Metal-coated liquid crystal polyester multifilament

The metal-coated liquid crystal polyester multifilament addresses the issue of bending fatigue resistance by adjusting Pd content and adhesion strength, ensuring resistance stability for conductive applications.

JP7562096B2Active Publication Date: 2024-10-07KURARAY CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020212685
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-22
Publication Date
2024-10-07
Estimated Expiration
2040-12-22

AI Technical Summary

Technical Problem

Metal-coated fibers with polyarylate fibers have insufficient bending fatigue resistance due to low adhesion between the metal and the fibers, leading to significant changes in resistance upon repeated bending.

Method used

A metal-coated liquid crystal polyester multifilament with a Pd content of 0.33% by mass or more and interfacial adhesion strength of 15N/mm², achieved by applying a surfactant to the fiber surface and contacting it with a high-pressure carbon dioxide fluid containing a Pd complex, followed by metal coating.

Benefits of technology

The solution enhances bending fatigue resistance, allowing the multifilament to maintain resistance stability even with repeated bending, making it suitable for conductive applications like electric wires and electromagnetic shielding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562096000010
    Figure 0007562096000010
  • Figure 0007562096000001
    Figure 0007562096000001
  • Figure 0007562096000002
    Figure 0007562096000002
Patent Text Reader

Abstract

To provide a metal coated liquid crystalline polyester multifilament excellent in flexural fatigue resistance.SOLUTION: A metal coated liquid crystalline polyester multifilament includes two or more metal coated liquid crystal polyester monofilaments obtained by coating metal having a thickness of 0.1-20 μm on the surface of a liquid crystal polyester monofilament. A Pd content obtained by ICP emission spectrometry is 0.33 mass% or more to the mass of the multifilament except the coated metal, and the interface adhesion strength of the coated metal measured by a micro drop method is 15 N / mm2 or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a metal-coated liquid crystal polyester multifilament that can be used as a conductive member in applications such as electric wires and electromagnetic wave shielding, and a method for producing the same. [Background technology]

[0002] Traditionally, metal wires have been used as electric wires and electromagnetic wave shielding materials, but in recent years, research and development has been progressing on conductive fiber materials in which organic fibers are coated with metal to reduce weight and cost. Metal-coated fibers in which high-strength fibers such as polyarylate fibers are coated with metal have been studied as conductive fibers with particularly high conductivity and strength (see, for example, Patent Document 1). Such metal-coated fibers are generally obtained by adding a catalyst such as a palladium complex to an aqueous system followed by electroless plating. On the other hand, a method of electroless plating is also known in which a catalyst is applied to a polyarylate fiber by contacting the fiber with a supercritical fluid containing an organic palladium complex. For example, Patent Document 2 discloses a metal-coated fiber obtained by adding a fatty acid surfactant to a polyarylate fiber or the like, contacting the fiber with supercritical carbon dioxide containing an organic palladium complex, and then plating the fiber. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Laid-Open No. 2011-231382 [Patent Document 2] Japanese Patent Application Laid-Open No. 2012-144762 Summary of the Invention [Problem to be solved by the invention]

[0004] However, according to the investigations of the present inventors, it was found that metal-coated fibers plated with polyarylate fibers, such as those described in Patent Documents 1 and 2, have poor adhesion between the metal and the fiber, and therefore do not have sufficient resistance to bending fatigue, and the resistance may change significantly when repeatedly bent.

[0005] Therefore, an object of the present invention is to provide a metal-coated liquid crystal polyester multifilament having excellent resistance to flex fatigue and a method for producing the same. [Means for solving the problem]

[0006] As a result of intensive research to solve the above problems, the present inventors have found that, in a metal-coated liquid crystal polyester multifilament, the Pd content determined by ICP emission spectrometry is adjusted to 0.33 mass% or more, and the interfacial adhesive strength of the coating metal is adjusted to 15 N / mm 2 The inventors have found that the above problems can be solved by adjusting the above, and have thus completed the present invention. That is, the present invention includes the following aspects.

[0007] [1] A metal-coated liquid crystal polyester multifilament comprising two or more metal-coated liquid crystal polyester monofilaments each having a surface coated with a metal having a thickness of 0.1 to 20 μm on the surface of a liquid crystal polyester monofilament, wherein the Pd content obtained by ICP emission spectrometry is 0.33 mass% or more relative to the mass of the multifilament excluding the coating metal, and a microdrop Let The interfacial adhesive strength of the coated metal measured by the method is 15N / mm 2 This is the metal-coated liquid crystal polyester multifilament. [2] The metal-coated liquid crystal polyester multifilament according to [1], having a tensile strength of 16 cN / dtex or more. [3] The metal-coated liquid crystal polyester multifilament according to [1] or [2], wherein the metal comprises at least one selected from the group consisting of copper, silver, gold, iron, zinc, lead, palladium, nickel, chromium, and tin. [4] A method for producing a metal-coated liquid crystal polyester multifilament according to any one of [1] to [3], comprising: step (1) of applying a surfactant to the surface of the liquid crystal polyester multifilament; step (2) of contacting the surfactant-containing liquid crystal polyester multifilament obtained in step (1) with a high-pressure carbon dioxide fluid having a Pd complex dissolved therein; and step (3) of coating a metal on the Pd-containing liquid crystal polyester multifilament obtained in step (2). [5] The method according to [4], wherein the surfactant comprises a halogen atom- and nitrogen atom-containing cationic surfactant. [6] The method according to [4] or [5], wherein the residual surfactant rate when the surfactant-containing liquid crystal polyester multifilament is brought into contact with a high-pressure carbon dioxide fluid is 10 mass % or more. [Effects of the Invention]

[0008] The metal-coated liquid crystalline polyester multifilament of the present invention has excellent resistance to bending fatigue, and can therefore be suitably used as a conductive material in applications such as electric wires and electromagnetic wave shielding. [Brief explanation of the drawings]

[0009] [Figure 1] 1 is a schematic diagram of a supercritical processing apparatus according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE INVENTION

[0010] [Metal-coated liquid crystal polyester multifilament] The metal-coated liquid crystalline polyester multifilament of the present invention comprises two or more metal-coated liquid crystalline polyester monofilaments each having a liquid crystalline polyester monofilament surface coated with a metal having a thickness of 0.1 to 20 μm, and the Pd content (sometimes referred to as the Pd content of the entire fiber) obtained by ICP emission spectrometry is 0.33 mass % or more relative to the mass of the multifilament excluding the coating metal, and Let The interfacial adhesive strength of the coated metal measured by the method (sometimes simply referred to as interfacial adhesive strength) is 15 N / mm2 That's all.

[0011] The present inventors have determined that the Pd content of the entire fiber in the metal-coated liquid crystal polyester multifilament is 0.33 mass % or more, and the interfacial adhesive strength of the coating metal is 15 N / mm 2 It was unexpectedly found that adjusting the above-mentioned conditions improves the bending fatigue resistance of the metal-coated fiber and effectively suppresses changes in resistance value due to repeated bending. This is presumably because a sufficient amount of the coating metal is present not only on the surface of the fiber but also inside the fiber, improving the adhesion between the coating metal and the fiber and effectively suppressing detachment of the coating metal during bending. In this specification, "filament" may be referred to as "fiber," "monofilament" as "single fiber," "coated" as "plated," "liquid crystal polyester multifilament" simply as "multifilament," and "liquid crystal polyester monofilament" simply as "monofilament," and "liquid crystal polyester multifilament" and "liquid crystal polyester monofilament" may be collectively referred to as "liquid crystal polyester fiber."

[0012] <Liquid Crystal Polyester Monofilament> High-strength liquid crystal polyester fibers can be produced, for example, by melt-spinning liquid crystal polyester and then solid-phase polymerizing the resulting spun yarn. Liquid crystal polyester multifilament is a fiber consisting of two or more liquid crystal polyester monofilaments. Liquid crystal polyesters are polyesters that exhibit optical anisotropy (liquid crystallinity) in the molten phase, and can be identified by, for example, placing a sample on a hot stage, heating it under a nitrogen atmosphere, and observing the transmitted light through the sample with a polarizing microscope. Liquid crystal polyesters are composed of repeating structural units derived from, for example, aromatic diols, aromatic dicarboxylic acids, or aromatic hydroxycarboxylic acids, and the chemical structure of these structural units is not particularly limited as long as it does not impair the effects of the present invention. Furthermore, liquid crystal polyesters may also contain structural units derived from aromatic diamines, aromatic hydroxyamines, or aromatic aminocarboxylic acids, provided that the effects of the present invention are not impaired.

[0013] For example, preferred structural units include those shown in Table 1. [Table 1]

[0014] Here, Y is present in a number ranging from 1 to the maximum number that can be substituted on the aromatic ring, and each Y is independently selected from the group consisting of a hydrogen atom, a halogen atom (e.g., a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, etc.), an alkyl group (e.g., an alkyl group having 1 to 4 carbon atoms such as a methyl group, an ethyl group, an isopropyl group, a t-butyl group, etc.), an alkoxy group (e.g., a methoxy group, an ethoxy group, an isopropoxy group, a n-butoxy group, etc.), an aryl group (e.g., a phenyl group, a naphthyl group, etc.), an aralkyl group [benzyl group (phenylmethyl group), phenethyl group (phenylethyl group), etc.], an aryloxy group (e.g., a phenoxy group, etc.), and an aralkyloxy group (e.g., a benzyloxy group, etc.).

[0015] More preferred structural units include the structural units described in Examples (1) to (18) shown in the following Tables 2, 3, and 4. When the structural unit in the formula is a structural unit that can exhibit multiple structures, two or more of such structural units may be combined and used as structural units that constitute the polymer.

[0016] [Table 2]

[0017] [Table 3]

[0018] [Table 4]

[0019] In the structural units of Tables 2, 3, and 4, n is an integer of 1 or 2, and each of the structural units n=1 and n=2 may exist alone or in combination; Y1 and Y2 may each independently represent a hydrogen atom, a halogen atom (e.g., a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, etc.), an alkyl group (e.g., an alkyl group having 1 to 4 carbon atoms, such as a methyl group, an ethyl group, an isopropyl group, or a t-butyl group), an alkoxy group (e.g., a methoxy group, an ethoxy group, an isopropoxy group, an n-butoxy group, etc.), an aryl group (e.g., a phenyl group, a naphthyl group, etc.), an aralkyl group [e.g., a benzyl group (phenylmethyl group), a phenethyl group (phenylethyl group), etc.], an aryloxy group (e.g., a phenoxy group), an aralkyloxy group (e.g., a benzyloxy group), etc. Among these, preferred Ys include a hydrogen atom, a chlorine atom, a bromine atom, or a methyl group.

[0020] Furthermore, examples of Z include substituents represented by the following formulas. [ka]

[0021] A preferred liquid crystal polyester preferably has two or more types of naphthalene skeletons as a structural unit. Particularly preferably, the liquid crystal polyester contains both a structural unit (A) derived from hydroxybenzoic acid and a structural unit (B) derived from hydroxynaphthoic acid. For example, the structural unit (A) can be represented by the following formula (A), and the structural unit (B) can be represented by the following formula (B). From the viewpoint of easily improving melt moldability, the ratio of the structural unit (A) to the structural unit (B) may be preferably in the range of 9 / 1 to 1 / 1, more preferably 7 / 1 to 1 / 1, and even more preferably 5 / 1 to 1 / 1.

[0022] [ka] [ka]

[0023] The total of the structural units (A) and the structural units (B) may be, for example, 65 mol % or more, more preferably 70 mol % or more, and even more preferably 80 mol % or more, based on the total structural units. Liquid crystal polyesters in which the structural units (B) account for 4 to 45 mol % of the polymer are particularly preferred.

[0024] The melting point of the liquid crystal polyester preferably used in the present invention is preferably 250 to 360°C, more preferably 260 to 320°C. Here, the melting point refers to the main absorption peak temperature observed when measured using a differential scanning calorimeter (DSC; Mettler "TA3000") according to JIS K7121. Specifically, 10 to 20 mg of sample is placed in an aluminum pan and sealed in the DSC apparatus. Nitrogen is passed through the sample as a carrier gas at 100 cc / min, and the endothermic peak is measured when the temperature is increased at 20°C / min. If a clear peak does not appear in the first run of DSC measurement due to the type of polymer, it is recommended to increase the temperature to 50°C higher than the expected flow temperature at a heating rate of 50°C / min, hold the temperature at that temperature for 3 minutes, completely melt the polymer, and then cool it to 50°C at a cooling rate of -80°C / min. The endothermic peak is then measured at a heating rate of 20°C / min.

[0025] The liquid crystal polyester may contain thermoplastic polymers such as polyethylene terephthalate, modified polyethylene terephthalate, polyolefin, polycarbonate, polyamide, polyphenylene sulfide, polyether ether ketone, and fluororesin, as long as the effects of the present invention are not impaired. Furthermore, various additives may be added, such as inorganic substances such as titanium oxide, kaolin, silica, and barium oxide, colorants such as carbon black, dyes, and pigments, antioxidants, ultraviolet absorbers, and light stabilizers.

[0026] In the liquid crystal polyester fiber obtained by melt spinning the liquid crystal polyester, the fineness of the liquid crystal polyester monofilament is preferably 1.5 dtex or more, more preferably 2.5 dtex or more, even more preferably 5.0 dtex or more, and preferably 100 dtex or less, more preferably 50 dtex or less. When the fineness of the liquid crystal polyester monofilament is above the above lower limit, the coating metal easily penetrates into the fiber, making it easy to improve bending fatigue resistance. On the other hand, when the fineness of the liquid crystal polyester monofilament is below the above upper limit, it is easy to improve the solidification efficiency immediately after melt spinning and the solid-state polymerization rate.

[0027] <Metal> The metal-coated liquid crystal polyester multifilament of the present invention is a liquid crystal polyester monofilament having a surface coated with a metal having a thickness of 0.1 to 20 μm. In this specification, the metal includes not only the metals described later, but also conductive metal oxides and metal nitrides using the metals described later.

[0028] The metal is not particularly limited, but preferably contains at least one selected from the group consisting of copper, silver, gold, iron, zinc, lead, palladium, nickel, chromium, tin, titanium, aluminum, indium, and vanadium, more preferably contains at least one selected from the group consisting of copper, silver, gold, iron, zinc, lead, palladium, nickel, chromium, and tin, and even more preferably contains at least one selected from the group consisting of copper, silver, gold, iron, and nickel. The inclusion of these metals tends to improve the electrical conductivity and flexural fatigue resistance of the metal-coated liquid crystal polyester multifilament. These metals can be used alone or in combination.

[0029] The thickness of the metal coating on the surface of the liquid crystal polyester monofilament is 0.1 to 20 μm, preferably 0.2 μm or more, more preferably 0.5 μm or more, and preferably 15 μm or less, more preferably 10 μm or less. If the metal thickness is above the lower limit, the conductivity increases and the initial resistance value is easily reduced, while if it is below the upper limit, the bending fatigue resistance is easily improved. The thickness of the coating metal can be measured by cross-sectional observation using X-ray CT, for example, by the method described in the Examples.

[0030] <Metal-coated liquid crystal polyester multifilament> The metal-coated liquid crystal polyester multifilament comprises two or more metal-coated liquid crystal polyester monofilaments each having the metal coated on the surface of the liquid crystal polyester monofilament.

[0031] The metal-coated liquid crystal polyester multifilament of the present invention has a Pd content of 0.33% by mass or more based on the mass of the multifilament excluding the coating metal, as determined by ICP emission spectrometry, and Let The interfacial adhesive strength of the coated metal measured by the method is 15N / mm 2 For these reasons, the composite has excellent resistance to bending fatigue, and can therefore be suitably used as a conductive material in applications such as electric wires and electromagnetic wave shielding.

[0032] In the present invention, the Pd content obtained by ICP atomic emission spectrometry (also referred to as the Pd content of the entire fiber) is the content of Pd atoms (palladium atoms) based on the mass of the metal-coated liquid crystal polyester multifilament excluding the coating metal, and the mass of the multifilament excluding the coating metal means the mass obtained by subtracting the mass of the coating metal from the mass of the metal-coated liquid crystal polyester multifilament. Specifically, the Pd content of the entire fiber is preferably calculated by measuring the mass of the metal-coated liquid crystal polyester multifilament, then measuring the Pd content (mass%) and metal content (mass%) contained in the metal-coated liquid crystal polyester multifilament by ICP atomic emission spectrometry, and using these to calculate the Pd content (mass%) relative to the mass (100 mass%) of the metal-coated liquid crystal polyester multifilament excluding the coating metal, and can be calculated, for example, by the method described in the Examples.

[0033] The metal-coated liquid crystal polyester multifilament of the present invention has a Pd content of 0.33% by mass or more in the entire fiber. If the Pd content of the entire fiber is less than 0.33% by mass, the amount of Pd catalyst used in metal plating may be insufficient, which may result in poor adhesion between the plated metal and the fiber when bent, and the resulting metal-coated fiber may tend to have insufficient bending fatigue resistance. The Pd content of the entire fiber of the metal-coated liquid crystal polyester multifilament of the present invention is preferably 0.34% by mass or more, more preferably 0.36% by mass or more, even more preferably 0.38% by mass or more, even more preferably 0.40% by mass or more, and particularly preferably 0.45% by mass or more. When the Pd content of the entire fiber is equal to or greater than the above-mentioned lower limit, an effective amount of Pd catalyst can be utilized during metal plating, which facilitates improving the flex fatigue resistance of the metal-coated fiber. The Pd content of the entire fiber of the metal-coated liquid crystal polyester multifilament of the present invention is preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 1% by mass or less. When the Pd content of the entire fiber is equal to or less than the above-mentioned upper limit, the amount of expensive palladium used can be reduced, and further, a decrease in fiber strength due to excess palladium added to the fiber can be easily prevented.

[0034] In the metal-coated liquid crystal polyester multifilament of the present invention, microdrops Let The interfacial adhesive strength of the coated metal measured by the method is 15N / mm 2 The interfacial adhesive strength of the coated metal is 15N / mm 2 If the bending fatigue resistance is less than this, the resistance value tends to increase significantly when the material is repeatedly bent.

[0035] In the present invention, the coating metal not only coats the fiber surface but also partially penetrates the fiber interior, resulting in high adhesion between the coating metal and the fiber during bending, and sufficient bending fatigue resistance. The interfacial adhesive strength may be adjusted by appropriately changing the type and fineness of the liquid crystal polyester multifilament, or by using a suitable method for producing the metal-coated liquid crystal polyester multifilament. For example, the interfacial adhesive strength may be adjusted to fall within the above range of the present invention by appropriately adjusting the type and amount of the surfactant applied in step (1) or the type and amount of the Pd catalyst contacted in step (2).

[0036] The interfacial adhesive strength of the metal-coated liquid crystal polyester multifilament of the present invention is preferably 16 N / mm 2 More preferably, 18N / mm 2 More preferably, 20 N / mm 2 More than 22N / mm 2 When the interfacial adhesive strength is equal to or greater than the lower limit, the bending fatigue resistance is easily improved. The interfacial adhesive strength of the metal-coated liquid crystal polyester multifilament is preferably 100 N / mm 2 Less than or equal to 50N / mm 2 The interfacial adhesive strength (N / mm 2 ) is a microdroplet to More specifically, after preparing a resin sphere on the surface of the metal-coated liquid crystal polyester multifilament, the sphere is peeled off with a universal testing machine, and the stress (N) at the maximum point is divided by the coating area measured with a scanning electron microscope (SEM). For example, it can be calculated by the method described in the examples.

[0037] In one embodiment of the present invention, the tensile strength of the metal-coated liquid crystalline polyester multifilament is preferably 16 cN / dtex or more, more preferably 18 cN / dtex or more, and even more preferably 21 cN / dtex or more. When the tensile strength is at or above the above lower limit, the mechanical strength is easily increased. The upper limit of the tensile strength of the metal-coated liquid crystalline polyester multifilament is preferably 35 cN / dtex or less, more preferably 30 cN / dtex or less. When the tensile strength is at or below the above upper limit, flexibility is easily maintained while maintaining flexural fatigue resistance and tensile strength. The tensile strength can be measured using a benchtop precision universal testing machine, for example, by the method described in the Examples. Since the tensile strength of the multifilament after plating is dominated by the tensile strength of the multifilament before plating, the tensile strength of the metal-coated liquid crystalline polyester multifilament may be a value measured using a liquid crystalline polyester multifilament before plating.

[0038] In this specification, flexural fatigue resistance refers to the property of resistance value being resistant to change even when a metal-coated liquid crystalline polyester multifilament is repeatedly bent. For example, it can be evaluated by the specific resistance value, which is the ratio of the resistance value after a flexural fatigue test to the resistance value before the test. The specific resistance value can be measured by the following method. First, the initial resistance value of the metal-coated liquid crystalline polyester multifilament is measured using a resistance measuring device. Next, the metal-coated liquid crystalline polyester multifilament is bent using a flexural fatigue testing device under the following conditions: bending radius R at bending: 2.5 mm, bending angle: 120°, bending speed: 60 rpm, load: 100 g, and number of flexions: 10,000. The resistance value is then measured again and can be calculated by substituting the result into the following formula. For example, the specific resistance value may be calculated by the method described in the Examples. Resistivity value = (resistivity value after flexural fatigue test) / (initial resistance value before flexural fatigue test)

[0039] In one embodiment of the present invention, the resistivity of the metal-coated liquid crystal polyester multifilament after 10,000 flexings is preferably 10 or less, more preferably 8.0 or less, even more preferably 6.0 or less, even more preferably 5.0 or less, and particularly preferably 4.0 or less. When the resistivity is equal to or less than the above upper limit, excellent flex fatigue resistance and high conductivity after flexing are likely to be exhibited. The lower limit of the resistivity is usually 0 or more.

[0040] In one embodiment of the present invention, the initial resistance value of the metal-coated liquid crystalline polyester multifilament is preferably 0.01 Ω / 10 cm or more, more preferably 0.1 Ω / 10 cm or more, even more preferably 0.5 Ω / 10 cm or more, and is preferably 10 Ω / 10 cm or less, more preferably 5 Ω / 10 cm or less, even more preferably 3 Ω / 10 cm or less. When the initial resistance value is within the above range, the conductivity is easily increased.

[0041] The total fineness of the liquid crystal polyester multifilaments in the metal-coated liquid crystal polyester multifilament is not particularly limited, but is preferably 10 dtex or more, more preferably 50 dtex or more, even more preferably 100 dtex or more, particularly preferably 200 dtex or more, and is preferably 10,000 dtex or less, more preferably 5,000 dtex or less, even more preferably 3,000 dtex or less, particularly preferably 2,000 dtex or less. The number of metal-coated liquid crystal polyester monofilaments in the metal-coated liquid crystal polyester multifilament is preferably 3 or more, more preferably 5 or more, and preferably 1,000 or less, more preferably 500 or less. When the total fineness of the liquid crystal polyester multifilaments and the number of metal-coated liquid crystal polyester monofilaments in the metal-coated liquid crystal polyester multifilament are within the above ranges, bending fatigue resistance, light weight, and strength are likely to be improved.

[0042] The metal-coated liquid crystal polyester multifilament may be untwisted or loosely twisted, and from the viewpoint of stabilizing the resistance value, loosely twisted is preferred. Furthermore, the metal-coated liquid crystal polyester multifilament may be subjected to an opening treatment and / or smoothing treatment. For example, by producing a woven fabric using such a multifilament that has been opened and / or smoothed, the woven fabric can be made thin.

[0043] The form of the metal-coated liquid crystal polyester multifilament is not particularly limited, and may be, for example, UD (Unidirectional), nonwoven fabric, woven fabric, knitted fabric, braided cord, or mixed yarn.

[0044] [Metal-coated liquid crystal polyester multifilament manufacturing method] The method for producing the metal-coated liquid crystalline polyester multifilament of the present invention is not particularly limited, but may include the following steps: The method preferably includes the steps of: applying a surfactant to the surface of the liquid crystal polyester multifilament; contacting the surfactant-containing liquid crystal polyester multifilament obtained in step (1) with a high-pressure carbon dioxide fluid having a Pd complex dissolved therein; and coating the Pd-containing liquid crystal polyester multifilament obtained in step (2) with a metal (3). In this specification, the surfactant-containing liquid crystal polyester multifilament, which is an intermediate obtained in step (1), is referred to as surfactant-containing liquid crystal polyester multifilament (X), and the Pd-containing liquid crystal polyester multifilament, which is an intermediate obtained in step (2), is referred to as Pd-containing liquid crystal polyester multifilament (Y).

[0045] <Process (1)> Step (1) is a step of applying a surfactant to the surface of the liquid crystal polyester multifilament. The liquid crystal polyester multifilament used as a fiber raw material may be a solid-phase polymerized liquid crystal polyester multifilament. By subjecting the multifilament to solid-phase polymerization, the strength and elastic modulus of the resulting metal-coated fiber can be improved. The heat treatment temperature during solid-phase polymerization is preferably 200 to 350°C, and the solid-phase polymerization time is preferably 30 minutes to 30 hours. The solid-phase polymerization can be carried out in an inert atmosphere such as nitrogen, an oxygen-containing active atmosphere such as air, or under reduced pressure.

[0046] In step (1), examples of surfactants to be applied include cationic surfactants, anionic surfactants, nonionic surfactants, and amphoteric surfactants, with cationic surfactants being preferred. Surfactants can be used alone or in combination. By applying a surfactant, preferably a cationic surfactant, to the surface of the liquid crystal polyester multifilament in step (1), the surfactant is likely to remain on the fiber surface even after supercritical treatment, and the Pd complex is unlikely to be reduced. This allows the Pd complex to be continuously introduced (or dissolved) into the surfactant in step (2), making it easier to increase the Pd content on the surface of the liquid crystal polyester multifilament. Furthermore, since the anchoring effect is easily exerted, part of the Pd complex can penetrate into the interior of the fiber. This makes it easier to have sufficient plating metal present on the surface and interior of the fiber, improving the adhesion and flex fatigue resistance of the metal-coated fiber.

[0047] Examples of cationic surfactants include nitrogen atom-containing cationic surfactants such as hexadecylpyridinium chloride, benzirconium chloride, octadecylamine, tetramethylammonium hydroxide, stearyltrimethylammonium chloride, monomethylamine hydrochloride, lauric acid diethanolamide, oleic acid diethanolamide, and stearic acid diethanolamide. From the viewpoint of easily improving the adhesion and flexural fatigue resistance of the metal-coated fiber, nitrogen atom-containing cationic surfactants having a cyclic structure (particularly a heterocyclic or aromatic ring), such as hexadecylpyridinium chloride and benzirconium chloride, are preferred. In a preferred embodiment of the present invention, from the viewpoint of more easily improving the adhesion and flexural fatigue resistance of the metal-coated fiber, the cationic surfactant is preferably a halogen atom- and nitrogen atom-containing cationic surfactant such as hexadecylpyridinium chloride or benzilconium chloride, and more preferably a halogen atom- and nitrogen atom-containing cationic surfactant having a cyclic structure. Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom, and preferably a chlorine atom. Examples of the heterocycle include a pyridine ring, and examples of the aromatic ring include a benzene ring. Furthermore, the nitrogen atom-containing cationic surfactant is preferably a quaternary ammonium cation. The cationic surfactants can be used alone or in combination.

[0048] In step (1), additives other than surfactants may be applied. Examples of additives include antistatic agents and various compounds that impart dispersibility, convergence, smoothness, etc. These additives may be used alone or in combination.

[0049] In step (1), the surfactant may be applied using, for example, a knife coater, a bar coater, an applicator, a roll coater, a squeeze roll, a nip roll, or the like.

[0050] In step (1), the amount of surfactant applied (or added) can be appropriately selected depending on the type and amount of catalyst added in step (2). It is preferably at least 0.01 parts by mass, more preferably at least 0.05 parts by mass, and even more preferably at least 0.1 parts by mass, relative to 100 parts by mass of the liquid crystal polyester multifilament (surfactant-free liquid crystal polyester multifilament), and is preferably at most 10 parts by mass, more preferably at most 5 parts by mass, and even more preferably at most 3 parts by mass. When the amount of surfactant applied is at least the above-mentioned lower limit, the Pd complex is easily introduced onto the fiber surface, preferably onto the fiber surface and the interior, in step (2). This facilitates the presence of a sufficient amount of plating metal on the fiber surface, preferably onto the fiber surface and the interior, in step (3), thereby improving the adhesion and flex fatigue resistance of the metal-coated fiber. Furthermore, when the amount of surfactant applied is at most the above-mentioned upper limit, excess surfactant can be prevented from remaining on the fiber, thereby preventing the excessive surfactant from impairing adhesion between the fiber and the metal.

[0051] The surfactant-containing liquid crystal polyester multifilament (X) obtained in step (1) comprises two or more liquid crystal polyester monofilaments each having a surfactant coated on the surface thereof. The surfactant-containing liquid crystal polyester multifilament (X) preferably has a surfactant residual rate of 10% by mass or more when contacted with a high-pressure carbon dioxide fluid. When the surfactant residual rate is 10% by mass or more, a large amount of surfactant can be present on the fiber surface during the supercritical treatment in step (2), allowing a relatively large amount of Pd complex to be introduced onto the fiber surface, preferably onto the fiber surface and into the fiber interior. This allows a sufficient amount of plating metal to be present on the fiber surface, preferably onto the fiber surface and into the fiber interior, in step (3), facilitating the formation of a metal-coated liquid crystal polyester multifilament having excellent adhesion between the metal and the fiber and excellent resistance to flex fatigue.

[0052] The residual surfactant rate upon contact with a high-pressure carbon dioxide fluid is preferably 15% by mass or more, more preferably 30% by mass or more, even more preferably 50% by mass or more, even more preferably 70% by mass or more, particularly preferably 80% by mass or more, and especially preferably 90% by mass or more. When the residual surfactant rate upon contact with a high-pressure carbon dioxide fluid is equal to or greater than the above-mentioned lower limit, adhesion and flex fatigue resistance are likely to be improved. The upper limit of the residual surfactant rate upon contact with a high-pressure carbon dioxide fluid is 100% by mass or less. The residual surfactant rate may be adjusted within the range of the present invention by, for example, appropriately changing the type and fineness of the liquid crystal polyester multifilament, or the type and amount of the surfactant.

[0053] The residual surfactant rate can be calculated from the masses before and after contacting the liquid crystal polyester multifilament to which the surfactant has been added with high-pressure carbon dioxide fluid, using the following formula. Surfactant residual rate (mass%)=(mass of fiber after supercritical treatment−mass of fiber itself) / (mass of fiber after surfactant addition−mass of fiber itself)×100 The residual surfactant rate can be measured and calculated, for example, by the method described in the Examples.

[0054] <Process (2)> The step (2) is a step of contacting the surfactant-containing liquid crystalline polyester multifilament (X) obtained in the step (1) with a high-pressure carbon dioxide fluid having a Pd complex dissolved therein.

[0055] In step (2), the Pd complex can be efficiently impregnated into or attached to the surfactant-containing liquid crystalline polyester multifilament (X) using a high-pressure carbon dioxide fluid with high diffusivity and high permeability, and the resulting Pd-containing liquid crystalline polyester multifilament (Y) can be reduced and plated, thereby producing a metal-coated liquid crystalline polyester multifilament in a short time with few steps.

[0056] When a high-pressure carbon dioxide fluid containing a Pd complex is brought into contact with a surfactant-containing liquid crystalline polyester multifilament (X), the fiber swells, and the Pd complex becomes embedded in the gaps created by the swelling. Furthermore, the Pd complex is exposed by a reduction treatment described below, allowing for a plating treatment with a high anchoring effect on the fiber surface. In particular, the present invention uses a surfactant-containing liquid crystalline polyester multifilament (X) whose fiber surface is coated with a specific surfactant, allowing for the introduction of a large amount of Pd complex into the fiber surface and the interior of the fiber, and allowing for the formation of a metal coating with excellent adhesion by plating.

[0057] In this specification, "high-pressure carbon dioxide fluid" refers to carbon dioxide in a supercritical or subcritical state (also referred to as "supercritical carbon dioxide"). Carbon dioxide (CO2) becomes a supercritical fluid at a critical temperature of 304 K and a critical pressure of 7.4 MPa, and can become a subcritical fluid at a temperature approximately 10 K lower than the critical temperature and at a pressure close to the critical pressure. Therefore, contact can be carried out under such critical or subcritical conditions. Generally, the contacting temperature is between the supercritical temperature and 650 K, the contacting pressure is between the supercritical pressure and 35 MPa, and the contact time is 5 to 120 minutes. Therefore, for example, a method in which a high-pressure carbon dioxide fluid containing a Pd complex is immersed in the surface of the surfactant-containing liquid crystalline polyester multifilament (X) and contacted for 5 to 120 minutes at a temperature between the supercritical temperature and 650 K and a pressure between the supercritical temperature and 35 MPa can be suitably used in step (2).

[0058] The pressure during contact is preferably 5.0 to 35.0 MPa, the temperature during contact is preferably 323 K to 473 K, and the time during contact is preferably 5 to 60 minutes.

[0059] In step (2), examples of the Pd complex (palladium complex) used as a catalyst include palladium acetate complex, palladium nitrate complex, palladium acetylcetonate complex, and palladium trifluoroacetate complex. Palladium acetate complex is preferred from the viewpoints of easy penetration into surfactants and high catalytic function. The Pd complexes can be used alone or in combination of two or more.

[0060] In step (2), the amount of Pd complex used (or added) is preferably at least 0.01 parts by mass, more preferably at least 0.05 parts by mass, and even more preferably at least 0.1 parts by mass, relative to 100 parts by mass of the liquid crystal polyester multifilament (a liquid crystal polyester multifilament containing no surfactant or Pd atoms), and is preferably at most 20 parts by mass, more preferably at most 15 parts by mass, and even more preferably at most 10 parts by mass. When the amount of Pd complex used is at least the above-mentioned lower limit, the Pd complex is easily introduced onto the fiber surface, preferably onto the fiber surface and the interior, which makes it easier to have a sufficient amount of plating metal present on the fiber surface, preferably onto the fiber surface and the interior, in step (3), thereby improving the adhesion and flex fatigue resistance of the metal-coated fiber. When the amount of Pd complex added is at most the above-mentioned upper limit, the catalytic action is easily exerted efficiently while suppressing the amount of expensive palladium used.

[0061] The high-pressure carbon dioxide fluid may contain additives other than the Pd catalyst, such as an accelerator that accelerates the decomposition of the Pd complex or an accelerator that accelerates the penetration of the high-pressure carbon dioxide fluid into the surfactant-containing liquid crystal polyester multifilament (X).

[0062] In step (2), the Pd-containing liquid crystalline polyester multifilament (Y) to which a Pd complex has been added as a catalyst is preferably subjected to a reduction treatment. A reducing agent may be used for the reduction, but thermal reduction is preferred because the Pd complex can be easily reduced by heating. Examples of thermal reduction methods include a method in which the Pd-containing liquid crystalline polyester multifilament (Y) is exposed to high temperatures. The heating temperature during thermal reduction is preferably 100°C or higher, more preferably 150°C or higher, and even more preferably 180°C or higher, and is preferably 300°C or lower, and more preferably 250°C or lower. When the heating temperature during thermal reduction is equal to or higher than the lower limit, the Pd complex is easily reduced. When the heating temperature during thermal reduction is equal to or lower than the upper limit, the metallized palladium is easily prevented from being oxidized to palladium oxide. The heating time during thermal reduction is preferably 1 minute to 24 hours, more preferably 5 minutes to 10 hours, and even more preferably 10 minutes to 1 hour. When the heating time during thermal reduction is within the above range, the Pd complex is easily reduced.

[0063] Step (2) of the present invention can be carried out using, for example, a supercritical processing apparatus. Hereinafter, a supercritical processing apparatus according to one embodiment of the present invention will be described, but the present invention is not limited to this embodiment.

[0064] The supercritical processing apparatus includes a high-pressure cylinder 1 containing liquid carbon dioxide, a syringe pump 2 that supplies liquid at a set flow rate, a reactor 3 consisting of a pressure-resistant container, a filter 4, and a cleaning container 5 that contains a cleaning liquid. A valve V1 is provided in the line connecting the high-pressure cylinder 1 and the syringe pump 2, and valves V2 and V3 and a pressure sensor S1 are provided in the line connecting the syringe pump 2 and the reactor 3. A pressure sensor S2 and a valve V4 are provided in the line connecting the reactor 3 and the filter 4, and valves V5 and V6 are provided in the line connecting the filter 4 and the high-pressure cylinder 1. The cleaning container 5 is connected to the line between valves V2 and V3 via valve V7.

[0065] The reactor 3 is partitioned into a reaction chamber 30 in which the surfactant-containing liquid crystalline polyester multifilament M is placed and a supply chamber 31 disposed above the reaction chamber 30, and a Pd complex C is introduced into the supply chamber 31. Heaters 32 are disposed above and below the reactor 3, and a stirrer 33 is attached to the bottom of the reaction chamber 30. A temperature sensor S3 is also provided to detect the temperature inside the reaction chamber 30.

[0066] When operating the apparatus, an appropriate amount of surfactant-containing liquid crystalline polyester multifilament M is placed in the reaction chamber 30 of the reactor 3 in advance. Then, valve V1 is opened to supply liquid carbon dioxide from the high-pressure cylinder 1 to the syringe pump 2, which then pressurizes the liquid carbon dioxide to a predetermined pressure and places it in a supercritical state. Next, valves V2 and V3 are opened, and high-pressure carbon dioxide fluid is supplied from the syringe pump 2 to the reactor 3 at a set flow rate. The high-pressure carbon dioxide fluid is introduced into the supply chamber 31 from the top of the reactor 3 and mixed with the Pd complex. The high-pressure carbon dioxide fluid mixed with the Pd complex C flows down into the reaction chamber 30. The high-pressure carbon dioxide fluid remaining in the reaction chamber 30 is stirred by the stirrer 33 until the Pd complex is sufficiently dissolved and impregnated into the surfactant-containing liquid crystalline polyester multifilament M. While the surfactant-containing liquid crystalline polyester multifilament M is impregnated with the high-pressure carbon dioxide fluid in the reaction chamber 30 for a predetermined time, the temperature inside the reaction chamber 30 is controlled by the heater 32 to a temperature at which the Pd complex C is thermally reduced.

[0067] In addition, when the surfactant-containing liquid crystal polyester multifilament is easily dissolved in the high-pressure carbon dioxide fluid, it is not necessary to operate the stirring device 33 .

[0068] The surfactant-containing liquid crystalline polyester multifilament M is impregnated with high-pressure carbon dioxide fluid for a predetermined time to thermally reduce the Pd complex, and then valves 6 and 7 are opened to reduce the pressure inside the reactor 3. When reducing the pressure, a needle valve is used to control the pressure reduction so that it gradually reaches atmospheric pressure. Since a sudden reduction in pressure may affect the surfactant-containing liquid crystalline polyester multifilament M, the pressure reduction time is preferably 3 to 120 minutes.

[0069] The carbon dioxide discharged from the reactor 3 is collected in the filter 4 together with the excess Pd complex and its decomposition products. The Pd complex is then separated in the filter 4 and sent to the high-pressure cylinder 1. Therefore, the carbon dioxide used in the treatment can be reused, making it possible to minimize waste and making this a treatment method with a low environmental impact.

[0070] When the surfactant-containing liquid crystalline polyester multifilament M is affected by, for example, deterioration at the thermal reduction temperature of the Pd complex C, reduction treatment may be performed by introducing a reducing agent such as hydrogen gas into the reaction chamber 30 after the surfactant-containing liquid crystalline polyester multifilament M is impregnated with the Pd complex C. Alternatively, reduction treatment may be performed by removing the surfactant-containing liquid crystalline polyester multifilament M from the reaction chamber 30 and immersing it in a container containing a reducing agent solution.

[0071] By the above-described pretreatment, the Pd catalyst can be uniformly attached in an activated state to the surface of the surfactant-containing liquid crystalline polyester multifilament. Note that, although the above-described device supplies supercritical carbon dioxide, it is also possible to supply subcritical carbon dioxide by changing the pressure conditions of the syringe pump 2.

[0072] In the above-mentioned supercritical treatment apparatus, the temperature inside the reaction chamber 30 was set by the heater 32 to a temperature at which the Pd complex C could be thermally reduced, and thermal reduction was carried out. However, the Pd-containing liquid crystalline polyester multifilament (Y) may be taken out of the supercritical treatment apparatus in an unreduced state and then separately subjected to thermal reduction in an oven or the like. Note that the step (2) may be carried out with reference to the supercritical treatment described in Japanese Patent No. 4314370.

[0073] <Process (3)> The step (3) is a step of coating the Pd-containing liquid crystalline polyester multifilament (Y) obtained in the step (2) with a metal.

[0074] Various methods such as wet and dry methods can be used for metal coating. Dry metal coating methods include extrusion, sputtering, vapor deposition, and conventional methods. Wet metal coating can also be carried out by conventional methods, such as electroless plating and electroless plating followed by electrolytic plating.

[0075] As the method for electroless plating, a conventional method can be used, for example, a method of immersing the Pd-containing liquid crystalline polyester multifilament (Y) in an electroless plating solution, etc. Examples of metals to be electrolessly plated include the metals described in the section [Metal-coated liquid crystalline polyester monofilament].

[0076] The electroless plating solution may contain, for example, a metal salt as the main component and other additives (for example, a reducing agent, a complexing agent, a leveler, etc.) The temperature of the electroless plating solution can be appropriately selected depending on the type of electroless plating solution and is, for example, 20 to 130°C, preferably 30 to 100°C, and the electroless plating treatment time is, for example, 5 minutes to 24 hours, preferably 10 minutes to 20 hours.

[0077] Commercially available electroless plating solutions can be used, including, for example, electroless copper plating solutions "ATS-ADDCOPPER IW-A," "ATS-ADDCOPPER IW-M," and "ATS-ADDCOPPER IW-C" manufactured by Okuno Pure Chemical Industries, Ltd., electroless gold plating solution "Selfgold OTK-IT," electroless silver plating solution "Dyne Silver EL-3S," and electroless nickel-phosphorus plating solution "Top Nicoron BL80" manufactured by Uemura Kogyo Co., Ltd., and electroless nickel plating solutions "Nimden KTB-3-M" and "Nimden KTB-3-A" manufactured by Uemura Kogyo Co., Ltd. Note that electroless plating can also be followed by, for example, electroplating.

[0078] The uses of the metal-coated polyester multifilament of the present invention are not particularly limited, and it can be widely used in fields where conductive fibers are used, such as electric wires and electromagnetic wave shielding. [Example]

[0079] The present invention will be described in more detail below with reference to examples, but these examples are not intended to limit the scope of the present invention. Measurement and evaluation methods are shown below.

[0080] <Tensile strength> The tensile strength (cN / dtex) of the metal-coated liquid crystal polyester multifilaments obtained in the examples and comparative examples was measured under the following conditions. Since the strength of the plated fiber is dominated by the strength of the polyarylate fiber before plating, the tensile strength was calculated using the original fiber fineness. (conditions) Testing equipment: Autograph AGS-100B (Shimadzu Corporation) Test conditions: JIS L1013 ·Thread length: 200mm ·Initial load: 0.09cN / dtex Pulling speed: 100mm / min

[0081] <Resistance measurement and bending fatigue test> Using a resistance measuring machine (manufactured by Texio Technology Co., Ltd.), the initial resistance values (Ω / 10 cm) of the metal-coated liquid crystal polyester multifilaments obtained in the examples and comparative examples were measured. Next, using a bending fatigue testing machine (“TC111L”, manufactured by YUASA), under the conditions of a bending diameter of 2.5 mm, a bending angle of 120°, a bending speed of 60 rpm, a load of 100 g, and a bending number of 10,000 times, the metal-coated liquid crystal polyester multifilament was bent, and the resistance value was measured again. The specific resistance value was calculated using the following formula, and the bending fatigue resistance was evaluated. Specific resistance value = (resistance value after bending fatigue test) / (initial resistance value before bending fatigue test)

[0082] <ICP emission spectrometry> After measuring the mass of the metal-coated liquid crystal polyester multifilaments obtained in the examples and comparative examples, it was weighed into a quartz decomposition vessel (capacity: 80 ml), nitric acid, hydrochloric acid, and sulfuric acid were added, and microwave decomposition was performed using an automatic microwave decomposition device (manufactured by CEM, “Discover SP-D80”). After decomposition, it was made up to 100 ml with ultrapure water, filtered through a filtration filter (0.45 μm), and using an ICP emission analyzer (manufactured by Thermo Fisher Scientific K.K., “iCAP6500 Duo”), the content (mass%) of Pd and the content (mass%) of the coating metal contained in the metal-coated liquid crystal polyester multifilament were measured. From this, the amount (mass) of Pd and the amount (mass) of the metal contained in the metal-coated liquid crystal polyester multifilament were determined. Next, the content (mass%) of Pd with respect to the mass of the metal-coated liquid crystal polyester multifilament excluding the coating metal was calculated by dividing the amount (mass) of Pd by the mass obtained by subtracting the amount of the metal from the mass of the metal-coated liquid crystal polyester multifilament and multiplying by 100.

[0083] <Microdroplet law > On the surface of the metal-coated liquid crystal polyester multifilaments obtained in the examples and comparative examples, a thermosetting epoxy resin (manufactured by Huntsman Japan, “Araldite (registered trademark) RapidAfter preparing resin spheres of 100 to 300 μm using a tester (RT30), the resin spheres were peeled off using a universal testing machine (Shimadzu Corporation) equipped with a jig that could hook the spheres. The interfacial adhesive strength (N / mm) was calculated from the stress at the maximum point and the coated area measured by SEM. 2 ) was measured.

[0084] <Thickness of the coated metal> The thickness of the coating metal of the metal-coated liquid crystal polyester multifilament obtained in the examples and comparative examples was determined by X-ray CT according to the following method. First, 10 cross-sectional photographs of the liquid crystal polyester multifilament before plating used in Examples and Comparative Examples were taken at 50 μm intervals by X-ray CT, and the fiber diameters of 10 fibers were measured for each cross-sectional photograph. The average value of the fiber diameters of the liquid crystal polyester multifilament measured for a total of 100 fibers was defined as the fiber diameter of the liquid crystal polyester multifilament. Next, the fiber diameters of a total of 100 metal-coated liquid crystal polyester multifilaments after plating used in the examples and comparative examples were measured by the same method, and the average value of the measured fiber diameters of the metal-coated liquid crystal polyester multifilaments was taken as the fiber diameter of the metal-coated liquid crystal polyester multifilaments. Finally, the thickness of the metal coating was calculated using the following formula. Thickness of the coated metal = [(fiber diameter of metal-coated liquid crystal polyester multifilament) - (fiber diameter of liquid crystal polyester multifilament)] ÷ 2

[0085] [Example 1] <Preparation of surfactant-containing liquid crystalline polyester multifilament (X)> As the fiber material, a liquid crystal polyester multifilament with a total fineness of 1670 dtex and 300 filaments (polyarylate fiber, manufactured by Kuraray Co., Ltd., trade name: Vectran HT) was used. To this liquid crystal polyester multifilament, 0.5 parts by mass of hexadecylpyridinium chloride, a cationic surfactant, was added (applied) as a surfactant, and a surfactant-containing liquid crystal polyester multifilament (X) having the surfactant coated on the surface of the liquid crystal polyester monofilament was obtained. The addition amount of the above surfactant is the amount based on 100 parts by mass of the fiber material.

[0086] <Production of Pd-containing liquid crystal polyester multifilament (Y)> The surfactant-containing liquid crystal polyester monofilament (X) was subjected to catalyst application by supercritical treatment as follows, and a Pd-containing liquid crystal polyester multifilament (Y) containing a surfactant and Pd atoms was obtained on the surface and inside of the liquid crystal polyester monofilament.

[0087] (Catalyst application) For the pretreatment before plating, the apparatus shown in Fig. 1 was used. The internal volume of the reactor 3 was 10 ml, and liquid carbon dioxide was supplied from the high-pressure cylinder 1 at a pressure of 25 MPa. Palladium acetate complex was used as the catalyst. The fiber material was set in the reaction chamber 30, palladium acetate was charged into the supply chamber 31, and the reactor 3 was sealed. The addition amount of the palladium acetate complex was 2.0 parts by mass with respect to 100 parts by mass of the fiber material. Next, the liquid carbon dioxide was pressurized by the syringe pump 2 (manufactured by ISCO, "MODEL260D") to a supercritical state and supplied to the reactor 3 at a flow rate of 40 to 50 ml / min. The pressure in the syringe pump 2 was set to 25 MPa. The temperature in the reaction chamber 31 was maintained at 80 °C for 30 minutes by heating control of the heater. By maintaining this temperature, the palladium acetate complex could be quickly dissolved by utilizing the high diffusibility and high permeability of the supercritical carbon dioxide fluid. After removing the carbon dioxide from the supercritical reactor, the Pd-containing liquid crystalline polyester multifilament (Y) obtained changed from yellow before the catalyst was added to a deep orange color, the same color as palladium acetate. Furthermore, after the reduction process described below, the Pd-containing liquid crystalline polyester multifilament (Y) changed to a glossy black color, suggesting that a large amount of catalyst was added to the fiber surface.

[0088] The obtained Pd-containing liquid crystalline polyester multifilament (Y) was subjected to thermal reduction to obtain a reduced Pd-containing liquid crystalline polyester multifilament (Y).

[0089] (thermal reduction) The Pd-containing liquid crystal polyester multifilament (Y) to which the catalyst had been applied was treated in an oven (manufactured by Yamato Scientific Co., Ltd.) set at 200° C. for 30 minutes to thermally reduce the palladium acetate complex.

[0090] <Preparation of metal-coated liquid crystal polyester multifilament> The reduced Pd-containing liquid crystal polyester multifilament (Y) was subjected to electroless plating as follows to obtain a metal-coated liquid crystal polyester multifilament.

[0091] (Electroless Cu plating) To a 300 ml beaker (manufactured by AS ONE Corporation) were added 10 ml of ATS-ADDCOPPER IW-A (manufactured by Okuno Junyaku Co., Ltd.), 16 ml of ATS-ADDCOPPER (manufactured by Okuno Junyaku Co., Ltd.), 2 ml of ATS-ADDCOPPER (manufactured by Okuno Junyaku Co., Ltd.), and 172 ml of ion-exchanged water, and the reduced Pd-containing liquid crystalline polyester multifilament (Y) was added, followed by stirring in a water bath at 40°C for 15 minutes.

[0092] [Example 2] Except for changing the surfactant to be added to the cationic surfactant benzylconium chloride, surfactant-containing liquid crystalline polyester multifilament (X), Pd-containing liquid crystalline polyester multifilament (Y), and metal-coated liquid crystalline polyester multifilament were obtained in the same manner as in Example 1. The Pd-containing liquid crystalline polyester multifilament (Y) changed to a deep orange color after catalyst addition, and changed to a glossy dark black color after reduction, suggesting that a large amount of catalyst had been introduced.

[0093] [Example 3] Except for changing the amount of surfactant added to 1.5 parts by mass and the amount of palladium acetate complex added to 6 parts by mass, a surfactant-containing liquid crystalline polyester multifilament (X), a Pd-containing liquid crystalline polyester multifilament (Y), and a metal-coated liquid crystalline polyester multifilament were obtained in the same manner as in Example 1. The Pd-containing liquid crystalline polyester multifilament (Y) changed to a deep orange color after catalyst addition and to a glossy jet black after reduction, suggesting that a large amount of catalyst had been introduced.

[0094] [Example 4] A surfactant-containing liquid crystal polyester multifilament (X), a Pd-containing liquid crystal polyester multifilament (Y), and a metal-coated liquid crystal polyester multifilament were obtained in the same manner as in Example 1, except that a liquid crystal polyester multifilament (polyarylate fiber, manufactured by Kuraray Co., Ltd., product name: Vectran HT) having a total fineness of 440 dtex and 80 filaments was used as the fiber material. The Pd-containing liquid crystal polyester multifilament (Y) changed to a deep orange color after the addition of the catalyst and to a glossy black color after reduction, suggesting that a large amount of catalyst had been introduced.

[0095] [Example 5] A surfactant-containing liquid crystalline polyester multifilament (X), a Pd-containing liquid crystalline polyester multifilament (Y), and a metal-coated liquid crystalline polyester multifilament were obtained in the same manner as in Example 1, except that the plating metal was nickel.

[0096] (Electroless Ni plating) 60 ml of Nimden KTB-3-M (manufactured by Uemura Kogyo Co., Ltd.), 21.6 ml of Nimden KTB-3-A (manufactured by Uemura Kogyo Co., Ltd.) and 318.4 ml of ion-exchanged water were added, and the reduced Pd-containing liquid crystalline polyester multifilament (Y) was added, followed by stirring in a hot water bath at 80°C for 15 hours.

[0097] [Comparative Example 1] Except for not adding a surfactant, a liquid crystal polyester multifilament (X) (surfactant-free), a Pd-containing liquid crystal polyester multifilament (Y), and a metal-coated liquid crystal polyester multifilament were obtained in the same manner as in Example 1. The Pd-containing liquid crystal polyester multifilament (Y) showed almost no change in color after adding the catalyst, and turned slightly black after reduction, indicating that only a small amount of catalyst had been introduced.

[0098] Comparative Example 2 Except for changing the surfactant to the anionic oil oleic acid, a surfactant-containing liquid crystalline polyester multifilament (X), a Pd-containing liquid crystalline polyester multifilament (Y), and a metal-coated liquid crystalline polyester multifilament were obtained in the same manner as in Example 1. The Pd-containing liquid crystalline polyester multifilament (Y) was slightly darker after the catalyst was added, and turned slightly black after reduction, suggesting that a small amount of catalyst had been introduced.

[0099] Comparative Example 3 Except for changing the surfactant to octadecanol, a nonionic surfactant, surfactant-containing liquid crystalline polyester multifilament (X), Pd-containing liquid crystalline polyester multifilament (Y), and metal-coated liquid crystalline polyester multifilament were obtained in the same manner as in Example 1. The Pd-containing liquid crystalline polyester multifilament (Y) after catalyst addition was slightly darker in color, and after reduction it turned slightly black, suggesting that a small amount of catalyst had been introduced.

[0100] Comparative Example 4 Except for changing the surfactant to the nonionic surfactant sorbitan monourate, a surfactant-containing liquid crystalline polyester multifilament (X), a Pd-containing liquid crystalline polyester multifilament (Y), and a metal-coated liquid crystalline polyester multifilament were obtained in the same manner as in Example 1. The Pd-containing liquid crystalline polyester multifilament (Y) was slightly black after the catalyst was added, and changed to a dark black after reduction, suggesting that a large amount of catalyst had been introduced.

[0101] Comparative Example 5 A liquid crystal polyester multifilament (X) (surfactant-free), a Pd-containing liquid crystal polyester multifilament (Y), and a metal-coated liquid crystal polyester multifilament were obtained in the same manner as in Comparative Example 1, except that a liquid crystal polyester multifilament (polyarylate fiber, manufactured by Kuraray Co., Ltd., product name: Vectran UM) having a total fineness of 440 dtex and 80 filaments was used as the fiber material. The Pd-containing liquid crystal polyester multifilament (Y) was slightly darker after the catalyst was added, and turned slightly black after reduction, suggesting that a small amount of catalyst had been introduced.

[0102] Comparative Example 6 A surfactant-containing liquid crystalline polyester multifilament (X), a Pd-containing liquid crystalline polyester multifilament (Y), and a metal-coated liquid crystalline polyester multifilament were obtained in the same manner as in Example 1, except that the catalyst application and reduction methods were changed to aqueous systems as follows.

[0103] (Catalyst addition and reduction) To clean the surface of the surfactant-containing liquid crystalline polyester multifilament (X), 50 ml of acetone was placed in a beaker, and the multifilament cut to 1 m was added and stirred at 30°C for 5 minutes. Next, to adsorb the catalyst, 13 g of OPC-SAL-M (Okuno Pharmaceutical Industries Co., Ltd.) and 2.25 ml of OPC-80 Catalyst ML (Okuno Pharmaceutical Industries Co., Ltd.) were added, and the mixture was diluted to 60 ml with ion-exchanged water. The washed multifilament was then added and treated at 25°C for 5 minutes. Finally, to activate the catalyst, 5 g of sulfuric acid was added to 95 ml of ion-exchanged water, and the catalyst-absorbed multifilament was added and stirred at 35°C for 6 minutes.

[0104] Comparative Example 7 A surfactant-containing liquid crystalline polyester multifilament (X), a Pd-containing liquid crystalline polyester multifilament (Y), and a metal-coated liquid crystalline polyester multifilament were obtained in the same manner as in Comparative Example 6, except that the filaments were treated with a 15% aqueous sodium hydroxide solution at 65°C for 2 minutes before the catalyst was added.

[0105] [Comparative Example 8] A polyester multifilament (X) (surfactant-free), a Pd-containing liquid crystalline polyester multifilament (Y), and a metal-coated liquid crystalline polyester multifilament were obtained in the same manner as in Comparative Example 1, except that electroless Ni plating was performed in the same manner as in Example 5.

[0106] [Example 6] The surfactant-containing liquid crystalline polyester multifilament (X) obtained in Example 1 was treated with supercritical carbon dioxide without adding a catalyst under the same conditions as in Example 1. The residual surfactant rate was calculated from the mass before and after the treatment using the following formula. Surfactant residual rate (mass%)=(mass of fiber after supercritical treatment−mass of fiber itself) / (mass of fiber after surfactant addition−mass of fiber itself)×100

[0107] [Example 7] The residual surfactant rate was calculated in the same manner as in Example 6, except that the surfactant-containing liquid crystal polyester multifilament (X) obtained in Example 2 was used.

[0108] Comparative Example 9 The residual surfactant rate was calculated in the same manner as in Example 6, except that the surfactant-containing liquid crystal polyester multifilament (X) obtained in Comparative Example 2 was used.

[0109] [Comparative Example 10] The residual surfactant rate was calculated in the same manner as in Example 6, except that the surfactant-containing liquid crystal polyester multifilament (X) obtained in Comparative Example 3 was used.

[0110] [Comparative Example 11] The residual surfactant rate was calculated in the same manner as in Example 6, except that the surfactant-containing liquid crystal polyester multifilament (X) obtained in Comparative Example 4 was used.

[0111] For the metal-coated liquid crystalline polyester multifilaments obtained in Examples 1 to 5 and Comparative Examples 1 to 8, the thickness of the coating metal, the Pd content in the multifilaments excluding the coating metal obtained by ICP atomic emission spectrometry, interfacial adhesive strength, tensile strength, initial resistance, and specific resistance were measured according to the above-mentioned measurement methods, and the results are shown in Table 5. Furthermore, the surfactant residual rates obtained in Examples 6 and 7 and Comparative Examples 9 to 11 are shown in Table 6. The total fineness, number of filaments (number of monofilaments), surfactant name, surfactant addition amount (parts by mass), complex addition amount (parts by mass), catalyst treatment conditions, and type of plating metal of the metal-coated liquid crystalline polyester multifilaments are also shown in Table 5. The same applies to Table 6.

[0112] [Table 5]

[0113] [Table 6]

[0114] As shown in Table 5, it was confirmed that the metal coated liquid crystal polyester multifilaments obtained in Examples 1 to 5 had lower specific resistance values ​​and better resistance to bending fatigue than those of Comparative Examples 1 to 8. [Explanation of symbols]

[0115] 1...High-pressure cylinder, 2...Syringe pump, 3...Reactor, 4...Filter, 5...Ultrasonic vibrator, 30...Reaction chamber, 31...Supply chamber, 32...Heater, 33...Agitator, V1 to V7...Valves, S1 to S3...Pressure sensors

Claims

1. A metal-coated liquid crystal polyester multifilament comprising two or more metal-coated liquid crystal polyester monofilaments each having a surface coated with a metal having a thickness of 0.1 to 20 μm, wherein the Pd content determined by ICP emission spectrometry is 0.33 mass% or more relative to the mass of the multifilament excluding the coating metal, and the interfacial adhesive strength of the coating metal measured by the microdroplet method is 15 N / mm 2 As described above, the interfacial adhesion strength of the coated metal measured by the microdroplet method is calculated from the stress at the maximum point when peeling off a resin sphere of 100 to 300 μm created on the surface of the metal-coated liquid crystal polyester multifilament using Araldite (registered trademark) Rapid RT30, a thermosetting epoxy resin manufactured by Huntsman Japan, and the area covered by the resin sphere.

2. The metal-coated liquid crystal polyester multifilament according to claim 1, wherein the tensile strength is 16 cN / dtex or more.

3. 3. The metal-coated liquid crystal polyester multifilament according to claim 1, wherein the metal comprises at least one selected from the group consisting of copper, silver, gold, iron, zinc, lead, palladium, nickel, chromium, and tin.

4. The method for producing the metal-coated liquid-crystalline polyester multifilament according to any one of claims 1 to 3, comprising: step (1) of applying a cationic surfactant to the surface of the liquid-crystalline polyester multifilament; step (2) of contacting the surfactant-containing liquid-crystalline polyester multifilament obtained in step (1) with a high-pressure carbon dioxide fluid having a Pd complex dissolved therein; and step (3) of coating the Pd-containing liquid-crystalline polyester multifilament obtained in step (2) with a metal.

5. The method of claim 4 , wherein the surfactant comprises a halogen atom and a nitrogen atom-containing cationic surfactant.

6. The method according to claim 4 or 5, wherein the residual surfactant rate when the surfactant-containing liquid crystal polyester multifilament is brought into contact with a high-pressure carbon dioxide fluid is 10 mass % or more.

Citation Information

Patent Citations

  • Method for producing surface-hydrophilized high-strength fiber yarn

    JP2011058117A

  • Fiber plating implement, and fiber plating method using the same

    JP2011190476A

  • Plating liquid for polymer fiber, method for plating polymer fiber using the same, and method for producing the same

    JP2011231382A

  • Method for pretreatment before plating

    JP2012144762A

  • Polymer fiber conductive wire and manufacturing method thereof

    JP2016212960A