Concrete oyster attachment base and manufacturing method, construction method for marine ecological project

A lightweight concrete adhesion base with controlled alkalinity and biocalcium promotes rapid oyster attachment and growth, addressing slow attachment rates and alkalinity issues in traditional methods, enhancing marine project durability and ecological benefits.

JP7563779B2Active Publication Date: 2024-10-08HARBIN ENG UNIV
View PDF 25 Cites 0 Cited by

Patent Information

Application Number
JP2022533425
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-02
Filing Date
2020-12-01
Publication Date
2024-10-08
Estimated Expiration
2040-12-01

AI Technical Summary

Technical Problem

Traditional aquaculture methods struggle to meet the increasing demand for oysters due to slow attachment rates on substrates, and existing oyster adhesion bases release high alkalinity that inhibits larval attachment and change color, making them less attractive for oysters.

Method used

A lightweight concrete adhesion base with controlled water-cement ratio, low alkalinity, and added biocalcium, calcium carbonate, and trace elements, combined with dark pigments and fibers, to promote early oyster attachment and growth, while maintaining durability and resistance to extreme loads.

Benefits of technology

The solution enhances oyster attachment rates, reduces transportation and labor costs, and increases the durability of marine projects, allowing oysters to purify water bodies effectively.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563779000007
    Figure 0007563779000007
  • Figure 0007563779000008
    Figure 0007563779000008
  • Figure 0007563779000009
    Figure 0007563779000009
Patent Text Reader

Abstract

This technology is related to oyster attachment technology, particularly concrete oyster attachment bases and their manufacturing and construction methods. The concrete oyster attachment bases are characterized by their ability to rapidly attract and transform sessile organisms, promote long-term growth, and provide excellent durability. By applying the material to the concrete surface and rationally arranging the spaces between them, each concrete pile (lump) effectively dissipates waves and ensures smooth exchange of water between both sides. After the oysters attached to each concrete pile (lump) have significantly multiplied, the water body is purified, improving the ecological environment of the surrounding sea area.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority to Chinese Patent Application No. 201911210542.0, filed on December 2, 2019, for "Rough-surfaced cement concrete oyster attachment base and manufacturing method thereof," and claims the benefit of priority to Chinese Patent Application No. 201911210403.8, filed on December 2, 2019, for "Construction method for marine ecological projects," the entire contents of which are incorporated herein by reference.

[0002] The present invention relates to the technology of oyster attachment base and the construction technology of marine ecological projects, in particular to a concrete oyster attachment base and a manufacturing method thereof, and a construction method thereof, which belongs to the interdisciplinary field of marine sessile organisms and concrete. [Background technology]

[0003] With the improvement of people's living standards, the demand for oysters as a health food is increasing. Traditional small-scale aquaculture and farming methods cannot meet the growing demand for oysters. At the same time, with the increase in the amount of oyster reef restoration and the construction of marine ecological projects such as oyster reefs, the demand for oyster attachment substrates is increasing. Common farming methods include crack-building farming, ground seeding farming, bridge stone and standing stone farming, and hanging farming, but there is a problem that it takes a long time for oysters to reach a sufficient attachment rate on the attachment substrate. In addition, with the increase in the amount of oyster farming, the oyster attachment substrate of shellfish such as the shell of the mussel cannot fully meet the needs of oyster larvae, and the price of shellfish attachment substrates is rising. In addition, in patent application CN106719186 recently filed by Ocean University of China, a new oyster attachment base was produced by mixing 15%-20% shell powder and 5%-15% shell waste into the cement paste mass, the shell waste roughens the surface of the attachment base and increases the amount of oysters that attach, the shell waste is easier to collect seedlings from than the shells of the sea mussel, and has a superior larval attachment effect. However, since the water reducer is not taken into consideration in controlling the amount of water used and curing, the permeability of the concrete is determined by the water-cement ratio and curing. As a result, a large amount of alkali contained in the adhesion base is released, increasing the alkalinity of the seawater that comes into contact with it, and inhibiting the attachment of oyster larvae. In particular, when larvae are raised in aquaculture ponds, if the water area is small, the pH value of the water area will rise and the oyster larvae may die. At the same time, if a large amount of shell powder is mixed in, the color of the cement adhesion base will change from dark gray to a light color, which is unfavorable for oyster attachment. Summary of the Invention

[0004] The object of the present invention is to provide a durable lightweight concrete adhesion base that induces sessile organisms to attach quickly and densely to the concrete surface, thereby solving the problems that currently exist: due to the lack of control over the amount of water used and curing (the permeability of concrete is determined by the water-cement ratio and curing), a large amount of alkali contained in the adhesion base is released, increasing the alkalinity of seawater that comes into contact with it, inhibiting the attachment of marine sessile organism larvae, and at the same time, due to the mixing of a large amount of shell powder, the color of the cement adhesion base changes from dark gray to a light color, which is unfavorable for oyster attachment.

[0005] The realization method of the present invention is as follows. The present invention reduces the amount of segments used in the adhesion base, selects the appropriate cement type, adds appropriate mineral admixtures, obtains low-alkalinity cement, and at the same time controls the water-cement ratio of the concrete of the adhesion base, controls its release rate, and mixes in adhesion color, biocalcium, calcium carbonate and trace elements according to the preferences of oysters, thus promoting the early attachment, metamorphosis and later growth of oysters, and designing the structure of the adhesion base. In addition, the adhesion base is directly attached to the larvae in the culture pond, and does not need to be used after being immersed in seawater for a long time. If there is no severe collision or destruction, the service life of the adhesion base can be more than 50 years.

[0006] By using lightweight aggregate concrete, the weight of the concrete attachment base can be reduced, and transportation and labor costs can be reduced during the manufacturing, transportation, and curing of test specimens. In addition, in actual marine aquaculture, the labor costs of fishermen who move the attachment base to harvest oysters can be reduced, and costs such as transportation and fixing of concrete projects can be reduced. Furthermore, the risk of the concrete accidentally falling to the ground and being damaged during use can be reduced.

[0007] The use of fibers can increase the strength of concrete, especially its tensile strength. In the present invention, the combination of alkali-resistant fibers with eco-concrete improves the crack resistance, bending resistance, and fatigue resistance of concrete. It can reduce early cracking of concrete when applied to breakwater members, reduce the failure rate of members during transportation and fixing at the seaside, and increase the ability to withstand extreme loads, especially typhoons.

[0008] The present invention further has the following structural features.

[0009] The ingredients of the material include cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water, dark color pigment, bio-calcium powder, calcium carbonate powder, trace elements, short fiber, and superplasticizer, and the weight percentages thereof are 21.8%-34.5%, 24.6%-37.5%, 15.8%-29.6%, 8.4%-16.4%, 0.6%-3.0%, 0.4%-2.0%, 0.4%-2.0%, 0.2%-1.8%, 0.15%-1.5%, and 0.03%-0.18%, respectively.

[0010] Preferably, the deep color pigment is one or two of iron black, aniline black, carbon black, antimony sulfide, red iron oxide, and organic pigment red.

[0011] Preferably, the dark pigments are modified with one of the following materials depending on their impact on the performance of the concrete: transparent resin, organosilicon, dimethylsiloxane, and superhydrophobic material.

[0012] Preferably, the bio-calcium powder is cow bone powder, and the bio-calcium carbonate powder includes one or more combinations of oyster shell powder, fish bone powder, eggshell powder, and coral powder, and the fineness thereof is 100 mesh to 1000 mesh.

[0013] Preferably, the biocalcium powder is prepared by treating eggshell powder, coral powder, oyster shell powder and fish bone powder of 100 mesh to 500 mesh with one or two of ethanoic acid, acetic acid, silicic acid and sulfurous acid, and treating cow bone powder of 100 mesh to 500 mesh with one or two of diluted phosphoric acid, sulfuric acid, hydrochloric acid and nitric acid.

[0014] Preferably, the calcium carbonate powder is one or more of calcite, chalk, limestone, marble, aragonite, travertine powder, and processed precipitated calcium carbonate, activated calcium carbonate, calcium carbonate whiskers, and ultra-fine precipitated calcium carbonate, and has a fineness of greater than 200 mesh.

[0015] Preferably, the trace elements zinc, iron, potassium and phosphorus are modified by selecting natural minerals, industrial products or chemical reagents including one or more of zinc sulfate, calcium phosphate, zinc phosphate, potassium sulfate, potassium nitrate, iron sulfate, ammonium nitrate, potassium phosphate, ammonium phosphate and iron phosphate to achieve sustained release of the corresponding ions and reduce or eliminate the adverse effects on the performance of concrete. However, in the case of eutrophication areas, materials containing nitrogen or phosphorus elements are not selected.

[0016] Preferably, the cementitious material is one of Portland cement mixed with mineral admixtures, sulfoaluminate cement, and alkali-activated cementitious material, where the Portland cement mixed with mineral admixtures includes one or more combinations of silica fume, slag powder, and fly ash, the sulfoaluminate cement includes one or two of fast-setting sulfoaluminate cement, high-strength sulfoaluminate cement, and expanded sulfoaluminate cement, and the alkali-activated cementitious material includes one of alkali-activated slag and alkali-activated slag + fly ash.

[0017] Preferably, the short fibers are inorganic fibers (length 12 to 20 mm) including one or more of basalt fibers, alkali-resistant glass fibers, and carbon fibers.

[0018] Preferably, the lightweight coarse aggregate is one or two of crushed lightweight porous basalt, lightweight ceramsite having a maximum particle size of less than 20mm.

[0019] Preferably, the lightweight fine aggregate is one or two of crushed zeolite and lightweight ceramic sand, and has a particle size of 0.2 mm to 5 mm.

[0020] A method for manufacturing a rough-surfaced cement concrete oyster-attached base, comprising: Step S1 of designing different roughness according to the preferred characteristics of oyster larvae to attach to rough surfaces, and then manufacturing molding forms with different roughness; Step S2 of measuring the cementitious material, the lightweight coarse aggregate, the lightweight fine aggregate, the water, the dark color pigment, the bio-calcium powder, the calcium carbonate powder, the trace elements, the short fibers and the superplasticizer; First, put the lightweight coarse aggregate and the lightweight fine aggregate into the concrete mixer and mix for 0.5-1 minute, then add the cementitious material, dark color pigment, bio-calcium powder, calcium carbonate powder and trace elements and mix for another 1-2 minutes, then add short fiber, water and superplasticizer and mix for 2-6 minutes, and then mix evenly, then pour and vibrate; step S3; The concrete specimens are placed in a high-concentration CO2 curing box according to the circumstances and cured for 0.5 to 5 hours to reduce the alkalinity of the cement specimens. Then, they are cured for 28 days as standard or according to the actual circumstances. A method for producing a rough-surfaced cement concrete oyster-attached base, characterized in that step S4 can produce a rough-surfaced cement concrete oyster-attached base having an excellent attracting effect.

[0021] The objective of the present invention is to provide a method for constructing a marine project, so that oysters can be attached quickly and densely to the surface of the marine project, the durability of the marine project can be improved, and the oysters, as "ecological engineers", can purify the water body and restore the ecosystem, thus realizing a highly ecological marine project.

[0022] The construction method of the present invention comprises the following parts:

[0023] (1) Survey of marine areas for constructing ecological projects; (2) Manufacturing of a cement-based attachment base; (3) Timely and quantitative harvesting and cultivation of oyster larvae; (4) Design of concrete components; (5) Manufacturing of concrete components; (6) Placement of concrete specimens; (7) On-site placement of oyster attachment substrates; (8) Management and monitoring of larval attachment.

[0024] The specific technical solutions are as follows:

[0025] (1) The survey of the marine area where the ecological project described in (1) will be constructed shall include investigating the dominant species of oysters in said marine area and the presence or absence of oysters attached thereto, and also investigating the air temperature, seawater temperature, dissolved oxygen, planktonic organisms, total dissolved inorganic nitrogen, active phosphate, active silicate, Ca in said marine area in different seasons. 2+ , Zn 2+ , K + The study will involve investigating these issues, and will also look into the number of typhoons that have occurred in the past and their intensity.

[0026] The manufacture of the cement-based adhesive base described in (2) involves the manufacture of a lightweight concrete oyster adhesive base having a rough surface, which is one of a plate-shaped adhesive base, a corrugated adhesive base, and a cylindrical adhesive base.

[0027] The timely and quantitative harvest and cultivation of oyster larvae described in (3) is carried out by placing an attachment base in a nearby sea area during the period when the floating oyster larvae in the local sea area are concentrated and attach to the sea and metamorphose, and the attachment amount of oyster larvae is 15 to 25 oysters / 100 cm. 2 In this case, seedling collection is stopped and the attached substrate is then moved to an area of ​​the sea where food is abundant, for floating culture.

[0028] The design of the concrete members described in (4) takes into consideration the impact of oyster attachment on the environment and wave dissipation, and the concrete members of the ecological project are constructed to maximize the amount of oyster attachment and provide space for other organisms. In order to do so, the members have an internal void ratio of >40%, are thin-walled, and have multiple openings, and several inclined columns are installed on top of them. The size of the members is 0.5 to 15 cubic meters.

[0029] The concrete components described in (5) are manufactured by using fiber-reinforced eco-concrete, which is highly attractive to marine sessile organisms, and by using elastic molds to manufacture components of special shapes, particularly groove structures with larger interiors and smaller exteriors, and by determining the curing method according to the concrete mix ratio, its alkalinity and seepage resistance.

[0030] The placement of the concrete specimens described in (6) is such that in the second year, planktonic oyster larvae are dispersed during the period when they will be concentrating in local waters to attach and metamorphose, and the concrete members are connected with ropes to take into account the interaction of multiple specimens.

[0031] The on-site deployment of the oyster attachment base described in (7) involves transporting the attachment base for oysters at the mature stage of gonad development in (3) to the construction area of ​​the marine ecological project, placing a rough-surfaced lightweight concrete oyster attachment base on each component, and fastening it to the concrete components with ropes. In addition, according to the conditions of planktonic organisms in the local sea area, feed or feed nutrients are added as necessary.

[0032] The management and monitoring of oyster larvae attachment described in (8) involves monitoring the attachment status of oyster larvae on the concrete surface and determining whether the attachment density of oyster larvae is 30-40 / 100cm. 2 In this case, the rough surface of the lightweight concrete oyster attachment base is removed, and the ecological condition of the breakwater is monitored in the long term, and improvement measures are taken according to the actual situation.

[0033] Regarding the concentrated attachment metamorphosis period of oyster larvae described in the specific measures in (6), it is generally from May to August in North China and from April to October in South China.

[0034] The thin-walled, multi-opening member described in the specific measure in (4) is a concrete member with an internal void ratio of 40%-90% and several inclined columns installed thereon, which includes a base and a thin-walled, hollow concrete housing connected to the base, and six or more concrete rods are installed in the housing. The housing can be one of a sphere, a cube, etc., and the concrete rods can be one of a cylinder, a rectangle, etc.

[0035] Regarding the concrete curing method described in the specific measures in (5), the concrete curing method and curing time are determined based on the concrete mix ratio. For example, concrete made with Portland cement is cured with CO2 and the curing time is 0.5 to 5 hours.

[0036] In the cement-based bioadhesion base described in the specific measures in (3), a round hole with a diameter of 3 to 5 mm is created during molding, and the size of the plate-shaped attachment base is 10 x 10 x 2 to 3 cm.

[0037] The ropes mentioned in the specific measures in (7) are one of palm ropes, glass fiber ropes, and basalt fiber ropes.

[0038] For the lightweight concrete adhesion base with a rough surface described in the specific measures in (2), the ingredients of the material are cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water, dark color pigment, bio-calcium powder, calcium carbonate powder, trace elements, short fiber, and superplasticizer, and the weight percentages thereof are 21.8%~34.5%, 24.6%~37.5%, 15.8%~29.6%, 8.4%~16.4%, 0.6%~3.0%, 0.4%~2.0%, 0.4%~2.0%, 0.2%~1.8%, 0.15%~1.5%, and 0.03%~0.18%, respectively.

[0039] Preferably, the deep color pigment is one or two of iron black, aniline black, carbon black, antimony sulfide, red iron oxide, and organic pigment red.

[0040] Preferably, the dark pigments are modified with one of the following materials depending on their impact on the performance of the concrete: transparent resin, organosilicon, dimethylsiloxane, and superhydrophobic material.

[0041] Preferably, the bio-calcium powder is cow bone powder, and the bio-calcium carbonate powder includes one or more combinations of oyster shell powder, fish bone powder, eggshell powder, and coral powder, and the fineness thereof is 100 mesh to 1000 mesh.

[0042] Preferably, the biocalcium powder is prepared by treating eggshell powder, coral powder, oyster shell powder and fish bone powder of 100 mesh to 500 mesh with one or two of ethanoic acid, acetic acid, silicic acid and sulfurous acid, and treating cow bone powder of 100 mesh to 500 mesh with one or two of diluted phosphoric acid, sulfuric acid, hydrochloric acid and nitric acid.

[0043] Preferably, the calcium carbonate powder is one or more of calcite, chalk, limestone, marble, aragonite, travertine powder, and processed precipitated calcium carbonate, activated calcium carbonate, calcium carbonate whiskers, and ultra-fine precipitated calcium carbonate, and has a fineness of greater than 200 mesh.

[0044] Preferably, the trace elements zinc, iron, potassium and phosphorus are modified by selecting natural minerals, industrial products or chemical reagents including one or more of zinc sulfate, calcium phosphate, zinc phosphate, potassium sulfate, potassium nitrate, iron sulfate, ammonium nitrate, potassium phosphate, ammonium phosphate and iron phosphate to achieve sustained release of the corresponding ions and reduce or eliminate the adverse effects on the performance of concrete. However, in the case of eutrophication areas, materials containing nitrogen or phosphorus elements are not selected.

[0045] Preferably, the cementitious material is one of Portland cement mixed with mineral admixtures, sulfoaluminate cement, and alkali-activated cementitious material, where the Portland cement mixed with mineral admixtures includes one or more combinations of silica fume, slag powder, and fly ash, the sulfoaluminate cement includes one or two of fast-setting sulfoaluminate cement, high-strength sulfoaluminate cement, and expanded sulfoaluminate cement, and the alkali-activated cementitious material includes one of alkali-activated slag and alkali-activated slag + fly ash.

[0046] Preferably, the short fibers are inorganic fibers (length 12 to 20 mm) including one or more of basalt fibers, alkali-resistant glass fibers, and carbon fibers.

[0047] Preferably, the lightweight coarse aggregate is one or two of crushed lightweight porous basalt, lightweight ceramsite having a maximum particle size of less than 20mm.

[0048] Preferably, the lightweight fine aggregate is one or two of crushed zeolite and lightweight ceramic sand, and has a particle size of 0.2 mm to 5 mm.

[0049] The method for manufacturing a cement concrete oyster-attached base is as follows: Step S1 of designing different roughness according to the preferred characteristics of oyster larvae to attach to rough surfaces, and then manufacturing molding forms with different roughness; Step S2 of measuring the cementitious material, the lightweight coarse aggregate, the lightweight fine aggregate, the water, the dark color pigment, the bio-calcium powder, the calcium carbonate powder, the trace elements, the short fibers and the superplasticizer; First, put the lightweight coarse aggregate and the lightweight fine aggregate into the concrete mixer and mix for 0.5-1 minute, then add the cementitious material, dark color pigment, bio-calcium powder, calcium carbonate powder and trace elements and mix for another 1-2 minutes, then add short fiber, water and superplasticizer and mix for 2-6 minutes, and then mix evenly, then pour and vibrate; step S3; The concrete specimens are placed in a high-concentration CO2 curing box according to the circumstances and cured for 0.5 to 5 hours to reduce the alkalinity of the cement specimens. Then, they are cured for 28 days as standard or according to the actual circumstances. and step S4, which can produce a cement concrete oyster attachment base having a rough surface with excellent attracting effect.

[0050] The fiber-reinforced eco-concrete described in the specific measures in step (5) is composed of cementitious material, crushed stone, sand, water, dark pigment, bio-calcium powder, calcium carbonate powder, trace elements, short fiber and superplasticizer, and the weight percentages of the cementitious material, crushed stone, sand, water, dark pigment, bio-calcium powder, calcium carbonate powder, trace elements, short fiber and superplasticizer are 12.5%-22.0%, 39.4%-49.8%, 24.9%-37.3%, 6.2%-8.7%, 0.2%-1.7%, 0.15-1.0%, 0.15-1.0%, 0.1%-1.0%, 0.1%-1.0% and 0.02%-0.1% respectively.

[0051] The raw materials of the fiber-reinforced eco-concrete described in the specific measures in step (5) are as follows:

[0052] Preferably, the dark pigment is one or two of iron black, aniline black, carbon black, antimony sulfide, red iron oxide, and organic pigment red. In addition, depending on the degree of influence on the performance of concrete, these pigments are modified, and one of transparent resin, organosilicon, dimethylsiloxane, and superhydrophobic material is used for the modification treatment.

[0053] Preferably, the bio-calcium powder is cow bone powder, and the bio-calcium carbonate powder includes one or more combinations of oyster shell powder, fish bone powder, eggshell powder, and coral powder, and the fineness thereof is 100 mesh to 1000 mesh.

[0054] Preferably, the method for modifying the bio-calcium powder is to treat eggshell powder, coral powder, oyster shell powder and fish bone powder of 100 mesh to 500 mesh with one or two of ethanoic acid, acetic acid, silicic acid and sulfurous acid, and treat cow bone powder of 100 mesh to 500 mesh with one or two of diluted phosphoric acid, sulfuric acid, hydrochloric acid and nitric acid.

[0055] Preferably, the calcium carbonate powder is one or more of calcite, chalk, limestone, marble, aragonite, travertine powder, and processed precipitated calcium carbonate, activated calcium carbonate, calcium carbonate whiskers, and ultra-fine precipitated calcium carbonate, and has a fineness of greater than 200 mesh.

[0056] Preferably, the trace elements are zinc, iron, potassium and phosphorus, which are modified with natural minerals, industrial products or chemical reagents, including one or more of zinc sulfate, calcium phosphate, zinc phosphate, potassium sulfate, potassium nitrate, iron sulfate, ammonium nitrate, potassium phosphate, ammonium phosphate and iron phosphate, to achieve sustained release of the corresponding ions and reduce or eliminate the adverse effects on the performance of concrete. However, in the case of eutrophication areas, do not select materials containing nitrogen or phosphorus elements.

[0057] Preferably, the short fibers are inorganic fibers (length 12 to 40 mm) selected from the group consisting of basalt fibers, alkali-resistant glass fibers, and carbon fibers.

[0058] Preferably, the cementitious material is one of Portland cement mixed with mineral admixtures, sulfoaluminate cement, and alkali-activated cementitious material, where the Portland cement mixed with mineral admixtures includes one or more combinations of silica fume, slag powder, and fly ash, the sulfoaluminate cement includes one or two of fast-setting sulfoaluminate cement, high-strength sulfoaluminate cement, and expanded sulfoaluminate cement, and the alkali-activated cementitious material is one of alkali-activated slag and alkali-activated slag + fly ash.

[0059] Preferably, the sand is one or more of river sand, machine-made sand (parent material is basalt or granite), or desalinated sea sand.

[0060] The manufacturing method of fiber reinforced eco-concrete is as follows: Step S1: weighing cementitious material, crushed stone, sand, water, dark color pigment, biocalcium powder, calcium carbonate powder, trace elements, short fibers, and superplasticizer; First, crushed stone and sand are put into a concrete mixer and mixed for 0.5 to 1 minute, then cementitious material, dark color pigment, bio-calcium powder, calcium carbonate powder and trace elements are added and mixed for another 0.5 to 1 minute, then short fiber, water and superplasticizer are added and mixed for 3 to 8 minutes, and after uniform mixing, the mixture is poured and vibrated, and then the mixture is cured for 28 days as standard or according to actual conditions, so that fiber-reinforced eco-concrete can be produced in step S2.

[0061] The raw materials of the fiber-reinforced eco-concrete described in the specific measures in step (5) are dark pigment, cementitious material, crushed stone, sand, water and superplasticizer, of which the weight percentages of dark pigment, cementitious material, crushed stone, sand, water and superplasticizer are 0.2%-1.7%, 12.5%-22.0%, 39.4%-49.8%, 24.9%-37.3%, 6.2%-8.7% and 0.02%-0.1%, respectively.

[0062] The raw materials of the fiber-reinforced eco-concrete described in the specific measures in step (5) are cow bone powder, cementitious material, crushed stone, sand, water and superplasticizer, of which the weight percentages of cow bone powder, cementitious material, crushed stone, sand, water and superplasticizer are 0.15%-1.37%, 12.5%-22.0%, 39.4%-49.8%, 24.9%-37.3%, 6.2%-8.7% and 0.02%-0.1%, respectively.

[0063] The raw materials of the fiber-reinforced eco-concrete described in the specific measures in step (5) are calcium carbonate powder, cementitious material, crushed stone, sand, water and superplasticizer, in which the weight percentages of calcium carbonate powder, cementitious material, crushed stone, sand, water and superplasticizer are 0.15%-1.37%, 12.5%-22.0%, 39.4%-49.8%, 24.9%-37.3%, 6.2%-8.7% and 0.02%-0.1%, respectively.

[0064] The beneficial effects of the present invention are as follows:

[0065] The present invention utilizes the dilute acid modification and composite crushing technology to fully exert the attracting ability of cow bone powder, greatly reducing the dosage of cow bone powder, and carrying out anti-corrosion treatment and modification to produce a composite attractant mainly made of cow bone powder, which has a low dosage, high oyster larvae attachment ability, and solves the problem of mold growth on concrete. The amount of oyster larvae attached to concrete mixed with the attractant is significantly higher than that of concrete without the attractant.

[0066] The present invention allows marine projects to be constructed, oysters to be attached to the projects at a higher density, the durability of the marine projects to be improved, and based on the characteristics of oysters as "ecological engineers" to purify water bodies and improve water areas, a very ecological marine project can be realized. [Brief description of the drawings]

[0067] [Figure 1] This is a situation where mold grows on the surface of concrete containing 10% cow bone powder with a different mix ratio (under standard curing). [Diagram 2] The powder size is 200 mesh, and the mixing ratio is different when 10% modified cow bone powder is mixed. [Diagram 3] FIG. 1 is a schematic diagram of a 210-day actual marine adhesion experiment. [Figure 4] FIG. 1 is a schematic diagram of a 300-day actual marine adhesion experiment. [Diagram 5] FIG. 1 is a schematic diagram of a concrete oyster attachment base. [Figure 6] FIG. 1 is a schematic diagram of a concrete oyster attachment base. [Figure 7] FIG. 1 is a schematic diagram of a concrete oyster attachment base. [Figure 8] Design schematic diagram of biomimetic concrete member. In Fig. 8, 1. concrete thin wall with thickness of about 5 cm, 2. concrete bar with length of about 1.5 m, 3. base of thin wall structure, 4. connection reinforcement area of ​​concrete bar, 5. through holes with different diameters. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0068] The invention will now be further described with reference to the drawings and specific embodiments.

[0069] These examples are used only to illustrate the present invention and are not intended to limit the scope of the present invention.

[0070] The implementation methods of Examples 1 to 21 are the same, but the concrete mix ratios are as shown in the following examples. The present invention uses the above concrete to design concrete hook attachment bases with different shapes, specifically, see Figures 5 to 7.

[0071] In Example 1, the concrete mix ratio of ordinary Portland cement is as follows: ordinary Portland cement, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water-reducing agent powder are 29.37%, 33.53%, 24.48%, 12.59% and 0.03% by weight, respectively.

[0072] Wherein, the lightweight coarse aggregate is one or two of crushed lightweight porous basalt and lightweight ceramsite with a maximum particle size of less than 20mm. The lightweight fine aggregate is one or two of crushed zeolite and lightweight ceramic sand, with a particle size of 0.2mm-5mm and high grade. The water needs to meet the quality standard for water for concrete (JGJ63-2006), with Cl- content <1000mg / L, PH value >4.5, and has little effect on the initial setting time difference and final setting time, strength, and permeability of cement. In addition, the above materials selected in Examples 1 to 21 are the same.

[0073] For Example 2, the standard concrete mix ratio, the weight percentages of ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water-reducing agent powder were 17.62%, 1.47%, 10.28%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.

[0074] The weight percentages of Example 3, unmodified dark pigment, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 1.47%, 17.62%, 1.29%, 8.99%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.

[0075] In Example 4, the weight percentages of the modified dark pigment (mass ratio of iron black:aniline black mixture = 1:1), ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 0.87%, 17.62%, 1.36%, 9.52%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.

[0076] The weight percentages of Example 5, modified dark pigment (mass ratio of iron black:aniline black mixture = 1:1), ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 1.47%, 17.62%, 1.29%, 8.99%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.

[0077] The weight percentages of Example 6, modified dark pigment (mass ratio of iron black:aniline black mixture = 1:1), ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 2.35%, 17.62%, 1.17%, 8.23%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.

[0078] The modified dark pigment is 196 transparent resin, mixed with 3% hardener and 1.5% accelerator, and the volume ratio of pigment to resin is 1:0.2. It is cured at room temperature for 4 hours and then cured at 60℃ for 4 hours. Then, it is crushed by beating and crushed by vibration mill until the powder size exceeds 400 mesh.

[0079] In Example 7, the weight percentages of calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 0.87%, 17.62%, 1.36%, 9.52%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.

[0080] In Example 8, the weight percentages of calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 1.47%, 17.62%, 1.29%, 8.99%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.

[0081] In Example 9, the weight percentages of calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 2.35%, 17.62%, 1.17%, 8.23%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.

[0082] In Example 10, the weight percentages of modified dark pigment (iron black:aniline black mixture in a mass ratio of 1:1), calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 1.47%, 0.87%, 17.62%, 1.18%, 8.23%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.

[0083] In Example 11, the weight percentages of modified dark pigment (iron black:aniline black mixture in a mass ratio of 1:1), calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 1.47%, 1.47%, 17.62%, 1.10%, 7.71%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.

[0084] In Example 12, the weight percentages of modified dark pigment (iron black:aniline black mixture in a mass ratio of 1:1), calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 1.47%, 2.35%, 17.62%, 0.99%, 6.94%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.

[0085] In Example 13, the weight percentages of unmodified cow bone powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water-reducing agent powder were 1.47%, 17.62%, 1.29%, 8.99%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.

[0086] In Example 14, the weight percentages of modified cow bone powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 0.87%, 17.62%, 1.36%, 9.52%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.

[0087] In Example 15, the weight percentages of modified cow bone powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 1.47%, 17.62%, 1.29%, 8.99%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.

[0088] In Example 16, the weight percentages of modified cow bone powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 2.35%, 17.62%, 1.17%, 8.23%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.

[0089] The method for modifying the beef bone powder is as follows: add 100 mesh beef bone powder to a 2% concentration phosphoric acid solution, the weight ratio of the two is 1:3, the temperature is 20-30°C, mix with a mixer at 200-500 revolutions / min for 30 minutes, centrifuge with a centrifuge at 3000-5000 revolutions / min for 3 minutes, discard the supernatant, and wash the centrifuged solid with water 2-3 times, the washing water is not acidic, vacuum dry the centrifuged solid at 40°C, mix the dried beef bone powder with slag powder at 1:4, and crush with a vibration mill until the fineness exceeds 200 mesh, and prepare for use.

[0090] In Example 17, the weight percentages of calcium carbonate powder, zinc sulfate, modified dark pigment (iron black:aniline black mixture in a mass ratio of 1:1), ordinary Portland cement, blast furnace slag powder, silica fume, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 2.35%, 0.5%, 1.47%, 17.62%, 0.93%, 6.50%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.

[0091] In Example 18, the weight percentages of calcium carbonate powder, zinc sulfate, modified dark pigment (iron black:aniline black mixture in a mass ratio of 1:1), ordinary Portland cement, blast furnace slag powder, silica fume, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 2.35%, 1.2%, 1.47%, 17.62%, 0.84%, 5.89%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.

[0092] In Example 19, the weight percentages of zinc sulfate, modified dark pigment (mass ratio of iron black:aniline black mixture = 1:1), modified bio-calcium powder (modified cow bone powder:oyster shell powder = 2:1), calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 0.5%, 1.47%, 1.47%, 0.87%, 17.62%, 0.94%, 6.50%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.

[0093] In Example 20, the weight percentages of zinc sulfate, modified dark pigment (mass ratio of iron black:aniline black mixture = 1:1), bio-calcium powder (modified cow bone powder:oyster shell powder = 2:1), calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 0.6%, 1.47%, 1.47%, 0.87%, 17.62%, 0.92%, 6.42%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.

[0094] The method of modifying zinc sulfate is as follows: select diatomaceous earth with SiO2 content >90% and fineness of 600 mesh, add 150g water in a mixer at 60°C, then add 100g zinc sulfate, stir until completely dissolved, and prepare for use; then heat 150g of the above diatomaceous earth to 60°C, add it to the solution, stir for 10 minutes in a mixer with a rotation speed of 200-500 revolutions / min, and then dry in a drying oven with a drying temperature of 100°C to obtain the modified zinc sulfate.

[0095] In Example 21, the weight percentages of zinc sulfate, modified dark pigment (iron black:aniline black mixture in a mass ratio of 1:1), modified bio-calcium powder (modified cow bone powder:oyster shell powder in a ratio of 2:1), calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water, short fiber and polycarboxylate water reducer powder are 0.5%, 1.47%, 1.47%, 0.87%, 17.62%, 0.94%, 6.50%, 33.07%, 24.14%, 12.59%, 0.8%, and 0.03%, respectively.

[0096] The specific operation steps of the methods of carrying out Examples 1 to 21 are as follows:

[0097] According to the above-mentioned rough surface cement concrete oyster attachment base manufacturing method, three Φ100×50mm cylindrical specimens and five 200×200×30mm rectangular specimens are manufactured, which are respectively used to test the concrete's 28-day chloride ion penetration resistance and the oyster larvae attachment transformation situation in the laboratory after 28-day standard curing. The specific operation steps are as follows:

[0098] (1) Formation of specimen

[0099] 1. Calculate and accurately weigh out ordinary Portland cement, lightweight coarse aggregate, lightweight fine aggregate, water, dark color pigment, bio-calcium powder (modified cow bone powder: oyster shell powder = 2:1), calcium carbonate powder, trace elements, short fibers and superplasticizer according to the above mass.

[0100] 2. Sandpaper with different surface roughness (including 20 mesh, 60 mesh, and 200 mesh) was attached to the inside of the mold of the rectangular concrete specimen in preparation for use.

[0101] 3. First, put the lightweight coarse aggregate and lightweight fine aggregate into a concrete mixer and mix for 0.5 to 1 minute. Next, add ordinary Portland cement, bio-calcium powder (modified cow bone powder: oyster shell powder = 2:1), calcium carbonate powder, trace elements, and dark pigment, and continue mixing for 0.5 to 1 minute. After that, add short fiber, water, and superplasticizer and mix for 2 to 6 minutes. After mixing evenly, pour in and vibrate to cut out into molds, and three cylindrical specimens with Φ100×50mm and five rectangular specimens with 200×200×30mm will be obtained.

[0102] 4. The molded concrete specimens were immediately placed in a CO2 curing box under 10 atmospheres of pressure and cured for 2 hours to reduce the alkalinity of the cement specimens. They were then cured for 28 days as per the standard procedure, and permeability evaluations were performed for each stage. After 28 days, oyster larvae attachment and metamorphosis tests were performed in the laboratory.

[0103] (II) The specific steps of the rapid chloride ion permeability test are as follows:

[0104] According to the standard "Standard Test Method for Electrical Indication of Concrete's Ability to Resist Chloride Ion Penetration" (ASTM1202-2017), when curing for 28 days, take out three cylindrical specimens of Φ100×50mm from the curing chamber, and clean the water and impurities on their surfaces. After the surfaces are dried, apply a thin layer of epoxy to the surface of the cylindrical specimen. Then, place the specimen in a vacuum saturator for 20-24 hours. Then, take out the specimen, clean its surface, and place it in an organic glass mold. At the same time, detect the sealing between the specimen and the mold, and then put a 3% sodium chloride solution (electrode is connected to the negative pole of the power supply) and a 0.3 mol / L sodium hydroxide solution (electrode is connected to the positive pole of the power supply) into the mold on both sides. Then start the experimental equipment, and after 6 hours, record the test data, and repeat the above operations for the last two specimens. Finally, calculate the strength according to the norm.

[0105] (3) The specific steps of the laboratory oyster larvae attachment and metamorphosis test are as follows:

[0106] After 28 days of standard curing, the rectangular specimens of 200 x 200 x 30 mm were taken out of the curing room, and the water and impurities on their surfaces were washed off. Then, they were placed in a test pond to create a test pond in the laboratory, and the abundance of oyster larvae was 0.85ind / ml. 3 The seawater in the pond is sand-filtered seawater from the Yellow Sea, with a salinity of about 32% to 34%. After the seawater level is higher than the concrete specimen, oxygen pipes are evenly arranged in the test pond to prepare for throwing oyster larvae in. After slowly stirring the oyster larvae in the bucket, a beaker is used to accurately measure the mass of the seawater containing the oyster larvae, and then the mass is evenly thrown into the test pond.

[0107] After the oyster attachment attraction test began, the seawater in the test pond was replaced every day, with the amount of water replaced being 1 / 3 of the total capacity of the test pond. A screen (200 mesh or more) was used to block the drainage outlet to prevent unattached oyster larvae from being washed away with the water. The larvae on the screen were then thrown back into the test pond. Chlorella was fed at regular intervals and in quantitative amounts using a Pasteur pipette at 9:00 and 19:00 every day, and the attachment situation of the oysters was observed.

[0108] After the test has been continued for a specified age, the water in the test pond is drained, the specimens are taken out, and the number and survival rate of oysters on the surface of the specimens are counted, recorded and analyzed. For the statistics, the smooth bottom surface is used when pouring and molding the concrete.

[0109] Compared with Reference 1 (a novel concrete artificial reef and its manufacturing method CN104529286 A), the differences are as follows:

[0110] The object of the present invention is different from that of Reference 1, in which oyster shell powder is mixed into concrete, but the purpose is waste utilization, restoration and improvement of artificial fish reefs. The object of the present invention is to attract oyster larvae to attach.

[0111] Compared with Reference 2 (Biomimetic concrete artificial reef and its manufacturing method 2015 CN104938384 A), the differences are as follows:

[0112] (1) The object of the present invention is different from that of Reference 2, in which oyster shells or oyster shell powder are mixed into concrete, but the object is to improve the aquatic environment by attracting fish, microorganisms, and algae through biomimetic surface and increasing the number of microorganisms, and oysters are not mentioned. The object of the present invention is to attract oyster larvae to attach.

[0113] (2) According to Reference 2, biocalcium carbonate powder (150-200 mesh) less than 10% of the dosage of the segment is ineffective for attraction and attachment. However, in the course of research, it is found that the optimal dosage of bovine bone powder and biocalcium carbonate powder (fineness of 100-1000 mesh) is less than 10% of the cementitious material by using modified bovine bone powder and biocalcium carbonate powder.

[0114] (3) The modification of beef bone powder and biocalcium carbonate powder specifically involves treating eggshell powder, coral powder, oyster shell powder, and fish bone powder of 100 mesh to 500 mesh with one or two of ethanoic acid, acetic acid, silicic acid, sulfurous acid, etc., and treating beef bone powder of 100 mesh to 500 mesh with one or two of diluted phosphoric acid, sulfuric acid, hydrochloric acid, and nitric acid.

[0115] (4) In the references, it is difficult to embed oyster shells on the concrete surface, and not all project surfaces use this method, which is not feasible. The present invention adds shell powder into the concrete to attract organisms to attach, and the dosage of shell powder accounts for 10% of the cementitious material mass, which is easy to implement and can greatly improve the amount of oyster attachment.

[0116] (5) In recent years, serious corrosion of artificial reefs has been observed in marine environments. The serious corrosion is mainly caused by the combined action of biological sulfuric acid secreted by anaerobic microorganisms such as Thiobacillus subtilis and acidic substances secreted by other bacteria. However, calcium carbonate has very poor resistance to acid corrosion. If the content of calcium carbonate with large fineness is too high, it can cause serious acid corrosion.

[0117] Compared to Reference 3 (Fan Ruiliang. The effects of substrate type on oyster attachment, growth, population establishment and reef body development [D]), the differences are as follows:

[0118] (1) In Reference 3, take 80 mesh cow bone powder, calcium powder, and gypsum powder, and add them into concrete independently. The fineness of all calcium materials in this invention is more than 100 mesh, which is larger than the fineness of the materials in Reference 3. Similarly, modify the cow bone powder to mix it, taking into account the grading of concrete particles and its attracting ability.

[0119] (2) When the cow bone powder is ground by a vibrating mill under normal temperature conditions, after the fineness exceeds 80 mesh, the cow bone powder contains a large amount of collagen, so it becomes lumpy and cannot be ground further. In the present invention, by using the dilute acid modification technology and grinding together with other substances, cow bone powder with small particle size and modified bio-calcium powder with fineness > 200 mesh can be obtained. The obtained bio-calcium powder retains the original substance of bio-calcium, improves the release rate of the substance for attracting oyster larvae to attach, and reduces the dosage of bio-calcium powder, thereby reducing the impact on cement concrete performance.

[0120] (3) Bone powder contains a large amount of collagen and other organic substances. Mixing a large amount of these substances will reduce the strength and permeability of concrete. Especially when the dosage exceeds 5%, the strength of concrete will rapidly decrease, the permeability will be significantly reduced, and mold will grow on the concrete surface under standard curing conditions. Figure 1 shows the mold growing on the concrete surface. Figure 2 shows the surface of the modified concrete.

[0121] As can be seen from Figure 1, the mold on the concrete surface is white and cotton-like, covering almost the entire concrete surface, while when the cow bone powder, age and curing conditions are the same, there is no mold on the concrete surface in Figure 2.

[0122] The present invention utilizes the dilute acid modification and composite crushing technology to fully exert the attracting ability of cow bone powder, greatly reducing the dosage of cow bone powder, and carrying out anti-corrosion treatment and modification to produce a composite attractant mainly made of cow bone powder, which has a low dosage, high oyster larvae attachment ability, and solves the problem of mold growth on concrete. The amount of oyster larvae attached to concrete mixed with the attractant is significantly higher than that of concrete without the attractant.

[0123] As can be seen from the references and the materials examined, calcium content is essential for the attachment of oyster larvae, and some current test results also prove that adding an appropriate amount of calcium carbonate material to cement-based materials can promote the attachment and growth of oyster larvae. However, cement concrete contains a large amount of calcium ions, and the pH value of the pore solution is generally above 12.5, and at room temperature, the pH value of saturated calcium hydroxide solution is about 12, so the calcium ion concentration in the concrete pore solution is about 5 mmol / L, and the solubility of calcium carbonate is very low, at 25°C, it is 9.5×10 -5 mol / L(9.5×10 -2 Currently, the optimal range of calcium ion concentration for attracting oysters to attach is thought to be 10-25 mmol / L, and even when oyster larvae are placed in a saturated calcium carbonate solution, there is not enough Ca to provide the ion concentration suitable for oyster attachment. 2+ Furthermore, while Ca(OH)2 in cement concrete can be released quickly, it takes time for calcium carbonate to dissolve. Therefore, when calcium carbonate material is added to concrete to promote the attachment of oyster larvae, Ca 2+ It can be determined that HCO3 does not play a dominant role. - In the case of transformation, Ca 2+ Together with the calcium carbonate, a secondary shell of calcium carbonate is formed. After calcium carbonate is mixed in, it reacts with CO2 and water to generate Ca(HCO3)2, which is involved in adhesion and is the basic mechanism that promotes the adhesion of oyster larvae.

[0124] There is an optimal amount of calcium carbonate for cement-based materials, which can be explained by the following three aspects:

[0125] 1) With the same amount of substitute cement, as the dosage of calcium carbonate increases, the alkali in the concrete is diluted and the total alkalinity decreases. However, as the dosage of calcium carbonate increases, the probability of dissolving calcium carbonate in the concrete increases, and the amount of HCO3 in the solution increases. - The content is improved, which promotes the adhesion and transformation of oysters. However, if the dosage is too large, the permeability of concrete will increase rapidly, and the alkali and carbonate radicals in the concrete will rapidly leach out, the adverse effects of alkali will become obvious, and the critical effect or adverse effects of carbonate will begin to appear, resulting in a decrease in the adhesion amount; 2) With the same amount of substitute aggregate, with the increase in dosage, the permeability of concrete decreases, and the leaching of calcium ions and OH- decreases. However, the permeability of carbonate ions gradually improves and reaches a certain value, and the attachment of oysters reaches a maximum value. With the continued increase in dosage, calcium ions may decrease significantly and carbonate may also decrease. The calcium ion concentration limits the attachment of oyster larvae, which is manifested as a decrease in the amount of attachment. 3) With the same amount of alternative mineral admixture, the permeability improved with increasing dosage, and the increase in calcium carbonate reduced the amount of HCO3 required for oyster attachment. - As the concentration reaches the appropriate range, which is manifested as improved oyster larval attachment, and the mineral admixture dosage continues to increase, the mineral admixture dosage decreases, and the amount of leached alkali and carbonate increases, but the alkali and HCO3 - Too many ions inhibit the attachment of oyster larvae.

[0126] Compared to Reference 4 (Li Zhenzhen, Gong Pihai, Guan Changtao, et al. Bioadhesion effect of concrete artificial reefs with different cement types [J]. Progress in Fisheries Science, 2017, 38(5):57-63.), the differences are as follows:

[0127] In Reference 4, composite Portland cement, slag Portland cement, pozzolanic Portland cement, fly ash Portland cement and alumina cement are used, and in the present invention, ordinary Portland cement is mixed with mineral admixtures to realize low alkalinity segments, where silica fume is one of the mineral admixtures, which has high activity and its appropriate dosage has obvious effect on improving the durability of reinforced concrete in marine environment, and low alkalinity cement with excellent strength and durability can be obtained through optimization design and testing. At the same time, due to the high penetration prevention characteristics of silica fume concrete, even if the alkalinity inside the concrete is high, a large number of oyster larvae can attach, transform and grow. In addition, the low alkalinity sulfoaluminate cement is mixed to adjust the alkalinity of cement concrete and provide a suitable pH value for the attachment of oyster larvae. In addition, marine plants and sessile organisms such as oysters and barnacles have different alkali tolerances, and the environments required during the attachment and later stages are different; for example, barnacles and oysters require large amounts of calcium ions for attachment, metamorphosis, and later growth.

[0128] In Reference 4, concrete is used to attract marine organisms, which mainly starts from the size and diversity of the attached organisms, the main attached organisms being various algae. In the present invention, the research objective is to attract oysters to attach, but the alkali resistance of oysters and barnacles is higher than that of algae, and the attachment and transformation of oysters requires a large amount of calcium ions, so although the two types of concrete look similar, they are actually quite different. Figures 3 and 4 respectively show a comparison of the biofouling situation after about 210 days of actual sea attachment experiment in Reference 4 and the biofouling situation after 300 days of actual sea attachment experiment in the present invention.

[0129] The unique features and beneficial effects of the present invention are as follows:

[0130] Deep color pigment

[0131] Taking advantage of the phototaxis of oyster eyespot larvae, dark color pigments (one or two of iron black, aniline black, carbon black, antimony sulfide, red iron oxide, and organic pigment red) are mixed into the concrete to change the color of the concrete, making the concrete darker and making the oyster larvae think that it is a dark environment, attracting the oyster larvae to reach the dark colored concrete surface by themselves, increasing the probability of contact between the oyster larvae and the concrete surface, and increasing the probability of attracting the oyster larvae to attach. Specifically, it is as follows.

[0132] Marine biology researchers have studied the attachment of marine sessile organisms using different colored substrates to breed and grow or eliminate undesirable populations, which belongs to the field of marine biology. It is completely different from marine concrete engineering and concrete materials science, which are two major fields entirely. Through the interdisciplinary fusion of marine sessile organisms and concrete materials science, dark colored concrete is used to attract oyster larvae to attach. The present invention adds dark color pigments to darken the color of the concrete surface and promote the attachment of oyster larvae. Since other materials are mixed into the concrete, it affects the concrete performance. The present invention considers that concrete with different cements has different surface colors. Therefore, the dosage of the dark color material is determined based on the cement type and dosage. The dark color pigment also affects the concrete performance. Most importantly, the dark color pigment is mixed in while simultaneously reducing the alkali and Ca in the concrete. 2+ If the permeability of concrete is not controlled, the released alkali will affect the attachment, metamorphosis and growth of sessile organism larvae, and if the dosage exceeds a certain value, the amount of larvae attachment will decrease. In the present invention, the permeability prevention of concrete is designed and controlled, and the main measures are the selection of the type of dark color pigment, the control of the dosage and modification. With the increase in the dosage of dark color material, the amount of larvae attachment will increase, and when the dosage is 0.5% to 6% of the glued material, the amount of larvae attachment is the highest, but then increases slightly or remains unchanged.

[0133] trace elements

[0134] The oyster body contains a large amount of zinc, much higher than the seawater in which it lives, and at the same time, the oyster body contains a lot of Fe, P, and K elements. At the same time, adequate Zn in the solution 2+ and K + The concentration can promote the early attachment and metamorphosis of oyster larvae. Therefore, zinc sulfate, potassium sulfate, potassium nitrate, iron sulfate, zinc phosphate, ammonium nitrate, potassium phosphate, ammonium phosphate, iron phosphate, and calcium phosphate are used as trace elements and mixed into concrete, and the modification of these substances basically does not change the strength and penetration prevention properties of the concrete, but greatly improves the attachment attraction rate of oyster larvae. The details are as follows:

[0135] Marine biology researchers have studied the effects of different ions on the attachment and metamorphosis of marine sessile organisms, in order to clarify the attachment mechanism of oysters and the purpose of reproduction and growth, which belongs to the field of marine biology. It is quite different from marine concrete engineering and concrete materials science, which are two major fields entirely. Through the interdisciplinary fusion of marine sessile organisms and concrete materials science, it is possible to add corresponding substances into concrete, so that oyster larvae can live in it. ConIt can be seen that the inorganic salts are attracted to the cleat surface. Since soluble salts have a significant effect on concrete performance such as early workability, hardening time, and later strength and permeation resistance, the present invention uses diatomaceous earth as a carrier to fix these inorganic salts inside the diatomaceous earth, thereby reducing the effect of soluble salts on concrete performance, and at the same time, utilizing the effect of diatomaceous earth in improving concrete performance, it is possible to maintain the excellent mechanical properties and permeation resistance of concrete even when these attractants are added. In addition, since diatomaceous earth has a sustained release effect as a carrier, the release of soluble salts is relatively slow, and the release rate is maintained at a very low level, especially after immersion in seawater for a certain period of time. Therefore, similarly, this part of knowledge relates to the interdisciplinary fusion of marine sessile organisms, chemistry and marine concrete engineering, and whether a person skilled in the field of concrete engineering or a person skilled in the field of marine biology, due to the conventional background, cannot obtain technical characteristics closely related to concrete with excellent ability to attract oyster larvae to attach in the present invention by mixing trace elements into concrete, changing the ion content of trace elements on the concrete surface, and controlling the permeability of the concrete.

[0136] Permeability of concrete

[0137] The strength and permeability of concrete are the two most important performances of concrete. Adding different attractants into standard concrete will affect the performance of concrete, so when mixing different substances to promote the attachment, metamorphosis and subsequent growth of oyster larvae, first, it is necessary to control it as a whole so as not to have a significant effect on the strength and permeability of concrete; second, raw materials are selected according to the suitability of various raw materials; if the performance of the raw materials cannot meet the actual requirements, the desired function can be achieved by modifying them before adding the raw materials. However, in fact, the above-mentioned related studies consider the effect of calcium content on the attachment of oyster larvae, but do not consider the performance of the concrete itself, and do not consider the water-cement ratio, calcium content and curing, etc., and the change in the permeability of concrete will change the permeability of alkali and ions inside the concrete, and the lower the permeability of concrete, the higher the permeability of alkali and ions inside it will be, which may increase exponentially. Therefore, these released alkali and ions have a great impact on the larvae, changing from promoting attachment to inhibiting attachment, and this situation may be more serious, especially when the cement content is high. Therefore, it is necessary to ensure that the change in the permeability of the concrete by mixing the attractant into the concrete is within a controllable range, for example, the change does not exceed 10%, so that their attractant effects can be compared, otherwise the influence of mixing the attractant independently or mixing the attractants in combination on the attractant effect of the claw larvae cannot be evaluated.

[0138] It is necessary to grasp the optimum environment required for marine sessile organisms to attach, transform and grow later, and to design concrete starting from the seepage prevention of concrete, and not to ignore the fact that only considering the dosage of various raw materials will bring about changes in the seepage prevention of concrete. Therefore, similarly, this part of knowledge concerns the interdisciplinary fusion of marine sessile organisms, chemistry and marine concrete engineering, and whether one skilled in the art of concrete engineering or marine biology, according to the prior background, in the present invention, the overall control of the seepage prevention of concrete cannot obtain the technical characteristics that are closely related to the ability of the attractant to effectively attract oysters to attach.

[0139] Increased roughness

[0140] Rough surfaces provide better tactile stimulation for oyster larvae to crawl and attach, increasing the attachment force and extending the residence time of oyster larvae on the substrate; at the same time, the presence of cracks and holes can protect the larvae and reduce the possibility of being attacked by predators, and the attachment rate of oyster larvae is improved on rough attachment substrates because the surface area available for attachment is larger than that on smooth attachment substrates.

[0141] In addition, the use of fibers can increase the strength of concrete, especially the tensile strength. In the present invention, the alkali-resistant fibers are combined with eco-concrete to improve the crack resistance, bending resistance, and fatigue resistance of concrete. When applied to breakwater members, it can reduce early cracks in concrete, reduce the damage rate of members during transportation and fixing at the seaside, and increase the ability to withstand extreme loads, especially typhoons. At the same time, the present invention can reduce the weight of the concrete attachment base by using lightweight aggregate concrete, and reduce the transportation and labor costs in the process of manufacturing, transporting, and curing the specimens. In addition, in actual sea culture, it can reduce the labor costs of fishermen who move the attachment base to harvest oysters, and reduce the costs of transportation and fixing of concrete projects, and further reduce the risk of accidentally falling to the ground and breaking during use.

[0142] Thus, similarly, this part of knowledge concerns the interdisciplinary fusion of marine sessile organisms, marine plants, and marine concrete engineering, and neither a person skilled in the field of concrete engineering nor a person skilled in the field of marine biology can obtain the technical features closely related to the ability to effectively attract oysters to attach and the high durability of concrete in the present invention, which are the color change by mixing dark color pigments into concrete, the modification of cow bone powder, the crushing technique, and the control of concrete permeability, according to References 1 to 3. Also, according to Reference 4, the reduction in concrete alkalinity and the balance of calcium ion concentration in the present invention cannot obtain the technical features closely related to the attachment of marine sessile organisms.

[0143] The present invention is described in detail below through Examples A, which are only used to illustrate the present invention and do not limit the scope of the present invention. The specific technical solutions of the project plan are as follows:

[0144] (Example A1) (1) In the survey of the marine area where the ecological project is to be constructed, the dominant species of oysters in the said marine area and the presence or absence of oysters shall be surveyed, and tests shall be conducted 10 times every quarter to measure the air temperature, seawater temperature, dissolved oxygen, planktonic organisms, total dissolved inorganic nitrogen, active phosphate, active silicate, Ca in the said marine area. 2+ , Zn 2+ , K + Record the occurrence of typhoons, study the number of typhoons and their intensity in the past, examine meteorological and hydrological data of the sea area over the years, and analyze feasible methods and solutions for the construction of ecological sabotage breakwaters.

[0145] (2) In the manufacture of the concrete adhesion base, eco-concrete is used to manufacture a lightweight concrete oyster adhesion base with a rough surface. The size of the adhesion base is 10 cm x 10 cm x 2 cm. After being demolded, it is immediately subjected to CO2 curing at 10 atmospheres for 1 hour, and then to standard curing for 28 days.

[0146] (3) For the regular and quantitative harvesting and cultivation of oyster larvae, a rough lightweight concrete oyster attachment base was placed in a nearby sea area in July, and the attachment rate of oyster larvae was set at 20 oysters / 100 cm. 2 In this case, seedling collection is stopped and the attached substrate is then moved to an area of ​​sea where food is abundant for floating culture.

[0147] (4) In the design of concrete components, taking into consideration the impact of oyster adhesion on the environment and wave dissipation, the concrete components of the ecological project are designed to maximize the amount of oyster adhesion and provide space for other organisms. In order to do so, a thin-walled, multi-opening hemispherical component is used, with an internal void ratio of less than 40%, and six rectangular concrete rods are installed at an angle on the surface of the hemispherical component, so that the total size of the component is 10m 3 It is.

[0148] (5) In manufacturing the concrete components, fiber-reinforced eco-concrete, which is highly attractive to marine sessile organisms, is used, and elastic molds are used to manufacture hemispherical components, especially groove structures with larger interiors and smaller exteriors, which are then cured with CO2 for two hours, followed by standard curing for 28 days.

[0149] (6) In the second year, the concrete specimens were placed in a dispersed manner during the period when the floating oyster larvae in the local sea area concentrated and attached to the ground. Taking into consideration the interaction between multiple specimens, the concrete members were connected with ropes.

[0150] (7) For the on-site placement of oyster attachment substrates, oyster substrates with a concrete surface on which oysters (at the mature stage of gonad development) can attach well are transported to the sea area where the breakwater is to be constructed, and a lightweight concrete oyster attachment substrate with a rough surface is placed on each hemispherical member, and secured to the hemispherical member with ropes. Chlorella concentrated feed is also thrown in according to the planktonic organism conditions in the local sea area. At the same time, the feeding amount is increased from 25,000 cells / mL, 40,000 cells / mL, 60,000 cells / mL to 80,000 cells / mL according to the developmental status of the oyster larvae.

[0151] (8) In the management and monitoring of larval adhesion, the adhesion density of oyster larvae on the concrete surface was 35 / 100cm. 2 If the number of oysters reaches this number, the oyster attachment substrate is removed, and at the same time, a decision is made as to whether or not to feed the oysters based on the type and number of planktonic organisms in the sea area.

[0152] (Example A2) (1) In the survey of the marine area where the ecological project is to be constructed, the dominant species of oysters in the said marine area and the presence or absence of oysters shall be surveyed, and tests shall be conducted 15 times every quarter to measure the air temperature, seawater temperature, dissolved oxygen, planktonic organisms, total dissolved inorganic nitrogen, active phosphate, active silicate, Ca in the said marine area. 2+ , Zn 2+ , K + record the occurrence of typhoons, and also investigate the number of typhoons and their intensity in the past, examine meteorological and hydrological data of the sea area over the years, and analyze feasible methods and solutions for the construction of the ecological sabotage breakwater;

[0153] (2) In the manufacture of the concrete adhesion base, eco-concrete is used to manufacture a lightweight concrete oyster adhesion base with a rough surface. The size of the adhesion base is 10 cm x 10 cm x 3 cm. After being demolded, it is immediately subjected to CO2 curing at 10 atmospheres for 1.5 hours, and then to standard curing for 28 days.

[0154] (3) For the regular and quantitative harvesting and cultivation of oyster larvae, a rough lightweight concrete oyster attachment base was placed in a nearby sea area in August, and the attachment rate of oyster larvae was set at 25 oysters / 100 cm. 2 In this case, seedling collection is stopped and the attached substrate is then transported to an area of ​​sea where food is abundant for floating culture.

[0155] (4) In the design of concrete components, taking into consideration the impact of oyster adhesion on the environment and wave dissipation, the concrete components of the ecological project are designed to maximize the amount of oyster adhesion and provide space for other organisms. In order to achieve this, a thin-walled, multi-opening hemispherical component with an internal void ratio of less than 50% is used. Six cylindrical concrete rods are installed at an angle on the surface of the hemispherical component, and the total size of the component is 15m. 3 It is.

[0156] (5) In manufacturing the concrete components, fiber-reinforced eco-concrete, which is highly attractive to marine sessile organisms, is used, and elastic molds are used to manufacture hemispherical components, especially groove structures with larger interiors and smaller exteriors, which are then cured with CO2 for two hours, followed by standard curing for 28 days.

[0157] (6) In the second year, the concrete specimens are placed in a dispersed manner, and in consideration of the interaction between multiple hemispherical components, each component is connected with ropes.

[0158] (7) For the on-site placement of oyster attachment substrates, oyster substrates with a concrete surface on which oysters (at the mature stage of gonad development) can attach well are transported to the sea area where the breakwater is to be constructed, and a lightweight concrete oyster attachment substrate with a rough surface is placed on each hemispherical member, and secured to the hemispherical member with ropes. Chlorella concentrated feed is also thrown in according to the planktonic organism conditions in the local sea area. At the same time, the feeding amount is increased from 30,000 cells / mL, 50,000 cells / mL, 70,000 cells / mL to 90,000 cells / mL according to the developmental status of the oyster larvae.

[0159] (8) In the management and monitoring of larval adhesion, the adhesion density of oyster larvae on the concrete surface was 40 / 100cm. 2 When the number of oysters reaches 100, the oyster attachment substrate is removed, and at the same time, it is decided whether or not to feed the oysters based on the type and number of planktonic organisms in the sea area.

[0160] The mix ratio of the oyster attachment base and the concrete for injection described in Examples A1 and A2 is as follows.

[0161] The concrete mix ratio of the fiber-reinforced eco-concrete (1-22) which is highly attractive to marine sessile organisms is that of the biomimetic concrete member (23), and the concrete mix ratio of the lightweight concrete oyster attachment base with a rough surface is the same as that of the above-mentioned Examples 1-21, and the shape design of the concrete oyster attachment base is specifically shown in Figures 5-7.

[0162] Using an elastic mold, a specially shaped component is manufactured, especially a groove structure with a larger inner part and a smaller outer part, and the curing method is determined according to the concrete mix ratio, its alkalinity and anti-seepage property.

[0163] 1. Regarding the concrete mix ratio of ordinary Portland cement, the weight percentages of ordinary Portland cement, crushed stone, sand, water and polycarboxylate water-reducing agent powder are 17.1%, 46.67%, 29.0%, 7.2% and 0.03%, respectively.

[0164] The base material of the crushed stone is one of basalt and diabase, the maximum grain size of which does not exceed 50 mm and has a high grade, and the sand is one or more of river sand, machine-made sand (base material is one of granite and basalt) or desalinated sea sand, and has a high grade. The water meets the quality standards for water for concrete ( People's Republic of China Industry Standards ( JGJ63-2006 ): Water standard for concrete ) must be satisfied, Cl- content <1000mg / L, PH value >4.5, and have little effect on the initial hardening time difference, final hardening time, strength, and permeability of cement. In addition, the above materials selected in Examples A1 to A22 are the same.

[0165] 2. Regarding the standard concrete mix ratio, the weight percentages of ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 10.26%, 0.86%, 5.98%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively. [Table 1]

[0166] As can be seen from the above examples, when blast furnace slag powder and silica fume are mixed into concrete, it can not only fill the gaps between particles such as cement, but also cause a pozzolanic reaction, which then improves the interface microstructure of the transition area, not only ensures the basic strength of the concrete, but also reduces the alkalinity and permeability of the concrete itself. It plays an important role in reducing the alkalinity difference caused by the contact between the concrete and seawater in contact with it, and at the same time, the low permeability suppresses the release rate of alkali, and finally, it makes it easier for oyster larvae to attach to the concrete surface.

[0167] 3. The weight percentages of unmodified dark pigment, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 0.51%, 10.26%, 0.79%, 5.54%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively.

[0168] 4. The weight percentages of unmodified dark pigment, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 0.86%, 10.26%, 0.75%, 5.23%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively.

[0169] 5. The weight percentages of unmodified dark pigment, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 1.37%, 10.26%, 0.68%, 4.79%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively.

[0170] 6. The weight percentages of modified dark pigment (mass ratio of iron black:aniline black mixture = 1:1), ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 0.51%, 10.26%, 0.79%, 5.54%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively.

[0171] 7. The weight percentages of modified dark pigment (mass ratio of iron black:aniline black mixture = 1:1), ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 0.86%, 10.26%, 0.75%, 5.23%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively.

[0172] 8. The weight percentages of modified dark pigment (mass ratio of iron black:aniline black mixture = 1:1), ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 1.37%, 10.26%, 0.68%, 4.79%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively.

[0173] The modified dark pigment is 196 transparent resin, mixed with 3% hardener and 1.5% accelerator, and the volume ratio of pigment to resin is 1:0.2. It is cured at room temperature for 4 hours and then cured at 60℃ for 4 hours. Then, it is crushed by beating and crushed by vibration mill until the powder size exceeds 400 mesh. [Table 2]

[0174] Black pigments have a significant effect on the permeability of concrete, and as the dosage increases, the amount of oyster larvae attached decreases. On the one hand, the permeability of concrete improves, so the leaching of alkali in concrete increases, and on the other hand, iron oxide is converted into iron ions, and the concentration of iron ions increases, which may inhibit the attachment of oyster larvae. To address this problem, the pigment is covered with resin and then crushed into powder, which can greatly improve the permeability prevention of concrete, and especially when the dosage is 1.37%, its electric flux increases by only 3.2%. At the same time, with the increase in dark pigment, the amount of oyster attachment also increases, and when the dosage is 1.37%, it appears as a decrease in the attachment rate of oyster larvae, unlike before the modification.

[0175] 9. The weight percentages of unmodified cow bone powder, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 0.51%, 10.26%, 0.79%, 5.54%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively.

[0176] 10. The weight percentages of unmodified cow bone powder, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 0.86%, 10.26%, 0.75%, 5.23%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively.

[0177] 11. The weight percentages of unmodified cow bone powder, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 1.37%, 10.26%, 0.68%, 4.79%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively.

[0178] 12. The weight percentages of modified cow bone powder, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 0.51%, 10.26%, 0.79%, 5.54%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively.

[0179] 13. The weight percentages of modified cow bone powder, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 0.86%, 10.26%, 0.75%, 5.23%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively.

[0180] 14. The weight percentages of modified cow bone powder, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 1.37%, 10.26%, 0.68%, 4.79%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively.

[0181] Add 100 mesh cow bone powder to 2% phosphoric acid solution, the weight ratio of the two is 1:3, the temperature is 20-30℃, mix in a mixer with a rotation speed of 200-500 rpm for 30 minutes, centrifuge in a centrifuge with a rotation speed of 3000-5000 rpm for 3 minutes, discard the supernatant, and wash the centrifuged solid with water 2-3 times, the washing water is not acidic, vacuum dry the centrifuged solid at 40℃, mix the dried cow bone powder with slag powder in a ratio of 1:4, and crush in a vibrating mill until the fineness exceeds 200 mesh, and prepare for use. [Table 3] Note: The modified cow bone powder is ground to a powder size of 200 mesh to 300 mesh.

[0182] In response to the problem that cow bone powder is difficult to grind and generally difficult to continue grinding to about 100 mesh, here, 100 mesh cow bone powder is first chemically modified with 2% concentration dilute phosphoric acid, and then dried cow bone powder and 1:4 slag powder are ground in a vibrating mill until the fineness exceeds 200 mesh. In this way, the contact between the modified cow bone powder and the alkaline substances in the concrete is improved, and at the same time, the microstructure inside the concrete is denser and there is no mold phenomenon that occurred before. After modification, in the case of a low dosage, the anti-penetration property of the concrete is also improved. Even when the dosage reaches 1.37%, the electric flux (This is an index of concrete permeability, and is defined in standards for concrete performance testing and evaluation methods, such as ASTMC1202 and GB / T 50082-2009.) increases to only 4.2%, while the attachment change rate of oyster larvae increases from 205% to 400%.

[0183] 15. The weight percentages of modified cow bone powder, modified dark pigment, oyster shell powder, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 0.51%, 0.86%, 0.51%, 10.26%, 0.62%, 4.34%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively.

[0184] 16. The weight percentages of modified cow bone powder, modified dark pigment, oyster shell powder, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 0.86%, 0.51%, 0.86%, 10.26%, 0.58%, 4.03%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively. [Table 4]

[0185] In this example, dark pigment, oyster shell powder, and cow bone powder are mixed into standard concrete. The standard concrete does not have enough Ca for adhesion and transformation. 2+ and has low alkalinity. At the same time, the dark pigment makes the concrete dark, absorbs almost all visible light, turns the concrete surface black, and provides a shady environment. In addition, the addition of shell powder and cow bone powder reduces the required HCO3 - , PO4 3- and various trace elements are provided, which jointly promote the attachment of oysters. Therefore, in the case of 0.86% dark pigment, 0.51% oyster shell powder, and 0.51% cow bone powder, the attachment change rate of oyster larvae reaches 317%, but in the case of 0.86% dark pigment, 0.51% oyster shell powder, and 0.86% cow bone powder, the attachment change rate increases to 517%.

[0186] 17. The weight percentages of calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 0.51%, 10.26%, 0.79%, 5.54%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively.

[0187] 18. The weight percentages of calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 0.86%, 10.26%, 0.75%, 5.23%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively.

[0188] 19. The weight percentages of calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 1.37%, 10.26%, 0.68%, 4.79%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively. [Table 5]

[0189] In this embodiment A, the mineral admixture is replaced with the same amount of 600 mesh calcium carbonate powder with different dosages. As the dosage of calcium carbonate powder increases, the penetration prevention of concrete decreases, but the electric flux of concrete is lower than the reference value, and even when the dosage is 1.37%, its penetration prevention is better than that of the reference group. As the dosage of calcium carbonate powder increases, the dissolution probability of calcium carbonate in concrete is improved, and therefore the adhesion change rate is improved. Specifically, when the dosage is 0.51%, 0.86%, and 1.37%, respectively, the adhesion change rate of oyster larvae is 20%, 40%, and 50%.

[0190] 20. The weight percentages of zinc sulfate, modified dark pigment, modified cow bone powder, calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 0.3%, 0.86%, 0.86%, 0.51%, 10.26%, 0.54%, 3.77%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively.

[0191] 21. The weight percentages of zinc sulfate, modified dark pigment, modified cow bone powder, calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 0.6%, 0.86%, 0.86%, 0.51%, 10.26%, 0.50%, 3.51%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively.

[0192] The method of modifying zinc sulfate is as follows: select diatomaceous earth with SiO2 content >90% and fineness of 600 mesh, add 150g water in a mixer at 60°C, then add 100g zinc sulfate, stir until completely dissolved, and prepare for use; then heat 150g of the above diatomaceous earth to 60°C, add it to the solution, stir for 10 minutes in a mixer with a rotation speed of 200-500 revolutions / min, and then dry in a drying oven with a drying temperature of 100°C to obtain the modified zinc sulfate. [Table 6] Note: The dark pigments are modified iron black and aniline black, and the mass ratio is 2:1.

[0193] In this example, zinc sulfate, cow bone powder, calcium carbonate powder, and dark pigment are mixed into standard concrete. The standard concrete does not have enough Ca, which is necessary for the adhesion of the hook and transformation. 2+ and has low alkalinity. At the same time, the dark pigment makes the concrete dark, absorbs almost all visible light, turns the concrete surface black, and provides a shady environment. In addition, the addition of cow bone powder and calcium carbonate powder reduces the required HCO3 - , PO4 3- and various trace elements in cow bone powder, and Zn provided by zinc sulfate. 2+ It fully meets the requirements of inducing early attachment of oyster larvae, ions necessary for metamorphosis and dark color, and has excellent effects. In the case of 0.86% dark color pigment, 0.51% cow bone powder, 0.51% calcium carbonate powder and 0.2% zinc sulfate, the attachment change rate reaches 580%, and in the case of 0.86% dark color pigment, 0.51% cow bone powder, 0.51% calcium carbonate powder and 0.6% zinc sulfate, the attachment change rate is 652%.

[0194] 22. The weight percentages of zinc sulfate, modified dark pigment, modified cow bone powder, calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water, short fiber and polycarboxylate water reducer powder are 0.6%, 0.86%, 0.86%, 0.51%, 10.26%, 0.50%, 3.51%, 46.42%, 28.85%, 7.2%, 0.4%, and 0.03%, respectively.

[0195] 23. The present invention uses the above concrete to carry out biomimetic shape design for concrete members, specifically see FIG. 8.

[0196] In addition, the specific operation steps of the implementation method of the above embodiment are the same as those of the above-mentioned embodiments 1 to 21, and reference documents 2 to 4 are the same as those of the above-mentioned reference documents, and therefore are deleted.

[0197] Reference 5 is "Living Breakwaters - Green Infrastructure along the New York Coast - Mago Ichiro."

[0198] The object of the present invention is different from that of Reference 5, which is to construct a "living" breakwater, and to increase the number of marine organisms through macro design, surface texture, and concrete members made with low-alkali cement, and the increased marine organisms are marine organisms and marine sessile organisms, mainly marine organisms. In addition to the low alkalinity of cement, the present invention also mixes dark color pigments, bio-calcium powder, calcium carbonate powder, and trace elements into the concrete to attract oyster larvae, which are characterized by rapid and dense attraction, and are highly effective, greatly improving the ecological environment of the marine area.

[0199] Thus, similarly, this part of knowledge relates to the interdisciplinary fusion of marine sessile organisms, marine plants and marine concrete engineering, and neither a person skilled in the field of concrete engineering nor a person skilled in the field of marine biology can obtain, according to References 2-3, the technical features in the present invention in which the reduction in alkalinity of concrete and the balance of calcium ion concentration are closely related to the attachment of marine sessile organisms.

[0200] In addition, the unique features and beneficial effects of the present invention are as follows: The content of the aspects of deep color pigment, trace elements, and concrete permeability are the same as the above, so please refer to the above unique features and beneficial effects.

[0201] It is necessary to grasp the optimum environment required for marine sessile organisms to attach, transform and grow later, and to design concrete starting from the seepage prevention of concrete, and not to ignore the fact that only considering the dosage of various raw materials will bring about changes in the seepage prevention of concrete. Therefore, similarly, this part of knowledge concerns the interdisciplinary fusion of marine sessile organisms, chemistry and marine concrete engineering, and whether one skilled in the art of concrete engineering or marine biology, according to the prior background, in the present invention, the overall control of the seepage prevention of concrete cannot obtain the technical characteristics that are closely related to the ability of the attractant to effectively attract oysters to attach.

[0202] Thus, similarly, this part of knowledge concerns the interdisciplinary fusion of marine sessile organisms, marine plants, and marine concrete engineering, and neither a person skilled in the field of concrete engineering nor a person skilled in the field of marine biology can obtain the technical features closely related to the ability to effectively attract oysters to attach and the high durability of concrete in the present invention, which are the color change by mixing dark color pigments into concrete, the modification of cow bone powder, the crushing technique, and the control of concrete permeability, according to References 2-3. Also, according to Reference 4, the reduction in concrete alkalinity and the balance of calcium ion concentration in the present invention cannot obtain the technical features closely related to the attachment of marine sessile organisms.

[0203] Although embodiments of the present invention will be shown and described, it will be understood that those skilled in the art can make various changes, modifications, substitutions and variations to these embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is limited by the claims and their equivalents.

Claims

1. A cement concrete oyster adhesion base, comprising a cementitious material, a lightweight coarse aggregate, a lightweight fine aggregate, water, a dark pigment, a bio-calcium powder, a calcium carbonate powder, a trace element, a short fiber and a superplasticizer, wherein the weight percentages of the cementitious material, the lightweight coarse aggregate, the lightweight fine aggregate, the water, the dark pigment, the bio-calcium powder, the calcium carbonate powder, the trace element, the short fiber and the superplasticizer are respectively 21.8% to 34.5%, 24.6% to 37.5%, 15.8% to 29.6%, 8.4% to 16.4%, 0.6% to 3.0%, 0.4% to 2.0%, 0.4% to 2.0%, 0.2% to 1.8%, 0.15% to 1.5% and 0.03% to 0. 18%, wherein the biocalcium powder comprises cow bone powder and biocalcium carbonate powder, the biocalcium carbonate powder comprises one or more combinations of oyster shell powder, fish bone powder, eggshell powder, and coral powder, the fineness of the biocalcium powder is 100 mesh to 1000 mesh, the trace elements are zinc, iron, potassium, and phosphorus, and the cement concrete oyster attachment base comprises one or more of zinc sulfate, calcium phosphate, zinc phosphate, potassium sulfate, potassium nitrate, iron sulfate, ammonium nitrate, potassium phosphate, ammonium phosphate, and iron phosphate.

2. The cement concrete oyster adhesion base according to claim 1, characterized in that the dark color pigment is one or two of iron black, aniline black, carbon black, antimony sulfide, red iron oxide, and organic pigment red.

3. The bio-calcium powder comprises one or more composites of 100 mesh to 500 mesh eggshell powder, coral powder, oyster shell powder or fish bone powder, and 100 mesh to 500 mesh cow bone powder. The cement concrete oyster attachment base according to claim 1.

4. The calcium carbonate powder is one or more of calcite, chalk, limestone, marble, aragonite, travertine powder, processed light calcium carbonate, activated calcium carbonate, calcium carbonate whisker, and the fineness of the calcium carbonate powder is more than 200 mesh.

5. The cement concrete oyster adhesion base according to claim 1, wherein the short fibers are inorganic fibers including one or more of basalt fibers, alkali-resistant glass fibers, and carbon fibers.

6. The lightweight coarse aggregate is one or two of crushed lightweight porous basalt and lightweight ceramsite with a maximum particle size of less than 20 mm, and the lightweight fine aggregate is one or two of crushed zeolite and lightweight ceramic sand, and the particle size is 0.2 mm to 5 mm. The cement concrete oyster adhesion base of claim 1.

Citation Information

Patent Citations

  • Novel concrete artificial fish reef and preparation method thereof

    CN104529286A

  • Bionic concrete artificial fish reef and preparation method thereof

    CN104938384A

  • Utilization method of livestock and poultry slaughtering waste

    CN106495517A

  • Preparation method of low-shrinkage 3D (three-dimensional) printing material

    CN106986579A

  • Building lime formula

    CN107056096A