Modified polyphenylene ether, its production method, prepreg and laminate
A modified polyphenylene ether with controlled molecular weight and impurity content addresses the heat and dielectric property challenges of conventional polyphenylene ethers, enhancing substrate materials for high-frequency applications by maintaining excellent dielectric properties post-curing.
Patent Information
- Application Number
- JP2020188249
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-11
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2040-11-11
AI Technical Summary
Conventional polyphenylene ethers used as substrate materials lack sufficient heat resistance and dielectric properties, particularly when used in high-frequency applications, and require additional components like thermosetting resins to enhance these properties, which can lead to deterioration of dielectric properties.
A modified polyphenylene ether with specific molecular structure and composition, characterized by a high glass transition temperature, low impurity content, and controlled molecular weight, is produced through a reaction with unsaturated compounds in the presence of catalysts, resulting in a thermosetting composition suitable for high-frequency applications.
The modified polyphenylene ether composition exhibits improved heat resistance and dielectric properties, reducing the need for crosslinking initiators and maintaining excellent dielectric properties post-curing, suitable for electronic materials and substrates.
Smart Images

Figure 0007563948000001 
Figure 0007563948000002 
Figure 0007563948000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a modified polyphenylene ether, a method for producing the modified polyphenylene ether, a prepreg, and a laminate. [Background technology]
[0002] Polyphenylene ether (hereinafter, also referred to as "PPE") has excellent high-frequency characteristics, flame retardancy, and heat resistance, and is therefore widely used as a material in the fields of electrical and electronics, automobiles, and various other industrial materials. In recent years, it has been expected that polyphenylene ethers exhibiting an extremely low molecular weight are more effective for electronic material applications such as substrate materials than ordinary high-molecular-weight polyphenylene ethers. For this reason, Patent Document 1 proposes a low-molecular-weight polyphenylene ether that uses 2,6-dimethylphenol as a raw material and has a lower dielectric constant than ordinary high-molecular-weight polyphenylene ethers, and an efficient method for producing the same.
[0003] On the other hand, when polyphenylene ether is used as a molding material for substrate materials, etc., it is required to have not only excellent dielectric properties but also excellent heat resistance and moldability. However, conventional polyphenylene ether is thermoplastic, and there are cases where sufficient heat resistance cannot be obtained. For this reason, it has been proposed to use polyphenylene ether to which a thermosetting resin such as an epoxy resin has been added, or to use a modified polyphenylene ether.
[0004] Patent Document 2 describes a modified polyphenylene ether compound having a specific polyphenylene ether moiety in its molecular structure and having at least one p-ethenylbenzyl group, m-ethenylbenzyl group, or the like at the molecular end. Furthermore, Patent Document 3 describes a modified polymer having a polyphenylene ether portion in its molecular structure and having a methacryl group at the molecular end.
[0005] In order to easily ensure the heat resistance of the terminal-modified thermosetting polyphenylene ether, such as the compounds disclosed in Patent Document 2 and Patent Document 3, a method of increasing the crosslink density between the thermosetting polyphenylene ether and the thermosetting crosslinking agent is effective. Therefore, a multifunctional polyphenylene ether having multiple terminals in one molecule is required. For this reason, low molecular weight multifunctional polyphenylene ethers obtained by polymerization in the presence of a multifunctional phenol compound have been proposed in Patent Documents 4, 5, and 6. Since these multifunctional polyphenylene ethers have a branched structure, they have a lower solution viscosity than linear polymers at the same molecular weight, and have higher fluidity than linear polymers at the same molecular weight, so that a polymer with a relatively high molecular weight can be used in the curing process, and the physical properties of the cured product can be improved. In addition, since the number of crosslinking reaction points increases, it is expected that in addition to contributing to the improvement of the above physical properties, it is also easier to control the crosslinking reaction. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2004-99824 A [Patent Document 2] JP 2004-339328 A [Patent Document 3] Patent No. 5147397 [Patent Document 4] U.S. Patent No. 9,012,572 [Patent Document 5] Patent No. 5176336 [Patent Document 6] Patent No. 5439700 Summary of the Invention [Problem to be solved by the invention]
[0007] In general, a thermosetting composition for a high frequency compatible substrate is obtained by impregnating a support material such as a glass cloth with a varnish in which a low dielectric polymer material such as modified polyphenylene ether, a thermosetting crosslinking agent, a crosslinking initiator, etc. are dissolved, and then thermally curing the varnish. If a modified polyphenylene ether composition capable of exhibiting a high glass transition temperature after curing is used as a raw material, the addition rate of a crosslinking initiator, etc. that causes deterioration of the dielectric properties can be reduced, resulting in a substrate material with better dielectric properties.
[0008] The present invention has been made in view of the above problems, and an object of the present invention is to provide a modified polyphenylene ether that has a high glass transition temperature after curing. [Means for solving the problem]
[0009] That is, the present invention is as follows. [1] A modified polyphenylene ether represented by the following formula (1): The number average molecular weight in terms of polystyrene is 500 to 15,000. The content of methacrylic acid is based on the total amount of the modified polyphenylene ether. More than 70 ppm Less than 200 ppm, total content of methacrylic anhydride and vinyl methacrylate 10 ppm or more Less than 200 ppm, organic amine catalyst content More than 40 ppm Less than 200 ppm and chloride ion content 10 ppm or more The modified polyphenylene ether is characterized in that the content of the phenylene oxide is less than 1500 ppm. [ka] ...Equation (1) In formula (1), Z is an a-valent partial structure represented by formula (2) below, a represents an integer of 2 to 6, each Y is independently a divalent linking group having a structure represented by formula (4) below, n represents the number of repetitions of Y and each n is independently an integer of 0 to 200, at least one n among the a (-Yn-A) is an integer of 1 or more, and A is a group represented by formula (5) below. [ka] ...Equation (2) In formula (2), X is an arbitrary linking group having a valence of a, and R 4 is either a linear alkyl group having 1 to 8 carbon atoms or a partial structure represented by the following formula (3), in which the carbon atom of the benzene ring to which -O- is bonded is the 1st position and it is bonded to at least one of the 2nd and 6th carbon atoms, and each k is independently an integer of 1 to 4. [ka] ...Equation (3) In formula (3), R 11 each independently represents an optionally substituted alkyl group having 1 to 8 carbon atoms; R 12 each independently represents an optionally substituted alkylene group having 1 to 8 carbon atoms; each b independently represents 0 or 1; R 13 is any one of a hydrogen atom, an optionally substituted alkyl group having 1 to 8 carbon atoms, and an optionally substituted phenyl group. [ka] ...Equation (4) In formula (4), R 21 each independently represents any one of an optionally substituted hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, and a halogen atom. [ka] ...Equation (5) In the above formula (5), R 31 each independently represents a hydrogen atom, a hydroxyl group, a hydrocarbon group having 1 to 30 carbon atoms (e.g., a linear hydrocarbon group, a cyclic hydrocarbon group), an aryl group, an alkoxy group, an aryloxy group, an amino group, or a hydroxyalkyl group; R 32 are each independently a hydrocarbon group having 1 to 30 carbon atoms (for example, an alkylene group), and s is an integer of 0 to 5. [2] A method for producing a modified polyphenylene ether, comprising a step of reacting an unmodified polyphenylene ether represented by the following formula (8) with an unsaturated compound represented by the following formula (10): [ka] ...Equation (8) In formula (8), Z is an a-valent partial structure represented by formula (2) below, a represents an integer of 2 to 6, each Y is independently a divalent linking group having a structure represented by formula (4) below, n represents the number of repetitions of Y, each n is independently an integer of 0 to 200, and at least one n among the a (-Yn-A) is an integer of 1 or more. [ka] ...Equation (2) In formula (2), X is an arbitrary linking group having a valence of a, and R 4 is either a linear alkyl group having 1 to 8 carbon atoms or a partial structure represented by the following formula (3), in which the carbon atom of the benzene ring to which -O- is bonded is the 1st position and it is bonded to at least one of the 2nd and 6th carbon atoms, and each k is independently an integer of 1 to 4. [ka] ...Equation (3) In formula (3), R 11 each independently represents an optionally substituted alkyl group having 1 to 8 carbon atoms; R 12 each independently represents an optionally substituted alkylene group having 1 to 8 carbon atoms; each b independently represents 0 or 1; R 13 is any one of a hydrogen atom, an optionally substituted alkyl group having 1 to 8 carbon atoms, and an optionally substituted phenyl group. [ka] ...Equation (4) In formula (4), R 21 each independently represents any one of an optionally substituted hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, and a halogen atom. [ka] ...Equation (10) In the above formula (10), R 31 each independently represents a hydrogen atom, a hydroxyl group, a hydrocarbon group having 1 to 30 carbon atoms (e.g., a linear hydrocarbon group, a cyclic hydrocarbon group), an aryl group, an alkoxy group, an aryloxy group, an amino group, or a hydroxyalkyl group; R 32 are each independently a hydrocarbon group having 1 to 30 carbon atoms (for example, an alkylene group), and s is an integer of 0 to 5. [3] The method according to [2], wherein the reaction of the unmodified polyphenylene ether represented by the formula (8) with the unsaturated compound represented by the formula (10) is carried out in the presence of an organic amine catalyst or a Lewis acid catalyst. [4] The method according to [3], wherein the reaction of the unmodified polyphenylene ether represented by the formula (8) with the unsaturated compound represented by the formula (10) is carried out in the presence of the organic amine catalyst, and the organic amine catalyst is dimethylaminopyridine. [5] A thermosetting composition comprising the modified polyphenylene ether according to claim 1. [6] A prepreg comprising a substrate and the thermosetting composition according to claim 5. [7] 7. The prepreg according to claim 6, wherein the substrate is a glass cloth. [8] 8. A laminate comprising the cured prepreg according to claim 6 or 7 and a metal foil. Effect of the Invention
[0010] According to the present invention, it is possible to provide a modified polyphenylene ether having a high glass transition temperature after curing, and a thermosetting composition containing the modified polyphenylene ether. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, an embodiment for carrying out the present invention (hereinafter, referred to as "the present embodiment") will be described in detail. The following embodiment is an example for explaining the present invention, and the present invention is not limited to only this embodiment, and the present invention can be carried out by appropriately modifying it within the scope of the gist of the present invention. In this specification, A (numeric value) to B (numeric value) means A or more and B or less.
[0012] <Modified polyphenylene ether> The modified polyphenylene ether of the present embodiment is represented by the following formula (1), and based on the total amount of the modified polyphenylene ether, the content of methacrylic acid is less than 200 ppm, the total content of methacrylic anhydride and vinyl methacrylate is less than 200 ppm, the content of organic amine catalyst is less than 200 ppm, and the content of chloride ions is less than 1500 ppm, and the number average molecular weight in terms of polystyrene is 500 to 15,000. [ka] ...Equation (1) In formula (1), Z is an a-valent partial structure represented by formula (2) below, a represents an integer of 2 to 6, each Y is independently a divalent linking group having a structure represented by formula (4) below, n represents the number of repetitions of Y, each n is independently an integer of 0 to 200, and at least one n among the a (-Yn-A) is an integer of 1 or more. [ka] ...Equation (2) In formula (2), X is an arbitrary linking group having a valence of a, and R 4 is either a linear alkyl group having 1 to 8 carbon atoms or a partial structure represented by the following formula (3), in which the carbon atom of the benzene ring to which -O- is bonded is the 1st position and it is bonded to at least one of the 2nd and 6th carbon atoms, and each k is independently an integer of 1 to 4. [ka] ...Equation (3) In formula (3), R 11each independently represents an optionally substituted alkyl group having 1 to 8 carbon atoms; R 12 each independently represents an optionally substituted alkylene group having 1 to 8 carbon atoms; each b independently represents 0 or 1; R 13 is any one of a hydrogen atom, an optionally substituted alkyl group having 1 to 8 carbon atoms, and an optionally substituted phenyl group. [ka] ...Equation (4) In formula (4), R 21 each independently represents any one of an optionally substituted hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, and a halogen atom. [ka] ...Equation (5) In formula (5), R 31 each independently represents a hydrogen atom, a hydroxyl group, a hydrocarbon group having 1 to 30 carbon atoms (e.g., a linear hydrocarbon group, a cyclic hydrocarbon group), an aryl group, an alkoxy group, an aryloxy group, an amino group, or a hydroxyalkyl group; R 32 are each independently a hydrocarbon group having 1 to 30 carbon atoms (e.g., an alkylene group), and s is an integer of 0 to 5.
[0013] In this embodiment, the above Z (partial structure represented by formula (2)) is also called the central phenol moiety, and means the central skeleton that is the starting point of the reaction when polymerizing the multifunctional unmodified polyphenylene ether that is the raw material of the modified polyphenylene ether of this embodiment, and its structure can be identified by analyzing the modified polyphenylene ether by techniques such as NMR, mass spectrometry, and pyrolysis GC-MS. As a specific method for identifying the structure of the central phenol moiety from the modified polyphenylene ether, it is possible to carry out field desorption mass spectrometry (FD-MS), which is known to be less likely to cause fragmentation, and to estimate the repeating unit based on the interval between the detected ions. Furthermore, there is a method of estimating the structure of the central phenol moiety by combining peak analysis of fragment ions by electron ionization (EI) and structural analysis by NMR.
[0014] As described above, the modified polyphenylene ether has a number of partial structures (R 4 and the like) is bonded, and (-Yn-A) in formula (1) is bonded to an a-valent partial structure (i.e., Z represented by formula (2)). [ka] ...Equation (2) In formula (2), a is the same integer as a in formula (1). In the central phenol moiety represented by formula (2), each of the a partial structures may be the same structure or different structures. In particular, from the viewpoint of obtaining a modified polyphenylene ether having better solubility in a solvent and a higher glass transition temperature after curing, each of the a partial structures is preferably the same structure. The a -O- termini in formula (2) may be directly bonded to Y in formula (1).
[0015] In formula (2), X is any a-valent linking group, and is not particularly limited, and examples thereof include hydrocarbon groups such as chain hydrocarbons and cyclic hydrocarbons; hydrocarbon groups containing one or more atoms selected from nitrogen, phosphorus, silicon, and oxygen; atoms such as nitrogen, phosphorus, and silicon; or groups combining these; etc. X may be a linking group other than a single bond. X may be a linking group that links a-valent partial structures to each other. The above X is R 4 R is bonded to a benzene ring via an a-valent alkyl skeleton, a single bond, an ester bond, etc. 4 R is bonded to a benzene ring via an a-valent aryl skeleton, a single bond, an ester bond, or the like. 4 and an a-valent heterocyclic skeleton bonded to a benzene ring to which is bonded. Here, the alkyl skeleton is not particularly limited, but examples thereof include a skeleton in which the branched ends of a chain hydrocarbon (e.g., a chain saturated hydrocarbon) having 2 to 6 carbon atoms and branched to at least a units are directly bonded to a benzene ring in a partial structure (as long as a benzene ring is bonded to the a units of branched ends, there may be a branched end to which no benzene ring is bonded). In addition, the aryl skeleton is not particularly limited, but examples thereof include a skeleton in which a benzene ring, a mesitylene group, or a 2-hydroxy-5-methyl-1,3-phenylene group is bonded to R 4 Furthermore, the heterocyclic skeleton is not particularly limited, but examples thereof include a skeleton in which a triazine ring is bonded to a benzene ring to which R 4 and the like.
[0016] In formula (2), R 4 are each independently any one of a linear alkyl group having 1 to 8 carbon atoms, such as a methyl group, an ethyl group, and an n-propyl group, and a partial structure represented by the following formula (3), in which the carbon atom of the benzene ring to which -O- is bonded is the 1st position, and each k is independently an integer of 1 to 4. [ka] ...Equation (3) In the above formula (3), R 11 each independently represents an optionally substituted alkyl group having 1 to 8 carbon atoms; R 12 each independently represents an optionally substituted alkylene group having 1 to 8 carbon atoms; each b independently represents 0 or 1; R 13 is any one of a hydrogen atom, an optionally substituted alkyl group having 1 to 8 carbon atoms, and an optionally substituted phenyl group. 12 ) side end) may be directly bonded to a carbon atom of the benzene ring. The substituent includes, for example, a halogen atom.
[0017] The above formula (3) is preferably a group containing a secondary and / or tertiary carbon, such as an isopropyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a tert-amyl group, a 2,2-dimethylpropyl group, or a structure having a phenyl group at the terminal of any of these groups, and more preferably a tert-butyl group.
[0018] In the benzene ring of the above formula (2), when the carbon atom to which (Yn-A) in the above formula (1) is bonded via an oxygen atom is regarded as the 1st position, the central part X may be bonded to a carbon atom other than the 2nd and 6th positions, and it is preferable that the central part X is bonded to the 4th position.
[0019] Each Y is independently a divalent linking group having a structure of the following formula (4). [ka] ...Equation (4) In the above formula (4), R 21 each independently represents an optionally substituted hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom; R 21 is preferably a methyl group. The left end of formula (4) may be directly bonded to Z in formula (1) (for example, —O— in formula (2)), and the right end may be directly bonded to A.
[0020] In the above formula (1), A is a hydrogen atom or a group represented by the following formula (5), and is preferably a group represented by the following formula (5). [ka] ...Equation (5) In the above formula (5), R 31 are each independently any one of a hydrogen atom, a hydroxyl group, a hydrocarbon group having 1 to 30 carbon atoms (for example, a linear hydrocarbon group, a cyclic hydrocarbon group), an aryl group, an alkoxy group, an aryloxy group, an amino group, and a hydroxyalkyl group. R 32 are each independently a hydrocarbon group having 1 to 30 carbon atoms (for example, an alkylene group). s is an integer from 0 to 5. The left end in formula (5) may be directly bonded to Y in formula (1) (eg, the right end in formula (4)).
[0021] From the viewpoint of obtaining a modified polyphenylene ether having a higher glass transition temperature after curing and having better solubility in a solvent, the substituent represented by the above formula (5) is preferably a methacryloyl group.
[0022] R 31Specific examples of the hydrocarbon group include methyl, ethyl, n-propyl, 2-propyl, n-butyl, isobutyl, t-butyl, n-pentyl, 1-ethylpropyl, 1-methylbutyl, 2-methylbutyl, 3-methylbutyl, amyl, cyclopentyl, 2,2-dimethylpropyl, 1,1-dimethylpropyl, n-hexyl, cyclohexyl, 1-ethylbutyl, 2-ethylbutyl, 3-ethylbutyl, 1-methylpentyl, 2-methylpentyl, 3-methylpentylene, 4-methylpentylene, 1,1-dimethylbutylene, 2,2-dimethylbutylene, 3,3-dimethylbutyl, 1,2-dimethylbutyl, 1,3-dimethylbutyl, 2,3-dimethylbutyl, n-heptyl, 1-methylhexyl, 2-methylhexyl, 3-methylhexyl, 4-methylhexyl, 5-methylhexyl, 1-ethylpentyl, 2-ethylpentyl, 3-ethylpentyl, 1,1-dimethylpentyl, 2,2-dimethylpentyl, 3,3-dimethylpentyl, 4,4-dimethylpentyl, 1,2-dimethylpentyl, 1,3-dimethylpentyl, 1,4-dimethylpentyl, 2,3-dimethylpentyl, 2,4-dimethylpentyl butyl, 3,4-dimethylpentyl, 2-methyl-3,3-dimethylbutyl, 1-methyl-3,3-dimethylbutyl, 1,2,3-trimethylbutyl, 1,3-dimethyl-2-pentyl, 2-isopropylbutyl, 2-methylcyclohexyl, 3-methylcyclohexyl, 4-methylcyclohexyl, 1-cyclohexylmethyl, 2-ethylcyclopentyl, 3-ethylcyclopentyl, 2,3-dimethylcyclopentyl, 2,4-dimethylcyclopentyl, 2-methylcyclopentylmethyl, 2-cyclopentylethyl, 1-cyclopentylethyl, n-Octyl, 2-Octyl, 3-Octyl, 4-Octyl, 2-Methylheptyl, 3-Methylheptyl, 4-Methylheptyl, 5-Methylheptyl, 6-Methylheptyl, 2-Ethylhexyl, 3-Ethylhexyl, 4-Ethylhexyl, 5-Ethylhexyl, 1,1-Dimethylhexyl, 2,2-Dimethylhexyl, 3,3-Dimethylhexyl, 4,4-Dimethylhexyl, 5,5-Dimethylhexyl, 1,2-Dimethylhexyl, 1,3-Dimethylhexyl, 1,4-Dimethylhexyl, 1,5-Dimethylhexyl, 2,3-Dimethylhexyl,2,4-dimethylhexyl, 2,5-dimethylhexyl, 1,1-ethylmethylpentyl, 2,2-ethylmethylpentyl, 3,3-ethylmethylpentyl, 4,4-ethylmethylpentyl, 1-ethyl-2-methylpentyl, 1-ethyl-3-methylpentyl, 1-ethyl-4-methylpentyl, 2-ethyl-1-methylpentyl, 3-ethyl-1-methylpentyl, 4-ethyl-1-methylpentyl, 2-ethyl-3-methylpentyl, 2-ethyl-4-methylpentyl, 3-ethyl-2-methylpentyl, 4-ethyl-3-methylpentyl, 3-ethyl-4-methylpentyl, 4-ethyl-3-methylpentyl, 1-(2-methylpropyl)butyl, 1-(2-methylpropyl)-2-methylbutyl, 1,1-(2-methylpropyl)ethyl, 1,1-(2-methylpropyl)ethylpropionate pyryl, 1,1-diethylpropyl, 2,2-diethylpropyl, 1,1-ethylmethyl-2,2-dimethylpropyl, 2,2-ethylmethyl-1,1-dimethylpropyl, 2-ethyl-1,1-dimethylbutyl, 2,3-dimethylcyclohexyl, 2,3-dimethylcyclohexyl, 2,5-dimethylcyclohexyl, 2,6-dimethylcyclohexyl, 3,5-dimethylcyclohexyl, 2-methylcyclohexylmethyl, 3-methylcyclohexylmethyl, 4-methylcyclohexylmethyl, 2-ethylcyclohexyl, 3-ethylcyclohexyl, 4-ethylcyclohexyl, 2-cyclohexylethyl, 1-cyclohexylethyl, 1-cyclohexyl-2-ethylene, nonyl, isononyl, decyl, isodecyl, undecyl, dodecyl, benzyl, 2-phenylethyl, and the like. Preferably, methyl, ethyl, n-propyl, 2-propyl, n-butyl, isobutyl, t-butyl, n-pentyl, 1-ethylpropyl, 1-methylbutyl, 2-methylbutyl, 3-methylbutyl, amyl, cyclopentyl, n-hexyl, cyclohexyl, 1-ethylbutyl, 2-ethylbutyl, 3-ethylbutyl, 1-methylpentyl, 2-methylpentyl, 3-methylpentyl, 4-methylpentyl, n-heptyl, 1-methylhexyl, 2-methylhexyl, 3-methylhexyl, 4-methylhexyl, 5-methylhexyl, 1-ethylpentyl, 2-ethylpentyl, 3-ethylpentyl, 2-methylcyclohexyl,3-methylcyclohexyl, 4-methylcyclohexyl, n-octyl, 2-octyl, 3-octyl, 4-octyl, 2-methylheptyl, 3-methylheptyl, 4-methylheptyl, 5-methylheptyl, 6-methylheptyl, 2-ethylhexyl, 3-ethylhexyl, 4-ethylhexyl, 5-ethylhexyl, nonyl, isononyl, decyl, isodecyl, undecyl, dodecyl, and benzyl, and more preferably methyl, ethyl, n-propyl, 2-propyl, n-butyl, isobutyl, t-butyl, n-pentyl, 1-ethylpropyl, 1-methylbutyl, 2-methylbutyl, 3-methylbutyl, amyl, cyclopentyl, n-hexyl, cyclohexyl, n-heptyl, n-octyl, 2-octyl, 3-octyl, 4-octyl, 2-methylheptyl, and 3-methylheptyl. , 4-methylheptyl, 5-methylheptyl, 6-methylheptyl, 2-ethylhexyl, 3-ethylhexyl, 4-ethylhexyl, 5-ethylhexyl, nonyl, isononyl, decyl, isodecyl, undecyl, dodecyl, and benzyl, and more preferably methyl, ethyl, n-propyl, 2-propyl, n-butyl, isobutyl, t-butyl, n-pentyl, amyl, cyclopentyl, n-hexyl, cyclohexyl, n-heptyl, n-octyl, 2-octyl, 3-octyl, 4-octyl, 2-methylheptyl, 3-methylheptyl, 4-methylheptyl, 5-methylheptyl, 6-methylheptyl, 2-ethylhexyl, 3-ethylhexyl, 4-ethylhexyl, 5-ethylhexyl, nonyl, isononyl, decyl, isodecyl, undecyl, dodecyl, and benzyl. ,
[0023] R 32Specific examples of the hydrocarbon group include methylene, ethylene, trimethylene, 1,2-propylene, tetramethylene, 2-methyl-1,3-trimethylene, 1,1-dimethylethylene, pentamethylene, 1-ethyl-1,3-propylene, 1-methyl-1,4-butylene, 2-methyl-1,4-butylene, 3-methyl-1,4-butylene, 2,2-dimethyl-1,3-propylene, 1,2-cyclopentylene, 1,3-cyclopentylene, 2,2-dimethyl-1,3-propylene, 1,1-dimethyl-1,3-propylene, and 3,3-dimethyl-1,3-propylene. Propylene, hexamethylene, 1,2-cyclohexylene, 1,3-cyclohexylene, 1,4-cyclohexylene, 1-ethyl-1,4-butylene, 2-ethyl-1,4-butylene, 3-ethyl-1,4-butylene, 1-methyl-1,5-pentylene, 2-methyl-1,5-pentylene, 3-methyl-1,5-pentylene, 4-methylpentylene, 1,1-dimethyl-1,4-butylene, 2,2-dimethyl-1,4-butylene, 3,3-dimethyl-1,4-butylene, 1,2-dimethyl-1,4-butylene, 1,3-dimethyl-1,4-butylene, 2 ,3-Dimethyl-1,4-butylene, heptamethylene, 1-methyl-1,6-hexylene, 2-methyl-1,6-hexylene, 3-methyl-1,6-hexylene, 4-methyl-1,6-hexylene, 5-methyl-1,6-hexylene, 1-ethyl-1,5-pentylene, 2-ethyl-1,5-pentylene, 3-ethyl-1,5-pentylene, 1,1-dimethyl-1,5-pentylene, 2,2-dimethyl-1,5-pentylene, 3,3-dimethyl-1,5-pentylene, 4,4-dimethyl-1,5-pentylene, 1,2-dimethyl-1,5-pentylene , 1,3-dimethyl-1,5-pentylene, 1,4-dimethyl-1,5-pentylene, 2,3-dimethyl-1,5-pentylene, 2,4-dimethyl-1,5-pentylene, 3,4-dimethyl-1,5-pentylene, 2-methyl-3,3-dimethyl-1,4-butylene, 1-methyl-3,3-dimethyl-1,4-butylene, 1,2,3-trimethyl-1,4-butylene, 1,3-dimethyl-1,4-pentylene, 2-isopropyl-1,4-butylene, 2-methyl-1,4-cyclohexylene, 3-methyl-1,4-cyclohexylene, 4-methyl-1,4-cyclohexylene, 1-cyclohexylmethylene, 2-ethyl-1,3-cyclopentylene, 3-ethyl-1,3-cyclopentylene, 2,3-dimethyl-1,3-cyclopentylene, 2,4-dimethyl-1,3-cyclopentylene, 2-methyl-1,3-cyclopentylmethylene, 2-cyclopentylethylene, 1-cyclopentylethylene, octamethylene, 1-methyl-1,7-heptylene, 1-ethyl-1,6-hexylene, 1-propyl-1,5-pentylene, 2-methyl-1,7-heptylene, 3-methyl-1,7-heptylene, 4- Methyl-1,7-heptylene, 5-methyl-1,7-heptylene, 6-methyl-1,7-heptylene, 2-ethyl-1,6-hexylene, 3-ethyl-1,6-hexylene, 4-ethyl-1,6-hexylene, 5-ethyl-1,6-hexylene, 1,1-dimethyl-1,6-hexylene, 2,2-dimethyl-1,6-hexylene, 3,3-dimethyl-1,6-hexylene, 4,4-dimethyl-1,6-hexylene, 5,5-dimethyl-1,6-hexylene, 1,2-dimethyl-1,6-hexylene, 1,3-dimethyl-1,6-hexylene, 1,4- Dimethyl-1,6-hexylene, 1,5-dimethyl-1,6-hexylene, 2,3-dimethyl-1,6-hexylene, 2,4-dimethyl-1,6-hexylene, 2,5-dimethyl-1,6-hexylene, 1,1-ethylmethyl-1,5-pentylene, 2,2-ethylmethyl-1,5-pentylene, 3,3-ethylmethyl-1,5-pentylene, 4,4-ethylmethyl-1,5-pentylene, 1-ethyl-2-methyl-1,5-pentylene, 1-ethyl-3-methyl-1,5-pentylene, 1-ethyl-4-methyl-1,5-pentylene, 2-ethyl -1-methyl-1,5-pentylene, 3-ethyl-1-methyl-1,5-pentylene, 4-ethyl-1-methyl-1,5-pentylene, 2-ethyl-3-methyl-1,5-pentylene, 2-ethyl-4-methyl-1,5-pentylene, 3-ethyl-2-methyl-1,5-pentylene, 4-ethyl-3-methyl-1,5-pentylene, 3-ethyl-4-methyl-1,5-pentylene, 4-ethyl-3-methyl-1,5-pentylene, 1-(2-methylpropyl)-1,4-butylene, 1-(2-methylpropyl)-2-methyl-1,4-butylene, 1,1-(2-methylpropyl)ethylene, 1,1-(2-methylpropyl)ethyl-1,3-propylene, 1,1-diethyl-1,3-propylene, 2,2-diethyl-1,3-propylene, 1,1-ethylmethyl-2,2-dimethyl-1,3-propylene, 2,2-ethylmethyl-1,1-dimethyl-1,3-propylene, 2-ethyl-1,1-dimethyl-1,4-butylene, 2,3-dimethyl-1,4-cyclohexylene, 2,3-dimethyl-1,4-cyclohexylene, 2,5-dimethyl-1,4-cyclohexylene, 2,6-dimethyl-1,4-cyclohexylene, 3,5-dimethyl-1,4-cyclohexylene, 2-methyl-1,4-cyclohexyl-1- Examples of the alkyl group include methylene, 3-methyl-1,4-cyclohexyl-1-methylene, 4-methyl-1,4-cyclohexyl-1-methylene, 2-ethyl-1,4-cyclohexylene, 3-ethyl-1,4-cyclohexylene, 4-ethyl-1,4-cyclohexylene, 2-cyclohexylethylene, 1-cyclohexylethylene, 1-cyclohexyl-2-ethylene, nonylmethylene, 1-methyl-1,8-octylene, decylmethylene, 1-methyl-1,8-nonylene, undecylmethylene, dodecylmethylene, 1,4-phenylene, 1,3-phenylene, 1,2-phenylene, methylene-1,4-phenylene-methylene, and ethylene-1,4-phenylene-ethylene. Preferred are methylene, ethylene, trimethylene, 1,2-propylene, tetramethylene, 2-methyl-1,2-propylene, 1,1-dimethylethylene, pentamethylene, 1-ethyl-1,3-propylene, 1-methyl-1,4-butylene, 2-methyl-1,4-butylene, 3-methyl-1,4-butylene, 2,2-dimethyl-1,3-propylene, 1,3-cyclopentylene, 1,6-hexamethylene, 1,4-cyclohexylene, 1-ethyl -1,4-butylene, 2-ethyl-1,4-butylene, 3-ethyl-1,4-butylene, 1-methyl-1,5-pentylene, 2-methyl-1,5-pentylene, 3-methyl-1,5-pentylene, 4-methyl-1,5-pentylene, heptamethylene, 1-methyl-1,6-hexylene, 2-methyl-1,6-hexylene, 3-methyl-1,6-hexylene, 4-methyl-1,6-hexylene, 5-methyl-1,6-hexylene, 1-ethyl-1,5-pentylene, 2-ethyl-1,5-pentylene, 3-ethyl-1,5-pentylene, 2-methyl-1,4-cyclohexylene, 3-methyl-1,4-cyclohexylene, 4-methyl-1,4-cyclohexylene, octamethylene, 1-methyl-1,7-heptylene, 3-methyl-1,7-heptylene, 4-methyl-1,7-heptylene, 2-methyl-1,7-heptylene, 5-methyl-1,7-heptylene, 6-methyl-1,7-heptylene, 2-ethyl-1,6-hexylene, 3-ethyl-1,6-hexylene, 4-ethyl-1,6-hexylene 1,3-cyclopentylene, 1,6-hexylene, 5-ethyl-1,6-hexylene, nonylmethylene, decylmethylene, undecylmethylene, and dodecylmethylene, and more preferably methylene, ethylene, trimethylene, 1,2-propylene, tetramethylene, 2-methyl-1,2-propylene, 1,1-dimethylethylene, pentamethylene, 1-ethyl-1,3-propylene, 1-methyl-1,4-butylene, 2-methyl-1,4-butylene, 3-methyl-1,4-butylene, 2,2-dimethyl-1,3-propylene, 1,3-cyclopentylene, 1,6-hexamethylene, and 1,4-cyclopentylene. Preferred are diethyl ether, heptamethylene, octamethylene, 1-methyl-1,7-heptylene, 3-methyl-1,7-heptylene, 4-methyl-1,7-heptylene, 2-methyl-1,7-heptylene, 5-methyl-1,7-heptylene, 6-methyl-1,7-heptylene, 2-ethyl-1,6-hexylene, 3-ethyl-1,6-hexylene, 4-ethyl-1,6-hexylene, 5-ethyl-1,6-hexylene, nonylmethylene, decylmethylene, undecylmethylene, and dodecylmethylene. More preferred are methylene, ethylene, trimethylene, and 1 ,2-propylene, tetramethylene, 2-methyl-1,2-propylene, 1,1-dimethylethylene, pentamethylene, 2,2-dimethyl-1,3-propylene, 1,3-cyclopentylene, 1,6-hexamethylene, 1,4-cyclohexylene, heptamethylene, octamethylene, 1-methyl-1,7-heptylene, 3-methyl-1,7-heptylene, 4-methyl-1,7-heptylene, 2-methyl-1,7-heptylene, 5-methyl-1,7-heptylene, 6-methyl-1,7-heptylene, 2-ethyl-1,6-hexylene, 3-ethyl-1,6-hexylene, 4-ethyl-1,6-hexylene, 5-ethyl-1,6-hexylene, nonylmethylene, decylmethylene, undecylmethylene, and dodecylmethylene.
[0024] The modified polyphenylene ether of the present embodiment may contain a polyphenylene ether in which one or more A's are hydrogen atoms in the structure of the above formula (1). However, from the viewpoint of obtaining a high glass transition temperature in the thermosetting composition, it is more preferable that the modified polyphenylene ether does not contain a polyphenylene ether in which one or more A's are hydrogen atoms in the structure of the above formula (1).
[0025] The modified polyphenylene ether of the present embodiment preferably contains less than 200 ppm by mass of methacrylic acid, less than 200 ppm by mass of methacrylic anhydride and vinyl methacrylate, less than 200 ppm by mass of an organic amine catalyst, and less than 1,500 ppm by mass of chloride ions, based on the modified polyphenylene ether represented by the above formula (1), and more preferably contains less than 100 ppm by mass of methacrylic acid, less than 100 ppm by mass of methacrylic anhydride and vinyl methacrylate, less than 100 ppm by mass of an organic amine catalyst, and less than 1,000 ppm by mass of chloride ions, based on the modified polyphenylene ether represented by the above formula (1).
[0026] The modified polyphenylene ether can be obtained, for example, by copolymerizing a monovalent phenol compound represented by the following formula (6) with a polyvalent (a-valent) phenol compound (central phenol) represented by the following formula (7) to obtain an unmodified polyphenylene ether, which is then modified. The details of the production method will be described later. [ka] ...Equation (6) (In formula (6), R 21 is the same as the group in the above formula (4), and is preferably the same as the group in the above formula (4). [ka] ...Equation (7) (In formula (7), X, R 4 , k, and a are the same as those in the above formula (2), and are preferably the same as those in the above formula (2). The a partial structures bonded to X may be the same or different, but are preferably the same.
[0027] Examples of the monohydric phenol compound represented by the above formula (6) include 2,6-dimethylphenol, 2-methyl-6-ethylphenol, 2,6-diethylphenol, 2-ethyl-6-n-propylphenol, 2-methyl-6-chlorophenol, 2-methyl-6-bromophenol, 2-methyl-6-n-propylphenol, 2-ethyl-6-bromophenol, 2-methyl-6-n-butylphenol, 2,6-di-n-propylphenol, 2-ethyl-6-chlorophenol, 2-methyl-6-phenylphenol, 2,6-diphenylphenol, 2-methyl-6-tolylphenol, 2,6-ditolylphenol, etc. Among them, 2,6-dimethylphenol, 2,6-diethylphenol, and 2,6-diphenylphenol are particularly preferred because they are inexpensive and easily available.
[0028] The above phenol compounds may be used alone or in combination of two or more.
[0029] The a-hydric phenol compound represented by the above formula (7) can be industrially advantageously produced by reacting the corresponding monohydric phenol compound with an aldehyde (e.g., formaldehyde, etc.), a ketone (e.g., acetone, methyl ethyl ketone, methyl isobutyl ketone, acetophenone, cyclohexanone, etc.) or a dihalogenated aliphatic hydrocarbon, or by reacting the corresponding monohydric phenol compounds with each other.
[0030] Among the phenol compounds represented by the above formula (7), examples of the phenol compounds having two phenol units in the molecule are listed below. Examples of the hydroxyphenyl ether include, but are not limited to, 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 4,4'-methylenebis(2,6-dimethylphenol), bis(4-hydroxy-3-methylphenyl)sulfide, bis(4-hydroxy-3,5-dimethylphenyl)sulfone, α,α'-bis(4-hydroxy-3,5-dimethylphenyl)-1,4-diisopropylbenzene, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 1,1-bis(4-hydroxy-3-methylphenyl)cyclohexane, and 1,1-bis(2-methyl-4-hydroxy-5-t-butylphenyl)butane.
[0031] Further, among the phenol compounds represented by the above formula (7), examples of the phenol compounds having three or more phenol units in the molecule are listed below. 4,4'-[(3-hydroxyphenyl)methylene]bis(2,6-dimethylphenol), 4,4'-[(3-hydroxyphenyl)methylene]bis(2,3,6-trimethylphenol), 4,4'-[(4-hydroxyphenyl)methylene]bis(2,6-dimethylphenol), 4,4'-[(4-hydroxyphenyl)methylene]bis(2,3,6-trimethylphenol), 4,4'-[(2-hydroxy-3-methoxyphenyl)methylene]bis(2,6-dimethylphenol), 4,4'-[(4-hydroxy-3-ethoxyphenyl)methylene]bis(2,6-dimethylphenol), 4,4'-[(3,4-dihydroxyphenyl)methylene]bis(2,3,6-trimethylethylphenol), 4,4'-[(3,4-dihydroxyphenyl)methylene]bis(2,3,6-trimethylphenol), 2,2'-[(4-hydroxyphenyl)methylene]bis(3,5,6-trimethylphenol), 4,4'-[4-(4-hydroxyphenyl)cyclohexylidene]bis(2,6-dimethylphenol), 4,4'-[(2-hydroxyphenyl)methylene] -Bis(2,3,6-trimethylphenol), 4,4'-[1-[4-[1-(4-hydroxy-3,5-dimethylphenyl)-1-methylethyl]phenyl]ethylidene]bis(2,6-dimethylphenol), 4,4'-[1-[4-[1-(4-hydroxy-3-fluorophenyl)-1-methylethyl]phenyl]ethylidene]bis(2,6-dimethylphenol), 2,6-bis[(4-hydroxy-3,5-dimethylphenyl)ethyl]-4-methylphenol, 2,6-bis[(4-hydroxy-2,3,6-trimethylphenol)ethyl] 2,6-bis[(4-hydroxy-3,5,6-trimethylphenyl)methyl]-4-methylphenol, 2,6-bis[(4-hydroxy-3-methylphenyl)methyl]-4-ethylphenol, 2,4-bis[(4-hydroxy-3-methylphenyl)methyl]-6-methylphenol, 2,6-bis[(4-hydroxy-3-methylphenyl)methyl]-4-methylphenol, 2,4-bis[(4-hydroxy-3-cyclohexylphenyl)methyl]-6-methylphenol, 2,4-bis[(4-hydroxy-3-methylphenyl)methyl]-6-cyclohexylphenol, 2,4-Bis[(2-hydroxy-5-methylphenyl)methyl]-6-cyclohexylphenol, 2,4-bis[(4-hydroxy-2,3,6-trimethylphenyl)methyl]-6-cyclohexylphenol, 3,6-bis[(4-hydroxy-3,5-dimethylphenyl)methyl]-1,2-benzenediol, 4,6-bis[(4-hydroxy-3,5-dimethylphenyl)methyl]-1,3-benzenediol, 2,4,6-tris[(4-hydroxy-3,5-dimethylphenyl)methyl]-1,3-benzenediol , 2,4,6-tris[(2-hydroxy-3,5-dimethylphenyl)methyl]-1,3-benzenediol, 2,2'-methylenebis[6-[(4 / 2-hydroxy-2,5 / 3,6-dimethylphenyl)methyl]-4-methylphenol], 2,2'-methylenebis[6-[(4-hydroxy-3,5-dimethylphenyl)methyl]-4-methylphenol], 2,2'-methylenebis[6-[(4 / 2-hydroxy-2,3,5 / 3,4,6-trimethylphenyl)methyl]-4-methylphenol], 2,2'-methylene Bis[6-[(4-hydroxy-2,3,5-trimethylphenyl)methyl]-4-methylphenol], 4,4'-methylenebis[2-[(2,4-dihydroxyphenyl)methyl]-6-methylphenol], 4,4'-methylenebis[2-[(2,4-dihydroxyphenyl)methyl]-3,6-dimethylphenol], 4,4'-methylenebis[2-[(2,4-dihydroxy-3-methylphenyl)methyl]-3,6-dimethylphenol], 4,4'-methylenebis[2-[(2,3,4-trihydroxyphenyl)methyl]- ethyl]-3,6-dimethylphenol], 6,6'-methylenebis[4-[(4-hydroxy-3,5-dimethylphenyl)methyl]-1,2,3-benzenetriol], 1,1-bis(2-methyl-4-hydroxy-5-t-butylphenyl)butane, 4,4'-cyclohexylidenebis[2-cyclohexyl-6-[(2-hydroxy-5-methylphenyl)methyl]phenol], 4,4'-cyclohexylidenebis[2-cyclohexyl-6-[(4-hydroxy-3,5-dimethylphenyl)methyl]phenol], 4,Examples of the phenol include, but are not limited to, 4'-cyclohexylidenebis[2-cyclohexyl-6-[(4-hydroxy-2-methyl-5-cyclohexylphenyl)methyl]phenol], 4,4'-cyclohexylidenebis[2-cyclohexyl-6-[(2,3,4-trihydroxyphenyl)methyl]phenol], 4,4',4'',4'''-(1,2-ethanediylidene)tetrakis(2,6-dimethylphenol), 4,4',4'',4'''-(1,4-phenylenedimethylidene)tetrakis(2,6-dimethylphenol), and 1,1,3-tris-(2-methyl-4-hydroxy-5-tertiarybutylphenyl)butane.
[0032] Particularly preferred a-hydric phenol compounds (central phenols) are 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane, 1,1-bis(2-methyl-4-hydroxy-5-t-butylphenyl)butane, 4,4'-[(4-hydroxyphenyl)methylene]bis(2,6-dimethylphenol), 4,4'-[(3-hydroxyphenyl)methylene]bis(2,6-dimethylphenol), 4,4'-[(4-hydroxyphenyl)methylene]bis(2,6-dimethylphenol), The compounds that are being investigated are 4,4'-[(3-hydroxyphenyl)methylene]bis(2,3,6-trimethylphenol), 4,4',4'',4''-(1,4-phenylenedimethylidene)tetrakis(2,6-dimethylphenol), 1,1,3-tris-(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, and 1,1-bis(2-methyl-4-hydroxy-5-t-butylphenyl)butane.
[0033] The number of phenolic hydroxyl groups in the a-valent phenol compound (central phenol) is not particularly limited as long as it is 2 or more. However, since an increase in the number of polyphenylene ether ends may make it difficult to control the thermal curing rate, the number is preferably 2 to 6, and more preferably 2 to 4.
[0034] When an a-hydric phenol compound (central phenol) represented by formula (7) is contained, the amount of the dihydric phenol compound of formula (7) relative to the total monohydric phenols represented by formula (6) is not particularly limited, but is preferably 2 to 30 mol % relative to the total monohydric phenols.
[0035] In the modified polyphenylene ether of this embodiment, the polyfunctional polyphenylene ether serving as the raw material of the modified polyphenylene ether having the structure of the above formula (1) can also be produced by a redistribution reaction in which a monofunctional polyphenylene ether is equilibrated with a polyhydric phenol in the presence of an oxidizing agent. The redistribution reaction is known in the art and is described, for example, in U.S. Patent No. 3,496,236 to Cooper et al. and U.S. Patent No. 5,880,221 to Liska et al.
[0036] However, when producing a polyfunctional polyphenylene ether using a redistribution reaction, peroxides are often used as a reaction initiator and an oxidizing agent, but these peroxides are highly reactive and produce by-products in various forms. A typical example of such by-products is a peroxide adduct to the produced polyphenylene ether. In addition, by-products in which peroxides are added to the raw materials, monofunctional polyphenylene ether and polyhydric phenol, as well as the target polyfunctional polyphenylene ether, are produced, so that the purity of the target modified polyphenylene ether having the structure of the above formula (1) is reduced, and the average number of functional groups per central phenol moiety is also reduced.
[0037] The number average molecular weight (Mn) of the modified polyphenylene ether in this embodiment is preferably 500 to 15,000, more preferably 1,000 to 10,000, and even more preferably 1,500 to 8,000. When the number average molecular weight (Mn) is within the above range, the fluidity is improved when dissolved in a solvent for preparing a varnish in the step of applying the modified polyphenylene ether to a substrate material, and the processability when applied to the substrate material can be ensured. The number average molecular weight can be measured by the method described in the Examples below.
[0038] The average number of functional groups of the modified polyphenylene ether in the present embodiment is preferably 1.8 to 6.0, more preferably 2.0 to 4.0, and even more preferably 2.5 to 4.0. When the average number of functional groups is within the above range, the thermal curing speed of the polyphenylene ether terminals can be controlled, and thermal curing defects can be suppressed. The average number of functional groups can be measured by the method described in the Examples below.
[0039] <Method of producing modified polyphenylene ether> The modified polyphenylene ether of the present embodiment can be produced, for example, by synthesizing a polyfunctional polyphenylene ether having hydroxyl groups at its molecular terminals, represented by the following formula (8), by a polymerization method (also referred to herein as an unmodified polyfunctional polyphenylene ether or an unmodified polyphenylene ether), and introducing the A substituent in formula (1) into the terminal hydroxyl group, i.e., modifying the polyphenylene ether. [ka] ...Equation (8) (In (8), Z, Y, n, and a are the same as those in formula (1), and are preferably the same.)
[0040] (Polymerization process) In the method for producing the unmodified polyfunctional polyphenylene ether, it is preferable to use, as the polymerization solvent in the polymerization step, an aromatic solvent which is a good solvent for the unmodified polyfunctional polyphenylene ether. Here, a good solvent for an unmodified polyfunctional polyphenylene ether is a solvent capable of dissolving the polyfunctional polyphenylene ether. Examples of such solvents include aromatic hydrocarbons such as benzene, toluene, xylene (including o-, m-, and p-isomers), ethylbenzene, and styrene; halogenated hydrocarbons such as chlorobenzene and dichlorobenzene; and nitro compounds such as nitrobenzene.
[0041] As the polymerization catalyst used in this embodiment, a known catalyst system that can be generally used for the production of polyphenylene ether can be used. A generally known catalyst system is one that is composed of a transition metal ion having redox ability and an amine compound that can form a complex with the transition metal ion, such as a catalyst system composed of a copper compound and an amine compound, a catalyst system composed of a manganese compound and an amine compound, a catalyst system composed of a cobalt compound and an amine compound, etc. Since the polymerization reaction proceeds efficiently under slightly alkaline conditions, a small amount of alkali or an additional amine compound may be added thereto.
[0042] The polymerization catalyst preferably used in the present embodiment is a catalyst containing a copper compound, a halogen compound, and an amine compound as catalyst components, and more preferably a catalyst containing a diamine compound represented by the following formula (9) as the amine compound.
[0043] [ka] ...Equation (9) In formula (9), R 14 , R 15 , R 16 , R 17 are each independently a hydrogen atom or a linear or branched alkyl group having 1 to 6 carbon atoms, but are not all hydrogen atoms at the same time. 18 is a linear or methyl-branched alkylene group having 2 to 5 carbon atoms.
[0044] Examples of the copper compound of the catalyst component described herein are listed below. Suitable copper compounds include cuprous compounds, cupric compounds, and mixtures thereof. Examples of cupric compounds include, for example, cupric chloride, cupric bromide, cupric sulfate, and cupric nitrate. Examples of cuprous compounds include, for example, cuprous chloride, cuprous bromide, cuprous sulfate, and cuprous nitrate. Particularly preferred metal compounds among these are cuprous chloride, cupric chloride, cuprous bromide, and cupric bromide. These copper salts may be synthesized at the time of use from oxides (e.g., cuprous oxide), carbonates, hydroxides, and the like and corresponding halogens or acids. A method that is often used is to mix the cuprous oxide exemplified above with hydrogen halide (or a solution of hydrogen halide) to prepare the copper salt.
[0045] Examples of halogen compounds include hydrogen chloride, hydrogen bromide, hydrogen iodide, sodium chloride, sodium bromide, sodium iodide, potassium chloride, potassium bromide, potassium iodide, tetramethylammonium chloride, tetramethylammonium bromide, tetramethylammonium iodide, tetraethylammonium chloride, tetraethylammonium bromide, and tetraethylammonium iodide. These compounds can be used as aqueous solutions or solutions using appropriate solvents. These halogen compounds can be used alone as components, or in combination of two or more. Preferred halogen compounds are aqueous solutions of hydrogen chloride and hydrogen bromide. The amount of these compounds used is not particularly limited, but is preferably 2 to 20 times the molar amount of halogen atoms relative to the molar amount of copper atoms, and the amount of copper atoms used is preferably in the range of 0.02 to 0.6 moles per 100 moles of the phenol compound added to the polymerization reaction.
[0046] Examples of the diamine compound of the catalyst component are as follows: N,N,N',N'-tetramethylethylenediamine, N,N,N'-trimethylethylenediamine, N,N'-dimethylethylenediamine, N,N-dimethylethylenediamine, N-methylethylenediamine, N,N,N',N'-tetraethylethylenediamine, N,N,N'-triethylethylenediamine, N,N'-diethylethylenediamine, N,N-diethylethylenediamine, N-ethylethylenediamine, N,N-dimethyl-N'-ethylethylenediamine, N,N'-dimethyl-N-ethylethylenediamine, Nn-propylethylenediamine, N,N'-n-propylethylenediamine, Ni-propylethylenediamine, N,N'-i-propylethylenediamine, Nn-butylethylenediamine, amine, N,N'-n-butylethylenediamine, Ni-butylethylenediamine, N,N'-i-butylethylenediamine, Nt-butylethylenediamine, N,N'-t-butylethylenediamine, N,N,N',N'-tetramethyl-1,3-diaminopropane, N,N,N'-trimethyl-1,3-diaminopropane, N,N'-dimethyl-1,3-diaminopropane, N-methyl-1,3-diaminopropane, N,N,N',N'-tetramethyl-1,3-diamino-1-methylpropane, N,N,N',N'-tetramethyl-1,3-diamino-2-methylpropane, N,N,N',N'-tetramethyl-1,4-diaminobutane, and N,N,N',N'-tetramethyl-1,5-diaminopentane. A preferred diamine compound for this embodiment is one in which the number of carbon atoms in the alkylene group connecting the two nitrogen atoms is 2 or 3. The amount of these diamine compounds used is not particularly limited, but is preferably in the range of 0.01 mol to 10 mol per 100 mol of the phenol compound added to the polymerization reaction.
[0047] In this embodiment, the polymerization catalyst may contain a primary amine and a secondary monoamine as a component. Examples of the secondary monoamine include, but are not limited to, dimethylamine, diethylamine, di-n-propylamine, di-i-propylamine, di-n-butylamine, di-i-butylamine, di-t-butylamine, dipentylamines, dihexylamines, dioctylamines, didecylamines, dibenzylamines, methylethylamine, methylpropylamine, methylbutylamine, cyclohexylamine, N-phenylmethanolamine, N-phenylethanolamine, N-phenylpropanolamine, N-(m-methylphenyl)ethanolamine, N-(p-methylphenyl)ethanolamine, N-(2',6'-dimethylphenyl)ethanolamine, N-(p-chlorophenyl)ethanolamine, N-ethylaniline, N-butylaniline, N-methyl-2-methylaniline, N-methyl-2,6-dimethylaniline, and diphenylamine.
[0048] The polymerization catalyst of the present embodiment may also contain a tertiary monoamine compound as a component thereof. The tertiary monoamine compound is an aliphatic tertiary amine including an alicyclic tertiary amine. Examples of the tertiary monoamine compound include trimethylamine, triethylamine, tripropylamine, tributylamine, triisobutylamine, dimethylethylamine, dimethylpropylamine, allyldiethylamine, dimethyl-n-butylamine, diethylisopropylamine, and N-methylcyclohexylamine. These tertiary monoamines may be used alone or in combination of two or more. The amount of these compounds used is not particularly limited, but is preferably in the range of 15 moles or less relative to 100 moles of the phenol compound added to the polymerization reaction.
[0049] In this embodiment, there is no limitation on adding a surfactant that has been known to have an effect of improving polymerization activity. Examples of such surfactants include trioctylmethylammonium chloride, known under the trade names Aliquat 336 and Capriquat. The amount of the surfactant used is preferably within a range not exceeding 0.1% by mass relative to the total amount (100% by mass) of the polymerization reaction mixture.
[0050] As the oxygen-containing gas in the polymerization of this embodiment, in addition to pure oxygen, a mixture of oxygen and an inert gas such as nitrogen in any ratio, air, and a mixture of air and an inert gas such as nitrogen in any ratio can be used. Normal pressure is sufficient for the pressure in the system during the polymerization reaction, but reduced or increased pressure can be used as necessary.
[0051] The polymerization temperature is not particularly limited, but if it is too low, the reaction will not proceed easily, and if it is too high, there is a risk of a decrease in reaction selectivity and the production of high molecular weight components. Therefore, the temperature is in the range of 0 to 60°C, preferably 10 to 50°C.
[0052] In the method for producing unmodified polyfunctional polyphenylene ether, it is preferable to polymerize polyphenylene ether in a solution state (also referred to as "solution polymerization" in this specification). By producing by solution polymerization, even when a central phenol having a bulky structure is used, the ratio of polyphenylene ether components not containing the structure of the above formula (8) and by-products due to peroxides produced during the production of unmodified polyfunctional polyphenylene ether can be reduced, and the desired modified polyphenylene ether containing the structure of the above formula (1) can be produced with high purity.
[0053] (Copper extraction and by-product removal process) In this embodiment, there is no particular restriction on the post-treatment method after the polymerization reaction is completed. Usually, an acid such as hydrochloric acid or acetic acid, or ethylenediaminetetraacetic acid (EDTA) and its salts, nitrilotriacetic acid and its salts, etc. are added to the reaction liquid to deactivate the catalyst. In addition, a method for removing and treating the dihydric phenol by-product generated by the polymerization of polyphenylene ether can be performed using a conventionally known method. If the metal ions, which are the catalyst, are substantially deactivated as described above, the mixture can be decolorized simply by heating it. Alternatively, a method of adding a required amount of a known reducing agent is also possible. Examples of known reducing agents include hydroquinone and sodium dithionite.
[0054] (Liquid-liquid separation process) In the method for producing unmodified polyfunctional polyphenylene ether, water may be added to extract the compound in which the copper catalyst has been deactivated, and then the organic phase and the aqueous phase may be separated into liquid-liquid phases, and the aqueous phase may be removed to remove the copper catalyst from the organic base. This liquid-liquid separation step is not particularly limited, and may include methods such as static separation and separation using a centrifuge. In order to promote the liquid-liquid separation, a known surfactant or the like may be used.
[0055] (concentration / drying process) Next, in the method for producing the modified polyphenylene ether of the present embodiment, the organic phase containing the unmodified polyfunctional polyphenylene ether after the liquid-liquid separation may be concentrated and dried by volatilizing the solvent. This step may be omitted when the subsequent modification reaction (the reaction of introducing the substituent A in formula (1) to the terminal of the unmodified polyfunctional polyphenylene ether) is carried out.
[0056] The method for volatilizing the solvent contained in the organic phase is not particularly limited, but examples thereof include a method of transferring the organic phase to a high-temperature concentration tank and distilling off the solvent to concentrate it, and a method of distilling off toluene using equipment such as a rotary evaporator to concentrate it, and the like.
[0057] The temperature of the drying treatment in the drying step is preferably at least 60° C. or higher, more preferably 80° C. or higher, even more preferably 120° C. or higher, and most preferably 140° C. or higher. When the polyfunctional polyphenylene ether is dried at a temperature of 60° C. or higher, the content of high-boiling-point volatile components in the polyphenylene ether powder can be efficiently reduced.
[0058] In order to obtain unmodified polyfunctional polyphenylene ether with high efficiency, a method of increasing the drying temperature, a method of increasing the degree of vacuum in the drying atmosphere, a method of stirring during drying, etc. are effective, but a method of increasing the drying temperature is particularly preferable from the viewpoint of production efficiency. In the drying step, it is preferable to use a dryer equipped with a mixing function. Examples of the mixing function include a stirring type and a rolling type dryer. This allows the processing amount to be increased and the productivity to be maintained high.
[0059] (Modification reaction process) There is no limitation on the method for introducing the substituent A (the functional group of the above formula (5)) to the terminal of the obtained unmodified polyphenylene ether. For example, it can be obtained by a reaction to form an ester bond between a hydroxyl group at the terminal of the unmodified polyphenylene ether and a carboxylic acid having a carbon-carbon double bond (hereinafter simply referred to as "carboxylic acid"). The formation of ester bonds can be achieved by various known methods. For example, the formation of ester bonds can be achieved by a. reaction of a carboxylic acid halide with a hydroxyl group at the polymer end, b. reaction with a carboxylic acid anhydride, c. direct reaction with a carboxylic acid, d. transesterification with an ester, etc. The carboxylic acid halides, carboxylic acid anhydrides, carboxylic acids, and esters described above in a to d are called modifiers. The reaction of a with an carboxylic acid halide is one of the most common methods. Although chlorides and bromides are generally used as carboxylic acid halides, other halogens may also be used. The reaction may be either a direct reaction with a hydroxyl group or a reaction with an alkali metal salt of a hydroxyl group. In the direct reaction of a carboxylic acid halide with a hydroxyl group, an acid such as hydrogen halide is generated, so a weak base such as an amine may be used to trap the acid. In the reaction of b with a carboxylic acid anhydride or the direct reaction of c with a carboxylic acid, a compound such as a carbodiimide or dimethylaminopyridine may be used to activate the reaction site and promote the reaction. In the case of the transesterification reaction of d, it is desirable to remove the generated alcohols as necessary. In addition, known metal catalysts may be used to promote the reaction. After the reaction, the reaction mixture may be washed with water, an acidic or alkaline aqueous solution to remove by-products such as amine salts, or the polymer solution may be dropped into a poor solvent such as an alcohol to recover the target product by reprecipitation. After washing the polymer solution, the solvent may be distilled off under reduced pressure to recover the polymer.
[0060] As a method for introducing the substituent A (functional group of the above formula (5)) to the end of the obtained unmodified polyphenylene ether, vinyl carboxylate represented by formula (10) may be used. In order to activate the reaction site and promote the reaction, an organic amine catalyst or a Lewis acid catalyst may be coexisted. As the organic amine catalyst, diaminopyridine (particularly preferably dimethylaminopyridine) having a high carbonyl group activation ability is preferable. As the Lewis acid catalyst, although there is no particular limitation, aluminum chloride, trifluoroborane, scandium (III) triflate, etc. are preferable. [ka] ...Equation (10) In the above formula (10), R 31are each independently any one of a hydrogen atom, a hydroxyl group, a hydrocarbon group having 1 to 30 carbon atoms (for example, a linear hydrocarbon group, a cyclic hydrocarbon group), an aryl group, an alkoxy group, an aryloxy group, an amino group, and a hydroxyalkyl group. R 32 are each independently a hydrocarbon group having 1 to 30 carbon atoms (for example, an alkylene group). R 31 Examples of the compound include the same compounds as those described above, and the same compounds are preferable. 32 Examples of the compound include the same compounds as those mentioned above, and the same compounds are preferred. s is an integer from 0 to 5.
[0061] As the above-mentioned modifier, methacrylic anhydride, methacryloyl chloride, and vinyl methacrylate are preferred because they are commercially produced and easily available. In the case of methacrylic anhydride, methacrylic acid is generated as a leaving group, and in the case of methacryloyl chloride, chloride ions are generated as a leaving group, so that after the introduction of the substituent A, a large amount of methacrylic acid and chloride ions are contained in the system. On the other hand, when vinyl methacrylate is used, the leaving group is acetaldehyde gas, and it is easy to remove the leaving group from the reaction solution, so vinyl methacrylate is preferred. Methods for removing acetaldehyde gas include bubbling nitrogen into the reaction solution and vacuum drying.
[0062] Impurities contained in the modified polyphenylene ether represented by the following formula (1) include methacrylic anhydride, vinyl methacrylate, etc. derived from the modifying agent, methacrylic acid, methyl methacrylate, chloride ions, etc. generated as a leaving group due to the inactivation of the modifying agent, and organic amines used as catalysts.
[0063] It is preferable that the modified polyphenylene ether represented by the above formula (1) contains as few impurities as possible. The present inventors have found that by lowering the mass proportions of methacrylic acid, methacrylic anhydride, vinyl methacrylate, an organic amine catalyst, and chloride ions, among the impurities contained in the modified polyphenylene ether represented by the above formula (1), the glass transition temperature becomes particularly high after curing a composition containing the modified polyphenylene ether represented by the above formula (1). The organic amine catalyst is a compound having a tertiary amine, and examples thereof include 4-dimethylaminopyridine, 4-pyrrolidinopyridine, 1,8-diazabicyclo[5.4.0]undecene-7, 1,5-diazabicyclo[4.3.0]nonene-5, 1,4-diazabicyclo[2.2.2]octane, and 1-azabicyclo[2.2.2]octane. The organic amine catalyst may be an organic amine catalyst added to the reaction of introducing the substituent A into the unmodified polyphenylene ether described above. The chloride ion is Cl - This refers to. The mass ratio of methacrylic acid in the modified polyphenylene ether can be reduced by, for example, using vinyl methacrylate with low reactivity to water, avoiding the use of methacrylic acid halides and methacrylic acid anhydrides, which are used in the formation of ester bonds by a. reaction of methacrylic acid halides with hydroxyl groups at the polymer terminals, and b. reaction with methacrylic acid anhydride, which are introduction methods that have high reactivity of the modifying agent and can easily achieve a high introduction rate of the substituent A. Furthermore, in the case of methacrylic acid anhydride, an amount of methacrylic acid equivalent to the methacrylic acid anhydride is by-produced as a leaving group. It is difficult to completely remove the by-produced methacrylic acid, for example, by washing the modified polyphenylene ether with an alcohol-based solvent, which is a poor solvent, and it is important to change the type of modifying agent and prevent it from being generated in the system. The total mass proportion of methacrylic anhydride and vinyl methacrylate in the modified polyphenylene ether can be reduced, for example, by selecting a more active chemical species as the organic amine catalyst used in the reaction of the modifying agent with the unmodified polyphenylene ether and avoiding the addition of an excess of the modifying agent. The mass proportion of the organic amine catalyst in the modified polyphenylene ether can be lowered, for example, by reducing the addition rate of the organic amine catalyst or by using a highly active Lewis acid catalyst. The mass proportion of chloride ions in the modified polyphenylene ether can be reduced by, for example, using vinyl methacrylate, which has low reactivity to water, and avoiding the use of a methacrylic acid halide, which is used in the reaction between a methacrylic acid halide and a hydroxyl group at the polymer terminal, and which is easily deactivated by reaction with a trace amount of moisture in the system and which generates an amine hydrochloride by a side reaction with hydrochloric acid or the coexisting organic amine catalyst. By reducing the amounts of methacrylic acid, methacrylic anhydride, vinyl methacrylate, organic amine catalyst, and chloride ions in the thermosetting composition described below, poor curing due to acids and low molecular weight components can be suppressed, and the Tg of the thermosetting composition can be improved. The contents of methacrylic acid, methacrylic anhydride, vinyl methacrylate, organic amine catalyst and chloride ions in the modified polyphenylene ether can be measured by the method described in the Examples below.
[0064] The method for producing the modified polyphenylene ether of the present embodiment is not limited to the above-described method for producing the modified polyphenylene ether of the present embodiment, and the order and number of the above-described polymerization step, copper extraction and by-product removal step, liquid-liquid separation step, and concentration and drying step may be appropriately adjusted.
[0065] <Thermosetting composition> The modified polyphenylene ether of the present embodiment can be used as a thermosetting composition. The thermosetting composition is not particularly limited as long as it contains the modified polyphenylene ether, but it is preferable that the thermosetting composition further contains a crosslinking agent and an organic peroxide, and if desired, it can further contain a thermoplastic resin, a flame retardant, other additives, a silica filler, a solvent, etc. The components of the thermosetting composition of the present embodiment will be described below.
[0066] (Modified polyphenylene ether) As described above, the modified polyphenylene ether of the present embodiment may be used as the sole resin component in the thermosetting composition, or may be used in combination with polyphenylene ethers having other structures, or may be used in combination with various known additives. When used in combination with other components, the content of the modified polyphenylene ether in the thermosetting composition is preferably 0.5 to 95 mass %, more preferably 20 to 93 mass %, and even more preferably 40 to 90 mass %.
[0067] (Crosslinking agent) Any crosslinking agent capable of initiating or facilitating a crosslinking reaction can be used in the thermosetting composition of the present embodiments. The crosslinking agent preferably has a number average molecular weight of not more than 4000. When the number average molecular weight of the crosslinking agent is not more than 4000, an increase in the viscosity of the thermosetting composition can be suppressed, and good resin fluidity can be obtained during thermoforming. The number average molecular weight may be a value measured by a general molecular weight measurement method, specifically, a value measured by GPC, etc.
[0068] From the viewpoint of the crosslinking reaction, the crosslinking agent preferably has an average of two or more carbon-carbon unsaturated double bonds per molecule. The crosslinking agent may be composed of one type of compound or two or more types of compounds. In addition, the term "carbon-carbon unsaturated double bond" as used herein refers to a double bond located at an end branched from the main chain when the crosslinking agent is a polymer or oligomer. An example of the carbon-carbon unsaturated double bond is a 1,2-vinyl bond in polybutadiene.
[0069] When the number average molecular weight of the crosslinking agent is less than 600, the number (average value) of carbon-carbon unsaturated double bonds per molecule of the crosslinking agent is preferably 2 to 4. When the number average molecular weight of the crosslinking agent is 600 or more and less than 1,500, the number (average value) of carbon-carbon unsaturated double bonds per molecule of the crosslinking agent is preferably 4 to 26. When the number average molecular weight of the crosslinking agent is 1,500 or more and less than 4,000, the number (average value) of carbon-carbon unsaturated double bonds per molecule of the crosslinking agent is preferably 26 to 60. When the number average molecular weight of the crosslinking agent is within the above range, the number of carbon-carbon unsaturated double bonds is equal to or more than the specific value, so that the thermosetting composition of this embodiment has a higher reactivity of the crosslinking agent and a higher crosslink density of the cured product of the thermosetting composition, and as a result, it can provide better heat resistance. On the other hand, when the number average molecular weight of the crosslinking agent is within the above range, the number of carbon-carbon unsaturated double bonds is equal to or less than the specific value, so that it can provide better resin fluidity during hot molding.
[0070] Examples of the crosslinking agent include trialkenyl isocyanurate compounds such as triallyl isocyanurate (TAIC), trialkenyl cyanurate compounds such as triallyl cyanurate (TAC), polyfunctional methacrylate compounds having two or more methacrylic groups in the molecule, polyfunctional acrylate compounds having two or more acrylic groups in the molecule, polyfunctional vinyl compounds having two or more vinyl groups in the molecule such as polybutadiene, vinylbenzyl compounds such as divinylbenzene having a vinylbenzyl group in the molecule, and polyfunctional maleimide compounds having two or more maleimide groups in the molecule such as 4,4'-bismaleimide diphenylmethane. These crosslinking agents are used alone or in combination of two or more. Of these, the crosslinking agent preferably contains at least one compound selected from the group consisting of triallyl cyanurate, triallyl isocyanurate, and polybutadiene. When the crosslinking agent contains at least one or more compounds described above, the thermosetting composition has better compatibility between the crosslinking agent and the modified polyphenylene ether, and better coatability, and when mounted on an electronic circuit board, the board properties tend to be better.
[0071] The mass ratio of the modified polyphenylene ether to the crosslinking agent (modified polyphenylene ether:crosslinking agent) is preferably 25:75 to 95:5, and more preferably 32:68 to 85:15, from the viewpoints of improving the compatibility between the crosslinking agent and the modified polyphenylene ether, the coatability of the thermosetting composition, and achieving even better properties of the mounted electronic circuit board.
[0072] (organic peroxide) In this embodiment, any organic peroxide capable of promoting the polymerization reaction of the thermosetting composition containing the modified polyphenylene ether and the crosslinking agent can be used. Examples of organic peroxides include benzoyl peroxide, cumene hydroperoxide, 2,5-dimethylhexane-2,5-dihydroperoxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3, di-t-butyl peroxide, t-butylcumyl peroxide, di(2-t-butylperoxyisopropyl)benzene, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, dicumyl peroxide, di-t-butylperoxyisophthalate, t-butylperoxybenzoate, 2,2-bis(t-butylperoxy)butane, 2,2-bis(t-butylperoxy)octane, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, di(trimethylsilyl)peroxide, and trimethylsilyltriphenylsilyl peroxide. In addition, radical generators such as 2,3-dimethyl-2,3-diphenylbutane can also be used as reaction initiators for the thermosetting composition. Among them, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3, di(2-t-butylperoxyisopropyl)benzene, and 2,5-dimethyl-2,5-di(t-butylperoxy)hexane are preferred from the viewpoint of providing a cured product having excellent heat resistance and mechanical properties, and further low dielectric constant and dielectric loss tangent.
[0073] The one-minute half-life temperature of the organic peroxide is preferably 155 to 185° C., more preferably 160 to 180° C., and even more preferably 165 to 175° C. When the one-minute half-life temperature of the organic peroxide is within the range of 155 to 185° C., the compatibility of the organic peroxide with the modified PPE, the coatability of the thermosetting composition, and the properties of the mounted electronic circuit board tend to be further improved. In this specification, the one-minute half-life temperature is the temperature at which the organic peroxide decomposes and the amount of active oxygen is reduced to half in one minute. The one-minute half-life temperature is a value confirmed by a method in which an organic peroxide is dissolved in a solvent inactive against radicals, such as benzene, to a concentration of 0.05 to 0.1 mol / L, and the organic peroxide solution is thermally decomposed in a nitrogen atmosphere.
[0074] Examples of organic peroxides having a one-minute half-life temperature in the range of 155 to 185°C include t-hexylperoxyisopropyl monocarbonate (155.0°C), t-butylperoxy-3,5,5-trimethylhexanoate (166.0°C), t-butylperoxylaurate (159.4°C), t-butylperoxyisopropyl monocarbonate (158.8°C), t-butylperoxy2-ethylhexyl monocarbonate (161.4°C), t-hexylperoxybenzoate (160.3°C), 2,5-dimethyl-2,5-di(benzoylperoxy)hexane (158.2°C), and the like. ), t-butyl peroxyacetate (159.9°C), 2,2-di-(t-butylperoxy)butane (159.9°C), t-butyl peroxybenzoate (166.8°C), n-butyl 4,4-di-(t-butylperoxy)valerate (172.5°C), di(2-t-butylperoxyisopropyl)benzene (175.4°C), dicumyl peroxide (175.2°C), di-t-hexyl peroxide (176.7°C), 2,5-dimethyl-2,5-di(t-butylperoxy)hexane (179.8°C), and t-butylcumyl peroxide (173.3°C).
[0075] The content of the organic peroxide, based on 100 parts by mass in total of the modified polyphenylene ether and the crosslinking agent, is preferably 0.05 parts by mass or more, more preferably 0.5 parts by mass or more, even more preferably 1 part by mass or more, and still more preferably 1.5 parts by mass or more, from the viewpoint of achieving even better compatibility between the organic peroxide and the modified PPE and even better coatability of the thermosetting composition, and is preferably 5 parts by mass or less, more preferably 4.5 parts by mass or less, from the viewpoint of achieving excellent board properties when the thermosetting composition is mounted on an electronic circuit board.
[0076] (thermoplastic resin) In this embodiment, any thermoplastic resin can be used. The thermoplastic resin is preferably at least one selected from the group consisting of a block copolymer of a vinyl aromatic compound and an olefin-based alkene compound and a hydrogenated product thereof (a hydrogenated block copolymer obtained by hydrogenating a block copolymer of a vinyl aromatic compound and an olefin-based alkene compound), and a homopolymer of a vinyl aromatic compound. From the viewpoint of achieving better compatibility with the modified polyphenylene ether, resin fluidity, coatability of the thermosetting composition, and heat resistance during curing, the weight average molecular weight of the thermoplastic resin is preferably more than 50,000 and not more than 780,000, more preferably 60,000 to 750,000, and even more preferably 70,000 to 700,000. When the thermosetting composition contains a modified polyphenylene ether, a crosslinking agent, an organic peroxide, and a thermoplastic resin having the type and weight-average molecular weight described above, the compatibility of the modified PPE with other components and the coatability onto substrates tend to be good, and thus the substrate properties when incorporated into an electronic circuit board may also be excellent. The weight average molecular weight can be determined by the method described in the Examples below.
[0077] The content of the vinyl aromatic compound-derived unit in the block copolymer or its hydrogenated product is preferably 20% by mass or more, more preferably 22% by mass or more, 24% by mass or more, 26% by mass or more, 28% by mass or more, 30% by mass or more, or 32% by mass or more. The upper limit is preferably 70% by mass or less, more preferably 69% by mass or less, 68% by mass or less, or 67% by mass or less. When the content of the vinyl aromatic compound-derived unit in the block copolymer or its hydrogenated product is 20 to 70% by mass, the compatibility with the modified polyphenylene ether tends to be further improved, and / or the adhesive strength with the metal foil tends to be further improved.
[0078] The vinyl aromatic compound may be any compound having an aromatic ring and a vinyl group in the molecule, and examples thereof include styrene. The olefin-based alkene compound may be any alkene having a linear or branched structure in the molecule, and examples thereof include ethylene, propylene, butylene, isobutylene, butadiene, and isoprene. From the viewpoint of having even better compatibility with the modified polyphenylene ether, the thermoplastic resin is preferably at least one selected from the group consisting of styrene-butadiene block copolymers, styrene-ethylene-butadiene block copolymers, styrene-ethylene-butylene block copolymers, styrene-butadiene-butylene block copolymers, styrene-isoprene block copolymers, styrene-ethylene-propylene block copolymers, styrene-isobutylene block copolymers, hydrogenated styrene-butadiene block copolymers, hydrogenated styrene-ethylene-butadiene block copolymers, hydrogenated styrene-butadiene-butylene block copolymers, hydrogenated styrene-isoprene block copolymers, and homopolymers of styrene (polystyrene), and more preferably at least one selected from the group consisting of styrene-butadiene block copolymers, hydrogenated styrene-butadiene block copolymers, and polystyrene.
[0079] The hydrogenation rate in the hydrogenated product is not particularly limited, and some of the carbon-carbon unsaturated double bonds derived from the olefin-based alkene compound may remain.
[0080] The content of the thermoplastic resin is 2 to 20 parts by mass, preferably 3 to 19 parts by mass, more preferably 4 to 18 parts by mass, and even more preferably 5 to 17 parts by mass, based on 100 parts by mass of the total of the modified polyphenylene ether and the crosslinking agent. By having this content within the above numerical range, the thermosetting composition of the present embodiment has better compatibility between the thermoplastic resin and the modified polyphenylene ether and better coatability, and tends to have better board properties when mounted on an electronic circuit board.
[0081] The thermosetting composition of the present embodiment may also contain a thermoplastic resin other than the thermoplastic resin having the type and weight average molecular weight described above.
[0082] (Flame retardant) The thermosetting composition of the present embodiment may contain any flame retardant. The flame retardant is not particularly limited as long as it is incompatible with other components contained in the thermosetting composition after the thermosetting composition is cured, from the viewpoint of improving heat resistance. Preferably, the flame retardant is incompatible with the modified polyphenylene ether and / or the crosslinking agent in the thermosetting composition after the thermosetting composition is cured. Examples of the flame retardant include inorganic flame retardants such as antimony trioxide, aluminum hydroxide, magnesium hydroxide, and zinc borate; aromatic bromine compounds such as hexabromobenzene, decabromodiphenylethane, 4,4-dibromobiphenyl, and ethylene bistetrabromophthalimide; and phosphorus-based flame retardants such as resorcinol bis-diphenyl phosphate and resorcinol bis-dixylenyl phosphate. These flame retardants may be used alone or in combination of two or more. Among these, the flame retardant is preferably decabromodiphenylethane from the viewpoints of compatibility between the flame retardant and the modified PPE, coatability of the thermosetting composition, and superior properties of the mounted electronic circuit board.
[0083] The content of the flame retardant is not particularly limited, but from the viewpoint of maintaining flame retardancy at the V-0 level of UL Standard 94, it is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more, relative to 100 parts by mass of the total of the modified polyphenylene ether and the crosslinking agent. Moreover, from the viewpoint of maintaining low dielectric constant and dielectric dissipation factor of the obtained cured product, the content of the flame retardant is preferably 50 parts by mass or less, more preferably 45 parts by mass or less, and even more preferably 40 parts by mass or less.
[0084] (Silica filler) The thermosetting composition of the present embodiment may contain a silica filler. Examples of the silica filler include natural silica, fused silica, synthetic silica, amorphous silica, aerosil, and hollow silica. The content of the silica filler may be 10 to 100 parts by mass relative to 100 parts by mass of the total of the modified polyphenylene ether and the crosslinking agent. The silica filler may be surface-treated with a silane coupling agent or the like.
[0085] The thermosetting composition of the present embodiment may further contain additives such as a heat stabilizer, an antioxidant, a UV absorber, a surfactant, and a lubricant, a solvent, and the like, in addition to the flame retardant and silica filler. When the thermosetting composition of the present embodiment contains a solvent, it can be in the form of a varnish in which the solid components in the thermosetting composition are dissolved or dispersed in the solvent, and a resin film can be formed from the thermosetting composition of the present embodiment.
[0086] (solvent) From the viewpoint of solubility, the solvent is preferably an aromatic compound such as toluene or xylene, methyl ethyl ketone (MEK), cyclopentanone, cyclohexanone, chloroform, etc. These solvents may be used alone or in combination of two or more.
[0087] <Prepreg> The prepreg of the present embodiment is a composite material including a substrate and the thermosetting composition, preferably including a substrate and the thermosetting composition of the present embodiment impregnated or applied to the substrate. The prepreg can be obtained, for example, by impregnating a substrate such as a glass cloth with a varnish of the thermosetting composition, and then drying and removing the solvent with a hot air dryer or the like.
[0088] Examples of the substrate include various glass cloths such as roving cloth, cloth, chopped mat, and surfacing mat; asbestos cloth, metal fiber cloth, and other synthetic or natural inorganic fiber cloths; woven or nonwoven fabrics obtained from liquid crystal fibers such as fully aromatic polyamide fibers, fully aromatic polyester fibers, and polybenzoxazole fibers; natural fiber cloths such as cotton cloth, linen cloth, and felt; natural cellulose-based substrates such as carbon fiber cloth, craft paper, cotton paper, and cloth obtained from paper-glass mixed fiber yarn; polytetrafluoroethylene porous film, etc. These substrates may be used alone or in combination of two or more.
[0089] The proportion of the solid content of the thermosetting composition of this embodiment in the prepreg (components other than the solvent of the thermosetting composition) is preferably 30 to 80 mass %, more preferably 40 to 70 mass %. When the proportion is 30 mass % or more, the insulation reliability tends to be more excellent when the prepreg is used for electronic boards, etc. When the proportion is 80 mass % or less, the mechanical properties such as flexural modulus tend to be more excellent in applications such as electronic boards.
[0090] <Laminate> The laminate of the present embodiment is a metal-clad laminate obtained by laminating and curing the thermosetting composition of the present embodiment or the prepreg of the present embodiment and a metal foil. The metal-clad laminate preferably has a configuration in which a cured product of the prepreg (hereinafter also referred to as a "cured product composite") and a metal foil are laminated and adhered to each other, and is suitably used as a material for electronic substrates. Examples of the metal foil include aluminum foil and copper foil. Among these, copper foil is preferred because of its low electrical resistance. The cured composite to be combined with the metal foil may be one or more sheets, and depending on the application, the composite is processed into a laminate by overlaying metal foil on one or both sides thereof.
[0091] Examples of methods for producing a metal-clad laminate include a method in which a composite (e.g., the above-mentioned prepreg) is formed from a thermosetting composition and a substrate, this is layered with metal foil, and then the thermosetting composition is cured to obtain a laminate in which the cured laminate and the metal foil are laminated together. One particularly preferred application of the metal-clad laminate is a printed wiring board, which is preferably formed by removing at least a portion of the metal foil from the metal-clad laminate.
[0092] <Printed wiring board> The printed wiring board of this embodiment is obtained by removing at least a part of the metal foil from the metal-clad laminate of this embodiment. The printed wiring board of this embodiment can typically be formed by a method of pressurizing and hot molding using the prepreg of this embodiment described above. Examples of the substrate include the same as those described above for the prepreg. The printed wiring board of the present embodiment contains the thermosetting composition of the present embodiment, and thus has excellent heat resistance and electrical properties (low dielectric constant and low dielectric tangent), can suppress fluctuations in electrical properties due to environmental changes, and has excellent insulation reliability and mechanical properties. EXAMPLES
[0093] Hereinafter, the present embodiment will be described in more detail based on Production Examples and Examples, but the present embodiment is not limited to the following Production Examples and Examples. It should be noted that Examples 5 to 7 are described as reference examples.
[0094] First, the measurement methods and evaluation criteria for each physical property will be described below.
[0095] (1) Number average molecular weight (Mn) As a measuring device, a gel permeation chromatography System 21 manufactured by Showa Denko KK was used, and a calibration curve was prepared using standard polystyrene and ethylbenzene. Using this calibration curve, the number average molecular weight (Mn) of the obtained modified polyphenylene ether was measured. The standard polystyrenes used had molecular weights of 3,650,000, 2,170,000, 1,090,000, 681,000, 204,000, 52,000, 30,200, 13,800, 3,360, 1,300, and 550. The columns used were two Showa Denko K-805L columns connected in series. The solvent used was chloroform, with a solvent flow rate of 1.0 mL / min and a column temperature of 40°C. A 1 g / L chloroform solution of modified polyphenylene ether was prepared and used as the measurement sample. The UV wavelength of the detection unit was 254 nm for standard polystyrene and 283 nm for polyphenylene ether. The number average molecular weight (Mn) (g / mol) was calculated from the peak area ratio based on the curve showing the molecular weight distribution obtained by GPC based on the above measurement data.
[0096] (2) Glass transition temperature (Tg) of the cured product of the thermosetting composition The dynamic viscoelasticity of the laminates produced in the examples and comparative examples was measured, and the temperature at which tan δ was maximum was determined as the glass transition temperature (Tg) (°C). A dynamic viscoelasticity device (RHEOVIBRON model DDV-01FP, manufactured by ORIENTEC) was used as the measuring device. The laminates were cut into strips of approximately 35 mm in length, 12 mm in width, and 0.5 mm in thickness so that the warp yarns of the glass cloth were the long sides, and measurements were performed in tension mode at a frequency of 10 rad / s.
[0097] (3) Dielectric constant of the cured product of the thermosetting composition The dielectric constant at 10 GHz of the laminates manufactured in the examples and comparative examples was measured by a cavity resonance method. As a measuring device, a network analyzer (N5230A, manufactured by Agilent Technologies) and a cavity resonator (Cavity Resornator CP series) manufactured by Kanto Electronics Application Development Co., Ltd. were used. The laminates were cut into strips with a width of about 2 mm, a length of 50 mm, and a thickness of about 0.5 mm so that the warp of the glass cloth was the long side. Next, the laminates were placed in an oven at 105°C ± 2°C and dried for 2 hours, and then left to stand for 24 ± 5 hours in an environment of 23°C and relative humidity of 50 ± 5%. Thereafter, the dielectric constant was measured using the above measuring device in an environment of 23°C and relative humidity of 50 ± 5%.
[0098] (4) Determination of impurities in modified polyphenylene ether Analysis was performed by GC / MS. An Agilent GC-6890 MSD-5973 was used, with a column: HP-5MS (L: 30 m, ID: 0.25 mm, film thickness: 0.25 μm), and carrier gas: helium. The temperature of the sample inlet was set at 325°C, and the column temperature was kept at 325°C. Detection was performed with an MSD detector, and the by-products were quantified by electron ionization mass spectrometry of the separated gas.
[0099] (5) Determination of chloride ions in modified polyphenylene ether The chloride ion content (ppm by mass) in the modified polyphenylene ether was determined by ion chromatography of the modified polyphenylene ether to be measured.
[0100] The methods for producing the modified polyphenylene ethers of the Examples and Comparative Examples will be described below.
[0101] (Production Example 1) A 1.5-liter jacketed reactor equipped with a sparger for introducing an oxygen-containing gas at the bottom of the reactor, stirring turbine blades and baffles, and a reflux condenser on the vent gas line at the top of the reactor was charged with a previously prepared mixture of 0.12 g of cuprous oxide and 1.29 g of 47% hydrogen bromide, 0.28 g of N,N'-di-t-butylethylenediamine, 10.22 g of dimethyl-n-butylamine, 2.23 g of di-n-butylamine, 885.6 g of toluene, 69.39 g of 2,6-dimethylphenol, 30.61 g of 1,1,3-tris(2-methyl-4-hydroxy-5-t-butylphenyl)butane (ADEKA: AO-30), and 0.05 g of trioctylmethylammonium chloride. Next, while vigorously stirring, air was started to be introduced into the reactor from the sparger at a rate of 1.05 L / min, and at the same time, a heat medium was passed through the jacket to adjust the polymerization temperature so as to maintain it at 20° C. 200 minutes after the start of air introduction, the air supply was stopped and the inside of the reactor was replaced with nitrogen gas, and then the polymerization mixture was added as an aqueous solution of 1.49 g of ethylenediaminetetraacetic acid tetrasodium salt tetrahydrate (a reagent manufactured by Dojindo Laboratories) and 200 g of water. Further, a mixture of 1.0 g of hydroquinone and 40 g of water was added, and the mixture was kept at 20°C for 1 hour to carry out reduction treatment of the by-product diphenoquinone, and then heated to 70°C and copper extraction was carried out at 70°C for 1 hour. Thereafter, the mixture was separated by standing to separate into an unmodified polyphenylene ether solution (organic phase) and an aqueous phase to which the catalyst metal had been transferred. The organic layer was concentrated by an evaporator to obtain unmodified polyphenylene ether in a solid state.
[0102] (Production Example 2) A 1.5-liter jacketed reactor equipped with a sparger for introducing an oxygen-containing gas at the bottom of the reactor, a stirring turbine blade and a baffle, and a reflux condenser on the vent gas line at the top of the reactor was charged with a mixture of 0.062 g of cuprous oxide and 0.69 g of 47% hydrogen bromide, which had been previously prepared, 0.20 g of N,N'-di-t-butylethylenediamine, 2.81 g of dimethyl-n-butylamine, 1.31 g of di-n-butylamine, 865.0 g of toluene, 72.3 g of 2,6-dimethylphenol, 34.53 g of 2,3,6-trimethylphenol, 23.16 g of 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane, and 0.05 g of trioctylmethylammonium chloride. Next, while vigorously stirring, air was introduced into the reactor from the sparger at a rate of 1.37 L / min, and at the same time, the polymerization temperature was adjusted by passing a heat medium through the jacket so as to maintain it at 20°C. 200 minutes after the start of air introduction, the air was stopped and the inside of the reactor was replaced with nitrogen gas, and then 0.70 g of ethylenediaminetetraacetic acid tetrasodium salt tetrahydrate (a reagent manufactured by Dojindo Laboratories) was added to the polymerization mixture as an aqueous solution of 200 g of water. Further, a mixture of 1.2 g of hydroquinone and 40 g of water was added, and the mixture was kept at 20°C for 1 hour, and the by-product diphenoquinone was reduced, and then the mixture was heated to 70°C and copper extraction was carried out at 70°C for 1 hour. Thereafter, the mixture was separated into an unmodified polyphenylene ether solution (organic phase) and an aqueous phase to which the catalyst metal had been transferred by standing separation. The organic layer was concentrated by an evaporator to obtain unmodified polyphenylene ether in a solid state.
[0103] Example 1 30 g of unmodified polyphenylene ether obtained in Production Example 1 was put into a 500 mL jacketed reactor equipped with a line for introducing nitrogen gas at the top of the reactor, stirring turbine blades and baffles, and a reflux condenser on the vent gas line at the top of the reactor. After replacing the inside of the reactor with nitrogen, 70 g of toluene and 104 g of dimethyl sulfoxide were added to prepare an unmodified polyphenylene ether solution. While stirring, 13.57 g of triethylamine was added using a syringe, and 2.34 g of dimethylaminopyridine was further added. Then, 8.58 g of vinyl methacrylate was collected in a syringe and dropped into the system, and stirring was continued at 110 ° C. for 18 hours. After returning to room temperature, 2.00 g of methanol was added to stop the reaction. Next, the reaction liquid was concentrated until the solid content concentration was 22 mass%, and then the reaction liquid was dropped into 665.06 g of methanol to obtain a precipitate of modified polyphenylene ether. The wet modified polyphenylene ether recovered by filtration under reduced pressure was dissolved again in 180 g of toluene, and 207.01 g of an aqueous sodium hydroxide solution with a pH of 10 was added to perform liquid separation. The organic layer was concentrated to 110 g, and the organic layer was dropped into 567.67 g of methanol to obtain a wet modified polyphenylene ether. The wet modified polyphenylene ether was washed with 200 mL of methanol and vacuum dried at 110° C. for 2 hours to obtain a modified polyphenylene ether. Next, 79 parts by mass of modified polyphenylene ether, 20 parts by mass of TAIC (manufactured by Nippon Kasei Co., Ltd.), and 1 part by mass of organic peroxide (Perbutyl P, manufactured by NOF Corp.) were added to toluene, stirred, and dissolved to obtain a varnish (solid content concentration 58% by mass). L glass cloth (manufactured by Asahi Schwebel Co., Ltd., style: 2116) was impregnated with this varnish, and then passed through a specified slit to scrape off excess varnish, and dried in a drying oven at 105°C for a specified time to remove toluene, thereby obtaining a prepreg. This prepreg was cut to a specified size, and the solid content of the thermosetting composition in the prepreg was calculated by comparing the mass of the prepreg with the mass of a glass cloth of the same size, and was found to be 52% by mass. A predetermined number of these prepregs were stacked, and copper foil (GTS-MP foil, 35 μm thick, manufactured by Furukawa Electric Co., Ltd.) was placed on both sides of the stacked prepregs, and the resulting laminate was vacuum pressed to obtain a copper-clad laminate. In this vacuum pressing process, the laminate was first heated from room temperature at a temperature increase rate of 2°C / min while applying a pressure of 40 kg / cm. 2 After the temperature reached 200°C, the pressure was increased to 40 kg / cm while maintaining the temperature at 200°C. 2 and duration of 60 minutes were adopted. Next, the copper foil was removed from the copper-clad laminate by etching to obtain a laminate (thickness: about 0.5 mm). The analytical results are shown in Table 1.
[0104] Example 2 The same procedure as in Example 1 was carried out except that the solvent for the modification reaction was changed to 136 g of toluene and 34 g of dimethyl sulfoxide, to obtain a modified polyphenylene ether and a laminate. The analytical results are shown in Table 1.
[0105] Example 3 The same procedure as in Example 1 was carried out except that the solvent for the modification reaction was changed to 34 g of toluene and 136 g of dimethyl sulfoxide, to obtain a modified polyphenylene ether and a laminate. The analytical results are shown in Table 1.
[0106] Example 4 30 g of unmodified polyphenylene ether obtained in Production Example 2 was put into a 500 mL jacketed reactor equipped with a line for introducing nitrogen gas at the top of the reactor, stirring turbine blades and baffles, and a reflux condenser on the vent gas line at the top of the reactor. After replacing the inside of the reactor with nitrogen, 70 g of toluene and 104 g of dimethyl sulfoxide were added to prepare an unmodified polyphenylene ether solution. While stirring, 10.62 g of triethylamine was added using a syringe, and 1.83 g of dimethylaminopyridine was further added. Then, 6.72 g of vinyl methacrylate was collected in a syringe and dropped into the system, and stirring was continued at 110°C for 18 hours. The rest of the procedure was the same as in Example 1, to obtain a modified polyphenylene ether and a laminate. The analytical results are shown in Table 1.
[0107] Example 5 The modification reaction was carried out using 4.74 g of scandium triflate without using dimethylaminopyridine or triethylamine. In addition, the modification reaction was carried out using only 192 g of toluene as a solvent. The rest of the procedure was the same as in Example 1, and a modified polyphenylene ether and a laminate were obtained. The analytical results are shown in Table 1.
[0108] Example 6 The modification reaction was carried out using 4.74 g of scandium triflate without using dimethylaminopyridine or triethylamine. In addition, the modification reaction was carried out using 76.8 g of toluene and 115.2 g of dimethyl sulfoxide as a solvent. The rest of the procedure was the same as in Example 1, and a modified polyphenylene ether and a laminate were obtained. The analytical results are shown in Table 1.
[0109] Example 7 The modification reaction was carried out using 4.74 g of scandium triflate without using dimethylaminopyridine or triethylamine. In addition, the modification reaction was carried out using only 192 g of toluene as a solvent. The rest of the procedure was the same as in Example 4, and a modified polyphenylene ether and a laminate were obtained. The analytical results are shown in Table 1.
[0110] Comparative Example 1 A stirrer was placed in a 300 ml three-neck flask, a Dimroth condenser with a three-way cock was installed on the main tube, and a rubber stopper with a thermometer was attached to one side tube. 73.5 g of toluene and 26.0 g of the unmodified polyphenylene ether obtained in Production Example 1 were mixed and heated to about 85°C. 0.33 g of dimethylaminopyridine was added. When it appeared that all the solids had dissolved, 4.2 g of methacrylic anhydride was gradually added. The resulting solution was maintained at 85°C for 3 hours with continuous mixing. The rest of the procedure was the same as in Example 1, to obtain a modified polyphenylene ether and a laminate. The analytical results are shown in Table 1.
[0111] Comparative Example 2 A stirrer was placed in a 300 ml three-neck flask, a Dimroth condenser with a three-way cock was installed on the main tube, and a rubber stopper with a thermometer was attached to one of the side tubes. 73.5 g of toluene and 26.0 g of the unmodified polyphenylene ether obtained in Production Example 2 were mixed and heated to about 85°C. 0.33 g of dimethylaminopyridine was added. When it appeared that all the solids had dissolved, 4.2 g of methacrylic anhydride was gradually added. The resulting solution was maintained at 85°C for 3 hours with continuous mixing. The rest of the procedure was the same as in Example 1, to obtain a modified polyphenylene ether and a laminate. The analytical results are shown in Table 1.
[0112] Comparative Example 3 A stirrer was placed in a 300 ml three-neck flask, a Dimroth condenser with a three-way cock was installed on the main tube, and a rubber stopper with a thermometer was attached to one side tube. 20 g of the unmodified polyphenylene ether composition obtained in Production Example 1 was added from the other side tube, and a rubber stopper was attached. After the inside of the flask was replaced with nitrogen, the mixture was dissolved in 140 g of toluene using a syringe while stirring the inside with a magnetic stirrer, and then 6.32 g of triethylamine was added. Then, 3.27 g of methacryloyl chloride was collected in a syringe and dropped into the system through the rubber stopper. After the dropwise addition, stirring was continued at room temperature for 3 hours, and then the flask was heated in an oil bath to continue the reaction under reflux. Heating was stopped 2 hours after the start of reflux, and after the temperature returned to room temperature, 1.00 g of methanol was added to stop the reaction. Next, the reaction liquid was concentrated until the solid concentration was 20% by weight, and then washed with ion-exchanged water of the same weight as the concentrated liquid. Thereafter, the water bath was removed, and the organic layer was added dropwise to methanol (5 times the weight of the organic layer) with stirring. The precipitate was then filtered, and the residue was vacuum dried at 110° C. for 1 hour to obtain a modified polyphenylene ether composition. The rest of the procedure was the same as in Example 1, to obtain a modified polyphenylene ether and a laminate. The analytical results are shown in Table 1.
[0113] [Table 1]
[0114] As shown in Table 1, in comparison with Comparative Examples 1 to 3, by using the modified polyphenylene ethers of Examples 1 to 7, it was possible to obtain thermosetting compositions of modified polyphenylene ethers with increased glass transition temperatures. [Industrial Applicability]
[0115] The modified polyphenylene ether and thermosetting composition of the present invention have a high glass transition temperature and are therefore industrially valuable as electronic materials.
Claims
1. A modified polyphenylene ether represented by the following formula (1): The number average molecular weight calculated as polystyrene is 500 to 15,000, The modified polyphenylene ether has a methacrylic acid content of 70 ppm or more and less than 200 ppm, a combined content of methacrylic anhydride and vinyl methacrylate of 10 ppm or more and less than 200 ppm, an organic amine catalyst content of 40 ppm or more and less than 200 ppm, and a chloride ion content of 10 ppm or more and less than 1500 ppm, based on the total amount of the modified polyphenylene ether. 【Chemistry 1】 ...Formula (1) (In formula (1), Z is an a-valent partial structure represented by the following formula (2), a represents an integer of 2 to 6, each Y is independently a divalent linking group having a structure represented by the following formula (4), n represents the number of repetitions of Y and each n is independently an integer of 0 to 200, at least one n among the a (-Yn-A) is an integer of 1 or more, and A is a group represented by the following formula (5). 【Chemistry 2】 ...Formula (2) In formula (2), X is an arbitrary linking group having a valence of a, and R 4 is either a linear alkyl group having 1 to 8 carbon atoms or a partial structure represented by the following formula (3), in which the carbon atom of the benzene ring to which -O- is bonded is the 1st position, and -O- is bonded to at least one of the 2nd and 6th carbon atoms, and each k is independently an integer of 1 to 4. 【Chemistry 3】 ...Formula (3) In formula (3), R 11 each independently represents an optionally substituted alkyl group having 1 to 8 carbon atoms; R 12 each independently represents an optionally substituted alkylene group having 1 to 8 carbon atoms; each b independently represents 0 or 1; R 13 is any one of a hydrogen atom, an optionally substituted alkyl group having 1 to 8 carbon atoms, and an optionally substituted phenyl group. 【Chemistry 4】 ...Formula (4) In formula (4), R 21 each independently represents an optionally substituted hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom. 【Chemistry 5】 ...Formula (5) In the above formula (5), R 31 each independently represents a hydrogen atom, a hydroxyl group, a hydrocarbon group having 1 to 30 carbon atoms (e.g., a linear hydrocarbon group, a cyclic hydrocarbon group), an aryl group, an alkoxy group, an aryloxy group, an amino group, or a hydroxyalkyl group; R 32 are each independently a hydrocarbon group having 1 to 30 carbon atoms (e.g., an alkylene group), and s is an integer of 0 to 5.
2. A method for producing a modified polyphenylene ether, comprising a step of reacting an unmodified polyphenylene ether represented by the following formula (8) with an unsaturated compound represented by the following formula (10): 【Chemistry 6】 ...Formula (8) In formula (8), Z is an a-valent partial structure represented by formula (2) below, a represents an integer of 2 to 6, each Y is independently a divalent linking group having a structure represented by formula (4) below, n represents the number of repetitions of Y, each n is independently an integer of 0 to 200, and at least one n among the a (-Y-A) is an integer of 1 or more. 【Chemistry 7】 ...Formula (2) In formula (2), X is an arbitrary linking group having a valence of a, and R 4 is either a linear alkyl group having 1 to 8 carbon atoms or a partial structure represented by the following formula (3), in which the carbon atom of the benzene ring to which -O- is bonded is the 1st position, and -O- is bonded to at least one of the 2nd and 6th carbon atoms, and each k is independently an integer of 1 to 4. 【Chemistry 8】 ...Formula (3) In formula (3), R 11 each independently represents an optionally substituted alkyl group having 1 to 8 carbon atoms; R 12 each independently represents an optionally substituted alkylene group having 1 to 8 carbon atoms; each b independently represents 0 or 1; R 13 is any one of a hydrogen atom, an optionally substituted alkyl group having 1 to 8 carbon atoms, and an optionally substituted phenyl group. 【Chemistry 9】 ...Formula (4) In formula (4), R 21 each independently represents an optionally substituted hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom. 【Chemistry 10】 ...Formula (10) In the above formula (10), R 31 each independently represents a hydrogen atom, a hydroxyl group, a hydrocarbon group having 1 to 30 carbon atoms (e.g., a linear hydrocarbon group, a cyclic hydrocarbon group), an aryl group, an alkoxy group, an aryloxy group, an amino group, or a hydroxyalkyl group; R 32 are each independently a hydrocarbon group having 1 to 30 carbon atoms (e.g., an alkylene group), and s is an integer of 0 to 5.
3. The method according to claim 2, wherein the reaction of the unmodified polyphenylene ether represented by the formula (8) with the unsaturated compound represented by the formula (10) is carried out in the presence of an organic amine catalyst or a Lewis acid catalyst.
4. The method according to claim 3, wherein the reaction of the unmodified polyphenylene ether represented by the formula (8) with the unsaturated compound represented by the formula (10) is carried out in the presence of the organic amine catalyst, and the organic amine catalyst is dimethylaminopyridine.
5. A thermosetting composition comprising the modified polyphenylene ether of claim 1.
6. A prepreg comprising a substrate and the thermosetting composition of claim 5.
7. The prepreg according to claim 6 , wherein the substrate is a glass cloth.
8. A laminate comprising a cured product of the prepreg according to claim 6 or 7 and a metal foil.
Citation Information
Patent Citations
UV-LED photocuring ink-jet ink for glass substrate and preparation method of UV-LED photocuring ink-jet ink
CN112898824A
Chataringukenshutsusochi
JP1976047397A
Ryomensetsuchakushiryonotantaiguntenchakubanto sonoseizohoho
JP1976076336A
Ticket issuing apparatus
JP1979039700A
Resin composition for production of metal-clad laminated board, prepreg, laminate, metal-clad laminated board and multilayer printed wiring board
JP2003119371A