Wood-based material and decorative material using same

By incorporating organic peroxide and alkoxysilane compounds in a thermoplastic resin composition, the mechanical strength and water resistance of wood base materials are enhanced, addressing the limitations of conventional adhesives.

JP7562984B2Active Publication Date: 2024-10-08TOPPAN HOLDINGS INC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020077529
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-04-24
Publication Date
2024-10-08
Estimated Expiration
2040-04-24

AI Technical Summary

Technical Problem

Conventional wood base materials using adhesives without formaldehyde face insufficient mechanical properties and water resistance, posing challenges for practical applications.

Method used

A wood base material is formed by heating and pressing a mixture of wood material and a thermoplastic resin composition containing organic peroxide, alkoxysilane compound, and optionally unsaturated dicarboxylic acid or acidic group-containing resin, enhancing mechanical strength and water resistance.

Benefits of technology

The solution provides wood base materials with improved mechanical strength and water resistance, suitable for practical use, as demonstrated by successful bending strength and reduced water absorption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562984000003
    Figure 0007562984000003
  • Figure 0007562984000004
    Figure 0007562984000004
  • Figure 0007562984000001
    Figure 0007562984000001
Patent Text Reader

Abstract

To provide a woody base material having superior mechanical strength and water resistance, and a decorative material using the woody base material.SOLUTION: A woody base material 20 is made by heating and pressurizing a raw material mixture 10 containing a powdery or chip-like woody material 11 and a powdery thermoplastic resin composition 12. The thermoplastic resin composition 12 contains a thermoplastic resin and 0.1-3 pts.mass of an organic peroxide based on 100 pts.mass of the thermoplastic resin, and the raw material mixture 10 contains 0.1-8 pts.mass of alkoxysilane compound based on the 100 pts.mass of the sum total of the woody material 11 and the thermoplastic resin composition 12. Further, the alkoxysilane compound may contain at least one of a vinyl group and a meth(acrylic) group, and the alkoxysilane compound may further contain at least one of an amino group, an epoxy group and a mercapto group, and the thermoplastic resin composition 12 may contain an unsaturated dicarboxylic acid.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a wood base material having excellent mechanical strength and water resistance, and a decorative material using the same. [Background technology]

[0002] Wood base materials are obtained by heating and pressurizing a mixture of wood materials such as wood flour, wood chips, and wood fiber with an adhesive. Depending on the type of wood material, they are called particle boards, medium-density fiberboards, etc., and are used for a wide range of applications, such as underlayment for floors and walls, as well as for building materials and furniture. Adhesives for wood substrates usually include urea resin adhesives, melamine resin adhesives, and phenol resin adhesives, together with hardeners containing formaldehyde. Formaldehyde is a harmful substance that causes sick house syndrome, so its emission from wood substrates is a problem, and although various measures to reduce the amount of formaldehyde emission have been considered, it is not possible to completely suppress it.

[0003] In response to this, a method has been proposed in the past in which a formaldehyde-free adhesive whose main components are powdered sugars and powdered polycarboxylic acids is used, and this is mixed with plant fibers and heated and pressurized to produce a fiberboard (see paragraph

[0017] of Patent Document 1). Furthermore, a method for producing a laminate including a wood base material using an adhesive made of polyvinyl alcohol and water has been proposed (see paragraph

[0017] and FIG. 1 of Patent Document 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2016-55620 A [Patent Document 2] Patent No. 5553279 Summary of the Invention [Problem to be solved by the invention]

[0005] However, the wood substrates using the above-mentioned conventional adhesives are not practically sufficient in terms of mechanical properties such as bending strength and water resistance. Therefore, an object of one aspect of the present invention is to provide a wood base material having excellent mechanical strength and water resistance, and a decorative material using the same. That is, as a result of intensive research aimed at solving the above-mentioned problems, one aspect of the present invention is that it was found that, in a wood base material formed by heating and pressurizing a powder mixture of a wood material and a thermoplastic resin composition, the above-mentioned problems can be solved by incorporating an organic peroxide into the thermoplastic resin composition and further incorporating an alkoxysilane compound into the powder mixture, thereby arriving at the present invention. [Means for solving the problem]

[0006] The wood substrate according to one embodiment of the present invention is formed by heating and pressurizing a raw material mixture containing a powdered or chipped wood material and a powdered thermoplastic resin composition, wherein the thermoplastic resin composition contains a thermoplastic resin and 0.1 to 3 parts by mass of an organic peroxide per 100 parts by mass of the thermoplastic resin, and the raw material mixture contains 0.1 to 8 parts by mass of an alkoxysilane compound per 100 parts by mass of the wood material and the thermoplastic resin composition in total. In addition, the wood substrate according to one embodiment of the present invention is characterized in that the alkoxysilane compound contains at least one of a vinyl group and a meth(acrylic) group.

[0007] In addition, a wood substrate according to one embodiment of the present invention is characterized in that the alkoxysilane compound further contains at least one of an amino group, an epoxy group, and a mercapto group. A wood substrate according to one embodiment of the present invention is characterized in that the thermoplastic resin composition contains an unsaturated dicarboxylic acid. A wood substrate according to one embodiment of the present invention is characterized in that the thermoplastic resin composition contains an acidic group-containing resin having at least one of a carboxy group and a structure formed by dehydration condensation of carboxy groups.

[0008] The wood base material according to one embodiment of the present invention is characterized in that the mass ratio of the wood material to the thermoplastic resin composition in the raw material mixture (wood material / thermoplastic resin composition) is 95 / 5 to 70 / 30. A wood base material according to one aspect of the present invention is characterized in that the wood material contains a mushroom bed as a raw material.

[0009] A decorative material according to one embodiment of the present invention is a wood base material formed by heating and pressurizing a raw material mixture containing a powdered or chipped wood material and a powdered thermoplastic resin composition, wherein the thermoplastic resin composition contains a thermoplastic resin and 0.1 to 3 parts by mass of an organic peroxide per 100 parts by mass of the thermoplastic resin, and the raw material mixture contains 0.1 to 8 parts by mass of an alkoxysilane compound per 100 parts by mass of the wood material and the thermoplastic resin composition in total, with a decorative substrate laminated on the wood base material. Effect of the Invention

[0010] According to one aspect of the present invention, it is possible to provide a wood base material having practical mechanical strength and water resistance, and a decorative material using the same. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a schematic diagram of a raw material mixture for a wood base material according to a first embodiment of the present invention. [Diagram 2] FIG. 4 is a cross-sectional view of a decorative material according to a second embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] (First embodiment shown in FIG. 1) In FIG. 1, reference numeral 20 denotes a wood base material according to a first embodiment of the present invention. Depending on the type of wood material 11, it is called a particle board, a medium density fiberboard, or the like, and is used for a wide range of applications, such as underlayment for floors and walls, fittings, and furniture. As shown in FIG. 1, the wood base material 20 is formed by heating and pressurizing a raw material mixture 10 containing a powdered or chipped wood material 11 and a powdered thermoplastic resin composition 12 . The thermoplastic resin composition 12 contains a thermoplastic resin and an organic peroxide.

[0013] The raw material mixture 10 contains an alkoxysilane compound. That is, the form of the raw material mixture 10 includes at least one of the following forms. (1) A mixture of a wood material 11, a thermoplastic resin composition 12, and an alkoxysilane compound (2) A mixture of a wood material 11 and a thermoplastic resin composition 12 containing an alkoxysilane compound.

[0014] (Wood material 11) Examples of the wood material 11 include wood powder, wood fiber, and wood crushed into chips, and raw materials that can be used include thinned wood, sawdust, waste wood, etc. In addition to wood, other candidates include bamboo, hemp, coconut fiber, walnut shells, and other materials that contain cellulose components like wood. Used mushroom beds, which are generated in large quantities during mushroom cultivation, can be suitably used as the raw material for the wood material 11. The mushroom beds are made by mixing wood chips and sawdust with nutrients such as bran and rice bran. It is estimated that around 300,000 tons of mushroom beds are discarded annually in Japan after mushroom cultivation, making them a promising source of biomass, but recycling is currently not progressing, and using them as a wood raw material is beneficial in reducing the environmental burden.

[0015] (thermoplastic resin) The thermoplastic resin contained in the thermoplastic resin composition 12 can be various types such as polyester, polyamide, polyolefin, ethylene-propylene-diene rubber, ethylene vinyl acetate, and silicone rubber, but polyethylene is preferred in terms of the mechanical strength and water resistance of the wood substrate. The polyethylene resin is not particularly limited, and may be appropriately selected from existing materials such as high density polyethylene, low density polyethylene, very low density polyethylene, and linear low density polyethylene, taking into consideration reactivity and fluidity when heated and pressurized.

[0016] (organic peroxide) The organic peroxide contained in the thermoplastic resin composition 12 is used to radically crosslink the thermoplastic resin when the raw material mixture is heated and pressurized, and can be appropriately selected from existing materials such as peroxyketals, dialkyl peroxides, diacyl peroxides, and peroxy esters, taking into consideration their reactivity and stability. The amount of the organic peroxide added is 0.1 to 3 parts by mass with respect to 100 parts by mass of the thermoplastic resin. If the amount added is less than 0.1 parts by mass, the raw material mixture will not be sufficiently reactive when heated and pressurized, and the wood base material will not have sufficient strength. If the amount added is more than 3 parts by mass, the amount of decomposition products produced during the reaction will increase, which may cause deformation of the wood base material, and is therefore undesirable.

[0017] (Thermoplastic resin composition 12) By blending a radically polymerizable material into the thermoplastic resin composition 12, it may be possible to chemically bond the material to the thermoplastic resin when the base material is formed. For example, by bonding an unsaturated dicarboxylic acid such as maleic acid, the mechanical strength of the wood base material 1 can be further improved.

[0018] Furthermore, by blending the thermoplastic resin composition 12 with an acidic group-containing resin having at least one carboxy group or a structure formed by dehydration condensation of carboxy groups, the mechanical strength of the wood substrate 1 can be further improved. Examples of the acidic group-containing resin that can be used include maleic anhydride-modified polyolefins such as maleic anhydride-modified polyethylene and maleic anhydride polypropylene, and ethylene (meth)acrylic acid copolymers.

[0019] (Unsaturated dicarboxylic acid) The unsaturated dicarboxylic acid is used to improve the adhesion between the wood material 11 and the thermoplastic resin, and preferably contains at least one of fumaric acid, maleic acid, and maleic anhydride. The amount of unsaturated dicarboxylic acid added is 0.01 to 3 parts by mass relative to 100 parts by mass of thermoplastic resin. If the amount added is less than 0.01 part by mass, the adhesion between the thermoplastic resin and the wood material 11 is insufficient, and sufficient strength cannot be obtained for the wood substrate 1. If the amount added is more than 3 parts by mass, unreacted unsaturated dicarboxylic acid is likely to remain in the wood substrate, which may cause odor and reduced water resistance, and is therefore undesirable. The thermoplastic resin composition 12 containing an organic peroxide and an unsaturated dicarboxylic acid can be prepared by various known methods. For example, the organic peroxide and the unsaturated dicarboxylic acid can be heated and kneaded together with a thermoplastic resin using a single-axis kneader or a batch kneader, and then powdered by a method such as mechanical crushing or freeze-crushing.

[0020] (Acidic group-containing resin) The acidic group-containing resin is a resin containing at least one of carboxylic acid and carboxylic acid anhydride in order to improve the adhesion between the wood material 11 and the thermoplastic resin. Specific examples include maleic anhydride-modified polyolefins such as maleic anhydride-modified polyethylene and maleic anhydride polypropylene, and ethylene (meth)acrylic acid copolymers. The amount of the acidic group-containing resin added is 1 to 50 parts by mass per 100 parts by mass of the thermoplastic resin. If the amount added is less than 1 part by mass, the adhesion between the thermoplastic resin and the wood material 11 will be insufficient, making it impossible to obtain sufficient strength for the wood substrate 1. If the amount added is more than 50 parts by mass, the strength will often decrease, which is not preferable. The thermoplastic resin composition 12 containing an organic peroxide and an acidic group-containing resin can be prepared by various known methods. For example, the organic peroxide and the acid-containing resin can be heated and kneaded together with the thermoplastic resin using a single-screw kneader or a batch kneader, and then powdered by a method such as mechanical crushing or freeze-crushing.

[0021] (Alkoxysilane compounds) The alkoxysilane compound is used to improve the mechanical strength of the wood substrate 1, and examples of the alkoxysilane compound include methyltrimethoxysilane, tetramethoxysilane, methyltriethoxysilane, tetraethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, and 3-acryloxypropyltrimethoxysilane. , N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-isocyanatopropyltriethoxysilane, 3-trimethoxysilylpropylsuccinic anhydride, and the like. Examples of the "vinyl group"-containing processed material include vinyltrimethoxysilane and vinyltriethoxysilane. Furthermore, examples of the "(meth)acrylic group"-containing processed products include 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, and 3-acryloxypropyltrimethoxysilane.

[0022] The alkoxysilane compound includes a state where at least a part of the alkoxy group is hydrolyzed or partially condensed. For example, known materials such as alkoxysilane hydrolyzates and condensates called oligomers or resins can be used, but they may be subjected to hydrolysis treatment before being mixed into the raw material mixture 10.

[0023] From the viewpoint of mechanical strength of wood substrates, the alkoxysilane compound is preferably a compound having a vinyl group or a (meth)acrylic group, and more preferably, the compound is used in combination with at least one of alkoxysilane compounds containing an amino group, an epoxy group, and a mercapto group. The compounds containing the vinyl group, the (meth)acrylic group, the amino group, the epoxy group, and the mercapto group can be, for example, the various known materials described above.

[0024] (Amount of alkoxysilane compound) The amount of the alkoxysilane compound is 0.1 to 8 parts by mass per 100 parts by mass of the raw material mixture 10. If the amount added is less than 0.1 part by mass, sufficient strength cannot be obtained for the wood substrate 1. If the amount added exceeds 8 parts by mass, the strength and water resistance of the wood substrate often decrease, which is not preferable.

[0025] (Mass ratio of wood material 11 to thermoplastic resin composition 12) The mass ratio of the wood material 11 to the thermoplastic resin composition 12 is in the range of 95 / 5 to 70 / 30 (wood material / thermoplastic resin composition). If the content of the wood material is greater than this range, sufficient bending strength cannot be imparted to the wood base material 1. On the other hand, if the content of the wood material is less than this range, the wood base material is likely to deform when heated and pressed, which is not preferable.

[0026] (Method for producing thermoplastic resin composition 12) The thermoplastic resin composition 12 can be prepared by various known methods. For example, a single-axis kneader or a batch kneader can be used to heat and knead a thermoplastic resin together with an organic peroxide and (if necessary) an alkoxysilane compound, and then the mixture can be powdered by mechanical crushing, freeze-pulverization, or other methods.

[0027] (Method of heating and pressurizing raw material mixture 10) Various known methods can be used for heating and pressurizing the raw material mixture 10, but press molding using a mold is preferred. The heating temperature is usually 120°C to 250°C, and must be equal to or higher than the melting point of the thermoplastic resin. If the temperature exceeds 250°C, significant thermal deterioration of the wood material 11 may occur. The pressing pressure is usually 10 kgf / cm. 2 ~400kgf / cm 2 and the value is appropriately set according to the desired density of the wood base material. The density and shape of the wood substrate 1 obtained above are appropriately determined depending on the application. The density is preferably 0.5 to 1.2 g / cm 3 , especially 0.6 to 1.1 g / cm 2 is preferred.

[0028] (Second embodiment shown in FIG. 2) The second embodiment will be described with reference to FIG. The second embodiment is characterized in that a decorative material 30 is formed by laminating a designable base material 31 having design properties onto the wood base material 20 according to the first embodiment described above with reference to Figure 1. According to the second embodiment, by laminating the decorative base material 31 on the wood base material 20, a decorative feature can be imparted. In other words, the wood base material 20 can be used as a decorative material by itself, but in order to impart a design, a decorative base material 31 such as paper or film with a design such as a picture is laminated onto the wood base material 20 to form the decorative material 30, as shown in Figure 2. EXAMPLES

[0029] Below, examples 1 to 8 and comparative examples 1 to 4 of the wood base material according to the first embodiment of the present invention will be explained. Note that the present invention is not limited to the following examples 1 to 8.

[0030] Example 1 In Example 1, 100 parts by weight of low-density polyethylene resin (hereinafter also referred to as "LDPE") and 1.5 parts by weight of an organic peroxide (product name: Perhexa C, manufactured by NOF Corporation, hereinafter also referred to as "PO") were heated and kneaded in a batch kneader, and then mechanically pulverized to obtain a powdered thermoplastic resin composition. The wood material is made from mushroom beds that have been washed and dried after harvesting. As the alkoxysilane compound, a methacryloxy group-containing silane (3-methacryloxypropyltrimethoxysilane, product name KBM503, manufactured by Shin-Etsu Chemical Co., Ltd., hereinafter also referred to as "KBM503") and an amino group-containing silane (3-aminopropyltrimethoxysilane, product name KBM903, manufactured by Shin-Etsu Chemical Co., Ltd., hereinafter also referred to as "KBM903") are used. The wood material / thermoplastic resin composition / KBM503 / KBM903 were mixed in a mass ratio of 85 / 15 / 1 / 1 to obtain a raw material mixture for the wood base material. The composition of the raw material mixture is as shown in Table 1 below.

[0031] [Table 1]

[0032] This raw material mixture was introduced into an aluminum mold and heated and pressed with a heat press to obtain a wood substrate (pressing conditions: 100 kgf / cm 2 , 200℃ 10 minutes, base material thickness: 10 mm, base material density: 0.7 g / cm 3 ).

[0033] Example 2 In Example 2, the amino group-containing silane in Example 1 was replaced with an epoxy group-containing silane (3-glycidoxypropyltrimethoxysilane, product name KBM403, manufactured by Shin-Etsu Chemical Co., Ltd., hereinafter also referred to as "KBM403"), and otherwise a wood base material was obtained in the same manner as in Example 1.

[0034] Example 3 In Example 3, the amino group-containing silane in Example 1 was replaced with a mercapto group-containing silane (3-mercaptopropyltrimethoxysilane, product name KBM803, manufactured by Shin-Etsu Chemical Co., Ltd., hereinafter also referred to as "KBM803"), and otherwise a wood base material was obtained in the same manner as in Example 1.

[0035] Example 4 In Example 4, 1 part by mass of maleic anhydride powder (product name CRYSTAL MAN, manufactured by NOF Corporation, hereinafter also referred to as "MA") was added to the components of the thermoplastic resin composition of Example 1, and otherwise a wood base material was obtained in the same manner as in Example 1.

[0036] Example 5 In Example 5, the amino group-containing silane (KBM903) of Example 1 was not used, and the mass ratio of wood material / thermoplastic resin composition / KBM503 was 85 / 15 / 2. Otherwise, a wood base material was obtained in the same manner as in Example 1.

[0037] Example 6 In Example 6, tetraethoxysilane oligomer was used as the alkoxysilane compound in Example 1, and the mass ratio of wood material / thermoplastic resin composition / alkoxysilane compound was 85 / 15 / 5. Otherwise, a wood base material was obtained in the same manner as in Example 1.

[0038] Example 7 In Example 7, the amino group-containing silane (KBM903) of Example 1 was not used, and the mass ratio of wood material / thermoplastic resin composition / KBM503 was 85 / 15 / 0.1. Otherwise, a wood base material was obtained in the same manner as in Example 1.

[0039] Example 8 In Example 8, the amino group-containing silane (KBM903) of Example 1 was not used, and the mass ratio of wood material / thermoplastic resin composition / KBM503 was 85 / 15 / 8. Otherwise, a wood base material was obtained in the same manner as in Example 1.

[0040] Comparative Example 1 In Comparative Example 1, a wood base material was obtained in the same manner as in Example 1, except that the alkoxysilane compound of Example 1 was not used.

[0041] Comparative Example 2 In Comparative Example 2, a wood base material was obtained in the same manner as in Example 1, except that the organic peroxide in Example 1 was not used.

[0042] Comparative Example 3 In Comparative Example 3, a wood base material was obtained in the same manner as in Example 1, except that the mass ratio of wood material / thermoplastic resin composition / KBM503 / KBM903 in Example 1 was changed to 85 / 15 / 5 / 5.

[0043] Comparative Example 4 In Comparative Example 4, a wood base material was obtained in the same manner as in Example 1, except that the amount of organic peroxide used in Example 1 was changed to 5 parts by mass.

[0044] (Evaluation of wood-based materials) The physical properties of the wood substrate were evaluated based on the following three points: (1) mechanical strength, (2) water resistance, and (3) substrate deformation.

[0045] (Mechanical strength) The mechanical strength was measured by bending strength according to the method of JISA5908. Measured value (unit: N / mm 2 The evaluation criteria for mechanical strength for the above-mentioned materials are as follows, based on the JIS standard values: The mechanical strength was evaluated based on the following four-level scale: "◎", "○", "△", and "×". "◎", "○", and "△" were considered pass, and "×" was considered fail. Note (1)◎:18 or above (pass) (2)○:13 or higher (pass) (3) △: 8 or more but less than 13 (pass) (4) ×: Less than 8 (Failed)

[0046] (water resistance) The water resistance was measured by measuring the water absorption thickness swelling rate according to a method in accordance with JISA5908. The evaluation criteria for water resistance for the measured values ​​(unit: %) are as follows, based on the JIS standard values. The evaluation criteria for water resistance were as follows: 3 levels: "○", "△", and "×". "○" and "△" were considered pass, and "×" was considered fail. Note (1)○: Less than 8 (pass) (2) △: 8 or more but less than 12 (pass) (3) ×: 12 or more (fail)

[0047] (Substrate deformation) The substrate deformation is a state in which the substrate surface is partially swollen, and is mainly caused by the retention of gas generated inside the substrate during pressing. Since the deformation of the substrate is clearly reflected by the state of the substrate edge, the appearance of the substrate edge was visually evaluated. The evaluation criteria were as follows: The evaluation criteria for substrate deformation were as follows: 3 levels of "○", "△", and "×", with "○" and "△" representing pass and "×" representing fail. Note (1) ○: No voids (passed) (2) △: Traces of voids (passed) (3) ×: Voids present (failed)

[0048] (Evaluation Results) The evaluation results of the wood-based substrates are as shown in Table 2 below.

[0049] [Table 2]

[0050] Eight of Examples 1 to 8 were "passed" in all three physical property evaluations, while the remaining four of Comparative Examples 1 to 4 included one or more failures.

[0051] (Mechanical strength evaluation results) Comparative Examples 1 to 3 were the three cases in which the mechanical strength did not meet the criteria. It is presumed that the cause of the failure in Comparative Example 1 is that an alkoxysilane compound was not used. It is presumed that the cause of the failure in Comparative Example 2 is that an organic peroxide was not used. It is presumed that the cause of the failure in Comparative Example 3 is that the total amount of the alkoxysilane compound, KBM503 and KBM903, added was too large.

[0052] (Water resistance evaluation results) Comparative Example 3 was the only sample that failed the water resistance test. In Comparative Example 3, it is presumed that the reason for this is that the total amount of the alkoxysilane compounds, KBM503 and KBM903, added was too large.

[0053] (Evaluation results of substrate deformation) Comparative Examples 3 and 4 were the two cases in which the deformation of the substrate was unacceptable. It is presumed that the cause of the problem in Comparative Example 3 was that the total amount of alkoxysilane compounds, KBM503 and KBM903, was too large.It is presumed that the cause of the problem in Comparative Example 4 was that the amount of organic peroxide, Perhexa-C (PO), was too large.

[0054] (Overall evaluation results) As a comprehensive evaluation result, all three physical property evaluations for Examples 1 to 8 were "passed." As is clear from Table 2, it was shown that the wood base material of the present invention has excellent mechanical strength and water resistance, and there is no problem with substrate deformation. Comparing Examples 1 to 8, the evaluation result of the mechanical strength in Example 4 was "A". It is presumed that this was due to the addition of 1 part by mass of maleic anhydride powder (MA) in Example 4. Moreover, among Examples 1 to 8, four cases (Examples 5 to 8) were given a "△" evaluation result for mechanical strength. This is presumably because Examples 5 to 8 did not use an amino group-containing silane (KBM903) or the like. The evaluation result of water resistance was "△" for two cases, Example 6 and Example 8. In Example 6, it is presumed that the cause is the use of tetraethoxysilane oligomer as the alkoxysilane compound. Also, in Example 6, it is presumed that the cause is the increase in the ratio of the alkoxysilane compound. The evaluation result of the substrate deformation was "△" in one case, which was Example 6. It is presumed that the cause of this in Example 6 was the use of tetraethoxysilane oligomer as the alkoxysilane compound. [Explanation of symbols]

[0055] 10 Raw material mixture 11 Wood materials 12 Thermoplastic resin composition 20 Wood base material 30 Cosmetic materials 31 Designable substrates

Claims

1. A wood substrate formed by heating and pressurizing a raw material mixture containing a powdered or chipped wood material and a powdered thermoplastic resin composition, The thermoplastic resin composition comprises a thermoplastic resin and 0.1 to 3 parts by mass of an organic peroxide per 100 parts by mass of the thermoplastic resin, The raw material mixture contains 0.1 to 8 parts by mass of an alkoxysilane compound per 100 parts by mass of the total of the wood material and the thermoplastic resin composition, the alkoxysilane compound contains a meth(acrylic) group, The thermoplastic resin composition contains a polyethylene resin as the thermoplastic resin and does not contain an unsaturated dicarboxylic acid, The wood base material is characterized in that the organic peroxide is 1,1-di-(t-butylperoxy)cyclohexane.

2. 2. The wood base material according to claim 1, wherein the alkoxysilane compound further contains at least one of an amino group, an epoxy group, and a mercapto group.

3. 2. The wood base material according to claim 1, wherein the alkoxysilane compound further contains at least one of an epoxy group and a mercapto group.

4. The wood substrate according to any one of claims 1 to 3, characterized in that the thermoplastic resin composition contains an acidic group-containing resin having at least one of a carboxy group and a structure in which carboxy groups are dehydrated and condensed together.

5. 5. The wood base material according to claim 4, wherein the acidic group-containing resin is a maleic anhydride modified polyolefin or an ethylene (meth)acrylic acid copolymer.

6. 6. The wood base material according to claim 5, wherein the amount of the acidic group-containing resin added is 1 to 50 parts by mass per 100 parts by mass of the thermoplastic resin.

7. The wood base material according to any one of claims 1 to 6, characterized in that in the raw material mixture, a mass ratio of the wood material to the thermoplastic resin composition (wood material / thermoplastic resin composition) is 95 / 5 to 70 / 30.

8. A wood substrate formed by heating and pressurizing a raw material mixture containing a powdered or chipped wood material and a powdered thermoplastic resin composition, The thermoplastic resin composition comprises a thermoplastic resin and 0.1 to 3 parts by mass of an organic peroxide per 100 parts by mass of the thermoplastic resin, The raw material mixture is a wood substrate containing an alkoxysilane compound in an amount of 0.1 to 8 parts by mass per 100 parts by mass of the wood material and the thermoplastic resin composition, and a decorative substrate is laminated on the wood substrate; The alkoxysilane compound contains a meth(acrylic) group, The thermoplastic resin composition contains a polyethylene resin as the thermoplastic resin and does not contain an unsaturated dicarboxylic acid, The decorative material is characterized in that the organic peroxide is 1,1-di-(t-butylperoxy)cyclohexane.

Citation Information

Patent Citations

  • Guanidine derivative*its manufacture and pharmaceutic composition containing it and having secretion controlling activity

    JP1980053279A

  • Manufacture of lightweight wooden product

    JP1989171801A

  • Particle board and its production

    JP1997267311A

  • Manufacture of composite pellet and composite molded item

    JP2001062901A

  • Method and apparatus for manufacturing wood / Plastic composite material

    JP2002144399A