How lithium sulfide is produced

By using lithium sulfate and activated carbon in a furnace to produce lithium sulfide, the method addresses the inefficiencies and safety concerns of existing methods, achieving high ionic conductivity and cost-effective production.

JP7562968B2Active Publication Date: 2024-10-08MITSUBISHI MATERIALS CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020046246
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-17
Publication Date
2024-10-08
Estimated Expiration
2040-03-17

AI Technical Summary

Technical Problem

Existing methods for producing lithium sulfide are costly due to the use of organic solvents, require repeated reaction cycles, involve toxic hydrogen sulfide gas, and increase the risk of scattering fine particles, leading to reduced recovery and safety concerns.

Method used

A method using lithium sulfate as a raw material, combined with a reducing agent like activated carbon, is heated in a furnace to produce lithium sulfide, eliminating the need for fine particle formulation and reducing the number of steps, while ensuring safety and cost-effectiveness.

Benefits of technology

This method produces lithium sulfide with high ionic conductivity, reduces unreacted residues, and ensures safety by avoiding toxic gases and scattering issues, thereby enhancing productivity and cost-efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562968000002
    Figure 0007562968000002
  • Figure 0007562968000003
    Figure 0007562968000003
  • Figure 0007562968000004
    Figure 0007562968000004
Patent Text Reader

Abstract

To provide a method for producing lithium sulfide with high ionic conductivity in a more suitable manner.SOLUTION: This method for producing lithium sulfide comprises a preparation step (step S12) for charging a starting material containing, as a main component, lithium sulfate and having such a property that the weight thereof is decreased by 5-25% inclusive up to 120°C, and a reducing agent into a furnace, and a temperature rising step (S14) for heating the starting material and the reducing agent in the furnace to raise the temperature.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing lithium sulfide. [Background technology]

[0002] Lithium sulfide is known as a solid electrolyte for lithium batteries. Patent Document 1 discloses a method in which lithium hydroxide is reacted with hydrogen sulfide in an aprotic organic solvent to produce lithium hydrosulfide, and the reaction is further carried out to produce lithium sulfide.

[0003] Patent Document 2 discloses a method for producing lithium sulfide without using an organic solvent. In Patent Document 2, metallic lithium is reacted with sulfur vapor or hydrogen sulfide to generate lithium sulfide on metallic lithium. Then, the unreacted metallic lithium is heated to a high temperature to melt it, and diffuses and permeates the lithium sulfide that has already been generated, and then cooled. Then, metallic lithium is reacted again with sulfur vapor or hydrogen sulfide to generate lithium sulfide. This cycle is repeated to react 100% of metallic lithium.

[0004] Patent Document 3 discloses a method for producing lithium sulfide by reacting lithium carbonate with hydrogen sulfide.

[0005] Patent Document 4 discloses a method for producing lithium sulfide without using hydrogen sulfide. In Patent Document 4, lithium sulfate and carbon powder are each adjusted to fine particles and mixed together to increase the reaction area and reduce the amount of unreacted raw materials. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2006-151725 A [Patent Document 2] Japanese Patent Application Publication No. 9-110404 [Patent Document 3] JP 2012-221819 A [Patent Document 4] JP 2013-227180 A Summary of the Invention [Problem to be solved by the invention]

[0007] The technology described in Patent Document 1 uses organic solvents, which increases costs. The technology described in Patent Document 2 requires repeated reaction cycles, which increases costs. The technology described in Patent Document 3 uses toxic hydrogen sulfide gas, which is difficult to manage and may make it difficult to ensure safety. The technology described in Patent Document 4 requires fine particles to be adjusted and mixed, which increases the number of steps. In addition, when manufacturing in equipment such as a rotary kiln, the fine particles may scatter inside the equipment, reducing the amount of recovery. Thus, there is room for improvement in the manufacturing method of lithium sulfide, which has high ionic conductivity and is used in lithium batteries.

[0008] The present invention has been made in view of the above, and has an object to provide a more appropriate method for producing lithium sulfide having high ionic conductivity. [Means for solving the problem]

[0009] In order to solve the above-mentioned problems and achieve the object, a method for producing lithium sulfide of the present invention includes a preparation step of charging a raw material containing lithium sulfate as a main component and having a property of reducing its weight by 5% to 25% by 120°C, and a reducing agent into a furnace, and a temperature increasing step of heating the raw material and the reducing agent in the furnace to increase the temperature. Effect of the Invention

[0010] The method for producing lithium sulfide according to the present invention has an effect of more appropriately producing lithium sulfide having high ionic conductivity. [Brief description of the drawings]

[0011] [Figure 1]FIG. 1 is a flow chart showing steps of a method for producing lithium sulfide. [Diagram 2] FIG. 2 is a schematic diagram showing an example of a production apparatus including a rotary kiln. [Diagram 3] FIG. 3 is a SEM photograph of the lithium sulfate raw material when the temperature is increased in this embodiment. [Figure 4] FIG. 4 is a graph showing the test results of the examples, and is a graph showing the measurement results of X-ray diffraction measurement. [Diagram 5] FIG. 5 is a graph showing the test results of the example, and is a graph showing AC impedance measurements. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention will be described in detail below with reference to the drawings. Note that the present invention is not limited to the following modes for carrying out the invention (hereinafter, referred to as embodiments). Furthermore, the components in the following embodiments include those that a person skilled in the art can easily imagine, those that are substantially the same, and those that are within the so-called equivalent range. Furthermore, the components disclosed in the following embodiments can be appropriately combined.

[0013] The method for producing lithium sulfide will be described with reference to Figures 1 and 2. Figure 1 is a flow chart showing steps of the method for producing lithium sulfide. Figure 2 is a schematic diagram showing an example of a production apparatus including a rotary kiln.

[0014] In the method for producing lithium sulfide of the present embodiment, lithium sulfate as a raw material, which is mainly composed of lithium sulfate having a property of losing weight by 5% to 25% by the time the temperature reaches 120° C., and a reducing agent are placed in a furnace and heated to produce lithium sulfide.

[0015] A raw material mainly composed of lithium sulfate, which has the characteristic of losing weight by 5% to 25% by 120°C, is a mixture of hydrated lithium sulfate in lithium sulfate N-hydrate (N=0-1) in which a weight loss of 5% to 25% occurs. In the case of such lithium sulfate N-hydrate, the volume change during heating causes fine cracks on the surface of the lithium sulfate, increasing the surface area and reducing the amount of unreacted residue. A weight loss of less than 5% is not enough to crack the entire raw material. In addition, if the weight loss is 25% or more, the water content is high and the particles bond together, making it difficult to mix with the reducing agent. In addition, more water than is necessary to form cracks must be volatilized, which is not efficient.

[0016] The lithium sulfate has an average particle size of preferably 10 μm or more and 100 μm or less, more preferably 15 μm or more and 80 μm or less, and further preferably 30 μm or more and 50 μm or less. The lithium sulfate, which is the raw material of the lithium sulfide production method of the present embodiment, does not need to be in the form of fine particles. Therefore, even when producing lithium sulfide using equipment such as the rotary kiln 11, for example, the possibility that powdered lithium sulfate will scatter inside the kiln body (furnace) 12 of the rotary kiln 11 and become difficult to recover is reduced.

[0017] The reducing agent is not limited as long as it is a material mainly composed of carbon, such as activated carbon. In this embodiment, the reducing agent is activated carbon. The activated carbon preferably has an average particle size of 1 μm or more and 10 μm or less.

[0018] As shown in FIG. 1, the method for producing lithium sulfide includes a preparation step (step S12) of charging lithium sulfate and a reducing agent into a furnace, a heating step (step S14) of heating the furnace, and a cooling step (step S16) of cooling the furnace.

[0019] [Preparation process] In the preparation step, lithium sulfate and a reducing agent are charged into a furnace in a predetermined molar ratio. In addition, in the preparation step, lithium sulfate and a reducing agent are mixed in a predetermined molar ratio. The molar ratio of lithium sulfate to activated carbon, which is a reducing agent, is preferably, for example, 2 to 4 in terms of the C / Li2SO4 ratio.

[0020] [Heating process] In the temperature raising process, lithium sulfate and a reducing agent are heated in a furnace to raise the temperature. In the temperature raising process, lithium sulfate is dehydrated and reduced by the reducing agent. In the temperature raising process, for example, the temperature is raised to a temperature range of 700°C to 950°C, preferably 800°C to 850°C, in an inert atmosphere with a dew point of -60°C. The type of inert gas is argon or nitrogen. In the temperature range of 700°C or less, the reaction rate between lithium sulfate and the reducing agent is slow, and the productivity is low. In the temperature range of 950°C or more, the temperature is higher than the melting point of lithium sulfide, so lithium sulfide dissolves. In the temperature range of 850°C or more, the temperature is higher than the melting point of lithium sulfate, which is the raw material, so lithium sulfate remaining unreacted dissolves. In the temperature range of 800°C to 850°C, lithium sulfate does not melt, and lithium sulfide that maintains a particle shape is obtained. In the temperature range of 800°C to 850°C, the reaction rate is high and the productivity is high.

[0021] In the temperature-raising step, the temperature is preferably raised at a rate of 10° C. / min or more after the start of heating to reach the desired temperature range. In the temperature-raising step, the heating time in the desired temperature range is preferably 5 minutes or more and 90 minutes or less. The reason why the heating time is preferably within the above range is that if the material is held at a high temperature for a long time, grain growth gradually occurs, resulting in a decrease in reactivity.

[0022] Fig. 3 is an SEM photograph of the lithium sulfate raw material when the temperature is raised in this embodiment. In the temperature raising process, the lithium sulfate particles undergo a large volume change under the conditions of this embodiment, causing fine cracks as shown in Fig. 3, and the reaction area becomes larger. This reduces the amount of lithium sulfate remaining unreacted. Since the lithium sulfate particles have fine cracks, it is not necessary to prepare lithium sulfate in a fine powder form.

[0023] [Cooling process] In the cooling step, after the heating step, the furnace is cooled to 200° C. or lower. In the cooling step, the heated furnace is naturally cooled.

[0024] After the cooling step, the lithium sulfide is removed from the furnace.

[0025] The preparation step, the heating step, and the cooling step may be carried out using, for example, a manufacturing apparatus 10 having a rotary kiln 11.

[0026] [Manufacturing equipment] The manufacturing apparatus 10 is an apparatus for manufacturing lithium sulfide by heating lithium sulfate as a raw material and activated carbon as a reducing agent in a furnace. The manufacturing apparatus 10 includes a rotary kiln 11, a material charging device 18, and a discharge pipe 24.

[0027] The rotary kiln 11 includes a kiln body 12, a heater 14, and a drive unit 16. The kiln body 12 is a cylindrical member. It is preferable that the central axis of the cylindrical shape of the kiln body 12 is inclined with respect to the horizontal direction so that the end on the material charging device 18 side is vertically higher than the other end. The heater 14 heats the kiln body 12.

[0028] The driving unit 16 rotates the kiln body 12 around the central axis of the cylindrical shape as the rotation axis. The driving unit 16 includes a driving source 30 and a transmission mechanism 32. The driving source 30 generates a rotational force such as a motor. The transmission mechanism 32 transmits the rotational force of the driving source 30 to the kiln body 12.

[0029] The material supply device 18 supplies lithium sulfate and activated carbon to the rotary kiln 11. The material supply device 18 includes a material storage section 21 and a supply pipe 22. The material storage section 21 stores lithium sulfate and activated carbon. The supply pipe 22 connects the material storage section 21 to the kiln body 12. The supply pipe 22 is connected to the upstream side of the transport path for lithium sulfate and activated carbon in the kiln body 12. The supply pipe 22 supplies lithium sulfate and activated carbon from the material storage section 21 to the kiln body 12.

[0030] The discharge pipe 24 is connected to an end of the kiln body 12 opposite to the end to which the supply pipe 22 is connected. The discharge pipe 24 is connected to the downstream side of the transport path for lithium sulfate and activated carbon in the kiln body 12. The discharge pipe 24 discharges lithium sulfide produced by passing through the kiln body 12.

[0031] In the manufacturing apparatus 10 configured as above, first, a predetermined molar ratio of lithium sulfate and activated carbon is charged from the material charging device 18 into the kiln body 12 of the rotary kiln 11. The lithium sulfate and reducing agent charged into the kiln body 12 are mixed. Then, in the temperature raising process, the kiln body 12 is rotated around the rotation axis by the driving unit 16 while being heated by the heater 14. The lithium sulfate and activated carbon supplied to the kiln body 12 move from the supply pipe 22 to the discharge pipe 24 along the conveying path by the rotation of the kiln body 12. The lithium sulfate and activated carbon moving along the conveying path are heated to a desired temperature by the heater 14. Since the lithium sulfate and activated carbon are not in the form of fine particles, scattering in the conveying path is suppressed. Then, in the cooling process, the heater 14 is stopped to cool the kiln body 12 and the lithium sulfide. Then, the manufactured lithium sulfide is discharged from the discharge pipe 24 and recovered.

[0032] [Effects of this embodiment] According to this embodiment, lithium sulfide can be produced by putting lithium sulfate and a reducing agent into one furnace and raising the temperature. In this embodiment, since it is not necessary to mix lithium sulfate used as a raw material into fine particles, an increase in the number of steps can be suppressed. When lithium sulfide is produced using a production apparatus 10 having a rotary kiln 11, scattering in the transport path can be suppressed, and a reduction in the amount of recovery can be suppressed. In this way, this embodiment can provide a method suitable for producing lithium sulfide using a production apparatus 10 having a rotary kiln 11.

[0033] In this embodiment, no toxic hydrogen sulfide gas is used in the manufacturing process, which makes it easier to manage the manufacturing process and ensures safety.

[0034] In the present embodiment, the manufacturing process uses lithium sulfate and a reducing agent, but does not use an organic solvent, thereby reducing costs.

[0035] In this embodiment, since it is not necessary to repeat the manufacturing process, the time required for manufacturing can be shortened and costs can be suppressed.

[0036] In this way, according to this embodiment, lithium sulfide can be more appropriately produced.

[0037] [Example] Next, a method for producing lithium sulfide will be described using a specific example. In a preparation step, 0.84 g of lithium sulfate monohydrate, which is a raw material, and 0.19 g of activated carbon, which is a reducing agent, were weighed in an inert atmosphere and mixed in a mortar. The weight loss of the lithium sulfate monohydrate used here when heated to 120°C is about 15%. The mixture of lithium sulfate monohydrate and activated carbon was placed in a crucible made of aluminum oxide.

[0038] After the preparation step, in the heating step, the crucible containing the mixture of lithium sulfate monohydrate and activated carbon was placed in a small muffle furnace and heated to 850°C in 10 minutes. The state of 850°C was maintained for 30 minutes.

[0039] After the heating step was completed, the inside of the muffle furnace was naturally cooled in the cooling step, and the sample was recovered.

[0040] The produced sample was crushed in an agate mortar, and then powder X-ray diffraction measurement was performed using a Burker D8ADVANCE device to evaluate the unreacted residue. In addition, 0.3 g of the crushed sample was filled into a conductivity measurement cell, and AC impedance measurement was performed in the measurement range of 1 Hz to 7 MHz at room temperature (25°C) with a pressure of 360 MPa applied.

[0041] In the examples, lithium sulfate monohydrate was used as the raw material. In the examples, activated carbon was used as the reducing agent. In the examples, the molar ratio of carbon to oxygen (C / O2) of the activated carbon was 1.2. In the examples, the temperature of the temperature increase step was 850°C. In the examples 1 to 3, the average particle size of the raw material was changed.

[0042] The average particle size of the raw material lithium sulfate monohydrate was categorized as "large" when it was between 80 μm and 100 μm, "medium" when it was between 30 μm and 50 μm, and "small" when it was 15 μm or less.

[0043] In the comparative examples, lithium sulfate anhydride was used as the raw material instead of lithium sulfate monohydrate. In the comparative examples, the same reducing agent as in the examples was used. In the comparative examples 1 to 5, the average particle size and temperature of the raw material were changed.

[0044] [Example 1] In Example 1, the average particle size of lithium sulfate monohydrate was set to “large.” The results of AC impedance measurement of the sample produced in Example 1 are shown in FIG.

[0045] [Example 2] In Example 2, the average particle size of lithium sulfate monohydrate was set to "medium". The measurement results of powder X-ray diffraction measurement of the sample produced in Example 2 are shown in Figure 4. The measurement results of AC impedance measurement of the sample produced in Example 2 are shown in Figure 5.

[0046] [Example 3] In Example 3, the average particle size of lithium sulfate monohydrate was set to “medium.” The measurement results of AC impedance measurement of the sample produced in Example 3 are shown in FIG.

[0047] [Comparative Example 1] In Comparative Example 1, the average particle size of the lithium sulfate anhydride was set to "large." In Comparative Example 1, the temperature in the heating step was set to 850°C. The weight loss of the lithium sulfate anhydride used in the Comparative Example when heated to 120°C was approximately less than 5%.

[0048] [Comparative Example 2] In Comparative Example 2, the average particle size of the lithium sulfate anhydride was set to "medium". In Comparative Example 2, the temperature in the heating step was set to 850°C. The measurement results of the powder X-ray diffraction measurement of the sample produced in Comparative Example 2 are shown in Figure 4. The measurement results of the AC impedance measurement of the sample produced in Comparative Example 2 are shown in Figure 5.

[0049] [Comparative Example 3] In Comparative Example 3, the average particle size of the lithium sulfate anhydride was set to "small." In Comparative Example 3, the temperature in the temperature increasing step was set to 850° C. The measurement results of the AC impedance measurement of the sample produced in Comparative Example 3 are shown in FIG.

[0050] [Comparative Example 4] In Comparative Example 4, the average particle size of the lithium sulfate anhydride was set to "small." In Comparative Example 4, the temperature in the temperature increasing step was set to 750°C.

[0051] [Comparative Example 5] In Comparative Example 5, the average particle size of the lithium sulfate anhydride was set to "small." In Comparative Example 5, the temperature in the temperature increasing step was set to 900°C.

[0052] The measurement results of the above-mentioned Examples 1, 2, 3, Comparative Examples 1, 2, 3, 4, and 5 are shown in Table 1 below. [Table 1]

[0053] FIG. 4 is a graph showing the test results of the examples, and is a graph showing the measurement results of the X-ray diffraction measurement. From Table 1, in Examples 1 to 3, no unreacted residue is observed. In Example 1, the unreacted residue is in the form of gray powder. In Examples 2 and 3, the unreacted residue is in the form of white powder. From FIG. 4, it can be seen that in Example 2, only the peak of lithium sulfide appears, and the peak of the raw material lithium sulfate does not appear. In Examples 1 and 3, the measurement results of the similar X-ray diffraction measurement are obtained. In Comparative Example 1, there is unreacted carbon residue, and it is black powder. In Comparative Example 2, there is a little unreacted carbon residue, and it is gray powder. In Comparative Example 3, there is no unreacted residue, and it is white powder. In Comparative Example 4, there is unreacted carbon residue, and it is black powder. In Comparative Example 5, there is no unreacted residue, but the sample is melted and lumpy. From these, the Examples can reduce the unreacted residue more than the Comparative Examples. In the examples, the smaller the average particle size of lithium sulfate monohydrate, the more the unreacted residue can be reduced. Comparative Example 3 has the same results as the examples, but requires a raw material fine-graining process. This test confirmed that when lithium sulfate monohydrate is used as a raw material, the unreacted residue can be reduced and lithium sulfide can be more appropriately produced.

[0054] FIG. 5 is a graph showing the test results of the examples, and is a graph showing the AC impedance measurement. From FIG. 5 and Table 1, in Examples 1 to 3, the AC impedance is small. In Comparative Example 2 and Comparative Example 3, since there is a little or no carbon remaining, the AC impedance can be measured, but it is inferior to Examples 1 to 3. In Comparative Example 1 and Comparative Example 4, since carbon remains, a short circuit occurs and the AC impedance cannot be measured. In Comparative Example 5, the molten sample adheres to the crucible and cannot be recovered by processing a small amount. As a result, the examples can have a higher ionic conductivity than the comparative examples. In the examples, the smaller the average particle size of lithium sulfate monohydrate, the higher the ionic conductivity can be. From this test, it was confirmed that when lithium sulfate monohydrate is used as a raw material, lithium sulfide with high ionic conductivity can be more appropriately produced.

[0055] From the above, in the method for producing lithium sulfide, by using lithium sulfate monohydrate whose average particle size falls within the range of "medium" or "small", lithium sulfate with a small amount of unreacted residue and high ionic conductivity can be obtained. From the above, it can be seen that by carrying out the production under the above-mentioned conditions, lithium sulfate with a desired ionic conductivity can be appropriately produced. [Explanation of symbols]

[0056] 10 Manufacturing equipment 11 Rotary Kiln 12 Kiln body (furnace) 14 Heater 16 Drive unit 18 Material feeding device 21 Material storage section 22 Supply pipe

Claims

1. A preparation step of charging a raw material containing lithium sulfate as a main component, the raw material having a characteristic of reducing by 5% to 25% by 120°C, and a reducing agent into a furnace; a temperature increasing step of heating the raw material and the reducing agent in the furnace to increase the temperature; Including, the reducing agent is a material containing carbon as a main component, The method for producing lithium sulfide, wherein a molar ratio of the raw material and the reducing agent charged into the furnace is 2 or more and 4 or less in terms of a C / Li 2 SO 4 ratio.

2. In the temperature increasing step, the mixed raw material and the reducing agent are heated. The method for producing lithium sulfide according to claim 1.

3. In the temperature increasing step, the temperature is increased to 700° C. or higher and 950° C. or lower in an inert atmosphere having a dew point of −60° C. The method for producing lithium sulfide according to claim 1 or 2.

4. In the temperature increasing step, the temperature is increased to 800°C or higher and 850°C or lower in an inert atmosphere having a dew point of -60°C. The method for producing lithium sulfide according to claim 1 or 2.

5. The temperature increasing step has a temperature increasing rate of 10° C. / min or more. The method for producing lithium sulfide according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Production of lithium sulfide

    JP1997110404A

  • Lithium ion conductive solid electrolyte and its manufacture

    JP1997283156A

  • Lithium sulfide particle powder, production method therefor and inorganic solid electrolyte

    JP2006151725A

  • Method for manufacturing lithium sulfide for solid electrolyte material of lithium ion battery

    JP2012221819A

  • Method for producing lithium sulfide

    JP2013227180A