Bridging frustrated Lewis pairs as thermal triggers for Si-H and Si-O-Si reactions.

Bridged frustrated Lewis pairs (B-FLP) act as thermal triggers for silyl hydrides and siloxanes, enabling a one-component, storage-stable system that cures rapidly upon heating, addressing the need for efficient, moisture-free curing in coatings and adhesives.

JP7560487B2Active Publication Date: 2024-10-02DOW SILICONES CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021571819
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-04
Filing Date
2020-06-02
Publication Date
2024-10-02
Estimated Expiration
2040-06-02

AI Technical Summary

Technical Problem

Existing chemical reaction systems for silyl hydrides and siloxanes require a two-part system to maintain storage stability and need a catalyst that can be triggered to cure without water or moisture, lacking a one-component system that remains stable at room temperature but initiates rapid curing upon heating.

Method used

Utilizing bridged frustrated Lewis pairs (B-FLP) as a thermal trigger, which dissociate upon heating to release a Lewis acid catalyst, allowing a storage-stable, one-component system to catalyze the rearrangement reaction between silyl hydrides and siloxanes.

Benefits of technology

The B-FLP system provides unprecedented control over irreversible triggering of rapid curing reactions, forming transparent cured compositions with minimal volatile by-products, suitable for coatings, adhesives, and elastomers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560487000001
    Figure 0007560487000001
  • Figure 0007560487000002
    Figure 0007560487000002
  • Figure 0007560487000003
    Figure 0007560487000003
Patent Text Reader

Abstract

The composition contains a mixture of silyl hydrides, siloxanes, and crosslinkable frustrated Lewis pairs and can be thermally triggered to cure.
Need to check novelty before this filing date? Find Prior Art

Description

[Background technology]

[0001] FIELD OF THEINVENTION The present invention relates to the use of a bridged frustrated Lewis pair as a thermal trigger for the chemical reaction of silyl hydrides with siloxanes. The bridged frustrated Lewis pair dissociates upon heating to release a Lewis acid, which acts as a catalyst for the chemical reaction of silyl hydrides with siloxanes.

[0002] Introduction Frustrated Lewis pairs ("FLPs") are a term used to refer to pairs of Lewis acids and Lewis bases where steric congestion prevents the Lewis acid and Lewis base from complexing and neutralizing each other. When the Lewis acid and Lewis base of an FLP are mixed, they remain independent of each other, rather than mixing and neutralizing each other. In addition, FLPs have been found to indirectly bind to each other in the form of bridged frustrated Lewis pairs ("B-FLPs"), where a bridge molecule binds to both the acid and base of the FLP, forming a complex with the bridge molecule between the Lewis acid and the Lewis base. In some cases, the bridge molecule can be cleaved to generate a blocked Lewis acid and a blocked Lewis base, with a portion of the bridge molecule complexed with each of the Lewis acid and Lewis base, blocking further complexation or reaction. Hydrogen (H2) is an example of a bridge molecule that cleaves in this manner upon forming a B-FLP.

[0003] B-FLP has been used to activate bridge molecules for use in chemical reactions. For example, hydrogen (H2) has been used as a bridge molecule in B-FLP to activate hydrogen for use in hydrogenation reactions (see, for example, JACS 2015, 137, 10018-10032), and carbon dioxide has been used as a bridge molecule in B-FLP to activate carbon dioxide for deoxygenation hydrosilylation (see, for example, JACS 2010, 132, 10660-10661). Other molecules used as bridge molecules in B-FLP for use in activation for chemical reactions include nitrous oxide (N2O), sulfur dioxide (SO2), alkenes, and alkynes. See, for example, Angew. Chem. Int. Ed. 2009, 48, 6643-6646; Angew. Chem. Int. Ed. 2015, 54, 6400-6441 and JACS 2015, 137, 10018-10032. Summary of the Invention [Problem to be solved by the invention]

[0004] It would be surprising and useful to discover additional uses for B-FLP, especially if such uses allow for the control of chemical reactions other than those involving cross-linking molecules.

[0005] The present invention provides a surprising and unexpected use of B-FLP as a thermal trigger for the reaction of silyl hydrides (Si-H) with siloxane bonds (Si-O-Si).

[0006] It has been found that Si-H and Si-O-Si undergo a rearrangement reaction in the presence of a strong Lewis acid, where the silicon from the siloxane bond is bonded to the hydrogen of the silyl hydride, while the silicon of the silyl hydride is bonded to the oxygen of the siloxane bond. Surprisingly, the silyl hydride and siloxane bond involved in the rearrangement reaction may be on the same molecule or on different molecules. This rearrangement reaction tends to be rapid in the presence of a strong Lewis acid. Such a reaction may be useful for a fast-cure system containing Si-H and siloxane bonds without the need for water or moisture. However, it requires a two-part system for storage that keeps the Lewis acid catalyst away from the combination of the silyl hydride and the siloxane bond until such a cure is desired. It would be desirable to be able to provide a storage-stable one-component system utilizing a rearrangement reaction that is storage-stable at 23°C, but can be triggered to cure.

[0007] The present invention is the result of the discovery that B-FLP can be used in these rearrangement reaction systems as a latent thermally triggered Lewis acid catalyst. That is, B-FLP containing a Lewis acid PR reaction catalyst can be mixed with a silyl hydride and a siloxane bond to form a reaction system that is storage stable, but can be triggered to cure when heated. Upon sufficient heating, the Lewis acid dissociates from the B-FLP, allowing the Lewis acid to function as an acid catalyst to initiate the rearrangement reaction of the silyl hydride with the siloxane bond.

[0008] B-FLP was found to be a particularly efficient triggering agent because it is difficult to remix once destroyed. This means that once the Lewis acid is liberated, it continues to catalyze the reaction without being inhibited by the reformation of B-FLP. This is an advantage over Lewis acids directly inhibited with a Lewis base, since the Lewis base remains in solution and can remix with the free Lewis acid to neutralize it. B-FLP requires the reformation of a bridging complex between the Lewis acid and the base, and this reformation is much less likely to occur randomly. This is especially true for labile bridging molecules, such as those that are gaseous and will retreat from the reaction system once B-FLP is destroyed. As a result, the use of B-FLP offers unprecedented control over irreversibly triggering the reaction without forming a catalytic inhibitor, since once heated sufficiently to dissociate the B-FLP, the acid catalyst is irreversibly released to catalyze the rapid rearrangement reaction.

[0009] In a first aspect, the invention is a composition comprising a mixture of a silyl hydride, a siloxane, and a bridged frustrated Lewis pair.

[0010] In a second aspect, the invention is a chemical reaction process comprising the steps of: (a) providing a composition of the first aspect; and (b) heating the composition to a temperature sufficient to dissociate a Lewis acid from a bridged frustrated Lewis pair.

[0011] The present invention is useful for preparing coatings, adhesives, and elastomers. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Test methods refer to the most recent test method as of the priority date of this document unless a date is given with the test method number. Reference to a test method includes both a reference to the testing society and the test method number. The following test method abbreviations and identifiers apply herein: ASTM refers to ASTM International, EN refers to European Norm, DIN refers to Deutsches Institut fuer Normung, and ISO refers to the International Organization for Standardization.

[0013] Products identified by trade names refer to compositions available under those trade names from suppliers as of the priority date of this application.

[0014] "Plurality" means two or more. "And / or" means "and, or alternatively." All ranges are inclusive of endpoints unless otherwise indicated. Products identified by trade names refer to compositions available from suppliers under those trade names as of the priority date of this document, unless otherwise indicated herein.

[0015] The compositions of the present invention comprise a mixture of a siloxane, a silyl hydride, and a bridged frustrated Lewis pair.

[0016] "Siloxane" refers to a molecule that contains at least one siloxane (Si-O-Si) bond. Desirably, the siloxanes of the present invention are "polysiloxanes," which refers to molecules that contain multiple Si-O-Si bonds. Polysiloxanes typically contain siloxane units, referred to as M, D, T, or Q units. The standard M unit has the formula (CH3)3SiO 1 / 2 The standard D unit has the formula (CH3)2SiO 2 / 2 The standard T unit has the formula (CH3)SiO 3 / 2 The standard Q unit has the formula SiO 4 / 2The M, D, and T units can have one or more methyl groups replaced with hydrogen or some other moiety.

[0017] A "silyl hydride" is a molecule that contains a silicon-hydrogen (Si-H) bond and can contain multiple Si-H bonds.

[0018] An "alkyl" is a hydrocarbon group derived from an alkane by removing a hydrogen atom. A "substituted alkyl" is an alkyl having an atom or chemical moiety other than carbon and hydrogen in place of at least one carbon or hydrogen.

[0019] An "aryl" is a group derived from an aromatic hydrocarbon by removing a hydrogen atom. A "substituted aryl" is an aryl that has an atom or chemical moiety other than carbon and hydrogen in place of at least one carbon or hydrogen.

[0020] A "frustrated Lewis pair," or "FLP," is a system of Lewis acids and Lewis bases in which the Lewis acid and Lewis base are unable to complex and completely neutralize ("block") each other due to steric congestion. FLPs are known in the art and have been characterized in papers such as JACS 2015, 137, 10018-10032 and papers identified therein. Desirably, an FLP is a system of Lewis acids and Lewis bases in which congestion makes complexation and neutralization impossible at 20 degrees Celsius (°C). Although FLPs are known in the art, it can be determined whether any Lewis pair is an FLP by combining equimolar amounts of a Lewis acid and a Lewis base at 20°C in a solvent that dissolves both. If more than 10 mole percent of the Lewis acid and Lewis base remain dissociated, then the Lewis acid and Lewis base can be considered an FLP. The extent of dissociation is determined by any reasonable means, such as nuclear magnetic resonance spectroscopy or, preferably, ion chromatography using a conductivity or photometric detector.

[0021] Upon heating the compositions of the present invention, the B-FLP releases a Lewis acid that catalyzes the reaction of the siloxane with the silyl hydride. The composition is heated to a temperature of 80° C. or more, 90° C. or more, 100° C. or more, 110° C. or more, 120° C. or more, 130° C. or more, 140° C. or more, 150° C. or more, 160° C. or more, 170° C. or more, 180° C. or more, 190° C. or more, 200° C. or more, 210° C. or more, while generally reacting and curing the components in the composition at temperatures of 300° C. or less, 250° C. or less, 240° C. or less, 230° C. or less, 220° C. or less, 210° C. or less, 200° C. or less, 175° C. or less, 150° C. or less, 140° C. or less, 130° C. or less, 120° C. or less, 110° C. or less, or even 100° C. or less in less than half the time, preferably one-fifth or less, and more preferably one-tenth or less of the time required for the composition to gel at 23° C.

[0022] The Lewis acid catalyzed reaction of siloxanes with silyl hydrides is a rearrangement reaction that is generally represented by the following reaction: Si'-H + Si-O-Si + Lewis acid → Si'-O-Si + Si-H + Lewis acid

[0023] This rearrangement reaction is useful for forming new siloxane bonds and forming crosslinked polysiloxane systems. A particularly desirable property of this reaction over other Lewis acid catalyzed reactions, such as the Piers-Rubinsztajn (PR) reaction, is that this reaction typically produces no more volatile by-products than the PR reaction. Volatile by-products can produce bubbles when the reaction is used to cure siloxane polymers, resulting in cloudy siloxane polymers. Thus, the reaction is ideal for producing clear cured compositions and films.

[0024] The compositions of the present invention are storage stable. By "storage stable" is meant that the composition does not form a gel at 23° C. in 5 hours or less, preferably 24 hours or less, more preferably 48 hours or less, and even more preferably 1 week or less.

[0025] Siloxane Desirably, the siloxane component is a polysiloxane containing multiple siloxane bonds. The polysiloxane comprises multiple siloxy (SiO) groups. The siloxy-containing groups are typically designated as M, D, T, or Q groups. The polysiloxane may be linear, with M(≡SiO 1 / 2 ) type and D(=SiO 2 / 2 ) type units. Alternatively, the polysiloxane may be branched and contain only T(-SiO 3 / 2 ) type and / or Q(SiO 4 / 2 ) type units. Typically, M, D, T, and Q units have a methyl group bonded to a silicon atom that does not have an oxygen bonded to it, providing a valence of four for each silicon atom, with each oxygen bonded to the silicon of another unit. By referring to these as M, D, T, and Q "type" units, it is meant that a group such as one selected from the group consisting of hydrogen, alkyl, substituted alkyl, aryl, and substituted aryl groups can be bonded to the silicon atom in place of one or more methyls. For example, M H is an M-type unit in which one methyl is replaced by a hydrogen.

[0026] The polysiloxane can have a degree of polymerization (DP) of 10 or more, preferably 20 or more, more preferably 30 or more, and may be 40 or more, 50 or more, 75 or more, 100 or more, 250 or more, 500 or more, 1000 or more, 2,000 or more, 4,000 or more, 6,000 or more, and 8,000 or more, but at the same time is typically 10,00 or less, preferably 8,000 or less, 6,000 or less, 4,000 or less, 2,000 or less, 1,000 or less, 800 or less, 600 or less, 400 or less, 200 or less, or even 100 or less. DP corresponds to the number of siloxy groups present in the molecule and is determined by silicon-29 nuclear magnetic resonance ( 29 This can be determined by Si NMR spectroscopy.

[0027] The siloxane component may contain Si-H bonds, which means that it may also function as a silyl hydride component.In fact, the siloxane component and the silyl hydride component may be the same molecule in the present invention.Alternatively, the siloxane component and the silyl hydride component may be different molecules.In fact, the siloxane molecule may not contain Si-H bonds and / or the silyl hydride component may not contain Si-O-Si bonds.

[0028] An example of a suitable siloxane that does not have Si-H bonds is XIAMETER™ PMX-200 silicone fluid available from Dow Chemical Company.

[0029] Examples of suitable siloxanes containing Si-H bonds include poly(methylhydrosiloxane) and poly(dimethylsiloxane-co-methylhydrosiloxane), trimethylsilyl terminated, both of which are available from Sigma-Aldrich. Further examples of suitable siloxanes containing Si-H bonds include pentamethyldisiloxane, bis(trimethylsiloxy)methyl-silane, tetramethyldisiloxane, tetramethycyclotetrasiloxane, and hydride terminated poly(dimethylsiloxane), such as those available from Gelest under the trade designations DMS-H03, DMS-H25, DMS-H31, and DMS-H41.

[0030] Typically, the concentration of the siloxane in the composition is 70 weight percent (wt%) or more, 75 wt% or more, 80 wt% or more, 85 wt% or more, or even 90 wt% or more, based on the combined weight of the silyl hydride, siloxane, and B-FLP in the composition, while at the same time typically is 90 wt% or less, 85 wt% or less, 80 wt% or less, or even 75 wt% or less.

[0031] Silyl hydride Silyl hydrides contain one, preferably two or more Si-H bonds. The Si-H bonds are typically part of polysilanes (molecules containing multiple Si-H bonds) or polysiloxanes. Silyl hydrides containing multiple Si-H bonds are desirable as crosslinkers in the compositions of the present invention because they can react with multiple siloxane bonds.

[0032] The silyl hydrides of the present invention may be polymeric. The silyl hydrides may be linear, branched, or contain a combination of linear and branched silyl hydrides. The silyl hydrides may be polysilanes, polysiloxanes, or combinations of polysilanes and polysiloxanes.

[0033] Desirably, the silyl hydride is a polysiloxane molecule with one Si-H bond or two or more Si-H bonds. When the silyl hydride is a polysiloxane, the Si-H bond is on the silicon atom of an M-type or D-type siloxane unit. The polysiloxane may be linear and may contain only M-type and D-type units. Alternatively, the polysiloxane may be branched and may contain T-type and / or Q-type units.

[0034] Examples of suitable silyl hydrides include pentamethyldisiloxane, bis(trimethylsiloxy)methyl-silane, tetramethyldisiloxane, tetramethylcyclotetrasiloxane, and hydride-terminated poly(dimethylsiloxane), such as those available from Gelest under the trade names DMS-H03, DMS-H25, DMS-H31, and DMS-H41.

[0035] The concentration of silyl hydride is typically sufficient to provide a molar ratio of Si-H groups to siloxane bonds that is 0.2 or more, 0.5 or more, 0.7 or more, 0.8 or more, 0.9 or more, 1.0 or more, 1.2 or more, 1.4 or more, 1.6 or more, 1.8 or more, 2.0 or more, 2.2 or more, or even 2.5 or more, while at the same time typically is 5.0 or less, 4.5 or less, 4.0 or less, 3.5 or less, 3.0 or less, 2.8 or less, 2.5 or less, 2.3 or less, 2.0 or less, 1.8 or less, 1.6 or less, 1.4 or less, 1.2 or less, or even 1.0 or less.

[0036] Siloxane or silyl hydride (or both) can function as crosslinkers in the reaction. Crosslinkers have at least two reactive groups in one molecule and react with two different molecules through these reactive groups to crosslink them together. Increasing the length of the linear chain between the reactive groups in the crosslinker tends to increase the flexibility of the resulting crosslinked product. In contrast, shortening the length of the linear chain between the reactive groups in the crosslinker tends to reduce the flexibility of the resulting crosslinked product. In general, to obtain a more flexible crosslinked product, a linear crosslinker is desired, and the length between the reactive sites is selected to obtain the desired flexibility. To obtain a less flexible crosslinked product, a shorter linear crosslinker or even a branched crosslinker is desired to reduce the flexibility between the crosslinked molecules.

[0037] The silyl hydride may be the same molecule as the siloxane, i.e., a single molecule containing both siloxane bonds and silyl hydride functional groups can provide roles as both silyl hydride and siloxane. Alternatively, the silyl hydride may be a different molecule than the siloxane. The silyl hydride may not contain siloxane bonds. The siloxane may not contain silyl hydride groups.

[0038] The compositions (and reaction processes) of the present invention may contain two or more silyl hydrides, two or more siloxanes, and / or two or more components that function as both silyl hydrides and siloxanes.

[0039] Typically, the concentration of the silyl hydride in the composition is 5% by weight or more, 10% by weight or more, 15% by weight or more, 20% by weight or more, or even 25% by weight or more, while at the same time, typically is 30% by weight or less, 25% by weight or less, 20% by weight or less, 15% by weight or less, or even 5% by weight or less, based on the combined weight of the silyl hydride, siloxane, and B-FLP in the composition.

[0040] Bridged frustrated Lewis pair A bridged frustrated Lewis pair ("B-FLP") is a complex that includes an FLP, where the Lewis acid and Lewis base of the FLP are both bound to a bridge molecule to form a neutralized complex with the bridge molecule that resides between the Lewis acid and the Lewis base (i.e., "bridged"). As in the case of H2, the bridge molecule can be cleaved with one portion of the bridge molecule blocking the Lewis acid and another portion of the bridge molecule blocking the Lewis base. Alternatively, and preferably, the bridge molecule remains intact, and the B-FLP is a stable complex (at least at 23°C) with the bridge molecule simultaneously bound to the Lewis acid and Lewis base of the FLP.

[0041] The Lewis acid is selected from the group consisting of aluminum alkyls, aluminum aryls, arylboranes including triarylboranes (including substituted aryl and triarylboranes such as fluorinated arylboranes including tris(pentafluorophenyl)borane), boron halides, aluminum halides, gallium alkyls, gallium aryls, gallium halides, silium cations, and phosphonium cations. Examples of suitable aluminum alkyls include trimethylaluminum and triethylaluminum. Examples of suitable aluminum aryls include triphenylaluminum and tris-pentafluorophenylaluminum. Examples of triarylboranes include the following formula: [ka] where R is independently selected at each occurrence from H, F, Cl, and CF3. Examples of suitable boron halides include (CH3CH2)2BCl and boron trifluoride. Examples of suitable aluminum halides include aluminum trichloride. Examples of suitable gallium alkyls include trimethylgallium. Examples of suitable gallium aryls include triphenylgallium. Examples of suitable gallium halides include trichlorogallium. Examples of suitable silium cations include (CH3CH2)3Si + X - and Ph3Si + X - Examples of suitable phosphonium cations include FP(C6F5)3 + X - Examples include:

[0042] Lewis bases are the following bases: PR3, P(NR2)3, NR3, N(SiR3) x R 3-x , RC(NR)N, P(NR)R3, guanidine (C(=NR)(NR2)2), amidine (RC(=NR)NR2), phosphazene, and [ka] , where R is independently selected at each occurrence from the group consisting of hydrogen, alkyl, substituted alkyl, aryl, and substituted aryl. Examples of suitable Lewis bases for structure PR3 include tri(t-butyl)phosphine, tri(cyclohexyl)phosphine, PhP(tBu), (cyclohexyl)P(tBu), nBuP(tBu), Me(tBu), tBuP(i-Pr), P(CH 11)3, P(iBu)3, and P(n-Bu)3. Examples of suitable Lewis bases of the structure RC(NR)N include 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-methyl-1,5,7-triazabicyclo4.4.0dec-5-ene, and 2,3,4,6,7,8,9,10-octahydropyrimidol[1,2-a]azepine (DBU). Examples of suitable guanidines include guanidine, biguanidine, and 1,1-dimethylguanidine. Examples of suitable amidines include diethylamide and diisopropylamide. Examples of suitable phosphazenes include tert-butylimino-tri(pyrrolidino)phosphone, tert-octylimino-tris(dimethylamino)phosphorene, and 2-tert-butylimino-2-diethylamino-1,3-dimethylperhydro-1,3,2-diazaphosphorine. Examples of suitable Lewis bases of the following structure are: [ka] Examples include 1,3-dimesityl-imidazol-4,5-dihydro-2-ylidene, 1,3-bis(2,6-diisopropylphenyl)imidazol-2-ylidene, and 1,3-bis(2,4,6-trimethylphenyl)-4,5-dihydroimidazol-2-ylidene.

[0043] A crosslinking molecule within the broadest scope of the present invention includes any molecule that simultaneously binds and blocks the Lewis acid and Lewis base of the FLP to form a B-FLP. The interaction of the crosslinking molecule with the Lewis acid and Lewis base is such that the Lewis acid and Lewis base are blocked by the crosslinking molecule (or a portion thereof) at 23°C, but at least the Lewis acid is unblocked at a temperature of 120°C or higher, preferably 110°C or higher, more preferably 100°C or higher, even more preferably 90°C or higher, 80°C or higher, or even 70°C or higher, and at the same time, desirably 300°C or lower, 240°C or lower, 220°C or lower, 200°C or lower, 180°C or lower, 160°C or lower, 150°C or lower, 125°C or lower, or even 100°C or lower. Unblocking the Lewis acid of the B-FLP can be demonstrated by the composition of the present invention containing the B-FLP curing in less than half the time required to gel at 23°C.

[0044] Examples of suitable cross-linking molecules include carbon dioxide, hydrogen molecules (H2), nitriles, alkenes, alkynes, ketones, esters, and aldehydes. Desirably, the cross-linking molecules contain 10 or less, preferably 9 or less, and may contain 8 or less, 7 or less, 6 or less, 5 or less, 4 or less, 3 or less, 2 or less, and even 1 or less or 0 carbon atoms, while at the same time, the cross-linking molecules may contain 1 or more, 2 or more, 3 or more, 4 or more, 5 or more, and even 6 or more carbon atoms. As mentioned earlier in this specification, in B-FLP, some cross-linking molecules can be cleaved, with some of the cross-linking molecules blocking Lewis acids and Lewis bases and some of the cross-linking molecules blocking Lewis bases. It is preferred that the cross-linking molecules remain uncleaved while cross-linking the Lewis acids and Lewis bases of the FLP. In that respect, the cross-linking molecules are preferably not H2. More preferably, the cross-linking molecules do not include any molecules that cleave while cross-linking the Lewis acids and Lewis bases of the FLP.

[0045] B-FLP is desirably "stable" in the compositions of the present invention, meaning that it does not dissociate and release a Lewis acid at temperatures below 23° C. B-FLP may be stable at temperatures below 30° C., below 50° C., below 70° C., or even below 80° C. At the same time, B-FLP dissociates at temperatures above 120° C., preferably above 110° C., more preferably above 110° C., above 100° C., above 90° C., and even above 80° C. B-FLP may be stable at temperatures below 120° C., preferably above 110° C., more preferably above 110° C., above 100° C., above 90° C., and even above 80° C. B-FLP may be stable at temperatures below 120° C., preferably above 110° C., more preferably above 110° C., above 100° C., above 90° C., or ... 1 H and 31 P, 11 B and / or 27 Dissociation of B-FLP can be determined by examining evidence of free Lewis acid by ion exchange (I) or by the addition of 1,2-dichlorophenyl ether (I) or ...

[0046] One method for preparing B-FLP is by mixing the Lewis acid and Lewis base of FLP together with the crosslinking molecule in a solvent at 23° C. The mixing promotes the formation of B-FLP. B-FLP may be isolated from the solvent, typically by evaporating the solvent or filtering if B-FLP precipitates from the solvent. B-FLP can be stored for long periods at or below 23° C. B-FLP can be mixed with silyl hydride and siloxane to form the composition of the present invention.

[0047] In contrast to typical blocked Lewis acid systems, the Lewis acid of the B-FLP of the present invention is complexed with a Lewis base via a bridging molecule, thus complexing the two molecules. Prior art suggests direct complexation of a blocking agent that is sensitive to ultraviolet (UV) light with the Lewis acid, such that irradiation with UV light dissociates the blocking agent from the Lewis acid. The B-FLP of the present invention does not require a UV-sensitive blocking agent and may not include any component that liberates the Lewis acid from the B-FLP upon irradiation with UV light. The B-FLP and compositions of the present invention may not include a photoacid generator or any other component that generates a Lewis acid upon exposure to UV radiation.

[0048] The composition of the present invention offers the advantage of a one-component reactive system that is storage stable even when exposed to UV light. Unlike the prior art, the composition does not need to be reacted with UV light, and the composition does not need to be blocked from exposure to UV light to maintain storage stability. Desirably, the stability of the B-FLP of the present invention is not dependent on (i.e., independent of) exposure to UV light.

[0049] The compositions of the present invention typically contain sufficient B-FLP to provide a Lewis acid concentration that is 0.1 parts per million (ppm) or more, 1 ppm or more, 10 ppm or more, 50 ppm or more, 100 ppm or more, 200 ppm or more, 300 ppm or more, 400 ppm or more, 500 ppm or more, 600 ppm or more, 700 ppm or more, 800 ppm or more, 900 ppm or more, 1000 ppm or more, but at the same time, typically 10,000 ppm or less, 5,000 ppm or less, 1,000 ppm or less, based on the combined weight of silyl hydride and siloxane in the composition.

[0050] The compositions of the present invention may be free of water, or may comprise water, preferably at a concentration of 1 weight percent (wt%) or less, 0.75 wt% or less, 0.5 wt% or less, 0.25 wt% or less, 0.1 wt% or less, 0.05 wt% or less, or even 0.01 wt% or less, based on the weight of the composition.

[0051] Optional Ingredients The composition of the present invention may consist of silyl hydride, siloxane, and B-FLP. Alternatively, the composition of the present invention may further comprise one optional ingredient or a combination of two or more optional ingredients. The optional ingredients are desirably present at a concentration of 50% by weight or less, 40% by weight or less, 30% by weight or less, 20% by weight or less, 10% by weight or less, 5% by weight or less, or even 1% by weight or less based on the weight of the composition.

[0052] Examples of possible optional components include one or a combination of two or more components selected from the group consisting of hydrocarbyl solvents (typically at a concentration of 10% by weight or less, 5% by weight or less, or even 1% by weight or less based on the weight of the composition), pigments such as carbon black or titanium dioxide, fillers such as metal oxides including SiO2 (typically at a concentration of 50% by weight or less based on the weight of the composition), moisture scavengers, optical brighteners, stabilizers (such as antioxidants and UV stabilizers), and corrosion inhibitors. The composition of the present invention may also be free of one or a combination of two or more of such additional components.

[0053] In particular, the composition of the invention may contain up to 1% by weight of water, up to 0.5% by weight of water, relative to the weight of the composition. Desirably, the composition is free of water.

[0054] Chemical Reaction Process The present invention includes a chemical reaction process comprising the steps of (a) providing a composition of the present invention, and (b) heating the composition to a temperature sufficient to dissociate the Lewis acid from the B-FLP. Upon heating the composition of the present invention, the Lewis acid is released from the B-FLP and catalyzes the reaction of the silyl hydride with the siloxane, as described above. The composition of the present invention can be provided in step (a) by mixing together the B-FLP, the silyl hydride, and the siloxane. As described above, the silyl hydride and the siloxane can be the same molecule.

[0055] The chemical reaction process can be carried out in the absence of water or with a concentration of water that is 1 weight percent (wt%) or less, 0.75 wt% or less, 0.5 wt% or less, 0.25 wt% or less, 0.1 wt% or less, 0.05 wt% or less, or even 0.01 wt% or less, based on the weight of the composition provided in step (a).

[0056] The composition has use, for example, as a coating that undergoes a thermally triggered curing reaction, or as a reactive composition for molding applications where the fluid is placed in a mold and heated to trigger curing to form a molded article. In such applications, the process of the present invention further comprises, after step (a) and before step (b), the composition is applied to a substrate or placed in a mold. EXAMPLES

[0057] Preparation of B-FLP(1) In a glovebox, a Schlenk flask equipped with a magnetic stir bar is charged with tri(t-butyl)phosphine (200 milligrams (mg), 1.0 millimole (mmol), 1 equivalent (equiv)) and tris-pentafluorophenylborane (500 mg, 1 mmol, 1 equiv) and the components are dissolved in 10 milliliters (mL) of toluene. The Schlenk flask is sealed and removed from the glovebox. The Schlenk flask is connected to a Schlenk line. The contents of the Schlenk flask are stirred throughout the next step. The Schlenk line is purged with nitrogen and then carbon dioxide is bubbled into the line for 2 minutes. The Schlenk flask is exposed to a carbon dioxide atmosphere and then the cap of the flask is replaced with a septum. A needle is inserted through the septum to create an outlet for carbon dioxide gas and improve the carbon dioxide circulation. After 5 minutes, a white solid precipitates from the reaction mixture. The flask is sealed and stirred at room temperature for an additional hour. The flask is moved to the glovebox. Add 20 mL of hexane and isolate the white solid by filtration through a glass frit. Wash the white solid three times with hexane (10 mL each time). The white solid is B-FLP(1) (540 mg, 71% yield). B-FLP(1) can be stored without decomposition even when exposed to UV light. 1 H, 31 P, and 11 The solid is characterized by B nuclear magnetic resonance spectroscopy (NMR) to confirm the absence of impurities and starting materials. The predicted reaction and structure of B-FLP (1) is as follows: [ka]

[0058] Comparative Example (Comp Ex) A: No Lewis Acid Maximum 10g dental cup with 5.0g M H D H 8D 20 M H (available from Gelest as HMS-271) is added. The material is spun in a FlackTek SpeedMixer at 3500 revolutions per minute (rpm) for 1 minute. The resulting material is poured into an aluminum pan and heated to 100°C on a hot plate. After 2 minutes no air bubbles are evident, indicating no reaction. After leaving the material at 23°C for 2 weeks, no cure is still evident. Comparative Example A was spun at either 23°C or 100°C for 10 minutes. H D H 8D 20 M H This shows the need for a curing catalyst to cure the

[0059] Comparative example B: Comparative example A+BCF M H D 376 M H Comparative Example A is repeated, except that 0.0253 g of tris(pentafluorophenyl)borane ("BCF") is included per million parts by weight of M. Even without heating to 100° C., air bubbles are clearly visible when the mixture is poured into an aluminum pan after swirling. The mixture is left unheated at 23° C. and hardens to a hard material within 2 hours at 23° C. Comparative Example B shows that M can be cured in the presence of a Lewis acid catalyst even at 23° C. H D 376 M H This indicates that the material hardens rapidly.

[0060] Example (Ex) 1: Comparative Example A+B-FLP(1) Comparative Example B is repeated, except that 0.253 g of B-FLP(1) is used instead of 0.0253 g of BCF. After the mixture was left at 23° C. for 14 days, it still did not cure or show any signs of reaction. During the test, the composition is exposed to ambient (including ultraviolet) light. The mixture was heated to 100° C. on a hot place, and within 2 minutes bubbles began to form, indicating that reaction was occurring. After 5 minutes on the hot plate, the mixture was removed and left at 23° C. The mixture cured hard within 24 hours.

[0061] Example 2: Mixed Reactants For dental cups up to 10g, 0.243g of B-FLP(1), 2.5g of M H D H 8D 20 M H (commercially available as HMS-271 from Gelest) and 2.5 g of MD 80 M (commercially available from Dow Chemical Company as XIAMETER™ 100 centistoke (cSt) PMX-200 fluid) is added and mixed. The ingredients are spun together in a FlackTek SpeedMixer at 3500 rpm for 1 minute to form a mixture. The mixture is poured into an aluminum pan and allowed to stand at 23° C. After 14 days, there are no signs of reaction or hardening. During testing, the composition is exposed to ambient (including ultraviolet) light. The mixture in the aluminum pan is heated to 100° C. After 2 minutes, air bubbles are clearly visible, indicating that reaction is occurring. After heating for 5 minutes, the mixture and aluminum pan are removed from the hot plate and allowed to stand at 23° C. The mixture hardens within 48 hours.

[0062] Example 3: Mixed Reactions For dental cups up to 10g, 0.243g of B-FLP(1), 2.5g of M H D H 8D 20 M H (commercially available as HMS-271 from Gelest) and 2.5 g of MD 185M (commercially available as XIAMETER™ 350 cSt PMX-200 fluid from Dow Chemical Company) is added and mixed. The ingredients are spun together in a FlackTek SpeedMixer at 3500 rpm for 1 minute to form a mixture. The mixture is poured into an aluminum pan and allowed to stand at 23° C. After 14 days, there are no signs of reaction or hardening. During testing, the composition is exposed to ambient (including ultraviolet) light. The mixture in the aluminum pan is heated to 100° C. After 2 minutes, air bubbles are clearly visible, indicating that reaction is occurring. After heating for 5 minutes, the mixture and aluminum pan are removed from the hot plate and allowed to stand at 23° C. The mixture hardens within 36 hours.

[0063] Examples 1-3 show that B-FLP can provide a latent catalyst to a reaction system to provide a reaction system that is storage stable at 23° C., but upon heating, the Lewis acid catalyst is released and continues to react even when the mixture is cooled back to 23° C., indicating that B-FLP provides a blocked catalyst that is irreversibly unblocked upon heating.

Claims

1. 1. A composition comprising a mixture of a silyl hydride, a siloxane, and a bridged frustrated Lewis pair, comprising: The bridged frustrated Lewis pair is (a) a Lewis acid which is a fluorinated arylborane; (b) a Lewis base selected from the group consisting of PR 3 , NR 3 , guanidine, amidine, and phosphazene, where R is independently selected at each occurrence from the group consisting of hydrogen, alkyl, substituted alkyl, aryl, and substituted aryl; (c) a bridging molecule that binds said Lewis acid and Lewis base, said bridging molecule being selected from the group consisting of carbon dioxide, a nitrile, an alkene, and an alkyne.

2. The Lewis acid is a fluorinated arylborane and the Lewis base is PR 3 and N.R. 3 2. The composition of claim 1, wherein R is independently selected at each occurrence from the group consisting of hydrogen, alkyl, substituted alkyl, aryl, and substituted aryl, and the bridging molecule is selected from the group consisting of carbon dioxide, an alkene, an alkyne, and a nitrile.

3. The composition of claim 1 or 2, wherein the silyl hydride and the siloxane are the same molecule.

4. 4. The composition of claim 1, wherein the crosslinked frustrated Lewis pair does not include a photoacid generator or other component that generates a Lewis acid upon exposure to ultraviolet radiation.

5. (a) providing a composition according to any one of claims 1 to 4; (b) heating the composition to a temperature sufficient to dissociate the Lewis acid from the bridged frustrated Lewis pair; A chemical reaction process comprising:

6. 6. The process of claim 5, wherein step (a) comprises mixing together a bridged frustrated Lewis pair, a silyl hydride, and a siloxane.

7. 7. The process of claim 5 or 6, wherein after step (a) and before step (b), the composition is applied to a substrate or placed in a mold.

Citation Information

Patent Citations

  • Use of boron derivatives as heat-activated catalysts for the polymerization and / or crosslinking of silicones by dehydrogenative condensation

    JP2003531925A

  • Disproportionation of hydridosiloxanes and induction crosslinked polysiloxane networks

    JP2008537753A

  • Curable polysiloxane composition and polysiloxane cured material using the same, optical member and component for aerospace and aircraft industry including the cured material, semiconductor light emitter with the optical member, and illminating device and image display device provided with the emitter

    JP2009256670A

  • Method for dissociating organoborane-amine complexes

    JP2012530601A