AI Technical Summary
Existing curable silicone compositions used in semiconductor applications suffer from discoloration and increased hardness or embrittlement when exposed to high temperatures, limiting their effectiveness in advanced semiconductor devices.
A curable silicone composition comprising organopolysiloxane resins with specific siloxane units and a mass loss rate of 2.0% or less at 200°C, combined with a curing agent, to maintain hot-melt properties and prevent embrittlement, allowing for the formation of sheets, pellets, and laminates suitable for semiconductor applications.
The composition maintains flexibility and mechanical strength at high temperatures, preventing damage to semiconductor devices and improving their durability and reliability, while being easily processable and applicable in various forms.
Smart Images

Figure 0007560441000006 
Figure 0007560441000001 
Figure 0007560441000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a curable silicone composition which can be obtained by a simple production method, which has good hot melt properties / moldability, and which is resistant to a significant increase in hardness and embrittlement even when the cured product is exposed to temperatures of 150° C. or higher for an extended period of time, and to a molded product (pellets, sheets, etc.) and a cured product of the composition. The present invention also relates to a cured product of the composition and uses thereof (including in particular semiconductor members and semiconductors containing the cured product), a method for producing the composition, and a method for molding the cured product. [Background technology]
[0002] Curable silicone compositions are used in a wide range of industrial fields because they cure to form cured products that have excellent heat resistance, cold resistance, electrical insulation, weather resistance, water repellency, and transparency. Cured products of such curable silicone compositions generally do not discolor as easily as other organic materials, and the deterioration of physical properties is small, so they are also suitable as optical materials and sealants for semiconductor devices.
[0003] The present applicant has proposed a hot-melt curable granular silicone composition and a reactive silicone composition for molding in Patent Documents 1 and 2. These silicone compositions are made of so-called phenyl silicone resins, and have the advantages of superior hot-melt properties compared to methyl silicone resins, as well as superior hardness and strength of the cured product.
[0004] Meanwhile, in recent years, optical semiconductor devices and the like have become smaller and have higher output, and when these hot-melt curable granular silicone compositions and the like are used, coloring due to the phenyl silicone resin may occur, particularly at high temperatures of 200° C. or higher, and the light reflectance may decrease, particularly in the field of reflective materials. For this reason, there is a strong demand for silicone compositions that achieve hot-melt properties and mechanical strength of the cured product after molding, while also meeting the requirements for higher heat resistance and coloring resistance.
[0005] Here, Patent Document 3 discloses a transparent hot-melt curable silicone sheet using a methylsilicone resin. However, when a cured product made of this composition is exposed to a temperature of 150° C. or higher for a long period of time, there is a problem that the hardness increases dramatically and embrittlement progresses, making it difficult to use the product for applications such as sealing semiconductor elements. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2016 / 136243 Brochure [Patent Document 2] JP 2014-009322 A [Patent Document 3] Special Publication No. 2017-512224 Summary of the Invention [Problem to be solved by the invention]
[0007] The object of the present invention is to provide a curable silicone composition that has hot melt properties, is less colored at high temperatures, and gives a cured product that is less likely to increase in hardness or become embrittled when exposed to high temperatures of 150°C or higher for long periods of time.Furthermore, the present invention is to provide such a curable silicone composition in the form of granules, pellets, sheets, etc., and in the form of a peelable laminate containing the curable silicone composition sheet.Furthermore, the object of the present invention is to provide a semiconductor device member made of a cured product of the curable silicone composition, a semiconductor device having the cured product, and a method for molding the cured product. [Means for solving the problem]
[0008] As a result of intensive research, the present inventors have found that the SiO 4 / 2The inventors have discovered that the above-mentioned problems can be solved by using an organopolysiloxane resin that exhibits a mass loss rate of 2.0 mass % or less when exposed to 200°C for 1 hour, and have arrived at the present invention. The present invention relates to a curable silicone composition that contains an organopolysiloxane resin that contains siloxane units represented by the following formula (I) at least 20 mol % of all siloxane units, a liquid linear or branched organopolysiloxane, and a curing agent, and that has hot melt properties as a whole composition. The present invention relates to an organopolysiloxane resin that exhibits a mass loss rate of 2.0 mass % or less when exposed to 200°C for 1 hour, and that has a mass loss rate of 2.0 mass % or less when exposed to 200°C for 1 hour.
[0009] In more detail, (A) 100 parts by mass of an organopolysiloxane resin containing the following components (A1) and (A2) in a mass ratio of 0:100 to 90:10, and which exhibits a mass loss of 2.0% or less when components (A1) and (A2) are exposed to 200°C for 1 hour: (A1) The molecule as a whole does not have hot melt properties, has a curing reactive functional group containing a carbon-carbon double bond in the molecule, and is SiO 4 / 2 The siloxane units represented by the formula 2 0 mol % or more of an organopolysiloxane resin; (A2) The molecule as a whole does not have hot melt properties, does not have a curing reactive functional group containing a carbon-carbon double bond in the molecule, and is SiO 4 / 2 The siloxane units represented by the formula 2 0 mol % or more of an organopolysiloxane resin; (B) 10 to 100 parts by mass of a linear or branched organopolysiloxane that is liquid or plastic at 25°C and has a curing reactive functional group containing at least two carbon-carbon double bonds in the molecule, (C) one or more curing agents selected from (c1) or (c2) below, in an amount necessary for curing the present composition. ( c 1)Organic peroxide ( c 2) An organohydrogenpolysiloxane having at least two silicon-bonded hydrogen atoms in the molecule and a hydrosilylation reaction catalyst. The above problems can be solved by a curable silicone composition characterized by containing and having hot melt properties as a whole composition. Here, the curable silicone composition may optionally contain a functional filler (D), and may contain component (D) in the range of 10 to 2000 parts by mass per 100 parts by mass of the sum of components (A) and (B). Furthermore, the curable silicone composition may be in the form of granules, pellets, or sheets.
[0010] The above-mentioned curable silicone composition may be in the form of a substantially flat curable silicone composition sheet having a thickness of 10 to 1000 μm.
[0011] The above curable silicone composition can also be used in a release laminate having the following configuration. That is, the release laminate may be in the form of a sheet-like substrate having the above curable silicone composition sheet and a release surface facing the curable silicone composition sheet on one or both sides of the curable silicone composition sheet. Such a curable silicone composition sheet may be used as a film-like or sheet-like silicone adhesive.
[0012] Furthermore, the present inventors have discovered that the above problems can be solved by using a cured product of the above-mentioned curable silicone composition, in particular the use of the cured product as a component for a semiconductor device, and by a semiconductor device having the cured product (including one or more selected from power semiconductor devices, optical semiconductor devices, and semiconductor devices mounted on a flexible circuit board), and have arrived at the present invention.
[0013] Similarly, the present inventors have found that the above-mentioned curable silicone composition Coming soon The present inventors have discovered that the above problems can be solved by a production method which comprises granulating the components by mixing only the components under temperature conditions not exceeding 50°C, and a method for molding a cured product using the above-mentioned curable granular silicone composition, and have arrived at this invention.
[0014] The above molding methods include transfer molding, compression molding, and injection molding, and the curable silicone composition of the present invention is suitable for use as a molding material for these methods. Furthermore, the curable silicone composition of the present invention is suitable for use as a molding material for the so-called overmolding method, a process in which a semiconductor element or a semiconductor circuit board is covered by a cured product through overmolding.
[0015] Similarly, the present inventors provide a method for producing a curable silicone composition sheet, comprising the steps of: Step 1: The above-mentioned curable silicone composition Nohara The process involves mixing ingredients at a temperature of 50°C or higher. Step 2: The mixture obtained in step 1 is kneaded while being heated and melted. Step 3: Laminating the heated and melted mixture obtained in step 2 between at least one film having a release surface. Step 4: Stretching the laminate obtained in step 3 between rolls to form a curable silicone sheet having a specific thickness. Effect of the Invention
[0016] The curable silicone composition of the present invention has hot melt properties, and is excellent in handling and curing properties, such as in overmolding, and the cured product of the curable silicone composition is unlikely to increase in hardness or become brittle even when exposed to temperatures exceeding 150°C for a long period of time. Therefore, when the composition is used for sealing and protecting a semiconductor device used at high temperatures, the cured product layer is prevented from being damaged or cracked over time, and the durability and reliability of the semiconductor device are improved. In addition, the curable silicone composition of the present invention can be blended with a relatively large amount of functional inorganic filler without impairing the flexibility and stress relaxation properties of the cured product, and the cured product can be given a desired function such as heat dissipation. Moreover, such a curable silicone composition can be produced by a simple mixing process alone, and can be produced efficiently. Furthermore, the present invention can provide such a curable silicone composition in the form of granules, pellets, sheets, etc., and in the form of a peelable laminate containing the curable silicone composition sheet, and therefore the composition can be cut to a desired size and used as necessary in the manufacturing process of a semiconductor device, and has excellent applicability to industrial production processes. [Brief description of the drawings]
[0017] [Figure 1] FIG. 1 is a diagram showing the overall configuration (entire section including sheet forming) of a production example of a curable hot-melt silicone composition sheet production apparatus. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] [Curable Silicone Composition] The curable silicone composition of the present invention is SiO 4 / 2 The siloxane units represented by the formula 2The composition of the present invention is characterized in that it has as one of its main components an organopolysiloxane resin containing 0.0 mol% or more of dimethylaminopropanediol, and that the mass loss rate of the organopolysiloxane resin when exposed to 200°C for 1 hour is 2.0 mass% or less. The composition of the present invention is further characterized in that it has hot melt properties as a whole. In the present invention, unless otherwise specified, "having hot melt properties" means that the softening point is between 50 and 200°C, the melt viscosity is at 150°C (preferably a melt viscosity of less than 1000 Pa s), and the property of flowing.
[0019] [Technical significance of weight loss rate of organopolysiloxane resin] Here, the mass loss rate of the organopolysiloxane resin when exposed to 200° C. for 1 hour is 2.0% by mass or less, which means that the amount of volatile components in the organopolysiloxane resin is small. 4 / 2 The first feature of the present invention is to use an organopolysiloxane resin having a high content of volatile components, which is very low in the resin. Specifically, when the organopolysiloxane resin, which is component (A) described below, is exposed to 200°C for 1 hour, the mass loss rate must be 2.0% by mass or less, preferably 1.5% by mass or less, and more preferably 1.0% by mass or less.
[0020] In general, in the production process of organopolysiloxane resins containing a large number of branched siloxane units, volatile low molecular weight components are generated and easily mixed into the resin, and these volatile components have the effect of significantly reducing the hardness of the cured product obtained from the composition defined in the present invention. Therefore, if the cured product is exposed to a temperature exceeding 150°C for a long period of time, the low molecular weight components will volatilize, resulting in a significant increase in the hardness of the cured product. In addition, SiO 4 / 2When the resin contains a large amount of siloxane units represented by the formula (I), the cured product tends to be extremely brittle even when it has a high hardness, resulting in embrittlement. By adopting the configuration defined in the present invention, it is possible to obtain a cured product that is unlikely to increase in hardness or become embrittled even when exposed to a temperature exceeding 150°C for a long period of time. Therefore, if the mass loss rate of the organopolysiloxane resin when exposed to 200°C for 1 hour exceeds the upper limit, the hardness of the obtained cured product increases rapidly, particularly at high temperatures, and embrittlement is likely to occur. The lower limit of the mass loss rate is 0.0% by mass, and it is particularly preferable that the resin does not contain volatile low molecular weight components, but in the range of 0.1 to 2.0% by mass, 0.2 to 1.5% by mass, or 0.3 to 0.8% by mass, the change in hardness of the cured product can be sufficiently suppressed in practice.
[0021] The type of the volatile low molecular weight component is not particularly limited, but the organopolysiloxane resin of the present invention is preferably SiO 4 / 2 Since it contains a large number of branched siloxane units (Q units) represented by the formula RSiO 1 / 2 In the present invention, it is particularly preferable that the above-mentioned mass reduction rate is realized by removing, from the organopolysiloxane resin, the volatile low-molecular-weight components mainly composed of the volatile siloxane components.
[0022] [Hot melt properties and composition of the curable silicone composition] The curable silicone composition of the present invention has hot-melt properties as a whole composition, a softening point of 50° C. or higher, and a melt viscosity at 150° C. (preferably a melt viscosity of less than 1000 Pa s), giving it the property of flowing. Note that the individual components that make up the composition do not need to have hot-melt properties, and in particular when the curable reactive or non-reactive organopolysiloxane resin is in particulate form, it is particularly preferable that it does not have hot-melt properties at temperatures of 200° C. or lower.
[0023] The curable silicone composition of the present invention may be, and is preferably, molded into granules, pellets, or sheets depending on the application. Each component and optional component of the composition will be described below. In the present invention, the term "average particle size" refers to the primary average particle size of the particles unless otherwise defined.
[0024] More specifically, the curable silicone composition according to the present invention comprises: (A) 100 parts by mass of an organopolysiloxane resin containing the following components (A1) and (A2) in a mass ratio of 0:100 to 90:10, and which exhibits a mass loss of 2.0% or less when components (A1) and (A2) are exposed to 200°C for 1 hour: (A1) The molecule as a whole does not have hot melt properties, has a curing reactive functional group containing a carbon-carbon double bond in the molecule, and is SiO 4 / 2 The siloxane units represented by the formula 2 0 mol % or more of an organopolysiloxane resin; (A2) The molecule as a whole does not have hot melt properties, does not have a curing reactive functional group containing a carbon-carbon double bond in the molecule, and is SiO 4 / 2 The siloxane units represented by the formula 2 0 mol % or more of an organopolysiloxane resin; (B) 10 to 100 parts by mass of a linear or branched organopolysiloxane that is liquid at 25°C and has a curing reactive functional group containing at least two carbon-carbon double bonds in the molecule; (C) one or more curing agents selected from (c1) or (c2) below, in an amount necessary for curing the present composition. (c1) Organic peroxide (c2) an organohydrogenpolysiloxane having at least two silicon-bonded hydrogen atoms in the molecule and a hydrosilylation reaction catalyst; and may further contain, optionally, (D) a functional inorganic filler, (E) hot-melt particles or other additives having a dropping point of 50°C or higher and a melt viscosity of 10 Pas or lower as measured by a rotational viscometer at 150°C, and the like. Each component and its content will be described below.
[0025] [Component (A)] The curable silicone composition of the present invention does not have hot melt properties as a whole molecule, and 4 / 2 The siloxane units represented by the formula 2 The organopolysiloxane resin further contains RSiO 1 / 2 , R2SiO 2 / 2 , RSiO 3 / 2 (R is a monovalent organic group) and R 2 O 1 / 2 (R 2 may contain a hydroxyl group or an alkoxy group represented by (a hydrogen atom or an alkyl group having 1 to 10 carbon atoms), but preferably, at least 40 mol % of the total siloxane units, particularly 40 to 90 mol %, of SiO 4 / 2 It contains a siloxane unit represented by SiO 4 / 2 If the content of the siloxane unit represented by the formula (I) is less than the lower limit, other branched siloxane units (e.g., RSiO 3 / 2 ) in large amounts, the technical effects of the present invention may not be achieved.
[0026] As described above, the organopolysiloxane resin must have a low content of volatile low molecular weight components, and it is necessary to remove the volatile components that are generated during the production process. The degree of removal is equivalent to the mass loss rate when exposed to 200°C for 1 hour, and it is necessary that the volatile low molecular weight components are removed from the organopolysiloxane resin so that the mass loss rate is 2.0% by mass or less.
[0027] Such organopolysiloxane resins include (A1) The molecule as a whole does not have hot melt properties, has a curing reactive functional group containing a carbon-carbon double bond in the molecule, and is SiO 4 / 2An organopolysiloxane resin containing siloxane units represented by the formula: (A2) The molecule as a whole does not have hot melt properties, does not have a curing reactive functional group containing a carbon-carbon double bond in the molecule, and is SiO 4 / 2 An organopolysiloxane resin containing siloxane units represented by the formula: in a mass ratio of 0:100 to 90:10, and exhibiting a mass loss of 2.0 mass% or less when components (A1) and (A2) are exposed to 200° C. for 1 hour. Note that component (A1) is an optional component in component (A), and only component (A2), described below, may be used in component (A).
[0028] Although the above-mentioned (A) component does not have hot melt properties as a whole molecule, by using it in combination with the later-described (B) component in a specified quantitative range, the hot melt properties of the whole composition can be realized. Such (A) component may be used alone or in combination with other components in the form of fine particles, in which case it is preferable that the component is a spherical silicone fine particle having an average primary particle size of 1 to 20 μm.
[0029] [(A1) Organopolysiloxane resin having a curable reactive functional group] The component (A1) is one of the main components of the composition, and is SiO 4 / 2 The siloxane units represented by the formula 2 The organopolysiloxane resin contains 0 mol % or more of organosiloxane, does not have hot melt properties by itself, and has a curing reactive functional group that contains a carbon-carbon double bond in the molecule, and exhibits a weight loss of 2.0 mass % or less when exposed to 200°C for 1 hour.
[0030] The component (A1) must have a curing reactive group having a carbon-carbon double bond in the molecule. Such a curing reactive group is a functional group that is hydrosilylation reactive or organic peroxide curable, and forms a cured product by a crosslinking reaction with other components. Such a curing reactive group is an alkenyl group or an acrylic group, and examples of such a curing reactive group include alkenyl groups having 2 to 10 carbon atoms, such as vinyl groups, allyl groups, butenyl groups, pentenyl groups, hexenyl groups, and heptenyl groups; and acrylic group-containing monovalent organic groups, such as 3-methacryloxypropyl groups and 3-acryloxypropyl groups. In particular, a vinyl group or a hexenyl group is preferable.
[0031] The component (A1) is an organopolysiloxane resin that does not have hot melt properties as a whole molecule and is solid in a solvent-free state. Here, not having hot melt properties means that the resin that is the component (A1) does not exhibit heat melting behavior at 200°C or less by itself, specifically, that it has no softening point or melt viscosity at 200°C or less. In the component (A1), such physical properties are not particularly limited structurally, but it is preferable that the functional group in the organopolysiloxane resin is a monovalent hydrocarbon group having 1 to 10 carbon atoms, particularly a functional group selected from an alkyl group having 1 to 10 carbon atoms such as a methyl group, and that it does not substantially contain an aryl group such as a phenyl group. If the component contains a large amount of a phenyl group or the like, the component may have hot melt properties, and the SiO 4 / 2 The effect of reinforcing the cured product specific to the group may decrease.
[0032] Preferably, the functional groups bonded to silicon atoms in component (A1) are selected from alkenyl groups such as methyl and vinyl, and it is preferred that 70 to 99 mol% of all functional groups bonded to silicon atoms are methyl, more preferably 80 to 99 mol% are methyl, and particularly preferably 88 to 99 mol% are methyl, and the remaining functional groups bonded to silicon atoms are alkenyl groups such as vinyl. In this range, component (A1) can be designed as a component that is not hot-melt, but is particularly excellent in the color resistance of the cured product at high temperatures. Note that component (A1) may contain a small amount of hydroxyl or alkoxy groups.
[0033] Component (A1) is an organopolysiloxane resin that is solid in the absence of a solvent and contains SiO 4 / 2 The branched siloxane units preferably account for at least 40 mol % of the total siloxane units, more preferably at least 50 mol %, and particularly preferably in the range of 50 to 90 mol %. 。
[0034] Preferably, the component (A1) is a copolymer having the following average unit formula: (R 1 3SiO 1 / 2 ) a (R 1 2SiO 2 / 2 ) b (R 1 SiO 3 / 2 ) c (SiO 4 / 2 ) d (R 2 O 1 / 2)e (In the formula, each R 1 are independently monovalent hydrocarbon groups having 1 to 10 carbon atoms, provided that the total number of R 1 are 1 to 12 mole percent alkenyl groups; 2is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms; a, b, c, d, and e are numbers that satisfy the following: 0.10≦a≦0.60, 0≦b≦0.70, 0≦c≦0.80, 0 .2 ≦d≦0.65, 0≦e≦0.05, provided that c+d>0.20 and a+b+c+d=1) The organopolysiloxane resin is a non-hot melt organopolysiloxane resin represented by the formula:
[0035] In the above average unit formula, each R 1 are independently monovalent hydrocarbon radicals having 1 to 10 carbon atoms, such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, or similar alkyl groups; vinyl, allyl, butenyl, pentenyl, hexenyl, or similar alkenyl groups; phenyl, tolyl, xylyl, or similar aryl groups; benzyl, phenethyl, or similar aralkyl groups; and chloromethyl, 3-chloropropyl, 3,3,3-trifluoropropyl, or similar halogenated alkyl groups. Furthermore, the total R 1 Preferably, 1 to 12 mol % of the total R 1 Of these, 2 to 10 mol % is an alkenyl group. If the content of alkenyl groups is less than the lower limit of the above range, the mechanical strength (hardness, etc.) of the resulting cured product may be insufficient. On the other hand, if the content of alkenyl groups is equal to or less than the upper limit of the above range, the composition containing this component can achieve good hot melt performance as a whole composition. 1 is preferably a functional group selected from an alkyl group having 1 to 10 carbon atoms, such as a methyl group, and an alkenyl group, such as a vinyl group or a hexenyl group. From the viewpoint of the technical effect of the invention, R 1 It is preferable that the component (A) is substantially free of aryl groups such as phenyl groups. If the component (A) contains a large amount of aryl groups such as phenyl groups, the component (A) itself may become hot-melt, making it impossible to achieve the technical effects of the present invention. In addition, in the cured product, SiO 4 / 2 The effect of reinforcing the cured product specific to the group may decrease.
[0036] In the formula, R 2R is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms. 2 The alkyl group of R is exemplified by methyl, ethyl, propyl, butyl, pentyl, or hexyl. 2 Functional group R containing 2 O 1 / 2 corresponds to a hydroxyl group or an alkoxy group in component (A).
[0037] In the formula, a represents the general formula: R 1 3SiO 1 / 2 a is a number indicating the proportion of siloxane units. This number satisfies 0.1≦a≦0.60, and preferably 0.15≦a≦0.55. When a is equal to or greater than the lower limit of the above range, a composition containing this component can achieve good hot melt performance as a whole composition. On the other hand, when a is equal to or less than the upper limit of the above range, the mechanical strength (hardness, elongation, etc.) of the obtained cured product is not too low.
[0038] In the formula, b represents the general formula: R 1 2SiO 2 / 2 This number satisfies 0≦b≦0.70, and preferably 0≦b≦0.60. When b is equal to or less than the upper limit of the range, a composition containing this component can achieve good hot melt performance as a whole composition, and can also provide a composition that is less sticky at room temperature.
[0039] In the formula, c represents a group represented by the general formula: R 3 SiO 3 / 2 c is a number indicating the proportion of siloxane units. This number satisfies 0≦c≦0.80, and preferably 0≦c≦0.75. When c is equal to or less than the upper limit of the range, the composition containing this component can achieve good hot melt performance as a whole composition, and can obtain a tack-free composition with little stickiness at room temperature. In the present invention, c may be, and is preferably, 0.
[0040] In the formula, d is SiO 4 / 2 It is a number that indicates the proportion of siloxane units in 0. 2 It is necessary that 0≦d≦0.65. 、0It is particularly preferable that .25≦d≦0.65, because within this numerical range, a composition containing this component can achieve good hot melt performance as a whole composition, and the resulting cured product has sufficient flexibility.
[0041] In the present invention, c is 0, but it is necessary that c+d>0.20. If the value of c+d is less than the lower limit, the composition as a whole may not achieve good hot melt performance, and the technical effects of the present invention may not be fully achieved.
[0042] In the formula, e represents the general formula: R 2 O 1 / 2 e is a number indicating the proportion of units, which means a hydroxyl group or an alkoxy group bonded to a silicon atom that may be contained in the organopolysiloxane resin. This number satisfies 0≦e≦0.05, preferably 0≦e≦0.03. If e is equal to or less than the upper limit of the range, a material that realizes good hot melt performance as a whole composition can be obtained. In addition, the sum of a, b, c, and d, which are the sums of each siloxane unit, is ultimately equal to 1.
[0043] The component (A1) is an organopolysiloxane resin having the above characteristics, and from the viewpoint of ease of handling, it may be used as spherical organopolysiloxane resin fine particles having an average primary particle diameter of 1 to 20 μm as measured by a laser diffraction / scattering method or the like. By using such a fine particle component, the present composition can be prepared or produced as a curable granular composition having excellent handling, workability and hot melt properties. Here, the method for producing the component (A1) is not limited, and known methods can be used.
[0044] The method for producing the fine particle (A1) component may be, for example, a method for pulverizing the above-mentioned organopolysiloxane resin using a pulverizer or a method for directly pulverizing the resin in the presence of a solvent. The pulverizer is not limited, and may be, for example, a roll mill, a ball mill, a jet mill, a turbo mill, or a planetary mill. In addition, the method for directly pulverizing the above-mentioned organopolysiloxane resin in the presence of a solvent may be, for example, spraying with a spray dryer, or pulverization with a twin-screw kneader or a belt dryer. When obtaining the fine particle (A1) component, a part of the (C) component described later, for example, a hydrosilylation reaction catalyst, may be pulverized together with the (A1) component, but from the viewpoint of the storage stability of the obtained composition, it is not preferable to pulverize a mixture having a property of being cured by heating.
[0045] In particular, by using a spray dryer or the like, it is possible to produce component (A1) that is truly spherical and has an average primary particle size of 1 to 500 μm, preferably 1 to 20 μm. The heating and drying temperature of the spray dryer must be appropriately set based on the heat resistance of the organopolysiloxane resin fine particles. In order to prevent secondary aggregation of the obtained fine particles, it is preferable to control the temperature of the organopolysiloxane resin fine particles to a temperature equal to or lower than their glass transition temperature. The organopolysiloxane resin fine particles thus obtained can be collected using a cyclone, bag filter, or the like.
[0046] The above-mentioned microparticulation may be carried out using a solvent within a range that does not inhibit the curing reaction.The solvent is not limited, but examples thereof include aliphatic hydrocarbons such as n-hexane, cyclohexane, and n-heptane; aromatic hydrocarbons such as toluene, xylene, and mesitylene; ethers such as tetrahydrofuran and dipropyl ether; silicones such as hexamethyldisiloxane, octamethyltrisiloxane, and decamethyltetrasiloxane; esters such as ethyl acetate, butyl acetate, and propylene glycol monomethyl ether acetate; and ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone.
[0047] [(A2) component] The component (A2) is one of the main components of the composition, and is an organopolysiloxane resin containing a curing reactive functional group that does not have hot melt properties by itself, and is a component that realizes hot melt properties of the entire composition and excellent stress relaxation properties of the cured product by combining it with the above-mentioned components (A1) and (B) in a specified quantitative range. Such component (A2) may be used alone or in the form of fine particles together with other components (for example, the component (A1) which is a non-reactive organopolysiloxane resin, and a part of the component (C) which is a curing agent), or it may be mixed with the components (A1) and (B) and treated as a hot melt solid.
[0048] The (A2) component is an organopolysiloxane resin that does not have hot melt properties as a whole molecule and is solid in a solvent-free state. Here, not having hot melt properties means that the resin that is the (A2) component does not exhibit heat melting behavior by itself, specifically, it means that it has no softening point and no melt viscosity. In the (A2) component, such physical properties are not particularly limited structurally, but it is preferable that the functional group in the organopolysiloxane resin is a monovalent hydrocarbon group having 1 to 10 carbon atoms, in particular a functional group selected from an alkyl group having 1 to 10 carbon atoms such as a methyl group, and that it does not substantially contain an aryl group such as a phenyl group. If the component contains a large amount of a phenyl group or the like, the component may have hot melt properties and may be insufficient to form a SiO 4 / 2 The effect of reinforcing the cured product specific to the group may decrease.
[0049] Component (A2) is a solid like component (A1), and is SiO 4 / 2The organopolysiloxane resin contains siloxane units represented by the formula (I) in an amount of at least 20 mol % of all siloxane units, but is characterized in that it does not have a curing reactive functional group containing at least one carbon-carbon double bond in the molecule. In other words, component (A2) is characterized in that it does not contain an alkenyl group such as a vinyl group as a functional group in the organopolysiloxane resin. Examples of functional groups in this organopolysiloxane include monovalent hydrocarbon groups having 1 to 10 carbon atoms, particularly alkyl groups having 1 to 10 carbon atoms such as a methyl group, and it is preferable that it does not substantially contain aryl groups such as a phenyl group.
[0050] Preferably, the functional groups bonded to silicon atoms in component (A2) are alkyl groups having 1 to 10 carbon atoms, such as methyl groups, and it is preferable that 70 to 100 mol % of all the functional groups bonded to silicon atoms are methyl groups, more preferably 80 to 100 mol %, and particularly preferably 88 to 100 mol %. Within this range, component (A2) is not hot-melt and has a SiO 4 / 2 It is possible to design this component as one that has an especially excellent reinforcing effect on the cured product containing the siloxane unit represented by the following formula: The component (A2) may contain a small amount of hydroxyl groups or alkoxy groups.
[0051] The component (A2) does not form a cured product by itself because it does not have a curing reactive group having a carbon-carbon double bond in the molecule, but it has an effect of improving the hot melt properties of the composition as a whole and reinforcing the cured product. In addition, it is a necessary component for achieving the technical effects of the present invention by using it in combination with the component (A1) having a curing reactive group as necessary.
[0052] Component (A2) is a solid organopolysiloxane resin in the absence of a solvent, and contains branched siloxane units, such as SiO 4 / 2 The siloxane unit represented by the formula (1) is contained in an amount of at least 20 mol % of all siloxane units. The amount of the siloxane unit is preferably at least 40 mol % of all siloxane units, more preferably at least 50 mol %, and particularly preferably in the range of 50 to 65 mol %.
[0053] Preferably, the component (A2) is (A2-1) a copolymer having the following average unit formula: (R 3 3SiO 1 / 2 ) f (R 3 2SiO 2 / 2 ) g (R 3 SiO 3 / 2 ) h (SiO 4 / 2 ) i (R 2 O 1 / 2)j (In the formula, each R 3 each independently represents a monovalent hydrocarbon group having 1 to 10 carbon atoms and no carbon-carbon double bonds; R 2 is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms; f, g, h, i, and j are numbers that satisfy the following: 0.35≦f≦0.55, 0≦g≦0.20, 0≦h≦0.20, 0.45≦i≦0.65, 0≦j≦0.05, and f+g+h+i=1). The organopolysiloxane resin is a non-hot melt organopolysiloxane resin represented by the formula:
[0054] In the above average unit formula, each R 3 are independently monovalent hydrocarbon radicals having 1 to 10 carbon atoms and no carbon-carbon double bonds, such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, or similar alkyl radicals; phenyl, tolyl, xylyl, or similar aryl radicals; benzyl, phenethyl, or similar aralkyl radicals; and chloromethyl, 3-chloropropyl, 3,3,3-trifluoropropyl, or similar halogenated alkyl radicals, where the total R 3 It is preferable that 70 mol % or more of R are alkyl groups having 1 to 10 carbon atoms such as methyl groups, and it is particularly preferable that 88 mol % or more of R are methyl groups from the viewpoint of industrial production and the technical effect of the invention. 3It is preferable that the component (B) is substantially free of aryl groups such as phenyl groups. If the component (B) contains a large amount of aryl groups such as phenyl groups, the component (B) itself may become hot-melt, making it impossible to achieve the technical effects of the present invention, and the color resistance of the cured product at high temperatures may deteriorate.
[0055] In the formula, R 2 is the same group as defined above.
[0056] In the formula, f represents the general formula: R 3 3SiO 1 / 2 f is a number indicating the proportion of siloxane units. This number satisfies 0.35≦f≦0.55, and preferably 0.40≦f≦0.50. When f is equal to or greater than the lower limit of the above range, a composition containing this component can achieve good hot melt performance as a whole composition. On the other hand, when f is equal to or less than the upper limit of the above range, the mechanical strength (hardness, etc.) of the obtained cured product is not too low.
[0057] In the formula, g represents a group represented by the general formula: R 1 2SiO 2 / 2 g is a number indicating the proportion of siloxane units. This number satisfies 0≦g≦0.20, and preferably 0≦g≦0.10. When g is equal to or less than the upper limit of the range, the composition containing this component can achieve good hot melt performance as a whole composition, and can obtain a composition that is less sticky at room temperature. In the present invention, g may be 0, and is preferred.
[0058] In the formula, h represents the general formula: R 1 SiO 3 / 2 h is a number indicating the proportion of siloxane units. This number satisfies 0≦h≦0.20, and preferably 0≦h≦0.10. When h is equal to or less than the upper limit of the range, a composition containing this component can achieve good hot melt performance as a whole composition, and can obtain a composition that is less sticky at room temperature. In the present invention, h may be 0, and is preferred.
[0059] In the formula, i is SiO 4 / 2i is a number indicating the proportion of siloxane units, and it is necessary that 0.45≦i≦0.65, preferably 0.40≦i≦0.65, and particularly preferably 0.50≦i≦0.65. Within this numerical range, a composition containing this component can achieve good hot melt performance as a whole composition, excellent mechanical strength of the obtained cured product, and a composition that is not sticky as a whole and has good handling and workability can be realized.
[0060] In the formula, j represents the general formula: R 2 O 1 / 2 This unit means a hydroxyl group or an alkoxy group bonded to a silicon atom that may be contained in the organopolysiloxane resin. This number satisfies 0≦j≦0.05, and preferably 0≦j≦0.03. j If the amount of each siloxane unit is equal to or less than the upper limit of the range, a material that realizes good hot melt performance as a whole composition can be obtained. ruf , g 、 h and i The sum of is equal to 1.
[0061] The component (A2) is an organopolysiloxane resin having the above characteristics, and from the viewpoint of ease of handling, it may be used as spherical organopolysiloxane resin fine particles having an average primary particle diameter of 1 to 20 μm as measured by a laser diffraction / scattering method or the like. By using such a fine particle component, the present composition can be prepared or produced as a curable granular composition having excellent handling, workability and hot melt properties. Here, the method of producing the component (A2) can be the same as the method exemplified for the component (A1) above.
[0062] [Removal of volatile low molecular weight components from component (A)] In the production process of components (A1) and (A2), volatile low molecular weight components are generated. Specifically, the structure is M4Q, and the M unit (R 3 3SiO 1 / 2 ) and Q units (SiO 4 / 2) is polymerized as a by-product. This structure has the effect of significantly lowering the hardness of the cured product of the composition of the present invention. The organopolysiloxane resin is polymerized in the presence of a highly compatible organic solvent, and the solid organopolysiloxane resin is obtained by removing the organic solvent by drying under reduced pressure or the like, but the M4Q structure has high mutual solubility with the organopolysiloxane resin, and cannot be removed under drying conditions that remove the organic solvent. It was known that this structure can be removed by exposure to a temperature of 200°C or higher for a short period of time, but if it is removed by exposure to high temperatures after being integrally molded with a substrate such as a semiconductor, the volume of the cured product will decrease and the hardness will increase significantly, causing the dimensions of the molded product to change and warping to occur. For this reason, in order to apply this invention to the applications, it is necessary to remove the M4Q structure before the molding process with the substrate, that is, at the stage of the raw material.
[0063] Methods for removing this structure include removing it together with the organic solvent in a twin-screw kneader, or forming a particulate organopolysiloxane resin using the method described below, and then drying it in an oven or the like to remove it.
[0064] More specifically, components (A1) and (A2) are produced in the presence of an organic solvent, and volatile components appear as by-products during synthesis. The volatile components can be removed by treating the obtained crude organopolysiloxane resin at a high temperature of about 200 degrees for a short period of time, so it is possible to simultaneously remove the organic solvent and volatile components from components (A1) and (A2) using a twin-screw kneader set at about 200°C. In addition, when components (A1) and (A2) are handled as spherical powders, it is possible to powder them by removing the organic solvent with a spray dryer, but this method does not allow the volatile components to be removed. If the obtained powder is treated at a low temperature of about 120°C for 24 hours, the volatile components can be removed without the powder agglomerating.
[0065] [Mass ratio of component (A1) to component (A2) in component (A)] In order to impart hot melt properties to the composition as a whole, it is necessary to mix the (A2) component or a mixture of the (A1) and (A2) components with the (B) component described later at a predetermined ratio, but the ratio of the (A1) and (A2) components may be in the range of 0:100 to 90:10, preferably in the range of 0:100 to 85:15, and more preferably 0:100 to 80:20. The (A2) component does not have curability by itself, but by adding a small amount of the (A1) component to the composition and using it in combination, it is possible to control the elastic modulus of the cured product of the composition at high temperatures, and when a functional inorganic filler described later is added to the composition, it is possible to achieve a suitable elastic modulus and flexibility by appropriately adjusting the amount of the functional inorganic filler added and the amount of the (A1) component used. For example, when a large amount of the functional inorganic filler is added or when it is desired to reduce the elastic modulus of the resulting cured product as much as possible, it is also possible to compound the composition with only the (A2) component without adding the (A1) component. On the other hand, when a functional inorganic filler described below is not added, it is possible to adjust the elastic modulus at room temperature and at high temperatures to the desired values by increasing the amount of component (A2) added.
[0066] [(B) Component] Component (B) is one of the main components of the composition, and is a linear or branched organopolysiloxane that is liquid or plastic at 25° C. and has a curing reactive functional group containing at least two carbon-carbon double bonds in the molecule. When this type of curing reactive chain organopolysiloxane is mixed with the above-mentioned solid organopolysiloxane resin, the composition as a whole exhibits hot melt properties.
[0067] The (B) component must have a curing reactive group having a carbon-carbon double bond in the molecule. Such a curing reactive group is a hydrosilylation reactive or organic peroxide curing functional group, and forms a cured product by a crosslinking reaction with other components. Such a curing reactive group is an alkenyl group or an acrylic group, and examples thereof include the same groups as those described above, and in particular, a vinyl group or a hexenyl group is preferable.
[0068] Component (B) is a linear or branched organopolysiloxane that is liquid or plastic at 25°C (room temperature), and when mixed with component (A), which is solid at room temperature, the composition as a whole exhibits hot melt properties. The structure of this component is a small number of branched siloxane units (for example, the general formula: R 4 SiO 3 / 2 T units (R 4 are independently monovalent hydrocarbon radicals having 1 to 10 carbon atoms) or SiO 4 / 2 The organopolysiloxane may be a branched organopolysiloxane having a Q unit represented by the formula: (B1) The following structural formula: R 4 3SiO(SiR 4 2O) k SiR 4 3 (In the formula, each R 4 are independently monovalent hydrocarbon groups having 1 to 10 carbon atoms, provided that R 4 at least two of the groups are alkenyl groups, and k is a number from 20 to 5,000. It is a linear diorganopolysiloxane represented by the following formula: Preferably, it is a linear diorganopolysiloxane having one alkenyl group at each of both ends of the molecular chain.
[0069] In the formula, each R 4 are independently monovalent hydrocarbon radicals having 1 to 10 carbon atoms, such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, or similar alkyl groups; vinyl, allyl, butenyl, pentenyl, hexenyl, or similar alkenyl groups; phenyl, tolyl, xylyl, or similar aryl groups; benzyl, phenethyl, or similar aralkyl groups; and chloromethyl, 3-chloropropyl, 3,3,3-trifluoropropyl, or similar halogenated alkyl groups. 4 At least two of R are alkenyl groups, preferably vinyl groups. 4 is preferably a functional group selected from an alkyl group having 1 to 10 carbon atoms, such as a methyl group, and an alkenyl group, such as a vinyl group or a hexenyl group, and all of R 4At least two of R are alkenyl groups, and the remaining R 4 From the viewpoint of the technical effect of the invention, it is preferable that R 4 It is preferable that R is substantially free of aryl groups such as phenyl groups. If it contains a large amount of aryl groups such as phenyl groups, the color resistance of the cured product at high temperatures may deteriorate. Particularly preferably, R has an alkenyl group such as a vinyl group at each end of the molecular chain and other R 4 is preferably a methyl group.
[0070] In the formula, k is a number of 20 to 5,000, preferably 30 to 3,000, and particularly preferably 45 to 800. When k is equal to or greater than the lower limit of the above range, a composition that is less sticky at room temperature can be obtained. On the other hand, when k is equal to or less than the upper limit of the above range, the composition as a whole can achieve good hot melt performance.
[0071] Here, in order to achieve hot melt properties for the entire composition, the mass ratio of the linear or branched organopolysiloxane (B) component to 100 parts by mass of the organopolysiloxane resin (A) component is in the range of 10 to 100 parts by mass, preferably in the range of 10 to 70 parts by mass, and more preferably in the range of 15 to 50 parts by mass. If the content of the (B) component is in the above range, the composition achieves good hot melt properties, the mechanical strength of the obtained cured product can be increased, and the stickiness of the obtained composition at room temperature can be reduced, improving the handling and workability.
[0072] [(C) component] The component (C) is a curing agent for curing the components (A) and (B), and is specifically one or more curing agents selected from the following (c1) or (c2). Two or more of these curing agents may be used in combination, for example, a curing system containing both the components (c1) and (c2). (c1) Organic peroxide (c2) an organohydrogenpolysiloxane having at least two silicon-bonded hydrogen atoms in the molecule and a hydrosilylation reaction catalyst;
[0073] The (c1) organic peroxide is a component that cures the above-mentioned (A) and (B) components by heating, and examples thereof include alkyl peroxides, diacyl peroxides, ester peroxides, and carbonate peroxides. Note that the (c1) component can also react with a part of the (A2) component.
[0074] Examples of alkyl peroxides include dicumyl peroxide, di-tert-butyl peroxide, di-tert-butylcumyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3, tert-butylcumyl, 1,3-bis(tert-butylperoxyisopropyl)benzene, and 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxonane.
[0075] Examples of diacyl peroxides include benzoyl peroxide, lauroyl peroxide, and decanoyl peroxide.
[0076] Examples of peroxy esters include 1,1,3,3-tetramethylbutyl peroxy neodecanoate, α-cumyl peroxy neodecanoate, tert-butyl peroxy neodecanoate, tert-butyl peroxy neoheptanoate, tert-butyl peroxy pivalate, tert-hexyl peroxy pivalate, 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate, and tert-amyl peroxy-2-ethylhexanoate. , tert-butylperoxy-2-ethylhexanoate, tert-butylperoxyisobutyrate, di-tert-butylperoxyhexahydroterephthalate, tert-amylperoxy-3,5,5-trimethylhexanoate, tert-butylperoxy-3,5,5-trimethylhexanoate, tert-butylperoxyacetate, tert-butylperoxybenzoate, and di-butylperoxytrimethyladipate are examples.
[0077] Examples of peroxycarbonates include di-3-methoxybutyl peroxydicarbonate, di(2-ethylhexyl) peroxydicarbonate, diisopropyl peroxycarbonate, tert-butylperoxyisopropyl carbonate, di(4-tert-butylcyclohexyl) peroxydicarbonate, dicetyl peroxydicarbonate, and dimyristyl peroxydicarbonate.
[0078] The organic peroxide preferably has a half-life of 10 hours at a temperature of 90° C. or higher, or 95° C. or higher. Examples of such organic peroxides include dicumyl peroxide, di-t-butyl peroxide, di-t-hexyl peroxide, t-butylcumyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, 1,3-bis(tert-butylperoxyisopropyl)benzene, di-(2-t-butylperoxyisopropyl)benzene, and 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxonane.
[0079] The content of the (c1) organic peroxide is not limited, but is preferably within a range of 0.05 to 10 parts by mass, or 0.10 to 5.0 parts by mass, relative to the sum (100 parts by mass) of the (A) and (B) components.
[0080] (c2) An organohydrogenpolysiloxane having at least two silicon-bonded hydrogen atoms in its molecule and a hydrosilylation catalyst are components that cure the composition by undergoing an addition reaction (hydrosilylation reaction) between the organohydrogenpolysiloxane, which is a crosslinking agent, and the carbon-carbon double bonds in components (A) and (C) in the presence of the hydrosilylation catalyst.
[0081] The structure of the organohydrogenpolysiloxane crosslinking agent is not particularly limited, and may be linear, branched, cyclic, or resinous. c 2) The composition is HR2SiO 1 / 2 Hydrogenorganosiloxy units (D H R is independently a monovalent organic group) as the main structural unit, HRSiO 2 / 2 Hydrogen diorganosiloxy units (M H In particular, in applications other than the molding process described below, the present curable silicone composition may be an organohydrogenpolysiloxane having the above-mentioned D H Even if the organohydrogenpolysiloxane is a chain organohydrogenpolysiloxane consisting of units, it can be cured sufficiently for practical use.
[0082] On the other hand, when the present curable silicone composition is used in a molding process, the content of curing reactive functional groups containing carbon-carbon double bonds in the present composition is low, and therefore, from the standpoint of the curing speed, moldability, and curability, the organohydrogenpolysiloxane is RSiO 3 / 2 Monoorganosiloxy units (T units, R is a monovalent organic group or a silicon-bonded hydrogen atom) represented by the formula: 4 / 2 The branching unit is a siloxy unit (Q unit) represented by the formula:1 / 2 Hydrogen diorganosiloxy units (M H unit, R is independently a monovalent organic group), and M H Organohydrogenpolysiloxane resins having units are preferred.
[0083] Particularly suitable organohydrogenpolysiloxanes have the average unit formula: (R 5 3SiO 1 / 2 ) l (R 6 2SiO 2 / 2 ) m (R 6 SiO 3 / 2 ) n (SiO 4 / 2 ) p (R 2 O 1 / 2 ) q The organohydrogenpolysiloxane resin is represented by the formula:
[0084] In the formula, each R 5 are the same or different, and are monovalent hydrocarbon groups having 1 to 10 carbon atoms that do not have an aliphatic unsaturated carbon bond, or hydrogen atoms, provided that at least two R 5 is a hydrogen atom. R other than a hydrogen atom 5 The monovalent hydrocarbon radicals are, for example, methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, or similar alkyl radicals; phenyl, tolyl, xylyl, or similar aryl radicals; benzyl, phenethyl, or similar aralkyl radicals; and chloromethyl, 3-chloropropyl, 3,3,3-trifluoropropyl, or similar halogenated alkyl radicals. From an industrial point of view, the methyl or phenyl radicals are preferred.
[0085] In the formula, R 6 is a monovalent hydrocarbon group having 1 to 10 carbon atoms that does not have an aliphatic unsaturated carbon bond, and examples of the monovalent hydrocarbon group include the same groups as those described above. 2is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, and R in the above component (A1) or (A2) 2 Examples of the groups are the same as those shown below.
[0086] In the formula, l, m, n, and p are numbers that satisfy the following: 0.1≦l≦0.80, 0≦m≦0.5, 0≦n≦0.8, 0≦p≦0.6, 0≦q≦0.05, provided that n+p>0.1 and l+m+n+p=1. Here, when the present composition is used in a molding process, ( c 2) The organohydrogenpolysiloxane resin, which is one of the components, is specifically M H MT resin, M H MTT H Resin, M H MTQ resin, M H MQ resin, M H MTT H Q, M H Q resin is preferred.
[0087] Particularly preferably, the organohydrogenpolysiloxane which is a part of the component (c2) is (H(CH3)2SiO 1 / 2 ) l1 (SiO 4 / 2 ) p1 Represented by M H Q resin. Here, it is preferable that l1+p1=1, 0.1≦l1≦0.80, and 0.20≦p1≦0.90.
[0088] Similarly, the organohydrogenpolysiloxane that is a part of component (c2) may contain a linear diorganopolysiloxane, organohydrogenpolysiloxane, or diorganopolysiloxane-organohydrogensiloxane copolymer whose molecular chain ends are blocked with silicon-bonded hydrogen atoms or trimethylsiloxy groups. The degree of siloxane polymerization of these linear organohydrogenpolysiloxanes is not particularly limited, but is in the range of 2 to 200, and preferably in the range of 5 to 100.
[0089] The content of the organohydrogenpolysiloxane, which is part of component (c2), is an amount sufficient to cure the curable silicone composition of the present invention, and ( A ) components and ( B The molar ratio of silicon-bonded hydrogen atoms in the organohydrogenpolysiloxane to the curing reactive functional groups containing carbon-carbon double bonds (for example, alkenyl groups such as vinyl groups) in the component () is 0.5 or more, and an amount in the range of 0.5 to 20 is preferable. c 2) When the component contains the above organohydrogenpolysiloxane resin, ( A ) components and ( B It is preferable that the molar ratio of silicon-bonded hydrogen atoms in the organohydrogenpolysiloxane resin to the curing reactive functional groups containing carbon-carbon double bonds in the component (a) is in the range of 0.5 to 20, or 1.0 to 10.
[0090] Examples of the hydrosilylation catalyst, which is a part of component (c2), include platinum-based catalysts, rhodium-based catalysts, and palladium-based catalysts, with platinum-based catalysts being preferred because they can significantly accelerate the curing of the composition. Examples of platinum-based catalysts include platinum fine powder, chloroplatinic acid, alcohol solutions of chloroplatinic acid, platinum-alkenylsiloxane complexes, platinum-olefin complexes, platinum-carbonyl complexes, and catalysts in which these platinum-based catalysts are dispersed or encapsulated in thermoplastic resins such as silicone resins, polycarbonate resins, and acrylic resins, with platinum-alkenylsiloxane complexes being particularly preferred. Examples of the alkenylsiloxane include 1,3-divinyl-1,1,3,3-tetramethyldisiloxane, 1,3,5,7-tetramethyl-1,3,5,7-tetravinylcyclotetrasiloxane, alkenylsiloxanes in which a part of the methyl groups of these alkenylsiloxanes is replaced with an ethyl group, a phenyl group, or the like, and alkenylsiloxanes in which the vinyl groups of these alkenylsiloxanes are replaced with an allyl group, a hexenyl group, or the like. In particular, since the stability of this platinum-alkenylsiloxane complex is good, 1,3-divinyl-1,1,3,3-tetramethyldisiloxane is preferred, and it is preferred to add the complex in the form of an alkenylsiloxane solution. In addition, from the viewpoint of improving the handling and workability and the pot life of the composition, a platinum-containing hydrosilylation reaction catalyst in the form of fine particles dispersed or encapsulated in a thermoplastic resin may be used. As a catalyst for promoting the hydrosilylation reaction, a non-platinum metal catalyst such as iron, ruthenium, or iron / cobalt may be used.
[0091] The amount of the hydrosilylation reaction catalyst, which is part of component (c2), added is preferably an amount such that the metal atoms are in the range of 0.01 to 500 ppm, 0.01 to 100 ppm, or 0.01 to 50 ppm, by mass, relative to the entire composition.
[0092] Particularly preferred component (c2) is one that contains at least (c2-1) an organohydrogenpolysiloxane resin represented by the above average unit formula and a hydrosilylation reaction catalyst.
[0093] When the above-mentioned hydrosilylation reaction catalyst is used as part of component (C), from the viewpoint of the storage stability of the curable silicone composition, it is preferable to have it contained in the fine particles when producing organopolysiloxane resin particles such as components (A1) and (A2). However, it is preferable that the entire mixture constituting the fine particles does not exhibit curing reactivity on its own.
[0094] If it is desired to impart functionality to the resulting cured product, the curable silicone composition of the present invention can further contain (D) a functional filler, in addition to the above components (A) to (C).
[0095] The functional filler, which is the component (D), is a component that imparts mechanical properties and other properties to the cured product, and examples thereof include inorganic fillers, organic fillers, and mixtures thereof. Examples of the inorganic fillers include reinforcing fillers, white pigments, thermally conductive fillers, conductive fillers, phosphors, and mixtures of at least two of these, and examples of the organic fillers include silicone resin-based fillers, fluororesin-based fillers, and polybutadiene resin-based fillers. The shape of these fillers is not particularly limited, and may be spherical, spindle-shaped, flat, needle-shaped, or amorphous.
[0096] When the present composition is used as a sealant, protective agent, adhesive, or the like, it is preferable for at least a part of component (D) to contain a reinforcing filler, from the viewpoint of improving the mechanical strength, protective properties, and adhesive properties of the cured product.
[0097] The reinforcing filler may be added to improve the mechanical strength of the cured product, improve the protectiveness and adhesiveness, and maintain the solid particulate state as a binder filler of the curable silicone composition before curing. Examples of such reinforcing fillers include fumed silica, precipitated silica, fused silica, calcined silica, fumed titanium dioxide, quartz, calcium carbonate, diatomaceous earth, aluminum oxide, aluminum hydroxide, zinc oxide, and zinc carbonate. In addition, these reinforcing fillers may be surface-treated with organoalkoxysilanes such as methyltrimethoxysilane; organohalosilanes such as trimethylchlorosilane; organosilazanes such as hexamethyldisilazane; siloxane oligomers such as α,ω-silanol group-blocked dimethylsiloxane oligomers, α,ω-silanol group-blocked methylphenylsiloxane oligomers, and α,ω-silanol group-blocked methylvinylsiloxane oligomers. The particle size of the reinforcing filler is not limited, but the median size measured by laser diffraction / scattering particle size distribution measurement is preferably within the range of 1 nm to 500 μm.Furthermore, fibrous fillers such as calcium metasilicate, potassium titanate, magnesium sulfate, sepiolite, zonolite, aluminum borate, rock wool, and glass fiber may be used as the reinforcing filler.
[0098] Furthermore, in order to impart other functions to the cured product obtained by using the composition, a white pigment, a thermally conductive filler, an electrically conductive filler, or a fluorescent material may be blended in. Also, in order to improve the stress relaxation properties of the cured product, an organic filler such as silicone elastomer fine particles may be blended in.
[0099] The white pigment is a component that imparts whiteness to the cured product and improves light reflectivity, and the cured product obtained by curing the composition by blending the component can be used as a light reflector for light emitting / optical devices. Examples of the white pigment include metal oxides such as titanium oxide, aluminum oxide, zinc oxide, zirconium oxide, and magnesium oxide; hollow fillers such as glass balloons and glass beads; and other materials such as barium sulfate, zinc sulfate, barium titanate, aluminum nitride, boron nitride, and antimony oxide. Titanium oxide is preferred because of its high light reflectance and hiding power. Aluminum oxide, zinc oxide, and barium titanate are preferred because of their high light reflectance in the UV region. The average particle size and shape of the white pigment are not limited, but the average particle size is preferably within the range of 0.05 to 10.0 μm, or 0.1 to 5.0 μm. The white pigment may be surface-treated with a silane coupling agent, silica, aluminum oxide, or the like.
[0100] The thermally conductive filler or the conductive filler is added for the purpose of imparting thermal conductivity / conductivity (electrical conductivity) to the cured product, and specific examples thereof include fine metal powders such as gold, silver, nickel, copper, and aluminum; fine powders of ceramics, glass, quartz, organic resins, and the like, on whose surfaces metals such as gold, silver, nickel, and copper are vapor-deposited or plated; metal compounds such as aluminum oxide, magnesium oxide, aluminum nitride, boron nitride, and zinc oxide; graphite, and mixtures of two or more of these. When electrical insulation is required for the composition, metal oxide powders or metal nitride powders are preferred, and aluminum oxide powder, zinc oxide powder, and aluminum nitride powder are particularly preferred, and these may be used in combination with each other in terms of type, particle size, particle shape, and the like according to the requirements for thermal conductivity / conductivity.
[0101] The phosphor is a component that is blended to convert the wavelength of light emitted from a light source (optical semiconductor element) when the cured product is used as a wavelength conversion material. There are no particular limitations on the phosphor, and examples of the phosphor include yellow, red, green, and blue light-emitting phosphors made of oxide-based phosphors, oxynitride-based phosphors, nitride-based phosphors, sulfide-based phosphors, oxysulfide-based phosphors, etc., which are widely used in light-emitting diodes (LEDs).
[0102] Examples of silicone fine particles include non-reactive silicone resin fine particles and silicone elastomer fine particles, with silicone elastomer fine particles being preferred from the standpoint of improving the flexibility or stress relaxation properties of the cured product.
[0103] Silicone elastomer microparticles are crosslinked products of linear diorganopolysiloxanes mainly composed of diorganosiloxy units (D units). Silicone elastomer microparticles can be prepared by crosslinking diorganopolysiloxanes by hydrosilylation reaction or condensation reaction of silanol groups, and can be preferably obtained by crosslinking an organohydrogenpolysiloxane having silicon-bonded hydrogen atoms at the side chain or end with a diorganopolysiloxane having unsaturated hydrocarbon groups such as alkenyl groups at the side chain or end under a hydrosilylation reaction catalyst. Silicone elastomer microparticles can take various shapes such as spherical, flat, and irregular, but from the viewpoint of dispersibility, spherical is preferable, and among them, true sphere is more preferable. Examples of commercially available silicone elastomer microparticles include "Trefil E Series" and "EP Powder Series" manufactured by Toray Dow Corning Co., Ltd., and "KMP Series" manufactured by Shin-Etsu Chemical Co., Ltd.
[0104] For the purpose of stably blending the functional filler as described above in the present composition, the filler may be surface-treated using a specific surface treatment agent in an amount of 0.1 to 2.0 mass%, 0.1 to 1.0 mass%, or 0.2 to 0.8 mass% relative to the total mass of component (D). Examples of such surface treatment agents include methylhydrogenpolysiloxane, silicone resin, metal soap, silane coupling agent, perfluoroalkylsilane, and fluorine compounds such as perfluoroalkyl phosphate salt.
[0105] In particular, when component (D) is a thermally conductive filler and is blended in large amounts in the curable silicone composition of the present invention, the thermally conductive filler is preferably a plate-shaped boron nitride powder having a suitable average particle size of 0.1 to 30 μm, a granular boron nitride powder having an average particle size of 0.1 to 50 μm, a spherical and / or crushed aluminum oxide powder having an average particle size of 0.01 to 50 μm, or a spherical and / or crushed graphite having an average particle size of 0.01 to 50 μm, or a mixture of two or more of these. Most preferably, it is a mixture of two or more of spherical and crushed aluminum oxide powders having an average particle size of 0.01 to 50 μm. In particular, by combining an aluminum oxide powder having a large particle size and an aluminum oxide powder having a small particle size in a ratio that follows the closest packing theoretical distribution curve, the packing efficiency is improved, and low viscosity and high thermal conductivity are possible.
[0106] Furthermore, it is particularly preferred that at least a part of the surface of the thermally conductive filler is treated with one or more types of organosilicon compounds. The preferred range of the treatment amount is as described above. Here, examples of the organosilicon compound that is the surface treatment agent are low molecular weight organosilicon compounds such as silane, silazane, siloxane, or the like, and organosilicon polymers or oligomers such as polysiloxane, polycarbosiloxane, or the like. A preferred example of silane is a so-called silane coupling agent. Representative examples of such silane coupling agents include alkyltrialkoxysilanes (methyltrimethoxysilane, vinyltrimethoxysilane, hexyltrimethoxysilane, octyltrimethoxysilane, decyltrimethoxysilane, or the like), and organofunctional group-containing trialkoxysilanes (glycidoxypropyltrimethoxysilane, epoxycyclohexylethyltrimethoxysilane, methacryloxypropyltrimethoxysilane, aminopropyltrimethoxysilane, or the like). Preferred siloxanes and polysiloxanes include hexamethyldisiloxane, 1,3-dihexyl-tetramethyldisiloxane, trialkoxysilyl single-terminated polydimethylsiloxane, trialkoxysilyl single-terminated dimethylvinyl single-terminated polydimethylsiloxane, trialkoxysilyl single-terminated organofunctional group single-terminated polydimethylsiloxane, trialkoxysilyl doubly terminated polydimethylsiloxane, organofunctional group doubly terminated polydimethylsiloxane, or the like. When siloxanes are used, the number of siloxane bonds n is preferably in the range of 2 to 150. Examples of preferred silazanes are hexamethyldisilazane, 1,3-dihexyl-tetramethyldisilazane, or the like. Examples of preferred polycarbosiloxanes are polymers with Si-C-C-Si bonds in the polymer backbone.
[0107] The content of the (D) component is not limited, but in order to obtain a cured product with excellent hardness and mechanical strength, it is preferable that the content be within the range of 10 to 2000 parts by mass, 10 to 1500 parts by mass, or 10 to 1000 parts by mass relative to the sum (100 parts by mass) of the (A) and (B) components.
[0108] The curable silicone composition of the present invention is C )component and optionally component (D). From the viewpoint of further improving the melting properties, it is also possible and preferable to add (E) hot-melt particles having a dropping point of 50° C. or higher and a melt viscosity of 10 Pas or lower as measured by a rotational viscometer at 150° C.
[0109] As long as the dropping point conditions and the kinetic viscosity conditions at 150°C are satisfied, the type of component (E) is not particularly limited, and one or more selected from various hot-melt synthetic resins, waxes, fatty acid metal salts, etc. can be used. The component (E) exhibits low kinetic viscosity at high temperatures (150°C) and forms a molten material with excellent fluidity. Furthermore, by using the above components (A) to (C) in combination, the component (E) in the molten material of this composition spreads quickly throughout the entire composition at high temperatures, thereby reducing the viscosity of the substrate surface to which the molten composition is applied and the entire composition, and also rapidly reducing the surface friction of the substrate and the molten composition, thereby significantly increasing the fluidity of the entire composition. Therefore, the viscosity and fluidity of the molten composition can be greatly improved by adding only a small amount of the component (E) relative to the total amount of other components.
[0110] The component (E) may be a petroleum wax such as paraffin as long as it satisfies the above-mentioned conditions of dropping point and kinetic viscosity when melted, but from the viewpoint of the technical effect of the present invention, it is preferably a hot melt component consisting of a fatty acid metal salt or a fatty acid ester of an erythritol derivative, and particularly preferably a metal salt of a higher fatty acid such as stearic acid, palmitic acid, oleic acid, isononanoic acid, etc., pentaerythritol tetrastearate, dipentaerythritol adipic acid stearate, glycerin tri-18-hydroxystearate, or pentaerythritol full stearate. The type of the fatty acid metal salt is not particularly limited, but suitable examples include alkali metal salts such as lithium, sodium, potassium, etc.; alkaline earth metal salts such as magnesium, calcium, barium, etc.; or zinc salts.
[0111] Particularly preferred as the component (E) are fatty acid metal salts (E0) with a free fatty acid content of 5.0% or less, 4.0% or less, and 0.05 to 3.5% fatty acid metal salts and erythritol derivatives. Examples of such components include at least one metal stearate. Specifically, it is most preferred to use a hot melt component with a melting point of 150°C or less selected from calcium stearate (melting point 150°C), zinc stearate (melting point 120°C), magnesium stearate (melting point 130°C), pentaerythritol tetrastearate (melting point 60-70°C), pentaerythritol adipate stearate (melting point 55-61°C), pentaerythritol full stearate (melting point 62-67°C), etc.
[0112] The amount of the (E) component used is in the range of 0.01 to 5.0 parts by mass, and may be 0.01 to 3.5 parts by mass, or 0.01 to 3.0 parts by mass, when the entire composition is taken as 100 parts by mass. If the amount of the (E) component used exceeds the upper limit, the adhesiveness and mechanical strength of the cured product obtained from the curable silicone composition of the present invention may be insufficient. If the amount of the (E) component used is less than the lower limit, sufficient fluidity may not be achieved when heated and melted.
[0113] The composition may also contain other optional components such as a cure retarder and an adhesion promoter, provided that the object of the present invention is not impaired.
[0114] Examples of the curing retarder include alkyne alcohols such as 2-methyl-3-butyn-2-ol, 3,5-dimethyl-1-hexyn-3-ol, 2-phenyl-3-butyn-2-ol, and 1-ethynyl-1-cyclohexanol; enyne compounds such as 3-methyl-3-penten-1-yne and 3,5-dimethyl-3-hexen-1-yne; alkenyl-containing low molecular weight siloxanes such as tetramethyltetravinylcyclotetrasiloxane and tetramethyltetrahexenylcyclotetrasiloxane; and alkynyloxysilanes such as methyl-tris(1,1-dimethylpropynyloxy)silane and vinyl-tris(1,1-dimethylpropynyloxy)silane. The content of this curing retarder is not limited, but is preferably within the range of 10 to 10,000 ppm by mass with respect to the present composition.
[0115] As the adhesion promoter, an organic silicon compound having at least one alkoxy group bonded to a silicon atom in one molecule is preferred. Examples of this alkoxy group include methoxy, ethoxy, propoxy, butoxy, and methoxyethoxy groups, and particularly preferred is methoxy. Examples of groups bonded to silicon atoms other than the alkoxy group in the organic silicon compound include halogen-substituted or unsubstituted monovalent hydrocarbon groups such as alkyl groups, alkenyl groups, aryl groups, aralkyl groups, and halogenated alkyl groups; glycidoxyalkyl groups such as 3-glycidoxypropyl and 4-glycidoxybutyl groups; epoxycyclohexylalkyl groups such as 2-(3,4-epoxycyclohexyl)ethyl and 3-(3,4-epoxycyclohexyl)propyl groups; epoxyalkyl groups such as 3,4-epoxybutyl and 7,8-epoxyoctyl groups; acrylic group-containing monovalent organic groups such as 3-methacryloxypropyl groups; and hydrogen atoms. The organosilicon compound preferably has a group capable of reacting with the alkenyl group or silicon-bonded hydrogen atom in the composition, and more specifically, preferably has a silicon-bonded hydrogen atom or an alkenyl group.In addition, since it can provide good adhesion to various substrates, the organosilicon compound preferably has at least one epoxy-containing monovalent organic group in one molecule.Examples of such organosilicon compounds include organosilane compounds, organosiloxane oligomers, and alkyl silicates.Examples of the molecular structure of the organosiloxane oligomer or alkyl silicate include linear, partially branched linear, branched, cyclic, and net-like, and in particular, linear, branched, and net-like are preferred.Examples of the organosilicon compounds include silane compounds such as 3-glycidoxypropyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and 3-methacryloxypropyltrimethoxysilane; siloxane compounds having at least one silicon-bonded alkenyl group or one silicon-bonded hydrogen atom, and at least one silicon-bonded alkoxy group in one molecule; a mixture of a silane compound or siloxane compound having at least one silicon-bonded alkoxy group and a siloxane compound having at least one silicon-bonded hydroxy group and at least one silicon-bonded alkenyl group in one molecule; a reaction mixture of an amino group-containing organoalkoxysilane and an epoxy group-containing organoalkoxysilane; an organic compound having at least two alkoxysilyl groups in one molecule and containing a bond other than a silicon-oxygen bond between the silyl groups; a n Si(OR b ) 4-n (In the formula, R a is a monovalent epoxy-containing organic group, and R b is an alkyl group having 1 to 6 carbon atoms or a hydrogen atom; and n is a number ranging from 1 to 3. Examples of the adhesion promoter include epoxy group-containing silanes represented by the formula (I) or partial hydrolysis condensates thereof, a reaction mixture of a vinyl group-containing siloxane oligomer (including those with a chain or cyclic structure) and an epoxy group-containing trialkoxysilane, methyl polysilicate, ethyl polysilicate, and epoxy group-containing ethyl polysilicate. The adhesion promoter is preferably a low-viscosity liquid, and although there are no limitations on its viscosity, it is preferably within the range of 1 to 500 mPa·s at 25°C. The content of the adhesion promoter is also not limited, but is preferably within the range of 0.01 to 10 parts by mass per 100 parts by mass of the total of the present composition.
[0116] In the present invention, a particularly suitable adhesion promoter is a reaction mixture of an amino-containing organoalkoxysilane and an epoxy-containing organoalkoxysilane. This component improves the initial adhesion to various substrates that come into contact with the composition during curing, and in particular the low-temperature adhesion to unwashed substrates. Depending on the curing system of the curable silicone composition to which the adhesion promoter is added, the adhesion promoter may also act as a crosslinking agent. Such reaction mixtures are disclosed in JP-B-52-8854 and JP-A-10-195085.
[0117] Examples of alkoxysilanes having an amino group-containing organic group that constitute such a component include aminomethyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)aminomethyltributoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, and 3-anilinopropyltriethoxysilane.
[0118] Examples of epoxy group-containing organoalkoxysilanes include 3-glycidoxyprolyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and 2-(3,4-epoxycyclohexyl)ethylmethyldimethoxysilane.
[0119] The molar ratio of these alkoxysilanes having an amino group-containing organic group to those having an epoxy group-containing organic group is preferably within the range of (1:1.5) to (1:5), and particularly preferably within the range of (1:2) to (1:4). This component (e1) can be easily synthesized by mixing the above-mentioned alkoxysilanes having an amino group-containing organic group and alkoxysilanes having an epoxy group-containing organic group and reacting them at room temperature or under heating.
[0120] In particular, in the present invention, when an alkoxysilane having an amino group-containing organic group is reacted with an alkoxysilane having an epoxy group-containing organic group by the method described in JP-A-10-195085, a cyclic silane having the general formula: [ka] {where, R 1 is an alkyl group, an alkenyl group, or an alkoxy group, and R 2 may have the same or different general formula: [ka] (In the formula, R 4 is an alkylene group or an alkyleneoxyalkylene group, R 5 is a monovalent hydrocarbon group, R 6 is an alkyl group, and R 7 is an alkylene group, and R 8 is an alkyl group, an alkenyl group, or an acyl group, and a is 0, 1, or 2. R is a group selected from the group consisting of groups represented by 3 are the same or different hydrogen atoms or alkyl groups. It is particularly preferred that the compound contains a carbasilatrane derivative represented by the following structure: Examples of such carbasilatrane derivatives include carbasilatrane derivatives having a silicon-bonded alkoxy group or a silicon-bonded alkenyl group in one molecule, as represented by the following structure: [ka] (wherein Rc is a group selected from a methoxy group, an ethoxy group, a vinyl group, an allyl group, and a hexenyl group).
[0121] In the present invention, a silatrane derivative represented by the following structural formula may be used as an adhesion promoter. [ka] R in the formula 1are the same or different hydrogen atoms or alkyl groups, in particular R 1 is preferably a hydrogen atom or a methyl group. 2 represents a hydrogen atom, an alkyl group, or a group of the general formula: -R 4 -Si(OR 5 ) x R 6 (3-x) are the same or different groups selected from the group consisting of alkoxysilyl group-containing organic groups represented by the formula: 2 At least one of R is an alkoxysilyl group-containing organic group. 2 Examples of the alkyl group of R include a methyl group. 2 In the alkoxysilyl group-containing organic group, R 4 is a divalent organic group, and examples thereof include an alkylene group or an alkyleneoxyalkylene group, and particularly preferably an ethylene group, a propylene group, a butylene group, a methyleneoxypropylene group, or a methyleneoxypentylene group. 5 is an alkyl group having 1 to 10 carbon atoms, and is preferably a methyl group or an ethyl group. 6 is a substituted or unsubstituted monovalent hydrocarbon group, preferably a methyl group, and x in the formula is 1, 2, or 3, preferably 3.
[0122] Such an R 2 Examples of the alkoxysilyl group-containing organic group include the following groups. -(CH2)2Si(OCH3)2-(CH2)2Si(OCH3)2CH3 -(CH2)3Si(OC2H5)2-(CH2)3Si(OC2H5)(CH3)2 -CH2O(CH2)3Si(OCH3)3 -CH2O(CH2)3Si(OC2H5)3 -CH2O(CH2)3Si(OCH3)2CH3 -CH2O(CH2)3Si(OC2H5)2CH3 -CH2OCH2Si(OCH3)2-CH2OCH2Si(OCH3)(CH3)2
[0123] R in the above formula 3 is at least one group selected from the group consisting of substituted or unsubstituted monovalent hydrocarbon groups, alkoxy groups having 1 to 10 carbon atoms, glycidoxyalkyl groups, oxiranylalkyl groups, and acyloxyalkyl groups; R 3 Examples of the monovalent hydrocarbon group include alkyl groups such as methyl groups. 3 Examples of the alkoxy group of R include a methoxy group, an ethoxy group, and a propoxy group. 3 An example of the glycidoxyalkyl group of R is a 3-glycidoxypropyl group. 3 Examples of the oxiranylalkyl group of R include a 4-oxiranylbutyl group and an 8-oxiranyloctyl group. 3 Examples of the acyloxyalkyl group include an acetoxypropyl group and a 3-methacryloxypropyl group. 3 Preferably, the alkyl group, alkenyl group, or alkoxy group is used, more preferably an alkyl group or an alkenyl group, and particularly preferably a group selected from a methyl group, a vinyl group, an allyl group, and a hexenyl group.
[0124] Furthermore, the composition may contain other optional components, such as heat resistance agents such as iron oxide (red oxide), cerium oxide, cerium dimethylsilanolate, fatty acid cerium salts, cerium hydroxide, and zirconium compounds, as well as dyes, pigments other than white, and flame retardants, so long as the object of the present invention is not impaired.
[0125] The present composition may be used in the form of granules, pellets, or sheets or films. The pellets are obtained by tableting the present composition, and are excellent in handling and curing properties. The "pellets" are also sometimes called "tablets". The shape of the pellets is not limited, but they are usually spherical, elliptical or cylindrical. The size of the pellets is not limited, but they have an average particle diameter or equivalent circle diameter of, for example, 500 μm or more. When producing such a pellet-like composition, tableting the present composition molded into granules is an efficient production method. When it is desired to make the composition of the present invention into granules, it is possible to produce a granular composition by stirring the components (A) to (C) constituting the curable silicone composition of the present invention together with other additives, if any, using a powder kneader described later, and the obtained granular composition can be tableted to produce a pellet-like composition.
[0126] The present curable silicone composition is a non-flowable solid at 25°C. Here, non-flowable means that it does not deform and / or flow in the absence of external force, and preferably, when the present cured silicone composition is molded into pellets, tablets, etc., it does not deform and / or flow in the absence of external force at 25°C. Such non-flowable can be evaluated, for example, by placing the molded composition on a hot plate at 25°C and not substantially deforming and / or flowing the composition even when no external force is applied to the composition or a certain load is applied to the composition. When the composition is non-flowable at 25°C, the shape retention of the composition at that temperature is good and the surface adhesion is low, so that the composition can be easily handled even in an uncured state.
[0127] The softening point of the composition is preferably 100° C. or lower. The softening point means the temperature at which, when a 2 cm-high composition is pressed from above on a hot plate with a load of 100 grams for 10 seconds, and the deformation of the composition is measured after the load is removed, the deformation in the height direction is 1 mm or more.
[0128] The viscosity of the present composition tends to decrease rapidly with increasing temperature under high temperature and pressure (i.e., for example, in the manufacturing process of the laminate described above), and it is preferable to use a value measured under high temperature and pressure similar to the conditions when the present composition is actually used as a useful melt viscosity value for handling the composition. Therefore, it is preferable to measure the melt viscosity of the present composition under high pressure using a Koka-shiki flow tester (manufactured by Shimadzu Corporation) rather than measuring it with a rotational viscometer such as a rheometer. Specifically, it is preferable that the melt viscosity of the present composition at 150°C measured using a Koka-shiki flow tester is 200 Pa·s or less, more preferably 150 or less. This is because the adhesion of the present composition to the substrate is good after the present composition is cooled to 25°C after hot melting (i.e., after being heated and melted).
[0129] [Method of producing the curable silicone composition] The composition can be produced by powder mixing components (A) to (C), and optionally other optional components, at a temperature below 50°C, further heating and melting to mix the components uniformly, and then cooling as necessary, but the composition may be produced by any method without being limited to this method. The powder mixer that can be used in the production method is not particularly limited, but examples include single- or double-screw continuous mixers, two-roll mixers, Ross mixers, Hobart mixers, dental mixers, planetary mixers, kneader mixers, laboratory millers, small grinders, and Henschel mixers, with laboratory millers and Henschel mixers being preferred.
[0130] [Manufacturing method of curable silicone sheet] A curable silicone sheet having hot melt properties made from the present composition may be produced by, but is not limited to, the following production method, using organopolysiloxane resin fine particles as a raw material (Method A), or by dispersing an organopolysiloxane resin that is solid at room temperature, and optionally a chain diorganopolysiloxane, in an organic solvent, and then removing the organic solvent, using the resulting hot melt solid as a raw material (hot bulk method) (Method B). Specifically, the former (Method A) comprises the following steps: Step 1: mixing organopolysiloxane resin microparticles, a curing agent, and optionally a functional filler; Step 2: kneading the mixture obtained in step 1 while heating and melting it at a temperature of 120°C or less; Step 3: Laminating the heated, melted and kneaded mixture obtained in step 2 between two films, each having at least one release surface, to form a laminate; Step 4: stretching the mixture in the laminate obtained in step 3 between rolls to form a curable hot-melt silicone sheet having a specific thickness; The manufacturing method includes:
[0131] On the other hand, the latter (Method B) comprises the following steps: Step 1: A step of obtaining a hot-melt solid content by removing the organic solvent at a temperature of 150° C. or higher from a solution in which an organopolysiloxane resin that is solid at room temperature and, optionally, a linear diorganopolysiloxane are dispersed or dissolved in an organic solvent; Step 2: adding all the curing agents to the hot-melt solid obtained in step 1, and then kneading the mixture while heating and melting it at a temperature of 120°C or less; Step 3: Laminating the heated and melted mixture obtained in step 2 between two films, each having at least one release surface, to form a laminate; Step 4: A step of stretching the mixture in the laminate obtained in step 3 between rolls to form a curable hot melt silicone sheet having a specific thickness. The manufacturing method includes:
[0132] In either manufacturing method (Method A or Method B), steps 3 and 4 may be continuous and integrated steps, for example, the mixture obtained after heating and melting in step 2 may be laminated by being discharged or applied between films having at least one release surface directly below the rolls, and at the same time, the gap between the rolls may be adjusted to stretch the film to a specific thickness. In this way, a manufacturing method having a substantially integrated process of steps 3 and 4 is also included in the scope of the above manufacturing method. That is, steps 3 and 4 may be performed continuously and integrally by discharging or applying the mixture obtained in step 2 between two release films to sandwich the mixture between the two release films, for example, between two long release films, and passing the resulting laminate consisting of the two release films and the mixture sandwiched between them between rolls to stretch and mold the mixture between the release films and adjust the thickness to a predetermined value to obtain the desired laminate. Such a method of performing steps 3 and 4 integrally is also included in the above-mentioned production method.
[0133] In step 3 of the above-mentioned method A or method B, the step of laminating the mixture after heat melting between films is not particularly limited, and may be a step of (i) discharging or applying the mixture after heat melting from step 2 onto a first release film having a release surface, and then contacting the second release film with the surface of the mixture opposite to the surface contacting the first release film to interpose the mixture after heat melting between the first release film and the second release film, i.e., sandwiching the mixture, or (ii) discharging or applying the mixture after heat melting from step 2 between the first release film and the second release film having a release surface to interpose the mixture after heat melting between both release films. (ii) can be exemplified by a method in which the first and second release films are brought close to each other by an appropriate means, such as two rolls, and the mixture from step 2 is discharged or applied at the location where the two release films are close to each other, and the mixture is simultaneously or almost simultaneously sandwiched between the gap between the two release films. It is particularly preferable that the above-mentioned steps 3 and 4 are continuous steps.
[0134] Regarding these manufacturing methods, the applicants have proposed the entire process, including the manufacturing method and manufacturing apparatus used therefor, for curable silicone sheets in Japanese Patent Application No. 2019-167832, Japanese Patent Application No. 2019-167833, and their priority applications. In the present invention, these methods and manufacturing apparatus can be applied when forming the curable hot-melt silicone composition into a sheet or film.
[0135] There are no particular limitations on the type of film-like substrate used in producing a curable silicone sheet having hot melt properties, and suitable materials include polyester films, polyolefin films, polycarbonate films, acrylic films, etc. It is preferable for the sheet-like substrate to be non-porous.
[0136] The release layer is a necessary component for easily peeling off the sheet-like member made of the curable silicone composition from the film-like substrate, and may be called a release liner, separator, release layer, or release coating layer.Preferably, the release layer may be a release layer having release coating ability such as a silicone-based release agent, a fluorine-based release agent, an alkyd-based release agent, or a fluorosilicone-based release agent, or may be a substrate itself that forms physically fine irregularities on the substrate surface, or is difficult to adhere to the adhesive layer made of the curable reactive silicone composition of the present invention or its cured product.In particular, in the laminate of the present invention, it is preferable to use a release layer made by curing a fluorosilicone-based release agent as the release layer.
[0137] The above laminate can be used, for example, by applying a sheet-like member made of the curable silicone composition to an adherend and then peeling the uncured sheet-like member from the film-like substrate.
[0138] Here, the sheet-like member made of the curable silicone composition may be a film-like adhesive having a thickness of 1 mm or less. That is, the laminate may include a peelable film-like adhesive held by a base film, and is preferred. The film-like adhesive has hot melt properties, and may be an adhesive used for temporary fixing of semiconductor members, or may be used as a die attachment film.
[0139] Furthermore, a sheet-like member made of the curable silicone composition may be directly molded into a substrate by compression molding or press molding, and in this case, molding may be performed while leaving the film-like substrate on one side in place, and this may be used as a release film to prevent adhesion to the mold during molding.
[0140] [Curable silicone sheet] The curable silicone sheet obtained by the above manufacturing method is a curable silicone composition that contains at least an organopolysiloxane resin, an optional chain-like organopolysiloxane, and a curing agent, and may further contain a functional filler or other components. It has hot melt properties and can be used as a heat-melting adhesive material, and forms a silicone cured product with excellent heat resistance and stress relaxation by curing. In particular, the curable silicone sheet has excellent moldability, gap filling properties, and adhesive strength / adhesive strength, and can be used as a die attachment film or a film adhesive. It can also be suitably used as a curable silicone sheet that forms a sealing layer by compression molding, press molding, or vacuum lamination. Regardless of the purpose of use, the curable silicone sheet is a sheet-like product with hot melt properties, so it can be suitably applied to adhesion and sealing of a large area.
[0141] Specifically, the curable silicone sheet obtained by the above-mentioned manufacturing method is peeled off from the release film, and then placed on a desired portion of a semiconductor or the like, and a film adhesive layer that utilizes the gap filling property for unevenness and gaps is formed on the adherend, and the adherends are temporarily fixed, placed, and bonded together, and the curable silicone sheet is heated to 150°C or higher to bond the adherends with the cured product of the curable silicone sheet. The release film may be peeled off after the curable silicone sheet is heated to form a cured product, and such use is preferable when used as a layer for sealing a substrate such as a semiconductor. The timing of peeling may be selected according to the application and method of use of the curable silicone sheet.
[0142] Since the curable silicone sheet is hot-melt, it can be softened or fluidized by heating the sheet before final curing, and even if the adherend has unevenness on its surface, it can fill the unevenness and gaps without gaps to form an adhesive surface.As a heating means for the curable silicone sheet, for example, various thermostatic baths, hot plates, electromagnetic heating devices, heating rolls, etc. can be used.In order to perform lamination and heating more efficiently, for example, an electric heating press, a diaphragm type laminator, a roll laminator, etc. are preferably used.
[0143] As described above, the curable silicone sheet according to the present invention has excellent gap-filling properties when melted and excellent flexibility of the cured product at room temperature to high temperatures, and therefore can be very suitably used in a molding method including a covering step (so-called mold underfill method) in which the cured product is used to simultaneously overmold and underfill a semiconductor element including an optical semiconductor. Furthermore, due to the above-mentioned properties, the composition can be suitably used in a molding method including a covering step (so-called wafer molding) in which the surface of a semiconductor wafer substrate carrying a single or multiple semiconductor elements is covered and overmolded so that the gaps between the semiconductor elements are filled with the cured product.
[0144] In the above steps, it is possible to use a compression molding machine, an injection molding machine, an auxiliary ram molding machine, a slide molding machine, a double ram molding machine, or a low pressure encapsulation molding machine, a heat press, a vacuum laminator, etc. In particular, the curable silicone sheet according to the present invention can be suitably used for the purpose of obtaining a cured product by press molding, compression molding, and vacuum lamination.
[0145] The optimum temperature for thermally curing the curable silicone sheet can be selected according to the curing system. For hydrosilylation reactions, temperatures of 150°C or higher are preferred, and for organic peroxide curing, temperatures of 170°C or higher are preferred.
[0146] Since the curable silicone sheet according to the present invention is suitable as a protective material for semiconductors and the like, it is preferable that the cured product obtained by curing the curable silicone sheet according to the present invention has a Type D durometer hardness at 25° C. of at least 20. This Type D durometer hardness is determined using a Type D durometer in accordance with JIS K 6253-1997 "Testing method for hardness of vulcanized rubber and thermoplastic rubber."
[0147] Furthermore, since the composition is suitable as an encapsulating material for semiconductors in flexible applications where flexibility is required, it is preferable that the bending elongation of the cured product measured by the method specified in JIS K 6911-1995 "General testing methods for thermosetting plastics" is 2% or more, or 4% or more.
[0148] [Uses of the curable silicone sheet according to the present invention] The curable silicone sheet according to the present invention has hot melt properties and is excellent in gap filling properties, handling workability and curing properties when melted (hot melt), so it is suitable as a sealant or underfill agent for semiconductors; a sealant or underfill agent for power semiconductors such as SiC and GaN; a sealant or light reflector for optical semiconductors such as light-emitting diodes, photodiodes, phototransistors and laser diodes; and an adhesive, potting agent, protective agent and coating agent for electrical and electronic devices. In addition, since the composition has hot melt properties, it is also suitable as a material for molding by press molding, compression molding or vacuum lamination. In particular, it is suitable for use as a sealant for semiconductors that use a mold underfill method or a wafer molding method during molding.
[0149] In particular, the curable silicone sheet according to the present invention can be used for sealing large areas of semiconductor substrates (including wafers and optical semiconductor substrates). Furthermore, sheets obtained by molding the curable silicone composition of the present invention into a sheet shape can be used as die attach films, sealing flexible devices, and stress relief layers for bonding two different substrates, such as a large-area substrate and a panel, or between panels.
[0150] [Uses of the cured product of the curable silicone sheet according to the present invention] Although there are no particular limitations on the applications of the cured product of the present invention, the composition of the present invention has hot melt properties, excellent moldability and gap fill properties, and the cured product has the above-mentioned flexibility at room temperature, high stress relaxation properties, bending elongation, etc. Therefore, the cured product obtained by curing the present composition can be suitably used as a member for semiconductor device, and can be suitably used as an encapsulant for semiconductor elements including optical semiconductors and IC chips, a light reflector for optical semiconductor devices, an adhesive / bonding member for semiconductor devices, and an adhesive / bonding member for display panels.
[0151] The semiconductor device having a member made of the above-mentioned cured product is not particularly limited, but is particularly preferably a power semiconductor device, an optical semiconductor device, or a semiconductor device mounted on a flexible circuit board.
[0152] [Molding method for the cured product] The present composition can be cured by a method comprising at least the following steps (I) to (III). (I) heating the composition to 100° C. or higher to melt it; (II) a step of injecting the curable silicone composition obtained in step (I) into a mold, or a step of spreading the curable silicone composition obtained in step (I) throughout the mold by clamping the mold; and (III) A step of curing the curable silicone composition injected in the step (II)
[0153] In the above steps, a transfer molding machine, a compression molding machine, an injection molding machine, an auxiliary ram type molding machine, a slide type molding machine, a double ram type molding machine, a low pressure encapsulation molding machine, a vacuum laminator, etc. can be used. In particular, the composition of the present invention can be suitably used for the purpose of obtaining a cured product by transfer molding, compression molding, press molding, or a vacuum laminator.
[0154] Finally, in step (III), the curable silicone composition injected (applied) in step (II) is cured. When (c1) an organic peroxide is used as component (C), the heating temperature is preferably 150°C or higher, or 170°C or higher, and when (c2) an organohydrogenpolysiloxane having at least two silicon-bonded hydrogen atoms in the molecule and a hydrosilylation reaction catalyst are used, the heating temperature is preferably 100°C or higher, or 130°C or higher. EXAMPLES
[0155] The hot-melt curable silicone composition of the present invention and its manufacturing method will be described in detail with reference to examples and comparative examples. In the formula, Me and Vi represent a methyl group and a vinyl group, respectively. The softening point of the curable silicone composition of each example and comparative example was measured by the following method. The curable silicone composition was heated at 150°C for 2 hours to prepare a cured product, and the elastic modulus (initial and after standing at 150°C for 1000 hours) was measured by the following method. The results are shown in Table 1.
[0156] [Softening point] The curable silicone composition was molded into a cylindrical pellet of φ14 mm×22 mm. The pellet was placed on a hot plate set at 25° C. to 100° C., and pressed from above with a load of 100 grams for 10 seconds. After removing the load, the deformation of the pellet was measured. The temperature at which the deformation in the height direction became 1 mm or more was taken as the softening point.
[0157] [Storage modulus] The curable silicone composition was heated at 150°C for 2 hours to produce a cured product (initial cured product). This cured product was left in an oven set at 150°C for 1000 hours to produce a cured product after aging. The storage modulus of these cured products from -50°C to 250°C was measured using a rheometer ARES (manufactured by TA Instruments Japan, Inc.), and the values at 25°C were read. Table 1 shows the measured values at 25°C.
[0158] Organopolysiloxane resins containing a hydrosilylation catalyst were prepared by the methods shown in Reference Examples 1 and 2 below, and the presence or absence of hot melt properties was evaluated based on the presence or absence of softening point / melt viscosity. Also, organopolysiloxane resin fine particles were prepared by the methods shown in Reference Examples 3 to 10, and their loss on heating (= mass loss rate) was evaluated. In the Reference Examples, 1,1,3,3-tetramethyl-1,3-divinyldisiloxane used in the platinum complex, which is a hydrosilylation catalyst, is referred to as "1,3-divinyltetramethyldisiloxane."
[0159] [Reference example 1] In a 1 L flask, at 25°C, a white solid was obtained with the average unit formula: (Me2ViSiO 1 / 2 ) 0.05 (Me3SiO 1 / 2 ) 0.39 (SiO 4 / 2 ) 0.56 (HO 1 / 2 ) 0.02 270.5 g of a 55 mass % xylene solution of an organopolysiloxane resin represented by the formula (1) and 0.375 g of a 1,3-divinyltetramethyldisiloxane solution of a platinum 1,3-divinyltetramethyldisiloxane complex (platinum metal content = about 4000 ppm) were added and stirred uniformly at room temperature (25°C) to prepare a xylene solution of organopolysiloxane resin (1) containing 10 ppm by mass as platinum metal. Furthermore, this organopolysiloxane resin (1) did not soften / melt even when heated to 200°C, and did not have hot melt properties.
[0160] [Reference example 2] In a 1 L flask, at 25°C, a white solid was obtained with the average unit formula: (Me3SiO 1 / 2 ) 0.44 (SiO 4 / 2 ) 0.56 (HO 1 / 2 ) 0.02 270.5 g of a 55 mass % xylene solution of an organopolysiloxane resin represented by the formula (1) and 0.375 g of a 1,3-divinyltetramethyldisiloxane solution of a platinum 1,3-divinyltetramethyldisiloxane complex (platinum metal content = approximately 4000 ppm) were added and stirred uniformly at room temperature (25°C) to prepare a xylene solution of organopolysiloxane resin (2) containing 10 ppm by mass as platinum metal. Furthermore, this organopolysiloxane resin (2) did not soften / melt even when heated to 200°C, and did not have hot melt properties.
[0161] [Reference Example 3: Non-hot melt organopolysiloxane resin fine particles (1)] The xylene solution of the organopolysiloxane resin (1) prepared in Reference Example 1 was granulated at 50°C by a spray method using a spray dryer while removing the xylene, to prepare spherical non-hot melt organopolysiloxane resin microparticles (1). When the microparticles were observed with an optical microscope, the particle size was 5 to 10 μm, and the average particle size was 6.9 μm. When the microparticles were exposed to 200°C for 1 hour, the heat loss was 4.7 wt%.
[0162] [Reference Example 4: Non-hot melt organopolysiloxane resin fine particles (2)] The organopolysiloxane resin microparticles prepared in Reference Example 3 were aged for 4 hours in an oven set at 120°C to prepare spherical non-hot melt organopolysiloxane resin microparticles (2). When these microparticles were observed with an optical microscope, the particle diameter was 5 to 10 μm, and no aggregation due to aging was observed. In addition, when these microparticles were exposed to 200°C for 1 hour, the heat loss was 2.3 wt%.
[0163] [Reference Example 5: Non-hot melt organopolysiloxane resin fine particles (3)] The organopolysiloxane resin microparticles prepared in Reference Example 3 were aged for 8 hours in an oven set at 120°C to prepare spherical non-hot melt organopolysiloxane resin microparticles (3). When these microparticles were observed with an optical microscope, the particle diameter was 5 to 10 μm, and no aggregation due to aging was observed. In addition, when these microparticles were exposed to 200°C for 1 hour, the heat loss was 1.3 wt%.
[0164] [Reference Example 6: Non-hot melt organopolysiloxane resin fine particles (4)] The organopolysiloxane resin microparticles prepared in Reference Example 3 were aged for 24 hours in an oven set at 120°C to prepare spherical non-hot melt organopolysiloxane resin microparticles (4). When these microparticles were observed with an optical microscope, the particle diameter was 5 to 10 μm, and no aggregation due to aging was observed. In addition, when these microparticles were exposed to 200°C for 1 hour, the heat loss was 0.7 wt%.
[0165] [Reference Example 7: Non-hot melt organopolysiloxane resin fine particles (5)] The xylene solution of the organopolysiloxane resin (2) prepared in Reference Example 2 was granulated at 50°C by a spray method using a spray dryer while removing the xylene, to prepare spherical non-hot melt organopolysiloxane resin microparticles (5). When the microparticles were observed with an optical microscope, the particle size was 5 to 10 μm, and the average particle size was 7.4 μm. When the microparticles were exposed to 200°C for 1 hour, the heat loss was 4.8 wt%.
[0166] [Reference Example 8: Non-hot melt organopolysiloxane resin fine particles (6)] The organopolysiloxane resin microparticles prepared in Reference Example 7 were aged for 4 hours in an oven set at 120°C to prepare spherical non-hot melt organopolysiloxane resin microparticles (2). When these microparticles were observed with an optical microscope, the particle diameter was 5 to 10 μm, and no aggregation due to aging was observed. In addition, when these microparticles were exposed to 200°C for 1 hour, the heat loss was 2.1 wt%.
[0167] [Reference Example 9: Non-hot melt organopolysiloxane resin fine particles (7)] The organopolysiloxane resin microparticles prepared in Reference Example 7 were aged for 8 hours in an oven set at 120°C to prepare spherical non-hot melt organopolysiloxane resin microparticles (7). When these microparticles were observed with an optical microscope, the particle diameter was 5 to 10 μm, and no aggregation due to aging was observed. In addition, when these microparticles were exposed to 200°C for 1 hour, the heat loss was 1.2 wt%.
[0168] [Reference Example 10: Non-hot melt organopolysiloxane resin fine particles (8)] The organopolysiloxane resin microparticles prepared in Reference Example 7 were aged for 24 hours in an oven set at 120°C to prepare spherical non-hot melt organopolysiloxane resin microparticles (8). When these microparticles were observed with an optical microscope, the particle diameter was 5 to 10 μm, and no aggregation due to aging was observed. In addition, when these microparticles were exposed to 200°C for 1 hour, the heat loss was 0.8 wt%.
[0169] [Example 1] Non-hot melt organopolysiloxane resin fine particles (7) (vinyl group content = 0 mass%) 67.0 g, formula: ViMe2SiO(Me2SiO) 800 SiViMe2 33.0 g of dimethylpolysiloxane terminated at both molecular chain ends with dimethylvinylsiloxy groups (vinyl group content = 0.09% by mass), formula: Me3SiO(MeHSiO)7(Me2SiO) 6.5 SiMe3 0.21 g of an organohydrogenpolysiloxane represented by the formula {the amount of silicon-bonded hydrogen atoms in the organohydrogenpolysiloxane is 1.3 moles per mole of vinyl groups in the dimethylpolysiloxane terminally blocked with dimethylvinylsiloxy groups}, 234.4 g of alumina with an average particle size of 0.44 μm (AES-12 manufactured by Sumitomo Chemical Co., Ltd.); 1-ethynyl-1-cyclohexanol (in an amount equivalent to 1000 ppm by mass of the composition) was added all at once to a small grinder and stirred at room temperature (25°C) for 1 minute to prepare a uniform curable granular silicone composition. Additionally, the results of measuring the softening point and other properties of this composition are shown in Table 1.
[0170] [Example 2] Non-hot melt organopolysiloxane resin fine particles (7) (vinyl group content = 0 mass%) 63.3 g, 3.5 g of non-hot melt organopolysiloxane resin fine particles (3) (vinyl group content = 1.91% by mass), formula: ViMe2SiO(Me2SiO) 800 SiViMe2 33.2 g of dimethylpolysiloxane terminated at both molecular chain ends with dimethylvinylsiloxy groups (vinyl group content = 0.09% by mass), formula: Me3SiO(MeHSiO)7(Me2SiO) 6.5 SiMe3 0.6 g of an organohydrogenpolysiloxane represented by the formula {an amount such that the organohydrogenpolysiloxane contains 1.2 moles of silicon-bonded hydrogen atoms per mole of vinyl groups in the organopolysiloxane resin fine particle (3) and the dimethylpolysiloxane terminally blocked with dimethylvinylsiloxy groups}, 218.4 g of alumina with an average particle size of 0.44 μm (AES-12 manufactured by Sumitomo Chemical Co., Ltd.); 1-ethynyl-1-cyclohexanol (in an amount equivalent to 1000 ppm by mass of the composition) was added all at once to a small grinder and stirred at room temperature (25°C) for 1 minute to prepare a uniform curable granular silicone composition. Additionally, the results of measuring the softening point and other properties of this composition are shown in Table 1.
[0171] [Example 3] Non-hot melt organopolysiloxane resin fine particles (8) (vinyl group content = 0 mass%) 60.2 g, 7.0 g of non-hot melt organopolysiloxane resin fine particles (4) (vinyl group content = 1.91% by mass), formula: ViMe2SiO(Me2SiO) 800 SiViMe2 32.8 g of dimethylpolysiloxane terminated at both molecular chain ends with dimethylvinylsiloxy groups (vinyl group content = 0.09% by mass), formula: (HMeSiO 1 / 2 ) 0.67 (SiO 4 / 2 ) 0.33 0.65g of organohydrogenpolysiloxane resin (content of silicon-bonded hydrogen atoms = 0.95% by mass) {an amount such that the organohydrogenpolysiloxane resin contains 1.0 mole of silicon-bonded hydrogen atoms per mole of vinyl groups in the organopolysiloxane resin fine particles (4) and the dimethylpolysiloxane terminally blocked with dimethylvinylsiloxy groups}, 273.0 g of alumina with an average particle size of 0.44 μm (AES-12 manufactured by Sumitomo Chemical Co., Ltd.); 1-ethynyl-1-cyclohexanol (in an amount equivalent to 1000 ppm by mass of the composition) was added all at once to a small grinder and stirred at room temperature (25°C) for 1 minute to prepare a uniform curable granular silicone composition. Additionally, the results of measuring the softening point and other properties of this composition are shown in Table 1.
[0172] [Example 4] Non-hot melt organopolysiloxane resin fine particles (8) (vinyl group content = 0 mass%) 56.4 g, Non-hot melt organopolysiloxane resin fine particles (4) (vinyl group content = 1.91% by mass) 10.3 g, formula: ViMe2SiO(Me2SiO) 800 SiViMe2 33.3 g of dimethylpolysiloxane terminated at both molecular chain ends with dimethylvinylsiloxy groups (vinyl group content = 0.09% by mass), formula: Me3SiO(MeHSiO)7(Me2SiO) 6.5 SiMe3 1.57 g of an organohydrogenpolysiloxane represented by the formula {an amount such that the number of silicon-bonded hydrogen atoms in the organohydrogenpolysiloxane is 1.3 moles per mole of vinyl groups in the organopolysiloxane resin fine particle (4) and the dimethylpolysiloxane capped at both molecular chain terminals with dimethylvinylsiloxy groups}, 203.1 g of alumina (AES-12 manufactured by Sumitomo Chemical) with an average particle size of 0.44 μm; 1-ethynyl-1-cyclohexanol (in an amount equivalent to 1000 ppm by mass of the composition) was added all at once to a small grinder and stirred at room temperature (25°C) for 1 minute to prepare a uniform curable granular silicone composition. Additionally, the results of measuring the softening point and other properties of this composition are shown in Table 1.
[0173] [Example 5] 30.5 g of non-hot melt organopolysiloxane resin fine particles (8) (vinyl group content = 0 mass%), 32.5 g of non-hot melt organopolysiloxane resin fine particles (4) (vinyl group content = 1.91% by mass), formula: ViMe2SiO(Me2SiO) 800 SiViMe2 30.0 g of dimethylpolysiloxane terminated at both molecular chain ends with dimethylvinylsiloxy groups (vinyl group content = 0.09% by mass), formula: Me3SiO(MeHSiO)7(Me2SiO) 6.5 SiMe3 2.0 g of an organohydrogenpolysiloxane represented by the formula: formula: HMe2SiO(Me2SiO) 17 SiMe2H 5.0g of organohydrogenpolysiloxane represented by the formula {the amount of the two organohydrogenpolysiloxanes such that the number of silicon-bonded hydrogen atoms is 0.9 moles per mole of vinyl groups in the organopolysiloxane resin fine particle (4) and the dimethylpolysiloxane capped at both molecular chain terminals with dimethylvinylsiloxy groups}, 1-ethynyl-1-cyclohexanol (in an amount equivalent to 1000 ppm by mass of the composition) was added all at once to a small grinder and stirred at room temperature (25°C) for 1 minute to prepare a uniform curable granular silicone composition. Additionally, the results of measuring the softening point and other properties of this composition are shown in Table 1.
[0174] [Comparative Example 1] Non-hot melt organopolysiloxane resin fine particles (5) (vinyl group content = 0 mass%) 69.8 g, formula: ViMe2SiO(Me2SiO) 800 SiViMe2 29.9 g of dimethylpolysiloxane terminated at both molecular chain ends with dimethylvinylsiloxy groups (vinyl group content = 0.09% by mass), formula: Me3SiO(MeHSiO)7(Me2SiO) 6.5 SiMe3 0.2 g of an organohydrogenpolysiloxane represented by the formula {the amount of silicon-bonded hydrogen atoms in the organohydrogenpolysiloxane resin is 1.4 moles per mole of vinyl groups in the dimethylpolysiloxane terminally blocked with dimethylvinylsiloxy groups}, 234.4 g of alumina with an average particle size of 0.44 μm (AES-12 manufactured by Sumitomo Chemical Co., Ltd.); 1-ethynyl-1-cyclohexanol (in an amount equivalent to 1000 ppm by mass of the composition) was added all at once to a small grinder and stirred at room temperature (25°C) for 1 minute to prepare a uniform curable granular silicone composition. Additionally, the results of measuring the softening point and other properties of this composition are shown in Table 1.
[0175] [Comparative Example 2] Non-hot melt organopolysiloxane resin fine particles (5) (vinyl group content = 0 mass%) 66.0 g, 3.0 g of non-hot melt organopolysiloxane resin fine particles (1) (vinyl group content = 1.91% by mass), formula: ViMe2SiO(Me2SiO) 800 SiViMe2 29.8 g of dimethylpolysiloxane terminated at both molecular chain ends with dimethylvinylsiloxy groups (vinyl group content = 0.09% by mass), formula: Me3SiO(MeHSiO)7(Me2SiO) 6.5 SiMe3 0.6 g of an organohydrogenpolysiloxane represented by the formula {an amount such that the organohydrogenpolysiloxane contains 1.2 moles of silicon-bonded hydrogen atoms per mole of vinyl groups in the organopolysiloxane resin fine particle (1) and the dimethylpolysiloxane terminally blocked with dimethylvinylsiloxy groups}, 218.4 g of alumina with an average particle size of 0.44 μm (AES-12 manufactured by Sumitomo Chemical Co., Ltd.); 1-ethynyl-1-cyclohexanol (in an amount equivalent to 1000 ppm by mass of the composition) was added all at once to a small grinder and stirred at room temperature (25°C) for 1 minute to prepare a uniform curable granular silicone composition. Additionally, the results of measuring the softening point and other properties of this composition are shown in Table 1.
[0176] [Comparative Example 3] Non-hot melt organopolysiloxane resin fine particles (6) (vinyl group content = 0 mass%) 62.5 g, Non-hot melt organopolysiloxane resin fine particles (2) (vinyl group content = 1.91% by mass) 7.0 g, formula: ViMe2SiO(Me2SiO) 800 SiViMe2 29.8 g of dimethylpolysiloxane terminated at both molecular chain ends with dimethylvinylsiloxy groups (vinyl group content = 0.44% by mass), formula: (HMeSiO 1 / 2 ) 0.67 (SiO 4 / 2 ) 0.33 0.65g of organohydrogenpolysiloxane resin (content of silicon-bonded hydrogen atoms = 0.95% by mass) {an amount such that the amount of silicon-bonded hydrogen atoms in the organohydrogenpolysiloxane is 1.0 mole per mole of vinyl groups in the organopolysiloxane resin fine particle (2) and the dimethylpolysiloxane terminally blocked with dimethylvinylsiloxy groups}, 273.0 g of alumina with an average particle size of 0.44 μm (AES-12 manufactured by Sumitomo Chemical Co., Ltd.); 1-ethynyl-1-cyclohexanol (in an amount equivalent to 1000 ppm by mass of the composition) was added all at once to a small grinder and stirred at room temperature (25°C) for 1 minute to prepare a uniform curable granular silicone composition. Additionally, the results of measuring the softening point and other properties of this composition are shown in Table 1.
[0177] [Comparative Example 4] Non-hot melt organopolysiloxane resin fine particles (5) (vinyl group content = 0 mass%) 32.5 g, Non-hot melt organopolysiloxane resin fine particles (1) (vinyl group content = 1.91% by mass) 32.5 g, formula: ViMe2SiO(Me2SiO) 800 SiViMe2 28.0 g of dimethylpolysiloxane terminated at both molecular chain ends with dimethylvinylsiloxy groups (vinyl group content = 0.09% by mass), formula: Me3SiO(MeHSiO)7(Me2SiO) 6.5 SiMe3 2.0 g of an organohydrogenpolysiloxane represented by the formula: formula: HMe2SiO(Me2SiO) 17 SiMe2H 5.0 g of an organohydrogenpolysiloxane represented by the formula: {the amount of the two organohydrogenpolysiloxanes is 0.9 moles of silicon-bonded hydrogen atoms per mole of vinyl groups in the organopolysiloxane resin fine particle (1) and the dimethylpolysiloxane capped at both molecular chain terminals with dimethylvinylsiloxy groups}, 1-ethynyl-1-cyclohexanol (in an amount equivalent to 1000 ppm by mass of the composition) was added all at once to a small grinder and stirred at room temperature (25°C) for 1 minute to prepare a uniform curable granular silicone composition. Additionally, the results of measuring the softening point and other properties of this composition are shown in Table 1. [Table 1]
[0178] [Summary] The curable silicone compositions of Examples 1 to 5 according to the present invention are hot-melt compositions using an organopolysiloxane resin with a weight loss rate of 2.0% by mass and having a softening point of 100°C or less, and the cured products thereof did not show a significant increase in storage modulus even when left at 150°C for 1000 hours. From this, it was found that the cured products obtained using the compositions according to each Example tend to be inhibited from hardening by high-temperature storage and maintain flexibility. Therefore, it is considered that the compositions are particularly suitable for applications in which they are integrally molded with a substrate and used at high temperatures.
[0179] On the other hand, in all of Comparative Examples 1 to 4, the weight loss rate of the organopolysiloxane resin component after standing at 200° C. for 1 hour was 2% by mass or more, and cured products having softening points and initial storage moduli similar to those of the respective Examples were obtained, but a significant increase in the storage modulus was confirmed when the resulting cured products were left for 1000 hours at 150° C. This indicates that the compositions in the comparative experiments tend to become hard and brittle when stored at high temperatures.
[0180] <Production Example 1> The granulated curable silicone composition of Example 1 or the like is heated to 80°C, and is melt-kneaded by using a twin-screw extruder, and is fed in the form of a semi-solid softened material onto a release film (FL2-01, manufactured by Takara Corporation) at a feed rate of 5 kg / hour, and is laminated between two release films. The laminate is then stretched between rolls to form a laminate in which a hot-melt curable silicone sheet having a thickness of 500 μm is laminated between two release films, and the whole is cooled by a cooling roll set at −15°C. The release film is separated from the laminate to obtain a flat and homogeneous hot-melt curable silicone sheet.
[0181] <Production Example 2> The granulated curable silicone composition of Example 1 and the like is heated to 80°C, melted and kneaded using a twin-screw extruder, and molded into a roughly sheet-like shape using a T-shaped die (opening size: 800 μm×100 mm, heated to 80°C), while being fed onto a release film (FL2-01, manufactured by Takara Corporation) at a feed rate of 5 kg / hour, and the whole is cooled by a cooling roll set to −15°C, and then laminated between two release films. The laminate is then stretched between rolls to form a laminate in which a 500 μm-thick hot-melt curable silicone sheet is laminated between two release films. In the laminate, the release film is separated to obtain a flat and homogeneous hot-melt curable silicone sheet.
[0182] <Production Example 3> At 25°C it is a white solid, with the average formula: (Me2ViSiO 1 / 2 ) 0.05 (Me3SiO 1 / 2 ) 0.39 (SiO 4 / 2 ) 0.56 (HO 1 / 2 ) 0.02 3.76 kg of an organopolysiloxane resin (vinyl group content = 1.9% by mass) represented by the formula At 25°C it is a white solid, with the average formula: (Me3SiO 1 / 2 ) 0.44 (SiO 4 / 2 ) 0.56 (HO 1 / 2 ) 0.02 3.08 kg of an organopolysiloxane resin (vinyl group content = 0 mass%) represented by the formula: ViMe2SiO(Me2SiO) 800 SiViMe2 2.56 kg of dimethylpolysiloxane terminated at both molecular chain ends with dimethylvinylsiloxy groups (vinyl group content = 0.09% by mass), was dissolved in 4.00 kg of xylene using a three-one motor in a pail can. The resulting solution was fed into a twin-screw extruder with a maximum temperature set to 230°C, and the xylene and low molecular weight organopolysiloxane components were removed under a vacuum of -0.08 MPa, yielding a transparent hot-melt mixture 1. Mixture 1 was received in a round-bottom pail can and cooled as is to solidify. The amount of volatile components in this mixture was measured at 200°C for 1 hour, and was found to be 0.7% by mass. The resulting hot-melt mixture 1 was then fed to a twin-screw extruder at 170° C. using a hot melter for cylindrical pails (VersaPail melter manufactured by Nordson Corporation) from line 1 shown in FIG. 1 at a rate of 9.67 kg / hr. next, formula: Me3SiO(Me2SiO) 37 (MeHSiO) 37 Sim 23 Organohydrogenpolysiloxane represented by 0.500 kg / hr, 1-ethynyl-1-cyclohexanol: 500 ppm based on the total composition; The mixture was fed from line 3-b shown in Figure 1. The temperature of the feed port was set to 150°C. Next, ViMe2SiO(Me2SiO) 800 SiViMe2 0.15 kg / hr, dimethylpolysiloxane terminated at both molecular chain ends with dimethylvinylsiloxy groups (vinyl group content = 0.09% by mass), A mixture consisting of a 1,3-divinyltetramethyldisiloxane solution of platinum 1,3-divinyltetramethyldisiloxane complex (an amount equivalent to 4.0 ppm by mass of platinum metal relative to the entire composition) was fed from line 3-a in Figure 1 (the set temperature of the feeding section was 80°C), and the vacuum level in the extruder was -0.08 MPa, and degassing and melt kneading were performed. The outlet temperature of the twin-screw extruder was 80°C, and the mixture was in the form of a semi-solid softened material. A release film (FL2-01, manufactured by Takara Line Corporation) with a width of 330 mm and a thickness of 125 μm was conveyed at a speed of 1.0 m / min, and the mixture was fed onto the film at a feed rate of 5 kg / hr, and the mixture was sandwiched between two release films to form a laminate. The laminate was then pressed between rolls controlled at a temperature of 90°C to stretch the mixture, forming a laminate in which a 300 μm thick curable hot-melt silicone composition sheet was laminated between two release films, and the entire product was then cooled by air cooling. The configuration of the manufacturing apparatus is shown in FIG. 1. When the release film was peeled off from the resulting laminate, a bubble-free, flat, homogeneous, tack-free, transparent curable hot-melt silicone composition sheet was obtained, and the softening temperature was 80°C. [Explanation of symbols]
[0183] Figure 1 1: Hot melter 2: Extruder 3-a: Pump 3-b: Pump 3-c: Vacuum pump 4-a: Release sheet 4-b: Release sheet 5-a: Stretching roll (optionally may further include temperature control function) 5-b: Stretching roll (optionally may further include temperature control function) 6: Cooling roll 7: Film thickness gauge 8: Sheet cutter 9: Foreign body inspection machine
Claims
1. (A) 100 parts by mass of an organopolysiloxane resin containing the following components (A1) and (A2) in a mass ratio of 0:100 to 90:10, and which exhibits a mass loss of 2.0% or less when components (A1) and (A2) are exposed to 200° C. for 1 hour: (A1) A compound having no hot melt properties as a whole molecule, having a curing reactive functional group containing a carbon-carbon double bond in the molecule, and having SiO 4/2 An organopolysiloxane resin containing 40 to 90 mol % of all siloxane units represented by the formula: (A2) The molecule as a whole does not have hot melt properties, does not have a curing reactive functional group containing a carbon-carbon double bond in the molecule, and has SiO 4/2 An organopolysiloxane resin containing 40 to 90 mol % of all siloxane units represented by the formula: (B) 10 to 100 parts by mass of a linear organopolysiloxane that is liquid or plastic at 25° C. and has a curing reactive functional group containing at least two carbon-carbon double bonds in the molecule, (C) one or more curing agents selected from (c1) or (c2) below, in an amount necessary for curing the present composition. (c1) Organic peroxide (c2) an organohydrogenpolysiloxane having at least two silicon-bonded hydrogen atoms in the molecule and a hydrosilylation reaction catalyst; and wherein the composition as a whole has hot melt properties.
2. The curable silicone composition according to claim 1, further comprising a functional filler (D), wherein the amount of component (D) is in the range of 10 to 2,000 parts by mass per 100 parts by mass of the combined total of components (A) and (B).
3. 3. The curable silicone composition according to claim 1, wherein components (A1) and (A2) are spherical organopolysiloxane resin fine particles having an average primary particle size of 1 to 20 μm.
4. The component (C) is (c2-1) an organohydrogenpolysiloxane having at least two silicon-bonded hydrogen atoms in the molecule; and (c2-2) a hydrosilylation reaction catalyst; The curable silicone composition according to any one of claims 1 to 3, wherein the content of the organohydrogenpolysiloxane of (c2-1) above is an amount such that the molar ratio of silicon-bonded hydrogen atoms in the organohydrogenpolysiloxane resin to the curable reactive functional groups containing carbon-carbon double bonds in components (A) and (B) is in the range of 0.5 to 20.
5. 3. The curable silicone composition according to claim 2, wherein component (D) is a functional filler comprising at least one selected from the group consisting of a reinforcing filler, a white pigment, a thermally conductive filler, an electrically conductive filler, and an organic filler.
6. The curable silicone composition according to any one of claims 1 to 5, which is in the form of granules, pellets, or sheets.
7. 6. A substantially flat curable silicone composition sheet having a thickness of 10 to 1000 μm, which comprises the curable silicone composition according to any one of claims 1 to 5.
8. A film-like adhesive which is a sheet of the curable silicone composition according to claim 7.
9. The curable silicone composition sheet of claim 7, and A release laminate comprising a sheet-like substrate on one or both sides of the curable silicone composition sheet, the sheet having a release surface facing the curable silicone composition sheet.
10. A cured product obtained by curing the curable silicone composition according to any one of claims 1 to 5.
11. Use of the cured product according to claim 10 as a member for a semiconductor device or an optical semiconductor device.
12. A semiconductor device or optical semiconductor device comprising the cured product according to claim 10.
13. A method for producing the curable silicone composition according to any one of claims 1 to 5, characterized in that the curable silicone composition is granulated by mixing at a temperature not exceeding 50°C.
14. A method for molding a cured product comprising at least the following steps (I) to (III): (I) a step of heating the curable silicone composition according to any one of claims 1 to 5 to at least 50°C to melt it; (II) a step of injecting the liquid curable silicone composition obtained in step (I) into a mold, or a step of spreading the curable silicone composition obtained in step (I) throughout the mold by clamping the mold; and (III) A step of curing the curable silicone composition injected in the step (II)
Citation Information
Patent Citations
Conductive hot melt silicone adhesive composition
JP2002155261A
Hot-melt type silicone adhesive
JP2006274007A
Reactive silicone composition, reactive thermoplastic body, cured product and optical semiconductor device
JP2014009322A
Reactive silicone composition, hot melt material produced therefrom, and curable hot melt composition containing the same
JP2017512224A
Actinic energy ray-curable hot-melt silicone composition, cured product thereof, and method for producing film
JP2018519369A