Functionalized initiators, methods for making initiators, and functionalized elastomers

Functionalized elastomers synthesized using alkyllithium compounds and specific initiators improve filler affinity, addressing the challenge of balancing viscoelastic properties in tire treads for enhanced tire performance.

JP7560958B2Active Publication Date: 2024-10-03ジー-スリー チカディー パーチェイサーエルエルシー
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
JP2020080236
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-05-03
Filing Date
2020-04-30
Publication Date
2024-10-03
Estimated Expiration
2040-04-30

AI Technical Summary

Technical Problem

Existing functionalized polymers used in tire treads face challenges in achieving contrasting viscoelastic properties for improved wet skid resistance and reduced rolling resistance, with filler affinity being a critical factor in determining physical properties.

Method used

The use of alkyllithium compounds and specific functionalized polymerization initiators, such as organolithium compounds, to synthesize functionalized elastomers that enhance the affinity of rubbery polymers for fillers like carbon black and silica, thereby improving tire performance characteristics.

Benefits of technology

The synthesis of functionalized elastomers with enhanced filler affinity leads to improved rolling resistance and traction properties in tires, balancing viscoelastic properties for better tire performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560958000001
    Figure 0007560958000001
  • Figure 0007560958000002
    Figure 0007560958000002
  • Figure 0007560958000003
    Figure 0007560958000003
Patent Text Reader

Abstract

To provide a functionalized polymerization initiator.SOLUTION: The present invention provides a functionalized polymerization initiator, comprising the reaction product of an alkyl lithium compound and a compound of formula 1 (where R1=alkyl (C1-C8), aryl, substituted aryl, or -SiR3, where R3 independently represent C1-C8 alkyl, preferably -SiMe3; Me is methyl or -Si(CH3)2C(CH3)3; R2=C1-C8 alkyl, aryl, or substituted aryl, or -SiR3, preferably -CH3; n=0-3). The present invention further provides a method of making a functionalized initiator, and method of making a functionalized elastomer using the initiator.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] In recent years, there has been an increasing demand for functionalized polymers. Functionalized polymers can be synthesized by various living / controlled polymerization techniques. In living polymerization processes based on active carbanion centers, metals from Groups I and II of the periodic table are commonly used to initiate the polymerization of monomers into polymers. For example, lithium, barium, magnesium, sodium, and potassium are metals frequently utilized in such polymerizations. This type of initiator system is commercially important because they can be used to produce stereoregulatory polymers. For example, lithium initiators can be utilized to initiate the anionic polymerization of isoprene into synthetic polyisoprene rubber or to initiate the polymerization of 1,3-butadiene into polybutadiene rubber with the desired microstructure. [Background technology]

[0002]

[0002] The polymers formed in such polymerizations have the metal used to initiate the polymerization at the growing end of their polymer chains and are sometimes called living polymers. They are called living polymers because their polymer chains containing the terminal metal initiator continue to grow or remain until all of the available monomer is exhausted. Polymers prepared by utilizing such metal initiators usually have an essentially linear structure and usually do not contain significant amounts of branching.

[0003]

[0003] This invention details the synthesis of functionalized polymers. In general, functionalized polymers are highly desirable to achieve the best tire performance characteristics. To reduce rolling resistance and improve tire treadwear characteristics, functionalized elastomers having high resilience physical properties (low hysteresis) have been used for tire tread rubber compositions. However, to increase the wet skid resistance of tire treads, rubbery polymers having relatively low resilience physical properties (higher hysteresis) and thus undergoing greater energy loss have also been used for such tread rubber compositions. To achieve such relatively opposing viscoelastic properties for tire tread rubber compositions, various types of synthetic and natural rubber blends (mixtures) can be utilized in tire treads.

[0004]

[0004] Functionalized rubbery polymers made by living polymerization techniques are typically compounded with sulfur, accelerators, antidegradants, fillers such as carbon black, silica, or starch, and other desired rubber chemicals, and then subsequently vulcanized or cured into a useful product such as a tire or power transmission belt. It has been established that the physical properties of such cured rubber depend on the degree to which the filler is homogeneously dispersed throughout the rubber. This in turn relates to the level of affinity of the filler for a particular rubbery polymer. This may be of practical importance in improving the physical properties of rubber articles made utilizing such rubber compositions. For example, the rolling resistance and traction properties of a tire can be improved by improving the affinity of carbon black and / or silica for the rubbery polymer utilized in the tire. It would therefore be highly desirable to improve the affinity of a given rubbery polymer for fillers such as carbon black and silica. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] U.S. Patent No. 6,242,534 [Patent Document 2] U.S. Patent No. 6,207,757 [Patent Document 3] U.S. Patent No. 6,133,364 [Patent Document 4] U.S. Patent No. 6,372,857 [Patent Document 5] U.S. Patent No. 5,395,891 [Patent Document 6] U.S. Patent No. 6,127,488 [Patent Document 7] U.S. Patent No. 5,672,639 [Patent Document 8] U.S. Patent No. 6,608,125 [Patent Document 9] US Patent Application Publication No. 2003 / 0130535 [Non-patent literature]

[0006] [Non-Patent Document 1] Standard Methods for Analysis & Testing of Petroleum and Related Products and British Standard 2000 Parts, 2003, 62nd edition, Institute of Petroleum, United Kingdom [Non-Patent Document 2] Journal of the American Chemical Society, Vol. 60, p. 304 (1930) [Non-Patent Document 3] The Vanderbilt Rubber Handbook (1978), pp. 344-346 Summary of the Invention

[0007] The present invention relates to an alkyllithium compound and a compound of formula 1

[0008] [ka]

[0009] (wherein R1=alkyl(C1-C8), aryl, substituted aryl, or -SiR3, R3 is independently C1-C8 alkyl, preferably -SiMe3, and Me is methyl or -Si(CH3)2C(CH3)3; R2=C1-C8 alkyl, aryl, or substituted aryl, or -SiR3, preferably -CH3; and n=0-3). The present invention relates to a functionalized polymerization initiator comprising the reaction product of

[0010] The present invention is further directed to a method of making the functionalized initiator and a method of using the initiator to make a functionalized elastomer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Alkyllithium compounds and compounds of formula 1

[0012] [ka]

[0013] (wherein R1=alkyl(C1-C8), aryl, substituted aryl, or -SiR3, where R3 is independently C1-C8 alkyl, preferably -SiMe3, where Me is methyl or -Si(CH3)2C(CH3)3; R2=C1-C8 alkyl, aryl, or substituted aryl, or -SiR3, preferably -CH3; and n=0-3). A functionalized polymerization initiator is disclosed comprising the reaction product of:

[0014] Further disclosed are methods of making the functionalized initiators and methods of making functionalized elastomers using the initiators. In one embodiment, the compound of formula 1 is a compound of formula 2

[0015] [ka]

[0016] (wherein R is a C1-C3 alkyl group or a trimethylsilyl group). It is.

[0010] Functional initiators can be prepared by reacting a compound of formula 1 with an initiator having the general structural formula PM, where P represents a hydrocarbyl group and M represents a Group I or Group II metal.

[0017]

[0011] The metals used in the functional initiators are typically selected from the group consisting of barium, lithium, magnesium, sodium, and potassium. Lithium and potassium are the most commonly utilized metals in the synthesis of metal-terminated polymers (living polymers). Lithium initiators are usually more preferred.

[0018] Organolithium compounds are preferred initiators for use in preparing the functionalized initiators. The organolithium compounds utilized are typically organomonolithium compounds. Preferred organolithium compounds are monofunctional compounds that can be represented by the formula R-Li, where R represents a hydrocarbyl radical containing from 1 to about 20 carbon atoms. Generally, such monofunctional organolithium compounds will contain from 1 to about 10 carbon atoms. Some representative examples of preferred initiators include n-butyllithium, sec-butyllithium, n-hexyllithium, n-octyllithium, tert-octyllithium, n-decyllithium, phenyllithium, 1-naphthyllithium, 4-butylphenyllithium, p-tolyllithium, 4-phenylbutyllithium, cyclohexyllithium, 4-butylcyclohexyllithium, and 4-cyclohexylbutyllithium. Secondary butyllithium is highly preferred.

[0019] To make the functional initiator, the compound of formula 1 is combined with an organolithium compound in a molar ratio ranging from 1:2 to 2:1 in a hydrocarbon solvent such as hexane. A polymerization modifier such as TMEDA or the like may be added to the mixture. The mixture of the compound of formula 1 and the organolithium compound is then heated at a temperature ranging from 40 to 80° C. for a time period ranging from 1 to 10 minutes to form the functional initiator as a reaction product of the compound of formula 1 and the organolithium compound. The reaction product in solution may be transferred to a polymerization mixture of monomers in the solvent to form a functional diene elastomer.

[0020] The amount of functional initiator utilized during polymerization will vary depending on the molecular weight desired for the rubbery polymer being synthesized, as well as the exact polymerization temperature that will be employed. The exact amount of organolithium compound required to produce a polymer of the desired molecular weight can be readily ascertained by one skilled in the art. However, typically, 0.01 to 1 phm (parts per 100 parts by weight of monomer) of organolithium initiator will be utilized. In most cases, 0.01 to 0.1 phm of organolithium initiator will be utilized, with 0.025 to 0.07 phm being preferred.

[0021]

[0015] In one embodiment, the monomers used to synthesize the functionalized elastomer include a first monomer and an optional second monomer, where the first monomer is a conjugated diene monomer and the second monomer is a vinyl aromatic monomer.

[0022] As the first monomer, suitable conjugated diene monomers include 1,3-butadiene, isoprene, 1,3-pentadiene, 2,3-dimethyl-1,3-butadiene, 2-methyl-1,3-pentadiene, 2,3-dimethyl-1,3-pentadiene, 2-phenyl-1,3-butadiene, and 4,5-diethyl-1,3-octadiene, and the like.

[0023] Also, as the second monomer, suitable vinyl aromatic monomers include styrene, 1-vinylnaphthalene, 3-methylstyrene, 3,5-diethylstyrene, 4-propylstyrene, 2,4,6-trimethylstyrene, 4-dodecylstyrene, 3-methyl-5-normal-hexylstyrene, 4-phenylstyrene, 2-ethyl-4-benzylstyrene, 3,5-diphenylstyrene, 2,3,4,5-tetraethylstyrene, 3-ethyl-1-vinylnaphthalene, 6-isopropyl-1-vinylnaphthalene, 6-cyclohexyl-1-vinylnaphthalene, 7-dodecyl-2-vinylnaphthalene, α-methylstyrene, and the like.

[0024] In one embodiment, the monomers used to synthesize the copolymer include 1,3-butadiene and styrene. The copolymers are generally prepared by solution polymerization utilizing inert organic solvents such as aliphatic saturated hydrocarbons, aromatic hydrocarbons, or ethers. The solvents used in such solution polymerizations will usually contain from about 4 to about 10 carbon atoms per molecule and will be liquid under the conditions of the polymerization. Some representative examples of suitable organic solvents include pentane, isooctane, cyclohexane, normal hexane, benzene, toluene, xylene, ethylbenzene, tetrahydrofuran, and the like, either alone or in admixture. For example, the solvent may be a mixture of different hexane isomers. Such solution polymerizations result in the formation of a polymer cement (a highly viscous solution of the polymer).

[0025]

[0020] The functionalized elastomers can be produced using either batch or continuous anionic polymerization processes. The polymerization medium may contain modifiers such as tetramethylethylenediamine (TMEDA), sodium mentholate (SMT), ditetrahydrofurfurylpropane (DTP), tetrahydrofuran (THF), polyethers, or combinations thereof. Branching agents such as divinylbenzene, silicon tetrachloride, etc., may also be used during the polymerization.

[0026] After the polymerization reaction is complete, it will usually be desirable to "kill" any remaining living polydiene chains. This can be accomplished by adding water, an organic acid, or an alcohol such as methanol or ethanol to the polymer cement after the functionalization reaction is complete to remove any living polymer. The block copolymer can then be recovered from the solution using standard techniques.

[0027] The functionalized elastomer may be compounded into a rubber composition. The rubber composition may contain the elastomer comprising the block copolymer alone or may contain the block copolymer together with additional elastomers as described below. Generally, in compositions comprising the block copolymer and additional elastomers, the rubber composition may contain 95 to 5 phr of the block copolymer, and optionally 5 to 95 phr of the additional elastomer.

[0028]

[0023] The rubber composition may optionally contain, in addition to the functional polymer, one or more rubbers or elastomers containing olefinic unsaturation. The phrase "rubber or elastomer containing olefinic unsaturation" or "diene-based elastomer" is intended to include natural rubber and its various virgin and recycled forms, as well as various synthetic rubbers. In describing this invention, the terms "rubber" and "elastomer" may be used interchangeably unless otherwise specified. The terms "rubber composition," "compounded rubber," and "rubber compound" are used interchangeably to refer to rubber compounded or mixed with various ingredients and materials, such terms being well known to those skilled in the art of rubber mixing or compounding. Representative synthetic polymers are butadiene and its homologs and derivatives, such as the homopolymerization products of methylbutadiene, dimethylbutadiene, and pentadiene, as well as copolymers such as copolymers formed from butadiene or its homologs or derivatives with other unsaturated monomers. Among the latter are acetylenes, such as vinyl acetylene; olefins, such as isobutylene, which copolymerizes with isoprene to form butyl rubber; vinyl compounds, such as acrylic acid, acrylonitrile (which polymerizes with butadiene to form NBR), methacrylic acid, and styrene, the latter compound polymerizing with butadiene to form SBR, as well as vinyl esters and various unsaturated aldehydes, ketones, and ethers, such as acrolein, methyl isopropenyl ketone, and vinyl ethyl ether. Specific examples of synthetic rubbers include neoprene (polychloroprene), polybutadiene (including cis 1,4 polybutadiene), polyisoprene (including cis 1,4 polyisoprene), butyl rubber, halobutyl rubber such as chlorobutyl rubber or bromobutyl rubber, styrene / isoprene / butadiene rubber, copolymers of 1,3-butadiene or isoprene with monomers such as styrene, acrylonitrile, and methyl methacrylate, and ethylene / propylene terpolymers, also known as ethylene / propylene / diene monomer (EPDM), particularly ethylene / propylene / dicyclopentadiene terpolymer.Additional examples of rubbers that may be used include alkoxy-silyl end-functionalized solution polymerized polymers (SBR, PBR, IBR, and SIBR), silicon-coupled and tin-coupled star-branched polymers. Preferred rubbers or elastomers are polyisoprene (natural or synthetic), polybutadiene, and SBR.

[0029] In one embodiment, the at least one additional rubber is preferably a combination of at least two diene-based rubbers, such as cis 1,4-polyisoprene rubber (natural or synthetic, but preferably natural), 3,4-polyisoprene rubber, styrene / isoprene / butadiene rubber, emulsion and solution polymerization derived styrene / butadiene rubber, cis 1,4-polybutadiene rubber, and emulsion polymerization modified butadiene / acrylonitrile copolymer.

[0030] In one embodiment of the invention, emulsion polymerization-derived styrene / butadiene (E-SBR) may be used having a relatively conventional styrene content of from about 20 to about 28 percent bound styrene, or, for some applications, E-SBR having a moderate to relatively high bound styrene content, i.e., from about 30 to about 45 percent bound styrene.

[0031] By emulsion polymerization prepared E-SBR is meant that styrene and 1,3-butadiene are copolymerized as an aqueous emulsion, as is well known to those skilled in the art. The bound styrene content may vary, for example, from about 5 to about 50 percent. In one embodiment, the E-SBR may also contain acrylonitrile, for example, in an amount of from about 2 to about 30 weight percent bound acrylonitrile in the terpolymer, to form a terpolymer rubber as an E-SBAR.

[0032] Emulsion polymerization prepared styrene / butadiene / acrylonitrile copolymer rubbers containing from about 2 to about 40 weight percent bound acrylonitrile in the copolymer are also contemplated as diene based rubbers for use in this invention.

[0033] Solution polymerization prepared SBR (S-SBR) typically has a bound styrene content ranging from about 5 to about 50, preferably from about 9 to about 36 percent. S-SBR can be conveniently prepared, for example, by organolithium catalysis in the presence of an organic hydrocarbon solvent.

[0034] In one embodiment, cis 1,4-polybutadiene rubber (BR) can be used. Such BR can be prepared, for example, by organic solution polymerization of 1,3-butadiene. The BR can be conveniently characterized, for example, as having a cis 1,4-content of at least 90 percent.

[0035]

[0030] cis 1,4-polyisoprene and cis 1,4-polyisoprene natural rubber are well known to those skilled in the rubber art.

[0031] As used herein, the term "phr" refers, in accordance with conventional practice, to "parts by weight of a respective material per 100 parts by weight of rubber or elastomer."

[0036] The rubber composition may also contain up to 70 phr of processing oil. The processing oil may be included in the rubber composition as an extender oil typically used to extend the elastomer. The processing oil may also be included in the rubber composition by adding the oil directly during rubber compounding. The processing oil used may include both the extender oil present in the elastomer and the processing oil added during compounding. Suitable processing oils include various oils as known in the art, including aromatic, paraffinic, naphthenic, vegetable, and low PCA oils, such as MES, TDAE, SRAE, and heavy naphthenic oils. Suitable low PCA oils include those having a polycyclic aromatic content of less than 3 weight percent as measured by the method of IP346. The procedures for the IP346 method can be found in Standard Methods for Analysis & Testing of Petroleum and Related Products and British Standard 2000 Parts, 62nd Edition, 2003, published by the Institute of Petroleum, United Kingdom.

[0037] The rubber composition may contain silica, carbon black, or a combination of silica and carbon black. The rubber composition may contain from about 1 to about 150 phr of silica. In another embodiment, from 10 to 100 phr of silica may be used.

[0038]

[0035] Commonly employed siliceous pigments that may be used in the rubber compounds include conventional calcined and precipitated siliceous pigments (silica). In one embodiment, precipitated silicas are used. Conventional siliceous pigments employed in the present invention are precipitated silicas such as those obtained by the acidification of soluble silicates (e.g., sodium silicate).

[0039] Such conventional silicas may be characterized as having a BET surface area, for example, as measured using nitrogen gas. In one embodiment, the BET surface area may be in the range of about 40 to about 600 square meters per gram. In another embodiment, the BET surface area may be in the range of about 80 to about 300 square meters per gram. The BET method for measuring surface area is described in the Journal of the American Chemical Society, Vol. 60, p. 304 (1930).

[0040]

[0037] Conventional silicas may also be characterized as having a dibutyl phthalate (DBP) absorption value ranging from about 100 to about 400, alternatively from about 150 to about 300.

[0038] Conventional silica is expected to have an average particle size in the range of 0.01 to 0.05 microns as measured, for example, by electron microscopy, although silica particles may be smaller or even larger in size.

[0041]

[0039] By way of example only and not by way of limitation herein, various commercially available silicas may be used, such as those commercially available from PPG Industries under the Hi-Sil trademark, such as those designated 210, 243, etc.; those available from Rhodia, such as those designated Z1165MP and Z165GR, and those available from Degussa AG, such as those designated VN2 and VN3. Silicas that have been pretreated and prereacted with organosilanes, such as PPG's Agilon 400, etc., may also be used.

[0042]

[0040] Carbon black, as commonly employed, may be used in combination with the silica as a conventional filler in an amount ranging from 1 to 150 phr. In another embodiment, 10 to 100 phr of carbon black may be used. Although carbon black may be used with silica, in one embodiment, essentially no carbon black is used except in an amount required to impart a black color to the tire, which is 1 to 10 phr. Representative examples of such carbon blacks include N110, N121, N134, N220, N231, N234, N242, N293, N299, N315, N326, N330, N332, N339, N343, N347, N351, N358, N375, N539, N550, N582, N630, N642, N650, N683, N754, N762, N765, N774, N787, N907, N908, N990, and N991. These carbon blacks have iodine absorptions ranging from 9 to 145 g / kg, and DBP numbers ranging from 34 to 150 cm3 / 100 g.

[0043]

[0041] A combination of silica and carbon black may be used in the composition. In one embodiment, the weight ratio of silica to carbon black is 1 or greater. Other fillers may be used in the rubber composition, including particulate fillers including, but not limited to, ultra-high molecular weight polyethylene (UHMWPE), crosslinked particulate polymer gels including, but not limited to, those disclosed in U.S. Patent No. 6,242,534; U.S. Patent No. 6,207,757; U.S. Patent No. 6,133,364; U.S. Patent No. 6,372,857; U.S. Patent No. 5,395,891; or U.S. Patent No. 6,127,488, and plasticized starch composite fillers including, but not limited to, those disclosed in U.S. Patent No. 5,672,639. Such other fillers may be used in amounts ranging from 1 to 30 phr.

[0044] In one embodiment, the rubber composition may contain a conventional sulfur-containing organosilicon compound. In one embodiment, the sulfur-containing organosilicon compound is 3,3'-bis(trimethoxy or triethoxysilylpropyl) polysulfide. In one embodiment, the sulfur-containing organosilicon compound is 3,3'-bis(triethoxysilylpropyl) disulfide and / or 3,3'-bis(triethoxysilylpropyl) tetrasulfide.

[0045] In another embodiment, suitable sulfur-containing organosilicon compounds include those disclosed in U.S. Patent No. 6,608,125. In one embodiment, the sulfur-containing organosilicon compound includes 3-(octanoylthio)-1-propyltriethoxysilane, CH3(CH2)6C(=O)-S-CH2CH2CH2Si(OCH2CH3)3, commercially available as NXT from Momentive Performance Materials.

[0046] In another embodiment, suitable sulfur-containing organosilicon compounds include those disclosed in US Patent Application Publication No. 2003 / 0130535. In one embodiment, the sulfur-containing organosilicon compound is Si-363 from Degussa.

[0047] The amount of the sulfur-containing organosilicon compound in the rubber composition will vary depending on the concentration of other additives used. Generally, the amount of the compound will range from 0.5 to 20 phr. In one embodiment, the amount will range from 1 to 10 phr.

[0048] It will be readily understood by those skilled in the art that the rubber composition will be compounded by methods generally known in the art of rubber compounding, such as mixing the various sulfur vulcanizable constituent rubbers with various commonly used additive materials, such as sulfur donors and curing aids, activators and retarders, and processing additives, such as oils, resins including tackifying resins, and plasticizers, fillers, pigments, fatty acids, zinc oxide, waxes, antioxidants and antiozonants, and peptizers. Depending on the intended use of the sulfur vulcanizable and sulfur vulcanized materials (rubbers), as known to those skilled in the art, the above additives are selected and conventional amounts are generally used. Representative examples of sulfur donors include elemental sulfur (free sulfur), amine disulfides, polymeric polysulfides, and sulfur olefin adducts. In one embodiment, the sulfur vulcanizing agent is elemental sulfur. The sulfur vulcanizing agent may be used in an amount ranging from 0.5 to 8 phr, alternatively from 1.5 to 6 phr. Typical amounts of tackifying resins, if used, include from about 0.5 to about 10 phr, usually from about 1 to about 5 phr. Typical amounts of processing aids include from about 1 to about 50 phr. Typical amounts of antioxidants include from about 1 to about 5 phr. Representative antioxidants may be, for example, diphenyl-p-phenylenediamines, such as those disclosed in The Vanderbilt Rubber Handbook (1978), pages 344-346. Typical amounts of antiozonants include from about 1 to 5 phr. Typical amounts of fatty acids, including stearic acid, if used, include from about 0.5 to about 3 phr. Typical amounts of zinc oxide include from about 2 to about 5 phr. Typical amounts of waxes include from about 1 to about 5 phr. Microcrystalline waxes are often used. Typical amounts of peptizers include from about 0.1 to about 1 phr. Exemplary peptizers may be, for example, pentachlorothiophenol and dibenzamidodiphenyl disulfide.

[0049] Accelerators are used to control the time and / or temperature required for vulcanization and to improve the properties of the vulcanizate. In one embodiment, a single accelerator system may be used, i.e., a primary accelerator. The primary accelerator may be used in a total amount ranging from about 0.5 to about 4, alternatively from about 0.8 to about 1.5 phr. In another embodiment, a combination of primary and secondary accelerators may be used, with the secondary accelerator being used in a lower amount, for example, from about 0.05 to about 3 phr, to activate and improve the properties of the vulcanizate. These accelerator combinations are expected to produce a synergistic effect on the final properties, somewhat better than those produced by the use of either accelerator alone. In addition, delayed action accelerators may be used that are not affected by standard processing temperatures but produce a satisfactory cure at normal vulcanization temperatures. Vulcanization retarders may also be used. Suitable types of accelerators that may be used in the present invention are amines, disulfides, guanidines, thioureas, thiazoles, thiurams, sulfenamides, dithiocarbamates, xanthates. In one embodiment, the primary accelerator is a sulfenamide. If a second accelerator is used, the secondary accelerator may be a guanidine, dithiocarbamate, or thiuram compound.

[0050] The step of mixing the rubber composition can be accomplished by methods known to those skilled in the art of rubber mixing. For example, the components are typically mixed in at least two stages, namely, at least one non-productive stage followed by a productive mix stage. The final curatives, including sulfur vulcanizing agents, are typically mixed in a final stage, conventionally referred to as the "productive" mix stage, where mixing typically occurs at a temperature or extreme temperature lower than the mixing temperature of the previous non-productive mix stage. The terms "non-productive" and "productive" mix stages are well known to those skilled in the art of rubber mixing. The rubber composition may be subjected to a thermodynamic mixing step. The thermodynamic mixing step generally involves machining in a mixer or extruder for a suitable time to produce a rubber temperature between 140°C and 190°C. The suitable duration of the thermal mechanical working varies depending on the process conditions and the volume and nature of the components. For example, the thermal mechanical working may be from 1 to 20 minutes.

[0051]

[0050] The rubber composition may be incorporated into various rubber components of a tire. For example, the rubber component may be a tread (including a tread cap and a tread base), a sidewall, an apex, a chafer, a sidewall insert, a wire coat, or an innerliner. In one embodiment, the component is a tread.

[0052] The pneumatic tire of the present invention may be a race tire, a passenger tire, an aircraft tire, an agricultural tire, an earthmoving tire, an off-road tire, a truck tire, etc. In one embodiment, the tire is a passenger tire or a truck tire. The tire may also be a radial or a bias.

[0053]

[0052] Vulcanization of the pneumatic tires of this invention is generally carried out at conventional temperatures ranging from about 100°C to 200°C. In one embodiment, vulcanization is carried out at a temperature ranging from about 110°C to 180°C. Any of the conventional vulcanization processes may be used, such as heating with superheated steam or hot air, heating in a press or mold, etc. Such tires can be built, formed, shaped and cured by a variety of methods which are known and will be readily apparent to those skilled in such art.

[0054] The present invention is illustrated by the following examples which are merely illustrative and are not to be construed as limiting the scope of the invention or the manner in which it may be practiced. Unless specifically indicated otherwise, parts and percentages are given by weight. EXAMPLES

[0055] This example illustrates the synthesis of a monomer of formula 1. The monomer was synthesized according to the following scheme:

[0056] [ka]

[0057] It was produced using. EXAMPLES

[0058] This example illustrates the synthesis of a functionalized elastomer via a functionalized initiator. The comonomer of Example 1 was reacted with nBuLi (1:1) to produce the in situ initiator. TMEDA (360 uL) was added to nBuLi (0.5 mL, 1.6 M in hexane) and preheated to 65° C. A solution of comonomer 1 (0.5 mL, 1.6 M in hexane) was added quickly and the solution was heat aged at 65° C. for 5 minutes. An aliquot (240 uL, approximately 0.59 M active Li) was added to a solution of butadiene (12.6 wt %) in hexane (115.00 g) and the polymerization was heated to 65° C. for 1 hour and terminated with a solution of BHT in 2-propanol. The cement was pan-dried and the polymer yield was 96% by weight. GPC analysis showed the polymer to have Mn=150,000 / Mw=176,000 g / mol (PDI=1.17). [Embodiment of the invention] 1. Alkyllithium compounds and compounds of formula 1

[0059] [ka]

[0060] (wherein R1=alkyl(C1-C8), aryl, substituted aryl, or -SiR3, where R3 is independently C1-C8 alkyl, preferably -SiMe3, where Me is methyl or -Si(CH3)2C(CH3)3; R2=C1-C8 alkyl, aryl, or substituted aryl, or -SiR3, preferably -CH3; and n=0-3). 1. A functionalized polymerization initiator comprising the reaction product of 2. The compound of formula 1 is a compound of formula 2

[0061] [ka]

[0062] (wherein R is a C1-C3 alkyl group or a trimethylsilyl group). 2. The functionalized polymerization initiator according to 1, 3. The functionalized polymerization initiator according to 1, wherein the alkyl lithium compound is selected from the group consisting of n-butyl lithium, sec-butyl lithium, n-hexyl lithium, n-octyl lithium, tert octyl lithium, n-decyl lithium, phenyl lithium, 1-naphthyl lithium, 4-butylphenyl lithium, p-tolyl lithium, 4-phenylbutyl lithium, cyclohexyl lithium, 4-butylcyclohexyl lithium, and 4-cyclohexylbutyl lithium. 4. A method for making a functionalized polymerization initiator comprising reacting an alkyllithium compound in a hydrocarbon solvent with a compound of formula 1.

[0063] [ka]

[0064] (wherein R1=alkyl(C1-C8), aryl, substituted aryl, or -SiR3, where R3 is independently C1-C8 alkyl, preferably -SiMe3, where Me is methyl or -Si(CH3)2C(CH3)3; R2=C1-C8 alkyl, aryl, or substituted aryl, or -SiR3, preferably -CH3; and n=0-3). The method comprises the step of reacting with 5. The compound of formula 1 is a compound of formula 2

[0065] [ka]

[0066] (wherein R is a C1-C3 alkyl group or a trimethylsilyl group). 5. The method according to claim 4, 6. The method of claim 4, wherein the alkyllithium compound is selected from the group consisting of n-butyllithium, sec-butyllithium, n-hexyllithium, n-octyllithium, tertoctyllithium, n-decyllithium, phenyllithium, 1-naphthyllithium, 4-butylphenyllithium, p-tolyllithium, 4-phenylbutyllithium, cyclohexyllithium, 4-butylcyclohexyllithium, and 4-cyclohexylbutyllithium. 7. A method of making a functionalized elastomer, comprising polymerizing at least one conjugated diene monomer and optionally an aromatic vinyl monomer in the presence of a functionalized polymerization initiator, the functionalized polymerization initiator being selected from the group consisting of an alkyl lithium compound and a compound of formula 1.

[0067] [ka]

[0068] (wherein R1=alkyl(C1-C8), aryl, substituted aryl, or -SiR3, R3 is independently C1-C8 alkyl, preferably -SiMe3, and Me is methyl or -Si(CH3)2C(CH3)3; R2=C1-C8 alkyl, aryl, or substituted aryl, or -SiR3, preferably -CH3; and n=0-3). The method of claim 1, further comprising the reaction product of 8. The compound of formula 1 is a compound of formula 2

[0069] [ka]

[0070] (wherein R is a C1-C3 alkyl group or a trimethylsilyl group). 8. The method according to claim 7, 9. The method of claim 7, wherein prior to the step of polymerizing, the reaction product of the alkyllithium compound and the compound of formula 1 is formed by reacting the alkyllithium compound with the compound of formula 1 in a hydrocarbon solvent. 10. The method of claim 9, further comprising the step of adding at least one diene monomer, and optionally an aromatic vinyl monomer, after the step of forming the reaction product of the alkyllithium compound and the compound of formula 1. 11. The method of claim 7, wherein the conjugated diene monomer is selected from the group consisting of 1,3-butadiene, isoprene, 1,3-pentadiene, 2,3-dimethyl-1,3-butadiene, 2-methyl-1,3-pentadiene, 2,3-dimethyl-1,3-pentadiene, 2-phenyl-1,3-butadiene, and 4,5-diethyl-1,3-octadiene. 12. The method of claim 7, wherein the vinyl aromatic monomer is selected from the group consisting of styrene, 1-vinylnaphthalene, 3-methylstyrene, 3,5-diethylstyrene, 4-propylstyrene, 2,4,6-trimethylstyrene, 4-dodecylstyrene, 3-methyl-5-normal-hexylstyrene, 4-phenylstyrene, 2-ethyl-4-benzylstyrene, 3,5-diphenylstyrene, 2,3,4,5-tetraethylstyrene, 3-ethyl-1-vinylnaphthalene, 6-isopropyl-1-vinylnaphthalene, 6-cyclohexyl-1-vinylnaphthalene, 7-dodecyl-2-vinylnaphthalene, and α-methylstyrene. 13. The method of claim 7, wherein the first monomer is 1,3-butadiene. 14. The method of claim 7, wherein the first monomer comprises 1,3-butadiene and styrene. 15. The method of claim 7, wherein the alkyllithium compound is selected from the group consisting of n-butyllithium, sec-butyllithium, n-hexyllithium, n-octyllithium, tertoctyllithium, n-decyllithium, phenyllithium, 1-naphthyllithium, 4-butylphenyllithium, p-tolyllithium, 4-phenylbutyllithium, cyclohexyllithium, 4-butylcyclohexyllithium, and 4-cyclohexylbutyllithium. 16. A functionalized elastomer made by the method described in 7.

Claims

1. Alkyllithium Compounds and Compounds of Formula 1 【Chemistry 1】 (In the formula, R 1 = alkyl (C1-C8), aryl, or -SiR 3 (In the formula, R 3 is independently C1-C8 alkyl; R 2 =C1 to C8 alkyl, aryl, or -SiR 3 and n=0 to 3.

1. A functionalized polymerization initiator, characterized in that it is the reaction product of:

2. The functionalized polymerization initiator of claim 1, wherein --SiR 3 is SiMe 3 , where Me is methyl, or --Si(CH 3 ) 2 C(CH 3 ) 3 .

3. The functionalized polymerization initiator of claim 1, wherein R 2 is --CH 3 .

4. The compound of formula 1 is a compound of formula 2 【Chemistry 2】 (wherein R is a C1-C3 alkyl group or a trimethylsilyl group).

2. The functionalized polymerization initiator of claim 1, wherein

5. 2. The functionalized polymerization initiator of claim 1, wherein the alkyl lithium compound is selected from the group consisting of n-butyl lithium, sec-butyl lithium, n-hexyl lithium, n-octyl lithium, tert-octyl lithium, n-decyl lithium, phenyl lithium, 1-naphthyl lithium, 4-butylphenyl lithium, p-tolyl lithium, 4-phenylbutyl lithium, cyclohexyl lithium, 4-butylcyclohexyl lithium, and 4-cyclohexylbutyl lithium.

6. A method for making a functionalized polymerization initiator comprising reacting an alkyllithium compound in a hydrocarbon solvent with a compound of formula 1 【Chemistry 3】 (In the formula, R 1 = alkyl (C1-C8), aryl, or -SiR 3 (In the formula, R 3 is independently C1-C8 alkyl; R 2 =C1 to C8 alkyl, aryl, or -SiR 3 and n=0 to 3. The method of claim 1, further comprising the step of reacting 7. The method of claim 6, wherein --SiR.sub.3 is SiMe.sub.3 (wherein Me is methyl) or --Si(CH.sub.3).sub.2C(CH.sub.3).sub.

3.

8. The method according to claim 6 or 7, wherein R 2 is -CH 3 .

9. A method of making a functionalized elastomer, comprising the step of polymerizing at least one conjugated diene monomer and, optionally, an aromatic vinyl monomer in the presence of a functionalized polymerization initiator, the functionalized polymerization initiator being selected from the group consisting of an alkyl lithium compound and a compound of formula 1: 【Chemistry 4】 (In the formula, R 1 = alkyl (C1-C8), aryl, or -SiR 3 (In the formula, R 3 is independently C1-C8 alkyl; R 2 =C1 to C8 alkyl, aryl, or -SiR 3 and n=0 to 3. The method of claim 1, further comprising the reaction product of 10. The method of claim 9, wherein --SiR.sub.3 is SiMe.sub.3 (wherein Me is methyl) or --Si(CH.sub.3).sub.2C(CH.sub.3).sub.

3.

11. The method according to claim 9 or 10, wherein R 2 is -CH 3 .

Citation Information

Patent Citations

  • Crosslinker and chain extender for vulcanizing or crosslinking polymer at room temperature

    JP1992338396A

  • Olefinic and acetylenic azasilacyclopentane and preparation thereof

    JP1993059072A

  • Aminosilane initiators and functionalized polymers using the same

    JP2014507405A

  • Vinylsilanes for use in elastomeric functionalized polymers

    JP2016540730A

  • Modified butadiene polymer and rubber composition

    JP2018188598A