Solar cell and its manufacturing method, photovoltaic module
The solar cell design optimizes polysilicon doped layers with barrier layers to balance light absorption and metallization, enhancing efficiency by reducing thickness, parasitic absorption, and preventing burn-through, thus improving open-circuit voltage and short-circuit current.
Patent Information
- Application Number
- JP2023169004
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-02-02
- Filing Date
- 2023-09-29
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2043-09-29
AI Technical Summary
Existing solar cell technologies face challenges in balancing light absorption and metallization in thin polysilicon layers, which can lead to issues such as short-circuit current loss, increased production costs, and risks of silver particle burn-through in tunnel oxide layers.
A solar cell design featuring a silicon substrate with a tunnel oxide layer and multiple polysilicon doped layers separated by barrier layers, where the doping concentrations and thicknesses are optimized to reduce parasitic absorption and prevent burn-through, while maintaining effective electron transport.
The solution enhances the photoelectric conversion efficiency by reducing polysilicon layer thickness, increasing short-circuit current, and preventing metal recombination, thereby improving open-circuit voltage and overall battery performance.
Smart Images

Figure 0007562796000001 
Figure 0007562796000002 
Figure 0007562796000003
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of photovoltaics, and more particularly to solar cells and their manufacturing methods, and photovoltaic modules. [Background technology]
[0002] TOPcon (Tunnel Oxide Passivated Contact) cells are manufactured using tube LPCVD (Low Pressure Chemical Vapor Deposition) or PECVD (Plasma Enhanced Chemical Vapor Deposition) equipment. The tunnel oxide layer and the polysilicon doping layer together form a passivation contact structure. This tunnel oxide passivation contact structure allows majority carriers to pass through the oxide layer and blocks minority carriers, effectively realizing carrier selectivity, greatly reducing the recombination rate of minority carriers and improving cell efficiency.
[0003] In TOPCon cells, a polysilicon doping layer of about 30 nm can generally be used to achieve good passivation effect, but due to the limitations of current paste and sintering technology, the polysilicon doping layer should be about 110-120 nm to effectively reduce the risk of silver particles burning through the tunnel oxide layer. And because the polysilicon doping layer itself has strong near-infrared light absorption ability, a thick polysilicon layer not only causes short-circuit current loss, but also affects the performance of the battery and increases production costs. For these reasons, the problem of balancing the light absorption and metallization of thin polysilicon cannot be solved.
[0004] Therefore, there is a need to provide a solar cell and method for fabricating the same, and a photovoltaic module that comprehensively solves the problem of balancing light absorption and metallization of thin polysilicon. Summary of the Invention [Means for solving the problem]
[0005] In view of the above, the present invention provides a solar cell including a silicon substrate, a first electrode, and a second electrode, a tunnel oxide layer is provided on one surface of the silicon substrate along a direction away from the silicon substrate, at least two polysilicon doped layers are provided on the side of the tunnel oxide layer away from the silicon substrate, a barrier layer is provided between adjacent polysilicon doped layers, and a plurality of the first electrodes are electrically connected to different polysilicon doped layers.
[0006] Optionally, the doping concentration of phosphorus in the polysilicon doped layer closer to the silicon substrate is less than the doping concentration of phosphorus in the polysilicon doped layer further from the silicon substrate.
[0007] Optionally, the at least two polysilicon doped layers include a first polysilicon doped layer, a second polysilicon doped layer, and a third polysilicon doped layer, with a first barrier layer between the first polysilicon doped layer and the second polysilicon doped layer, and a second barrier layer between the second polysilicon doped layer and the third polysilicon doped layer, where the first polysilicon doped layer is located closer to the tunnel oxide layer, and the third polysilicon doped layer is located farther from the tunnel oxide layer; The first polysilicon doped layer is doped with phosphorus, and the second polysilicon doped layer and the third polysilicon doped layer are doped with phosphorus and carbon or nitrogen, respectively.
[0008] Optionally, the first electrode includes a first sub-electrode and a second sub-electrode, the first sub-electrode being electrically connected to the third polysilicon doped layer, and the second sub-electrode being electrically connected to the first polysilicon doped layer and / or the second polysilicon doped layer.
[0009] Optionally, the doping concentration of phosphorus in the first polysilicon doped layer is less than the doping concentration of phosphorus in the second polysilicon doped layer, and the doping concentration of phosphorus in the second polysilicon doped layer is less than the doping concentration of phosphorus in the third polysilicon doped layer.
[0010] Optionally, the doping ratio of carbon and nitrogen in the second polysilicon doped layer and the third polysilicon doped layer is less than 5 wt %.
[0011] Optionally, the ratio of the doping concentration of phosphorus in the first polysilicon doped layer to the third polysilicon doped layer is 0.4-1.
[0012] Optionally, the total thickness of the first polysilicon doped layer, the second polysilicon doped layer and the third polysilicon doped layer along a direction perpendicular to the silicon substrate does not exceed 70 nm.
[0013] Optionally, the thickness of the first polysilicon doped layer, the second polysilicon doped layer and / or the third polysilicon doped layer along a direction perpendicular to the silicon substrate ranges from 5 nm to 40 nm.
[0014] Optionally, along a direction perpendicular to the silicon substrate, the first barrier layer and the second barrier layer each have a thickness in the range of 0.5 nm to 2.5 nm.
[0015] Optionally, the silicon substrate includes a base area and an emitter, the emitter being located on a side of the base area remote from the tunnel oxide layer, a passivation layer being provided on a side of the emitter remote from the base area, and the second electrode being electrically connected to the emitter through the passivation layer.
[0016] The present invention provides a photovoltaic module, which includes a first sealing panel, a first sealing adhesive film, a cell string, a second sealing adhesive film and a second sealing panel, which are stacked together, and the cell string is formed by electrically connecting a plurality of the above-mentioned solar cells. Effect of the Invention
[0017] Compared with the prior art, the solar cell and its manufacturing method, and photovoltaic module provided by the present invention have at least the following beneficial effects:
[0018] The solar cell and its manufacturing method, and photovoltaic module provided by the present invention include a silicon substrate, a first electrode, and a second electrode, a tunnel oxide layer is provided on one surface of the silicon substrate along a direction away from the silicon substrate, at least two polysilicon doped layers are provided on the tunnel oxide layer away from the silicon substrate, a barrier layer is provided between adjacent polysilicon doped layers, and a plurality of first electrodes are electrically connected to different polysilicon doped layers. The above method solves the problem of balancing the light absorption and metallization of the thin polysilicon, specifically, not only can the total thickness of the polysilicon layer be reduced, but the thin polysilicon layer can also reduce parasitic absorption and increase short circuit current, and the barrier layer can prevent the risk of paste burning through the tunnel oxide layer, reduce metal recombination, increase the open circuit voltage of the solar cell, and thus increase the photoelectric conversion efficiency of the solar cell.
[0019] Of course, any given product embodying the present invention need not specifically achieve all of the technical advantages discussed above simultaneously.
[0020] Other features and advantages of the present invention will become apparent from the following detailed description of exemplary embodiments of the invention, taken in conjunction with the accompanying drawings, in which: FIG. [Brief description of the drawings]
[0021] The accompanying drawings, which are incorporated in and constitute a part of the specification, illustrate embodiments of the invention and, together with the description, serve to explain the principles of the invention. [Figure 1] FIG. 1 is a diagram showing the configuration of a solar cell according to the present invention. [Diagram 2] FIG. 2 is a flow chart of the method for manufacturing a solar cell according to the present invention. [Diagram 3] FIG. 3 is a diagram showing the configuration of a photovoltaic module according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Hereinafter, each exemplary embodiment of the present invention will be described in detail with reference to the drawings. Note that, unless otherwise specified, the relative arrangement of the members and steps, the formulas and the numerical values described in these embodiments do not limit the scope of the present invention.
[0023] The following description of at least one exemplary embodiment is intended to be exemplary in nature and is not intended to be in any way limiting of the invention and its application or uses.
[0024] Techniques, methods and apparatus well known to those skilled in the art may not be described in detail, but where appropriate, said techniques, methods and apparatus shall be considered part of the description.
[0025] In all examples shown and discussed herein, any specific numerical values should be construed as merely illustrative and not limiting, and therefore other examples of the illustrative embodiments may have different numerical values.
[0026] It should be noted that like symbols and letters indicate like items in the following drawings, and thus, once an item is defined in one drawing, it need not be further considered in the next drawing.
[0027] FIG. 1 is a structural schematic diagram of a solar cell provided by the present invention. As shown in FIG. 1, in this embodiment, a solar cell is provided, which includes a silicon substrate 1, a first electrode 2, and a second electrode 3. A tunnel oxide layer 4 is provided on one surface of the silicon substrate 1 along a direction away from the silicon substrate 1. At least two polysilicon doped layers 5 are provided on the side of the tunnel oxide layer 4 away from the silicon substrate 1. A barrier layer 6 is provided between adjacent polysilicon doped layers 5. A plurality of first electrodes 2 are electrically connected to different polysilicon doped layers 5.
[0028] Specifically, the solar cell may be a TOPCon cell and includes a silicon substrate 1, a first electrode 2, and a second electrode 3, where the silicon substrate 1 may be an N-type silicon substrate, and the first electrode 2 and the second electrode 3 may both be metals such as silver, aluminum, copper, nickel, etc.
[0029] A tunnel oxide layer 4 is provided on one surface of the silicon substrate 1 along a direction away from the silicon substrate 1, the tunnel oxide layer 4 allows majority carrier electrons to tunnel into the polysilicon doped layer 5 while blocking minority carrier hole recombination, and the electrons are transported laterally in the polysilicon doped layer 5 and collected in the metal, which greatly reduces the metal contact recombination current and increases the open circuit voltage and short circuit current of the TOPCon cell. A plurality of polysilicon doped layers 5 are provided on the side of the tunnel oxide layer 4 away from the silicon substrate 1, and a barrier layer 6 is provided between adjacent polysilicon doped layers 5, and the plurality of polysilicon doped layers 5 may be three polysilicon doped layers 5, four polysilicon doped layers 5, or five polysilicon doped layers 5, and preferably, a three polysilicon doped layer 5 is provided on the side of the tunnel oxide layer 4 away from the silicon substrate 1, and a barrier layer 6 is provided between two adjacent polysilicon doped layers 5, and the barrier layer 6 is denser than the polysilicon doped layers 5, which can provide a barrier effect. Specifically, the barrier layer 6 can act to prevent burn-through of the paste (e.g., silver particles) without affecting electron transport. Barrier layers 6 include, but are not limited to, silicon oxide, silicon oxynitride, and aluminum oxide.
[0030] The multiple first electrodes 2 are electrically connected to different polysilicon doped layers 5; for example, some of the first electrodes 2 are sintered to the outermost polysilicon doped layer 5 (the side farthest from the tunnel oxide layer 4), some of the first electrodes 2 are sintered to the innermost polysilicon doped layer 5 (the side closer to the tunnel oxide layer 4), and some of the first electrodes 2 are sintered to the polysilicon doped layer 5 between the innermost and outermost layers. The presence of the barrier layer 6 reduces the risk of burning through the tunnel oxide layer 4 as much as possible, preventing it from affecting the open circuit voltage, backing factor and battery conversion efficiency of the TOPCon cell.
[0031] The silicon substrate 1 includes a base area 11 and an emitter 12, the emitter 12 being located on the side of the base area 11 away from the tunnel oxide layer 4, a passivation layer 7 being provided on the side of the emitter 12 away from the base area 11, and a second electrode 3 penetrating the passivation layer 7 and electrically connected to the emitter.
[0032] As can be seen from the above examples, the solar cell provided by this embodiment has at least the following beneficial effects.
[0033] The solar cell provided by this embodiment includes a silicon substrate 1, a first electrode 2, and a second electrode 3, and a tunnel oxide layer 4 is provided on one surface of the silicon substrate 1 along a direction away from the silicon substrate 1, at least two polysilicon doping layers 5 are provided on the side of the tunnel oxide layer 4 away from the silicon substrate 1, a barrier layer 6 is provided between adjacent polysilicon doping layers 5, and a plurality of first electrodes 2 are electrically connected to different polysilicon doping layers 5. The above invention solves the problem of balancing the light absorption and metallization of thin polysilicon in an overall manner, specifically, not only can the total thickness of the polysilicon layer be reduced, but the thin polysilicon layer can also reduce parasitic absorption and increase short circuit current. In addition, the barrier layer 6 reduces the risk of paste burning through the tunnel oxide layer 4, and reduces metal recombination, increasing the open circuit voltage of the solar cell, and thus improving the photoelectric conversion efficiency of the solar cell.
[0034] 1, in one embodiment of the present invention, the phosphorus doping concentration in the polysilicon doped layer 5 close to the silicon substrate 1 is smaller than the phosphorus doping concentration in the polysilicon doped layer 5 far from the silicon substrate 1, which not only ensures a good passivation effect of the battery, but also reduces the risk of phosphorus diffusing into the silicon substrate 1, effectively improves the open circuit and short circuit current, ensures good contact between the battery and the paste, reduces the contact resistance, and enhances the backing factor of the battery. Specifically, for example, the phosphorus doping concentration range in the polysilicon doped layer 5 close to the silicon substrate 1 is 2×10 20 / cm 3 ~2×10 21 / cm 3 Specifically, for example, the phosphorus doping concentration in the polysilicon doped layer 5 close to the silicon substrate 1 may be 2×10 20 / cm 3 , 11×10 20 / cm 3 , or 2 × 10 21 / cm 3 and the phosphorus doping concentration in the polysilicon doped layer 5 far from the silicon substrate 1 may range from 5×10 20 / cm 3 ~5×10 21 / cm 3 Specifically, the phosphorus doping concentration in the polysilicon doped layer 5 far from the silicon substrate 1 may be 5×10 20 / cm 3 , 27.5×10 20 / cm 3 Or 5 x 10 21 / cm 3 may be also possible.
[0035] Continuing to refer to FIG. 1, in one embodiment of the present invention, the at least two polysilicon doped layers 5 include a first polysilicon doped layer 51, a second polysilicon doped layer 52, and a third polysilicon doped layer 53, with a first barrier layer 61 between the first polysilicon doped layer 51 and the second polysilicon doped layer 52, and a second barrier layer 62 between the second polysilicon doped layer 52 and the third polysilicon doped layer 53, where the first polysilicon doped layer 51 is located closer to the tunnel oxide layer 4, and the third polysilicon doped layer 53 is located farther from the tunnel oxide layer 4.
[0036] The first polysilicon doped layer 51 is doped with phosphorus, and the second polysilicon doped layer 52 and the third polysilicon doped layer 53 are doped with phosphorus and carbon or nitrogen, respectively. That is, the first polysilicon doped layer 51, the second polysilicon doped layer 52 and the third polysilicon doped layer 53 are all doped with phosphorus, and the second polysilicon doped layer 52 and the third polysilicon doped layer 53 are further doped with carbon or nitrogen in addition to phosphorus, thereby increasing the optical gap and reducing parasitic absorption. Of course, according to the actual situation, the second polysilicon doped layer 52 may be doped with only phosphorus, and may not be doped with carbon or nitrogen. In addition, the third polysilicon doped layer 53 is doped with phosphorus and then doped with carbon or nitrogen, thereby increasing the optical gap and reducing parasitic absorption.
[0037] Continuing to refer to FIG. 1, in one embodiment of the present invention, the first electrode 2 includes a first sub-electrode 21 and a second sub-electrode 22, where the first sub-electrode 21 is electrically connected to the third polysilicon doped layer 53, and the second sub-electrode 22 is electrically connected to the first polysilicon doped layer 51 and / or the second polysilicon doped layer 52.
[0038] Specifically, the first electrode 2 includes a first sub-electrode 21 and a second sub-electrode 22, the first sub-electrode 21 is electrically connected to the third polysilicon doped layer 53, and the second sub-electrode 22 is electrically connected to the second polysilicon doped layer 52, or the second sub-electrode 22 is electrically connected to the first polysilicon doped layer 51, or a part of the second sub-electrode 22 is electrically connected to the second polysilicon doped layer 52, and the remaining part of the second sub-electrode 22 is electrically connected to the first polysilicon doped layer 51, thereby more effectively reducing metal recombination, improving the open circuit voltage of the solar cell, and thus enhancing the photoelectric conversion efficiency of the solar cell.
[0039] Continuing to refer to FIG. 1, in one embodiment of the present invention, the doping concentration of phosphorus in the first polysilicon doped layer 51 is less than the doping concentration of phosphorus in the second polysilicon doped layer 52, which is less than the doping concentration of phosphorus in the third polysilicon doped layer 53.
[0040] Specifically, the doping concentration of phosphorus in the first polysilicon doped layer 51, the second polysilicon doped layer 52 and the third polysilicon doped layer 53 is gradually increased. Specifically, the doping concentration of phosphorus in the first polysilicon doped layer 51 is low, which reduces the risk of phosphorus diffusing into the battery, and ensures a good passivation effect of the battery. The doping concentration of phosphorus in the third polysilicon doped layer 53 is high, which ensures good contact between the battery and the paste, reduces the contact resistance, and increases the backing factor of the battery. The doping concentration of phosphorus in the second polysilicon doped layer 52 is between the doping concentration of phosphorus in the first polysilicon doped layer 51 and the doping concentration of phosphorus in the third polysilicon doped layer 53.
[0041] Continuing to refer to FIG. 1, in one embodiment of the present invention, the doping ratio of carbon and nitrogen in the second polysilicon doped layer 52 and the third polysilicon doped layer 53 is less than 5 wt %.
[0042] Specifically, if the doping ratio of carbon and nitrogen in the second polysilicon doped layer 52 and the third polysilicon doped layer 53 exceeds 5 wt%, it will affect the electron transport and passivation effect, and thus affect the battery efficiency. Therefore, the doping ratio of carbon and nitrogen in the second polysilicon doped layer 52 and the third polysilicon doped layer 53 is less than 5 wt%, which is beneficial to the electron transport and passivation effect, and thus improves the battery efficiency. Optionally, the third polysilicon doped layer 53 is doped with carbon and nitrogen, and specifically, the doping ratio of carbon and nitrogen in the second polysilicon doped layer 52 and the third polysilicon doped layer 53 may be 0.01 wt%, 1 wt%, 2 wt%, 3 wt%, 4 wt% or 5 wt%.
[0043] Continuing to refer to FIG. 1, in one embodiment of the present invention, the ratio of the doping concentration of phosphorus in the first polysilicon doped layer 51 and the third polysilicon doped layer 53 is in the range of 0.4-1.
[0044] Specifically, when the ratio of the phosphorus doping concentration in the first polysilicon doped layer 51 to the third polysilicon doped layer 53 is lower than 0.4, the phosphorus doping concentration in the third polysilicon doped layer 53 is too high, which causes severe Auger recombination, affecting the short circuit current and passivation effect of the battery, and thus affecting the battery efficiency. When the ratio of the phosphorus doping concentration in the first polysilicon doped layer 51 to the third polysilicon doped layer 53 is higher than 1, the phosphorus doping concentration in the third polysilicon doped layer 53 is too low, which causes large contact resistance, lowers the backing factor of the battery, and affects the battery efficiency. Therefore, by setting the ratio of the phosphorus doping concentration in the first polysilicon doped layer 51 to the third polysilicon doped layer 53 to 0.4 to 1, it is possible to prevent the phosphorus doping concentration in the third polysilicon doped layer 53 from being too high, reduce Auger recombination, and increase the short circuit current and passivation effect of the battery, as well as to prevent the phosphorus doping concentration in the third polysilicon doped layer 53 from being too low, reduce the contact resistance, improve the backing factor of the battery, and ultimately increase the battery efficiency. Specifically, the ratio of the phosphorus doping concentration in the first polysilicon doped layer 51 to the third polysilicon doped layer 53 may be 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, or 1.
[0045] Continuing to refer to FIG. 1, in one embodiment of the present invention, the total thickness of the first polysilicon doped layer 51, the second polysilicon doped layer 52 and the third polysilicon doped layer 53 along the direction perpendicular to the silicon substrate 1 does not exceed 70 nm.
[0046] Specifically, if the total thickness of the first polysilicon doped layer 51, the second polysilicon doped layer 52, and the third polysilicon doped layer 53 exceeds 70 nm along the direction perpendicular to the silicon substrate 1, the total thickness of the polysilicon layer cannot be reduced and the parasitic absorption of light cannot be increased, so by setting the total thickness of the first polysilicon doped layer 51, the second polysilicon doped layer 52, and the third polysilicon doped layer 53 not to exceed 70 nm along the direction perpendicular to the silicon substrate 1, the total thickness of the polysilicon layer can be reduced, the parasitic absorption of light can be reduced, and the manufacturing cost can be reduced. Specifically, the total thickness of the first polysilicon doped layer 51, the second polysilicon doped layer 52, and the third polysilicon doped layer 53 along the direction perpendicular to the silicon substrate 1 can be 60 nm, 65 nm, or 70 nm.
[0047] Continuing to refer to FIG. 1, in one embodiment of the present invention, the thickness range of the first polysilicon doped layer 51, the second polysilicon doped layer 52 and / or the third polysilicon doped layer 53 along the direction perpendicular to the silicon substrate 1 is 5 nm to 40 nm.
[0048] Specifically, if the thickness of the first polysilicon doped layer 51, the second polysilicon doped layer 52, and the third polysilicon doped layer 53 along the direction perpendicular to the silicon substrate 1 is less than 5 nm, there is a risk that the paste will burn through the tunnel oxide layer 4. If the thickness of the first polysilicon doped layer 51, the second polysilicon doped layer 52, or the third polysilicon doped layer 53 along the direction perpendicular to the silicon substrate 1 is less than 5 nm, it is difficult to control the uniformity of the polysilicon doped layer of each layer. If the thickness of the first polysilicon doped layer 51, the second polysilicon doped layer 52, and / or the third polysilicon doped layer 53 along the direction perpendicular to the silicon substrate 1 is more than 40 nm, the manufacturing cost will be high. Therefore, by setting the thickness of the first polysilicon doped layer 51, the second polysilicon doped layer 52 and / or the third polysilicon doped layer 53 to 5 nm to 40 nm along the direction perpendicular to the silicon substrate 1, it is possible to reduce the risk of the paste burning through the tunnel oxide layer 4, as well as to control the uniformity of the polysilicon doped layer of each layer, and to reduce the manufacturing cost. Specifically, the thickness of the first polysilicon doped layer 51 along the direction perpendicular to the silicon substrate 1 may be 40 nm, 35 nm, 30 nm, 25 nm, 20 nm, 15 nm, 10 nm or 5 nm. The thickness of the second polysilicon doped layer 52 along the direction perpendicular to the silicon substrate 1 may be 40 nm, 30 nm, 20 nm, 10 nm or 5 nm. The thickness of the third polysilicon doped layer 53 along the direction perpendicular to the silicon substrate 1 may be 5 nm, 10 nm, 20 nm, 30 nm or 40 nm. Alternatively, the first polysilicon doped layer 51 may be 40 nm thick, the second polysilicon doped layer 52 may be 25 nm thick, and the third polysilicon doped layer 53 may be 5 nm thick. Alternatively, the first polysilicon doped layer 51 may be 35 nm thick, the second polysilicon doped layer 52 may be 30 nm thick, and the third polysilicon doped layer 53 may be 5 nm thick.Alternatively, the first polysilicon doped layer 51 may be 30 nm thick, the second polysilicon doped layer 52 may be 30 nm thick, and the third polysilicon doped layer 53 may be 10 nm thick.
[0049] Continuing to refer to FIG. 1, in one embodiment of the present invention, the thickness range of the first barrier layer 61 and the second barrier layer 62 along the direction perpendicular to the silicon substrate 1 is 0.5 nm to 2.5 nm, respectively.
[0050] Specifically, if the thickness of the first barrier layer 61 and the second barrier layer 62 is less than 0.5 nm along the direction perpendicular to the silicon substrate 1, the thickness of the first barrier layer 61 and the second barrier layer 62 is too thin, making it difficult to control the uniformity in the manufacturing process and reducing the effect of preventing burn-through by the paste. If the thickness of the first barrier layer 61 and the second barrier layer 62 is more than 2.5 nm along the direction perpendicular to the silicon substrate 1, it affects the transport of electrons and greatly affects the backing factor of the battery. Therefore, by setting the thickness range of the first barrier layer 61 and the second barrier layer 62 to 0.5 nm to 2.5 nm along the direction perpendicular to the silicon substrate 1, it is possible to avoid the thickness of the first barrier layer 61 and the second barrier layer 62 being too thin, which helps to control the uniformity of the first barrier layer 61 and the second barrier layer 62 in the process and is also advantageous for the transport of electrons, thereby increasing the backing factor of the battery. Specifically, along the direction perpendicular to the silicon substrate 1, the thickness of the first barrier layer 61 may be 0.5 nm, 1 nm, 1.5 nm, 2 nm or 2.5 nm, and along the direction perpendicular to the silicon substrate 1, the thickness of the second barrier layer 62 may be 0.5 nm, 1 nm, 1.5 nm, 2 nm or 2.5 nm.
[0051] FIG. 2 is a flow chart of a method for manufacturing a solar cell provided by the present invention. Continue to refer to FIG. 1 and FIG. 2, in this embodiment, a method for manufacturing a solar cell is provided, and the method for manufacturing a solar cell includes the following steps. Specifically, S1 cleaning and texturing a silicon substrate 1; performing boron diffusion on the textured silicon substrate 1 to form a boron-doped silicon layer (S2); S3 removing the borosilicate glass in the boron-doped silicon layer on the back surface, and then performing alkaline polishing on the back surface; depositing a polysilicon doped layer 5 on the backside stack after alkaline polishing S4; After depositing the polysilicon doped layer 5, phosphorus is diffused on the back surface, and annealing is performed after the phosphorus diffusion to crystallize the polysilicon doped layer 5 and activate the impurities (S5); After annealing, the wraparound of the front polysilicon doped layer, the front borosilicate glass and the back phosphosilicate glass are removed, and then coating is performed on the front and back surfaces (S6); S7 printing the first electrode 2 and the second electrode 3 on the surface of the front and back coatings, respectively; After printing the first electrodes 2 and the second electrodes 3, sintering is performed, in which the first electrodes 2 are electrically connected to different polysilicon doping layers 5 (S8).
[0052] Specifically, this embodiment further provides a method for manufacturing a solar cell. The method for manufacturing a solar cell may be a method for manufacturing a TOPCon cell, and may use an N-type single crystal silicon wafer with a resistivity range of 0.3-2.1 Ohm.cm and a minority carrier lifetime greater than 2.5 ms. The damaged layer on the surface of the silicon wafer is removed in a mixed solution of KOH and H2O2, and then texturing is performed in a KOH solution to form a pyramid texture surface on the surface of the silicon wafer, the size of the pyramid texture surface is controlled to 1-5 μm, and after the texture surface is completed, an emitter is manufactured on the front surface of the silicon wafer using B diffusion, the sheet resistance is 110-150 Ohm.cm, the thickness of the front borosilicate glass is 50-120 nm, and after removing the borosilicate glass from the back surface of the silicon wafer, alkaline polishing is performed to make the reflectance of the back surface of the silicon wafer greater than 40%. After alkaline polishing, a polysilicon doping layer 5 is deposited on the backside stack in an LPCVD apparatus, and after the deposition of the polysilicon doping layer 5 is completed, it is doped in a phosphorus diffusion apparatus, and directly annealed in the phosphorus diffusion apparatus to crystallize the polysilicon and push out the impurities (P) to activate it. The conditions of the annealing process are annealing at 800-1000°C for 10-150 min, the annealing atmosphere is N2 (nitrogen gas), or N2 at the beginning and O2 (oxygen gas) at the end, and cleaning is performed after annealing. Alternatively, a polysilicon doping layer is deposited in a PECVD apparatus, and phosphorus is doped while the doped polysilicon is deposited, and then annealing is performed to crystallize the polysilicon and push out the impurities (P) to activate it. After annealing, the wrap-around of the front polysilicon doping layer, the front borosilicate glass and the back phosphosilicate glass are removed, and then the wafer is cleaned again. After cleaning, the wafer is coated on the front and back sides, for example, an aluminum oxide layer is deposited on the front side of the silicon wafer by ALD, a silicon nitride layer is produced by PECVD, and a first passivation layer is deposited on the back side of the silicon wafer to complete the manufacture of the battery precursor.After the surface passivation is completed, the front and back surfaces of the silicon wafer are metallized, and the first electrode 2 is printed on the back surface of the silicon wafer and the second electrode 3 is printed on the front surface by screen printing. Since the paste (silver particles) has different sizes and shapes, the depth to which the first electrode 2 is dissolved into the polysilicon doped layer 5 is also different. For example, multiple first electrodes 2 are electrically connected to different polysilicon doped layers 5. After the first electrode 2 and the second electrode 3 are screen printed, the first electrode 2 is dissolved into the polysilicon doped layer 5 at a high temperature of 850° to 950°, and the second electrode 3 is dissolved into the emitter layer, and finally the battery is manufactured.
[0053] As can be seen from the above examples, the method for manufacturing a solar cell provided by the present examples has at least the following beneficial effects.
[0054] According to the manufacturing method of the solar cell in this embodiment, the silicon substrate 1 is cleaned and textured, and the silicon substrate 1 after textured is subjected to boron diffusion to form a boron-doped silicon layer, and the borosilicate glass in the boron-doped silicon layer on the back surface is removed, and then the back surface is subjected to alkali polishing, and after alkali polishing, the polysilicon doping layer 5 is deposited on the back surface stack, and the wraparound of the front polysilicon doping layer 5 is removed, and then the phosphorus-containing liquid doping agent is roller-coated on the back surface, and then dried, and the dried phosphorus-containing liquid doping agent is annealed to crystallize the polysilicon doping layer 5 and activate the impurities, and after annealing, the front and back surfaces are coated, and the first electrode 2 and the second electrode 3 are printed on the surfaces of the front and back coating, respectively, and after the first electrode 2 and the second electrode 3 are printed, sintering is performed, where the multiple first electrodes 2 are electrically connected to different polysilicon doping layers 5. By adopting the above method, it is possible to reduce metal recombination, improve the open circuit voltage of the solar cell, and thus improve the photoelectric conversion efficiency of the solar cell.
[0055] Continuing to refer to FIG. 1, in one embodiment of the present invention, after alkaline polishing, depositing a polysilicon doped layer 5 on the backside stack includes fabricating a tunnel oxide layer 4 and depositing a first polysilicon doped layer 51, fabricating a first barrier layer 61 and depositing a second polysilicon doped layer 52, and fabricating a second barrier layer 62 and depositing a third polysilicon doped layer 53.
[0056] Specifically, the polysilicon doped layer 5 is deposited on the stack by PECVD (Plasma Enhanced Chemical Vapor Deposition), with a deposition temperature of 350-480° C. and a power of 6000w-15000w, the tunnel oxide layer 4 is grown with N2O (laughing gas) and the process time is in the range of 10-60s, the first polysilicon doped layer 51 is grown in situ with a mixture of PH3 (phosphine) and SiH4 (silane) and the process time is 100-300s, and after the first polysilicon doped layer 51 is grown, the first barrier layer 61 is grown with N2O and the process time is in the range of 100-300s. Alternatively, the first barrier layer 61 is deposited using a mixed gas of SiH4, N2O and NH3, and the process time is 1 to 10 s. After the first barrier layer 61 is grown, the second polysilicon doped layer 52, the second barrier layer 62 and the third polysilicon doped layer 53 are sequentially grown as described above, and the second polysilicon doped layer 52 and / or the third polysilicon doped layer 53 can be grown using a mixed gas of PH3, SiH4 and CH4 (or NH3), and the process time is 30 to 300 s. The above method not only reduces the total thickness of the polysilicon layer, but also reduces parasitic absorption, increases short circuit current, and prevents the risk of the paste burning through the tunnel oxide layer 4 by the barrier layer 6.
[0057] 1, in one embodiment of the present invention, the first electrode 2 includes a first sub-electrode 21 and a second sub-electrode 22, in which the first sub-electrode 21 is electrically connected to the third polysilicon doped layer 53, and the second sub-electrode 22 is electrically connected to the first polysilicon doped layer 51 and / or the second polysilicon doped layer 52. The first electrode 2 has been described in detail in the solar cell, so there is no need to repeat the description here.
[0058] FIG. 3 is a diagram showing the structure of a photovoltaic module provided by the present invention. As shown in FIG. 3, in this embodiment, a photovoltaic module is provided, and the photovoltaic module includes a first sealing panel 201, a first sealing adhesive film 202, a cell string 203, a second sealing adhesive film 204 and a second sealing panel 205, which are stacked and arranged, and the cell string 203 is formed by electrically connecting a plurality of the above-mentioned solar cells.
[0059] Specifically, the photovoltaic module includes a first sealing panel 201, a first sealing adhesive film 202, a cell string 203, a second sealing adhesive film 204, and a second sealing panel 205, which are stacked together. The cell string 203 is formed by electrically connecting a plurality of the above solar cells. The first sealing panel 201 may adopt reinforced glass, which has high light transmittance and can reach 92% or more, and generally adopts low-iron reinforced embossed glass. The second sealing panel 205 can adopt glass material, TPT (polyvinyl fluoride composite film) or TPE (thermoplastic elastomer), which is used to protect the internal sealing material and the battery from mechanical damage and the external environment, and further has good insulation performance, which greatly determines the life of the module, and has excellent weather resistance, low water vapor transmission rate, good electrical insulation, and certain adhesive strength. The first sealing adhesive film 202 and the second sealing adhesive film 204 can be made of EVA (ethylene vinyl acetate copolymer), POE (random copolymer elastomer of ethylene and high carbon number α-olefin) or PVB (polyvinyl butyral). The EVA material can be made to have a low crystallinity and high toughness, impact resistance, filler compatibility and heat sealability by introducing vinyl acetate monomer into the molecular chain. The POE material has excellent mechanical properties, rheology and UV resistance due to its molecular structure, good affinity with polyolefin, good toughness at low temperature, and high cost performance. The PVB material can be dissolved in methanol, ethanol, ketones, alkyl halides, and aromatic hydrocarbon solvents, and has good compatibility with phthalic acid esters, sebacic acid ester plasticizers, nitrocellulose, phenolic resins, epoxy resins, etc., and has high transparency, cold resistance, impact resistance, and UV radiation resistance, and has good adhesion to metals, glass, wood, ceramics, textile products, etc.The first sealing adhesive film 202 and the second sealing adhesive film 204 are used for sealing and protecting the battery cells, preventing the external environment from affecting the performance of the battery cells, and bonding the first sealing panel 201, the solar cell, and the second sealing panel 205 to provide a certain adhesive strength, high light transmittance, a reasonable degree of cross-linking, excellent resistance to ultraviolet aging and excellent resistance to moist heat aging, and an extremely low shrinkage rate, and have long-term strong adhesive performance and high volume resistivity for various first sealing panels 201 and second sealing panels 205. The cell string 203 is formed by electrically connecting the above-mentioned multiple solar cells (not shown), and two adjacent solar cells are electrically connected via a PV ribbon (not shown).
[0060] As can be seen from the above examples, the solar cell, the manufacturing method thereof, and the photovoltaic module provided by the present invention have at least the following beneficial effects.
[0061] The solar cell and its manufacturing method, and photovoltaic module provided by the present invention include a silicon substrate, a first electrode, and a second electrode, a tunnel oxide layer is provided on one surface of the silicon substrate along a direction away from the silicon substrate, at least two polysilicon doped layers are provided on the tunnel oxide layer away from the silicon substrate, a barrier layer is provided between adjacent polysilicon doped layers, and a plurality of first electrodes are electrically connected to different polysilicon doped layers. The above method solves the problem of balancing the light absorption and metallization of the thin polysilicon, specifically, not only can the total thickness of the polysilicon layer be reduced, but the thin polysilicon layer can also reduce parasitic absorption and increase short circuit current, and the barrier layer can prevent the risk of paste burning through the tunnel oxide layer, reduce metal recombination, increase the open circuit voltage of the solar cell, and thus increase the photoelectric conversion efficiency of the solar cell.
[0062] Although several specific embodiments of the present invention have been described in detail by way of examples, those skilled in the art should understand that the above examples are for illustrative purposes only and are not intended to limit the scope of the present invention. Those skilled in the art should understand that the above examples can be modified without departing from the scope and spirit of the present invention. The scope of the present invention is limited by the claims.
Claims
1. The semiconductor device includes a silicon substrate, a plurality of first electrodes, and a second electrode, A tunnel oxide layer is provided on one surface of the silicon substrate, and at least two polysilicon doped layers are sequentially provided on a surface of the tunnel oxide layer away from the silicon substrate, and a barrier layer is provided between adjacent polysilicon doped layers to prevent burn-through of the tunnel oxide layer by a paste that is a material of the first electrode without affecting electron transport, each of the polysilicon doped layers is electrically connected to at least one of the first electrodes, and each of the first electrodes is electrically connected to at least one of the polysilicon doped layers, and some of the first electrodes are not sintered to the polysilicon doped layer that is closest to the tunnel oxide layer among the at least two polysilicon doped layers. A solar cell characterized by:
2. a doping concentration of phosphorus in the polysilicon doped layer closer to the silicon substrate is smaller than a doping concentration of phosphorus in the polysilicon doped layer farther from the silicon substrate; The solar cell according to claim 1 .
3. The at least two polysilicon doped layers include a first polysilicon doped layer, a second polysilicon doped layer, and a third polysilicon doped layer, and have a first barrier layer between the first polysilicon doped layer and the second polysilicon doped layer, and have a second barrier layer between the second polysilicon doped layer and the third polysilicon doped layer, where the first polysilicon doped layer is located closer to the tunnel oxide layer, and the third polysilicon doped layer is located farther from the tunnel oxide layer; The first polysilicon doped layer is doped with phosphorus, and the second polysilicon doped layer and the third polysilicon doped layer are doped with phosphorus and carbon or nitrogen, respectively. The solar cell according to claim 1 .
4. The first electrode includes a first sub-electrode and a second sub-electrode, the first sub-electrode being electrically connected to the third polysilicon doped layer, and the second sub-electrode being electrically connected to the first polysilicon doped layer and / or the second polysilicon doped layer. The solar cell according to claim 3 .
5. a doping concentration of phosphorus in the first polysilicon doped layer is less than a doping concentration of phosphorus in the second polysilicon doped layer, and a doping concentration of phosphorus in the second polysilicon doped layer is less than a doping concentration of phosphorus in the third polysilicon doped layer; The solar cell according to claim 3 .
6. In the second polysilicon doped layer, the mass percentage of doped carbon is less than 5 wt %, and the mass percentage of doped nitrogen is less than 5 wt %, and in the third polysilicon doped layer, the mass percentage of doped carbon is less than 5 wt %, and the mass percentage of doped nitrogen is less than 5 wt %. The solar cell according to claim 3 .
7. a ratio of a doping concentration of phosphorus in the first polysilicon doped layer to a doping concentration of phosphorus in the third polysilicon doped layer is 0.4 to 1; The solar cell according to claim 3 .
8. Along a direction perpendicular to the silicon substrate, the total thickness of the first polysilicon doped layer, the second polysilicon doped layer and the third polysilicon doped layer does not exceed 70 nm; The solar cell according to claim 3 .
9. Along a direction perpendicular to the silicon substrate, the first polysilicon doped layer, the second polysilicon doped layer and the third polysilicon doped layer each have a thickness ranging from 5 nm to 40 nm; The solar cell according to claim 8 .
10. Along a direction perpendicular to the silicon substrate, the thickness range of the first barrier layer and the second barrier layer is 0.5 nm to 2.5 nm, respectively. The solar cell according to claim 3 .
11. the silicon substrate includes a base area and an emitter, the emitter being located on a side of the base area remote from the tunnel oxide layer, and a passivation layer being provided on a side of the emitter remote from the base area; the second electrode passes through the passivation layer and is electrically connected to the emitter; The solar cell according to claim 1 .
12. The solar cell according to any one of claims 1 to 11, comprising a first sealing panel, a first sealing adhesive film, a cell string, a second sealing adhesive film, and a second sealing panel, which are stacked and arranged, and the cell string is formed by electrically connecting a plurality of solar cells according to any one of claims 1 to 11. A photovoltaic module comprising:
Citation Information
Patent Citations
Method for preparing non-masked P-type full back electrode contact crystalline silicon solar cell
CN109509813A
Preparation method of crystalline silicon solar passivation contact cell
CN111599895A
POLO-IBC solar cell and preparation method thereof
CN113224202A
Photovoltaic device and photovoltaic device manufacturing method
JP2015138959A
Solar battery and solar battery module
JP2022058069A
Cited By
Solar cell, method for manufacturing the same, and photovoltaic power generation module
JP2026116657A