Hydrogen production device, hydrogen separation membrane, and method for producing hydrogen separation membrane
The hydrogen production device employs a silica-based hydrogen separation membrane with a 0.3 nm pore diameter to efficiently produce high-purity hydrogen from biogas, addressing the inefficiencies and durability issues of palladium-based membranes.
Patent Information
- Application Number
- JP2020161352
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-25
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2040-09-25
AI Technical Summary
Existing hydrogen separation membranes for biogas have poor hydrogen separation performance and durability, particularly those using palladium, which are expensive and suffer from hydrogen embrittlement, while silica membranes with larger pore diameters offer limited efficiency in membrane reactors.
A hydrogen production device using a hydrogen separation membrane with an amorphous silica layer having a pore diameter of 0.3 nm or less, integrated with a porous support, which selectively permeates hydrogen gas and is produced without noble metals like palladium, ensuring high purity and durability.
The device efficiently produces hydrogen from biogas with high purity (99%) and durability, overcoming the limitations of palladium-based membranes by using a silica layer with improved hydrogen separation performance and resistance to hydrogen embrittlement.
Smart Images

Figure 0007561416000005 
Figure 0007561416000006 
Figure 0007561416000007
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a hydrogen production device, a hydrogen separation membrane, and a method for producing a hydrogen separation membrane. [Background technology]
[0002] From the perspective of environmental conservation and efficient energy use, effective use of sewage sludge biogas generated in sewerage projects has been considered. However, biogas power generation, which uses biogas directly to generate electricity, has the problem of low energy efficiency. Sewage sludge biogas is a mixed gas whose main components are methane and carbon dioxide, and methods for producing hydrogen from sewage sludge biogas by utilizing the steam reforming reaction of methane are being attempted. In recent years, hydrogen has been attracting attention as a clean energy source. Since natural hydrogen is rarely found in nature, hydrogen is produced by generating hydrogen from compounds containing hydrogen atoms. However, hydrogen production by, for example, reforming fossil fuels or electrolysis of water has problems such as energy inefficiency and carbon dioxide emissions.
[0003] For this reason, methods for selectively extracting only hydrogen from compounds containing hydrogen have been investigated. For example, hydrogen can be efficiently produced by extracting only the hydrogen produced by the steam reforming reaction of methane from the reaction system. Palladium membranes are one example of membranes that have been put to practical use as hydrogen separation membranes for selective hydrogen permeation. Palladium (hereinafter also referred to as Pd) is known as a metal that can absorb large amounts of hydrogen, and is used as a hydrogen separation membrane by making it thin. A hydrogen separation membrane made of Pd can selectively separate only hydrogen from a mixed gas by dissociating and recombining hydrogen on the surface of the Pd membrane through a dissolution-diffusion mechanism. In addition to the fact that Pd is a precious metal and expensive, there are problems such as the occurrence of hydrogen embrittlement, in which the membrane deteriorates over time as hydrogen dissolves, and therefore a method that does not use Pd as a selective hydrogen separation membrane is desired.
[0004] As an example of a hydrogen separation membrane that does not use Pd, a hydrogen separation membrane with good heat resistance has been proposed in which silica is formed using oxygen and a vaporized silica source so as to partially block the pores of a porous substrate (see Patent Document 1). The use of dimethoxydimethylsilane as a silica source for hydrogen separation membranes has been proposed, and it has been disclosed that by using dimethoxydimethylsilane as a silica source, it is possible to obtain a hydrogen separation membrane that is thinner and has better temperature stability than conventional hydrogen separation membranes that use tetramethoxysilane as a silica source (see Non-Patent Document 1). Furthermore, although still in the experimental stage, a hydrogen separation method that reduces the amount of Pd used is being investigated, in which a Pd membrane is formed inside a porous ceramic substrate and combined with a silica membrane for hydrogen separation, thereby improving reaction efficiency and reducing reaction temperature (see Non-Patent Document 2). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 4728308 [Non-patent literature]
[0006] [Non-Patent Document 1] J.Membr.Sci.Vol.580 pp.268-274(2019) [Non-Patent Document 2] Toyama Hydrogen Energy Promotion Council, "Survey on research and development trends of carbon dioxide-free hydrogen production technology from hydrocarbon fuels, etc." pp.34-35 (2019) Summary of the Invention [Problem to be solved by the invention]
[0007] The silica membrane described in Patent Document 1 has a good hydrogen permeation rate, but its pore size is 0.4 nm or more, and there is still room for improvement in terms of hydrogen separation properties as a hydrogen separation membrane used in a membrane reactor for producing hydrogen from biogas. Although it is disclosed that the hydrogen separation membrane described in Non-Patent Document 1 is thin and has good temperature stability, there has been no attention paid to applying the obtained hydrogen separation membrane to a membrane reactor or the like for treating biogas.
[0008] The hydrogen separation device described in Non-Patent Document 2 is a technology that is intended to improve the durability of the palladium membrane due to temperature, and is premised on the use of palladium. Furthermore, no particular ingenuity is given to the hydrogen separation membrane used in combination, and there is no description of a hydrogen separation membrane that uses a hydrogen separation membrane containing silica.
[0009] An object of one embodiment of the present invention is to provide a hydrogen production device that can efficiently produce hydrogen from biogas by using a hydrogen separation membrane that is manufactured without using a precious metal such as palladium as a membrane material. An object of another embodiment of the present invention is to provide a hydrogen separation membrane that can be used in a hydrogen production apparatus and has good hydrogen separability and durability, and a method for producing a hydrogen separation membrane that has good hydrogen separability and durability. [Means for solving the problem]
[0010] Means for solving the above problems include the following embodiments. <1> A hydrogen production device comprising: a biogas supplying device that supplies biogas; a membrane reactor having a cylindrical body and a catalyst for producing hydrogen gas from the biogas supplied from the biogas supplying device and a hydrogen separation membrane that selectively permeates hydrogen gas disposed inside the membrane reactor; and a recovery device that recovers hydrogen gas with a purity of 99% or more separated by the membrane reactor, wherein the hydrogen separation membrane is a hydrogen separation membrane composed of a porous support and an amorphous silica layer formed on the porous support and having an average pore diameter of 0.3 nm or less. <2> The present invention is provided with a biogas supplying device for supplying biogas, a membrane reactor in which a catalyst for producing hydrogen gas from the biogas supplied from the biogas supplying device and a hydrogen separation membrane that selectively permeates hydrogen gas are disposed inside a cylindrical body, and a recovery device for recovering hydrogen gas with a purity of 99% or more separated by the membrane reactor, the hydrogen separation membrane being formed on a porous support and having a hydrogen permeability of 2×10 or more as measured by the following measurement method. -7 mol m -2 s -1 Pa -1 and an amorphous silica layer having a gas permeability for gases other than hydrogen gas and helium gas that is 1 / 100 or less of the hydrogen permeability. (Measurement method) Hydrogen gas is supplied to the supply side of the hydrogen separation membrane after the membrane is formed, and the supply side pressure is set to 0.2 MPaG. Hydrogen gas is allowed to permeate using a dead-end method with a transmembrane pressure difference of 0.2 MPa. The flow rate of the permeated gas obtained from the permeation side is measured using a soap film flowmeter, and the hydrogen gas permeability is calculated from the obtained permeated gas flow rate. The measurement is performed at 500°C.
[0011] <3> The amorphous silica layer is a layer made of amorphous silica derived from a dimethoxydimethylsilane (hereinafter also referred to as DMDMS) silica source. <1> or <2> The hydrogen production device according to claim 1. <4> The porous support has a two-layer structure including at least a support layer and an intermediate layer, the support layer being a porous body having an average pore diameter of 30 nm to 1000 nm, and the intermediate layer being a porous body having an average pore diameter of 1 nm to 20 nm. <1> ~ <3> 13. The hydrogen production device according to claim 12, <5> The intermediate layer has an amorphous silica layer inside the pores and on the surface of the intermediate layer. <4> The hydrogen separation device according to claim 1.
[0012] <6> A hydrogen separation membrane comprising an aluminum oxide porous support having an average pore diameter of 30 nm to 1000 nm, and an amorphous silica layer formed on one surface of the porous support, the amorphous silica layer being made of dimethoxydimethylsilane-derived amorphous silica and having an average pore diameter of 0.2 nm to 0.3 nm. <7> The intermediate layer has an amorphous silica layer inside the pores and on the surface of the intermediate layer, the thickness of the hydrogen separation active region in the amorphous silica layer is 5 nm to 15 nm, and the film length of the amorphous silica layer is 6 cm or more. <6> The hydrogen separation membrane according to claim 1. <8> A method for manufacturing a hydrogen separation membrane, comprising the step of forming an amorphous silica layer having an average pore diameter of 0.2 nm to 0.3 nm on one side of a porous aluminum oxide body having an average pore diameter of 30 nm to 1000 nm by a chemical vapor deposition method using dimethoxydimethylsilane as a silica source. <9> The chemical vapor deposition method is a counter diffusion chemical vapor deposition method (counter diffusion CVD method). <8> A method for producing the hydrogen separation membrane according to claim 1. Effect of the Invention
[0013] According to one embodiment of the present invention, it is possible to provide a hydrogen production device capable of efficiently producing hydrogen from biogas without using a precious metal such as palladium as a membrane material. According to another embodiment of the present invention, it is possible to provide a hydrogen separation membrane having good hydrogen separability and durability that can be used in a hydrogen production device, and a method for producing a hydrogen separation membrane having good hydrogen separability and durability. [Brief description of the drawings]
[0014] [Figure 1] 1 is a schematic configuration diagram showing one embodiment of a hydrogen production device according to the present disclosure. [Diagram 2] FIG. 2 is a schematic cross-sectional view of a membrane reactor used in the hydrogen production device shown in FIG. [Diagram 3] FIG. 2 is a schematic cross-sectional view showing another embodiment of a membrane reactor that can be used in a hydrogen production device. [Figure 4]2 is a partially enlarged cross-sectional view showing one embodiment of a hydrogen separation membrane used in the hydrogen production apparatus shown in FIG. [Diagram 5] FIG. 2 is a schematic diagram of an amorphous silica layer in a hydrogen separation membrane used in the hydrogen production device shown in FIG. [Figure 6] 1 is a graph showing the relationship between hydrogen / nitrogen selectivity and hydrogen permeability in an example of a hydrogen separation membrane of the present disclosure. [Figure 7] 4 is an Arrhenius plot showing the temperature dependence of hydrogen permeability and nitrogen permeability in a dry atmosphere after the formation of the hydrogen separation membrane in the hydrogen production apparatus of Example 1. [Figure 8] Graph (A) shows the relationship between the methane supply amount and the methane conversion rate in a mixed gas containing 70 vol. % methane and 30 vol. % carbon dioxide in the hydrogen production apparatus of Example 1 and the hydrogen production apparatus of Comparative Example 1, and graph (B) shows the relationship between temperature and the methane conversion rate. [Figure 9] Graph (A) shows the relationship between the methane supply amount and the methane conversion rate in a mixed gas containing 50 vol. % methane and 50 vol. % carbon dioxide for the hydrogen production apparatus of Example 1 and the hydrogen production apparatus of Comparative Example 1, and graph (B) shows the relationship between the temperature and the methane conversion rate. [Figure 10] 4 is a graph showing the change over time in methane conversion rate when the mixture composition of methane and carbon dioxide in the mixed gas is changed every six hours in the hydrogen production device of Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The hydrogen production device, hydrogen separation membrane, and method for producing a hydrogen separation membrane of the present disclosure will be described in detail below with reference to specific embodiments. The present disclosure is not limited to the following embodiments, and can be implemented in various modified forms as long as they are within the scope of the present disclosure. Modifications include, for example, scaling up the device, replacing each component in the device with a component having equivalent performance, changing the position of each component in the device as long as the effect is not impaired, and changing the type, amount, and packing mode of the catalyst that constitutes the hydrogen separation membrane.
[0016] In the present disclosure, a numerical range described using "~" indicates a numerical range including the numerical values before and after "~" as the lower and upper limits. In the numerical ranges described in stages in the present disclosure, the upper or lower limit described in a certain numerical range may be replaced with the upper or lower limit of another numerical range described in stages. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit described in a certain numerical range may be replaced with a value shown in the examples. In the present disclosure, the term "process" includes not only an independent process but also a process that cannot be clearly distinguished from other processes as long as the intended purpose of the process is achieved. In the present disclosure, when a plurality of substances corresponding to each component are present in the composition, the amount of each component in the composition means the total amount of the plurality of substances present in the composition, unless otherwise specified. Also, in the present disclosure, combinations of two or more preferred aspects are more preferred aspects. In the drawings, components that are designated by the same reference numerals are meant to be the same components. The dimensional ratios in the drawings do not necessarily represent the actual dimensional ratios.
[0017] <Hydrogen production equipment> One embodiment of the hydrogen production device disclosed herein includes a biogas supplyer that supplies biogas, a membrane reactor inside a cylinder in which a catalyst for producing hydrogen gas from the biogas supplied from the biogas supplyer and a hydrogen separation membrane that selectively allows hydrogen gas to permeate are disposed, and a recovery device that recovers hydrogen gas with a purity of 99% or more separated by the membrane reactor, the hydrogen separation membrane being composed of a porous support and an amorphous silica layer formed on the porous support and having an average pore diameter of 0.3 nm or less.
[0018] As another embodiment of the hydrogen production device of the present disclosure, there is provided a biogas supplying device for supplying biogas, a membrane reactor in which a catalyst for producing hydrogen gas from the biogas supplied from the biogas supplying device and a hydrogen separation membrane that selectively permeates hydrogen gas are disposed inside a cylindrical body, and a recovery device for recovering hydrogen gas with a purity of 99% or more separated by the membrane reactor, the hydrogen separation membrane being formed on a porous support and having a hydrogen permeability of 2×10 or more as measured by the following measurement method. -7 mol m -2 s -1 Pa -1 and an amorphous silica layer having a gas permeability to gases other than hydrogen gas and helium gas of 1 / 100 or less of the hydrogen permeability. (Measurement method) Hydrogen gas is supplied to the supply side of the hydrogen separation membrane after the membrane is formed, and the supply side pressure is set to 0.2 MPaG. Hydrogen gas is allowed to permeate using a dead-end method with a transmembrane pressure difference of 0.2 MPa. The flow rate of the permeated gas obtained from the permeation side is measured using a soap film flowmeter, and the hydrogen gas permeability is calculated from the obtained permeated gas flow rate. The measurement is performed at 500°C. The average pore size of the amorphous silica layer in the hydrogen separation membrane is 0.3 nm or less, and the amorphous silica layer functions as an active layer for hydrogen separation. The hydrogen permeability of the hydrogen separation membrane at 500°C measured above is 2×10 -7 mol m -2 s -1 Pa -1 This is estimated based on the above and the fact that the gas permeability of gases other than hydrogen gas and helium gas is 1 / 100 or less of the hydrogen permeability. The gas permeability of the hydrogen separation membrane to be evaluated for gases other than hydrogen gas and helium gas can be measured, for example, by the method described in Journal of Membrane Science Vol. 251 (2005) pp. 151-158.
[0019] The hydrogen production device of the present disclosure will be described with reference to the drawings. Fig. 1 is a schematic diagram showing an embodiment of a hydrogen production device according to the present disclosure. The hydrogen production device 10 shown in Fig. 1 includes a biogas supply device 12, a pipe 24A connected to the biogas supply device 12 for conveying the biogas supplied from the biogas supply device 12 to a membrane reactor 14A, and the membrane reactor 14A for treating the biogas. In the embodiment shown in FIG. 1, the membrane reactor 14A is provided with, inside a hollow cylinder, a catalyst 18 for producing hydrogen gas from biogas, and a hydrogen separation membrane 16 that selectively allows permeation of high-purity hydrogen gas produced by the catalyst, specifically, hydrogen gas with a purity of 99% or more. The biogas conveyed from pipe 24A is supplied to the center of the inner cylinder (hydrogen separation membrane) filled with catalyst 18, and is separated into hydrogen gas and carbon dioxide by the function of catalyst 18 to produce hydrogen gas. The produced hydrogen gas passes through hydrogen separation membrane 16 and is guided between hydrogen separation membrane 16, which is the outermost layer of membrane reactor 14A consisting of a double cylinder, and the outer cylinder, and is discharged to the outside of membrane reactor 14A. The extracted hydrogen gas is supplied to a gas-liquid separator 20A equipped with a cooler via a pipe 24A equipped with a temperature control device 24B for the pipe, where the remaining water vapor is separated into water and the high-purity hydrogen gas is recovered via the pipe 24A in a hydrogen gas recovery device (not shown).
[0020] The temperature control device for the pipe is appropriately selected from known temperature control devices depending on the size, material, etc. of the pipe in the hydrogen production device. In general, a heater having a temperature control function can be used. In a small-scale hydrogen production device, a ribbon heater can be used. A temperature control device 22 for controlling the temperature inside the membrane reactor 14A is attached to the outside of the membrane reactor 14A, and controls the temperature inside the membrane reactor 14A to a temperature suitable for reaction efficiency. A pipe temperature control device 24B is attached to the outside of the pipe 24A connecting the biogas supply device 12 and the membrane reactor 14A, and the pipe 24A for discharging the obtained hydrogen gas, and the temperature is controlled within a range that does not cause liquefaction of the gas transported through the pipe. The mixed gas containing carbon dioxide from which hydrogen gas has been separated in the membrane reactor 14A passes through the center of the cylindrical membrane reactor 14A and is discharged to the outside of the membrane reactor 14A. The discharged mixed gas is supplied to a gas-liquid separator 20B equipped with a cooler via a pipe 24A equipped with a temperature control device 24B for the pipe, and the remaining water vapor is separated as water in the gas-liquid separator 20B and collected in a collector (not shown).
[0021] Fig. 2 is a schematic cross-sectional view of the membrane reactor 14A of the hydrogen production device 10 shown in Fig. 1. As shown in Fig. 2, the membrane reactor 14A has a double-tube structure consisting of a cylindrical outer tube 17 and an inner tube made of a hydrogen separation membrane 16. Biogas is introduced into a flow path inside a cylindrical inner tube, a hydrogen separation membrane 16 filled with a catalyst 18, and hydrogen produced by the catalyst 18 passes through the hydrogen separation membrane 16 in the direction of the arrow shown in Figure 2 and is discharged into the space between the double cylindrical hydrogen separation membrane 16 and the outer tube 17. In the cylindrical membrane reactor 14A shown in FIG. 2, the catalyst 18 is filled in the center of the cylindrical membrane reactor 14A, i.e., inside the inner tube which is the hydrogen separation membrane 16, but the embodiment of the membrane reactor is not limited to this. Fig. 3 is a schematic cross-sectional view showing another embodiment of a cylindrical membrane reactor. In the membrane reactor 14B shown in Fig. 3, a catalyst 18 is filled in the space between the hydrogen separation membrane 16 and the outer tube 17 of the cylindrical membrane reactor 14B. In the membrane reactor 14B shown in Fig. 3, the biogas supplied from the biogas supplier 12 is introduced into the space between the outer tube 17 and the hydrogen separation membrane 16 of the cylindrical membrane reactor 14B, and the hydrogen gas generated by the catalyst 18 passes through the hydrogen separation membrane 16, which is a cylindrical inner tube of a double structure, in the direction of the arrow shown in the figure, and is led to the inside of the hydrogen separation membrane 16 in the cylindrical membrane reactor 14B. In addition, FIG. 3 shows an embodiment in which only one hydrogen separation membrane 16 is provided in the outer tube 17, but this is not limited to this, and the structure may also include a plurality of hydrogen separation membranes provided in the outer tube.
[0022] The membrane reactor may have any shape as long as it is partitioned by a hydrogen separation membrane into an area containing a catalyst for producing hydrogen from biogas and an area for extracting the hydrogen thus produced. Among these, the double-structured cylindrical reactor shown in Figures 2 and 3, in which the inner cylinder is a hydrogen separation membrane 16, is preferred because it has a simple structure and can efficiently separate hydrogen. The size of the cylindrical membrane reactor shown in FIG. 2 and FIG. 3 can be arbitrarily selected depending on the purpose. From the viewpoint of being able to set the size of the hydrogen production device in an appropriate range, the outer diameter is preferably in the range of 30 mm to 150 mm, and more preferably in the range of 40 mm to 80 mm. The outer diameter of the inner cylinder equipped with the hydrogen separation membrane is preferably in the range of 5 mm to 20 mm, and more preferably in the range of 5 mm to 10 mm. If the length of the membrane reactor, ie, the length of the cylinder of a cylindrical membrane reactor, is long, a hydrogen separation membrane having a larger size can be accommodated. From the viewpoint of producing a sufficient amount of hydrogen, the membrane length of the hydrogen separation membrane housed in the membrane reactor is preferably 6 cm or more, and more preferably 8 cm or more. Note that the membrane length of the hydrogen separation membrane means the length from the end of the hydrogen separation membrane housed in the membrane reactor on the biogas inlet side to the end on the opposite side.
[0023] When the size of the membrane reactor is within the above range, more efficient hydrogen production becomes possible. One hydrogen production device may include only one membrane reactor, or may include two or more membrane reactors. The membrane reactors may be provided in parallel or in series, but from the viewpoint of hydrogen production efficiency, it is preferable to arrange multiple membrane reactors in parallel. In order to further increase the amount of hydrogen produced, it is possible to arrange two or more membrane reactors in parallel for one hydrogen production device. The number of membrane reactors for one hydrogen production device can be appropriately selected depending on the purpose of the hydrogen production device. For example, when a hydrogen production device is installed in a sewage treatment facility, it is possible to install more than 1,000 membrane reactors to process a large amount of biogas.
[0024] The catalyst packed in the membrane reactor to produce hydrogen from biogas is not particularly limited, and any known reforming catalyst can be used. As the reforming catalyst, a catalyst containing nickel (Ni), rhodium (Rh), ruthenium (Ru), or the like as an active species can be used. The catalyst may be commercially available or may be prepared from a metal precursor. An example of a commercially available product is reforming catalyst TRC10-2A (product name, diameter approximately 2 mm) manufactured by Tanaka Kikinzoku Kogyo Co., Ltd. As a method for preparing the catalyst, for example, Ni catalyst is prepared by adding Ce to the precursor, Nickel (II) Nitrate Hexahydrate aqueous solution, with Ni as the active species. 0.15 Zr 0.85 O2 is added to cause a reaction, then dried and powdered, which is extracted and fired in an electric furnace at a temperature of about 500°C to 600°C, and then heated at another temperature of about 500°C to 600°C and reduced with hydrogen to obtain the desired product. The catalyst is usually a spherical carrier carrying a metal precursor for the catalyst. The size of the catalyst depends on the size of the carrier, and for Ni catalyst, it can be 400 μm to 2000 μm, and preferably 500 μm to 750 μm. The Rh catalyst is preferably an Rh / ALO-6 catalyst obtained by impregnation using γ-alumina as a support. The average particle size of the spherical ALO-6 support is about 1.6 mm. The amount of catalyst packed in the membrane reactor may be appropriately selected depending on the purpose.
[0025] <Hydrogen separation membrane> Fig. 4 is a partially enlarged cross-sectional view showing one embodiment of the hydrogen separation membrane 16 used in the hydrogen production device 10. The hydrogen separation membrane 16 shown in Fig. 4 has an amorphous silica layer 30 having a hydrogen separation function on one surface of a porous support 25. As described later, the amorphous silica layer may be formed not only on the surface of the porous support 25 but also inside the pores of the porous support 25. The porous support 25 that holds the amorphous silica layer 30 can be any support having pores that are gas permeable, without any particular limitations. In the embodiment shown in FIG. 4, the porous support 25 has a two-layer structure consisting of a support layer 26 and an intermediate layer 28, and it is preferable that the support layer 26 is a porous body having an average pore diameter of 50 nm to 200 nm, and the intermediate layer 28 is a porous body having an average pore diameter of 3 nm to 5 nm. The use of a two-layer porous support 25 as shown in FIG. 4, which includes a support layer 26 that has good strength, gas permeability, and is cost-effective, and an intermediate layer 28 that has better retention of the amorphous silica layer 30 and has smaller pores than the support layer 26, is preferable from the viewpoint of more stably fixing the amorphous silica layer and ensuring that the amorphous silica layer remains stable for a longer period of time. In the present disclosure, the surface of the intermediate layer opposite to the surface in contact with the support layer is referred to as the "surface of the intermediate layer."
[0026] In the two-layered porous support, an amorphous silica layer is provided at least on the side of the intermediate layer opposite to the support layer side. The amorphous silica layer may be formed only on the surface of the intermediate layer, or the amorphous silica layer may be formed not only on the surface of the intermediate layer but also extending into the pores of the intermediate layer. In particular, in a porous support having a two-layer structure, it is preferable that an amorphous silica layer is provided inside the pores of the intermediate layer and on the surface of the intermediate layer. It is believed that the amorphous silica layer in the pores is denser and more stable when filled in the pores, and therefore the amorphous silica layer functions as a molecular sieve more effectively, and the amorphous silica layer functions as a separation active region with good hydrogen separation function. The separation active region will be described later.
[0027] Here, "having an amorphous silica layer inside the pore" refers to both the state where the amorphous silica layer is formed on the inner wall surface of the pore and the state where the pore is filled with an amorphous silica layer. For example, when forming an amorphous silica layer by a chemical vapor deposition method described later, a silica precursor in a gaseous state penetrates into the inside of the pore and is converted into an amorphous silica layer on the inner wall surface of the pore. If the chemical vapor deposition is continued, the thickness of the amorphous silica layer formed on the inner wall surface of the pore increases, and the inside of the pore diameter may be filled with an amorphous silica layer. Either of these is referred to as having an amorphous silica layer inside the pore. A preferred embodiment of the hydrogen separation membrane of the present disclosure includes an embodiment having an amorphous silica layer inside the pores of the intermediate layer and on the surface of the intermediate layer, the thickness of the hydrogen separation active region in the amorphous silica layer being 5 nm to 15 nm, and the membrane length of the amorphous silica layer being 6 cm or more.
[0028] As the porous support, porous ceramics are preferred because they have an appropriate pore size and are easily available. Metal oxides, metal nitrides, and metal nitrides are preferred because they have good heat resistance. More specifically, supports such as alumina, silica, titania, zirconia, and magnesia are preferred, with α-alumina supports being more preferred. In the case of a tubular porous support, for example, a porous tubular support having an outer diameter of about 3 mm to 20 mm, an inner diameter of about 1 mm to 15 mm, and a tube thickness of about 1 mm to 3 mm is suitable. The average pore diameter of the porous support is preferably in the range of 30 nm to 1000 nm, more preferably in the range of 50 nm to 500 nm, and further preferably in the range of 80 nm to 180 nm.
[0029] As a porous support having a two-layer structure, a support layer made of tubular α-alumina having an average pore diameter of 20 nm to 1000 nm, preferably 80 nm to 180 nm, and a γ-alumina layer having an average pore diameter of 1 nm to 20 nm, preferably 3 nm to 5 nm, serving as an intermediate layer on the outer surface of the tubular support layer is preferred. The thickness of the support layer can be selected arbitrarily depending on the purpose. Considering the size of the hydrogen production device, the thickness of the support layer can be 0.5 mm to 3 mm, and a range of 1 mm to 2 mm is preferable from the viewpoint of the balance between strength and gas permeability. The thickness of the intermediate layer can usually be set to 0.5 μm to 10 μm, and is preferably in the range of 1 μm to 5 μm.
[0030] There is no particular limitation on the method for providing an intermediate layer on a support layer serving as a porous support, and any known method for producing a porous layer can be appropriately applied. Among these, when the support layer is made of a material having good heat resistance such as alumina, a method of coating the support layer with an intermediate layer forming material containing boehmite sol, which will be described in detail below, and firing the same is preferred. According to the method of forming an intermediate layer using an intermediate layer forming material containing boehmite sol, an intermediate layer of any thickness can be formed by adjusting the coating amount of the intermediate layer forming material, the firing temperature, and further by carrying out coating and firing multiple times.
[0031] As a method for producing a porous support having a two-layer structure, for example, a method is available in which the outer surface of a ring of a tubular porous support layer made of α-alumina is dip-coated with boehmite sol as an intermediate layer forming material two to three times, and then fired to form a γ-alumina intermediate layer having an average pore size of 3 nm to 5 nm. When coating the intermediate layer forming material onto the tubular support layer, it is preferable to carry out a process such as sealing the ends of the ring to prevent the intermediate layer forming material from penetrating into the inside of the ring, which is the support layer. The boehmite sol can be produced by a conventional method using aluminum s-butoxide (ALSB), 2-propanol, and gallium (III) nitrate-8-hydrate, or using aluminum s-butoxide (ALSB), 2-propanol, and 1 mol / L (liter) nitric acid.
[0032] The average pore size of the porous support can be measured by measuring the pore size distribution using a through-pore size evaluation device based on the ASTM F316-86 (JIS K 3832) bubble point method. Examples of the device used for the measurement include a Perm Porometer manufactured by Seika Digital Image Co., Ltd.
[0033] Fig. 5 is a schematic diagram of an amorphous silica layer 30 in a hydrogen separation membrane 16. In Fig. 5, the amorphous silica layer is shown diagrammatically, with silicon (Si) atoms shown as black circles and oxygen atoms shown as white circles. As shown in Fig. 5, an amorphous silica layer made of Si atoms and oxygen atoms has an amorphous structure in which siloxane bonds shown as Si-O-Si form a three-dimensional network, and it is believed that the three-dimensionally formed network structure of silicon dioxide plays a role as a molecular sieve. In the amorphous silica layer of the present disclosure, the average pore size of the pores formed by the network structure of silicon dioxide is 0.3 nm or less, so hydrogen (molecular size 0.289 nm) and water vapor (molecular size 0.265 nm) can pass through, but methane (molecular size 0.38 nm) and carbon dioxide (molecular size 0.33 nm) contained in biogas cannot pass through. Furthermore, since silica is hydrophobic, water vapor is less likely to pass through the amorphous silica layer than hydrogen. Therefore, it is considered that hydrogen can be separated efficiently by an amorphous silica layer with an average pore size of 0.3 nm or less. For example, even if a small amount of water vapor passes through the hydrogen separation membrane, the water vapor is recovered as water in a gas-liquid separator installed downstream of the device, so that highly pure hydrogen is produced. The average pore size of the amorphous silica layer being 0.3 nm or less and functioning as an active region for hydrogen separation in the amorphous silica layer can be expressed, for example, by a hydrogen separation membrane comprising a porous support and an amorphous silica layer, a recovery device for recovering hydrogen gas with a purity of 99% or more, and a hydrogen permeability of the hydrogen separation membrane measured by the above-mentioned measurement method being 2×10 -7 mol m -2 s -1 Pa -1This is estimated based on the above and the fact that the gas permeability of gases other than hydrogen gas and helium gas is 1 / 100 or less of the hydrogen permeability.
[0034] The hydrogen permeability of the hydrogen separation membrane used in the hydrogen production device of the present disclosure measured separately after film formation is as described above. However, when this hydrogen separation membrane is incorporated into a membrane reactor and the hydrogen production device is actually operated, the hydrogen permeability of the membrane reactor tends to be lower than the hydrogen permeability of the hydrogen separation membrane measured separately after film formation, because the gas to be separated contains water vapor. The hydrogen permeability of the membrane reactor is 5×10 -8 mol m -2 s -1 Pa -1 If it is above 1×10, it is at a level where there is no practical problem. -7 mol m -2 s -1 Pa -1 More preferably, it is equal to or greater than this.
[0035] <Method of manufacturing hydrogen separation membrane> There is no particular limitation on the method for producing the hydrogen separation membrane that can be used in the hydrogen production device of the present disclosure, and any method for forming an amorphous silica layer on the surface of a known porous support can be used. Examples of the method for producing the amorphous silica layer include the sol-gel method and the chemical vapor deposition method (hereinafter sometimes referred to as the CVD method). Among them, from the viewpoint of obtaining an amorphous silica layer having better durability, particularly water vapor resistance, the method of forming a silica source on a porous support by a CVD method is preferred. A large number of silanol groups remain in the silica layer formed by a sol-gel method, but the present inventors believe that the amorphous silica layer obtained by the CVD method has fewer silanol groups remaining, and therefore has better water vapor resistance.
[0036] CVD methods used for forming an amorphous silica layer include a one-way diffusion CVD method in which a silica precursor derived from a silica source and an oxidizing agent, preferably oxygen, are supplied to one side of a porous support to form an amorphous silica layer, and a counter diffusion CVD method in which a silica precursor derived from a silica source is supplied to one side of a porous support and an oxidizing agent is supplied to the other side of the porous support. In particular, according to the counter diffusion CVD method, by keeping both sides of the porous support at equal pressure, the silica precursor diffused in the pores of the porous support comes into contact with the oxidizing agent in the pores to generate silica, and an amorphous silica layer is formed on the pore walls in the porous pores, and the reaction automatically ends when the pores are filled with the silica layer. Meanwhile, in the porous support, the reaction between the silica precursor and oxygen continues in the pores that are not filled with the silica layer. Therefore, the reaction continues until all the pores are filled with the amorphous silica layer, making it easy to obtain a high-performance amorphous silica layer with good reproducibility. In other words, by using the counter diffusion CVD method, it is possible to easily produce a hydrogen separation membrane having an amorphous silica layer not only on the surface of the intermediate layer of the double-structure porous support, which is the preferred embodiment described above, but also inside the pores of the intermediate layer.
[0037] For example, the amorphous silica layer is formed by counter diffusion CVD, in which a silicon compound as a silica source is placed in a bubbler and heated while supplying nitrogen gas, and the vapor of the silicon compound is supplied into the housing. The temperature inside the housing can be 300°C to 650°C. The vapor of the silicon compound as a silica source inside the housing is supplied to one side of a porous support, and oxygen is circulated to the other side to react the two inside the porous support. The reaction is carried out with a silicon compound vapor concentration of approximately 0.93 mol / m in the case of a tubular porous support with a membrane length of 10 mm to 100 mm. 3 With an oxygen flow rate of 200 mL / min, a sufficient amount of amorphous silica layer is formed in about 60 minutes. Thereafter, the supply of the silicon compound vapor is stopped, the inside of the housing is purged with oxygen, the supply of oxygen is stopped, and nitrogen is supplied into the inside of the porous support for purging to obtain an amorphous silica layer.
[0038] Examples of silica sources that can be used to produce the amorphous silica layer include dimethoxydimethylsilane (DMDMS), tetraethylorthosilicate (TEOS), hexamethyldisiloxane (HMDS), tetramethylorthosilicate (TMOS), trimethyloxy(methyl)silicate (TMMS), methoxytrimethylsilicate (MTMS), phenyltrimethoxysilane (PTMS), dimethoxydiphenylsilane (DMDPS), triethoxyethylsilane, diethoxydiethylsilane, ethoxytriethylsilane, methoxytriphenylsilane, and the like. The abbreviation for the compound is written in parentheses after the compound name, and hereinafter each compound may be referred to by the abbreviation in parentheses. The structures of DMDMS, TEOS, HMDS, TMOS, TMMS, MTMS, PTMS, and DMDPS are shown below.
[0039] [ka]
[0040] Among them, as the silica source which easily forms an amorphous silica layer having pores of 0.3 nm or less, DMDMS, TMOS, HMDS, TEOS, TMMS, MTMS, etc. are preferable, and DMDMS is more preferable. That is, it is more preferable that the silica layer is an amorphous silica layer derived from a silica source containing DMDMS.
[0041] The method for producing a hydrogen separation membrane of the present disclosure preferably includes a step of forming an amorphous silica layer having an average pore diameter of 0.2 nm to 0.3 nm on an aluminum oxide porous body having an average pore diameter of 30 nm to 1000 nm by a CVD method using a silica source containing dimethoxydimethylsilane. As described above, the porous support has a two-layer structure including at least a support layer and an intermediate layer, the support layer being preferably a porous body having an average pore diameter of 50 nm to 200 nm and the intermediate layer being preferably a porous body having an average pore diameter of 3 nm to 5 nm, and it is more preferable to form an amorphous silica layer not only on the surface of the intermediate layer but also within the pores of the intermediate layer of the two-layer support by a counter diffusion CVD method. An example of the method for producing the porous support having a two-layer structure is as described above.
[0042] The thickness of the support layer and the intermediate layer in the porous support can be measured by cutting the hydrogen separation membrane to obtain a cross section, platinum sputtering the cross section, and observing it with a field emission scanning electron microscope (FE-SEM). An example of the FE-SEM device is JSM-6701F (manufactured by JEOL Ltd.). The acceleration voltage of the FE-SEM can be, for example, 10.0 kV.
[0043] There is no particular limit to the thickness of the amorphous silica layer. In general, the thicker the silica layer in the hydrogen separation membrane, the better the hydrogen separation efficiency, but the lower the gas permeability. From this point of view, the thickness of the separation active region in the amorphous silica layer can be 5 nm to 100 nm, and is preferably in the range of 5 nm to 15 nm. Here, the separation active region in the amorphous silica layer refers to a region in the amorphous silica layer that is dense and contributes to hydrogen separation. The present inventors presume that a region of the amorphous silica layer formed inside the pores of the intermediate layer and having a denser structure functions as a separation active region with higher hydrogen separation activity than a silica film formed in a free state on the surface of the intermediate layer that does not have pores, and this region is called the separation active region in the amorphous silica layer. The separation active region in the amorphous silica layer can be confirmed as a region where Al2p increases and Si2p decreases from the elemental composition in the depth direction of the formed amorphous silica layer as a result of analysis by X-ray photoelectron spectroscopy (XPS) described later.
[0044] The thickness of the amorphous silica layer and the thickness of the separation active region in the amorphous silica layer can be measured by performing elemental composition analysis of the amorphous silica layer in the formed hydrogen separation membrane from the surface opposite to the porous support side in the membrane depth direction by X-ray photoelectron spectroscopy (hereinafter referred to as XPS). In this disclosure, an XPS VG ESCALAB 250 spectrometer (manufactured by Thermo Fisher Scientific) equipped with an Al K radiation source is used, and the chamber pressure is 10 -8 The values were measured at less than Pa and an etching rate of 0.05 nm / s. The elements and electron orbitals analyzed by XPS were Si: 2p, Al: 2p, O: 1s, and C: 1s.
[0045] The hydrogen separation membrane used in the hydrogen production device of the present disclosure is preferably an aluminum oxide porous support having an average pore diameter of 30 nm to 1000 nm, and an amorphous silica layer on one side of the porous support, the amorphous silica layer including a separation active region having an average pore diameter of 0.2 nm to 0.3 nm, derived from a silica source containing dimethoxydimethylsilane, and more preferably a hydrogen separation membrane in which an amorphous silica layer is formed all the way to the inside of the pores of the porous support.
[0046] The hydrogen separation membrane of the present disclosure has good hydrogen separation properties and gas permeability. The gas permeability (also referred to as gas transmission rate) of a hydrogen separation membrane can be measured by the following method. When the flow rate of the permeating gas is relatively high, for example, about 1 mL / min or more, the gas permeability can be measured using a bubble flow meter (hereinafter also referred to as BFM). On the supply side, for example, in the case of a membrane reactor having the cross-sectional view shown in Figure 2, gas is supplied to the outside of the tubular porous support (the outside of the tubular porous support, i.e., the side having the hydrogen separation membrane) to set the supply side pressure to 0.2 MPaG, and the gas is allowed to permeate by a dead-end method with a transmembrane pressure difference of 0.2 MPa, and the flow rate of the permeated gas obtained from the permeation side (the inside of the tubular porous support, i.e., the support layer side of the porous support) can be measured using a soap film flow meter (BFM) (manufactured by Horiba, Ltd.).
[0047] When the permeation gas flow rate is small and cannot be measured by BFM, the flow rate of the permeation gas is measured by the pressure change method. In the pressure change method, the supply side pressure is set to 0.25 MPaG, and the permeation side is evacuated for at least one hour using an oil rotary vacuum pump (manufactured by ULVAC, Inc.), giving a transmembrane pressure difference of approximately 0.35 MPa. By cutting off the line leading to the vacuum pump on the permeation side, the permeation gas accumulates on the permeation side and the pressure rises, so the rate of this pressure rise can be measured and the amount of permeation gas can be calculated from the volume of the permeation side.
[0048] <Hydrogen permeation rate in hydrogen production equipment> The relationship between the hydrogen permeability and the theoretical value of the hydrogen selectivity over nitrogen for a hydrogen separation membrane having an amorphous silica layer prepared by the counter-diffusion CVD method using DMDMS as the silica source is shown as a white circle (○) in Figure 6. According to the study by the present inventors, the selectivity of hydrogen to nitrogen (H2 / N2) is 10 3 In FIG. 6, the H2 / N2 selectivity is preferably 10 3 The line is indicated by a dashed line. In other words, the range beyond this dashed line is the range in which H2 / N2 selectivity is preferable.
[0049] Figure 6 shows the results for hydrogen separation membranes produced by the CVD method (CVD: represented by black circles: ●), the results for hydrogen separation membranes produced by the plasma CVD method (PECVD: represented by white triangles: △), and the results for hydrogen separation membranes produced by the sol-gel method (sol-gel: represented by white squares: □). All of the hydrogen separation membranes shown above were produced using a silica source other than DMDMS. It is generally known that there is a trade-off between gas permeability and selectivity between different gases. As can be seen in Figure 6, the H2 / N2 selectivity is 10 3 In the range above 1000 nm, the hydrogen separation membrane of the present disclosure, which is equipped with a silica membrane produced by counter-diffusion CVD using DMDMS used in the hydrogen production device of the present disclosure, exhibits the best hydrogen permeability. This shows that the hydrogen separation membrane of the present disclosure achieves both high levels of H2 / N2 gas selectivity and hydrogen permeability. Thus, the hydrogen-permeable membrane used in the hydrogen production device of the present disclosure is expected to have both good hydrogen permeability and good hydrogen selectivity. EXAMPLES
[0050] Below, the hydrogen production device and hydrogen separation membrane of the present disclosure will be specifically described together with their manufacturing methods using examples. However, the present disclosure is not limited to the following examples and can be embodied in various modified examples as long as they do not deviate from the spirit of the present disclosure. In addition, "%" indicating the mixing ratio of gas represents "volume %" unless otherwise specified.
[0051] Example 1 - Manufacturing of hydrogen separation membranes - 1. Preparation of Porous Support (1-1. Preparation of porous substrate) A tubular α-alumina substrate (manufactured by Noritake Co., Ltd.) was used as the support layer of the porous support. The tubular substrate had an outer diameter of 6 mm, an inner diameter of 4 mm, and a pore diameter of 150 nm according to the catalog value. The tubular substrate was cut to a length of 120 mm using a diamond cutter, and both ends of 20 mm were glass sealed. Therefore, in the tubular substrate with a length of 120 mm, the portion that functions as a porous substrate, that is, the portion that functions as a hydrogen separation membrane by forming a silica membrane described later, is 80 mm (8 cm) long.
[0052] (1-2. Preparation of Coating Solution for Forming Intermediate Layer) The prepared substrate was coated with γ-alumina to form an intermediate layer. 500 g of aluminum s-butoxide (ALSB: Fujifilm Wako Pure Chemical Industries, Ltd.), 500 mL of 2-propanol (Fujifilm Wako Pure Chemical Industries, Ltd.), and 25 g of gallium(III) nitrate 8-hydrate (Fujifilm Wako Pure Chemical Industries, Ltd.) were prepared. The boehmite sol was prepared in a nitrogen-substituted glove box (manufactured by AS ONE Corporation).
[0053] 3.60 g (0.06 mol) of 2-propanol was placed in a beaker to wet the inner wall of the beaker. 24.6 g (0.10 mol) of ALSB was added directly from the reagent bottle to the beaker whose wall was wetted, and the mixture was stirred for 1 hour. 360 mL of pure water was placed in a 500 mL beaker and heated to 90° C. on a hot stirrer. The 500 mL beaker was replenished with pure water as needed using pure water for adjusting the liquid level. In a glove box, the mixture of ALSB and 2-propanol was placed in a 100 mL dropping bottle, and a nitrogen balloon was attached to the top of the dropping bottle. The dropping bottle with the nitrogen balloon attached was removed from the glove box, and the 90°C pure water prepared on a hot stirrer was vigorously stirred, and the mixture of ALSB and 2-propanol was dropped into it. Stirring was continued at 90° C. until 2-propanol was evaporated. Evaporation of 2-propanol was confirmed by the disappearance of the alcohol odor. Gallium (III) nitrate 8-hydrate (17.14 g, 0.04 mol) was added to pure water (108 g, 6 mol), and the mouth of the beaker was covered with Parafilm (product name, plastic paraffin film, LMS Co., Ltd.) and stirred for at least 1 hour to prepare an aqueous gallium nitrate solution. The 2-propanol was evaporated and the mixture was transferred to a 500 mL Erlenmeyer flask, the mouth of the Erlenmeyer flask was covered with aluminum foil and allowed to cool. After cooling, the gallium nitrate solution was slowly added dropwise with vigorous stirring. After stirring for 12 hours or more, a boehmite sol was obtained.
[0054] The obtained boehmite sol was used to prepare a coating liquid. 47.5 mL of pure water was placed in a 50 mL graduated cylinder, and 2.5 mL of 1M-HNO3 (FUJIFILM Wako Pure Chemical Industries, Ltd.) was added. This solution was transferred to a 100 mL Erlenmeyer flask containing a stirrer. 1.75 g of Poly(vinyl alcohol) 500 [Completely Hydrolyzed (PVA) (FUJIFILM Wako Pure Chemical Industries, Ltd.)] was added to the 100 L Erlenmeyer flask while gently stirring with a stirrer to avoid foaming. The 100 mL Erlenmeyer flask was transferred to a hot plate stirrer, and the poorly soluble PVA was heated and dissolved. The mouth of the Erlenmeyer flask was sealed with aluminum foil, and stirring was continued while heating to 90°C. After 40 minutes, the mixture was left to cool while still stirring, and a PVA solution was obtained. 20 mL of the obtained PVA solution and 30 mL of the boehmite sol obtained above were placed in a 50 mL beaker, a stirrer was placed inside, the mouth of the beaker was covered with parafilm, and the mixture was stirred for 15 minutes to obtain a coating solution.
[0055] (1-3. Formation of the intermediate layer) In order to form an intermediate layer on the outer surface of the tubular support layer (substrate) prepared in 1-1, one side of the substrate, i.e., the lower side during dipping, was sealed with sealing tape to prevent the coating solution from penetrating inside the tubular substrate. The coating solution obtained in 1-2 was poured into a test tube while being careful not to trap air bubbles, and a substrate with a total length of 120 mm was dipped into the coating solution for 5 seconds. When inserting and removing the substrate, care was taken not to touch the wall of the test tube. The dipped substrate was placed in an electric muffle furnace KM-600 (Advantec Corporation), first heated to 60°C and held there for 3 hours, then the temperature inside the furnace was raised from 60°C to 600°C over 6 hours, held at 600°C for 3 hours, and then cooled to room temperature (25°C) over 3 hours. This dip coating and firing process was repeated three times to produce a porous support with a two-layer structure in which an α-alumina support layer was laminated with a γ-alumina intermediate layer. For the purpose of measuring the pore diameter, a substrate having a length of 20 mm was prepared and an intermediate layer was formed in the same manner to obtain an evaluation sample of the porous support.
[0056] 2. Hydrogen separation membrane production The hydrogen separation membrane was produced by a known method. Oxygen gas was supplied from a cylinder equipped with a Mass Flow Controller (MFC: manufactured by Kofloc Corporation), and the silica source was placed in a bubbler and supplied by bubbling with a carrier gas. In order to control the flow rate of the gas containing the silica source, nitrogen was supplied as a carrier gas from a cylinder equipped with an MFC as necessary. The silicon compound that serves as the silica source was placed in a bubbler, and nitrogen was supplied to the bubbler at a flow rate of 200 mL / min. Vapor of the silicon compound that serves as the silica source was supplied to the case by bubbling. To prevent condensation of the silicon compound in the piping, a ribbon heater was wrapped around the piping as a temperature control device, and the piping temperature was kept at 180°C by heating with the heater. In addition, an ice water cold trap (gas-liquid separator) The temperature of the bubbler was controlled by immersing it in a thermostatic water bath made using COOLNIT CL-150R (manufactured by Taitec Co., Ltd.).
[0057] The silica source used was DMDMS manufactured by Tokyo Chemical Industry Co., Ltd. (product code: D1052). DMDMS has the molecular formula: CH 12 O2Si, molecular weight: 120.22, specific gravity: 0.846-0.8660, boiling point: 81°C, melting point: -5°C. The structural formula is as described above.
[0058] First, the temperature control of the furnace, ribbon heater, and bubbler in the film formation device was turned on. The furnace was heated from room temperature (25°C) to 600°C over 1.5 hours, and the ribbon heater outside the pipe was set to 180°C. After all temperatures were stabilized, an ice-water cold trap was prepared and the DMDMS vapor concentration was measured using a gas line that did not pass through the enclosure. The DMDMS vapor concentration was found to be approximately 0.93 mol / m -3 The bubbler temperature was adjusted so that After adjusting the bubbler temperature, DMDMS vapor was supplied to the outside of the tubular porous support in the housing, and after 2 minutes, oxygen was circulated inside the tubular porous support at 200 mL / min to start the deposition of a hydrogen separation membrane by the counter diffusion CVD method. After 60 minutes, the supply of DMDMS vapor was stopped, and nitrogen was circulated at full flow rate outside the porous support, while oxygen was circulated at 200 mL / min inside the case to purge the inside of the case. After one hour, the supply of oxygen was stopped, and nitrogen was purged into the inside of the substrate at full flow rate for several minutes to complete the deposition of the hydrogen separation membrane. The length of the amorphous silica layer formed on the porous substrate was 8 cm.
[0059] -Evaluation of hydrogen separation membranes- 1. Pore size of the porous support The pore size of the porous support was measured using a Nano-Perm Porometer (manufactured by Seika Digital Image Co., Ltd.) When measuring the pore size, one end of the tubular porous support was fixed to a metal base using an epoxy adhesive (DEV-TUBE S-208, manufactured by ITW Performance Polymers & Fluids Japan Co., Ltd.) or the like, and the other end was sealed. When the relationship between the dimensionless permeability coefficient and the Kelvin diameter of the γ-alumina intermediate layer was analyzed, it was estimated that the peak of the pore size distribution was between 3.2 nm and 4.2 nm, since the dimensionless permeability coefficient decreased the most when the Kelvin diameter was between 3.2 nm and 4.2 nm.
[0060] 2. Gas permeability A gas permeation test was carried out using the membrane production apparatus used for producing the hydrogen separation membrane. Hydrogen gas was supplied to the supply side (outside the tubular porous support) to set the supply side pressure to 0.2 MPaG, and hydrogen gas was allowed to permeate using a dead-end method with a transmembrane pressure difference of 0.2 MPa. The flow rate of the permeated gas obtained from the permeation side (inside the annular porous support) was measured using a bubble flow meter (BFM) (manufactured by Horiba, Ltd.). The gas permeability of the hydrogen separation membrane was calculated from the permeated gas flow rate measured using the BFM. Measurements were performed at 500°C. As a result, the hydrogen permeability at 500°C was 3.36×10 -7 mol m -2 s -1 Pa -1 It was confirmed that the hydrogen permeability was good.
[0061] 3.Water vapor resistance A gas containing water vapor was passed through the outside of the hydrogen separation membrane at 500°C, and the change in hydrogen permeability over time was measured. In addition, the nitrogen permeability was measured before and after the water vapor resistance test. Since methane steam reforming reactions are generally performed at S / C=3, a mixed gas with a Steam / H2 molar ratio of 3 (i.e., a gas with a water vapor pressure of 76 kPa) was circulated using hydrogen as a carrier gas. Water flow rate: 32 μL min -1 , hydrogen flow rate 13 mL min -1 Using a high-pressure chemical pump NRX type (manufactured by Nippon Seimitsu Kagaku Co., Ltd.), water was vaporized by supplying it into a pipe kept at 180° C. by a ribbon heater, and water vapor was supplied. As a result, the hydrogen permeability decreased in the first 20 hours, but the hydrogen permeability was 1×10 -7 mol m -2 s -1 Pa -1 The above conditions were maintained for 95 hours. It was confirmed that even when subjected to the effects of water vapor, the membrane reactor still exhibited satisfactory hydrogen permeability. As a result of the above evaluation, it was confirmed that the amorphous silica layer had good water vapor resistance. In addition, the nitrogen permeability before the test was 2.08×10 -10 mol m -2 s -1 Pa -1 After the test, the -10 mol m -2 s -1 Pa -1 The nitrogen permeability was measured by the pressure change method.
[0062] 4. Cross-sectional observation of amorphous silica layer As a result of cross-sectional observation by SEM at 5000x, the α-alumina layer serving as the support layer and the γ-alumina layer serving as the intermediate layer could be observed, confirming that the porous support has a double structure and that the thickness of the intermediate layer is approximately 5 μm. As a result of the XPS analysis, it was found that the thickness of the portion where Al2p, which is thought to be the separation active layer, increased and Si2p decreased based on the elemental composition in the depth direction, i.e., the separation active region with good hydrogen separation activity in the amorphous silica layer, was approximately 10 nm.
[0063] 5. Hydrogen permeability and nitrogen permeability in a dry atmosphere after film formation FIG. 7 shows an Arrhenius plot created by applying the logarithm of the Arrhenius equation to the hydrogen permeability and nitrogen permeability of the hydrogen separation membrane used in this evaluation in a dry atmosphere after membrane formation. As is clear from FIG. 7, the hydrogen separation membrane of Example 1, which has a membrane length of 8 cm and an amorphous silica layer of the separation active layer having a thickness of approximately 10 nm, is presumed to have both high levels of gas permeability and gas selectivity.
[0064] -Manufacturing of membrane reactors- The inside of the tubular porous support provided with the obtained hydrogen separation membrane was filled with a rhodium catalyst. Both ends of the annular porous support were filled with glass wool to fix the filled rhodium catalyst. In this way, a membrane reactor was obtained.
[0065] - Creation of hydrogen production device - The obtained membrane reactor was set as the membrane reactor 14A in the hydrogen production device 10 shown in Fig. 1. A stainless steel pipe (SUS pipe made by Swagelok) was used for the piping pipe 24A. Using a high-pressure chemical pump NRX type (Nihon Seimitsu Kagaku Co., Ltd.), water was supplied into the pipe 24A, which was kept at 180° C. by a ribbon heater serving as the pipe temperature control device 24B, and the water was vaporized to supply water vapor. The reaction pressure was controlled by a back pressure regulator (44-2362-24 manufactured by TESCOM Corporation). The outlet gas on the permeation side was trapped by a gas-liquid separator 20A, and the outlet gas on the reaction side was trapped by a gas-liquid separator 20B, respectively, to collect only the gas.
[0066] The hydrogen gas recovered through the gas-liquid separator 20A was analyzed using gas chromatography (GC)-A. Various standard gases (GL Sciences) were collected in gas-tight syringes (HAMILTON) and injected into the GC injection to create calibration curves. In GC-A, calibration curves for hydrogen and methane were created. The detector used for the GC was a thermal conductivity detector (TCD). The GC measurement conditions are shown in Table 1 below.
[0067] [Table 1]
[0068] The gas containing carbon dioxide recovered through the gas-liquid separator 20B was analyzed using a gas chromatograph (GC)-B. In the GC-B, calibration curves for hydrogen, carbon monoxide, methane, and carbon dioxide were prepared. The measurement conditions are shown in Table 2 below.
[0069] [Table 2]
[0070] -Evaluation of hydrogen production equipment- 1. Mixed gas of CH4 70% + CO2 30% As a model of biogas, a mixed gas of 70% CH4 + 30% CO2 was used and supplied to the hydrogen production device from the biogas supply device 12. The methane conversion rate by the hydrogen production device was measured. Fig. 8(A) shows the relationship between the methane supply amount and the methane conversion rate in the hydrogen production device equipped with the hydrogen separation membrane of Example 1. Also, Fig. 8(B) shows the relationship between the temperature of the supplied biogas and the methane conversion rate. As a reference example, the evaluation results of a conventional catalyst-packed reactor in which a non-perforated tube was packed with a catalyst and which does not have hydrogen separation performance are also shown. The results of Figures 8(A) and 8(B) show that the hydrogen production device of Example 1 has a better methane conversion rate and can produce hydrogen more efficiently than a hydrogen production device equipped with a conventional catalyst-filled reactor.
[0071] 2. CH4 50% + CO2 50% mixed gas As a model of biogas, a mixed gas of 50% CH4 + 50% CO2 was supplied from the biogas supply 12 to the hydrogen production device and evaluated in the same manner. Fig. 9(A) shows the relationship between the methane supply amount and the methane conversion rate in the hydrogen production device equipped with the hydrogen separation membrane of Example 1. Also, Fig. 9(B) shows the relationship between the temperature of the supplied biogas and the methane conversion rate. As a reference example, the evaluation results of a hydrogen production device equipped with a conventional catalyst-packed reactor in which a non-perforated tube was packed with a catalyst and no hydrogen separation membrane are also shown. The results of Figures 9(A) and 9(B) show that the hydrogen production device of Example 1 has a better methane conversion rate and can produce hydrogen more efficiently than a hydrogen production device equipped with a conventional catalyst-filled reactor.
[0072] 3. Evaluation of fluctuations in methane concentration in biogas The composition of the model biogas was switched to the composition shown in Table 3 below every six hours, and the hydrogen production device equipped with a membrane reactor was operated continuously for 30 hours.
[0073] [Table 3]
[0074] Fig. 10 is a graph showing the relationship between operation time and methane conversion rate when the mixture composition of methane and carbon dioxide in the mixed gas was changed every 6 hours in the hydrogen production apparatus of Example 1. As is clear from Fig. 10, when the composition of the mixed gas was changed and the apparatus was operated continuously for 30 hours, the hydrogen production apparatus of Example 1 maintained a good methane conversion rate of about 80% or more. The hydrogen permeability of the hydrogen separation membrane used in the evaluation was 7.19×10 -8 mol m -2 s -1 Pa -1 After the evaluation test, the -8 mol m -2 s -1 Pa -1 The hydrogen / nitrogen selectivity of the hydrogen separation membrane after deposition was 2.54 × 10 3 It was. From this, it was confirmed that the hydrogen separation membrane in the hydrogen production device of Example 1 has excellent stability against fluctuations in the composition of biogas.
[0075] From the results of Example 1, the hydrogen production device of the present disclosure had good hydrogen selectivity and gas permeability. In addition, stable reactivity can be expected even when used to process gases with fluctuating compositions, such as biogas, and the range of applications is wide. [Explanation of symbols]
[0076] 10 Hydrogen production equipment 12 Biogas supply unit 14A Membrane Reactor 14B Membrane Reactor 16 Hydrogen separation membrane 18 Catalyst 20A gas-liquid separator 20B Gas-liquid separator 22 Temperature control device 24A Pipe (Plumbing) 24B Pipe Temperature Control Device 26 Support layer 28 Middle Class 30 Amorphous silica layer
Claims
1. A biogas supply device that supplies biogas; a membrane reactor in which a catalyst for producing hydrogen gas from the biogas supplied from the biogas supply device and a hydrogen separation membrane that selectively permeates hydrogen gas are disposed inside the cylindrical body; and A recovery vessel is provided for recovering hydrogen gas having a purity of 99% or more separated by the membrane reactor, The hydrogen separation membrane is a hydrogen separation membrane comprising a porous support and an amorphous silica layer formed on the porous support and having an average pore diameter of 0.2 nm to 0.3 nm; The porous support has a two-layer structure including at least a support layer and an intermediate layer, the support layer being a porous body having an average pore diameter of 30 nm to 1000 nm and a thickness of 0.5 mm to 3 mm, and the intermediate layer being a porous body having an average pore diameter of 1 nm to 20 nm and a thickness of 0.5 μm to 10 μm.
2. A biogas supply device that supplies biogas; a membrane reactor in which a catalyst for producing hydrogen gas from the biogas supplied from the biogas supply device and a hydrogen separation membrane that selectively permeates hydrogen gas are disposed inside the cylindrical body; and A recovery vessel is provided for recovering hydrogen gas having a purity of 99% or more separated by the membrane reactor, The hydrogen separation membrane is formed on a porous support and has a hydrogen permeability of 2×10 -7 mol m -2 s -1 P -1 and an amorphous silica layer having a gas permeability for gases other than hydrogen gas and helium gas of 1 / 100 or less of the hydrogen permeability, The porous support has a two-layer structure including at least a support layer and an intermediate layer, the support layer being a porous body having an average pore diameter of 30 nm to 1000 nm and a thickness of 0.5 mm to 3 mm, and the intermediate layer being a porous body having an average pore diameter of 1 nm to 20 nm and a thickness of 0.5 μm to 10 μm. (Measurement method) Hydrogen gas is supplied to the supply side of the hydrogen separation membrane after the membrane formation, the supply side pressure is set to 0.2 MPaG, and the hydrogen gas is allowed to permeate in a dead-end manner with a transmembrane pressure difference of 0.2 MPa. The flow rate of the permeated gas obtained from the permeation side is measured using a soap film flowmeter, and the hydrogen gas permeability is calculated from the obtained permeated gas flow rate. The measurement is performed at 500°C.
3. 3. The hydrogen production device according to claim 1, wherein the amorphous silica layer is a layer made of amorphous silica derived from a silica source containing dimethoxydimethylsilane.
4. 4. The hydrogen production device according to claim 1, further comprising an amorphous silica layer inside the pores of the intermediate layer and on the surface of the intermediate layer.
5. an aluminum oxide porous support having an average pore size of 30 nm to 1000 nm and a thickness of 0.5 mm to 3 mm; A hydrogen separation membrane having, on one surface of the porous support, an intermediate layer which is a porous body having an average pore size of 1 nm to 20 nm and a thickness of 0.5 μm to 10 μm, and an amorphous silica layer which is made of amorphous silica derived from a silica source containing dimethoxydimethylsilane and has an average pore size of 0.2 nm to 0.3 nm.
6. 6. The hydrogen separation membrane according to claim 5, further comprising an amorphous silica layer inside the pores of the intermediate layer and on the surface of the intermediate layer, the thickness of the hydrogen separation active region in the amorphous silica layer being 5 nm to 15 nm, and the membrane length, which is the length from the end of the amorphous silica layer on the permeation gas introduction side to the end on the opposite side, being 6 cm or more.
7. A method for producing a hydrogen separation membrane, comprising the steps of: forming an intermediate layer, which is a porous body having an average pore size of 1 nm to 20 nm and a thickness of 0.5 μm to 10 μm, on one surface of an aluminum oxide porous body having an average pore size of 30 nm to 1000 nm and a thickness of 0.5 mm to 3 mm; and forming an amorphous silica layer having an average pore size of 0.2 nm to 0.3 nm on a surface of the intermediate layer opposite to the surface in contact with the aluminum oxide porous body, by a chemical vapor deposition method using a silica source containing dimethoxydimethylsilane.
8. 8. The method for producing a hydrogen separation membrane according to claim 7, wherein the chemical vapor deposition is a counter diffusion chemical vapor deposition.
Citation Information
Patent Citations
Hydrogen selective silica membrane
JP2005528198A
Production method of hydrogen gas separation membrane
JP2006239663A
HYDROGEN SEPARATING SYSTEM USING Nb MEMBRANE AND PERIODIC TABLE 5A GROUP METAL ALLOY MEMBRANE
JP2010240637A
Hydrogen generation apparatus and hydrogen loading apparatus
JP2019137580A
Hydrogen separation membrane and method for manufacturing a hydrogen separation membrane
JP4728308B2