Ceria-zirconia composite oxide and method for producing ceria-zirconia composite oxide

The ceria-zirconia composite oxide addresses thickness limitations and bulkiness issues by achieving high density, specific surface area, and OSC, enhancing catalyst performance and reducing pressure loss.

JP7560688B1Active Publication Date: 2024-10-02DAIICHI KIGENSO KAGAKU KOGYO CO LTD

Patent Information

Application Number
JP2024051620
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-03-27
Publication Date
2024-10-02
Estimated Expiration
2044-03-27

AI Technical Summary

Technical Problem

Existing composite oxides used as exhaust gas purification catalysts face limitations in thickness due to increased pressure loss with thicker layers, and achieving high specific surface area leads to bulkiness, restricting coating amount, while also needing high oxygen storage and release capacity (OSC).

Method used

A ceria-zirconia composite oxide with specific ceria and zirconia content ranges and a production method involving neutralization, oxidizing agent addition, high-pressure solid-liquid separation, and controlled moisture and heat treatment to achieve high density, specific surface area, and OSC.

Benefits of technology

The ceria-zirconia composite oxide achieves high density, specific surface area, and OSC, suitable for catalyst carriers with improved performance and reduced pressure loss.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560688000001_ABST
    Figure 0007560688000001_ABST
Patent Text Reader

Abstract

The present invention provides a ceria-zirconia composite oxide having high density, a large specific surface area, and a high OSC. [Solution] A ceria-zirconia composite oxide containing ceria and zirconia, the ceria content being 25% by mass or more and 75% by mass or less based on the entire ceria-zirconia composite oxide, the zirconia content being 25% by mass or more and 75% by mass or less based on the entire ceria-zirconia composite oxide, and the total content of ceria and zirconia being 75% by mass or more based on the entire ceria-zirconia composite oxide, and satisfying the following (1) to (3): (1) an oxygen storage / release capacity at 600°C measured by an O2 pulse method being 290 μmol / g or more and 1000 μmol / g or less; (2) a specific surface area of ​​15 m 2 / g or more 80m 2 / g or less. (3) Tap density is 1.75 g / mL or more and 3.00 g / mL or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a ceria-zirconia composite oxide and a method for producing the ceria-zirconia composite oxide. [Background technology]

[0002] In recent years, exhaust gas regulations have become increasingly stringent, particularly with regard to nitrogen oxides (NOx), increasing the need for exhaust gas purification catalysts with excellent purification performance.

[0003] 2. Description of the Related Art Conventionally, composite oxides containing cerium and zirconium elements have been known for use as supports for exhaust gas purification catalysts (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2021 / 049525 Summary of the Invention [Problem to be solved by the invention]

[0005] When composite oxide powder is used as an exhaust gas purification catalyst, the composite oxide is used as a carrier for catalytic metal elements such as Pt, Pd, and Rh. The powder carrying the catalytic metal elements is applied to a honeycomb, so as the thickness of the applied layer increases, the pressure loss also increases. For this reason, there is a limit to the thickness that the powder can be applied, and it is important to form a high-density coating layer per unit surface area of ​​the honeycomb in order to improve purification performance. On the other hand, in general, it is important for the composite oxide used as the support for the catalytic metal element to be a porous material having a high specific surface area in order to improve the purification performance. However, in order to obtain a high specific surface area, the material becomes bulky, and the amount of the material applied to the substrate is limited. In addition, it is desirable for the material to have a high oxygen storage and release capacity (hereinafter, also referred to as "OSC").

[0006] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a ceria-zirconia-based composite oxide having a high density, a large specific surface area, and a high OSC, and to provide a method for producing the ceria-zirconia-based composite oxide by which the ceria-zirconia-based composite oxide can be obtained. [Means for solving the problem]

[0007] The present inventors have conducted extensive research into the above-mentioned problems, and as a result have succeeded in producing a ceria-zirconia composite oxide having high density, a large specific surface area, and a high OSC, thereby completing the present invention.

[0008] That is, the present invention provides the following. [1] Contains ceria and zirconia, The content of the ceria is 25% by mass or more and 75% by mass or less based on the entire ceria-zirconia-based composite oxide, The content of the zirconia is 25% by mass or more and 75% by mass or less based on the entire ceria-zirconia-based composite oxide, a total content of the ceria and the zirconia is 75 mass% or more based on the entire ceria-zirconia-based composite oxide; A ceria-zirconia composite oxide characterized by satisfying the following (1) to (3): (1) Oxygen storage and release capacity at 600°C measured by the O2 pulse method is 290 μmol / g or more and 1000 μmol / g or less. (2) Specific surface area is 15m 2 / g or more 80m 2 / g or less. (3) Tap density is 1.75 g / mL or more and 3.00 g / mL or less.

[0009] According to the above-mentioned configuration, since ceria and zirconia are contained within the above-mentioned numerical range, a high OSC can be realized. Furthermore, since the above-mentioned (1) to (3) are satisfied, it can be said that the density is high, the specific surface area is large, and the OSC is high. Such a ceria-zirconia-based composite oxide is useful as a support for an exhaust gas purification catalyst.

[0010] Furthermore, the present invention provides the following: [2] The specific surface area is 30 m 2 / g or more 80m 2 / g or less of the ceria-zirconia composite oxide according to [1] above.

[0011] The specific surface area is 30m 2 / g or more, it can be said that the specific surface area is higher.

[0012] Furthermore, the present invention provides the following: [3] The specific surface area is 40 m 2 / g or more 80m 2 / g or less according to the ceria-zirconia composite oxide described in [1] or [2] above.

[0013] The specific surface area is 40m 2 / g or more, it can be said that the specific surface area is even higher.

[0014] Furthermore, the present invention provides the following: [4] The ceria-zirconia composite oxide according to any one of [1] to [3] above, wherein the tap density is 1.8 g / mL or more and 2.8 g / mL or less.

[0015] When the tap density is 1.8 g / mL or more, it can be said that the density is high.

[0016] Furthermore, the present invention provides the following: [5] The ceria-zirconia composite oxide according to any one of [1] to [4], wherein the tap density is 1.85 g / mL or more and 2.6 g / mL or less.

[0017] When the tap density is 1.85 g / mL or more, it can be said that the density is even higher.

[0018] Furthermore, the present invention provides the following: [6] The ceria-zirconia-based composite oxide according to any one of [1] to [5], wherein the ceria content is 35 mass % or more and 70 mass % or less based on the entire ceria-zirconia-based composite oxide.

[0019] When the ceria content is 35 mass % or more, a high OSC is more easily achieved.

[0020] Furthermore, the present invention provides the following: [7] The ceria-zirconia-based composite oxide according to any one of [1] to [6] above, which contains one or more oxides of rare earth elements other than Ce and Pm.

[0021] If one or more oxides of rare earth elements other than Ce and Pm are included, the specific surface area can be increased. More specifically, when comparing samples with the same (similar) ZrO2:CeO2 ratio and firing conditions, the sample containing oxides of rare earth elements other than Ce and Pm tends to have a higher specific surface area. For example, the specific surface areas of Examples 2, 5 to 9, in which rare earth elements are added to Example 31, which has a composition of ZrO2:CeO2=42:58 and a firing temperature of 700°C, are higher than that of Example 31 (see Tables 1 and 2 described later). Similarly, the specific surface area of ​​Example 3, in which rare earth elements are added to Example 29, which has a composition of ZrO2:CeO2=70:30 and a firing temperature of 700°C, is higher than that of Example 29. Moreover, the specific surface area of ​​Example 1, in which rare earth elements were added to Example 30 having a composition of ZrO2:CeO2=30:70 and a firing temperature of 700° C., is higher than that of Example 30.

[0022] Furthermore, the present invention provides the following: [8] Particle size D 90The ceria-zirconia composite oxide according to any one of the above [1] to [7], wherein the average particle size is 8 μm or more and 80 μm or less.

[0023] Particle size D 90 If the particle size D is 80 μm or less, the particle is relatively small. 90 When the thickness is 80 μm or less, a denser coating layer of ceria-zirconia based composite oxide can be formed on the honeycomb.

[0024] Furthermore, the present invention provides the following: [9] A step 1 of neutralizing an aqueous solution of a raw material salt containing cerium and zirconium with a base to obtain a precursor of a ceria-zirconia composite oxide; Step 2 of adding an oxidizing agent to the obtained precursor; A step 3 of subjecting the suspension obtained in the step 2 to solid-liquid separation and applying a pressure of 1.5 MPa or more; A step 4 of mixing water with the solid obtained in the step 3 so that the water content is 90% by mass or more; Step 5 of heat-treating the mixture obtained in step 4; The method for producing a ceria-zirconia composite oxide according to any one of the above [1] to [8], comprising:

[0025] According to the above-mentioned configuration, an aqueous solution of raw material salts containing cerium and zirconium is neutralized with a base to obtain a precursor of a ceria-zirconia composite oxide, and then an oxidizing agent is added to the obtained precursor (step 2). The addition of the oxidizing agent makes it possible to convert cerium into a tetravalent ion. When cerium is converted into a tetravalent ion, the ionic radius becomes smaller. By reducing the ionic radius of cerium, solid solution diffusion during firing becomes more likely to occur. As a result, a high OSC is obtained. In other words, a solid solution in which cerium and zirconium are uniform at the atomic level can be obtained, and therefore a high OSC is obtained. In addition, the suspension obtained in step 2 is subjected to solid-liquid separation and pressurized at 1.5 MPa or more (step 3), so that the pores in the particles are crushed and most of the large pores disappear in step 3. This results in a dense aggregate state. Thereafter, water is mixed with the solid obtained in step 3 so that the water content is 90 mass % or more (step 4), and the resulting mixture is heat-treated (step 5). As a result, fine pores are formed during drying by heat treatment. Since no large pores are present as described above, the resulting ceria-zirconia composite oxide has no large pores and only fine pores. The ceria-zirconia composite oxide obtained by the above manufacturing process has a high specific surface area due to the formation of fine pores, has a high density due to the almost complete absence of large pores, and has a high OSC due to the cerium and zirconium being uniform at the atomic level. Effect of the Invention

[0026] According to the present invention, it is possible to provide a ceria-zirconia-based composite oxide having a high density, a large specific surface area, and a high OSC, and a method for producing the ceria-zirconia-based composite oxide capable of obtaining the ceria-zirconia-based composite oxide. [Brief description of the drawings]

[0027] [Figure 1] 1 is an X-ray diffraction spectrum of the ceria-zirconia based composite oxide of Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] Hereinafter, embodiments of the present invention will be described. However, the present invention is not limited to these embodiments. In this specification, the ceria-zirconia composite oxide is a general one that contains impurity metal compounds of 10 mass% or less in terms of oxide including hafnium. In addition, in this specification, the expressions "contain" and "include" include the concepts of "contain", "include", "substantially consists of", and "consist only of".

[0029] The maximum and minimum values ​​of the content of each component shown below are independently the preferred minimum and maximum values ​​of the present invention, regardless of the contents of other components. Furthermore, the maximum and minimum values ​​of various parameters (measured values, etc.) shown below are independently preferred minimum and maximum values ​​of the present invention, regardless of the content (composition) of each component.

[0030] [Ceria-zirconia composite oxide] The ceria-zirconia composite oxide according to this embodiment is Contains ceria and zirconia, The content of the ceria is 25% by mass or more and 75% by mass or less based on the entire ceria-zirconia-based composite oxide, The content of the zirconia is 25% by mass or more and 75% by mass or less based on the entire ceria-zirconia-based composite oxide, a total content of the ceria and the zirconia is 75 mass% or more based on the entire ceria-zirconia-based composite oxide; The following requirements (1) to (3) are met. (1) Oxygen storage and release capacity at 600°C measured by the O2 pulse method is 290 μmol / g or more and 1000 μmol / g or less. (2) Specific surface area is 15m 2 / g or more 80m 2 / g or less. (3) Tap density is 1.75 g / mL or more and 3.00 g / mL or less.

[0031] As described above, the ceria-zirconia composite oxide according to the present embodiment contains ceria and zirconia. The ceria-zirconia composite oxide may be composed only of ceria and zirconia, or may contain other components as long as the effects of the present invention are achieved (as long as the effects of the present invention are not significantly impaired).

[0032] The content of the ceria is from 25% by mass to 75% by mass based on the entire ceria-zirconia based composite oxide (when the entire ceria-zirconia based composite oxide is taken as 100% by mass). Since the ceria content is 25 mass % or more, a high OSC can be obtained.

[0033] The content of the ceria is preferably 35 mass % or more, and more preferably 40 mass % or more, based on the entire ceria-zirconia based composite oxide. The content of the ceria is preferably 70 mass % or less, and more preferably 60 mass % or less, based on the entire ceria-zirconia based composite oxide. The content of the ceria is preferably from 35% by mass to 70% by mass, and more preferably from 40% by mass to 60% by mass, based on the entire ceria-zirconia-based composite oxide.

[0034] The content of the zirconia is 25% by mass or more and 75% by mass or less based on the entire ceria-zirconia-based composite oxide. Since the zirconia content is 25% by mass or more and 75% by mass or less, a high OSC can be obtained.

[0035] The content of the zirconia is preferably 27 mass % or more, and more preferably 35 mass % or more, based on the entire ceria-zirconia based composite oxide. The content of the zirconia is preferably 71 mass % or less, and more preferably 65 mass % or less, based on the entire ceria-zirconia-based composite oxide. The content of the zirconia is preferably from 27 mass % to 71 mass % and more preferably from 35 mass % to 65 mass % based on the entire ceria-zirconia based composite oxide.

[0036] The total content of the ceria and the zirconia is 75 mass % or more based on the entire ceria-zirconia based composite oxide. Since the total content of the ceria and the zirconia is 75 mass % or more, a high OSC can be obtained.

[0037] The total content of the ceria and the zirconia is preferably 80 mass % or more, more preferably 85 mass % or more, further preferably 90 mass % or more, and particularly preferably 95 mass % or more, based on the entire ceria-zirconia-based composite oxide. The total content of the ceria and the zirconia may be 100 mass %, 99 mass % or less, or 98.5 mass % or less, based on the entire ceria-zirconia-based composite oxide. The total content of the ceria and the zirconia is preferably 80 mass% or more and 100 mass% or less, more preferably 80 mass% or more and 99 mass% or less, still more preferably 85 mass% or more and 99 mass% or less, and particularly preferably 85 mass% or more and 98.5 mass% or less, based on the entire ceria-zirconia-based composite oxide.

[0038] The ceria-zirconia based composite oxide may contain one or more oxides of rare earth elements other than Ce and Pm. When one or more oxides of rare earth elements other than Ce and Pm are contained, the specific surface area can be increased.

[0039] The ceria-zirconia composite oxide preferably contains oxides of La, Nd, Pr, Y, and Sc among oxides of rare earth elements other than Ce and Pm. When the ceria-zirconia composite oxide contains oxides of La, Nd, Pr, Y, and Sc, sintering of crystallites can be suppressed in the calcination step, and the ceria-zirconia composite oxide is particularly excellent in terms of specific surface area.

[0040] When an oxide of a rare earth element other than Ce and Pm is contained, the content of the oxide of the rare earth element other than Ce and Pm is preferably 0.5 mass % or more and 25 mass % or less based on the entire ceria-zirconia based composite oxide. When the content of the oxide of a rare earth element other than Ce and Pm is 0.5 mass % or more, the effect of improving the specific surface area due to the addition is easily observed.

[0041] When an oxide of a rare earth element other than Ce and Pm is contained, the content of the oxide of the rare earth element other than Ce and Pm is more preferably 1 mass % or more, and further preferably 1.5 mass % or more, based on the entire ceria-zirconia based composite oxide. When an oxide of a rare earth element other than Ce and Pm is contained, the content of the oxide of the rare earth element other than Ce and Pm is more preferably 20 mass % or less, further preferably 15 mass % or less, particularly preferably 10 mass % or less, and particularly preferably 5 mass % or less, based on the entire ceria-zirconia-based composite oxide. When an oxide of a rare earth element other than Ce and Pm is contained, the content of the oxide of the rare earth element other than Ce and Pm is more preferably 1 mass % or more and 20 mass % or less, and further preferably 1.5 mass % or more and 15 mass % or less, based on the entire ceria-zirconia-based composite oxide.

[0042] The ceria-zirconia composite oxide may contain one or more oxides selected from the group consisting of (A) an oxide of at least one element selected from the group consisting of In, Si, Sn, Bi, P, and Zn, (B) a transition metal oxide (excluding oxides of rare earth elements and oxides of precious metal elements), and (C) an alkaline earth metal oxide. These components (A) to (C) are hereinafter also referred to as "other oxides".

[0043] The transition metal oxide may be one or more oxides selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Nb, Mo, Ta and W.

[0044] The alkaline earth metal oxide may be one or more oxides selected from the group consisting of Mg, Ca, Sr and Ba.

[0045] When the ceria-zirconia-based composite oxide contains the other oxides, the content of the other oxides is preferably 0.5% by mass or more and 25% by mass or less based on the entire ceria-zirconia-based composite oxide.

[0046] The content of the other oxides is more preferably 1 mass % or more, and further preferably 1.5 mass % or more, based on the entire ceria-zirconia based composite oxide. The content of the other oxides is more preferably 15 mass % or less, further preferably 10 mass % or less, and particularly preferably 5 mass % or less, based on the entire ceria-zirconia based composite oxide. The content of the other oxides is more preferably from 1 mass % to 15 mass %, and further preferably from 1.5 mass % to 10 mass %, based on the entire ceria-zirconia based composite oxide.

[0047] The ceria-zirconia based composite oxide may contain alumina, but may not contain alumina.

[0048] The ceria-zirconia-based composite oxide has an oxygen storage / release capacity of 290 μmol / g or more and 1000 μmol / g or less at 600° C. as measured by an O 2 pulse method. The oxygen storage / release capacity at 600°C measured by the O2 pulse method is 290 μmol / g or more, which means that the oxygen storage / release capacity (OSC) is high.

[0049] The oxygen storage and release capacity is preferably 310 μmol / g or more, and more preferably 340 μmol / g or more. The higher the oxygen storage / release capacity, the more preferable, and it is, for example, 700 μmol / g or less, 500 μmol / g or less. The oxygen storage / release capacity is preferably 310 μmol / g or more and 700 μmol / g or less, and more preferably 340 μmol / g or more and 500 μmol / g or less.

[0050] The ceria-zirconia composite oxide has a specific surface area of ​​15 m 2 / g or more 80m 2 / g or less. Specific surface area is 15m 2 / g or more, it can be said that the specific surface area is high.

[0051] The specific surface area is preferably 20 m 2 / g or more, more preferably 25m 2 / g or more, more preferably 30m 2 / g or more, most preferably 40m 2 / g or more. The larger the specific surface area, the more preferable. For example, 2 / g or less, 70m 2 / g or less. The specific surface area is preferably 20 m 2 / g or more 75m 2 / g or less, more preferably 25m 2 / g or more 70m 2 / g or less, more preferably 30m 2 / g or more 70m 2 / g or less, most preferably 40m 2 / g or more 70m 2 / g or less.

[0052] The ceria-zirconia-based composite oxide has a tap density of 1.75 g / mL or more and 3.00 g / mL or less. Since the tap density is 1.75 g / mL or more, the density can be said to be high.

[0053] The tap density is preferably 1.8 g / mL or more, and more preferably 1.85 g / mL or more. The higher the tap density, the more preferable it is, and for example, 2.8 g / mL or less, 2.6 g / mL or less. The tap density is preferably 1.8 g / mL or more and 2.8 g / mL or less, and more preferably 1.85 g / mL or more and 2.6 g / mL or less.

[0054] The ceria-zirconia composite oxide preferably has a pore volume (total pore volume of pores with a pore diameter of 20 nm or more and 500 nm or less) of 0.1 cm 3 / g or less, more preferably 0.07 cm 3 / g or less. The ceria-zirconia composite oxide has a pore volume of 0.1 cm 3 / g or less, it can be said that there are few large pores. 3 / g or less, there are few large pores, but the specific surface area is 15m 2 / g or more, there are many small pores.

[0055] The pore volume is not particularly limited, but is preferably 0.01 cm 3 / g or more, more preferably 0.02 cm 3 / g or more. The pore volume is preferably less than 0.01 cm 3 / g or more 0.1cm 3 / g or less, more preferably 0.02 cm 3 / g or more 0.07cm 3 / g or less.

[0056] The ceria-zirconia composite oxide has a particle diameter D 90 It is preferable that the particle diameter D is 8 μm or more and 80 μm or less. 90 If the particle size D is 80 μm or less, the particle is relatively small. 90 When the thickness is 80 μm or less, a denser coating layer of ceria-zirconia based composite oxide can be formed on the honeycomb.

[0057] The particle diameter D 90 is more preferably 70 μm or less, and further preferably 60 μm or less. The particle diameter D 90 is not particularly limited, but is, for example, 9 μm or more, 15 μm or more, etc. The particle diameter D 90 is more preferably 9 μm or more and 70 μm or less, and further preferably 15 μm or more and 60 μm or less.

[0058] The crystal phase of the ceria-zirconia-based composite oxide is not particularly limited, but it is preferable that the ceria-zirconia-based composite oxide does not contain a pyrochlore phase.

[0059] The use of the ceria-zirconia composite oxide is not limited, but it is particularly suitable for use as a catalyst support for an exhaust gas purification catalyst (exhaust gas purification catalyst support).

[0060] When the ceria-zirconia composite oxide is used as a catalyst support for an exhaust gas purification catalyst, the metal to be supported is not particularly limited, but examples thereof include Pt, Pd, and Rh.

[0061] [Method of producing ceria-zirconia composite oxide] An example of a method for producing a ceria-zirconia-based composite oxide will be described below, however, the method for producing a ceria-zirconia-based composite oxide of the present invention is not limited to the following example.

[0062] The method for producing a ceria-zirconia-based composite oxide according to this embodiment includes the steps of: A step 1 of neutralizing an aqueous solution of raw material salts containing cerium and zirconium with a base to obtain a precursor of a ceria-zirconia composite oxide; Step 2 of adding an oxidizing agent to the obtained precursor; A step 3 of subjecting the suspension obtained in the step 2 to solid-liquid separation and applying a pressure of 1.5 MPa or more; A step 4 of mixing water with the solid obtained in the step 3 so that the water content is 90% by mass or more; Step 5 of heat-treating the mixture obtained in step 4; Includes.

[0063] Hereinafter, each step of the method for producing a ceria-zirconia-based composite oxide according to this embodiment will be described.

[0064] An aqueous solution of raw material salts containing cerium and zirconium is neutralized with a base to obtain a precursor of a ceria-zirconia composite oxide (Step 1).

[0065] The raw material salt containing cerium may be any salt that supplies cerium ions, and examples thereof include at least one of cerium nitrate, cerium chloride, cerium acetate, and hydrates thereof. Among these, chloride raw materials are preferred from the viewpoint of wastewater regulations.

[0066] The raw material salt containing zirconium may be any salt capable of supplying zirconium ions, and examples thereof include at least one of zirconium oxynitrate, zirconium oxychloride, zirconium nitrate, and hydrates thereof. Among these, chloride raw materials are preferred from the viewpoint of wastewater regulations.

[0067] The aqueous solution may further contain a raw material salt containing a rare earth element other than Ce and Pm, if necessary.

[0068] Examples of rare earth elements other than Ce and Pm include Sc, Y, La, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb and Lu.

[0069] In addition to the above, the composition may contain one or more elements selected from the group consisting of (A) at least one element selected from the group consisting of In, Si, Sn, Bi, P, and Zn, (B) transition metal elements (excluding rare earth elements and precious metal elements), and (C) alkaline earth metal elements.

[0070] The raw materials for (A) at least one element selected from the group consisting of In, Si, Sn, Bi, P, and Zn, (B) transition metal elements (excluding rare earth elements and noble metal elements), and (C) alkaline earth metal elements are not particularly limited as long as they are water-soluble. Examples include nitrates, sulfates, acetates, chlorides, and bromides. The purity of these raw materials is preferably 95% or more, and more preferably 98% or more.

[0071] The solvent for preparing the aqueous solution may be appropriately selected depending on the type of raw material salt, etc., but it is usually preferable to use water (pure water, ion-exchanged water, etc.: the same applies below).

[0072] When these raw material salts are mixed in a predetermined ratio to obtain an aqueous solution, the metal salt concentration in the aqueous solution is preferably 1% by mass or more and 5% by mass or less in terms of oxide. If it is 1% by mass or more, the concentration is sufficient for reaction. If it is 5% by mass or less, the increase in viscosity during neutralization can be suppressed, stirring can be performed sufficiently, and compounding is easy.

[0073] Examples of the base for neutralizing the aqueous solution include alkali hydroxides such as sodium hydroxide and potassium hydroxide, aqueous ammonia, etc. Among these, aqueous ammonia is preferred from the viewpoint of containing fewer impurities.

[0074] Neutralization is carried out until the pH falls within a range of preferably 8 or more and 11 or less, more preferably 9 or more and 11 or less. This makes it possible to suitably obtain a precursor (precipitate) of a ceria-zirconia composite oxide.

[0075] Next, an oxidizing agent is added to the obtained precursor (step 2). By adding an oxidizing agent, cerium can be made into a tetravalent ion. When cerium is made into a tetravalent ion, its ionic radius becomes smaller. By making the ionic radius of cerium smaller, solid solution diffusion during firing becomes more likely to occur. As a result, a high OSC can be obtained. In other words, a solid solution in which cerium and zirconium are uniform at the atomic level can be formed, resulting in a high OSC.

[0076] Examples of the oxidizing agent include perchloric acid, persulfuric acid, percarboxylic acid, salts thereof, hydrogen peroxide, etc. Among these, perchloric acid is preferred from the viewpoints of having fewer impurities, being capable of oxidizing and removing chloride ions, and being decomposed and removed by itself.

[0077] The amount of the oxidizing agent added is preferably as large as possible from the viewpoint of oxidation of cerium (III), and is preferably 0.25 to 0.5 times, and more preferably 0.3 to 0.4 times, the weight of ceria.

[0078] Next, the suspension obtained in step 2 is subjected to solid-liquid separation and pressurized at 1.5 MPa or more (step 3). Since the suspension obtained in step 2 is subjected to solid-liquid separation and pressurized at 1.5 MPa or more (step 3), the pores in the particles are crushed in step 3, and most of the large pores disappear. This results in a dense aggregate state.

[0079] The method for solid-liquid separation is not particularly limited, and for example, filtration, centrifugation, decantation, etc. can be used.

[0080] After recovering the solid matter by solid-liquid separation, it is preferable to wash the solid matter with water, if necessary, to remove any adhering impurities.

[0081] The pressurizing method includes a filter press. The temperature during the pressurization is not particularly limited, but is preferably from room temperature to 50° C. or less.

[0082] The pressure during the pressurization is not particularly limited as long as it is 1.5 MPa or more, and is more preferably 1.6 MPa or more, and even more preferably 1.7 MPa or more. The higher the pressure during pressing, the more preferable it is, and for example, 2 MPa or less, 1.9 MPa or less. The pressure during the pressurization is more preferably 1.6 MPa or more and 2.0 MPa or less, and further preferably 1.7 MPa or more and 1.9 MPa or less.

[0083] The pressurizing time is preferably 60 minutes or more, and more preferably 120 minutes or more. The longer the pressurizing time, the better. From the viewpoint of shortening the production time, however, it is preferably 240 minutes or less, and more preferably 180 minutes or less. The time for applying pressure is preferably from 60 minutes to 240 minutes, and more preferably from 120 minutes to 180 minutes.

[0084] Next, water is mixed with the solid obtained in step 3 so that the water content is 90% by mass or more (step 4).

[0085] The method for mixing the solid material with water may be such that the solid material is stirred so as to be uniformly dispersed in the water.

[0086] The water content is preferably 90% by mass or more, and more preferably 93% by mass or more. The moisture content is preferably 98% by mass or less, and more preferably 95% by mass or less. The moisture content is preferably from 90% by mass to 98% by mass, and more preferably from 93% by mass to 95% by mass.

[0087] Next, the mixture obtained in the step 4 is heat-treated (step 5). When heat treatment is performed after the moisture content is set to 90 mass% or more, fine pores are formed during drying by heat treatment. Since there are no large pores as described above, the obtained ceria-zirconia composite oxide has no large pores and only fine pores are formed.

[0088] The temperature of the heat treatment is preferably 500° C. or higher, and more preferably 600° C. or higher. The temperature of the heat treatment is preferably 1100° C. or less, and more preferably 1050° C. or less. The temperature of the heat treatment is preferably 500° C. or higher and 1100° C. or lower, and more preferably 600° C. or higher and 1050° C. or lower.

[0089] The heat treatment time is preferably 5 hours or more, and more preferably 7 hours or more. The heat treatment time is preferably 15 hours or less, and more preferably 10 hours or less. The time for the heat treatment is preferably from 5 hours to 15 hours, and more preferably from 7 hours to 10 hours.

[0090] The atmosphere for the heat treatment is not particularly limited, and may be air, an inert gas (eg, nitrogen), or the like.

[0091] The heat treatment can be carried out, for example, in an electric furnace using an alumina sheath.

[0092] In this manner, a ceria-zirconia composite oxide can be obtained.

[0093] Furthermore, the obtained ceria-zirconia composite oxide may be pulverized as necessary, preferably so that the ceria-zirconia composite oxide has a desired particle size. The pulverization can be carried out using a general pulverizer such as a planetary mill, a ball mill, a hammer mill, or a jet mill, without any particular limitation. The pulverization may be performed by either a wet method or a dry method, but a dry method is preferred. The time for the grinding is not particularly limited, but is, for example, from 2 hours to 8 hours. The balls used for the grinding are not particularly limited as long as they are harder than the ceria-zirconia composite oxide, and for example, zirconia balls can be used. The diameter of the balls used may be 5 μm or more and 20 μm or less.

[0094] The ceria-zirconia composite oxide obtained by the above manufacturing process has a high specific surface area due to the formation of fine pores, has a high density due to the almost complete absence of large pores, and has a high OSC due to the cerium and zirconium being uniform at the atomic level.

[0095] As described above, the ceria-zirconia composite oxide obtained by the production method according to this embodiment has a high density, a large specific surface area, and a high OSC. EXAMPLES

[0096] The present invention will be described in detail below using examples, but the present invention is not limited to the following examples as long as it does not depart from the gist of the invention. Note that the ceria-zirconia composite oxides obtained in the examples and comparative examples contain 1 to 3 mass % of hafnium as an inevitable impurity relative to zirconium in terms of oxide (calculated according to the following formula (X)). <Formula (X)> ([Mass of hafnium] / ([Mass of zirconium]+[Mass of hafnium]))×100(%)

[0097] The maximum and minimum values ​​of the content of each component shown in the following examples should be considered as the preferred minimum and maximum values ​​of the present invention, regardless of the contents of other components. Furthermore, the maximum and minimum values ​​of the measured values ​​shown in the following examples should be considered as the preferred minimum and maximum values ​​of the present invention, regardless of the content (composition) of each component.

[0098] [Preparation of ceria-zirconia composite oxide] Example 1 Zirconium oxychloride octahydrate (Wako Pure Chemical Industries, Ltd., Wako Special Grade, 0.93 kg in terms of zirconium oxide), cerium (III) chloride heptahydrate (Wako Pure Chemical Industries, Ltd., 97%, 2.01 kg in terms of cerium (IV) oxide), and praseodymium (III) chloride heptahydrate (Wako Pure Chemical Industries, Ltd., 0.06 kg in terms of praseodymium oxide) were dissolved in ion-exchanged water to prepare a 5 mass % mixed solution in terms of oxide. This mixed solution was neutralized to pH 9 with 25 mass % ammonium water to obtain a precursor (precipitate) of a ceria-zirconia composite oxide. Next, 60% perchloric acid (Wako Pure Chemical Industries, special grade reagent, 0.84 kg) was added to the obtained precursor slurry. The resulting suspension was then recovered by solid-liquid separation and washed, and the resulting solid matter was pressurized at 1.5 MPa for 1 hour using a filter press device. Water was mixed with the pressed solid so that the water content was 90% by mass. Next, the mixture obtained was fired in an electric furnace in air at 700°C for 5 hours using an alumina sheath to obtain a ceria-zirconia composite oxide. The ceria-zirconia composite oxide was pulverized in a ball mill for 4 hours to obtain the ceria-zirconia composite oxide according to Example 1. <Ball mill grinding conditions> The ceria-zirconia composite oxide (total amount) and 1% alcohol (ethanol) based on the ceria-zirconia composite oxide were added to a 10 L nylon pod, and pulverized and mixed in a dry ball mill with 15 kg balls for 4 hours. Zirconia balls with a diameter of 10 mm were used for pulverization.

[0099] (Examples 2-4, 20-24, 26-28) The ceria-zirconia composite oxides according to Examples 2-4, 20-24, and 26-28 were obtained in the same manner as in Example 1, except that the contents of zirconium oxide, cerium oxide, and praseodymium oxide, the firing temperature, and the grinding time were changed as shown in Table 1-2.

[0100] Example 5 A ceria-zirconia composite oxide according to Example 5 was obtained in the same manner as in Example 1, except that the mixed solution was prepared as follows. <Preparation of mixed solution> Zirconium oxychloride octahydrate (Wako Pure Chemical Industries, Ltd., Wako Special Grade, 1.23 kg in terms of zirconium oxide), cerium (III) chloride heptahydrate (Wako Pure Chemical Industries, Ltd., 97%, 1.71 kg in terms of cerium (IV) oxide), and lanthanum (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., 99.0%, 0.06 kg in terms of lanthanum oxide) were dissolved in ion-exchanged water to prepare a 5% by mass mixed solution in terms of oxide.

[0101] Example 6 A ceria-zirconia composite oxide according to Example 6 was obtained in the same manner as in Example 1, except that the mixed solution was prepared as follows. <Preparation of mixed solution> Zirconium oxychloride octahydrate (Wako Pure Chemical Industries, Ltd., Wako Special Grade, 1.23 kg in terms of zirconium oxide), cerium (III) chloride heptahydrate (Wako Pure Chemical Industries, Ltd., 97%, 1.71 kg in terms of cerium (IV) oxide), and neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., 99.5%, 0.06 kg in terms of neodymium oxide) were dissolved in ion-exchanged water to prepare a 5% by mass mixed solution in terms of oxide.

[0102] Example 7 A ceria-zirconia composite oxide according to Example 7 was obtained in the same manner as in Example 1, except that the mixed solution was prepared as follows. <Preparation of mixed solution> Zirconium oxychloride octahydrate (Wako Pure Chemical Industries, Ltd., Wako Special Grade, 1.23 kg in terms of zirconium oxide), cerium (III) chloride heptahydrate (Wako Pure Chemical Industries, Ltd., 97%, 1.71 kg in terms of cerium (IV) oxide), and yttrium (III) nitrate n-hydrate (Wako Pure Chemical Industries, Ltd., 99.9%, 0.06 kg in terms of yttrium oxide) were dissolved in ion-exchanged water to prepare a 5% by mass mixed solution in terms of oxide.

[0103] Example 8 A ceria-zirconia composite oxide according to Example 8 was obtained in the same manner as in Example 1, except that the mixed solution was prepared as follows. <Preparation of mixed solution> Zirconium oxychloride octahydrate (Wako Pure Chemical Industries, Ltd., Wako Special Grade, 1.23 kg in terms of zirconium oxide), cerium (III) chloride heptahydrate (Wako Pure Chemical Industries, Ltd., 97%, 1.71 kg in terms of cerium (IV) oxide), lanthanum (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., 99.0%, 0.03 kg in terms of lanthanum oxide), and neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., 99.5%, 0.03 kg in terms of neodymium oxide) were dissolved in ion-exchanged water to prepare a 5% by mass mixed solution in terms of oxide.

[0104] Example 9 A ceria-zirconia composite oxide according to Example 9 was obtained in the same manner as in Example 1, except that the mixed solution was prepared as follows. <Preparation of mixed solution> Zirconium oxychloride octahydrate (Wako Pure Chemical Industries, Ltd., Wako Special Grade, 1.215 kg in terms of zirconium oxide), cerium (III) chloride heptahydrate (Wako Pure Chemical Industries, Ltd., 97%, 1.695 kg in terms of cerium (IV) oxide), lanthanum (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., 99.0%, 0.03 kg in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., 99.5%, 0.03 kg in terms of neodymium oxide), and yttrium (III) nitrate n-hydrate (Wako Pure Chemical Industries, Ltd., 99.9%, 0.03 kg in terms of yttrium oxide) were dissolved in ion-exchanged water to prepare a 5% by mass mixed solution in terms of oxide.

[0105] Example 10 A ceria-zirconia composite oxide according to Example 10 was obtained in the same manner as in Example 1, except that the mixed solution was prepared as follows. <Preparation of mixed solution> Zirconium oxychloride octahydrate (Wako Pure Chemical Industries, Wako Special Grade, 1.23 kg in terms of zirconium oxide), cerium (III) chloride heptahydrate (Wako Pure Chemical Industries, 97%, 1.71 kg in terms of cerium (IV) oxide), and scandium (III) nitrate hydrate (Sigma-Aldrich, 99.9%, 0.06 kg in terms of scandium oxide) were dissolved in ion-exchanged water to prepare a 5% by mass mixed solution in terms of oxide.

[0106] Example 11 A ceria-zirconia composite oxide according to Example 11 was obtained in the same manner as in Example 1, except that the mixed solution was prepared as follows. <Preparation of mixed solution> Zirconium oxychloride octahydrate (Wako Pure Chemical Industries, Ltd., Wako Special Grade, 1.23 kg in terms of zirconium oxide), cerium (III) chloride heptahydrate (Wako Pure Chemical Industries, Ltd., 97%, 1.71 kg in terms of cerium (IV) oxide), and magnesium carbonate (Wako Pure Chemical Industries, Ltd., 0.06 kg in terms of magnesium oxide) were dissolved in ion-exchanged water to prepare a 5% by mass mixed solution in terms of oxide.

[0107] Example 12 A ceria-zirconia composite oxide according to Example 12 was obtained in the same manner as in Example 1, except that the mixed solution was prepared as follows. <Preparation of mixed solution> Zirconium oxychloride octahydrate (Wako Pure Chemical Industries, Wako Special Grade, 1.23 kg in terms of zirconium oxide), cerium (III) chloride heptahydrate (Wako Pure Chemical Industries, 97%, 1.71 kg in terms of cerium (IV) oxide), and calcium carbonate (Wako Pure Chemical Industries, Reagent Grade, 0.06 kg in terms of calcium oxide) were dissolved in ion-exchanged water to prepare a 5% by mass mixed solution in terms of oxide.

[0108] (Example 13) A ceria-zirconia composite oxide according to Example 13 was obtained in the same manner as in Example 1, except that the mixed solution was prepared as follows. <Preparation of mixed solution> Zirconium oxychloride octahydrate (Wako Pure Chemical Industries, Ltd., Wako Special Grade, 1.23 kg in terms of zirconium oxide), cerium (III) chloride heptahydrate (Wako Pure Chemical Industries, Ltd., 97%, 1.71 kg in terms of cerium (IV) oxide), and strontium carbonate (Wako Pure Chemical Industries, Ltd., 95.0%, 0.06 kg in terms of strontium oxide) were dissolved in ion-exchanged water to prepare a 5% by mass mixed solution in terms of oxide.

[0109] Example 14 A ceria-zirconia composite oxide according to Example 14 was obtained in the same manner as in Example 1, except that the mixed solution was prepared as follows. <Preparation of mixed solution> Zirconium oxychloride octahydrate (Wako Pure Chemical Industries, Ltd., Wako Special Grade, 1.23 kg in terms of zirconium oxide), cerium (III) chloride heptahydrate (Wako Pure Chemical Industries, Ltd., 97%, 1.71 kg in terms of cerium (IV) oxide), and barium carbonate (Wako Pure Chemical Industries, Ltd., 99.0%, 0.06 kg in terms of barium oxide) were dissolved in ion-exchanged water to prepare a 5% by mass mixed solution in terms of oxide.

[0110] Example 15 A ceria-zirconia composite oxide according to Example 15 was obtained in the same manner as in Example 1, except that the mixed solution was prepared as follows. <Preparation of mixed solution> Zirconium oxychloride octahydrate (Wako Pure Chemical Industries, Ltd., Wako Special Grade, 1.23 kg in terms of zirconium oxide), cerium (III) chloride heptahydrate (Wako Pure Chemical Industries, Ltd., 97%, 1.71 kg in terms of cerium (IV) oxide), and sodium silicate solution (Wako Pure Chemical Industries, Ltd., Wako Grade 1, 0.06 kg in terms of silicon dioxide) were dissolved in ion-exchanged water to prepare a 5% by mass mixed solution in terms of oxide.

[0111] (Example 16) A ceria-zirconia composite oxide according to Example 16 was obtained in the same manner as in Example 1, except that the mixed solution was prepared as follows. <Preparation of mixed solution> Zirconium oxychloride octahydrate (Wako Pure Chemical Industries, Wako Special Grade, 1.23 kg in terms of zirconium oxide), cerium (III) chloride heptahydrate (Wako Pure Chemical Industries, 97%, 1.71 kg in terms of cerium (IV) oxide), and ammonium dihydrogen phosphate (Wako Pure Chemical Industries, Reagent Grade, 0.06 kg in terms of phosphate (PO4)) were dissolved in ion-exchanged water to prepare a 5% by mass mixed solution in terms of oxide.

[0112] (Example 17) A ceria-zirconia composite oxide according to Example 17 was obtained in the same manner as in Example 1, except that the mixed solution was prepared as follows. <Preparation of mixed solution> Zirconium oxychloride octahydrate (Wako Pure Chemical Industries, Wako Special Grade, 1.275 kg in terms of zirconium oxide), cerium (III) chloride heptahydrate (Wako Pure Chemical Industries, 97%, 1.71 kg in terms of cerium (IV) oxide), and iron (III) chloride hexahydrate (Wako Pure Chemical Industries, Reagent Grade, 0.015 kg in terms of iron oxide (Fe2O3)) were dissolved in ion-exchanged water to prepare a 5 mass% mixed solution in terms of oxide.

[0113] (Example 18) A ceria-zirconia composite oxide according to Example 18 was obtained in the same manner as in Example 1, except that the mixed solution was prepared as follows. <Preparation of mixed solution> Zirconium oxychloride octahydrate (Wako Pure Chemical Industries, Ltd., Wako Special Grade, 1.23 kg in terms of zirconium oxide), cerium (III) chloride heptahydrate (Wako Pure Chemical Industries, Ltd., 97%, 1.71 kg in terms of cerium (IV) oxide), and titanium (IV) chloride (Wako Pure Chemical Industries, Ltd., Wako Special Grade, 0.06 kg in terms of titanium oxide) were dissolved in ion-exchanged water to prepare a 5% by mass mixed solution in terms of oxide.

[0114] (Example 19) A ceria-zirconia composite oxide according to Example 19 was obtained in the same manner as in Example 1, except that the mixed solution was prepared as follows. <Preparation of mixed solution> Zirconium oxychloride octahydrate (Wako Pure Chemical Industries, Ltd., Wako Special Grade, 1.26 kg in terms of zirconium oxide), cerium (III) chloride heptahydrate (Wako Pure Chemical Industries, Ltd., 97%, 1.71 kg in terms of cerium (IV) oxide), and rhodium (III) nitrate solution (Wako Pure Chemical Industries, Ltd., 0.03 kg in terms of rhodium) were dissolved in ion-exchanged water to prepare a 5 mass % mixed solution in terms of oxide.

[0115] (Example 25) A ceria-zirconia composite oxide according to Example 25 was obtained in the same manner as in Example 8, except that the firing temperature was changed as shown in Table 2.

[0116] (Example 29) A ceria-zirconia composite oxide according to Example 29 was obtained in the same manner as in Example 1, except that the mixed solution was prepared as follows. <Preparation of mixed solution> Zirconium oxychloride octahydrate (Wako Pure Chemical Industries, Ltd., Wako Special Grade, 2.10 kg in terms of zirconium oxide) and cerium (III) chloride heptahydrate (Wako Pure Chemical Industries, Ltd., 97%, 0.90 kg in terms of cerium (IV) oxide) were dissolved in ion-exchanged water to prepare a 5% by mass mixed solution in terms of oxide.

[0117] (Example 30) A ceria-zirconia composite oxide according to Example 30 was obtained in the same manner as in Example 1, except that the mixed solution was prepared as follows. <Preparation of mixed solution> Zirconium oxychloride octahydrate (Wako Pure Chemical Industries, Ltd., Wako Special Grade, 0.90 kg in terms of zirconium oxide) and cerium (III) chloride heptahydrate (Wako Pure Chemical Industries, Ltd., 97%, 2.10 kg in terms of cerium (IV) oxide) were dissolved in ion-exchanged water to prepare a 5% by mass mixed solution in terms of oxide.

[0118] (Example 31) A ceria-zirconia composite oxide according to Example 31 was obtained in the same manner as in Example 1, except that the mixed solution was prepared as follows. <Preparation of mixed solution> Zirconium oxychloride octahydrate (Wako Pure Chemical Industries, Ltd., Wako Special Grade, 1.26 kg in terms of zirconium oxide) and cerium (III) chloride heptahydrate (Wako Pure Chemical Industries, Ltd., 97%, 1.74 kg in terms of cerium (IV) oxide) were dissolved in ion-exchanged water to prepare a 5% by mass mixed solution in terms of oxide.

[0119] (Comparative Example 1-2) A ceria-zirconia composite oxide according to Comparative Example 1-2 was prepared in the same manner as in Example 1, except that the contents of zirconium oxide and cerium oxide were changed as shown in Table 3.

[0120] Comparative Example 3 A ceria-zirconia composite oxide according to Comparative Example 3 was obtained in the same manner as in Example 2, except that the firing temperature was changed as shown in Table 3.

[0121] Comparative Example 4 Zirconium oxychloride octahydrate (58 g in terms of zirconium oxide) was dissolved in ion-exchanged water, and then 35% hydrochloric acid and ion-exchanged water were added to adjust the acid concentration to 0.67 N and the zirconium oxide concentration to 4 w / v% (mass volume percent concentration). The resulting solution was placed in an autoclave and the pressure was adjusted to 2×10 5The mixture was heated to 120° C. and 1,065 g of 5% sodium sulfate (sulfating agent) was added at the same temperature, and the mixture was maintained for another 15 minutes. After sulfation, the mixture was allowed to cool to room temperature to obtain a basic zirconium sulfate-containing slurry. A cerium nitrate solution (28 g in terms of cerium (IV) oxide), a neodymium nitrate solution (7 g in terms of neodymium oxide), and a praseodymium nitrate solution (7 g in terms of praseodymium oxide) were added to the basic zirconium sulfate-containing slurry. Next, 500 g of 25% sodium hydroxide (neutralizing alkali) was added over a period of 60 minutes. Zirconium hydroxide was produced by this neutralization. Next, the zirconium hydroxide-containing slurry was filtered and washed with water, and then fired at 700° C. for 5 hours without pressurizing the precursor or adjusting the water content to obtain an oxide. The oxide was pulverized with a hammer mill to obtain a ceria-zirconia composite oxide according to Comparative Example 4. <Crushing conditions using a hammer mill> The powder was ground at 8000 rpm using an IKA continuous mill with a hammer head and a screen diameter of φ1 mm.

[0122] Comparative Example 5 Zirconium oxynitrate dihydrate (72.9 g in terms of zirconium oxide) was dissolved in ion-exchanged water, and the zirconium oxide concentration was adjusted to 10 wt / v% (mass volume percent concentration) to obtain a zirconium salt solution. The obtained solution was placed in an autoclave, heated to 120°C, and held for 1 hour, after which 1021 g of 5% sodium sulfate (sulfating agent) was added and held for 30 minutes. It was then allowed to cool to room temperature (25°C) to obtain a basic zirconium sulfate-containing slurry. A cerium nitrate solution (20.4 g in terms of cerium (IV) oxide), a neodymium nitrate solution (5.0 g in terms of neodymium oxide), and a lanthanum nitrate solution (1.8 g in terms of lanthanum oxide) were added to the basic zirconium sulfate-containing slurry. Next, 500 g of 25% sodium hydroxide (neutralizing alkali) was added over 60 minutes to generate hydroxide precipitates (zirconium hydroxide-containing slurry). The obtained hydroxide precipitate was filtered and thoroughly washed with water, and the obtained hydroxide was dried at 105°C for 24 hours. The dried hydroxide was heat-treated (calcined) at 800°C in air for 5 hours to obtain an oxide. The oxide was pulverized with a hammer mill to obtain a ceria-zirconia composite oxide according to Comparative Example 5. The pulverization conditions with the hammer mill were the same as those of Comparative Example 4.

[0123] Comparative Example 6 Zirconium oxychloride octahydrate (46 g in terms of zirconium oxide) was dissolved in ion-exchanged water, and then 35% hydrochloric acid and ion-exchanged water were added to adjust the acid concentration to 0.67 N and the zirconium oxide concentration to 4 w / v% (mass volume percent concentration). The resulting solution was placed in an autoclave and the pressure was increased to 2×10 5 The mixture was heated to 120° C. and 1,065 g of 5% sodium sulfate (sulfating agent) was added at the same temperature, and the mixture was maintained for another 15 minutes. After sulfation, the mixture was allowed to cool to room temperature to obtain a basic zirconium sulfate-containing slurry. A cerium nitrate solution (52 g in terms of cerium (IV) oxide) and a praseodymium nitrate solution (2 g in terms of praseodymium oxide) were added to the basic zirconium sulfate-containing slurry. Next, 500 g of 25% sodium hydroxide (neutralizing alkali) was added over 60 minutes. Zirconium hydroxide was produced by this neutralization. Next, the zirconium hydroxide-containing slurry was filtered and washed with water, and then fired at 850°C for 5 hours without pressurizing the precursor or adjusting the water content to obtain an oxide. The oxide was pulverized in a hammer mill to obtain a ceria-zirconia composite oxide according to Comparative Example 6. The pulverization conditions in the hammer mill were the same as those in Comparative Example 4.

[0124] Comparative Example 7 Zirconium oxynitrate dihydrate (46 g in terms of zirconium oxide) was dissolved in ion-exchanged water, and the zirconium oxide concentration was adjusted to 10 wt / v% (mass volume percent concentration) to obtain a zirconium salt solution. The obtained solution was placed in an autoclave, heated to 120°C, and held for 1 hour, after which 1021 g of 5% sodium sulfate (sulfating agent) was added and held for 30 minutes. It was then allowed to cool to room temperature (25°C) to obtain a basic zirconium sulfate-containing slurry. A cerium nitrate solution (52 g in terms of cerium (IV) oxide) and a praseodymium nitrate solution (2 g in terms of praseodymium oxide) were added to the basic zirconium sulfate-containing slurry. Next, 500 g of 25% sodium hydroxide (neutralizing alkali) was added over 60 minutes to generate a hydroxide precipitate (zirconium hydroxide-containing slurry). The obtained hydroxide precipitate was filtered and thoroughly washed with water, and the obtained hydroxide was dried at 105°C for 24 hours. The dried hydroxide was heat-treated (calcined) in air at 850°C for 5 hours to obtain an oxide. The oxide was pulverized in a hammer mill to obtain a ceria-zirconia composite oxide according to Comparative Example 7. The pulverization conditions in the hammer mill were the same as those in Comparative Example 4.

[0125] Comparative Example 8 Zirconium oxynitrate (46.0 g in terms of zirconium oxide) was dispersed in ion-exchanged water to a concentration of 3% in terms of oxide, to prepare a nitrate aqueous solution. In an autoclave, a sulfating agent was added to the nitrate aqueous solution at a temperature of 150°C to generate a basic zirconium sulfate salt. Cerium (III) nitrate hexahydrate (52.0 g in terms of cerium (IV) oxide), praseodymium (III) nitrate hexahydrate (2.0 g in terms of praseodymium oxide) and the basic zirconium sulfate salt were mixed. Neutralization was performed using an alkali to obtain a precipitate of a cerium-zirconium composite hydroxide. The generated precipitate was collected after solid-liquid separation, dried at 200°C, and then fired in an electric furnace at 800°C for 5 hours. Furthermore, the obtained oxide was pulverized with a hammer mill to obtain a ceria-zirconia composite oxide according to Comparative Example 8. The pulverization conditions with the hammer mill were the same as those in Comparative Example 4.

[0126] Comparative Example 9 High-purity zirconium oxide (99.9% purity) was used as the raw material for zirconium, and high-purity cerium oxide (99.9% purity) was used as the raw material for cerium. High-purity zirconium oxide (4.2 kg) and high-purity cerium oxide (5.8 kg) were separated and mixed, and melted at 2200°C or higher in an arc-type electric furnace with a secondary voltage of 85 V, average load power of 99.5 kW, current application time of 1 hour 50 minutes, and total power of 182 kWh. 500 g of coke was used to promote initial current application. After melting, the electric furnace was covered with a carbon cover and cooled slowly in the air for 24 hours to obtain an ingot. The ingot was crushed to 3 mm or less using a jaw crusher and a roll crusher, and the powder of 1 mm or less was collected using a sieve. Next, in order to remove suboxides and distortions in the crystals due to supercooling during the melting process, the mixture was fired in air at 800°C for 3 hours using an electric furnace, and then pulverized in a ball mill for 8 hours to obtain a powder. This powder was used as the ceria-zirconia composite oxide according to Comparative Example 9. Note that in this process, the pressurization process of the intermediate slurry and the adjustment of the moisture content before firing were not performed.

[0127] Comparative Example 10 A ceria-zirconia composite oxide according to Comparative Example 10 was obtained in the same manner as in Comparative Example 9, except that the pulverization was performed for 4 hours in a ball mill instead of for 8 hours in a ball mill.

[0128] Comparative Example 11 Zirconium oxychloride octahydrate (0.93 kg in terms of zirconium oxide), cerium (III) chloride heptahydrate (Wako Pure Chemical Industries, 97%, 2.01 kg in terms of cerium (IV) oxide), and praseodymium (III) chloride heptahydrate (Wako Pure Chemical Industries, 0.06 kg in terms of praseodymium oxide) were dissolved in ion-exchanged water to prepare a 5 mass % mixed solution in terms of oxide. This mixed solution was neutralized with 25 mass % ammonium water to a pH of 9, to obtain a precursor (precipitate) of a ceria-zirconia composite oxide. Next, the precursor was recovered and washed by solid-liquid separation without adding perchloric acid to the obtained precursor slurry. The obtained solid was pressurized at 1.5 MPa. Water was mixed with the pressed solid so that the water content was 90% by mass. Next, the obtained mixture was fired in an alumina sheath in an electric furnace at 700°C in air for 5 hours to obtain a ceria-zirconia composite oxide. The ceria-zirconia composite oxide was pulverized in a ball mill for 4 hours to obtain a ceria-zirconia composite oxide according to Comparative Example 11.

[0129] Comparative Example 12 Zirconium oxychloride octahydrate (1.38 kg in terms of zirconium oxide), cerium (III) chloride heptahydrate (Wako Pure Chemical Industries, Ltd., 97%, 1.56 kg in terms of cerium (IV) oxide), and praseodymium (III) chloride heptahydrate (Wako Pure Chemical Industries, Ltd., 0.06 kg in terms of praseodymium oxide) were dissolved in ion-exchanged water to prepare a 5 mass % mixed solution in terms of oxide. This mixed solution was neutralized with 25 mass % ammonium water to a pH of 9, to obtain a precursor precipitate of a ceria-zirconia composite oxide. Next, 60% perchloric acid (Wako Pure Chemical Industries, special grade reagent, 0.84 kg) was added to the obtained precursor slurry. Next, the obtained suspension was recovered by solid-liquid separation and washed. The obtained solid was fired in an electric furnace at 700°C in air for 5 hours without pressure or adjustment of the moisture content to obtain a ceria-zirconia composite oxide. The ceria-zirconia composite oxide was pulverized in a ball mill for 4 hours to obtain a ceria-zirconia composite oxide according to Comparative Example 12.

[0130] [Measurement of specific surface area] The specific surface area of ​​the ceria-zirconia composite oxides of the examples and comparative examples was measured by the BET method using a specific surface area meter ("Maxsorb", manufactured by Mountec Co., Ltd.) The results are shown in Tables 1-3.

[0131] [Measurement of tap density] As a measuring device for tap density, TAPDENSER KYT-3000 (manufactured by Seishin Enterprise Co., Ltd.) was used. 100 g of sample powder (ceria-zirconia composite oxide according to the examples and comparative examples) was filled into a tapping cell, and the height of the spacer was set to 3 cm. The tapping cell was set on a tapping table, and tapping was performed 800 times with the measuring device. After tapping was completed, the scale on the cell was read, and the tap density was obtained by calculating [(powder weight) / (volume)]. More detailed measuring conditions were as follows. The results are shown in Tables 1-3. <Conditions for measuring tap density> Tapping stroke: 3cm Tapping speed: 100 times / 50 seconds

[0132] [Oxygen storage capacity (OSC) measurement] The oxygen storage and release capacity was measured by the O2 pulse method using a commercially available measuring device (Microtrack Bell Co., Ltd., "BELCAT II"). Specifically, the measurement was performed through the following steps (a) to (i) in order. (a) 0.2 g of each of the ceria-zirconia composite oxides of the examples and comparative examples was weighed out. (b) The weighed powder was placed in a flow-type reactor, and the temperature inside was raised to 600°C in a He gas flow and then held at that temperature for 1 hour. (c) The temperature of the ceria-zirconia composite oxide was adjusted to 600°C. (d) A constant concentration of H2 / Ar mixed gas (concentration: 5%, H2:Ar ratio: 5:95) was introduced to reduce the ceria-zirconia composite oxide. (e) The atmosphere was replaced with He. (f) A fixed amount (0.9 mL) of oxygen was introduced into the atmosphere. (g) The amount of unadsorbed oxygen was confirmed using a thermal conductivity detector (TCD). (h) The introduction of a fixed amount of oxygen into the atmosphere in (f) and the confirmation of the amount of unadsorbed oxygen in (g) were repeated until the amount of introduced oxygen became equal to the amount of unadsorbed oxygen. (i) The amount of adsorbed oxygen, i.e., the amount of OSC, was calculated by subtracting the amount of unadsorbed oxygen from the amount of introduced oxygen, which was determined in advance. The results are shown in Table 1-3.

[0133] [Particle diameter D 90 Measurement of 0.15 g of the ceria-zirconia composite oxide of each of the Examples and Comparative Examples and 40 ml of 0.2% aqueous sodium hexametaphosphate solution were placed in a 50 ml beaker and dispersed for 5 minutes in an ultrasonic cleaner "VS-100 III" (Velvoclear), and then placed in a device (laser diffraction / scattering particle size distribution measuring device ("LA-950" Horiba, Ltd.)) for measurement. The results are shown in Table 1-3.

[0134] [Measurement of pore volume] For the ceria-zirconia composite oxides of the examples and comparative examples, the pore size distribution was obtained by the mercury intrusion method using a pore size distribution measuring device ("Autopore IV9500" manufactured by Micromeritics). The measurement conditions were as follows. <Measurement conditions> Measurement equipment: Pore size distribution measurement equipment (Micromeritics Autopore IV9500) Measurement range: 0.018~10.0μm Number of measurement points: 62 points Mercury contact angle: 140degrees Mercury surface tension: 480dyne / cm

[0135] The total pore volume (pore volume of pores having a diameter of 20 nm or more and 500 nm or less) was calculated using the obtained pore distribution. The results are shown in Table 1-3.

[0136] [X-ray diffraction spectrum] An X-ray diffraction spectrum was obtained using an X-ray diffractometer ("UltIma IV" manufactured by Rigaku) ​​for the ceria-zirconia composite oxide of Example 2. The measurement conditions were as follows: <Measurement conditions> Measurement equipment: X-ray diffraction equipment (Rigaku, UltIma IV) Source: CuKα source Tube voltage: 50kV Tube current: 30mA Scanning speed: 2θ=20~65°: 4° / min

[0137] The X-ray diffraction spectrum of the ceria-zirconia composite oxide of Example 2 is shown in FIG. As shown in Figure 1, the ceria-zirconia composite oxide of Example 2 does not have a pyrochlore phase. That is, there is no peak around 2θ=14.5°, which is observed in the pyrochlore phase, in Figure 1. Although not shown, it has been confirmed that the ceria-zirconia composite oxides of all other Examples also do not have a pyrochlore phase.

[0138] [Table 1]

[0139] [Table 2]

[0140] [Table 3]

Claims

1. Contains ceria and zirconia, The content of the ceria is 25% by mass or more and 75% by mass or less based on the entire ceria-zirconia-based composite oxide, The content of the zirconia is 25% by mass or more and 75% by mass or less based on the entire ceria-zirconia-based composite oxide, The total content of the ceria and the zirconia is 75 mass% or more based on the entire ceria-zirconia-based composite oxide, A ceria-zirconia composite oxide characterized by satisfying the following (1) to (3): (1) O 2 The oxygen storage / release capacity at 600° C. measured by a pulse method is 290 μmol / g or more and 1000 μmol / g or less. (2) Specific surface area is 15 m 2 / g or more 80m 2 / g or less. (3) Tap density is 1.75 g / mL or more and 3.00 g / mL or less.

2. The specific surface area is 30 m 2 / g or more 80m 2 2. The ceria-zirconia composite oxide according to claim 1, wherein the ceria-zirconia composite oxide has a molecular weight of 1 / g or less.

3. The specific surface area is 40 m 2 / g or more 80m 2 2. The ceria-zirconia composite oxide according to claim 1, wherein the ceria-zirconia composite oxide has a molecular weight of 1 / g or less.

4. 3. The ceria-zirconia composite oxide according to claim 1, wherein the tap density is 1.8 g / mL or more and 2.8 g / mL or less.

5. 3. The ceria-zirconia composite oxide according to claim 1, wherein the tap density is 1.85 g / mL or more and 2.6 g / mL or less.

6. 4. The ceria-zirconia composite oxide according to claim 1, wherein the content of the ceria is 35% by mass or more and 70% by mass or less based on the entire ceria-zirconia composite oxide.

7. 4. The ceria-zirconia composite oxide according to any one of claims 1 to 3, further comprising at least one oxide of a rare earth element other than Ce and Pm.

8. A particle diameter D measured by the following [Method of measuring particle diameter D90] 90 The ceria-zirconia composite oxide according to any one of claims 1 to 3, characterized in that the average particle size is 8 µm or more and 80 µm or less. [Method of measuring particle diameter D90] 0.15 g of ceria-zirconia composite oxide and 40 ml of a 0.2% aqueous solution of sodium hexametaphosphate are placed in a 50 ml beaker and dispersed for 5 minutes in an ultrasonic cleaner "VS-100 III" (manufactured by Vervoclear), and then the beaker is placed in an apparatus (a laser diffraction / scattering particle size distribution measuring apparatus ("LA-950" manufactured by Horiba, Ltd.)) for measurement.

Citation Information

Patent Citations

  • Porous zirconia-based powder and its manufacture method

    JP2008081392A

  • Metal oxide composite material and purification catalyst using the same and method for producing these

    JP2013014458A

  • Ceria-zirconia mixed oxide and method for producing same

    WO2014196100A1

  • Powdered complex oxide containing elemental cerium and element zirconium, exhaust gas purification catalyst composition using same, and method for producing same

    WO2021049525A1

  • Zirconia-based porous body and production method for zirconia-based porous body

    WO2022107900A1

Cited By

  • Zirconia-based composite oxide powder and method for producing zirconia-based composite oxide powder

    JP2026101010A

  • Zirconia-based composite oxide powder and method for producing zirconia-based composite oxide powder

    WO2026126909A1