Resin composite and circuit board material using same
A resin composite using a cyclic polyolefin resin copolymer and glass cloth addresses thermal expansion issues in circuit boards, improving signal transmission efficiency and reliability by combining low dielectric loss and thermal expansion.
Patent Information
- Application Number
- JP2020124407
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-21
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2040-07-21
AI Technical Summary
Circuit board materials experience curling or warping due to large differences in linear thermal expansion coefficients between resin and metal layers, which is exacerbated by increasing communication frequencies leading to higher transmission losses.
A resin composite is formed using a cyclic polyolefin resin copolymer with specific properties and glass cloth, which includes a hydrogenated aromatic vinyl polymer block unit and hydrogenated conjugated diene polymer block unit, and optionally modified with unsaturated carboxylic acid, combined with glass cloth to achieve low dielectric properties and thermal expansion.
The resin composite achieves low dielectric loss and thermal expansion, reducing curling and warping, thereby enhancing signal transmission efficiency and reliability in circuit boards.
Smart Images

Figure 0007562321000001 
Figure 0007562321000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composite having excellent low dielectric properties and low thermal expansion coefficient, and a circuit board material using the same. [Background technology]
[0002] Generally, the main circuit board materials used in electrical and electronic devices are copper-clad laminates (CCL), which are made by layering resin-impregnated sheets (prepregs) on substrates such as paper or glass, and then applying pressure and heat to obtain an insulating plate on which copper foil is applied, and flexible printed circuit boards (FPC), which are made by forming an insulating adhesive layer on a base film and then laminating a conductor foil such as copper on top of that.
[0003] In recent years, communication frequencies have been increasing in order to increase the amount and speed of information transmission in electrical and electronic devices, and the increase in transmission loss (α) has become a major issue. The lower the value of this transmission loss (α), the less attenuation of the information signal, which means that high communication reliability can be ensured. Since transmission loss (α) is proportional to frequency (f), α becomes large in communications in the high frequency range, leading to reduced reliability. One method of suppressing transmission loss (α) is to reduce the dielectric tangent (tan δ), which is proportional to α, just like frequency (f). For high-speed transmission of communication signals, materials with low dielectric tangent (tan δ), i.e., materials with low dielectric properties, are required.
[0004] As a material having low dielectric properties, for example, Patent Document 1 describes a low dielectric resin composition and a laminate, and a metal-clad laminate, which contain a polyimide having a specific structure and a bisimide-based compound having a specific structure. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2001-006437 A Summary of the Invention [Problem to be solved by the invention]
[0006] Incidentally, when a circuit board material is produced by laminating a low dielectric resin and a metal layer as in Patent Document 1, if there is a large difference in the linear thermal expansion coefficient between the resin layer and the metal layer, curling or warping may occur after lamination. In recent years, as electric and electronic devices have become smaller and more multi-layered, there is a demand to reduce the linear thermal expansion coefficient of the resin layer to improve curling and warping of the laminate. SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to provide a resin composite having low dielectric properties and a low linear thermal expansion coefficient, and a circuit board material using the same. [Means for solving the problem]
[0007] Means of the Invention The present inventors have conducted extensive research to solve the above problems and have found that the above problems can be solved by using a specific cyclic polyolefin resin copolymer and glass cloth and forming a composite therebetween. That is, the present invention has the following features.
[0008] [1] A resin composite comprising a cyclic polyolefin resin copolymer having a crystalline melting peak temperature of less than 100°C and a glass cloth. [2] The resin composite according to [1], wherein the cyclic polyolefin resin copolymer has cyclohexane in a polyolefin side chain. [3] The resin composite according to [1] or [2], wherein the cyclic polyolefin resin copolymer is a resin copolymer containing at least one hydrogenated aromatic vinyl polymer block unit and at least one hydrogenated conjugated diene polymer block unit, or a modified product of this resin copolymer with an unsaturated carboxylic acid and / or an anhydride thereof. [4] The resin composite according to [3], wherein the cyclic polyolefin resin copolymer is a resin copolymer containing at least two of the hydrogenated aromatic vinyl polymer block units.
[0009] [5] The resin composite according to [3] or [4], wherein the cyclic polyolefin resin copolymer is a hydrogenated triblock copolymer or a hydrogenated pentablock copolymer of styrene and butadiene, or a modified product thereof with an unsaturated carboxylic acid and / or an anhydride thereof. [6] The resin composite according to any one of [1] to [5], wherein the resin composite contains the glass cloth in an amount of 1 vol % or more and 60 vol % or less based on 100 vol % of the resin composite. [7] The resin complex according to any one of [1] to [6], wherein the cyclic polyolefin resin copolymer has a dielectric loss tangent of less than 0.005 at 12 GHz.
[0010] [8] The resin composite according to any one of [1] to [7], wherein the glass cloth has a dielectric tangent of less than 0.005 at 10 GHz. [9] The resin composite according to any one of [1] to [8], which has a dielectric loss tangent at 12 GHz of less than 0.005.
[10] A circuit board material obtained by laminating the resin composite according to any one of [1] to [9] and a conductor. Effect of the Invention
[0011] According to the present invention, it is possible to obtain a resin composite having low dielectric properties and a low linear thermal expansion coefficient, and a circuit board material using the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will be described in detail below. However, the following description is an example of an embodiment of the present invention, and the present invention is not limited to the contents of the following description as long as it does not deviate from the gist of the present invention. In the following, when the expression "~" is used, it is used as an expression including the numerical values or physical properties before and after it.
[0013] <<Resin composite>> The resin composite of the present invention is a composite containing a cyclic polyolefin resin copolymer having a crystalline melting peak temperature of less than 100° C. and a glass cloth.
[0014] <Cyclic polyolefin resin copolymer> The term "cyclic" in the cyclic polyolefin resin copolymer of the present invention refers to the alicyclic structure of the cyclic polyolefin resin copolymer, specifically, the alicyclic structure in the side chain of the polyolefin. Suitable examples of the alicyclic structure include cycloalkanes, bicycloalkanes, polycyclic compounds, etc., among which cycloalkanes are preferred, and cyclohexane is more preferred. The alicyclic structure is more preferably an alicyclic structure formed by hydrogenation of an aromatic ring contained in a hydrogenated aromatic vinyl polymer block unit described below.
[0015] (Physical properties of cyclic polyolefin resin copolymer) The cyclic polyolefin resin copolymer of the present invention has a crystalline melting peak temperature of less than 100°C.
[0016] The crystalline melting peak temperature of the cyclic polyolefin resin copolymer is preferably 50° C. or higher, more preferably 60° C. or higher, and even more preferably 65° C. or higher. The crystalline melting peak temperature is preferably 90° C. or lower, and more preferably 85° C. or lower. The crystalline melting peak temperature in the present invention is the temperature at which a crystalline melting peak is detected in differential scanning calorimetry (DSC) measured at a heating rate of 10° C. / min.
[0017] The dielectric loss tangent of the cyclic polyolefin resin copolymer of the present invention is preferably less than 0.005 at 12 GHz, more preferably less than 0.001. The smaller the dielectric loss tangent, the smaller the dielectric loss, and therefore the more efficient and faster the electrical signal transmission can be obtained when used as a circuit board material, which is preferable. The lower limit of the dielectric loss tangent is not particularly limited, and may be 0 or more.
[0018] The melt flow rate (MFR) of the cyclic polyolefin resin copolymer of the present invention is not particularly limited, but is usually 0.1 g / 10 min or more, and from the viewpoint of the molding method and the appearance of the molded product, it is preferably 0.5 g / 10 min or more, and is usually 20.0 g / 10 min or less, and from the viewpoint of material strength, it is preferably 10.0 g / 10 min or less, more preferably 5.0 g / 10 min or less. The MFR is determined in accordance with ISO R1133, by measuring at a temperature of 230°C and a load of 2.16 kg.
[0019] <Cyclic polyolefin (A)> From the viewpoint of low dielectric properties, the cyclic polyolefin resin copolymer of the present invention is preferably a cyclic polyolefin resin copolymer containing at least one type of hydrogenated aromatic vinyl polymer block unit and at least one type of hydrogenated conjugated diene polymer block unit (hereinafter also referred to as "cyclic polyolefin (A)"), or a modified product of the cyclic polyolefin (A) with an unsaturated carboxylic acid and / or anhydride thereof (hereinafter also referred to as "modified cyclic polyolefin (B)").
[0020] For purposes of this invention, "block" refers to a polymeric segment of a copolymer that exhibits microphase separation from structurally or compositionally distinct polymeric segments of the copolymer. Microphase separation occurs due to the immiscibility of the polymeric segments in the block copolymer. Microphase separation and block copolymers are extensively discussed in "Block Copolymers - Designer Soft Materials" in the February 1999 issue of PHYSICS TODAY, pp. 32-38.
[0021] Examples of the cyclic polyolefin (A) include a diblock copolymer consisting of a hydrogenated aromatic vinyl polymer block unit (hereinafter also referred to as "block A") and a hydrogenated conjugated diene polymer block unit (hereinafter also referred to as "block B"), a triblock copolymer containing two or more of at least one of block A and block B, a tetrablock copolymer, and a pentablock copolymer. The cyclic polyolefin (A) preferably contains at least two blocks A, and suitable examples thereof include an ABA type, an ABAB type, and an ABABA type.
[0022] In addition, the cyclic polyolefin (A) preferably contains a segment made of an aromatic vinyl polymer at each end. Therefore, the hydrogenated block copolymer of the present invention preferably has at least two hydrogenated aromatic vinyl polymer block units (blocks A) and has at least one hydrogenated conjugated diene polymer block unit (block B) between the two hydrogenated aromatic vinyl polymer block units (blocks A). From these viewpoints, the cyclic polyolefin (A) is more preferably an ABA type or an ABABA type.
[0023] The content of the hydrogenated aromatic vinyl polymer block unit (block A) in the cyclic polyolefin (A) is preferably 30 to 99 mol %, more preferably 40 to 90 mol %, still more preferably 50 mol % or more, and even more preferably 60 mol % or more. If the ratio of the hydrogenated aromatic vinyl polymer block unit (block A) is equal to or higher than the lower limit, the rigidity is not decreased and the heat resistance and the linear thermal expansion coefficient are also good. On the other hand, if the ratio is equal to or lower than the upper limit, the brittleness is not deteriorated.
[0024] The content of the hydrogenated conjugated diene polymer block unit (block B) in the cyclic polyolefin (A) is preferably 1 to 70 mol %, more preferably 10 to 60 mol %, still more preferably 50 mol % or less, and even more preferably 40 mol % or less. If the ratio of the hydrogenated conjugated diene polymer block unit (block B) is equal to or higher than the lower limit, the brittleness does not deteriorate, whereas if it is equal to or lower than the upper limit, the rigidity does not decrease, and the heat resistance and the linear thermal expansion coefficient are also good.
[0025] The hydrogenated aromatic vinyl polymer block unit and the hydrogenated conjugated diene polymer block unit constituting the cyclic polyolefin (A) can be obtained by hydrogenating a polymer block composed of an aromatic vinyl monomer and a conjugated diene monomer such as 1,3-butadiene, which will be described in detail later. Moreover, the cyclic polyolefin (A) is preferably a block copolymer having no functional groups. The term "no functional groups" means that the block copolymer does not have any functional groups, i.e., groups containing atoms other than carbon and hydrogen atoms.
[0026] The monomers for forming the aromatic vinyl polymer block unit and the conjugated diene polymer block unit before hydrogenation will be described below.
[0027] (Aromatic vinyl monomer) The aromatic vinyl monomer serving as a raw material for the aromatic vinyl polymer block unit before hydrogenation is a monomer represented by the general formula (1).
[0028] [ka]
[0029] In the above general formula (1), R is hydrogen or an alkyl group, and Ar is a phenyl group, a halophenyl group, an alkylphenyl group, an alkylhalophenyl group, a naphthyl group, a pyridinyl group, or an anthracenyl group.
[0030] When R is an alkyl group, the number of carbon atoms is preferably 1 to 6, and the alkyl group may be mono- or polysubstituted with functional groups such as a halo group, a nitro group, an amino group, a hydroxyl group, a cyano group, a carbonyl group, and a carboxyl group. Moreover, the Ar is preferably a phenyl group or an alkylphenyl group, and more preferably a phenyl group.
[0031] Examples of aromatic vinyl monomers include styrene, α-methylstyrene, vinyltoluene (including all isomers, with p-vinyltoluene being particularly preferred), ethylstyrene, propylstyrene, butylstyrene, vinylbiphenyl, vinylnaphthalene, vinylanthracene (including all isomers), and mixtures thereof. Of these, styrene is preferred.
[0032] (Conjugated Diene Monomer) The conjugated diene monomer serving as the raw material of the conjugated diene polymer block unit before hydrogenation is not particularly limited as long as it is a monomer having two conjugated double bonds. Examples of conjugated diene monomers include 1,3-butadiene, 2-methyl-1,3-butadiene (isoprene), 2-methyl-1,3-pentadiene and similar compounds, and mixtures thereof. Of these, 1,3-butadiene is preferred.
[0033] When 1,3-butadiene is used as the conjugated diene monomer, its polymer, polybutadiene, contains 1,4-bond units ([-CH 2 -CH=CH-CH 2 -]) and 1,2-bond units ([-CH 2 -CH(CH=CH 2 )-]), the former gives a structure similar to the repeating unit of polyethylene (ethylene structure) upon hydrogenation, and the latter gives a structure similar to the repeating unit obtained by polymerization of 1-butene (1-butene structure). Therefore, the hydrogenated conjugated diene polymer block unit according to the present invention preferably contains at least one of an ethylene structure and a 1-butene structure. In addition, when isoprene is used as the conjugated diene monomer, its polymer, polyisoprene, contains 1,4-bond units ([-CH 2 -C(CH 3 )=CH-CH 2 -]), 3,4-bond units ([-CH 2 -CH(C(CH 3 )=CH 2 )-]) and 1,2-bond units ([-CH 2-C(CH 3 )(CH=CH 2 )-]) is present, and contains at least one of the three types of repeating units obtained by hydrogenation.
[0034] (Block structure) The cyclic polyolefin (A) is preferably produced by hydrogenation of a multiblock copolymer such as a triblock copolymer, a tetrablock copolymer, a pentablock copolymer, etc., such as SBS, SBSB, SBSBS, SBSBSB, SIS, SISIS, and SISBS (where S is polystyrene, B is polybutadiene, and I is polyisoprene). The block may be a linear block or may be branched. When branched, the polymerization chain may be bonded at any position along the backbone of the copolymer. In addition to a linear block, the block may be a tapered block or a star block.
[0035] The block copolymer constituting the cyclic polyolefin (A) before hydrogenation may contain one or more additional block units other than the aromatic vinyl polymer block units and the conjugated diene polymer block units. For example, in the case of a triblock copolymer, these additional block units may be bonded to any position of the triblock polymer skeleton.
[0036] A preferred example of the hydrogenated aromatic vinyl polymer block unit is hydrogenated polystyrene, and a preferred example of the hydrogenated conjugated diene polymer block unit is hydrogenated polybutadiene or hydrogenated polyisoprene, with hydrogenated polybutadiene being more preferred. A preferred embodiment of the cyclic polyolefin (A) is a hydrogenated triblock or pentablock copolymer of styrene and butadiene, and it is preferred that the cyclic polyolefin (A) does not contain any other functional group or structural modifier.
[0037] (Hydrogenation level) The cyclic polyolefin (A) is a polyolefin in which the aromatic rings derived from styrene and the like as well as the double bonds derived from conjugated dienes such as butadiene are hydrogenated, and the polyolefin is substantially completely hydrogenated. Specifically, the polyolefin has the following hydrogenation levels: That is, the hydrogenation level of the cyclic polyolefin (A) is preferably 90% or more for hydrogenated aromatic vinyl polymer block units and 95% or more for hydrogenated conjugated diene polymer block units; more preferably 95% or more for hydrogenated aromatic vinyl polymer block units and 99% or more for hydrogenated conjugated diene polymer block units; even more preferably 98% or more for hydrogenated aromatic vinyl polymer block units and 99.5% or more for hydrogenated conjugated diene polymer block units; and particularly preferably 99.5% or more for hydrogenated aromatic vinyl polymer block units and 99.5% or more for hydrogenated conjugated diene polymer block units. Such high levels of hydrogenation can reduce dielectric losses. The hydrogenation level of the hydrogenated aromatic vinyl polymer block unit refers to the proportion of the aromatic vinyl polymer block unit that is saturated by hydrogenation, and the hydrogenation level of the hydrogenated conjugated diene polymer block unit refers to the proportion of the conjugated diene polymer block unit that is saturated by hydrogenation. The hydrogenation level of each block unit is determined using proton NMR.
[0038] The cyclic polyolefin (A) may be used alone or in combination of two or more kinds. As the cyclic polyolefin (A) of the present invention, commercially available products can be used, specifically, TEFABLOC (registered trademark) manufactured by Mitsubishi Chemical Corporation can be mentioned.
[0039] <Modified cyclic polyolefin (B)> The cyclic polyolefin resin copolymer of the present invention may be a modified cyclic polyolefin (B). The modified cyclic polyolefin (B) is a product of the above-mentioned cyclic polyolefin (A) modified with an unsaturated carboxylic acid and / or anhydride thereof. By modifying the cyclic polyolefin (A), the polarity of the polymer increases, which is expected to improve adhesion to metal layers such as copper foil.
[0040] (Modification of cyclic polyolefin (A)) The modification of the cyclic polyolefin (A) is described below. This modification is preferably carried out by adding an unsaturated carboxylic acid and / or anhydride thereof as a modifier to the cyclic polyolefin (A) and reacting the mixture.
[0041] [Denaturant] Examples of the unsaturated carboxylic acid and / or anhydride thereof as the modifying agent include unsaturated carboxylic acids such as acrylic acid, methacrylic acid, α-ethylacrylic acid, maleic acid, fumaric acid, tetrahydrophthalic acid, methyltetrahydrophthalic acid, itaconic acid, citraconic acid, crotonic acid, isocrotonic acid, and nadic acids, and their anhydrides. Specific examples of the acid anhydride include maleic anhydride, citraconic anhydride, and nadic anhydrides. Examples of nadic acids or their anhydrides include endo-cis-bicyclo[2.2.1]hept-2,3-dicarboxylic acid (nadic acid), methyl-endo-cis-bicyclo[2.2.1]hept-5-ene-2,3-dicarboxylic acid (methylnadic acid), and the like, and their anhydrides.
[0042] Among these unsaturated carboxylic acids and / or their anhydrides, acrylic acid, maleic acid, nadic acid, maleic anhydride, and nadic acid anhydride are preferred. The unsaturated carboxylic acid and / or anhydride thereof may be used alone or in combination of two or more kinds.
[0043] [Denaturation method] The cyclic polyolefin (A) can be modified with the unsaturated carboxylic acid and / or its anhydride to obtain the modified cyclic polyolefin (B). As the modification method, solution modification, melt modification, solid-phase modification by irradiation with an electron beam or ionizing radiation, modification in a supercritical fluid, etc. are preferably used. Among these, melt modification is preferred because of its excellent equipment and cost competitiveness, and melt kneading modification using an extruder because of its excellent continuous productivity is more preferred. Examples of the apparatus used at this time include a single screw extruder, a twin screw extruder, a Banbury mixer, and a roll mixer. Among these, a single screw extruder and a twin screw extruder, which are excellent in continuous productivity, are preferred.
[0044] In general, modification of the cyclic polyolefin (A) with an unsaturated carboxylic acid and / or anhydride thereof is carried out by a graft reaction in which a carbon-hydrogen bond of a hydrogenated conjugated diene polymer block unit, which is one of the block units constituting the cyclic polyolefin (A), is cleaved to generate a carbon radical, to which an unsaturated functional group is added. As a source of carbon radical generation, in addition to the above-mentioned electron beam and ionizing radiation, a method using high temperature and radical generators such as organic peroxides, inorganic peroxides, azo compounds, etc. are also usable. As the radical generator, it is preferable to use an organic peroxide from the viewpoint of cost and operability.
[0045] Examples of the azo compound include azobisisobutyronitrile, azobisdimethylvaleronitrile, azobis(2-methylbutyronitrile), and diazonitrophenol. Examples of the inorganic peroxides include hydrogen peroxide, potassium peroxide, sodium peroxide, calcium peroxide, magnesium peroxide, and barium peroxide.
[0046] The organic peroxides include those belonging to the groups of hydroperoxides, dialkyl peroxides, diacyl peroxides, peroxy esters, and ketone peroxides. Specific examples of the peroxides include hydroperoxides such as cumene hydroperoxide and t-butyl hydroperoxide; dialkyl peroxides such as dicumyl peroxide, di-t-butyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane and 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3; diacyl peroxides such as lauryl peroxide and benzoyl peroxide; peroxy esters such as t-butyl peroxyacetate, t-butyl peroxybenzoate and t-butylperoxyisopropyl carbonate; and ketone peroxides such as cyclohexanone peroxide. These radical generators may be used alone or in combination of two or more kinds.
[0047] [Melt kneading modification] A commonly used melt-kneading modification operation involves blending a cyclic polyolefin (A), an unsaturated carboxylic acid and / or its anhydride, and an organic peroxide, feeding the mixture into a kneader and extruder, extruding the mixture while heating, melt-kneading, and cooling the molten resin emerging from the tip of a die in a water tank or the like to obtain a modified cyclic polyolefin (B).
[0048] The blending ratio of the cyclic polyolefin (A) and the unsaturated carboxylic acid and / or anhydride thereof is 0.2 to 5 parts by mass of the unsaturated carboxylic acid and / or anhydride thereof per 100 parts by mass of the cyclic polyolefin (A). When the blending ratio of the unsaturated carboxylic acid and / or its anhydride to the cyclic polyolefin (A) is equal to or higher than the lower limit, a required modification rate for achieving the effects of the present invention can be obtained. When the blending ratio is equal to or lower than the upper limit, no unreacted unsaturated carboxylic acid and / or its anhydride remain, which is also favorable in terms of dielectric properties.
[0049] The blending ratio of the unsaturated carboxylic acid and / or its anhydride to the organic peroxide is 20 to 100 parts by mass of the organic peroxide per 100 parts by mass of the unsaturated carboxylic acid and / or its anhydride. When the blending ratio of the organic peroxide to the unsaturated carboxylic acid and / or its anhydride is not less than the lower limit, a desired modification rate required to achieve the effects of the present invention can be obtained, while when the blending ratio is not more than the upper limit, the cyclic polyolefin (A) does not deteriorate and the color does not deteriorate.
[0050] As for the melt kneading modification conditions, for example, extrusion at a temperature of 150 to 300° C. is preferred in a single screw extruder or a twin screw extruder.
[0051] [Degeneration rate] The degree of modification of the modified cyclic polyolefin (B) with the unsaturated carboxylic acid and / or anhydride thereof is preferably from 0.1 to 2% by mass. If the modification rate is equal to or higher than the lower limit, the polarity of the polymer increases, and the adhesion to a metal layer such as a copper foil is improved, which is preferable. If the modification rate is equal to or lower than the upper limit, the dielectric loss of the cyclic polyolefin (A) can be prevented from increasing. In addition, odor generation and color deterioration can be prevented. The modification rate of the modified cyclic polyolefin (B) can be measured by proton NMR after the modified cyclic polyolefin (B) is subjected to a methyl esterification treatment.
[0052] <Glass cloth> The resin composite of the present invention contains a glass cloth. As a method for suppressing the linear thermal expansion coefficient of a resin, there is generally a method of filling an inorganic filler having a low linear thermal expansion coefficient. However, the effect cannot be expected unless a large amount of inorganic filler is filled, and in the case of a thermoplastic resin, filling a large amount of inorganic filler is not preferable because it makes melt kneading and extrusion molding difficult. Another method for suppressing the linear thermal expansion coefficient of a resin is to impregnate glass fibers, but there is a problem that anisotropy is easily generated. Therefore, by using glass cloth as in the present invention, the effect of suppressing the linear thermal expansion coefficient isotropically can be expected. Furthermore, the advantage that the content of glass cloth in the resin composite can be easily adjusted can be expected.
[0053] The content of the glass cloth is preferably 1% by volume or more, more preferably 3% by volume or more, and even more preferably 4% by volume or more, based on 100% by volume of the resin composite. Also, it is preferably 60% by volume or less, more preferably 40% by volume or less, and even more preferably 20% by volume or less. By making the content of the glass cloth equal to or more than a predetermined lower limit, it is expected that the linear thermal expansion coefficient of the resin composite can be reduced, and by making the content equal to or less than a predetermined upper limit, the light weight and bendability of the resin composite can be maintained.
[0054] The dielectric loss tangent of the glass cloth is preferably less than 0.005 at 10 GHz, more preferably less than 0.0005. The smaller the dielectric loss tangent, the smaller the dielectric loss, and therefore the more efficient and faster the electrical signal transmission can be obtained when the glass cloth is used as a circuit board material. The lower limit of the dielectric loss tangent is not particularly limited, and it is sufficient if it is 0 or more.
[0055] The average linear thermal expansion coefficient of the glass cloth is preferably less than 5 ppm / ° C., and more preferably less than 3 ppm / ° C., in the temperature range of 0° C. to 100° C. When the linear thermal expansion coefficient of the glass cloth is equal to or less than the above upper limit, the linear thermal expansion coefficient of the resin composite can be reduced.
[0056] The thickness of the glass cloth is preferably 10 μm or more and 200 μm or less. By having the thickness within the above range, the glass cloth has flexibility to bend easily, so it is expected that the linear thermal expansion coefficient can be suppressed while maintaining the flexibility of the resin. Furthermore, it is suitable as a circuit board material that can accommodate the miniaturization of electric and electronic devices.
[0057] The glass cloth used in the present invention may be surface-treated with a silane compound, such as vinyltriethoxysilane, 2-aminopropyltriethoxysilane, or 2-glycidoxypropyltrimethoxysilane, in order to improve its affinity with the resin and prevent peeling.
[0058] Specific examples of the glass cloth used in the present invention include NE glass manufactured by Nitto Boseki Co., Ltd. and quartz glass "SQX series" manufactured by Shin-Etsu Chemical Co., Ltd.
[0059] <Other ingredients> The resin composite of the present invention may contain, as necessary, flame retardants, heat stabilizers, weather stabilizers, antistatic agents, slip agents, antiblocking agents, antifogging agents, lubricants, dyes, pigments, natural oils, synthetic oils, waxes, organic fillers, inorganic fillers, thermoplastic resins and thermosetting resins other than the cyclic polyolefin resin copolymer, and the like, to the extent that the object of the present invention is not impaired, and the blending ratios of the additives are appropriate. Specific examples of stabilizers that may be added as optional components include phenolic antioxidants such as tetrakis[methylene-3(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane, beta-(3,5-di-t-butyl-4-hydroxyphenyl)propionic acid alkyl esters, and 2,2'-oxamidobis[ethyl-3(3,5-di-t-butyl-4-hydroxyphenyl)]propionate; fatty acid metal salts such as zinc stearate, calcium stearate, and calcium 12-hydroxystearate; and polyhydric alcohol fatty acid esters such as glycerin monostearate, glycerin monolaurate, glycerin distearate, and pentaerythritol tristearate. These may be added alone or in combination, and examples include combinations of tetrakis[methylene-3(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane with stearate sulfite and glycerin monostearate.
[0060] <Composition of resin composite> The resin composite of the present invention only needs to have the above-mentioned cyclic polyolefin resin copolymer and the above-mentioned glass cloth, and these may be integrated or separate. That is, for example, a configuration may be used in which a glass cloth is impregnated with a cyclic polyolefin resin copolymer, and the cyclic polyolefin resin copolymer and the glass cloth are integrated together, or a configuration may be used in which a resin layer made of a cyclic polyolefin resin copolymer is laminated on one or both surfaces of the glass cloth. Among these, from the viewpoint of low dielectric properties and low linear thermal expansion coefficient, a configuration in which the glass cloth is impregnated with the cyclic polyolefin resin copolymer and the cyclic polyolefin resin copolymer and the glass cloth are integrated is preferred.
[0061] <Characteristics of resin composite> The dielectric loss tangent of the resin composite of the present invention is preferably less than 0.005 at 12 GHz, more preferably less than 0.002. The smaller the dielectric loss tangent, the smaller the dielectric loss, and therefore the more efficient and faster the electrical signal transmission can be obtained when used as a circuit board material, which is preferable. The lower limit of the dielectric loss tangent is not particularly limited, and may be 0 or more.
[0062] The average linear thermal expansion coefficient of the resin composite is preferably less than 80 ppm / ° C., and more preferably less than 65 ppm / ° C., in the temperature range of 0° C. to 100° C. When the linear thermal expansion coefficient of the resin composite is equal to or less than the above upper limit, the difference with the linear thermal expansion coefficient of a metal layer such as a copper foil can be reduced, thereby suppressing curling or warping when laminated with a metal layer.
[0063] The thickness of the resin complex is preferably from 10 μm to 200 μm. By keeping the thickness within the above range, it is possible to obtain a circuit board material that can accommodate the miniaturization of electric and electronic devices while maintaining an appropriate level of strength.
[0064] <<Manufacturing method for resin composite>> A method for producing a resin composite of the present invention will be described below. However, the following description is one example of a method for producing a resin composite of the present invention, and the resin composite of the present invention is not limited to resin composites produced by the method described below.
[0065] <First manufacturing method> The first method for producing a resin composite of the present invention includes the following steps (1) and (2). (1) A film-forming process for obtaining a resin sheet from a cyclic polyolefin resin copolymer. (2) A lamination step in which a resin sheet and a glass cloth are laminated to obtain a resin composite.
[0066] (1. Film forming process) In the film-forming step, the cyclic polyolefin resin copolymer is formed into a sheet to obtain a resin sheet. The film-forming method is not particularly limited and may be a known method, for example, a method in which a cyclic polyolefin resin copolymer is melt-extruded from a T-die and cast-molded with a cast roll (chill roll, cast drum, etc.). In addition, when various additives other than the cyclic polyolefin resin copolymer are used, the cyclic polyolefin resin copolymer and various additives may be kneaded in a kneading device before film formation. The kneading method and kneading device used are not particularly limited, and known extruders such as single-screw extruders, twin-screw extruders, and multi-screw extruders can be used.
[0067] (2.Lamination process) In the lamination step, the resin sheet obtained in the film-forming step and a glass cloth are laminated to obtain a resin composite. The lamination method is not particularly limited and may be a known method, for example, a method in which a resin sheet and a glass cloth are bonded together with an adhesive.
[0068] In addition, after the resin sheet and the glass cloth are laminated together, a press impregnation step may be carried out in which the glass cloth is impregnated with the cyclic polyolefin resin copolymer by hot pressing. When hot pressing is performed, the pressing method and pressing temperature are not particularly limited, but for example, a method can be mentioned in which a resin sheet and a glass cloth are overlapped and sandwiched between two flat plates, and hot pressed at a temperature equal to or higher than the flow temperature of the resin for 0.5 to 10 minutes at a pressure of 0.1 to 1 MPa, cooled to room temperature, and then the pressure is released to obtain a laminate. In this case, the resin sheet may be overlapped on one side of the glass cloth, or the resin sheets may be overlapped on both sides of the glass cloth.
[0069] <Second manufacturing method> The second method for producing a resin composite of the present invention includes a direct coating step of directly coating a cyclic polyolefin resin copolymer onto a glass cloth. The glass cloth may be impregnated with the cyclic polyolefin resin copolymer by the direct coating. The method for applying the cyclic polyolefin resin copolymer is not particularly limited, and examples thereof include a comma coating method, a reverse coating method, a knife coating method, a dip coating method, a dip-nip method, a kiss coating method, an air knife coating method, a spin coating method, a roll coating method, a printing method, a dip method, a slide coating method, a curtain coating method, a die coating method, a casting method, and an extrusion coating method.
[0070] <<Applications of resin composites>> Examples of applications of the resin composite of the present invention include, but are not limited to, copper foil laminates, flexible printed circuit boards, multilayer printed wiring boards, circuit board materials for electric and electronic devices such as capacitors, underfill materials, interchip fills for 3D-LSI, insulating sheets, and heat dissipation substrates.
[0071] <Circuit board materials> The resin composite of the present invention can be used as a circuit board material by laminating it with a conductor.
[0072] The conductor may be a metal foil made of a conductive metal such as copper or aluminum, or an alloy containing such a metal, or a metal layer formed by plating or sputtering.
[0073] When used as a circuit board material for electric and electronic devices, the thickness of the resin composite is preferably 10 μm or more and 200 μm or less, and the thickness of the conductor is preferably 0.2 μm or more and 70 μm or less.
[0074] The circuit board material of the present invention is characterized by having a sufficiently low dielectric tangent. The dielectric loss tangent of the circuit board material is preferably less than 0.01 at 12 GHz, and more preferably less than 0.008. The lower the dielectric loss tangent, the more efficient and faster the electrical signal transmission can be when the circuit board is used. There is no particular lower limit for the dielectric loss tangent, and it is sufficient if it is 0 or more.
[0075] <Method of manufacturing circuit board materials> The circuit board material of the present invention can be produced, for example, by the following method. After laminating a conductor on the resin composite of the present invention, a circuit is formed using a photoresist or the like, and the required number of such layers are laminated. The lamination of the resin composite and the conductor may be performed by directly laminating a conductive metal foil on the resin composite, by bonding the resin composite and the conductive metal foil with an adhesive, by forming a conductive metal layer by plating or sputtering, or by a combination of these methods. EXAMPLES
[0076] The present invention will be described in more detail below using examples, but the present invention is not limited to the following examples as long as it does not exceed the gist of the invention. The values of various production conditions and evaluation results in the following examples are meant as preferred upper or lower limit values in the embodiment of the present invention, and the preferred range may be a range defined by a combination of the above-mentioned upper or lower limit values and the values of the following examples or values of the examples. In the following description, "parts" refers to "parts by mass".
[0077] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the following examples and comparative examples, various physical properties were measured by the following methods.
[0078] <Measurement method> (1) Dielectric tangent The dielectric loss tangent of the resin composite in the in-plane direction at 12 GHz was measured using a cavity resonator method and evaluated according to the following criteria. [Evaluation Criteria] A (good): Dielectric tangent less than 0.005 B (poor): Dielectric tangent is 0.005 or more
[0079] (2) Linear thermal expansion coefficient A test piece measuring 3 mm in width and 10 mm in length was cut out from the resin composite, and the linear thermal expansion coefficient of the test piece was measured in accordance with JIS K7197 using TMA / SS7100 manufactured by Hitachi High-Tech Science Corporation, and evaluated according to the following criteria. [evaluation] A (good): Average linear thermal expansion coefficient from 0°C to 100°C is less than 65 ppm / °C B (poor): Average linear thermal expansion coefficient from 0°C to 100°C is 65 ppm / °C or more
[0080] <Raw materials> [Cyclic polyolefin resin copolymer] A-1: As the modified cyclic polyolefin (B), "TEFABLOCK (registered trademark) CP MC940AP" manufactured by Mitsubishi Chemical Corporation was used. Crystal melting peak temperature: 75℃ - Dielectric tangent: 0.0009 (12GHz) ·Density (ASTM D792): 0.94g / cm 3 ·MFR (230℃, 2.16kg): 3g / 10 minutes Hydrogenated aromatic vinyl polymer block unit: Hydrogenated polystyrene with a content of 67 mol% and a hydrogenation level of 99.5% or more Hydrogenated conjugated diene polymer block unit: Hydrogenated polybutadiene with a content of 33 mol% and a hydrogenation level of 99.5% or more Block structure: Pentablock structure, Total hydrogenation level: 99.5% or more Maleic acid modification rate: 1.2% by mass Mw:68000
[0081] [Glass cloth] B-1: Quartz glass (Shin-Etsu Chemical Co., Ltd., thickness: 50 μm, dielectric loss tangent: 0.0001 (10 GHz), linear thermal expansion coefficient: 0.5 ppm / ℃)
[0082] <Example 1> The cyclic polyolefin resin copolymer A-1 was melt-kneaded using an extruder to produce a resin sheet A-1 having a thickness of 100 μm. The resin sheet A-1 and the glass cloth B-1 were each cut into 10 cm squares, and two sheets of the resin sheet A-1 were laminated on each side of the glass cloth so as to obtain the volume ratio shown in Table 1. The laminate was sandwiched between two smooth metal plates and hot-pressed at 200° C. for 60 seconds at a pressure of 20 MPa to obtain a resin composite. The dielectric loss tangent and linear thermal expansion coefficient of the obtained resin composite were evaluated. The results are shown in Table 1.
[0083] <Examples 2 to 3> A resin composite was prepared in the same manner as in Example 1, except that the volume ratio of the cyclic polyolefin resin copolymer A-1 and the glass cloth B-1 was adjusted as shown in Table 1. The dielectric loss tangent and linear thermal expansion coefficient of the obtained resin composite were evaluated. The results are shown in Table 1.
[0084] <Comparative Example 1> The resin sheet A-1 was evaluated for dielectric tangent and linear thermal expansion coefficient. The results are shown in Table 1.
[0085] [Table 1]
[0086] The results of Examples 1 to 3 in Table 1 above show that by combining a specific cyclic polyolefin resin with glass cloth to prepare a composite, it is possible to reduce the linear thermal expansion coefficient while maintaining a low dielectric tangent. When such a resin composite is used as a circuit board material, for example, it is possible to reduce the dielectric loss and suppress curling and warping of the board caused by the difference in the thermal expansion coefficient with the metal layer.
[0087] On the other hand, in the case of Comparative Example 1, a sheet of a single cyclic polyolefin resin not compounded with glass cloth had an excellent dielectric loss tangent but a large linear thermal expansion coefficient.
Claims
1. The present invention comprises a cyclic polyolefin resin copolymer having a crystal melting peak temperature of less than 100° C. and a glass cloth, A resin composite having a dielectric loss tangent at 12 GHz of less than 0.
002.
2. The resin composite according to claim 1 , wherein the cyclic polyolefin resin copolymer has cyclohexane in a polyolefin side chain.
3. The resin composite according to claim 1 or 2, wherein the cyclic polyolefin resin copolymer is a resin copolymer containing at least one hydrogenated aromatic vinyl polymer block unit and at least one hydrogenated conjugated diene polymer block unit, or a modified product of the resin copolymer with an unsaturated carboxylic acid and / or an anhydride thereof.
4. The resin composite according to claim 3 , wherein the cyclic polyolefin resin copolymer is a resin copolymer containing at least two of the hydrogenated aromatic vinyl polymer block units.
5. The resin composite according to claim 3 or 4, wherein the cyclic polyolefin resin copolymer is a hydrogenated triblock copolymer or a hydrogenated pentablock copolymer of styrene and butadiene, or a modified product thereof with an unsaturated carboxylic acid and / or an anhydride thereof.
6. The resin composite according to any one of claims 1 to 5, wherein the glass cloth is contained in an amount of 1 volume % or more and 60 volume % or less based on 100 volume % of the resin composite.
7. The resin composite according to any one of claims 1 to 6, wherein the cyclic polyolefin resin copolymer has a dielectric loss tangent of less than 0.005 at 12 GHz.
8. The resin composite according to any one of claims 1 to 7, wherein the glass cloth has a dielectric loss tangent of less than 0.005 at 10 GHz.
9. A circuit board material obtained by laminating the resin composite according to any one of claims 1 to 8 and a conductor.
Citation Information
Patent Citations
Low dielectric resin composition and circuit laminated board
JP2001006437A
Terminal-modified vinyl alicyclic hydrocarbon polymer and manufacturing method of the same
JP2005239851A
Fiber woven fabric-reinforcing material using modified cyclic olefin copolymer and resin substrate for printed circuit board
JP2006307405A
Insulating material for electronic component
JP2011001473A
Crystalline cyclic olefin resin film, laminate film and method for producing the same
JP2014105291A