Resin materials and multilayer printed wiring boards

The use of cyclohexane ring-containing compounds in resin materials for multilayer printed wiring boards addresses issues of high dielectric loss tangent and surface roughness, enhancing thermal stability and reducing side lobes, thereby improving the performance of insulating layers.

JP7563913B2Active Publication Date: 2024-10-08SEKISUI CHEMICAL CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2020130792
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-08-01
Filing Date
2020-07-31
Publication Date
2024-10-08
Estimated Expiration
2040-07-31

AI Technical Summary

Technical Problem

Conventional resin materials for multilayer printed wiring boards suffer from high dielectric loss tangent, insufficient thermal dimensional stability, surface roughness after etching, and formation of large side lobes during via formation due to heat from lasers.

Method used

A resin material containing a cyclohexane ring-containing compound, such as a cyclohexane ring-containing maleimide or benzoxazine compound, along with a curing accelerator, is used to form insulating layers, which includes specific proportions of aliphatic diamine compounds and avoids dimer diamine-derived skeletons, enhancing thermal stability and reducing surface roughness.

Benefits of technology

The resin material achieves lower dielectric loss tangent, increased thermal dimensional stability, reduced surface roughness after etching, and minimized side lobes, while improving adhesion and thermal stability of the cured product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563913000026
    Figure 0007563913000026
  • Figure 0007563913000001
    Figure 0007563913000001
  • Figure 0007563913000002
    Figure 0007563913000002
Patent Text Reader

Abstract

To provide a resin material capable of 1) reducing dielectric loss tangent of a cured product, 2) improving thermal dimensional stability of a cured product, 3) reducing surface roughness after etching and 4) reducing a side lobe.SOLUTION: There is provided a resin material containing a specific cyclohexane ring-containing compound and a curing accelerator, wherein: the cyclohexane ring-containing compound has a first skeleton derived from an aliphatic diamine compound having a cyclohexane ring; the aliphatic diamine compound having a cyclohexane ring is different from a dimer diamine; the cyclohexane ring-containing compound has no second skeleton or has a skeleton derived from a dimer diamine; and the average ratio of the first skeleton is 50 mol% or more and the average ratio of the second skeleton is 15 mol% or less based on 100 mol% of the whole structural unit of the skeleton derived from a diamine compound in the cyclohexane ring-containing compound.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin material containing a compound having a cyclohexane ring, and also to a multilayer printed wiring board using the resin material. [Background technology]

[0002] Conventionally, various resin materials have been used to obtain electronic components such as semiconductor devices, laminates, and printed wiring boards. For example, in a multilayer printed wiring board, a resin material is used to form an insulating layer for insulating between internal layers, or to form an insulating layer located on a surface layer. Wiring, which is generally metal, is laminated on the surface of the insulating layer. In addition, a resin film obtained by filming the resin material may be used to form the insulating layer. The resin material and the resin film are used as insulating materials for multilayer printed wiring boards, including build-up films.

[0003] The following Patent Document 1 discloses a resin composition containing a compound having a maleimide group, a divalent group having at least two imide bonds, and a saturated or unsaturated divalent hydrocarbon group. Patent Document 1 also describes that a cured product of this resin composition can be used as an insulating layer for a multilayer printed wiring board or the like.

[0004] The following Patent Document 2 discloses a resin composition for electronic materials that contains a bismaleimide compound having two maleimide groups and one or more polyimide groups having a specific structure. In the bismaleimide compound, the two maleimide groups are each independently bonded to both ends of the polyimide group via at least a first linking group in which eight or more atoms are linearly linked.

[0005] Patent Document 3 listed below discloses a resin composition containing (A) an epoxy compound and (B) a maleimide compound, in which the maleimide compound (B) contains either an alkyl group having 5 or more carbon atoms or an alkylene group having 5 or more carbon atoms. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] WO2016 / 114286A1 [Patent Document 2] JP 2018-90728 A [Patent Document 3] JP 2019-44128 A Summary of the Invention [Problem to be solved by the invention]

[0007] When an insulating layer is formed using a conventional resin material such as those described in Patent Documents 1 to 3, the dielectric tangent of the cured product may not be sufficiently low, or the thermal dimensional stability may not be sufficiently high.

[0008] Furthermore, when an insulating layer is formed using a conventional resin material as described in Patent Documents 1 to 3, the surface roughness after etching may not be sufficiently small.

[0009] Furthermore, in the case of conventional resin materials such as those described in Patent Documents 1 to 3, the resin material may deteriorate due to heat from a laser or the like during via formation, which may result in relatively large side lobes around the formed via.

[0010] The object of the present invention is to provide a resin material that can 1) reduce the dielectric tangent of the cured product, 2) increase the thermal dimensional stability of the cured product, 3) reduce the surface roughness after etching, and 4) reduce the side lobe. Another object of the present invention is to provide a multilayer printed wiring board using the resin material. [Means for solving the problem]

[0011] According to a broad aspect of the present invention, there is provided a resin material comprising at least one cyclohexane ring-containing compound selected from a maleimide compound having a cyclohexane ring and a benzoxazine compound having a cyclohexane ring, and a curing accelerator, wherein the cyclohexane ring-containing compound has a first skeleton derived from an aliphatic diamine compound having a cyclohexane ring, the aliphatic diamine compound having the cyclohexane ring is different from a dimer diamine, the cyclohexane ring-containing compound does not have or has a second skeleton derived from a dimer diamine, and an average proportion of the first skeleton derived from the aliphatic diamine compound having a cyclohexane ring is 50 mol % or more in 100 mol % of all structural units of the skeleton derived from the diamine compound contained in the cyclohexane ring-containing compound, and when the cyclohexane ring-containing compound has a second skeleton derived from the dimer diamine, an average proportion of the second skeleton derived from the dimer diamine is 15 mol % or less in 100 mol % of all structural units of the skeleton derived from the diamine compound contained in the cyclohexane ring-containing compound.

[0012] In a specific aspect of the resin material according to the present invention, the cyclohexane ring-containing compound does not have a second skeleton derived from the dimer diamine.

[0013] In a specific aspect of the resin material according to the present invention, an average proportion of a first skeleton derived from an aliphatic diamine compound having a cyclohexane ring is 100 mol % in 100 mol % of all structural units of a skeleton derived from a diamine compound possessed by the cyclohexane ring-containing compound.

[0014] In a specific aspect of the resin material according to the present invention, the cyclohexane ring-containing compound has a third skeleton derived from a diamine compound other than the aliphatic diamine compound having a cyclohexane ring, and the diamine compound other than the aliphatic diamine compound having a cyclohexane ring is different from a dimer diamine.

[0015] In a specific aspect of the resin material according to the present invention, a third skeleton derived from a diamine compound different from the aliphatic diamine compound having a cyclohexane ring has an aromatic ring.

[0016] In a specific aspect of the resin material according to the present invention, a third skeleton derived from a diamine compound different from the aliphatic diamine compound having a cyclohexane ring has a fluorine atom.

[0017] In a specific aspect of the resin material according to the present invention, in the first skeleton derived from the aliphatic diamine compound having a cyclohexane ring, a nitrogen atom constituting the first amino group and a carbon atom constituting the cyclohexane ring are bonded directly or via two or less atoms.

[0018] In a specific aspect of the resin material according to the present invention, in the first skeleton derived from the aliphatic diamine compound having a cyclohexane ring, a nitrogen atom constituting a second amino group different from the first amino group is directly bonded to a carbon atom constituting the cyclohexane ring or is bonded via three or less atoms.

[0019] In a specific aspect of the resin material according to the present invention, the aliphatic diamine compound having a cyclohexane ring is tricyclodecane diamine, norbornane diamine, or isophorone diamine.

[0020] In a specific aspect of the resin material according to the present invention, the cyclohexane ring-containing compound has a glass transition temperature of 100° C. or higher and 300° C. or lower.

[0021] In a specific aspect of the resin material according to the present invention, the cyclohexane ring-containing compound has a weight average molecular weight of 2,000 or more and 100,000 or less.

[0022] In a specific aspect of the resin material according to the present invention, the resin material contains a thermosetting compound different from the cyclohexane ring-containing compound and a curing agent.

[0023] In a specific aspect of the resin material according to the present invention, the cyclohexane ring-containing compound is a maleimide compound having the cyclohexane ring, and the thermosetting compound includes a maleimide compound.

[0024] In a specific aspect of the resin material according to the present invention, the maleimide compound has a skeleton derived from dimer diamine.

[0025] In a specific aspect of the resin material according to the present invention, the maleimide compound having a cyclohexane ring does not have a second skeleton derived from the dimer diamine, and the maleimide compound has a skeleton derived from the dimer diamine.

[0026] In a specific aspect of the resin material according to the present invention, the thermosetting compound includes an epoxy compound.

[0027] In a specific aspect of the resin material according to the present invention, the curing agent includes an active ester compound.

[0028] In a specific aspect of the resin material according to the present invention, the thermosetting compound includes a radically curable compound.

[0029] In a specific aspect of the resin material according to the present invention, the resin material contains an inorganic filler.

[0030] In a specific aspect of the resin material according to the present invention, the content of the inorganic filler is 50% by weight or more based on 100% by weight of the components excluding the solvent in the resin material.

[0031] In a specific aspect of the resin material according to the present invention, the inorganic filler is silica.

[0032] In a specific aspect of the resin material according to the present invention, the resin material is a resin film.

[0033] The resin material according to the present invention is suitably used for forming an insulating layer in a multilayer printed wiring board.

[0034] According to a broad aspect of the present invention, there is provided a multilayer printed wiring board comprising a circuit board, a plurality of insulating layers disposed on a surface of the circuit board, and a metal layer disposed between the plurality of insulating layers, wherein at least one of the plurality of insulating layers is a cured product of the resin material described above. Effect of the Invention

[0035] The resin material according to the present invention includes at least one of a cyclohexane ring-containing compound, which is a maleimide compound having a cyclohexane ring and a benzoxazine compound having a cyclohexane ring, and a curing accelerator. In the resin material according to the present invention, the cyclohexane ring-containing compound has a first skeleton derived from an aliphatic diamine compound having a cyclohexane ring, and the aliphatic diamine compound having a cyclohexane ring is different from a dimer diamine. In the resin material according to the present invention, the cyclohexane ring-containing compound does not have or has a second skeleton derived from a dimer diamine. In the resin material according to the present invention, the average proportion of the first skeleton derived from the aliphatic diamine compound having a cyclohexane ring is 50 mol % or more in 100 mol % of all structural units of the skeleton derived from the diamine compound possessed by the cyclohexane ring-containing compound. In the resin material according to the present invention, when the cyclohexane ring-containing compound has a second skeleton derived from the dimer diamine, the average proportion of the second skeleton derived from the dimer diamine is 15 mol % or less in 100 mol % of all structural units of the skeleton derived from the diamine compound possessed by the cyclohexane ring-containing compound. Since the resin material according to the present invention has the above-mentioned configuration, 1) the dielectric tangent of the cured product can be reduced, 2) the thermal dimensional stability of the cured product can be increased, 3) the surface roughness after etching can be reduced, and 4) the side lobe can be reduced. The resin material according to the present invention can achieve all of the above-mentioned effects 1) to 4). [Brief description of the drawings]

[0036] [Figure 1] FIG. 1 is a cross-sectional view showing a schematic diagram of a multilayer printed wiring board using a resin material according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0037] The present invention will be described in detail below.

[0038] The resin material according to the present invention contains at least one cyclohexane ring-containing compound selected from a maleimide compound having a cyclohexane ring and a benzoxazine compound having a cyclohexane ring, and a curing accelerator.

[0039] In the resin material according to the present invention, the cyclohexane ring-containing compound has a first skeleton derived from an aliphatic diamine compound having a cyclohexane ring, and the aliphatic diamine compound having a cyclohexane ring is different from a dimer diamine.

[0040] In the resin material according to the present invention, the cyclohexane ring-containing compound does not have a second skeleton derived from dimer diamine or has a second skeleton derived from dimer diamine.

[0041] In the resin material according to the present invention, the average proportion of the first skeleton derived from the aliphatic diamine compound having a cyclohexane ring is 50 mol % or more out of 100 mol % of all structural units of the skeleton derived from the diamine compound possessed by the cyclohexane ring-containing compound.

[0042] In the resin material according to the present invention, when the cyclohexane ring-containing compound has a second skeleton derived from the dimer diamine, the average proportion of the second skeleton derived from the dimer diamine is 15 mol % or less in 100 mol % of all structural units of the skeleton derived from the diamine compound contained in the cyclohexane ring-containing compound.

[0043] Since the resin material according to the present invention has the above-mentioned configuration, 1) the dielectric tangent of the cured product can be reduced, 2) the thermal dimensional stability of the cured product can be increased, 3) the surface roughness after etching can be reduced, and 4) the side lobes can be reduced.

[0044] In addition, since the resin material according to the present invention has the above-mentioned structure, it is possible to increase the plating peel strength. Furthermore, since the resin material according to the present invention has the above-mentioned structure, it is possible to increase the glass transition temperature (Tg) of the cured product.

[0045] Furthermore, since the resin material according to the present invention has the above-mentioned configuration, it is possible to enhance the compatibility between the cyclohexane ring-containing compound and a thermosetting compound different from the cyclohexane ring-containing compound.

[0046] The resin material according to the present invention may be a resin composition or a resin film. The resin composition has fluidity. The resin composition may be in a paste form. The paste form includes a liquid form. In view of excellent handling properties, the resin material according to the present invention is preferably a resin film.

[0047] The resin material according to the present invention is preferably a thermosetting resin material. When the resin material is a resin film, the resin film is preferably a thermosetting resin film.

[0048] Hereinafter, details of each component used in the resin material according to the present invention and applications of the resin material according to the present invention will be described. In addition, below, preferred structures that can more effectively exert the effects of the present invention will be specifically described.

[0049] [Cyclohexane ring-containing compounds] The resin material according to the present invention includes a cyclohexane ring-containing compound. The cyclohexane ring-containing compound is at least one of a maleimide compound having a cyclohexane ring and a benzoxazine compound having a cyclohexane ring. In this specification, the "maleimide compound having a cyclohexane ring" may be described as a "maleimide compound containing a cyclohexane ring", and the "benzoxazine compound having a cyclohexane ring" may be described as a "benzoxazine compound containing a cyclohexane ring". Therefore, the cyclohexane ring-containing compound is at least one of a maleimide compound containing a cyclohexane ring and a benzoxazine compound containing a cyclohexane ring. The cyclohexane ring-containing compound may be used alone or in combination of two or more.

[0050] The cyclohexane ring-containing maleimide compound preferably has a maleimide skeleton at the terminal. The cyclohexane ring-containing maleimide compound may have a maleimide skeleton at a portion other than the terminal. The cyclohexane ring-containing maleimide compound may be used alone or in combination of two or more.

[0051] The cyclohexane ring-containing benzoxazine compound has a benzoxazine skeleton. The cyclohexane ring-containing benzoxazine compound may be used alone or in combination of two or more kinds.

[0052] In this specification, the cyclohexane ring means a six-membered alicyclic structure in which six carbon atoms are bonded in a ring. The carbon atoms constituting the cyclohexane ring may be bonded to a hydrocarbon group having 1 to 20 carbon atoms, or may be bonded to a hydrocarbon group having 1 to 4 carbon atoms. The cyclohexane ring-containing compound may have a cyclohexane ring as a ring constituting a tricyclodecane ring, a norbornane ring, an adamantane skeleton, or the like. The cyclohexane ring-containing compound may have a structure in which a plurality of cyclohexane rings are connected via a hydrocarbon group such as an alkyl group.

[0053] Examples of the cyclohexane ring include rings represented by the following formula (X1), (X2), (X3), (X4), and (X5).

[0054] [ka]

[0055] In the above formula (X1), R1 to R10 each represent a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms. In the above formula (X1), R1 to R10 each preferably represent a hydrogen atom or a methyl group. In the above formula (X1), R1 to R10 may be the same or different.

[0056] [ka]

[0057] In the above formula (X2), R1 to R10 each represent a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms. In the above formula (X2), R1 to R10 each preferably represent a hydrogen atom or a methyl group. In the above formula (X2), R1 to R10 may be the same or different.

[0058] [ka]

[0059] In the above formula (X3), R1 to R18 each represent a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, and Q represents any group. In the above formula (X3), R1 to R18 each preferably represent a hydrogen atom or a methyl group. In the above formula (X3), Q is preferably a hydrocarbon group having 1 to 4 carbon atoms or a group having an aromatic ring, more preferably an alkylene group, and even more preferably a methylene group. In the above formula (X3), when Q is a group having an aromatic ring, Q may be a group in which the aromatic rings are bonded to each other via an ester bond. In the above formula (X3), R1 to R18 may be the same or different.

[0060] [ka]

[0061] In the above formula (X4), R1 to R8 each represent a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms. The ring represented by the above formula (X4) is a norbornane ring. In the above formula (X4), it is preferable that R1 to R8 each represent a hydrogen atom or a methyl group. In the above formula (X4), R1 to R8 may be the same or different.

[0062] The cyclohexane ring may be a ring represented by the following formula (X4-1).

[0063] [ka]

[0064] In the above formula (X4-1), R1 to R10 each represent a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, and two of R1 to R10 represent a group bonded to the nitrogen atom constituting the imide skeleton. In the above formula (X4-1), when R9 and R10 represent a group bonded to the nitrogen atom constituting the imide skeleton, it corresponds to the above formula (X4).

[0065] [ka]

[0066] In the above formula (X5), R1 to R12 each represent a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms. The ring represented by the above formula (X5) is a tricyclodecane ring. In the above formula (X5), it is preferable that R1 to R12 each represent a hydrogen atom or a methyl group. In the above formula (X5), R1 to R12 may be the same or different.

[0067] The cyclohexane ring may be a ring represented by the following formula (X5-1).

[0068] [ka]

[0069] In the above formula (X5-1), R1 to R14 each represent a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, and two of R1 to R14 represent a group bonded to the nitrogen atom constituting the imide skeleton. In the above formula (X5-1), when R13 and R14 represent a group bonded to the nitrogen atom constituting the imide skeleton, it corresponds to the above formula (X5).

[0070] The cyclohexane ring-containing compound has a first skeleton derived from an aliphatic diamine compound having a cyclohexane ring, and the aliphatic diamine compound having the cyclohexane ring is different from a dimer diamine. Therefore, the aliphatic diamine compound is different from a dimer diamine and is an aliphatic diamine compound having a cyclohexane ring. The first skeleton has a cyclohexane ring.

[0071] In this specification, "an aliphatic diamine compound which is different from dimer diamine and has a cyclohexane ring" may be referred to as "aliphatic diamine compound A".

[0072] The cyclohexane ring-containing compound does not have a second skeleton derived from dimer diamine or has a second skeleton derived from dimer diamine. Dimer diamine is a diamine compound. The second skeleton is different from the first skeleton. The cyclohexane ring-containing compound may or may not have a second skeleton derived from dimer diamine.

[0073] The cyclohexane ring-containing compound may or may not have a third skeleton derived from a diamine compound different from an aliphatic diamine compound having a cyclohexane ring. However, with respect to the third skeleton, the aliphatic diamine compound having the cyclohexane ring (the diamine compound constituting the third skeleton) is different from a dimer diamine. Therefore, the diamine compound constituting the third skeleton is a diamine compound different from a dimer diamine and different from an aliphatic diamine compound having a cyclohexane ring. The third skeleton is different from the first skeleton. The third skeleton is different from the second skeleton. The third skeleton may or may not have a cyclohexane ring.

[0074] In this specification, "a diamine compound different from dimer diamine and different from an aliphatic diamine compound having a cyclohexane ring" may be referred to as "diamine compound B".

[0075] The skeleton and other details of the cyclohexane ring-containing compound will be described in more detail below. In addition, preferred structures that can more effectively exert the effects of the present invention will be specifically described below.

[0076] <First skeleton derived from aliphatic diamine compound A> The cyclohexane ring-containing compound has a first skeleton derived from an aliphatic diamine compound A. The cyclohexane ring-containing compound has the cyclohexane ring by having at least the first skeleton derived from an aliphatic diamine compound A. The first skeleton derived from an aliphatic diamine compound A exists as a partial skeleton in the cyclohexane ring-containing compound.

[0077] The aliphatic diamine compound A is an aliphatic diamine compound different from dimer diamine. The aliphatic diamine compound A has a cyclohexane ring. The aliphatic diamine compound A has a first amino group and a second amino group.

[0078] The number of carbon atoms contained in the aliphatic diamine compound A is preferably smaller than the number of carbon atoms contained in the dimer diamine (36). That is, the number of carbon atoms contained in the aliphatic diamine compound A is preferably less than 36.

[0079] The aliphatic diamine compound A may have one, two, or three or more of the above cyclohexane rings.

[0080] The carbon atom constituting the cyclohexane ring of the aliphatic diamine compound A may be bonded to a hydrocarbon group having from 1 to 20 carbon atoms. The aliphatic diamine compound A may have a cyclohexane ring as a ring constituting a tricyclodecane ring, a norbornane ring, an adamantane skeleton, or the like.

[0081] Examples of the cyclohexane ring contained in the aliphatic diamine compound A include rings represented by the above formula (X1), (X2), (X3), (X4), and (X5).

[0082] From the viewpoint of exerting the effects of the present invention more effectively, in the first skeleton derived from the aliphatic diamine compound A, the nitrogen atom constituting the first amino group and the carbon atom constituting the cyclohexane ring are preferably bonded directly or via two or less atoms, and the atoms are preferably carbon atoms.

[0083] From the viewpoint of exerting the effects of the present invention more effectively, in the first skeleton derived from the aliphatic diamine compound A, the nitrogen atom constituting the second amino group and the carbon atom constituting the cyclohexane ring are preferably bonded directly or via three or less atoms, and the atoms are preferably carbon atoms.

[0084] When the aliphatic diamine compound A has the tricyclodecane ring as the cyclohexane ring, it is preferable that the nitrogen atom constituting the first amino group and the carbon atom constituting the tricyclodecane ring are directly bonded or bonded via two or less atoms in the first skeleton derived from the aliphatic diamine compound A. The atoms are preferably carbon atoms. In this case, the effect of the present invention can be more effectively exhibited.

[0085] When the aliphatic diamine compound A has the tricyclodecane ring as the cyclohexane ring, it is preferable that the nitrogen atom constituting the second amino group and the carbon atom constituting the tricyclodecane ring are directly bonded or bonded via two or less atoms in the first skeleton derived from the aliphatic diamine compound A. In this case, the effect of the present invention can be more effectively exhibited. The atom is preferably a carbon atom.

[0086] Examples of the first skeleton derived from the aliphatic diamine compound A include skeletons represented by the following formula (A1), (A2), (A3), (A4), (A5), and (A6).

[0087] [ka]

[0088] In the above formula (A1), R1 to R10 each represent a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, and R11 and R12 each represent a group constituting a heterocycle together with a nitrogen atom. In the above formula (A1), it is preferable that R1 to R10 each represent a hydrogen atom or a methyl group. In the above formula (A1), R1 to R10 may be the same or different. In the above formula (A1), R11 and R12 may be the same or different.

[0089] In the skeleton represented by the above formula (A1), the nitrogen atom constituting the first amino group (the amino group on the left) and an atom constituting the cyclohexane ring are bonded via one carbon atom, and the nitrogen atom constituting the second amino group (the amino group on the right) and an atom constituting the cyclohexane ring are bonded via one carbon atom.

[0090] [ka]

[0091] In the above formula (A2), R1 to R10 each represent a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, and R11 and R12 each represent a group constituting a heterocycle together with a nitrogen atom. In the above formula (A2), it is preferable that R1 to R10 each represent a hydrogen atom or a methyl group. In the above formula (A2), R1 to R10 may be the same or different. In the above formula (A2), R11 and R12 may be the same or different.

[0092] In the skeleton represented by the above formula (A2), the nitrogen atom constituting the first amino group (the amino group on the left side) and an atom constituting the cyclohexane ring are directly bonded to each other, and the nitrogen atom constituting the second amino group (the amino group on the right side) and an atom constituting the cyclohexane ring are bonded to each other via one carbon atom.

[0093] [ka]

[0094] In the above formula (A3), R1 to R10 each represent a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, and R11 and R12 each represent a group constituting a heterocycle together with a nitrogen atom. In the above formula (A3), it is preferable that R1 to R10 each represent a hydrogen atom or a methyl group. In the above formula (A3), R1 to R10 may be the same or different. In the above formula (A3), R11 and R12 may be the same or different.

[0095] In the skeleton represented by the above formula (A3), the nitrogen atom constituting the first amino group (amino group on the left) and an atom constituting the cyclohexane ring are bonded via two carbon atoms, and the nitrogen atom constituting the second amino group (amino group on the right) and an atom constituting the cyclohexane ring are directly bonded.

[0096] [ka]

[0097] In the above formula (A4), R1 to R18 each represent a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, R19 and R20 each represent a group constituting a heterocycle together with a nitrogen atom, and Q represents any group. In the above formula (A4), R1 to R18 each preferably represent a hydrogen atom or a methyl group. In the above formula (A4), Q is preferably a hydrocarbon group having 1 to 4 carbon atoms or a group having an aromatic ring, more preferably an alkylene group, and even more preferably a methylene group. In the above formula (A4), when Q is a group having an aromatic ring, Q may be a group in which the aromatic rings are bonded to each other via an ester bond. In the above formula (A4), R1 to R18 may be the same or different. In the above formula (A4), R19 and R20 may be the same or different.

[0098] In the skeleton represented by the above formula (A4), the nitrogen atom constituting the first amino group (the amino group on the left side) and an atom constituting the cyclohexane ring are directly bonded to each other, and the nitrogen atom constituting the second amino group (the amino group on the right side) and an atom constituting the cyclohexane ring are directly bonded to each other.

[0099] [ka]

[0100] In the above formula (A5), R1 to R8 each represent a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, and R9 and R10 each represent a group constituting a heterocycle together with a nitrogen atom. In the above formula (A5), it is preferable that R1 to R8 each represent a hydrogen atom or a methyl group. In the above formula (A5), R1 to R8 may be the same or different. In the above formula (A5), R9 and R10 may be the same or different.

[0101] In the skeleton represented by the above formula (A5), the nitrogen atom constituting the first amino group (amino group on the left) and an atom constituting the cyclohexane ring are bonded via one carbon atom, and the nitrogen atom constituting the second amino group (amino group on the right) and an atom constituting the cyclohexane ring are bonded via one carbon atom.

[0102] The first skeleton derived from the aliphatic diamine compound A may be a skeleton represented by the following formula (A5-1).

[0103] [ka]

[0104] In the above formula (A5-1), R1 to R8, R11 and R12 each represent a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, two of R1 to R8, R11 and R12 each represent a group bonded to a nitrogen atom constituting an imide skeleton, and R9 and R10 each represent a group constituting a heterocycle together with the nitrogen atom. In the above formula (A5-1), when R11 and R12 each represent a group bonded to a nitrogen atom constituting an imide skeleton, this corresponds to the above formula (A5). In the above formula (A5-1), it is preferable that R1 to R8, R11 and R12 each represent a hydrogen atom or a methyl group. In the above formula (A5-1), R1 to R8, R11 and R12 may be the same or different. In the above formula (A5-1), R9 and R10 may be the same or different.

[0105] [ka]

[0106] In the above formula (A6), R1 to R12 each represent a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, and R13 and R14 each represent a group constituting a heterocycle together with a nitrogen atom. In the above formula (A6), it is preferable that R1 to R12 each represent a hydrogen atom or a methyl group. In the above formula (A6), R1 to R12 may be the same or different. In the above formula (A6), R13 and R14 may be the same or different.

[0107] In the skeleton represented by the above formula (A6), the nitrogen atom constituting the first amino group (amino group on the left) is bonded to an atom constituting the cyclohexane ring via one carbon atom, and the nitrogen atom constituting the second amino group (amino group on the right) is bonded to an atom constituting the cyclohexane ring via two carbon atoms. In the skeleton represented by the above formula (A6), the nitrogen atom constituting the second amino group is bonded to a carbon atom constituting the tricyclodecane ring via one carbon atom.

[0108] The first skeleton derived from the aliphatic diamine compound A may be a skeleton represented by the following formula (A6-1).

[0109] [ka]

[0110] In the above formula (A6-1), R1 to R12, R15 and R16 each represent a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, two of R1 to R12, R15 and R16 each represent a group bonded to a nitrogen atom constituting an imide skeleton, and R13 and R14 each represent a group constituting a heterocycle together with the nitrogen atom. In the above formula (A6-1), when R15 and R16 each represent a group bonded to a nitrogen atom constituting an imide skeleton, this corresponds to the above formula (A6). In the above formula (A6-1), it is preferable that R1 to R12, R15 and R16 each represent a hydrogen atom or a methyl group. In the above formula (A6-1), R1 to R12, R15 and R16 may be the same or different. In the above formula (A6-1), R13 and R14 may be the same or different.

[0111] In the above formulae (A1), (A2), (A3), (A4), (A5), (A5-1), (A6), and (A6-1), examples of the group constituting a heterocycle together with the nitrogen atom include groups represented by the following formula (A11), (A12), or (A13).

[0112] [ka]

[0113] [ka]

[0114] [ka]

[0115] Hereinafter, the compounds capable of forming the skeletons of the above formulae (A1), (A2), (A3), (A4), (A5), and (A6), as well as the compounds capable of forming skeletons derived from aliphatic diamine compounds having a cyclohexane ring other than the skeletons of the above formulae (A1), (A2), (A3), (A4), (A5), and (A6), will be further described.

[0116] Examples of the aliphatic diamine compound A include tricyclodecane diamine, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, bis(aminomethyl)norbornane, 3(4),8(9)-bis(aminomethyl)tricyclo[5.2.1.02,6]decane, 1,3-cyclohexanediamine, 1,4-cyclohexanediamine, isophoronediamine, 4,4'-methylenebis(cyclohexylamine), and 4,4'-methylenebis(2-methylcyclohexylamine). The aliphatic diamine compound A may be used alone or in combination of two or more.

[0117] From the viewpoint of more effectively exerting the effects of the present invention, it is preferable that the aliphatic diamine compound A is tricyclodecane diamine, norbornane diamine, or isophorone diamine. When the aliphatic diamine compound A is tricyclodecane diamine, the cyclohexane ring-containing compound has, for example, a skeleton represented by the above formula (A6). When the aliphatic diamine compound A is norbornane diamine (bis(aminomethyl)norbornane), the cyclohexane ring-containing compound has, for example, a skeleton represented by the above formula (A5). When the aliphatic diamine compound A is isophorone diamine, the cyclohexane ring-containing compound has, for example, a skeleton represented by the above formula (A2).

[0118] The first skeleton derived from the aliphatic diamine compound A is preferably a skeleton derived from a reaction product of the aliphatic diamine compound A and an acid dianhydride. The skeleton derived from the reaction product of the aliphatic diamine compound A and an acid dianhydride has the first skeleton derived from the aliphatic diamine compound A. However, by using a diisocyanate compound instead of a diamine compound as the first skeleton derived from the aliphatic diamine compound A, the skeletons of the above formula (A1), formula (A2), formula (A3), formula (A4), formula (A5) and formula (A6) can also be formed.

[0119] The acid dianhydride may, for example, be a tetracarboxylic dianhydride.

[0120] Examples of the tetracarboxylic dianhydride include pyromellitic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 3,3',4,4'-biphenylsulfone tetracarboxylic dianhydride, 1,4,5,8-naphthalene tetracarboxylic dianhydride, 2,3,6,7-naphthalene tetracarboxylic dianhydride, 3,3',4,4'-biphenyl ether tetracarboxylic dianhydride, 3,3',4,4'-dimethyldiphenylsilane tetracarboxylic dianhydride, 3,3',4,4'-tetraphenylsilane tetracarboxylic dianhydride, 1,2,3,4-furan tetracarboxylic dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)diphenyl sulfide dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)diphenyl sulfone ... 4,4'-(hexafluoroisopropylidene)diphthalic anhydride, bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride, and 5-(2,5-dioxotetrahydrofuryl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride.

[0121] In order to exert the effects of the present invention, the average proportion of the first skeleton derived from the aliphatic diamine compound A is 50 mol % or more in the total structural units (100 mol %) of the skeleton derived from the diamine compound contained in the cyclohexane ring-containing compound.

[0122] The average ratio of the first skeleton derived from the aliphatic diamine compound A in 100 mol % of all structural units of the skeleton derived from the diamine compound contained in the cyclohexane ring-containing compound is preferably 60 mol % or more, more preferably 70 mol % or more, even more preferably 80 mol % or more, and particularly preferably 90 mol % or more. The average ratio of the first skeleton derived from the aliphatic diamine compound A in 100 mol % of all structural units of the skeleton derived from the diamine compound contained in the cyclohexane ring-containing compound may be 100 mol % (total number). When the average ratio of the first skeleton derived from the aliphatic diamine compound A is the above lower limit or more, the effect of the present invention can be more effectively exhibited. In addition, when the average ratio of the first skeleton derived from the aliphatic diamine compound A is the above lower limit or more, the compatibility of the cyclohexane ring-containing compound with a thermosetting compound different from the cyclohexane ring-containing compound can be increased, the glass transition temperature (Tg) of the cured product can be increased, and the concentration of the imide skeleton can be increased, so that the desmear property can be improved. Furthermore, when the average proportion of the first skeleton derived from the aliphatic diamine compound A is equal to or more than the above lower limit, the glass transition temperature of the cured product can be increased and the linear expansion coefficient can be reduced, so that peeling of the copper wiring and cracks in the via part after a thermal shock test can be effectively suppressed.

[0123] <Second skeleton derived from dimer diamine> The cyclohexane ring-containing compound does not have a second skeleton derived from dimer diamine or has a second skeleton derived from dimer diamine. When the cyclohexane ring-containing compound has a second skeleton derived from dimer diamine, the second skeleton derived from the dimer diamine exists as a partial skeleton in the cyclohexane ring-containing compound. The dimer diamine has a cyclohexane ring. However, since the dimer diamine is, for example, a mixture (natural product), it may be difficult to define the structure of the dimer diamine as a single structure. Therefore, the dimer diamine may contain, for example, a dimer diamine having a cyclohexene ring.

[0124] From the viewpoint of further increasing the thermal dimensional stability of the cured product and effectively reducing the surface roughness after etching, it is preferable that the cyclohexane ring-containing compound does not have a second skeleton derived from dimer diamine. From the viewpoint of further increasing the thermal dimensional stability of the cured product and effectively reducing the surface roughness after etching, it is also preferable that the cyclohexane ring-containing compound has an average ratio of the second skeleton derived from dimer diamine of 15 mol % or less in 100 mol % of all structural units of the skeleton derived from the diamine compound contained in the cyclohexane ring-containing compound.

[0125] From the viewpoint of further reducing the dielectric tangent of the cured product, it is preferable that the cyclohexane ring-containing compound has a second skeleton derived from dimer diamine. The second skeleton derived from the dimer diamine is a flexible skeleton. Therefore, when the cyclohexane ring-containing compound has a second skeleton derived from the dimer diamine, the sheet property of a resin film such as a B-stage film can be improved. In addition, since the stress relaxation property of the cured product can be improved, the occurrence of warping can be effectively suppressed, and the reliability of a multilayer printed wiring board or the like can be improved. In addition, the desmear property can also be improved.

[0126] The second skeleton derived from the dimer diamine is preferably a skeleton derived from a reaction product of the dimer diamine and an acid dianhydride. The skeleton derived from the reaction product of the dimer diamine and an acid dianhydride has the second skeleton derived from the dimer diamine.

[0127] Examples of the dimer diamine include VERSAMINE 551 (trade name, manufactured by BASF Japan, 3,4-bis(1-aminoheptyl)-6-hexyl-5-(1-octenyl)cyclohexene), VERSAMINE 552 (trade name, manufactured by Cognics Japan, hydrogenated VERSAMINE 551), and PRIAMINE 1075 and PRIAMINE 1074 (trade names, all manufactured by Croda Japan).

[0128] Examples of the acid dianhydride include the above-mentioned tetracarboxylic acid dianhydrides.

[0129] In order to exert the effects of the present invention, the average proportion of the second skeleton derived from the dimer diamine is 15 mol % or less in 100 mol % of all structural units of the skeleton derived from the diamine compound contained in the cyclohexane ring-containing compound.

[0130] In the total 100 mol% of the structural units of the skeleton derived from the diamine compound in the cyclohexane ring-containing compound, the average ratio of the second skeleton derived from the dimer diamine is preferably 5 mol% or more, more preferably 8 mol% or more, preferably 12 mol% or less, more preferably 10 mol% or less. When the average ratio of the second skeleton derived from the dimer diamine is equal to or less than the upper limit, the effect of the present invention can be more effectively exhibited. When the average ratio of the second skeleton derived from the dimer diamine is equal to or more than the lower limit, the linear expansion coefficient can be kept low while smears can be more effectively removed by desmearing, and the compatibility of the resin material can be further improved. In the total 100 mol% of the structural units of the skeleton derived from the diamine compound in the cyclohexane ring-containing compound, the average ratio of the second skeleton derived from the dimer diamine may be 0 mol% or more than 0 mol%.

[0131] <Third skeleton derived from diamine compound B> The cyclohexane ring-containing compound does not have a third skeleton derived from diamine compound B or has a third skeleton derived from diamine compound B. When the cyclohexane ring-containing compound has a third skeleton derived from diamine compound B, the third skeleton derived from diamine compound B exists as a partial skeleton in the cyclohexane ring-containing compound.

[0132] The diamine compound B is a diamine compound different from both the aliphatic diamine compound A and the dimer diamine. The diamine compound B may or may not have an aromatic ring. The diamine compound B may or may not have an aromatic ring. The diamine compound B may or may not have an aliphatic ring. The diamine compound B may or may not have an aliphatic ring.

[0133] The diamine compound B may or may not have a fluorine atom. The diamine compound B may or may not have a phenolic hydroxyl group. When the diamine compound B is an aromatic diamine compound having a phenolic hydroxyl group, the linear expansion coefficient can be further reduced.

[0134] The diamine compound B may be an aliphatic diamine compound having no cyclohexane skeleton, a diamine compound having a cyclohexane skeleton and no aliphatic skeleton, or a diamine compound having no cyclohexane skeleton and no aliphatic skeleton. The diamine compound B may be an aliphatic diamine compound having no cyclohexane skeleton, a diamine compound having a cyclohexane skeleton and no aliphatic skeleton, or a diamine compound having no cyclohexane skeleton and no aliphatic skeleton. When the diamine compound B is a diamine compound having an aromatic ring, the diamine compound B may or may not have a carbon chain between the aromatic ring and the amino group.

[0135] Examples of the aromatic ring include a benzene ring, a naphthalene ring, an anthracene ring, a phenanthrene ring, a tetracene ring, a chrysene ring, a triphenylene ring, a tetraphene ring, a pyrene ring, a pentacene ring, a picene ring, and a perylene ring.

[0136] Examples of the aliphatic ring include a monocycloalkane ring, a bicycloalkane ring, a tricycloalkane ring, a tetracycloalkane ring, and a dicyclopentadiene ring.

[0137] From the viewpoint of further increasing the thermal dimensional stability of the cured product and increasing the glass transition temperature, it is preferable that the cyclohexane ring-containing compound has a third skeleton derived from the diamine compound B.

[0138] From the viewpoint of further reducing the surface roughness after etching, the cyclohexane ring-containing compound preferably has a third skeleton derived from diamine compound B. From the viewpoint of further increasing the thermal dimensional stability of the cured product, the cyclohexane ring-containing compound preferably has a third skeleton derived from diamine compound B having an aromatic ring. From the viewpoint of further increasing the thermal dimensional stability of the cured product, the third skeleton derived from diamine compound B preferably has an aromatic ring.

[0139] The third skeleton derived from the diamine compound B is preferably a skeleton derived from a reaction product of the diamine compound B and an acid dianhydride. The skeleton derived from the reaction product of the diamine compound B and an acid dianhydride has a third skeleton derived from the diamine compound B. From the viewpoint of reducing the dielectric tangent and dielectric constant of the cured product, the third skeleton derived from the diamine compound B preferably has a fluorine atom.

[0140] Examples of the diamine compound B include 1,1-bis(4-aminophenyl)cyclohexane, 2,7-diaminofluorene, 4,4'-ethylenedianiline, 4,4'-methylenebis(2,6-diethylaniline), 4,4'-methylenebis(2-ethyl-6-methylaniline), 1,4-diaminobutane, 1,10-diaminodecane, 1,12-diaminododecane, 1,7-diaminoheptane, 1,6-diaminohexane, 1,5-diaminopentane, 1,8-diaminooctane, 1,3-diaminopropane, 1,11-diaminoundecane, 2-methyl-1,5-diaminopentane, 4,4'-isopropylidenebis(2-aminophenol), 4,4'-(hexafluoroisopropylidene)bis(2-aminophenol), and 4,4'-(hexafluoroisopropylidene)dianiline. The diamine compound B may be used alone or in combination of two or more kinds.

[0141] Examples of the acid dianhydride include the above-mentioned tetracarboxylic acid dianhydrides.

[0142] In order to exert the effects of the present invention, the average proportion of the third skeleton derived from diamine compound B is less than 50 mol % in 100 mol % of all structural units of the skeleton derived from the diamine compound contained in the cyclohexane ring-containing compound.

[0143] In the total structural units 100 mol% of the skeleton derived from the diamine compound contained in the cyclohexane ring-containing compound, the average ratio of the third skeleton derived from the diamine compound B is preferably 10 mol% or more, more preferably 20 mol% or more, preferably 30 mol% or less, more preferably 25 mol% or less. When the average ratio of the third skeleton derived from the diamine compound B is the above lower limit or more and the above upper limit or less, the effects of the present invention can be more effectively exhibited. In particular, when a diamine compound having an aromatic ring is used as the diamine compound B, it is preferable to satisfy the above preferred range from the viewpoint of solubility. However, in the total structural units 100 mol% of the skeleton derived from the diamine compound contained in the cyclohexane ring-containing compound, the average ratio of the third skeleton derived from the diamine compound B may be 0 mol% or may exceed 0 mol%.

[0144] The average proportion of the first skeleton derived from the aliphatic diamine compound A, the average proportion of the second skeleton derived from the dimer diamine compound, and the average proportion of the third skeleton derived from the diamine compound B in 100 mol % of all structural units derived from the diamine compound in the cyclohexane ring-containing compound are, for example, 1 It can be calculated from the H-NMR peak area.

[0145] The cyclohexane ring-containing compound may or may not have a branched structure.

[0146] The weight average molecular weight of the cyclohexane ring-containing compound is preferably 1000 or more, more preferably 2000 or more, even more preferably 3100 or more, particularly preferably 3500 or more, preferably 100000 or less, more preferably 70000 or less, even more preferably 25000 or less, even more preferably 18000 or less, and particularly preferably 15000 or less. When the weight average molecular weight is the lower limit or more, the linear expansion coefficient can be kept low. In addition, when the weight average molecular weight exceeds 25000, the melt viscosity of the resin material becomes higher than when the weight average molecular weight is 25000 or less, and the embeddability to the uneven surface may decrease.

[0147] The weight average molecular weight is a weight average molecular weight measured by gel permeation chromatography (GPC) and calculated as polystyrene.

[0148] From the viewpoint of further enhancing the thermal dimensional stability of the cured product and further enhancing the adhesion between the insulating layer and the metal layer, the glass transition temperature of the cyclohexane ring-containing compound is preferably 75°C or higher, more preferably 85°C or higher, even more preferably 100°C or higher, and preferably 300°C or lower.

[0149] The glass transition temperature can be determined from the inflection point of the reverse heat flow when the material is heated in a nitrogen atmosphere from -30°C to 260°C at a heating rate of 3°C / min using a differential scanning calorimeter (e.g., TA Instruments' "Q2000").

[0150] The content of the cyclohexane ring-containing compound in 100% by weight of the components in the resin material excluding the inorganic filler and the solvent is preferably 3% by weight or more, more preferably 5% by weight or more, even more preferably 10% by weight or more, and preferably 80% by weight or less, more preferably 70% by weight or less. When the content of the cyclohexane ring-containing compound is equal to or more than the lower limit, the glass transition temperature Tg of the cured product can be further increased, the linear expansion coefficient can be reduced, and the adhesion between the insulating layer and the metal layer can be further increased.

[0151] The cyclohexane ring-containing maleimide compound can be prepared, for example, as follows: aliphatic diamine compound A is reacted with acid dianhydride to obtain a first reactant; the obtained first reactant is reacted with dimer diamine to obtain a second reactant; and the obtained second reactant is reacted with maleic anhydride.

[0152] The number of the maleimide skeletons in the cyclohexane ring-containing maleimide compound is preferably 2 or more, more preferably 3 or more, and preferably 10 or less, more preferably 6 or less. When the number of the maleimide skeletons is equal to or more than the above lower limit and equal to or less than the above upper limit, the effects of the present invention can be more effectively exhibited.

[0153] The cyclohexane ring-containing maleimide compound preferably has an imide skeleton. The number of imide skeletons in the cyclohexane ring-containing maleimide compound is preferably 1 or more, more preferably 2 or more, and is preferably 15 or less, more preferably 10 or less.

[0154] The cyclohexane ring-containing compound may have an even number of imide skeletons, or an odd number of imide skeletons, or may be a mixture of a compound having an even number of imide skeletons and a compound having an odd number of imide skeletons.

[0155] The cyclohexane ring-containing benzoxazine compound can be prepared, for example, as follows: An aliphatic diamine compound A is reacted with an acid dianhydride to obtain a first reactant having amino groups at both ends, and the obtained first reactant is reacted with paraform and phenol.

[0156] [Thermosetting compound] The resin material preferably contains a thermosetting compound different from the cyclohexane ring-containing compound. The thermosetting compound preferably has a cyclohexane ring, and preferably does not have a skeleton derived from an aliphatic diamine compound different from dimer diamine. The resin material preferably contains a thermosetting compound that does not have a skeleton derived from an aliphatic diamine compound (excluding dimer diamine) having a cyclohexane ring. The thermosetting compound may have a skeleton derived from dimer diamine. The thermosetting compound may be used alone or in combination of two or more.

[0157] Examples of the thermosetting compound include a maleimide compound, an epoxy compound, a cyanate compound, a vinyl compound, a phenoxy compound, an oxetane compound, a polyarylate compound, a diallyl phthalate compound, an episulfide compound, a (meth)acrylic compound, an amino compound, an unsaturated polyester compound, a polyurethane compound, and a silicone compound.

[0158] The thermosetting compound is preferably a maleimide compound, an epoxy compound, or a vinyl compound, more preferably contains an epoxy compound or a vinyl compound, and even more preferably contains an epoxy compound. The vinyl compound preferably contains a styrene compound or an acrylate compound, and more preferably contains a styrene compound. In this case, the dielectric tangent of the cured product can be further lowered and the thermal dimensional stability of the cured product can be further improved.

[0159] <Maleimide compounds> The maleimide compound is a maleimide compound (hereinafter, sometimes referred to as "maleimide compound X") that does not have a skeleton derived from an aliphatic diamine compound having a cyclohexane ring (excluding dimer diamine). The maleimide compound X is a maleimide compound different from the cyclohexane ring-containing maleimide compound. The maleimide compound X may be used alone or in combination of two or more kinds.

[0160] The maleimide compound X may be a bismaleimide compound.

[0161] Examples of the maleimide compound X include N-phenylmaleimide and N-alkylbismaleimide.

[0162] The maleimide compound X may or may not have a skeleton derived from a dimer diamine.

[0163] In order to more effectively exert the effects of the present invention, it is preferable that the maleimide compound X has a skeleton derived from a diamine compound other than a dimer diamine or a triamine compound other than a trimer triamine.

[0164] When the cyclohexane ring-containing compound is the cyclohexane ring-containing maleimide compound, the resin material preferably contains the maleimide compound X, and more preferably contains a maleimide compound X having a skeleton derived from dimer diamine. In this case, the average proportion of the skeleton derived from dimer diamine in 100 mol % of the structural units derived from the diamine compound contained in the maleimide compound X is preferably more than 15 mol %. In this case, the effect of the present invention can be more effectively exhibited.

[0165] In the case where the cyclohexane ring-containing maleimide compound does not have the second skeleton derived from the dimer diamine, the resin material preferably contains the maleimide compound X, and more preferably contains a maleimide compound X having a skeleton derived from a dimer diamine. In this case, the average proportion of skeletons derived from a dimer diamine in 100 mol % of the structural units derived from a diamine compound contained in the maleimide compound X is preferably more than 15 mol %. In this case, the effect of the present invention can be more effectively exhibited.

[0166] The maleimide compound X preferably has an aromatic ring.

[0167] In the maleimide compound X, it is preferable that the nitrogen atom in the maleimide skeleton is bonded to an aromatic ring.

[0168] From the viewpoint of further enhancing the thermal dimensional stability of the cured product, the content of the maleimide compound X is preferably 0.5% by weight or more, more preferably 1% by weight or more, and preferably 15% by weight or less, more preferably 10% by weight or less, based on 100% by weight of the components excluding the solvent in the resin material.

[0169] In 100% by weight of the components in the resin material excluding the inorganic filler and the solvent, the content of the maleimide compound X is preferably 2% by weight or more, more preferably 5% by weight or more, preferably 50% by weight or less, more preferably 35% by weight or less, and even more preferably 20% by weight or less. When the content of the maleimide compound X is equal to or more than the lower limit and equal to or less than the upper limit, the thermal dimensional stability of the cured product can be further improved.

[0170] In order to effectively exert the effects of the present invention, the molecular weight of the maleimide compound X is preferably 500 or more, more preferably 1,000 or more, and preferably less than 30,000, more preferably less than 20,000.

[0171] The molecular weight of the maleimide compound X means a molecular weight that can be calculated from the structural formula when the maleimide compound X is not a polymer and when the structural formula of the maleimide compound X can be specified. When the maleimide compound X is a polymer, the molecular weight of the maleimide compound X means a weight average molecular weight in terms of polystyrene measured by gel permeation chromatography (GPC).

[0172] Commercially available examples of the maleimide compound X include "BMI-4000" and "BMI-5100" manufactured by Daiwa Chemical Industry Co., Ltd., "MIR-3000" manufactured by Nippon Kayaku Co., Ltd., and "BMI-3000" and "BMI-689" manufactured by Designer Molecules Inc.

[0173] <Epoxy compounds> As the epoxy compound, a conventionally known epoxy compound can be used. The epoxy compound is an organic compound having at least one epoxy group. The epoxy compound may be used alone or in combination of two or more kinds.

[0174] Examples of the epoxy compound include bisphenol A type epoxy compounds, bisphenol F type epoxy compounds, bisphenol S type epoxy compounds, phenol novolac type epoxy compounds, biphenyl type epoxy compounds, biphenyl novolac type epoxy compounds, biphenol type epoxy compounds, naphthalene type epoxy compounds, fluorene type epoxy compounds, phenol aralkyl type epoxy compounds, naphthol aralkyl type epoxy compounds, dicyclopentadiene type epoxy compounds, anthracene type epoxy compounds, epoxy compounds having an adamantane skeleton, epoxy compounds having a tricyclodecane skeleton, naphthylene ether type epoxy compounds, and epoxy compounds having a triazine nucleus in the skeleton.

[0175] The epoxy compound may be a glycidyl ether compound, which is a compound having at least one glycidyl ether group.

[0176] From the viewpoint of further lowering the dielectric tangent of the cured product, the epoxy compound preferably contains an epoxy compound having a fluorine atom.

[0177] From the viewpoint of further lowering the dielectric tangent of the cured product and enhancing the thermal dimensional stability and flame retardancy of the cured product, the epoxy compound preferably contains an epoxy compound having an aromatic skeleton, preferably contains an epoxy compound having a naphthalene skeleton or a phenyl skeleton, and is more preferably an epoxy compound having an aromatic skeleton.

[0178] From the viewpoint of further lowering the dielectric tangent of the cured product and improving the coefficient of linear expansion (CTE) of the cured product, it is preferable that the epoxy compound contains an epoxy compound that is liquid at 25°C and an epoxy compound that is solid at 25°C.

[0179] The viscosity at 25°C of the epoxy compound that is liquid at 25°C is preferably 1000 mPa·s or less, and more preferably 500 mPa·s or less.

[0180] The viscosity of the epoxy compound can be measured, for example, using a dynamic viscoelasticity measuring device ("VAR-100" manufactured by Rheologica Instruments).

[0181] It is more preferable that the molecular weight of the epoxy compound is 1000 or less. In this case, even if the content of the inorganic filler is 50% by weight or more in 100% by weight of the components excluding the solvent in the resin material, a resin material having high fluidity during the formation of an insulating layer can be obtained. Therefore, when the uncured or B-staged resin material is laminated on a circuit board, the inorganic filler can be uniformly present.

[0182] The molecular weight of the epoxy compound means a molecular weight that can be calculated from the structural formula when the epoxy compound is not a polymer and when the structural formula of the epoxy compound can be specified, and means a weight average molecular weight when the epoxy compound is a polymer.

[0183] From the viewpoint of further enhancing the thermal dimensional stability of the cured product, the content of the above-mentioned epoxy compound is preferably 4 wt % or more, more preferably 7 wt % or more, and preferably 15 wt % or less, more preferably 12 wt % or less, based on 100 wt % of the components excluding the solvent in the resin material.

[0184] The content of the epoxy compound is preferably 15% by weight or more, more preferably 25% by weight or more, and preferably 50% by weight or less, more preferably 40% by weight or less, based on 100% by weight of the components in the resin material excluding the inorganic filler and the solvent. When the content of the epoxy compound is equal to or more than the lower limit and equal to or less than the upper limit, the thermal dimensional stability of the cured product can be further improved.

[0185] The weight ratio of the content of the epoxy compound to the total content of the cyclohexane ring-containing compound and the curing agent described later (the content of the epoxy compound / the total content of the cyclohexane ring-containing compound and the curing agent described later) is preferably 0.2 or more, more preferably 0.3 or more, and preferably 1 or less, more preferably 0.8 or less. When the weight ratio is equal to or more than the lower limit and equal to or less than the upper limit, the dielectric tangent can be further lowered and the thermal dimensional stability can be further improved.

[0186] <Vinyl compounds> As the vinyl compound, a conventionally known vinyl compound can be used. The vinyl compound is an organic compound having at least one vinyl group. The vinyl compound may be used alone or in combination of two or more kinds.

[0187] The vinyl compound may be a styrene compound, an acrylate compound, a divinyl compound, etc. The divinyl compound may be a divinyl benzyl ether compound. The vinyl compound may be a divinyl compound having an aliphatic skeleton or a divinyl ether compound.

[0188] The styrene compound may be a phenylene ether compound modified with a terminal styrene. The styrene compound may be used alone or in combination of two or more kinds.

[0189] An example of a commercially available styrene compound is "OPE-2St" manufactured by Mitsubishi Gas Chemical Company, Inc.

[0190] In addition, the vinyl compounds such as the styrene compound and the acrylate compound also correspond to radical curing compounds. Therefore, the thermosetting compound preferably includes a radical curing compound. The thermosetting compound preferably includes a radical curing compound other than a maleimide compound. The resin material preferably includes a radical curing compound.

[0191] The content of the vinyl compound in 100% by weight of the components in the resin material excluding the inorganic filler and the solvent is preferably 3% by weight or more, more preferably 5% by weight or more, even more preferably 20% by weight or more, preferably 80% by weight or less, and more preferably 70% by weight or less. When the content of the vinyl compound is equal to or more than the lower limit and equal to or less than the upper limit, the dielectric tangent of the cured product can be further lowered and the thermal dimensional stability can be further improved.

[0192] [Inorganic filler] The resin material preferably contains an inorganic filler. By using the inorganic filler, the dielectric tangent of the cured product can be further reduced. In addition, by using the inorganic filler, the dimensional change of the cured product due to heat can be further reduced. The inorganic filler may be used alone or in combination of two or more kinds.

[0193] Examples of the inorganic filler include silica, talc, clay, mica, hydrotalcite, alumina, magnesium oxide, aluminum hydroxide, diamond, aluminum nitride, and boron nitride.

[0194] The inorganic filler is preferably an inorganic filler having a thermal conductivity of 10 W / mK or more, such as alumina or boron nitride, which can enhance heat dissipation.

[0195] From the viewpoint of reducing the surface roughness of the cured product, further increasing the adhesive strength between the cured product and the metal layer, forming finer wiring on the surface of the cured product, and imparting better insulation reliability to the cured product, the inorganic filler is preferably silica or alumina, more preferably silica, and even more preferably fused silica. The silica may be hollow silica. By using silica, the thermal expansion coefficient of the cured product is further reduced, and the dielectric tangent of the cured product is further reduced. In addition, by using silica, the surface roughness of the cured product is effectively reduced, and the adhesive strength between the cured product and the metal layer is effectively increased. The shape of the silica is preferably spherical.

[0196] From the viewpoints of promoting resin curing regardless of the curing environment, effectively increasing the glass transition temperature of the cured product, and effectively reducing the coefficient of linear thermal expansion of the cured product, it is preferable that the inorganic filler be spherical silica.

[0197] From the viewpoint of increasing the thermal conductivity and the insulating property, the inorganic filler is preferably alumina or boron nitride. In particular, boron nitride has anisotropy, and therefore can further reduce the coefficient of linear thermal expansion.

[0198] The inorganic filler has an average particle size of preferably 50 nm or more, more preferably 100 nm or more, even more preferably 500 nm or more, and preferably 5 μm or less, more preferably 3 μm or less, and even more preferably 1 μm or less. When the inorganic filler has an average particle size of not less than the lower limit and not more than the upper limit, the surface roughness after etching can be reduced and the plating peel strength can be increased, and the adhesion between the insulating layer and the metal layer can be further improved.

[0199] The median diameter (d50) at 50% is used as the average particle diameter of the inorganic filler. The average particle diameter can be measured using a particle size distribution measuring device using a laser diffraction scattering method. In addition, when the inorganic filler is an aggregated particle, the average particle diameter of the inorganic filler means the primary particle diameter.

[0200] The inorganic filler is preferably spherical, more preferably spherical silica. In this case, the surface roughness of the cured product is effectively reduced, and the adhesive strength between the cured product and the metal layer is effectively increased. When the inorganic filler is spherical, the aspect ratio of the inorganic filler is preferably 2 or less, more preferably 1.5 or less.

[0201] The inorganic filler is preferably surface-treated, more preferably surface-treated with a coupling agent, and even more preferably surface-treated with a silane coupling agent.By surface-treating the inorganic filler, the surface roughness of the roughened cured product is further reduced, and the adhesive strength between the cured product and the metal layer is further increased.In addition, by surface-treating the inorganic filler, finer wiring can be formed on the surface of the cured product, and better inter-wiring insulation reliability and inter-layer insulation reliability can be imparted to the cured product.

[0202] The coupling agent includes a silane coupling agent, a titanium coupling agent, an aluminum coupling agent, etc. The silane coupling agent includes a methacrylsilane, an acrylsilane, an aminosilane, an imidazole silane, a vinylsilane, an epoxysilane, etc.

[0203] The content of the inorganic filler in 100% by weight of the resin material excluding the solvent is preferably 50% by weight or more, more preferably 60% by weight or more, even more preferably 65% ​​by weight or more, particularly preferably 68% by weight or more, preferably 90% by weight or less, more preferably 85% by weight or less, even more preferably 80% by weight or less, particularly preferably 75% by weight or less. When the content of the inorganic filler is equal to or more than the lower limit, the dielectric loss tangent is effectively lowered. When the content of the inorganic filler is equal to or less than the upper limit, the thermal dimensional stability is improved and the warping of the cured product can be effectively suppressed. When the content of the inorganic filler is equal to or more than the lower limit and equal to or less than the upper limit, the surface roughness of the cured product can be further reduced, and finer wiring can be formed on the surface of the cured product. Furthermore, with this content of the inorganic filler, it is possible to lower the thermal expansion coefficient of the cured product and at the same time improve the smear removability.

[0204] [Hardening agent] The resin material preferably contains a curing agent. The curing agent is not particularly limited. A conventionally known curing agent can be used as the curing agent. The curing agent may be used alone or in combination of two or more kinds.

[0205] Examples of the curing agent include a phenol compound (phenol curing agent), an active ester compound, a cyanate ester compound (cyanate ester curing agent), a benzoxazine compound not having a cyclohexane ring (benzoxazine curing agent), a carbodiimide compound (carbodiimide curing agent), an amine compound (amine curing agent), a thiol compound (thiol curing agent), a phosphine compound, dicyandiamide, and an acid anhydride. The curing agent preferably has a functional group capable of reacting with the epoxy group of the epoxy compound.

[0206] From the viewpoint of further lowering the dielectric tangent of the cured product and further increasing the thermal dimensional stability of the cured product, the curing agent preferably contains at least one component selected from the group consisting of phenolic compounds, active ester compounds, cyanate ester compounds, benzoxazine compounds having no cyclohexane rings, carbodiimide compounds, and acid anhydrides. From the viewpoint of further lowering the dielectric tangent and further increasing the thermal dimensional stability, the curing agent more preferably contains at least one component selected from the group consisting of phenolic compounds, active ester compounds, cyanate ester compounds, benzoxazine compounds having no cyclohexane rings, and carbodiimide compounds, and even more preferably contains an active ester compound.

[0207] From the viewpoint of further enhancing the thermal dimensional stability, it is preferable that the thermosetting compound contains an epoxy compound, and the curing agent contains both a phenol compound and an active ester compound.

[0208] Examples of the phenol compound include novolak type phenols, biphenol type phenols, naphthalene type phenols, dicyclopentadiene type phenols, aralkyl type phenols, and dicyclopentadiene type phenols.

[0209] Commercially available phenol compounds include novolac phenols ("TD-2091" manufactured by DIC Corporation), biphenyl novolac phenols ("MEH-7851" manufactured by Meiwa Kasei Co., Ltd.), aralkyl phenol compounds ("MEH-7800" manufactured by Meiwa Kasei Co., Ltd.), and phenols having an aminotriazine skeleton ("LA-1356" and "LA-3018-50P" manufactured by DIC Corporation).

[0210] The above-mentioned active ester compound refers to a compound that contains at least one ester bond in the structure and has an aliphatic chain, an aliphatic ring, or an aromatic ring bonded to both sides of the ester bond. The active ester compound is obtained, for example, by a condensation reaction between a carboxylic acid compound or a thiocarboxylic acid compound and a hydroxy compound or a thiol compound. An example of the active ester compound is a compound represented by the following formula (1).

[0211] [ka]

[0212] In the above formula (1), X1 represents a group containing an aliphatic chain, a group containing an aliphatic ring, or a group containing an aromatic ring, and X2 represents a group containing an aromatic ring. Preferred examples of the group containing an aromatic ring include a benzene ring which may have a substituent, and a naphthalene ring which may have a substituent. Examples of the substituent include a hydrocarbon group. The number of carbon atoms in the hydrocarbon group is preferably 12 or less, more preferably 6 or less, and even more preferably 4 or less.

[0213] In the above formula (1), the combination of X1 and X2 includes a combination of an optionally substituted benzene ring and an optionally substituted benzene ring, and a combination of an optionally substituted benzene ring and an optionally substituted naphthalene ring. Furthermore, in the above formula (1), the combination of X1 and X2 includes a combination of an optionally substituted naphthalene ring and an optionally substituted naphthalene ring.

[0214] The active ester compound is not particularly limited. From the viewpoint of further improving thermal dimensional stability and flame retardancy, the active ester compound is preferably an active ester compound having two or more aromatic skeletons. From the viewpoint of lowering the dielectric tangent of the cured product and improving the thermal dimensional stability of the cured product, the active ester compound more preferably has a naphthalene ring or a dicyclopentadiene skeleton in the main chain skeleton.

[0215] Commercially available products of the above active ester compound include "HPC-8000-65T", "EXB9416-70BK", "EXB8100-65T", "HPC-8150-62T" and "EXB-8" manufactured by DIC Corporation.

[0216] From the viewpoint of lowering the melt viscosity of the resin material, shortening the distance between crosslinking points, and further reducing the linear expansion coefficient of the cured product, the active ester compound is preferably an ester compound having low molecular weight activity. Commercially available ester compounds having low molecular weight activity include the above-mentioned "EXB-8" manufactured by DIC Corporation.

[0217] Examples of the cyanate ester compound include novolac-type cyanate ester resins, bisphenol-type cyanate ester resins, and prepolymers obtained by partially trimerizing these. Examples of the novolac-type cyanate ester resins include phenol novolac-type cyanate ester resins and alkylphenol-type cyanate ester resins. Examples of the bisphenol-type cyanate ester resins include bisphenol A-type cyanate ester resins, bisphenol E-type cyanate ester resins, and tetramethylbisphenol F-type cyanate ester resins.

[0218] Commercially available products of the cyanate ester compound include phenol novolac type cyanate ester resins ("PT-30" and "PT-60" manufactured by Lonza Japan) and prepolymers in which bisphenol type cyanate ester resins are trimerized ("BA-230S", "BA-3000S", "BTP-1000S" and "BTP-6020S" manufactured by Lonza Japan).

[0219] The content of the cyanate ester compound in 100% by weight of the components in the resin material excluding the inorganic filler and the solvent is preferably 10% by weight or more, more preferably 15% by weight or more, even more preferably 20% by weight or more, and preferably 85% by weight or less, more preferably 75% by weight or less. When the content of the cyanate ester compound is equal to or more than the lower limit and equal to or less than the upper limit, the thermal dimensional stability of the cured product can be further improved.

[0220] Examples of the benzoxazine compound not having a cyclohexane ring include Pd-type benzoxazine and Fa-type benzoxazine.

[0221] Commercially available benzoxazine compounds not having a cyclohexane ring include "Pd type" manufactured by Shikoku Chemical Industry Co., Ltd. and "ODA-BOZ" manufactured by JFE Chemical Corporation.

[0222] In 100% by weight of the components in the resin material excluding the inorganic filler and the solvent, the content of the benzoxazine compound not having a cyclohexane ring is preferably 1% by weight or more, more preferably 5% by weight or more, even more preferably 10% by weight or more, preferably 70% by weight or less, more preferably 60% by weight or less. When the content of the benzoxazine compound not having a cyclohexane ring is equal to or more than the lower limit and equal to or less than the upper limit, the dielectric tangent of the cured product can be lowered and the thermal dimensional stability can be further improved.

[0223] The carbodiimide compound is a compound having a structural unit represented by the following formula (2). In the following formula (2), the right end and the left end are bonding sites with other groups. The above carbodiimide compounds may be used alone or in combination of two or more kinds.

[0224] [ka]

[0225] In the above formula (2), X represents an alkylene group, a group in which a substituent is bonded to an alkylene group, a cycloalkylene group, a group in which a substituent is bonded to a cycloalkylene group, an arylene group, or a group in which a substituent is bonded to an arylene group, and p represents an integer of 1 to 5. When a plurality of Xs are present, the plurality of Xs may be the same or different.

[0226] In one preferred embodiment, at least one X is an alkylene group, a group in which a substituent is bonded to an alkylene group, a cycloalkylene group, or a group in which a substituent is bonded to a cycloalkylene group.

[0227] Commercially available examples of the carbodiimide compound include "Carbodilite V-02B", "Carbodilite V-03", "Carbodilite V-04K", "Carbodilite V-07", "Carbodilite V-09", "Carbodilite 10M-SP", and "Carbodilite 10M-SP (modified)" manufactured by Nisshinbo Chemical Inc., as well as "Stavaxol P", "Stavaxol P400", and "Hi-Kasil 510" manufactured by Rhein Chemie.

[0228] Examples of the acid anhydride include tetrahydrophthalic anhydride and alkylstyrene-maleic anhydride copolymer.

[0229] Commercially available products of the above acid anhydrides include "Rikacid TDA-100" manufactured by New Japan Chemical Co., Ltd.

[0230] The content of the curing agent relative to 100 parts by weight of the epoxy compound is preferably 70 parts by weight or more, more preferably 85 parts by weight or more, and preferably 150 parts by weight or less, and more preferably 120 parts by weight or less. When the content of the curing agent is equal to or more than the lower limit and equal to or less than the upper limit, the curing property is more excellent, the thermal dimensional stability is more improved, and the volatilization of the remaining unreacted components can be more suppressed.

[0231] The total content of the cyclohexane ring-containing compound, the thermosetting compound, and the curing agent in the resin material (100% by weight, excluding the inorganic filler and the solvent) is preferably 40% by weight or more, more preferably 60% by weight or more, and preferably 98% by weight or less, more preferably 95% by weight or less. When the total content is equal to or more than the lower limit and equal to or less than the upper limit, the curability is more excellent and the thermal dimensional stability can be further improved.

[0232] [Cure accelerator] The resin material includes a curing accelerator. The use of the curing accelerator further accelerates the curing speed. By quickly curing the resin material, the crosslinked structure in the cured product becomes uniform, and the number of unreacted functional groups decreases, resulting in a high crosslink density. The curing accelerator is not particularly limited, and conventionally known curing accelerators can be used. The curing accelerator may be used alone or in combination of two or more.

[0233] Examples of the curing accelerator include anionic curing accelerators such as imidazole compounds, cationic curing accelerators such as amine compounds, curing accelerators other than anionic and cationic curing accelerators such as phosphorus compounds and organometallic compounds, and radical curing accelerators such as peroxides.

[0234] Examples of the imidazole compound include 2-undecylimidazole, 2-heptadecylimidazole, 2-methylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1,2-dimethylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, and 1-cyanoethyl-2-phenylimidazolium trimethylolate. remellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-methylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, and 2-phenyl-4-methyl-5-dihydroxymethylimidazole.

[0235] Examples of the amine compound include diethylamine, triethylamine, diethylenetetramine, triethylenetetramine, and 4,4-dimethylaminopyridine.

[0236] The phosphorus compound includes a triphenylphosphine compound.

[0237] Examples of the organometallic compound include zinc naphthenate, cobalt naphthenate, tin octoate, cobalt octoate, cobalt bisacetylacetonate (II), and cobalt trisacetylacetonate (III).

[0238] The peroxides include dicumyl peroxide and Perhexyl 25B.

[0239] From the viewpoint of further reducing the curing temperature and effectively suppressing warping of the cured product, the curing accelerator preferably contains the anionic curing accelerator, and more preferably contains the imidazole compound.

[0240] From the viewpoint of further suppressing the curing temperature and effectively suppressing warping of the cured product, the content of the anionic curing accelerator in 100% by weight of the curing accelerator is preferably 20% by weight or more, more preferably 50% by weight or more, even more preferably 70% by weight or more, and most preferably 100% by weight (total amount). Therefore, it is most preferable that the curing accelerator is the anionic curing accelerator.

[0241] When the thermosetting compound contains a radically curable compound such as the vinyl compound, the acrylate compound, or the styrene compound, radical curing proceeds, so the curing accelerator preferably contains the radical curing accelerator, and more preferably contains a radical curing accelerator having a one-minute half-life temperature of 170° C. or more and 200° C. or less. Commercially available radical curing accelerators having a one-minute half-life temperature of 170° C. or more and 200° C. or less include NOF Corp.'s "Perhexine 25B."

[0242] The content of the curing accelerator is not particularly limited. In 100% by weight of the components in the resin material excluding the inorganic filler and the solvent, the content of the curing accelerator is preferably 0.01% by weight or more, more preferably 0.05% by weight or more, preferably 5% by weight or less, more preferably 3% by weight or less. When the content of the curing accelerator is equal to or more than the lower limit and equal to or less than the upper limit, the resin material is cured efficiently. When the content of the curing accelerator is within a more preferred range, the storage stability of the resin material is further increased, and a better cured product is obtained.

[0243] [Thermoplastic resin] The resin material preferably contains a thermoplastic resin. Examples of the thermoplastic resin include polyvinyl acetal resin, polyimide resin, phenoxy resin, and styrene-butadiene resin. The thermoplastic resin may be used alone or in combination of two or more.

[0244] From the viewpoint of effectively lowering the dielectric tangent and effectively increasing the adhesion of the metal wiring regardless of the curing environment, the thermoplastic resin is preferably a phenoxy resin. By using the phenoxy resin, the deterioration of the embedding ability of the resin film in the holes or irregularities of the circuit board and the non-uniformity of the inorganic filler are suppressed. In addition, by using the phenoxy resin, the melt viscosity can be adjusted, so that the dispersibility of the inorganic filler is improved, and the resin composition or the B-stage product is less likely to wet and spread to unintended areas during the curing process.

[0245] The phenoxy resin contained in the resin material is not particularly limited. As the phenoxy resin, a conventionally known phenoxy resin can be used. The phenoxy resin may be used alone or in combination of two or more kinds.

[0246] Examples of the phenoxy resin include phenoxy resins having a skeleton such as a bisphenol A skeleton, a bisphenol F skeleton, a bisphenol S skeleton, a biphenyl skeleton, a novolac skeleton, a naphthalene skeleton, and an imide skeleton.

[0247] Commercially available examples of the phenoxy resin include "YP50", "YP55", and "YP70" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd., and "1256B40", "4250", "4256H40", "4275", "YX6954BH30", and "YX8100BH30" manufactured by Mitsubishi Chemical Corporation.

[0248] From the viewpoints of improving handleability, plating peel strength at low roughness, and adhesion between the insulating layer and the metal layer, the thermoplastic resin is preferably a polyimide resin (polyimide compound).

[0249] From the viewpoint of improving solubility, the polyimide compound is preferably a polyimide compound obtained by a method of reacting a tetracarboxylic dianhydride with a dimer diamine.

[0250] Examples of the tetracarboxylic dianhydride include pyromellitic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 3,3',4,4'-biphenylsulfone tetracarboxylic dianhydride, 1,4,5,8-naphthalene tetracarboxylic dianhydride, 2,3,6,7-naphthalene tetracarboxylic dianhydride, 3,3',4,4'-biphenyl ether tetracarboxylic dianhydride, 3,3',4,4'-dimethyldiphenylsilane tetracarboxylic dianhydride, 3,3',4,4'-tetraphenylsilane tetracarboxylic dianhydride, 1,2,3,4-furan tetracarboxylic dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)diphenylsulfonate, and 4,4'-bis(3,4-dicarboxyphenoxy)diphenylsulfonate. sulfide dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)diphenylsulfone dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)diphenylpropane dianhydride, 3,3',4,4'-perfluoroisopropylidenediphthalic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, bis(phthalic acid)phenylphosphine oxide dianhydride, p-phenylene-bis(triphenylphthalic acid) dianhydride, m-phenylene-bis(triphenylphthalic acid) dianhydride, bis(triphenylphthalic acid)-4,4'-diphenyl ether dianhydride, and bis(triphenylphthalic acid)-4,4'-diphenylmethane dianhydride.

[0251] Examples of the dimer diamine include VERSAMINE 551 (trade name, manufactured by BASF Japan, 3,4-bis(1-aminoheptyl)-6-hexyl-5-(1-octenyl)cyclohexene), VERSAMINE 552 (trade name, manufactured by Cognics Japan, hydrogenated VERSAMINE 551), PRIAMINE 1075, and PRIAMINE 1074 (trade names, all manufactured by Croda Japan).

[0252] The polyimide compound may have an acid anhydride structure, a maleimide structure, or a citraconic imide structure at the end. In this case, the polyimide compound may be reacted with an epoxy compound. By reacting the polyimide compound with an epoxy compound, the thermal dimensional stability of the cured product can be improved.

[0253] From the viewpoint of obtaining a resin material having even better storage stability, the weight average molecular weight of the thermoplastic resin, the polyimide resin and the phenoxy resin is preferably 10,000 or more, more preferably 15,000 or more, and preferably 100,000 or less, more preferably 50,000 or less.

[0254] The weight average molecular weights of the thermoplastic resin, the polyimide resin and the phenoxy resin indicate weight average molecular weights in terms of polystyrene measured by gel permeation chromatography (GPC).

[0255] The contents of the thermoplastic resin, the polyimide resin, and the phenoxy resin are not particularly limited. In 100% by weight of the components in the resin material excluding the inorganic filler and the solvent, the content of the thermoplastic resin (when the thermoplastic resin is a polyimide resin or a phenoxy resin, the content of the polyimide resin or the phenoxy resin) is preferably 1% by weight or more, more preferably 2% by weight or more, preferably 30% by weight or less, more preferably 20% by weight or less. When the content of the thermoplastic resin is equal to or more than the lower limit and equal to or less than the upper limit, the resin material has good embedding properties in holes or irregularities in a circuit board. When the content of the thermoplastic resin is equal to or more than the lower limit, the formation of a resin film becomes easier, and a better insulating layer is obtained. When the content of the thermoplastic resin is equal to or less than the upper limit, the thermal expansion coefficient of the cured product becomes even lower. When the content of the thermoplastic resin is equal to or less than the upper limit, the surface roughness of the surface of the cured product becomes even smaller, and the adhesive strength between the cured product and the metal layer becomes even higher.

[0256] [solvent] The resin material does not contain or contains a solvent. By using the solvent, the viscosity of the resin material can be controlled within a suitable range, and the coatability of the resin material can be improved. The solvent may be used to obtain a slurry containing the inorganic filler. The solvent may be used alone or in combination of two or more.

[0257] Examples of the solvent include acetone, methanol, ethanol, butanol, 2-propanol, 2-methoxyethanol, 2-ethoxyethanol, 1-methoxy-2-propanol, 2-acetoxy-1-methoxypropane, toluene, xylene, methyl ethyl ketone, N,N-dimethylformamide, methyl isobutyl ketone, N-methyl-pyrrolidone, n-hexane, cyclohexane, cyclohexanone, and naphtha, which is a mixture.

[0258] Most of the solvent is preferably removed when the resin composition is molded into a film. Therefore, the boiling point of the solvent is preferably 200°C or less, more preferably 180°C or less. The content of the solvent in the resin composition is not particularly limited. The content of the solvent can be appropriately changed in consideration of the coatability of the resin composition.

[0259] When the resin material is a B-stage film, the content of the solvent in 100% by weight of the B-stage film is preferably 1% by weight or more, more preferably 2% by weight or more, preferably 10% by weight or less, more preferably 5% by weight or less.

[0260] [Other ingredients] For the purpose of improving impact resistance, heat resistance, resin compatibility, workability, and the like, the resin material may contain an organic filler, a leveling agent, a flame retardant, a coupling agent, a colorant, an antioxidant, an ultraviolet degradation inhibitor, a defoaming agent, a thickener, a thixotropy imparting agent, and the like.

[0261] The organic filler may be a particulate material made of benzoxazine resin, benzoxazole resin, fluororesin, acrylic resin, styrene resin, or the like. The fluororesin may be polytetrafluoroethylene (PTFE), or the like. By using fluororesin particles as the organic filler, the relative dielectric constant of the cured product can be further reduced. The average particle size of the organic filler is preferably 1 μm or less. When the average particle size of the organic filler is equal to or less than the upper limit, the surface roughness after etching can be reduced and the plating peel strength can be increased, and the adhesion between the insulating layer and the metal layer can be further improved. The average particle size of the organic filler may be 50 nm or more.

[0262] The median diameter (d50) at 50% is used as the average particle diameter of the organic filler. The average particle diameter can be measured using a particle size distribution measuring device using a laser diffraction scattering method.

[0263] The coupling agent includes a silane coupling agent, a titanium coupling agent, an aluminum coupling agent, etc. The silane coupling agent includes a vinyl silane, an amino silane, an imidazole silane, an epoxy silane, etc.

[0264] (Resin film) The above-mentioned resin composition is molded into a film to obtain a resin film (B-stage product / B-stage film). The above-mentioned resin material is preferably a resin film. The resin film is preferably a B-stage film.

[0265] Examples of methods for forming a resin composition into a film to obtain a resin film include the following: an extrusion molding method in which a resin composition is melt-kneaded and extruded using an extruder, and then molded into a film using a T-die or a circular die; a casting molding method in which a resin composition containing a solvent is cast into a film; and other conventionally known film molding methods. The extrusion molding method and the casting molding method are preferred because they can be made thinner. Films include sheets.

[0266] The resin composition is molded into a film and dried by heating at, for example, 50° C. to 150° C. for 1 minute to 10 minutes to the extent that curing by heat does not proceed too much, to obtain a resin film that is a B-stage film.

[0267] The film-like resin composition obtained by the drying process as described above is called a B-stage film. The B-stage film is in a semi-cured state. The semi-cured product is not completely cured and can be further cured.

[0268] The resin film does not have to be a prepreg. When the resin film is not a prepreg, migration does not occur along the glass cloth, etc. In addition, when the resin film is laminated or precured, unevenness due to the glass cloth does not occur on the surface.

[0269] The resin film can be used in the form of a laminated film comprising a metal foil or a base film and a resin film laminated on the surface of the metal foil or the base film. The metal foil is preferably a copper foil.

[0270] Examples of the base film of the laminated film include polyester resin films such as polyethylene terephthalate film and polybutylene terephthalate film, olefin resin films such as polyethylene film and polypropylene film, and polyimide resin films. The surface of the base film may be subjected to a release treatment as necessary.

[0271] From the viewpoint of controlling the degree of cure of the resin film more uniformly, the thickness of the resin film is preferably 5 μm or more and preferably 200 μm or less. When the resin film is used as an insulating layer of a circuit, the thickness of the insulating layer formed by the resin film is preferably equal to or more than the thickness of the conductor layer (metal layer) forming the circuit. The thickness of the insulating layer is preferably 5 μm or more and preferably 200 μm or less.

[0272] (Semiconductor devices, printed wiring boards, copper-clad laminates and multi-layer printed wiring boards) The above-mentioned resin material is suitably used for forming a molding resin in which a semiconductor chip is embedded in a semiconductor device.

[0273] The resin material is preferably used as an insulating material, and is preferably used for forming an insulating layer in a printed wiring board.

[0274] The printed wiring board is obtained, for example, by hot-pressing and molding the resin material.

[0275] A laminated member having a metal layer on one or both sides can be laminated to the resin film. A laminated structure can be suitably obtained, which includes a laminated member having a metal layer on its surface and a resin film laminated on the surface of the metal layer, and the resin film is the above-mentioned resin material. The method for laminating the resin film and the laminated member having the metal layer on its surface is not particularly limited, and a known method can be used. For example, the resin film can be laminated to a laminated member having a metal layer on its surface while applying pressure with or without heating using a device such as a parallel plate press or a roll laminator.

[0276] The material of the metal layer is preferably copper.

[0277] The lamination target member having the metal layer on the surface thereof may be a metal foil such as a copper foil.

[0278] The resin material is preferably used to obtain a copper-clad laminate. An example of the copper-clad laminate is a copper-clad laminate including a copper foil and a resin film laminated on one surface of the copper foil.

[0279] The thickness of the copper foil of the copper-clad laminate is not particularly limited. The thickness of the copper foil is preferably within a range of 1 μm to 50 μm. In addition, in order to increase the adhesive strength between the cured product of the resin material and the copper foil, the copper foil preferably has fine irregularities on its surface. The method of forming the irregularities is not particularly limited. Examples of the method of forming the irregularities include a forming method by treatment using a known chemical solution.

[0280] The above resin materials are suitably used to obtain multi-layer substrates.

[0281] An example of the multilayer board is a multilayer board including a circuit board and an insulating layer laminated on the circuit board. The insulating layer of the multilayer board is formed of the resin material. The insulating layer of the multilayer board may be formed of the resin film of the laminate film by using a laminate film. The insulating layer is preferably laminated on the surface of the circuit board on which the circuit is provided. A part of the insulating layer is preferably embedded between the circuits.

[0282] In the multilayer board, the surface of the insulating layer opposite to the surface on which the circuit board is laminated is preferably roughened.

[0283] The roughening treatment method is not particularly limited and may be any conventionally known roughening treatment method. The surface of the insulating layer may be subjected to a swelling treatment before the roughening treatment.

[0284] Preferably, the multilayer substrate further comprises a copper plating layer laminated on the roughened surface of the insulating layer.

[0285] Another example of the multilayer board is a multilayer board comprising a circuit board, an insulating layer laminated on the surface of the circuit board, and a copper foil laminated on the surface of the insulating layer opposite to the surface on which the circuit board is laminated. The insulating layer is preferably formed by using a copper-clad laminate comprising copper foil and a resin film laminated on one surface of the copper foil, and curing the resin film. Furthermore, the copper foil is preferably etched to form a copper circuit.

[0286] Another example of the multilayer board is a multilayer board including a circuit board and a plurality of insulating layers laminated on a surface of the circuit board. At least one of the insulating layers arranged on the circuit board is formed using the resin material. The multilayer board preferably further includes a circuit laminated on at least one surface of the insulating layer formed using the resin film.

[0287] In the case of a multilayer printed wiring board among multilayer substrates, a low dielectric tangent and high insulation reliability due to an insulating layer are required, and therefore the resin material according to the present invention is suitably used for forming an insulating layer in the multilayer printed wiring board.

[0288] The multilayer printed wiring board includes, for example, a circuit board, a plurality of insulating layers disposed on a surface of the circuit board, and a metal layer disposed between the plurality of insulating layers, at least one of which is a cured product of the resin material.

[0289] FIG. 1 is a cross-sectional view showing a schematic diagram of a multilayer printed wiring board using a resin material according to one embodiment of the present invention.

[0290] In the multilayer printed wiring board 11 shown in FIG. 1, a plurality of insulating layers 13-16 are laminated on the upper surface 12a of the circuit board 12. The insulating layers 13-16 are cured layers. A metal layer 17 is formed on a partial region of the upper surface 12a of the circuit board 12. Of the plurality of insulating layers 13-16, the insulating layers 13-15 other than the insulating layer 16 located on the outer surface opposite to the circuit board 12 side have the metal layer 17 formed on a partial region of the upper surface. The metal layer 17 is a circuit. The metal layer 17 is disposed between the circuit board 12 and the insulating layer 13, and between each of the laminated insulating layers 13-16. The lower metal layer 17 and the upper metal layer 17 are connected to each other by at least one of a via hole connection and a through hole connection not shown.

[0291] In the multilayer printed wiring board 11, the insulating layers 13-16 are formed of a cured product of the above-mentioned resin material. In this embodiment, the surfaces of the insulating layers 13-16 are roughened, so that fine holes (not shown) are formed on the surfaces of the insulating layers 13-16. The metal layer 17 reaches the inside of the fine holes. In the multilayer printed wiring board 11, the width dimension (L) of the metal layer 17 and the width dimension (S) of the portion where the metal layer 17 is not formed can be reduced. In the multilayer printed wiring board 11, good insulation reliability is provided between the upper metal layer and the lower metal layer that are not connected by via hole connection and through hole connection (not shown).

[0292] (Roughening treatment and swelling treatment) The resin material is preferably used to obtain a cured product to be subjected to roughening treatment or desmear treatment. The cured product also includes a pre-cured product that can be further cured.

[0293] In order to form fine irregularities on the surface of the cured product obtained by pre-curing the resin material, the cured product is preferably subjected to a roughening treatment. The cured product is preferably subjected to a swelling treatment before the roughening treatment. The cured product is preferably subjected to a swelling treatment after the pre-curing and before the roughening treatment, and is further preferably cured after the roughening treatment. However, the cured product does not necessarily have to be subjected to a swelling treatment.

[0294] As a method of the swelling treatment, for example, a method of treating the cured product with an aqueous solution or an organic solvent dispersion solution of a compound mainly composed of ethylene glycol or the like is used. The swelling liquid used in the swelling treatment generally contains an alkali as a pH adjuster or the like. The swelling liquid preferably contains sodium hydroxide. Specifically, for example, the swelling treatment is performed by treating the cured product with a 40 wt% ethylene glycol aqueous solution or the like at a treatment temperature of 30°C to 85°C for 1 minute to 30 minutes. The temperature of the swelling treatment is preferably within the range of 50°C to 85°C. If the temperature of the swelling treatment is too low, the swelling treatment takes a long time, and the adhesive strength between the cured product and the metal layer tends to be lowered.

[0295] In the roughening treatment, a chemical oxidizing agent such as a manganese compound, a chromium compound, or a persulfate compound is used. These chemical oxidizing agents are used as an aqueous solution or an organic solvent dispersion after water or an organic solvent is added. The roughening solution used in the roughening treatment generally contains an alkali as a pH adjuster. The roughening solution preferably contains sodium hydroxide.

[0296] The manganese compounds include potassium permanganate and sodium permanganate. The chromium compounds include potassium dichromate and potassium chromate anhydride. The persulfate compounds include sodium persulfate, potassium persulfate, and ammonium persulfate.

[0297] The arithmetic mean roughness Ra of the surface of the cured product is preferably 10 nm or more, preferably less than 300 nm, more preferably less than 200 nm, and even more preferably less than 150 nm. In this case, the adhesive strength between the cured product and the metal layer is increased, and finer wiring is formed on the surface of the insulating layer. Furthermore, conductor loss can be suppressed, and signal loss can be suppressed. The arithmetic mean roughness Ra is measured in accordance with JIS B0601:1994.

[0298] (Desmear processing) A through hole may be formed in the cured product obtained by pre-curing the resin material. In the multilayer board, etc., a via or a through hole is formed as the through hole. For example, a via can be formed by irradiating a laser such as a CO2 laser. The diameter of the via is not particularly limited, but is about 60 μm to 80 μm. Due to the formation of the through hole, a smear, which is a resin residue derived from the resin component contained in the cured product, is often formed at the bottom of the via.

[0299] In order to remove the smears, the surface of the cured product is preferably subjected to a desmear treatment. The desmear treatment may also serve as a roughening treatment.

[0300] In the desmear treatment, a chemical oxidizing agent such as a manganese compound, a chromium compound, or a persulfate compound is used, as in the roughening treatment. These chemical oxidizing agents are used as an aqueous solution or an organic solvent dispersion after water or an organic solvent is added. The desmear treatment liquid used in the desmear treatment generally contains an alkali. The desmear treatment liquid preferably contains sodium hydroxide.

[0301] By using the above resin material, the surface roughness of the surface of the cured product after the desmear treatment is sufficiently small.

[0302] The present invention will be specifically described below by way of examples and comparative examples, but the present invention is not limited to the following examples.

[0303] The following materials were prepared:

[0304] (Cyclohexane ring-containing compounds) Cyclohexane ring-containing maleimide compound 1: A cyclohexane ring-containing maleimide compound 1 (molecular weight 4200) represented by the following formula (1A) was synthesized according to the following Synthesis Example 1. In the obtained cyclohexane ring-containing maleimide compound 1, the average proportion of the first skeleton derived from the aliphatic diamine compound A was 100 mol %, and the average proportion of the second skeleton derived from the dimer diamine was 0 mol %, relative to 100 mol % of all structural units of the skeleton derived from the diamine compound.

[0305] <Synthesis Example 1> As the aliphatic diamine compound A, tricyclodecanediamine was used.

[0306] In a 500 mL eggplant flask, 90 g of toluene, 46 g of N-methyl-2-pyrrolidone (NMP), and 9 g of methanesulfonic acid were placed. Then, 15.6 g (80 mmol) of tricyclodecanediamine was added. Then, 17.7 g (60 mmol) of biphenyl dianhydride was added little by little. Then, the eggplant flask was attached to a Dean-Stark apparatus and heated under reflux for 3.5 hours. In this way, a compound having an acid anhydride structure at the end and a plurality of imide skeletons was obtained. After removing the moisture discharged during condensation and returning to room temperature, 4.42 g (45 mmol) of maleic anhydride was added and stirred, and similarly heated to react. The organic layer was washed with a mixed solvent of water and ethanol, and the mixed solvent was removed to obtain a toluene solution. Then, isopropanol was added to the toluene solution to reprecipitate the product. After that, it was dried in a vacuum oven to obtain a cyclohexane ring-containing maleimide compound 1.

[0307] [ka]

[0308] Cyclohexane ring-containing maleimide compound 2: A cyclohexane ring-containing maleimide compound 2 (molecular weight 13,000) represented by the following formula (2A) was synthesized according to the following Synthesis Example 2. In the obtained cyclohexane ring-containing maleimide compound 2, the average proportion of the first skeleton derived from the aliphatic diamine compound A was 90 mol %, and the average proportion of the second skeleton derived from the dimer diamine was 10 mol %, relative to 100 mol % of all structural units derived from the diamine compound.

[0309] <Synthesis Example 2> As the aliphatic diamine compound A, tricyclodecanediamine was used.

[0310] In a 500 mL eggplant flask, 90 g of toluene, 46 g of N-methyl-2-pyrrolidone (NMP), and 8 g of methanesulfonic acid were placed. Then, 3.1 g (7.5 mmol) of dimer diamine ("PRIAMINE 1075" manufactured by Croda Japan) and 13.1 g (67.5 mmol) of tricyclodecane diamine were added. Then, 13.1 g (60 mmol) of pyromellitic dianhydride was added little by little. The eggplant flask was attached to a Dean-Stark apparatus and heated under reflux for 3.5 hours. In this way, a compound having amines at both ends and multiple imide skeletons was obtained. After removing the moisture discharged during condensation and returning to room temperature, 4.42 g (45 mmol) of maleic anhydride was added and stirred, and similarly heated and reacted. In this way, a compound having maleimide skeletons at both ends was obtained. The organic layer was washed with a mixed solvent of water and ethanol, and the mixed solvent was removed to obtain a toluene solution. Next, isopropanol was added to the toluene solution to reprecipitate the product, which was then dried in a vacuum oven to obtain cyclohexane ring-containing maleimide compound 2.

[0311] [ka]

[0312] Cyclohexane ring-containing maleimide compound 3: A cyclohexane ring-containing maleimide compound 3 (molecular weight 3800) represented by the following formula (3A) was synthesized according to the following Synthesis Example 3. In the obtained cyclohexane ring-containing maleimide compound 3, the average proportion of the first skeleton derived from the aliphatic diamine compound A was 88 mol %, and the average proportion of the second skeleton derived from the dimer diamine was 12 mol %, relative to 100 mol % of all structural units of the skeleton derived from the diamine compound.

[0313] <Synthesis Example 3> In a 500 mL eggplant flask, 90 g of toluene, 46 g of N-methyl-2-pyrrolidone (NMP), and 8 g of methanesulfonic acid were placed. Then, 3.3 g (8.0 mmol) of dimer diamine ("PRIAMINE 1075" manufactured by Croda Japan) and 11.1 g (72 mmol) of norbornane diamine ("Pro-NBDA" manufactured by Mitsui Fine Chemicals) were added. Next, 15.9 g (54 mmol) of biphenyl dianhydride and 1.5 g (6 mmol) of bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride were mixed and then added little by little. The eggplant flask was attached to a Dean-Stark apparatus and heated under reflux for 3.5 hours. In this way, a compound having amines at both ends and multiple imide skeletons was obtained. The water discharged during the condensation was removed, and the mixture was returned to room temperature. Then, 4.42 g (45 mmol) of maleic anhydride was added, stirred, and similarly heated to react. In this way, a compound having a maleimide skeleton at both ends was obtained. The organic layer was washed with a mixed solvent of water and ethanol, and the mixed solvent was removed to obtain a toluene solution. Next, isopropanol was added to the toluene solution to reprecipitate the product. The mixture was then dried in a vacuum oven to obtain cyclohexane ring-containing maleimide compound 3.

[0314] [ka]

[0315] Cyclohexane ring-containing maleimide compound 4: Cyclohexane ring-containing maleimide compound 4 (molecular weight 4000) was synthesized according to the following Synthesis Example 4. In the obtained cyclohexane ring-containing maleimide compound 4, the average proportion of the first skeleton derived from aliphatic diamine compound A was 82 mol %, the average proportion of the second skeleton derived from dimer diamine compound A was 11 mol %, and the average proportion of the third skeleton derived from diamine compound B was 7 mol %, relative to 100 mol % of all structural units derived from the diamine compound.

[0316] <Synthesis Example 4> In a 500 mL eggplant flask, 90 g of toluene, 46 g of N-methyl-2-pyrrolidone (NMP), and 8 g of methanesulfonic acid were placed. Next, 3.3 g (8.0 mmol) of dimer diamine ("PRIAMINE 1075" manufactured by Croda Japan Co., Ltd.), 9.5 g (66.7 mmol) of norbornane diamine ("Pro-NBDA" manufactured by Mitsui Fine Chemicals Co., Ltd.), and 1.8 g (5.3 mmol) of 4,4'-(hexafluoroisopropylidene)dianiline were added. Next, 15.9 g (54 mmol) of biphenyl dianhydride and 1.5 g (6 mmol) of bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride were mixed and then added little by little. The eggplant flask was attached to a Dean-Stark apparatus and heated to reflux for 3.5 hours. In this way, a compound having amines at both ends and multiple imide skeletons was obtained. After removing the moisture discharged during condensation and returning to room temperature, 4.42 g (45 mmol) of maleic anhydride was added and stirred, and similarly heated to react. In this way, a compound having maleimide skeletons at both ends was obtained. The organic layer was washed with a mixed solvent of water and ethanol, and the mixed solvent was removed to obtain a toluene solution. Next, isopropanol was added to the toluene solution to reprecipitate the product. After that, it was dried in a vacuum oven to obtain cyclohexane ring-containing maleimide compound 4.

[0317] The molecular weights of the cyclohexane ring-containing maleimide compounds synthesized in Synthesis Examples 1 to 4 were determined as follows.

[0318] GPC (Gel Permeation Chromatography) Measurement: The measurements were performed using a Shimadzu high-performance liquid chromatograph system, with tetrahydrofuran (THF) as the developing medium, at a column temperature of 40°C and a flow rate of 1.0 ml / min. The detector used was an SPD-10A, and two Shodex KF-804L columns (with an exclusion limit of 400,000) were connected in series. Tosoh TSK Standard Polystyrene was used as the standard polystyrene, and a calibration curve was created using substances with weight-average molecular weights Mw = 354,000, 189,000, 98,900, 37,200, 17,100, 9,830, 5,870, 2,500, 1,050, and 500, and the molecular weights were calculated.

[0319] The average ratio of each skeleton of the cyclohexane ring-containing maleimide compounds synthesized in Synthesis Examples 2 to 4 is as follows: 1 It was calculated from the peak area ratio of H-NMR.

[0320] (thermosetting compound) Biphenyl-type epoxy compound ("NC-3000" manufactured by Nippon Kayaku Co., Ltd.) Naphthalene-type epoxy compound ("ESN-475V" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd.) Resorcinol diglycidyl ether (Nagase Chemtex Corporation "EX-201") Epoxy compound with a glycidylamine skeleton ("630" manufactured by Mitsubishi Chemical Corporation) Epoxy compound with a polybutadiene skeleton (Daicel Corporation's "PB3600") Epoxy compound with an amide skeleton ("WHR-991S" manufactured by Nippon Kayaku Co., Ltd.) Hyperbranched aliphatic epoxy compound (Nissan Chemical's "FoldiE101") Maleimide compound 1 (N-alkyl bismaleimide compound, "BMI-1500" manufactured by Designer Molecules Inc.) Maleimide compound 2 (N-alkyl bismaleimide compound, "BMI-1700" manufactured by Designer Molecules Inc.) Maleimide compound 3 (Daiwa Kasei Co., Ltd. "BMI-4100") Maleimide compound 4 ("MIR-3000" manufactured by Nippon Kayaku Co., Ltd.) Styrene compound ("OPE-2St-1200" manufactured by Mitsubishi Gas Chemical Company, Inc., radical curing compound, styrene compound having a phenylene ether skeleton) Acrylate compound (Kyoeisha Chemical's "Light Acrylate DCP-A", a radical curing compound, abbreviated as "DCP-A" in the table)

[0321] (Inorganic filler) Silica-containing slurry (75% silica by weight: Admatechs "SC4050-HOA", average particle size 1.0 μm, aminosilane treatment, cyclohexanone 25% by weight)

[0322] (hardening agent) Active ester compound 1-containing liquid (DIC Corporation "EXB-9416-70BK", solid content 70% by weight) Active ester compound 2-containing liquid (DIC Corporation "HPC-8150-62T", solid content 62% by weight) Active ester compound 3-containing liquid (DIC Corporation "HPC-8000L-65T", solid content 65% by weight) Active ester compound 4 (DIC "EXB-8", solid content 100% by weight) Carbodiimide compound ("Carbodilite V-03" manufactured by Nisshinbo Chemical Co., Ltd., abbreviated as "V-03" in the table) Phenol compound-containing liquid (DIC "LA-1356", solid content 60% by weight)

[0323] (Cure accelerator) Dimethylaminopyridine ("DMAP" manufactured by Wako Pure Chemical Industries, Ltd.) 2-Phenyl-4-methylimidazole ("2P4MZ" manufactured by Shikoku Chemical Industry Co., Ltd., anionic curing accelerator) Dicumyl Peroxide

[0324] (thermoplastic resin) Styrene butadiene resin ("Tuftec H1043" manufactured by Asahi Kasei Corporation, abbreviated as "H1043" in the table) Alicyclic thermoplastic resin ("Neoresin EP-140" manufactured by JXTG Corporation, abbreviated as "EP-140" in the table) Polyimide compounds (polyimide resins): A solution containing a polyimide compound (non-volatile content: 26.8% by weight), which is a reaction product of tetracarboxylic dianhydride and dimer diamine, was synthesized according to Synthesis Example 5 below.

[0325] <Synthesis Example 5> In a reaction vessel equipped with a stirrer, a water divider, a thermometer, and a nitrogen gas inlet tube, 300.0 g of tetracarboxylic dianhydride ("BisDA-1000" manufactured by SABIC Japan LLC) and 665.5 g of cyclohexanone were placed, and the solution in the reaction vessel was heated to 60°C. Next, 89.0 g of dimer diamine ("PRIAMINE1075" manufactured by Croda Japan) and 54.7 g of 1,3-bisaminomethylcyclohexane (manufactured by Mitsubishi Gas Chemical Co., Ltd.) were dropped into the reaction vessel. Next, 121.0 g of methylcyclohexane and 423.5 g of ethylene glycol dimethyl ether were added to the reaction vessel, and the imidization reaction was carried out at 140°C for 10 hours. In this way, a polyimide compound-containing solution (non-volatile content 26.8% by weight) was obtained. The molecular weight (weight average molecular weight) of the obtained polyimide compound was 20,000. The molar ratio of acid component / amine component was 1.04.

[0326] The molecular weight of the polyimide compound synthesized in Synthesis Example 5 was determined as follows.

[0327] GPC (Gel Permeation Chromatography) Measurement: The measurements were performed using a Shimadzu high-performance liquid chromatograph system, with tetrahydrofuran (THF) as the developing medium, at a column temperature of 40°C and a flow rate of 1.0 ml / min. The detector used was an SPD-10A, and two Shodex KF-804L columns (with an exclusion limit of 400,000) were connected in series. Tosoh TSK Standard Polystyrene was used as the standard polystyrene, and a calibration curve was created using substances with weight-average molecular weights Mw = 354,000, 189,000, 98,900, 37,200, 17,100, 9,830, 5,870, 2,500, 1,050, and 500, and the molecular weights were calculated.

[0328] (Examples 1 to 10 and Comparative Examples 1 and 2) The components shown in Tables 1 and 2 below were mixed in the amounts (unit: parts by weight of solid content) shown in Tables 1 and 2 below, and stirred at room temperature until a homogeneous solution was obtained, to obtain a resin material.

[0329] Preparation of resin film: The obtained resin material was applied to the release-treated surface of a release-treated PET film (Toray Industries, Inc., "XG284", thickness 25 μm) using an applicator, and then dried for 2 minutes and 30 seconds in a gear oven at 100°C to volatilize the solvent. In this way, a laminated film (a laminated film of a PET film and a resin film) was obtained in which a resin film (B-stage film) with a thickness of 40 μm was laminated on the PET film.

[0330] (evaluation) (1) Dielectric tangent The obtained resin film was heated at 190°C for 90 minutes to obtain a cured product. The obtained cured product was cut into a size of 2 mm in width and 80 mm in length, and 10 sheets were stacked together. The dielectric tangent was measured at room temperature (23°C) and a frequency of 5.8 GHz by the cavity resonance method using a "Cavity Resonance Perturbation Method Dielectric Constant Measurement Device CP521" manufactured by Kanto Electronics Application Development Co., Ltd. and a "Network Analyzer N5224A PNA" manufactured by Keysight Technologies, Inc.

[0331] [Criteria for dielectric tangent] 〇: Dielectric tangent is 3.0×10 -3 less than ×: Dielectric tangent is 3.0×10 -3 End

[0332] (2) Thermal dimensional stability (average coefficient of linear expansion (CTE)) The resulting 40μm thick resin film (B-stage film) was heated at 190℃ for 90 minutes, and the resulting cured product was cut into pieces measuring 3mm x 25mm. Using a thermomechanical analyzer (SII NanoTechnology's "EXSTAR TMA / SS6100"), the average linear expansion coefficient (ppm / ℃) of the cut cured product from 25℃ to 150℃ was calculated under conditions of a tensile load of 33mN and a heating rate of 5℃ / min.

[0333] [Criteria for determining average linear expansion coefficient] ○○: Average linear expansion coefficient is 23ppm / ℃ or less ○: Average linear expansion coefficient is more than 23 ppm / ℃ and less than 25 ppm / ℃ ×: Average linear expansion coefficient exceeds 25 ppm / ℃

[0334] (3) Surface roughness after etching and uniformity of surface roughness Lamination process and semi-curing process: A double-sided copper-clad laminate (CCL substrate) (Hitachi Chemical's "E679FG") was prepared. Both sides of the copper foil surface of this double-sided copper-clad laminate were immersed in MEC's ​​"Cz8101" to roughen the copper foil surface. On both sides of the roughened copper-clad laminate, the resin film (B stage film) side of the laminate film was laminated on the copper-clad laminate using Meiki Seisakusho's "Batch Vacuum Laminator MVLP-500-IIA" to obtain a laminated structure. The lamination conditions were reduced pressure for 30 seconds to make the air pressure 13 hPa or less, and then pressed at 100°C and a pressure of 0.4 MPa for 30 seconds. Then, the resin film was semi-cured by heating at 180°C for 30 minutes. In this way, a laminate in which a semi-cured resin film was laminated on a CCL substrate was obtained.

[0335] Roughening treatment: (a) Swelling treatment: The obtained laminate was placed in a swelling liquid (Swelling Dip Securigant P, manufactured by Atotech Japan) at 60° C. and shaken for 10 minutes, after which it was washed with pure water.

[0336] (b) Permanganate treatment (roughening and desmearing): The laminate after the swelling treatment was placed in a roughening aqueous solution of potassium permanganate ("Concentrate Compact CP" manufactured by Atotech Japan) at 80° C. and swung for 30 minutes. Next, it was treated for 2 minutes using a cleaning solution ("Reduction Securigant P" manufactured by Atotech Japan) at 25° C., and then washed with pure water to obtain an evaluation sample.

[0337] Surface roughness measurement: Ten areas of 94 μm × 123 μm were arbitrarily selected on the surface of the evaluation sample (roughened cured product). The arithmetic mean roughness Ra was measured for each of the ten areas using a non-contact three-dimensional surface shape measuring device (Veeco's "WYKO NT1100"). The surface roughness was evaluated as follows from the average value of the arithmetic mean roughness Ra measured at the ten locations, and the uniformity of the surface roughness was evaluated as follows from the absolute value of the difference between the maximum and minimum values ​​of the arithmetic mean roughness Ra measured at the ten locations. The arithmetic mean roughness Ra was measured in accordance with JIS B0601:1994.

[0338] [Criteria for surface roughness after etching] ○: The average value of the arithmetic mean roughness Ra is less than 50 nm △: The average value of the arithmetic mean roughness Ra is 50 nm or more and less than 80 nm ×: The average value of the arithmetic mean roughness Ra is 80 nm or more.

[0339] [Criteria for judging uniformity of surface roughness after etching] ○: The absolute value of the difference between the maximum and minimum values ​​of the arithmetic mean roughness Ra is less than 10 nm △: The absolute value of the difference between the maximum and minimum values ​​of the arithmetic mean roughness Ra is 10 nm or more and less than 20 nm ×: The absolute value of the difference between the maximum and minimum values ​​of the arithmetic mean roughness Ra is 20 nm or more.

[0340] (4) Plating peel strength Lamination process and semi-curing process: A 100 mm square double-sided copper-clad laminate (CCL substrate) (Hitachi Chemical's "E679FG") was prepared. Both sides of the copper foil surface of this double-sided copper-clad laminate were immersed in MEC's ​​"Cz8101" to roughen the copper foil surface. On both sides of the roughened copper-clad laminate, the resin film (B stage film) side of the laminate film was laminated on the copper-clad laminate using Meiki Seisakusho's "Batch Vacuum Laminator MVLP-500-IIA" to obtain a laminated structure. The lamination conditions were reduced pressure for 30 seconds to make the air pressure 13 hPa or less, then laminated at 100°C and pressure 0.7 MPa for 30 seconds, and further pressed at a press pressure of 0.8 MPa and a press temperature of 100°C for 60 seconds. Thereafter, with the PET film still attached, the resin film in the laminate structure was heated at 100°C for 30 minutes, and then further heated at 180°C for 30 minutes to semi-cure the resin film. The PET film was then peeled off to obtain a laminate in which the semi-cured resin film was laminated on the CCL substrate.

[0341] Roughening treatment: (a) Swelling treatment: The obtained laminate was placed in a swelling liquid (Swelling Dip Securigant P, manufactured by Atotech Japan) at 60° C. and shaken for 10 minutes, after which it was washed with pure water.

[0342] (b) Permanganate treatment (roughening and desmearing): The laminate after the swelling treatment was placed in a roughening aqueous solution of potassium permanganate ("Concentrate Compact CP" manufactured by Atotech Japan) at 80° C. and swung for 30 minutes. Next, it was treated for 2 minutes with a cleaning solution ("Reduction Securigant P" manufactured by Atotech Japan) at 25° C., and then washed with pure water to perform a roughening treatment.

[0343] Electroless plating process: The surface of the roughened cured product was treated with an alkaline cleaner (Atotech Japan's "Cleaner Securigant 902") at 60°C for 5 minutes, and degreased and washed. After washing, the cured product was treated with a pre-dip liquid (Atotech Japan's "Pre-dip Neogant B") at 25°C for 2 minutes. The cured product was then treated with an activator liquid (Atotech Japan's "Activator Neogant 834") at 40°C for 5 minutes to attach a palladium catalyst. Next, the cured product was treated with a reducing liquid (Atotech Japan's "Reducer Neogant WA") at 30°C for 5 minutes.

[0344] Next, the above cured product was placed in a chemical copper solution ("Basic Printganth MSK-DK", "Copper Printganth MSK", "Stabilizer Printganth MSK", and "Reducer Cu" manufactured by Atotech Japan) and electroless plating was performed until the plating thickness reached approximately 0.5 μm. After electroless plating, an annealing treatment was performed at a temperature of 120° C. for 30 minutes to remove residual hydrogen gas. All steps up to the electroless plating step were performed using 2 L of treatment solution on a beaker scale while the cured product was rocked.

[0345] Electrolytic plating process: Next, electrolytic plating was performed on the electroless plated cured product until the plating thickness reached 25 μm. For electrolytic copper plating, a copper sulfate solution ("Copper Sulfate Pentahydrate" manufactured by Wako Pure Chemical Industries, Ltd., "Sulfuric Acid" manufactured by Wako Pure Chemical Industries, Ltd., "Basic Leveler Cupracid HL" manufactured by Atotech Japan, and "Correction Agent Cupracid GS" manufactured by Atotech Japan) was used at 0.6 A / cm 2 A current of 1000 vol / min was applied to the copper plated material, and electrolytic plating was performed until the plating thickness reached about 25 μm. After the copper plating process, the cured product was heated at 200° C. for 60 minutes to further cure the cured product. In this way, a cured product having a copper plating layer laminated on the upper surface was obtained.

[0346] Plating peel strength measurement: A total of six 10 mm-wide rectangular cuts were made at 5 mm intervals on the surface of the copper plating layer of the cured product with the copper plating layer laminated on the upper surface. The cured product with the copper plating layer laminated on the upper surface was placed in a 90° peel tester (TE-3001, manufactured by Tester Sangyo Co., Ltd.), the end of the copper plating layer with the cut was picked up with a gripper, and the copper plating layer was peeled off by 20 mm to measure the peel strength (plating peel strength). The peel strength (plating peel strength) was measured for each of the six cut locations, and the average plating peel strength was calculated. The plating peel strength was evaluated according to the following criteria.

[0347] [Criteria for determining plating peel strength] ○: Average plating peel strength is 0.45kgf / cm or more △: Average plating peel strength is 0.35kgf / cm or more and less than 0.45kgf / cm ×: Average plating peel strength is less than 0.35kgf / cm

[0348] (5) Glass transition temperature Tg The obtained 40 μm thick resin film (B-stage film) was heated at 190 °C for 90 minutes, and the cured product was cut into pieces of 5 mm x 50 mm. Measurements were performed using a thermomechanical analyzer (SII NanoTechnology's "DMS6100") under the following conditions: chuck distance 20 mm, amplitude 10 μm, initial tension amplitude value 400 mN, temperature increase rate of 5 °C / min from 50 °C to 330 °C, and frequency of 10 Hz. The peak temperature of the loss tangent in the obtained measurement results was taken as the glass transition temperature Tg (°C).

[0349] [Criteria for determining glass transition temperature Tg] ○○: Tg is 185℃ or higher ○: Tg is 175℃ or higher and less than 185℃ ×: Tg is less than 175°C

[0350] (6) Thermal shock test An evaluation board for thermal shock testing (an evaluation board including a copper-clad laminate and a six-layer insulation-wiring circuit composite layer) was fabricated as follows. In the evaluation board, the via holes formed in each layer were connected. In other words, the following evaluation was performed on the evaluation board with multi-stage stacked vias.

[0351] Formation of the first insulation-wiring circuit composite layer: (a1) Lamination process: A double-sided copper-clad laminate (copper foil thickness of 18 μm on each side, substrate thickness of 0.7 mm, substrate size of 100 mm × 100 mm, Hitachi Chemical Co., Ltd. "MCL-E679FG") was prepared. Both sides of the copper foil surface of this double-sided copper-clad laminate were immersed in MEC Co., Ltd.'s "Cz8101" to roughen the copper foil surface. On both sides of the roughened copper-clad laminate, the resin film (B stage film) side of the laminate film was laminated on the copper-clad laminate using Meiki Seisakusho Co., Ltd.'s "Batch Vacuum Laminator MVLP-500 / 600-IIA". The lamination conditions were reduced pressure for 30 seconds to make the air pressure 13 hPa or less, and then pressed at 100 ° C and a pressure of 0.4 MPa for 30 seconds. After peeling off the PET film, the resin film was semi-cured (pre-cured) by heating at 130 ° C for 60 minutes. In this way, a laminate (1) was obtained in which a semi-cured resin film was laminated on a CCL substrate.

[0352] (b1) Via hole formation process: Using a CO2 laser processing machine ("LC-4KF212" manufactured by Via Mechanics), via holes with a diameter of approximately 60 μm were formed under the conditions of burst mode, energy of 0.4 mJ, pulse of 27 μsec, and 3 shots.

[0353] (c1) Desmearing and roughening treatment: (c1-1) Swelling treatment: The obtained laminate (1) was placed in a swelling liquid (Swelling Dip Securigant P, manufactured by Atotech Japan) at 60° C. and swung for 10 minutes, after which it was washed with pure water.

[0354] (c1-2) Permanganate treatment (roughening and desmearing): The laminate (1) after the swelling treatment was placed in a roughening aqueous solution of potassium permanganate ("Concentrate Compact CP" manufactured by Atotech Japan) at 80° C. and swung for 30 minutes. Next, it was treated for 2 minutes using a cleaning solution ("Reduction Securigant P" manufactured by Atotech Japan) at 25° C., and then washed with pure water to obtain the laminate (1) after the roughening treatment.

[0355] (c1-3) Measurement of surface roughness: The surface of the laminate (1) (roughened cured product) after the roughening treatment was measured for arithmetic mean roughness Ra in a measurement area of ​​95.6 μm × 71.7 μm using a non-contact three-dimensional surface profiler (Bruker's "Contour GT-K"). The arithmetic mean roughness Ra was measured in accordance with JIS B0601:1994. It was confirmed that the surface roughness of the roughened cured product was 200 nm or less.

[0356] (d1) Electroless plating process: The surface of the cured laminate (1) after the roughening treatment was treated with an alkaline cleaner at 60°C (Atotech Japan's "Cleaner Securigant 902") for 5 minutes, and degreased and washed. After washing, the cured product was treated with a pre-dip liquid at 25°C (Atotech Japan's "Pre-dip Neogant B") for 2 minutes. Thereafter, the cured product was treated with an activator liquid at 40°C (Atotech Japan's "Activator Neogant 834") for 5 minutes, and a palladium catalyst was applied. Next, the cured product was treated with a reducing liquid at 30°C (Atotech Japan's "Reducer Neogant WA") for 5 minutes.

[0357] Next, the above cured product was placed in a chemical copper solution ("Basic Printganth MSK-DK", "Copper Printganth MSK", "Stabilizer Printganth MSK", and "Reducer Cu" manufactured by Atotech Japan) and electroless plating was performed until the plating thickness reached approximately 0.5 μm. After electroless plating, an annealing treatment was performed at a temperature of 120° C. for 30 minutes to remove residual hydrogen gas. All steps up to the electroless plating step were performed using 2 L of treatment solution on a beaker scale while the cured product was rocked.

[0358] (e1) Resist formation: A dry film resist ("RY5125" manufactured by Hitachi Chemical Co., Ltd.) was applied using a hot roll laminator. The lamination conditions were a temperature of 100°C, a pressure of 0.4 MPa, and a lamination speed of 1.5 m / min, and the lamination was held for 15 minutes. Then, a fluence of 85 mJ / cm 2 After exposure to light at 400° C., the resist was developed by spraying a 1 wt % aqueous solution of sodium carbonate at a spray pressure of 1.2 MPa for 30 seconds at 27° C.

[0359] (f1) Electrolytic plating process: Next, electrolytic plating was performed on the electroless plated cured product until the plating thickness reached 25 μm. For electrolytic copper plating, a copper sulfate solution ("Copper Sulfate Pentahydrate" manufactured by Wako Pure Chemical Industries, Ltd., "Sulfuric Acid" manufactured by Wako Pure Chemical Industries, Ltd., "Basic Leveler Cupracid HL" manufactured by Atotech Japan, and "Correction Agent Cupracid GS" manufactured by Atotech Japan) was used at 0.6 A / cm 2 A current of 1000 vol. was applied and electrolytic plating was carried out until the plating thickness reached about 25 μm.

[0360] (g1) DFR stripping and etching process: The dry film resist (DFR) was removed by spraying with a 3 wt% aqueous solution of sodium hydroxide, followed by quick etching with a sulfuric acid peroxide-based acid etching solution (JCU's "SAC Process").

[0361] (h1) Main curing process: Heated at 200°C for 1.5 hours.

[0362] In this manner, a first insulating-wiring circuit composite layer was formed on the copper-clad laminate.

[0363] Formation of the second insulation-wiring circuit composite layer: (a2) Lamination process: The first wiring circuit layer was roughened under the same conditions as those used in the lamination step (a1). Then, the resin film (B-stage film) side of the laminate film was laminated onto the first insulation-wiring circuit composite layer under the same lamination conditions as those used in the lamination step (a1). The PET film was then peeled off and the resin film was semi-cured by heating at 130°C for 60 minutes. In this way, a laminate (2) was obtained in which a semi-cured resin film was laminated onto the first insulation-wiring circuit composite layer.

[0364] (b2) Via hole formation process: (b1) A via hole was formed in the same manner as in the via hole forming step, except that the laminate (1) was replaced with the laminate (2).

[0365] (c2) Desmearing and roughening treatment: (c1) The steps of the desmear treatment and the roughening treatment were carried out in the same manner, except that the laminate (1) was replaced by the laminate (2), to obtain a laminate (2) after the roughening treatment.

[0366] (d2) Electroless plating process: (d1) An electroless plating treatment was performed in the same manner as in the electroless plating treatment, except that the roughening-treated laminate (1) was replaced with the roughening-treated laminate (2).

[0367] (f2) Electrolytic plating process: After (d2) electroless plating treatment was performed, electroless plating treatment was performed in the same manner as (f1) electrolytic plating treatment.

[0368] (h2) Main curing process: (h1) In the same manner as in the main curing step, the substrate was heated at 200°C for 1.5 hours.

[0369] In this manner, a second insulation-wiring circuit composite layer was formed on the first insulation-wiring circuit composite layer.

[0370] Formation of the third insulation-wiring circuit composite layer: A third insulation-wiring circuit composite layer was formed on the second insulation-wiring circuit composite layer in the same manner as in the process performed in forming the second insulation-wiring circuit composite layer.

[0371] Formation of the fourth insulation-wiring circuit composite layer: A fourth insulation-wiring circuit composite layer was formed on the third insulation-wiring circuit composite layer in the same manner as in the process performed in forming the second insulation-wiring circuit composite layer.

[0372] Formation of the fifth insulation-wiring circuit composite layer: (a5) Lamination process: (a2) A laminate (5) was obtained in which a semi-cured resin film was laminated on the fourth insulation-wiring circuit composite layer in the same manner as in the lamination step.

[0373] (b5) Via hole formation process: (b1) A via hole was formed in the same manner as in the via hole forming step, except that the laminate (1) was replaced with the laminate (5).

[0374] (c5) Desmearing and roughening treatment: (c1) The steps of the desmear treatment and the roughening treatment were carried out in the same manner, except that the laminate (1) was replaced with the laminate (5), to obtain a laminate (5) after the roughening treatment.

[0375] (d5) Electroless plating process: (d1) An electroless plating treatment was performed in the same manner as in the electroless plating treatment, except that the roughening-treated laminate (1) was replaced with the roughening-treated laminate (5).

[0376] (e5) Resist formation: (e1) Development was carried out in the same manner as in the resist formation.

[0377] (f5) Electrolytic plating process: After the dry film resist pattern was formed, an electroless plating process was carried out in the same manner as in (f1) electrolytic plating process.

[0378] (g5) DFR stripping and etching process: (g1) DFR stripping and etching treatment was carried out in the same manner as in the DFR stripping and etching treatment.

[0379] (h5) Main curing process: (h1) In the same manner as in the main curing step, the substrate was heated at 200°C for 1.5 hours.

[0380] In this manner, a fifth insulation-wiring circuit composite layer was formed on the fourth insulation-wiring circuit composite layer.

[0381] Formation of the sixth insulation-wiring circuit composite layer: A sixth insulation-wiring circuit composite layer was formed on the fifth insulation-wiring circuit composite layer in the same manner as in the process performed in forming the second insulation-wiring circuit composite layer.

[0382] In this way, an evaluation board was produced in which the first to sixth insulation-wiring circuit composite layers were formed on the copper-clad laminate. In the obtained evaluation board, of the first to sixth wiring circuit layers, only the first and fifth wiring circuit layers had patterns.

[0383] Thermal shock test (cracks or cracks in the insulation layer) evaluation: The obtained evaluation board was subjected to a liquid bath thermal shock test under the following two conditions.

[0384] Test condition 1: -55℃~125℃, 5 minutes each, 1000 cycles Test condition 2: -65℃~150℃, 5 minutes each, 1000 cycles

[0385] (6-1) Cracks or cracks in the insulation layer and wiring circuit layer For the evaluation board that underwent the liquid bath thermal shock test, the insulating layer around the via holes and the wiring circuit layer in the vias were observed using a scanning electron microscope (SEM).The insulating layer and wiring circuit layer in areas other than the via holes were also observed.

[0386] [Criteria for cracks or breaks in the insulation layer and wiring circuit layer (around via holes)] ○: No cracks or breaks were observed in the insulating layer around the via hole and in the wiring circuit layer of the via hole. ×: Cracks or breaks are observed in the insulating layer around the via hole or in the wiring circuit layer of the via hole.

[0387] [Criteria for cracks or breaks in the insulation layer and wiring circuit layer (other than around via holes)] ○: No cracks or breaks were observed in the insulating layer and wiring circuit layer in the area other than the area around the via hole. ×: Cracks or breaks are observed in the insulating layer or wiring circuit layer in the area other than the area around the via hole.

[0388] (6-2) Connection reliability (resistance change rate) Before and after the liquid bath thermal shock test, the resistance of the via connection was measured using a resistance meter ("RM3545" manufactured by HIOKI E.E.C. Co., Ltd.) The resistance change rate of the evaluation board (resistance value after liquid bath thermal shock test / resistance value after liquid bath thermal shock test x 100) was calculated before and after the liquid bath thermal shock test.

[0389] [Connection reliability criteria] ○: Resistance change rate is less than 10% ×: Resistance change rate is 10% or more

[0390] (7) Side lobe Lamination and semi-curing process: The obtained resin film was vacuum laminated onto a CCL substrate ("E679FG" manufactured by Hitachi Chemical Co., Ltd.) and semi-cured by heating at 180°C for 30 minutes. In this way, a laminate A in which a semi-cured resin film was laminated onto a CCL substrate was obtained.

[0391] Via formation: A via (through hole) having a diameter of 60 μm at the top and 40 μm at the bottom (bottom) was formed using a CO2 laser (manufactured by Hitachi Via Mechanics) in the semi-cured resin film of the obtained laminate A. In this way, a laminate B was obtained in which a semi-cured resin film was laminated on a CCL substrate and a via (through hole) was formed in the semi-cured resin film.

[0392] Via Bottom Residue Removal Treatment: (a) Swelling treatment The obtained laminate B was placed in a swelling liquid ("Swelling Dip Securigant P" manufactured by Atotech Japan) at 60° C. and was shaken for 10 minutes, after which it was washed with pure water.

[0393] (b) Permanganate treatment (roughening and desmearing) The laminate B after the swelling treatment was placed in a roughening aqueous solution of potassium permanganate ("Concentrate Compact CP" manufactured by Atotech Japan) at 80° C. and swung for 30 minutes. Next, it was treated for 2 minutes using a cleaning solution ("Reduction Securigant P" manufactured by Atotech Japan) at 25° C., and then washed with pure water to obtain an evaluation sample.

[0394] The periphery of the via of the evaluation sample was observed with a scanning electron microscope (SEM), and the side lobe length around the via was measured.

[0395] [Side lobe criteria] ○○: Maximum side lobe length is less than 15 μm ○: Maximum side lobe length is 15 μm or more and less than 30 μm ×: Maximum side lobe length is 30 μm or more

[0396] The compositions and results are shown in Tables 1 and 2 below.

[0397] [Table 1]

[0398] [Table 2] [Explanation of symbols]

[0399] 11...Multilayer printed wiring board 12...Circuit board 12a…Top surface 13~16…Insulating layer 17...Metal layer

Claims

1. a cyclohexane ring-containing compound which is a maleimide compound having a cyclohexane ring; a thermosetting compound different from the cyclohexane ring-containing compound; A hardener; and a curing accelerator; the cyclohexane ring-containing compound has a first skeleton derived from an aliphatic diamine compound having a cyclohexane ring, the aliphatic diamine compound having a cyclohexane ring is different from a dimer diamine, the cyclohexane ring-containing compound does not have or has a second skeleton derived from a dimer diamine, an average ratio of a first skeleton derived from an aliphatic diamine compound having a cyclohexane ring to a total structural unit (100 mol %) derived from a diamine compound in the cyclohexane ring-containing compound is 50 mol % or more; when the cyclohexane ring-containing compound has a second skeleton derived from the dimer diamine, an average ratio of the second skeleton derived from the dimer diamine to the total structural units (100 mol %) of the skeleton derived from the diamine compound contained in the cyclohexane ring-containing compound is 15 mol % or less, The resin material, wherein the thermosetting compound includes an epoxy compound.

2. The resin material according to claim 1 , wherein the cyclohexane ring-containing compound does not have a second skeleton derived from the dimer diamine.

3. 3. The resin material according to claim 1, wherein an average ratio of a first skeleton derived from an aliphatic diamine compound having a cyclohexane ring is 100 mol % in 100 mol % of all structural units of a skeleton derived from a diamine compound contained in the cyclohexane ring-containing compound.

4. 3. The resin material according to claim 1, wherein the cyclohexane ring-containing compound has a third skeleton derived from a diamine compound different from an aliphatic diamine compound having a cyclohexane ring, and the diamine compound different from the aliphatic diamine compound having a cyclohexane ring is different from a dimer diamine.

5. The resin material according to claim 4 , wherein the third skeleton derived from a diamine compound different from the aliphatic diamine compound having a cyclohexane ring has an aromatic ring.

6. The resin material according to claim 4 or 5, wherein the third skeleton derived from the diamine compound different from the aliphatic diamine compound having a cyclohexane ring has a fluorine atom.

7. 7. The resin material according to claim 1, wherein in the first skeleton derived from the aliphatic diamine compound having a cyclohexane ring, a nitrogen atom constituting a first amino group and a carbon atom constituting a cyclohexane ring are bonded directly or via two or less atoms.

8. 8. The resin material according to claim 7, wherein in the first skeleton derived from the aliphatic diamine compound having a cyclohexane ring, a nitrogen atom constituting a second amino group different from the first amino group is directly bonded to a carbon atom constituting the cyclohexane ring or is bonded to a carbon atom constituting the cyclohexane ring via three or less atoms.

9. The resin material according to any one of claims 1 to 8, wherein the aliphatic diamine compound having a cyclohexane ring is tricyclodecane diamine, norbornane diamine, or isophorone diamine.

10. The resin material according to any one of claims 1 to 9, wherein the cyclohexane ring-containing compound has a glass transition temperature of 100°C or higher and 300°C or lower.

11. The resin material according to any one of claims 1 to 10, wherein the weight average molecular weight of the cyclohexane ring-containing compound is 2,000 or more and 100,000 or less.

12. A resin material described in any one of claims 1 to 11, wherein the thermosetting compound includes a maleimide compound.

13. The resin material described in claim 12, wherein the maleimide compound, which is the thermosetting compound, has a skeleton derived from dimer diamine.

14. the maleimide compound having a cyclohexane ring does not have a second skeleton derived from the dimer diamine, The resin material according to claim 12 or 13, wherein the maleimide compound which is the thermosetting compound has a skeleton derived from a dimer diamine.

15. The resin material according to any one of claims 1 to 14, wherein the curing agent comprises an active ester compound.

16. The resin material according to any one of claims 1 to 15, wherein the thermosetting compound comprises a radically curable compound.

17. The resin material according to any one of claims 1 to 16, further comprising an inorganic filler.

18. The resin material according to claim 17, wherein the content of the inorganic filler is 50% by weight or more based on 100% by weight of components excluding the solvent in the resin material.

19. The resin material according to claim 17 or 18, wherein the inorganic filler is silica.

20. The resin material according to any one of claims 1 to 19, which is a resin film.

21. The resin material according to any one of claims 1 to 20, which is used to form an insulating layer in a multilayer printed wiring board.

22. A circuit board; a plurality of insulating layers disposed on a surface of the circuit board; a metal layer disposed between a plurality of the insulating layers; A multilayer printed wiring board, wherein at least one of the insulating layers is a cured product of the resin material according to any one of claims 1 to 21.

Citation Information

Patent Citations

  • Polyimide precursor, polyimide precursor composition, polyimide resin and electronic part

    JP2004043827A

  • Resin for optical-semiconductor-element encapsulation containing polyimide and optical semiconductor device obtained with the same

    JP2009114415A

  • Thermosetting resin composition, its cured product, and interlayer adhesive film for print wiring board

    JP2012041382A

  • Epoxy resin composition

    JP2013234328A

  • Resin composition for electronic material

    JP2018090728A