Curable silicone composition, cured product thereof, and method for producing same

JP7560442B2Active Publication Date: 2024-10-02DOW TORAY CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021511423
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-29
Filing Date
2020-03-18
Publication Date
2024-10-02
Estimated Expiration
2040-03-18

AI Technical Summary

Technical Problem

Existing curable silicone compositions suffer from impaired flexibility, toughness, and stress relaxation properties when a large amount of functional inorganic filler is added, compromising their hot-melt properties and moldability.

Method used

A curable silicone composition with a specific molecular weight range (2,000 to 15,000) and vinyl group content (0.05 to 1.50 mol%) in SiO4/2 organopolysiloxane resin, combined with a balanced ratio of components (A1, A2, B, C, and D) to maintain hot-melt properties and flexibility, even with high filler content.

Benefits of technology

The composition retains excellent hot-melt properties, flexibility, and stress relaxation properties, allowing for efficient production of cured products without significant impairment, suitable for semiconductor applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560442000001
    Figure 0007560442000001
  • Figure 0007560442000002
    Figure 0007560442000002
  • Figure 0007560442000003
    Figure 0007560442000003
Patent Text Reader

Abstract

[Problem] To provide: a curable silicone composition which has excellent hot melt properties and excellent moldability, and which enables the achievement of a cured product that is not deteriorated in terms of flexibility, toughness and stress relaxation characteristics even if a large amount of a functional inorganic filler is blended therein; and the like. [Solution] A curable silicone composition which contains one or more kinds of functional fillers and an organopolysiloxane resin that has a weight average molecular weight within the range of 2,000-15,000, while containing a siloxane unit represented by SiO4 / 2 in an amount of at least 20% by mole or more of the all siloxane units, and which is configured such that: the content of a vinyl group moiety (CH2=CH-) in a curing reactive functional group containing a carbon-carbon double bond per 100 g of the silicone component in the composition is 0.05-1.50% by mole; and the composition as a whole has hot melt properties. In addition, applications of this curable silicone composition.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a curable silicone composition which can be obtained by a simple production method, has excellent hot melt properties and moldability, and the flexibility, toughness, and stress relaxation properties of the cured product obtained are not impaired even when a large amount of functional inorganic filler is blended, and to a molded product (pellet, sheet, etc.) and the cured product of the composition. The present invention also relates to a cured product of the composition and uses thereof (particularly including semiconductor members and semiconductors having the cured product), a method for producing the composition, and a method for molding the cured product. [Background technology]

[0002] Curable silicone compositions are used in a wide range of industrial fields because they cure to form cured products that have excellent heat resistance, cold resistance, electrical insulation, weather resistance, water repellency, and transparency. Cured products of such curable silicone compositions generally do not discolor as easily as other organic materials, and the deterioration of physical properties is small, so they are also suitable as optical materials and sealants for semiconductor devices.

[0003] The applicant has proposed a hot-melt curable granular silicone composition and a reactive silicone composition for molding in Patent Document 1 and Patent Document 2. The applicant has also disclosed a transparent hot-melt curable silicone composition using a methylsilicone resin in Patent Document 3.

[0004] Meanwhile, in recent years, optical semiconductor devices and the like have become smaller and have higher output, and in addition to improving the physical properties such as the linear expansion coefficient of the cured product, there is a strong demand for silicone compositions that satisfy the requirements of improved thermal conductivity and improved heat dissipation properties by blending functional fillers such as heat dissipation fillers such as alumina into the composition. For example, Patent Document 4 proposes a hot-melt curable silicone composition in which the composition is highly filled with functional fillers.

[0005] However, when a large amount of functional inorganic filler is mixed in these compositions, there is a problem that the melting characteristics (=hot melt property) of the composition and the toughness and flexibility of the cured product are significantly impaired.For this reason, it is difficult to achieve high thermal conductivity by mixing a large amount of thermally conductive inorganic filler such as alumina, or to significantly reduce the linear expansion coefficient by mixing a large amount of dimensionally stable inorganic filler such as silica.For this reason, there is a strong demand for a curable silicone composition that does not impair the flexibility, toughness, and stress relaxation properties of the cured product obtained even when a large amount of functional inorganic filler is mixed, and has excellent hot melt property and moldability. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2016 / 136243 Brochure [Patent Document 2] JP 2014-009322 A [Patent Document 3] Special Publication No. 2017-512224 [Patent Document 4] JP 2013-221082 A Summary of the Invention [Problem to be solved by the invention]

[0007] The object of the present invention is to provide a curable silicone composition that has hot melt properties, is excellent in handling workability and curing properties such as overmolding, and gives a cured product that does not lose flexibility, toughness, and stress relaxation properties even when a large amount of functional inorganic filler is blended.Furthermore, the present invention is to provide such a curable silicone composition in the form of granules, pellets, sheets, etc., and in the form of a peelable laminate containing the curable silicone composition sheet.Furthermore, the present invention is to provide a semiconductor device member made of a cured product of the curable silicone composition, a semiconductor device having the cured product, and a method for molding the cured product. [Means for solving the problem]

[0008] As a result of extensive investigations, the present inventors have discovered that the weight average molecular weight (Mw) of the SiO 4 / 2 The inventors have found that the above problems can be solved by a curable silicone composition which comprises an organopolysiloxane resin containing siloxane units represented by the formula (I) at least 20 mol % of all siloxane units and one or more types of functional fillers, wherein the content of vinyl (CH2=CH-) group moieties in curable reactive functional groups containing a carbon-carbon double bond is 0.05 to 1.50 mol % per 100 g of silicone component in the composition, and the composition as a whole has hot melt properties, and have arrived at the present invention.

[0009] More specifically, the weight average molecular weight (Mw) measured by gel permeation chromatography (GPC) using toluene as a solvent is in the range of 2,000 to 15,000, and SiO 4 / 2 and one or more types of functional fillers, wherein the content of vinyl (CH2=CH-) group moieties among curing-reactive functional groups containing a carbon-carbon double bond per 100 g of silicone component in the composition is 0.05-1.50 mol %, and the composition as a whole has hot melt properties.

[0010] (A) 100 parts by mass of an organopolysiloxane resin containing the following components (A1) and (A2) in a mass ratio of 0:100 to 75:25, and having a weight average molecular weight (Mw) of 2,000 to 15,000 as measured by gel permeation chromatography (GPC) using toluene as a solvent. (A1) The molecule as a whole does not have hot melt properties, has a curing reactive functional group containing a carbon-carbon double bond in the molecule, and is SiO 4 / 2An organopolysiloxane resin containing siloxane units represented by the formula: (A2) The molecule as a whole does not have hot melt properties, does not have a curing reactive functional group containing a carbon-carbon double bond in the molecule, and is SiO 4 / 2 An organopolysiloxane resin containing siloxane units represented by the formula: (B) 10 to 100 parts by mass of a linear or branched organopolysiloxane that is liquid at 25°C and has a curing reactive functional group containing at least two carbon-carbon double bonds in the molecule; (C) one or more curing agents selected from (c1) or (c2) below, in an amount necessary for curing the present composition. (c1) Organic peroxide (c2) an organohydrogenpolysiloxane having at least two silicon-bonded hydrogen atoms in the molecule and a hydrosilylation reaction catalyst; (D) Functional fillers The composition comprises The weight average molecular weight (Mw) measured by gel permeation chromatography (GPC) using toluene as a solvent is in the range of 2,000 to 15,000, and the amount of the component (D) is in the range of 10 to 2,000 parts by mass per 100 parts by mass of the sum of the components (A) and (B). 4 / 2 and one or more types of functional fillers, and the content of vinyl (CH2=CH-) group moieties in curing reactive functional groups containing a carbon-carbon double bond per 100 g of the silicone component in the composition is 0.05 to 1.50 mol wherein the composition as a whole has hot melt properties.

[0011] (A) 100 parts by mass of an organopolysiloxane resin containing the following components (A1) and (A2) in a mass ratio of 0:100 to 75:25, and having a weight average molecular weight (Mw) of 2,000 to 15,000 as measured by gel permeation chromatography (GPC) using toluene as a solvent. (A1) The molecule as a whole does not have hot melt properties, has a curing reactive functional group containing a carbon-carbon double bond in the molecule, and is SiO 4 / 2 An organopolysiloxane resin containing siloxane units represented by the formula: (A2) The molecule as a whole does not have hot melt properties, does not have a curing reactive functional group containing a carbon-carbon double bond in the molecule, and is SiO 4 / 2 An organopolysiloxane resin containing siloxane units represented by the formula: (B) 10 to 100 parts by mass of a linear or branched organopolysiloxane that is liquid at 25°C and has a curing reactive functional group containing at least two carbon-carbon double bonds in the molecule; (C) one or more curing agents selected from (c1) or (c2) below, in an amount necessary for curing the present composition. (c1) Organic peroxide (c2) an organohydrogenpolysiloxane having at least two silicon-bonded hydrogen atoms in the molecule and a hydrosilylation reaction catalyst; (D) Functional fillers The composition comprises The inventors have found that the above problems can be solved by the above curable silicone composition, characterized in that the amount of component (D) is in the range of 10 to 2000 parts by mass per 100 parts by mass of the sum of components (A) and (B), and have arrived at the present invention. The above curable silicone composition may be in the form of granules, pellets, or sheets.

[0012] The above-mentioned curable silicone composition may be in the form of a substantially flat curable silicone composition sheet having a thickness of 10 to 1000 μm.

[0013] The above curable silicone composition can also be used in a release laminate having the following configuration. That is, the release laminate may be in the form of a sheet-like substrate having the above curable silicone composition sheet and a release surface facing the curable silicone composition sheet on one or both sides of the curable silicone composition sheet. Such a curable silicone composition sheet may be used as a film-like or sheet-like silicone adhesive.

[0014] Furthermore, the present inventors have discovered that the above problems can be solved by using a cured product of the above-mentioned curable silicone composition, in particular the use of the cured product as a component for a semiconductor device, and by a semiconductor device having the cured product (including one or more selected from power semiconductor devices, optical semiconductor devices, and semiconductor devices mounted on a flexible circuit board), and have arrived at the present invention.

[0015] Similarly, the inventors have discovered that the above problems can be solved by a production method characterized by granulating only the components that make up the above-mentioned curable silicone composition by mixing them at a temperature not exceeding 50°C, and by a method for molding a cured product using the above-mentioned curable granular silicone composition, and have arrived at the present invention.

[0016] The above molding methods include transfer molding, compression molding, and injection molding, and the curable silicone composition of the present invention is suitable for use as a molding material for these methods. Furthermore, the curable silicone composition of the present invention is suitable for use as a molding material for the so-called overmolding method, a process in which a semiconductor element or a semiconductor circuit board is covered by a cured product through overmolding.

[0017] Similarly, the present inventors provide a method for producing a curable silicone composition sheet, comprising the steps of: Step 1: Mixing the raw material components of the curable silicone composition at a temperature of 50° C. or higher Step 2: The mixture obtained in step 1 is kneaded while being heated and melted. Step 3: Laminating the heated and melted mixture obtained in step 2 between at least one film having a release surface. Step 4: Stretching the laminate obtained in step 3 between rolls to form a curable silicone sheet having a specific thickness. Effect of the Invention

[0018] The curable silicone composition of the present invention has hot melt properties, is excellent in handling and curing properties such as overmolding, and gives a cured product that does not lose flexibility and stress relaxation even when a large amount of filler is mixed. In addition, such a curable silicone composition can be produced by a simple mixing process alone, and can be produced efficiently. Furthermore, the present invention can provide such a curable silicone composition in the form of granules, pellets, sheets, etc., and in the form of a peelable laminate containing the curable silicone composition sheet. Furthermore, it can provide a semiconductor device member made of a cured product of the curable silicone composition, a semiconductor device having the cured product, and a molding method for the cured product. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] [Curable Silicone Composition] The curable silicone composition of the present invention has a weight average molecular weight (Mw) in the range of 2,000 to 15,000 as measured by gel permeation chromatography (GPC) using toluene as a solvent, and 4 / 2The composition is characterized in that it contains an organopolysiloxane resin containing siloxane units represented by the formula (I) at least 20 mol % of all siloxane units, and one or more types of functional fillers, the content of vinyl (CH2=CH-) group moieties in curing reactive functional groups containing carbon-carbon double bonds is 0.05-1.50 mol % per 100 g of silicone component in the composition, and the composition as a whole has hot melt properties. In the present invention, unless otherwise specified, "having hot melt properties" means that the softening point is between 50 and 200°C, the melt viscosity is at 150°C (preferably a melt viscosity of less than 1000 Pa s), and the composition has the property of flowing.

[0020] That is, the curable silicone composition of the present invention contains a functional filler such as a reinforcing filler or a thermally conductive filler, and contains branched siloxane units (SiO 4 / 2 The present invention is characterized in that it uses an organopolysiloxane resin having a high content of ) and the content of curable functional groups in the entire silicone component is relatively small. By adopting such a constitution, even when a large amount of functional filler is blended, it is possible to obtain a cured product that does not significantly impair flexibility and stress relaxation properties. The curable silicone composition of the present invention may be, and is preferably, molded into granules, pellets, or sheets depending on the application. Each component of the composition and optional components will be described below. In the present invention, the term "average particle size" refers to the primary average particle size of the particles unless otherwise defined.

[0021] [Weight average molecular weight of organopolysiloxane resin] The curable silicone composition according to the present invention has a weight average molecular weight (Mw) in the range of 2,000 to 15,000 as measured by gel permeation chromatography (GPC) using toluene as a solvent, and 4 / 2The organopolysiloxane resin contains siloxane units represented by the formula (I) at least 20 mol % or more of the total siloxane units. The weight average molecular weight (Mw) of the organopolysiloxane resin is preferably in the range of 2,000 to 10,000. On the other hand, if the weight average molecular weight (Mw) of the organopolysiloxane resin exceeds the upper limit, when a large amount of functional inorganic filler is blended, the melting characteristics may deteriorate, the hardness may increase significantly, embrittlement may occur, and the problem of the present invention may not be solved. Also, if the weight average molecular weight (Mw) of the organopolysiloxane resin is less than the lower limit, the organopolysiloxane resin becomes liquid at room temperature, and the obtained blend may not be able to have good hot melt properties. In other words, if an organopolysiloxane resin having a molecular weight outside the above weight average molecular weight (Mw) range is used, the technical effect of the present invention may not be achieved.

[0022] The organopolysiloxane resin further comprises RSiO 1 / 2 , R2SiO 2 / 2 , RSiO 3 / 2 (R is a monovalent organic group) and R 2 O 1 / 2 (R 2 may contain a hydroxyl group or an alkoxy group represented by (a hydrogen atom or an alkyl group having 1 to 10 carbon atoms), but preferably, at least 40 mol % of the total siloxane units, particularly 40 to 90 mol %, of SiO 4 / 2 As long as it falls within the above molecular weight range, it contains a siloxane unit represented by SiO 4 / 2 The amount of SiO 4 / 2 If the content of the siloxane unit represented by the formula (I) is less than the lower limit, other branched siloxane units (e.g., RSiO 3 / 2 ) in large amounts, the technical effects of the present invention may not be achieved.

[0023] [Functional fillers] The curable silicone composition according to the present invention contains one or more kinds of functional fillers. The functional filler is a component that imparts mechanical properties and other properties to the cured product, and examples thereof include inorganic fillers, organic fillers, and mixtures thereof. Examples of the inorganic fillers include reinforcing fillers, white pigments, thermally conductive fillers, conductive fillers, phosphors, and mixtures of at least two of these. Examples of the organic fillers include silicone resin-based fillers, fluororesin-based fillers, and polybutadiene resin-based fillers. The shape of these fillers is not particularly limited, and may be spherical, spindle-shaped, flat, needle-shaped, or amorphous. In particular, even if a large amount of functional filler is blended into the curable silicone composition according to the present invention, the toughness and stress relaxation properties of the cured product are not significantly impaired, and the composition can be suitably used in compositions that require the addition of a large amount of inorganic fillers to impart functions, such as thermally conductive fillers. The type and amount of the functional filler, optional configurations such as surface treatment thereof, etc. will be described later.

[0024] [Vinyl content in composition] The curable silicone composition according to the present invention is a silicone component, specifically, the total of components including the organopolysiloxane resin and the linear organopolysiloxane, and the content of vinyl (CH2=CH-) group moiety in the curing reactive functional group containing a carbon-carbon double bond per 100 g of components excluding components other than the silicone component such as functional filler must be 0.05 to 1.50 mol%, preferably 0.05 to 1.25 mol%, and more preferably 0.05 to 1.00 mol%. Examples of the curing reactive functional group include an alkenyl group having 2 to 20 carbon atoms, a 3-methacryloxypropyl group, a 3-acryloxypropyl group, or other acrylic group-containing monovalent organic group having a vinyl group moiety in the functional group. By suppressing the content of these curing reactive functional groups, there is an advantage that the stress relaxation property of the cured product is high even if a large amount of functional filler is blended into the composition.

[0025] [Hot melt properties and composition of the curable silicone composition] The curable silicone composition of the present invention has hot-melt properties as a whole composition, a softening point of 50° C. or higher, and a melt viscosity at 150° C. (preferably a melt viscosity of less than 1000 Pa s), giving it the property of flowing. Note that the individual components that make up the composition do not need to have hot-melt properties, and in particular when the curable reactive or non-reactive organopolysiloxane resin is in particulate form, it is particularly preferable that it does not have hot-melt properties at temperatures of 200° C. or lower.

[0026] The curable silicone composition of the present invention may be, and is preferably, molded into granules, pellets, or sheets depending on the application. Each component and optional component of the composition will be described below. In the present invention, the term "average particle size" refers to the primary average particle size of the particles unless otherwise defined.

[0027] The curable silicone composition according to the present invention is not limited in its composition as long as it contains at least the above components and has hot melt properties as a whole. In particular, the composition preferably contains: (A) 100 parts by mass of an organopolysiloxane resin containing the following components (A1) and (A2) in a mass ratio of 0:100 to 75:25, and wherein components (A1) and (A2) have a weight average molecular weight (Mw) in the range of 2,000 to 15,000 as measured by gel permeation chromatography (GPC) using toluene as a solvent: (A1) The molecule as a whole does not have hot melt properties, has a curing reactive functional group containing a carbon-carbon double bond in the molecule, and is SiO 4 / 2 An organopolysiloxane resin containing siloxane units represented by the formula: (A2) The molecule as a whole does not have hot melt properties, does not have a curing reactive functional group containing a carbon-carbon double bond in the molecule, and is SiO 4 / 2 An organopolysiloxane resin containing siloxane units represented by the formula: (B) 10 to 100 parts by mass of a linear or branched organopolysiloxane that is liquid at 25°C and has a curing reactive functional group containing at least two carbon-carbon double bonds in the molecule; (C) one or more curing agents selected from (c1) or (c2) below, in an amount necessary for curing the present composition. (c1) Organic peroxide (c2) an organohydrogenpolysiloxane having at least two silicon-bonded hydrogen atoms in the molecule and a hydrosilylation reaction catalyst; (D) Functional fillers The composition comprises Preferably, the amount of component (D) is in the range of 10 to 2000 parts by mass per 100 parts by mass of the sum of components (A) and (B). Furthermore, the curable silicone composition of the present invention may optionally contain (E) hot-melt particles or other additives having a dropping point of 50°C or higher and a melt viscosity of 10 Pas or less as measured with a rotational viscometer at 150°C. Each component and its content will be described below.

[0028] [Component (A)] The curable silicone composition of the present invention does not have hot melt properties as a whole molecule, and 4 / 2 The organopolysiloxane resin further comprises an organopolysiloxane resin containing siloxane units represented by the formula: 1 / 2 , R2SiO 2 / 2 , RSiO 3 / 2 (R is a monovalent organic group) and R 2 O 1 / 2 (R 2 may contain a hydroxyl group or an alkoxy group represented by (wherein the siloxane unit is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms), but preferably, SiO 4 / 2 It contains a siloxane unit represented by SiO 4 / 2If the content of the siloxane unit represented by the formula (I) is less than the lower limit, other branched siloxane units (e.g., RSiO 3 / 2 ) in large amounts, the technical effects of the present invention may not be achieved.

[0029] As described above, the organopolysiloxane resin must have a weight average molecular weight (Mw) in the range of 2,000 to 15,000 as measured by gel permeation chromatography (GPC) using toluene as a solvent. Optionally, volatile components generated during the production process may be removed. The degree of removal is synonymous with the mass loss rate when exposed to 200°C for 1 hour, and it is particularly preferable that volatile low molecular weight components are removed from the organopolysiloxane resin so that the mass loss rate is 2.0% by mass or less.

[0030] Such organopolysiloxane resins include (A1) The molecule as a whole does not have hot melt properties, has a curing reactive functional group containing a carbon-carbon double bond in the molecule, and is SiO 4 / 2 An organopolysiloxane resin containing siloxane units represented by the formula: (A2) The molecule as a whole does not have hot melt properties, does not have a curing reactive functional group containing a carbon-carbon double bond in the molecule, and is SiO 4 / 2 An organopolysiloxane resin containing siloxane units represented by the formula: in a mass ratio of 0:100 to 75:25, and the weight average molecular weight (Mw) of components (A1) and (A2) is in the range of 2,000 to 15,000 as measured by gel permeation chromatography (GPC) using toluene as a solvent. Note that component (A1) is an optional component in component (A), and only component (A2), described below, may be used in component (A).

[0031] Although the above-mentioned (A) component does not have hot melt properties as a whole molecule, by using it in combination with the later-described (B) component in a specified quantitative range, the hot melt properties of the whole composition can be realized. Such (A) component is preferably in the form of fine particles, either alone or together with other components, and in this case, it is particularly preferable that the component is a spherical silicone fine particle having an average primary particle size of 1 to 20 μm.

[0032] [(A1) Organopolysiloxane resin having a curing reactive functional group] The component (A1) is one of the main components of the composition, and is SiO 4 / 2 The organopolysiloxane resin contains siloxane units represented by the formula (I) in an amount of at least 20 mol % or more of all siloxane units, does not have hot melt properties by itself, and has a curing reactive functional group containing a carbon-carbon double bond in the molecule, and exhibits a weight loss of 2.03.0 mass % or less when exposed to 200°C for 1 hour.

[0033] The component (A1) must have a curing reactive group having a carbon-carbon double bond in the molecule. Such a curing reactive group is a functional group that is hydrosilylation reactive or organic peroxide curable, and forms a cured product by a crosslinking reaction with other components. Such a curing reactive group is an alkenyl group or an acrylic group, and examples of such a curing reactive group include alkenyl groups having 2 to 10 carbon atoms, such as vinyl groups, allyl groups, butenyl groups, pentenyl groups, hexenyl groups, and heptenyl groups; and acrylic group-containing monovalent organic groups, such as 3-methacryloxypropyl groups and 3-acryloxypropyl groups. In particular, a vinyl group or a hexenyl group is preferable.

[0034] The component (A1) is an organopolysiloxane resin that does not have hot melt properties as a whole molecule and is solid in a solvent-free state. Here, not having hot melt properties means that the resin that is the component (A1) does not exhibit heat melting behavior at 200°C or less by itself, specifically, that it has no softening point or melt viscosity at 200°C or less. In the component (A1), such physical properties are not particularly limited structurally, but it is preferable that the functional group in the organopolysiloxane resin is a monovalent hydrocarbon group having 1 to 10 carbon atoms, particularly a functional group selected from an alkyl group having 1 to 10 carbon atoms such as a methyl group, and that it does not substantially contain an aryl group such as a phenyl group. If the component contains a large amount of a phenyl group or the like, the component may have hot melt properties, and the SiO 4 / 2 The effect of reinforcing the cured product specific to the group may decrease.

[0035] Preferably, the functional groups bonded to silicon atoms in component (A1) are selected from alkenyl groups such as methyl and vinyl, and it is preferred that 70 to 99 mol% of all functional groups bonded to silicon atoms are methyl, more preferably 80 to 99 mol% are methyl, and particularly preferably 88 to 99 mol% are methyl, and the remaining functional groups bonded to silicon atoms are alkenyl groups such as vinyl. In this range, component (A1) can be designed as a component that is not hot-melt, but is particularly excellent in the color resistance of the cured product at high temperatures. Note that component (A1) may contain a small amount of hydroxyl or alkoxy groups.

[0036] Component (A1) is an organopolysiloxane resin that is solid in the absence of a solvent and contains SiO 4 / 2The branched siloxane units are preferably at least 40 mol % or more of the total siloxane units, and more preferably in the range of 40 to 90 mol %. R is a monovalent organic group, preferably a functional group selected from monovalent hydrocarbon groups having 1 to 10 carbon atoms, particularly alkyl and alkenyl groups having 1 to 10 carbon atoms such as methyl groups, and from the viewpoint of technical effect, it is preferable that R does not substantially contain aryl groups such as phenyl groups.

[0037] Preferably, the component (A1) is a copolymer having the following average unit formula: (R 1 3SiO 1 / 2 ) a (R 1 2SiO 2 / 2 ) b (R 1 SiO 3 / 2 ) c (SiO 4 / 2 ) d (R 2 O 1 / 2)e (In the formula, each R 1 are independently monovalent hydrocarbon groups having 1 to 10 carbon atoms, provided that the total R 1 are 1 to 12 mole percent alkenyl groups; 2 is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms; and a, b, c, d, and e are numbers that satisfy the following: 0.10≦a≦0.60, 0≦b≦0.70, 0≦c≦0.80, 0≦d≦0.65, 0≦e≦0.05, with the proviso that c+d>0.20 and a+b+c+d=1). The organopolysiloxane resin is a non-hot melt organopolysiloxane resin represented by the formula:

[0038] In the above average unit formula, each R 1are independently monovalent hydrocarbon radicals having 1 to 10 carbon atoms, such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, or similar alkyl groups; vinyl, allyl, butenyl, pentenyl, hexenyl, or similar alkenyl groups; phenyl, tolyl, xylyl, or similar aryl groups; benzyl, phenethyl, or similar aralkyl groups; and chloromethyl, 3-chloropropyl, 3,3,3-trifluoropropyl, or similar halogenated alkyl groups. Furthermore, the total R 1 Preferably, 1 to 12 mol % of the total R 1 Of these, 2 to 10 mol % is an alkenyl group. If the content of alkenyl groups is less than the lower limit of the above range, the mechanical strength (hardness, etc.) of the resulting cured product may be insufficient. On the other hand, if the content of alkenyl groups is equal to or less than the upper limit of the above range, the composition containing this component can achieve good hot melt performance as a whole composition. 1 is preferably a functional group selected from an alkyl group having 1 to 10 carbon atoms, such as a methyl group, and an alkenyl group, such as a vinyl group or a hexenyl group. From the viewpoint of the technical effect of the invention, R 1 It is preferable that the component (A) is substantially free of aryl groups such as phenyl groups. If the component (A) contains a large amount of aryl groups such as phenyl groups, the component (A) itself may become hot-melt, making it impossible to achieve the technical effects of the present invention. In addition, in the cured product, SiO 4 / 2 The effect of reinforcing the cured product specific to the group may decrease.

[0039] In the formula, R 2 R is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms. 2 The alkyl group of R is exemplified by methyl, ethyl, propyl, butyl, pentyl, or hexyl. 2 Functional group R containing 2 O 1 / 2 corresponds to a hydroxyl group or an alkoxy group in component (A).

[0040] In the formula, a represents the general formula: R 1 3SiO 1 / 2a is a number indicating the proportion of siloxane units. This number satisfies 0.1≦a≦0.60, and preferably 0.15≦a≦0.55. When a is equal to or greater than the lower limit of the above range, a composition containing this component can achieve good hot melt performance as a whole composition. On the other hand, when a is equal to or less than the upper limit of the above range, the mechanical strength (hardness, elongation, etc.) of the obtained cured product is not too low.

[0041] In the formula, b represents the general formula: R 1 2SiO 2 / 2 This number satisfies 0≦b≦0.70, and preferably 0≦b≦0.60. When b is equal to or less than the upper limit of the range, a composition containing this component can achieve good hot melt performance as a whole composition, and a granular composition with little stickiness at room temperature can be obtained.

[0042] In the formula, c represents a group represented by the general formula: R 3 SiO 3 / 2 c is a number indicating the proportion of siloxane units. This number satisfies 0≦c≦0.80, and preferably 0≦c≦0.75. When c is equal to or less than the upper limit of the range, the composition containing this component can achieve good hot melt performance as a whole composition, and can obtain a tack-free composition with little stickiness at room temperature. In the present invention, c may be, and is preferably, 0.

[0043] In the formula, d is SiO 4 / 2 It is necessary that d is 0.00≦d≦0.65, preferably 0.20≦d≦0.65, and particularly preferably 0.25≦d≦0.65. This is because within this numerical range, a composition containing this component can achieve good hot melt performance as a whole composition, and the resulting cured product has sufficient flexibility.

[0044] In the present invention, c or d may be 0, but it is necessary that c+d>0.20. If the value of c+d is less than the lower limit, the composition as a whole may not achieve good hot melt performance, and the technical effects of the present invention may not be fully achieved.

[0045] In the formula, e represents the general formula: R 2 O 1 / 2 e is a number indicating the proportion of units, which means a hydroxyl group or an alkoxy group bonded to a silicon atom that may be contained in the organopolysiloxane resin. This number satisfies 0≦e≦0.05, preferably 0≦e≦0.03. If e is equal to or less than the upper limit of the range, a material that realizes good hot melt performance as a whole composition can be obtained. In addition, the sum of a, b, c, and d, which are the sums of each siloxane unit, is ultimately equal to 1.

[0046] The component (A1) is an organopolysiloxane resin having the above characteristics, and from the viewpoint of ease of handling, is preferably a spherical organopolysiloxane resin fine particle having an average primary particle diameter of 1 to 20 μm as measured by a laser diffraction / scattering method or the like. By using such a fine particle component, the present composition can be prepared or produced as a curable granular composition having excellent handling, workability and hot melt properties. Here, the method for producing the component (A1) is not limited, and any known method can be used.

[0047] The method for producing the fine particle (A1) component may be, for example, a method for pulverizing the above-mentioned organopolysiloxane resin using a pulverizer or a method for directly pulverizing the resin in the presence of a solvent. The pulverizer is not limited, and may be, for example, a roll mill, a ball mill, a jet mill, a turbo mill, or a planetary mill. In addition, the method for directly pulverizing the above-mentioned organopolysiloxane resin in the presence of a solvent may be, for example, spraying with a spray dryer, or pulverization with a twin-screw kneader or a belt dryer. When obtaining the fine particle (A1) component, a part of the (C) component described later, for example, a hydrosilylation reaction catalyst, may be pulverized together with the (A1) component, but from the viewpoint of the storage stability of the obtained composition, it is not preferable to pulverize a mixture having a property of being cured by heating.

[0048] In particular, by using a spray dryer or the like, it is possible to produce component (A1) that is truly spherical and has an average primary particle size of 1 to 500 μm, preferably 1 to 20 μm. The heating and drying temperature of the spray dryer must be appropriately set based on the heat resistance of the organopolysiloxane resin fine particles. In order to prevent secondary aggregation of the obtained fine particles, it is preferable to control the temperature of the organopolysiloxane resin fine particles to a temperature equal to or lower than their glass transition temperature. The organopolysiloxane resin fine particles thus obtained can be collected using a cyclone, bag filter, or the like.

[0049] The above-mentioned microparticulation may be carried out using a solvent within a range that does not inhibit the curing reaction.The solvent is not limited, but examples thereof include aliphatic hydrocarbons such as n-hexane, cyclohexane, and n-heptane; aromatic hydrocarbons such as toluene, xylene, and mesitylene; ethers such as tetrahydrofuran and dipropyl ether; silicones such as hexamethyldisiloxane, octamethyltrisiloxane, and decamethyltetrasiloxane; esters such as ethyl acetate, butyl acetate, and propylene glycol monomethyl ether acetate; and ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone.

[0050] [(A2) component] The component (A2) is one of the main components of the composition, and is an organopolysiloxane resin containing a curing reactive functional group that does not have hot melt properties by itself, and is a component that realizes hot melt properties of the composition as a whole and color resistance of the cured product by combining it with the above-mentioned components (A1) and (B) in a specified quantitative range. Such component (A2) is preferably in the form of fine particles alone or together with other components (for example, the component (A1) which is a non-reactive organopolysiloxane resin, and a part of the component (C) which is a curing agent), and is particularly preferably spherical silicone fine particles with an average primary particle size of 1 to 20 μm.

[0051] The (A2) component is an organopolysiloxane resin that does not have hot melt properties as a whole molecule and is solid in a solvent-free state. Here, not having hot melt properties means that the resin that is the (A2) component does not exhibit heat melting behavior by itself, specifically, it means that it has no softening point and no melt viscosity. In the (A2) component, such physical properties are not particularly limited structurally, but it is preferable that the functional group in the organopolysiloxane resin is a monovalent hydrocarbon group having 1 to 10 carbon atoms, in particular a functional group selected from an alkyl group having 1 to 10 carbon atoms such as a methyl group, and that it does not substantially contain an aryl group such as a phenyl group. If the component contains a large amount of a phenyl group or the like, the component may have hot melt properties and may be insufficient to form a SiO 4 / 2 The effect of reinforcing the cured product specific to the group may decrease.

[0052] Component (A2) is a solid like component (A1), and is SiO 4 / 2 The organopolysiloxane resin fine particles contain siloxane units represented by the formula (I) in an amount of at least 20 mol % or more of the total siloxane units, but are characterized by not having a curing reactive functional group containing at least one carbon-carbon double bond in the molecule. That is, component (A2) is characterized by not containing an alkenyl group such as a vinyl group as a functional group in the organopolysiloxane resin. Examples of functional groups in the organopolysiloxane include monovalent hydrocarbon groups having 1 to 10 carbon atoms, particularly alkyl groups having 1 to 10 carbon atoms such as a methyl group, and it is preferable that the organopolysiloxane is substantially free of aryl groups such as a phenyl group.

[0053] Preferably, the functional groups bonded to silicon atoms in component (A2) are alkyl groups having 1 to 10 carbon atoms, such as methyl groups, and it is preferable that 70 to 100 mol % of all the functional groups bonded to silicon atoms are methyl groups, more preferably 80 to 100 mol %, and particularly preferably 88 to 100 mol %. Within this range, component (A2) is not hot-melt and has a SiO 4 / 2It is possible to design this component as one that has an especially excellent reinforcing effect on the cured product containing the siloxane unit represented by the following formula: The component (A2) may contain a small amount of hydroxyl groups or alkoxy groups.

[0054] The component (A2) does not form a cured product by itself because it does not have a curing reactive group having a carbon-carbon double bond in the molecule, but it has an effect of improving the hot melt properties of the composition as a whole and reinforcing the cured product. In addition, it is a necessary component for achieving the technical effects of the present invention by using it in combination with the component (A1) having a curing reactive group as necessary.

[0055] Component (A2) is a solid organopolysiloxane resin in the absence of a solvent, and contains branched siloxane units, such as SiO 4 / 2 The siloxane unit represented by the formula (1) is contained in an amount of at least 20 mol % of all siloxane units. The amount of the siloxane unit is preferably at least 40 mol % of all siloxane units, more preferably at least 50 mol %, and particularly preferably in the range of 50 to 65 mol %.

[0056] Preferably, the component (A2) is (A2-1) a copolymer having the following average unit formula: (R 3 3SiO 1 / 2 ) f (R 3 2SiO 2 / 2 ) g (R 3 SiO 3 / 2 ) h (SiO 4 / 2 ) i (R 2 O 1 / 2)j (In the formula, each R 3 each independently represents a monovalent hydrocarbon group having 1 to 10 carbon atoms and no carbon-carbon double bonds; R 2 is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms; f, g, h, i, and j are numbers that satisfy the following: 0.35≦f≦0.55, 0≦g≦0.20, 0≦h≦0.20, 0.45≦i≦0.65, 0≦j≦0.05, and f+g+h+i=1). The organopolysiloxane resin is a non-hot melt organopolysiloxane resin represented by the formula:

[0057] In the above average unit formula, each R 3 are independently monovalent hydrocarbon radicals having 1 to 10 carbon atoms and no carbon-carbon double bonds, such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, or similar alkyl radicals; phenyl, tolyl, xylyl, or similar aryl radicals; benzyl, phenethyl, or similar aralkyl radicals; and chloromethyl, 3-chloropropyl, 3,3,3-trifluoropropyl, or similar halogenated alkyl radicals, where the total R 3 It is preferable that 70 mol % or more of R are alkyl groups having 1 to 10 carbon atoms such as methyl groups, and it is particularly preferable that 88 mol % or more of R are methyl groups from the viewpoint of industrial production and the technical effect of the invention. 3 It is preferable that the component (B) is substantially free of aryl groups such as phenyl groups. If the component (B) contains a large amount of aryl groups such as phenyl groups, the component (B) itself may become hot-melt, making it impossible to achieve the technical effects of the present invention, and the color resistance of the cured product at high temperatures may deteriorate.

[0058] In the formula, R 2 is the same group as defined above.

[0059] In the formula, f represents the general formula: R 3 3SiO 1 / 2 f is a number indicating the proportion of siloxane units. This number satisfies 0.35≦f≦0.55, and preferably 0.40≦f≦0.50. When f is equal to or greater than the lower limit of the above range, a composition containing this component can achieve good hot melt performance as a whole composition. On the other hand, when f is equal to or less than the upper limit of the above range, the mechanical strength (hardness, etc.) of the obtained cured product is not too low.

[0060] In the formula, g represents a group represented by the general formula: R 1 2SiO 2 / 2g is a number indicating the proportion of siloxane units. This number satisfies 0≦g≦0.20, and preferably 0≦g≦0.10. When g is equal to or less than the upper limit of the range, the composition containing this component can achieve good hot melt performance as a whole composition, and can obtain a composition that is less sticky at room temperature. In the present invention, g may be 0, and is preferred.

[0061] In the formula, h represents the general formula: R 1 SiO 3 / 2 h is a number indicating the proportion of siloxane units. This number satisfies 0≦h≦0.20, and preferably 0≦h≦0.10. When h is equal to or less than the upper limit of the range, a composition containing this component can achieve good hot melt performance as a whole composition, and can obtain a composition that is less sticky at room temperature. In the present invention, h may be 0, and is preferred.

[0062] In the formula, i is SiO 4 / 2 i is a number indicating the proportion of siloxane units, and it is necessary that 0.45≦i≦0.65, preferably 0.40≦i≦0.65, and particularly preferably 0.50≦i≦0.65. Within this numerical range, a composition containing this component can achieve good hot melt performance as a whole composition, excellent mechanical strength of the obtained cured product, and a composition that is not sticky as a whole and has good handling and workability can be realized.

[0063] In the formula, j represents the general formula: R 2 O 1 / 2 is a number indicating the proportion of units, and the unit means a hydroxyl group or alkoxy group bonded to a silicon atom that may be contained in the organopolysiloxane resin. This number satisfies 0≦j≦0.05, preferably 0≦j≦0.03. If e is equal to or less than the upper limit of the range, a material that realizes good hot melt performance as a whole composition can be obtained. In addition, the sum of e, f, g, and h, which are the sums of each siloxane unit, is ultimately equal to 1.

[0064] Component (A2) is an organopolysiloxane resin having the above characteristics, and from the viewpoint of ease of handling, is preferably a spherical organopolysiloxane resin fine particle having an average primary particle diameter of 1 to 20 μm as measured by a laser diffraction / scattering method or the like. By using such a fine particle component, the present composition can be prepared or produced as a curable granular composition having excellent handling, workability and hot melt properties. Here, the method of producing component (A2) can be the same as the method exemplified for component (A1) above.

[0065] [Removal of volatile low molecular weight components from component (A)] In the production process of components (A1) and (A2), volatile low molecular weight components are generated. Specifically, the structure is M4Q, and the M unit (R 3 3SiO 1 / 2 ) and Q units (SiO 4 / 2 ) is polymerized as a by-product. This structure has the effect of significantly lowering the hardness of the cured product of the composition of the present invention. The organopolysiloxane resin is polymerized in the presence of a highly compatible organic solvent, and the solid organopolysiloxane resin is obtained by removing the organic solvent by drying under reduced pressure or the like, but the M4Q structure has high mutual solubility with the organopolysiloxane resin, and cannot be removed under drying conditions that remove the organic solvent. It was known that this structure can be removed by exposure to a temperature of 200°C or higher for a short period of time, but if it is removed by exposure to high temperatures after being integrally molded with a substrate such as a semiconductor, the volume of the cured product will decrease and the hardness will increase significantly, causing the dimensions of the molded product to change and warping to occur. For this reason, in order to apply this invention to the applications, it is necessary to remove the M4Q structure before the molding process with the substrate, that is, at the stage of the raw material.

[0066] Methods for removing this structure include removing it together with the organic solvent in a twin-screw kneader, or forming a particulate organopolysiloxane resin using the method described below, and then drying it in an oven or the like to remove it.

[0067] More specifically, components (A1) and (A2) are produced in the presence of an organic solvent, and volatile components appear as by-products during synthesis. The volatile components can be removed by treating the obtained crude organopolysiloxane resin at a high temperature of about 200 degrees for a short period of time, so it is possible to simultaneously remove the organic solvent and volatile components from components (A1) and (A2) using a twin-screw kneader set at about 200°C. In addition, when components (A1) and (A2) are handled as spherical powders, it is possible to powder them by removing the organic solvent with a spray dryer, but this method does not allow the volatile components to be removed. If the obtained powder is treated at a low temperature of about 120°C for 24 hours, the volatile components can be removed without the powder agglomerating.

[0068] [Mass ratio of component (A1) to component (A2) in component (A)] In order to impart hot melt properties to the composition as a whole, it is necessary to mix the (A2) component or a mixture of the (A1) and (A2) components with the (B) component described below at a predetermined ratio, but the ratio of the (A) component to the (B) component may be in the range of 0:100 to 75:25, preferably in the range of 0:100 to 60:40, and more preferably in the range of 0:100 to 55:45. The (A2) component does not have curability by itself, but by adding a small amount of the (A1) component to the composition and using it in combination, it is possible to control the elastic modulus of the cured product of the composition at high temperatures, and when a functional inorganic filler described below is added to the composition, it is possible to achieve a suitable elastic modulus and flexibility by appropriately adjusting the amount of the functional inorganic filler added and the amount of the (A1) component used. For example, when a large amount of the functional inorganic filler is added or when it is desired to reduce the elastic modulus of the resulting cured product as much as possible, it is also possible to compound the composition with only the (A2) component without adding the (A1) component.

[0069] [(B) Component] Component (B) is one of the main components of the composition, and is a linear or branched organopolysiloxane that is liquid at 25° C. and has a curing reactive functional group containing at least two carbon-carbon double bonds in the molecule. When this type of curing reactive chain organopolysiloxane is mixed with the above-mentioned solid organopolysiloxane resin, the composition as a whole exhibits hot melt properties.

[0070] The (B) component must have a curing reactive group having a carbon-carbon double bond in the molecule. Such a curing reactive group is a hydrosilylation reactive or organic peroxide curing functional group, and forms a cured product by a crosslinking reaction with other components. Such a curing reactive group is an alkenyl group or an acrylic group, and examples thereof include the same groups as those described above, and in particular, a vinyl group or a hexenyl group is preferable.

[0071] Component (B) is a linear or branched organopolysiloxane that is liquid at 25°C (room temperature), and when mixed with component (A), which is solid at room temperature, the composition as a whole exhibits hot melt properties. Its structure is a small number of branched siloxane units (for example, the general formula: R 4 SiO 3 / 2 T units (R 4 are independently monovalent hydrocarbon radicals having 1 to 10 carbon atoms) or SiO 4 / 2 The organopolysiloxane may be a branched organopolysiloxane having a Q unit represented by the formula: (B1) The following structural formula: R 4 3SiO(SiR 4 2O) k SiR 4 3 (In the formula, each R 4 are independently monovalent hydrocarbon groups having 1 to 10 carbon atoms, provided that R 4 at least two of the groups are alkenyl groups, and k is a number from 20 to 5,000. It is a linear diorganopolysiloxane represented by the following formula: Preferably, it is a linear diorganopolysiloxane having one alkenyl group at each of both ends of the molecular chain.

[0072] In the formula, each R 4 are independently monovalent hydrocarbon radicals having 1 to 10 carbon atoms, such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, or similar alkyl groups; vinyl, allyl, butenyl, pentenyl, hexenyl, or similar alkenyl groups; phenyl, tolyl, xylyl, or similar aryl groups; benzyl, phenethyl, or similar aralkyl groups; and chloromethyl, 3-chloropropyl, 3,3,3-trifluoropropyl, or similar halogenated alkyl groups. 4 At least two of R are alkenyl groups, preferably vinyl groups. 4 is preferably a functional group selected from an alkyl group having 1 to 10 carbon atoms, such as a methyl group, and an alkenyl group, such as a vinyl group or a hexenyl group, and all of R 4 At least two of R are alkenyl groups, and the remaining R 4 From the viewpoint of the technical effect of the invention, it is preferable that R 4 It is preferable that R is substantially free of aryl groups such as phenyl groups. If it contains a large amount of aryl groups such as phenyl groups, the color resistance of the cured product at high temperatures may deteriorate. Particularly preferably, R has an alkenyl group such as a vinyl group at each end of the molecular chain and other R 4 is preferably a methyl group.

[0073] In the formula, k is a number of 20 to 5,000, preferably 100 to 3,000, and particularly preferably 300 to 1500. If k is equal to or greater than the lower limit of the above range, a composition with little stickiness at room temperature can be obtained. On the other hand, if k is equal to or less than the upper limit of the above range, the composition as a whole can achieve good hot melt performance. Furthermore, it is preferable to select the above-mentioned curing reactive linear organopolysiloxane having a relatively high degree of polymerization and a high molecular weight as the component (B). This is because, when a low molecular weight component (B) is used, even if the above-mentioned component (A) is used, the toughness and stress relaxation properties of the obtained cured product tend to be low depending on the type and amount of the functional filler, so when the amount of the functional inorganic filler is very large, the cured product may become significantly embrittled. Therefore, when a large amount of inorganic filler is blended in the curable silicone composition, it is preferable to combine an organopolysiloxane resin (A) in the above molecular weight range with a relatively high molecular weight component (B) in order to prevent the cured product from becoming too hard or embrittled.

[0074] Here, in order to achieve hot melt properties for the entire composition, the mass ratio of the linear or branched organopolysiloxane (B) component to 100 parts by mass of the organopolysiloxane resin (A) component is in the range of 10 to 100 parts by mass, preferably in the range of 10 to 70 parts by mass, and more preferably in the range of 15 to 50 parts by mass. If the content of the (B) component is in the above range, the composition achieves good hot melt properties, the mechanical strength of the obtained cured product can be increased, and the stickiness of the obtained composition at room temperature can be reduced, improving the handling and workability.

[0075] [(C) component] The component (C) is a curing agent for curing the components (A) and (B), and is specifically one or more curing agents selected from the following (c1) or (c2). Two or more of these curing agents may be used in combination, for example, a curing system containing both the components (c1) and (c2). (c1) Organic peroxide (c2) an organohydrogenpolysiloxane having at least two silicon-bonded hydrogen atoms in the molecule and a hydrosilylation reaction catalyst;

[0076] The (c1) organic peroxide is a component that cures the above-mentioned (A) and (B) components by heating, and examples thereof include alkyl peroxides, diacyl peroxides, ester peroxides, and carbonate peroxides. Note that the (c1) component can also react with a part of the (A2) component.

[0077] Examples of alkyl peroxides include dicumyl peroxide, di-tert-butyl peroxide, di-tert-butylcumyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3, tert-butylcumyl, 1,3-bis(tert-butylperoxyisopropyl)benzene, and 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxonane.

[0078] Examples of diacyl peroxides include benzoyl peroxide, lauroyl peroxide, and decanoyl peroxide.

[0079] Examples of peroxy esters include 1,1,3,3-tetramethylbutyl peroxy neodecanoate, α-cumyl peroxy neodecanoate, tert-butyl peroxy neodecanoate, tert-butyl peroxy neoheptanoate, tert-butyl peroxy pivalate, tert-hexyl peroxy pivalate, 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate, and tert-amyl peroxy-2-ethylhexanoate. , tert-butylperoxy-2-ethylhexanoate, tert-butylperoxyisobutyrate, di-tert-butylperoxyhexahydroterephthalate, tert-amylperoxy-3,5,5-trimethylhexanoate, tert-butylperoxy-3,5,5-trimethylhexanoate, tert-butylperoxyacetate, tert-butylperoxybenzoate, and di-butylperoxytrimethyladipate are examples.

[0080] Examples of peroxycarbonates include di-3-methoxybutyl peroxydicarbonate, di(2-ethylhexyl) peroxydicarbonate, diisopropyl peroxycarbonate, tert-butylperoxyisopropyl carbonate, di(4-tert-butylcyclohexyl) peroxydicarbonate, dicetyl peroxydicarbonate, and dimyristyl peroxydicarbonate.

[0081] The organic peroxide preferably has a half-life of 10 hours at a temperature of 90° C. or higher, or 95° C. or higher. Examples of such organic peroxides include dicumyl peroxide, di-t-butyl peroxide, di-t-hexyl peroxide, t-butylcumyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, 1,3-bis(tert-butylperoxyisopropyl)benzene, di-(2-t-butylperoxyisopropyl)benzene, and 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxonane.

[0082] The content of the (c1) organic peroxide is not limited, but is preferably within a range of 0.05 to 10 parts by mass, or 0.10 to 5.0 parts by mass, relative to the sum (100 parts by mass) of the (A) and (B) components.

[0083] (c2) An organohydrogenpolysiloxane having at least two silicon-bonded hydrogen atoms in its molecule and a hydrosilylation catalyst are components that cure the composition by undergoing an addition reaction (hydrosilylation reaction) between the organohydrogenpolysiloxane, which is a crosslinking agent, and the carbon-carbon double bonds in components (A) and (C) in the presence of the hydrosilylation catalyst.

[0084] The structure of the organohydrogenpolysiloxane crosslinking agent is not particularly limited, and may be linear, branched, cyclic, or resinous. 1 / 2 Hydrogenorganosiloxy units (D H The main structural unit is HR2SiO 1 / 2 Hydrogen diorganosiloxy units (M H In particular, in applications other than the molding process described below, the present curable silicone composition may be an organohydrogenpolysiloxane having the above-mentioned D H Even if the organohydrogenpolysiloxane is a chain organohydrogenpolysiloxane consisting of units, it can be cured sufficiently for practical use.

[0085] On the other hand, when the present curable silicone composition is used in a molding process, the content of curing reactive functional groups containing carbon-carbon double bonds in the present composition is low, and therefore, from the standpoint of the curing speed, moldability, and curability, the organohydrogenpolysiloxane is RSiO 3 / 2 Monoorganosiloxy units (T units, R is a monovalent organic group or a silicon-bonded hydrogen atom) represented by the formula: 4 / 2 The branching unit is a siloxy unit (Q unit) represented by the formula: 1 / 2Hydrogen diorganosiloxy units (M H unit, R is independently a monovalent organic group), and M H Organohydrogenpolysiloxane resins having units are preferred.

[0086] Particularly suitable organohydrogenpolysiloxanes have the average unit formula: (R 5 3SiO 1 / 2 ) l (R 6 2SiO 2 / 2 ) m (R 6 SiO 3 / 2 ) n (SiO 4 / 2 ) p (R 2 O 1 / 2 ) q The organohydrogenpolysiloxane resin is represented by the formula:

[0087] In the formula, each R 5 are the same or different, and are monovalent hydrocarbon groups having 1 to 10 carbon atoms that do not have an aliphatic unsaturated carbon bond, or hydrogen atoms, provided that at least two R 5 is a hydrogen atom. R other than a hydrogen atom 5 The monovalent hydrocarbon radicals are, for example, methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, or similar alkyl radicals; phenyl, tolyl, xylyl, or similar aryl radicals; benzyl, phenethyl, or similar aralkyl radicals; and chloromethyl, 3-chloropropyl, 3,3,3-trifluoropropyl, or similar halogenated alkyl radicals. From an industrial point of view, the methyl or phenyl radicals are preferred.

[0088] In the formula, R 6 is a monovalent hydrocarbon group having 1 to 10 carbon atoms that does not have an aliphatic unsaturated carbon bond, and examples of the monovalent hydrocarbon group include the same groups as those described above. 2 is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, and R in the above component (A1) or component (A2)2 Examples of the groups are the same as those shown below.

[0089] In the formula, l, m, n, and p are numbers that satisfy the following: 0.1≦l≦0.80, 0≦m≦0.5, 0≦n≦0.8, 0≦p≦0.6, 0≦q≦0.05, with the proviso that n+p>0.1 and l+m+n+p=1. When this composition is used in a molding process, the organohydrogenpolysiloxane resin that is a part of component (d2) is specifically, H MT resin, M H MTT H Resin, M H MTQ resin, M H MQ resin, M H MTT H Q, M H Q resin is preferred.

[0090] Particularly preferably, the organohydrogenpolysiloxane which is a part of the component (c2) is (H(CH3)2SiO 1 / 2 ) l1 (SiO 4 / 2 ) p1 Represented by M H Q resin. Here, it is preferable that l1+p1=1, 0.1≦l1≦0.80, and 0.20≦p1≦0.90.

[0091] Similarly, the organohydrogenpolysiloxane that is a part of component (c2) may contain a linear diorganopolysiloxane, organohydrogenpolysiloxane, or diorganopolysiloxane-organohydrogensiloxane copolymer whose molecular chain ends are blocked with silicon-bonded hydrogen atoms or trimethylsiloxy groups. The degree of siloxane polymerization of these linear organohydrogenpolysiloxanes is not particularly limited, but is in the range of 2 to 200, and preferably in the range of 5 to 100.

[0092] The content of the organohydrogenpolysiloxane that is part of component (c2) is an amount sufficient to cure the curable silicone composition of the present invention, and is an amount such that the molar ratio of silicon-bonded hydrogen atoms in the organohydrogenpolysiloxane to the curing-reactive functional groups containing carbon-carbon double bonds in components (B) and (C) (for example, alkenyl groups such as vinyl groups) is 0.5 or more, and preferably in the range of 0.5 to 20. In particular, when component (d2) contains the above-mentioned organohydrogenpolysiloxane resin, it is preferable that the molar ratio of silicon-bonded hydrogen atoms in the organohydrogenpolysiloxane resin to the curing-reactive functional groups containing carbon-carbon double bonds in components (B) and (C) is in the range of 0.5 to 20, or in the range of 1.0 to 10.

[0093] Examples of the hydrosilylation catalyst, which is a part of component (c2), include platinum-based catalysts, rhodium-based catalysts, and palladium-based catalysts, with platinum-based catalysts being preferred because they can significantly accelerate the curing of the composition. Examples of platinum-based catalysts include platinum fine powder, chloroplatinic acid, alcohol solutions of chloroplatinic acid, platinum-alkenylsiloxane complexes, platinum-olefin complexes, platinum-carbonyl complexes, and catalysts in which these platinum-based catalysts are dispersed or encapsulated in thermoplastic resins such as silicone resins, polycarbonate resins, and acrylic resins, with platinum-alkenylsiloxane complexes being particularly preferred. Examples of the alkenylsiloxane include 1,3-divinyl-1,1,3,3-tetramethyldisiloxane, 1,3,5,7-tetramethyl-1,3,5,7-tetravinylcyclotetrasiloxane, alkenylsiloxanes in which a part of the methyl groups of these alkenylsiloxanes is replaced with an ethyl group, a phenyl group, or the like, and alkenylsiloxanes in which the vinyl groups of these alkenylsiloxanes are replaced with an allyl group, a hexenyl group, or the like. In particular, since the stability of this platinum-alkenylsiloxane complex is good, 1,3-divinyl-1,1,3,3-tetramethyldisiloxane is preferred, and it is preferred to add the complex in the form of an alkenylsiloxane solution. In addition, from the viewpoint of improving the handling and workability and the pot life of the composition, a platinum-containing hydrosilylation reaction catalyst in the form of fine particles dispersed or encapsulated in a thermoplastic resin may be used. As a catalyst for promoting the hydrosilylation reaction, a non-platinum metal catalyst such as iron, ruthenium, or iron / cobalt may be used.

[0094] The amount of the hydrosilylation reaction catalyst, which is part of component (c2), added is preferably an amount such that the metal atoms are in the range of 0.01 to 500 ppm, 0.01 to 100 ppm, or 0.01 to 50 ppm, by mass, relative to the entire composition.

[0095] Particularly preferred component (c2) is one that contains at least (c2-1) an organohydrogenpolysiloxane resin represented by the above average unit formula and a hydrosilylation reaction catalyst.

[0096] When the hydrosilylation reaction catalyst is used as part of component (C), it is preferable, from the viewpoint of the storage stability of the curable silicone composition, to have it contained in the fine particles when producing the organopolysiloxane resin particles of components (A1) and (A2), etc. However, it is preferable that the entire mixture constituting the fine particles does not exhibit curing reactivity on its own.

[0097] [(D) component] The functional filler (D) is an essential component of the present invention, and is a component that imparts mechanical properties and other properties to the cured product. Examples of the functional filler include inorganic fillers, organic fillers, and mixtures thereof. Examples of the inorganic fillers include reinforcing fillers, white pigments, thermally conductive fillers, conductive fillers, phosphors, and mixtures of at least two of these. Examples of the organic fillers include silicone resin-based fillers, fluororesin-based fillers, and polybutadiene resin-based fillers. The shape of these fillers is not particularly limited, and may be spherical, spindle-shaped, flat, needle-shaped, or amorphous.

[0098] When the present composition is used as a sealant, protective agent, adhesive, or the like, it is preferable for at least a part of component (D) to contain a reinforcing filler, from the viewpoint of improving the mechanical strength, protective properties, and adhesive properties of the cured product.

[0099] The reinforcing filler may be added to improve the mechanical strength of the cured product, improve the protectiveness and adhesiveness, and maintain the solid particulate state as a binder filler of the curable silicone composition before curing. Examples of such reinforcing fillers include fumed silica, precipitated silica, fused silica, calcined silica, fumed titanium dioxide, quartz, calcium carbonate, diatomaceous earth, aluminum oxide, aluminum hydroxide, zinc oxide, and zinc carbonate. In addition, these reinforcing fillers may be surface-treated with organoalkoxysilanes such as methyltrimethoxysilane; organohalosilanes such as trimethylchlorosilane; organosilazanes such as hexamethyldisilazane; siloxane oligomers such as α,ω-silanol group-blocked dimethylsiloxane oligomers, α,ω-silanol group-blocked methylphenylsiloxane oligomers, and α,ω-silanol group-blocked methylvinylsiloxane oligomers. The particle size of the reinforcing filler is not limited, but the median size measured by laser diffraction / scattering particle size distribution measurement is preferably within the range of 1 nm to 500 μm.Furthermore, fibrous fillers such as calcium metasilicate, potassium titanate, magnesium sulfate, sepiolite, zonolite, aluminum borate, rock wool, and glass fiber may be used as the reinforcing filler.

[0100] Furthermore, in order to impart other functions to the cured product obtained by using the composition, a white pigment, a thermally conductive filler, an electrically conductive filler, or a fluorescent material may be blended in. Also, in order to improve the stress relaxation properties of the cured product, an organic filler such as silicone elastomer fine particles may be blended in.

[0101] The white pigment is a component that imparts whiteness to the cured product and improves light reflectivity, and the cured product obtained by curing the composition by blending the component can be used as a light reflector for light emitting / optical devices. Examples of the white pigment include metal oxides such as titanium oxide, aluminum oxide, zinc oxide, zirconium oxide, and magnesium oxide; hollow fillers such as glass balloons and glass beads; and other materials such as barium sulfate, zinc sulfate, barium titanate, aluminum nitride, boron nitride, and antimony oxide. Titanium oxide is preferred because of its high light reflectance and hiding power. Aluminum oxide, zinc oxide, and barium titanate are preferred because of their high light reflectance in the UV region. The average particle size and shape of the white pigment are not limited, but the average particle size is preferably within the range of 0.05 to 10.0 μm, or 0.1 to 5.0 μm. The white pigment may be surface-treated with a silane coupling agent, silica, aluminum oxide, or the like.

[0102] The thermally conductive filler or the conductive filler is added for the purpose of imparting thermal conductivity / conductivity (electrical conductivity) to the cured product, and specific examples thereof include fine metal powders such as gold, silver, nickel, copper, and aluminum; fine powders of ceramics, glass, quartz, organic resins, and the like, on whose surfaces metals such as gold, silver, nickel, and copper are vapor-deposited or plated; metal compounds such as aluminum oxide, magnesium oxide, aluminum nitride, boron nitride, and zinc oxide; graphite, and mixtures of two or more of these. When electrical insulation is required for the composition, metal oxide powders or metal nitride powders are preferred, and aluminum oxide powder, zinc oxide powder, and aluminum nitride powder are particularly preferred, and these may be used in combination with each other in terms of type, particle size, particle shape, and the like according to the requirements for thermal conductivity / conductivity.

[0103] The phosphor is a component that is blended to convert the wavelength of light emitted from a light source (optical semiconductor element) when the cured product is used as a wavelength conversion material. There are no particular limitations on the phosphor, and examples of the phosphor include yellow, red, green, and blue light-emitting phosphors made of oxide-based phosphors, oxynitride-based phosphors, nitride-based phosphors, sulfide-based phosphors, oxysulfide-based phosphors, etc., which are widely used in light-emitting diodes (LEDs).

[0104] Examples of silicone fine particles include non-reactive silicone resin fine particles and silicone elastomer fine particles, with silicone elastomer fine particles being preferred from the standpoint of improving the flexibility or stress relaxation properties of the cured product.

[0105] Silicone elastomer microparticles are crosslinked products of linear diorganopolysiloxanes mainly composed of diorganosiloxy units (D units). Silicone elastomer microparticles can be prepared by crosslinking diorganopolysiloxanes by hydrosilylation reaction or condensation reaction of silanol groups, and can be preferably obtained by crosslinking an organohydrogenpolysiloxane having silicon-bonded hydrogen atoms at the side chain or end with a diorganopolysiloxane having unsaturated hydrocarbon groups such as alkenyl groups at the side chain or end under a hydrosilylation reaction catalyst. Silicone elastomer microparticles can take various shapes such as spherical, flat, and irregular, but from the viewpoint of dispersibility, spherical is preferable, and among them, true sphere is more preferable. Examples of commercially available silicone elastomer microparticles include "Trefil E Series" and "EP Powder Series" manufactured by Toray Dow Corning Co., Ltd., and "KMP Series" manufactured by Shin-Etsu Chemical Co., Ltd.

[0106] For the purpose of stably blending the functional filler as described above in the present composition, the filler may be surface-treated using a specific surface treatment agent in an amount of 0.1 to 2.0 mass%, 0.1 to 1.0 mass%, or 0.2 to 0.8 mass% relative to the total mass of component (D). Examples of such surface treatment agents include methylhydrogenpolysiloxane, silicone resin, metal soap, silane coupling agent, perfluoroalkylsilane, and fluorine compounds such as perfluoroalkyl phosphate salt.

[0107] In particular, when component (D) is a thermally conductive filler and is blended in large amounts in the curable silicone composition of the present invention, the thermally conductive filler is preferably a plate-shaped boron nitride powder having a suitable average particle size of 0.1 to 30 μm, a granular boron nitride powder having an average particle size of 0.1 to 50 μm, a spherical and / or crushed aluminum oxide powder having an average particle size of 0.01 to 50 μm, or a spherical and / or crushed graphite having an average particle size of 0.01 to 50 μm, or a mixture of two or more of these. Most preferably, it is a mixture of two or more of spherical and crushed aluminum oxide powders having an average particle size of 0.01 to 50 μm. In particular, by combining an aluminum oxide powder having a large particle size and an aluminum oxide powder having a small particle size in a ratio that follows the closest packing theoretical distribution curve, the packing efficiency is improved, and low viscosity and high thermal conductivity are possible.

[0108] Furthermore, it is particularly preferred that at least a part of the surface of the thermally conductive filler is treated with one or more types of organosilicon compounds. The preferred range of the treatment amount is as described above. Here, examples of the organosilicon compound that is the surface treatment agent are low molecular weight organosilicon compounds such as silane, silazane, siloxane, or the like, and organosilicon polymers or oligomers such as polysiloxane, polycarbosiloxane, or the like. A preferred example of silane is a so-called silane coupling agent. Representative examples of such silane coupling agents include alkyltrialkoxysilanes (methyltrimethoxysilane, vinyltrimethoxysilane, hexyltrimethoxysilane, octyltrimethoxysilane, decyltrimethoxysilane, or the like), and organofunctional group-containing trialkoxysilanes (glycidoxypropyltrimethoxysilane, epoxycyclohexylethyltrimethoxysilane, methacryloxypropyltrimethoxysilane, aminopropyltrimethoxysilane, or the like). Preferred siloxanes and polysiloxanes include hexamethyldisiloxane, 1,3-dihexyl-tetramethyldisiloxane, trialkoxysilyl single-terminated polydimethylsiloxane, trialkoxysilyl single-terminated dimethylvinyl single-terminated polydimethylsiloxane, trialkoxysilyl single-terminated organofunctional group single-terminated polydimethylsiloxane, trialkoxysilyl doubly terminated polydimethylsiloxane, organofunctional group doubly terminated polydimethylsiloxane, or the like. When siloxanes are used, the number of siloxane bonds n is preferably in the range of 2 to 150. Examples of preferred silazanes are hexamethyldisilazane, 1,3-dihexyl-tetramethyldisilazane, or the like. Examples of preferred polycarbosiloxanes are polymers with Si-C-C-Si bonds in the polymer backbone.

[0109] The content of the (D) component is not limited, but in order to obtain a cured product with excellent hardness and mechanical strength, it is preferable that the content be within the range of 10 to 2000 parts by mass, 10 to 1500 parts by mass, or 10 to 1000 parts by mass relative to the sum (100 parts by mass) of the (A) and (B) components.

[0110] The curable silicone composition of the present invention has the advantage that the toughness and stress relaxation properties of the cured product obtained are not impaired even when a large amount of functional inorganic filler is blended therein, and therefore it is possible, and preferably, to blend a functional filler such as alumina into the composition in an amount of 100 to 2,000 parts by mass, 150 to 1,500 parts by mass, or 300 to 1,200 parts by mass relative to the sum (100 parts by mass) of components (A) and (B).

[0111] The curable silicone composition of the present invention contains the above components (A) to (D). From the standpoint of further improving the melting properties, it is possible and preferable to add (E) hot-melt particles having a dropping point of 50°C or higher and a melt viscosity of 10 Pas or less as measured with a rotational viscometer at 150°C.

[0112] As long as the dropping point conditions and the kinetic viscosity conditions at 150°C are satisfied, the type of component (E) is not particularly limited, and one or more selected from various hot-melt synthetic resins, waxes, fatty acid metal salts, etc. can be used. The component (E) exhibits low kinetic viscosity at high temperatures (150°C) and forms a molten material with excellent fluidity. Furthermore, by using the above components (A) to (C) in combination, the component (E) in the molten material of this composition spreads quickly throughout the entire composition at high temperatures, thereby reducing the viscosity of the substrate surface to which the molten composition is applied and the entire composition, and also rapidly reducing the surface friction of the substrate and the molten composition, thereby significantly increasing the fluidity of the entire composition. Therefore, the viscosity and fluidity of the molten composition can be greatly improved by adding only a small amount of the component (E) relative to the total amount of other components.

[0113] The component (E) may be a petroleum wax such as paraffin as long as it satisfies the above-mentioned conditions of dropping point and kinetic viscosity when melted, but from the viewpoint of the technical effect of the present invention, it is preferably a hot melt component consisting of a fatty acid metal salt or a fatty acid ester of an erythritol derivative, and particularly preferably a metal salt of a higher fatty acid such as stearic acid, palmitic acid, oleic acid, isononanoic acid, etc., pentaerythritol tetrastearate, dipentaerythritol adipic acid stearate, glycerin tri-18-hydroxystearate, or pentaerythritol full stearate. The type of the fatty acid metal salt is not particularly limited, but suitable examples include alkali metal salts such as lithium, sodium, potassium, etc.; alkaline earth metal salts such as magnesium, calcium, barium, etc.; or zinc salts.

[0114] Particularly preferred as the component (E) are fatty acid metal salts (E0) with a free fatty acid content of 5.0% or less, 4.0% or less, and 0.05 to 3.5% fatty acid metal salts and erythritol derivatives. Examples of such components include at least one metal stearate. Specifically, it is most preferred to use a hot melt component with a melting point of 150°C or less selected from calcium stearate (melting point 150°C), zinc stearate (melting point 120°C), magnesium stearate (melting point 130°C), pentaerythritol tetrastearate (melting point 60-70°C), pentaerythritol adipate stearate (melting point 55-61°C), pentaerythritol full stearate (melting point 62-67°C), etc.

[0115] The amount of the (E) component used is in the range of 0.01 to 5.0 parts by mass, and may be 0.01 to 3.5 parts by mass, or 0.01 to 3.0 parts by mass, when the entire composition is taken as 100 parts by mass. If the amount of the (E) component used exceeds the upper limit, the adhesiveness and mechanical strength of the cured product obtained from the curable silicone composition of the present invention may be insufficient. If the amount of the (E) component used is less than the lower limit, sufficient fluidity may not be achieved when heated and melted.

[0116] The composition may also contain other optional components such as a cure retarder and an adhesion promoter, provided that the object of the present invention is not impaired.

[0117] Examples of the curing retarder include alkyne alcohols such as 2-methyl-3-butyn-2-ol, 3,5-dimethyl-1-hexyn-3-ol, 2-phenyl-3-butyn-2-ol, and 1-ethynyl-1-cyclohexanol; enyne compounds such as 3-methyl-3-penten-1-yne and 3,5-dimethyl-3-hexen-1-yne; alkenyl-containing low molecular weight siloxanes such as tetramethyltetravinylcyclotetrasiloxane and tetramethyltetrahexenylcyclotetrasiloxane; and alkynyloxysilanes such as methyl-tris(1,1-dimethylpropynyloxy)silane and vinyl-tris(1,1-dimethylpropynyloxy)silane. The content of this curing retarder is not limited, but is preferably within the range of 10 to 10,000 ppm by mass with respect to the present composition.

[0118] As the adhesion promoter, an organic silicon compound having at least one alkoxy group bonded to a silicon atom in one molecule is preferred. Examples of this alkoxy group include methoxy, ethoxy, propoxy, butoxy, and methoxyethoxy groups, and particularly preferred is methoxy. Examples of groups bonded to silicon atoms other than the alkoxy group in the organic silicon compound include halogen-substituted or unsubstituted monovalent hydrocarbon groups such as alkyl groups, alkenyl groups, aryl groups, aralkyl groups, and halogenated alkyl groups; glycidoxyalkyl groups such as 3-glycidoxypropyl and 4-glycidoxybutyl groups; epoxycyclohexylalkyl groups such as 2-(3,4-epoxycyclohexyl)ethyl and 3-(3,4-epoxycyclohexyl)propyl groups; epoxyalkyl groups such as 3,4-epoxybutyl and 7,8-epoxyoctyl groups; acrylic group-containing monovalent organic groups such as 3-methacryloxypropyl groups; and hydrogen atoms. The organosilicon compound preferably has a group capable of reacting with the alkenyl group or silicon-bonded hydrogen atom in the composition, and more specifically, preferably has a silicon-bonded hydrogen atom or an alkenyl group.In addition, since it can provide good adhesion to various substrates, the organosilicon compound preferably has at least one epoxy-containing monovalent organic group in one molecule.Examples of such organosilicon compounds include organosilane compounds, organosiloxane oligomers, and alkyl silicates.Examples of the molecular structure of the organosiloxane oligomer or alkyl silicate include linear, partially branched linear, branched, cyclic, and net-like, and in particular, linear, branched, and net-like are preferred.Examples of the organosilicon compounds include silane compounds such as 3-glycidoxypropyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and 3-methacryloxypropyltrimethoxysilane; siloxane compounds having at least one silicon-bonded alkenyl group or one silicon-bonded hydrogen atom, and at least one silicon-bonded alkoxy group in one molecule; a mixture of a silane compound or siloxane compound having at least one silicon-bonded alkoxy group and a siloxane compound having at least one silicon-bonded hydroxy group and at least one silicon-bonded alkenyl group in one molecule; a reaction mixture of an amino group-containing organoalkoxysilane and an epoxy group-containing organoalkoxysilane; an organic compound having at least two alkoxysilyl groups in one molecule and containing a bond other than a silicon-oxygen bond between the silyl groups; a n Si(OR b ) 4-n (In the formula, R a is a monovalent epoxy-containing organic group, and R b is an alkyl group having 1 to 6 carbon atoms or a hydrogen atom; and n is a number ranging from 1 to 3. Examples of the adhesion promoter include epoxy group-containing silanes represented by the formula (I) or partial hydrolysis condensates thereof, a reaction mixture of a vinyl group-containing siloxane oligomer (including those with a chain or cyclic structure) and an epoxy group-containing trialkoxysilane, methyl polysilicate, ethyl polysilicate, and epoxy group-containing ethyl polysilicate. The adhesion promoter is preferably a low-viscosity liquid, and although there are no limitations on its viscosity, it is preferably within the range of 1 to 500 mPa·s at 25°C. The content of the adhesion promoter is also not limited, but is preferably within the range of 0.01 to 10 parts by mass per 100 parts by mass of the total of the present composition.

[0119] In the present invention, a particularly suitable adhesion promoter is a reaction mixture of an amino-containing organoalkoxysilane and an epoxy-containing organoalkoxysilane. This component improves the initial adhesion to various substrates that come into contact with the composition during curing, and in particular the low-temperature adhesion to unwashed substrates. Depending on the curing system of the curable silicone composition to which the adhesion promoter is added, the adhesion promoter may also act as a crosslinking agent. Such reaction mixtures are disclosed in JP-B-52-8854 and JP-A-10-195085.

[0120] Examples of alkoxysilanes having an amino group-containing organic group that constitute such a component include aminomethyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)aminomethyltributoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, and 3-anilinopropyltriethoxysilane.

[0121] Examples of epoxy group-containing organoalkoxysilanes include 3-glycidoxyprolyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and 2-(3,4-epoxycyclohexyl)ethylmethyldimethoxysilane.

[0122] The molar ratio of these alkoxysilanes having an amino group-containing organic group to those having an epoxy group-containing organic group is preferably within the range of (1:1.5) to (1:5), and particularly preferably within the range of (1:2) to (1:4). This component (e1) can be easily synthesized by mixing the above-mentioned alkoxysilanes having an amino group-containing organic group and alkoxysilanes having an epoxy group-containing organic group and reacting them at room temperature or under heating.

[0123] In particular, in the present invention, when an alkoxysilane having an amino group-containing organic group is reacted with an alkoxysilane having an epoxy group-containing organic group by the method described in JP-A-10-195085, a cyclic silane having the general formula: [ka] {where, R 1 is an alkyl group, an alkenyl group, or an alkoxy group, and R 2 may have the same or different general formula: [ka] (In the formula, R 4 is an alkylene group or an alkyleneoxyalkylene group, R 5 is a monovalent hydrocarbon group, R 6 is an alkyl group, and R 7 is an alkylene group, and R 8 is an alkyl group, an alkenyl group, or an acyl group, and a is 0, 1, or 2. R is a group selected from the group consisting of groups represented by 3 are the same or different hydrogen atoms or alkyl groups. It is particularly preferred that the compound contains a carbasilatrane derivative represented by the following structure: Examples of such carbasilatrane derivatives include carbasilatrane derivatives having a silicon-bonded alkoxy group or a silicon-bonded alkenyl group in one molecule, as represented by the following structure: [ka] (wherein Rc is a group selected from a methoxy group, an ethoxy group, a vinyl group, an allyl group, and a hexenyl group).

[0124] In the present invention, a silatrane derivative represented by the following structural formula may be used as an adhesion promoter. [ka] R in the formula 1are the same or different hydrogen atoms or alkyl groups, in particular R 1 is preferably a hydrogen atom or a methyl group. 2 represents a hydrogen atom, an alkyl group, or a group of the general formula: -R 4 -Si(OR 5 ) x R 6 (3-x) are the same or different groups selected from the group consisting of alkoxysilyl group-containing organic groups represented by the formula: 2 At least one of R is an alkoxysilyl group-containing organic group. 2 Examples of the alkyl group of R include a methyl group. 2 In the alkoxysilyl group-containing organic group, R 4 is a divalent organic group, and examples thereof include an alkylene group or an alkyleneoxyalkylene group, and particularly preferably an ethylene group, a propylene group, a butylene group, a methyleneoxypropylene group, or a methyleneoxypentylene group. 5 is an alkyl group having 1 to 10 carbon atoms, and is preferably a methyl group or an ethyl group. 6 is a substituted or unsubstituted monovalent hydrocarbon group, preferably a methyl group, and x in the formula is 1, 2, or 3, preferably 3.

[0125] Such an R 2 Examples of the alkoxysilyl group-containing organic group include the following groups. -(CH2)2Si(OCH3)3-(CH2)2Si(OCH3)2CH3 -(CH2)3Si(OC2H5)3-(CH2)3Si(OC2H5)(CH3)2 -CH2O(CH2)3Si(OCH3)3 -CH2O(CH2)3Si(OC2H5)3 -CH2O(CH2)3Si(OCH3)2CH3 -CH2O(CH2)3Si(OC2H5)2CH3 -CH2OCH2Si(OCH3)3-CH2OCH2Si(OCH3)(CH3)2

[0126] R in the above formula 3 is at least one group selected from the group consisting of substituted or unsubstituted monovalent hydrocarbon groups, alkoxy groups having 1 to 10 carbon atoms, glycidoxyalkyl groups, oxiranylalkyl groups, and acyloxyalkyl groups; R 3 Examples of the monovalent hydrocarbon group include alkyl groups such as methyl groups. 3 Examples of the alkoxy group of R include a methoxy group, an ethoxy group, and a propoxy group. 3 An example of the glycidoxyalkyl group of R is a 3-glycidoxypropyl group. 3 Examples of the oxiranylalkyl group of R include a 4-oxiranylbutyl group and an 8-oxiranyloctyl group. 3 Examples of the acyloxyalkyl group include an acetoxypropyl group and a 3-methacryloxypropyl group. 3 Preferably, the alkyl group, alkenyl group, or alkoxy group is used, more preferably an alkyl group or an alkenyl group, and particularly preferably a group selected from a methyl group, a vinyl group, an allyl group, and a hexenyl group.

[0127] Furthermore, the composition may contain other optional components, such as heat resistance agents such as iron oxide (red oxide), cerium oxide, cerium dimethylsilanolate, fatty acid cerium salts, cerium hydroxide, and zirconium compounds, as well as dyes, pigments other than white, and flame retardants, so long as the object of the present invention is not impaired.

[0128] The present composition may be used in the form of granules, pellets, or sheets. The pellets are obtained by tableting the present composition, and are excellent in handling, workability, and hardening properties. The "pellets" are also called "tablets". The shape of the pellets is not limited, but they are usually spherical, elliptical, or cylindrical. The size of the pellets is not limited, but they have an average particle diameter or equivalent circle diameter of, for example, 500 μm or more. When producing such a pellet-shaped composition, tableting the present composition in granular form is an efficient production method. When it is desired to make the composition of the present invention in granular form, it is possible to produce it by stirring the components (A) to (C), and optionally the component (D), using a powder kneader described below.

[0129] The composition may be molded into a sheet for use. For example, a sheet made of the curable silicone composition having an average thickness of 10 to 1000 μm has hot-melt properties and is heat-curable at high temperatures, and is therefore advantageous in that it is easy to handle and has excellent melting properties, particularly when used in compression molding.

[0130] Such sheet-like compositions may be produced by first mixing all of the components in a single- or double-screw continuous kneader and then passing the mixture through a twin roll or the like to achieve the desired thickness. Alternatively, the granular curable silicone composition described above may be obtained, and then these may be mixed in a kneader to adjust the thickness.

[0131] [Use as a laminate and film adhesive] The present composition can be used in sheet form, and in particular can be used as a laminate having a structure including a sheet-like member made of the curable silicone composition described above between two film-like substrates equipped with a release layer.

[0132] The method for producing such a peelable laminate is not particularly limited, but Step 1: Mixing the components of the curable silicone composition Step 2: The mixture obtained in step 1 is kneaded while being heated and melted. Step 3: Laminating the heated and melted mixture obtained in step 2 between at least one film having a release surface. Step 4: Stretching the laminate obtained in step 3 between rolls to form a curable silicone sheet having a specific thickness. Optionally, in step 4 etc., a roll with a cooling or temperature regulating function may be used, and after step 4, a step of cutting the obtained laminate comprising the curable silicone sheet may be included.

[0133] The type of the film-like substrate is not particularly limited, and it is possible to appropriately use a polyester film, a polyolefin film, a polycarbonate film, an acrylic film, etc. It is preferable that the sheet-like substrate is non-porous.

[0134] The release layer is a necessary component for easily peeling off the sheet-like member made of the curable silicone composition from the film-like substrate, and may be called a release liner, separator, release layer, or release coating layer.Preferably, the release layer may be a release layer having release coating ability such as a silicone-based release agent, a fluorine-based release agent, an alkyd-based release agent, or a fluorosilicone-based release agent, or a substrate itself that forms physically fine irregularities on the substrate surface or is difficult to adhere to the adhesive layer made of the curable reactive silicone pressure-sensitive adhesive composition of the present invention or its cured product.In particular, in the laminate of the present invention, it is preferable to use a release layer made by curing a fluorosilicone-based release agent as the release layer.

[0135] The above laminate can be used, for example, by applying a sheet-like member made of the curable silicone composition to an adherend and then peeling the uncured sheet-like member from the film-like substrate.

[0136] The present composition is handled in the form of granules, pellets, or sheets at room temperature, and is therefore a non-fluid solid at 25°C. Here, non-fluidity means that it does not deform or flow in an unloaded state, and preferably, when molded into pellets, tablets, or the like, it does not deform or flow in an unloaded state at 25°C. Such non-fluidity can be evaluated, for example, by placing the molded composition on a hot plate at 25°C and not substantially deforming or flowing even when no load or a certain load is applied. If the composition is non-fluid at 25°C, the shape retention at that temperature is good and the surface adhesion is low.

[0137] The softening point of the present composition is preferably 100° C. or lower. Such a softening point means the temperature at which, when a load of 100 grams is applied to a hot plate for 10 seconds and the deformation of the composition is measured after the load is removed, the deformation in the height direction is 1 mm or more.

[0138] The viscosity of the composition tends to decrease rapidly under high temperature and high pressure (i.e., during the molding process), and it is preferable to use a value measured under similar high temperature and high pressure as a useful melt viscosity value. Therefore, it is preferable to measure the melt viscosity of the composition under high pressure using a Koka-shiki flow tester (manufactured by Shimadzu Corporation) rather than measuring it with a rotational viscometer such as a rheometer. Specifically, it is preferable that the melt viscosity of the composition at 150°C is 200 Pa·s or less, more preferably 150 or less. This is because the composition has good adhesion to the substrate after being cooled to 25°C after being hot melted.

[0139] [Method of producing the curable silicone composition] The present composition can be produced by powder mixing components (A) to (C) and any other optional components (including components (D) and (E)) at a temperature of less than 50° C. There are no limitations on the powder mixer used in this production method, and examples include a single-screw or twin-screw continuous mixer, a twin roll, a Ross mixer, a Hobart mixer, a dental mixer, a planetary mixer, a kneader mixer, a laboratory miller, a small grinder, and a Henschel mixer, with a laboratory miller and a Henschel mixer being preferred.

[0140] [Manufacturing method of curable silicone sheet] The curable silicone sheet of the present invention has hot melt properties and is characterized by being made of a curable silicone composition that contains an organopolysiloxane resin, a curing agent, and a functional filler. The manufacturing method of the present invention comprises the following steps 1 to 4. Step 1: Mixing the components of the curable silicone composition at a temperature of 50° C. or higher Step 2: The mixture obtained in step 1 is kneaded while being heated and melted. Step 3: Laminating the heated and melted mixture obtained in step 2 between at least one film having a release surface. Step 4: Stretching the laminate obtained in step 3 between rolls to form a curable silicone sheet having a specific thickness. Here, "having hot-melt properties" refers to a softening point within the range of 50° C. to 200° C. and the property of softening or flowing when heated. Furthermore, the curable silicone sheet according to the present invention is suitable as long as the mixture of the organopolysiloxane resin, curing agent, and functional filler has hot-melt properties, regardless of the hot-melt properties of the organopolysiloxane resin that is a component of the curable silicone sheet.

[0141] [Process 1] The above step 1 is a mixing step of the components of the curable silicone composition, which are an organopolysiloxane resin (preferably in the form of fine particles), a curing agent, and a curable granular silicone composition containing a functional filler. Each of these components is as described above.

[0142] The mixture provided by step 1 is a curable granular silicone composition, and the mixture as a whole has hot melt properties. Meanwhile, the mixture is non-fluid at 25°C. Here, non-fluid means that it does not deform or flow in an unloaded state, and preferably does not deform or flow in an unloaded state at 25°C when molded into pellets, tablets, or the like. Such non-fluidity can be evaluated, for example, by placing the molded composition on a hot plate at 25°C and not substantially deforming or flowing even when no load or a certain load is applied. Non-fluidity at 25°C means that the shape retention at that temperature is good and the surface adhesion is low.

[0143] The softening point of the mixture provided in step 1 is 200° C. or less, and preferably 150° C. or less. Such a softening point means a temperature at which, when a load of 100 grams is pressed down from above on a hot plate for 10 seconds and the load is removed, the deformation of the composition is measured and the deformation in the height direction is 1 mm or more.

[0144] The softening point of the mixture provided in step 1 is 200°C or lower, and in step 2 described below, the entire mixture is heated to a temperature equal to or higher than the softening point of the mixture, thereby heating and melting the mixture to provide it with a certain degree of fluidity. By molding the softened or molten product, a curable silicone sheet consisting of the curable granular silicone composition and having hot melt properties can be obtained.

[0145] The process of mixing the organopolysiloxane resin, the curing agent, the functional filler, and any other optional components is not particularly limited, but the mixture as a whole, preferably the organopolysiloxane resin fine particles, can be powder-mixed at a temperature below the softening point. The powder mixer used in this production method is not limited, and examples thereof include a single-shaft or double-shaft continuous mixer, a two-roll mill, a Ross mixer, a Hobart mixer, a dental mixer, a planetary mixer, a kneader mixer, a laboratory miller, a small grinder, and a Henschel mixer, and preferably a laboratory miller, a small grinder, and a Henschel mixer.

[0146] [Process 2] Step 2 is a step of kneading the mixture obtained in step 1 while heating and melting it. By heating and kneading the mixture having heat meltability at a temperature equal to or higher than its softening point, preferably at a temperature range of 50°C to 200°C, the entire composition melts or softens, and the organopolysiloxane resin fine particles, the curing agent, and the functional filler can be uniformly dispersed throughout. When the mixture is pressure-molded into a sheet in step 3 and then in step 4, a uniform thin-layer molded sheet can be formed by one pressurization, and there is a practical benefit in that molding defects and cracks in the sheet body can be avoided. On the other hand, if the temperature is below the lower limit, softening may be insufficient, making it difficult to obtain a molten or softened mixture in which each component is uniformly dispersed throughout, even when mechanical force is used. Even if such a mixture is pressure-molded into a sheet in step 3 and then in step 4, a uniform thin-layer molded sheet cannot be formed, which may cause breakage or cracking of the sheet. Conversely, if the temperature exceeds the upper limit, the curing agent will react during mixing, causing the entire mixture to thicken or harden significantly, losing hot-melt properties and forming a cured product, which is not preferred. For this reason, when a hydrosilylation catalyst is used in component (C), it is preferable to use a platinum-containing hydrosilylation catalyst in the form of fine particles dispersed or encapsulated in a thermoplastic resin.

[0147] When the mixture obtained in step 1 has a low heat melt viscosity and is highly fluid, it can be pre-molded in advance in step 3 described below and then laminated on a release film. Specifically, when the melt viscosity of the mixture obtained in step 2 after heat melting at 150°C as measured by a high-temperature flow tester is in the range of 1 to 1,000 Pas, pre-molding can be performed in step 3.

[0148] On the other hand, when the mixture obtained in step 1 has a high heat melt viscosity and poor fluidity, in step 2, the mixture obtained in step 1 is melt-kneaded at a temperature equal to or higher than its softening point to obtain a homogeneous composition form, and then, in step 3, the mixture may be laminated on a release film without being pre-molded.

[0149] The mixing device in step 2 is not limited, and may be a batch type kneader, Banbury mixer, Henschel mixer, planetary mixer, 2-roll mill, 3-roll mill, Ross mixer, Labo Plastomill, etc., equipped with heating and cooling functions, or a continuous type heating and kneading device, such as a single screw extruder or a twin screw extruder, equipped with heating and cooling functions, and is not particularly limited, but is selected according to the efficiency of the processing time and the control ability of shear heat generation. In terms of processing time, it may be a continuous type heating and kneading device, such as a single screw extruder or a twin screw extruder, or a batch type mixer, such as a Labo Plastomill. However, from the viewpoint of production efficiency of the curable silicone sheet, a continuous type heating and kneading device, such as a single screw extruder or a twin screw extruder, is preferably used.

[0150] [Process 3] Step 3 is a step in which the heat-melted mixture obtained in step 2 is laminated between films having at least one release surface, and is a preliminary step for pressure molding in step 4. By forming a laminate in which the mixture obtained in step 2 is sandwiched between films, pressure molding by roll stretching can be performed from above the film to obtain a sheet-like molded product, and after molding, only the film can be removed from the sheet-like molded product by using the release surface.

[0151] The mixture obtained in step 2 after heat melting is laminated between two films. Depending on the use form of the obtained curable silicone sheet, it is preferable that both of the two films have a release surface, and it is particularly preferable that the mixture obtained in step 2 is laminated between the release surfaces of each film in step 3. By adopting such a laminated form, a laminated sheet that can be peeled off from both sides can be obtained through pressure molding in step 4 and subsequent arbitrary cutting, in which a thin-layer curable silicone sheet is sandwiched between release films, and when used, the films on both sides can be peeled off to expose only the curable silicone sheet without worrying about damaging the formed curable silicone sheet.

[0152] The substrate of the film used in step 3 is not particularly limited, and examples thereof include paperboard, cardboard paper, clay-coated paper, polyolefin-laminated paper, particularly polyethylene-laminated paper, synthetic resin film / sheet, natural fiber cloth, synthetic fiber cloth, artificial leather cloth, and metal foil. In particular, synthetic resin films / sheets are preferred, and examples of synthetic resins include polyimide, polyethylene, polypropylene, polystyrene, polyvinyl chloride, polyvinylidene chloride, polycarbonate, polyethylene terephthalate, and nylon. In particular, when heat resistance is required, films of heat-resistant synthetic resins such as polyimide, polyether ether ketone, polyethylene naphthalate (PEN), liquid crystal polyarylate, polyamide imide, and polyether sulfone are suitable. On the other hand, in applications requiring visibility such as display devices, transparent substrates, specifically transparent materials such as polypropylene, polystyrene, polyvinylidene chloride, polycarbonate, polyethylene terephthalate, and PEN are suitable.

[0153] The thickness of the film is not particularly limited, but is usually about 5 to 300 μm.

[0154] The film has at least one release layer, and the release layer is preferably in contact with the mixture obtained in step 2. This allows the hot-melt curable silicone sheet that has been pressure-molded through steps 3 and 4 to be easily peeled off from the film. The release layer may also be called a release liner, separator, release layer, or release coating layer, and may be a release layer having release coating ability such as a silicone-based release agent, a fluorine-based release agent, an alkyd-based release agent, or a fluorosilicone-based release agent, or a substrate itself that physically forms fine irregularities on the substrate surface or is difficult to adhere to the hot-melt curable silicone sheet of the present invention.

[0155] In step 3, the mixture obtained in step 2 is laminated between two films. The process is not particularly limited, but the mixture obtained in step 2 is supplied by being discharged or applied onto the release layer of one film, and the release layer of the other film is attached onto the mixture to form a laminate. At this time, in the continuous manufacturing process of the curable silicone sheet, each film is transported via a rotating roll to the supply position of the mixture in step 2, and the lamination operation between the films is performed.

[0156] The amount of the mixture obtained in step 2 to be supplied between the films in step 3 can be designed according to the production speed and scale. As an example, the mixture obtained in step 2 can be supplied between the films at a supply rate of 1 to 10 kg / hour, but it goes without saying that this is not limited to this. However, the amount of the mixture obtained in step 2 to be laminated between the films in step 3 must be determined according to the average thickness of the curable silicone sheet designed in step 4, and must be a thickness that allows rolling processing in step 4.

[0157] When the mixture obtained in step 1 has a low heat melt viscosity and is highly fluid, it is preferable that the heat melted mixture obtained in step 2 is extruded while being molded into a film using a die, and laminated between the films in step 3. Here, the die is used to pre-mold the mixture, and the type and thickness at the time of pre-mold are not particularly limited, but it is possible and preferable to use a T-shaped die to pre-mold into a substantially sheet-like shape having a thickness in the range of 100 to 2000 μm (= 2 mm).

[0158] When the mixture obtained in step 1 has a low heat melt viscosity and is highly fluid, it is preferable to include a step of cooling or temperature adjustment of the entire laminate obtained in step 3 after the above-mentioned provisional molding, either as a step prior to step 4 or in step 4. This is because the heat melt is cooled to make it solid so that the pressure molding in step 4 can be effectively performed. The cooling step is not particularly limited, but can be performed by cooling the mixture supplied or laminated on the film by a cooling roll or the like to a range of −50° C. to room temperature using a cooling means such as air cooling or a cooling solvent. Details of the temperature adjustment will be described in step 4.

[0159] On the other hand, when the mixture obtained in step 1 has a high heat melt viscosity and poor fluidity, in step 3, the semi-solid mixture may be supplied onto a film and laminated without being pre-molded.

[0160] [Step 4] Step 4 is a step in which the laminate obtained in step 3 above is stretched between rolls to form a curable silicone sheet having a specific thickness, and this step involves pressurizing the mixture obtained in step 2 and stretching it from above the film to form a uniform curable silicone sheet.

[0161] The rolling process in step 4 can be carried out on the laminate obtained in step 3 using a known rolling method such as roll rolling. In particular, roll rolling has the advantage that a curable silicone sheet of the desired thickness can be designed by adjusting the gap between the rolls. For example, by rolling while adjusting the gap between the rolls to a constant value so that the average thickness is in the range of 10 to 2000 μm, a curable silicone sheet with excellent flatness and extremely few defects on the surface and inside of the sheet can be obtained. More specifically, in the case of roll rolling, it is particularly preferable that the gap between the rolls is adjusted to a range of 1.5 to 4.0 times the average thickness of the desired organopolysiloxane cured film.

[0162] A substantially flat curable silicone sheet having a thickness of 10 to 2000 μm can be obtained by performing the stretching in step 4. The mixture after heating and melting in step 2 can be roll-stretched in step 3 in a state in which it is laminated between release films to obtain a peelable laminate containing a curable silicone sheet having hot melt properties, which has few defects and excellent handling workability when peeled off.

[0163] [Temperature adjustment in step 4] In step 4, when the laminate obtained in step 3 is stretched between rolls, it is preferable that the rolls further have a temperature control function, and adjust the temperature of the entire laminate during roll rolling, and heat or cool it as necessary. This temperature control has the practical benefit of keeping the gap between the rolls stable and improving the flatness and uniformity (uniformity of film thickness) of the obtained hot-melt curable silicone sheet. The specific temperature control range can be appropriately designed depending on the heat resistance of the film, the thickness (design thickness) of the curable silicone sheet, its reactivity, etc., but is generally within the range of 5 to 150 ° C.

[0164] [Cutting process] By step 4, a release laminate in which a hot-melt curable silicone sheet is interposed between release films can be obtained, and optionally, a step of cutting the laminate containing the curable silicone sheet may be included. In addition, the curable silicone sheet may be wound up by a winding device. This allows a release laminate containing a hot-melt curable silicone sheet of a desired size to be obtained.

[0165] [Laminate] The laminate obtained by the above steps is a laminate having a structure in which a substantially flat curable silicone sheet having hot melt properties and a thickness of 10 to 2000 μm, which is made of organopolysiloxane resin fine particles, a curing agent, and a functional filler, is laminated between films having at least one release surface. Note that both of the films may and preferably have a release surface.

[0166] [Curable silicone sheet] The curable silicone sheet obtained by the manufacturing method of the present invention is a curable silicone granular composition consisting of an organopolysiloxane resin, a curing agent and a functional filler, has hot melt properties, and can be used as a heat-melting adhesive material.In particular, the curable silicone sheet has excellent moldability, gap filling properties and adhesive strength, and can be used as a die attachment film or a film adhesive.It can also be suitably used as a curable silicone sheet for compression molding or press molding.

[0167] Specifically, the curable silicone sheet obtained by the production method of the present invention may be peeled off from the release film, and then placed at a desired location on a semiconductor or the like, a film adhesive layer that utilizes gap-filling properties for unevenness and gaps may be formed on the adherend, and the adherends may be temporarily fixed, positioned, and bonded together, and the curable silicone sheet may be heated to 150° C. or higher to bond the adherends together with the cured product of the curable silicone sheet. The release film may be peeled off after the curable silicone sheet is heated to form a cured product, and the timing of peeling may be selected depending on the application and method of use of the curable silicone sheet.

[0168] Since the curable silicone sheet is hot-melt, it can be softened or fluidized by heating the sheet before final curing, and even if the adherend has unevenness on its surface, it can fill the unevenness and gaps without gaps to form an adhesive surface.As a heating means for the curable silicone sheet, for example, various thermostatic baths, hot plates, electromagnetic heating devices, heating rolls, etc. can be used.In order to perform lamination and heating more efficiently, for example, an electric heating press, a diaphragm type laminator, a roll laminator, etc. are preferably used.

[0169] [Method of molding the cured product] The present composition can be cured by a method comprising at least the following steps (I) to (III). (I) heating the composition to 100° C. or higher to melt it; (II) a step of injecting the curable silicone composition obtained in step (I) into a mold, or a step of spreading the curable silicone composition obtained in step (I) throughout the mold by clamping the mold; and (III) A step of curing the curable silicone composition injected in the step (II)

[0170] In the above steps, a transfer molding machine, a compression molding machine, an injection molding machine, an auxiliary ram type molding machine, a slide type molding machine, a double ram type molding machine, a low pressure encapsulation molding machine, etc. can be used. In particular, the composition of the present invention can be suitably used for the purpose of obtaining a cured product by transfer molding and compression molding.

[0171] Finally, in step (III), the curable silicone composition injected (applied) in step (II) is cured. When (c1) an organic peroxide is used as component (C), the heating temperature is preferably 150°C or higher, or 170°C or higher, and when (c2) an organohydrogenpolysiloxane having at least two silicon-bonded hydrogen atoms in the molecule and a hydrosilylation reaction catalyst are used, the heating temperature is preferably 100°C or higher, or 130°C or higher.

[0172] Meanwhile, the curable silicone composition of the present invention can be molded into a thin film sheet having a thickness in the range of 100 to 1000 μm by sandwiching it between sheet-like substrates equipped with a release layer and molding it to a predetermined thickness through a two-roll machine or the like, as described above. A thin film sheet made of the curable silicone composition can be used as a die attach film for use in the manufacture of semiconductor chips or the like, or as a film-like curable silicone adhesive.

[0173] [Use of the composition] This composition has hot melt properties, excellent handling and curing properties when melted (hot melt), and excellent coloring resistance at high temperatures of the resulting cured product, so it is useful for semiconductor components such as light reflectors for light emitting / optical devices and optical semiconductors having the cured product. Furthermore, since the cured product has excellent mechanical properties, it is suitable as a sealant for semiconductors; a sealant for power semiconductors such as SiC and GaN; and an adhesive, potting agent, protective agent, and coating agent for electrical and electronic products. In addition, since this composition has hot melt properties, it is also suitable as a material for transfer molding, compression molding, or injection molding. In particular, it is suitable for use as a sealant for semiconductors that use an overmolding method during molding. Furthermore, the composition in a sheet form can be used as a curable film adhesive or a stress buffer layer between two types of substrates with different linear expansion coefficients.

[0174] The curable silicone composition of the present invention, particularly a pellet- or sheet-shaped curable silicone composition, can be used for sealing a large area of ​​a semiconductor substrate (including a wafer). Furthermore, a sheet obtained by molding the curable silicone composition of the present invention into a sheet can be used for a die attach film, sealing of a flexible device, a stress relaxation layer for bonding two different substrates, etc.

[0175] [Uses of the cured product] The use of the cured product of the present invention is not particularly limited, but the composition of the present invention has hot melt properties, is excellent in moldability and mechanical properties, and the cured product exhibits the above-mentioned characteristic behavior of the average linear expansion coefficient and storage modulus at room temperature to high temperatures. Therefore, the cured product obtained by curing the composition can be suitably used as a member for semiconductor devices, and can be suitably used as a sealing material for semiconductor elements, IC chips, etc., and an adhesive / bonding material for semiconductor devices.

[0176] Although the semiconductor device having a member made of the cured product of the present invention is not particularly limited, it is particularly preferably a light-emitting semiconductor device that is a light-emitting / optical device. The cured product of the present invention has excellent coloring resistance at high temperatures, and therefore can be suitably used as a light reflecting material for optical semiconductor devices in which whiteness is important. EXAMPLES

[0177] The hot-melt curable silicone composition of the present invention and its manufacturing method are described in detail with reference to examples and comparative examples. In the formula, Me and Vi represent a methyl group and a vinyl group, respectively. The softening point of the curable silicone composition of each example and comparative example was measured by the following method. The curable silicone composition was heated at 150°C for 2 hours to prepare a cured product, and the elastic modulus and tensile elongation were measured by the following method. The results are shown in Table 1.

[0178] [Melt Viscosity] The melt viscosity of the curable silicone composition at 150° C. was measured using a Koka-shiki Flow Tester CFT-500EX (manufactured by Shimadzu Corporation) under a pressure of 100 kgf using a nozzle with a diameter of 0.5 mm.

[0179] [Storage modulus] The curable silicone composition was heated at 150° C. for 2 hours to produce a cured product. The storage modulus of this cured product was measured from -50° C. to 250° C. using a rheometer ARES (manufactured by TA Instruments Japan, Inc.), and the value at 25° C. was read. Table 1 shows the measured values ​​at 25° C.

[0180] [Tensile elongation] A cured product was produced by heating the curable silicone composition for 2 hours at 150° C. The tensile elongation of this cured product was measured according to the method specified in JIS K 6251-2010 "Vulcanized rubber and thermoplastic rubber -- Determination of tensile properties."

[0181] [Thermal Conductivity] The curable silicone composition was heated at 150°C for 2 hours to produce a cured product measuring 1.5cm x 1.5cm x 1.0cm (thickness). The thermal conductivity of this cured product was measured by the hot disk method using a TPS500S (manufactured by Hot Disk Co., Ltd.). The results are shown in Table 1.

[0182] Organopolysiloxane resins containing hydrosilylation catalysts were prepared by the methods shown in Reference Examples 1 to 7 below, and the presence or absence of hot melt properties was evaluated based on the presence or absence of softening point / melt viscosity. Also, organopolysiloxane resin fine particles were prepared by the methods shown in Reference Examples 8 to 13. In the Reference Examples, 1,1,3,3-tetramethyl-1,3-divinyldisiloxane used in the platinum complex, which is the hydrosilylation catalyst, is referred to as "1,3-divinyltetramethyldisiloxane."

[0183] (Measurement of molecular weight of organopolysiloxane resin) The weight average molecular weight (Mw) of the organopolysiloxane resin in each Reference Example was determined in terms of standard polystyrene using a gel permeation chromatography (GPC) manufactured by Waters Corporation and toluene as a solvent.

[0184] [Reference example 1] In a 1 L flask, at 25°C, a white solid was obtained with the average unit formula: (Me3SiO 1 / 2 ) 0.44 (SiO 4 / 2 ) 0.56 (HO 1 / 2 ) 0.02 270.5 g of a 55 mass% xylene solution of an organopolysiloxane resin represented by the formula (I) and 0.375 g of a 1,3-divinyltetramethyldisiloxane solution of a platinum 1,3-divinyltetramethyldisiloxane complex (platinum metal content = about 4000 ppm) were added and stirred uniformly at room temperature (25 ° C) to prepare a xylene solution of organopolysiloxane resin (1) containing 10 ppm platinum metal by mass. In addition, this organopolysiloxane resin (1) did not soften / melt even when heated to 200 ° C, and did not have hot melt properties. In addition, the weight average molecular weight obtained by GPC measurement in toluene solvent was 18,500 Da.

[0185] [Reference example 2] In a 1 L flask, at 25°C, a white solid was obtained with the average unit formula: (Me3SiO 1 / 2 ) 0.46 (SiO 4 / 2 ) 0.54 (HO 1 / 2 ) 0.02 270.5 g of a 55 mass% xylene solution of an organopolysiloxane resin represented by the formula (I) and 0.375 g of a 1,3-divinyltetramethyldisiloxane solution of a platinum 1,3-divinyltetramethyldisiloxane complex (platinum metal content = about 4000 ppm) were added and stirred uniformly at room temperature (25 ° C) to prepare a xylene solution of organopolysiloxane resin (2) containing 10 ppm by mass as platinum metal. In addition, this organopolysiloxane resin (2) did not soften / melt even when heated to 200 ° C, and did not have hot melt properties. In addition, the weight average molecular weight obtained by GPC measurement in toluene solvent was 11,000 Da.

[0186] [Reference example 3] In a 1 L flask, at 25°C, a white solid was obtained with the average unit formula: (Me3SiO 1 / 2 ) 0.475 (SiO 4 / 2 ) 0.525 (HO 1 / 2 ) 0.02 270.5 g of a 55 mass% xylene solution of an organopolysiloxane resin represented by the formula (I) and 0.375 g of a 1,3-divinyltetramethyldisiloxane solution of a platinum 1,3-divinyltetramethyldisiloxane complex (platinum metal content = about 4000 ppm) were added and stirred uniformly at room temperature (25 ° C) to prepare a xylene solution of organopolysiloxane resin (3) containing 10 ppm by mass as platinum metal. In addition, this organopolysiloxane resin (3) did not soften / melt even when heated to 200 ° C, and did not have hot melt properties. In addition, the weight average molecular weight obtained by GPC measurement in toluene solvent was 7,000 Da.

[0187] [Reference example 4] In a 1 L flask, at 25°C, a white solid was obtained with the average unit formula: (Me3SiO 1 / 2 ) 0.49 (SiO 4 / 2 ) 0.51 (HO 1 / 2 ) 0.02 270.5 g of a 55 mass% xylene solution of an organopolysiloxane resin represented by the formula (I) and 0.375 g of a 1,3-divinyltetramethyldisiloxane solution of a platinum 1,3-divinyltetramethyldisiloxane complex (platinum metal content = about 4000 ppm) were added and stirred uniformly at room temperature (25 ° C) to prepare a xylene solution of organopolysiloxane resin (4) containing 10 ppm by mass as platinum metal. In addition, this organopolysiloxane resin (4) did not soften / melt even when heated to 200 ° C, and did not have hot melt properties. In addition, the weight average molecular weight obtained by GPC measurement in toluene solvent was 4,000 Da.

[0188] [Reference example 5] Average unit formula: (Me3SiO 1 / 2 ) 0.65 (SiO 4 / 2 ) 0.35 (HO 1 / 2 ) 0.01 A 55% by mass xylene solution of the organopolysiloxane resin represented by the formula was dried under reduced pressure to remove the xylene, yielding an organopolysiloxane resin that was liquid at room temperature. The weight average molecular weight obtained by GPC measurement in a toluene solvent was 1,100 Da. 70.0 g of this organopolysiloxane resin and ViMe2SiO(Me2SiO) 800 SiViMe2 When 30.0 g of a dimethylpolysiloxane capped at both molecular chain terminals with dimethylvinylsiloxy groups (vinyl group content = 0.09 mass %) was mixed, a mixture that was liquid at room temperature and did not exhibit hot melt properties.

[0189] [Reference example 6] In a 1 L flask, at 25°C, a white solid was obtained with the average unit formula: (Me2ViSiO 1 / 2 ) 0.05 (Me3SiO 1 / 2 ) 0.39 (SiO 4 / 2 ) 0.56 (HO 1 / 2 ) 0.02 270.5 g of a 55 mass% xylene solution of an organopolysiloxane resin represented by the formula (I) and 0.375 g of a 1,3-divinyltetramethyldisiloxane solution of a platinum 1,3-divinyltetramethyldisiloxane complex (platinum metal content = about 4000 ppm) were added and stirred uniformly at room temperature (25 ° C) to prepare a xylene solution of organopolysiloxane resin (6) containing 10 ppm by mass as platinum metal. In addition, this organopolysiloxane resin (6) did not soften / melt even when heated to 200 ° C, and did not have hot melt properties. In addition, the weight average molecular weight obtained by GPC measurement in toluene solvent was 18,000 Da.

[0190] [Reference example 7] In a 1 L flask, at 25°C, a white solid was obtained with the average unit formula: (Me2ViSiO 1 / 2 ) 0.09 (Me3SiO 1 / 2 )0.43 (SiO 4 / 2 ) 0.48 (HO 1 / 2 ) 0.03 270.5 g of a 55 mass% xylene solution of an organopolysiloxane resin represented by the formula (I) and 0.375 g of a 1,3-divinyltetramethyldisiloxane solution of a platinum 1,3-divinyltetramethyldisiloxane complex (platinum metal content = about 4000 ppm) were added and stirred uniformly at room temperature (25 ° C) to prepare a xylene solution of organopolysiloxane resin (7) containing 10 ppm by mass as platinum metal. In addition, this organopolysiloxane resin (7) did not soften / melt even when heated to 200 ° C, and did not have hot melt properties. In addition, the weight average molecular weight obtained by GPC measurement in toluene solvent was 2,900 Da.

[0191] [Reference Example 8: Non-hot melt organopolysiloxane resin fine particles (1)] The xylene solution of organopolysiloxane resin (1) prepared in Reference Example 1 was granulated at 50°C by a spray method using a spray dryer while removing the xylene, to obtain spherical resin microparticles. The microparticles were aged for 24 hours in an oven set at 120°C to prepare spherical non-hot melt organopolysiloxane resin microparticles (1). When the microparticles were observed with an optical microscope, the particle diameter was 5 to 10 μm, and when the microparticles were exposed to 200°C for 1 hour, the heat loss was 0.8 wt%.

[0192] [Reference Example 9: Non-hot melt organopolysiloxane resin fine particles (2)] The xylene solution of organopolysiloxane resin (2) prepared in Reference Example 2 was granulated at 50°C by a spray method using a spray dryer while removing the xylene, to obtain spherical resin microparticles. The microparticles were aged for 24 hours in an oven set at 120°C to prepare spherical non-hot melt organopolysiloxane resin microparticles (2). When the microparticles were observed with an optical microscope, the particle diameter was 5 to 10 μm, and when the microparticles were exposed to 200°C for 1 hour, the heat loss was 0.8 wt%.

[0193] [Reference Example 10: Non-hot melt organopolysiloxane resin fine particles (3)] The xylene solution of organopolysiloxane resin (3) prepared in Reference Example 3 was granulated at 50°C by a spray method using a spray dryer while removing the xylene, to obtain spherical resin microparticles. The microparticles were aged for 24 hours in an oven set at 120°C to prepare spherical non-hot melt organopolysiloxane resin microparticles (3). When the microparticles were observed with an optical microscope, the particle diameter was 5 to 10 μm, and when the microparticles were exposed to 200°C for 1 hour, the heat loss was 0.7 wt%.

[0194] [Reference Example 11: Non-hot melt organopolysiloxane resin fine particles (4)] The xylene solution of organopolysiloxane resin (4) prepared in Reference Example 4 was granulated at 50°C by a spray method using a spray dryer while removing the xylene, to obtain spherical resin microparticles. The microparticles were aged for 24 hours in an oven set at 120°C to prepare spherical non-hot melt organopolysiloxane resin microparticles (4). When the microparticles were observed with an optical microscope, the particle diameter was 5 to 10 μm, and when the microparticles were exposed to 200°C for 1 hour, the heat loss was 0.7 wt%.

[0195] [Reference Example 12: Non-hot melt organopolysiloxane resin fine particles (6)] The xylene solution of organopolysiloxane resin (6) prepared in Reference Example 6 was granulated at 50°C by a spray method using a spray dryer while removing the xylene, to obtain spherical resin microparticles. The microparticles were aged for 24 hours in an oven set at 120°C to prepare spherical non-hot melt organopolysiloxane resin microparticles (6). When the microparticles were observed with an optical microscope, the particle diameter was 5 to 10 μm, and when the microparticles were exposed to 200°C for 1 hour, the heat loss was 0.7 wt%.

[0196] [Reference Example 13: Non-hot melt organopolysiloxane resin fine particles (7)] The xylene solution of organopolysiloxane resin (7) prepared in Reference Example 7 was granulated at 50°C by a spray method using a spray dryer while removing the xylene, to obtain spherical resin microparticles. The microparticles were aged for 24 hours in an oven set at 120°C to prepare spherical non-hot melt organopolysiloxane resin microparticles (7). When the microparticles were observed with an optical microscope, the particle diameter was 5 to 10 μm, and when the microparticles were exposed to 200°C for 1 hour, the heat loss was 0.7 wt%.

[0197] [Example 1] Non-hot melt organopolysiloxane resin fine particles (2) (vinyl group content = 0 mass%) 69.9 g, formula: ViMe2SiO(Me2SiO) 800 SiViMe2 29.9 g of dimethylpolysiloxane terminated at both molecular chain ends with dimethylvinylsiloxy groups (vinyl group content = 0.09% by mass), formula: Me3SiO(MeHSiO)7(Me2SiO) 6.5 SiMe3 0.2 g of an organohydrogenpolysiloxane represented by the formula {the amount of silicon-bonded hydrogen atoms in the organohydrogenpolysiloxane is 1.4 moles per mole of vinyl groups in the dimethylpolysiloxane terminally blocked with dimethylvinylsiloxy groups}, 82.8 g of alumina having an average particle size of 0.44 μm (AES-12 manufactured by Sumitomo Chemical), 166.1 g of alumina having an average particle size of 3.0 μm (AL-M73A manufactured by Sumitomo Chemical), 364.1 g of alumina having an average particle size of 37.4 μm (AZ35-125 manufactured by Micron Company of Nippon Steel & Sumikin Materials Co., Ltd.), and 1-ethynyl-1-cyclohexanol (an amount equivalent to 1000 ppm by mass relative to the composition) were all charged into a small grinder at once and stirred at room temperature (25° C.) for 1 minute to prepare a uniform curable granular silicone composition. This composition contained 0.10 mol % of vinyl groups per 100 g of silicone component. The results of measuring the melt viscosity and other properties of this composition are shown in Table 1.

[0198] [Example 2] Non-hot melt organopolysiloxane resin fine particles (3) (vinyl group content = 0 mass%) 68.5 g, 1.5 g of non-hot melt organopolysiloxane resin fine particles (7) (vinyl group content = 3.10 mass%), formula: ViMe2SiO(Me2SiO) 800 SiViMe2 29.7 g of dimethylpolysiloxane terminated at both molecular chain ends with dimethylvinylsiloxy groups (vinyl group content = 0.09% by mass), formula: (HMeSiO 1 / 2 ) 0.67 (SiO 4 / 2 ) 0.33 0.30 g of organohydrogenpolysiloxane resin (content of silicon-bonded hydrogen atoms = 0.95% by mass) {an amount such that the organohydrogenpolysiloxane contains 1.1 moles of silicon-bonded hydrogen atoms per mole of vinyl groups in the organopolysiloxane resin fine particle (7) and the dimethylpolysiloxane terminally blocked with dimethylvinylsiloxy groups}, 82.8 g of alumina having an average particle size of 0.44 μm (AES-12 manufactured by Sumitomo Chemical), 166.1 g of alumina having an average particle size of 3.0 μm (AL-M73A manufactured by Sumitomo Chemical), 364.1 g of alumina having an average particle size of 37.4 μm (AZ35-125 manufactured by Micron Company of Nippon Steel & Sumikin Materials Co., Ltd.), and 1-ethynyl-1-cyclohexanol (an amount equivalent to 1000 ppm by mass relative to the composition) were all charged into a small grinder at once, and stirred at room temperature (25° C.) for 1 minute to prepare a uniform curable granular silicone composition. This composition contained 0.27 mol % of vinyl groups per 100 g of silicone component. The results of measuring the melt viscosity and other properties of this composition are shown in Table 1.

[0199] [Example 3] Non-hot melt organopolysiloxane resin fine particles (4) (vinyl group content = 0 mass%) 68.6 g, 1.5 g of non-hot melt organopolysiloxane resin fine particles (7) (vinyl group content = 1.91% by mass), formula: ViMe2SiO(Me2SiO) 800 SiViMe2 29.5 g of dimethylpolysiloxane terminated at both molecular chain ends with dimethylvinylsiloxy groups (vinyl group content = 0.09% by mass), formula: Me3SiO(MeHSiO)7(Me2SiO) 6.5 SiMe3 0.4 g of an organohydrogenpolysiloxane represented by the formula {an amount such that the amount of silicon-bonded hydrogen atoms in the organohydrogenpolysiloxane resin is 1.0 mole per mole of vinyl groups in the organopolysiloxane resin fine particle (7) and the dimethylpolysiloxane terminally blocked with dimethylvinylsiloxy groups}, 82.8 g of alumina having an average particle size of 0.44 μm (AES-12 manufactured by Sumitomo Chemical), 166.1 g of alumina having an average particle size of 3.0 μm (AL-M73A manufactured by Sumitomo Chemical), 364.1 g of alumina having an average particle size of 37.4 μm (AZ35-125 manufactured by Micron Company of Nippon Steel & Sumikin Materials Co., Ltd.), and 1-ethynyl-1-cyclohexanol (an amount equivalent to 1000 ppm by mass relative to the composition) were all charged into a small grinder at once, and stirred at room temperature (25° C.) for 1 minute to prepare a uniform curable granular silicone composition. This composition contained 0.27 mol % of vinyl groups per 100 g of silicone component. The results of measuring the melt viscosity and other properties of this composition are shown in Table 1.

[0200] [Example 4] The mixture was 112.5 g of alumina having an average particle size of 0.44 μm (AES-12 manufactured by Sumitomo Chemical), 234.0 g of alumina having an average particle size of 3.0 μm (AL-M73A manufactured by Sumitomo Chemical), 553.1 g of alumina having an average particle size of 37.4 μm (AZ35-125 manufactured by Micron Company, Nippon Steel & Sumikin Materials Co., Ltd.), and had a viscosity of 23 mPa s. The formula: Me2ViSiO(Me2SiO) 29 Si(OMe)3 3.6 g of dimethylpolysiloxane (vinyl group content = 1.30 mass%) represented by the formula was added to a small crusher at once, and stirred at room temperature (150 ° C) for 1 minute to perform a surface treatment on the alumina, and the temperature of the crusher was returned to 25 ° C. Next, Non-hot melt organopolysiloxane resin fine particles (3) (vinyl group content = 0 mass%) 67.1 g, formula: ViMe2SiO(Me2SiO) 800 SiViMe2 29.0 g of dimethylpolysiloxane terminated at both molecular chain ends with dimethylvinylsiloxy groups (vinyl group content = 0.09% by mass), formula: (HMeSiO 1 / 2 ) 0.67 (SiO 4 / 2 ) 0.33 0.30 g of organohydrogenpolysiloxane resin (content of silicon-bonded hydrogen atoms = 0.95% by mass) {an amount such that the amount of silicon-bonded hydrogen atoms in the organohydrogenpolysiloxane is 1.0 mole per mole of vinyl groups in the dimethylpolysiloxane capped at both molecular chain terminals and one terminal with dimethylvinylsiloxy groups}, 1-ethynyl-1-cyclohexanol (in an amount equivalent to 1000 ppm by mass of the composition) was added all at once to a small grinder and stirred at room temperature (25°C) for 1 minute to prepare a uniform curable granular silicone composition. This composition contained 0.3 mol % of vinyl groups per 100 g of silicone component. Measurement results for the melt viscosity of this composition are shown in Table 1.

[0201] [Example 5] The mixture was 112.5 g of alumina having an average particle size of 0.44 μm (AES-12 manufactured by Sumitomo Chemical), 234.0 g of alumina having an average particle size of 3.0 μm (AL-M73A manufactured by Sumitomo Chemical), 553.1 g of alumina having an average particle size of 37.4 μm (AZ35-125 manufactured by Micron Company, Nippon Steel & Sumikin Materials Co., Ltd.), and had a viscosity of 23 mPa s. The formula: Me2ViSiO(Me2SiO) 29 Si(OMe)3 3.6 g of dimethylpolysiloxane (vinyl group content = 1.30 mass%) represented by the formula was added to a small crusher at once, and stirred at room temperature (150 ° C) for 1 minute to perform a surface treatment on the alumina, and the temperature of the crusher was returned to 25 ° C. Next, Non-hot melt organopolysiloxane resin fine particles (4) (vinyl group content = 0 mass%) 67.1 g, formula: ViMe2SiO(Me2SiO) 800 SiViMe2 28.8 g of dimethylpolysiloxane terminated at both molecular chain ends with dimethylvinylsiloxy groups (vinyl group content = 0.09% by mass), formula: Me3SiO(MeHSiO)7(Me2SiO) 6.5 SiMe3 0.5 g of an organohydrogenpolysiloxane represented by the formula {the amount of silicon-bonded hydrogen atoms in the organohydrogenpolysiloxane is 1.3 moles per mole of vinyl groups in the dimethylpolysiloxane capped at both molecular chain terminals and one terminal with dimethylvinylsiloxy groups}, 1-ethynyl-1-cyclohexanol (in an amount equivalent to 1000 ppm by mass of the composition) was added all at once to a small grinder and stirred at room temperature (25°C) for 1 minute to prepare a uniform curable granular silicone composition. This composition contained 0.3 mol % of vinyl groups per 100 g of silicone component. Measurement results for the melt viscosity of this composition are shown in Table 1.

[0202] [Example 6] The mixture was 112.5 g of alumina having an average particle size of 0.44 μm (AES-12 manufactured by Sumitomo Chemical), 234.0 g of alumina having an average particle size of 3.0 μm (AL-M73A manufactured by Sumitomo Chemical), 553.1 g of alumina having an average particle size of 37.4 μm (AZ35-125 manufactured by Micron Company, Nippon Steel & Sumikin Materials Co., Ltd.), and had a viscosity of 23 mPa s. The formula: Me2ViSiO(Me2SiO) 29 Si(OMe)3 3.6 g of dimethylpolysiloxane (vinyl group content = 1.30 mass%) represented by the formula was added to a small crusher at once, and stirred at room temperature (150 ° C) for 1 minute to perform a surface treatment on the alumina, and the temperature of the crusher was returned to 25 ° C. Next, Non-hot melt organopolysiloxane resin fine particles (4) (vinyl group content = 0 mass%) 66.8 g, 0.5 g of non-hot melt organopolysiloxane resin fine particles (7) (vinyl group content = 1.91% by mass), formula: ViMe2SiO(Me2SiO) 800 SiViMe2 28.8 g of dimethylpolysiloxane terminated at both molecular chain ends with dimethylvinylsiloxy groups (vinyl group content = 0.09% by mass), formula: (HMeSiO 1 / 2 )0.67 (SiO 4 / 2 ) 0.33 0.35g of organohydrogenpolysiloxane resin (content of silicon-bonded hydrogen atoms = 0.95% by mass) {the amount of silicon-bonded hydrogen atoms in the organohydrogenpolysiloxane is 1.0 mole per mole of vinyl groups in the dimethylpolysiloxane capped at both molecular terminals and one terminal with dimethylvinylsiloxy groups, and the organopolysiloxane resin fine particle (7)}, 1-ethynyl-1-cyclohexanol (in an amount equivalent to 1000 ppm by mass of the composition) was added all at once to a small grinder and stirred at room temperature (25°C) for 1 minute to prepare a uniform curable granular silicone composition. This composition contained 0.3 mol % of vinyl groups per 100 g of silicone component. Measurement results for the melt viscosity of this composition are shown in Table 1.

[0203] [Comparative Example 1] Non-hot melt organopolysiloxane resin fine particles (1) (vinyl group content = 0 mass%) 67.0 g, ViMe2SiO(Me2SiO) 800 SiViMe2 33.0 g of dimethylpolysiloxane terminated at both molecular chain ends with dimethylvinylsiloxy groups (vinyl group content = 0.09% by mass), formula: Me3SiO(MeHSiO)7(Me2SiO) 6.5 SiMe3 0.2 g of an organohydrogenpolysiloxane represented by the formula {the amount of silicon-bonded hydrogen atoms in the organohydrogenpolysiloxane resin is 1.4 moles per mole of vinyl groups in the dimethylpolysiloxane terminally blocked with dimethylvinylsiloxy groups}, 82.8 g of alumina having an average particle size of 0.44 μm (AES-12 manufactured by Sumitomo Chemical), 166.1 g of alumina having an average particle size of 3.0 μm (AL-M73A manufactured by Sumitomo Chemical), 364.1 g of alumina having an average particle size of 37.4 μm (AZ35-125 manufactured by Micron Company of Nippon Steel & Sumikin Materials Co., Ltd.), and 1-ethynyl-1-cyclohexanol (an amount equivalent to 1000 ppm by mass relative to the composition) were all charged into a small grinder at once and stirred at room temperature (25° C.) for 1 minute to prepare a uniform curable granular silicone composition. This composition contained 0.1 mol % of vinyl groups per 100 g of silicone component. Measurement results for the melt viscosity and other properties of this composition are shown in Table 1.

[0204] [Comparative Example 2] Non-hot melt organopolysiloxane resin fine particles (1) (vinyl group content = 0 mass%) 62.5 g, 5.0 g of non-hot melt organopolysiloxane resin fine particles (7) (vinyl group content = 3.1 mass%), ViMe2SiO(Me2SiO) 800 SiViMe2 31.3 g of dimethylpolysiloxane terminated at both molecular chain ends with dimethylvinylsiloxy groups (vinyl group content = 0.09% by mass), formula: Me3SiO(MeHSiO)7(Me2SiO) 6.5 SiMe3 1.2 g of an organohydrogenpolysiloxane represented by the formula: {an amount such that the organohydrogenpolysiloxane resin contains 1.2 moles of silicon-bonded hydrogen atoms per mole of vinyl groups in the organopolysiloxane resin fine particles (7) and the dimethylpolysiloxane terminally blocked with dimethylvinylsiloxy groups}, 82.8 g of alumina having an average particle size of 0.44 μm (AES-12 manufactured by Sumitomo Chemical), 166.1 g of alumina having an average particle size of 3.0 μm (AL-M73A manufactured by Sumitomo Chemical), 364.1 g of alumina having an average particle size of 37.4 μm (AZ35-125 manufactured by Micron Company of Nippon Steel & Sumikin Materials Co., Ltd.), and 1-ethynyl-1-cyclohexanol (an amount equivalent to 1000 ppm by mass of the composition) were all charged into a small grinder at once and stirred at room temperature (25° C.) for 1 minute to prepare a uniform curable granular silicone composition. This composition contained 0.7 mol % of vinyl groups per 100 g of silicone component. Measurement results of the melt viscosity and other properties of this composition are shown in Table 1.

[0205] [Comparative Example 3] Non-hot melt organopolysiloxane resin fine particles (1) (vinyl group content = 0 mass%) 60.2 g, 7.0 g of non-hot melt organopolysiloxane resin fine particles (6) (vinyl group content = 1.91% by mass), formula: ViMe2SiO(Me2SiO) 800 SiViMe2 32.8 g of dimethylpolysiloxane terminated at both molecular chain ends with dimethylvinylsiloxy groups (vinyl group content = 0.09% by mass), formula: (HMeSiO 1 / 2 ) 0.67 (SiO 4 / 2 ) 0.33 0.65g of organohydrogenpolysiloxane resin (content of silicon-bonded hydrogen atoms = 0.95% by mass) {an amount such that the amount of silicon-bonded hydrogen atoms in the organohydrogenpolysiloxane is 1.0 mole per mole of vinyl groups in the organopolysiloxane resin fine particle (6) and the dimethylpolysiloxane capped at both molecular chain terminals with dimethylvinylsiloxy groups}, 82.8 g of alumina having an average particle size of 0.44 μm (AES-12 manufactured by Sumitomo Chemical), 166.1 g of alumina having an average particle size of 3.0 μm (AL-M73A manufactured by Sumitomo Chemical), 364.1 g of alumina having an average particle size of 37.4 μm (AZ35-125 manufactured by Micron Company of Nippon Steel & Sumikin Materials Co., Ltd.), and 1-ethynyl-1-cyclohexanol (an amount equivalent to 1000 ppm by mass of the composition) were all charged into a small grinder at once and stirred at room temperature (25° C.) for 1 minute to prepare a uniform curable granular silicone composition. This composition contained 0.6 mol % of vinyl groups per 100 g of silicone component. The results of measuring the melt viscosity and other properties of this composition are shown in Table 1.

[0206] [Comparative Example 4] The mixture was 112.5 g of alumina having an average particle size of 0.44 μm (AES-12 manufactured by Sumitomo Chemical), 234.0 g of alumina having an average particle size of 3.0 μm (AL-M73A manufactured by Sumitomo Chemical), 553.1 g of alumina having an average particle size of 37.4 μm (AZ35-125 manufactured by Micron Company, Nippon Steel & Sumikin Materials Co., Ltd.), and had a viscosity of 23 mPa s. The formula: Me2ViSiO(Me2SiO) 29 Si(OMe)3 3.6 g of dimethylpolysiloxane (vinyl group content = 1.30 mass%) represented by the formula was added to a small crusher at once, and stirred at room temperature (150 ° C) for 1 minute to perform a surface treatment on the alumina, and the temperature of the crusher was returned to 25 ° C. Next, Non-hot melt organopolysiloxane resin fine particles (1) (vinyl group content = 0 mass%) 67.0 g, ViMe2SiO(Me2SiO) 800 SiViMe2 33.0 g of dimethylpolysiloxane terminated at both molecular chain ends with dimethylvinylsiloxy groups (vinyl group content = 0.09% by mass), formula: Me3SiO(MeHSiO)7(Me2SiO) 6.5 SiMe3 0.5 g of an organohydrogenpolysiloxane represented by the formula {the amount of silicon-bonded hydrogen atoms in the organohydrogenpolysiloxane resin is 1.2 moles per mole of vinyl groups in the dimethylpolysiloxane capped at both molecular chain terminals and at one end with dimethylvinylsiloxy groups described below}, 1-ethynyl-1-cyclohexanol (in an amount equivalent to 1000 ppm by mass of the composition) was added all at once to a small grinder and stirred at room temperature (25°C) for 1 minute to prepare a uniform curable granular silicone composition. This composition contained 0.3 mol % of vinyl groups per 100 g of silicone component. Measurement results for the melt viscosity of this composition are shown in Table 1.

[0207] [Comparative Example 5] The mixture was 112.5 g of alumina having an average particle size of 0.44 μm (AES-12 manufactured by Sumitomo Chemical), 234.0 g of alumina having an average particle size of 3.0 μm (AL-M73A manufactured by Sumitomo Chemical), 553.1 g of alumina having an average particle size of 37.4 μm (AZ35-125 manufactured by Micron Company, Nippon Steel & Sumikin Materials Co., Ltd.), and had a viscosity of 23 mPa s. The formula: Me2ViSiO(Me2SiO) 29 Si(OMe)3 3.6 g of dimethylpolysiloxane (vinyl group content = 1.30 mass%) represented by the formula was added to a small crusher at once, and stirred at room temperature (150 ° C) for 1 minute to perform a surface treatment on the alumina, and the temperature of the crusher was returned to 25 ° C. Next, Non-hot melt organopolysiloxane resin fine particles (1) (vinyl group content = 0 mass%) 67.0 g, ViMe2SiO(Me2SiO) 300 SiViMe2 33.0 g of dimethylpolysiloxane terminated at both molecular chain ends with dimethylvinylsiloxy groups (vinyl group content = 0.22% by mass), formula: Me3SiO(MeHSiO)7(Me2SiO) 6.5 SiMe3 0.7 g of an organohydrogenpolysiloxane represented by the formula {the amount of silicon-bonded hydrogen atoms in the organohydrogenpolysiloxane resin is 1.1 moles per mole of vinyl groups in the dimethylpolysiloxane capped at both molecular chain terminals and at one end with a dimethylvinylsiloxy group described below}, 1-ethynyl-1-cyclohexanol (in an amount equivalent to 1000 ppm by mass of the composition) was added all at once to a small grinder and stirred at room temperature (25°C) for 1 minute to prepare a uniform curable granular silicone composition. This composition contained 0.5 mol % of vinyl groups per 100 g of silicone component. Measurement results for the melt viscosity of this composition are shown in Table 1.

[0208] [Table 1]

[0209] [Summary] The curable silicone compositions of Examples 1 to 6 according to the present invention are hot-melt compositions having a relatively low melt viscosity even when a large amount of alumina filler is blended, and the storage modulus of the cured product is not extremely high, and no extreme decrease in tensile elongation is observed. Furthermore, the thermal conductivity of the obtained cured product increases with the alumina content. That is, the curable compositions of Examples 1 to 6 give cured products that exhibit good hot-melt properties and moderate flexibility, despite the incorporation of an extremely large amount of functional inorganic filler.

[0210] On the other hand, all of Comparative Examples 1 to 5 include organopolysiloxane resins whose weight-average molecular weight exceeds the value specified in the present invention, but Comparative Examples 1, 2, 3, and 5 all showed extremely low tensile elongation values. In addition, Comparative Example 4 resulted in extremely poor melting properties. As in Reference Example 5, when the weight-average molecular weight of the organopolysiloxane resin was less than the lower limit of the specification of the present invention, a hot-melt composition could not be obtained.

[0211] <Production Example 1> The granulated curable silicone composition of Example 1 or the like is heated to 80°C and kneaded by heating using a twin-screw extruder, and is fed in the form of a semi-solid softened material onto a peelable film (Biwaliner, manufactured by Takara Line Corporation) at a feed rate of 5 kg / hour, and laminated between two peelable films.The laminate is then stretched between rolls to form a laminate in which a 500 μm thick hot-melt curable silicone sheet is laminated between two peelable films, and the entire laminate is cooled by a cooling roll set at -15°C.The peelable film is separated from the laminate to obtain a flat and homogeneous hot-melt curable silicone sheet.

[0212] <Production Example 2> The granulated curable silicone composition of Example 1 and the like is heated to 80°C, melted and kneaded using a twin-screw extruder, and molded into a roughly sheet-like shape using a T-shaped die (opening size: 800 μm×100 mm, heated to 80°C), while being fed onto a release film (Takaraline Corporation, Biwa Liner) at a feed rate of 5 kg / hour, and the whole is cooled by a cooling roll set to −15°C, and then laminated between two release films. The laminate is then stretched between rolls to form a laminate in which a 500 μm thick hot-melt curable silicone sheet is laminated between two release films. In the laminate, the release film is separated to obtain a flat and homogeneous hot-melt curable silicone sheet.

Claims

1. (A) 100 parts by mass of an organopolysiloxane resin containing the following components (A1) and (A2) in a mass ratio of 0:100 to 75:25, and having a weight average molecular weight (Mw) of 2,000 to 15,000 for components (A1) and (A2) as measured by gel permeation chromatography (GPC) using toluene as a solvent. (A1) A compound having no hot melt properties as a whole molecule, having a curing reactive functional group containing a carbon-carbon double bond in the molecule, and having SiO 4/2 An organopolysiloxane resin containing 40 to 90 mol % or more of siloxane units represented by the formula: (A2) The molecule as a whole does not have hot melt properties, does not have a curing reactive functional group containing a carbon-carbon double bond in the molecule, and has SiO 4/2 An organopolysiloxane resin containing 40 to 90 mol % or more of siloxane units represented by the formula: (B) 10 to 100 parts by mass of a linear organopolysiloxane that is liquid at 25° C. and has a curing reactive functional group containing at least two carbon-carbon double bonds in the molecule, (c2) an organohydrogenpolysiloxane having at least two silicon-bonded hydrogen atoms in the molecule and a hydrosilylation reaction catalyst, in an amount necessary for curing the present composition; (D) Functional filler wherein the content of vinyl (CH2=CH-) group moieties among curable reactive functional groups containing a carbon-carbon double bond is 0.05 to 1.50 mol % per 100 g of silicone component in the composition, and the composition as a whole has hot melt properties.

2. 2. The curable silicone composition according to claim 1, wherein the amount of component (D) is in the range of 10 to 2,000 parts by mass per 100 parts by mass of the combined total of components (A) and (B).

3. 3. The curable silicone composition according to claim 1, wherein components (A1) and (A2) are spherical organopolysiloxane resin fine particles having an average primary particle size of 1 to 20 μm.

4. The component (C) is (c2-1) an organohydrogenpolysiloxane having at least two silicon-bonded hydrogen atoms in the molecule; and (c2-2) a hydrosilylation reaction catalyst; The curable silicone composition according to any one of claims 1 to 3, wherein the content of the organohydrogenpolysiloxane of (c2-1) above is an amount such that the molar ratio of silicon-bonded hydrogen atoms in the organohydrogenpolysiloxane resin to the curable reactive functional groups containing carbon-carbon double bonds in components (A) and (B) is in the range of 0.5 to 20.

5. The curable silicone composition according to any one of claims 1 to 4, wherein component (D) is a functional filler comprising at least one type selected from the group consisting of a reinforcing filler, a white pigment, a thermally conductive filler, an electrically conductive filler, and an organic filler.

6. The curable silicone composition according to any one of claims 1 to 5, which is in the form of granules, pellets, or sheets.

7. 6. A substantially flat curable silicone composition sheet having a thickness of 10 to 1000 μm, which comprises the curable silicone composition according to any one of claims 1 to 5.

8. A film-like adhesive which is a sheet of the curable silicone composition according to claim 7.

9. The curable silicone composition sheet of claim 7, and A release laminate comprising a sheet-like substrate on one or both sides of the curable silicone composition sheet, the sheet having a release surface facing the curable silicone composition sheet.

10. A cured product obtained by curing the curable silicone composition according to any one of claims 1 to 5.

11. Use of the cured product according to claim 10 as a member for a semiconductor device.

12. A semiconductor device comprising the cured product according to claim 10.

13. A method for producing the curable silicone composition according to any one of claims 1 to 5, characterized in that the curable silicone composition is granulated by mixing at a temperature not exceeding 50°C.

14. A method for molding a cured product comprising at least the following steps (I) to (III): (I) a step of heating the curable silicone composition according to any one of claims 1 to 5 to at least 100°C to melt it; (II) a step of injecting the liquid curable silicone composition obtained in step (I) into a mold, or a step of spreading the curable silicone composition obtained in step (I) around the mold by clamping the mold; and (III) A step of curing the curable silicone composition injected in the step (II)

15. A method for producing the curable silicone composition sheet according to claim 7, comprising the steps of: Step 1: A step of mixing the raw material components of the curable silicone composition according to any one of claims 1 to 5 at a temperature of 50°C or higher. Step 2: A step of kneading the mixture obtained in step 1 while heating and melting it. Step 3: Laminating the heat-melted mixture obtained in step 2 between at least one film having a release surface. Step 4: Stretching the laminate obtained in step 3 between rolls to form a curable silicone sheet having a specific thickness.

Citation Information

Patent Citations

  • Conductive hot melt silicone adhesive composition

    JP2002155261A

  • Hot-melt type silicone adhesive

    JP2006274007A

  • Addition-curing type silicone resin composition, and sheet comprising the composition, sheet-like cured product, and die attach material

    JP2013221082A

  • Reactive silicone composition, reactive thermoplastic body, cured product and optical semiconductor device

    JP2014009322A

  • Reactive silicone composition, hot melt material produced therefrom, and curable hot melt composition containing the same

    JP2017512224A