Curable resin composition, cured product, adhesive, and adhesive film

The curable resin composition with a sea-island structure and imide oligomer addresses the issue of stress relaxation and adhesion in conventional compositions, offering superior heat resistance and cycle durability for electronic bonding applications.

JP7563988B2Active Publication Date: 2024-10-08SEKISUI CHEMICAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021000489
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-05
Publication Date
2024-10-08
Estimated Expiration
2041-01-05

AI Technical Summary

Technical Problem

Conventional curable resin compositions with excellent long-term heat resistance fail to exhibit sufficient stress relaxation properties during cold and hot cycles, leading to cracks and poor adhesion after cycle tests.

Method used

A curable resin composition with a sea-island structure, containing a curable resin and a curing agent, specifically an imide oligomer, which maintains an initial adhesive strength of 5.0N/mm to a silicon chip and retains 5.0N/mm after 1000 hours at 150°C, along with a glass transition temperature range of 30°C to 200°C, enhancing stress relaxation properties.

Benefits of technology

The composition provides excellent long-term heat resistance and stress relaxation properties, ensuring robust adhesion and crack resistance during cooling and heating cycles, suitable for bonding electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563988000001
    Figure 0007563988000001
  • Figure 0007563988000002
    Figure 0007563988000002
  • Figure 0007563988000003
    Figure 0007563988000003
Patent Text Reader

Abstract

To provide a curable resin composition that has excellent long-term heat resistance and stress relaxation property in a cooling / heating cycle, a cured product of the curable resin composition, and an adhesive and an adhesive film using the curable resin composition.SOLUTION: Provided is a curable resin composition that contains a curable resin and a curing agent and in which the initial adhesive strength of the cured product to silicon chip is 5.0 N / mm2 or more, and the adhesive strength of the cured product to silicon chip after storage at 150°C for 1000 hours is 5.0 N / mm2 or more, and the cured product has a sea-island structure.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a curable resin composition having excellent long-term heat resistance and stress relaxation properties in thermal cycles. The present invention also relates to a cured product of the curable resin composition, and an adhesive and an adhesive film using the curable resin composition. [Background technology]

[0002] In recent years, the use of flexible printed circuit boards (FPCs) has expanded to include in-vehicle applications, and adhesives used in FPCs and coverlay films that protect FPCs are required to have high-temperature long-term heat resistance. For such adhesives, curable resin compositions using curable resins such as epoxy resins that have low shrinkage and excellent adhesion, insulation, and chemical resistance are used, and in particular, curable resin compositions that provide good results in solder reflow tests for short-term heat resistance and thermal cycle tests for repeated heat resistance are required. For example, Patent Documents 1 and 2 disclose curable resin compositions that contain an epoxy resin and an imide compound as a curing agent as a curing agent, as curable resin compositions that are excellent in heat resistance and adhesion. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Publication No. 61-270852 [Patent Document 2] Special Publication No. 2004-502859 Summary of the Invention [Problem to be solved by the invention]

[0004] Conventional curable resin compositions having excellent long-term heat resistance were unable to provide sufficient stress relaxation properties to the cured product in a thermal cycle test, and cracks were sometimes generated or the adhesiveness was poor after the thermal cycle test. The present invention aims to provide a curable resin composition having excellent long-term heat resistance and stress relaxation properties in thermal cycles. It is also an object of the present invention to provide a cured product of the curable resin composition, and an adhesive and an adhesive film using the curable resin composition. [Means for solving the problem]

[0005] The present invention contains a curable resin and a curing agent, and the initial adhesive strength of the cured product to a silicon chip is 5.0 N / mm 2 After storage at 150°C for 1000 hours, the adhesive strength of the cured product to the silicon chip was 5.0N / mm 2 The curable resin composition has the above structure and the cured product has an island-sea structure. The present invention will be described in detail below.

[0006] The present inventors have investigated how to control the initial adhesive strength of a cured product of a curable resin composition to a silicon chip and the adhesive strength of the cured product to a silicon chip after storage at 150°C for 1000 hours within specific ranges, and how to make the cured product have a sea-island structure. As a result, they have found that it is possible to obtain a curable resin composition that is excellent in long-term heat resistance and stress relaxation properties in thermal cycles, and have completed the present invention.

[0007] The curable resin composition of the present invention has a lower limit of the initial adhesive strength of the cured product to a silicon chip of 5.0 N / mm 2 The initial adhesive strength of the above cured product to the silicon chip is 5.0 N / mm 2 Due to the above, the curable resin composition of the present invention can be suitably used for bonding electronic components. The preferable lower limit of the initial adhesive strength of the cured product to a silicon chip is 5.1 N / mm 2 , and a more preferable lower limit is 5.2N / mm 2 It is. The initial adhesive strength of the cured product to a silicon chip can be measured by the following method. That is, first, a curable resin composition is applied to a polyimide substrate, and a silicon chip is placed on top of it. Next, the curable resin composition is cured by heating at 190°C for 1 hour to obtain a test piece. The die shear strength of the obtained test piece is measured at a speed of 100 μm / s and a test height of 100 μm at 25°C using a die shear tester. The obtained die shear strength is taken as the initial adhesive strength of the cured product to the silicon chip. Kapton 200H (manufactured by Toray DuPont Co., Ltd., surface roughness 0.03 to 0.07 μm) can be used as the polyimide substrate, and a silicon chip (surface roughness 0.5 to 1.0 nm) manufactured by Global Wafer Co., Ltd. can be used as the silicon chip. In addition, DAGE4000 (manufactured by Nordson) can be used as the die shear tester.

[0008] The curable resin composition of the present invention has a lower limit of adhesive strength to a silicon chip of 5.0 N / mm after storage at 150°C for 1000 hours. 2 After storing the above-mentioned material at 150°C for 1000 hours, the adhesive strength of the cured material to the silicon chip was 5.0 N / mm 2 Due to the above, the curable resin composition of the present invention can be suitably used for bonding electronic components used in high temperature environments. The preferable lower limit of the adhesive strength of the cured product to a silicon chip after storage at 150° C. for 1000 hours is 5.1 N / mm 2 , and a more preferable lower limit is 5.2N / mm 2 It is. There is no particular upper limit to the adhesive strength of the cured product after storage at 150°C for 1000 hours to a silicon chip, but the practical upper limit is 7.0 N / mm 2 It is. The adhesive strength of the cured product after storage at 150° C. for 1000 hours to a silicon chip can be measured by the following method. That is, first, a test piece obtained in the same manner as in the above-mentioned "initial adhesive strength of the cured product to the silicon chip" is stored in an oven at 150°C for 1000 hours. Next, for the test piece after storage, the die shear strength is measured at 25°C at a speed of 100 μm / s and a test height of 100 μm using a die shear tester. The obtained adhesive strength is the adhesive strength of the cured product to the silicon chip after storage at 150°C for 1000 hours.

[0009] The curable resin composition of the present invention has a sea-island structure when cured, and the cured product has excellent stress relaxation properties during thermal cycles. In the present invention, the "sea-island structure" refers to a structure in which a phase consisting of a certain component (island component) is dispersed in a phase consisting of another component (sea component). The sea-island structure can be confirmed by observing with a transmission electron microscope at a magnification of 2,000 to 10,000 times.

[0010] The lower limit of the average diameter of the islands in the sea-island structure is preferably 0.05 μm, and the upper limit is preferably 1.0 μm. When the average diameter of the islands is within this range, the curable resin composition of the present invention has better stress relaxation properties in thermal cycles. The lower limit of the average diameter of the islands is more preferably 0.1 μm, and the upper limit is more preferably 0.8 μm. The average diameter of the islands means the average of the major axes of five islands that can be observed when the cured product of the curable resin composition is observed at a magnification of 10,000 times using a transmission electron microscope.

[0011] The curable resin composition of the present invention preferably has a low-temperature glass transition temperature in the range of 30°C to 160°C and a high-temperature glass transition temperature in the range of 150°C to 200°C. By having such a low-temperature glass transition temperature and a high-temperature glass transition temperature, the curable resin composition of the present invention has better stress relaxation properties in a thermal cycle. The lower limit of the low-temperature glass transition temperature is preferably 35°C, more preferably 40°C, and preferably 155°C, and more preferably 150°C. The high-temperature glass transition temperature is preferably more than 155°C, more preferably 160°C, and preferably 195°C, and more preferably 190°C. The curable resin composition of the present invention may have two or more low-temperature glass transition temperatures. The curable resin composition of the present invention may have two or more high-temperature glass transition temperatures. In this specification, the "glass transition temperature" refers to a temperature at which a maximum due to micro-Brownian motion appears among the maximums of loss tangent (tan δ) obtained by dynamic viscoelasticity measurement, and can be measured by a conventionally known method using a dynamic viscoelasticity measuring device.

[0012] In the curable resin composition of the present invention, a method for adjusting the initial adhesive strength of the cured product to a silicon chip, the adhesive strength of the cured product to a silicon chip after storage at 150°C for 1000 hours, and the glass transition temperature of the cured product to be within the above-mentioned ranges, respectively, or for making the cured product have a sea-island structure, is preferably a method of adjusting the type and content ratio of each of the components contained in the curable resin composition.

[0013] The curable resin composition of the present invention contains a curable resin and a curing agent. In particular, the curable resin composition of the present invention is preferably a thermosetting resin composition, and more preferably contains a curable resin and a heat curing agent as a curing agent. The curable resin and the curing agent are usually components that constitute the sea part of the sea-island structure.

[0014] Examples of the curable resin include epoxy resin, acrylic resin, phenol resin, cyanate resin, isocyanate resin, maleimide resin, benzoxazine resin, silicone resin, and fluororesin. Among them, the curable resin preferably contains an epoxy resin. These curable resins may be used alone or in combination of two or more.

[0015] Examples of the epoxy resin include bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol E type epoxy resin, bisphenol S type epoxy resin, 2,2'-diallyl bisphenol A type epoxy resin, hydrogenated bisphenol type epoxy resin, propylene oxide-added bisphenol A type epoxy resin, triazine type epoxy resin, resorcinol type epoxy resin, biphenyl type epoxy resin, sulfide type epoxy resin, diphenyl ether type epoxy resin, dicyclopentadiene type epoxy resin, naphthalene type epoxy resin, fluorene type epoxy resin, naphthylene ether type epoxy resin, phenol novolac type epoxy resin, ortho-cresol novolac type epoxy resin, dicyclopentadiene novolac type epoxy resin, biphenyl novolac type epoxy resin, naphthalene phenol novolac type epoxy resin, glycidyl amine type epoxy resin, alkyl polyol type epoxy resin, rubber modified type epoxy resin, and glycidyl ester compound.

[0016] Examples of the heat curing agent include imide oligomers having an imide skeleton in the main chain and a crosslinkable functional group at the end, acid anhydride curing agents, phenolic curing agents, thiol curing agents, amine curing agents, cyanate curing agents, and active ester curing agents. Among them, from the viewpoint of the adhesiveness and long-term heat resistance of the cured product of the curable resin composition obtained, it is preferable that the heat curing agent contains an imide oligomer. Furthermore, the curable resin composition of the present invention is excellent in adhesiveness and long-term heat resistance of the cured product, and is also excellent in coatability and thixotropy, so it is preferable that the heat curing agent contains an imide oligomer and a polymer compound described later.

[0017] The imide oligomer preferably has an acid anhydride group or a phenolic hydroxyl group at an end of the main chain as the crosslinkable functional group, and more preferably has an acid anhydride group or a phenolic hydroxyl group at both ends of the main chain.

[0018] The imide oligomer preferably has a structure represented by the following formula (1-1) or (1-2), or the following formula (2-1) or (2-2): By having a structure represented by the following formula (1-1) or (1-2), or the following formula (2-1) or (2-2), the imide oligomer has better reactivity and compatibility with the curable resin.

[0019] [ka]

[0020] In formula (1-1) and formula (1-2), A is an acid dianhydride residue, B is an aliphatic diamine residue or an aromatic diamine residue, and in formula (1-2), Ar is an optionally substituted divalent aromatic group.

[0021] [ka]

[0022] In formula (2-1) and formula (2-2), A is an acid dianhydride residue, B is an aliphatic triamine residue or an aromatic triamine residue, and in formula (2-2), Ar is an optionally substituted divalent aromatic group.

[0023] The acid dianhydride residue is preferably a tetravalent group represented by the following formula (3-1) or (3-2).

[0024] [ka]

[0025] In formula (3-1) and formula (3-2), * is a bonding position, and in formula (3-1), Z is a bond, an oxygen atom, a carbonyl group, a sulfur atom, a sulfonyl group, a linear or branched divalent hydrocarbon group which may have an oxygen atom at the bonding position, or a divalent group having an aromatic ring which may have an oxygen atom at the bonding position. The hydrogen atoms of the aromatic ring in formula (3-1) and formula (3-2) may be substituted.

[0026] When Z in the above formula (3-1) is a linear or branched divalent hydrocarbon group which may have an oxygen atom at the bonding position, or a divalent group having an aromatic ring which may have an oxygen atom at the bonding position, these groups may be substituted. In the case where the linear or branched divalent hydrocarbon group which may have an oxygen atom at the bonding position, or the divalent group having an aromatic ring which may have an oxygen atom at the bonding position, is substituted, examples of the substituent include a halogen atom, a linear or branched alkyl group, a linear or branched alkenyl group, an alicyclic group, an aryl group, an alkoxy group, a nitro group, and a cyano group.

[0027] Examples of the acid dianhydride from which the above acid dianhydride residue is derived include the acid dianhydride represented by the formula (9) described below.

[0028] When B in the above formula (1-1), (1-2), (2-1), or (2-2) is the above aliphatic diamine residue and / or the above aliphatic triamine residue, the preferred lower limit of the number of carbon atoms in the aliphatic diamine residue and the aliphatic triamine residue is 4. When the aliphatic diamine residue and the aliphatic triamine residue have 4 or more carbon atoms, the obtained curable resin composition has better flexibility and processability before curing, and better dielectric properties after curing. The more preferred lower limit of the number of carbon atoms in the aliphatic diamine residue and the aliphatic triamine residue is 5, and the even more preferred lower limit is 6. Further, there is no particular upper limit on the number of carbon atoms in the aliphatic diamine residue and the aliphatic triamine residue, but the substantial upper limit is 60.

[0029] Examples of the aliphatic diamine from which the aliphatic diamine residue is derived include aliphatic diamines derived from dimer acids, linear or branched aliphatic diamines, aliphatic ether diamines, and aliphatic alicyclic diamines. Examples of the aliphatic diamine derived from the dimer acid include dimer diamine and hydrogenated dimer diamine. Examples of the linear or branched aliphatic diamine include 1,4-butanediamine, 1,6-hexanediamine, 1,8-octanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,11-undecanediamine, 1,12-dodecanediamine, 1,14-tetradecanediamine, 1,16-hexadecanediamine, 1,18-octadecanediamine, 1,20-eicosanediamine, 2-methyl-1,8-octanediamine, 2-methyl-1,9-nonanediamine, and 2,7-dimethyl-1,8-octanediamine. Examples of the aliphatic ether diamine include 2,2'-oxybis(ethylamine), 3,3'-oxybis(propylamine), 1,2-bis(2-aminoethoxy)ethane, and the like. Examples of the aliphatic alicyclic diamine include 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, cyclohexanediamine, methylcyclohexanediamine, and isophoronediamine. Among these, the aliphatic diamine residue is preferably an aliphatic diamine residue derived from the dimer acid.

[0030] Examples of the aliphatic triamine from which the aliphatic triamine residue is derived include aliphatic triamines derived from trimer acids, linear or branched aliphatic triamines, aliphatic ether triamines, and aliphatic alicyclic triamines. Examples of the aliphatic triamine derived from the trimer acid include trimer triamine and hydrogenated trimer triamine. Examples of the linear or branched aliphatic triamine include 3,3'-diamino-N-methyldipropylamine, 3,3'-diaminodipropylamine, diethylenetriamine, bis(hexamethylene)triamine, and 2,2'-bis(methylamino)-N-methyldiethylamine. Among these, the aliphatic triamine residue is preferably an aliphatic triamine residue derived from the trimer acid.

[0031] As the aliphatic diamine and / or the aliphatic triamine, a mixture of the dimer triamine and the trimer triamine can also be used.

[0032] Commercially available aliphatic diamines and / or aliphatic triamines derived from the dimer acids and / or trimer acids include, for example, aliphatic diamines and / or aliphatic triamines manufactured by BASF, and aliphatic diamines and / or aliphatic triamines manufactured by Croda. Examples of the aliphatic diamines and / or aliphatic triamines manufactured by BASF include Versamine 551, Versamine 552, and the like. Examples of the aliphatic diamines and / or aliphatic triamines manufactured by Croda include Priamine 1071, Priamine 1073, Priamine 1074, Priamine 1075, and the like.

[0033] When B in the above formula (1-1), (1-2), (2-1), or (2-2) is the above aromatic diamine residue, the aromatic diamine residue is preferably a divalent group represented by the following formula (4-1) or (4-2).

[0034] [ka]

[0035] In formula (4-1) and formula (4-2), * is a bonding position, and in formula (4-1), Y is a bond, an oxygen atom, a carbonyl group, a sulfur atom, a sulfonyl group, a linear or branched divalent hydrocarbon group which may have an oxygen atom at the bonding position, or a divalent group having an aromatic ring which may have an oxygen atom at the bonding position. The hydrogen atoms of the aromatic ring in formula (4-1) and formula (4-2) may be substituted.

[0036] When Y in the above formula (4-1) is a straight-chain or branched-chain divalent hydrocarbon group which may have an oxygen atom at the bonding position, or a divalent group having an aromatic ring which may have an oxygen atom at the bonding position, these groups may be substituted. In the case where the linear or branched divalent hydrocarbon group which may have an oxygen atom at the bonding position, or the divalent group having an aromatic ring which may have an oxygen atom at the bonding position, is substituted, examples of the substituent include a halogen atom, a linear or branched alkyl group, a linear or branched alkenyl group, an alicyclic group, an aryl group, an alkoxy group, a nitro group, and a cyano group.

[0037] Examples of the aromatic diamine from which the aromatic diamine residue is derived include those in which the diamine represented by the formula (10) described below is an aromatic diamine.

[0038] Furthermore, when the imide oligomer has a siloxane skeleton in its structure, the glass transition temperature after curing is lowered and the adherend is contaminated, which may cause poor adhesion. Therefore, it is preferable that the imide oligomer does not have a siloxane skeleton in its structure.

[0039] The weight average molecular weight of the imide oligomer is preferably 500 or more and 5000 or less. When the weight average molecular weight of the imide oligomer is in this range, the cured product of the obtained curable resin composition has excellent long-term heat resistance and is easy to form a sea-island structure. The weight average molecular weight of the imide oligomer is more preferably 1000 in lower limit and 4000 in upper limit. In this specification, the "weight average molecular weight" is a value obtained by measuring using tetrahydrofuran as a solvent by gel permeation chromatography (GPC) and converting the weight average molecular weight into polystyrene equivalent. Examples of columns used in measuring the weight average molecular weight converted into polystyrene equivalent by GPC include JAIGEL-2H-A (manufactured by Japan Analytical Industry Co., Ltd.).

[0040] Specifically, the imide oligomer is preferably an imide oligomer represented by the following formula (5-1), (5-2), (5-3), (5-4), or (5-5), or an imide oligomer represented by the following formula (6-1), (6-2), (6-3), (6-4), or (6-5).

[0041] [ka]

[0042] In formulae (5-1) to (5-5), A is the above-mentioned acid dianhydride residue, and in formulae (5-1) to (5-5), A may be the same or different. In formulae (5-1) to (5-4), B is the above-mentioned aliphatic diamine residue or aromatic diamine residue, and in formulae (5-3) and (5-4), B may be the same or different. In formula (5-5), B is the above-mentioned aliphatic triamine residue or aromatic triamine residue. In formula (5-2), X is a hydrogen atom, a halogen atom, or an optionally substituted monovalent hydrocarbon group, and in formula (5-4), W is a hydrogen atom, a halogen atom, or an optionally substituted monovalent hydrocarbon group. In formulae (5-3) and (5-4), n is the number of repetitions.

[0043] [ka]

[0044] In formulae (6-1) to (6-5), A is the above-mentioned acid dianhydride residue, and in formulae (6-1) to (6-5), A may be the same or different. In formulae (6-1) to (6-5), R is a hydrogen atom, a halogen atom, or an optionally substituted monovalent hydrocarbon group, and in formulae (6-1), (6-3), and (6-5), R may be the same or different. In formulae (6-2) and (6-4), W is a hydrogen atom, a halogen atom, or an optionally substituted monovalent hydrocarbon group. In formulae (6-1) to (6-4), B is the above-mentioned aliphatic diamine residue or the above-mentioned aromatic diamine residue, and in formulae (6-3) and (6-4), B may be the same or different. In formula (6-5), B is the above aliphatic triamine residue or the above aromatic triamine residue.

[0045] In the above formulas (5-1) to (5-5) and (6-1) to (6-5), A is preferably a tetravalent group represented by the following formula (7-1) or (7-2).

[0046] [ka]

[0047] In formula (7-1) and formula (7-2), * is a bonding position, and in formula (7-1), Z is a bond, an oxygen atom, a carbonyl group, a sulfur atom, a sulfonyl group, a linear or branched divalent hydrocarbon group which may have an oxygen atom at the bonding position, or a divalent group having an aromatic ring which may have an oxygen atom at the bonding position. The hydrogen atoms of the aromatic ring in formula (7-1) and formula (7-2) may be substituted.

[0048] B in the above formulas (5-1) to (5-4) and (6-1) to (6-4) is preferably a divalent group represented by the following formula (8-1) or (8-2).

[0049] [ka]

[0050] In formula (8-1) and formula (8-2), * is a bonding position, and in formula (8-1), Y is a bond, an oxygen atom, a carbonyl group, a sulfur atom, a sulfonyl group, a linear or branched divalent hydrocarbon group which may have an oxygen atom at the bonding position, or a divalent group having an aromatic ring which may have an oxygen atom at the bonding position. The hydrogen atoms of the aromatic ring in formula (8-1) and formula (8-2) may be substituted.

[0051] An example of a method for producing an imide oligomer having a structure represented by the above formula (1-1) is a method of reacting an acid dianhydride represented by the following formula (9) with a diamine represented by the following formula (10). Alternatively, an imide oligomer having a structure represented by the above formula (2-1) can be produced by using an aliphatic triamine or aromatic triamine instead of the diamine represented by the following formula (10).

[0052] [ka]

[0053] In formula (9), A is the same tetravalent group as A in the above formula (1-1).

[0054] [ka]

[0055] In formula (10), B is the same divalent group as B in formula (1-1), and R 1 ~R 4 are each independently a hydrogen atom or a monovalent hydrocarbon group.

[0056] A specific example of the method for reacting the acid dianhydride represented by the above formula (9) with the diamine represented by the above formula (10) is shown below. First, the diamine represented by the above formula (10) is dissolved in a solvent (e.g., N-methylpyrrolidone, etc.) in which the amic acid oligomer obtained by the reaction is soluble, and the acid dianhydride represented by the above formula (9) is added to the obtained solution and reacted to obtain an amic acid oligomer solution. Next, the solvent is removed by heating or reducing pressure, and the amic acid oligomer is reacted by heating at about 200°C or higher for 1 hour or more. By adjusting the molar ratio of the acid dianhydride represented by the above formula (9) and the diamine represented by the above formula (10) and the imidization conditions, an imide oligomer having a desired weight average molecular weight and a structure represented by the above formula (1-1) at both ends can be obtained. In addition, by replacing a part of the acid dianhydride represented by the above formula (9) with the acid anhydride represented by the following formula (11), it is possible to obtain an imide oligomer having a desired weight average molecular weight, a structure represented by the above formula (1-1) at one end, and a structure derived from the acid anhydride represented by the following formula (11) at the other end. In this case, the acid dianhydride represented by the above formula (9) and the acid anhydride represented by the following formula (11) may be added simultaneously or separately. Furthermore, by replacing a portion of the diamine represented by the above formula (10) with a monoamine represented by the following formula (12), it is possible to obtain an imide oligomer having a desired weight average molecular weight, a structure represented by the above formula (1-1) at one end, and a structure derived from the monoamine represented by the following formula (12) at the other end. In this case, the diamine represented by the above formula (10) and the monoamine represented by the following formula (12) may be added simultaneously or separately.

[0057] [ka]

[0058] In formula (11), Ar is an optionally substituted divalent aromatic group.

[0059] [ka]

[0060] In formula (12), Ar is an optionally substituted monovalent aromatic group, and R 5 and R 6 are each independently a hydrogen atom or a monovalent hydrocarbon group.

[0061] Examples of a method for producing an imide oligomer having a structure represented by the above formula (1-2) include a method of reacting an acid dianhydride represented by the above formula (9), a diamine represented by the above formula (10), and a phenolic hydroxyl group-containing monoamine represented by the following formula (13). Also, by using an aliphatic triamine or aromatic triamine instead of the diamine represented by the above formula (10), an imide oligomer having a structure represented by the above formula (2-2) can be produced.

[0062] [ka]

[0063] In formula (13), Ar is an optionally substituted divalent aromatic group, and R 7 and R 8 are each independently a hydrogen atom or a monovalent hydrocarbon group.

[0064] A specific example of the method for reacting the acid dianhydride represented by the above formula (9), the diamine represented by the above formula (10), and the phenolic hydroxyl group-containing monoamine represented by the above formula (13) is shown below. First, the phenolic hydroxyl group-containing monoamine represented by the formula (13) and the diamine represented by the formula (10) are dissolved in a solvent (e.g., N-methylpyrrolidone) in which the amic acid oligomer obtained by the reaction is soluble, and the acid dianhydride represented by the formula (9) is added to the obtained solution and reacted to obtain an amic acid oligomer solution. Then, the solvent is removed by heating or reducing pressure, and the amic acid oligomer is reacted by heating at about 200°C or higher for 1 hour or more. By adjusting the molar ratio of the acid dianhydride represented by the formula (9), the diamine represented by the formula (10), and the phenolic hydroxyl group-containing monoamine represented by the formula (13), and the imidization conditions, an imide oligomer having a desired weight average molecular weight and a structure represented by the formula (1-2) at both ends can be obtained. In addition, by replacing a part of the phenolic hydroxyl group-containing monoamine represented by the above formula (13) with the monoamine represented by the above formula (12), it is possible to obtain an imide oligomer having a desired weight average molecular weight, a structure represented by the above formula (1-2) at one end, and a structure derived from the monoamine represented by the above formula (12) at the other end. In this case, the phenolic hydroxyl group-containing monoamine represented by the above formula (13) and the monoamine represented by the above formula (12) may be added simultaneously or separately.

[0065] Examples of the acid dianhydride represented by the above formula (9) include pyromellitic anhydride, 3,3'-oxydiphthalic anhydride, 3,4'-oxydiphthalic anhydride, 4,4'-oxydiphthalic anhydride, 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride, 4,4'-bis(2,3-dicarboxylphenoxy)diphenyl ether acid dianhydride, p-phenylene bis(trimellitate anhydride), and 2,3,3',4'-biphenyltetracarboxylic dianhydride. Among these, the acid dianhydride used as the raw material for the imide oligomer is preferably an aromatic acid dianhydride having a melting point of 240°C or less, more preferably an aromatic acid dianhydride having a melting point of 220°C or less, even more preferably an aromatic acid dianhydride having a melting point of 200°C or less, and particularly preferably 3,4'-oxydiphthalic dianhydride (melting point 180°C) or 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride (melting point 190°C), because it has superior solubility and heat resistance. In this specification, the "melting point" refers to a value measured as the endothermic peak temperature when the temperature is increased at 10° C. / min using a differential scanning calorimeter. Examples of the differential scanning calorimeter include EXTEAR DSC6100 (manufactured by SII NanoTechnology Inc.).

[0066] Among the diamines represented by the above formula (10), examples of aromatic diamines include 3,3'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, 3,3'-diaminodiphenylsulfone, 4,4'-diaminodiphenylsulfone, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, bis(4-(4-aminophenoxy)phenyl)methane, 2,2-bis(4-aminophenoxy)phenyl)methane, and the like. Examples of suitable bis(4-(4-aminophenoxy)phenyl)propane, 1,3-bis(2-(4-aminophenyl)-2-propyl)benzene, 1,4-bis(2-(4-aminophenyl)-2-propyl)benzene, 3,3'-diamino-4,4'-dihydroxyphenylmethane, 4,4'-diamino-3,3'-dihydroxyphenylmethane, 3,3'-diamino-4,4'-dihydroxyphenyl ether, bisaminophenylfluorene, bistruidinefluorene, 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-diamino-3,3'-dihydroxyphenyl ether, 3,3'-diamino-4,4'-dihydroxybiphenyl, and 4,4'-diamino-2,2'-dihydroxybiphenyl.Among these, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl ether, 1,3-bis(2-(4-aminophenyl)-2-propyl)benzene, 1,4-bis(2-(4-aminophenyl)-2-propyl)benzene, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, and 1,4-bis(4-aminophenoxy)benzene are preferred due to their excellent availability, and 1,3-bis(2-(4-aminophenyl)-2-propyl)benzene, 1,4-bis(2-(4-aminophenyl)-2-propyl)benzene, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, and 1,4-bis(4-aminophenoxy)benzene are more preferred due to their excellent solubility and heat resistance.

[0067] Examples of the acid anhydride represented by the above formula (11) include phthalic anhydride, 3-methylphthalic anhydride, 4-methylphthalic anhydride, 1,2-naphthalic anhydride, 2,3-naphthalic anhydride, 1,8-naphthalic anhydride, 2,3-anthracene dicarboxylic anhydride, 4-tert-butylphthalic anhydride, 4-ethynylphthalic anhydride, 4-phenylethynylphthalic anhydride, 4-fluorophthalic anhydride, 4-chlorophthalic anhydride, 4-bromophthalic anhydride, and 3,4-dichlorophthalic anhydride.

[0068] Examples of the monoamine represented by the above formula (12) include aniline, o-toluidine, m-toluidine, p-toluidine, 2,4-dimethylaniline, 3,4-dimethylaniline, 3,5-dimethylaniline, 2-tert-butylaniline, 3-tert-butylaniline, 4-tert-butylaniline, 1-naphthylamine, 2-naphthylamine, 1-aminoanthracene, 2-aminoanthracene, 9-aminoanthracene, 1-aminopyrene, 3-chloroaniline, o-anisidine, m-anisidine, p-anisidine, 1-amino-2-methylnaphthalene, 2,3-dimethylaniline, 2,4-dimethylaniline, 2,5-dimethylaniline, 3,4-dimethylaniline, 4-ethylaniline, 4-ethynylaniline, 4-isopropylaniline, 4-(methylthio)aniline, and N,N-dimethyl-1,4-phenylenediamine.

[0069] Examples of the phenolic hydroxyl group-containing monoamine represented by the above formula (13) include 3-aminophenol, 4-aminophenol, 4-amino-o-cresol, 5-amino-o-cresol, 4-amino-2,3-xylenol, 4-amino-2,5-xylenol, 4-amino-2,6-xylenol, 4-amino-1-naphthol, 5-amino-2-naphthol, 6-amino-1-naphthol, 4-amino-2,6-diphenylphenol, etc. Among these, 4-amino-o-cresol and 5-amino-o-cresol are preferred because they are easily available and have excellent storage stability and can provide a high glass transition temperature after curing.

[0070] When the imide oligomer is produced by the above-mentioned production method, the imide oligomer is obtained as a mixture (imide oligomer composition) of multiple types of imide oligomers having the structure represented by the above formula (1-1) or multiple types of imide oligomers having the structure represented by the above formula (1-2) and each raw material. When an aliphatic triamine or aromatic triamine is used instead of the diamine represented by the above formula (10), the imide oligomer is obtained as a mixture (imide oligomer composition) of multiple types of imide oligomers having the structure represented by the above formula (2-1) or multiple types of imide oligomers having the structure represented by the above formula (2-2) and each raw material. Since the imide oligomer composition has an imidization rate of 70% or more, when used as a curing agent, a cured product having excellent mechanical strength at high temperatures and long-term heat resistance can be obtained. The lower limit of the imidization rate of the imide oligomer composition is preferably 75%, and more preferably 80%. There is no particular upper limit of the imidization rate of the imide oligomer composition, but the substantial upper limit is 98%. The above "imidization rate" is measured by the attenuated total reflection method (ATR method) using a Fourier transform infrared spectrophotometer (FT-IR), and is calculated based on the 1660 cm -1 The absorbance area of ​​the peak near the peak can be calculated by the following formula. An example of the Fourier transform infrared spectrophotometer is UMA600 (manufactured by Agilent Technologies). Note that the "peak absorbance area of ​​the amic acid oligomer" in the following formula refers to the absorbance area of ​​the amic acid oligomer obtained by reacting an acid dianhydride with a diamine or a phenolic hydroxyl group-containing monoamine and then removing the solvent by evaporation or the like without carrying out an imidization step. Imidization rate (%)=100×(1-(peak absorbance area after imidization) / (peak absorbance area of ​​amic acid oligomer))

[0071] From the viewpoint of solubility in the curable resin composition, the imide oligomer composition is preferably dissolved in an amount of 3 g or more in 10 g of tetrahydrofuran at 25°C.

[0072] The content of the imide oligomer in the total of 100 parts by weight of the curable resin and the heat curing agent (and the curing accelerator when the curing accelerator described later is further included) is preferably 20 parts by weight in lower limit and 80 parts by weight in upper limit. By the content of the imide oligomer being within this range, the obtained curable resin composition has better flexibility and processability before curing and better heat resistance after curing. The more preferable lower limit of the content of the imide oligomer is 25 parts by weight, and the more preferable upper limit is 75 parts by weight. In addition, when the imide oligomer is contained in the above-mentioned imide oligomer composition, the content of the imide oligomer means the content of the imide oligomer composition (when another imide oligomer is used in combination, the total content of the imide oligomer composition and the other imide oligomer).

[0073] The curable resin composition of the present invention preferably contains a curing accelerator. By containing the curing accelerator, the curing time can be shortened and the productivity can be improved.

[0074] Examples of the curing accelerator include imidazole-based curing accelerators, tertiary amine-based curing accelerators, phosphine-based curing accelerators, phosphorus-based curing accelerators, photobase generators, sulfonium salt-based curing accelerators, etc. Among these, imidazole-based curing accelerators are preferred because of their excellent storage stability.

[0075] The content of the curing accelerator is preferably 0.01 parts by weight at the lower limit and 10 parts by weight at the upper limit with respect to 100 parts by weight of the total of the curable resin, the heat curing agent, and the curing accelerator. By setting the content of the curing accelerator within this range, the effect of shortening the curing time while maintaining excellent adhesiveness, etc. is excellent. The more preferable lower limit of the content of the curing accelerator is 0.05 parts by weight, and the more preferable upper limit is 5 parts by weight.

[0076] The curable resin composition of the present invention preferably contains a polymer compound. By containing the polymer compound, the cured product of the obtained curable resin composition has excellent long-term heat resistance and is easy to form a sea-island structure. When the curable resin composition of the present invention contains the polymer compound, the polymer compound is usually a component that constitutes the island parts of the sea-island structure.

[0077] The weight-average molecular weight of the polymer compound is preferably 10,000 in lower limit and 200,000 in upper limit. When the weight-average molecular weight of the polymer compound is within this range, the resulting curable resin composition has better flexibility and processability before curing and better long-term heat resistance after curing, and the formation of a sea-island structure becomes easier. The weight-average molecular weight of the polymer compound is more preferably 20,000 in lower limit and 100,000 in upper limit.

[0078] The polymer compound preferably contains an aliphatic skeleton, which makes it easier to form an island-in-a-sea structure.

[0079] Examples of the polymer compound include polyimide, phenoxy resin, polyamide, polyamideimide, polymaleimide, cyanate resin, benzoxazine resin, acrylic resin, urethane resin, polyester, etc. Among these, from the viewpoint of heat resistance, polyimide, polyamide, polyamideimide, and polymaleimide are preferred, and polyimide is more preferred.

[0080] The content of the polymer compound is preferably 5 parts by weight at the lower limit and 50 parts by weight at the upper limit, relative to 100 parts by weight of the total of the curable resin and the heat curing agent (and the curing accelerator when the curing accelerator is contained). When the content of the polymer compound is within this range, the cured product of the obtained curable resin composition has excellent long-term heat resistance, and the formation of a sea-island structure becomes easier. The more preferred lower limit of the content of the polymer compound is 10 parts by weight, and the more preferred upper limit is 40 parts by weight.

[0081] The curable resin composition of the present invention may contain an inorganic filler as long as the object of the present invention is not impaired.

[0082] The inorganic filler is preferably at least one of silica and barium sulfate. By containing at least one of silica and barium sulfate as the inorganic filler, the curable resin composition of the present invention has excellent reflow resistance, plating resistance, and processability.

[0083] Examples of inorganic fillers other than the silica and barium sulfate include alumina, aluminum nitride, boron nitride, silicon nitride, glass powder, glass frit, glass fiber, carbon fiber, and inorganic ion exchangers.

[0084] As the inorganic filler, one having an average particle size of 50 nm or more and less than 4 μm is suitably used.

[0085] The content of the inorganic filler is preferably 200 parts by weight per 100 parts by weight of the total of the curable resin and the heat curing agent (and the curing accelerator if the curing accelerator is contained). By setting the content of the inorganic filler within this range, the cured product of the obtained curable resin composition has excellent reflow resistance and plating resistance while maintaining excellent tackiness. The more preferred upper limit of the content of the inorganic filler is 150 parts by weight.

[0086] The curable resin composition of the present invention preferably contains a flow control agent for the purposes of improving the coatability onto an adherend in a short period of time and shape retention. Examples of the flow regulator include fumed silica such as Aerosil, layered silicates, and the like. The flow control agent preferably has an average particle size of less than 100 nm.

[0087] The content of the flow regulator is preferably 0.1 parts by weight at the lower limit and 50 parts by weight at the upper limit with respect to 100 parts by weight of the total of the curable resin and the heat curing agent (and the curing accelerator if the curing accelerator is contained). By setting the content of the flow regulator within this range, the effect of improving the short-term application property to the adherend and the shape retention is excellent. The more preferable lower limit of the content of the flow regulator is 0.5 parts by weight, and the more preferable upper limit is 30 parts by weight.

[0088] The curable resin composition of the present invention may contain an organic filler for the purposes of stress relief, toughness, and the like. Examples of the organic filler include silicone rubber particles, acrylic rubber particles, urethane rubber particles, polyamide particles, polyamideimide particles, polyimide particles, benzoguanamine particles, and core-shell particles thereof. Among these, polyamide particles, polyamideimide particles, and polyimide particles are preferred.

[0089] The content of the organic filler is preferably 300 parts by weight per 100 parts by weight of the total of the curable resin and the heat curing agent (and the curing accelerator if the curing accelerator is contained). By having the content of the organic filler in this range, the cured product of the obtained curable resin composition has excellent toughness while maintaining excellent adhesiveness. The more preferable upper limit of the content of the organic filler is 200 parts by weight.

[0090] The curable resin composition of the present invention may contain a flame retardant within a range that does not impair the object of the present invention. Examples of the flame retardant include boehmite-type aluminum hydroxide, metal hydrates such as aluminum hydroxide and magnesium hydroxide, halogen-based compounds, phosphorus-based compounds, nitrogen compounds, etc. Among these, boehmite-type aluminum hydroxide is preferred.

[0091] The content of the flame retardant is preferably 200 parts by weight per 100 parts by weight of the total of the curable resin and the heat curing agent (and the curing accelerator if the curing accelerator is contained). By having the content of the flame retardant in this range, the obtained curable resin composition has excellent flame retardancy while maintaining excellent adhesiveness, etc. The more preferable upper limit of the content of the flame retardant is 150 parts by weight.

[0092] The curable resin composition may contain a solvent from the viewpoint of coatability and the like. From the viewpoints of coatability, storage stability, and the like, the solvent is preferably one having a boiling point of less than 200°C. Examples of the solvent having a boiling point of less than 200° C. include alcohol-based solvents, ketone-based solvents, ester-based solvents, hydrocarbon-based solvents, halogen-based solvents, ether-based solvents, and nitrogen-containing solvents. Examples of the alcohol solvent include methanol, ethanol, isopropyl alcohol, normal propyl alcohol, isobutyl alcohol, normal butyl alcohol, tertiary butyl alcohol, and 2-ethylhexanol. Examples of the ketone solvent include acetone, methyl ethyl ketone, methyl isobutyl ketone, methyl propyl ketone, diisobutyl ketone, cyclohexanone, methylcyclohexanone, and diacetone alcohol. Examples of the ester solvent include methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, methoxybutyl acetate, amyl acetate, n-propyl acetate, isopropyl acetate, methyl lactate, ethyl lactate, and butyl lactate. Examples of the hydrocarbon solvent include benzene, toluene, xylene, normal hexane, isohexane, cyclohexane, methylcyclohexane, ethylcyclohexane, isooctane, normal decane, and normal heptane. Examples of the halogen-based solvent include dichloromethane, chloroform, and trichloroethylene. Examples of the ether solvents include diethyl ether, tetrahydrofuran, 1,4-dioxane, 1,3-dioxolane, diisopropyl ether, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, 3-methoxy-3-methyl-1-butanol, ethylene glycol monotertiary butyl ether, propylene glycol monomethyl ether propionate, 3-methoxybutanol, diethylene glycol dimethyl ether, anisole, and 4-methylanisole. Examples of the nitrogen-containing solvent include acetonitrile, N,N-dimethylformamide, and N,N-dimethylacetamide. Among these, from the viewpoints of ease of handling, solubility of the imide oligomer, etc., at least one solvent selected from the group consisting of ketone solvents having a boiling point of 60° C. or more and less than 200° C., ester solvents having a boiling point of 60° C. or more and less than 200° C., and ether solvents having a boiling point of 60° C. or more and less than 200° C. is preferred. Examples of such solvents include methyl ethyl ketone, methyl isobutyl ketone, ethyl acetate, isobutyl acetate, 1,4-dioxane, 1,3-dioxolane, tetrahydrofuran, cyclohexanone, methylcyclohexanone, diethylene glycol dimethyl ether, anisole, etc. The above "boiling point" refers to a value measured under a condition of 101 kPa, or a value converted to 101 kPa using a boiling point conversion chart or the like.

[0093] The preferred lower limit of the content of the solvent in 100 parts by weight of the curable resin composition containing the solvent is 20 parts by weight, and the preferred upper limit is 90 parts by weight. By having the content of the solvent in this range, the obtained curable resin composition has better coatability, etc. The more preferred lower limit of the content of the solvent is 30 parts by weight, and the more preferred upper limit is 80 parts by weight.

[0094] The curable resin composition of the present invention may contain a reactive diluent within a range that does not impair the object of the present invention. From the viewpoint of adhesive reliability, the reactive diluent is preferably one having two or more reactive functional groups in one molecule.

[0095] The curable resin composition of the present invention may further contain additives such as a coupling agent, a dispersant, a storage stabilizer, a bleeding inhibitor, a fluxing agent, and a leveling agent.

[0096] The method for producing the curable resin composition of the present invention may, for example, be a method of mixing a curable resin, a photopolymerization initiator, a heat curing agent, and a curing accelerator, which is added as necessary, using a mixer. Examples of the mixer include a homodisper, a universal mixer, a Banbury mixer, and a kneader.

[0097] The curable resin composition of the present invention can be used in a wide range of applications, but is particularly suitable for electronic material applications requiring high heat resistance. For example, it can be used as a die attachment agent for aviation and in-vehicle electric control units (ECUs) and power devices using SiC and GaN. It can also be used as an adhesive for power overlay packages, a sealant, an adhesive for flexible printed circuit boards or coverlay films, a copper-clad laminate, an adhesive for semiconductor bonding, an interlayer insulating film, a prepreg, a sealant for LEDs, an adhesive for structural materials, and the like. In particular, it is suitable for bonding flexible printed circuit boards or coverlay films.

[0098] A cured product of the curable resin composition of the present invention also constitutes the present invention. The adhesive using the curable resin composition of the present invention is also one of the present inventions. The adhesive film can be obtained by applying the adhesive of the present invention onto a film and then drying it. The adhesive film using the adhesive of the present invention is also one of the present inventions. Effect of the Invention

[0099] According to the present invention, it is possible to provide a curable resin composition having excellent long-term heat resistance and stress relaxation property in a thermal cycle. Also, according to the present invention, it is possible to provide a cured product of the curable resin composition, and an adhesive and an adhesive film using the curable resin composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0100] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0101] (Preparation of Imide Oligomer Composition) 104 parts by weight of 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride (Tokyo Chemical Industry Co., Ltd.) was dissolved in 300 parts by weight of N-methylpyrrolidone (Fujifilm Wako Pure Chemical Industries, Ltd., "NMP"). A solution of 28 parts by weight of dimer diamine Priamine 1074 (Croda) diluted with 100 parts by weight of N-methylpyrrolidone was added to the obtained solution, and the mixture was stirred at 25°C for 2 hours to react, thereby obtaining an amic acid oligomer solution. After removing N-methylpyrrolidone from the obtained amic acid oligomer solution under reduced pressure, the mixture was heated at 300°C for 2 hours to obtain an imide oligomer composition (imidization rate 93%). The obtained imide oligomer composition was 1 It was confirmed by H-NMR, GPC, and FT-IR analyses that the imide oligomer composition contained an aliphatic diamine residue having the structure represented by the above formula (4-1) or (4-3) (A is a 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride residue, and B is a dimer diamine residue). The weight average molecular weight of the imide oligomer composition was 2200.

[0102] (Synthesis Example 1 (Preparation of Polyimide Resin Solution A)) 50.5 parts by weight of 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride (manufactured by Tokyo Chemical Industry Co., Ltd.) and 200 parts by weight of cyclohexanone were charged and dissolved in a reaction vessel equipped with a stirrer, a water divider, and a nitrogen gas inlet tube. A mixed solution of 46.8 parts by weight of dimer diamine Priamine 1074 (manufactured by Croda) and 55.0 parts by weight of cyclohexanone was dropped into the obtained solution, and then an imidization reaction was carried out at 150 ° C. for 8 hours. Next, 40 parts by weight of toluene was charged as a dehydrating agent, and water accompanying the ring closure of polyimide was expelled into a moisture trap device while refluxing toluene at 180 ° C. for 3 hours, and then stirring was carried out for 4 hours while removing water and toluene via the moisture trap device to obtain a polyimide resin solution A. The solid content concentration of the obtained polyimide resin solution A was 30% by weight, and the weight average molecular weight of the polyimide resin was 20,000.

[0103] (Synthesis Example 2 (Preparation of Polyimide Resin Solution B)) A polyimide resin solution B was obtained in the same manner as in "(Preparation of polyimide resin solution A)" above, except that 45.8 parts by weight of dimer diamine Priamine 1074 (manufactured by Croda) was used. The solid content of the obtained polyimide resin solution B was 29% by weight, and the weight average molecular weight of the polyimide resin was 30,000.

[0104] (Synthesis Example 3 (Preparation of Polyimide Resin Solution C)) A polyimide resin solution C was obtained in the same manner as in "(Preparation of polyimide resin solution A)" above, except that 15.6 parts by weight of dimer diamine Priamine 1074 (manufactured by Croda) was used. The solid content concentration of the obtained polyimide resin solution C was 25% by weight, and the weight average molecular weight of the polyimide resin was 5,000.

[0105] (Examples 1 to 5, Comparative Examples 1 and 2) According to the compounding ratios shown in Table 1, the materials were mixed by stirring to prepare the curable resin compositions of Examples 1 to 5 and Comparative Examples 1 and 2.

[0106] (Initial adhesive strength of cured product to silicon chip) Each of the obtained curable resin compositions was applied to a polyimide substrate having a length of 10 mm and a width of 10 mm, and a silicon chip having a length of 50 μm, a width of 3 mm, and a thickness of 3 mm was overlaid. The curable resin composition was then cured by heating at 190° C. for 1 hour to obtain a test piece. The die shear strength of the obtained test piece was measured at a speed of 100 μm / s at 25° C. using a die shear tester, and the obtained die shear strength was taken as the initial adhesive strength of the cured product to the silicon chip. Kapton 200H (manufactured by Toray DuPont Co., Ltd., surface roughness 0.03 to 0.07 μm) was used as the polyimide substrate, and a silicon chip (surface roughness 0.5 to 1.0 nm) manufactured by Global Wafer Co., Ltd. was used as the silicon chip, and DAGE4000 (manufactured by Nordson Co., Ltd.) was used as the die shear tester. The results are shown in Table 1.

[0107] (Adhesion strength of cured material to silicon chip after storage at 150℃ for 1000 hours) The test pieces obtained in the same manner as in "(Initial adhesive strength of the cured product to the silicon chip)" above were stored in an oven at 150°C for 1000 hours. Next, the test pieces after storage were subjected to die shear at a speed of 100 μm / s using a die shear tester to measure the adhesive strength. The obtained adhesive strength was taken as the adhesive strength of the cured product to the silicon chip after storage at 150°C for 1000 hours. The results are shown in Table 1.

[0108] (glass transition temperature) Each of the curable resin compositions obtained in the Examples and Comparative Examples was applied to a substrate PET film to a thickness of about 20 μm, and dried to prepare a curable adhesive film on the substrate PET film. Each of the obtained curable adhesive films was laminated to a thickness of about 300 μm, cut into a width of 3 mm and a length of 5 cm, and cured by heating at 190° C. for 1 hour to prepare a cured product. The dynamic viscoelasticity of each of the obtained cured products was measured in the range of 30°C to 300°C using a dynamic viscoelasticity measuring device (SII Corporation, "EXSTAR6000") under the following conditions: deformation mode: tensile, strain amplitude: 10 μm, measurement frequency: 10 Hz, and heating rate: 10°C / min. The temperature at which the loss tangent (tan δ) was maximized was determined as the glass transition temperature. The results are shown in Table 1.

[0109] (Presence or absence of island structure) Each of the curable resin compositions obtained in the Examples and Comparative Examples was applied to a substrate PET film to a thickness of about 20 μm, and dried to prepare a curable adhesive film on the substrate PET film. Each of the obtained curable adhesive films was laminated to a thickness of about 300 μm, cut into a width of 3 mm and a length of 5 cm, and cured by heating at 190° C. for 1 hour to prepare a cured product. The obtained cured product was observed using a transmission electron microscope at magnifications of 2,000 to 10,000 to confirm the presence or absence of a sea-island structure. The results are shown in Table 1.

[0110] <Evaluation> The curable resin compositions obtained in the Examples and Comparative Examples were evaluated as follows. The results are shown in Table 1.

[0111] (Solubility of polymer compound in curable resin composition) The state of each of the curable resin compositions obtained in the Examples and Comparative Examples was visually observed after storage for 30 days at -15°C. The solubility of each of the curable resin compositions was evaluated by rating it as "○" when it was homogeneous and "×" when separation or precipitation was observed.

[0112] (Long term heat resistance) Each of the curable resin compositions obtained in the examples and comparative examples was coated on a substrate PET film to a thickness of about 20 μm, and dried to prepare a curable resin composition film on the substrate PET film. The substrate PET film was peeled off from the obtained curable resin composition film, and a 20 μm-thick polyimide film (manufactured by Toray DuPont Co., Ltd., "Kapton V") was laminated on both sides, and the film was cured by heating at 190°C for 1 hour to obtain a test piece. The obtained test piece was subjected to a heat treatment at 150°C for 1000 hours. The test piece after the heat treatment was visually observed to confirm the presence or absence of cracks in the cured product of the curable resin composition. The long-term heat resistance was evaluated as "○" when no cracks or cracks were observed, and "×" when cracks or cracks were observed.

[0113] (heat cycle test) A thermal cycle test was carried out for test pieces obtained in the same manner as in "(Initial adhesive strength of the cured product to a silicon chip)" above, in which 1000 cycles were performed, with one cycle being -55°C / 30 minutes and 200°C / 30 minutes. After the thermal cycle test, the test pieces were observed under an optical microscope to confirm the presence or absence of cracks in the cured product of the curable resin composition. The test pieces were evaluated as "○" when no cracks or breaks were observed, and as "×" when cracks or breaks were observed. In addition, the test pieces after the thermal cycle test were subjected to die shear at a speed of 100 μm / s using a die shear tester, and the adhesive strength was measured. The die shear tester used was DAGE4000 (manufactured by Nordson).

[0114] [Table 1] [Industrial Applicability]

[0115] According to the present invention, it is possible to provide a curable resin composition having excellent long-term heat resistance and stress relaxation property in a thermal cycle. Also, according to the present invention, it is possible to provide a cured product of the curable resin composition, and an adhesive and an adhesive film using the curable resin composition.

Claims

1. Contains a curable resin, a curing agent, and a polymer compound; the curable resin comprises an epoxy resin, the curing agent comprises an imide oligomer; The polymer compound has a weight average molecular weight of 10,000 or more and 200,000 or less, The initial adhesive strength of the cured product to the silicon chip is 5.0 N / mm 2 That's all. After storage at 150°C for 1000 hours, the adhesive strength of the cured product to a silicon chip was 5.0 N / mm 2 And, The cured product has an island-sea structure. A curable resin composition comprising:

2. 2. The curable resin composition according to claim 1, wherein the cured product has a low-temperature glass transition temperature in the range of 30°C or higher and 160°C or lower and a high-temperature glass transition temperature in the range of 150°C or higher and 200°C or lower.

3. The curable resin composition according to claim 1 or 2, wherein the imide oligomer has a weight average molecular weight of 500 or more and 5,000 or less.

4. A cured product of the curable resin composition according to claim 1, 2 or 3.

5. An adhesive comprising the curable resin composition according to claim 1, 2, 3 or 4.

6. An adhesive film obtained by using the adhesive according to claim 5.

Citation Information

Patent Citations

  • Semiconductor device

    JP1986270852A

  • Curable resin composition

    JP1991269047A

  • Polyimide hybrid adhesive

    JP2004502859A

  • Resin material, laminate film and multilayer printed wiring board

    JP2019173010A