Silicone composite antifouling sheet and graffiti prevention method using same

The silicone composite antifouling sheet, featuring a fluororesin base layer and silicone adhesive layer, addresses the challenges of long-term stability and ease of cleaning by preventing and easily removing graffiti, enhancing surface durability and adhesion to uneven surfaces.

JP7563964B2Active Publication Date: 2024-10-08SHIN ETSU CHEMICAL CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2020205325
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-10
Publication Date
2024-10-08
Estimated Expiration
2040-12-10

AI Technical Summary

Technical Problem

Existing antifouling technologies for surfaces such as bridge piers and walls fail to provide long-term stability, ease of cleaning, and resistance to graffiti, leading to repeated graffiti occurrences and poor workability in removal processes.

Method used

A silicone composite antifouling sheet comprising a fluororesin base material layer with a silicone adhesive layer having a hardness of 5 or less on the Asker C scale and an adhesive strength of 5N/25mm or more, which can be easily applied without a primer and adheres to uneven surfaces, providing long-term antifouling properties and ease of cleaning.

Benefits of technology

The silicone composite antifouling sheet effectively prevents graffiti by reducing the motivation to apply graffiti and allows easy removal, maintaining antifouling properties and cleanability over time, with excellent weather resistance and adhesion to uneven surfaces.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563964000002
    Figure 0007563964000002
  • Figure 0007563964000003
    Figure 0007563964000003
  • Figure 0007563964000004
    Figure 0007563964000004
Patent Text Reader

Abstract

To provide a silicone composite anti-fouling sheet expressing anti-fouling property, washability, easy washability, and abrasion resistance stably for a long period of time, and capable of easily attaching to an adherend, capable of following cracks and shears of a face to be constructed, and a scribble-proof construction method using the same.SOLUTION: A silicone anti-fouling sheet 4 includes a substrate layer 1, and a silicone adhesive layer 2 laminated on one side of the substrate layer, where the substrate layer is composed of a fluorocarbon resin, the silicone adhesive layer has a hardness of 5 or less measured by an Asker C hardness meter, the tack strength to a mortar test piece is 5 N / 25 mm or more, and a surface opposite to a face laminated with the silicone adhesive layer out of surfaces of the substrate layer is an anti-fouling face 7.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a silicone composite antifouling sheet and an anti-graffiti application method using the same. [Background technology]

[0002] The cases of graffiti being painted with oil-based paint on the surfaces of bridge piers, fences, and other structures have become a social problem. Furthermore, this kind of graffiti is not easy to remove, and so removing it requires a great deal of effort and expense.

[0003] There is an increasing demand for the ability to remove graffiti easily and quickly. For example, Patent Document 1 discloses that the surface of the concrete structure to be treated is coated with a primer and an undercoat clear paint, and then a topcoat clear paint that makes it easy to remove graffiti and posters is applied; by doing so, graffiti can be removed by attaching a cloth adhesive tape cut to a specified length to the graffitied surface, rubbing it firmly with one hand, and then forcefully peeling off the cloth adhesive tape.

[0004] However, in order to remove graffiti as described above, it was necessary to apply a piece of packaging cloth adhesive tape cut to a predetermined length to the surface on which the graffiti was stained, rub it firmly with one hand, and then forcefully peel off the packaging cloth adhesive tape, which resulted in poor workability during the graffiti removal work.

[0005] Therefore, in order to make the surfaces of these buildings less susceptible to graffiti, it has been proposed to form anti-pollution coatings by applying paint containing silicone oil or wax to the surfaces or by painting with reactive silicone resin paints (see Patent Documents 2 to 4). Patent Document 5 also proposes a method of spreading a surface treatment agent containing a specific organopolysiloxane on the coating surface of an automobile or the like to form a coating that allows adhered dirt components to be easily removed.

[0006] However, such reactive silicone resin-based paints and surface treatment agents have problems such as a decrease in graffiti prevention performance over time, and when applied thickly by roller coating or brush coating, cracks occur in the coating film over time when drying at room temperature. In addition, although these methods can remove graffiti, they can still graffiti, so there are many cases where graffiti is re-applied after the graffiti is removed. In other words, conventional technologies do not have the function to suppress the "act of graffitiing," and therefore the problem is that graffitiing and removal are repeated. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2005-262134 A [Patent Document 2] Japanese Patent Application Publication No. 6-182290 [Patent Document 3] Japanese Patent Application Publication No. 9-94524 [Patent Document 4] Japanese Patent Application Publication No. 10-216619 [Patent Document 5] JP 2005-97527 A Summary of the Invention [Problem to be solved by the invention]

[0008] As a measure to solve the above problem, it is considered to provide a stain-preventing layer having a stain-preventing surface. However, when considering long-term stain-preventing performance and washability, if the stain-preventing layer has low weather resistance, the stain-preventing performance and washability will gradually decrease, and the sheet will not be able to fully exhibit its functions of preventing graffiti and being easily washable. In addition, general stain-proofing agents have the problem that once stains have been established, they are difficult to clean off with a cloth adhesive tape for packaging, and when the surface is worn down, the stain-proofing properties are lost.

[0009] The present invention has been made in consideration of the above circumstances, and has an object to provide a silicone composite anti-fouling sheet which exhibits stable stain-resistant properties, cleanability, ease of cleaning, and abrasion resistance over the long term, which can be easily attached to an adherend, and which can adapt to cracks and shifts in the surface to which it is applied, and an anti-graffiti application method using the same. [Means for solving the problem]

[0010] In order to solve the above problems, the present invention provides a silicone composite antifouling sheet comprising a base layer and a silicone adhesive layer laminated on one side of the base layer, The silicone composite anti-fouling sheet is characterized in that the base layer is made of a fluororesin, the silicone adhesive layer has a hardness of 5 or less on the Asker C hardness scale and an adhesive strength to a mortar test piece of 5 N / 25 mm or more, and the surface of the base layer opposite the surface on which the silicone adhesive layer is laminated is an anti-fouling surface.

[0011] The silicone composite stain-resistant sheet of the present invention exhibits stain-resistant properties, washability, ease of cleaning, and abrasion resistance that are stable over the long term, and can be easily attached to an adherend and conform to any cracks or shifts in the surface to which it is applied.

[0012] In the present invention, it is preferred that at least the surface of the fluororesin constituting the base layer opposite the antifouling surface be treated to improve anchoring properties.

[0013] Since fluororesin is a poorly adhesive material, when laminating fluororesin and other layers, such as a silicone adhesive layer, it is preferable that the side of the fluororesin surface to be laminated (the surface opposite the antifouling surface) is treated to improve anchoring properties. If such a treatment is performed, the fluororesin layer can be easily laminated to the other layer.

[0014] In the present invention, it is further preferable that the base layer contains a reinforcing material.

[0015] Some fluororesins are very flexible and easily deformed, but if the base layer contains a reinforcing material, such deformation is less likely to occur.

[0016] It is also preferable that a reinforcing layer is further laminated between the base layer and the silicone adhesive layer.

[0017] Such a reinforcing material layer supports the base layer, so that dents are less likely to occur in the base layer.

[0018] In this case, it is preferable that the base material layer and the reinforcing material layer are laminated via an adhesive layer having UV resistance.

[0019] This can improve UV resistance.

[0020] It is also preferable that the reinforcing layer includes a PET film.

[0021] Such materials are advantageous in terms of cost, ease of availability, and ease of surface treatment, making them suitable.

[0022] In the present invention, it is preferable that at least one of the layers has a light reflection suppressing effect.

[0023] Such a material can suppress optical glare and light reflection on the silicone composite stain-resistant sheet, thereby preventing dazzling of nearby passersby.

[0024] In the present invention, it is preferable that the thickness of the base layer is 0.05 to 0.3 mm, the thickness of the adhesive layer is 0.5 to 3 mm, and the thickness of the entire silicone composite stain-resistant sheet is 0.55 to 3.3 mm.

[0025] Such a material has good adhesion and physical strength, and is also advantageous in terms of cost.

[0026] The silicone composite stain-resistant sheet is preferably for preventing graffiti.

[0027] Such a silicone composite stain-resistant sheet can be very suitably used for preventing graffiti.

[0028] The present invention also provides an anti-graffiti construction method, characterized in that the silicone adhesive layer of the above-mentioned silicone composite anti-fouling sheet is attached to a desired adherend, and the anti-fouling surface made of the fluororesin of the base material layer is exposed, thereby preventing graffiti on the adherend.

[0029] With this method, the silicone composite stain-resistant sheet of the present invention can be used for application without the need for a primer. Therefore, even if moisture remains on the adhesive surface, application can be completed by simply wiping it off thoroughly with a rag or the like, and application can begin immediately after the weather improves. Effect of the Invention

[0030] In the silicone composite stain-resistant sheet of the present invention, the surface of the substrate layer opposite to the surface on which the silicone adhesive layer is laminated is a stain-resistant surface, and the substrate layer is made of a fluororesin, so that it is possible to prevent people who would like to do graffiti from making the desired drawings. Furthermore, this effect can discourage people who would like to do graffiti, and thus it is possible to suppress the act of graffiti itself. Furthermore, even if graffiti is done, it can be easily washed and removed due to the fluororesin.

[0031] Furthermore, since the surface of the silicone composite stain-resistant sheet is made of a fluororesin, it has good weather resistance and can stably maintain its stain-resistant properties, washability, and ease of cleaning for a long period of time.

[0032] In addition, the laminated silicone adhesive layer can be easily attached to the adherend and can follow cracks, misalignments, unevenness, etc. of the applied surface. Since silicone is the main component, it has excellent weather resistance, heat resistance, and cold resistance, and can maintain its function for a longer period of time. Furthermore, since the silicone adhesive layer has a waterproof effect, it is possible to prevent moisture from entering the applied area and prevent deterioration of the applied object or significantly delay the progression of deterioration. [Brief description of the drawings]

[0033] [Figure 1] FIG. 1 is a schematic diagram showing an example of a silicone composite stain-resistant sheet of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing another example of the silicone composite stain-resistant sheet of the present invention. [Diagram 3] FIG. 2 is a schematic diagram showing yet another example of the silicone composite stain-resistant sheet of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0034] As described above, there has been a demand for the development of a silicone composite stain-resistant sheet that exhibits stable stain-resistant properties, cleanability, and ease of cleaning over the long term, that can be easily attached to an adherend, and that can adapt to cracks and shifts in the surface to which it is applied, as well as an anti-graffiti application method using the same.

[0035] As a result of extensive investigations into the above-mentioned problems, the inventors have discovered that a silicone composite stain-resistant sheet can be obtained by laminating a silicone adhesive layer, which has a hardness of 5 or less on an Asker C hardness scale and an adhesive strength of 5 N / 25 mm or more to a mortar test piece, on one side of a base layer, wherein the base layer is made of a fluororesin, which exhibits stable stain-resistant properties, washability and ease of cleaning over the long term, and which can be easily attached to an adherend and can adapt to cracks or shifts in the surface to which it is applied, and have completed the present invention.

[0036] That is, the present invention is a silicone composite anti-fouling sheet comprising a base layer and a silicone adhesive layer laminated on one side of the base layer, wherein the base layer is made of a fluororesin, the silicone adhesive layer has a hardness of 5 or less on the Asker C hardness scale and an adhesive strength to a mortar test piece of 5 N / 25 mm or more, and the surface of the base layer opposite the side on which the silicone adhesive layer is laminated is a stain-resistant surface.

[0037] The present invention also relates to an anti-graffiti construction method, which comprises attaching the silicone adhesive layer of the above-mentioned silicone composite anti-fouling sheet to a desired adherend and exposing the anti-fouling surface made of fluororesin of the base material layer, thereby preventing graffiti on the adherend.

[0038] The present invention will be described in detail below, but the present invention is not limited thereto.

[0039] <Silicone composite anti-stain sheet> The silicone composite stain-resistant sheet of the present invention comprises a base layer and a silicone adhesive layer laminated on one side of the base layer, the base layer being made of a fluororesin, the silicone adhesive layer having a hardness of 5 or less on the Asker C hardness scale and an adhesive strength to a mortar test piece of 5 N / 25 mm or more, and the surface of the base layer opposite the side on which the silicone adhesive layer is laminated is an anti-stain surface. The silicone composite antifouling sheet of the present invention can further include, in addition to the above-mentioned substrate layer and silicone adhesive layer, a reinforcing material layer, a protective layer, etc., as described below. In the following, of the various layers constituting the silicone composite antifouling sheet of the present invention, the layers other than the silicone adhesive layer are collectively referred to as "antifouling layers".

[0040] In such a silicone composite antifouling sheet, the surface opposite to the surface on which the silicone adhesive layer is laminated is an antifouling surface with exposed fluororesin, so that it is possible to prevent people who would like to do graffiti from drawing what they want. In addition, this effect makes it possible to discourage people who would like to do graffiti, thereby suppressing the act of graffiti itself. In addition, even if graffiti is done, it is possible to easily wash and remove the graffiti due to the fluororesin. Furthermore, by forming the base layer itself from a fluororesin, the surface of the silicone composite sheet becomes a fluororesin, and the antifouling properties, washability, ease of cleaning, and abrasion resistance are stably maintained for a long time.

[0041] In addition, the silicone adhesive layer laminated on the base layer can be easily attached to the adherend, and can follow cracks, misalignments, unevenness, and other issues on the surface to be applied. Since silicone is the main component, it has excellent weather resistance, heat resistance, and cold resistance, and can maintain its function for a longer period of time. Furthermore, since the silicone adhesive layer has a waterproof effect, it is possible to prevent moisture from entering the applied area, and to prevent deterioration of the applied object or to significantly delay the progression of deterioration. The physical properties of the silicone adhesive layer will be described later.

[0042] Furthermore, in order to significantly shorten the construction period, it is necessary to use a type that is already in sheet form before the work, rather than a type that is cured at the work site. From this point of view, the silicone composite antifouling sheet of the present invention has a multilayer structure consisting of a base layer and a silicone adhesive layer molded (laminated) on one side of the base layer, and can be stored for a long time, has a long usable life, and can be easily applied, which makes it possible to shorten the construction period. It is preferable that the silicone adhesive layer of the silicone composite antifouling sheet of the present invention is protected by a cover film (protective layer) when not in use or until immediately before use.

[0043] The silicone adhesive layer and the substrate layer contained in the silicone composite stain-resistant sheet of the present invention will be described below.

[0044] [Silicone adhesive layer] The silicone adhesive layer that constitutes the silicone composite stain-resistant sheet of the present invention is not particularly limited as long as it has a hardness of 5 or less on the Asker C hardness scale and an adhesive strength to a mortar test piece of 5 N / 25 mm or more. However, it is preferable that it has the following characteristics.

[0045] The silicone composition that can be used in the silicone adhesive layer that constitutes the silicone composite stain-resistant sheet of the present invention comprises the following components (A) to (D): (A) an organopolysiloxane containing, in each molecule, at least two alkenyl groups bonded to silicon atoms; (B)R 2 3SiO 1 / 2 Units (wherein R 2 is an unsubstituted or substituted monovalent hydrocarbon group, while R 2 an alkenyl group-containing resinous copolymer mainly composed of an SiO2 unit and an alkenyl group-containing copolymer (note that, although component (B) is preferably contained in the composition, it may be 0 part by mass); (C) an organohydrogenpolysiloxane containing at least two hydrogen atoms bonded to silicon atoms (SiH groups) per molecule; (D) an addition reaction catalyst; It is preferable that the silicone adhesive layer is formed from a cured product of the addition-curable silicone composition, which contains the above-mentioned formula (I) and has surface adhesion. The above components (A) to (D) will be described in more detail below.

[0046] [Component (A)] The component (A) of the addition-curable silicone composition is an organopolysiloxane having at least two alkenyl groups in one molecule, and the organopolysiloxane of component (A) is represented by the following average composition formula (I): R 1 a SiO (4-a) / 2 (I) can be used.

[0047] In the formula, R 1are the same or different, and are unsubstituted or substituted monovalent hydrocarbon groups, preferably having 1 to 10 carbon atoms, more preferably 1 to 8 carbon atoms, and a is a positive number preferably in the range of 1.5 to 2.8, more preferably 1.8 to 2.5, and even more preferably 1.95 to 2.05. 1 Examples of the unsubstituted or substituted monovalent hydrocarbon group bonded to a silicon atom represented by the formula (I) include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, neopentyl, hexyl, cyclohexyl, octyl, nonyl, and decyl; aryl groups such as phenyl, tolyl, xylyl, and naphthyl; aralkyl groups such as benzyl, phenylethyl, and phenylpropyl; alkenyl groups such as vinyl, allyl, propenyl, isopropenyl, butenyl, hexenyl, cyclohexenyl, and octenyl; and groups in which some or all of the hydrogen atoms of these groups have been substituted with halogen atoms such as fluorine, bromine, and chlorine, or with cyano groups, for example, chloromethyl, chloropropyl, bromoethyl, trifluoropropyl, and cyanoethyl. 1 It is preferable that 90 mol % or more of the groups are methyl groups.

[0048] In this case, in the above component (A), R 1 At least two of the organic groups R in one molecule are alkenyl groups (preferably having 2 to 8 carbon atoms, more preferably having 2 to 6 carbon atoms). The content of alkenyl groups is calculated based on the total organic groups R 1 (i.e., the above-mentioned unsubstituted or substituted monovalent hydrocarbon group), it is preferably 0.00001 to 0.05 mol / g, and more preferably 0.00001 to 0.01 mol / g. The alkenyl group may be bonded to a silicon atom at the molecular chain end, to a silicon atom in the middle of the molecular chain, or to both, but it is preferable that the alkenyl group contains at least an alkenyl group bonded to a silicon atom at both molecular chain ends. If the alkenyl group content is 0.00001 mol / g or more, sufficient rubber properties are obtained, and if it is 0.05 mol / g or less, the hardness is not too high and sufficient adhesion is maintained.

[0049] The degree of polymerization is not particularly limited, but it is preferably liquid at room temperature. In general, the average degree of polymerization, calculated as polystyrene by gel permeation chromatography (GPC), is preferably 50 to 20,000, more preferably 100 to 10,000, and even more preferably about 100 to 2,000.

[0050] The structure of the organopolysiloxane of component (A) is basically such that the main chain is made up of diorganosiloxane units (R 1 2SiO 2 / 2 ) repeating units, and both ends of the molecular chain are triorganosiloxy groups (R 1 3SiO 1 / 2 ) or hydroxydiorganosiloxy group ((HO)R 1 2SiO 1 / 2 ) is preferably a linear structure terminated with , but it may also be a partially branched structure, cyclic structure, or the like.

[0051] [(B) Component] The resin copolymer of component (B) (i.e., a copolymer having a three-dimensional network structure) is R 2 3SiO 1 / 2 The main components are SiO2 units and SiO2 units. Here, R 2 is an unsubstituted or substituted monovalent hydrocarbon group (including an alkenyl group), preferably having 1 to 10 carbon atoms, particularly preferably 1 to 8 carbon atoms; R 2Examples of the monovalent hydrocarbon group represented by the formula (I) include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, neopentyl, hexyl, cyclohexyl, octyl, nonyl, and decyl; aryl groups such as phenyl, tolyl, xylyl, and naphthyl; aralkyl groups such as benzyl, phenylethyl, and phenylpropyl; alkenyl groups such as vinyl, allyl, propenyl, isopropenyl, butenyl, hexenyl, cyclohexenyl, and octenyl; and groups in which some or all of the hydrogen atoms of these groups have been substituted with halogen atoms such as fluorine, bromine, and chlorine, or with cyano groups, for example, chloromethyl, chloropropyl, bromoethyl, trifluoropropyl, and cyanoethyl.

[0052] The resin copolymer of component (B) is 2 3SiO 1 / 2 units and SiO2 units, and may be, if necessary, 2 2SiO units and R 2 SiO 3 / 2 Units (R 2 The total amount of these may be preferably 50% or less, more preferably 40% or less, based on the total copolymer mass. 2 3SiO 1 / 2 The molar ratio of units to SiO2 units (R 2 3SiO 1 / 2 / SiO2) is preferably 0.5 to 1.5, and particularly preferably 0.5 to 1.3. If this molar ratio is within the above range, sufficient rubber hardness and strength can be obtained.

[0053] Furthermore, the resin copolymer of component (B) has an alkenyl group, preferably at least two alkenyl groups in one molecule, and the content of the alkenyl group is preferably 0.0001 mol / g or more, more preferably in the range of 0.0001 to 0.001 mol / g. If the content of the alkenyl group is 0.0001 mol / g or more, sufficient rubber properties are obtained, and if it is 0.001 mol / g or less, the hardness becomes appropriate and the adhesive force is more reliably maintained.

[0054] The resinous copolymer of component (B) may be a liquid having fluidity at room temperature (25°C) (e.g., 10 mPa·s or more, preferably 50 mPa·s or more), or a solid having no fluidity. If it is a solid, it may be dissolved in an organic solvent such as toluene. This resinous copolymer can usually be produced by hydrolyzing an appropriate chlorosilane or alkoxysilane by a method well known in the art.

[0055] The blending amounts of the above (A) and (B) components are preferably 20 to 100 parts by mass, more preferably 20 to 90 parts by mass, and particularly preferably 30 to 90 parts by mass, when the total of the (A) and (B) components is taken as 100 parts by mass, and the blending amount of the (A) component is preferably 0 to 80 parts by mass, more preferably 10 to 80 parts by mass, and particularly preferably 10 to 70 parts by mass. When the blending amounts of the (A) and (B) components are within the above ranges, the rubber physical properties are good. From the viewpoints of adhesion and strength, it is preferable to use the (B) component in combination with the (A) component.

[0056] [(C) component] Component (C) is an organohydrogenpolysiloxane having at least two, and preferably three or more, hydrogen atoms bonded to silicon atoms (SiH groups) in each molecule. The SiH groups in the molecule crosslink with the alkenyl groups bonded to silicon atoms in components (A) and (B) via a hydrosilylation addition reaction, and act as a curing agent for curing the composition.

[0057] The organohydrogenpolysiloxane of component (C) is represented by the following average composition formula (II): R 3 b H c SiO (4-b-c) / 2 (II) (In the formula, R 3 is an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms. In addition, b is a positive number that satisfies 0.7 to 2.1, c is a positive number that satisfies 0.001 to 1.0, and b+c is a positive number that satisfies 0.8 to 3.0. The compound represented by the formula (I) can be used, and preferably has at least 2 (usually 2 to 200), preferably 3 to 100, more preferably 3 to 50 silicon-bonded hydrogen atoms in one molecule. 3 As the monovalent hydrocarbon group, R 1 Examples of the organohydrogenpolysiloxane include those similar to those exemplified in 1., but those having no aliphatic unsaturated groups are preferred. Furthermore, b is preferably 0.8 to 2.0, c is preferably 0.01 to 1.0, and b+c is preferably 1.0 to 2.5, and the molecular structure of the organohydrogenpolysiloxane may be any of linear, cyclic, branched, and three-dimensional network structures.

[0058] In this case, the number of silicon atoms (or degree of polymerization) in one molecule is preferably 2 to 300, and particularly preferably about 4 to 150, which is liquid at room temperature (25°C). The hydrogen atoms bonded to the silicon atoms may be located either at the molecular chain end or in the middle of the molecular chain, or may be located at both ends, but those at the molecular chain end, which has a faster reaction rate, are preferred. That is, methylhydrogenpolysiloxane capped with trimethylsiloxy groups at both ends, dimethylsiloxane-methylhydrogensiloxane copolymer capped with trimethylsiloxy groups at both ends, dimethylpolysiloxane capped with dimethylhydrogensiloxy groups at both ends, dimethylsiloxane-methylhydrogensiloxane copolymer capped with dimethylhydrogensiloxy groups at both ends, (CH3)2HSiO 1 / 2 Units and SiO 4 / 2 A copolymer consisting of (CH3)2HSiO units. 1 / 2 Units and SiO 4 / 2 Units and (C6H5)SiO 3 / 2 and copolymers consisting of units.

[0059] The amount of the organohydrogenpolysiloxane of the (C) component is preferably 0.5 to 20 parts by mass, and more preferably 1.0 to 10 parts by mass, per 100 parts by mass of the total of the (A) and (B) components. If the amount is within this range, sufficient rubber strength can be obtained. In addition, the organohydrogenpolysiloxane of the (C) component is preferably blended in such an amount that the molar ratio of the amount of hydrogen atoms (SiH groups) bonded to silicon atoms in the (C) component to the amount of alkenyl groups bonded to silicon atoms contained in the (A) and (B) components is 0.5 to 1.1, and more preferably 0.6 to 1.0. In addition, it is preferable to blend an amount of organohydrogen of 0.005 to 0.010 mol / g, assuming that 100% addition crosslinking reaction proceeds.

[0060] Here, the molar ratio of the SiH group of the (C) component to the amount of alkenyl groups present in the system is represented as H / Vi. The theoretical crosslinking amount below refers to the amount of crosslinking when hydrogen atoms (SiH groups) bonded to silicon atoms in the (C) component added to the system react 100% with the alkenyl groups present in the system. That is, when H / Vi is 1 or less, the amount of SiH groups is the theoretical crosslinking amount, and when H / Vi is 1 or more, the amount of alkenyl groups is the theoretical crosslinking amount. These amounts of functional groups may be amounts based on a calculation formula when designing the composition, but it is more preferable to use actual measured values. The amount of functional groups can be measured by a known analytical method, such as measuring the amount of hydrogen gas generated or unsaturated groups, or analyzing by NMR. The amount of functional groups in the system is represented by X×Y mol / g when the amount of functional groups in the molecule is X mol / g and the amount added is Y parts by mass.

[0061] [(D) component] Component (D) may be any of the conventionally known catalysts, and typically contains a platinum group metal-based addition reaction catalyst such as platinum or a platinum compound (usually 1 to 1,000 ppm by metal mass relative to the total alkenyl-containing organopolysiloxane of components (A) and (B)).

[0062] [Other ingredients] In addition to the above-mentioned components, the composition forming the silicone adhesive layer may contain, as necessary, other components such as fillers such as fumed silica, precipitated silica, quartz powder, diatomaceous earth, and calcium carbonate, conductive agents such as carbon black, conductive zinc oxide, and metal powder, and heat-resistant agents such as iron oxide and cerium oxide. Furthermore, it is optional to add hydrosilylation reaction inhibitors such as nitrogen-containing compounds, acetylene compounds, phosphorus compounds, nitrile compounds, carboxylates, tin compounds, mercury compounds, and sulfur compounds, internal release agents such as dimethyl silicone oil, adhesion imparting agents, and thixotropy imparting agents.

[0063] [Physical properties of silicone adhesive layer] Next, the physical properties of the silicone adhesive layer contained in the silicone composite stain-resistant sheet of the present invention will be described.

[0064] The hardness of the silicone adhesive layer of the present invention is preferably 5 or less on the Asker C hardness scale, which is less than the hardness of the base layer, more preferably 2 or less, and even more preferably 1 or less. If the Asker C hardness exceeds 5, the adhesiveness decreases. The lower limit is 0.

[0065] It is also preferable to measure the hardness of the silicone adhesive layer using an Asker CSR-2 hardness scale, which can reduce measurement variability and more reliably evaluate the hardness of the silicone adhesive layer even when the hardness is in the range of less than 1 on the Asker C hardness scale.

[0066] That is, the hardness of the silicone adhesive layer is preferably smaller than the hardness of the base layer, and the hardness measured with a CSR-2 hardness tester (manufactured by Kobunshi Keiki Co., Ltd.) is preferably a positive number of 50 or less, more preferably a positive number in the range of 10 or more and 20 or less.

[0067] This CSR-2 hardness tester is suitable for measuring hardness in the range of less than 1 on the Asker C hardness scale. The sense of hardness in this range is the level of hardness at which the adhesive surface follows the finger when the finger is touched with the adhesive surface and then slowly removed from the adhesive surface. The greater the adhesive strength, the more advantageous it is to make the adhesive layer lower in hardness. Furthermore, if the hardness is 3 or more on the CSR-2 hardness tester, when the silicone composite antifouling sheet is applied, even if the surface to be adhered is a porous material such as asphalt or mortar, the hardness is sufficient and the adhesive layer does not wash away. Furthermore, the workability of the application process does not decrease significantly. Furthermore, if the CSR-2 hardness is 20 or less, the adhesive strength is sufficiently large and the adhesiveness to the surface to be adhered is sufficient, which is preferable. The hardness of the silicone adhesive layer can be easily controlled by controlling the molding and curing conditions described below.

[0068] As an index of adhesion, the adhesive strength to a mortar test piece is shown. A sheet prepared by the molding method described below is cut to a width of 25 mm on a mortar test piece (manufactured by Engineering Test Service Co., Ltd., manufactured in accordance with JIS R5201, width 50 mm x length 150 mm x thickness 10 mm), and the adhesive layer side of the sheet is adhered to the mortar test piece. After leaving it at room temperature for 30 minutes, a 180° peel test is performed at a peeling speed of 300 mm / min. The silicone adhesive layer contained in the silicone composite antifouling sheet of the present invention has an adhesive strength of 5 N / 25 mm or more at this time, preferably 5 to 30 N / 25 mm, and particularly preferably 10 to 25 N / 25 mm. As a guideline for adhesive strength, if it is less than 5 N / 25 mm against a mortar test piece, it will easily peel off with a light force when trying to peel it off by hand, but if it is 5 N / 25 mm or more, it will not easily peel off by hand.

[0069] [Base material layer] The substrate layer included in the silicone composite stain-resistant sheet of the present invention is made of a fluororesin, and the surface of the substrate opposite to the side on which the silicone adhesive layer is laminated serves as an anti-stain surface having stain-preventing properties.

[0070] Since the stain-resistant surface is made of fluororesin, it is possible to impart the silicone composite stain-resistant sheet with the effect of repelling either water-based or oil-based paint, or both. This effect makes it possible to restrain graffiti artists from creating the desired drawings, and to reduce their motivation to engage in graffiti activities. In addition, graffiti can be easily removed by washing with water or cleaning with a solvent, or by wiping, and it is possible to easily restore the surface to the state before the graffiti was created.

[0071] By using a fluororesin that has both water- and oil-repellent properties as the base layer itself, it is possible to maintain the anti-fouling function stably for a long period of time. Furthermore, because fluororesin has extremely high weather resistance, deterioration of the base layer can be prevented even when exposed to sunlight during outdoor use, and it is also possible to suppress a decrease in anti-graffiti performance and wear of the base layer when repeatedly washed.

[0072] In the present invention, the substrate layer itself is made of a fluororesin, and does not include a substrate layer that is not a fluororesin and has a fluororesin formed thereon by coating with a surface treatment agent, etc. For example, a reinforcing layer coated with a fluororesin, as described below, is outside the scope of the present invention.

[0073] The fluororesin used in the substrate layer is not particularly limited, but is preferably PTFE (polytetrafluoroethylene), ETFE (ethylene-tetrafluoroethylene copolymer), PFA (perfluoroalkoxyalkane), or FEP (perfluoroethylenepropene copolymer), and more preferably PTFE. These resins have high antifouling performance and washability among fluororesins, and therefore can further enhance the antifouling effect.

[0074] The substrate layer is preferably in the form of a film or sheet, which is advantageous in terms of cost because it can be continuously processed when laminating the silicone adhesive layer.

[0075] Examples of fluororesins include Skyd Tape MSF and Chukoh Flow Fabric FGF manufactured by Chukoh Chemical Industries, Ltd.

[0076] Since the fluororesin is a poorly adhesive material, when laminating with another layer that is laminated with the fluororesin, such as a silicone adhesive layer, it is preferable that the surface of the fluororesin to be laminated is treated to improve anchoring properties.Specific examples of such treatments include etching, corona treatment, EB treatment, plasma treatment, sand mat treatment, etc., but are not limited to these as long as they improve anchoring properties.

[0077] [Reinforcement, Reinforcement Layer] The present invention can also provide a silicone composite antifouling sheet in which a reinforcing material is contained in the base material layer, or a silicone composite antifouling sheet in which a reinforcing material layer, which will be described later, is further laminated between the base material layer and the silicone adhesive layer.

[0078] Some fluororesins are very flexible, and in film or sheet form, they can easily deform with even a small amount of pressure. Therefore, even the pressure applied during construction or when cleaning graffiti can cause dents, which can accumulate dirt and require cleaning. Therefore, it is preferable to reinforce the material with a reinforcing material such as a film, fabric, or metal plate to prevent deformation.

[0079] The fluororesin can be reinforced by impregnation, melt adhesion, adhesive processing, etc., but any processing method can be used as long as the reinforcing effect is achieved. In addition, the material, shape, and mode of compounding with the fluororesin of the reinforcing material are not particularly limited as long as the reinforcing effect is achieved. Examples of the compounding mode include glass cloth or aramid cloth impregnated with a fluororesin dispersion and baked, and extrusion molding or compression molding of the fluororesin together with the reinforcing material. The shape of the reinforcing material varies depending on the processing method, and examples include plate, film, net, woven fabric, and fiber. A layered reinforcing material is also called a reinforcing material layer.

[0080] In addition, when a reinforcing material layer is laminated for reinforcement, it is preferable to use an adhesive layer containing a UV-resistant compound for bonding the reinforcing material layer and the fluororesin (base material layer). In this case, deterioration of the adhesive layer can be prevented or significantly delayed, and the fluororesin and the reinforcing material layer can be stably bonded for a long period of time. Furthermore, it is more preferable that the reinforcing material is treated to be UV-resistant. Specifically, examples of such a reinforcing material include a material having a UV-resistant agent kneaded into it and a film that has been treated to be UV-resistant.

[0081] Furthermore, the reinforcing layer is preferably a film having a surface roughness Ra of 0.00 to 1.00 μm that is bonded to the fluororesin film so that the surface of the fluororesin film is smooth. As the film, in consideration of cost, availability, ease of surface treatment, etc., it is preferable to use a PEN film, a PC film, a PEEK film, a PET film, etc., and among these, it is more preferable to use a PET film.

[0082] Several embodiments of the silicone composite stain-resistant sheet of the present invention will now be described.

[0083] In the silicone composite stain-resistant sheet of the present invention, it is preferable that one or more of the layers constituting the silicone composite stain-resistant sheet, such as the substrate layer, reinforcing material layer, and silicone adhesive layer, have a light reflection suppressing effect. By having a light reflection suppressing effect, optical reflection and light reflection on the composite stain-resistant sheet can be suppressed, and dazzling of nearby passersby can be prevented.

[0084] Methods for imparting the light reflection suppressing effect include kneading a filler into the base layer, reinforcing material layer, or adhesive layer, or bonding the base layer and reinforcing material layer together using an adhesive containing a filler.

[0085] Regarding the thickness of the silicone composite stain-resistant sheet, the thickness of the base layer (the total thickness of the reinforcing layer, if any) is preferably 0.05 to 0.3 mm, the thickness of the adhesive layer is preferably 0.5 to 3 mm, and the thickness of the entire composite sheet is preferably 0.55 to 3. 3It is preferable that the thickness is mm.

[0086] If the combined thickness of the base layer and the reinforcing layer is 0.05 mm or more, the silicone composite stain-resistant sheet will have sufficient rigidity, and will have good adhesion and physical strength. If the combined thickness is 0.3 mm or less, the rigidity will be adequate, making it easy to apply to curved surfaces. It will also be cost-effective.

[0087] Furthermore, if the thickness of the fluororesin that forms the base layer is too thin, the abrasion resistance decreases, whereas if it is too thick, the cost increases, so the thickness is preferably 0.01 mm to 0.10 mm.

[0088] The thickness of the silicone adhesive layer is preferably in the range of 0.5 to 3 mm, more preferably in the range of 0.5 to 2 mm. If it is 0.5 mm or more, the silicone adhesive layer can more reliably absorb the surface irregularities of the part to be attached, and if it is 3 mm or less, the rubber strength of the attachment surface depends less on the adhesive layer, so that the rubber does not break.

[0089] The silicone composite stain-resistant sheet as described above is preferably used for preventing graffiti. Such a silicone composite stain-resistant sheet can be suitably used for preventing graffiti.

[0090] [Silicone composite antifouling sheet molding method] The method for forming the silicone composite antifouling sheet of the present invention will be described below, however, the method for forming the silicone composite antifouling sheet of the present invention is not limited to the method described below.

[0091] First, a fluororesin film as a base layer and a PET film as a reinforcing layer are laminated together by various methods such as dry lamination, wet lamination, adhesive processing, etc. to form an antifouling layer. If necessary, it is more preferable to subject the fluororesin film to a treatment for improving anchoring properties or an antireflection treatment, and it is more preferable to subject the PET film to a UV-resistant treatment or an antireflection treatment.

[0092] When laminating the silicone adhesive layer on the antifouling layer, a silicone composite antifouling sheet can be obtained by dipping, coating, screen printing, etc., of the silicone adhesive layer on the antifouling layer, but coating molding is preferred because it is easy to use. The curing conditions are preferably in the range of 80 to 250°C and 10 seconds to 1 hour. Furthermore, for the purpose of removing low molecular weight components and improving the strength of the film, it may be aged at room temperature to 40°C for about 1 to 7 days, or after-cured at 60°C to 150°C for about 10 to 60 minutes.

[0093] Next, specific examples of the silicone composite stain-resistant sheet of the present invention will be described with reference to the drawings.

[0094] An example of the silicone composite antifouling sheet of the present invention is shown in FIG. 1. The silicone composite antifouling sheet 4 shown in FIG. 1 is formed by laminating a silicone adhesive layer 2 on a substrate layer 1 made of a fluororesin. In this case, the substrate layer 1 corresponds to the antifouling layer 6. The surface of the substrate layer 1 opposite to the surface on which the silicone adhesive layer 2 is laminated is the antifouling surface 7. This silicone composite antifouling sheet 4 has a simple and long-term adhesive reliability, prevents the infiltration of moisture, and is effectively used to prevent deterioration of the target object or to make it difficult for deterioration over time to progress by attaching the adhesive layer in a liquid-tight manner so as to cover at least a part of the frame made of a concrete structure, a mortar structure, a metal structure, or the like.

[0095] FIG. 2 shows a schematic diagram of another example of the silicone composite antifouling sheet of the present invention. The explanation of FIG. 1 will be omitted. The silicone composite antifouling sheet 4 shown in FIG. 2 is a sheet in which a reinforcing material layer 3 is laminated between a substrate layer 1 whose surface is made of a fluororesin and a silicone adhesive layer 2. In this case, the substrate layer 1 and the reinforcing material layer 3 correspond to the antifouling layer 6. The reinforcing material layer 3 may be laminated on the surface of the substrate layer 1 that has been subjected to the anchoring property improvement treatment (the surface opposite to the antifouling surface 7), and the silicone adhesive layer 2 may be laminated on the reinforcing material layer 3. The substrate layer 1 and the reinforcing material layer 3 may be laminated via an adhesive layer not shown, and it is preferable that the substrate layer and the reinforcing material layer are laminated via an adhesive layer having UV resistance. In this embodiment, the reinforcing material layer 3 imparts physical properties to the silicone composite antifouling sheet 4 so that it has high strength, and further has the effect of preventing graffiti or facilitating the removal of graffiti in the long term, and can stably exhibit antifouling properties.

[0096] Yet another example of the silicone composite antifouling sheet of the present invention is shown diagrammatically in Figure 3. The silicone composite antifouling sheet 4 shown in Figure 3 has a base layer 1 containing a reinforcing material 5. In this case, the base layer 1 containing the reinforcing material 5 corresponds to the antifouling layer 6. Even in this embodiment, the reinforcing material 5 gives the silicone composite antifouling sheet 4 high strength, and the above-mentioned effects are achieved, allowing the sheet to exhibit stable antifouling properties.

[0097] Thus, the silicone composite stain-resistant sheet of the present invention is particularly excellent for preventing graffiti.

[0098] <Graffiti prevention construction method> The graffiti prevention application method of the present invention is characterized in that the silicone adhesive layer of the silicone composite anti-fouling sheet of the present invention is attached to a desired substrate, and the anti-fouling surface (anti-fouling treated surface) made of the fluororesin of the base material layer is exposed, thereby preventing graffiti on the substrate.

[0099] The silicone composite stain-resistant sheet of the present invention described above can be used for anti-graffiti work by attaching the adhesive layer to an object (adherend). One example of the method for this is now described.

[0100] The silicone composite stain-resistant sheet may be attached by pretreating the part of the adherend to make it easier to attach the sheet, but since the silicone composite stain-resistant sheet itself is adhesive, pretreating the part is not necessarily required. The sheet is attached with the silicone adhesive layer, which is the adhesive surface of the silicone composite stain-resistant sheet, as the attachment side. If it is expected that a step will occur at the boundary part of the adherend surface and excessive stress will be applied to the attachment surface, it is preferable to implement a measure to eliminate the step. For example, a method of using a back-up material for the step.

[0101] It is not necessary to use a sealant when attaching the silicone composite antifouling sheet, but in order to attach it more firmly or to simultaneously impart a waterproof function, a sealant may be used at the boundary of the sheet. There is no particular restriction on the sealant, and any of the known silicone, polysulfide, polyurethane, etc. may be used, but a silicone sealant is preferably used in terms of its affinity with the silicone composite sheet material of the present invention. As such a sealant, a commercially available product may be used, and for example, the silicone sealant may be Sealant Master 300, Sealant 70, Sealant 701, etc., manufactured by Shin-Etsu Chemical Co., Ltd.

[0102] In the anti-graffiti application method of the present invention, by using the adhesive silicone composite stain-resistant sheet of the present invention, application without the use of a primer is possible, enabling a significant reduction in construction time.

[0103] In many conventional methods, a paint containing silicone oil or wax is applied to the surface of a building, or a reactive silicone resin paint is applied to form a stain-preventive coating, or an antifouling film is attached with a primer, but there are problems with this, such as being unable to apply the film until the application surface dries due to temperature differences caused by climate, or weather conditions, particularly rain and snow, which cause a lot of moisture and condensation. By using the silicone composite antifouling sheet of the present invention, application is possible without a primer, so even if moisture remains on the adhesive surface, application can be started simply by wiping it off thoroughly with a rag, and the sheet has the revolutionary feature of being able to start application immediately after the weather improves.

[0104] The silicone composite antifouling sheet of the present invention exerts its adhesion and shape-retaining functions by its own adhesive power, so it can be peeled off after use without damaging the adherend. Furthermore, if the composite antifouling sheet is transparent, the inside can be observed without peeling off the sheet. Another major feature is that it can exert its adhesion function again by its adhesive power even after being reapplied.

[0105] As described above, the silicone composite antifouling sheet of the present invention has a surface opposite to the surface on which the silicone adhesive layer is laminated, which is a fluororesin and has antifouling properties, so that it is possible to prevent people who would like to graffiti from drawing what they want. This effect makes it possible to discourage people who would like to graffiti, thereby suppressing the act of graffiti itself. Furthermore, even if graffiti is done, it can be easily washed away.

[0106] In addition, the silicone adhesive layer laminated on the base layer can be easily attached to the adherend and can follow cracks and shifts in the applied surface. Since the main component is silicone, it has excellent weather resistance, heat resistance, and cold resistance, and can maintain its function for a longer period of time. Furthermore, since the silicone adhesive layer has a waterproof effect, it is possible to prevent moisture from entering the applied area, and to prevent deterioration of the applied object or to significantly delay the progression of deterioration.

[0107] Furthermore, due to its own characteristics, the fluororesin has good weather resistance and can stably maintain its antifouling properties, cleanability, and ease of cleaning for a long period of time. In addition, since the thickness of the fluororesin that forms the base layer is thick, it also has excellent abrasion resistance. EXAMPLES

[0108] The present invention will be specifically described below using examples and comparative examples, but the present invention is not limited to these. In the following examples, parts indicate parts by mass. The average polymerization degree, hardness, and adhesive strength were measured by the above-mentioned methods.

[0109] [Example 1] A fluororesin film (PTFE, Chukoh Flow Skived Tape MSF-100, manufactured by Chukoh Chemical Industry Co., Ltd.) having a thickness of 0.05 mm was prepared as the substrate layer A.

[0110] On the other hand, 92.5 parts of dimethylpolysiloxane with an average degree of polymerization of 1,000 and both ends blocked with dimethylvinylsiloxy groups, (CH2=CH)(CH3)2SiO 1 / 2 Unit: (CH3)3SiO 1 / 2 Resinous copolymer consisting of SiO2 units and SiO2 units [((CH2=CH)(CH3)2SiO 1 / 2 Unit + (CH3)3SiO 1 / 2 A 50% by mass toluene solution containing 7.5 parts of SiO2 (molar ratio) / SiO2 unit (molar ratio) = 0.85, CH2=CH- group content: 0.0008 mol / g was placed in a stirring mixer and mixed for 30 minutes, after which the toluene was completely removed (alkenyl group content 0.00865 mol / g). 100 g). 100 parts of this silicone base is mixed with (CH3)2HSiO as a crosslinker. 1 / 2 6.0 parts of a resinous copolymer having SiH groups (SiH group amount 0.0013 mol / g) mainly composed of SiO2 units and SiO2 units, and 0.1 parts of ethynylcyclohexanol as a reaction inhibitor were added, and the mixture was stirred for 15 minutes to obtain a silicone rubber composition A. 0.2 parts of a platinum catalyst (Pt concentration 1% by mass) was mixed with this silicone rubber composition to obtain an adhesive silicone composition A.

[0111] The adhesive silicone composition A was laminated and coated to a thickness of 1.0 mm on the substrate layer A (stain-resistant layer A) using a comma coater, and then cured by heating in a heating oven at 140°C for 5 minutes to form a silicone adhesive layer, yielding a silicone composite stain-resistant sheet A. The average thickness of the resulting silicone composite stain-resistant sheet A was 1.06 mm.

[0112] The physical properties of the silicone adhesive layer of the obtained silicone composite antifouling sheet A were also measured. The silicone adhesive layer had an Asker C hardness of less than 1 and an Asker CSR-2 hardness of 13. The adhesive strength to the mortar test piece measured by the method described above (adhesive strength to mortar listed in Table 1) was 18 N / 25 mm.

[0113] The silicone composite stain-resistant sheet A was evaluated by the following methods, and the results are shown in Table 1. The evaluation methods used in the following examples and comparative examples were the same as those used in Example 1.

[0114] [Example 2] A fluororesin film (ETFE, Chukoh Chemical Industry Co., Ltd., Chukoh Flow Skived Tape MSF-102) with a thickness of 0.05 mm and one side of which had been etched to give it anchoring properties was prepared as substrate layer B.

[0115] The etched surface of the above-mentioned base layer B (anti-fouling layer B) was laminated and coated with the above-mentioned adhesive silicone composition A using a comma coater to a thickness of 1.0 mm, and then heated and cured in a heating oven at 140°C for 5 minutes to form a silicone adhesive layer, thereby obtaining a silicone composite anti-fouling sheet B. The average thickness of the obtained silicone composite anti-fouling sheet B was 1.05 mm.

[0116] The physical properties of the silicone adhesive layer of the obtained silicone composite antifouling sheet B were also measured. The Asker C hardness of the silicone adhesive layer was less than 1, and the Asker CSR-2 hardness was 13. The adhesive strength to the mortar test piece measured by the method described above (adhesive strength to mortar shown in Table 1) was 19 N / 25 mm. It was.

[0117] The silicone composite stain-resistant sheet B was evaluated by the methods described below, and the results are shown in Table 1.

[0118] [Example 3] A fluororesin film (ETFE, Chukoh Flow Skived Tape MSF-102, manufactured by Chukoh Chemical Industry Co., Ltd.) with a thickness of 0.05 mm and one side etched to give it anchoring properties was prepared for use as the base layer, and a PET film with a thickness of 0.1 mm was prepared for use as the reinforcing layer. In addition, the etched surface of the fluororesin film and the PET film were attached to each other with 3 g / m of a polyester adhesive containing an inorganic UV-absorbing filler. 2 Thus, antifouling layer C having an adhesive strength of 5 N / 25 mm between the fluororesin film and the PET film was prepared.

[0119] The adhesive silicone composition A was laminated and coated to a thickness of 1.0 mm on the reinforcing material layer of the antifouling layer C using a comma coater, and then cured by heating in a heating oven at 140°C for 5 minutes to form a silicone adhesive layer, yielding a silicone composite antifouling sheet C. The average thickness of the resulting silicone composite antifouling sheet C was 1.15 mm.

[0120] The physical properties of the silicone adhesive layer of the obtained silicone composite antifouling sheet C were also measured. The silicone adhesive layer had an Asker C hardness of less than 1 and an Asker CSR-2 hardness of 14. The adhesive strength to the mortar test piece measured by the method described above (adhesive strength to mortar listed in Table 1) was 20 N / 25 mm.

[0121] [Example 4] A fluororesin film (ETFE, Chukoh Flow Skived Tape MSF-102, manufactured by Chukoh Chemical Industry Co., Ltd.) with a thickness of 0.05 mm and one side etched to give it anchoring properties was prepared for use as the base layer, and a UV-resistant PET film with a thickness of 0.1 mm was prepared for use as the reinforcing layer. In addition, the etched surface of the fluororesin film and the UV-resistant PET film were attached to each other with 3 g / m of polyester adhesive containing an inorganic UV-absorbing filler. 2 Thus, an antifouling layer D having an adhesive strength of 5 N / 25 mm between the fluororesin film and the UV-resistant PET film was prepared.

[0122] The adhesive silicone composition A was laminated and coated to a thickness of 1.0 mm on the reinforcing material layer of the antifouling layer D using a comma coater, and then cured by heating in a heating oven at 140°C for 5 minutes to form a silicone adhesive layer, yielding a silicone composite antifouling sheet D. The average thickness of the resulting silicone composite antifouling sheet D was 1.14 mm.

[0123] The physical properties of the silicone adhesive layer of the obtained silicone composite antifouling sheet D were also measured. The silicone adhesive layer had an Asker C hardness of less than 1 and an Asker CSR-2 hardness of 13. The adhesive strength to the mortar test piece measured by the method described above (adhesive strength to mortar listed in Table 1) was 17 N / 25 mm.

[0124] [Comparative Example 1] A 0.1 mm thick UV-resistant PET film was prepared for use as the base layer. In addition, a surface treatment liquid was prepared by adding and mixing 100 parts by mass of KR-400F, a silicone hard coat agent containing a fluorine-containing silicone compound, manufactured by Shin-Etsu Chemical Co., Ltd., and 0.05 parts by mass of FA-600, a defoamer, manufactured by Shin-Etsu Chemical Co., Ltd., as a surface treatment agent. This was spin-coated onto the UV-resistant PET film, and then cured at 120°C for 5 minutes to form a film, producing an antifouling layer E that had been subjected to an antifouling treatment.

[0125] The adhesive silicone composition A was laminated and coated to a thickness of 1.0 mm on the non-antifouling treated surface of the antifouling layer E using a comma coater, and then cured by heating in a heating oven at 140°C for 5 minutes to form a silicone adhesive layer, yielding a silicone composite antifouling sheet E. The average thickness of the resulting silicone composite antifouling sheet E was 1.10 mm.

[0126] The physical properties of the silicone adhesive layer of the obtained silicone composite antifouling sheet E were also measured. The silicone adhesive layer had an Asker C hardness of less than 1 and an Asker CSR-2 hardness of 13. The adhesive strength to a mortar test piece was 20 N / 25 mm.

[0127] [Comparative Example 2] The procedure was repeated in the same manner as in Example 1, except that a 0.1 mm thick untreated PET film (anti-stain layer F) that had not been subjected to anti-stain treatment, unlike in Examples 1 and 2, was used as the base layer, and a silicone composite anti-stain sheet F having an average thickness of 1.10 mm was obtained.

[0128] The physical properties of the silicone adhesive layer of the obtained silicone composite antifouling sheet F were also measured. The silicone adhesive layer had an Asker C hardness of less than 1 and an Asker CSR-2 hardness of 14. The adhesive strength to a mortar test piece was 19 N / 25 mm.

[0129] [Comparative Example 3] An antifouling layer C was obtained in the same manner as in Example 3. On the other hand, 92.5 parts of dimethylpolysiloxane with an average degree of polymerization of 1,000 and both ends blocked with dimethylvinylsiloxy groups, (CH2=CH)(CH3)2SiO 1 / 2 Unit: (CH3)3SiO 1 / 2 Resinous copolymer consisting of SiO2 units and SiO2 units [((CH2=CH)(CH3)2SiO 1 / 2 Unit + (CH3)3SiO 1 / 2A 50% by mass toluene solution containing 7.5 parts of SiO2 (molar ratio) / SiO2 unit (molar ratio) = 0.85, CH2=CH- group content: 0.0008 mol / g was placed in a stirring mixer and mixed for 30 minutes, after which the toluene was completely removed (alkenyl group content 0.00865 mol / g). 100 g). 100 parts of this silicone base is mixed with (CH3)2HSiO as a crosslinker. 1 / 2 8.0 parts of a resinous copolymer having SiH groups (SiH group amount 0.0013 mol / g) mainly composed of SiO2 units and SiO2 units, and 0.1 parts of ethynylcyclohexanol as a reaction inhibitor were added, and the mixture was stirred for 15 minutes to obtain silicone rubber composition B. 0.2 parts of a platinum catalyst (Pt concentration 1% by mass) was mixed with this silicone rubber composition to obtain adhesive silicone composition B.

[0130] The above-mentioned adhesive silicone composition B was laminated and coated to a thickness of 1.0 mm on the reinforcing material layer of the above-mentioned anti-fouling layer C using a comma coater, and then heated and cured in a heating oven at 140°C for 5 minutes to form a silicone adhesive layer, resulting in a silicone composite anti-fouling sheet G with an average thickness of 1.15 mm.

[0131] The physical properties of the silicone adhesive layer of the obtained silicone composite antifouling sheet G were also measured. The silicone adhesive layer had an Asker C hardness of 22 and an Asker CSR-2 hardness of 76. The adhesive strength to a mortar test piece was 2 N / 25 mm.

[0132] [Comparative Example 4] An antifouling layer C was obtained in the same manner as in Example 3. The above-mentioned adhesive composition B was laminated and coated to a thickness of 2.0 mm on the reinforcing material layer of the above-mentioned anti-fouling layer C using a comma coater, and then heated and cured in a heating furnace at 140°C for 5 minutes to form a silicone adhesive layer, thereby obtaining a silicone composite anti-fouling sheet H with an average thickness of 2.16 mm.

[0133] The physical properties of the silicone adhesive layer of the obtained silicone composite antifouling sheet H were also measured. The silicone adhesive layer had an Asker C hardness of 21 and an Asker CSR-2 hardness of 72. The adhesive strength to a mortar test piece was 3 N / 25 mm.

[0134] <Evaluation items> The evaluation items and evaluation methods for the composite sheet are shown below. In the following, the silicone composite stain-resistant sheet of each example is simply referred to as the "silicone composite stain-resistant sheet."

[0135] [Anti-stain properties] Oil-based lacquer spray and water-based lacquer spray were sprayed for 3 seconds on the stain-resistant surface of the silicone composite stain-resistant sheet to check the repelling properties. Those that did not repel and the sprayed area remained as it was were rated as ×, those that ran off and the spray shape was lost were rated as 〇, those that ran off partially were rated as △, and those that were not rated were rated as -. The test was carried out twice, once initially and once after a xenon arc accelerated exposure test (1000 hours aging). The xenon arc accelerated exposure test was in accordance with JIS K 7350-2 Method A.

[0136] [Repeat cleaning ability] The stain-resistant surface of the silicone composite stain-resistant sheet was sprayed with oil-based lacquer spray and water-based lacquer spray for 3 seconds and dried at room temperature for 6 hours. The stains were then transferred and cleaned using the adhesive side of an adhesive tape. The spray and transfer cleaning were repeated 5 times, and those that could not be transferred and cleaned were marked with an X, those that could be transferred and cleaned were marked with an ◯, and no evaluation was made. The test was carried out twice, once initially and once after a xenon arc accelerated exposure test (1000 hours aging). The xenon arc accelerated exposure test was in accordance with JIS K 7350-2 Method A.

[0137] [Easy to clean] The stain-resistant surface of the silicone composite stain-resistant sheet was sprayed with oil-based lacquer spray and water-based lacquer spray for 3 seconds and then dried at room temperature for 6 hours. The stains were then transferred and washed using the adhesive side of an adhesive tape. Tests that could be transferred and washed 5 times or less, which removed most of the lacquer spray, were rated as ◯, those that could be transferred and washed 10 times or less as △, those that could be transferred and washed more than that or could not be removed as ×, and those that were not rated at all as -. The test was carried out twice, once initially and once after a xenon arc accelerated exposure test (1000 hours aging). The xenon arc accelerated exposure test was conducted in accordance with JIS K 7350-2 Method A.

[0138] [Wear resistance] The substrate layer of the silicone antifouling sheet was slightly scraped off with fine sandpaper, and the initial sample was evaluated for antifouling properties, repeated cleaning properties, and ease of cleaning by the methods described above.

[0139] [Adhesiveness and followability] A composite sheet sample measuring 50mm x 100mm was cut out from the silicone composite antifouling sheet. This composite sheet sample was attached to one side of the two mortar test pieces arranged side by side against the adhesive layer so that the areas where the mortar test pieces were attached were equal in area, and left at room temperature for 24 hours. When the sheet was pulled from zero span to a maximum of 20mm, the sheet was rated as ◯ if the displacement was 10mm or more without peeling, △ if 5-10mm, and × if less than 5mm. Measuring device: Shimadzu Autograph Pulling speed: 50mm / min. Mortar test piece shape: 50mm x 72mm x thickness 10mm

[0140] [Table 1]

[0141] In Examples 1 to 4, the repetitive cleaning property and cleaning ease were good for a long time, the antifouling property was sufficient, and the adhesion and followability were also good. In particular, since the displacement was 10 mm or more, the followability against cracks and deviations of the applied surface was excellent. Furthermore, in Examples 3 to 4, the effect of the reinforcing material layer suppressed the deformation due to the stress of the base layer, and the smoothness of the silicone composite antifouling sheet surface (antifouling surface) was further improved. On the other hand, in Comparative Example 1, the base layer was treated with a silicone hard coat agent containing a fluorine-containing silicone compound, so that the initial antifouling property, repetitive cleaning property, and cleaning ease were good, but after the xenon arc accelerated exposure test, the antifouling property and cleaning ease were reduced, and the abrasion resistance was poor. In Comparative Example 2, a resin (PET) without antifouling property was used as the base layer, so that the antifouling property and repetitive cleaning property were poor. In Comparative Examples 3 and 4, although the films had antifouling properties and could be washed repeatedly for a long period of time, the silicone adhesive layer had too high a hardness and low adhesive strength, resulting in poor adhesion and conformability.

[0142] From the above, it has become clear that the silicone composite antifouling sheet of the present invention can maintain excellent antifouling properties, repeated cleaning properties, and cleaning ease for a long period of time, and also has excellent abrasion resistance, can be easily attached to an adherend, and can follow cracks and deviations of the applied surface. In particular, as can be understood from the results of Comparative Example 1, when a fluororesin is formed by coating using a surface treatment agent or the like (i.e., a non-fluororesin reinforcing material layer is coated with a fluororesin as a substrate layer), the adhesion between the coating layer (fluororesin) and its lower layer (reinforcing material layer) is insufficient, and if the coating layer is thin, it is easy to peel off and is easily scratched. Even if the coating layer is made thick, there is a problem that it is still easy to peel off due to the influence of the temperature difference due to the difference in thermal expansion coefficient between the coating layer and its lower layer (reinforcing material layer), and the problem of the present invention cannot be solved. On the other hand, in the present invention, the substrate layer is made of the fluororesin itself, so the above problem does not occur. In this way, the substrate layer of the present invention is completely different from one formed of a fluororesin by coating.

[0143] In addition, since the adhesive layer of the silicone composite stain-resistant sheet of the present invention is mainly composed of silicone, it has excellent weather resistance, heat resistance, and cold resistance, and can maintain its function for a long period of time. Furthermore, since the silicone adhesive layer has a waterproof effect, it is possible to prevent the infiltration of moisture into the application area and prevent deterioration of the application object or significantly delay the progress of deterioration.

[0144] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention. [Explanation of symbols]

[0145] 1...base material layer, 2...silicone adhesive layer, 3...reinforcing material layer, 4...silicone composite anti-fouling sheet, 5...reinforcing material, 6...anti-fouling layer, 7...anti-fouling surface.

Claims

1. A silicone composite antifouling sheet comprising a substrate layer and a silicone adhesive layer laminated on one side of the substrate layer, The silicone adhesive layer is (A) an organopolysiloxane containing, in each molecule, at least two alkenyl groups bonded to silicon atoms; (B) an alkenyl-containing resinous copolymer having R 2 3 SiO 1 / 2 units (wherein R 2 is an unsubstituted or substituted monovalent hydrocarbon group, including an alkenyl group) and SiO 2 units; (C) an organohydrogenpolysiloxane containing at least two hydrogen atoms bonded to silicon atoms (SiH groups) per molecule, and (D) an addition reaction catalyst, and the amount of the component (A) is 20 to 100 parts by mass and the amount of the component (B) is 0 to 80 parts by mass, where the total amount of the components (A) and (B) contained in the addition-curable silicone composition is 100 parts by mass; the amount of component (C) is such that the molar ratio of hydrogen atoms bonded to silicon atoms (SiH groups) in component (C) to alkenyl groups bonded to silicon atoms contained in components (A) and (B) is 0.5 to 1.1; the base layer is made of a fluororesin, the silicone adhesive layer has a hardness of 5 or less on an Asker C hardness scale and an adhesive strength to a mortar test piece of 5 N / 25 mm or more, and the surface of the base layer opposite to the side on which the silicone adhesive layer is laminated is an antifouling surface; A silicone composite anti-fouling sheet, characterized in that at least the surface of the fluororesin constituting the base material layer opposite the anti-fouling surface has been treated to improve anchoring properties, and the base material layer itself is made of the fluororesin.

2. 2. The silicone composite stain-resistant sheet according to claim 1, wherein the substrate layer further contains a reinforcing material.

3. 3. The silicone composite stain-resistant sheet according to claim 1, further comprising a reinforcing layer laminated between the base layer and the silicone adhesive layer.

4. 4. The silicone composite stain-resistant sheet according to claim 3, wherein the base layer and the reinforcing material layer are laminated via an adhesive layer having UV resistance.

5. 5. The silicone composite stain-resistant sheet according to claim 3, wherein the reinforcing material layer comprises a PET film.

6. 6. The silicone composite stain-resistant sheet according to claim 1, wherein at least one of the layers has a light reflection suppressing effect.

7. The silicone composite antifouling sheet according to any one of claims 1 to 6, characterized in that the base layer has a thickness of 0.05 to 0.3 mm, the adhesive layer has a thickness of 0.5 to 3 mm, and the silicone composite antifouling sheet has a total thickness of 0.55 to 3.3 mm.

8. 8. The silicone composite stain-resistant sheet according to claim 1, which is used to prevent graffiti.

9. 9. An anti-graffiti application method comprising attaching the silicone adhesive layer of the silicone composite anti-fouling sheet according to any one of claims 1 to 8 to a desired adherend and exposing the anti-fouling surface made of the fluororesin of the base material layer, thereby preventing graffiti on the adherend.

Citation Information

Patent Citations

  • Contamination preventing method for land structure

    JP1994182290A

  • Pollution preventive coating method

    JP1997094524A

  • Contamination preventing method

    JP1998216619A

  • Antifouling film and antifouling body

    JP2002249739A

  • Tape or sheet for sticking nonwoven fluororesin fabric

    JP2003138231A