Resin film with substrate, printed wiring board and electronic device

The use of an epoxy resin and benzoxazine compound in resin films with a base material addresses the issue of peeling during printed wiring board and electronic device manufacturing, ensuring strong adhesion and reliability under high-speed tests.

JP7562944B2Active Publication Date: 2024-10-08SUMITOMO BAKELITE CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2019215217
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-11-28
Publication Date
2024-10-08
Estimated Expiration
2039-11-28

AI Technical Summary

Technical Problem

There is a need for resin films with base materials that exhibit good adhesion and resist peeling during the manufacturing of printed wiring boards and electronic devices, particularly under high-speed accelerated life tests, and for those with low-roughness copper foils to maintain adhesion.

Method used

A resin film with a base material containing an epoxy resin and a benzoxazine compound, which forms a crosslinked structure through self-ring-opening polymerization, enhancing adhesion and resistance to peeling.

Benefits of technology

The resin film with a base material demonstrates improved adhesion and reduced peeling, even under high-speed accelerated life tests, and maintains strong bonding with low-roughness copper foils, enhancing the reliability of printed wiring boards and electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562944000021
    Figure 0007562944000021
  • Figure 0007562944000001
    Figure 0007562944000001
  • Figure 0007562944000002
    Figure 0007562944000002
Patent Text Reader

Abstract

To provide a resin membrane with a substrate, excellent in adhesion and difficult to cause a separation in manufacturing a printed wiring board or an electronic device.SOLUTION: A resin membrane with a substrate includes a substrate and a resin membrane formed in contact with the substrate. The resin membrane contains an epoxy resin and a benzoxazine compound. The resin membrane may contain an inorganic filler such as silica, a cyanate resin, a thermoplastic resin and a coupling agent. The substrate is preferably a copper foil or a resin film.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin film with a substrate, a printed wiring board, and an electronic device. [Background technology]

[0002] Resin films with substrates have been developed for use in the manufacture of printed wiring boards and the like. An example of this type of technology is the resin sheet described in Patent Document 1. This document describes a resin sheet that is characterized by using a thermosetting component and spherical silica. A similar technology is also described in Patent Document 2. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2005-330401 A [Patent Document 2] JP 2006-45388 A Summary of the Invention [Problem to be solved by the invention]

[0004] Recently, there has been a demand for continuous improvement of printed circuit boards in order to apply them to main boards in smartphones and the like. In the manufacture of printed wiring boards and the like, a resin film with a substrate is often laminated for use. A resin film with a substrate may also be used to fill a cavity on a substrate. In these cases, it is required that the resin film is not easily peeled off (has good adhesion). Particularly recently, from the viewpoint of improving the reliability of electronic devices, there is a demand to suppress peeling of the resin film (maintaining adhesion) even after conducting a high-speed accelerated life test (often abbreviated as HAST, an acronym for High Accelerated Stress Test). Recently, there are also cases where it is required that low-roughness or no-roughness copper foil and resin film have good adhesion and peeling is suppressed.

[0005] According to the findings of the present inventors, in the field of resin films with substrates, there is still room for improvement in terms of suppressing peeling of the resin film (good adhesion).

[0006] The present invention has been made in view of the above circumstances. One of the objects of the present invention is to provide a resin film with a substrate that has good adhesion and is less likely to peel off during the production of a printed wiring board or an electronic device. [Means for solving the problem]

[0007] The present inventors have completed the invention provided below and have solved the above problems.

[0008] According to the present invention, A substrate-attached resin film comprising a substrate and a resin film provided in contact with the substrate, The resin film is a substrate-attached resin film containing an epoxy resin and a benzoxazine compound. is provided.

[0009] Further, according to the present invention, A printed wiring board having an insulating layer formed of a cured product of the resin film provided in the resin film with a substrate. is provided.

[0010] Further, according to the present invention, The printed wiring board; an electronic element mounted on a circuit layer of the printed wiring board or embedded in the printed wiring board. is provided. Effect of the Invention

[0011] According to the present invention, there is provided a resin film with a substrate which has good adhesion and is less likely to peel off during the production of a printed wiring board or an electronic device. [Brief description of the drawings]

[0012] [Figure 1] 1A to 1C are diagrams for explaining a method for manufacturing a printed wiring board or an electronic device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. In the drawings, similar components are given similar symbols and descriptions thereof will be omitted as appropriate. In order to avoid complexity, when there are multiple identical components in the same drawing, only one of them may be labeled with a reference symbol, and not all of them. The drawings are for illustrative purposes only. The shapes and dimensional ratios of the components in the drawings do not necessarily correspond to the actual products.

[0014] In this specification, the term "approximately" means that a range taking into consideration manufacturing tolerances, assembly variations, and the like, is included, unless otherwise specified explicitly. In this specification, unless otherwise specified, the expression "X to Y" in the explanation of a numerical range means from X to Y. For example, "1 to 5% by mass" means "from 1% by mass to 5% by mass".

[0015] In the description of groups (atomic groups) in this specification, when a description is made without specifying whether the group is substituted or unsubstituted, the description includes both groups having no substituents and groups having a substituent. For example, an "alkyl group" includes not only an alkyl group having no substituents (unsubstituted alkyl group) but also an alkyl group having a substituent (substituted alkyl group). In this specification, the term "(meth)acrylic" refers to a concept that includes both acrylic and methacrylic. The same applies to similar terms such as "(meth)acrylate." In this specification, the term "organic group" means an atomic group obtained by removing one or more hydrogen atoms from an organic compound, unless otherwise specified. For example, a "monovalent organic group" refers to an atomic group obtained by removing one hydrogen atom from any organic compound. In this specification, the term "electronic device" is used to include elements, devices, final products, etc. to which electronic engineering technology is applied, such as semiconductor chips, semiconductor elements, printed wiring boards, electric circuit display devices, information and communication terminals, light-emitting diodes, physical batteries, and chemical batteries.

[0016] <Resin film with substrate> The substrate-attached resin film of the present embodiment includes a substrate and a resin film provided in contact with the substrate. The resin film contains an epoxy resin and a benzoxazine compound.

[0017] The benzoxazine compound contained in the resin film with the substrate of this embodiment is considered to form a regular crosslinked structure by self-ring-opening polymerization due to heat, and the structure has excellent rigidity due to planar orientation. In addition, it is considered that phenol is generated and acts as a curing agent for epoxy resin. Furthermore, it is considered that polar functional groups are generated during the curing reaction due to the reaction mechanism. It is considered that the polarity of the polar functional groups causes adhesion suitable for manufacturing printed wiring boards or electronic devices to be expressed and peeling is suppressed.

[0018] First, the components and physical properties of the resin film in the substrate-attached resin film of this embodiment will be specifically described below.

[0019] (Epoxy resin) The resin film in the substrate-attached resin film of this embodiment contains an epoxy resin. Examples of epoxy resins include bisphenol type epoxy resins such as bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol E type epoxy resins, bisphenol S type epoxy resins, bisphenol M type epoxy resins (4,4'-(1,3-phenylenediisopridiene) bisphenol type epoxy resins), bisphenol P type epoxy resins (4,4'-(1,4-phenylenediisopridiene) bisphenol type epoxy resins), and bisphenol Z type epoxy resins (4,4'-cyclohexydiene bisphenol type epoxy resins); novolac type epoxy resins such as phenol novolac type epoxy resins, cresol novolac type epoxy resins, tetraphenol group ethane type novolac type epoxy resins, and novolac type epoxy resins having a condensed ring aromatic hydrocarbon structure; biphenyl type epoxy resins; and xylylene type epoxy resins. aralkyl-type epoxy resins such as aryl epoxy resins and biphenyl aralkyl-type epoxy resins; phenol aralkyl-type epoxy resins such as phenol aralkyl-type epoxy resins having a phenylene skeleton, naphthol aralkyl-type epoxy resins having a phenylene skeleton, phenol aralkyl-type epoxy resins having a biphenylene skeleton, and naphthol aralkyl-type epoxy resins having a biphenylene skeleton; naphthalene-type epoxy resins such as naphthylene ether-type epoxy resins, naphthol-type epoxy resins, naphthalene diol-type epoxy resins, difunctional to tetrafunctional naphthalene-type epoxy resins, binaphthyl-type epoxy resins, and naphthalene aralkyl-type epoxy resins; anthracene-type epoxy resins; phenoxy-type epoxy resins; dicyclopentadiene-type epoxy resins; norbornene-type epoxy resins; adamantane-type epoxy resins; and fluorene-type epoxy resins.

[0020] From the viewpoint different from the chemical skeleton, the epoxy resin may contain a liquid epoxy resin that is liquid at 25° C. ("liquid at 25° C." means that it has fluidity at 25° C. and 1 atmosphere.) When the resin film contains such a liquid epoxy resin, the resin film becomes appropriately flexible, and better adhesion and embeddability can be easily obtained.

[0021] As a preferred epoxy resin, at least one selected from the group consisting of bisphenol A type epoxy resin, bisphenol F type epoxy resin, epoxy resin containing a biphenyl skeleton, and epoxy resin containing a naphthalene skeleton can be mentioned. Epoxy resin containing a biphenyl skeleton and epoxy resin containing a naphthalene skeleton are effective in improving heat resistance.

[0022] Among them, the epoxy resin preferably contains at least one selected from the group consisting of epoxy resins containing a naphthalene skeleton such as those listed above as "naphthalene-type epoxy resins" and liquid epoxy resins that are liquid at 25°C. As described above, epoxy resins containing a naphthalene skeleton are effective in improving heat resistance, and tend to provide sufficient peeling suppression effect even after HAST. In addition, liquid epoxy resins are effective in providing good adhesion and embeddability. In particular, by using these in combination, a particularly good balance of various properties including adhesion can be achieved.

[0023] The resin film may contain only one epoxy resin, or may contain two or more epoxy resins. The lower limit of the content of the epoxy resin in the resin film is preferably 3% by mass or more, more preferably 4% by mass or more, and even more preferably 5% by mass or more. By having the epoxy resin content of 3% by mass or more, the resin film is sufficiently cured by heat, leading to better adhesion and further improved reliability of the electronic device. The upper limit of the epoxy resin content in the resin film is preferably 50% by mass or less, more preferably 35% by mass or less, and even more preferably 20% by mass or less. If the epoxy resin content is 50% by mass or less, the strength and flame retardancy of the resulting printed wiring board may be improved, or the linear expansion coefficient of the printed wiring board may be reduced, improving the effect of reducing warpage.

[0024] (Benzoxazine compounds) The resin film in the substrate-attached resin film of the present embodiment contains a benzoxazine compound. The benzoxazine compound is not particularly limited as long as it reacts with an epoxy resin to harden the resin film.

[0025] The benzoxazine compound preferably includes a benzoxazine compound having a structure represented by the following general formula (B-1) and / or (B-2).

[0026] [ka]

[0027] In general formula (B-1), a represents an integer of 0 to 3; R 1 and R 2 each independently represents a hydrogen atom or a monovalent organic group, and when a is 2 or more, multiple R 2 may be the same or different. In general formula (B-2), b represents an integer of 0 to 4; R 3 represents a hydrogen atom or a monovalent organic group, and when b is 2 or more, multiple R 3 may be the same or different. * indicates a bond to another chemical structure.

[0028] R 1 Specific examples of R include a hydrogen atom, an alkyl group, an alkenyl group, a cycloalkyl group, an aryl group, an aralkyl group, and an alkynyl group. 1 may be substituted with any substituent. R 1 As the alkyl group, an aryl group is preferable, and a phenyl group is more preferable, which is considered to be able to further increase the heat resistance.

[0029] R 2 and R 3 Specific examples of the alkyl group include an aliphatic hydrocarbon group and an aromatic hydrocarbon group. a is preferably 0 or 1, and more preferably 0. b is preferably 0 or 1, and more preferably 0.

[0030] The benzoxazine compound preferably has a plurality of structures represented by general formula (B-1) and / or (B-2) in one molecule. More specifically, the benzoxazine compound preferably has 2 to 4, more preferably 2, structures represented by general formula (B-1) and / or (B-2) in one molecule. It is believed that the use of such a compound can further enhance the curing performance and improve the heat resistance.

[0031] The benzoxazine compound preferably includes a benzoxazine compound represented by the following general formula (b). Incidentally, the benzoxazine compound represented by the general formula (b) is often called Pd-type benzoxazine. According to the findings of the present inventors, by using the benzoxazine compound represented by the general formula (b), when a resin film is cured, it is easy to obtain a cured film having a high glass transition temperature (i.e., it is easy to obtain a cured film having high heat resistance) and a cured film having small thermal expansion.

[0032] [ka]

[0033] In general formula (b), X 2 is a single bond or a divalent linking group. More specifically, X 2 is a single bond, a linear or branched alkylene group having 1 to 10 carbon atoms, -O-, -SO 2 In terms of availability, X may be -, -CO-, or a structure in which two or more of these are linked. 2 Ha-CH 2 - is preferred.

[0034] The benzoxazine compound may include a benzoxazine compound represented by the following general formula (b'): Incidentally, the benzoxazine compound represented by the general formula (b') is often called Fa-type benzoxazine. In the general formula (b'), X 2 The definition and specific examples of X in general formula (b) are as follows: 2 is the same as:

[0035] [ka]

[0036] The resin film may contain only one benzoxazine compound, or it may contain two or more benzoxazine compounds. The lower limit of the content of the benzoxazine compound in the resin film is preferably 3% by mass or more, more preferably 4% by mass or more, and even more preferably 5% by mass or more. When the content of the benzoxazine compound is 3% by mass or more, the resin film is sufficiently cured by heat, leading to better adhesion and further improved reliability of the electronic device. The upper limit of the content of the benzoxazine compound in the resin film is preferably 50% by mass or less, more preferably 35% by mass or less, and even more preferably 20% by mass or less. When the content of the benzoxazine compound is 50% by mass or less, the strength and flame retardancy of the obtained printed wiring board may be improved, or the linear expansion coefficient of the printed wiring board may be reduced, improving the effect of reducing warpage.

[0037] (Cure accelerator) The resin film in the substrate-attached resin film of the present embodiment may contain a curing accelerator, which can improve the productivity of printed wiring boards by shortening the curing time, for example. The curing accelerator is not particularly limited as long as it can accelerate the curing reaction between the epoxy resin and the benzoxazine compound. For example, tertiary amine compounds such as benzyldimethylamine (BDMA) and 2,4,6-trisdimethylaminomethylphenol (DMP-30); imidazole compounds such as 2-methylimidazole, 2-ethyl-4-methylimidazole (EMI24), 2-phenyl-4-methylimidazole (2P4MZ), 2-phenylimidazole (2PZ), 2-phenyl-4-methyl-5-hydroxyimidazole (2P4MHZ), and 1-benzyl-2-phenylimidazole (1B2PZ); BF 3 Examples of the hardener include catalytic hardeners such as Lewis acids, such as complexes.

[0038] When a curing accelerator is used, only one curing accelerator may be used, or two or more curing accelerators may be used in combination. When a curing accelerator is used, the content of the curing accelerator in the resin film can be, for example, 0.01 to 10% by mass, and preferably 0.01 to 1% by mass.

[0039] (Inorganic filler) The resin film in the substrate-attached resin film of the present embodiment preferably contains an inorganic filler. The use of an inorganic filler makes it possible to adjust the linear expansion coefficient, etc. This makes it easier to prevent peeling due to temperature fluctuations.

[0040] The inorganic filler is not particularly limited. For example, silicates such as talc, calcined clay, uncalcined clay, mica, and glass; oxides such as titanium oxide, alumina, boehmite, silica, and fused silica; carbonates such as calcium carbonate, magnesium carbonate, and hydrotalcite; hydroxides such as aluminum hydroxide, magnesium hydroxide, and calcium hydroxide; sulfates or sulfites such as barium sulfate, calcium sulfate, and calcium sulfite; borates such as zinc borate, barium metaborate, aluminum borate, calcium borate, and sodium borate; nitrides such as aluminum nitride, boron nitride, silicon nitride, and carbon nitride; titanates such as strontium titanate and barium titanate. Among these, talc, alumina, glass, silica, mica, aluminum hydroxide, and magnesium hydroxide are preferred.

[0041] It is particularly preferable that the inorganic filler contains silica, which is preferable in terms of availability, cost, insulating properties, fluidity when heated, etc. The shape of the inorganic filler is not particularly limited, but is preferably approximately spherical in terms of fluidity when heated, embeddability, and the like.

[0042] The inorganic filler may be surface-modified. For example, the inorganic filler may be surface-modified with a silane coupling agent. This may increase the compatibility with the epoxy resin or the benzoxazine compound, and may further improve the adhesion and embeddability.

[0043] The average particle size of the inorganic filler is not particularly limited and is, for example, between 1 nm and 2 μm.

[0044] By using two or more inorganic fillers with different average particle diameters in combination, for example, when the resin film with a substrate of this embodiment is applied to embedding a substrate, it is easy to obtain an appropriate fluidity. Specifically, the inorganic filler preferably contains first inorganic particles having an average particle size of 0.1 to 2 μm and second inorganic particles having an average particle size of 2 to 100 nm. In this embodiment, the average particle size of the inorganic filler can be determined by measuring the particle size distribution of the particles on a volume basis using, for example, a laser diffraction particle size distribution measuring device (LA-500, manufactured by HORIBA). The particle size distribution can be measured by a wet method using cyclohexanone as a dispersion medium.

[0045] When the resin film contains an inorganic filler, it may contain only one inorganic filler, or it may contain two or more inorganic fillers. When the resin film contains an inorganic filler, the ratio of the inorganic filler in the resin film is preferably 50 to 90% by mass, and more preferably 55 to 85% by mass.

[0046] (Cyanate compounds) The resin film in the substrate-attached resin film of this embodiment may contain a cyanate compound. The cyanate compound reacts with the benzoxazine compound to form a strong chemical structure, which may further improve the heat resistance. The cyanate compound is not particularly limited as long as it has a cyanate group (a functional group represented by -O-CN). The cyanate compound preferably has a plurality of cyanate groups in one molecule. More specifically, the cyanate compound preferably has 2 to 4, more preferably 2, cyanate groups in one molecule. It is believed that the use of such a cyanate compound can further enhance the curing performance and improve the heat resistance.

[0047] An example of the cyanate compound is represented by the following general formula (a1).

[0048] [ka]

[0049] In general formula (a1), R is a divalent linking group, and is preferably a group containing a conjugated double bond. More specifically, R is of the general formula -A 1 -XA2 In this general formula, A 1 and A 2 each independently represents a group selected from an aromatic group, a condensed aromatic group, an alicyclic group, and an alicyclic heterocyclic group, and X represents a single bond or a divalent linking group.

[0050] Here, A 1 Or A 2 Preferred examples of the alkyl group include a hydrocarbon group having 6 to 12 carbon atoms and a benzene ring, a hydrocarbon group having 10 to 20 carbon atoms and a naphthalene ring, a hydrocarbon group having 12 to 24 carbon atoms and a biphenyl structure, a hydrocarbon group having 12 to 36 carbon atoms and having three or more benzene rings, a hydrocarbon group having 12 to 36 carbon atoms and a condensed aromatic group, and an alicyclic heterocyclic group having 4 to 36 carbon atoms. A 1 , A 2 Specific examples of the alkyl group include phenylene, biphenylene, naphthylene, anthracenylene, cyclohexyl, pyridyl, pyrimidyl, thiophenylene, etc. These may be unsubstituted or may have a substituent such as an aliphatic hydrocarbon group, a halogen group, a cyano group, or a nitro group. X is, for example, a single bond, -CH 2 -, -C(CH 3 ) 2 -, -CH 2 -CH 2 Divalent substituents selected from the group: -, -C=C-, -C≡C-, -CO-O-, -CO-NH-, -CH=N-, -CH=NN=CH-, -N=N- or -N(O)=N- are preferred.

[0051] In another embodiment, the cyanate compound may be in the form of a polymer or oligomer. That is, the cyanate compound may be a compound having a cyanate group in the main chain, side chain, or end of the polymer or oligomer. For example, a polymer or oligomer containing a structural unit represented by the following general formula (a2) can be mentioned. By using such a polymer or oligomer having an aromatic ring skeleton (i.e., a conjugated double bond) as the cyanate compound, the thermal conductivity (heat dissipation property) can be improved.

[0052] [ka]

[0053] In formula (a2), R represents a monovalent substituent, and n represents an integer of 0 to 3. Specific examples of the monovalent substituent of R include a monovalent organic group, a halogen atom, a hydroxyl group, a carboxyl group, etc. Examples of the monovalent organic group include an alkyl group, an alkenyl group, a cycloalkyl group, an aryl group, an aralkyl group, and an alkynyl group.

[0054] When the resin film in the substrate-attached resin film of the present embodiment contains a cyanate compound, it may contain only one cyanate compound, or it may contain two or more cyanate compounds. When the resin film in the substrate-attached resin film of the present embodiment contains a cyanate compound, the ratio of the cyanate compound in the resin film is preferably 0.1 to 10 mass %, more preferably 0.5 to 5 mass %.

[0055] (Coupling Agent) The resin film in the substrate-attached resin film of this embodiment may contain a coupling agent. The use of a coupling agent can further increase adhesion. In addition, the use of a coupling agent is expected to improve compatibility between the inorganic filler and other components, which is preferable from the viewpoint of improving embeddability.

[0056] Examples of the coupling agent include silane coupling agents such as epoxy silane coupling agents, cationic silane coupling agents, and amino silane coupling agents, titanate coupling agents, and silicone oil coupling agents, etc. The coupling agents may be used alone or in combination of two or more. This makes it possible to increase the wettability at the interface between the inorganic filler and each resin, and further improve the heat resistance of the cured resin film.

[0057] As the silane coupling agent, various types can be used, and examples thereof include epoxy silane, amino silane, alkyl silane, ureido silane, mercapto silane, vinyl silane, and the like.

[0058] Specific examples of the compounds include γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropylmethyldimethoxysilane, N-phenylγ-aminopropyltriethoxysilane, N-phenylγ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropyltriethoxysilane, N-6-(aminohexyl)3-aminopropyltrimethoxysilane, and N-(3-(trimethoxysilylpropyl)-1,3-phenylpropyl)-1,3-phenylpropyltriethoxysilane. Examples of the silane include benzenedimethanane, γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, methyltrimethoxysilane, γ-ureidopropyltriethoxysilane, vinyltriethoxysilane, etc. Among these, epoxysilane, mercaptosilane, and aminosilane are preferred, and as the aminosilane, primary aminosilane or anilidosilane is more preferred.

[0059] When a coupling agent is used, its amount in the resin film is preferably 0.01 to 5 mass %, more preferably 0.05 to 3 mass %. By using an appropriate amount of coupling agent, it is possible to obtain an effect of improving adhesion and an effect of improving compatibility between the inorganic filler and other components while keeping a balance of various performances.

[0060] (thermoplastic resin) The resin film in the substrate-attached resin film of this embodiment may contain a thermoplastic resin. This allows for adjustment of the fluidity during heating. In other words, the use of a thermoplastic resin may allow for adjustment of embeddability.

[0061] Examples of the thermoplastic resin include polyvinyl acetal resin, (meth)acrylic resin, polyamide resin (e.g., nylon, etc.), thermoplastic urethane resin, polyolefin resin (e.g., polyethylene, polypropylene, etc.), polycarbonate, polyester resin (e.g., polyethylene terephthalate, polybutylene terephthalate, etc.), polyacetal, polyphenylene sulfide, polyether ether ketone, liquid crystal polymer, fluororesin (e.g., polytetrafluoroethylene, polyvinylidene fluoride, etc.), modified polyphenylene ether, polysulfone, polyether sulfone, polyarylate, polyamide imide, polyether imide, thermoplastic polyimide, etc.

[0062] A preferred example of the thermoplastic resin is phenoxy resin. In a narrow sense, "phenoxy resin" is a polyhydroxy polyether synthesized from bisphenols and epichlorohydrin. In this specification, the term "phenoxy resin" also includes polymers (phenoxy resins in a broad sense) obtained by polyaddition reaction of polyfunctional epoxy resins and polyfunctional phenols.

[0063] Phenoxy resin contains a flexible ether skeleton derived from epoxy monomers. Therefore, it is believed to have the function of increasing the flexibility of the film. Therefore, for example, it can relieve stress caused by expansion and contraction due to sudden temperature changes during the manufacture and use of electronic devices, and it is believed that this can further improve the reliability of electronic devices. In addition, the flexibility of the phenoxy resin increases its fluidity when heated, which can further improve adhesion and embeddability.

[0064] Examples of the phenoxy resin include bisphenol A type phenoxy resin, bisphenol F type phenoxy resin, copolymer phenoxy resin of bisphenol A type and bisphenol F type, biphenyl type phenoxy resin, bisphenol S type phenoxy resin, copolymer phenoxy resin of biphenyl type phenoxy resin and bisphenol S type phenoxy resin, etc. Among them, bisphenol A type phenoxy resin or copolymer phenoxy resin of bisphenol A type and bisphenol F type is preferable. The phenoxy resins may be used alone or in combination of two or more kinds.

[0065] The weight average molecular weight (Mw) of the thermoplastic resin such as the phenoxy resin is preferably 10,000 to 100,000, more preferably 20,000 to 80,000, and further preferably 35,000 to 80,000. When Mw is relatively large, it is possible to further suppress the curing shrinkage and further improve the flatness. Although the details of this mechanism are unclear, it is presumed that when Mw is relatively large, the thermal motion of the molecular chain is suppressed, and as a result, the flatness is further improved. On the other hand, in terms of solvent solubility, etc., Mw is preferably 100,000 or less. The weight average molecular weight is measured, for example, as a polystyrene equivalent value by gel permeation chromatography (GPC).

[0066] The phenoxy resin may have a reactive group such as an epoxy group at both ends of the molecular chain or inside the molecular chain. The reactive group in the phenoxy resin is capable of crosslinking with the epoxy group in the epoxy resin. By using such a phenoxy resin, the solvent resistance and heat resistance of the resin film can be improved.

[0067] The phenoxy resin is preferably one that is solid at 25° C. Specifically, a phenoxy resin having a non-volatile content of 90% by mass or more is preferably used. By using such a phenoxy resin, the mechanical properties of the cured product can be improved.

[0068] When the resin film contains a thermoplastic resin, it may contain only one thermoplastic resin, or it may contain two or more thermoplastic resins. When the resin film contains a thermoplastic resin, the amount of the thermoplastic resin in the resin film can be, for example, 0.1 to 10 mass %, preferably 0.5 to 5 mass %. When the resin film contains 0.1 mass % or more of a thermoplastic resin, the effect of using the thermoplastic resin can be obtained sufficiently. When the resin film contains 10 mass % or less of a thermoplastic resin, the effect of using the thermoplastic resin can be obtained while keeping a balance of various performances.

[0069] (Other ingredients) The resin film in the substrate-attached resin film of the present embodiment may contain various components other than those described above, such as colorants such as dyes and pigments, stress reducing agents, antifoaming agents, leveling agents, surfactants, ultraviolet absorbing agents, foaming agents, antioxidants, flame retardants, ion trapping agents, etc.

[0070] Among the above, it is particularly preferable to use a leveling agent. Examples of the leveling agent include BYK-350, 352, 354, 355, 358N, 361N, 381N, 381, 392, BYK-300, 302, 306, 307, 310, 315, 320, 322, 323, 325, 330, 331, 333, 337, 340, 344, 348, 370, 375, 377, 378, 355, 356, 357, 390, UV3500, UV3510, and UV3570 manufactured by BYK-Chemie; Tegorad-2100, 2200, 2250, 2500, and 2700 manufactured by Tego Chemical; and TEGO (registered trademark) Glide manufactured by Evonik Degussa. 100, 110, 130, 403, 406, 410, 411, 415, 432, 435, 440, 450, 482, etc. Of course, the usable leveling agent is not limited to these.

[0071] (Glass transition temperature of the cured product) By designing the resin film so that the glass transition temperature of the heat-cured product of the resin film is an appropriate value, it is possible to further improve the reliability of the printed wiring board or electronic device.

[0072] Specifically, five resin films peeled off from the substrate are stacked and heat-treated at 200°C for 90 minutes to obtain a cured product. The glass transition temperature Tg is calculated from the peak value of tan δ when a dynamic viscoelasticity test is performed under the conditions of a tensile mode, a frequency of 1 Hz, and a temperature rise rate of 5°C / min. The glass transition temperature Tg is preferably 160°C or higher, more preferably 150°C or higher. A Tg of 160°C or higher can further improve the reliability of a printed wiring board or electronic device. There is no particular upper limit for Tg, but from the viewpoint of practical design, it is, for example, 250°C or lower, preferably 240°C or lower. Incidentally, the reason for "stacking five" resin films during measurement is that a single resin film may be too thin to allow for proper measurement.

[0073] (Thickness) The thickness of the resin film may be appropriately adjusted depending on the final structure of the printed wiring board. The resin film has a thickness of, for example, 1 to 200 μm, and preferably 5 to 50 μm. The thickness can be changed by adjusting the concentration of the coating solution or the coating conditions during coating, which will be described later.

[0074] Following the explanation of the components and properties of the resin film, the "substrate" in the substrate-attached resin film of this embodiment will be described.

[0075] As an example, the substrate can be copper foil, which can be obtained, for example, from Mitsui Kinzoku Co., Ltd. The thickness of the copper foil is not particularly limited and is, for example, 0.5 to 35 μm, and preferably 1.0 to 12 μm.

[0076] The maximum height Rz (defined by JIS B 0601) of the copper foil in contact with the resin film is, for example, 5 μm or less, preferably 0.5 to 5 μm, and more preferably 0.5 to 2.0 μm. In this embodiment, due to the good adhesion of the resin film, peeling between the copper foil and the resin film is unlikely to occur after curing, even if the roughness of the copper foil is relatively small.

[0077] As an alternative to copper foil, the substrate may be a resin film, such as polyolefins such as polyethylene and polypropylene, polyesters such as polyethylene terephthalate and polybutylene terephthalate, polycarbonate, release paper such as silicone sheets, and heat-resistant thermoplastic resin sheets such as fluorine-based resins and polyimide resins.

[0078] The resin film of the substrate is preferably a polyester film. Polyester films are preferably used from the viewpoint of heat resistance (resistance to high temperatures during pressing). Specific examples of polyester films include PET (polyethylene terephthalate) film and PBT (polybutylene terephthalate) film. The resin film used as the substrate may be one which has been subjected to an easy peeling treatment or which has a release layer.

[0079] <Method of manufacturing a resin film with a substrate> The resin film with substrate of this embodiment can usually be produced by (1) dissolving or dispersing the components of the resin film, such as the above-mentioned epoxy resin or benzoxazine compound, in a solvent (typically an organic solvent) to prepare a varnish-like coating liquid, and (2) applying the coating liquid to the substrate surface and drying the solvent.

[0080] The solvent in (1) is not particularly limited as long as it can dissolve or disperse the components of the resin film such as epoxy resin, benzoxazine compound, etc. Specific examples of the solvent include organic solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, toluene, ethyl acetate, cyclohexane, heptane, cyclohexane, cyclohexanone, tetrahydrofuran, dimethylformamide, dimethylacetamide, dimethylsulfoxide, ethylene glycol, cellosolve-based solvents, carbitol-based solvents, anisole, and N-methylpyrrolidone. The solvent may be a single solvent or a mixed solvent.

[0081] The coating in (2) can be carried out using a known coating device such as a comma coater, a die coater, a lip coater, or a bar coater. After coating, the coating film is properly dried to remove the solvent. The drying temperature is, for example, 100 to 170° C., and preferably 120 to 150° C. The drying time is, for example, 3 to 8 minutes, and preferably 4 to 6 minutes.

[0082] <Printed wiring boards / electronic devices> The resin film with a substrate of this embodiment can be used to manufacture a printed wiring board and / or an electronic device. Specifically, by using the resin film with a substrate of the present embodiment, it is possible to manufacture a printed wiring board having an insulating layer made of the cured product of the resin film. It is also possible to manufacture an electronic device comprising an electronic element mounted on a circuit layer of the printed wiring board or embedded in the printed wiring board.

[0083] As for the method of manufacturing the printed wiring board or the electronic device, known techniques can be appropriately applied. In the following, as an example, a process for manufacturing an electronic device by forming a build-up layer using the base-attached resin film of this embodiment on a cavity substrate equipped with a chip will be briefly described.

[0084] First, a cavity substrate 100 is prepared as shown in the lower half of I in Fig. 1. A chip 11 is disposed in the cavity of the cavity substrate 100. The cavity substrate 100 also includes copper wiring 5A and the like.

[0085] The resin film 1 with substrate, which includes the resin film 3 and the substrate 5 (the substrate 5 here is preferably copper foil), is heated and pressed from the upper surface of the cavity substrate 100 so that the resin film 3 comes into contact with the cavity substrate 100. As a result, a part of the resin film 3 hardens while deforming. Then, a structure is obtained in which the resin film 1 with substrate and the cavity substrate 100 are laminated and a part of the resin film 3 is embedded in the cavity substrate 100, as shown in II. of FIG. 1. The hardened resin film 3 functions as an insulating film. The hot pressing can be carried out, for example, by vacuum pressing. The pressure during vacuum pressing is, for example, 1 to 5 MPa, and preferably 2 to 4 MPa. The temperature during vacuum pressing is, for example, 180 to 220° C., and preferably 190 to 210° C. The time for vacuum pressing is, for example, 80 to 130 minutes, and preferably 90 to 120 minutes.

[0086] Next, holes 21 are formed by laser processing or the like as shown in III of Fig. 1. As the laser, for example, a carbon dioxide gas laser can be used.

[0087] Next, an electroless plating process is performed to form an electroless plated film (not shown) on the base material 5 (copper foil) and on the inner surfaces of the holes 21.

[0088] Next, resist application, exposure, development, electrolytic plating, resist removal, flash etching of the copper foil, etc. are performed. Through these processes, as shown in FIG. 1 IV, copper wiring 5A is formed where hole 21 was, and the electroless plating film and base material 5 (copper foil) are removed.

[0089] By repeating steps similar to those described in I. to IV. of FIG. 1, an electronic device having a build-up layer 200 provided on a cavity substrate 100 as shown in V. of FIG. 1 can be obtained.

[0090] For each of the above steps, please refer to the descriptions in JP 2017-84842 A and the like as necessary. For example, Figures 7 to 8 in the publication and the explanations accompanying them can be used as references for understanding III. to IV. in Figure 1 in this embodiment.

[0091] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of the present invention are included in the present invention. Below, examples of reference forms are given. 1. A substrate-attached resin film comprising a substrate and a resin film provided in contact with the substrate, The resin film with a substrate comprises an epoxy resin and a benzoxazine compound. 2. 1. The resin film with a substrate according to claim 1, The benzoxazine compound is a resin film with a substrate, the resin film comprising a benzoxazine compound having a structure represented by the above general formula (B-1) and / or (B-2). In general formula (B-1), a represents an integer of 0 to 3; R 1 and R 2 each independently represents a hydrogen atom or a monovalent organic group, and when a is 2 or more, multiple R 2 may be the same or different. In general formula (B-2), b represents an integer of 0 to 4; R 3 represents a hydrogen atom or a monovalent organic group, and when b is 2 or more, multiple R 3 may be the same or different. 3. 1. or 2. A substrate-attached resin film according to the present invention, The benzoxazine compound is a resin film with a substrate, which contains a benzoxazine compound represented by the above general formula (b). In general formula (b), X 2 is a single bond or a divalent linking group. 4. A resin film with a substrate according to any one of 1. to 3., The resin film further comprises an inorganic filler. 5. 4. The resin film with a substrate according to claim 1, The resin film with a substrate, wherein the inorganic filler contains silica. 6. 4. or 5. The substrate-attached resin film according to claim 4, The inorganic filler comprises first inorganic particles having an average particle size of 0.1 to 2 μm and second inorganic particles having an average particle size of 2 to 100 nm. 7. A resin film with a substrate according to any one of 4. to 6., A resin film with a substrate, wherein the ratio of the inorganic filler in the resin film is 50 to 90 mass %. 8. A resin film with a substrate according to any one of 1. to 7., The epoxy resin comprises at least one selected from the group consisting of an epoxy resin having a naphthalene skeleton and a liquid epoxy resin that is liquid at 25°C. 9. A resin film with a substrate according to any one of 1. to 8., The resin film with a substrate, further comprising a cyanate compound. 10. A resin film with a substrate according to any one of 1. to 9., The resin film with a substrate, further comprising a coupling agent. 11. A resin film with a substrate according to any one of 1. to 10., The resin film with a substrate, wherein the resin film further contains a thermoplastic resin. 12. 11. The resin film with a substrate according to claim 11, The resin film with a substrate, wherein the thermoplastic resin contains a phenoxy resin. 13. A resin film with a substrate according to any one of 1. to 12., Five of the resin films peeled off from the substrate are stacked together, and heat-treated at 200°C for 90 minutes to obtain a cured product, which is subjected to a dynamic viscoelasticity test in a tensile mode at a frequency of 1 Hz and a heating rate of 5°C / min. The cured product has a glass transition temperature of 160 to 250°C, as calculated from the peak value of tan δ. 14. A resin film with a substrate according to any one of 1. to 13., The resin film with a substrate, wherein the substrate is a copper foil. 15. 14. The resin film with a substrate according to claim 14, The resin film with a substrate, wherein the maximum height Rz of the copper foil at a portion in contact with the resin film is 5 μm or less. 16. A resin film with a substrate according to any one of 1. to 13., The substrate-attached resin film is a resin film. 17. 16. The substrate-attached resin film according to claim 15, The resin film is a polyester film. 18. A printed wiring board comprising an insulating layer made of a cured product of the resin film provided in the resin film with a substrate according to any one of 1. to 17. 19. 18. The printed wiring board according to claim 18. an electronic element mounted on a circuit layer of the printed wiring board or embedded in the printed wiring board. EXAMPLES

[0092] The embodiments of the present invention will be described in detail based on Examples and Comparative Examples. It should be noted that the present invention is not limited to the Examples.

[0093] Each component listed in the "Resin Film" column of Table 1 was dissolved or dispersed in methyl ethyl ketone using a high-speed stirrer at the solid content percentage listed in the table to prepare a resin varnish with a non-volatile content of 70 mass %. The numerical values ​​showing the blending ratio of each component in Table 1 indicate the blending ratio (mass %) of each component relative to the total solid content in the resin varnish.

[0094] [Table 1]

[0095] The materials and ingredients shown in Table 1 are as follows. (base material) Copper foil: Mitsui Mining & Smelting Co., Ltd. "MT18Ex" (Rz: 2.0 μm, thickness: 2 μm, with 18 μm thick carrier copper foil) PET: Unitika PET film with release layer "TR1"

[0096] (Inorganic filler) Silica (micro): Admatechs silica slurry, product number SC4050, average particle size 1.0 μm Silica (nano): manufactured by Admatechs Co., Ltd., product number Admanano, average particle size 50 nm, contains vinyl groups as reactive groups due to surface treatment with vinyl silane

[0097] (epoxy resin or other thermosetting resin) HP-4700: Manufactured by DIC, 4 functional groups, containing a naphthalene skeleton, and represented by the following chemical formula

[0098] [ka]

[0099] HP-4710: Manufactured by DIC, 4 functional groups, containing a naphthalene skeleton, and represented by the following chemical formula

[0100] [ka]

[0101] HP-4770: Manufactured by DIC, a mixture of the following bifunctional and trifunctional compounds, containing a naphthalene skeleton.

[0102] [ka]

[0103] HP-4750: Manufactured by DIC, trifunctional, contains a naphthalene skeleton, and is represented by the following chemical formula:

[0104] [ka]

[0105] NC-7000L: Manufactured by Nippon Kayaku Co., Ltd., naphthalene aralkyl type (n represents the number of repeating units, and is 1 or more)

[0106] [ka]

[0107] 830S (liquid): DIC, BisF type, liquid at 25℃, compound represented by the following chemical formula

[0108] [ka] HP-4032D: Manufactured by DIC, bifunctional, containing a naphthalene skeleton, and represented by the following chemical formula

[0109] [ka]

[0110] NC-3000: Manufactured by Nippon Kayaku Co., Ltd., biphenyl aralkyl type, compound represented by the following chemical formula (n represents the number of repeating units and is 1 or more)

[0111] [ka]

[0112] 1032H60: Mitsubishi Chemical Corporation, triphenylmethane type, compound represented by the following chemical formula

[0113] [ka]

[0114] MIR-3000-70T: Naphthalene aralkyl maleimide manufactured by Nippon Kayaku Co., Ltd.

[0115] (Benzoxazine, other hardeners, etc.) PT-30: Phenol novolac type cyanate resin manufactured by Lonza Japan Pd type: Shikoku Chemical Industry Co., Ltd., Pd type benzoxazine, general formula (b) X 2 Ga-CH 2 -What is Fa type: Shikoku Chemical Industry Co., Ltd., Fa type benzoxazine, general formula (b') is X 2 Ga-CH 2 -What is BS-BXZ: Benzoxazine of bisphenol S type manufactured by Konishi Chemical Co., Ltd., where X is the general formula (b). 2 -SO 2 -What is HF-3: Phenol novolac resin, manufactured by Sumitomo Bakelite Co., Ltd.

[0116] (thermoplastic resin) YX6954BH30: Mitsubishi Chemical Corporation, phenoxy resin, bisphenol acetophenone type

[0117] (Coupling Agent) A-187: Momentive Performance Materials, epoxy trimethoxysilane

[0118] (Leveling agent) BYK-356: BYK-Chemie, acrylic leveling agent

[0119] (Cure accelerator) TBZ: Shikoku Chemical Industry Co., Ltd., imidazole compound 2PHZ-PW: Shikoku Chemical Industry Co., Ltd., imidazole compound 2PZ: Shikoku Chemical Industry Co., Ltd., imidazole compound C-05MB: Sumitomo Bakelite, phosphonium salt

[0120] (Applying resin varnish to substrates, producing resin films with substrates) The resin varnish was applied to the surface of copper foil or PET film (those marked as "used" in Table 1) using a comma coater. The solvent was then removed at 150°C for 3 minutes to form a 30 μm thick resin film. In this way, a resin film with a substrate (having three layers: resin film-2 μm copper layer-18 μm thick carrier copper foil) was produced.

[0121] <Evaluation> (glass transition temperature Tg) First, the resin film was carefully peeled off from the substrate. Five of the peeled resin films were stacked and heat-treated in a vacuum press at 200°C for 90 minutes under a pressure of 0.5 MPa to obtain a cured product for Tg measurement. A test piece of 8 mm x 40 mm was cut out from this cured product to prepare the test piece. The dynamic viscoelasticity of the test pieces was measured in a tensile mode, at a temperature rise rate of 5° C. / min, and at a frequency of 1 Hz in the temperature range of 20° C. to 300° C. The temperature at which tan δ peaked in this dynamic viscoelasticity test was determined as the glass transition temperature.

[0122] (Linear expansion coefficient in the planar direction (50~150℃)) First, a test piece was obtained in the same manner as in the measurement of the glass transition temperature Tg. The test pieces were subjected to two cycles of thermomechanical analysis (TMA) using a thermomechanical analyzer TMA (Q400, manufactured by TA Instruments) under the conditions of a temperature range of 30 to 300°C, a heating rate of 10°C / min, a load of 10g, and tension mode. The average linear expansion coefficient in the planar direction (XY direction) in the range of 50°C to 150°C was calculated. The linear expansion coefficient was the value at the second cycle.

[0123] (Adhesion evaluation: chip tape test) The resin film surface of the resin film with substrate was placed on the mirror surface of the Si wafer, and laminated at 100°C using a vacuum laminator. The substrate (copper foil or PET film) was then peeled off. After that, a heat treatment was performed at 200°C for 1 hour in an oven in an air atmosphere. This created an evaluation specimen for chip tape testing, with the resin film attached to the Si wafer. Two specimens were prepared for each of the examples and comparative examples, one of which was subjected to HAST treatment at 130° C., 85% RH, and 100 hours.

[0124] For both the evaluation body without HAST treatment and the evaluation body with HAST treatment, the resin film with the attached substrate was cut by making 10 x 10 grid-like cuts at 1 mm intervals using a cutter, and the resin film was cut. After that, adhesive tape was applied to the cut areas, and the adhesive tape was peeled off. If all of the cut resin films (100 pieces of 1 mm x 1 mm) remained on the substrate side, it was evaluated as "no peeling", and if even one piece was attached to the adhesive tape side, it was evaluated as "peeling".

[0125] (Low roughness copper foil peel strength) -Preparation of measurement samples when the base material is copper foil A substrate was prepared by removing the copper foil of a copper-clad laminate (LAZ-4785TH-G manufactured by Sumitomo Bakelite Co., Ltd., thickness 0.15 mm, copper foil 12 μm) by etching. The resin surface of the resin film with the substrate was set on both sides of this substrate, and the substrate was obtained by vacuum pressing under the following conditions. Temperature conditions: Heat at a rate of 3℃ / min and heat at 200℃ for 1.5 hours Pressure condition: 2.0MPa

[0126] Then, the 18 μm thick carrier copper foil was peeled off from the obtained substrate. Further, an electrolytic plating film was formed on the 2 μm thick copper foil remaining on the substrate so that the total copper thickness was 18 μm, to obtain a plated substrate. This plated substrate was subjected to an etching treatment so that a 10 mm wide electrolytic plating copper film was left. In this way, a peel strength measurement sample was obtained. Two samples were prepared for each of the examples and comparative examples, one of which was subjected to HAST treatment at 130° C., 85% RH, and 100 hours.

[0127] -Preparation of measurement samples when the substrate is PET film A substrate was prepared by removing the copper foil of a copper-clad laminate (LAZ-4785TH-G manufactured by Sumitomo Bakelite Co., Ltd., thickness 0.15 mm, copper foil 12 μm) by etching. This substrate was contacted with the resin surface of the resin film with a substrate (PET film), and vacuum laminated under conditions of 100°C, 0.6 MPa, and 30 seconds. After this, the substrate (PET film) was peeled off to expose the resin film, and copper foil ("MT18Ex" manufactured by Mitsui Mining & Smelting Co., Ltd., Rz: 2.0 μm) was contacted with the resin surface and pressed under the following conditions. In this way, a peel strength measurement sample was obtained. Temperature conditions: Heat at a rate of 3℃ / min and heat at 200℃ for 1.5 hours Pressure condition: 2.0MPa Two samples were prepared for each of the examples and comparative examples, one of which was subjected to HAST treatment at 130° C., 85% RH, and 100 hours.

[0128] Peel strength measurement The obtained peel strength measurement sample was used to measure the peel strength in accordance with JIS C-6481: 1996. The larger this value is, the more peeling is suppressed and the better the adhesion is.

[0129] (Multi-reflow) -Preparation of evaluation samples when the base material is copper foil The resin film with the substrate was placed on both sides of an inner layer circuit substrate (Sumitomo Bakelite Co., Ltd., LAZ-4785TH-G, total thickness 0.15 mm, copper patterns with a thickness of 12 μm and L / S=15 / 15 μm on both sides). Then, it was pressurized at a pressure of 2 MPa and a temperature of 200° C. for 1.5 hours. Next, the 18 μm thick carrier copper foil was peeled off, and an electrolytically plated copper film was formed on the 2 μm thick copper foil remaining on the substrate so that the total copper thickness was 18 μm. The sample was then cut into 10 cm x 10 cm pieces, and etched so that five 10 mm wide strips of electrolytically plated copper film remained. In this manner, an evaluation sample was obtained.

[0130] -Preparation of evaluation samples when the substrate is PET film The resin film with the substrate was placed on both sides of an inner layer circuit substrate (Sumitomo Bakelite Co., Ltd., LAZ-4785TH-G, total thickness 0.15 mm, copper patterns with a thickness of 12 μm and L / S=15 / 15 μm on both sides). Then, vacuum lamination was performed under conditions of 100°C, 0.5 MPa, and 30 seconds. Next, the PET film was peeled off, and copper foil ("MT18Ex" manufactured by Mitsui Mining & Smelting Co., Ltd.) was placed in contact with both sides, and pressed under conditions of a pressure of 2 MPa, a temperature of 200°C, and 1.5 hours. After that, the 18 μm thick carrier copper foil of the attached copper foil was peeled off, and an electrolytically plated copper coating was formed on the 2 μm thick copper foil remaining on the substrate so that the total copper thickness was 18 μm. The sample was then cut into 10 cm x 10 cm pieces and etched so that five 10 mm wide electrolytically plated copper coatings remained. In this manner, an evaluation sample was obtained.

[0131] -Multiple reflow evaluation The evaluation was conducted in accordance with IPC / JEDEC J-STD-20. Specifically, the evaluation sample was passed 20 times through a reflow oven set at a reflow temperature of 260°C. After that, the presence or absence of peeling between the electrolytically plated copper coating and the resin film, and between the inner layer circuit and the resin film was confirmed. In the table below, the results are indicated as follows: ○: no peeling, ×: peeling.

[0132] (Inter-wire insulation) - Preparation of evaluation samples The resin film surface of the resin film with substrate was placed on a printed wiring board on which a copper circuit pattern with a line / space of 15 / 15 μm had been formed, and the substrate was heated and pressurized at a pressure of 2 MPa and a temperature of 200° C. for 1.5 hours. In this manner, an evaluation sample was prepared.

[0133] ·Evaluation of line insulation Using the above evaluation sample, the continuous humidity insulation resistance was evaluated for 200 hours under the conditions of a temperature of 130°C, a humidity of 85% RH, and an applied voltage of 3.5 V. Resistance value 10 6 A value of Ω or less was deemed to be a dielectric breakdown (failure). In Table 2, cases where no dielectric breakdown occurred are indicated as "pass."

[0134] (Interlayer insulation) - Preparation of measurement samples when the base material is copper foil (carrier copper foil) First, the copper foil of a copper-clad laminate (LAZ-4785TH-G manufactured by Sumitomo Bakelite Co., Ltd., thickness 0.15 mm, copper foil 12 μm) was subjected to a roughening treatment of about 1 μm. Next, the resin film with copper foil was placed so that its resin surface was in contact with the roughened surface of the copper-clad laminate, and heated and pressed at a pressure of 2 MPa and a temperature of 200° C. for 1.5 hours. After that, the copper foil of the outermost layer was etched to a shape of Φ10 mm. An evaluation sample was prepared as described above.

[0135] -Preparation of measurement samples when the substrate is PET film First, the copper foil of a copper-clad laminate (LAZ-4785TH-G manufactured by Sumitomo Bakelite Co., Ltd., thickness 0.15 mm, copper foil 12 μm) was subjected to a roughening treatment of about 1 μm. Next, a resin film with a substrate (PET film) was placed on both sides of the copper-clad laminate so that the resin surface was in contact with the roughened surface of the copper-clad laminate, and vacuum laminated under conditions of a pressure of 0.6 MPa, a temperature of 100 ° C, and 30 seconds. After that, the PET film was peeled off to expose the resin surface, and copper foil ("MT18Ex" manufactured by Mitsui Mining & Smelting Co., Ltd.) was pressed on the exposed surface (both front and back). The pressure of the press was 2 MPa, the temperature was 200 ° C, and the time was 1.5 hours. Then, the copper foil of the outermost layer was etched in a shape of Φ10 mm. An evaluation sample was produced by the above.

[0136] Using the evaluation sample, the continuous humidity insulation resistance was evaluated for 200 hours under the conditions of temperature 130°C, humidity 85% RH, and applied voltage 3.5 V. Resistance value 10 6 A value of Ω or less was deemed to be a dielectric breakdown (failure). In Table 2, cases where no dielectric breakdown occurred are indicated as "pass."

[0137] The evaluation results are summarized in Table 2. The evaluation results of the chip tape test and low-roughness copper foil peel strength are shown for both the initial state before HAST treatment and after HAST treatment.

[0138] [Table 2]

[0139] As shown in Table 2, the evaluation results of the resin film with a substrate containing an epoxy resin and a benzoxazine compound in Examples 1 to 10 were good. That is, in Examples 1 to 10, in the chip tape test, no peeling occurred even after the HAST treatment. In addition, the low-roughness copper foil peel strength was good even after the HAST treatment. Furthermore, in Examples 1 to 10, the evaluation results of multi-reflow, interline insulation, interlayer insulation, etc. were good. On the other hand, the evaluation results of the substrate-attached resin films not containing a benzoxazine compound as a curing agent for the epoxy resin in Comparative Examples 1 to 3 were inferior to those in Examples 1 to 10. In Comparative Examples 1 to 3, peeling occurred in the chip tape test after the HAST treatment, for example.

[0140] A more detailed analysis of Table 2 reveals that the low-roughness copper foil peel strengths of Examples 1 to 9 are better than that of Example 10. This is believed to be because Examples 1 to 9 use an epoxy resin containing a naphthalene skeleton as the epoxy resin. [Explanation of symbols]

[0141] 1 Resin film 3. Resin Film 5. Substrate (preferably copper foil) 5A copper wiring 11 Chips 100 Cavity Board 200 Build-up Layer

Claims

1. A substrate-attached resin film comprising a substrate and a resin film provided in contact with the substrate, The resin film contains an epoxy resin, a benzoxazine compound, a cyanate compound, and a coupling agent, The epoxy resin includes: (i) at least one epoxy resin selected from the group consisting of epoxy resins containing a biphenyl skeleton and epoxy resins containing a naphthalene skeleton, which is a solid at 25° C.; and (ii) a liquid epoxy resin that is liquid at 25° C.; The benzoxazine compound includes at least one selected from the group consisting of benzoxazine compounds represented by the following general formula (b) and benzoxazine compounds represented by the following general formula (b'): The resin film with a substrate has a content ratio of the benzoxazine compound in the resin film of 12.2 mass % or more and 50 mass % or less. 【Chemistry 1】 In general formula (b), X 2 is a single bond or a divalent linking group, and the divalent linking group is a linear or branched alkylene group having 1 to 10 carbon atoms, -O-, -SO 2 -, -CO-, or a structure in which two or more of these are linked together. 【Chemistry 2】 In the general formula (b'), X 2 The definition of X in general formula (b) 2 is the same as:

2. A substrate-attached resin film comprising a substrate and a resin film provided in contact with the substrate, the resin film contains an epoxy resin, a benzoxazine compound, a cyanate compound, and a coupling agent, and does not contain a bismaleimide compound; The epoxy resin includes: (i) at least one epoxy resin selected from the group consisting of epoxy resins containing a biphenyl skeleton and epoxy resins containing a naphthalene skeleton, which is a solid at 25° C.; and (ii) a liquid epoxy resin that is liquid at 25° C.; The benzoxazine compound includes at least one selected from the group consisting of benzoxazine compounds represented by the following general formula (b) and benzoxazine compounds represented by the following general formula (b'): 【Chemistry 3】 In general formula (b), X 2 is a single bond or a divalent linking group, and the divalent linking group is a linear or branched alkylene group having 1 to 10 carbon atoms, -O-, -SO 2 -, -CO-, or a structure in which two or more of these are linked together. 【Chemistry 4】 In the general formula (b'), X 2 The definition of X in general formula (b) 2 is the same as:

3. The resin film with a substrate according to claim 1 or 2, The resin film further comprises an inorganic filler.

4. The resin film with a substrate according to claim 3, The resin film with a substrate, wherein the inorganic filler contains silica.

5. The resin film with a substrate according to claim 3 or 4, The inorganic filler comprises first inorganic particles having an average particle size of 0.1 to 2 μm and second inorganic particles having an average particle size of 2 to 100 nm.

6. The resin film with a substrate according to any one of claims 3 to 5, A resin film with a substrate, wherein the ratio of the inorganic filler in the resin film is 50 to 90 mass %.

7. The resin film with a substrate according to any one of claims 1 to 6, The epoxy resin is an epoxy resin that is solid at 25°C and contains a naphthalene skeleton.

8. The resin film with a substrate according to any one of claims 1 to 7, The resin film with a substrate, wherein the resin film further contains a thermoplastic resin.

9. The resin film with a substrate according to claim 8, The resin film with a substrate, wherein the thermoplastic resin contains a phenoxy resin.

10. The resin film with a substrate according to any one of claims 1 to 9, Five of the resin films peeled off from the substrate are stacked and heat-treated at 200°C for 90 minutes to obtain a cured product, which is subjected to a dynamic viscoelasticity test under conditions of a tensile mode, a frequency of 1 Hz, and a temperature rise rate of 5°C / min. The cured product has a glass transition temperature of 160 to 250°C, as calculated from the peak value of tan δ.

11. The resin film with a substrate according to any one of claims 1 to 10, The resin film with a substrate, wherein the substrate is a copper foil.

12. The substrate-attached resin film according to claim 11, A resin film with a substrate, wherein the maximum height Rz of the portion of the copper foil in contact with the resin film is 5 μm or less.

13. The resin film with a substrate according to any one of claims 1 to 10, The substrate-attached resin film is a resin film.

14. The substrate-attached resin film according to claim 13, The resin film is a polyester film.

15. A printed wiring board comprising an insulating layer made of a cured product of the resin film provided in the substrate-attached resin film according to any one of claims 1 to 14.

16. The printed wiring board according to claim 15; an electronic element mounted on a circuit layer of the printed wiring board or embedded in the printed wiring board.

Citation Information

Patent Citations

  • Filler-containing resin composition and its utilization

    JP2005330401A

  • Insulating adhesive sheet and its application

    JP2006045388A

  • Resin composition and molded body

    JP2012062422A

  • Flexible bismaleimide, benzoxazine, epoxy-anhydride addition product composite adhesive

    JP2014523953A

  • Thermosetting resin composition for semiconductor package and prepreg and metal foil laminate using the same

    JP2016529371A