Optical sensor device and method for manufacturing optical sensor device
The graphene-based optical sensor device with periodic holes and ALD coating addresses sensitivity and environmental stability issues, enabling broadband infrared detection at room temperature with enhanced weather resistance.
Patent Information
- Application Number
- JP2021001497
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-07
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2041-01-07
AI Technical Summary
Existing infrared sensors face challenges in achieving broadband, high-sensitivity operation at room temperature due to environmental fluctuations and sensitivity issues, particularly with graphene-based sensors experiencing changes in electrical properties and moisture intrusion.
A graphene-based optical sensor device with periodic holes and a protective layer covered by an atomic layer deposition (ALD) thin film, which enhances light absorption and maintains stable operation by preventing moisture intrusion and peeling, using a back gate transistor configuration.
The device achieves broadband, high-sensitivity infrared detection at room temperature with improved weather resistance and reliability by stabilizing the Dirac point, reducing environmental sensitivity.
Smart Images

Figure 0007563184000001 
Figure 0007563184000002 
Figure 0007563184000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to optical sensor devices and methods for manufacturing optical sensor devices. [Background technology]
[0002] Infrared sensors detect infrared rays emitted by hot objects and are used in automatic doors, security cameras, infrastructure inspections, etc. Infrared sensors using compound semiconductors have been developed and manufactured as quantum infrared sensors that generate an amount of charge according to the incident light. Quantum type sensors can be made sensitive to infrared light in a certain wavelength range by controlling the combination, composition, film thickness, etc. of semiconductor materials. Quantum type infrared sensors are used at extremely low temperatures of 60K to 100K to suppress the effects of thermal noise, and require a cooling device.
[0003] Thermal infrared detectors, which detect resistance changes by utilizing the temperature change caused by heat when infrared rays are received, can be used at room temperature, but their sensitivity is inferior to that of quantum infrared sensors. A graphene infrared detector based on hot carrier generation using plasmons has been proposed (for example, see Non-Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-130669 A [Non-patent literature]
[0005] [Non-Patent Document 1] Alireza Sataei, et al., 'Dirac plasmon-assisted asymmetric hot carrier generation for room-temperature infrared detection', Nat. Comm., 10, 3498 (2019) Summary of the Invention [Problem to be solved by the invention]
[0006] The wavelength range of infrared light is wide, and there is a demand for a broadband, highly sensitive sensor that operates at room temperature. An object of the present disclosure is to provide a broadband, highly sensitive optical sensor device that operates at room temperature, and a method for manufacturing the same. [Means for solving the problem]
[0007] In one embodiment of the present disclosure, an optical sensor device includes a graphene layer disposed on a substrate, a pair of electrodes electrically connected to the graphene layer, and a resin protective layer covering the graphene layer; The graphene layer is provided with periodic holes, the protective layer is provided with periodic openings communicating with the holes; The side surface of the hole and the inner wall of the opening are continuously covered with an insulating thin film. Effect of the Invention
[0008] A broadband, highly sensitive optical sensor device that operates at room temperature is realized. [Brief description of the drawings]
[0009] [Figure 1] FIG. 2 is a schematic plan view of the optical sensor device according to the embodiment. [Diagram 2] FIG. 2 is a schematic cross-sectional view taken along line II' in FIG. [Figure 3A] 1A to 1C are diagrams illustrating a manufacturing process of an optical sensor device. [Figure 3B] 5A to 5C are diagrams illustrating a manufacturing process of the light-receiving element substrate according to the embodiment. [Figure 3C] 5A to 5C are diagrams illustrating a manufacturing process of the light-receiving element substrate according to the embodiment. [Figure 3D] 5A to 5C are diagrams illustrating a manufacturing process of the light-receiving element substrate according to the embodiment. [Figure 3E] 5A to 5C are diagrams illustrating a manufacturing process of the light-receiving element substrate according to the embodiment. [Figure 3F]5A to 5C are diagrams illustrating a manufacturing process of the light-receiving element substrate according to the embodiment. [Figure 3G] 5A to 5C are diagrams illustrating a manufacturing process of the light-receiving element substrate according to the embodiment. [Figure 3H] 5A to 5C are diagrams illustrating a manufacturing process of the light-receiving element substrate according to the embodiment. [Figure 3I] 5A to 5C are diagrams illustrating a manufacturing process of the light-receiving element substrate according to the embodiment. [Figure 4] 13 is a modified example of the optical sensor device. [Diagram 5] FIG. 1 is a diagram illustrating the need for improving weather resistance. [Figure 6] FIG. 1 illustrates the effect of an ALD layer. [Figure 7] FIG. 1 illustrates the effect of an ALD layer. [Figure 8] FIG. 1 illustrates the effect of an ALD layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] In the embodiment, graphene is used in the light receiving layer to enable infrared detection in a wide wavelength range. Graphene is a two-dimensional material in which carbon atoms are arranged in a two-dimensional honeycomb shape, and has high mobility and absorbs light in a wide wavelength band. This is due to the characteristic energy band structure of graphene. A problem with graphene optical sensors is the change in electrical characteristics due to the environment. Moisture on the device surface, etc., causes fluctuations in the Dirac point, that is, the gate voltage at which the drain current is minimized. Another problem is that when graphene is microfabricated, excessive graphene is removed, causing peeling and moisture intrusion, resulting in deterioration of the sensor characteristics. As will be described later, in the embodiment, these problems are solved to realize a wide-band, high-sensitivity optical sensor device that operates stably.
[0011] The conduction and valence bands of graphene can be modeled as symmetric cones whose vertices meet at the Dirac point (K or K' in wave number space). Because the conduction and valence bands intersect at the Dirac point and have no band gap, graphene absorbs light over a wide wavelength range. Three of the four electrons in a graphene carbon atom are bonded to adjacent atoms, while the fourth electron is in an orbit extending perpendicular to the graphene plane and moves rapidly within the graphene plane as a free electron.
[0012] Fig. 1 is a schematic plan view of an optical sensor device 10 according to an embodiment, and Fig. 2 is a schematic cross-sectional view taken along line I-I' in Fig. 1. In the optical sensor device 10, a graphene layer 15 having a periodic arrangement of holes 151 is disposed on an insulating film 12 on a substrate 11. When a silicon substrate is used as the substrate 11, the insulating film 12 may be a thermal oxide film or may be another insulating film such as a silicon nitride film or aluminum oxide.
[0013] In the optical sensor device 10, by providing holes 151 in the graphene layer 15, the absorption of light during reception can be increased. When light is incident, plasmons, i.e., collective oscillations of free electrons caused by the incident light, are excited on the surface of the graphene layer 15. In the vicinity of the edge of the hole 151, the oscillating electric field of light is strongly confined, and light absorption is greater than that of a graphene film without the hole 151. In other words, the detection sensitivity for incident light can be improved. The hole 151 does not necessarily have to completely penetrate the graphene and reach the insulating film 12.
[0014] A pair of electrodes 14a and 14b are disposed on both ends of the graphene layer 15 so as to overlap the graphene layer 15. One of the electrodes 14a and 14b is a source electrode, and the other is a drain electrode. Electrode pads 16a and 16b are connected to the electrodes 14a and 14b, respectively, so that the current flowing through the graphene layer 15 can be detected from the outside. A gate electrode 19 is provided on the back surface of the substrate 11, i.e., the surface opposite to the electrodes 14a and 14b, forming a back-gate type transistor configuration.
[0015] The surface of the graphene layer 15 is covered with a protective layer 21. Periodic openings 22 corresponding to the holes 151 of the graphene layer 15 are also formed in the protective layer 21. The openings 22 in the protective layer 21 communicate with the holes 151 in the graphene layer 15. The surface of the protective layer 21 and the inner walls of the openings 22, as well as the side surfaces of the holes 151 in the graphene layer 15, are covered with a thin film 25 formed by an atomic layer deposition (ALD) method. The ALD method allows the film thickness to be controlled at the atomic layer level, making it possible to form a thin and dense film. Hereinafter, the thin film 25 will be referred to as an "ALD layer 25" after the film formation method.
[0016] The ALD layer 25 fills the gap between the graphene layer 15 and the protective layer 21, improving the weather resistance of the device. Weather resistance generally refers to the ability to withstand the outdoor natural environment and its changes. In the case of the optical sensor device 10, weather resistance includes the ability to suppress the variation of the Dirac point even when the environment in which the optical sensor device 10 is used changes.
[0017] The protective layer 21 is also used to improve weather resistance. When a resist mask used for forming holes 151 in the graphene layer 15 is used as the protective layer 21, gaps may occur between the graphene layer 15 and the protective layer 21 due to the hydrophobic nature of the graphene layer 15. Such gaps may cause peeling or moisture intrusion, affecting the characteristics of the sensor. By covering the side surfaces of the holes 151 in the graphene layer 15 and the inner walls of the openings 22 in the protective layer 21 with the ALD layer 25, peeling and moisture intrusion are prevented. This suppresses the fluctuation of the Dirac point to a small value, as described later.
[0018] During operation, a constant bias voltage is applied between the source and drain electrodes 14a and 14b to observe the change in current (i.e., change in resistance) flowing through the graphene layer 15. The change in current is proportional to the amount of light absorption. By applying a gate voltage to the gate electrode 19, the carrier density of electrons, holes, etc. in the graphene layer 15 is controlled. The physical properties of graphene, such as light absorption characteristics, resistivity, and Seebeck coefficient, are affected by the carrier density of graphene. The light absorption characteristics of the optical sensor device 10 are optimally controlled by the gate voltage.
[0019] By applying a voltage between electrodes 14a and 14b, an electric field is applied to graphene layer 15, and electron-hole pairs generated by infrared light irradiated from above the device flow through the graphene layer. This drain current can be controlled by the gate voltage. If a gate voltage is applied that minimizes the drain current when the light is off, the drain current-gate voltage characteristics will shift due to light irradiation. The drain current increases due to the incidence of light, and by detecting this, the incidence of light can be detected.
[0020] The optical sensor device 10 operates at room temperature and detects a wide wavelength band of light (including visible and infrared light) by using the graphene layer 15. The periodic holes 151 in the graphene layer 15 enhance light absorption and improve sensitivity. Furthermore, the ALD layer 25 enhances weather resistance and maintains reliable device operation.
[0021] 3A to 3I are diagrams showing the manufacturing process of the optical sensor device 10. The process shown in Fig. 3A to 3I is one example of the process for manufacturing the optical sensor device 100, and is not limited to the materials, parameters, etc. described below.
[0022] In Fig. 3A, for example, a silicon substrate with a thermal oxide film is prepared. The silicon substrate is used as substrate 11, and the thermal oxide film is used as insulating film 12. A metal layer is formed on the surface (back surface) of substrate 11 opposite insulating film 12 by electron beam (EB) deposition, forming gate electrode 19 which serves as a back gate. The metal layer to be formed may be a two-layer structure of titanium (Ti) and gold (Au).
[0023] In FIG. 3B, a graphene layer 15 is provided on the entire surface of the insulating film 12. The graphene layer 15 may be disposed on the insulating film 12 by a mechanical peeling method, a transfer method, or the like. Alternatively, a catalyst metal may be deposited on the insulating film 12 by sputtering, and graphene may be grown directly on the insulating film 12 by a CVD method. The graphene layer 15 may be a single-layer graphene or a layer having a thickness of several atomic layers. After providing the graphene layer 15, annealing may be performed at a temperature of 150 to 200° C. to enhance adhesion between the insulating film 12 and the graphene.
[0024] 3C, the graphene layer 15 is patterned into a predetermined shape. Graphene can be processed by oxygen ashing, oxygen ion beam, or the like.
[0025] In FIG. 3D, a pair of electrodes 14a and 14b are formed to be electrically connected to the processed graphene layer 15. The electrodes 14a and 14b are formed of a good conductor such as Au or palladium (Pd). Au has good electrical conductivity but is easily peeled off, so a film of Ti or chromium (Cr) may be formed as an undercoat for the Au film to improve adhesion to the undercoat. In this case, it is desirable to make the thickness of the undercoat metal film as thin as possible in order to maintain the electrical conductivity as high as possible.
[0026] In FIG. 3E, a protective layer 21 is formed on the entire surface. The protective layer 21 may be made of a resin that is transparent in the wavelength region of the light to be detected and has a low dielectric constant that allows patterning by EB drawing. Such a resin may be an acrylic resin, polymethyl methacrylate (PMMA), hydrogen silsesquioxane (HSQ), or the like. Alternatively, a plurality of types of these may be superimposed. For example, the protective layer 21 may be formed by applying HSQ onto a PMMA layer. The thickness of the protective layer 21 is 1 to several μm.
[0027] In Fig. 3F, the protective layer 21 is processed into a predetermined shape. The protective layer 21 may be processed by exposure and development. An opening 22 is formed in the processed protective layer 21 by EB drawing, and a part of the graphene layer 15 is exposed in the opening 22. The diameter of the opening 22 is 200 to 400 nm.
[0028] In FIG. 3G, holes 151 are formed in the graphene layer 15 by ion beam etching using the protective layer 21 having the openings 22 as a mask. Using an ion beam shower device, ion beam irradiation for 10 seconds is repeated several times with 10 second intervals. The number of times is determined by the thickness of the graphene. By using ion beam etching, the graphene layer 15 can be selectively etched and the graphene layer 15 in the part covered by the protective layer 21 can be maintained. In oxygen ashing, which is generally used to remove resin, the graphene layer 15 under the protective layer 21 is also etched. By using ion beam etching, the graphene layer 15 in the area other than the hole 151 is maintained and the current flowing through the graphene layer 15 can be detected.
[0029] In FIG. 3H, an ALD layer 25 of, for example, Al2O3 is deposited on the entire surface. The ALD layer is formed by heating in a vacuum state to remove moisture from the surface (vacuum annealing effect). The source gas of the ALD layer 25, for example, trimethylaluminum (TMA) and water vapor, enters the opening 22 and penetrates not only the inner wall of the opening 22 and the side of the graphene layer 15, but also the interface between the graphene layer 15 and the protective layer 21. The ALD layer 25 fills the gap between the graphene layer 15 and the protective layer 21, and continuously covers the side of the hole 151 and the inner wall of the opening 22. Therefore, a part of the ALD layer 25 is also present at the interface between the graphene layer 15 and the ALD layer 25. By providing the ALD layer 25, the gap between the graphene layer 15 and the protective layer 21 is filled, and the intrusion of moisture and impurities into the graphene layer 15 is prevented.
[0030] In FIG. 3I, contact holes are formed at predetermined positions in the ALD layer 25, and an electrode pad 16a connected to the electrode 14a and an electrode pad 16b connected to the electrode 14b are formed, thereby obtaining the optical sensor device 10.
[0031] 4 shows an optical sensor device 10A as a modified example. The optical sensor device 10A has a buried gate electrode 18 instead of a back gate. The gate electrode 18 is provided on an insulating film 12 using a thermal oxide film, and another insulating film 17 is provided to cover the gate electrode 18. The graphene layer 15 is disposed on the insulating film 17. The insulating film 17 below the graphene layer 15 serves as a gate insulating film. By applying a gate voltage to the graphene layer 15 via the insulating film 17, the carrier density of the graphene layer 15, such as electrons and holes, is controlled.
[0032] In the optical sensor device 10A, a periodic arrangement of holes 151 is also formed in the graphene layer 15, and the edges and side surfaces of the holes 151 and the inner walls of the openings 22 in the protective layer 21 are covered with the ALD layer 25. The sensitivity and weather resistance of the optical sensor device 10A are improved, and operational reliability is achieved.
[0033] Figure 5 is a diagram explaining the necessity of improving weather resistance. The horizontal axis of Figure 5 is the gate voltage [V], and the vertical axis is the drain current [A]. The solid line shows the electrical characteristics when vacuum annealing was performed, and the dashed line shows the electrical characteristics of the sample without annealing.
[0034] As mentioned above, the electrical characteristics of an optical sensor device can change due to changes in the environment. The presence or absence of moisture on the device surface, or the amount of moisture, changes depending on whether or not annealing is performed. A change in the amount of moisture on the device surface can be seen as a change in the environment. A change in the environment changes the Dirac point. Here, the Dirac point is the gate voltage at which the drain current is at a minimum with no incident light. Ideally, it is desirable for the Dirac point to be at a gate voltage of 0V.
[0035] As samples for measurement, two types of optical sensor devices without the ALD layer 25 are fabricated. One is a sample in which the fabricated device is subjected to vacuum annealing at 150° C. for 1 hour, and the other is a sample without annealing. Au / Cr electrodes 14a and 14b are formed in the sample. The distance between the electrodes is 4.07 μm. The width (vertical length in FIG. 1) of the electrodes 14a and 14b is 8.24 μm, the width (vertical length in FIG. 1) of the graphene layer 15 is 5 μm, and the length (horizontal length in FIG. 1) is 20 μm. A hole with a diameter of 200 nm is formed in the graphene layer 15. The gate voltage is changed from −40 V to +4-V in the absence of incident light, and the drain current is measured. The vacuum annealed sample is cooled without being removed from the chamber and measured in vacuum.
[0036] For the sample without annealing, the Dirac point is near 40 V due to the influence of moisture on the device surface, and the drain current changes significantly over the measurement range. This indicates the sensor characteristics in a highly humid environment. On the other hand, the Dirac point of the sample that was annealed in vacuum is closer to 0 V, and even if the absolute value of the gate voltage is increased, the change in the drain current is not so great. This indicates the sensor characteristics in an environment with little influence of moisture.
[0037] It is desirable to maintain the electrical characteristics shown by the solid line even when the environment changes. In the optical sensor devices 10 and 10A, the ALD layer 25 is provided to prevent moisture intrusion and suppress the shift of the Dirac point. The ALD layer 25 provides electrical characteristics similar to those of the annealed sample.
[0038] 6 is a diagram showing the effect of the ALD layer 25. The solid line shows the electrical properties of a sample annealed after ALD, the dashed line shows the electrical properties measured in vacuum without annealing after ALD, and the dashed line shows the electrical properties measured in air without annealing after ALD. The measurements in vacuum represent a room temperature environment.
[0039] Regardless of whether annealing is performed or not, the Dirac point, i.e., the point at which the drain current is at a minimum in the absence of incident light, is almost constant and is located near a gate voltage of 0 V. This is the effect of providing the ALD layer 25. When the ALD layer 25 is provided, subsequent annealing is not necessary because the fluctuation of the Dirac point is suppressed even without annealing.
[0040] At the Dirac point, the current change is large when light is incident on the device. By applying a bias voltage between the source and drain, the current change can be read with high sensitivity.
[0041] FIG. 7 is another diagram showing the effect of the ALD layer 25. The horizontal axis is the initial Dirac point, and the vertical axis is the measured value of the Dirac point. The dashed straight line in the diagram shows the characteristics of the initial Dirac point. The initial Dirac point is 10 to 19 V. If the measurement point is on the dashed line, there is no effect of ALD, but if the measurement point is below the dashed line, it indicates that the Dirac point is small and approaching 0 V.
[0042] The gray circles indicate the measured value of the Dirac point when holes 151 are formed in the graphene layer 15 by ion beam etching and then vacuum annealed, and the white circles indicate the measured value of the Dirac point when the ALD layer 25 is formed and then vacuum annealed. By forming holes 151 in the graphene layer 15 by ion beam etching and then annealing, the Dirac point can be lowered below the initial Dirac point. In the sample in which the ALD layer 25 is formed and then annealed, the Dirac point can be brought even closer to 0 V. In this way, it can be seen that the ALD layer 25 has the effect of reducing the Dirac point and bringing it closer to 0 V.
[0043] FIG. 8 is another diagram showing the effect of the ALD layer 25. As in FIG. 7, the horizontal axis is the initial Dirac point, and the vertical axis is the measured value of the Dirac point. The open circles are the measured value of the Dirac point before forming the holes 151 in the graphene layer 15, and the closed circles are the measured value of the Dirac point after forming the holes 141. Neither was annealed. The measured value of the Dirac point for the sample after ion beam etching is near 40 V, which matches the characteristics of the sample without annealing in FIG. 5. Even before ion beam etching, the Dirac point is near 35 V.
[0044] The grey circles represent the measured value of the Dirac point when annealing was performed after etching of the graphene layer 15, and the white triangles represent the measured value of the Dirac point when the ALD layer 25 was formed without annealing after etching of the graphene layer 15, and measured in air. By annealing, the Dirac point can be reduced to 10 V or less. This measurement result is consistent with the characteristics of the annealed sample in FIG. 5.
[0045] By forming the ALD layer 25, the Dirac point can be brought even closer to 0 V without a separate annealing treatment. By forming the ALD layer 25, an effect equal to or greater than that achieved by vacuum annealing after forming the holes 151 in the graphene layer 15 can be achieved. In other words, even without an annealing treatment after forming the holes 151 in the graphene layer 15, annealing is performed when the ALD layer 25 is formed, preventing the intrusion of moisture, impurities, and the like into the graphene, and the Dirac point can be reduced to near 0 V.
[0046] In terms of process, forming the ALD layer 25 is easier and takes less time than performing an annealing treatment. In addition, since the Dirac point is near 0 V, the gate voltage in the initial state without light incidence can be set to near 0 V, so that power consumption can be reduced. As described with reference to FIG. 6, by providing the ALD layer 25, the fluctuation of the Dirac point is suppressed even if the surrounding environment changes, and the optical sensor device 10 or 10A with excellent weather resistance is realized.
[0047] Although the present disclosure has been described above based on specific examples, the present disclosure is not limited to the above examples. The shape (including width and length) of the graphene layer 15 and the number of layers can be appropriately designed. The holes 151 formed in the graphene layer 15 are not limited to circular holes, and may be polygonal, elliptical, or other holes. The arrangement of the holes 151 is not limited to a matrix arrangement as shown in FIG. 1, and may be an alternating arrangement or a closely packed arrangement. The ALD layer 25 is not limited to Al2O3, and may be a metal oxide such as HfO2 or SiO2 by plasma ALD, or TaN x , SiN x A thin film of a metal nitride such as [Explanation of symbols]
[0048] 10, 10A Optical Sensor Device 11 Substrate 12 Insulating film 14a, 14b electrode 15 graphene layers 151 holes 16a, 16b Electrode pads 18, 19 Gate electrode 21 Protective layer 22 Aperture 25 ALD layer (thin film)
Claims
1. a graphene layer disposed on a substrate; A pair of electrodes electrically connected to the graphene layer; a resin protective layer covering the graphene layer; having The graphene layer is provided with periodic holes, the protective layer is provided with periodic openings communicating with the holes; The side surface of the hole and the inner wall of the opening are continuously covered with an insulating thin film. Optical sensor device.
2. the protective layer is formed of a material that is transparent in a target wavelength region and can be patterned by an electron beam; The optical sensor device of claim 1 .
3. A portion of the thin film is at the interface between the graphene layer and the protective layer.
3. An optical sensor device according to claim 1 or 2.
4. a gate electrode provided on the substrate; an insulating film disposed between the graphene layer and the gate electrode; The optical sensor device according to any one of claims 1 to 3, further comprising:
5. forming a graphene layer on an insulating film on a substrate; forming a pair of electrodes electrically connected to the graphene layer; forming a resin protective layer covering the graphene layer; forming periodic openings in the protective layer; forming periodic holes in the graphene layer by using the protective layer in which the openings are formed as a mask; forming a thin film by atomic layer deposition on the entire surface of the substrate on which the holes and the openings are formed; A method for manufacturing an optical sensor device.
6. forming the opening by electron beam lithography; A method for manufacturing an optical sensor device according to claim 5 .
7. forming the holes by ion beam etching; A method for manufacturing the optical sensor device according to claim 5 or 6.
8. forming a gate electrode on the substrate; A method for manufacturing an optical sensor device according to any one of claims 5 to 7.
Citation Information
Patent Citations
Focussing system of synthetic-aperture radar image
JP1986013372A
Light receiving element and manufacturing method of the same
JP2013093385A
Method of increasing energy density and achievable power output of energy storage device
JP2017130669A
Method for producing graphene nanomesh and method for manufacturing semiconductor device
WO2013018153A1
Electromagnetic wave detector and electromagnetic wave detector array
WO2016121408A1