating film, second plating portion) 47b and a solder layer (not shown) in the same manner as the terminal pin 48a on the source pad 21a. The other end of the terminal pin 48b is exposed to the outside of a case (not shown) in which the semiconductor chip 70 is mounted, and is electrically connected to an external device (not shown). The terminal pin 48b is a round bar-shaped (cylindrical) wiring member having a smaller diameter than the terminal pin 48a. The terminal pin 48b serves as an external connection terminal for taking out the potential of the OC pad 22 to the outside, for example. The OC pad 22 is connected to a ground potential via the terminal pin 48b and an external resistor 14 (see FIG. 4).
[0057] The surface of the OC pad 22 other than the plating film 47b is covered with a first protective film 49b, similar to the source pad 21a. The boundary between the plating film 47b and the first protective film 49b is covered with a second protective film 50b. The materials of the plating film 47b and the first and second protective films 49b, 50b are the same as those of the plating film 47a and the first and second protective films 49a, 50a on the source pad 21a, respectively.
[0058] The temperature sensing unit 13 is a polysilicon diode formed by a pn junction between a p-type polysilicon layer 81, which is a p-type anode region, and an n-type polysilicon layer 82, which is an n-type cathode region. The p-type polysilicon layer 81 and the n-type polysilicon layer 82 are provided on a field insulating film 80 in the ineffective region 1b of the active region 1. The temperature sensing unit 13 is electrically insulated from the main semiconductor element 11 and the current sensing unit 12 by the field insulating film 80.
[0059] Directly below the p-type polysilicon layer 81 and the n-type polysilicon layer 82, inside the semiconductor chip 70, there are p-type base regions 34c, ++ Type contact region 36c and the second p + The p-type base region 34c and the p-type region 62c are selectively provided. ++ The p-type contact region 36c is connected to the p-type base region 34b and the p-type ++ The second contact region 36b extends to the region where the temperature sensor 13 is formed. + The n-type region 62c is in contact with the p-type base region 34c and has a larger n-type conductivity than the p-type base region 34c. + The gate is disposed close to the drain region.
[0060] Instead of the p-type polysilicon layer 81 and the n-type polysilicon layer 82, the temperature sensing unit 13 may be configured by a p-type anode region and an n-type cathode region formed adjacent to each other inside the semiconductor chip 70. The field insulating film 80, the p-type polysilicon layer 81, and the n-type polysilicon layer 82 are covered with an interlayer insulating film 83. The interlayer insulating film 83 is provided with third and fourth contact holes 83a and 83b that penetrate the interlayer insulating film 83 in the depth direction Z and expose the p-type polysilicon layer 81 and the n-type polysilicon layer 82, respectively.
[0061] The anode pad 23a and the cathode pad 23b are in contact with the p-type polysilicon layer 81 and the n-type polysilicon layer 82 at the third and fourth contact holes 83a and 83b, respectively. The anode pad 23a and the cathode pad 23b are formed, for example, from the same material as the source pad 21a at the same time as the source pad 21a. Terminal pins 48c and 48d are joined to the anode pad 23a and the cathode pad 23b via plating films 47c and 47d and solder layers (not shown), respectively, in the same manner as the source pad 21a.
[0062] The surfaces of the anode pad 23a and the cathode pad 23b other than the plating films 47c and 47d are covered with a first protective film 49c, similar to the source pad 21a. The boundary between the plating film 47c and the first protective film 49c is covered with a second protective film 50c. The materials of the plating film 47c and the first and second protective films 49c and 50c are the same as those of the plating film 47a and the first and second protective films 49a and 50a on the source pad 21a, respectively.
[0063] The operation of the semiconductor device 20 according to the first embodiment will be described. Fig. 4 is a circuit diagram showing an equivalent circuit of the semiconductor device 20 according to the first embodiment. As shown in Fig. 4, the current sense section 12 is composed of some unit cells among the unit cells of a plurality of MOSFETs constituting the main semiconductor element 11. The ratio of the sense current flowing through the current sense section 12 to the main current flowing through the main semiconductor element 11 (hereinafter referred to as the current sense ratio) is set in advance.
[0064] The current sense ratio can be set, for example, by changing the number of unit cells between the main semiconductor element 11 and the current sense section 12. A sense current that is smaller than the main current flowing through the main semiconductor element 11 flows through the current sense section 12 according to the current sense ratio. The source of the main semiconductor element 11 is connected to a ground point GND at a ground potential. A resistor 14, which is an external component, is connected between the source of the current sense section 12 and the ground point GND.
[0065] When the main semiconductor element 11 is turned on, a main current flows from the drain to the source of the main semiconductor element 11. At this time, the current sense unit 12 is also turned on at the same time as the main semiconductor element 11, and the sense current of the current sense unit 12 flows from the drain to the source of the current sense unit 12 and flows to the ground point GND through the resistor 14. For this reason, a voltage drop occurs in the resistor 14 due to the sense current of the current sense unit 12.
[0066] When an overcurrent is applied to the main semiconductor element 11, the sense current of the current sense unit 12 increases according to the magnitude of the overcurrent in the main semiconductor element 11, and the voltage drop across the resistor 14 also increases. For this reason, it is possible to detect an overcurrent in the main semiconductor element 11 by monitoring the magnitude of the voltage drop across the resistor 14. When the voltage drop across the resistor 14 reaches or exceeds a predetermined value, the gate voltage of the main semiconductor element 11 is cut off by the arithmetic circuit unit.
[0067] A constant voltage (forward voltage Vf) is always applied between the anode and cathode of the temperature sensing unit 13. By monitoring the amount of change in the forward voltage Vf of the temperature sensing unit 13 and utilizing the temperature dependency of the forward voltage Vf of the temperature sensing unit 13, it is possible to detect a temperature rise in the main semiconductor element 11. When the change in the forward voltage Vf of the temperature sensing unit 13 reaches or exceeds a predetermined value, the arithmetic circuit unit cuts off the gate voltage of the main semiconductor element 11.
[0068] Next, a method for manufacturing the semiconductor device 20 according to the first embodiment will be described. Figures 5 to 10 and 12 are cross-sectional views showing a state during the manufacturing of the semiconductor device according to the first embodiment. Figure 11 is a plan view showing a state during the manufacturing of the semiconductor device according to the first embodiment. Figure 13 is a cross-sectional view showing another example of a state during the manufacturing of the semiconductor device according to the first embodiment. Figures 5 to 10 only show the main semiconductor element 11, but each part of all elements fabricated (manufactured) on the same semiconductor wafer 10 as the main semiconductor element 11 are formed simultaneously with each part of the main semiconductor element 11.
[0069] FIG. 11 shows one chip region 10' of the semiconductor wafer 10 of FIG. 1 (the same applies to FIGS. 14 and 15). FIG. 12 is a cross-sectional view showing the cross-sectional structure along the cutting lines X1'-X2', X2'-X3', and Y1'-Y2' of FIG. 11. The cutting line X1'-Y2' in FIG. 11 cuts the same portion as the cutting line X1-Y2 in FIG. 2. That is, FIG. 12 shows the main semiconductor element 11, the current sensing section 12, and the temperature sensing section 13. Here, the formation of each part of the main semiconductor element 11 will be described with reference to FIGS. 5 to 13, and the formation of each part of the current sensing section 12 and the temperature sensing section 13 will be described with reference to FIGS. 1, 11 to 13.
[0070] First, as shown in FIG. 5, a silicon carbide n + A starting substrate (semiconductor wafer) 31 is prepared. + The starting substrate 31 may be, for example, a nitrogen (N) doped silicon carbide single crystal substrate. + On the front surface of the starting mold substrate 31, n + The n-type starting substrate 31 is doped with nitrogen at a lower concentration. - When the main semiconductor element 11 has a breakdown voltage of 3300V, the n-type silicon carbide layer 71 is epitaxially grown. - The thickness t1 of the type silicon carbide layer 71 may be, for example, about 30 μm.
[0071] Next, as shown in FIG. 6, photolithography and ion implantation of p-type impurities such as Al are performed to form n - The first p type silicon carbide layer 71 has a surface region. + Type regions 61a and p + The mold regions 91 are selectively formed. + The mold region 91 is a second p + It is a part of the mold region 62a. + Type regions 61a and p + Type region 91 is n + The molds are repeatedly arranged alternately in a direction parallel to the front surface of the starting mold substrate 31 (for example, the first direction X or the second direction Y in FIGS. 1 and 2).
[0072] 1st p. + Type regions 61a and p + The mold regions 91 are arranged in stripes extending in the second direction Y or the first direction X in FIGS. + Type regions 61a and p + The distance d2 between the first region 91 and the mold region 92 may be, for example, about 1.5 μm. + Type regions 61a and p + The depth d1 and impurity concentration of the mold region 91 are, for example, about 0.5 μm and 5.0×10 18 / cm 3 The first p + Type regions 61a and p + The ion implantation mask (not shown) used to form the mold region 91 is removed.
[0073] Next, by photolithography and ion implantation of an n-type impurity such as nitrogen, n is formed in each chip region 10′ over the entire effective region 1a of the active region 1. - An n-type region 92 is formed in a surface region of the type silicon carbide layer 71. The n-type region 92 is, for example, a first p + Type regions 61a and p + The n-type region 92 is formed between the n-type region 91 and in contact with these regions. The depth d3 and the impurity concentration of the n-type region 92 are, for example, about 0.4 μm and 1.0×1017 / cm 3 It may be to some extent.
[0074] The n-type region 92 is a part of the n-type current diffusion region 33a. - The n-type region 92 of the first p-type silicon carbide layer 71 + Type regions 61a and p + Type region 91 and n + The starting substrate 31 and the portion sandwiched therebetween are n - The n-type drift region 32 is then removed from the ion implantation mask (not shown) used to form the n-type region 92. + Type regions 61a and p + The order of forming the mold region 91 and the mold region 92 may be reversed.
[0075] Next, as shown in Figure 7, - The n-type silicon carbide layer 71 is further doped with an n-type impurity such as nitrogen. - A silicon carbide layer is epitaxially grown to a thickness t2 of, for example, 0.5 μm, and n - The thickness of the n-type silicon carbide layer 71 is increased. - The impurity concentration of the thickened portion 71a of the silicon carbide layer 71 is n - The thickened portion 71a and the n-type silicon carbide layer 71 are + The impurity concentration may be the same as that of the portion sandwiched between the mold starting substrate 31 .
[0076] Next, photolithography and ion implantation of p-type impurities such as Al are used to create n - The thickness of the thickened portion 71a of the silicon carbide layer 71 is increased in the depth direction. + In the portion facing the mold region 91, p + At a depth of 91, + The mold region 93 is selectively formed. + The mold regions 91 and 93 are connected to each other in the depth direction, forming a second p + A mold region 62a is formed. + The width and impurity concentration of the type region 93 are, for example, p + The area is approximately the same as the mold area 91. +The ion implantation mask (not shown) used to form the mold region 93 is removed.
[0077] Next, photolithography and ion implantation of n-type impurities such as nitrogen are used to form n - The thickened portion 71a of the silicon carbide layer 71 is connected to adjacent p + An n-type region 94 is formed between the n-type regions 93 to a depth that reaches the n-type region 92. The impurity concentration of the n-type region 94 is, for example, substantially the same as that of the n-type region 92. The n-type regions 92 and 94 are connected to each other in the depth direction to form an n-type current diffusion region 33a. + The order of forming the n-type region 93 and the n-type region 94 may be reversed. Then, the ion implantation mask (not shown) used for forming the n-type region 94 is removed.
[0078] Next, as shown in Figure 8, - A p-type silicon carbide layer 72 doped with a p-type impurity such as Al is epitaxially grown on the p-type silicon carbide layer 71. The thickness t3 and impurity concentration of the p-type silicon carbide layer 72 are, for example, about 1.3 μm and 4.0×10 17 / cm 3 This allows n + On a starting substrate 31, n - A semiconductor wafer 10 is formed by sequentially stacking a n-type silicon carbide layer 71 and a p-type silicon carbide layer 72.
[0079] Next, by photolithography and ion implantation of an n-type impurity such as phosphorus (P), n is formed in the surface region of the p-type silicon carbide layer 72 in the effective region 1a of the active region 1 of each chip region 10′. + The n-type source region 35a is selectively formed. + The ion implantation mask used for forming the source region 35a is removed.
[0080] Next, by photolithography and ion implantation of p-type impurities such as Al, p-type silicon carbide is formed in the surface region of the p-type silicon carbide layer 72 in the effective region 1a of the active region 1 of each chip region 10′. ++The p-type contact region 36a is selectively formed. ++ The ion implantation mask used to form the mold contact region 36a is removed.
[0081] Next, by photolithography and ion implantation of an n-type impurity such as phosphorus, n-type impurities are formed in the vicinity of the boundary between the effective region 1a and the ineffective region 1b of the active region 1 through the p-type silicon carbide layer 72 in the depth direction Z. - The n-type silicon carbide layer 71 - A mold region 32a (see FIG. 12) is formed. - The mold region 32a separates the effective region 1a and the ineffective region 1b of the active region 1. - The ion implantation mask used to form the mold region 32a is removed.
[0082] n + Type source region 35a,p ++ Type contact regions 36a and n - The order of forming the type regions 32a may be changed. + type source region 35a and p ++ type contact region 36a and - The portion sandwiched between the p-type silicon carbide layer 71 and the p-type base region 34a is formed. In each of the above-described ion implantations, for example, a resist film or an oxide film may be used as an ion implantation mask.
[0083] Next, all the diffusion regions (first and second p + n-type regions 61a, 62a, n-type current diffusion regions 33a, + Type source region 35a,p ++ Type contact regions 36a and n - The mold region 32a) is subjected to a heat treatment (activation annealing) for about 2 minutes at a temperature of about 1700° C. in order to activate the impurities. The activation annealing may be performed once after all the diffusion regions are formed, or may be performed each time a diffusion region is formed by ion implantation.
[0084] Next, as shown in FIG. 9, n + A first p-type current diffusion region 33a penetrates through the p-type source region 35a and the p-type base region 34a. + A trench 37a is formed so as to reach the mold region 61a. As an etching mask for forming the trench 37a, for example, a resist film or an oxide film may be used.
[0085] 10, a gate insulating film 38a is formed along the surface of the semiconductor wafer 10 and the inner wall of the trench 37a. The gate insulating film 38a may be formed by thermal oxidation at a temperature of about 1000° C. in an oxygen (O2) atmosphere. The gate insulating film 38a may also be a deposition film formed by a chemical reaction of high temperature oxidation (HTO: High Temperature Oxide).
[0086] Next, for example, a phosphorus-doped polysilicon (poly-Si) layer is deposited on the gate insulating film 38a and patterned so as to fill the trench 37a, leaving a portion that will become the gate electrode 39a only inside the trench 37a (first step). At this time, the portion of the polysilicon layer that will become the gate electrode 39a may be left so as to protrude outward from the front surface of the semiconductor wafer 10, or may be left so as to be lower than the front surface of the semiconductor wafer 10.
[0087] All elements other than the main semiconductor element 11 (e.g., the current sense unit 12, the diffusion diode serving as the overvoltage protection unit, and the CMOS (Complementary MOS) constituting the arithmetic circuit unit) are formed in the invalid region 1b of the active region 1 in each chip region 10' of the semiconductor wafer 10 simultaneously with the corresponding parts of the main semiconductor element 11 during the formation of each part of the main semiconductor element 11 described above.
[0088] For example, the diffusion regions of each element arranged on the semiconductor wafer 10 may be formed simultaneously with the diffusion regions constituting the main semiconductor element 11 and having the same conductivity type, impurity concentration, and diffusion depth. Also, the gate trenches, gate insulating films, and gate electrodes of the elements arranged on the semiconductor wafer 10 may be formed simultaneously with the trenches 37a, gate insulating films 38a, and gate electrodes 39a of the main semiconductor element 11, respectively (second step).
[0089] Next, a field insulating film 80 is formed on the front surface of the semiconductor wafer 10 in the region where the temperature sensing section 13 is to be formed. At this time, a field insulating film 80 is also formed on the front surface of the semiconductor wafer 10 in the short-circuit region 4. Next, a phosphorus-doped polysilicon layer, for example, that will become an n-type polysilicon layer 82 is deposited on the field insulating film 80, and a part of the polysilicon layer is made into a p-type region to become a p-type polysilicon layer 81. Next, the polysilicon layer is patterned to leave only the parts that will become the p-type polysilicon layer 81 and the n-type polysilicon layer 82.
[0090] A gate runner (not shown) may be formed at the same time as the formation of the p-type polysilicon layer 81 and the n-type polysilicon layer 82, using the polysilicon layer deposited to form the p-type polysilicon layer 81 and the n-type polysilicon layer 82. In this case, a field insulating film 80 is also formed on the front surface of the semiconductor wafer 10 in the edge termination region 2. Then, a portion of the polysilicon layer that will become the gate runner may be left in the edge termination region 2.
[0091] Next, interlayer insulating films 40, 83 are formed on the entire front surface of the semiconductor wafer 10 so as to cover the gate electrodes 39a, 39b, the p-type polysilicon layer 81, and the n-type polysilicon layer 82. An interlayer insulating film 40 is also formed on the field insulating film 80 in the short-circuit region 4. The interlayer insulating films 40, 83 may be, for example, PSG (Phospho Silicate Glass). The thickness of the interlayer insulating films 40, 83 may be, for example, about 1 μm. Next, the interlayer insulating film 40 and the gate insulating films 38a, 38b are selectively removed by photolithography and etching to form contact holes at predetermined locations.
[0092] Specifically, first and second contact holes 40a and 40b are formed in the interlayer insulating film 40, + The source regions 35a, 35b and p ++ The mold contact regions 36a, 36b are exposed. A fifth contact hole 40d is formed in the interlayer insulating film 40 near the boundary between the effective region 1a and the ineffective region 1b of the active region 1 to expose the short-circuit region 4 (see FIGS. 11 and 12). Next, the interlayer insulating films 40, 83 are planarized (reflowed) by heat treatment.
[0093] Next, a first TiN film (first and second metal films) 102 that serves as a barrier metal is formed on the entire front surface of the semiconductor wafer 10 by, for example, sputtering. The first TiN film 102 covers the entire surfaces of the interlayer insulating films 40 and 83, and also covers the portions (n + Type source area 35a, 35b, p ++ It covers the mold contact regions 36a, 36b and the short circuit region 4).
[0094] Next, the portions of the first TiN film 102 that cover the semiconductor wafer 10 inside the first and second contact holes 40a and 40b are removed by photolithography and etching to form n + The source regions 35a, 35b and p ++The mold contact regions 36a, 36b are exposed again. The first TiN film 102 is left in the short circuit region 4. As a result, the first TiN film 102 is left on the entire surfaces of the interlayer insulating films 40, 83 and in the short circuit region 4 (short circuit process).
[0095] The portion of the first TiN film 102 remaining on the interlayer insulating film 40 becomes the first TiN film 42a constituting the barrier metal 46a of the main semiconductor element 11, and the first TiN film 42b constituting the barrier metal 46b of the current sensing section 12. The portion of the first TiN film 102 remaining in the short-circuit region 4 (hereinafter referred to as the first TiN film) 42d becomes a short-circuit electrode 111 (the hatched portion in FIG. 11) that shorts the first TiN film 42a and the first TiN film 42b.
[0096] Next, a Ni film (not shown) is formed on the semiconductor portion (front surface of the semiconductor wafer 10) exposed in the first and second contact holes 40a, 40b, for example, by sputtering. At this time, a Ni film is also formed on the first TiN film 102. Next, the Ni film is silicided at the contact points with the semiconductor portion by heat treatment at, for example, about 970° C., to form a NiSi film (first metal film) 101 in ohmic contact with the semiconductor portion.
[0097] The NiSi film 101 in the first contact hole 40a is + type source region 35a and p ++ The NiSi film 41a is in ohmic contact with the n-type contact region 36a. The NiSi film 101 in the second contact hole 40b is the n-type contact region 36a of the current sensing unit 12. + Type source region 35b and p ++ This results in a NiSi film 41b in ohmic contact with the type contact region 36b.
[0098] During the heat treatment for silicidation of nickel, the first TiN film 102 is disposed between the interlayer insulating films 40, 83 and the Ni film, thereby preventing nickel atoms in the Ni film from diffusing into the interlayer insulating films 40, 83. The portion of the Ni film above the interlayer insulating films 40, 83 is not silicided because it is not in contact with the semiconductor portion. The portion of the Ni film above the interlayer insulating films 40, 83 is removed to expose the interlayer insulating films 40, 83.
[0099] Next, for example, a Ni film is formed on the back surface of the semiconductor wafer 10. Next, the Ni film is silicided by heat treatment at, for example, about 970° C. to form a NiSi film in ohmic contact with the semiconductor portion (the back surface of the semiconductor wafer 10) as the drain electrode 51. The heat treatment for silicidation when forming the NiSi film to be the drain electrode 51 may be performed simultaneously with the heat treatment when forming the NiSi film 101 on the front surface of the semiconductor wafer 10.
[0100] Next, a first Ti film 103, a second TiN film 104, and a second Ti film 105, which serve as barrier metals, and an Al film or an Al alloy film (hereinafter collectively referred to as an Al film) 106, which serves as an electrode pad, are laminated in this order on the front surface of the semiconductor wafer 10 by sputtering. The thicknesses of the first and second TiN films 102 and 104 are, for example, about 50 nm to 200 nm, and may be, for example, about 100 nm. The thicknesses of the first and second Ti films 103 and 105 are, for example, about 10 nm to 50 nm, and may be, for example, about 20 nm. The thickness of the Al film 106 is, for example, about 5 μm or less.
[0101] Next, the metal films (first and second metal films) 103-106 are patterned by photolithography and etching to leave portions that will become the barrier metals 46a and 46b and the electrode pads 21a, 21b, and 22. The portions of the metal films 103-106 in the effective region 1a of the active region 1 respectively become the first Ti film 43a, the second TiN film 44a, the second Ti film 45a, and the source pad 21a of the main semiconductor element 11. Parts of the portions of the metal films 103-106 in the ineffective region 1b of the active region 1 respectively become the first Ti film 43b, the second TiN film 44b, the second Ti film 45b, and the OC pad 22 of the current sense unit 12 (third step).
[0102] The metal films 103-106 in the short-circuit region 4 are also removed, leaving only the first TiN film 42d, which will become the short-circuit electrode 111, in the short-circuit region 4 (FIG. 12). This results in a state in which the source pad 21a of the main semiconductor element 11 and the OC pad 22 of the current sensing section 12 are short-circuited via the short-circuit electrode 111 and the barrier metals 46a, 46b. Since the short-circuit electrode 111 is formed only by the thin first TiN film 42d, it is easy to cut off the short-circuit electrode 111 in a later process.
[0103] When the short-circuit electrode 111 is formed only from the first TiN film 42d, the portion of the first TiN film 102 that will become the short-circuit electrode 111 (the first TiN film 42d) can be left by etching that is performed to leave the first TiN film 102 only on the interlayer insulating films 40 and 83. On the other hand, when any of the metal films 103 to 106 is to be left as the short-circuit electrode 111, an etching step is performed in the middle of depositing the metal films 103 to 106 in this order to pattern the metal films that are not to be left as the short-circuit electrode 111. Therefore, when the short-circuit electrode 111 is formed only from the first TiN film 42d, all of the metal films 103 to 106 can be deposited in succession without the etching step being performed in between, and the manufacturing process can be simplified.
[0104] The short-circuit electrode 111 may have a laminated structure in which the first TiN film 42d, the first Ti film 43d, the second TiN film 44d, the second Ti film 45d, and the Al film 24 are laminated in this order, leaving the short-circuit region 4 portions of all the metal films 103-106 (FIG. 13). The short-circuit electrode 111 may be formed by leaving one or more layers of the short-circuit region 4 portions of the metal films 102-105. When only the short-circuit region 4 portions of the metal film 102 are left, the configuration shown in FIG. 12 is obtained, and other configurations are not shown.
[0105] The NiSi films 41a, 41b and the barrier metals 46a, 46b are formed in a state where the p-type polysilicon layer 81 and the n-type polysilicon layer 82 of the temperature sensing unit 13 are entirely covered with the interlayer insulating film 83. The gate pad 21b of the main semiconductor element 11 and the OV pad (not shown) of the overvoltage protection unit may be formed with the same layered structure as the source pad 21a and the OC pad 22 (fourth step).
[0106] Next, the interlayer insulating film 83 is selectively removed by photolithography and etching to form third and fourth contact holes 83a and 83b, and the p-type polysilicon layer 81 and the n-type polysilicon layer 82 are exposed in the third and fourth contact holes 83a and 83b, respectively. Next, the interlayer insulating film 83 is flattened by heat treatment. Next, the anode pad 23a and the cathode pad 23b of the temperature sensing unit 13 are formed of an Al film or an Al alloy film.
[0107] The anode pad 23a and the cathode pad 23b of the temperature sensing unit 13 may be formed simultaneously with the formation of the source pad 21a by using parts of the Al film 106 deposited to form the source pad 21a. In this case, after the formation of the barrier metals 46a, 46b and before the formation of the Al film 106, third and fourth contact holes 83a, 83b may be formed in the interlayer insulating film 83 to expose parts of the p-type polysilicon layer 81 and the n-type polysilicon layer 82.
[0108] Next, for example, a Ti film, a Ni film and a gold (Au) film are laminated in this order on the surface of the drain electrode 51 by, for example, sputtering to form a drain pad (not shown).
[0109] Next, the front surface of the semiconductor wafer 10 is protected with a polyimide film by, for example, CVD. Next, the polyimide film is selectively removed by photolithography and etching to form first protective films 49a-49c that cover the electrode pads, and the first protective films 49a-49c are opened. At this time, the portion of the polyimide film corresponding to the short-circuit region 4 is also opened to expose the short-circuit electrode 111.
[0110] Next, after a general plating pretreatment, a general plating process is performed to form plating films (first and second plating films) 47a-47c on the electrode pads 21a, 21b, 22, 23a, and 23b on the portions exposed through the openings of the first protective films 49a-49c. At this time, the first protective films 49a-49c function as a mask (first gap portion) that suppresses the spreading of the plating films 47a-47c. The thickness of the plating films 47a-47c may be, for example, about 5 μm. The plating films 47a-47c do not have to be formed on the short-circuit electrode 111.
[0111] Next, polyimide films that become second protective films 50a-50c that cover the boundaries between the plating films 47a-47c and the first protective films 49a-49c are formed by, for example, CVD. Next, the terminal pins 48a-48c are bonded to the plating films 47a-47c by solder layers (not shown). At this time, the second protective films 50a-50c function as masks that suppress the spread of the solder layers.
[0112] After the short-circuit electrode 111 is formed, the steps up to this point (predetermined steps) are performed in a state in which the source pad 21a and the OC pad 22 are short-circuited by the short-circuit electrode 111. The reason is as follows. Before the formation of the metal film (NiSi films 41a, 41b formed first) that serves as the source potential, the source potential of the main semiconductor element 11 and the current sense unit 12 is in a floating state, so that the gate insulating film 38b of the current sense unit 12 is not easily affected by plasma or static electricity. On the other hand, when the metal film that serves as the source potential is formed, the source potential of both the main semiconductor element 11 and the current sense unit 12 is fixed to a certain extent.
[0113] As described above, the current sense section 12 has a structure including unit cells having the same configuration as the main semiconductor element 11, the number of which is about 1 / 1000 of the number of unit cells of the main semiconductor element 11. Therefore, in the current sense section 12, the surface area occupied by the gate electrode 39b is smaller and the gate capacitance is extremely small compared to the main semiconductor element 11. Furthermore, particularly when silicon carbide is used as the semiconductor material, the quality of the gate insulating film 38b provided along the sidewall of the trench 37b is poor and vulnerable to electric charge, so that the gate insulating film 38b is deteriorated by plasma and static electricity generated during CVD and sputtering in the manufacturing process (wafer process).
[0114] Therefore, when metal films that become the source potential are formed on the main semiconductor element 11 and the current sense unit 12 and the source potential is fixed, the source potential of the current sense unit 12 fluctuates due to plasma and static electricity generated during the manufacturing process. This makes it easier for the gate insulating film 38b to be destroyed in the current sense unit 12, which has a smaller gate capacitance than the main semiconductor element 11. Therefore, as described above, the processes following the formation of the short-circuit electrode 111 are performed in a state in which the source pad 21a and the OC pad 22 are short-circuited by the short-circuit electrode 111. This is because the source potential of the current sense unit 12 can be stabilized while the source pad 21a and the OC pad 22 are short-circuited.
[0115] By stabilizing the source potential of the current sense unit 12, the ESD resistance of the current sense unit 12 during the manufacturing process can be increased. The length w1 of the short-circuit electrode 111 (see FIG. 11) is preferably, for example, about 5 μm or more and 10 μm or less. The shorter the length w1 of the short-circuit electrode 111, the smaller the chip size can be. The length w1 of the short-circuit electrode 111 is the distance (width in the second direction Y) between the source pad 21a and the OC pad 22. When the Al film 106 is left as the short-circuit electrode 111, the width w2 of the short-circuit electrode 111 (width in the first direction X) is preferably 5 μm or less. The reason is that the thinner the Al film 106, the easier it is to cut the short-circuit electrode 111 in a later process.
[0116] Next, before a performance test (fifth step) for checking the electrical characteristics and the presence or absence of pass / fail of the semiconductor device 20 according to the first embodiment is performed, the short-circuit electrode 111 is cut to open (disconnect) the source pad 21a of the main semiconductor element 11 and the OC pad 22 of the current sense unit 12. The performance test may be performed in the state of the semiconductor wafer 10, or may be performed in the state in which the semiconductor wafer 10 (semiconductor wafer) is diced (cut) into individual chips. The short-circuit electrode 111 may be cut during the assembly process. In particular, in the test of the current sense unit 12, the test is performed by adding a resistor 14 (see FIG. 4) between the sources of the main semiconductor element 11 and the current sense unit 12. For this reason, it is preferable that the source pad 21a and the OC pad 22 are short-circuited as far as possible until immediately before the test.
[0117] The test of the current sense unit 12 in the performance test is, for example, a withstand voltage test (screening) for evaluating the reliability of the gate insulating film 38b. In the screening, a predetermined voltage is applied to the gate insulating film 38b while the OC pad 22 of the current sense unit 12 is connected to the ground potential via an external resistor 14 (see FIG. 4). Then, the time-dependent breakdown phenomenon of the gate insulating film 38b is observed, and the reliability of the gate insulating film 38b is evaluated by checking the leakage current of the gate insulating film 38b.
[0118] Furthermore, the performance test may be performed multiple times at a predetermined timing from the start of production to the shipment of the product. In this case, after the performance test, a new short-circuit electrode 111 is formed to short-circuit the source pad 21a and the OC pad 22. At this time, a portion between the source pad 21a and the OC pad 22 other than the portion where the short-circuit electrode 111 has already been formed is set as a short-circuit region 4 where the new short-circuit electrode 111 is to be formed. Then, in a state where the source pad 21a and the OC pad 22 are short-circuited by the new short-circuit electrode 111, the process after the formation of the new short-circuit electrode 111 is performed. Thereafter, the new short-circuit electrode 111 may be cut off before the next performance test is performed.
[0119] Specifically, when the performance test is performed multiple times, for example, the following first to third tests may be performed. The first test is a wafer test performed in the state of the semiconductor wafer 10. The second test is a test performed in the state of the semiconductor chips 70 after dicing (cutting) the semiconductor wafer 10. The third test is a test performed in the state of a module after the product assembly process. When prioritizing low cost as the product of the semiconductor device 20 according to the first embodiment, the ease of the performance test process, quality, etc. may be appropriately selected. For example, if the first test is performed, it is possible to select not to perform the second and third tests.
[0120] When all of the first to third tests are performed, first, the short-circuit electrode 111 is cut off before the first test. Then, the first test is performed, and if the first test results in a pass, a conductive film is applied to the front surface of the semiconductor wafer 10 and patterned, and the conductive film is left only in the portion between the source pad 21a and the OC pad 22 other than the portion where the short-circuit electrode 111 has already been formed, to form a new short-circuit electrode 111. Next, in a state in which the source pad 21a and the OC pad 22 are short-circuited by the new short-circuit electrode 111, the steps following the formation of the new short-circuit electrode 111 are performed.
[0121] Next, before performing the second test, a new short-circuit electrode 111 is cut off. Then, the second test is performed, and if the second test results in a pass, a conductive film is applied to the front surface of the semiconductor wafer 10 and patterned, and the conductive film is left again only in the portion between the source pad 21a and the OC pad 22 other than the portion where the short-circuit electrode 111 has already been formed, to form a new short-circuit electrode 111. Next, in a state in which the source pad 21a and the OC pad 22 are short-circuited by the second new short-circuit electrode 111, the process following the formation of the second new short-circuit electrode 111 is performed.
[0122] Next, the second new short-circuit electrode 111 is cut before the third test. Next, the third test is performed, and if the third test determines that the product is good, the product is shipped. The formation of the new short-circuit electrode 111 may be manual or automated. In this way, it is preferable to short-circuit the source pad 21a and the OC pad 22 with the new short-circuit electrode 111 and perform a predetermined process between multiple performance tests while protecting the gate insulating film 38b of the current sense unit 12. This can further improve the ESD tolerance of the current sense unit 12.
[0123] Regardless of which of the metal films 102 to 106 the short-circuit electrode 111 is made of, for example, a laser or etching can be used to cut the short-circuit electrode 111. When a laser is used to cut the short-circuit electrode 111, the short-circuit electrode 111 may be cut by one laser irradiation, or the short-circuit electrode 111 may be cut by repeatedly irradiating the laser multiple times. For example, when the short-circuit electrode 111 is made of the first and second TiN films 102 and 104 or the first and second Ti films 103 and 105 and is therefore thin, the short-circuit electrode 111 can be cut in a short time by using a laser. For example, when the short-circuit electrode 111 is a TiN film, the laser waveform may be continuously oscillated in 0.1 s steps and repeatedly irradiated in 10 ms steps when cutting the short-circuit electrode 111.
[0124] When the short-circuit electrode 111 includes the Al film 106, the short-circuit electrode 111 may be cut entirely by a laser, but it takes time to cut the short-circuit electrode 111. For example, when the short-circuit electrode 111 is an Al film, a laser waveform may be repeatedly irradiated in 100 ms steps with an energy of 0.5 mJ when cutting the short-circuit electrode 111. For this reason, when the short-circuit electrode 111 includes the Al film 106, for example, after removing the Al film 106 by etching, a laser may be used to cut the other metal films 102 to 105. This allows the short-circuit electrode 111 to be cut efficiently even when the short-circuit electrode 111 includes the Al film 106.
[0125] Furthermore, when the short-circuiting electrode 111 includes the Al film 106, when the short-circuiting electrode 111 cuts the laser, molten cutting debris may scatter around, and the cutting debris may short-circuit the electrode pads. For this reason, the metal film used to form the short-circuiting electrode 111 is preferably the metal films 102 to 105 other than the Al film 106. Furthermore, when the short-circuiting electrode 111 includes the Al film 106, after the short-circuiting electrode 111 is cut, a step of removing the cutting debris may be performed using, for example, a general exhaust treatment device (scrubber).
[0126] It is sufficient that the source pad 21a and the OC pad 22 are electrically isolated after the short-circuit electrode 111 is cut, and a part of the short-circuit electrode 111 may remain on the source pad 21a and the OC pad 22. Furthermore, by cutting the short-circuit electrode 111 with a laser, interference fringes due to the laser are generated on the source pad 21a and the OC pad 22, but this does not affect the performance of the semiconductor device 20.
[0127] Thereafter, when testing is performed in the state of semiconductor wafer 10, semiconductor wafer 10 is diced (cut) along scribe lines 3 to separate into individual chips (semiconductor chips 70). Through the above steps, semiconductor device 20 shown in FIGS. 1 to 3 is completed.
[0128] As described above, according to the first embodiment, the process after the formation of the short-circuit electrode is performed in a state in which the source pad of the main semiconductor element and the OC pad of the current sense unit are short-circuited by the short-circuit electrode. While the source pad of the main semiconductor element and the OC pad of the current sense unit are short-circuited, the source potential of the current sense unit can be stabilized. This can increase the ESD tolerance of the current sense unit during the manufacturing process, thereby suppressing deterioration of the gate insulating film in the current sense unit due to plasma and static electricity generated during CVD and sputtering during the manufacturing process. Therefore, it is possible to provide a semiconductor device in which insulation breakdown is less likely to occur in the current sense unit.
[0129] Moreover, according to the first embodiment, the source potential of the main semiconductor element can be stabilized by shorting the source pad of the main semiconductor element and the OC pad of the current sense unit with the short-circuit electrode, so that the ESD tolerance of the current sense unit during the manufacturing process can be increased. According to the first embodiment, by forming a short-circuit electrode between the source pad of the main semiconductor element and the OC pad of the current sense unit, it is possible to prevent the gate pad and the gate electrode from being damaged by a laser or the like when the short-circuit electrode is cut. Therefore, it is possible to prevent the gate characteristics of the main semiconductor element and the current sense unit from fluctuating due to the cutting of the short-circuit electrode.
[0130] (Embodiment 2) Next, a method for manufacturing a semiconductor device according to the second embodiment will be described. Fig. 14 is a plan view showing a state during the manufacturing of the semiconductor device according to the second embodiment. The method for manufacturing a semiconductor device 120 according to the second embodiment differs from the method for manufacturing a semiconductor device 20 according to the first embodiment (see Fig. 11) in that, instead of short-circuiting the source pad 21a and the OC pad 22, the source pad 21a and the gate pad 21b are short-circuited by a short-circuit electrode 112 (hatched portion in Fig. 14) and then the steps up to the performance test are performed.
[0131] The gate electrode 39b of the current sense unit 12 is electrically connected to the gate electrode 39a of the main semiconductor element 11 via the gate runner. Therefore, by shorting the source pad 21a and gate pad 21b of the main semiconductor element 11, the gate electrode 39b of the current sense unit 12 can be electrically connected to the source pad 21a of the main semiconductor element 11 via the gate pad 21b and the gate runner. This makes it possible to increase the ESD tolerance of the current sense unit 12 during the manufacturing process, similar to the first embodiment.
[0132] That is, the manufacturing method of the semiconductor device 120 according to the second embodiment is the same as the manufacturing method of the semiconductor device 20 according to the first embodiment, except for the arrangement of the short-circuit electrode 112. The short-circuit electrode 112 is arranged between the source pad 21a and the gate pad 21b. The short-circuit electrode 112 may be formed, for example, with the same layer structure, length w11 and width w12 as the short-circuit electrode 111 of the first embodiment, and by the same method as the short-circuit electrode 111. In FIG. 14, the portion (short-circuit region) between the source pad 21a and the gate pad 21b where the short-circuit electrode 112 is arranged is denoted by reference numeral 5.
[0133] As described above, according to the second embodiment, by electrically connecting the gate electrode of the current sense unit to the source pad of the main semiconductor element, the gate capacitance of the current sense unit can be artificially increased during the manufacturing process, thereby obtaining the same effect as in the first embodiment.
[0134] (Embodiment 3) Next, a method for manufacturing the semiconductor device according to the third embodiment will be described. Fig. 15 is a plan view showing a state in the middle of manufacturing the semiconductor device according to the third embodiment. The method for manufacturing the semiconductor device 120' according to the third embodiment is obtained by applying the method for manufacturing the semiconductor device 120 according to the second embodiment (see Fig. 14) to the method for manufacturing the semiconductor device 20 according to the first embodiment (see Fig. 11). That is, the OC pad 22 and the gate pad 21b are short-circuited to the source pad 21a.
[0135] Specifically, the manufacturing method of the semiconductor device 120' according to the third embodiment differs from the manufacturing method of the semiconductor device 20 according to the first embodiment in that the source pad 21a and the OC pad 22 are short-circuited by the short-circuit electrode 111 (hatched portion) formed in the short-circuit region 4, and the source pad 21a and the gate pad 21b are further short-circuited by the short-circuit electrode 112 (hatched portion) formed in the short-circuit region 5, and then the processes up to the performance test are performed in this state.
[0136] When disconnecting the short-circuit electrodes 111, 112 before a performance test, it is preferable to disconnect the short-circuit electrode 112 on the high potential side that short-circuits the source pad 21a and the gate pad 21b, and then disconnect the short-circuit electrode 111 on the low potential (ground potential) side that short-circuits the source pad 21a and the OC pad 22. The reason for this is that the short-circuit electrode 112 can be disconnected while the source pad 21a is grounded by the short-circuit electrode 111, thereby making it possible to prevent a high potential from being applied to the source pad 21a.
[0137] As described above, according to the third embodiment, the same effects as those of the first and second embodiments can be obtained even when the gate pad of the main semiconductor element and the OC pad of the current sensing section are short-circuited to the source pad of the main semiconductor element by different short-circuit electrodes.
[0138] (Embodiment 4) Next, a method for manufacturing the semiconductor device according to the fourth embodiment will be described. Fig. 16 is a plan view showing a state in the middle of manufacturing the semiconductor device according to the fourth embodiment. Fig. 16 shows the planar shape of the short-circuit electrode. The method for manufacturing the semiconductor device 20' according to the fourth embodiment differs from the method for manufacturing the semiconductor device 20 according to the first embodiment (see Fig. 11) in that the width w2' of a portion 111c of the short-circuit electrode 111' is narrowed.
[0139] Specifically, in the fifth embodiment, each of the connection portions 111a, 111b of the short-circuit electrode 111' between the source pad 21a and the OC pad 22 has a width w2 that prevents the short-circuit electrode 111' from being separated from the source pad 21a and the OC pad 22 during etching to leave any one of the metal films 102-106 (see Figures 12 and 13) as the short-circuit electrode 111' (hereinafter referred to as etching to form the short-circuit electrode 111').
[0140] The portion 111c of the short-circuit electrode 111' where the width w2' is narrowed (hereinafter referred to as the cut portion) is the cut portion when the short-circuit electrode 111' is cut before a performance test. The cut portion 111c of the short-circuit electrode 111' has a width w2' that is not cut during etching when the short-circuit electrode 111' is formed. The short-circuit electrode 111' may have, for example, a substantially I-shaped planar shape in which the cut portion 111c is narrower than the connecting portion 111a with the source pad 21a and the connecting portion 111b with the OC pad 22.
[0141] As described above, according to the fourth embodiment, it is possible to obtain the same effects as those of the first to third embodiments. Moreover, according to the fourth embodiment, by narrowing the width of the cut portion of the short-circuit electrode, it is possible to cut the short-circuit electrode more efficiently before the performance test.
[0142] The present invention is not limited to the above-mentioned embodiment, and various modifications can be made without departing from the spirit of the present invention. For example, in the above-mentioned embodiment, the short-circuit electrode is made of the thinnest metal film among the metal films constituting the barrier metal, so that the short-circuit electrode can be efficiently disconnected. The present invention is also applicable to the case where a wide band gap semiconductor is used as the semiconductor material instead of silicon carbide. The present invention is also applicable when the conductivity type (n-type, p-type) is reversed. [Industrial Applicability]
[0143] INDUSTRIAL APPLICABILITY As described above, the semiconductor device according to the present invention is useful as a power semiconductor device used in power conversion devices and power supply devices for various industrial machines. [Explanation of symbols]
[0144] 1 active area 1a Effective area of active region 1b Ineffective area of active region 2 Edge Termination Area 3 Scribe Line 4,5 Short circuit area 10. Semiconductor Wafers 10' Chip area of semiconductor wafer 11 Main semiconductor element 12 Current Sense Section 13 Temperature sensor 14 Resistor 20, 20', 120, 120' Semiconductor device 21a Source pad (electrode pad) 21b Gate pad (electrode pad) 22 OC pads (electrode pads) 23a Anode pad (electrode pad) 23b Cathode pad (electrode pad) 24,106 Aluminum film 31 n + Starting substrate 32n - Mold Drift Region 32a n - type area 33a,33b n-type current spreading region 34a~34c p-type base region 35a, 35b n + Type Source Area 36a~36c p ++ Mold Contact Area 37a, 37b trench 38a, 38b Gate insulating film 39a, 39b Gate electrode 40,83 Interlayer insulating film 40a~40d, 83a, 83b Contact holes 41a,41b,101 NiSi film 42a,42b,42d,102 1st TiN film 43a,43b,43d,103 1st Ti film 44a,44b,44d,104 2nd TiN film 45a,45b,45d,105 2nd Ti film 46a, 46b Barrier metal 47a~47d Plating film 48a~48d Terminal pins 49a~49c 1st protective film 50a~50c 2nd protective film 51 Drain electrode 61a, 61b, 62a-62c, 91p + type area 70 Semiconductor Chips 71 n - mold silicon carbide layer 71a n - The portion where the thickness of the silicon carbide layer is increased 72 p-type silicon carbide layer 80 Field insulating film 81 p-type polysilicon layer 82 n-type polysilicon layer 92,94 n-type region 111,111',112 Shorting electrode GND grounding point X is a direction parallel to the front surface of the semiconductor chip and in which the electrode pads in the ineffective area are arranged (first direction) Y: A direction (second direction) that is parallel to the front surface of the semiconductor chip and perpendicular to the first direction Z depth direction d1 p + Depth between mold regions d2p + Distance between mold regions d3 Depth of n-type region t1 n - of the n-type silicon carbide layer + The thickness of the first layer to be laminated on the starting substrate t2n - The thickness of the thickened portion of the silicon carbide layer t3 Thickness of p-type silicon carbide layer w1,w11 Length of short-circuit electrode w2, w2', w12 Width of shorting electrode
Claims
1. a semiconductor chip having a surface; a first metal film disposed on the surface; a first plating film disposed on the first metal film and having the same potential as the first metal film; Equipped with the first plating film includes portions spaced apart by a first gap portion in a cross-sectional view; The semiconductor device according to claim 1, wherein the first metal film has a planar shape that protrudes in part into the first gap.
2. the first plating film has at least a first plating portion and a second plating portion; The semiconductor device according to claim 1 , wherein the first gap is provided between the first plating portion and the second plating portion.
3. The semiconductor device according to claim 2 , wherein the first plating portion and the second plating portion are not directly connected to each other.
4. A first wiring connected to the first plating portion; A second wiring connected to the second plating portion; Equipped with 4. The semiconductor device according to claim 2, wherein the first wiring and the second wiring are connected to a ground potential.
5. 5. The semiconductor device according to claim 4, wherein the first wiring and the second wiring are not directly connected to each other.
6. The semiconductor device according to claim 1 , wherein the first gap overlaps at least a portion of the first metal film in a plan view.
7. A protective film is provided inside the first gap, 7. The semiconductor device according to claim 1, wherein at least a portion of an upper surface of the first plating film is exposed from the protective film.
8. the first metal film is composed of an Al film or an Al alloy film, the first metal film includes portions spaced apart by a second gap portion in a cross-sectional view; The semiconductor device according to claim 1 , wherein the first gap overlaps with the second gap in a plan view.
9. the first metal film has at least a first pad portion and a second pad portion; 9. The semiconductor device according to claim 8, wherein the second gap is provided between the first pad and the second pad.
10. 10. The semiconductor device according to claim 9, wherein the first pad portion and the second pad portion are not directly connected to each other.
11. 8. The semiconductor device according to claim 7, wherein the protective film is provided from an upper surface of the first metal film to an upper surface of the first plating film.
12. an insulating film covering the surface of the semiconductor chip; 11. The semiconductor device according to claim 8, wherein the second gap exposes at least a part of the insulating film.
13. a second metal film disposed on the surface; a second plating film disposed on the second metal film and having the same potential as the second metal film; The semiconductor device according to claim 1 , further comprising:
14. the second metal film is a gate electrode, The semiconductor device according to claim 13 , wherein the second plating film does not have a gap penetrating the second plating film in a cross-sectional view.
15. 15. The semiconductor device according to claim 1, wherein the first metal film is a source electrode.
16. the first plating film has at least a first plating portion and a second plating portion; The first gap portion is provided between the first plating portion and the second plating portion, 15. The semiconductor device according to claim 13, wherein the surface area of the first plating portion is larger than the surface area of the second plating portion.
17. the first metal film and the second metal film are composed of an Al film or an Al alloy film, the first metal film includes portions spaced apart by a second gap portion in a cross-sectional view; 15. The semiconductor device according to claim 13, wherein the first gap overlaps with the second gap in a plan view.
18. the first metal film has at least a first pad portion and a second pad portion; the second gap is provided between the first pad portion and the second pad portion, 18. The semiconductor device according to claim 17, wherein the second gap is narrower than the first gap in at least a portion of the second gap.
19. 19. The semiconductor device according to claim 1, wherein the first metal film includes, at least in part, an interference pattern formed by a laser.
20. 20. The semiconductor device according to claim 1, wherein the semiconductor chip uses silicon carbide as a semiconductor material.
21. A semiconductor chip having a surface; a first metal film disposed on the surface; a first plating film disposed on the first metal film and having the same potential as the first metal film; Equipped with the first plating film includes, in a cross-sectional view, a first plating portion and a second plating portion spaced apart by a first gap portion; A semiconductor device, characterized in that, in the first gap portion, the first metal film is provided so as to short-circuit the first plating portion and the second plating portion.
Citation Information
Patent Citations
Method of manufacturing semiconductor device, semiconductor device and apparatus for manufacturing the same
JP2001257264A
Semiconductor device
JP2002319677A
Method of manufacturing semiconductor device, method of estimating semiconductor device and semiconductor device
JP2015207736A
Semiconductor device
WO2017002255A1
Semiconductor device
WO2017208735A1