Semiconductor wafer cleaning method and semiconductor wafer manufacturing method

By measuring contact angles with higher surface tension solutions and applying pretreatment to enhance hydrophilicity, the method addresses inconsistent LPD reduction in semiconductor wafer cleaning, ensuring thorough coverage and effective particle removal.

JP7563329B2Active Publication Date: 2024-10-08SUMCO CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2021131785
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-08-12
Publication Date
2024-10-08
Estimated Expiration
2041-08-12

AI Technical Summary

Technical Problem

Existing semiconductor wafer cleaning methods fail to consistently reduce Light Point Defects (LPD) due to variations in wafer hydrophilicity, leading to incomplete spreading of cleaning solutions and residual particles.

Method used

A method involving contact angle measurement with aqueous solutions of higher surface tension than pure water, followed by pretreatment to enhance hydrophilicity, and subsequent single-wafer spin cleaning to ensure comprehensive coverage and reduce LPD.

Benefits of technology

The method reliably reduces LPD on semiconductor wafers by ensuring uniform spreading of cleaning solutions, thereby improving the cleaning process efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563329000004
    Figure 0007563329000004
  • Figure 0007563329000005
    Figure 0007563329000005
  • Figure 0007563329000006
    Figure 0007563329000006
Patent Text Reader

Abstract

To provide a cleaning method of a semiconductor wafer, capable of surely reducing an LPD of a front surface of the wafer.SOLUTION: A cleaning method of a semiconductor wafer of the present invention, includes: a first step of measuring a contact angle of a front surface of the semiconductor wafer under a plurality of conditions that an amount of a droplet dropping on the front surface is different; a second step of calculating a proportion of the change of a measurement value of the contact angle against the change of the amount of the droplet from a relation between the amount of the droplet and the measurement value of the contact angle under the plurality of conditions; a third step of measuring a requirement of previous processing against to the front surface of the semiconductor wafer on the basis of the proportion; a fourth step of performing the previous step against the front surface of the semiconductor wafer in accordance with the determination of the third step; and a fifth step of performing a single wafer spin washing against the front surface of the semiconductor wafer after those steps.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a semiconductor wafer cleaning method and a semiconductor wafer manufacturing method, which include a step of performing single-wafer spin cleaning on the surface of a semiconductor wafer. [Background technology]

[0002] The manufacturing process of semiconductor wafers such as silicon wafers includes a cleaning process in which a cleaning liquid is supplied onto the surface of the wafer while the wafer is rotating to remove particles adhering to the surface (hereinafter also referred to as "single wafer spin cleaning").

[0003] As an example of single wafer spin cleaning, there is a method in which spin cleaning with ozone water and spin cleaning with hydrofluoric acid are repeatedly performed. In this method, an oxide film is formed on the wafer surface by spin cleaning with ozone water, and then particles and the like on the wafer surface are removed together with the oxide film by spin cleaning with hydrofluoric acid. Patent Document 1 describes a wafer cleaning method including a cleaning step using ozone water and a cleaning step using hydrofluoric acid, which has a spin cleaning step using pure water between the cleaning step using ozone water and the cleaning step using hydrofluoric acid. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2015-220284 A Summary of the Invention [Problem to be solved by the invention]

[0005] In single wafer spin cleaning, in order to effectively reduce LPD (light point defect) in the subsequent wafer inspection process, it is necessary to spread the cleaning solution all over the wafer surface to form a film of the cleaning solution on the entire wafer surface. In this regard, a natural oxide film is formed on the wafer surface immediately before the single wafer spin cleaning, and the wafer surface is basically hydrophilic. Therefore, in the first step of the single wafer spin cleaning (e.g., spin cleaning with ozone water), the wafer surface should be in a state where the cleaning solution can easily spread. However, according to the study by the present inventors, even if the single wafer spin cleaning conditions are the same, it was found that while some wafers can reduce LPD, other wafers do not sufficiently reduce LPD.

[0006] In view of the above problems, an object of the present invention is to provide a method for cleaning a semiconductor wafer and a method for manufacturing a semiconductor wafer, which can reliably reduce LPD on the wafer surface. [Means for solving the problem]

[0007] In order to solve the above problems, the present inventors have conducted intensive research and obtained the following findings. First, as mentioned above, the wafer surface is basically hydrophilic immediately before the single wafer spin cleaning. Specifically, the contact angle of the wafer surface to be subjected to the single wafer spin cleaning is approximately 5° when measured by dropping pure water on the surface. However, In reality, the hydrophilicity level of the wafer surface varies depending on the storage conditions of the wafer before it is subjected to single-wafer spin cleaning, but the contact angle of the wafer surface measured with pure water does not vary. - For wafers with poor hydrophilicity, in the first step of single wafer spin cleaning (e.g., spin cleaning with ozone water), the cleaning solution does not spread all over the wafer surface, and the continuity of the cleaning solution film on the wafer surface is not maintained, resulting in localized areas on the wafer surface where the cleaning solution does not reach. -As a result, particles remain even after single-wafer spin cleaning, and etching unevenness occurs after single-wafer spin cleaning, resulting in an increase in LPD. The present inventors considered that this may be the case.

[0008] Therefore, the present inventors - measuring the contact angles of various wafer surfaces before single wafer spin cleaning under a plurality of conditions in which an aqueous solution having a surface tension greater than that of pure water is dropped and the amount of the dropped droplet is different from one another; -Then, each wafer is subjected to single-wafer spin cleaning under the same conditions. -Then, measure the number of LPDs on the wafer surface. The test was conducted.

[0009] This is because it was thought that if the contact angle of the wafer surface is measured with an aqueous solution having a surface tension greater than that of pure water, a larger contact angle would be obtained than the contact angle measured with pure water, and therefore it would be possible to detect severe differences in the hydrophilicity level of the wafer surface that cannot be detected by contact angle measurements using pure water. - Wafers with a small ratio of change in contact angle to change in droplet volume have a small number of LPDs. -Wafer with a large ratio of change in contact angle to change in droplet volume has a large number of LPDs We found that.

[0010] Therefore, the inventors have found that, based on this ratio, it is determined whether or not it is necessary to perform a pretreatment to increase the hydrophilicity of the wafer surface prior to single-wafer spin cleaning, and if it is determined that pretreatment is necessary, LPD on the wafer surface can be reliably reduced by performing the pretreatment before single-wafer spin cleaning.

[0011] The present invention, which was completed based on the above findings, has the following essential features. [1] A first step of measuring a contact angle on a surface of a semiconductor wafer under a plurality of conditions in which the amount of a droplet dropped on the surface is different from one another; A second step of calculating a ratio of a change in the measured value of the contact angle to a change in the amount of the droplet based on the relationship between the amount of the droplet and the measured value of the contact angle under the plurality of conditions; A third step of determining whether or not pretreatment is required for the surface of the semiconductor wafer based on the ratio; a fourth step of performing the pretreatment on the front surface of the semiconductor wafer according to the determination of the third step; Thereafter, a fifth step of performing single-wafer spin cleaning on the surface of the semiconductor wafer; A method for cleaning a semiconductor wafer comprising the steps of:

[0012] [2] After the first step and before the second step, a relative value of the measured values ​​of the contact angles under the plurality of conditions is obtained; The method for cleaning a semiconductor wafer according to [1] above, wherein in the second step, a ratio of a change in the relative value of the measured contact angle to a change in the amount of the droplet is calculated from a relationship between the amount of the droplet and the relative value of the measured contact angle under the multiple conditions.

[0013] [3] The method for cleaning a semiconductor wafer according to [2] above, wherein the relative value is a value normalized based on a measured value of the contact angle under any one of the plurality of conditions.

[0014] [4] The method for cleaning a semiconductor wafer according to the above [3], wherein the any one of the conditions is a condition under which the measured value of the contact angle is maximum.

[0015] [5] The method for cleaning a semiconductor wafer according to any one of [1] to [4] above, wherein in the second step, the ratio is a slope of a straight line obtained by applying a least squares method to the relationship.

[0016] [6] The method for cleaning a semiconductor wafer according to any one of the above [1] to [5], wherein the plurality of conditions is three or more conditions.

[0017] [7] The method for cleaning a semiconductor wafer according to any one of [1] to [6] above, wherein in the first step, an image of the droplet dropped on the surface of the semiconductor wafer is obtained, and the amount of the droplet is measured from the image in addition to the contact angle.

[0018] [8] The method for cleaning a semiconductor wafer according to any one of the above [1] to [7], wherein the droplets are made of an aqueous solution having a surface tension greater than that of pure water.

[0019] [9] The method for cleaning a semiconductor wafer according to the above [8], wherein the aqueous solution is at least one selected from the group consisting of an aqueous sodium chloride solution, an aqueous potassium chloride solution, and an aqueous magnesium chloride solution.

[0020]

[10] The method for cleaning a semiconductor wafer according to the above [9], wherein the concentration of the aqueous solution is 10 mass % or more.

[0021]

[11] The method for cleaning a semiconductor wafer according to any one of the above [1] to

[10] , wherein the amount of the droplets is set within a range of 0.3 to 3.0 μL.

[0022]

[12] The method for cleaning a semiconductor wafer according to any one of [1] to

[11] above, wherein in the third step, if the absolute value of the ratio is equal to or less than a predetermined threshold, it is determined that the pretreatment is unnecessary, and if the absolute value of the ratio exceeds the threshold, it is determined that the pretreatment is necessary.

[0023]

[13] The method for cleaning a semiconductor wafer according to

[12] above, wherein the predetermined threshold value is 0.050.

[0024]

[14] The method for cleaning a semiconductor wafer according to the above

[12] , wherein the predetermined threshold value is 0.020.

[0025]

[15] The method for cleaning a semiconductor wafer according to any one of the above [1] to

[14] , wherein the pretreatment includes one or more of: (i) immersing the semiconductor wafer in ozone water; (ii) exposing the surface of the semiconductor wafer to a downflow in a clean room; and (iii) irradiating the surface of the semiconductor wafer with infrared rays.

[0026]

[16] The method for cleaning a semiconductor wafer according to any one of [1] to

[15] above, wherein, when the pretreatment is performed in the fourth step, the first to third steps are subsequently repeated, and after it is determined that the pretreatment is not required again, the fifth step is performed.

[0027]

[17] The method for cleaning a semiconductor wafer according to any one of [1] to

[16] above, wherein in the fifth step, first, spin cleaning with ozone water is performed, and then one or more sets of a combination of spin cleaning with hydrofluoric acid and subsequent spin cleaning with ozone water are performed.

[0028]

[18] The method for cleaning a semiconductor wafer according to any one of the above [1] to

[17] , wherein the semiconductor wafer is a silicon wafer.

[0029]

[19] A method for producing a semiconductor wafer, comprising the method for cleaning a semiconductor wafer according to any one of the above [1] to

[18] . Effect of the Invention

[0030] According to the semiconductor wafer cleaning method and semiconductor wafer manufacturing method of the present invention, it is possible to reliably reduce LPD on the wafer surface. [Brief description of the drawings]

[0031] [Figure 1] 2 is a flow chart illustrating a method for cleaning a semiconductor wafer according to one embodiment of the present invention. [Diagram 2] 1 is a graph showing the relationship between the number of LPDs after single-wafer spin cleaning and the contact angle of the wafer surface measured with pure water before single-wafer spin cleaning in Experimental Example 1. [Diagram 3] 1 is a graph showing the results of contact angle measurement using an NaCl aqueous solution in Experimental Example 2. [Figure 4] 4 is a graph showing the relationship between the absolute value of the slope of the straight line in FIG. 3 and the number of LPDs after single-wafer spin cleaning. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0032] (Method of cleaning semiconductor wafers) The semiconductor wafer cleaning method of the present invention includes a first step of measuring the contact angle on the surface of a semiconductor wafer under multiple conditions in which the amount of droplets dropped on the surface is different from one another; a second step of calculating a ratio of a change in the measured contact angle to a change in the amount of droplets based on a relationship between the amount of droplets and the measured contact angle under the multiple conditions; a third step of determining whether or not pretreatment is required for the surface of the semiconductor wafer based on the ratio; a fourth step of performing the pretreatment on the surface of the semiconductor wafer in accordance with the determination in the third step; and a fifth step of thereafter performing single-wafer spin cleaning on the surface of the semiconductor wafer.

[0033] Preferably, after the first step and before the second step, relative values ​​of the measured values ​​of the contact angles under the multiple conditions are obtained, and in the second step, a ratio of a change in the relative value of the measured values ​​of the contact angles to a change in the amount of the droplet is calculated from a relationship between the amount of the droplet and the relative value of the measured values ​​of the contact angles under the multiple conditions. Preferably, the relative value is a value normalized based on the measured value of the contact angle under any one of the multiple conditions.

[0034] A method for cleaning a semiconductor wafer according to an embodiment of the present invention includes the steps of: - a first step (step S1) of measuring the contact angle of a surface of a semiconductor wafer under a plurality of conditions in which the amount of droplets dropped on the surface is different from one another; - a step (step S2A) of normalizing the contact angle measurement values ​​under the plurality of conditions based on the contact angle measurement value under any one of the plurality of conditions to obtain a relative value of the contact angle measurement values ​​under the plurality of conditions; A second step (step S2B) of plotting the measurement data on a plane with the droplet volume on the horizontal axis and the normalized contact angle on the vertical axis, and calculating the ratio of the change in the relative value of the measured contact angle to the change in the droplet volume by linear approximation to obtain a slope; a third step (step S3) of determining whether or not pretreatment is required for the surface of the semiconductor wafer based on the ratio; a fourth step (step S4) of performing the pretreatment on the front surface of the semiconductor wafer when it is determined in step S3 that the pretreatment is necessary; - returning to step S1 after step S4; a fifth step (step S5) of performing single-wafer spin cleaning on the front surface of the semiconductor wafer when it is determined in step S3 that pretreatment is not required; has.

[0035] The semiconductor wafer cleaning method according to the present invention and one embodiment of the present invention is characterized by determining whether or not a pretreatment step of single wafer spin cleaning is required, and this makes it possible to reliably reduce LPD on the wafer surface. Each step will be described in detail below.

[0036] [Semiconductor wafers] The semiconductor wafer subjected to the above-mentioned present invention and the method for cleaning a semiconductor wafer according to one embodiment of the present invention is not particularly limited, but is preferably a silicon wafer, and more preferably a single crystal silicon wafer.

[0037] Generally, the process immediately before the single wafer spin cleaning is a pre-cleaning process or an inspection process that follows the pre-cleaning process, and at the end of the pre-cleaning process, a natural oxide film is formed on the wafer surface. Specifically, in the pre-cleaning process, the wafer is cleaned using a combination of an SC1 cleaning tank, an HF tank, an ozone tank, etc., and then rinsed with pure water and dried. When the inspection process is performed, inspection of particles and scratches on the wafer surface, inspection of the wafer shape (flatness), etc. are performed. That is, a natural oxide film is formed on the surface of the semiconductor wafer subjected to the semiconductor wafer cleaning method according to the present invention and one embodiment of the present invention, and the wafer surface is basically hydrophilic. Specifically, the contact angle of the wafer surface is approximately 5° when measured by dropping pure water on the wafer.

[0038] However, in reality, the hydrophilicity level of the wafer surface varies depending on the storage conditions of the wafer before being subjected to single wafer spin cleaning, but the contact angle of the wafer surface measured with pure water does not vary. For example, after the above pre-cleaning process and optional inspection process, the wafer is stored in a container called a FOUP (Front-Opening Unified Pod), and as the storage period increases, slight deposition of organic matter may occur on the wafer surface. In addition, if the wafer is not dried sufficiently after the above pre-cleaning process, water vapor may be generated in the FOUP and adsorbed on the wafer surface, causing polarization of water molecules on the wafer surface. In such a wafer with a severely inferior hydrophilicity level, the cleaning solution does not spread all over the wafer surface in the first process of single wafer spin cleaning (e.g., spin cleaning with ozone water), and the continuity of the film of the cleaning solution on the wafer surface cannot be maintained, resulting in localized areas on the wafer surface where the cleaning solution does not reach. As a result, particles remain even after single wafer spin cleaning, or etching unevenness occurs after single wafer spin cleaning, resulting in an increase in LPD. Therefore, for wafers with such a severely inferior hydrophilicity level, a pretreatment is performed to enhance the hydrophilicity of the wafer surface prior to single-wafer spin cleaning. The above-mentioned present invention and the semiconductor wafer cleaning method according to one embodiment of the present invention are characterized by the determination of the necessity of this pretreatment.

[0039] [First step (Step S1)] First, in a first process (step S1), the contact angle on the surface of a semiconductor wafer is measured under a plurality of conditions in which the amount of droplet dropped on the surface is different from one another.

[0040] In this embodiment, it is preferable to measure the contact angle by dropping a droplet of an aqueous solution having a surface tension larger than that of pure water onto the wafer surface. This makes it possible to detect a severe difference in hydrophilicity level of the wafer surface that cannot be detected by contact angle measurement using pure water. Such an aqueous solution is preferably at least one selected from the group consisting of an aqueous sodium chloride solution, an aqueous potassium chloride solution, and an aqueous magnesium chloride solution. These aqueous solutions are easy to prepare and have a suitable surface tension. The concentration of these aqueous solutions is not particularly limited, but is preferably 10 mass % or more from the viewpoint of exerting a suitable surface tension, and the upper limit is allowed up to the solubility.

[0041] The amount of droplets used in contact angle measurement is preferably set within the range of 0.3 to 3.0 μL. If the amount of droplets is 0.3 μL or more, the effects of evaporation and volatilization of the droplets are small, and the error in the contact angle measurement is not large, and if the amount of droplets is 3.0 μm or less, the droplets are not easily crushed by their own weight, and the error in the contact angle measurement is not large.

[0042] From the viewpoint of determining the necessity of pretreatment with high accuracy, the contact angle is preferably measured under three or more conditions with different droplet amounts, and more preferably under five or more conditions. Although there is no particular upper limit on the number of conditions, the number of conditions can be eight or less since the determination accuracy becomes saturated.

[0043] In the first step, an image of the droplet dropped on the surface of the semiconductor wafer is obtained, and the contact angle is measured from the image. The contact angle can be measured by a standard method, for example, the θ / 2 method, the tangent method, or the curve fitting method.

[0044] In the first step, it is preferable to measure (calculate) the amount (volume) of the droplets that have actually been dropped from the image. The amount of droplets can be set by the contact angle meter used, but there may be a certain degree of error between the droplet amount set by the device and the amount of droplets that has actually been dropped. For example, see the variation in the plot in Figure 3. Therefore, by applying the actually measured droplet amount, rather than the device set value, to the next step and subsequent steps, more accurate judgments can be made.

[0045] [Standardization process (Step S2A)] Next, the relative values ​​of the measured values ​​of the contact angle under a plurality of conditions are obtained. The method of obtaining the relative values ​​is not particularly limited, but for example, as in step S2A, a method of normalizing the measured values ​​of the contact angle under a plurality of conditions based on the measured value of the contact angle under any one of the plurality of conditions can be preferably adopted. In this case, the reference condition is not particularly limited, but for example, the condition under which the measured value of the contact angle is maximum can be used as the reference.

[0046] [Second step (Step S2B)] Next, in the second step, the ratio of the change in the relative value of the measured value of the contact angle to the change in the amount of the droplet is calculated from the relationship between the amount of the droplet and the relative value of the measured value of the contact angle under the multiple conditions. The method of calculating the ratio is not particularly limited, but the slope of a line obtained by applying the least squares method to the relationship can be used as the ratio. That is, in step S2B of this embodiment, the measurement data is plotted on a plane with the horizontal axis representing the amount of droplet and the vertical axis representing the normalized contact angle, and the slope is calculated by linear approximation. The least squares method can be used as a method of linear approximation. For example, see FIG. 3.

[0047] [Third step (Step S3)] Next, in the third step (step S3), the necessity of pre-processing the surface of the semiconductor wafer is judged based on the ratio. As described above, the inventors' investigations revealed that the number of LPDs is small in a wafer in which the ratio of the change in contact angle to the change in droplet volume is small, and the number of LPDs is large in a wafer in which the ratio of the change in contact angle to the change in droplet volume is large. Therefore, in the third step, if the absolute value of the ratio is equal to or less than a predetermined threshold, it is judged that pre-processing is unnecessary, and if the absolute value of the ratio exceeds the predetermined threshold, it is judged that pre-processing is necessary.

[0048] Since the specified threshold value varies depending on the conditions of single-wafer spin cleaning, such as the type of cleaning liquid, the flow rate of the cleaning liquid, and the wafer rotation speed, it is preferable to determine an appropriate value in advance for each condition of single-wafer spin cleaning. As an example, the specified threshold value can be set to 0.050, and the specified threshold value can also be set to 0.020.

[0049] [Fourth step (Step S4)] If it is determined in step S3 that pretreatment is necessary, a pretreatment is performed on the surface of the semiconductor wafer in the fourth step (step S4). The pretreatment is a treatment for increasing the hydrophilicity of the wafer surface. For example, if it is believed that slight deposition of organic matter has occurred on the wafer surface, (i) a pretreatment of immersing the semiconductor wafer in ozone water can be performed to remove the organic matter. If it is believed that polarization of water molecules has occurred on the wafer surface, at least one of (ii) a pretreatment of exposing the semiconductor wafer surface to the downflow of a clean room and (iii) a pretreatment of irradiating the semiconductor wafer surface with infrared rays can be performed to control the orientation of water molecules on the wafer surface. As the pretreatment, one or more of the above (i) to (iii) can be appropriately performed.

[0050] As for the conditions of the pretreatment of the semiconductor wafer by immersing it in ozone water, the concentration of the ozone water is preferably within the range of 20 to 30 mg / L, and the immersion time in the ozone water is preferably within the range of 5 to 300 seconds, more preferably within the range of 60 to 300 seconds. Also, it is more preferable to perform single-wafer spin cleaning immediately after immersion in the ozone tank.

[0051] The pretreatment conditions for exposing the surface of the semiconductor wafer to the downflow in the clean room are preferably as follows: the semiconductor wafer is placed under the fan in the clean room in an atmosphere of room temperature: 20-25°C and humidity: 30-50%, and the surface of the semiconductor wafer is exposed to the downflow formed by the circulation of the atmosphere. The fan rotation speed is preferably within the range of 1000-2000 rpm, and the waiting time under the downflow is preferably within the range of 60-1200 seconds, more preferably within the range of 180-1200 seconds. It is preferable not to use an ionizer.

[0052] The pretreatment conditions for irradiating the surface of the semiconductor wafer with infrared rays are preferably such that the surface of the semiconductor wafer is irradiated with infrared rays having a wavelength of about 0.5 to 35 μm for 200 to 1800 seconds. The wafer temperature during irradiation is preferably within the range of 50 to 80° C.

[0053] [Fifth step (Step S5)] If it is determined in step S3 that pretreatment is not required, in the fifth step (step S5), single wafer spin cleaning is performed on the surface of the semiconductor wafer. In the fifth step, it is preferable to first perform spin cleaning with ozone water, and then perform one or more sets of a combination of spin cleaning with hydrofluoric acid and subsequent spin cleaning with ozone water. In this method, an oxide film is formed on the wafer surface by spin cleaning with ozone water, and then particles and the like on the wafer surface are removed together with the oxide film by spin cleaning with hydrofluoric acid. Since the final cleaning step is spin cleaning with ozone water, an oxide film is formed on the wafer surface after single wafer spin cleaning. The combination with spin cleaning with ozone water may be one or more sets, but preferably 1 to 5 sets can be performed.

[0054] In the spin cleaning with ozone water, the concentration of the ozone water is not particularly limited as long as an oxide film is formed on the wafer surface, but can be 20 to 30 mg / L. The flow rate of the ozone water is not particularly limited as long as an oxide film is formed on the wafer surface, but can be 0.5 to 1.5 L / min. The processing time per spin cleaning with ozone water is also not particularly limited as long as an oxide film is formed on the wafer surface, but can be 50 to 200 seconds.

[0055] In the spin cleaning with hydrofluoric acid, the concentration of hydrofluoric acid may be appropriately set depending on the contamination level of the wafer, and may be set to 0.5 to 3.0 mass % without any particular limitation. The flow rate of hydrofluoric acid may be appropriately set depending on the contamination level of the wafer, and may be set to 0.5 to 1.5 L / min without any particular limitation. The processing time for each spin cleaning with hydrofluoric acid may be appropriately set depending on the contamination level of the wafer, and may be set to 50 to 200 seconds without any particular limitation.

[0056] The rotation speed of the wafer in each cleaning step is not particularly limited, but may be set to 50 to 800 rpm.

[0057] After the single-wafer spin cleaning, it is preferable to perform spin drying by continuing to rotate the wafer without supplying the cleaning liquid, to remove the cleaning liquid from the wafer surface, and to dry the wafer surface. The rotation speed of the wafer is not particularly limited, but can be 1000 to 1500 rpm.

[0058] 1, when the pretreatment is performed in the fourth step, it is preferable to return to step S1, repeat steps S1, S2A, S2B, and S3, and perform single wafer spin cleaning in the fifth step after it is determined in step S3 that another pretreatment is not required. This makes it possible to more reliably obtain wafers with reduced LPD.

[0059] However, this is not essential, and after the pretreatment in step 4, the process may proceed directly to step S5 without returning to step S1, and single wafer spin cleaning may be performed. For example, when pretreatment conditions are adopted that are expected to make the wafer surface sufficiently hydrophilic, it is preferable to perform single wafer spin cleaning directly after the pretreatment in step 4 in order to simplify the entire process.

[0060] [Other embodiments] In the present embodiment shown in Fig. 1, in step S2A, the measured values ​​of the contact angle under a plurality of conditions are standardized to obtain a relative value, but this step is not essential. Instead of performing step S2A, in step S2B, the ratio of the change in the measured value of the contact angle to the change in the amount of the droplet may be calculated from the relationship between the amount of the droplet and the measured value of the contact angle under a plurality of conditions. However, if normalization is not performed, the absolute value of the contact angle may change depending on the measurement environment (temperature, humidity, droplet concentration, etc.), but since the normalized contact angle is a quantitative index that is not dependent on the measurement environment, it is preferable to perform step S2A (normalization step).

[0061] It is not necessary to apply the semiconductor wafer cleaning method according to the present invention and one embodiment of the present invention (i.e., contact angle measurement and pretreatment necessity judgment) to all semiconductor wafers that are sent to the manufacturing process. For example, for multiple semiconductor wafers that have the same storage conditions (temperature, humidity, storage time, etc.) after the pre-cleaning process until being subjected to single-wafer spin cleaning, the semiconductor wafer cleaning method according to the present invention and one embodiment of the present invention can be applied to at least one semiconductor wafer to judge whether pretreatment is necessary, and the remaining semiconductor wafers can be subjected to single-wafer spin cleaning with or without pretreatment according to the judgment result.

[0062] (Method of manufacturing semiconductor wafers) The method for producing a semiconductor wafer according to an embodiment of the present invention includes the above-mentioned semiconductor wafer cleaning method. This makes it possible to reliably produce a wafer with reduced LPD. The method for producing a semiconductor wafer according to this embodiment includes, for example, obtaining a monocrystalline ingot by the Czochralski method; - slicing the monocrystalline ingot into a plurality of wafers; a planarization step in which the wafer is lapped and ground; - a polishing step in which the wafer is subjected to double-sided polishing followed by single-sided finish polishing; - A pre-cleaning process in which the wafer is cleaned using a combination of SC1 cleaning tank, HF tank, ozone tank, etc., and then rinsed with pure water and dried. - An optional inspection process then follows. - a method for cleaning a semiconductor wafer according to the present invention, including contact angle measurement and single wafer spin cleaning; a final inspection step including measuring the number of LPDs on the front surface of the wafer; has. EXAMPLES

[0063] The experimental examples that led to the completion of the present invention will now be described.

[0064] (Experimental Example 1) After mirror polishing, the wafers were cleaned using a combination of an SC1 cleaning tank, an HF tank, an ozone tank, etc., and then rinsed with pure water and dried in a pre-cleaning process. Three single crystal silicon wafers (diameter 300 mm) were then prepared that had been stored under different storage conditions.

[0065] The contact angle on the surface of each silicon wafer was measured by the θ / 2 method under the following conditions. Equipment: Portable contact angle meter PCA-11 manufactured by Kyowa Interface Science Co., Ltd. Dripping liquid type: Pure water Set droplet volume: 1μL Measurement points: 25 points on the wafer

[0066] Each silicon wafer was first subjected to spin cleaning with ozone water, then to single-wafer spin cleaning with three sets of a combination of a spin cleaning with hydrofluoric acid and a subsequent spin cleaning with ozone water, and finally to spin drying at a wafer rotation speed of 1500 rpm. -Conditions for spin cleaning with ozone water Concentration: 25mg / L Flow rate: 1.0L / min Processing time per session: 200 seconds Wafer rotation speed: 500 rpm -Conditions for single wafer spin cleaning using hydrofluoric acid Concentration: 1% by mass Flow rate: 1.0L / min Processing time per session: 50 seconds Wafer rotation speed: 500 rpm

[0067] The surface of each silicon wafer was then measured in HS (High Sensitivity) mode using a laser particle counter (KLA-Tencor, Surfscan SP7) to determine the number of LPDs with a size of 15 nm or more. The number of LPDs on the three silicon wafers was over 100 (200), over 10 and 100 or less (32), and 10 or less (5), respectively.

[0068] Figure 2 shows the measured contact angles at 25 points on the surface of each silicon wafer. As is clear from Figure 2, the contact angles of the wafer surface measured by dropping pure water on each of the three silicon wafers with different levels of LPD counts were 5 to 6°. For this reason, the contact angle measurement using pure water was unable to detect differences in the surface conditions before single-wafer spin cleaning between wafers with different numbers of LPDs.

[0069] (Experimental Example 2) Seven single crystal silicon wafers (diameter 300 mm) were prepared by performing a pre-cleaning process in which the wafers were cleaned in a combination of an SC1 cleaning tank, an HF tank, an ozone tank, etc. after mirror polishing, then rinsed with pure water and then dried. It is believed that the seven silicon wafers were not dried sufficiently after the pre-cleaning process, causing water vapor to be generated in the FOUP and adsorbed onto the wafer surface, resulting in polarization of water molecules on the wafer surface.

[0070] Seven silicon wafers were pretreated by exposing the surfaces of the silicon wafers to the downflow in the clean room. The pretreatment conditions (fan rotation speed and waiting time) are shown in Nos. 1 to 7 in Table 1, respectively.

[0071] The contact angle on the surface of each silicon wafer was measured by the θ / 2 method under the following conditions. The set liquid amount was set under the following three conditions, and the actual amount of the dropped liquid was measured from the image of the dropped liquid. Equipment: Portable contact angle meter PCA-11 manufactured by Kyowa Interface Science Co., Ltd. Dropping liquid type: 20% by mass NaCl aqueous solution Set droplet volume: 3 conditions: 0.5μL, 1.0μL, 2.0μL Measurement points: 5 points on the wafer (1-2 cm intervals from the center to the edge)

[0072] The average value of the contact angle measurements (average value of five points) was calculated for each set droplet amount, and the maximum average value was set as 1 to normalize the average value of the measurements for each set droplet amount. The measurement data was plotted on a plane with the droplet amount measurements (average value of five points) on the horizontal axis and the normalized contact angle (average value of five points) on the vertical axis, and the slope of the line was calculated by linear approximation using the least squares method. Figure 3 shows the plots and approximated lines for Nos. 1, 2, and 4 as representatives of Nos. 1 to 7. Table 1 shows the absolute values ​​of the slope for Nos. 1 to 7.

[0073] Thereafter, each silicon wafer was first subjected to spin cleaning with ozone water, then subjected to single-wafer spin cleaning in which a combination of spin cleaning with hydrofluoric acid and subsequent spin cleaning with ozone water was performed three times, and finally, spin drying was performed at a wafer rotation speed of 1500 rpm. -Conditions for spin cleaning with ozone water Concentration: 25mg / L Flow rate: 1.0L / min Processing time per session: 200 seconds Wafer rotation speed: 500 rpm -Conditions for single wafer spin cleaning using hydrofluoric acid Concentration: 1% by mass Flow rate: 1.0L / min Processing time per session: 50 seconds Wafer rotation speed: 500 rpm

[0074] The surface of each silicon wafer was then measured in HS (High Sensitivity) mode using a laser particle counter (KLA-Tencor, Surfscan SP7) to determine the number of LPDs with a size of 15 nm or more. The results are shown in Table 1. The criteria for judging the number of LPDs were as follows. Figure 4 shows the relationship between the absolute value of the slope of the straight line in Figure 3 and the number of LPDs after single-wafer spin cleaning. ◎: 10 pieces or less ○: More than 10 and less than 100 ×: Over 100

[0075] [Table 1]

[0076] 3 and 4, when the absolute value of the slope of the normalized contact angle / droplet amount is 0.050 or less, the number of LPDs is judged as ◯, and when the absolute value of the slope of the normalized contact angle / droplet amount is 0.020 or less, the number of LPDs is judged as ◎. As described above, since there is a correlation between the absolute value of the slope of the normalized contact angle / droplet amount and the number of LPDs, it is found that it is effective to judge the necessity of pretreatment based on the absolute value of the slope for any silicon wafer, such as by performing single-wafer spin cleaning without performing pretreatment when the absolute value of the slope is, for example, 0.050 or less or 0.020 or less, and by performing single-wafer spin cleaning after performing pretreatment when the absolute value of the slope is, for example, more than 0.050 or more than 0.020.

[0077] (Experimental Example 3) After mirror polishing, two single crystal silicon wafers (diameter 300 mm) were prepared by cleaning the wafers in a combination of SC1 cleaning tank, HF tank, ozone tank, etc., rinsing the wafers with pure water, and then drying them in a pre-cleaning process. The two silicon wafers had been in the pre-cleaning process for more than three weeks, and it is believed that slight accumulation of organic matter has occurred on the wafer surfaces.

[0078] As shown in Table 2, one of two silicon wafers was not pretreated, and the other was pretreated by immersing it in ozone water with a concentration of 25 mg / L for 5 seconds. Then, the contact angle on the surface of each silicon wafer was measured using the same method as in Experimental Example 2, and the absolute value of the slope of the normalized contact angle / droplet amount was calculated. Then, each silicon wafer was subjected to single-wafer spin cleaning and spin drying under the same conditions as in Experimental Example 2, and the number of LPDs was measured using the same method as in Experimental Example 2. These results are shown in Table 2.

[0079] [Table 2]

[0080] (Experimental Example 4) After mirror polishing, the wafers were cleaned in a combination of an SC1 cleaning tank, an HF tank, an ozone tank, etc., and then rinsed with pure water and dried in a pre-cleaning process to prepare two single crystal silicon wafers (diameter 300 mm). It is believed that the two silicon wafers were not dried sufficiently after the pre-cleaning process, which caused water vapor to be generated in the FOUP and adsorbed onto the wafer surface, resulting in polarization of water molecules on the wafer surface.

[0081] As shown in Table 3, one of two silicon wafers was not pretreated, and the other was pretreated by irradiating infrared rays for 300 seconds. Then, the contact angle on the surface of each silicon wafer was measured using the same method as in Experimental Example 2, and the absolute value of the slope of the normalized contact angle / droplet amount was calculated. Then, each silicon wafer was subjected to single-wafer spin cleaning and spin drying under the same conditions as in Experimental Example 2, and the number of LPDs was measured using the same method as in Experimental Example 2. These results are shown in Table 3.

[0082] [Table 3] [Industrial Applicability]

[0083] According to the semiconductor wafer cleaning method and semiconductor wafer manufacturing method of the present invention, it is possible to reliably reduce LPD on the wafer surface.

Claims

1. A first step of measuring a contact angle on a surface of a semiconductor wafer under a plurality of conditions in which the amount of a droplet dropped on the surface is different from one another; a second step of calculating a ratio of a change in the measured value of the contact angle to a change in the amount of the droplet based on a relationship between the amount of the droplet and the measured value of the contact angle under the plurality of conditions; A third step of determining whether or not pretreatment is required for the surface of the semiconductor wafer based on the ratio; a fourth step of performing the pretreatment on the front surface of the semiconductor wafer according to the determination of the third step; Thereafter, a fifth step of performing single-wafer spin cleaning on the surface of the semiconductor wafer; A method for cleaning a semiconductor wafer comprising the steps of:

2. After the first step and before the second step, a relative value of the measured value of the contact angle under the plurality of conditions is obtained; 2. The semiconductor wafer cleaning method according to claim 1, wherein in the second step, a ratio of a change in the relative value of the measured contact angle to a change in the amount of the droplet is calculated from a relationship between the amount of the droplet and the relative value of the measured contact angle under the multiple conditions.

3. 3. The method for cleaning a semiconductor wafer according to claim 2, wherein the relative value is a standardized value based on a measured value of the contact angle under any one of the plurality of conditions.

4. 4. The method for cleaning a semiconductor wafer according to claim 3, wherein the any one of the conditions is a condition under which the measured value of the contact angle is maximum.

5. 5. The method for cleaning a semiconductor wafer according to claim 1, wherein in the second step, the ratio is a slope of a straight line obtained by applying a least squares method to the relationship.

6. The method for cleaning a semiconductor wafer according to any one of claims 1 to 5, wherein the plurality of conditions is three or more conditions.

7. 7. The semiconductor wafer cleaning method according to claim 1, wherein in the first step, an image of the droplet dropped on the surface of the semiconductor wafer is acquired, and the amount of the droplet is measured from the image in addition to the contact angle.

8. 8. The method for cleaning a semiconductor wafer according to claim 1, wherein the droplets are made of an aqueous solution having a surface tension greater than that of pure water.

9. 9. The method for cleaning a semiconductor wafer according to claim 8, wherein the aqueous solution is at least one selected from the group consisting of an aqueous sodium chloride solution, an aqueous potassium chloride solution, and an aqueous magnesium chloride solution.

10. 10. The method for cleaning a semiconductor wafer according to claim 9, wherein the concentration of the aqueous solution is 10 mass % or more.

11. 11. The method for cleaning a semiconductor wafer according to claim 1, wherein the amount of the droplets is set within a range of 0.3 to 3.0 μL.

12. 12. The method for cleaning a semiconductor wafer according to claim 1, wherein in the third step, when an absolute value of the ratio is equal to or less than a predetermined threshold, it is determined that the pretreatment is unnecessary, and when the absolute value of the ratio exceeds the threshold, it is determined that the pretreatment is necessary.

13. 13. The method of claim 12, wherein the predetermined threshold is 0.

050.

14. 13. The method of claim 12, wherein the predetermined threshold is 0.

020.

15. The method for cleaning a semiconductor wafer according to any one of claims 1 to 14, wherein the pretreatment includes one or more of: (i) immersing the semiconductor wafer in ozone water; (ii) exposing the surface of the semiconductor wafer to a downflow in a clean room; and (iii) irradiating the surface of the semiconductor wafer with infrared rays.

16. 16. The method for cleaning a semiconductor wafer according to claim 1, wherein, when the pretreatment is performed in the fourth step, the first to third steps are repeated thereafter, and after it is determined that the pretreatment is not required again, the fifth step is performed.

17. The semiconductor wafer cleaning method according to any one of claims 1 to 16, wherein in the fifth step, first, spin cleaning with ozone water is performed, and then, one or more sets of a combination of spin cleaning with hydrofluoric acid and subsequent spin cleaning with ozone water are performed.

18. The method for cleaning a semiconductor wafer according to any one of claims 1 to 17, wherein the semiconductor wafer is a silicon wafer.

19. A method for producing a semiconductor wafer, comprising the method for cleaning a semiconductor wafer according to any one of claims 1 to 18.

Citation Information

Patent Citations

  • Method for manufacturing semiconductor device

    JP1997321009A

  • Apparatus and method for processing substrate

    JP2007165366A

  • Wafer cleaning method

    JP2015220284A