Method for manufacturing liquid ejection head substrate
The method stabilizes the engraving process of a liquid ejection head substrate by using etching masks and reactive ion etching to form a supply port and dug region, addressing shape instability issues in existing methods.
Patent Information
- Application Number
- JP2020109837
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-06-25
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2040-06-25
AI Technical Summary
Existing methods for engraving the surface of a liquid ejection head substrate, such as mechanical means or chemical etching, often result in unstable shapes of the flow path, affecting liquid flow and discharge due to deformation of the supply port.
A method involving an etching mask that covers a member with an opening, followed by reactive ion etching to form a supply port and dug region on the substrate, using etching masks of SiN, SiC, or photosensitive resin to stabilize the shape.
Enables stable engraving of the substrate surface, ensuring consistent liquid flow and discharge by controlling the shape of the dug region and supply port.
Smart Images

Figure 0007562310000001 
Figure 0007562310000002 
Figure 0007562310000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a liquid ejection head substrate. [Background technology]
[0002] A liquid ejection device such as an inkjet printer has a liquid ejection head, which is a part that ejects liquid. The liquid ejection head has a liquid ejection head substrate, which is called a chip or the like. A known liquid ejection head substrate has a substrate having a supply port and a flow path forming member that forms a flow path on the substrate. The flow path formed by the flow path forming member includes a pressure chamber, and liquid is ejected from a discharge port by applying pressure to the liquid in the pressure chamber from a pressure generating element.
[0003] In such a liquid ejection head substrate, there is a need to eject liquid at high speeds and at short intervals. By ejecting liquid at high speeds, it becomes possible to record characters or images using liquid at high speeds. In order to eject liquid at high speeds, it is necessary to replenish the liquid into the pressure chamber more quickly when ejecting liquid.
[0004] By shortening the distance from the supply port of the substrate to the pressure chamber, the flow resistance is reduced and the speed at which the liquid is replenished to the pressure chamber is increased. Patent Document 1 describes a liquid ejection head substrate in which the surface of the substrate is dug in the vicinity of the opening of the supply port, thereby shortening the distance from the supply port to the pressure chamber and reducing the flow resistance. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 10-095119 Summary of the Invention [Problem to be solved by the invention]
[0006] In Patent Document 1, mechanical means such as drills, the use of light energy such as lasers, and chemical etching are exemplified as methods for engraving the surface of the substrate, but no specific engraving methods are described. When engraving the substrate using these methods, it is possible to directly process the surface of the substrate using mechanical means or lasers, or to provide an etching mask on the surface of the substrate and perform chemical etching. However, when engraving the substrate using these methods, the shape of the engraved portion may not be stable. For example, in direct processing using mechanical means, the width of the engraved portion is difficult to stabilize. In addition, in etching using an etching mask, the etching solution or etching gas may flow around to the supply port side, and the shape of the supply port itself may be deformed, which may affect the shape of the engraved portion. As a result, the shape of the flow path on the substrate may not be the desired shape, which may affect the flow of liquid in the flow path and the discharge of liquid.
[0007] SUMMARY OF THE PRESENT EMBODIMENTS Accordingly, an object of the present invention is to provide a method for manufacturing a liquid ejection head substrate, which is capable of stably engraving the surface of the substrate. [Means for solving the problem]
[0008] The above-mentioned problems are solved by the present invention. That is, the present invention provides a liquid supply device comprising: a substrate having a supply port; a pressure generating element and a flow path forming member for forming a flow path for liquid on the substrate; ,of A method for manufacturing a liquid ejection head substrate, comprising: It is made of at least one of Al, AlCu, and TaSiN. This method for manufacturing a liquid ejection head substrate comprises the steps of: providing a member; an etching mask covering the member and having an opening; removing the member to form a space from which the member has been removed; and etching the substrate through the opening in the etching mask by reactive ion etching to form a supply port in the substrate, the space being exposed to the opening; and in the step of forming the supply port in the substrate, the substrate is etched from the space, and an etched region of the substrate is formed below the space. Effect of the Invention
[0009] According to the present invention, it is possible to provide a method for manufacturing a liquid ejection head substrate, which enables the substrate surface to be etched stably. [Brief description of the drawings]
[0010] [Figure 1] 5A to 5C are diagrams illustrating a manufacturing process of a liquid ejection head substrate. [Diagram 2] FIG. 2 is a cross-sectional view of a liquid ejection head substrate. [Diagram 3] 5A to 5C are diagrams illustrating a manufacturing process of a liquid ejection head substrate. [Figure 4] 3A and 3B are a top view and a cross-sectional view of a liquid ejection head substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, a method for manufacturing a liquid ejection head substrate according to the present invention will be described with reference to the drawings. In the following embodiments, specific descriptions may be used to fully explain the present invention, but these are merely examples that are technically preferable and do not limit the scope of the present invention.
[0012] FIG. 1 shows a method for manufacturing a liquid ejection head substrate. FIG. 1(f) is a cross-sectional view of a part of a completed liquid ejection head substrate, and FIG. 1(f') is a top view of the same liquid ejection head substrate. FIG. 1 shows cross-sectional views ((a) to (f)) and top views ((a') to (f')) of the liquid ejection head substrate in each process. The liquid ejection head substrate has a substrate 5 having a supply port 10. On the substrate 5, a flow path forming member 14 is provided, which forms a flow path 12 and an ejection port 13 for ejecting liquid. On the surface (on the substrate) of the substrate 5, a pressure generating element 1 is provided, and an area of the flow path 12 above the pressure generating element 1 becomes a pressure chamber. Pressure is applied to the liquid in the pressure chamber from the pressure generating element 1 on the substrate, and the pressurized liquid is ejected from the ejection port 13. In this specification, the direction in which the liquid is ejected is from below to above.
[0013] A method for manufacturing such a liquid ejection head substrate will be described step by step. First, as shown in FIG. 1(a), a substrate 5 having an insulating layer 2 on the surface side is prepared. FIG. 2 is a diagram showing FIG. 1(a) in more detail. An example of the substrate 5 is a silicon single crystal substrate. An example of the insulating layer 2 is SiN, SiC, SiCN, SiO2, or the like. A multi-layered electrical wiring layer 3 is embedded in the insulating layer 2, and a pressure generating element 1 is provided on the surface side of the insulating layer 2. The electrical wiring layer 3 supplies electricity supplied from the outside to the pressure generating element 1, and the pressure generating element 1 is driven by the supplied electricity. The electrical wiring layer 3 and the pressure generating element 1 are formed of metals such as Al, AlCu, and TaSiN. At this time, a member 4 arranged on the substrate is embedded in the insulating layer 2. The member 4 is provided to dig into the surface of the substrate 5, and details thereof will be described later.
[0014] As shown in FIG. 2, an insulating layer (interlayer insulating layer 23) is sandwiched between multiple electrical wiring layers 21, and the electrical wiring layers 21 are electrically connected to each other by tungsten plugs 22. Member 4 is located on the surface of substrate 5, and its height (the thickness of member 4 in the vertical direction) is designated as L1. L1 affects the size of recessed region 11, which will be described later. From this perspective, L1 is preferably 0.2 μm or more and 10 μm or less, and more preferably 0.4 μm or more and 1.0 μm or less. As shown in FIG. 1(a'), when substrate 5 is viewed from above (the side facing the surface of substrate 5), one member 4 is provided corresponding to two pressure generating elements 1.
[0015] After preparing a substrate 5 as shown in FIG. 1(a), a first etching mask 6 is provided on the insulating layer 2 as shown in FIG. 1(b), and the insulating layer 2 is patterned using the first etching mask 6. The first etching mask 6 is preferably formed of SiN, SiC, SiCN, a photosensitive resin, or the like. For example, a layer to be the first etching mask is applied so as to cover the insulating layer 2, and then the layer is patterned to form an opening 6' to become the first etching mask. Then, the insulating layer 2 is etched from the opening 6' of the first etching mask 6 by dry etching or the like, and the insulating layer 2 is patterned. This patterning forms an opening 7 in the insulating layer 2. The opening 7 has a shape corresponding to the opening 6'. At this time, the member 4 is exposed in the opening 7, and when the substrate 5 is viewed from above as shown in FIG. 1(b'), the member 4 is disposed in the opening 7.
[0016] Next, the first etching mask 6 is removed, and a second etching mask 8 is provided (FIG. 1(c)). The second etching mask 8 is preferably formed of SiN, SiC, SiCN, photosensitive resin, or the like. For example, a layer to be the second etching mask is applied so as to cover the insulating layer 2 and the member 4, and then the layer is patterned to form an opening 8' to become the second etching mask 8. Here, when the substrate 5 is viewed from above, the opening 8' of the second etching mask 8 is formed to be located inside the opening 7 of the insulating layer 2. Also, the member 4 is covered by the second etching mask 8, but the member 4 is exposed in the opening 8' in the cross section of the substrate 5. For example, when the second etching mask 8 is formed of a photosensitive resin, the second etching mask 8 is patterned by photolithography to form the opening 8'. In the development process of this photolithography, the member 4 is removed together with the development of the second etching mask 8, and the area where the member 4 was present becomes a space 9. That is, when the opening 8' is formed, the member 4 is exposed in the opening 8', and the developer dissolves the member 4 from the exposed portion of the member 4, and finally the space 9 is formed. In order to form the space 9 in this way, the second etching mask 8 is preferably formed of a photosensitive resin. Also, the member 4 is preferably formed of a material that is dissolved and removed by the developer of the photosensitive resin. Examples of such materials include metal. Among them, if the member 4 is formed of the same material as the electrical wiring layer 21, it can be formed together with the electrical wiring layer 21. For example, examples of materials for forming the member 4 and the electrical wiring layer 21 include Al, AlCu, and TaSiN. The same material means that the material is the same as long as both are called Al, and it does not matter if the chemical structures are strictly the same. Considering the removal later, the member 4 is preferably formed of Al or AlCu. It is not necessary to remove the member 4 in the process of forming the opening 8', and for example, after the opening 8' is formed by the developer, it may be removed by another method (for example, a solvent of a material different from the developer).
[0017] Next, as shown in FIG. 1(d), the substrate 5 is etched from the opening 8' of the second etching mask 8. This etching is performed by reactive ion etching, and a liquid supply port 10 is formed in the substrate 5. At this time, since the space 9 between the substrate 5 and the second etching mask 8 is exposed to the opening 8', radical components that etch the substrate 5 enter the space 9. The radical components that have entered the space 9 also etch the substrate 5 below the space 9, forming a carved region 11. The carved region 11 is a carved portion of the substrate surface. In addition, the carved region 11 is adjacent to the supply port 10, and can also be said to be a part of the supply port.
[0018] The reactive ion etching process for etching the substrate 5 to form the supply port 10 and the recessed region 11 includes the Bosch process and the non-Bosch process. In the Bosch process, a substrate etching step and a coating step of the etched region are repeated. In the non-Bosch process, the sidewalls of the etched region are protected by a coating at the same time as the substrate is etched. In terms of easier control of the shape of the recessed region 11, etching by the Bosch process is preferable. In the Bosch process, the etching gas is preferentially introduced into the space 9 below the second etching mask 8 by increasing the time, power, and gas pressure of the first etching step, and the substrate below the space is preferentially etched. Then, by switching to the coating step after that, the substrate below the space is not etched any further, and the shape of the recessed region 11 is stabilized. On the other hand, in the supply port 10, the coating at the bottom is easily removed, and unlike the recessed region 11, it can be extended vertically downward in the next etching step. When the non-Bosch process is used, it is necessary to control the shape of the member 4 so that the substrate 5 below the space 9 is not etched as much as possible.
[0019] After the supply port 10 and the recessed region 11 are formed, the second etching mask 8 is removed to obtain the state shown in FIG. 1(e). Next, as shown in FIG. 1(f), a flow path forming member 14 for forming the flow path 12 and the discharge port 13 is provided on the surface of the substrate 5. The method for forming the flow path forming member 14 is not particularly limited, but for example, the flow path forming member 14 is formed using a plurality of dry films made of a photosensitive resin. Examples of the dry film include a polyethylene terephthalate (hereinafter referred to as PET) film, a polyimide film, and a polyamide film. In addition, the flow path forming member 14 can be formed of a metal or silicon. In this example, the flow path forming member 14 forms the flow path 12 and the discharge port 13, but the member forming the flow path 12 and the member forming the discharge port may be different members.
[0020] In this manner, the liquid ejection head substrate can be manufactured. As shown in FIG. 1(f), the surface of the liquid ejection head substrate is dug in the vicinity of the opening of the supply port 10 by the amount of the dug region 11. As described above, the dug region 11 is formed by reactive ion etching from the space 9. The space 9 can be controlled by the dimensions of the member 4. The member 4 is formed, for example, by applying the material of the member 4, forming a mask thereon, and then performing dry etching using this mask. That is, the dimensions of the member 4 are easier to control compared to when the substrate 5 is directly processed, and the shape of the dug region 11 can be controlled by the easily controllable member 4, so that the substrate surface can be dug in a stable manner.
[0021] As shown in FIG. 1(f) and FIG. 2, the liquid ejection head substrate is preferably in a form in which an interlayer insulating layer is sandwiched between multiple electrical wiring layers. In this way, the height of the entire insulating layer is higher than when the electrical wiring layer is a single layer. That is, when the end of the insulating layer is retreated from the opening of the supply port 10 as shown in FIG. 1(f), the efficiency of the flow of the liquid in the flow path (refill efficiency) can be further improved, similar to the case where the surface of the substrate is deeply dug. From this viewpoint, the thickness of the insulating layer is preferably 4 μm or more, and more preferably 6 μm or more. When the insulating layer is formed of a plurality of layers, the thickness of the insulating layer is the total thickness. In addition, when an electrical wiring layer is present between the insulating layers, the thickness includes the electrical wiring layer. The upper limit of the thickness of the insulating layer is preferably 20 μm or less, taking into consideration the overall design of the liquid ejection head substrate. EXAMPLES
[0022] The present invention will now be described more specifically with reference to examples.
[0023] <Example 1> A method for manufacturing a liquid ejection head substrate will be described with reference to Fig. 3(a) to (h). First, as shown in Fig. 3(a), a substrate 5 was prepared having a pressure generating element 1 made of TaSiN on the surface side, an insulating layer 2 made of SiO2, and an electric wiring layer (not shown) made of Al. The substrate 5 is a single crystal substrate of silicon. The insulating layer 2 has a thickness of 10 µm. Four electric wiring layers are provided inside the insulating layer 2, and are connected by tungsten plugs (not shown). In addition, a member 4 made of AlCu is disposed between the insulating layer 2 and the substrate 5 at a position corresponding to the opening of a supply port to be formed later.
[0024] Next, as shown in FIG. 3(b), an etching mask 31 was provided on the back surface, which is the surface opposite to the front surface of the substrate 5, and a common supply port 32 was formed by reactive ion etching. The common supply port 32 is a supply port provided commonly to a plurality of supply ports 35 to be formed later. The etching mask 31 was formed of a novolac-based photoresist. The depth of the common supply port 32 was set to 500 μm, and SF6 gas was used in the etching step and C4F8 gas in the coating step, with a gas pressure of 10 Pa and a gas flow rate of 500 sccm. The etching time was set to 20 seconds, the coating time to 5 seconds, and a platen power of 150 W was applied for 10 seconds of the etching time. The etching conditions at that time were set to SF6 gas in the etching step and C4F8 gas in the coating step, with a gas pressure of 10 Pa and a gas flow rate of 500 sccm. The etching time was set to 20 seconds, the coating time to 5 seconds, and a platen power of 150 W was applied for 10 seconds of the etching time. This is an etching technique called the Bosch process among reactive ion etching techniques.
[0025] Next, the etching mask 31 was removed, and a first etching mask 33 was provided on the front surface side of the substrate 5, as shown in Fig. 3(c). The first etching mask 33 was formed by applying a novolac-based positive resist to a thickness of 20 µm, pre-baking it at 150°C, and then exposing and developing it.
[0026] Next, the insulating layer 2 was etched by reactive ion etching using the first etching mask 33 as a mask, as shown in FIG. 3(d), to form an opening 7 in the insulating layer 2. After that, the first etching mask 33 was removed. The reactive ion etching for etching the insulating layer 2 was performed using a mixed gas of C4F8 gas, CF4 gas, and Ar gas, with the flow rate of C4F8 gas set to 10 sccm and the platen power set to 100 W. In this etching, the substrate 5 made of silicon was used as an etching stop layer. That is, as the etching of the insulating layer 2 progresses, the etching gas (etching area) reaches the substrate 5. Since the etching selectivity of the insulating layer 2 and the substrate 5 is about 100 (the substrate 5 is more difficult to etch), the etching is stopped after the etching gas reaches the substrate 5. In this way, the substrate 5 was used as an etching stop layer. It should be noted that if the insulating layer is etched by 10 μm and then additional etching (overetching) is performed by 20%, the substrate 5 is calculated to be shaved by about 0.02 μm. Therefore, the height of the insulating layer 2 became the height of the opening 7 almost directly.
[0027] Next, as shown in FIG. 3(e), a second etching mask 34 was formed. The second etching mask 34 was formed by applying a novolac-based positive resist to a thickness of 20 μm so as to cover the member 4 and the insulating layer 2, pre-baking at 150° C., and then exposing and developing the resist. The second etching mask 34 has an opening 34′. By using an alkaline developer (NMD3) as the developer for the second etching mask, the member 4 (AlCu) formed between the insulating layer 2 and the substrate 5 was removed by the developer that entered through the opening 34′. The portion from which the member 4 was removed is the space 9. As shown in FIG. 3(e), the space 9 is open (exposed) at the opening 34′.
[0028] Next, as shown in FIG. 3(f), the substrate 5 was etched from the opening 34' of the second etching mask 34 to form the supply port 35. Reactive ion etching was used for the etching. By performing reactive ion etching in a state where a space 9 exists between the etching mask and the substrate, the supply port 35 and the recessed region 11 located below the space 9 were formed at the same time. The supply port 35 was etched until the supply port 35 communicated with the common supply port 32. The etching conditions at that time were a Bosch process using an etching step and a coating step. In detail, SF6 gas was used in the etching step, and C4F8 gas was used in the coating step, with a gas pressure of 10 Pa and a gas flow rate of 500 sccm. The etching time was 20 seconds, the coating time was 5 seconds, and a platen power of 150 W was applied for 10 seconds of the etching time.
[0029] Thereafter, as shown in Fig. 3(g), the second etching mask 34 was removed. Next, a dry film formed of a negative photosensitive resin (epoxy resin) was attached to the substrate 5, and photolithography was performed to form the flow path forming member 14 that forms the flow path 12 and the discharge port 13 (Fig. 3(h)).
[0030] The liquid discharge head substrate manufactured as described above is shown in FIG. 4. FIG. 4(a) is a top view of the liquid discharge head substrate, and FIG. 4(b) is a cross-sectional view of the liquid discharge head substrate. FIG. 4(c) is an enlarged view of the dug region 11 in FIG. 4(b), that is, the portion where the surface of the substrate 5 is dug. According to the manufacturing method of this embodiment, the shape of the dug region 11 can be controlled by the dimensions of the member 4, so that the shape of the dug region 11 can be easily stabilized. In addition, the surface of the substrate 5 exists between the end of the insulating layer 2 on the supply port 35 side and the end of the region 11 where the substrate 5 is etched. The length of the surface of the substrate 5 is D1. D1 can be controlled by the positional relationship between the member 4 and the insulating layer 2, not by etching the substrate 5. As shown in FIG. 4(c), by configuring the sloped dug region 11, the flat surface of the substrate, and the inclined end of the insulating layer 2, the flow of the liquid in the flow path can be better controlled.
[0031] <Example 2> The differences from Example 1 will be described with reference to FIG. 3. After proceeding to the process shown in FIG. 3(e) as in Example 1, the etching conditions shown in FIG. 3(f) were changed. Specifically, the method of alternately performing the etching step and the coating step in the Bosch process described in Example 1 was used, but the etching time was increased only for the first etching step, from 20 seconds to 22 seconds (10% longer). By making the first etching step 10% or more longer than the other etching steps in this way, the etching gas was more likely to enter the space existing at the interface between the etching mask and the substrate, and the carved region 11 became larger. Compared to Example 1, the carved region 11 was made larger, so that the efficiency of the liquid flow in the flow path can be further improved. The same effect can be expected not only by increasing the etching step time but also by increasing the gas pressure, gas flow rate, and coil power of the first etching step by 10% or more compared to those of the other etching steps. [Explanation of symbols]
[0032] 1 Pressure generating element 4. Materials 5 Substrate 9 Space from which a component has been removed 11 Excavation Area 13 Outlet 14 Flow path forming member
Claims
1. A method for manufacturing a liquid ejection head substrate having a substrate having a supply port, and a pressure generating element and a flow path forming member forming a liquid flow path on the substrate, comprising the steps of: providing, on a substrate, a member formed of at least one of Al, AlCu, and TaSiN, and an etching mask covering the member and having an opening; removing the member to form a space from which the member has been removed; and etching the substrate through the openings in the etching mask by reactive ion etching to form supply ports in the substrate. A method for manufacturing a liquid ejection head substrate, characterized in that the space is exposed to the opening, and in a process of forming a supply port in the substrate, the substrate is etched from the space, and an etched region of the substrate is formed below the space.
2. A method for manufacturing a liquid ejection head substrate having a substrate having a supply port, and on the substrate, a pressure generating element, a flow path forming member that forms a flow path for liquid, and an ejection port for ejecting liquid, comprising: providing a member on a substrate and an etching mask covering the member and having an opening; removing the member to form a space from which the member has been removed; and etching the substrate through the openings in the etching mask by reactive ion etching to form supply ports in the substrate. the substrate has an electric wiring layer for supplying electricity to the pressure generating element, the member and the electric wiring layer are formed of the same material, A method for manufacturing a liquid ejection head substrate, characterized in that the space is exposed to the opening, and in a process of forming a supply port in the substrate, the substrate is etched from the space, and an etched region of the substrate is formed below the space.
3. A method for manufacturing a liquid ejection head substrate having a substrate having a supply port, and on the substrate, a pressure generating element, a flow path forming member that forms a flow path for liquid, and an ejection port for ejecting liquid, comprising: providing a member on a substrate and an etching mask covering the member and having an opening; removing the member to form a space from which the member has been removed; and etching the substrate through the openings in the etching mask by reactive ion etching according to the Bosch process to form supply ports in the substrate. In the Bosch process, the time of the first etching step is 10% or more longer than the time of the other etching steps; A method for manufacturing a liquid ejection head substrate, characterized in that the space is exposed to the opening, and in a process of forming a supply port in the substrate, the substrate is etched from the space, and an etched region of the substrate is formed below the space.
4. The method for manufacturing a liquid ejection head substrate according to claim 1 , wherein the etching mask is made of a photosensitive resin.
5. 4. The method for manufacturing a liquid ejection head substrate according to claim 1, wherein the substrate is a single crystal silicon substrate.
6. 4. A method for manufacturing a liquid ejection head substrate according to claim 1, further comprising a step of developing the etching mask with a developer to form the opening, the member being removed by the developer to form a space where the member has been removed.
7. A method for manufacturing a liquid ejection head substrate as described in any one of claims 1 to 3, wherein the substrate has an electrical wiring layer that supplies electricity to the pressure generating element, an insulating layer is formed on the substrate, the electrical wiring layer is multi-layered, and the multi-layered electrical wiring layer is embedded in the insulating layer.
8. 8. The method for manufacturing a liquid ejection head substrate according to claim 7, wherein the surface of the substrate is present between the end of the insulating layer on the supply port side and the end of the region where the substrate is etched.
Citation Information
Patent Citations
Method of forming fine pattern
JP1986159731A
Liquid discharge head and manufacture thereof
JP1998095119A
Manufacturing method of substrate for liquid discharge head
JP2011016350A
Liquid droplet discharge head, ink cartridge, and image forming device
JP2013193411A
Method of processing silicon substrate
JP2017030258A