Implanted Devices

A novel implantation device using a bioabsorbable material like gelatin forms a durable coating to enhance oxygen and nutrient delivery to cell-containing devices, addressing angiogenesis inefficiencies and preventing functional impairment.

JP7560068B2Active Publication Date: 2024-10-02SHIN ETSU CHEMICAL CO LTD +2
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2022580640
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-02-09
Filing Date
2022-02-08
Publication Date
2024-10-02
Estimated Expiration
2042-02-08

AI Technical Summary

Technical Problem

Existing cell-containing devices face challenges in efficiently delivering oxygen and nutrients to living cells due to insufficient angiogenesis and the accumulation of blood and exudate, which impede the functional expression of these devices, particularly when transplanted under the skin where there are few blood vessels.

Method used

A novel implantation device comprising a material with specific physical properties, such as a bioabsorbable material like gelatin, that activates the implantation site by forming a durable coating, promoting endogenous growth factor secretion and angiogenesis without exogenous growth factors, thereby enhancing oxygen and nutrient delivery to cells.

Benefits of technology

The device efficiently activates the implantation site, preventing central necrosis and apoptosis, ensuring effective functioning of cell-containing devices even in areas with few blood vessels, while avoiding complications like bleeding and inflammation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560068000001
    Figure 0007560068000001
Patent Text Reader

Abstract

Provided is a novel device (transplantation device). The transplantation device is either (1) or (2). (1) A transplantation device containing a material (A) having a density of 12 mg / cm3 or higher, and having a dissolution rate of 80% or less after immersion for 24 hours in a normal saline solution at 37°C. (2) A transplantation device containing a material (A) in which the ratio of X / Y is at least 0.24, with X (mg / cm3) being the density and Y (times) being the degree of swelling after immersion for 60 minutes in a normal saline solution at 37°C, and which has a dissolution rate of 80% or less after immersion for 24 hours in a normal saline solution at 37°C.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to novel implantable devices and the like. [Background technology]

[0002] In recent years, research has been conducted into therapies that involve transplanting devices containing cells or tissues (these may be collectively referred to as "cell-containing devices"). A cell-containing device is, for example, a device that contains living cells or living tissues and prevents and / or treats a patient's disease by supplying physiologically active substances such as hormones and proteins related to metabolic functions to the patient or by detoxifying harmful substances in place of organs of a diseased human or animal.

[0003] Such devices include devices composed of cells or tissues themselves, as well as devices that have an immunoisolation layer (immunoisolation function) that contains (embeds) cells or tissues (devices in which cells or tissues can be transplanted via an immunoisolation layer). In particular, devices having such an immunoisolation layer are superior to direct cell or tissue transplantation (e.g., living organ transplantation) in that they do not require the administration of immunosuppressants because the immunoisolation layer protects living cells and biological tissues from the body's defense mechanisms, eliminating the need to worry about side effects from immunosuppressants and making the procedure less invasive, potentially solving the shortage of donors.

[0004] There are various shapes of devices with immune isolation function, one example of which is a microcapsule- or macrocapsule-type preparation (e.g., a cell preparation) in which living cells or biological tissues are encapsulated in a polymer. These devices are characterized by protecting the cells and tissues contained therein from the body's defense mechanisms by the strong crosslinking structure of the polymer, and further by utilizing the molecular permeability of the polymer to supply hormones and the like secreted from the cells and tissues to the body.

[0005] As such a device, for example, Patent Document 1 discloses a cell or tissue embedding device having, as an immunoisolation layer, an aqueous gel containing, as components, a modified polyvinyl alcohol resin (A) having an active carbonyl group and a crosslinker (B). Patent Document 2 discloses a cell or tissue embedding device having, as an immunoisolation layer, an aqueous gel containing, as a component, a polyvinyl alcohol resin (A) having a syndiotacticity of 32 to 40% in triad expression.

[0006] In the above-mentioned devices, it may be difficult for sufficient oxygen and nutrients to reach living cells, biological tissues, etc., and this tendency is particularly likely to be more pronounced in cell-containing devices in which naked living cells, biological tissues, etc. are embedded in an immunoisolation layer. If sufficient oxygen and nutrients are not supplied to living cells, etc., the living cells, etc. may undergo central necrosis, and the effect of transplanting the cell-containing device may not be fully obtained (function may be significantly reduced). Such problems are particularly likely to occur when transplanting into the subcutaneous tissue, where there are few blood vessels. In larger animals, where the subcutaneous tissue is thicker, oxygen and nutrient deficiencies can become more severe.

[0007] In order to solve such problems of oxygen and nutrient deficiency, a method of using a cell growth factor to induce angiogenesis at the transplant site of living cells has been proposed. For example, Patent Document 3 discloses a method using a gelatin hydrogel containing basic fibroblast growth factor. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] WO2018 / 155621 [Patent Document 2] WO2018 / 155622 [Patent Document 3] Patent Publication No. 2002-145797 Summary of the Invention [Problem to be solved by the invention]

[0009] An object of the present invention is to provide a novel device and the like.

[0010] According to the inventor's research, even if angiogenesis is only performed at the transplantation site of the cell-containing device, the contact area between the cell-containing device and the newly generated blood vessels is small, so oxygen and nutrients may not be efficiently supplied to living cells, biological tissues, etc.

[0011] In addition, when angiogenesis is performed using cell growth factors, problems may occur such as the accumulation of blood and exudates due to bleeding and inflammation at the angiogenesis site. These blood and exudates form a liquid membrane between the newly formed blood vessels and the cells or cell-containing device, inhibiting the diffusion of oxygen and nutrients from the newly formed blood vessels to the cell-containing device, which may significantly reduce the functional expression of the cell-containing device.

[0012] In this situation, the present inventors conducted extensive research based on an idea completely different from that of exogenous administration of growth factors to induce angiogenesis as in Patent Document 3, and as a result, discovered that transplantation (placement) of a specific device (material, component) containing a material with specific physical properties can activate the transplant site (for example, transplantation (placement) of a specific device prior to transplantation of a cell-containing device can suppress or prevent the above-mentioned problems and efficiently express the functions of the cell-containing device), and further research led to the completion of the present invention.

[0013] That is, the present invention relates to the following inventions, etc. [1] Density is 12mg / cm 3 A transplant device (transplant material, transplant member) containing the above material (A), which has a dissolution rate of 80 mass % or less after immersion in physiological saline at 37°C for 24 hours. [2] Density is X (mg / cm 3), and the swelling degree (converted into mass) after immersion in 37°C saline for 60 minutes is Y (times, i.e., mass times), the ratio (X / Y) of these is 0.22 or more, and the dissolution rate after immersion in 37°C saline for 24 hours is 80% or less. [3] Density is 12mg / cm 3 The density is X (mg / cm 3 ), and the swelling degree (converted into mass) after immersion in 37°C physiological saline for 60 minutes is Y (times), the ratio (X / Y) of these is 0.22 or more, and the dissolution rate after immersion in 37°C physiological saline for 24 hours is 80 mass% or less. [4] The device according to any one of [1] to [3], wherein the dissolution rate of the material (A) after immersion in physiological saline at 37° C. for 24 hours is 60 mass % or less. [5] The device according to any one of [1] to [4], which has a degree of swelling of 70 times or less in mass terms (i.e., 70 times by mass) after immersion in physiological saline at 37°C for 60 minutes. [6] Density is X (mg / cm 3 ), and the swelling degree (converted into mass) after immersion in 37°C physiological saline for 60 minutes is Y (times), wherein the ratio (X / Y) of these factors is 0.23 or more. [7] Material (A) has a density of 14 mg / cm 3 The density is X (mg / cm 3 The device according to any one of [1] to [6], wherein, when the swelling degree after immersion in 37°C physiological saline for 60 minutes is Y (times, i.e., mass times), the ratio (X / Y) between them is 0.23 or more, and the dissolution rate after immersion in 37°C physiological saline for 24 hours is 3 to 50%. [8] The device according to any one of [1] to [7], wherein the material (A) comprises a bioabsorbable material (A1). [9] The device according to any one of [1] to [8], wherein the material (A) contains gelatin.

[10] The device according to any one of [1] to [9], wherein the material (A) constitutes (is exposed on) at least a part of the surface.

[11] The device according to any one of [1] to

[10] , comprising a material (A) and a non-bioabsorbable material (member) (B).

[12] The device according to any one of [1] to

[11] , comprising a material (A) [particularly, a material (A) containing a bioabsorbable material (A1)] and a non-bioabsorbable material (member) (B), wherein the material (A) and the non-bioabsorbable material (member) (B) are integrated together.

[13] A device described in any of [1] to

[12] , comprising a material (A) [particularly, a material (A) containing a bioabsorbable material (A1)] and a non-bioabsorbable material (member) (B), wherein the proportion of the non-bioabsorbable material (B) is 1 part by volume or more per 100 parts by volume of the material (A).

[14] A device according to any of [1] to

[13] , comprising a material (A) [particularly, a material (A) containing a bioabsorbable material (A1)] and a non-bioabsorbable material (member) (B), wherein the material (A) and the non-bioabsorbable material (member) (B) are integrated together, the proportion of the non-bioabsorbable material (B) is 10 parts by volume or more per 100 parts by volume of the material (A), and the material (A) constitutes at least a part of the device surface (is exposed on the device surface).

[15] The device according to any one of

[11] to

[14] , wherein the non-bioabsorbable material (member) (B) has an adhesion prevention ability.

[16] The device according to any one of [1] to

[15] , which is (substantially) free of growth factors.

[17] A device according to any one of [1] to

[16] for forming a coating.

[18] The device according to any one of [1] to

[17] , for transplantation (implantation or placement for a predetermined period of time) into a transplantation site of a cell- or tissue-containing device (prior to transplantation of the cell- or tissue-containing device).

[19] The device according to any one of [1] to

[18] , for use in combination with a cell or tissue-containing device.

[20] The device according to

[18] or

[19] , wherein the cell- or tissue-containing device has an immunoisolation layer containing a polyvinyl alcohol-based resin (A). [twenty one] The device according to any one of

[18] to

[20] , wherein the cell- or tissue-containing device has an immunoisolation layer containing at least one polyvinyl alcohol-based resin (A) selected from a modified polyvinyl alcohol-based resin (A1) having an active carbonyl group, a polyvinyl alcohol-based resin (A2) having a syndiotacticity of 32 to 40% expressed as triads, and a polyvinyl alcohol-based resin (A3) having a degree of saponification of 97 mol % or more. [twenty two] The device according to any one of

[18] to

[22] , wherein the cells or tissues include at least one type selected from pancreatic islets (pancreatic islet cells), hepatic cells, stem cells thereof, and progenitor cells thereof. [twenty three] A method for transplanting (implanting and leaving in place for a predetermined period of time) the device according to any one of [1] to

[22] . [twenty four] A method for activating (the transplantation site) by transplanting (implanting and leaving in place for a predetermined period of time) the device according to any one of [1] to

[22] . [twenty five] The method according to

[23] or

[24] , wherein a material containing a bioabsorbable material (A1) is used as the material (A), and the bioabsorbable material (A1) (at least a part of it) is bioabsorbed (at the transplant site).

[26] The method according to any one of

[23] to

[25] , wherein a material containing a bioabsorbable material (A1) is used as the material (A) to form a coating (at the transplant site).

[27] A method for implanting (implanting and leaving in place for a predetermined period of time) a device according to any one of [1] to

[22] , which includes a device containing a non-bioabsorbable member as material (A) or a device containing a non-bioabsorbable material (B), and then removing at least the non-bioabsorbable material (and forming a transplantation spot).

[28]

[27] The method described in the above, in which removal (and formation of a transplant spot) is achieved without bleeding, inflammation, and / or vascular damage.

[29] A transplantation method comprising transplanting a cell- or tissue-containing device into the transplantation site (removal site) of the device according to any one of [1] to

[22] .

[30] A method for preventing and / or treating a disease or symptom, comprising transplanting a cell- or tissue-containing device into the transplantation site (removal site) of the device according to any one of [1] to

[22] .

[31] The method described in

[29] or

[30] , comprising a step of transplanting a device described in any one of [1] to

[22] (and further comprising a step of removing at least a non-bioabsorbable material (component) (and further forming a transplantation spot)).

[32] The device or method described in any one of [1] to

[31] , wherein the transplantation site is subcutaneous (subcutaneous tissue). Effect of the Invention

[0014] The present invention can provide a novel device.

[0015] Such a device of the present invention can activate the implantation (placement) site. For example, if the implantation (placement) is performed prior to transplantation of the cell-containing device, the above-mentioned problems can be suppressed or prevented, and the function of the cell-containing device can be efficiently expressed.

[0016] In addition, by using a material containing a bioabsorbable material (gelatin, collagen, etc.) as the material (A) constituting the device, a coating can be formed at the implantation (placement) site (or in its vicinity).

[0017] Although it is not clear why the device of the present invention can so efficiently activate the transplant site, it is speculated that by setting certain physical properties (e.g., density, dissolution rate) of the device within a predetermined range (value), the transplant site can be activated, for example, by forming a strong coating of appropriate thickness at the transplant site (and further, this has the effect of creating a transplant environment in which the cell-containing device can function easily). In particular, by using a material that contains a bioabsorbable material (gelatin, collagen, etc.) as the material (A) that constitutes the device, it is expected that a coating with sufficient thickness will be formed because the bioabsorbed material (A) will be used as part of the coating that is formed. In addition, it is thought that it will be easier to attract effector cells that secrete growth factors, and that the attracted effector cells will tend to remain in material (A), making it easier to obtain the effects of endogenous increase (secretion promotion) of extracellular matrix (ECM) and growth factors. On the other hand, it is possible that constructing the device from a non-bioabsorbable material may induce a foreign body reaction and promote the formation of a membrane and the secretion of growth factors.

[0018] Therefore, such a device can be suitably used as a transplant device (a device for transplantation) and can also be utilized as a device for coating formation, etc.

[0019] The uses of the device of the present invention are not particularly limited, and depending on the type of device and the degree and manner of activation (whether or not a coating is formed, etc.), the device may be used for desired purposes, such as wound repair (e.g., tissue repair after surgery), a scaffold for injected cells, etc.

[0020] In particular, the device of the present invention can be suitably used as a device for transplantation (implantation or placement for a predetermined period of time) at the transplantation site of a cell-containing device (prior to transplantation of the cell-containing device).

[0021] By using the cell-containing device for such purposes, the functions of the cell-containing device can be efficiently expressed (improved), and the reproducibility (precision) of such functions can be high.

[0022] The reason for this is unclear, but it is speculated that, for example, as mentioned above, it has an appropriate thickness at the transplant site, forms a strong coating, and thereby activates the transplant site (and further serves to create a transplant environment in which the cell-containing device can function easily). Furthermore, if a coating can be formed using the device of the present invention, it is thought that the coating will improve the adhesion between the transplantation site and the cell-containing device, thereby making it possible to efficiently supply oxygen and nutrients to living cells and biological tissues, and effectively expressing (improving) the function of the cell-containing device. The coating is also believed to play a role in protecting the transplant site, and therefore, for example, it is likely to prevent the surrounding tissue from being damaged by instruments when the cell-containing device is transplanted, and to suppress the secretion of cytokines and the like that reduce the function of the cell-containing device. Furthermore, the coating makes it easier to prevent the implanted cell-containing device from shifting from the implantation site, making it easier to allow the cell-containing device to function efficiently at the targeted location.

[0023] Meanwhile, the device of the present invention can activate the transplant site without using growth factors, etc. Therefore, it is completely different from the exogenous activation of the transplant site from the outside using a device containing growth factors as in the above-mentioned Patent Document 3.

[0024] With exogenous administration, it is difficult to control the release or administration locally, and the substance may diffuse from the transplant site to the whole body, necessitating the administration of large amounts of the substance or causing unexpected side effects (e.g., bleeding, swelling, induction of tumor formation, etc.). In addition, with exogenous administration, it is difficult to target growth factors, etc., at the transplant site and increase (presence) them locally. The device of the present invention does not require such exogenous administration, and therefore can efficiently activate the transplant site (and, in the case of a cell-containing device being transplanted, improve the function of the cell-containing device) while suppressing or preventing such problems.

[0025] Furthermore, the device of the present invention is useful because it can be transplanted (and even activated) even in sites such as subcutaneous tissue that have few blood vessels and where cell-containing devices and the like are thought to have difficulty functioning.

[0026] For example, as described above, perhaps because the site where the cell-containing device is transplanted can be activated, central necrosis can be efficiently suppressed or prevented regardless of the amount of blood vessels (neogenesis), and the function of the cell-containing device can be greatly improved.

[0027] Such a device of the present invention does not require the administration of exogenous growth factors and the like (and further the angiogenesis that accompanies the administration) and can efficiently prevent the retention of blood and exudates due to bleeding and inflammation at the transplant site, so that such a device can fully exhibit the functions of a cell-containing device, etc.

[0028] The device of the present invention may also induce angiogenesis at the implantation site. However, even if such angiogenesis does occur, it is believed that the degree of angiogenesis will be less (or not as extreme) than that associated with exogenous administration, and since it is due to endogenous factors, bleeding, etc. can usually be suppressed or prevented to a high degree.

[0029] Another embodiment of the device of the present invention includes a non-bioabsorbable material. With such a device, at least the non-bioabsorbable material can be left without being absorbed even after implantation (placement), and therefore a space (implant pocket) corresponding to the non-bioabsorbable material can be efficiently formed after removal. Such implantation pockets facilitate the implantation (positioning) of cell-containing devices and the like.

[0030] Furthermore, such devices containing non-bioabsorbable materials can usually be removed efficiently. For example, such devices usually show little adhesion to the implantation site (and further to the formed coating) and surrounding areas, and are less likely to damage such areas when removed. Therefore, bleeding, inflammation (occurrence of inflammation), and exudate at the implantation site can be prevented or suppressed. Thus, devices containing non-bioabsorbable materials are extremely useful because they can be both activated and easily removed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0031] <Device> The device of the present invention (which may be referred to as device 1, material, member, etc.) contains at least a material (A).

[0032] [Material (A)] A material (component) (A) usually has specific physical properties.

[0033] For example, the density of material (A) is 1 mg / cm 3 or more (e.g., 5 mg / cm 3 or more), and 3 or more (e.g., 12 mg / cm 3 or more), preferably 14 mg / cm 3 or more (e.g., 15 mg / cm 3 or more), and 3 or more (e.g., 25 mg / cm 3 More than 30mg / cm 3 More than 35mg / cm 3 More than 40mg / cm 3 More than 45mg / cm 3 More than 50mg / cm 3 More than 55mg / cm 3 The above may be used.

[0034] The upper limit of the density of the material (A) is not particularly limited, but is, for example, 5000 mg / cm 3 , 3000mg / cm 3 , 2000mg / cm 3, 1500mg / cm 3 , 1200mg / cm 3 , 1000mg / cm 3 , 800mg / cm 3 , 700mg / cm 3 , 600mg / cm 3 , 500mg / cm 3 , 400mg / cm 3 , 350mg / cm 3 , 300mg / cm 3 , 250mg / cm 3 , 200mg / cm 3 , 180mg / cm 3 , 150mg / cm 3 , 120mg / cm 3 , 100mg / cm 3 , 90mg / cm 3 , 80mg / cm 3 , 70mg / cm 3 , 60 mg / cm 3 etc. In particular, when the material (A) is a bioabsorbable material, the density is preferably not too large, in particular, a relatively small value (e.g., 500 mg / cm 3 Below 300mg / cm 3 Below, 250mg / cm 3 Below 200mg / cm 3 Below 150mg / cm 3 Below 100mg / cm 3 Below, 1~500mg / cm 3 , 5-300mg / cm 3 , 10-200mg / cm 3 , 12-150mg / cm 3 , 14-100mg / cm 3 etc.).

[0035] The specific density range can be set by appropriately combining the above upper and lower limits (for example, 12 to 2000 mg / cm3). 3 , 15-1000mg / cm 3 etc., the same applies below to the description of ranges).

[0036] Density can be determined (measured) based on volume and mass (weight). If it is difficult to directly determine the volume or mass of the material (A), it may be determined by an indirect method. For example, the density of a water-absorbent material may be determined by measuring the moisture content (moisture content) by a conventional method and correcting (subtracting) the measured moisture content.

[0037] By having the above-mentioned density (relatively high density), the implantation site is easily activated. In particular, when a coating is formed, it is easy to prevent the coating (e.g., fibroblasts, etc.) from penetrating into the inside of the device (e.g., pores, voids, etc.), and it is easy to efficiently obtain a coating with the desired shape, a coating with a smooth surface, a durable coating, etc. In addition, when a coating is formed, if the material (A) is composed of a bioabsorbable material (A1), the above density allows the bioabsorbed material (A1) to be used as part of the coating, making it easy to form a coating with sufficient thickness and strength. In addition, it is easy to attract effector cells that secrete growth factors, and the attracted effector cells tend to remain in the material (A), making it easy to obtain the effect of endogenous increase (secretion promotion) of extracellular matrix (ECM) and growth factors. Furthermore, when material (A) is made of a non-bioabsorbable material, if it has the above density, it is less likely to adhere to the surrounding tissues and is easier to remove.

[0038] In addition, the material (A) may have a dissolution rate (dissolution rate, residual rate) after immersion in physiological saline at 37°C for 24 hours of 90% by mass or less (e.g., 80% by mass or less), preferably 70% by mass or less (e.g., 60% by mass or less), more preferably 50% by mass or less (e.g., 45% by mass or less), or may have a dissolution rate of 40% by mass or less (e.g., 35% by mass or less, 32% by mass or less, 30% by mass or less, 28% by mass or less, 25% by mass or less, 22% by mass or less, 20% by mass or less), etc., and may be 5% by mass or less, 3% by mass or less, 2% by mass or less, 1% by mass or less, 0% by mass, etc., depending on the material.

[0039] The lower limit of the dissolution rate can be selected depending on the type of material (A) and the like, and may be, for example, 0% (substantially not dissolved), 0.5% by mass, 1% by mass, 2% by mass, 3% by mass, 5% by mass, 8% by mass, 10% by mass, 12% by mass, 14% by mass, 15% by mass, 16% by mass, 17% by mass, 18% by mass, etc. In particular, when material (A) is a bioabsorbable material, the elution rate may be a value that is not too small, and in particular may be a somewhat large value (for example, 14 mass% or more, 15 mass% or more, 16 mass% or more, 17 mass% or more, 18 mass% or more, 14 to 70 mass%, 15 to 50 mass%, 16 to 40 mass%, etc.).

[0040] As described below, when material (A) is made of a bioabsorbable material, the lower limit of the above-mentioned dissolution rate is often a finite value, whereas when material (A) is made of a non-bioabsorbable material, the above-mentioned dissolution rate is often 0% by mass or a low value (e.g., 5% by mass or less, 3% by mass or less, 1% by mass or less, etc.).

[0041] By having the above-mentioned dissolution rate, the implantation site is easily activated. In particular, when the material (A) is composed of a bioabsorbable material (A1), the above-mentioned elution rate eases the absorption (decomposition) rate in the body and makes it easy to form a thick coating with sufficient thickness. In addition, the effector cells tend to be retained for a long time, making it easy to obtain the effect of endogenous increase (secretion promotion) of extracellular matrix (ECM) and growth factors. Furthermore, when material (A) is made of a non-bioabsorbable material, the above-mentioned elution rate makes it easy to suppress shape changes during placement, making it easy to form a coating of the desired shape. It also makes it easy to prevent a portion of the non-bioabsorbable material from remaining in the body, making it impossible to remove when necessary. It is preferable that the material (A) satisfies both the above-mentioned dissolution rate and density in combination, which makes it easier to efficiently activate the transplant site.

[0042] In the material (A), the degree of swelling after immersion in 37°C saline for 60 minutes can be selected depending on the type of material (A) and the like, and can be selected from a range of about 200 times or less (e.g., 150 times or less, 120 times or less, 100 times or less, 80 times or less) in terms of mass, and may be 70 times or less (e.g., 65 times or less), preferably 60 times or less (e.g., 55 times or less), more preferably about 50 times or less, and particularly may be 45 times or less (e.g., 40 times or less, 35 times or less, 32 times or less, 30 times or less, 28 times or less, 25 times or less, 22 times or less, 20 times or less, 18 times or less, 15 times or less, 12 times or less, 10 times or less).

[0043] The lower limit of the swelling degree may be, for example, 1 time (substantially no swelling), 1.5 times, 2 times, 3 times, 5 times, 6 times, 7 times, 8 times, 8.5 times, 9 times, etc., in terms of mass. In particular, when the material (A) is a bioabsorbable material, the swelling degree may be a value that is not too small, and in particular, a somewhat large value (for example, 6 times or more, 7 times or more, 8 times or more, 8.5 times or more, 9 times or more, 6 to 200 times, 7 to 100 times, 8 to 60 times, etc.).

[0044] As described below, when material (A) is made of a bioabsorbable material, the lower limit of the swelling degree is often a finite value, and when material (A) is made of a non-bioabsorbable material, the swelling degree is often 1x or a lower value.

[0045] For material (A), the density is X (mg / cm 3), and the swelling degree (in terms of mass) after immersion in 37°C physiological saline for 60 minutes is Y (times, i.e., mass times), the value of these ratios (X / Y) can be selected from a range of, for example, about 0.01 or more (e.g., 0.02 or more, 0.03 or more, 0.05 or more, 0.08 or more, 0.1 or more, 0.12 or more, 0.15 or more, 0.18 or more, 0.2 or more), and can be selected from a range of about 0.21 or more (e.g., 0.22 or more). , 0.23 or more, 0.24 or more, 0.25 or more, 0.28 or more, 0.3 or more), preferably 0.4 or more (e.g., 0.5 or more, 0.6 or more, 0.7 or more, 0.8 or more, 0.9 or more), more preferably 1 or more (e.g., 1.5 or more), or may be 2 or more (e.g., 2.5 or more, 3 or more, 3.5 or more, 4 or more, 4.5 or more, 5 or more, 5.5 or more, 6 or more, etc.).

[0046] The upper limit of the X / Y value depends on the quality of the material (A), and may be, for example, 3000, 2500, 2000, 1500, 1200, 1000, 500, 400, 300, 200, 150, 120, 100, 90, 80, 70, 60, 50, 40, 35, 30, 20, 18, 15, 12, 10, etc. In particular, when material (A) is a bioabsorbable material, the X / Y value may be a value that is not too large, in particular a somewhat small value (for example, 150 or less, 100 or less, 80 or less, 50 or less, 30 or less, 20 or less, 0.1 to 150, 0.2 to 120, 0.21 to 100, 0.25 to 50, etc.).

[0047] The swelling degree and X / Y value as described above make it easy to achieve the high density after transplantation. In addition, the handling property during transplantation is improved, and activation and arrangement (positioning) at a desired location are facilitated.

[0048] The material (A) may be, but is not limited to, a polymer (polymer, resin).

[0049] Furthermore, the material (A) may be a bioabsorbable material, or a non-bioabsorbable material.

[0050] Examples of bioabsorbable materials (bioabsorbable polymers) include proteins (e.g., gelatin, collagen, collagen peptides), polysaccharides or derivatives thereof [e.g., mucopolysaccharides (e.g., hyaluronic acid, heparin), alginic acid, chitin, chitosan, starch, dextran, etc.], aliphatic polyesters (e.g., polyglycolic acid, polylactic acid, glycolic acid / lactic acid copolymer, poly-β-hydroxybutyrate), etc.

[0051] The bioabsorbable material may be any material as long as it is bioabsorbable, and it does not matter whether it is actually absorbed by the body when the device is used.

[0052] Non-bioabsorbable materials include the materials described below (silicone-based resins, polyvinyl alcohol-based resins, etc.).

[0053] The material (A) may preferably comprise a bioabsorbable material (A1). When a bioabsorbable material (A1) is contained, when a coating is formed, the bioabsorbed material (A) is utilized as part of the coating to be formed, so that a coating having a sufficient thickness is easily formed. In addition, since effector cells that secrete growth factors are easily attracted, and the attracted effector cells tend to remain in the material (A), it is easy to obtain the effects of endogenous increase (promoted secretion) of extracellular matrix (ECM) and growth factors. In material (A) containing such a bioabsorbable material (A1), the proportion of the bioabsorbable material (A1) may be 10 mass% or more (e.g., 20 mass% or more), preferably 30 mass% or more (e.g., 40 mass% or more), more preferably 50 mass% or more (e.g., 60 mass% or more), 70 mass% or more (e.g., 80 mass% or more, 90 mass% or more, 95 mass% or more), or even 100 mass% (material (A) may essentially be composed of only the bioabsorbable material (A1)).

[0054] Among the bioabsorbable materials (A1), proteins are preferred, and gelatin is particularly preferred, so the material (A) (or the bioabsorbable material (A1)) may contain at least gelatin.

[0055] Gelatin (when gelatin is contained as the bioabsorbable material (A1)) will be described in detail below.

[0056] The gelatin is not particularly limited, and may be derived from any animal such as fish (fish), cow, or pig, or may be a recombinant form [recombinant gelatin (human recombinant gelatin, etc.)].

[0057] The method for producing gelatin is not particularly limited, and may be, for example, any of alkali-processed gelatin, acid-processed gelatin, and the like.

[0058] The isoelectric point, molecular weight, molecular weight distribution, viscosity, jelly strength, etc. of gelatin are not particularly limited and can be appropriately selected.

[0059] Gelatin may or may not be modified or derivatized {for example, by introducing a hydrophobic group [e.g., a hydrocarbon group (e.g., an alkyl group)] [for example, acylation of an amino group constituting gelatin (e.g., alkanoylation such as hexanoylation, dodecanoylation)], etc.}.

[0060] The site of modification or derivatization is not particularly limited, and may be a molecular terminal, a side chain, etc. Even if modification or derivatization is performed, it is often performed within a range that does not impair bioabsorbability before or after the modification or derivatization.

[0061] From the viewpoint of suppressing inflammation and swelling at the transplant site, gelatin that has not been modified (chemically modified) or derivatized (for example, by introduction of a hydrophobic group, etc.) or that has been modified (chemically modified) or derivatized (for example, by introduction of a hydrophobic group, etc.) to a small extent (for example, gelatin in which the amino groups constituting the gelatin have been modified or derivatized at a ratio of about 20 mol % or less (for example, 10 mol % or less, 5 mol % or less, 3 mol % or less, etc.)) may be preferably used.

[0062] The gelatin-containing material (A) may generally be biocompatible.

[0063] The gelatin-containing material (A) (or the bioabsorbable material (A1)) may contain other bioabsorbable materials as necessary. Such other materials may also generally be biocompatible.

[0064] Other materials (bioresorbable materials) include the materials exemplified above other than gelatin, such as proteins or peptides (e.g., collagen, collagen peptides), polysaccharides or derivatives thereof [e.g., mucopolysaccharides (e.g., hyaluronic acid, heparin), alginic acid, chitin, chitosan, starch, dextran, etc.], aliphatic polyesters (e.g., polyglycolic acid, polylactic acid, glycolic acid / lactic acid copolymer, poly-β-hydroxybutyrate), etc.

[0065] The other materials may be used alone or in combination of two or more.

[0066] When other materials (bioabsorbable materials) are included, the proportion of gelatin in the bioabsorbable material (bioabsorbable material, bioabsorbable polymer) depends on the type of other materials, but may be, for example, 30% by mass or more, 50% by mass or more, 70% by mass or more, 80% by mass or more, 90% by mass or more, 95% by mass or more, etc.

[0067] The bioabsorbable material (A1) [particularly gelatin, bioabsorbable material (A1) containing gelatin, and at least the gelatin contained in the bioabsorbable material (A1)] is preferably one which has been crosslinked.

[0068] Crosslinking treatment not only increases the strength, but also makes the material (A) (bioabsorbable material) more likely to be absorbed by the body over a certain period of time (e.g., one week to three months), and therefore may be advantageous in terms of activation (e.g., formation of a coating (uniform coating)).

[0069] The crosslinking method is not particularly limited, and crosslinking using a chemical reagent [for example, crosslinking using a crosslinking agent such as an aldehyde (e.g., formaldehyde, glutaraldehyde, etc.), carbodiimide, etc.], thermal crosslinking (thermal dehydration crosslinking, thermal crosslinking, etc.), enzymatic crosslinking, crosslinking by energy rays (photocrosslinking, ultraviolet light, electron beam, radiation, etc.), physical crosslinking (for example, hydrogen bond, hydrophobic interaction, ionic interaction, etc.), etc. can be used. Among them, thermal crosslinking (thermal dehydration crosslinking, etc.) is preferred.

[0070] The material (A) (or the device, bioabsorbable material (A1)) may contain other components. The other components are not particularly limited, but include, for example, components described below, such as cell culture components (e.g., alkali metals, alkaline earth metals, halogens, glucose, physiologically active substances, etc.).

[0071] The other component may be an angiogenic component (a component that contributes to angiogenesis).

[0072] Such angiogenic components (components that promote angiogenesis) may be any components that contribute to (promote) angiogenesis, and examples thereof include growth factors [or growth factors (cell growth factors), such as vascular endothelial growth factor (VEGF), fibroblast growth factor (FGF), hepatocyte growth factor (HGF), epidermal growth factor (EGF), insulin-like growth factors (IGFs) (e.g., IGF-1, IGF-2, etc.), platelet-derived growth factor (PDGF), placental growth factor (PlGF), insulin, etc.)], cells (e.g., cells that secrete growth factors (cell growth factors)), and the like.

[0073] Examples of cells include stem cells {e.g., mesenchymal stem cells (MSCs) [e.g., adipose-derived stem cells (ADSCs), bone marrow-derived stem cells (BMSCs), placenta-derived stem cells, umbilical cord-derived stem cells, etc.], etc.}.

[0074] Material (A) (or device 1, bioresorbable material (A1)) may be substantially free of such other components (e.g., angiogenic components), and may in particular be substantially free of growth factors.

[0075] As described above, the device of the present invention can activate the implantation site, and therefore can activate the implantation site without relying on angiogenesis caused by growth factors (or in a manner different from angiogenesis caused by growth factors).

[0076] The use of growth factors (exogenous administration), unlike the use of cells (ADSCs) etc., can cause disorders such as bleeding, inflammation, and blood / exudate retention associated with angiogenesis (excessive or extreme angiogenesis) (and furthermore, such disorders can lead to a decrease in the function (implantation results) of the cell-containing device, as described below). However, by not using growth factors, such disorders can be efficiently suppressed or prevented.

[0077] The material (A) (bioabsorbable material (A1)) may be a gel (gel-like) or may have a porous structure (porosity).

[0078] Material (A) may generally have any suitable shape (or be formed into any suitable shape).

[0079] The form (shape) of the material (component) (A) is not particularly limited, and may be selected depending on the desired physical properties (density, etc.), and examples include particulate (granular), film (sheet), columnar (e.g., cylindrical, rectangular), rod, tube, etc.

[0080] The size of the material (A) can be appropriately selected depending on the transplant site and its size, and is not particularly limited, but may be, for example, 0.01 mm or more (e.g., 0.03 mm or more), preferably 0.05 mm or more (e.g., 0.1 to 50 mm), more preferably 0.15 mm or more (e.g., 0.2 to 10 mm) in thickness, or 0.3 mm or more (e.g., 0.5 to 5 mm, 0.7 to 2 mm, 0.5 to 2 mm, 0.7 to 1.5 mm, etc.).

[0081] [Other materials] The device only needs to contain the material (A), and may be composed of only the material (A), or may contain other materials in addition to the material (A).

[0082] The device may include at least a non-bioabsorbable material (member) (hereinafter, sometimes referred to as non-bioabsorbable material (B), material (B), etc.) among such other materials (members). When the material (A) is made of a non-bioabsorbable material, it is possible to obtain effects such as less adhesion to surrounding tissues and easier removal. When material (A) is a non-bioabsorbable material, the device often does not contain other materials (non-bioabsorbable materials) (or contains a non-bioabsorbable material as material (A)).

[0083] In particular, by combining a bioabsorbable material (A1) (or a material (A) containing a bioabsorbable material (A1)) with a non-bioabsorbable material (B) to construct (form) a device, the non-bioabsorbable material can remain even if the bioabsorbable material (A1) is absorbed (dissolved) during implantation (placement). In such a device, the non-bioabsorbable material can function as a spacer (in a spacer-like manner).

[0084] Such remaining non-bioabsorbable material will form a pocket (void) at the implantation site following removal of the device (at least the non-bioabsorbable material, and in cases where the bioabsorbable material (part or all) has been absorbed, the non-bioabsorbed portion of the device (e.g., the non-bioabsorbable material)).

[0085] Such a pocket is likely to serve as a marker for the transplantation site (an activated site, such as a capsule formed), and can also serve as a pocket (transplantation pocket) when transplanting a cell-containing device, etc., as described below, and is particularly useful when such further transplantation is performed.

[0086] Non-bioabsorbable materials will be described in detail below.

[0087] (Non-bioabsorbable materials) The non-bioabsorbable material (B) usually contains (is composed of) a non-bioabsorbable polymer (non-bioabsorbable polymer).

[0088] Examples of non-bioabsorbable polymers (non-bioabsorbable polymers) include silicone-based resins, polyvinyl alcohol-based resins, polyvinyl acetal-based resins, polyurethane-based resins, fluororesins (e.g., polytetrafluoroethylene, perfluoroalkoxyalkane, etc.), olefin-based resins (e.g., polyethylene-based resins, polypropylene-based resins), polyacrylamide-based resins, polyester-based resins (e.g., polyethylene terephthalate, etc.), polyacrylonitrile-based resins, polystyrene butadiene copolymer resins, polysulfone-based resins, cellulose-based resins [e.g., cellulose ethers (e.g., carboxymethyl cellulose, hydroxypropyl cellulose, etc.)], polyoxyalkylene-based resins (e.g., resins having ethylene oxide or propylene oxide as a polymerization component, etc.), and the like.

[0089] Although the non-bioabsorbable material (non-bioabsorbable polymer) is non-bioabsorbable, it may generally be biocompatible (biocompatible polymer). The non-bioabsorbable material (non-bioabsorbable polymer) may be a hydrophilic polymer (or a water-soluble polymer). In addition, such hydrophilic (water-soluble) polymers are often made water-insoluble (for example, form a gel) in the device (non-bioabsorbable material) by crosslinking, chemical modification, etc.

[0090] It is preferable that the non-bioabsorbable material is unlikely to adhere to the transplant site (surrounding tissue), i.e., has an anti-adhesion ability. Note that the anti-adhesion ability means, for example, a function of preventing or suppressing adhesion between the device and the surrounding tissue or the formed coating when the device is placed at the transplant site.

[0091] Among these, silicone-based resins, polyvinyl alcohol-based resins, etc. are preferred. As the polyvinyl alcohol-based resin (polyvinyl alcohol-based resin (A)), the resins described below (e.g., modified polyvinyl alcohol-based resin (A1) having an active carbonyl group, polyvinyl alcohol-based resin (A2) having a syndiotacticity of 32 to 40% expressed as triads, polyvinyl alcohol-based resin (A3) having a degree of saponification of 97 mol % or more, etc.) may be suitably used. In such a polyvinyl alcohol-based resin, preferred embodiments may be the same as those described later.

[0092] If such a non-bioabsorbable material is used, it will adhere less to the surrounding tissues and will not damage the transplant site (the formed capsule) or the surrounding tissues (and even the vascular bed present at the transplant site) when it is removed. Therefore, bleeding, inflammation (the onset of inflammation) and exudate at the transplant site can be effectively prevented or suppressed, and the function of material (A) can be fully exerted.

[0093] The non-bioabsorbable material is not particularly limited, but may have a dissolution rate (dissolution rate, residual rate) after immersion in saline at 37°C for 24 hours of, for example, 5% by mass or less, preferably 3% by mass or less, more preferably 1% by mass or less, or may be 0% by mass (substantially not dissolved).

[0094] In the case of a non-bioabsorbable material, the degree of swelling after immersion in physiological saline at 37°C for 60 minutes may be, for example, 3 times or less, 2 times or less, 1.5 times or less, or 1 time (substantially no swelling), etc., in terms of mass. The rate of volume change when a non-bioabsorbable material is immersed in saline at 37°C for 60 minutes is not particularly limited, but may be, for example, 300% or less (e.g., 200% or less, 150% or less, 120% or less), preferably 100% or less (e.g., 80% or less, 70% or less, 60% or less), 50% or less (e.g., 40% or less, 30% or less, 20% or less, 10% or less), 0% (substantially no change in volume), etc.

[0095] When the elution rate, swelling degree, and volume change rate are within the above ranges, the shape of the non-bioabsorbable material is likely to be maintained when the device is implanted in the body, making it easy to obtain a transplant pocket of the desired size and shape.

[0096] The non-bioabsorbable material may generally have any suitable shape (or be formed into any suitable shape).

[0097] The form (shape) of the non-bioabsorbable material (component) is not particularly limited, and examples include particulate (granular), film (sheet), columnar (e.g., cylindrical, rectangular), rod, tubular, etc.

[0098] The non-bioabsorbable material may be fibrous and may be woven (eg, nonwoven) or may form a woven (eg, nonwoven) material.

[0099] The non-bioabsorbable material may be in a gel or rubber form, and may have a porous structure (sponge) or a network structure. For example, the polyvinyl alcohol-based resin used as the non-bioabsorbable material may be in the form of a gel, a sponge, etc. When the polyvinyl alcohol-based resin is used in this manner, the preferred aspects (physical properties, etc.) are the same as those described below.

[0100] The size of the non-bioabsorbable material is not particularly limited and can be appropriately selected depending on the transplant site and its size.

[0101] For example, a non-bioabsorbable material (a non-bioabsorbable material having a thickness) may have a thickness of 0.01 mm or more (e.g., 0.03 mm or more), preferably 0.05 mm or more (e.g., 0.1 to 50 mm), more preferably 0.15 mm or more (e.g., 0.2 to 10 mm), and particularly 0.3 mm or more (e.g., 0.5 to 5 mm, 0.7 to 2 mm, etc.).

[0102] The non-bioabsorbable material is not particularly limited, and depending on the type, form, and presence form of the non-bioabsorbable material (polymer) in the device, a commercially available product may be used, or the material may be manufactured (synthesized) using a conventional method.

[0103] For example, the silicone-based resin may be a commercially available or synthetic silicone rubber sheet.

[0104] In addition, when a polyvinyl alcohol-based resin is used as a non-bioabsorbable material, for example, a commercially available or synthesized polyvinyl alcohol-based resin may be used as a gel [particularly an aqueous gel (hydrogel)], sponge, etc. by a conventional method. For example, the polyvinyl alcohol resin may be gelled by a method described later (such as a method using a crosslinking agent) depending on the type, etc. In such a case, the preferred aspects are the same as those described later.

[0105] Furthermore, the non-bioabsorbable material, whether a commercially available product or a synthetic product, may be shaped (eg, punched to a predetermined size and shape) as needed depending on the shape of the transplant site and other factors.

[0106] (Other ingredients) The non-bioabsorbable material (non-bioabsorbable member) may contain other components. The other components are not particularly limited, and examples thereof include the components exemplified in the section on material (A).

[0107] Non-bioabsorbable materials (non-bioabsorbable polymers) may also be substantially free of such other components (e.g., angiogenic components), and may, for similar reasons, be substantially free of growth factors.

[0108] [device] The device must contain at least the material (A), and may contain other materials (components) as described above.

[0109] As mentioned above, the device [material (A) and further other materials (non-bioabsorbable material (B))] may be substantially free of growth factors.

[0110] In the device, the material (A) may usually constitute at least a part of the surface of the device (it may be exposed on the surface).

[0111] In such a device, material (A) may constitute 10% or more (e.g., 20% or more), preferably 30% or more (e.g., 40% or more), more preferably 50% or more (e.g., 60% or more) of the surface (surface area), and may constitute 70% or more [e.g., 80% or more, 90% or more, 95% or more, (substantially) 100%].

[0112] When the device contains other materials, it is preferable that the positional relationship (form of existence) between material (A) and the other materials (particularly non-bioabsorbable materials) is also such that material (A) constitutes at least a part of the device surface.

[0113] In a device containing other materials, the material (A) and the other materials may be in contact with each other or separated from each other, but are usually in contact with each other.

[0114] Examples of such devices include devices in which at least a portion of the surface of another material (non-bioabsorbable material) is covered with material (A) [for example, a device having (laminated) sheet-like material (A) on at least one surface (particularly both surfaces or upper and lower surfaces) of a sheet-like non-bioabsorbable material].

[0115] In devices containing other materials, the proportion of the other materials (non-bioabsorbable materials) may, for example, be 1 part by volume or more (e.g., 5 to 5,000 parts by volume), preferably 10 parts by volume or more (e.g., 15 to 3,000 parts by volume), more preferably 20 parts by volume or more (e.g., 25 to 1,000 parts by volume), 30 parts by volume or more (e.g., 35 parts by volume or more, 40 parts by volume or more, 45 parts by volume or more), etc., or 800 parts by volume or less (e.g., 500 parts by volume or less, 400 parts by volume or less, 300 parts by volume or less, 200 parts by volume or less, 150 parts by volume or less, etc.) relative to 100 parts by volume of material (A). Such a ratio makes it easy to achieve a good balance between activation of the transplant site (capsule formation, etc.) and formation of a transplant pocket.

[0116] In the device, the material (A) and other materials may usually be fixed (integrated). Typically, the material (A) and other materials (non-bioabsorbable materials) may be fixed (fixed to each other). Fixing the material (A) and the non-bioabsorbable materials makes it easier to efficiently match (correspond, position) the site of activation (film formation, etc.) and the position of the pocket.

[0117] The fixing method is not particularly limited, but examples thereof include suturing (suturing with suture thread, etc.), adhesion (adhesion (sticking) with medical adhesive, etc.), etc. Among these, suturing is preferably used. Note that the suture thread and adhesive may be biocompatible and / or bioabsorbable (degradable).

[0118] The material (A) and other materials (non-bioabsorbable materials) may be swollen with water or a predetermined liquid medium depending on the type, etc. In this case, they may be swollen before being combined, or may be combined and then swollen.

[0119] [Applications, etc.] The device (material, member) of the present invention can be used by transplantation (implantation into a living body) (used for transplantation or for use as a transplant).

[0120] Such implantation (placement) can revitalize the implant site. In particular, transplantation may result in (1) capsule formation, (2) an increase in extracellular matrix (promoted secretion), (3) an increase in growth factors (promoted secretion), and the like.

[0121] Thus, the device (material, component) of the present invention can be suitably used as a device for transplantation (transplant device, transplant material, transplant component), and if it can be activated in this manner, it can also be used as a device for use in at least one of these applications. In addition, the device of the present invention (especially a device containing a bioabsorbable material (A1) as material (A)) can often form at least a coating, and therefore the device of the present invention can often be used at least as a device for forming a coating (1).

[0122] In (1), the formation of the coating can be confirmed by visual inspection, etc., from the state before and after implantation. The coating is usually formed at the implantation site of the device (bioabsorbable material) or in the vicinity thereof (surroundings), and may be composed of at least a bioabsorbable material derived (bioabsorbed) from the device (bioabsorbable material).

[0123] In (2), examples of the extracellular matrix include collagen (eg, collagen III, collagen IV, etc.) and laminin. The extracellular matrix may contain these alone or in combination of two or more kinds.

[0124] If the device of the present invention can increase (secrete) ECM, it is believed that the ECM can be replenished, which will be even more advantageous in terms of activation (and ultimately lead to the suppression or prevention of functional decline of the cell-containing device described below).

[0125] The increase in extracellular matrix (promoted secretion) can be confirmed, for example, by immunohistochemical analysis.

[0126] Immunohistochemical analysis will be briefly described. After implantation of cells or cell-containing devices, surrounding tissues are collected, fixed with 4% paraformaldehyde, and then embedded in paraffin. For immunohistochemical staining, for example, anti-collagen III (ab7778; Abcam), anti-collagen IV (ab6586; Abcam), and laminin (ab11575; Abcam) antibodies are preferably used. In addition, EnVision+ System-HRP-labeled polymer rabbit antibody (4003; DAKO) is preferably used as a secondary antibody. By checking the positive rates of collagen III, collagen IV, and laminin staining in the surrounding tissues, the increase (promotion of secretion) of the extracellular matrix can be evaluated.

[0127] In (3), examples of growth factors (growth factors, cell growth factors) include epidermal growth factor (EGF), insulin-like growth factors (IGF) (e.g., IGF-1, IGF-2, etc.), fibroblast growth factors (FGF) (e.g., FGF12, etc.), hepatocyte growth factor (HGF), transforming growth factors (TGF) (e.g., TGF-β1, etc.), platelet-derived growth factors (PDGF) (e.g., PDGF-A, PDGF-B, etc.), etc. The growth factor may include these alone or in combination of two or more kinds.

[0128] Among these, IGF-2 may particularly be increased (secretion promoted) to a high level.

[0129] One factor that inhibits activation is thought to be apoptosis inducers due to the hypoxic environment specific to the subcutaneous environment, etc.; however, if the device of the present invention can increase (promote secretion of) growth factors (e.g., IGF-2, etc.), it is thought that apoptosis can be inhibited, which would be even more advantageous in terms of activation (ultimately, this would lead to suppression or prevention of functional decline of the cell-containing device).

[0130] Furthermore, it is possible that growth factors may contribute slightly to the induction of angiogenesis, and if the growth factors can be increased, this may also lead to more efficient activation (and ultimately to more efficient expression of the functions of the cell device, described below).

[0131] In addition, the device can increase (promote secretion of) (4) components that are not extracellular matrix or growth factors, such as cell adhesion molecules (N-cadherin, ICAM-1, VCAM-1, etc.), inducers [e.g., epithelial-mesenchymal transition inducer (c-MET), hypoxia-inducible factor 1 alpha subunit (HIF-1α), etc.], angiogenesis inhibitors (e.g., vasohibin 1), CD31, versican, thrombospondin (TSP) 2, etc.].

[0132] The increase (promotion of secretion) of growth factors etc. can be confirmed by, for example, real-time PCR.

[0133] A brief description of real-time PCR is given below. After cell or cell-containing device implantation, RNA is extracted from the surrounding tissue. Relative gene expression is determined, for example, using TaqMan Array 96-well FAST plates (4413257; Applied Biosystems). The TaqMan Array contains 46 target genes and two endogenous control gene candidates. Samples are analyzed using a StepOnePlus Real-Time polymerase chain reaction (PCR) system (Applied Biosystems) under amplification conditions of 50°C for 2 min, 95°C for 20 s, followed by 40 cycles of 95°C for 1 s and 60°C for 20 s. Results are analyzed with ExpressionSuite Software ver. 1.3 (Applied Biosystems). Growth factor augmentation (promoted secretion) can be evaluated by comparative quantification (RQ) using the comparative CT method. 18S is used as a housekeeping gene.

[0134] The extracellular matrix and growth factors (and also components that are not extracellular matrix or growth factors) are typically formed at or near the implantation site of the device (bioabsorbable material) and may be formed in the coating.

[0135] The device of the present invention may realize the above (1) to (3) (and further (4)) alone, but may also realize a combination of two or more of these. By realizing a combination of two or more of these (and further by combining angiogenesis, which will be described later), various factors can exert their combined effects, and the transplant site can be activated more efficiently.

[0136] The device is generally suitable for implantation, as described above.

[0137] Specifically, the device of the present invention can be used by being implanted (placed) in the body of an animal, including a human.

[0138] Then, through this implantation (placement), the implantation (placement) site can be activated. In cases such as when a device containing a bioabsorbable material (A1) is used as the material (A), such activation may be accompanied by at least one of (1) membrane formation, (2) increase in extracellular matrix (promoted secretion), and (3) increase in growth factors (promoted secretion) [and also increase in components other than the extracellular matrix and growth factors (promoted secretion)], as described above.

[0139] The device of the present invention may induce angiogenesis (the generation of new blood vessels) through implantation (placement). As described above, the device of the present invention can achieve the above-mentioned activation without exogenous administration of growth factors, but angiogenesis (mild angiogenesis) may occur along with activation (for example, endogenous increase (promotion of secretion) of growth factors, etc.), and such angiogenesis may be combined with capsule formation, etc., to activate the implantation site.

[0140] The degree of angiogenesis can be confirmed, for example, by immunohistochemical analysis, computed tomography (CT) angiography, and the like.

[0141] In immunohistochemical analysis, after implantation of the device, the surrounding tissue is collected, fixed with 4% paraformaldehyde, and embedded in paraffin. For immunohistochemical staining, for example, anti-von Willebrand factor (vWF) (ab7356; Merck Millipore) is preferably used. In addition, EnVision+ System-HRP-labeled polymer rabbit antibody (4003; DAKO) is preferably used as the secondary antibody. Angiogenesis can be evaluated by counting the cells themselves or vWF-positive cells in the interstitial region.

[0142] In computed tomography (CT) angiography, for example, ExiTron nano 12000, an alkaline earth metal-based nanoparticle contrast agent specially formulated for animal CT, is preferably used. The nanoparticle contrast agent is intravenously injected through the tail vein, etc., and angiography is performed using an X-ray CT scanner for laboratory animals (Latheta LCT-200; Hitachi). Angiogenesis can be evaluated by calculating the vascular volume of the tissue surrounding the transplanted cells or cell-containing device. In order to extract microvessels, it is preferable to set the CT value of the vascular region to 100 or more.

[0143] For transplantation, at least the device of the present invention may be used, and if necessary, it may be transplanted together with other devices [for example, a device containing a non-bioabsorbable material such as a polyvinyl alcohol resin (such as the resin described below), or a device in which the non-bioabsorbable material contains cells that secrete growth factors (such as ADSC)].

[0144] The transplantation site is not particularly limited, and examples thereof include subcutaneous, subfascial, visceral surface (liver surface, spleen surface, etc.), peritoneum (omentum, etc.), mesentery, abdominal cavity, inguinal, etc. The transplantation site may be muscle tissue, adipose tissue (adipocytes), etc. In particular, the transplantation site is preferably subcutaneous (subcutaneous tissue).

[0145] There are often few blood vessels subcutaneously, and the device of the present invention can efficiently activate such areas with few blood vessels (regardless of neovascularization).

[0146] The method for implanting (placement) the device is not particularly limited and may be a conventional or conventionally known method. For example, the implantation instrument may be a known one.

[0147] The subject (transplant subject) of the device of the present invention [and further the cell-containing device described below] (or transplantation) may be either a human or a non-human animal (e.g., a mammal such as a dog or a cat). The non-human animal may be a pet animal. The preferred subject is a human.

[0148] The period during which the device of the present invention is left in place will vary depending on factors such as the transplant site, but it is preferable for the device to be left in place at the transplant site for at least one week, more preferably for 10 days to 3 months, and particularly preferably for 2 weeks to 2 months.

[0149] By leaving it in place for such a period of time, sufficient activation (capsule formation, etc.) is likely to be achieved.

[0150] As described above, implantation (placement) of the device of the present invention usually results in the formation of a coating containing the bioabsorbable material (A1) derived from the device (material (A) containing the bioabsorbable material (A1)). It is considered that such bioabsorbable material (A1) will be bioabsorbed over time after coating formation, but the placement period (or the period until removal, described below) may be set within a range in which at least a coating containing the bioabsorbable material (A1) (a coating in which the bioabsorbable material (A1) remains) can be maintained.

[0151] The implanted device may be removed after a predetermined retention period. In particular, when a device containing a non-bioabsorbable material is used as the device of the present invention [for example, a device containing a non-bioabsorbable member as material (A), a device containing a non-bioabsorbable member (B) (particularly, a device containing a material (A) containing a bioabsorbable material (A1) and a non-bioabsorbable material (B)], at least the non-bioabsorbable material (usually only the non-bioabsorbable material) is often removed (removed from the implantation site) after implantation. The present invention also includes such a removal method.

[0152] When a device (material (A) containing bioabsorbable material (A1)) is left in the body for a predetermined period of time as described above (for example, one week to three months), the bioabsorbable material (A1) (part or all) is usually absorbed by the body, and at this time, a coating is often formed. On the other hand, non-bioabsorbable materials are not absorbed by the body and remain at the implanted site, so they must be removed when a cell-containing device or the like is to be implanted later.

[0153] Such removal is usually performed without bleeding, inflammation, damage to blood vessels (new blood vessels), capsule (formed capsule), etc. Such bleeding, inflammation, and damage to blood vessels and capsule can cause blood and exudate to accumulate at the removal site.

[0154] In the present invention, by selecting the above-mentioned non-bioabsorbable materials (e.g., silicone-based resins, polyvinyl alcohol-based resins, etc.) (and by selecting the retention period, etc.), and by combining this with the fact that adhesion to the transplant site is unlikely to occur, the prosthesis can often be removed efficiently without the bleeding, inflammation, or damage to blood vessels.

[0155] After removal, a transplant pocket is formed at the transplant site, into which a cell-containing device or the like may be subsequently transplanted, as described below.

[0156] As described above, the transplantation site of the device of the present invention is activated, and therefore, other devices, etc. may be transplanted into the transplantation site. Hereinafter, the case of transplanting a device containing cells or tissue will be described in detail.

[0157] <Cell or tissue-containing device> The present invention also includes a method for transplanting (placing) a device containing cells or tissues (a cell- or tissue-containing device, hereinafter sometimes referred to as a cell-containing device, device 2, etc.).

[0158] The implantation of such a cell-containing device (cell-containing component) may be performed in parallel (overlapping) with the implantation (placement) of the above-mentioned device (device 1, gelatin-containing device), or may not be performed in parallel (not overlapping). When in juxtaposition, the device 1 may be implanted in the vicinity (periphery) or adjacent to the cell-containing device.

[0159] In particular, the cell-containing device may be transplanted (placed) at the site (transplant site, transplant pocket) where the device 1 was transplanted (or removed) after the device 1 (or at least the non-bioabsorbable material) has been transplanted (or removed).

[0160] In either case, when a capsule is formed by the device 1, it is preferable to implant the cell-containing device in a state (timing) when the capsule is formed (maintained) [particularly when gelatin is contained (remains) in the capsule].

[0161] In other words, the device of the present invention (device 1) can be used as a device for use in combination with a cell-containing device, in particular, as a device for transplantation (before transplantation of the cell-containing device) into the transplantation site (an activated transplantation site such as a capsule formed) of the cell-containing device.

[0162] As described above, the device of the present invention (device 1) can activate the transplantation site (or its vicinity or surrounding area), making it easier for the cell-containing device to efficiently exert its functions. In such a method, since there is no need to transplant living cells or living tissues before the transplantation site is activated, central necrosis and apoptosis can be efficiently suppressed or prevented, and the function of the cell-containing device can be easily expressed. Furthermore, even if the cell-containing device needs to be replaced, it can be easily replaced.

[0163] In particular, as described above, in device 1 containing a non-bioabsorbable material, by selecting the type of non-bioabsorbable material, adhesions are less likely to occur, and it is possible to remove device 1 (at least the non-bioabsorbable material) without bleeding, inflammation, or blood vessel damage. By transplanting the device at such a removal site, it becomes easier to make the cell-containing device function even more efficiently.

[0164] It can also be said that by utilizing such an extraction site, the cell-containing device can be efficiently transplanted to a transplantation site where bleeding, inflammation, and blood vessel damage are not occurring.

[0165] According to the inventor's research, when bleeding, inflammation, or blood vessel damage occurs, blood or exudate tends to accumulate between the transplanted cell-containing device and the transplantation site. According to the present invention, the cell-containing device can be transplanted (placed) without such phenomena, and, combined with the activation effect of the transplantation site as described above, the function of the cell-containing device can be efficiently expressed.

[0166] It should be noted that bleeding, inflammation and blood vessel damage at the transplantation site can be visually confirmed, for example, before and after the transplantation (or removal (extraction)) of the device 1 or before the transplantation of the cell-containing device.

[0167] Examples of cell-containing devices include cells or tissues themselves, as well as devices in which cells or tissues are embedded (hereinafter sometimes referred to as cell-embedded devices). The cell-embedding device is not particularly limited, and for example, the cell-embedding devices described in the above-mentioned Patent Documents 1 and 2 may be used. A specific description will be given below.

[0168] The biological composition (cells or tissues) contained in the cell-containing device is not particularly limited and can be appropriately selected depending on the purpose of use.

[0169] As the biological composition, for example, differentiated cells or stem cells derived from the ectoderm, mesoderm or endoderm can be used.

[0170] Examples of differentiated cells that can be used include epidermal cells, smooth muscle cells, bone cells, bone marrow cells, chondrocytes, skeletal myoblasts, pancreatic parenchymal cells, pancreatic islet cells, pancreatic endocrine cells, pancreatic exocrine cells, pancreatic duct cells, liver cells (e.g., hepatocytes), thyroid cells, parathyroid cells, adrenal cells, pituitary cells, spleen cells, pineal cells, kidney cells (kidney cells), spleen cells, anterior lobe cells, growth hormone-secreting cells, dopamine-producing cells, blood cells, cardiac muscle cells, skeletal muscle cells, osteoblasts, nerve cells, pigment cells, adipocytes, etc. The above-mentioned cells may be not only cells isolated from a living body, but also cells induced to differentiate from stem cells, which will be described later.

[0171] For cells that can be induced to differentiate, such as stem cells (e.g., iPS cells), the cells that can be induced to differentiate may be transplanted or incorporated into a device and then induced to differentiate in vivo after transplantation, or the differentiated cells may be transplanted or incorporated into a device for use.

[0172] Furthermore, stem cells that can be used include, but are not limited to, tissue stem cells (e.g., epidermal stem cells, hair follicle stem cells, pancreatic stem cells / pancreatic progenitor cells, hepatic stem cells, neural stem cells, retinal stem cells, hematopoietic stem cells, etc.), embryonic stem cells (ES cells), iPS cells (induced pluripotent stem cells), etc.

[0173] These cells are preferably derived from mammals such as humans, monkeys, pigs, rats, mice, dogs, and cats, and are cells that produce and / or secrete physiologically active substances such as hormones and proteins useful to the living body of the patient, and the selection of the type of cells can be determined depending on the type of disease of the living body of the patient to be transplanted. In addition, when these cells are non-human cells, they may be cells into which a human gene has been introduced for therapeutic purposes. Examples of hormones useful to the living body include insulin, thyroid stimulating hormone, thyroid hormone, parathyroid hormone, growth hormone, thyroxine, glucocorticoids, glucagon, estradiol, and testosterone. Specific examples of proteins useful to the living body include blood coagulation factors, complement, albumin, globulin, and various enzymes (metabolic enzymes or digestive enzymes such as amylase, protease, and lipase). Examples of other physiologically active substances include neurotransmitters such as dopamine.

[0174] Specifically, pancreatic cells (pancreatic islet cells), hepatic cells, dopamine-producing cells, and their stem / progenitor cells are more preferable, and pancreatic cells (pancreatic islet cells) and pancreatic precursor (stem) cells are more preferable. As representative examples, pancreatic islets (pancreatic cells), hepatic cells, and their stem / progenitor cells may be preferably used.

[0175] The biological composition used in the cell-containing device may be any of cells or biological tissue established for laboratory use, or cells isolated from biological tissue, but is preferably a differentiated non-dividing cell. The isolation method is not particularly limited and may be any method known in the art. In addition, it is desirable that the cells isolated from biological tissue have been freed from pathogenic bacteria such as pathogenic viruses.

[0176] In the cell-containing device, the content of the biological composition can be appropriately changed depending on the type of the biological composition.

[0177] The dosage is determined by a doctor taking into consideration the age, sex, symptoms, side effects, etc. of the patient, so it cannot be generalized, but usually about 1 to 10 devices can be implanted into the body of an adult. For example, in the case of a diabetic patient, usually 1,000 to 1,000,000 IEQ (international unit of islet mass: the volume of a pancreatic islet with a diameter of 150 μm is defined as 1 IEQ), preferably 5,000 to 400,000 IEQ, more preferably 10,000 to 20,000 IEQ of islets can be implanted per kg of the patient's body weight.

[0178] As described above, the cell-embedded device is formed in a form in which a biological composition is embedded. The shape of such a cell-embedded device is not particularly limited, but may be the same type (particularly the same shape) as the device 1 (particularly the non-bioabsorbable material). Such shapes include the above-mentioned exemplary shapes, including disk-shaped, spherical, cylindrical, elliptical, etc., with disk-shaped being preferred.

[0179] The material of the cell-embedded device (the device portion of the cell-embedded device) is not particularly limited, and may be a polymer, metal, ceramic, or the like.

[0180] The polymer used in the cell-embedding device is not particularly limited, but examples thereof include structural proteins (e.g., collagen, elastin, keratin, etc.), gelatin, glycosaminoglycans (e.g., hyaluronic acid, chondroitin sulfate, keratan sulfate, dermatan sulfate, heparan sulfate, heparin, etc.), proteoglycan, cell adhesion molecules (e.g., fibronectin, laminin, fibrinogen, hydronectin, etc.), fibrin, fibroin, sericin, alginic acid, chitosan, agarose, cellulose, cellulose derivatives (e.g., cellulosic acid, cellulose esters ... Examples of suitable polymeric materials include polyvinyl alcohol-based resins (e.g., polystyrene nanofibers, carboxymethyl cellulose, hydroxypropyl cellulose, etc.), synthetic polypeptides, polylactic acid, polyglycolic acid, polycaprolactone, polyethylene glycol, polypropylene glycol, 2-methacryloyloxyethyl phosphorylcholine, poly(meth)acrylic acid, polyacrylamide, poly-N-isopropylacrylamide, dextrin, silicone, polyurethane, fluororesins (e.g., polytetrafluoroethylene, perfluoroalkoxyalkane, etc.), and polyvinyl alcohol-based resins.

[0181] The polymer may be a hydrophilic polymer (or a water-soluble polymer). Note that such hydrophilic (water-soluble) polymers are often made water-insoluble (for example, form a gel) in the cell-embedded device by crosslinking or the like.

[0182] The polymers may be used alone or in combination of two or more.

[0183] Among these, polyvinyl alcohol-based resins are particularly suitable for use, and therefore the polymer may contain at least a polyvinyl alcohol-based resin. The polyvinyl alcohol resin will be described in detail below.

[0184] (Polyvinyl alcohol resin) The polyvinyl alcohol resin may be a saponification product of a polymer having at least a vinyl ester monomer as a polymerization component. Such a polyvinyl alcohol resin may have a vinyl alcohol unit, and may have a vinyl ester unit (or a unit derived from a vinyl ester monomer, such as a vinyl acetate unit or a vinyl pivalate unit, which will be described later, derived from a fatty acid vinyl ester) or other units (such as a unit derived from an unsaturated monomer having an active carbonyl group, which will be described later, or a unit derived from another unsaturated monomer).

[0185] The viscosity of a 4 mass % aqueous solution of the polyvinyl alcohol resin (20°C) is not particularly limited, and may be, for example, 1 mPa·s or more, 2 mPa·s or more, 3 mPa·s or more, 5 mPa·s or more, 20 mPa·s or more, 30 mPa·s or more, 40 mPa·s or more, 50 mPa·s or more, or may be 800 mPa·s or less, 500 mPa·s or less, 300 mPa·s or less, 200 mPa·s or less, 150 mPa·s or less, 100 mPa·s or less, 80 mPa·s or less, for example.

[0186] Typically, a polyvinyl alcohol resin having a viscosity of a 4 mass % aqueous solution of about 3 to 300 mPa·s may be suitably used.

[0187] The viscosity of a 4 mass % aqueous solution of the polyvinyl alcohol resin can be measured, for example, in accordance with JIS K6726.

[0188] The polyvinyl alcohol-based resin can be selected depending on its type, composition, etc., and is not particularly limited. It may be a fully saponified polyvinyl alcohol-based resin (e.g., a saponification degree of 97 mol % or more) or a partially saponified polyvinyl alcohol-based resin (e.g., a saponification degree of less than 97 mol %).

[0189] The degree of saponification (average degree of saponification) can be measured, for example, according to JIS K6726.

[0190] In particular, as the polyvinyl alcohol-based resin (A), at least one selected from at least one selected from the group consisting of modified polyvinyl alcohol-based resin (A1) having an active carbonyl group, polyvinyl alcohol-based resin (A2) having a syndiotacticity of 32 to 40% expressed as triads, and polyvinyl alcohol-based resin (A3) having a degree of saponification of 97 mol % or more may be preferably used.

[0191] These resins will be described in detail below.

[0192] (Modified polyvinyl alcohol resin with active carbonyl groups) Examples of modified polyvinyl alcohol resins having active carbonyl groups (also referred to simply as "modified PVA-based resins" in this specification) that can be used include copolymerized modified PVA produced by copolymerizing a fatty acid vinyl ester with an unsaturated monomer having an active carbonyl group and saponifying the resulting copolymer, and post-modified PVA obtained by directly contacting a compound having an active carbonyl group, such as liquid diketene or diketene gas, with PVA or a modified PVA-based resin produced by a known method. From the viewpoints of the stability and safety of the PVA-based resin and the workability in the gelation step, copolymerized modified PVA is preferred.

[0193] The fatty acid vinyl ester used in producing the copolymerized modified PVA is not particularly limited, but examples thereof include vinyl formate, vinyl acetate, vinyl propionate, vinyl pivalate, etc., among which vinyl acetate is industrially preferred. These can be produced by various polymerization methods such as conventionally known bulk polymerization, solution polymerization, suspension polymerization, emulsion polymerization, etc., among which solution polymerization using an alcohol solvent such as methanol is industrially preferred.

[0194] In addition, the unsaturated monomer having an active carbonyl group is not particularly limited, but examples thereof include diacetone acrylamide, diacetone methacrylamide, diacetone acrylate, diacetone methacrylate, acetoacetoxy acrylamide, acetoacetoxy methacrylamide, etc. These may be used alone or in combination of two or more. Among them, diacetone acrylamide is industrially preferred, and as the copolymerized modified PVA, diacetone acrylamide modified PVA is preferred.

[0195] In the present invention, for the copolymerization of the fatty acid vinyl ester and the unsaturated monomer having an active carbonyl group, other unsaturated monomers copolymerizable with the fatty acid vinyl ester and the unsaturated monomer having an active carbonyl group may be used within a range that does not impair the effects of the present invention.

[0196] Examples of other unsaturated monomers include carboxyl group-containing unsaturated monomers [e.g., (meth)acrylic acid, maleic acid, maleic anhydride, fumaric acid, crotonic acid, itaconic acid, undecylenic acid, etc.], unsaturated dibasic acid monoalkyl esters (e.g., monomethyl maleate, monomethyl itaconate, etc.), amide group-containing unsaturated monomers (e.g., acrylamide, dimethylacrylamide, dimethylaminoethylacrylamide, diethylacrylamide, dimethylaminopropylacrylamide, isopropylacrylamide, N-methylolacrylamide, N-vinylacetamide, etc.), haloacrylamide, cycloacrylamide, cyclohexyl acrylate ... vinyl halides (e.g., vinyl chloride, vinyl fluoride, etc.), unsaturated monomers having a glycidyl group (e.g., allyl glycidyl ether, glycidyl methacrylate, etc.), lactam group-containing unsaturated monomers {e.g., N-vinylpyrrolidones [e.g., N-vinyl-2-pyrrolidone, N-vinyl-alkylpyrrolidone (e.g., N-vinyl-mono- or di-C such as N-vinyl-3-propyl-2-pyrrolidone, N-vinyl-5-methyl-2-pyrrolidone, N-vinyl-5-ethyl-2-pyrrolidone, N-vinyl-5,5-dimethyl-2-pyrrolidone, and N-vinyl-3,5-dimethyl-2-pyrrolidone, 1-4alkylpyrrolidones), N-allylpyrrolidones (e.g., N-allyl-2-pyrrolidone), N-vinylpiperidones [e.g., N-vinyl-2-piperidone, N-vinyl-alkylpiperidones (e.g., N-vinyl-6-methyl-2-piperidone, N-vinyl-6-ethyl-2-piperidone, and other N-vinyl-mono- or di-C 1-4 alkyl piperidones), N-vinyl caprolactams [e.g., N-vinyl-ε-caprolactam, N-vinyl-alkyl caprolactams (e.g., N-vinyl-mono- or di-C such as N-vinyl-7-methyl-2-caprolactam and N-vinyl-7-ethyl-2-caprolactam, etc. 1-4 alkyl caprolactams, etc.)]}, alkyl vinyl ethers [e.g., C 1―20 alkyl vinyl ethers (e.g., methyl vinyl ether, n-propyl vinyl ether, i-propyl vinyl ether, n-butyl vinyl ether, i-butyl vinyl ether, t-butyl vinyl ether, lauryl vinyl ether, dodecyl vinyl ether, stearyl vinyl ether, etc.), nitriles (e.g., acrylonitrile, methacrylonitrile, etc.), hydroxyl group-containing unsaturated monomers [e.g., C 1―20 Monoalkyl allyl alcohols (e.g., allyl alcohol, isopropenyl allyl alcohol, etc.), C 1―20 Dialkylallyl alcohol (e.g., dimethylallyl alcohol, etc.), hydroxy C 1―20 alkyl vinyl ethers (e.g., hydroxyethyl vinyl ether, hydroxybutyl vinyl ether, etc.)], acetyl group-containing unsaturated monomers [e.g., C 1―20 alkyl allyl acetates (e.g., allyl acetate, dimethyl allyl acetate, isopropenyl allyl acetate, etc.), (meth)acrylic acid esters {e.g., (meth)acrylic acid alkyl esters [e.g., (meth)acrylic acid C such as methyl (meth)acrylate, ethyl (meth)acrylate, 2-ethylhexyl acrylate, and n-butyl acrylate, etc. 1-20alkyl], etc.}, vinyl silanes (e.g., trimethoxyvinylsilane, tributylvinylsilane, diphenylmethylvinylsilane, etc.), polyoxyalkylene (meth)acrylates [e.g., polyoxyethylene (meth)acrylate, polyoxypropylene (meth)acrylate, etc.], polyoxyalkylene (meth)acrylic acid amides [e.g., polyoxyethylene (meth)acrylic acid amide, polyoxypropylene (meth)acrylic acid amide, etc.], polyoxyalkylene vinyl ethers (e.g., polyoxyethylene vinyl ether, polyoxypropylene vinyl ether, etc.), polyoxyalkylene alkyl vinyl ethers (e.g., polyoxyethylene allyl ether, polyoxypropylene allyl ether, polyoxyethylene butyl vinyl ether, polyoxypropylene butyl vinyl ether, etc.), α-olefins (e.g., ethylene, propylene, n-butene, 1-hexene, etc.), butenes (e.g., 3,4-dihydroxy-1-butene, 3,4-diacyloxy-1-butene, 3,4-dimethylamino ... -acyloxy-4-hydroxy-1-butene, 4-acyloxy-3-hydroxy-1-butene, 3,4-diacyloxy-2-methyl-1-butene, etc.), pentenes (e.g., 4,5-dihydroxy-1-pentene, 4,5-diacyloxy-1-pentene, 4,5-dihydroxy-3-methyl-1-pentene, 4,5-diacyloxy-3-methyl-1-pentene, etc.), hexenes (e.g., 5,6-dihydroxy-1-hexene, 5,6-diacyloxy-1-hexene, etc.), amine-based unsaturated monomers [e.g., N,N-dimethylallylamine, N-allylpropanol, 3-piperidine acrylic acid ethyl ester, 2-vinylpyridine, 4-vinylpyridine, 2-methyl-6-vinylpyridine, 5-ethyl-2-vinylpyridine, 5-butenylpyridine, 4-pentenylpyridine, 2-(4-pyridyl)allyl alcohol, etc.], unsaturated monomers having quaternary ammonium compounds (e.g., dimethylaminoethyl acrylate methyl chloride quaternary salt, N,N-dimethylaminopropylacrylamide methyl chloride quaternary salt, N,N-dimethylaminopropylacrylamidomethylbenzenesulfonic acid quaternary salt, etc.), aromatic unsaturated monomers (e.g., styrene, etc.), unsaturated monomers containing a sulfonic acid group (e.g., 2-acrylamido-2-methylpropanesulfonic acid or its alkali metal salt, ammonium salt, or organic amine salt; 2-acrylamido-1-methylpropanesulfonic acid or its alkali metal salt, ammonium salt, or organic amine salt; 2-methacrylamido-2-methylpropanesulfonic acid or its alkali metal salt, ammonium salt, or organic amine salt; vinylsulfonic acid or its alkali metal salt, ammonium salt, or organic amine salt; allylsulfonic acid or and methallylsulfonic acid or its alkali metal salt, ammonium salt or organic amine salt, etc.), glycerin monoallyl ether, 2,3-diacetoxy-1-allyloxypropane, 2-acetoxy-1-allyloxy-3-hydroxypropane, 3-acetoxy-1-allyloxy-3-hydroxypropane, 3-acetoxy-1-allyloxy-2-hydroxypropane, glycerin monovinyl ether, glycerin monoisopropenyl ether, acryloylmorpholine, vinyl ethylene carbonate, vinyl imidazole, vinyl carbazole, etc., may be mentioned.

[0197] The content of the other unsaturated monomer is not particularly limited, but may be, for example, 10 moles or less per 100 moles of the vinyl ester monomer.

[0198] In addition, the obtained copolymerized modified PVA may be post-modified by reactions such as acetalization, urethanization, etherification, grafting, phosphate esterification, acetoacetylation, and cationization using known methods within the scope of the invention.

[0199] The polymerization catalyst used in producing the copolymerized modified PVA is not particularly limited, but an azo compound or a peroxide is usually used. During the polymerization, an organic acid such as tartaric acid, citric acid, or acetic acid may be added for the purpose of preventing hydrolysis of the fatty acid vinyl ester. To terminate the polymerization, a polymerization terminator can be used, although it is not particularly limited. The polymerization terminator is not particularly limited, and examples thereof include m-dinitrobenzene.

[0200] In the present invention, when copolymerizing a fatty acid vinyl ester with an unsaturated monomer having an active carbonyl group, any of the shape of the polymerization vessel, the type of the polymerization stirrer, the polymerization temperature, the pressure inside the polymerization vessel, and the like may be selected from known methods.

[0201] In the present invention, the method for saponifying the copolymer of a fatty acid vinyl ester and an unsaturated monomer having an active carbonyl group is not particularly limited and may be according to a conventionally known method. For example, alcoholysis or hydrolysis using a conventionally known basic catalyst such as sodium hydroxide, potassium hydroxide, or sodium methoxide, or an acidic catalyst such as hydrochloric acid, sulfuric acid, or p-toluenesulfonic acid can be applied. Examples of the solvent used in the saponification reaction include alcohols such as methanol and ethanol, esters such as methyl acetate, ketones such as acetone and methyl ethyl ketone, aromatic hydrocarbons such as benzene and toluene, and tetrahydrofuran, which may be used alone or in combination of two or more. There are no particular limitations on the saponification temperature, time, etc. The methods for drying, pulverizing and washing the saponified product are not particularly limited, and known methods may be used.

[0202] When an unsaturated monomer having an active carbonyl group (e.g., diacetone acrylamide) modified PVA is used as the modified PVA resin, the content of the unsaturated monomer having an active carbonyl group (e.g., diacetone acrylamide) unit is, for example, 0.5 to 20 mol %, preferably 0.5 to 15 mol %, more preferably 1 to 12 mol %, and even more preferably 2 to 10 mol % (e.g., 3 to 8 mol %) relative to the total amount of the unsaturated monomer having an active carbonyl group (e.g., diacetone acrylamide) modified PVA (total amount of monomers). When the content of unsaturated monomer units having an active carbonyl group (e.g., diacetone acrylamide) is 0.5 mol % or more, there are many reaction sites with the crosslinker, and sufficient strength (stress) for a cell-embedded device can be obtained. On the other hand, when the content is 20 mol % or less, it is preferable from the viewpoint of improving solubility in water, etc.

[0203] The degree of saponification of the modified PVA resin is not particularly limited, but is preferably 80 mol % or more (e.g., 80 to 99.9 mol %), more preferably 88 mol % or more (e.g., 88 to 99.9 mol %), and even more preferably 95 mol % or more (e.g., 95 to 99.9 mol %).

[0204] The viscosity of the modified PVA resin may vary, but the viscosity of a 4% by mass aqueous solution of the modified PVA resin (20° C.) is preferably 2 to 500 mPa·s, more preferably 3 to 300 mPa·s, and further preferably 5 to 200 mPa·s (e.g., 5 to 80 mPa·s), and is typically 500 mPa·s or less (e.g., 20 to 500 mPa·s, 30 to 500 The viscosity may be 300 mPa·s or less (for example, 20 to 300 mPa·s, 30 to 300 mPa·s, 40 to 300 mPa·s, 50 to 300 mPa·s, etc.), 200 mPa·s or less (for example, 20 to 200 mPa·s, 30 to 200 mPa·s, 40 to 200 mPa·s, 50 to 200 mPa·s), etc. The above saponification degree and 4 mass % aqueous solution viscosity may be values ​​measured according to JIS K-6726.

[0205] (Polyvinyl alcohol resin with a syndiotacticity of 32-40% in triad format) As the polyvinyl alcohol resin, a polyvinyl alcohol-based resin having a syndiotacticity of 32 to 40% expressed in triads (also referred to simply as a "high syndiotactic PVA-based resin" in this specification) can also be preferably used. The syndiotacticity of the high-syndiotactic PVA resin is preferably 32 to 40%, more preferably 33 to 39%, and particularly preferably 34 to 38%, in terms of triads. If the syndiotacticity is 32% or more, it is easy to form an aqueous gel, and if it is 40% or less, it is easy to prepare an aqueous gel. The syndiotacticity indicated by triads can be determined by dissolving a high syndiotactic PVA resin in deuterated DMSO (dimethyl sulfoxide) and measuring the hydroxyl group peak by proton NMR.

[0206] The method for producing the high syndio PVA resin is not particularly limited as long as the syndiotacticity, as expressed by triads, is 32 to 40%, but the resin can be easily obtained by saponifying a vinyl ester polymer obtained by a conventional method. That is, the high-syndio PVA resin is a saponification product of a vinyl ester polymer. The method for producing the vinyl ester polymer is not particularly limited as long as it is a method for polymerizing a vinyl ester monomer, and may be any method known in the art. In the polymerization, any of the known methods may be used with respect to the shape of the polymerization vessel, the type of the polymerization agitator, the polymerization temperature, the pressure inside the polymerization vessel, etc. As the polymerization method, various polymerization methods such as conventionally known bulk polymerization, solution polymerization, suspension polymerization, emulsion polymerization, etc. are possible. Considering the control of the polymerization degree and the saponification reaction performed after polymerization, solution polymerization using alcohol as a solvent, or suspension polymerization using water or water and alcohol as a dispersion medium is preferable, but is not limited thereto.

[0207] Examples of vinyl ester monomers include vinyl esters such as fatty acid vinyl esters and non-fatty acid vinyl esters (e.g., vinyl formate, aromatic carboxylic acid vinyl esters, etc.). From the viewpoint of obtaining a PVA with high syndiotacticity, C 3-15 Fatty acid vinyl esters [e.g., straight-chain or branched-chain C vinyl esters such as vinyl propionate, vinyl butyrate, vinyl pivalate, etc. 3-15 Fatty acid vinyl esters, preferably C 3-10Fatty acid vinyl esters (e.g., linear or branched C 3-10 fatty acid vinyl esters, etc.], C having a substituent (e.g., a halogen group) 3-15 Examples of the vinyl ester include fatty acid vinyl esters [for example, vinyl trifluoroacetate, vinyl trichloroacetate, etc.], vinyl formate, etc. These vinyl esters may be used alone or in combination of two or more.

[0208] Specifically, examples of methods for producing high syndiotactic PVA resins include a method of homopolymerizing or copolymerizing a vinyl ester having a bulky side chain, such as vinyl propionate, vinyl butyrate, or vinyl pivalate, and then saponifying the resulting product with an alkaline catalyst, and a method of homopolymerizing or copolymerizing a highly polar vinyl ester, such as vinyl formate, vinyl trifluoroacetate, or vinyl trichloroacetate, and then saponifying the resulting product with an alkaline catalyst. Among these, a method of polymerizing vinyl pivalate and then saponifying the resulting product with an alkaline catalyst is preferably used. In the following examples, a production example is described in which the syndiotacticity represented by triads is 37.1%. The syndiotacticity represented by triads can be reduced to less than 37.1% by, for example, coexisting vinyl acetate during polymerization of vinyl pivalate to obtain a copolymer of vinyl pivalate and vinyl acetate, or by increasing the polymerization temperature. The syndiotacticity represented by triads can be increased to more than 37.1% by, for example, lowering the polymerization temperature in the above production examples. In either case, the resulting high-syndiotolin PVA resin can be dissolved in deuterated DMSO and the content can be determined from the hydroxyl group peak by proton NMR measurement, and one in the range of 32 to 40% can be appropriately selected and used in the present invention.

[0209] In addition to the above-mentioned vinyl ester, the vinyl ester polymer may contain other unsaturated monomers copolymerizable with the vinyl ester, as long as the effects of the present invention are not impaired. Examples of other unsaturated monomers include carboxyl group-containing unsaturated monomers [e.g., (meth)acrylic acid, maleic acid, maleic anhydride, fumaric acid, crotonic acid, itaconic acid, undecylenic acid, etc.], unsaturated dibasic acid monoalkyl esters (e.g., monomethyl maleate, monomethyl itaconate, etc.), amide group-containing unsaturated monomers (e.g., acrylamide, dimethylacrylamide, dimethylaminoethylacrylamide, diethylacrylamide, dimethylaminopropylacrylamide, isopropylacrylamide, N-methylolacrylamide, N-vinylacetamide, etc.), haloacrylamide, cycloacrylamide, cyclohexyl acrylate ... vinyl halides (e.g., vinyl chloride, vinyl fluoride, etc.), unsaturated monomers having a glycidyl group (e.g., allyl glycidyl ether, glycidyl methacrylate, etc.), lactam group-containing unsaturated monomers {e.g., N-vinylpyrrolidones [e.g., N-vinyl-2-pyrrolidone, N-vinyl-alkylpyrrolidone (e.g., N-vinyl-mono- or di-C such as N-vinyl-3-propyl-2-pyrrolidone, N-vinyl-5-methyl-2-pyrrolidone, N-vinyl-5-ethyl-2-pyrrolidone, N-vinyl-5,5-dimethyl-2-pyrrolidone, and N-vinyl-3,5-dimethyl-2-pyrrolidone, 1-4 alkylpyrrolidones), N-allylpyrrolidones (e.g., N-allyl-2-pyrrolidone), N-vinylpiperidones [e.g., N-vinyl-2-piperidone, N-vinyl-alkylpiperidones (e.g., N-vinyl-6-methyl-2-piperidone, N-vinyl-6-ethyl-2-piperidone, and other N-vinyl-mono- or di-C 1-4 alkyl piperidones), N-vinyl caprolactams [e.g., N-vinyl-ε-caprolactam, N-vinyl-alkyl caprolactams (e.g., N-vinyl-mono- or di-C such as N-vinyl-7-methyl-2-caprolactam and N-vinyl-7-ethyl-2-caprolactam, etc. 1-4 alkyl caprolactams, etc.)]}, alkyl vinyl ethers [e.g., C 1―20alkyl vinyl ethers (e.g., methyl vinyl ether, n-propyl vinyl ether, i-propyl vinyl ether, n-butyl vinyl ether, i-butyl vinyl ether, t-butyl vinyl ether, lauryl vinyl ether, dodecyl vinyl ether, stearyl vinyl ether, etc.), nitriles (e.g., acrylonitrile, methacrylonitrile, etc.), hydroxyl group-containing unsaturated monomers [e.g., C 1―20 Monoalkyl allyl alcohols (e.g., allyl alcohol, isopropenyl allyl alcohol, etc.), C 1―20 Dialkylallyl alcohol (e.g., dimethylallyl alcohol, etc.), hydroxy C 1―20 alkyl vinyl ethers (e.g., hydroxyethyl vinyl ether, hydroxybutyl vinyl ether, etc.)], acetyl group-containing unsaturated monomers [e.g., C 1―20 alkyl allyl acetates (e.g., allyl acetate, dimethyl allyl acetate, isopropenyl allyl acetate, etc.), (meth)acrylic acid esters {e.g., (meth)acrylic acid alkyl esters [e.g., (meth)acrylic acid C such as methyl (meth)acrylate, ethyl (meth)acrylate, 2-ethylhexyl acrylate, and n-butyl acrylate, etc. 1-20alkyl], etc.}, vinyl silanes (e.g., trimethoxyvinylsilane, tributylvinylsilane, diphenylmethylvinylsilane, etc.), polyoxyalkylene (meth)acrylates [e.g., polyoxyethylene (meth)acrylate, polyoxypropylene (meth)acrylate, etc.], polyoxyalkylene (meth)acrylic acid amides [e.g., polyoxyethylene (meth)acrylic acid amide, polyoxypropylene (meth)acrylic acid amide, etc.], polyoxyalkylene vinyl ethers (e.g., polyoxyethylene vinyl ether, polyoxypropylene vinyl ether, etc.), polyoxyalkylene alkyl vinyl ethers (e.g., polyoxyethylene allyl ether, polyoxypropylene allyl ether, polyoxyethylene butyl vinyl ether, polyoxypropylene butyl vinyl ether, etc.), α-olefins (e.g., ethylene, propylene, n-butene, 1-hexene, etc.), butenes (e.g., 3,4-dihydroxy-1-butene, 3,4-diacyloxy-1-butene, 3,4-dimethylamino ... -acyloxy-4-hydroxy-1-butene, 4-acyloxy-3-hydroxy-1-butene, 3,4-diacyloxy-2-methyl-1-butene, etc.), pentenes (e.g., 4,5-dihydroxy-1-pentene, 4,5-diacyloxy-1-pentene, 4,5-dihydroxy-3-methyl-1-pentene, 4,5-diacyloxy-3-methyl-1-pentene, etc.), hexenes (e.g., 5,6-dihydroxy-1-hexene, 5,6-diacyloxy-1-hexene, etc.), amine-based unsaturated monomers [e.g., N,N-dimethylallylamine, N-allylpropanol, 3-piperidine acrylic acid ethyl ester, 2-vinylpyridine, 4-vinylpyridine, 2-methyl-6-vinylpyridine, 5-ethyl-2-vinylpyridine, 5-butenylpyridine, 4-pentenylpyridine, 2-(4-pyridyl)allyl alcohol, etc.], unsaturated monomers having quaternary ammonium compounds (e.g., dimethylaminoethyl acrylate methyl chloride quaternary salt, N,N-dimethylaminopropylacrylamide methyl chloride quaternary salt, N,N-dimethylaminopropylacrylamidomethylbenzenesulfonic acid quaternary salt, etc.), aromatic unsaturated monomers (e.g., styrene, etc.), unsaturated monomers containing a sulfonic acid group (e.g., 2-acrylamido-2-methylpropanesulfonic acid or its alkali metal salt, ammonium salt, or organic amine salt; 2-acrylamido-1-methylpropanesulfonic acid or its alkali metal salt, ammonium salt, or organic amine salt; 2-methacrylamido-2-methylpropanesulfonic acid or its alkali metal salt, ammonium salt, or organic amine salt; vinylsulfonic acid or its alkali metal salt, ammonium salt, or organic amine salt; allylsulfonic acid or and methallylsulfonic acid or its alkali metal salt, ammonium salt or organic amine salt, etc.), glycerin monoallyl ether, 2,3-diacetoxy-1-allyloxypropane, 2-acetoxy-1-allyloxy-3-hydroxypropane, 3-acetoxy-1-allyloxy-3-hydroxypropane, 3-acetoxy-1-allyloxy-2-hydroxypropane, glycerin monovinyl ether, glycerin monoisopropenyl ether, acryloylmorpholine, vinyl ethylene carbonate, vinyl imidazole, vinyl carbazole, etc., may be mentioned. The content of the other unsaturated monomer is not particularly limited, but may be, for example, 10 moles or less per 100 moles of the vinyl ester monomer.

[0210] In addition, a polymerization catalyst can be used during the polymerization. The polymerization catalyst is not particularly limited, but an azo compound or a peroxide is usually used. During the polymerization, an organic acid such as tartaric acid, citric acid, or acetic acid may be added for the purpose of preventing hydrolysis of the fatty acid vinyl ester.

[0211] To terminate the polymerization, a polymerization terminator can be used, although it is not particularly limited. The polymerization terminator is not particularly limited, and examples thereof include m-dinitrobenzene.

[0212] The polymerization temperature is not particularly limited and may be any known polymerization temperature. From the viewpoint of easily obtaining a PVA-based resin with high syndiotacticity, the polymerization temperature is, for example, −50 to 200° C., preferably −50 to 150° C., and more preferably 0 to 120° C.

[0213] A vinyl ester polymer is obtained in the manner described above. The saponification reaction method of the obtained polymer is not particularly limited and may be according to a conventionally known method, for example, alcoholysis or hydrolysis using a conventionally known basic catalyst such as sodium hydroxide, potassium hydroxide, or sodium methoxide, or an acidic catalyst such as hydrochloric acid, sulfuric acid, or p-toluenesulfonic acid can be applied. Note that the syndiotacticity of the polymer usually does not change much before and after the saponification reaction. Examples of the solvent used in the saponification reaction include alcohols such as methanol and ethanol, esters such as methyl acetate and ethyl acetate, ketones such as acetone and methyl ethyl ketone, aromatic hydrocarbons such as benzene and toluene, and tetrahydrofuran, which may be used alone or in combination of two or more. There are no particular limitations on the saponification temperature, time, etc. The methods for drying, pulverizing and washing the saponified product are not particularly limited, and known methods may be used.

[0214] Thus, a saponification product of the vinyl ester polymer, i.e., the high-syndio PVA resin of the present invention, is obtained. The obtained high-syndio PVA resin may be post-modified by a known method such as acetalization, urethanization, etherification, grafting, phosphate esterification, acetoacetylation, cationization, etc., within the scope of not impairing the effects of the present invention.

[0215] The saponification degree of the high-Syndio PVA resin is preferably 90 to 99.9 mol%, more preferably 98 to 99.9 mol%, and further preferably 99 to 99.9 mol%. The saponification degree of the high-Syndio PVA resin can be determined, for example, by measuring proton NMR in a deuterated DMSO solution.

[0216] The degree of polymerization of the high-syndio PVA resin is preferably 100 to 10,000, more preferably 500 to 8,000, and even more preferably 1,000 to 5,000, and is particularly preferably 1,000 to 3,000 in terms of relatively easy handling. If the degree of polymerization is 100 or more, the resin strength (stress) is high, and an aqueous gel with shape retention is easily produced. If the degree of polymerization is 10,000 or less, the aqueous solution is easy to handle. The degree of polymerization is the degree of polymerization of the resin before saponification, calculated as polyvinyl acetate in a benzene solution at 30°C as described in JIS K6725.

[0217] (Polyvinyl alcohol resin with a degree of saponification of 97 mol% or more) As the polyvinyl alcohol-based resin, as described above, a polyvinyl alcohol-based resin having a degree of saponification of 97 mol % or more (also referred to simply as a "fully saponified PVA-based resin" in this specification) can also be used.

[0218] The degree of saponification of the fully saponified PVA resin is preferably 97 mol % or more (for example, 97 to 99.9 mol %), more preferably 98 mol % or more (for example, 98 to 99.9 mol %), and particularly preferably 98.5 mol % or more (for example, 98.5 to 99.9 mol %).

[0219] The degree of polymerization of the fully saponified PVA resin is, for example, 100 to 10,000, more preferably 500 to 9,000, further preferably 1,000 to 8,000, and particularly preferably 1,500 to 5,000.

[0220] (Crosslinking agent) The cell-embedded device (the polymer that constitutes the cell-embedded device) may further contain a crosslinking agent. The crosslinking agent is not particularly limited and can be selected depending on the type of polymer, etc. For example, when the modified PVA resin is used as the polymer, a crosslinking agent having a functional group (e.g., a hydrazino group, etc.) reactive with the carbonyl group of the modified PVA resin may be suitable.

[0221] Examples of the crosslinking agent include hydrazide compounds, semicarbazide compounds, etc. Among them, preferred are hydrazide compounds and semicarbazide compounds having two or more functional groups in the molecule selected from the group represented by the following formulas (1) to (3). These can be used alone or in combination of two or more. -NH-NH2(1) -CO-NH-NH2(2) -NH-CO-NH-NH2(3)

[0222] Specific examples of the hydrazide compound include carbohydrazide, dicarboxylic acid hydrazide [fatty acid dicarboxylic acid hydrazide (e.g., oxalic acid dihydrazide, malonic acid dihydrazide, succinic acid dihydrazide, glutaric acid dihydrazide, adipic acid dihydrazide, pimelic acid dihydrazide, suberic acid dihydrazide, azelaic acid dihydrazide, sebacic acid dihydrazide, dodecanedioic acid dihydrazide, hexadecanedioic acid dihydrazide, etc.), aromatic dicarboxylic acid hydrazide (e.g., terephthalic acid dihydrazide, isophthalic acid dihydrazide, 2,6-naphthoic acid dihydrazide, 4,4'-bisbenzene dihydrazide, etc.), alicyclic dicarboxylic acid hydrazide (e.g., 1,4-cyclohexanedicarboxylic acid dihydrazide, hydrazide, etc.), hydroxyl group-containing dicarboxylic acid dihydrazide (for example, tartaric acid dihydrazide, malic acid dihydrazide, etc.), iminodiacetic acid dihydrazide, itaconic acid dihydrazide, etc.), 1,3-bis(hydrazinocarbonoethyl)-5-isopropylhydantoin, 7,11-octadecadiene-1,18-dicarbohydrazide, tris(2-hydrazinocarbonylethyl)isocyanurate, citric acid trihydrazide, butane tricarbohydrazide, 1,2,3-benzene trihydrazide, ethylenediaminetetraacetic acid tetrahydrazide, 1,4,5,8-naphthoic acid tetrahydrazide, nitriloacetic acid trihydrazide, cyclohexane tricarboxylic acid trihydrazide, pyromellitic acid tetrahydrazide, etc. Examples of the semicarbazide compound include N,N'-hexamethylenebissemicarbazide, biurettri(hexamethylenesemicarbazide), and the like. In addition, derivatives obtained by reacting these hydrazide compounds and semicarbazide compounds with low boiling point ketones such as acetone and methyl ethyl ketone may also be used.

[0223] Among the above crosslinking agents, preferably dicarboxylic acid hydrazide, polyacrylic acid hydrazide, etc., more preferably adipic acid dihydrazide, polyacrylic acid hydrazide, etc., and particularly preferably polyacrylic acid hydrazide, can be suitably used from the viewpoints of low toxicity, high solubility in water, etc.

[0224] The crosslinking agent may be one of the above crosslinking agents or a combination of two or more of them. The amount of the crosslinking agent added is preferably 1 to 30 parts by mass, more preferably 2 to 25 parts by mass, and even more preferably 3 to 20 parts by mass (eg, 4 to 15 parts by mass) relative to 100 parts by mass of the polymer (eg, modified PVA-based resin). An amount of 1 part by mass or more increases the crosslinking density, making it possible to obtain sufficient strength (stress) as a cell-embedded device, while an amount of 30 parts by mass or less is preferable from the viewpoint of suppressing the residue of crosslinking agent that does not contribute to the reaction.

[0225] When polyacrylic hydrazide is used as the crosslinking agent, the molecular weight range is not particularly limited, but the weight average molecular weight (Mw) of the polyacrylic hydrazide is preferably about 3,000 to 6,000,000, preferably about 5,000 to 1,000,000, and more preferably about 8,000 to 800,000 (for example, about 10,000 to 300,000, about 1,000 to 200,000, or about 10,000 to 100,000).

[0226] When polyacrylic hydrazide is used as the crosslinking agent, the hydrazide ratio of polyacrylic hydrazide is not particularly limited, but is preferably 30% or more, more preferably 50% or more, further preferably 70% or more, and particularly preferably 80% or more.

[0227] The molecular weight and hydrazide ratio of polyacrylic acid hydrazide may be appropriately adjusted within a range that does not impair the effects of the present invention, for example, by increasing the hydrazide ratio when the molecular weight is small and decreasing the hydrazide ratio when the molecular weight is large.

[0228] In the cell-embedded device, the polyvinyl alcohol-based resin may particularly form a gel [particularly an aqueous gel (hydrogel)] or a sponge.

[0229] When a gel is formed, depending on the type of polymer, the polymer may be crosslinked (gel crosslinked) using, for example, a crosslinking agent described below, or the gel may be formed using a gel-forming polymer (for example, the high-syndiotopan PVA resin described above).

[0230] In the gel, the polymer concentration may be, for example, 0.3 to 20%, preferably 0.5 to 10%, more preferably 1 to 8% (e.g., 3 to 8%). Such a range is preferable from the viewpoint of being able to maintain the shape of the device in the body for a long period of time after implantation of the film-forming device in an animal.

[0231] Furthermore, when a crosslinking agent is used in the gel, the content of the crosslinking agent can be appropriately selected depending on the type of crosslinking agent, the desired strength, etc., and may be, for example, 0.5 parts by mass or more, preferably 1 part by mass or more, and more preferably 3 parts by mass or more, relative to 100 parts by mass of the polymer, or 20 parts by mass or less, preferably 18 parts by mass or less, and more preferably 15 parts by mass or less.

[0232] When forming a gel from a polyvinyl alcohol-based resin in this manner, examples of methods for molding (forming) the gel include a method in which a mixed liquid [particularly, an aqueous solution (which may be in a sol state)] containing a polymer [e.g., a polyvinyl alcohol-based resin and, if desired, a crosslinking agent, etc.] is poured into a mold of the desired shape before gelling, and a method in which the obtained gel is processed into the desired shape with a knife or the like.

[0233] Generally, a mixed liquid (particularly an aqueous solution) containing a polymer (e.g., a polyvinyl alcohol resin, and optionally a crosslinking agent, etc.) passes through a sol state before reaching a gel state. Such a sol state is also understood to be within the scope of the present invention as a gel equivalent of the present invention.

[0234] The solid content of the mixed liquid [particularly an aqueous solution (which may be in a sol state)] is, for example, 0.3 to 20% by mass, preferably 0.5 to 10% by mass, and more preferably 1 to 8% by mass. This range is preferable from the viewpoints of maintaining the device shape in the body for a long period of time and maintaining adhesion prevention ability.

[0235] In particular, when preparing an aqueous solution containing a polyvinyl alcohol-based resin, the preparation method is not particularly limited, but for example, the resin can be dispersed in water at room temperature, heated to 80°C or higher while stirring, completely dissolved, and then cooled according to a conventionally known method for dissolving PVA.

[0236] The crosslinking agent may be used as an aqueous solution. In this case, the method for preparing the aqueous solution of the crosslinking agent is not particularly limited, but for example, the crosslinking agent may be dispersed in water at room temperature, stirred and dissolved at room temperature, or stirred and dissolved under heating (for example, at 60°C for 10 minutes, etc.), and then allowed to stand at room temperature.

[0237] In addition, the aqueous solution of the polyvinyl alcohol resin and the aqueous solution of the crosslinking agent are desirably sterilized by a conventionally known method such as autoclaving, UV, gamma ray, or filtration, and during mixing with the biological composition or the subsequent production of the cell-embedded device, it is desirably worked on and stored in an environment that prevents the introduction of germs.

[0238] When forming a sponge, for example, a method in which a pore-forming agent is added during the production of the gel, or a method in which pores are formed by drying (for example, freeze-drying) the obtained gel is suitably used.

[0239] As the pore-forming agent, a water-soluble polymer, a water-soluble inorganic substance, an organic solvent, etc. can be used. Among them, starch is preferably used.

[0240] When starch is used as a pore-forming agent, a cross-linking agent (e.g., formalin) is added to an aqueous solution containing a polyvinyl alcohol-based resin and starch, the polyvinyl alcohol-based resin is gelled, and then the starch is washed with water to form a sponge.

[0241] When a pore-forming agent is used to form the sponge, a drying treatment may be carried out after the sponge is formed.

[0242] The cell-containing device may contain cell culture components. Examples of cell culture components include, but are not limited to, alkali metals, alkaline earth metals, halogens, glucose, etc., and among these, acetate or phosphate buffer solutions containing Na, K, Cl, Ca, glucose, etc. are preferably used.

[0243] When the cell culture components contain Na, the Na concentration may be adjusted to preferably 20 to 150 mEq / L, more preferably 80 to 140 mEq / L. When K is contained, the K concentration may be adjusted to preferably 2.5 to 130 mEq / L, more preferably 3.5 to 40 mEq / L. When Cl is contained, the Cl concentration may be adjusted to preferably 15 to 170 mEq / L, more preferably 100 to 150 mEq / L. When Ca is contained, the Ca concentration may be adjusted to preferably 0.5 to 5 mEq / L, more preferably 1 to 3 mEq / L. When glucose is contained, the glucose concentration may be adjusted to preferably 1 to 11 mM, more preferably 3 to 7 mM.

[0244] Examples of cell culture components include, but are not limited to, known cell culture media (e.g., Hank's balanced salt solution (HBSS)), commercially available preservation solutions (e.g., Euro-Collins solution, Cellbanker, UW solution (University of Wisconsin solution)), cell protective components (e.g., dimethyl sulfoxide (DMSO), serum albumin, etc.), components that prevent the infiltration of unwanted bacteria (e.g., antibiotics, etc.), components that maintain cell activity (e.g., vitamins such as nicotinamide, etc.), and the like. Preferred are known cell culture media, etc.

[0245] These can be used alone or in combination of two or more.

[0246] The cell culture components may also be used in combination with other components (eg, sustained release agents, tonicity agents, pH adjusters, etc.).

[0247] The cell-containing device may further contain other components than those mentioned above. For example, the cell-containing device may contain growth factors (cell growth factors), cytokines, other physiologically active substances, blood flow promoting substances, neurotrophic factors, etc.

[0248] These can be used alone or in combination of two or more.

[0249] Examples of the growth factor (cell growth factor) include the above-mentioned growth factors such as epidermal growth factor (EGF), hepatocyte growth factor (HGF), and insulin.

[0250] Examples of cytokines include hematopoietic factors (eg, interleukins, chemokines, colony-stimulating factors, etc.), tumor necrosis factors, interferons, etc.

[0251] Other physiologically active substances include, for example, amino acids (eg, glycine, phenylalanine, lysine, aspartic acid, glutamic acid, etc.), vitamins (eg, biotin, pantothenic acid, vitamin D, etc.), serum albumin, antibiotics, etc.

[0252] Examples of blood flow promoters include citrulline or a salt thereof, capsaicin, and capsaicinoids.

[0253] Examples of neurotrophic factors include NGF (nerve growth factor), BDNF (brain-derived neurotrophic factor), NT-3 (neurotrophin-3), NT-4 (neurotrophin-4), GDNF (Glial-Cell Derived Neurtrophic Factor), neurturin, artemin, and persephin.

[0254] The amounts of these components added are not particularly limited.

[0255] The cell-containing device (cell-embedded device) may form a gel.

[0256] Such gels usually have a certain strength (stress). Such strength may be a stress that does not easily collapse when transplanted. The strength of the gel cannot be generally stated because it varies depending on the type of polymer (e.g., type of polyvinyl alcohol resin, 4% aqueous solution viscosity, degree of saponification, degree of modification, syndiotacticity, etc.), type of crosslinker, amount added, solids concentration of the gel, etc., but may be, for example, a stress (20°C) of 0.5 to 100 kPa, preferably 0.6 to 95 kPa, more preferably 0.7 to 90 kPa, and even more preferably 0.7 to 85 kPa.

[0257] The stress of the gel can be measured, for example, using a small tabletop tester EZTest EZ-SX manufactured by Shimadzu Corporation, following the instructions for use.

[0258] The shape of the gel (particularly the aqueous gel) is not particularly limited, and examples thereof include a sheet shape, a plate shape, a disc shape, a rod shape, a tube shape, a bead shape, and the like.

[0259] The size of the gel (particularly the aqueous gel) can be appropriately selected depending on the transplant site and its size, and is not particularly limited. For example, the thickness is preferably 0.1 to 10 mm, more preferably 0.2 to 5 mm, even more preferably 0.5 to 2 mm, and particularly preferably 0.7 to 1.5 mm.

[0260] The cell-containing device may contain a support substrate. In particular, a gel (eg, a gel constituting a scaffold) may be combined with a supporting base material useful as a reinforcing material for the purpose of reinforcing it and / or simplifying its handling.

[0261] For example, when a gel (particularly an aqueous gel) is formed into a thin sheet, the gel may be fixed to a base material (reinforcing material) such as a resin mesh sheet for reinforcement and ease of handling.

[0262] The material of the support substrate is not limited, but examples include polymers [e.g., PET (polyethylene terephthalate), PE (polyethylene), PP (polypropylene), Teflon (registered trademark), etc.] and metals. It is preferable that the material does not decompose or change in quality in the body, but it may be one that decomposes in the body after a certain period of time.

[0263] The mesh (mesh) size of the mesh sheet is usually 5 to 100 nm, preferably 10 to 50 nm, and more preferably 20 to 30 nm, so as to allow the passage of oxygen, inorganic and organic nutrients, and various hormones that are assumed to have the largest diameter of about 5 nm (e.g., physiologically active substances including hormones such as insulin) and to prevent the passage of immune-related cells and immune-related substances that are assumed to have the smallest diameter of about 50 nm (e.g., antibodies, complement, etc.).

[0264] The cell-containing device (cell-embedded device) may have, for example, an immunoisolation layer containing a polymer [e.g., a polyvinyl alcohol-based resin (A)]. In other words, in the cell-containing device, the polymer (the polymer that has formed a gel) may constitute the immunoisolation layer (or have an immunoisolation function).

[0265] The immune isolation layer (immune isolation function) refers to a layer (function) that is permeable to, for example, glucose; hormones such as insulin, thyroid-stimulating hormone, thyroid hormone, parathyroid hormone, growth hormone, thyroxine, glucocorticoids, glucagon, estradiol, or testosterone; proteins such as blood clotting factors, albumin, globulin, and various enzymes (metabolic enzymes or digestive enzymes such as amylase, protease, or lipase); and neurotransmitters such as dopamine, but is not permeable to immune system proteins such as antibodies, complement, or white blood cells.

[0266] The cell-containing device (cell-embedded device) may be, for example, a bioartificial organ.

[0267] A cell-containing device (cell-embedded device) can be produced, for example, by the coexistence (presence) of a biological composition and a polymer (and possibly other components).

[0268] Specifically, the composition can be produced by a conventional method depending on the type, form, and existence form of each component.

[0269] For example, it is preferable to gel a mixture containing a polymer (and other components).

[0270] When forming a gel from a polymer in this manner, examples of methods for molding (forming) the gel include a method in which a mixed liquid [particularly, an aqueous solution (which may be in a sol state)] containing a polymer [e.g., a polyvinyl alcohol-based resin, and optionally a biological composition, a crosslinking agent, a cell culture component, etc.] is poured into a mold of the desired shape before gelling, and a method in which the obtained gel is processed into the desired shape with a knife or the like.

[0271] Generally, a mixed solution (particularly an aqueous solution) containing a polymer (e.g., a polyvinyl alcohol resin, and optionally a biological composition, a crosslinking agent, a cell culture component, etc.) passes through a sol state before reaching a gel state. Such a sol state is also understood to be within the scope of the present invention as a gel equivalent of the present invention.

[0272] The solid content of the mixed liquid [particularly an aqueous solution (which may be in a sol state)] is, for example, 0.3 to 20% by mass, preferably 0.5 to 10% by mass, and more preferably 1 to 8% by mass. This range is preferable from the viewpoint of maintaining the shape of the cell-embedded device in the body for a long period of time after implantation and maintaining adhesion prevention ability.

[0273] The mixed solution may be prepared by mixing each component simultaneously, or by first preparing a mixed solution (e.g., an aqueous solution of a polyvinyl alcohol resin) containing a polymer (and a crosslinking agent or cell culture components, if necessary) and then mixing the biological composition.

[0274] Additionally, other components may be mixed with the biological composition and / or cell culture components together or separately.

[0275] In particular, when preparing an aqueous solution containing a polyvinyl alcohol-based resin, the preparation method is not particularly limited, but for example, the resin can be dispersed in water at room temperature, heated to 80°C or higher while stirring, completely dissolved, and then cooled according to a conventionally known method for dissolving PVA.

[0276] The crosslinking agent may be used as an aqueous solution. In this case, the method for preparing the aqueous solution of the crosslinking agent is not particularly limited, but for example, the crosslinking agent may be dispersed in water at room temperature, stirred and dissolved at room temperature, or stirred and dissolved under heating (for example, at 60°C for 10 minutes, etc.), and then allowed to stand at room temperature.

[0277] In addition, the aqueous solution of the polyvinyl alcohol resin and the aqueous solution of the crosslinking agent are desirably sterilized by a conventionally known method such as autoclaving, UV, gamma ray, or filter treatment, and during mixing with the biological composition or the subsequent production of the cell-containing device, it is desirable to work with and store the solution in an environment that prevents the introduction of germs.

[0278] In producing a cell-embedded device, the mixture (or the aqueous solution thereof) of the aqueous solution of the polyvinyl alcohol resin and the crosslinking agent (in a state where a biological composition and / or cell culture components are mixed, if necessary) may be left to stand. The storage temperature may be a temperature suitable for storing the biological composition.

[0279] The time for leaving the gel (time for gelation, gelation time) when preparing the gel can be appropriately selected depending on the concentration of the polymer (polyvinyl alcohol resin, etc.), the amount of crosslinking agent, the leaving temperature, etc., but is usually about 1 hour to 1 week at room temperature. If it is 1 hour or more, it is preferable from the viewpoint that the cell-embedded device does not easily collapse when indwelled in the body.

[0280] When using a modified PVA-based resin to prepare a cell-embedded device, adding a pH buffer solution or the like to a mixture of the modified PVA-based resin and crosslinker (and further mixing with MSCs and / or cell culture components as necessary) to lower the pH of the system tends to shorten the gelation time, whereas increasing the pH tends to lengthen the gelation time; therefore, the gelation time can be controlled by changing the pH.

[0281] An example of the production of a cell-containing (embedded) device using a support substrate is shown below. A polymer mixture or its gel (e.g., a polyvinyl alcohol-based resin-containing aqueous solution or aqueous gel) containing cell culture components is placed on a substrate or base (such as a glass slide), and a support base such as a PET mesh (e.g., Sanplatic Co., Ltd., product name: PET mesh sheet (designation TN120), etc.) is placed on the substrate, and a mixture (dissolution or dispersion (suspension)) obtained by dissolving or dispersing (suspending) a biological composition in the polymer mixture or its gel (e.g., a polyvinyl alcohol-based resin-containing aqueous solution or aqueous gel) is placed on the support base, and the mixture is spread on the support base using a gel loading tip or the like, and a support base (such as a PET mesh) is further placed on top of the mixture so as to sandwich the mixture. Further, a polymer mixture or its gel (e.g., a polyvinyl alcohol-based resin-containing aqueous solution or aqueous gel) containing cell culture components is placed on the support base (such as a glass slide), and the substrate or base (such as a glass slide) is placed on top of the substrate to construct the device. By separating (removing) the substrate or base (such as a glass slide) from the substrate, a cell-containing device of one embodiment can be obtained.

[0282] As described above, the present invention also includes a transplantation method (a method for transplanting a cell-containing device). In such a transplantation method, as described above, a cell-containing device is transplanted to the transplantation site (removal site) after transplantation of the device 1 (and further removal of at least the non-bioabsorbable material). According to such a transplantation method, various diseases or symptoms can be prevented or ameliorated according to the biological composition (cells or tissue). Therefore, the present invention also includes a method for preventing and / or treating (ameliorating) such diseases or symptoms.

[0283] In such a method, a cell-containing device is implanted after implantation of the device 1 (and further after removal of at least the non-bioabsorbable material), although of course the method may also include a step of implanting (placing) the device 1 prior to such implantation.

[0284] Examples of symptoms or diseases include endocrine diseases (e.g., thyroid diseases, parathyroid diseases, adrenal diseases, pituitary diseases, pineal diseases, etc.), metabolic diseases (e.g., ornithine transcarbamylase deficiency, hyperammonemia, hypercholesterolemia, homocystinuria, glycogen storage diseases, Crigler-Nager syndrome, etc., Wilson's disease), diabetes (e.g., type 1 diabetes, type 2 diabetes, pancreatic diabetes, etc.), neurodegenerative diseases (e.g., Parkinson's disease, Alzheimer's disease, amyotrophic lateral sclerosis, spinocerebellar degeneration, etc.), hemophilia, bone diseases (e.g., osteoporosis), cancer (e.g., leukemia, etc.), etc.

[0285] The implantation (retention) period of the cell-containing device is not particularly limited, and may be, for example, 10 days or more, 1 month or more, 2 months or more, 3 months or more, 6 months or more, or 1 year or more.

[0286] As described above, the device 1 of the present invention can be suitably used in combination with a cell-containing device. Therefore, the present invention also includes a combined device (kit, device, combination) including the device 1 and a cell-containing device. EXAMPLES

[0287] Next, the present invention will be described in more detail with reference to examples. However, the present invention is not limited to these examples, and many modifications can be made by those skilled in the art within the technical spirit of the present invention.

[0288] [density] This was determined by measuring the volume and mass. For device material (A) containing a bioabsorbable material (gelatin), the moisture content of the bioabsorbable material (component) was determined using a thermogravimetric differential thermal analyzer (TG-DTA), and the volume of the bioabsorbable material was measured separately. The density was calculated using the weight of the bioabsorbable material (component) corrected for the moisture content.

[0289] [Elution rate] Material (A) was immersed in physiological saline at 37° C. so that the concentration was 5% by mass, and the mass was calculated from the mass of solids contained in the physiological saline after immersion for 24 hours. For the device material (A) containing a bioabsorbable material (gelatin), the moisture content was corrected in the same manner as for the density.

[0290] [Swelling degree] Material (A) was immersed in physiological saline at 37°C for 60 minutes, and the mass was calculated from the mass before and after immersion. For the device material (A) containing a bioabsorbable material (gelatin), the moisture content was corrected in the same manner as for the density.

[0291] [Analysis of modified PVA resin] The viscosity of a 4% aqueous solution and the degree of saponification were determined in accordance with JIS K 6726 (1994). The diacetone acrylamide unit content (denaturation degree) was measured using DMSO-d6 as a solvent. 1 H-NMR was measured, and calculations were made from the integral values ​​of the assigned peaks.

[0292] [Analysis of crosslinking agent (polyacrylic hydrazide)] The weight average molecular weight was determined by size exclusion chromatography measured under the following conditions. conditions: Solvent: 50 mM sodium dihydrogen phosphate aqueous solution Polymer concentration: 1mg / mL Flow rate: 1.0mL / min Column temperature: 40℃ Column: Shodex OHPack SB-803HQ, Shodex OHPack SB-805HQ Standard: Pullulan Detector: RI The hydrazide conversion rate was determined by back titration of I2 using a sodium thiosulfate standard solution. The detailed experimental procedure is as follows. Experimental Procedure: 1. An I2 / MeOH solution was prepared. 2. The I2 / MeOH solution was titrated with 0.1M sodium thiosulfate standard solution (0.047M in this measurement). 3. Each polymer sample was precisely weighed and dissolved in 20 mL of ion-exchanged water. 4. 2.0 mL of 0.047M I2 / MeOH solution was added to the solution of 3. 5. Back titration of iodine was performed with 0.1M sodium thiosulfate standard solution.

[0293] [Device Rating] After implantation (or placement, or even capsule formation by the device) of a device (implantation device, device 1), the islet-containing device was implanted subcutaneously (in adipose tissue) of a rat, and the function of the islet-containing device was evaluated. Specifically, the researchers measured blood glucose levels over time in streptozotocin-induced diabetic rats into which a pancreatic islet-containing device had been transplanted, and confirmed the healing effect.

[0294] [Example 1] (Preparation of material (A)) A 5% by weight aqueous solution of commercially available gelatin (RM-50, made by Gerais Co., Ltd., derived from pigskin, acid-treated) was freeze-dried and punched out into a cylindrical shape with a diameter of φ22 mm (thickness of 0.5 mm). The gelatin was then cross-linked by vacuum drying at 145°C for 24 hours to produce material (A). The resulting material (A) had a density of 58 mg / cm 3 The dissolution rate was 19.8%, the swelling degree was 9.1 times, and the density / swelling degree value was 6.4.

[0295] (Preparation of non-bioresorbable materials) A commercially available silicone rubber (manufactured by AS ONE, model number 6-611-02, thickness 1 mm) was punched out into a cylindrical shape with a diameter of φ26 mm (thickness 0.5 mm) to prepare a non-bioabsorbable material (B). For non-bioabsorbable materials (B), the density is 1200 mg / cm 3 The dissolution rate was 0%, the swelling degree was 1.0 times, and the density / swelling degree value was 1200.

[0296] (Device Fabrication) The material (A) was left to stand in physiological saline at 22° C. for 1 minute to allow it to swell sufficiently. The swollen material (A) was attached to the top and bottom surfaces of the non-bioabsorbable material (B) and then sewn together with sutures to fix the material (A) and the non-bioabsorbable material (B) together, thereby obtaining a device (implant device, device 1).

[0297] (Device implantation and placement process) The above device (implantation device, device 1) was placed subcutaneously in 12-14 week old male Wistar rats (Japan LSC) for 6 weeks. Before placement of the device, no bleeding or exudate was observed subcutaneously, and no capsule was observed. However, after the device was placed for 6 weeks, a capsule was observed subcutaneously that was clearly visible to the naked eye, even compared to before placement. In addition, the device material (A) was almost completely absorbed by the body as a coating (and by the surrounding tissue), leaving only the non-bioabsorbable material at the placement (implantation) site. Because the adhesion between the surface of the non-bioabsorbable material and the subcutaneous tissue was loose, it was extremely easy to peel off, and even after the non-bioabsorbable material was removed, no bleeding or exudate was observed under the skin at the removal site. Therefore, it was extremely easy to subsequently perform various transplants (for example, inserting the pancreatic islet embedding device described below) at the same site. The above implantation and placement process was performed on two rats, and both showed similar results (sufficient capsule formation, no bleeding or exudate after removal of the device).

[0298] (Preparation of islet cells for islet embedding device) Male Lewis rats (Japan SLC) aged 11 to 14 weeks were used for islet isolation. The pancreas was injected into the common bile duct of the rat with cold Hank's buffered saline (HBSS) containing 0.8 mg / mL collagenase type V (Sigma-Aldrich), and digested at 37°C for 12 minutes to isolate islets from the pancreatic tissue. The islets were collected by density gradient centrifugation using Histropaque-1119 (Sigma-Aldrich) and Lymphoprep (AXIS-SHIELD, Norway). The islets were cultured overnight at 37°C under 5% CO2 in RPMI1640 medium containing 5.5 mmol / L glucose and 10% fetal bovine serum (FBS).

[0299] (Polymer synthesis for islet embedding devices) In a flask equipped with a stirrer, a thermometer, a dropping funnel and a reflux condenser, 2000 parts of vinyl acetate, 143 parts of methanol and 3.7 parts of diacetone acrylamide were charged, and after replacing the inside of the system with nitrogen, the temperature was raised until the inside temperature reached 60°C. After the temperature was raised, a solution of 0.16 parts of 2,2-azobisisobutyronitrile dissolved in 100 parts of methanol was added to start polymerization. While continuing to flow nitrogen into the flask, a solution of 70.1 parts of diacetone acrylamide dissolved in 46.7 parts of methanol was dropped at a constant rate immediately after the start of polymerization, and 210 minutes after the start of polymerization, m-dinitrobenzene was added as a polymerization terminator to stop the polymerization. The yield at the end of polymerization was 47.1%. While adding methanol vapor to the obtained reaction mixture, the remaining vinyl acetate was distilled off to obtain a 35% methanol solution of diacetone acrylamide-vinyl acetate copolymer. 500 parts of this solution were mixed well with 70 parts of methanol, 1 part of ion-exchanged water, and 29.3 parts of a 4% methanol solution of sodium hydroxide, and the mixture was subjected to a saponification reaction at 45°C. The resulting gel-like material was crushed, washed thoroughly with methanol, and then dried to obtain D-PVA1. The viscosity of the 4% aqueous solution was 53.4 mPa s, the degree of saponification was 98.4 mol%, and the diacetone acrylamide unit was 3.6 mol%.

[0300] (Synthesis of crosslinker for islet embedding device) 16 parts of hydrazine monohydrate was added to an aqueous solution of 20 parts of polyacrylamide with a weight-average molecular weight of about 40,000 and 40 parts of ion-exchanged water, and the mixture was reacted at 80°C for 15 hours. Ethanol was added to the resulting mixture, and the resulting precipitate was filtered, washed, and dried to obtain APA1. The weight-average molecular weight was about 53,000, and the hydrazide conversion rate was 88%.

[0301] (Preparation of an aqueous solution of modified PVA resin in a sol state and a crosslinking agent) In a 25 mL tube, 8.0 g of the 6.25% aqueous solution of D-PVA1 prepared in Synthesis Example 1 was placed, and 1.0 mL of 10-fold concentrated HBSS (Hank's balanced salt solution) was added thereto, and the tube was shaken up and down to mix. Thereafter, the tube was spun down using a centrifuge (Kubota Shoji Co., Ltd., product name: Hybrid High-Speed ​​Refrigerated Centrifuge 6200) and allowed to stand at 37° C. for 10 minutes. 1.0 mL of a 5% aqueous solution of APA1 prepared in Synthesis Example 9 was added as a crosslinking agent, and the tube was shaken up and down 15 times. After spinning down using a centrifuge, the tube was shaken up and down again 15 times. Then, the tube was centrifuged at 25°C and 3000 rpm for 1 minute, and left to stand at 37°C. The viscosity of the sol-state aqueous solution obtained was checked appropriately, and when the time it took for the sol to become droplets reached 3 to 4 seconds and it was judged to be in an optimal state for embedding the islets, the tube was removed from the hot bath and left to stand on ice for 1 minute. Then, the tube was centrifuged at 25°C and 3000 rpm for 1 minute to obtain a sol containing 5% modified PVA resin and 0.5% crosslinking agent. In the gel (hydrogel), the concentration of D-PVA1 was 5.0%, the concentration of APA1 was 0.5%, and the stress corresponding to the above composition was 5.2 kPa.

[0302] (Preparation of islet-embedded device) 160μL of the sol prepared on the dish was placed on a glass slide. A PET mesh (manufactured by Sunplatic Co., Ltd., product name: PET mesh sheet (designation TN120)) was placed on top of it, and the suspension obtained by removing as much of the medium components as possible from the islet cells prepared above was suspended in 50μL of sol, and the suspension was spread on the PET mesh, and the PET mesh was further placed on top of it so as to sandwich the suspension of islet cells (18,000 Islet Equivalent (IEQ): IEQ is an international unit indicating the amount of islets, and a pancreatic islet with a diameter of 150μm is defined as 1 IEQ). 140μL of sol was placed on the PET mesh, and a glass slide was placed on top of it. The sol thus constructed was placed in a humid box and left to stand at 4℃ for 48 hours to obtain an islet-embedded device (aqueous gel).

[0303] (Preservation process of islet-embedded device) The islet-embedded device constructed above was removed from the slide glass and immersed in storage medium (RPMI1640 medium containing 10% FBS and with the glucose concentration adjusted to 5.5 mM) at a ratio of 5 mL / well in a 6-well plate and stored at 4°C for approximately 16 hours.

[0304] (Transplanting process) About 5 weeks after the placement of the above-mentioned Device 1 (about 1 week before the transplantation of the pancreatic islet-embedded device), streptozotocin was injected into the rats in which the Device 1 had been placed, to induce diabetes. Six weeks after device 1 was left in place, non-bioabsorbable material 2 was removed, and the preserved islet-embedded device (aqueous gel) was placed subcutaneously in the rat (the site where device 1 was implanted, the site where non-bioabsorbable material 2 was removed) to perform transplantation. At the time of transplantation of the islet-embedded device, the capsule [a capsule containing nonwoven fabric 1 (or gelatin)] was maintained.

[0305] (Diabetes Cure Evaluation) After the above transplantation, blood glucose levels were measured over time to confirm the healing effect. The evaluation of diabetes cure was carried out on two rats.

[0306] [Example 2] Commercially available gelatin (sponsel, manufactured by LTL Pharma Co., Ltd.) was punched out into a cylindrical shape with a diameter of φ30 mm (thickness of 0.5 mm), and approximately 400 small holes were made with a syringe needle to prepare material (A). The resulting material (A) had a density of 15 mg / cm 3 The dissolution rate was 33.4%, the swelling degree was 48.5 times, and the density / swelling degree value was 0.303.

[0307] The same procedure as in Example 1 was carried out, except that the material (A) in Example 1 was replaced with the material (A) obtained above, and diabetes cure evaluation was carried out.

[0308] The fabricated device showed the same tendency as in Example 1 (sufficient capsule formation, no bleeding or exudate after device removal) from placement to removal.

[0309] [Example 3] In Example 1, a diabetes cure evaluation was performed using the same procedures as in Example 1, except that a device without material (A) (only non-bioabsorbable material (B), and only material (A) using a non-bioabsorbable material as material (A)) was used as the device. The fabricated device showed the same tendency as in Example 1 (no bleeding or exudate after removal of the device) from placement to removal. A coating was also formed, but the thickness was smaller than in Examples 1 and 2.

[0310] [Reference example 1] The same procedure as in Example 1 was carried out, except that a commercially available gelatin sponge (Gelfoam, manufactured by Pfizer Inc.) was used instead of the material (A) in Example 1, and diabetes cure evaluation was carried out.

[0311] [Reference example 2] An attempt was made to use commercially available gelatin (RM-50, manufactured by Gellice Co., Ltd.) instead of material (A) in Example 1, but it dissolved in physiological saline, making it impossible to fabricate a device.

[0312] [Comparative Example 1] The same procedure as in Example 1 was carried out except that the implantation and placement of the device 1 was not carried out, and diabetes cure evaluation was carried out.

[0313] The results of the diabetes cure evaluation obtained in Examples 1 to 3, Reference Example 1, and Comparative Example 1 are shown in the table below. It should be noted that "pre-transplant blood glucose level" refers to the blood glucose level immediately before the device is removed and the pancreatic islet device is transplanted.

[0314] [Table 1]

[0315] As is clear from the above results, the transplantation device of the embodiment can activate the transplantation site (subcutaneous), and the islet device to be transplanted thereafter can function effectively. It was also confirmed that a membrane was formed at the transplantation site in the transplantation devices of the embodiments 1 to 3 (particularly the embodiments 1 and 2). In particular, it was unexpected that such an islet device could function effectively even though the device did not contain growth factors, etc. According to the present inventor's investigation, this suggests an endogenous increase in growth factors, extracellular matrix, etc.

[0316] Moreover, despite the fact that such activation could be achieved, no bleeding or exudate was observed upon removal of the device, and further transplantation could be performed efficiently, enabling the function of the transplanted device to be efficiently demonstrated or realized. [Industrial Applicability]

[0317] According to the present invention, a novel device can be provided. Such a device can be used for activating a transplant site, for example, for wound healing, or for fully bringing out the inherent performance of a cell-containing device to be transplanted separately.

Claims

1. Density is 15 mg / cm 3 The implant device comprises a material (A) having a dissolution rate of 80% by mass or less after immersion in physiological saline at 37° C. for 24 hours, The material (A) contains gelatin, A device for implantation at the site of transplantation of a cell or tissue containing device.

2. Density is X (mg / cm 3 ), and the swelling degree (calculated as mass) after immersion in physiological saline at 37°C for 60 minutes is Y (times), the ratio (X / Y) of these is 0.303 or more, and the dissolution rate after immersion in physiological saline at 37°C for 24 hours is 80 mass% or less, The material (A) contains gelatin, A device for implantation at the site of transplantation of a cell or tissue containing device.

3. Density is 15 mg / cm 3 The density is X (mg / cm 3 ), and the swelling degree (calculated as mass) after immersion in physiological saline at 37°C for 60 minutes is Y (times), the ratio (X / Y) of these is 0.303 or more, and the dissolution rate after immersion in physiological saline at 37°C for 24 hours is 80 mass% or less, The material (A) contains gelatin, A device for implantation at the site of transplantation of a cell or tissue containing device.

4. A transplant device comprising a material (A) having a density of 15 mg / cm3 or more and a dissolution rate of 80 mass % or less after immersion in physiological saline at 37°C for 24 hours, The material (A) contains gelatin, A device for use in combination with a cell or tissue containing device.

5. A transplant device comprising a material (A) having a density of X (mg / cm3), a swelling degree (converted to mass) after immersion in saline at 37°C for 60 minutes of Y (times), a ratio (X / Y) of these being 0.303 or more, and a dissolution rate of 80 mass% or less after immersion in saline at 37°C for 24 hours, The material (A) contains gelatin, A device for use in combination with a cell or tissue containing device.

6. A transplant device comprising a material (A) having a density of 15 mg / cm3 or more, a ratio (X / Y) of 0.303 or more when the density is X (mg / cm3) and the swelling degree (converted into mass) after immersion in physiological saline at 37°C for 60 minutes is Y (times), and the dissolution rate after immersion in physiological saline at 37°C for 24 hours is 80 mass% or less, The material (A) contains gelatin, A device for use in combination with a cell or tissue containing device.

7. The device according to any one of claims 1 to 6, wherein the dissolution rate of the material (A) after immersion in physiological saline at 37°C for 24 hours is 60 mass% or less.

8. 8. The device according to claim 1, which has a swelling degree of 70 times or less in mass terms after immersion in physiological saline at 37° C. for 60 minutes.

9. Density is X (mg / cm 3 9. The device according to claim 1, wherein the swelling degree (calculated as mass) after immersion in physiological saline at 37° C. for 60 minutes is Y (times), and the ratio (X / Y) between them is 0.303 or more and 6.4 or less.

10. Material (A) has a density of 15 mg / cm 3 or more and 58 mg / cm 3 or less, and the density is X (mg / cm 3), and the swelling degree after immersion in physiological saline at 37°C for 60 minutes is Y (times), the ratio (X / Y) of these is 0.303 to 6.4, and the dissolution rate after immersion in physiological saline at 37°C for 24 hours satisfies 3 to 50 mass%.

11. A device according to any one of claims 1 to 10, in which the material (A) constitutes at least a part of the surface.

12. The device according to any one of claims 1 to 11, comprising a material (A) and a non-bioabsorbable material (B).

13. A device described in any of claims 1 to 12, comprising a material (A) and a non-bioabsorbable material (B), wherein the material (A) and the non-bioabsorbable material (B) are integrated together.

14. A device described in any of claims 1 to 13, comprising a material (A) and a non-bioabsorbable material (B), wherein the proportion of the non-bioabsorbable material (B) is 1 part by volume or more per 100 parts by volume of the material (A).

15. A device described in any of claims 1 to 14, comprising a material (A) and a non-bioabsorbable material (B), wherein the material (A) and the non-bioabsorbable material (B) are integrated together, the proportion of the non-bioabsorbable material (B) is 10 parts by volume or more per 100 parts by volume of the material (A), and the material (A) constitutes at least a portion of the device surface.

16. The device according to any one of claims 12 to 15, wherein the non-bioabsorbable material (B) has an adhesion prevention ability.

17. The device according to any one of claims 1 to 16, which is substantially free of growth factors.

18. A device according to any one of claims 1 to 17 for coating.

19. A device described in any one of claims 1 to 18, wherein the implantation site is subcutaneous.

20. The device according to any one of claims 1 to 19, wherein the cell- or tissue-containing device has an immunoisolation layer containing a polyvinyl alcohol-based resin (A).

21. The device according to any one of claims 1 to 20, wherein the cell- or tissue-containing device has an immunoisolation layer containing at least one polyvinyl alcohol-based resin (A) selected from a modified polyvinyl alcohol-based resin (A1) having an active carbonyl group, a polyvinyl alcohol-based resin (A2) having a syndiotacticity of 32 to 40% expressed in triads, and a polyvinyl alcohol-based resin (A3) having a degree of saponification of 97 mol% or more.

22. The device according to any one of claims 1 to 21, wherein the cells or tissues comprise at least one selected from pancreatic islets, hepatic cells, stem cells thereof, and progenitor cells thereof.

23. A transplantation method comprising transplanting a cell- or tissue-containing device into the transplantation site of a device described in any one of claims 1 to 22, wherein the subject of the transplantation is a non-human animal.

24. A method for preventing and / or treating a disease or symptom, comprising transplanting a cell- or tissue-containing device into the transplantation site of a device described in any one of claims 1 to 22, wherein the subject of the transplantation is a non-human animal.

25. A method according to claim 23 or 24, comprising the step of implanting a device according to any one of claims 1 to 22.

26. The method according to claim 25, comprising implanting a device according to any one of claims 1 to 22 and activating the implantation site.

27. 27. The method of claim 25 or 26, wherein the material (A) is bioabsorbable.

28. A method according to any one of claims 25 to 27, wherein a capsule is formed at the transplant site.

29. The method according to any one of claims 25 to 28, wherein after implanting the device according to any one of claims 12 to 22, at least the non-bioabsorbable material (B) is removed.

30. 30. The method of claim 29, wherein removal occurs without bleeding, inflammation, and / or vascular damage.

31. The method according to any one of claims 23 to 30, wherein the implantation site is subcutaneous.

Citation Information

Patent Citations

  • JP1981501711A

  • Silcone rubber vapor-deposited intraocular lens

    JP1988115556A

  • Material comprising hydrogel and used for cell transplantation therapy

    JP2002145797A

  • Bioabsorbable adhesion preventing material

    JP2013226166A

  • Bone regeneration material kit, pasty bone regeneration material, bone regeneration material and bone junction material