Controlled rolling and controlled cooling method suitable for online normalizing of medium carbon boron-containing steel bars

The on-line normalizing treatment method for medium carbon boron-containing steel through controlled rolling and cooling addresses production inefficiencies by achieving desired hardness and structure without offline normalization, reducing costs and cycles.

JP7561289B2Active Publication Date: 2024-10-03DAYE SPECIAL STEEL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023569673
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-05-13
Filing Date
2022-05-11
Publication Date
2024-10-03
Estimated Expiration
2042-05-11

AI Technical Summary

Technical Problem

Conventional off-line normalizing processes for medium carbon boron-containing steel result in increased production costs, longer production cycles, and mixed crystal problems, limiting mass production efficiency and product application.

Method used

A rolling cooling control method for on-line normalizing treatment of medium carbon boron-containing steel, involving specific chemical compositions and controlled rolling and cooling processes, including heating, rough rolling, finish rolling, water cooling, and cold bed slow cooling, to achieve desired hardness and structural requirements without offline normalization.

Benefits of technology

The method reduces production costs and cycles, enhances production efficiency, and meets hardness and structural requirements, replacing offline normalizing processes and improving product competitiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007561289000005
    Figure 0007561289000005
  • Figure 0007561289000006
    Figure 0007561289000006
  • Figure 0007561289000007
    Figure 0007561289000007
Patent Text Reader

Abstract

The present invention provides a medium carbon boron-containing steel having chemical compositions, in mass%, of 0.37-0.45% C, 0.17-0.37% Si, 0.60-0.90% Mn, 0.020-0.060% Al, 0.0008-0.0035% B, 0.030-0.060% Ti, P≦0.025%, S≦0.025%, Cr≦0.25%, Ni≦0.20%, Mo≦0.10%, Cu≦0.20%, and the remainder being Fe and unavoidable impurities. A rolling cooling control method suitable for online normalizing of the medium carbon boron-containing steel includes the steps of heating, rough rolling, finish rolling, water cooling, and cold bed slow cooling in sequence. Medium carbon boron-containing steel can meet the requirements of hardness 190~220HBW, actual grain size ≧7 grade, and band structure ≦2 grade.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of rolled steel, specifically to medium carbon boron containing steel and a method for controlling the rolling cooling of an online normalizing process. [Background technology]

[0002] Medium carbon boron-containing steel is an alloy structural steel with good hardenability. It is widely used to manufacture important parts such as constant velocity transmission shafts of automobiles. Due to the requirements of processing and use conditions, there are strict requirements for material structure and hardness.

[0003] In the manufacturing process, the conventional technology generally requires the steel to be normalized offline to meet the structural hardness requirements of the steel, but because the finished material specifications used in production applications are small (20-50mm), it is necessary to use a specialized normalizing furnace to perform the normalization offline, which not only reduces production efficiency but also easily causes mixed crystal problems. At the same time, the production cycle due to the offline normalization of steel increases by about one week, and the corresponding production cost increases by about 400 yuan / ton, seriously restricting the mass production and application of the product. Summary of the Invention [Problem to be solved by the invention]

[0004] The objective of the present invention is to provide a medium carbon boron-containing steel and a rolling cooling control method for online normalizing treatment, which can clearly refine the structure of the medium carbon boron-containing steel in the hot rolling state, and meet the requirements of Brinell hardness 190-220HBW, grain size ≧7 grade, and band structure ≦2 grade, so as to replace the original offline normalizing process, while saving the production cycle and reducing the normalizing cost, thereby reducing the production cost of the enterprise and improving the product competitiveness. [Means for solving the problem]

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] A medium carbon boron containing steel, the chemical composition of which includes, in mass%, C 0.37-0.45%, Si 0.17-0.37%, Mn 0.60-0.90%, Al 0.020-0.060%, B 0.0008-0.0035%, Ti 0.030-0.060%, P ≦0.025%, S ≦0.025%, Cr ≦0.25%, Ni ≦0.20%, Mo ≦0.10%, Cu ≦0.20%, and the remainder being Fe and unavoidable impurities.

[0007] Furthermore, the medium carbon boron-containing steel satisfies the following requirements: Brinell hardness 190 to 220 HBW, grain size ≧ grade 7, and band structure ≦ grade 2.

[0008] Furthermore, the standard for the medium carbon boron-containing steel is Φ20 to Φ50 mm.

[0009] The present invention further provides a rolling cooling control method suitable for the online normalizing treatment of the above medium carbon boron-containing steel, which sequentially includes the steps of heating, rough rolling, finish rolling, water cooling, and cold bed slow cooling.

[0010] Furthermore, in the above-mentioned rolling cooling control method suitable for online normalizing treatment of medium carbon boron-containing steel, in the heating step, the heating temperature of the billet in the heating furnace is 1100 to 1200°C and the total heating time is 90 to 180 min, and preferably, the heating temperature of the billet in the heating furnace is 1130 to 1180°C and the total heating time is 120 to 150 min.

[0011] Furthermore, in the above-mentioned rolling cooling control method suitable for online normalizing treatment of medium carbon boron-containing steel, in the rough rolling step, the inlet temperature at which the billet enters the rough rolling unit is 1000 to 1050°C.

[0012] Furthermore, in the above-mentioned rolling cooling control method suitable for online normalizing treatment of medium carbon boron-containing steel, in the finish rolling step, the inlet temperature at which the billet enters the finish rolling unit is 780 to 830°C, preferably in the finish rolling step, the inlet temperature at which the billet enters the finish rolling unit is 780 to 810°C, and preferably in the finish rolling step, finish rolling is performed using a reduced sizing finish rolling unit.

[0013] Furthermore, in the above-mentioned rolling cooling control method suitable for online normalizing treatment of medium carbon boron-containing steel, the water cooling is fountain cooling using a water box, and after water cooling, the exit water temperature of the finished steel material is 700-750°C, preferably the amount of water in the water box is 40-60 L / min, the running speed of the finished steel material is 3-8 m / s, and preferably the exit water temperature of the finished steel material after water cooling is 710-730°C.

[0014] Furthermore, in the rolling cooling control method suitable for the online normalizing treatment of the above-mentioned medium carbon boron-containing steel, the cooling rate of the finished steel product in the cold bed slow cooling step is 0.10 to 0.15° C. / s.

[0015] Furthermore, in the rolling cooling control method suitable for the online normalizing treatment of the above-mentioned medium carbon boron-containing steel, in the cold bed slow cooling step, the finished steel material is placed in a heat-insulating cover and cooled on a cold bed, cooled to below 500°C, taken out of the heat-insulating cover and air-cooled.

[0016] Furthermore, in the above-mentioned rolling cooling control method suitable for online normalizing treatment of medium carbon boron-containing steel, in the cold bed slow cooling step, the cold bed is a stepping cold bed.

[0017] Furthermore, in the rolling cooling control method suitable for the online normalizing treatment of the above-mentioned medium carbon boron-containing steel, the cross-sectional dimensions of the billet are 240 mm x 240 mm. Effect of the Invention

[0018] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0019] (1) There is no need to adjust the composition of the steel during the production process, and no need to add additional offline normalizing production equipment. By simply adjusting the rolling and cooling processes, the online normalizing treatment of this type of product can be realized, and at the same time, the structural hardness requirements of the steel can be met.

[0020] (2) The temperature control range at each stage of the production process is wide, making it easy to control and realize industrial production.

[0021] (3) By using online normalizing instead of offline normalizing in the heating step, the fixed equipment investment was reduced, the production cycle was shortened (by about 1 week), the production cost was reduced (by about 400 RMB / ton), the production cycle was accelerated, the production cost was reduced, and the product competitiveness was improved.

[0022] (4) The medium carbon boron-containing steel produced by this method can meet the requirements of hardness 190~220HBW, actual grain size ≧7 grade, and band structure ≦2 grade, and can fully meet the technical index requirements of the user's product after offline normalizing. [Brief description of the drawings]

[0023] Hereinafter, specific embodiments of the present invention will be described in more detail with reference to the drawings. The drawings in the specification, which are a part of this application, are intended to provide a further understanding of the present invention, and the illustrative examples and the description thereof are not intended to unduly limit the present invention, but are intended to interpret the present invention. [Figure 1] FIG. 2 is a microstructure diagram of 40B steel having a standard of 32 mm and a radius of 1 / 2 produced in Example 1. [Diagram 2] FIG. 1 is a microstructure diagram of 40B steel having a standard of 28 mm and a radius of 1 / 2 produced in Example 2. [Diagram 3] FIG. 2 is a microstructure diagram of 40B steel having a standard of 30 mm and a radius of 1 / 2 produced in Comparative Example 1. [Figure 4]FIG. 2 is a microstructure diagram of 40B steel having a standard of 34 mm and a radius of 1 / 2 produced in Comparative Example 2. [Diagram 5] FIG. 1 is a microstructure diagram of 40B steel having a standard of 28 mm and a radius of 1 / 2 produced in Comparative Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] Hereinafter, the present invention will be described in detail based on the embodiments with reference to the drawings. Each example is provided by the interpretation of the present invention, not by limiting the present invention. In fact, it is obvious to those skilled in the art that modifications and variations are possible in the present invention without departing from the scope or spirit of the present invention. For example, some features of one embodiment can be applied to another embodiment to generate yet another embodiment. Therefore, it is desirable that the present invention includes modifications and variations that fall within the scope of the appended claims and their equivalents.

[0025] The accompanying drawings illustrate one or more examples of the present invention. In the detailed description, numerical and alphabetical symbols are used to refer to features in the drawings. Like or similar symbols in the drawings and description have been used to refer to like or similar parts of the invention.

[0026] As shown in Figs. 1 and 2, according to an embodiment of the present invention, there is provided a medium carbon boron-containing steel, the chemical components of which include, in mass%, 0.37-0.45% C, 0.17-0.37% Si, 0.60-0.90% Mn, 0.020-0.060% Al, 0.0008-0.0035% B, 0.030-0.060% Ti, P ≦0.025%, S ≦0.025%, Cr ≦0.25%, Ni ≦0.20%, Mo ≦0.10%, Cu ≦0.20%, and the remainder being Fe and unavoidable impurities. Medium carbon boron-containing steel mainly contains manganese (Mn) and boron (B) as alloying elements. If the content of alloying elements such as chromium (Cr), nickel (Ni), molybdenum (Mo) or copper (Cu) is too high, structures such as bainite are easily formed after rolling and cooling control, which makes the hardness too high.

[0027] The standard of the medium carbon boron-containing steel is Φ20~50mm, and the medium carbon boron-containing steel satisfies Brinell hardness 190~220HBW, grain size ≧7 grade, and band structure ≦2 grade, and the standard of the medium carbon boron-containing steel is Φ20~50mm.

[0028] According to an embodiment of the present invention, a rolling cooling control method is provided which is suitable for online normalizing of a medium carbon boron-containing steel, the method sequentially including the steps of heating, rough rolling, finish rolling, water cooling, and cold bed cooling, and the selected billet has a cross-sectional dimension of 240 mm×240 mm.

[0029] In the heating step, the heating temperature of the billet in the heating furnace is 1100°C to 1200°C (e.g., 1100°C, 1110°C, 1120°C, 1130°C, 1140°C, 1150°C, 1160°C, 1170°C, 1180°C, 1190°C, 1200°C, and a section or section point between any two of these temperatures), and the total heating time is 90 to 180 min (e.g., 90 min, 100 min, 110 min, 120 min, 130 min, 140 min, 150 min, 160 min, 170 min, 180 min, and a point between any two of these time periods).

[0030] In a preferred embodiment, in the heating step, the heating temperature of the billet in the heating furnace is 1130 to 1180°C (e.g., 1130°C, 1140°C, 1150°C, 1160°C, 1170°C, 1180°C, and a section or section point between any two of these temperatures), and the total heating time is 120 to 150 min (e.g., 120 min, 130 min, 140 min, 150 min, and a point between any two of these time periods), and the purpose of selecting the corresponding heating temperature and heating time is to ensure that the billet is heated sufficiently while preventing overheating.

[0031] In the rough rolling step, the inlet temperature of the billet entering the rough rolling unit is 1000 to 1050°C (for example, 1000°C, 1010°C, 1020°C, 1030°C, 1040°C, 1050°C, and a section or section point between any two of these temperatures). The rough rolling unit is a six-unit flat continuous rolling unit, and the working roll diameter is 650mm. The inlet temperature of the rough rolling unit is related to the temperature of the heating step, and the temperature of the billet is reduced between the heating step and the rough rolling step by removing phosphorus with high-pressure water.

[0032] In the finish rolling step, the finish rolling unit adopts a sizing finish rolling unit, and the inlet temperature entering the finish rolling unit is 780-830°C (for example, 780°C, 790°C, 800°C, 810°C, 820°C, 830°C, and a section or section point between any two of these temperatures), and the more preferred inlet temperature entering the finish rolling unit is 780-810°C (for example, 780°C, 790°C, 800°C, 810°C, and a section or section point between any two of these temperatures). The precision rolling unit is four 3-roll sizing finish rolling mills, and the deformation amount of the finished material using the 3-roll sizing finish rolling mill is large, which is advantageous for refining the crystal grains.

[0033] In the water cooling step, the temperature of the finished steel after water cooling is 700 to 750°C (for example, 700°C, 710°C, 720°C, 730°C, 740°C, 750°C, and a section or point between any two of these temperatures), and more preferably, the temperature of the finished steel after water cooling is 710 to 730°C (for example, 710°C, 720°C, 730°C, and a section or point between any two of these temperatures). The amount of water in the water box is 40 to 60L / min, and the running speed of the finished steel is preferably 3 to 8m / s (selectable according to the finished steel standard). Water cooling and the above parameter settings can prevent the coarsening of crystal grains due to recovery recrystallization caused by the temperature rise of the steel during rolling.

[0034] In the cold bed slow cooling step, the finished steel material after the water cooling step is cooled in a cold bed, and the cold bed is cooled using a stepping cold bed. The cooling rate of the finished steel material is 0.10 to 0.15°C / s. The finished steel material is cooled on the cold bed in an insulating cover, and cooled to below 500°C. The finished steel material is then removed from the insulating cover and cooled in air. Air cooling using an insulating cover has a slow cooling effect, and prevents the problem of deformation in the subsequent turning or heat treatment process due to the large internal residual stress of the finished steel material due to the fast cooling rate. If the finished steel material is directly air-cooled, the internal stress of the steel material will be large, which may cause deformation problems in the subsequent processing process. By cooling the finished steel material in an insulating cover on a cold bed, the problems caused by direct air cooling can be avoided.

[0035] The medium carbon boron-containing steel produced by the method disclosed in this application can meet the requirements of Brinell hardness 190-220HBW, actual grain size ≧7 grade, and band structure ≦2 grade without offline normalizing process, and can fully meet the technical index requirements of the user's product after offline normalizing. This rolling cooling control method for producing medium carbon boron-containing steel saves the cost and time of the offline normalizing step, reduces fixed equipment investment, shortens the production cycle, reduces production costs, accelerates the production cycle, and improves product competitiveness.

[0036] Example 1 The cross-sectional dimension of the selected billet is 240 mm x 240 mm, and the chemical composition of the medium carbon boron-containing steel billet is, in mass%, C 0.38%, Si 0.25%, Mn 0.86%, Al 0.032%, B 0.0017%, Ti 0.047%, P 0.013%, S 0.005%, Cr 0.14%, Ni 0.03%, Mo 0.02%, Cu 0.02%, and the remainder is Fe and unavoidable impurities, and the cross-sectional dimension of the billet is 240 mm x 240 mm.

[0037] Heating step: The heating temperature of the billet entering the heating furnace is 1140-1160℃, and the total heating time is 142min.

[0038] Rough rolling step: The inlet temperature into the rough rolling unit is 1038°C.

[0039] Finish rolling step: A reduced diameter finishing rolling unit is used, and the inlet temperature of the finishing rolling unit is 795℃.

[0040] Water cooling step: The finished steel material rolled by the reducing diameter finishing rolling unit is cut by the flying shear and then cooled by water spray in the water box. The temperature of the finished steel material coming out of the water box after water cooling is 728℃.

[0041] Cold bed slow cooling step: carried out in a stepping cold bed, the cooling rate of the finished steel is 0.10~0.15℃ / s.

[0042] After cutting, the finished steel product is covered with an insulation cover and cooled in a stepping cold bed. The insulation cover is then closed and the finished steel product is gradually cooled on the cold bed until it reaches 475°C, at which point it is removed from the insulation cover and air-cooled.

[0043] The finished steel product processed in the above steps has a hardness of 204 / 208 HBW at 1 / 2 of the cross section, an actual grain size of grade 8, and a band structure of grade 1.5, as shown in Figure 1.

[0044] Example 2 The chemical composition of the medium carbon boron-containing steel billet is, in mass%, C 0.38%, Si 0.25%, Mn 0.84%, Al 0.028%, B 0.0020%, Ti 0.045%, P 0.012%, S 0.008%, Cr 0.12%, Ni 0.02%, Mo 0.03%, Cu 0.03%, and the balance is Fe and unavoidable impurities. The cross-sectional dimension of the selected billet is 240 mm x 240 mm.

[0045] The steps of the rolling cooling control method suitable for online normalizing treatment of medium carbon boron-containing steel are as shown in Example 1, among which, the comparison of the parameters of each step of the rolling cooling control method suitable for online normalizing treatment of medium carbon boron-containing steel is shown in Table 1. The hardness at 1 / 2 of the cross section of the finished steel material processed in the steps of Example 2 is 212 / 215HBW, the actual grain size is grade 9, and the band structure is grade 1.5, as shown in Figure 2.

[0046] Table 1 shows the parameters of each step in Examples 1 and 2 and the performance of the resulting steel materials.

[0047] [Table 1]

[0048] Examples 3 to 5 The chemical composition of the medium carbon boron-containing steel billets in Examples 3 to 5 was the same as that in Example 1.

[0049] The parameters for each step of heating, rough rolling, finish rolling, water cooling, and cold bed cooling in Examples 3 to 5 are shown in Table 2, as are the properties of the finished steel products, including hardness at 1 / 2R, grain size, and band structure degree.

[0050] Table 2 shows the parameters for each step in Examples 3 to 5 and the performance of the resulting steel materials.

[0051] [Table 2]

[0052] As can be seen from Table 2, the hardness at 1 / 2R of the steel materials obtained in Examples 3 to 5 is 202 to 214HBW, the grain size is 8 to 8.5 class, and the band-like structure degree is 1.5 to 2.0 class.

[0053] Examples 6 to 8 The chemical compositions of the medium carbon boron-containing steel billets in Examples 6 to 8 were the same as those in Example 1.

[0054] The parameters for each step of heating, rough rolling, finish rolling, water cooling, and cold bed cooling in Examples 6 to 8 are shown in Table 3, as are the properties of the finished steel products, including hardness at 1 / 2R, grain size, and band structure.

[0055] Table 3 shows the parameters and performance of the steel materials obtained in Examples 6-8 at each step.

[0056] [Table 3]

[0057] As can be seen from Table 3, the hardness at 1 / 2R of the steel materials obtained in Examples 6 to 8 is 204 to 218HBW, the grain size is class 8 to 9, and the band-like structure degree is class 1.5 to 2.0.

[0058] Comparative Examples 1 to 3 The chemical components of the billets of the medium carbon boron-containing steels of Comparative Examples 1 to 3 are the same as those of Example 1.

[0059] The parameters of each step of heating, rough rolling, finish rolling, water cooling, and cold bed slow cooling in Comparative Examples 1 to 3 are shown in Table 4.

[0060] Table 4 shows the parameters and performance of the steel materials obtained in Comparative Examples 1 to 3 at different steps.

[0061] [Table 4]

[0062] As can be seen from Table 4, in Comparative Example 1, except for the fact that the temperature entering the rough rolling mill is higher due to the different heating temperature in the heating step, the process parameters of the other steps are all within the protection scope of the present application. Because the heating temperature in the heating step is too high, the original austenite grains of the raw material are coarsened, the amount of cooling water in the rolling process is increased, the local grain size after the finished material is coarsened, and the hardness is increased, as shown in Figure 3.

[0063] In Comparative Example 2, except for the total heating time in the heating step, the process parameters of the other steps are all within the scope of protection of the present application. Because the heating time is too long, the original austenite grains of the raw material become coarse, and the local grain size of the finished product becomes coarse, as shown in Figure 4.

[0064] In Comparative Example 3, except for the cold bed cooling step, which does not use a heat-insulating cover and goes directly into cold bed cooling, the process parameters of the other steps are all within the scope of protection of the present application. Since no heat-insulating cover is used, the cooling speed is too fast, which results in high hardness of the raw material and large residual internal stress, as shown in Figure 5, which creates the risk of subsequent processing deformation.

[0065] Based on the analysis of Examples 1 to 8 and Comparative Examples 1 to 3, the present invention provides a rolling cooling control method suitable for online normalizing treatment of medium carbon boron-containing steel, which is realized by adjusting the temperature and cooling rate during rolling of the steel material, and makes the hardness and structure of the hot-rolled steel material reach the requirements of the original normalized state.

[0066] The above is only a preferred embodiment of the present invention, not a limitation of the present invention. For those skilled in the art, the present invention can be modified and changed in various ways. Any amendments, equivalent replacements, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A controlled rolling and controlled cooling method suitable for online normalizing treatment of medium carbon boron-containing steel bars, comprising: The chemical composition of the medium carbon boron-containing steel bar is, in mass%, C 0.37-0.45%, Si 0.17-0.37%, Mn 0.60-0.90%, Al 0.020-0.060%, B 0.0008-0.0035%, Ti 0.030-0.060%, P ≦0.025%, S ≦0.025%, Cr ≦0.25% (excluding 0%), Ni ≦0.20% (excluding 0%), Mo ≦0.10% (excluding 0%), Cu ≦0.20% (excluding 0%), and the remainder being Fe and unavoidable impurities. The medium carbon boron-containing steel bar has a Brinell hardness of 190 to 220 HBW, a grain size of ≧7 grade, and a band structure of ≦2 grade; The method includes the steps of heating, rough rolling, finish rolling, water cooling, and cold bed annealing in sequence without the need for an offline normalizing process; In the heating step, the heating temperature of the billet in the heating furnace is 1100 to 1200 ° C., and the total heating time is 90 to 180 min; In the rough rolling step, the inlet temperature of the billet entering the rough rolling unit is 1000 to 1050 ° C.; In the finish rolling step, the inlet temperature of the billet entering the finish rolling unit is 780 to 830°C; Water cooling is performed by using a water box for fountain cooling. After water cooling, the temperature of the finished steel is 700-750°C. The amount of water in the water tank is 40 to 60 L / min, and the running speed of the finished steel material is 3 to 8 m / s. In the cold bed slow cooling step, the cooling rate of the finished steel is 0.10 to 0.15 ° C / s; In the cold bed slow cooling step, the finished steel material is cooled on the cold bed in a heat-insulating cover, cooled to 500°C or less, and then taken out of the heat-insulating cover and air-cooled. A controlled rolling and controlled cooling method suitable for on-line normalizing treatment of medium carbon boron-containing steel bars.

2. In the finish rolling step, the inlet temperature of the billet entering the finish rolling unit is 780 to 830°C; In the finish rolling step, finish rolling is performed using a reducing diameter finish rolling unit. A controlled rolling and controlled cooling method suitable for the on-line normalizing treatment of the medium carbon boron-containing steel bar according to claim 1.

3. The temperature of the finished steel material after water cooling is 710 to 730 ° C. A controlled rolling and controlled cooling method suitable for the on-line normalizing treatment of the medium carbon boron-containing steel bar according to claim 1.

4. In the cold bed slow cooling step, the cold bed is a stepping type cold bed; A controlled rolling and controlled cooling method suitable for the on-line normalizing treatment of the medium carbon boron-containing steel bar according to claim 1.

5. The cross-sectional dimensions of the billet are 240 mm x 240 mm. A controlled rolling and controlled cooling method suitable for the on-line normalizing treatment of the medium carbon boron-containing steel bar according to claim 1.

Citation Information

Patent Citations

  • Medium carbon steel wire rod with high strength and high plasticity and production method thereof

    CN109234508A

  • Production control method for improving curvature of 42CrMo bar

    CN110918642A

  • Rolling method for eliminating chilling layer on surface of medium-carbon steel

    CN112090966A

  • Non-quenched and tempered steel, preparation method of non-quenched and tempered steel, half shaft and preparation method of half shaft

    CN112899574A

  • Production of b-containing steel

    JP1991047918A