Beta-phase titanium and tungsten alloy
A beta titanium alloy with controlled tungsten content and equiaxed grain structure addresses segregation issues, achieving high strength and ductility for medical applications by leveraging stress-induced martensitic transformation, enhancing mechanical performance for implantable devices.
Patent Information
- Application Number
- JP2020567043
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-05-28
- Filing Date
- 2019-05-27
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2039-05-27
AI Technical Summary
Existing titanium alloys containing tungsten face challenges such as segregation issues and non-uniform mechanical properties due to the large density and melting point differences between titanium and tungsten, which affect biocompatibility and mechanical performance, making them unsuitable for medical applications requiring high strength and ductility.
A beta titanium alloy with a composition of 15% to 40% by weight tungsten and the balance titanium, featuring an equiaxed beta grain structure of 70% to 100% by volume, is developed through a specific manufacturing process involving high-temperature melting, controlled cooling, and heat treatment to achieve high strength and ductility, utilizing stress-induced martensitic transformation for enhanced mechanical properties.
The alloy exhibits high strength, uniform ductility, and strain transformation effects, suitable for medical applications by avoiding necking and improving mechanical properties, making it suitable for implantable medical devices.
Smart Images

Figure 0007561035000008 
Figure 0007561035000009 
Figure 0007561035000001
Abstract
Description
[Technical field]
[0001] This application claims the benefit of European Patent Application Publication No. 18382365.7, filed May 28, 2018.
[0002] The present invention relates to a tungsten-containing titanium alloy. In particular, it relates to a novel beta titanium alloy containing 15% to 40% by weight tungsten and the remainder up to 100% by weight titanium, the alloy containing 70% to 100% by volume of an equiaxed beta grain structure. The present invention also relates to an implantable medical device made of the tungsten-containing beta titanium alloy. [Background technology]
[0003] Titanium (Ti) has long been used in dentistry and medicine for implant purposes. Over the years, commercially pure Ti was used as well as several alloys, such as binary and ternary Ti alloys. Many metallic elements have been explored to create novel titanium alloys for medical use. Important criteria for selecting elements for alloys are to have high strength and high ductility. These properties can be achieved by using beta (β) phase titanium alloys. The beta phase of titanium or titania refers to one of the two allotropes of titanium with a body-centered cubic lattice structure that is typically found at high temperatures. The beta phase confers a lower modulus of elasticity and better fatigue resistance compared to the alpha (α) phase, which is typically found in titanium at low temperatures.
[0004] To stabilize the beta phase at low temperatures, "beta stabilizing" alloying elements can be added, including niobium (Nb), molybdenum (Mo), tantalum (Ta), vanadium (V), chromium (Cr), manganese (Mn), cobalt (Co), nickel (Ni), and copper (Cu), zirconium (Zr) or tin (Sn). However, these alloys have a major drawback, which is the biocompatibility of the alloying elements.
[0005] Highly ductile, high strength biocompatible alloys are desired for medical applications such as orthopedic implants and critical medical devices. Good ductility is desired both to be formable (soft) enough to be produced into final shapes by metal working, and to have sufficient fracture resistance to deformation for medical applications.
[0006] Other biocompatible titanium alloying elements, including tungsten among others, have been disclosed in the state of the art. Titanium alloys containing tungsten have excellent wear resistance. However, tungsten is a heavy metal element that causes serious segregation problems when incorporated into industrial ingot melting techniques. Indeed, the combination of the large difference in density between titanium and tungsten and the mismatch in their melting points leads to inhomogeneous alloys that impair the mechanical properties of the resulting alloy.
[0007] Therefore, there is a need to develop new titanium alloys containing tungsten that have advanced mechanical properties for use in the medical field. Summary of the Invention
[0008] The present inventors have discovered a beta titanium and tungsten alloy having 70% to 100% by volume equiaxed beta grain structure that is a metastable alloy with high strength and high uniform ductility. In particular, the alloy of the present invention has properties suitable for use in medical applications, for example, as implantable medical devices.
[0009] Furthermore, the inventors have found that the beta titanium alloys of the present invention are "strain-transformable" alloys that exhibit strain transformation effects when the beta phase is metastable (i.e., quenched from the beta region T near the beta transformation temperature). Without being bound by any theory, it is believed that the deformation mechanisms of the strain transformation effects can be characterized by stress-induced martensitic transformation (SIM), mechanical twinning, and dislocation slip. These mechanisms can be triggered simultaneously during mechanical deformation. The strain transformation effects of the alloys of the present invention are advantageous because they allow the dynamic strain hardening effects associated with the formation of martensite and / or twinning to strengthen the material as a function of plastic deformation, avoiding strain localization (i.e., necking) at the early stages of plastic flow and improving uniform ductility.
[0010] Thus, a first aspect of the present invention relates to a beta titanium alloy comprising 15% to 40% by weight tungsten and balance up to 100% by weight titanium, the alloy comprising 70% to 100% by volume equiaxed beta grain structure, in particular a beta titanium alloy comprising 15% to 28% by weight tungsten and balance up to 100% by weight titanium, the alloy comprising 70% to 100% by volume equiaxed beta grain structure.
[0011] The second aspect of the present invention relates to a method for producing the beta titanium alloy of the first aspect of the present invention, which includes the steps of: (a) high temperature melting of all elements used as raw materials under a protective atmosphere at a temperature between 3000°C and 3500°C; (b) cooling the melted material obtained in step (a) to room temperature to obtain an ingot; (c) heat treating the ingot obtained in step (b) at a temperature calculated by the following formula: Tbeta ± 100°C; (d) quenching the alloy obtained in step (c) to room temperature; (e) machining the alloy obtained in step (d) to obtain a processed alloy; (f) heat treating the processed alloy obtained in step (e) at a temperature calculated by the following formula: Tbeta ± 100°C; and (g) quenching the processed alloy obtained in step (f), where Tbeta is as defined below.
[0012] A third aspect of the present invention also relates to an implantable medical device made from the beta-titanium alloy defined in the first aspect of the present invention. [Brief description of the drawings]
[0013] [Figure 1] 1 shows optical microscope (OM) images of the microstructure of titanium tungsten alloy 1 of the present invention. Section A shows the OM image of alloy 1 with 100 vol. % beta phase at the end of heat treatment and machining, and section B shows the OM image of alloy 1 with about 82.4 vol. % beta phase, which is transformed into mechanical twins (62.0 vol. %) and martensite (20.4 vol. %) after deformation during tensile testing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] All terms used herein in this application are to be understood in their ordinary sense as known in the art, unless otherwise specified. Other, more specific definitions of certain terms used in this application are set forth below, and are intended to be applied equally throughout the specification and claims, unless another clearly defined definition gives a broader definition.
[0015] For purposes of the present invention, any range given includes both the lower and upper endpoints of the range. Unless otherwise specified, ranges specified, such as temperatures, times, percentages of ingredients, etc., should be considered as approximations.
[0016] The term "alloy" refers to a solid solution or liquid mixture of a metal and a second material, which may be a metal, a non-metal, or another alloy.
[0017] For purposes of the present invention, the term "solid solution" refers to a solid form of a solution. The term "solution" refers to a solid form of a solution that is composed of two or more substances. Homogeneous mixture In such a mixture, solute teeth solvent An alloy is a substance dissolved in another substance known as a solute. The solvent is the larger fraction of the mixture (i.e. titanium) and the remaining components present in the solution are called solutes. In particular, the solvent can be a gas, liquid, or solid. If the solvent is a solid, the solution is a solid solution that can dissolve gases, liquids, and other solids. Thus, the term "alloy" is meant to refer to a solid in a homogeneous mixture of solids. The method for producing a solid solution involves mixing the components in liquid form followed by subsequent solidification of the resulting mixture.
[0018] The terms "balance amount" and "balanced amount" have the same meaning and are used interchangeably. They refer to a sufficient amount of titanium needed to achieve 100% by weight of the composition.
[0019] The term "metastable" refers to a quasi-equilibrium state of titanium that has a higher free energy than the true equilibrium state, meaning that the alloy can accommodate flow stresses and strains not only by dislocation glide but also by mechanical twinning and activation of the martensite phase.
[0020] The "beta phase" of titanium or a titanium alloy refers to one of the two allotropes of titanium that has a body-centered cubic lattice structure that is thermodynamically stable at high temperatures (882°C for pure titanium).
[0021] The term "weight percent (%)" refers to the percentage of each ingredient of an alloy relative to the total weight.
[0022] The terms "volume percent (%)" or "volume / volume %" or "v / v%" or "vol%" have the same meaning and are used interchangeably. They refer to the volume of equiaxed beta grain structure relative to the total volume of the alloy or to the volume of the beta phase that has undergone mechanical twinning and transformation to martensite after deformation during tensile testing.
[0023] The term "protective" atmosphere refers to any atmosphere that replaces the surrounding air. For purposes of the present invention, a protective atmosphere is a vacuum or an atmosphere containing an inert gas such as argon, nitrogen or helium.
[0024] The term "quenching" refers to rapid cooling in a water-based or oil-based solution.
[0025] The term "room temperature" refers to the temperature of an environment without heating or cooling, and generally includes 20°C to 25°C.
[0026] As stated above, a first aspect of the present invention relates to a beta titanium alloy comprising 15% to 40% by weight tungsten and up to 100% by weight titanium, the alloy comprising 70% to 100% by volume equiaxed beta grain structure. In one embodiment, the beta titanium alloy comprises 15% to 35% by weight tungsten and up to 100% by weight titanium, the alloy comprising 70% to 100% by volume equiaxed beta grain structure. In one embodiment, the beta titanium alloy comprises 15% to 28% by weight tungsten and up to 100% by weight titanium, the alloy comprising 70% to 100% by volume equiaxed beta grain structure. In one embodiment, the beta titanium alloy comprises 18% to 22% by weight tungsten and up to 100% by weight titanium, the alloy comprising 70% to 100% by volume equiaxed beta grain structure. The volume fraction of the beta phase can be measured by several methods known in the art, such as quantitative X-ray diffraction (XRD) and electron backscatter diffraction (EBSD). In the present invention, the volume fraction of the beta phase is measured by a Cu-K α The analysis was performed by an X-ray diffractogram containing three characteristic peaks at 38.9, 56.4, and 70.7±0.3 degrees (2-theta) at λ=1.5406 Å, and the volume fraction of the beta phase was then quantified by the Rietveld method. The Rietveld method is a commonly used method for the post-processing of X-ray diffraction profiles. This method is performed by theoretical simulation of the experimental profile, which provides a quantification of the volume of the alloy that is in the beta phase (see DL Bish et al J. Appl. Cryst. ``Quantitative Phase Analysis Using the Rietveld Method'', 1988, Vol. 21, pp. 86-91).
[0027] In one embodiment, the beta titanium alloy of the present invention consists essentially of 15% to 40% by weight tungsten and the balance up to 100% by weight titanium, the alloy comprising 70% to 100% by volume equiaxed beta grain structure. In one embodiment, the beta titanium alloy of the present invention consists essentially of 15% to 35% by weight tungsten and the balance up to 100% by weight titanium, the alloy comprising 70% to 100% by volume equiaxed beta grain structure. In one embodiment, the beta titanium alloy of the present invention consists essentially of 15% to 28% by weight tungsten and the balance up to 100% by weight titanium, the alloy comprising 70% to 100% by volume equiaxed beta grain structure. In one embodiment, the beta titanium alloy of the present invention consists essentially of 18% to 22% by weight tungsten and the balance up to 100% by weight titanium, the alloy comprising 70% to 100% by volume equiaxed beta grain structure. As used herein, the term "consisting essentially of" refers to the essential elements of an alloy that are intentionally mixed together to form a desired alloy having the desired properties. However, it is understood that small amounts of other elements may be part of the claimed alloy that are not intentionally added but appear in the final alloy. Thus, such elements do not adversely affect the properties of the alloy and may be tolerated. Thus, the presence of such elements in the alloy is considered to be within the scope of the alloy of the present invention.
[0028] In one embodiment, the beta titanium alloy of the present invention comprises 80% to 100% by volume of an equiaxed beta grain structure. In one embodiment, the beta titanium alloy of the present invention comprises 90% to 100% by volume of an equiaxed beta grain structure. In one embodiment, the beta titanium alloy of the present invention comprises 95% to 100% by volume of an equiaxed beta grain structure. In one embodiment, the beta titanium alloy of the present invention comprises 98% to 100% by volume of an equiaxed beta grain structure. In one embodiment, the beta titanium alloy of the present invention comprises 99% to 100% by volume of an equiaxed beta grain structure. In one embodiment, the beta titanium alloy of the present invention comprises 100% by volume of an equiaxed beta grain structure.
[0029] In one embodiment, the beta titanium alloy of the present invention has an equiaxed beta grain structure with each grain having an average diameter of 0.01 μm to 200 μm. In one embodiment, the beta titanium alloy of the present invention has an equiaxed beta grain structure with each grain having an average diameter of 0.01 μm to 180 μm. In one embodiment, the beta titanium alloy of the present invention has an equiaxed beta grain structure with each grain having an average diameter of 0.01 μm to 160 μm. In one embodiment, the beta titanium alloy of the present invention has an equiaxed beta grain structure with each grain having an average diameter of 0.01 μm to 140 μm. In one embodiment, the beta titanium alloy of the present invention has an equiaxed beta grain structure with each grain having an average diameter of 0.5 μm to 120 μm. In one embodiment, the beta titanium alloy of the present invention has an equiaxed beta grain structure with each grain having an average diameter of 2 μm to 90 μm. In one embodiment, the beta titanium alloy of the present invention has an equiaxed beta grain structure with each grain having an average diameter of 5 μm to 70 μm. In one embodiment, the beta titanium alloy of the present invention has an equiaxed beta grain structure with each grain having an average diameter of 8 μm to 60 μm. In one embodiment, the beta titanium alloy of the present invention has an equiaxed beta grain structure with each grain having an average diameter of 10 μm to 50 μm. In one embodiment, the beta titanium alloy of the present invention has an equiaxed beta grain structure with each grain having an average diameter of 12 μm to 40 μm.
[0030] The term "average diameter" refers to the size of the equiaxed beta grains measured in μm. The measurements were carried out by conventional analytical techniques, for example microscopic measurements using a scanning electron microscope (SEM), using suitable equipment. In the present invention, the average diameter was measured according to the Standard Test Methods for Determining Average Grain Size according to ASTM E112.
[0031] In one embodiment, the beta titanium alloy of the present invention comprises 18% to 25% tungsten, and the balance up to 100% titanium, by weight. In one embodiment, the beta titanium alloy of the present invention comprises 20% to 23% tungsten, and the balance up to 100% titanium, by weight. In one embodiment, the beta titanium alloy of the present invention comprises 21% tungsten, and the balance up to 100% titanium, by weight. In one embodiment, the beta titanium alloy of the present invention consists essentially of 21% tungsten, and the balance up to 100% titanium, by weight.
[0032] In one embodiment, the beta titanium alloy of the present invention further comprises at least one metallic element selected from the group consisting of iridium, tantalum, platinum, gold, iron, niobium, zirconium, tin, and molybdenum. In one embodiment, the beta titanium alloy of the present invention consists essentially of 15% to 40% by weight tungsten, at least one metallic element selected from the group consisting of iridium, tantalum, platinum, gold, iron, niobium, zirconium, tin, and molybdenum, and the balance up to 100% by weight titanium. In one embodiment, the beta titanium alloy of the present invention consists essentially of 15% to 35% by weight tungsten, at least one metallic element selected from the group consisting of iridium, tantalum, platinum, gold, iron, niobium, zirconium, tin, and molybdenum, and the balance up to 100% by weight titanium. In one embodiment, the beta titanium alloy of the present invention consists essentially of 15% to 28% by weight tungsten, at least one metallic element selected from the group consisting of iridium, tantalum, platinum, gold, iron, niobium, zirconium, tin, and molybdenum, with the balance up to 100% by weight titanium. In one embodiment, the beta titanium alloy of the present invention consists essentially of 18% to 22% by weight tungsten, at least one metallic element selected from the group consisting of iridium, tantalum, platinum, gold, iron, niobium, zirconium, tin, and molybdenum, with the balance up to 100% by weight titanium.
[0033] In one embodiment, the beta titanium alloy of the present invention further comprises at least one metallic element selected from the group consisting of iridium, tantalum, platinum, gold, iron, niobium, zirconium, and tin. In one embodiment, the beta titanium alloy of the present invention consists essentially of 15% to 40% by weight tungsten, at least one metallic element selected from the group consisting of iridium, tantalum, platinum, gold, iron, niobium, zirconium, and tin, and the balance up to 100% by weight titanium. In one embodiment, the beta titanium alloy of the present invention consists essentially of 15% to 35% by weight tungsten, at least one metallic element selected from the group consisting of iridium, tantalum, platinum, gold, iron, niobium, zirconium, and tin, and the balance up to 100% by weight titanium. In one embodiment, the beta titanium alloy of the present invention consists essentially of 15% to 28% by weight tungsten, at least one metallic element selected from the group consisting of iridium, tantalum, platinum, gold, iron, niobium, zirconium, and tin, and the balance up to 100% by weight titanium. In one embodiment, the beta titanium alloy of the present invention consists essentially of 18% to 22% by weight tungsten, at least one metallic element selected from the group consisting of iridium, tantalum, platinum, gold, iron, niobium, zirconium, and tin, and the balance up to 100% by weight titanium. In one embodiment, the beta titanium alloy of the present invention consists essentially of 18% to 22% by weight tungsten, at least one metallic element selected from the group consisting of iridium, tantalum, platinum, gold, iron, niobium, zirconium, and tin, and the balance up to 100% by weight titanium.
[0034] In one embodiment, the beta-titanium alloy of the present invention further comprises iridium.
[0035] In one embodiment, the beta titanium alloy of the present invention further comprises at least one metal element (M) selected from the group consisting of iridium, tantalum, platinum, gold, iron, niobium, zirconium, tin, and molybdenum, the amount of the metal element (Weq wt%) being calculated according to the formula: Weq weight% = tungsten substitution amount (wt.%) / equivalent weightCoefficient (F) During the ceremony, equivalent weight The coefficients are as follows:
[0036] TIFF0007561035000001.tif57170
[0037] In one embodiment, the beta titanium alloy of the present invention further comprises 1 to 9 metallic elements M 1-9 If it contains, the amount of each metal element (y 1-9 ) and the amount of tungsten (x) are calculated by the following formula: Ti-Weq%W=Ti-x%W-y1 / F1%M1-y2 / F2%M2-y3 / F3%M3-y4 / F4%M4-y5 / F5%M5-y6 / F6%M6-y7 / F7%M7-y8 / F8%M8-y9 / F9%M9 During the ceremony, x is greater than 0, Each y 1-9 are independently selected from 0 or greater, [Weq=x+Σ(y1 / F1+y2 / F2+y3 / F3+y4 / F4+y5 / F5+y6 / F6+y7 / F7+y8 / F8+y9 / F9)] includes 15-40, and [x+Σ(y1+y2+y3+y4+y5+y6+y7+y8+y9)] ranges from 4.5 to 49.9 inclusive.
[0038] In one embodiment, the beta titanium alloy of the present invention further comprises at least one metal element (M) selected from the group consisting of iridium, tantalum, platinum, gold, iron, niobium, zirconium, tin, and molybdenum, the amount of the metal element (Weq wt%) being calculated according to the formula: Weq weight% = tungsten substitution amount (wt.%) / equivalent weight Coefficient (F) During the ceremony, equivalent weight The coefficients are as follows:
[0039] TIFF0007561035000002.tif57170
[0040] In one embodiment, the beta titanium alloy of the present invention further comprises 1 to 9 metallic elements M 1-9 If it contains, the amount of each metal element (y 1-9 ) and the amount of tungsten (x) are calculated by the following formula: Ti-Weq%W=Ti-x%W-y1 / F1%M1-y2 / F2%M2-y3 / F3%M3-y4 / F4%M4-y5 / F5%M5-y6 / F6%M6-y7 / F7%M7-y8 / F8%M8-y9 / F9%M9 During the ceremony, x is greater than 0, Each y 1-9 are independently selected from 0 or greater, [Weq=x+Σ(y1 / F1+y2 / F2+y3 / F3+y4 / F4+y5 / F5+y6 / F6+y7 / F7+y8 / F8+y9 / F9)] includes 15-40, and [x+Σ(y1+y2+y3+y4+y5+y6+y7+y8+y9)] ranges from 4.55 to 49.9 inclusive.
[0041] In one embodiment, [x+Σ(y1 / F1+y2 / F2+y3 / F3+y4 / F4+y5 / F5+y6 / F6+y7 / F7+y8 / F8+y9 / F9)] is inclusive between 15 and 28, and [x+Σ(y1+y2+y3+y4+y5+y6+y7+y8+y9)] is inclusive between 4.55 and 49.9.
[0042] In one embodiment, the beta titanium alloy of the present invention further comprises at least one metal element (M) selected from the group consisting of iridium, tantalum, platinum, gold, iron, niobium, zirconium, and tin, the amount of the metal element (Weq wt%) being calculated according to the formula: Weq weight% = tungsten substitution amount (wt.%) / equivalent weight Coefficient (F) During the ceremony, equivalent weight The coefficients are as follows:
[0043] TIFF0007561035000003.tif57170
[0044] In one embodiment, the beta titanium alloy of the present invention further comprises 1 to 8 metallic elements M 1-8 If it contains, the amount of each metal element (y 1-8 ) and the amount of tungsten (x) are calculated by the following formula: Ti-Weq%W=Ti-x%W-y1 / F1%M1-y2 / F2%M2-y3 / F3%M3-y4 / F4%M4-y5 / F5%M5-y6 / F6%M6-y7 / F7%M7-y8 / F8%M8 During the ceremony, x is greater than 0, Each y 1-8 are independently selected from 0 or greater, [Weq=x+Σ(y1 / F1+y2 / F2+y3 / F3+y4 / F4+y5 / F5+y6 / F6+y7 / F7+y8 / F8)] includes 15 to 40, and [x+Σ(y1+y2+y3+y4+y5+y6+y7+y8)] ranges from 4.5 to 49.9 inclusive.
[0045] In one embodiment, the beta titanium alloy of the present invention further comprises at least one metal element (M) selected from the group consisting of iridium, tantalum, platinum, gold, iron, niobium, zirconium, and tin, the amount of the metal element (Weq wt%) being calculated according to the formula: Weq weight% = tungsten substitution amount (wt.%) / equivalent weight Coefficient (F) During the ceremony, equivalent weight The coefficients are as follows:
[0046] TIFF0007561035000004.tif52170
[0047] In one embodiment, the beta titanium alloy of the present invention further comprises 1 to 8 metallic elements M 1-8 If it contains, the amount of each metal element (y 1-8 ) and the amount of tungsten (x) are calculated by the following formula: Ti-Weq%W=Ti-x%W-y1 / F1%M1-y2 / F2%M2-y3 / F3%M3-y4 / F4%M4-y5 / F5%M5-y6 / F6%M6-y7 / F7%M7-y8 / F8%M8 During the ceremony, x is greater than 0, Each y 1-8 are independently selected from 0 or greater, [Weq=x+Σ(y1 / F1+y2 / F2+y3 / F3+y4 / F4+y5 / F5+y6 / F6+y7 / F7+y8 / F8)] includes 15 to 40, and [x+Σ(y1+y2+y3+y4+y5+y6+y7+y8)] ranges from 4.55 to 49.9 inclusive.
[0048] In one embodiment, [x+Σ(y1 / F1+y2 / F2+y3 / F3+y4 / F4+y5 / F5+y6 / F6+y7 / F7+y8 / F8)] is inclusive between 15 and 28, and [x+Σ(y1+y2+y3+y4+y5+y6+y7+y8)] is inclusive between 4.55 and 49.9.
[0049] In one embodiment, the beta titanium alloy of the present invention further comprises 2% to 4% by weight of Iridium. In one embodiment, the beta titanium alloy of the present invention further comprises 3% to 4% by weight of Iridium. In one embodiment, the beta titanium alloy of the present invention further comprises 3.6% by weight of Iridium.
[0050] In one embodiment, the beta titanium alloy of the present invention comprises 18% to 40% tungsten, 2% to 4% iridium, and the balance up to 100% titanium by weight. The beta titanium alloy of the present invention comprises 18% to 35% tungsten, 2% to 4% iridium, and the balance up to 100% titanium by weight. In one embodiment, the beta titanium alloy of the present invention comprises 18% to 25% tungsten, 2% to 4% iridium, and the balance up to 100% titanium by weight. In one embodiment, the beta titanium alloy of the present invention comprises 18% to 22% tungsten, 2% to 4% iridium, and the balance up to 100% titanium by weight. In one embodiment, the beta titanium alloy of the present invention comprises 20% to 23% tungsten, 2% to 4% iridium, and the balance up to 100% titanium by weight. In one embodiment, the beta titanium alloy of the present invention comprises, by weight, 21% tungsten, 3.6% iridium, and the balance up to 100% titanium. In one embodiment, the beta titanium alloy of the present invention consists essentially of, by weight, 21% tungsten, 3.6% iridium, and the balance up to 100% titanium.
[0051] In one embodiment, in the beta titanium alloy of the present invention, the alloy has a yield stress of 400 MPa to 1000 MPa. In one embodiment, in the beta titanium alloy of the present invention, the alloy has a yield stress of 550 MPa to 900 MPa. In one embodiment, in the beta titanium alloy of the present invention, the alloy has a yield stress of 600 MPa to 800 MPa. The terms "yield stress", "YS", "yield strength", and "yield point" have the same meaning and are used interchangeably. They refer to the stress at which a material begins to deform plastically, i.e., irreversibly. That is, it is the maximum stress that can be applied without exceeding a specified value of permanent strain. In the present invention, "yield stress" was characterized by uniaxial tensile testing according to ASTM E8 / E8M.
[0052] In one embodiment, in the beta titanium alloy of the present invention, the alloy has an ultimate tensile strength of 650 MPa to 1100 MPa. In one embodiment, in the beta titanium alloy of the present invention, the alloy has an ultimate tensile strength of 700 MPa to 1000 MPa. In one embodiment, in the beta titanium alloy of the present invention, the alloy has an ultimate tensile strength of 730 MPa to 980 MPa. As used herein, the terms "ultimate tensile strength" and "UTS" have the same meaning and are used interchangeably. They refer to the maximum stress a material can withstand before fracture. In the present invention, UTS was measured by uniaxial tensile testing according to ASTM E8 / E8M.
[0053] In one embodiment, in the beta titanium alloy of the present invention, the alloy has an elongation to break of 30% to 65%. In one embodiment, in the beta titanium alloy of the present invention, the alloy has an elongation to break of 35% to 60%. The terms "elongation to break" and "EI" have the same meaning and are used interchangeably. They refer to the elongation reported in a tensile test, i.e., the maximum elongation in the gauge length divided by the original gauge length. In the present invention, EI is measured by the formula (Lu-Lo) / Lo x 100, where Lu represents the gauge length at break and Lo represents the original gauge length according to the European EN10002 standard and ASTM E8M.
[0054] In one embodiment, in the beta titanium alloy of the present invention, the alloy has a Young's modulus of 80 GPa to 140 GPa. In an embodiment, in the beta titanium alloy of the present invention, the alloy has a Young's modulus of 85 GPa to 130 GPa. The terms "Young's modulus" and "elastic modulus" have the same meaning and are used interchangeably. They refer to a measurement of the stiffness of a solid material. It is a mechanical property of linear elastic solid materials. It defines the relationship between stress (force per unit area) and strain (proportional deformation) of a material. In the present invention, it is measured by uniaxial tensile test ASTM E8 / E8M.
[0055] In one embodiment, in the beta titanium alloy of the present invention, the alloy has an average strain hardening rate of 1000 MPa to 2500 MPa. In one embodiment, in the beta titanium alloy of the present invention, the alloy has an average strain hardening rate of 1500 MPa to 2000 MPa. In one embodiment, in the beta titanium alloy of the present invention, the alloy has an average strain hardening rate of 1600 MPa to 1800 MPa. The terms "average strain hardening rate" and "SHR" have the same meaning and are used interchangeably. They refer to the average rate of hardening effect as a function of tensile strain, i.e., average (dσ / dε). In the present invention, it was measured from the true stress (σ)-true strain (ε) curve by uniaxial tensile testing ASTM E8 / E8M.
[0056] In one embodiment, the beta titanium alloy of the present invention has one or more of the following properties: a yield stress of 400 MPa to 1000 MPa; an ultimate tensile strength of 650 MPa to 1100 MPa; an elongation at break of 30% to 65%; and a Young's modulus of 80 GPa to 140 GPa.
[0057] In one embodiment, the beta titanium alloy of the present invention has a yield stress of 400 MPa to 1000 MPa and an ultimate tensile strength of 650 MPa to 1100 MPa. In one embodiment, the beta titanium alloy of the present invention has a yield stress of 400 MPa to 1000 MPa and an elongation to break of 30% to 65%. In one embodiment, the beta titanium alloy of the present invention has a yield stress of 400 MPa to 1000 MPa and a Young's modulus of 80 GPa to 140 GPa. In one embodiment, the beta titanium alloy of the present invention has a ultimate tensile strength of 650 MPa to 1100 MPa and an elongation to break of 30% to 65%. In one embodiment, the beta titanium alloy of the present invention has a beta titanium alloy of 30% to 65% and an elongation to break of 80 GPa to 140 GPa. In one embodiment, the beta titanium alloy of the present invention has an ultimate tensile strength of between 650 MPa and 1100 MPa, and a Young's modulus of between 80 GPa and 140 GPa.
[0058] In one embodiment, the beta titanium alloy of the present invention has an alloy with a yield stress of 400 MPa to 1000 MPa, an ultimate tensile strength of 650 MPa to 1100 MPa, and an elongation to break of 30% to 65%. In one embodiment, the beta titanium alloy of the present invention has an alloy with a yield stress of 400 MPa to 1000 MPa, an ultimate tensile strength of 650 MPa to 1100 MPa, and a Young's modulus of 80 GPa to 140 GPa. In one embodiment, the beta titanium alloy of the present invention has an alloy with a yield stress of 400 MPa to 1000 MPa, an elongation to break of 30% to 65%, and a Young's modulus of 80 GPa to 140 GPa. In one embodiment, the beta titanium alloy of the present invention has an alloy with a yield stress of 400 MPa to 1000 MPa, an ultimate tensile strength of 650 MPa to 1100 MPa, an elongation to break of 30% to 65%, and a Young's modulus of 80 GPa to 140 GPa.
[0059] It is worth noting that the appropriate structural and mechanical characteristics of the titanium-tungsten alloy of the present invention are determined by the chemical composition of the alloy and by the thermomechanical treatment of the mixture of metals forming the alloy. The beta titanium alloy of the present invention can also be defined by its manufacturing method. It can therefore be obtained by a method comprising the following steps: (a) high-temperature melting of all elements used as raw materials under a protective atmosphere at a temperature between 3000°C and 3500°C; (b) cooling the melted material obtained in step (a) to room temperature to obtain an ingot; (c) heat treating the ingot obtained in step (b) at a temperature calculated by the following formula: Tbeta±100°C; (d) quenching the alloy obtained in step (c) to room temperature; (e) machining the alloy obtained in step (d) to obtain a processed alloy; (f) heat treating the processed alloy obtained in step (e) at a temperature calculated by the following formula: Tbeta±100°C; and (g) quenching the processed alloy obtained in step (f). In the formula, Tbeta is calculated by the following formula: Tbeta=825-6.54Weq When the alloy further comprises at least one metallic element (M) selected from the group consisting of iridium, tantalum, platinum, gold, iron, niobium, zirconium, tin and molybdenum, Weq is calculated by the following formula: Ti-Weq%W=Ti-x%W-y1 / F1%M1-y2 / F2%M2-y3 / F3%M3-y4 / F4%M4-y5 / F5%M5-y6 / F6%M6-y7 / F7%M7-y8 / F8%M8-y9 / F9%M9 During the ceremony, Ti is the amount of titanium x is the amount of tungsten and is greater than 0; Each M 1-9 Unlike iridium, tantalum, platinum , gold, iron, niobium, zirconium, tin, and molybdenum; y 1-9 is each metal element M 1-9 is the amount of each y 1-9 are independently selected from 0 or greater, F 1-9 is defined above equivalent weight is the coefficient, [Weq=x+Σ(y1 / F1+y2 / F2+y3 / F3+y4 / F4+y5 / F5+y6 / F6+y7 / F7+y8 / F8+y9 / F9)] includes 15-40, and [x+Σ(y1+y2+y3+y4+y5+y6+y7+y8)] ranges from 4.5 to 49.9, especially 4.55 and 49.9 inclusive.
[0060] Or alternatively, when the alloy further comprises at least one metallic element (M) selected from the group consisting of iridium, tantalum, platinum, gold, iron, niobium, zirconium and tin, Weq is calculated by the following formula: Ti-Weq%W=Ti-x%W-y1 / F1%M1-y2 / F2%M2-y3 / F3%M3-y4 / F4%M4-y5 / F5%M5-y6 / F6%M6-y7 / F7%M7-y8 / F8%M8 During the ceremony, Ti is the amount of titanium x is the amount of tungsten and is greater than 0; Each M 1-8 Unlike iridium, tantalum, platinum , gold, iron, niobium, zirconium and tin; y 1-8 is each metal element M 1-8 is the amount of each y 1-8 are independently selected from 0 or greater, F 1-8 is described in claim 5 equivalent weight is the coefficient, [Weq=x+Σ(y1 / F1+y2 / F2+y3 / F3+y4 / F4+y5 / F5+y6 / F6+y7 / F7+y8 / F8] includes 15-28, and [x+Σ(y1+y2+y3+y4+y5+y6+y7+y8)] ranges from 4.5 to 49.9, especially 4.55 and 49.9 inclusive.
[0061] The term "by obtainable" is used herein to define each particular alloy of the present invention by the process for obtaining it, and refers to a product obtainable by any of the corresponding processes disclosed herein. For the purposes of the present invention, the expressions "obtainable", "obtained" and equivalent expressions are used interchangeably, and in each case the expression "obtainable" encompasses the expression "obtained".
[0062] In one embodiment, the beta titanium alloy of the present invention is obtainable by a method in which the high temperature melting step (a) is achieved by carrying out a method selected from the group consisting of electric arc, induction, plasma and electron beam. In one embodiment, the beta titanium alloy of the present invention is obtainable by a method in which step (a) is carried out by electric arc. As mentioned before, this method allows to obtain a complete melting of all the raw materials. Thus, the ingot obtained after step (b) is a homogeneous solid solution.
[0063] The term "raw material" refers to the materials used to form the alloy of the present invention. Specifically, the raw material is the source of material that provides the components of the alloy. For purposes of the present invention, raw material refers to titanium, tungsten, and metallic elements selected from the group consisting of iridium, tantalum, platinum, gold, iron, niobium, zirconium, tin, and molybdenum. In one embodiment, the beta titanium alloy of the present invention can be obtained by a process in which the raw material is not in powder form. In one embodiment, the beta titanium alloy of the present invention can be obtained by a process in which the raw material is not pulverized or crushed.
[0064] The term "machining" refers to a physical operation that transforms a material into a desired shape. Machining includes both low-temperature and high-temperature machining. Examples of machining suitable for the present invention include bending, cutting, drawing, grinding, hammering, rolling, shaving, twisting, drilling, and extruding, among others. In one embodiment, the beta-titanium alloy of the present invention can be obtained by a method that includes repeating step (e) until the desired processed alloy is obtained.
[0065] In one embodiment, the beta-titanium alloy of the present invention is obtainable by a method in which the machining is selected from the group consisting of rolling, drawing, punching, and extrusion. In one embodiment, the beta-titanium alloy of the present invention is obtainable by machining including extrusion to form bars, wires, tubes, and plates.
[0066] In one embodiment, the beta titanium alloy of the present invention comprises 15% to 40% by weight tungsten and balance up to 100% by weight titanium, the alloy comprises 70% to 100% by volume equiaxed beta grain structure, and the alloy can be obtained by a process in which the heat treatments of steps (c) and (f) are carried out at a temperature of 640° C. to 925° C. In one embodiment, the beta titanium alloy of the present invention comprises 15% to 35% by weight tungsten and balance up to 100% by weight titanium, the alloy comprises 70% to 100% by volume equiaxed beta grain structure, and the alloy can be obtained by a process in which the heat treatments of steps (c) and (f) are carried out at a temperature of 640° C. to 925° C. In one embodiment, the beta titanium alloy of the present invention comprises 15% to 28% by weight tungsten and balance up to 100% by weight titanium, the alloy comprises 70% to 100% by volume equiaxed beta grain structure, and the alloy can be obtained by a process in which the heat treatments of steps (c) and (f) are carried out at a temperature of 640° C. to 925° C. In one embodiment, the beta titanium alloy of the present invention comprises 18% to 22% by weight tungsten and balance up to 100% by weight titanium, the alloy comprises 70% to 100% by volume equiaxed beta grain structure, and the alloy can be obtained by a process in which the heat treatments of steps (c) and (f) are carried out at a temperature of 640° C. to 925° C.
[0067] In one embodiment, the beta titanium alloy of the present invention comprises 15% to 40% by weight tungsten, 2% to 4% by weight iridium, and the balance up to 100% by weight titanium, the alloy comprises 70% to 100% by volume equiaxed beta grain structure, and the alloy can be obtained by a method in which the heat treatments of steps (c) and (f) are carried out at a temperature of 640° C. to 925° C. In one embodiment, the beta titanium alloy of the present invention comprises 15% to 35% by weight tungsten, 2% to 4% by weight iridium, and the balance up to 100% by weight titanium, the alloy comprises 70% to 100% by volume equiaxed beta grain structure, and the alloy can be obtained by a method in which the heat treatments of steps (c) and (f) are carried out at a temperature of 640° C. to 925° C. In one embodiment, the beta titanium alloy of the present invention comprises 18% to 25% by weight tungsten, 2% to 4% by weight iridium, and the balance up to 100% by weight titanium, the alloy comprises 70% to 100% by volume equiaxed beta grain structure, and the alloy can be obtained by a method in which the heat treatment of steps (c) and (f) is carried out at a temperature of 645° C. to 895° C. In one embodiment, the beta titanium alloy of the present invention comprises 18% to 22% by weight tungsten, 2% to 4% by weight iridium, and the balance up to 100% by weight titanium, the alloy comprises 70% to 100% by volume equiaxed beta grain structure, and the alloy can be obtained by a method in which the heat treatment of steps (c) and (f) is carried out at a temperature of 640° C. to 925° C.
[0068] In one embodiment, the beta titanium alloy of the present invention can be obtained by the method defined in the present invention, further comprising an additional step (b') of remelting the ingot obtained in step (b) by repeating the high temperature melting of steps (a) and (b) 1 to 5 times. In one embodiment, the beta titanium alloy of the present invention can be obtained by the method defined in the present invention, further comprising an additional step (b') of remelting the ingot obtained in step (b) by repeating the high temperature melting of steps (a) and (b) 2 to 4 times.
[0069] In one embodiment, the beta-titanium alloy of the present invention can be obtained by a method defined in the present invention, which further comprises, after step (d), or after step (g), or after steps (d) and (g), an additional step (h) of drying and polishing the alloy obtained in the previous step. In one embodiment, the drying and polishing steps can be carried out according to any method known in the art. Typically, these steps include drying at room temperature with clean compressed air until no liquid residues remain, followed by mechanical polishing of the obtained alloy by using an abrasive for the removal of the oxide layer.
[0070] A second aspect of the present invention relates to a method for producing the beta titanium alloy of the present invention as defined above, which comprises the steps of: (a) high temperature melting of all elements used as raw materials under a protective atmosphere at a temperature between 3000°C and 3500°C; (b) cooling the melted material obtained in step (a) to room temperature to obtain an ingot; (c) heat treating the ingot obtained in step (b) at a temperature calculated by the formula: Tbeta ± 100°C; (d) quenching the alloy obtained in step (c) to room temperature; (e) machining the alloy obtained in step (d) to obtain a processed alloy; (f) heat treating the processed alloy obtained in step (e) at a temperature calculated by the formula: Tbeta ± 100°C; and (g) quenching the processed alloy obtained in step (f), where Tbeta is as defined above.
[0071] All embodiments disclosed above for the beta-titanium alloy of the first aspect of the invention characterized by the method also apply to the method for the production of the alloy of the second aspect of the invention.
[0072] In one embodiment, step (a) of the method of the invention is carried out under a protective atmosphere at a temperature between 3000° C. and 3500° C. for a period between 1 min and 30 min, in particular between 5 min and 10 min.
[0073] In one embodiment, step (b) of the method of the invention is carried out over a period of between 2 minutes and 20 minutes, in particular between 5 minutes and 10 minutes.
[0074] In one embodiment, steps (c) and (f) of the method of the invention are carried out for a period of between 10 seconds and 1 hour, in particular between 1 minute and 30 minutes.
[0075] A third aspect of the present invention relates to an implantable medical device made of a beta-titanium alloy as defined in the first aspect of the present invention. The term "implantable medical device" refers to any type of instrument that is intended to be placed, in whole or in part, surgically or medically, inside a patient's body or by medical intervention in a natural orifice, and to remain in place after the procedure.
[0076] In one embodiment, an implantable medical device made with a beta titanium alloy as defined in the present invention has an equiaxed beta grain structure with each grain having an average diameter of 10 μm to 50 μm.In one embodiment, an implantable medical device made with a beta titanium alloy as defined in the present invention has an equiaxed beta grain structure with each grain having an average diameter of 12 μm to 40 μm.
[0077] In one embodiment, the implantable medical device made of a beta-titanium alloy as defined in the first aspect of the invention is a stent. The term "stent" refers to an intravascular prosthesis used to repair, strengthen or maintain a lumen in the vasculature. In one embodiment, the implantable medical device made of a beta-titanium alloy as defined in the first aspect of the invention is a balloon-expandable stent. In a balloon-expandable stent, the implant is clipped onto the top of a balloon at the distal part of the catheter. Once clipped, the diameter of the stent is reduced, ensuring that it can be transported to the desired part of the patient's vasculature. Once the stent is positioned in the desired area, the balloon is pressurized and the stent expands, exerting a force on the artery.
[0078] In one embodiment, a stent made with a beta titanium alloy as defined in the present invention has an equiaxed beta grain structure with each grain having an average diameter of 10 μm to 50 μm.In one embodiment, a stent made with a beta titanium alloy as defined in the present invention has an equiaxed beta grain structure with each grain having an average diameter of 12 μm to 40 μm.
[0079] A method for manufacturing implantable medical devices, in particular stents, made of beta-titanium alloy is also part of the invention. The manufacture of the stents of the invention can be achieved by any method known in the art, typically by braiding wires, by laser cutting of sheets or by cutting tubes with a laser. Once the shape of the stent has been cut, the stent is cleaned to remove unwanted metal remains and also to remove the oxide layer formed during laser cutting. This method can include an additional heat treatment of the laser cut part of the stent, for example to improve the mechanical properties of the stent, such as radial force and fracture resistance, among others. After a descaling step, which usually consists of immersing the stent in an acidic solution, the stent is polished. This polishing method can be carried out by several methods, such as sandblasting in a tumbler or electropolishing. Finally, a passivation treatment of the surface of the stent thus obtained can be carried out to improve the biocompatibility and corrosion resistance of the implant.
[0080] Throughout the specification and claims, the word "comprise" and variations of the word are not intended to exclude other technical features, additives, components or steps. Furthermore, the word "comprise" encompasses the term "consisting of". Further objects, advantages and features of the present invention will become apparent to those skilled in the art upon examination of the description or may be learned by the practice of the present invention. The following examples and drawings are provided for illustrative purposes and are not intended to limit the present invention. Reference signs placed in parentheses in the claims in connection with the drawings are intended to enhance the understanding of the claims only and should not be construed as limiting the scope of the claims. Furthermore, the present invention encompasses all possible combinations of the specific preferred embodiments described herein.
[0081] Working Example General Considerations The volume of the beta phase was measured using Cu-K α This was performed by X-ray or diffractogram containing three characteristic peaks at 38.9, 56.4, and 70.7 ± 0.3 degrees (2-theta) with a line, λ = 1.5406 Å. The volume fraction of the beta phase was then quantified by the Rietveld method defined above.
[0082] Measurement of the average diameter of equiaxed beta grains was performed according to the Standard Test Methods for Determining Average Grain Size in accordance with ASTM E112.
[0083] Measurements of the volume of mechanical twins and beta phase transformed to martensite after deformation during tensile testing were performed by transmission electron microscopy (TEM). Discs with a diameter of 3 mm were removed from the samples after tensile testing. The discs were first mechanically polished to 150 μm and then carefully thinned to about 100 nm by electrolytic polishing. Bright-field (BF) and dark-field (DF) images, as well as selected-area electron diffraction (SEAD) were performed to qualitatively identify the location and type of deformation products (twins and martensite). Then, automated crystallographic orientation mapping (ACOM) was performed on several zones to quantify the fraction of each deformation product.
[0084] 1. Alloy composition The qualitative and quantitative compositions of the alloys of the present invention (see Alloys 1 and 2) are disclosed as follows:
[0085] TIFF0007561035000005.tif27144
[0086] 2. Manufacturing method The method for producing the alloy of the present invention is as follows.
[0087] 2.1.Alloy 1 A. Starting Materials Pure (+99.6%) titanium plate in an annealed condition (commercially available from Goodfellow). Pure (99.95%) tungsten tungsten in rolled condition (commercially available from Goodfellow).
[0088] B.Details -Ingot production The raw plate was cut into square pieces using a disc cutter, and the cut pieces were weighed separately. The square pieces thus obtained were washed with ethanol and acetone, and then dried with clean compressed air.
[0089] The cleaned pieces were sealed in a high-temperature melting furnace with a chamber containing a copper crucible. Specifically, the cleaned pieces were placed in the copper crucible and the chamber was sealed and isolated from the atmosphere. The atmosphere of the melting chamber was purged five times with pure argon and then filled with pure argon. Prior to heating the raw pieces, the Ti-Zr ingot was remelted to capture any remaining impurity elements in the furnace atmosphere.
[0090] All raw pieces were worked up by melting and mixing them to a liquid state at 3000-3500 °C to form a single Ti-W ingot. The Ti-W ingot thus obtained was cooled to room temperature in a furnace under argon atmosphere. The ingot was turned upside down in the furnace and remelted at 3000-3500 °C. The ingot was turned upside down and remelted three times.
[0091] -Heat treatment and machining The resulting Ti-W ingot was suspended in a vertical tube furnace. The furnace was sealed and heated for 10 -5 After pumping to a pressure of 1000 mbar (vacuum), the ingot was heated to 850° C. and annealed at this temperature for 30 minutes.
[0092] After 30 minutes, the ingots were removed and quenched in a tank containing room temperature water. The quenched ingots were mechanically polished to remove surface oxidation caused by quenching. The ingots were then washed with acetone and ethanol and dried with clean compressed air.
[0093] The cleaned ingot was rolled in a rolling mill at room temperature. The rolling step was started from the thickness of the ingot and repeated in the same direction by gradually decreasing the distance between the two rollers. The rolling step was ended at a thickness reduction of 95% (thickness reduction = (start thickness - end thickness) / start thickness).
[0094] The rolled Ti-W sheet was washed and -5The Ti-W sheet was suspended in a vertical quenching furnace under a vacuum of 100000000 mbar. The sheet was heated to 850°C and annealed at this temperature for 15 minutes. After 15 minutes, the Ti-W sheet was removed and quenched in a tank containing water at room temperature. The quenched Ti-W sheet was mechanically polished, then washed and dried to obtain the final sheet made of Alloy 1 of the present invention.
[0095] 2.2.Alloy 2 A. Starting Materials Pure (+99.6%) titanium plate in an annealed condition (commercially available from Goodfellow). Pure (99.95%) tungsten tungsten in rolled condition (commercially available from Goodfellow). As drawn pure (99.90%) iridium rod (commercially available from Goodfellow).
[0096] B.Details -Ingot production The manufacturing method for the Ti-W-Ir ingots is the same as that disclosed for Alloy 1, in which the titanium and tungsten feedstock plates are cut into squares by a disc cutter, and the iridium feedstock rods are cut into short cylinders by a disc cutter.
[0097] -Heat treatment and machining The manufacturing method of the final sheet made of the alloy 2 of the present invention is the same as that disclosed for alloy 2, except that a Ti-W-Ir ingot is used as the starting ingot instead of a Ti-W ingot.
[0098] 3. Mechanical properties A. Tensile test method Tensile specimens sized according to ASTM E8M were machined from the alloys of the present invention obtained in sections 2.1 and 2.2.
[0099] The tensile testing protocol was in accordance with the ASTM E8 / E8M standard for test methods for tensile testing of metallic materials.
[0100] The long axis of the tensile specimen was parallel to the rolling direction.
[0101] The specimens were secured to an Instron tensile tester using mechanical wedge clips.
[0102] The clamping stress was monitored and automatically compensated by a tensile testing machine (Instron 5966 equipped with a 10 kN force detector) during clamping of the specimens to avoid preloading.
[0103] A high-precision strain extensometer (Instron 2630-102, maximum strain + / - 50%) was attached to the center of the gauge for deformation measurement.
[0104] The transformation speed is 10 -3 S -1 was fixed.
[0105] Several specimens were tested under the same conditions and the tensile curves were processed with Bluehill software to produce the final results.
[0106] B. Results The tensile test results are summarized in the following table.
[0107] TIFF0007561035000006.tif41119
[0108] As shown by the tensile test results, the alloy of the present invention has a chemical composition and mechanical properties suitable for fabricating implantable medical devices, which should have a yield stress of 400 MPa to 1000 MPa and an elongation at break of 30% to 65%.
[0109] 4. Phases and Microstructure A. Method Test specimen: The alloy obtained after heat treatment and machining. The alloy obtained after tensile testing.
[0110] method: After the specimens were mechanically polished to a mirror finish, the polished surfaces were immersed in Kroll's reagent (a mixture of HF, HNO3, and H2O) for 1 min at room temperature. The polished specimens were washed with water and ethanol, then dried with compressed air. Optical microscope images were taken of the etched surfaces before and after tensile deformation.
[0111] Optical microscopy images were taken by an Olympus PME metallurgical microscope equipped with a CCD camera.
[0112] B. Results alloy 1 Alloy 1 has 100 vol. % beta phase after heat treatment and machining, which is formed into equiaxed grains with an average diameter of about 122 μm (see FIG. 1A). Nevertheless, about 82 vol. % beta phase was strain-transformable to mechanical twins and martensite after deformation during tensile testing (see FIG. 1B).
[0113] alloy 2 Alloy 2 had about 95% by volume of beta phase after heat treatment and machining, which formed into equiaxed grains with an average diameter of about 65 μm, with fine precipitates dispersed within the beta grains and at the grain boundaries. Nevertheless, about 80% by volume of the beta phase was capable of strain transformation into mechanical twins and martensite after deformation during tensile testing.
[0114] Citation List 1.Standard Test Methods for Determining Average Grain Size according to ASTM E112 2.Standard Test Methods according to ASTM E8 / E8M 3.European EN 10002 standard ASTM E8M 4.DLBish et al J.Appl.Cryst.''Quantitative Phase Analysis Using the Rietveld Method'',1988,Vol.21,pp.86-91)
[0115] For reasons of completeness, the various aspects of the invention are set out in the following numbered clauses.
[0116] Clause 1. A beta titanium alloy comprising 15% by weight to 28% by weight tungsten, and the balance up to 100% by weight titanium, the alloy comprising 70% by volume to 100% by volume equiaxed beta grain structure.
[0117] Clause 2. The beta titanium alloy of clause 1, comprising 100 volume percent equiaxed beta grain structure.
[0118] Clause 3. The beta titanium alloy of clause 1 or 2, wherein each beta grain in the equiaxed beta grain structure has an average diameter of 0.01 μm to 200 μm.
[0119] Clause 4. The beta titanium alloy of any one of clauses 1-3, wherein the alloy further comprises at least one metallic element selected from the group consisting of iridium, tantalum, platinum, gold, iron, niobium, zirconium, and tin.
[0120] Article 5. The amount of metallic element (W-eq) is calculated according to the following formula: W-eq weight% = tungsten substitution amount (weight%) / equivalent weight Coefficient (F) During the ceremony, equivalent weight The coefficients are: 5. A beta titanium alloy as defined in clause 4. TIFF0007561035000007.tif52170
[0121] Clause 6. The beta-titanium alloy of any one of clauses 1-5, wherein the alloy contains 18% to 22% tungsten by weight.
[0122] Clause 7. A beta-titanium alloy according to any one of clauses 1-6, wherein the alloy contains 2% to 4% iridium by weight.
[0123] Clause 8. The beta titanium alloy of any one of clauses 1-7, wherein the alloy has one or more of the following characteristics: Yield stress of 400MPa~1000MPa, Maximum tensile strength of 650MPa~1100MPa, Elongation at break of 30% to 65%, and Young's modulus of 80GPa to 140GPa.
[0124] Clause 9. A beta titanium alloy according to any one of clauses 1 to 8, obtained by a process comprising the steps of: (a) high-temperature melting of all elements used as raw materials under a protective atmosphere at a temperature of 3000°C to 3500°C; (b) cooling the molten material obtained in step (a) to room temperature to obtain an ingot; (c) heat treating the ingot obtained in step (b) at a temperature calculated by the following formula: Tbeta±100° C.; (d) quenching the alloy obtained in step (c) to room temperature; (e) machining the alloy obtained in step (d) to obtain a machined alloy; (f) heat treating the processed alloy obtained in step (e) at a temperature calculated by the following formula: Tbeta±100° C.; and (g) quenching the processed alloy obtained in step (f) to room temperature; In the formula, Tbeta is calculated as follows: Tbeta=825-6.54Weq Weq is calculated as follows: Ti-x%W-y1 / F1%M1-y2 / F2%M2-y3 / F3%M3-y4 / F4%M4-y5 / F5%M5-y6 / F6%M6-y7 / F7%M7-y8 / F8%M8 During the ceremony, Ti is the amount of titanium x is the amount of tungsten, greater than 0; Each M 1-8and corresponds to a metal element selected from iridium, tantalum, platinum, gold, iron, niobium, zirconium and tin; y 1-8 is each metal element M 1-8 is the amount of each y 1-8 are independently selected from 0 or greater, F 1-8 is as stated in clause 5 equivalent weight is the coefficient, [x+Σ(y1 / F1+y2 / F2+y3 / F3+y4 / F4+y5 / F5+y6 / F6+y7 / F7+y8 / F8)] is 15-28 inclusive, [x+Σ(y1+y2+y3+y4+y5+y6+y7+y8)] ranges from 4.55 to 49.9 inclusive.
[0125] Clause 10. The beta titanium alloy of clause 9, wherein the method further comprises an additional step (b') of remelting the ingot obtained in step (b) by repeating the high temperature melting of steps (a) and (b) one to five times.
[0126] Clause 11. The beta titanium alloy according to clause 9 or 10, wherein the method further comprises an additional step (h) after step (d), or after step (g), or after steps (d) and (g), respectively, of drying and polishing the alloy obtained in the previous step.
[0127] Clause 12. A method for producing a beta titanium alloy according to any one of clauses 1 to 11, comprising the steps of: (a) high-temperature melting of all elements used as raw materials under a protective atmosphere at a temperature of 3000°C to 3500°C; (b) cooling the molten material obtained in step (a) to room temperature to obtain an ingot; (c) heat treating the ingot obtained in step (b) at a temperature calculated by the following formula: Tbeta±100° C.; (d) quenching the alloy obtained in step (c) to room temperature; (e) machining the alloy obtained in step (d) to obtain a machined alloy; (f) heat treating the processed alloy obtained in step (e) at a temperature calculated by the following formula: Tbeta±100° C.; and (g) quenching the processed alloy obtained in step (f); where Tbeta is as defined in clause 9.
[0128] Clause 13. An implantable medical device made from a beta-titanium alloy according to any one of clauses 1 to 11.
[0129] Clause 14. An implantable medical device according to clause 13 which is a stent.
[0130] Clause 15. The implantable medical device of clause 14 which is a balloon-expandable stent.
Claims
1. 15% to 40% by weight tungsten, and The balance is titanium, A beta titanium alloy consisting of: or alternatively, 15% to 40% by weight tungsten; 2% to 4% by weight of iridium, and The balance is titanium, A beta titanium alloy consisting of: the alloy comprises 70% to 100% by volume of an equiaxed beta grain structure; Beta titanium alloy.
2. 2. The beta titanium alloy of claim 1, wherein the amount of tungsten is 15% to 35% by weight.
3. 3. A beta titanium alloy as claimed in claim 1 or 2, wherein the amount of tungsten is between 15% and 28% by weight.
4. A beta titanium alloy according to any one of claims 1 to 3, comprising 100% by volume of said equiaxed beta grain structure.
5. A beta titanium alloy according to any one of the preceding claims, wherein each beta grain of the equiaxed beta grain structure has an average diameter of between 0.01 μm and 200 μm.
6. A beta titanium alloy according to any one of the preceding claims, wherein the amount of tungsten in the alloy is between 18% and 22% by weight.
7. A beta titanium alloy according to any one of claims 1 to 6, wherein the alloy has one or more of the following properties: Yield stress of 400MPa to 1000MPa Ultimate tensile strength of 650MPa to 1100MPa Elongation at break: 30% to 65% Young's modulus of 80GPa to 140GPa
8. A method for producing a beta titanium alloy according to any one of claims 1 to 7, comprising the steps of: (a) high-temperature melting of all elements used as raw materials under a protective atmosphere at a temperature of 3000°C to 3500°C; (b) cooling the molten material obtained in step (a) to room temperature to obtain an ingot; (c) heat treating the ingot obtained in step (b) at a temperature calculated by the following formula: Tbeta±100° C.; (d) quenching the alloy obtained in step (c) to room temperature; (e) machining the alloy obtained in step (d) to obtain a machined alloy; (f) heat treating the processed alloy obtained in step (e) at a temperature calculated by the following formula: Tbeta±100° C.; and (g) quenching the processed alloy obtained in step (f).
9. An implantable medical device made from the beta-titanium alloy of any one of claims 1 to 7.
10. 10. The implantable medical device of claim 9 which is a stent.
11. 11. The implantable medical device of claim 10 which is a balloon-expandable stent.
Citation Information
Patent Citations
Composite titanium plate manufacturing process and system
CN106392483A
Ti-base alloy for hot working tool and its manufacture
JP1991229837A
Titanium alloy and golf club head made of titanium alloy
JP1997194968A
beta TYPE TITANIUM ALLOY FOR LIVING BODY
JP2005048235A
Method for manufacturing titanium alloys for biomedical devices
JP2015503025A