Stainless steel slag, its manufacturing method, and material for burial in soil
By controlling the composition and particle size of stainless steel slag components, the elution of hexavalent chromium is suppressed, addressing production challenges and enabling its use in construction materials and underground burial applications.
Patent Information
- Application Number
- JP2021022057
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-15
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2041-02-15
AI Technical Summary
Conventional methods for producing stainless steel slag face challenges in uniformly mixing divalent S compounds, require high temperatures for slag treatment, necessitate non-oxidizing atmospheres, and struggle with the elution of hexavalent chromium, leading to increased costs and environmental concerns.
Control the composition of stainless steel slag by adjusting the proportions of Cr2O3, Al2O3, MgO, Mn, and S, and limit the average particle size of the MnS phase to 25.0 μm or less, while cooling the slag to maintain a surface temperature above 500°C for 10 hours or less.
The solution effectively suppresses the elution of hexavalent chromium, enabling the slag's use in road and civil engineering materials, particularly for underground burial, while reducing energy consumption and operational costs.
Smart Images

Figure 0007564011000004 
Figure 0007564011000001 
Figure 0007564011000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a stainless steel slag and a method for producing the same, as well as a material for burial in the ground. [Background technology]
[0002] In the manufacture of stainless steel, steelmaking slag is generally generated when raw materials are melted to obtain molten stainless steel (hereinafter referred to as the "melting process") and when the molten stainless steel is refined (hereinafter referred to as the "refining process"). Such steelmaking slag contains oxides such as SiO2 and Al2O3, which are formed by oxidizing Si and Al in the molten stainless steel, and CaO and MgO, which are contained in the refractories of the melting furnace. Steelmaking slag also contains Cr oxides, which are generated by the oxidation of part of Cr during the low-temperature period of the melting process and the oxygen-blowing period of the refining process. Depending on the conditions during slag discharge and cooling, some of the Cr oxides may turn into small amounts of hexavalent chromium, which has been a cause for concern in the utilization of steelmaking slag as a resource (for example, for use in road materials and civil engineering materials).
[0003] Therefore, as a method for suppressing the elution of hexavalent chromium, Patent Document 1 proposes a method for modifying stainless steel slag in which, after decarburization smelting of stainless steel and reduction treatment, molten chromium oxide-containing slag is subjected to agitation with an inert gas injected thereinto to add a divalent S compound such as FeS, thereby increasing the S concentration in the slag to 0.20 wt% or more. However, this method has the difficulty of uniformly mixing the divalent S compounds with the chromium-containing slag, and therefore, when the stainless steel slag obtained by this method comes into contact with water, the divalent S compounds dissolve, resulting in the production of "yellow water," which is yellow in color.
[0004] Moreover, Patent Document 2 proposes a method for treating chromium-containing steel refining slag in which the basicity (CaO / SiO2) of the slag is adjusted to 1.2 or less, free unformed CaO is turned into slag, and then the slag is discharged. However, this method requires the temperature to be kept at 1550° C. or higher in order to completely convert the free undissolved CaO into slag, which increases the amount of power consumed and is very costly.
[0005] Furthermore, Patent Document 3 proposes a method for treating Cr2O3-containing slag in which the slag is cooled in a non-oxidizing atmosphere to a predetermined temperature according to the ratio of the amount of Cr contained in MgO·Cr2O3 to the total amount of Cr contained in the slag containing Cr2O3. However, this method requires a sealed container to provide a non-oxidizing atmosphere in actual operation, and the cost, including the use of the non-oxidizing atmosphere, is very high.
[0006] Furthermore, Patent Document 4 proposes a method for modifying chromium oxide-containing slag, in which 1 to 30% by weight of aluminum ash and 0.5 to 15% by weight of magnesia-based industrial waste are added to the molten chromium oxide-containing slag, based on the total weight after addition. However, with this method, it is difficult to uniformly mix the molten chromium oxide-containing slag with the aluminum ash and magnesia-based industrial waste, and the amount of chromium oxide-containing slag increases due to the aluminum ash and magnesia-based industrial waste. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Japanese Patent Application Publication No. 8-104553 [Patent Document 2] JP 2003-301215 A [Patent Document 3] JP 2014-237556 A [Patent Document 4] Japanese Patent Application Publication No. 6-171993 Summary of the Invention [Problem to be solved by the invention]
[0008] Conventional methods and the stainless steel slag obtained thereby have various problems as described above, and therefore there has been a demand for stainless steel slag and a method for producing the same that does not cause the above-mentioned problems. Therefore, the present invention has been made to solve the above-mentioned problems, and aims to provide a stainless steel slag that can suppress the leaching of hexavalent chromium, a method for producing the same, and a material for burial in the ground. [Means for solving the problem]
[0009] As a result of extensive research into stainless steel slag, the inventors have found that the composition (particularly the contents of Cr2O3, Al2O3, MgO, Mn, and S) and the average particle size of the MnS phase are closely related to the elution of hexavalent chromium. They have also found that the above problems can be solved by controlling the composition of stainless steel slag and the average particle size of the MnS phase, and have completed the present invention. The inventors also discovered that the composition of the stainless steel slag and the average particle size of the MnS phase can be controlled by controlling the composition of the molten stainless steel and the cooling conditions of the produced steelmaking slag (particularly, the time during which the surface temperature is 500°C or higher), and thus completed the present invention.
[0010] That is, the present invention comprises CaO and SiO2 in a total amount of 50 mass% or more, When the total amount of Cr2O3, CaO, SiO2, Al2O3, MgO, Mn, S and F is taken as 100 mass%, Cr2O3 is 0.2 to 8.0 mass%, Al2O3 is 2.0 to 15.0 mass%, MgO is 3.0 to 20.0 mass%, Mn is 0.10 to 5.00 mass%, S is 0.010 to 0.500 mass%, and F is 0.50 mass% or less, The basicity (CaO / SiO2) is 0.8 to 1.5. The stainless steel slag has an average particle size of MnS phase of 25.0 μm or less.
[0011] The present invention also provides a method for producing the stainless steel slag, comprising the steps of: The C concentration is 1.7 mass% or more, the Si concentration is 0.2 mass% or more, and X represented by formula (1) is 10.0 or less. By melting and refining the raw materials Controlling the composition of the molten stainless steel; Above the molten stainless steel The resulting steelmaking slag When the stainless steel is separated from the molten steel and cooled, surface temperature but A step of cooling the material so that the time at or above 500°C is 10 hours or less. The present invention relates to a method for producing stainless steel slag, the method comprising the steps of: X=Cr / (0.5×C+Si+Mn) (1) In the formula, Cr, C, Si, and Mn represent the contents (mass%) of the respective elements.
[0012] Furthermore, the present invention relates to a material for burial in the ground, which contains the stainless steel slug. Effect of the Invention
[0013] According to the present invention, it is possible to provide a stainless steel slag capable of suppressing the elution of hexavalent chromium, a method for producing the same, and a material to be buried in the ground. [Brief description of the drawings]
[0014] [Figure 1] FIG. 2 is a schematic diagram of an SEM image of a cross section of a stainless steel slug according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The following is a detailed description of the embodiments of the present invention. The present invention is not limited to the following embodiments, and it should be understood that modifications and improvements to the following embodiments, which are made based on the ordinary knowledge of those skilled in the art, fall within the scope of the present invention, without departing from the spirit of the present invention.
[0016] The stainless steel slag (hereinafter, sometimes simply referred to as "slag") according to an embodiment of the present invention is obtained by solidifying steelmaking slag that is generated during the melting process in which raw materials are melted to obtain molten stainless steel and the refining process in which the molten stainless steel is refined. The method for refining stainless steel is not particularly limited, and can be carried out in accordance with a method known in the art using an electric furnace, a converter, or the like. For example, raw materials are charged into an electric furnace and heated to produce molten stainless steel, and then the molten stainless steel is refined by blowing oxygen into the lance. After completion of refining, the steelmaking slag in the electric furnace is discharged into a container (e.g., a slag pot), cooled and solidified to produce stainless steel slag.
[0017] The slag is mainly composed of CaO and SiO2. That is, the slag contains CaO and SiO2 in a total amount of 50 mass% or more. CaO is added as a deoxidizing and desulfurizing agent during refining, and is also added to prevent the refractories in the furnace from melting when the raw materials are melted; it is a component contained in slag. SiO2 is produced by the oxidation of Si, a deoxidizing element, in molten stainless steel, and is a component contained in slag.
[0018] The basicity of slag (CaO / SiO2) is 0.8 to 1.5. If the basicity is less than 0.8, the S concentration in the slag decreases, resulting in more hexavalent chromium elution. On the other hand, if the basicity is more than 1.5, CaS is generated in the slag and elutes into the water, causing yellow water.
[0019] The slag further contains Cr2O3, Al2O3, MgO, Mn, S and F. Cr2O3 is produced by the oxidation of Cr in molten stainless steel and is a component contained in slag. The Cr2O3 content in the slag is 0.2-8.0 mass%, preferably 0.5-6.0 mass%, when the total amount of Cr2O3, CaO, SiO2, Al2O3, MgO, Mn, S and F is taken as 100 mass%. If the Cr2O3 content is less than 0.2 mass%, hexavalent chromium is not generated, and therefore the present invention is not applicable. On the other hand, if the Cr2O3 content exceeds 8.0 mass%, the amount of hexavalent chromium eluted increases and much of the valuable metal Cr is wasted.
[0020] Al2O3 is a component contained in slag that is produced when the refractories in the furnace melt during the melting of raw materials and when Al, a deoxidizing element, is oxidized in molten stainless steel. The content of Al2O3 in the slag is 2.0-15.0% by mass, preferably 5.0-12.0% by mass, when the total amount of Cr2O3, CaO, SiO2, Al2O3, MgO, Mn, S and F is taken as 100% by mass. If the content of Al2O3 is less than 2.0% by mass, the melting property of the slag decreases and the viscosity increases. As a result, it becomes difficult to remove the slag, and it becomes unsuitable for operation. On the other hand, if the content of Al2O3 exceeds 15.0% by mass, the amount of MgO·Al2O3·Cr2O3, which is the cause of the generation of hexavalent chromium, increases, and the amount of hexavalent chromium eluted increases.
[0021] MgO is contained in the slag due to the melting of the furnace refractories when the raw materials are melted, and is also a component that is added for the purpose of suppressing the melting of the furnace refractories. The content of MgO in the slag is 3.0-20.0% by mass, preferably 4.0-18.0% by mass, when the total amount of Cr2O3, CaO, SiO2, Al2O3, MgO, Mn, S and F is taken as 100% by mass. If the content of MgO is less than 3.0% by mass, the refractory material in the melting furnace is severely damaged. On the other hand, if the content of MgO exceeds 20.0% by mass, the amount of MgO·Al2O3·Cr2O3, which is the cause of the generation of hexavalent chromium, increases, and the amount of hexavalent chromium eluted increases.
[0022] MnO and MnS are components that are produced by oxidation and / or sulfurization of Mn in the molten stainless steel and are contained in the slag. Thus, Mn exists in the form of MnO and MnS in the slag after cooling and solidification, but since it is difficult to distinguish between these compounds based on their composition, the composition is specified as Mn in the present invention. The Mn content in the slag is 0.10-5.00 mass%, preferably 0.50-3.00 mass%, when the total amount of Cr2O3, CaO, SiO2, Al2O3, MgO, Mn, S and F is taken as 100 mass%. If the Mn content is less than 0.10 mass%, it becomes difficult to generate MnS, which is effective in suppressing the generation of hexavalent chromium, and the amount of hexavalent chromium eluted increases. On the other hand, if the Mn content exceeds 5.00 mass%, a large amount of Mn, which is a valuable metal, is wasted.
[0023] S is a component contained in the raw material (molten stainless steel) and is contained in the slag. The content of S in the slag is 0.010 to 0.500 mass%, preferably 0.050 to 0.500 mass%, when the total amount of Cr2O3, CaO, SiO2, Al2O3, MgO, Mn, S and F is taken as 100 mass%. If the content of S is less than 0.010 mass%, it becomes difficult to form MnS, which is effective in suppressing the formation of hexavalent chromium, and the amount of hexavalent chromium eluted increases. On the other hand, if the content of S exceeds 0.500 mass%, CaS is formed in the slag and elutes into water, causing yellow water.
[0024] F is included in the slag former (CaF2) and is a component contained in the slag. The slag former is used to lower the melting point of the slag, improve the fluidity of the slag, and increase the reactivity with molten stainless steel. Note that since it is difficult to distinguish CaF2 from CaO in terms of its chemical composition, the composition of CaF2 is specified as F in the present invention. The F content in the slag is 0.50% by mass or less, preferably 0.30% by mass or less, when the total amount of Cr2O3, CaO, SiO2, Al2O3, MgO, Mn, S and F is taken as 100% by mass. If the F content exceeds 0.50% by mass, the water solubility of the slag increases, and the amount of hexavalent chromium and F eluted increases. The lower limit of the F content is not particularly limited and may be zero, but is preferably 0.01 mass %.
[0025] If necessary, the slag may further contain at least one selected from Fe, Ti, B and P. These components are contained in the raw materials and various additives, and are contained in the slag. The contents of these components in the slag (total amount of slag) are not particularly limited since they have almost no effect on the elution of hexavalent chromium, but the total amount is preferably 5.00 mass % or less, more preferably 4.50 mass % or less.
[0026] In addition to the above components, the slag may contain unavoidable impurities. Inevitable impurities include trace components contained in the raw materials and trace components unintentionally mixed in during each process.
[0027] The slag may contain a MgO·Al2O3·Cr2O3 phase, and preferably contains a MnS phase. These phases can be identified by observing a cross section of the slag with a SEM. A schematic diagram of an SEM image of a cross section of the slag is shown in Figure 1. As shown in Figure 1, the slag contains a phase 10 containing CaO and SiO2, an MnS phase 20, and an MgO·Al2O3·Cr2O3 phase 30. The MnS phase is a phase in which the Mn concentration is 20 mass% or more and the S concentration is 20 mass% or more. The MgO·Al2O3·Cr2O3 phase is a phase in which the Mg concentration is 10 mass% or more, the Al concentration is 10 mass% or more, and the Cr concentration is 10 mass% or more.
[0028] The inventors prepared slags with various compositions and investigated the MnS and MgO·Al2O3·Cr2O3 phases in the slags. As a result, they found that the average particle size of the MnS phase in particular is closely related to the elution of hexavalent chromium. From the viewpoint of suppressing the elution of hexavalent chromium, the average particle size of the MnS phase is 25.0 μm or less, preferably 10.0 μm or less. If the average particle size of the MnS phase exceeds 25.0 μm, the number density of the MnS phase decreases. As a result, when the stainless steel slag is crushed, when the MgO·Al2O3·Cr2O3 phase is exposed on the surface, there is not enough MnS phase in the vicinity thereof, and Cr is easily oxidized, so that the effect of suppressing the elution of hexavalent chromium is not sufficiently obtained. On the other hand, the lower limit of the average particle size of the MnS phase is not particularly limited, but is preferably 0.50 μm, and more preferably 1.0 μm. In this specification, the average particle size refers to the average value of the equivalent circle diameter measured in a SEM image of the cross section of the slag. The equivalent circle diameter refers to the diameter of a circle having an area equal to the area of the phase appearing on the observed surface.
[0029] On the other hand, the average particle size of the MgO·Al2O3·Cr2O3 phase is not particularly limited because it does not have much effect on the dissolution of hexavalent chromium. The typical average particle size of the MgO·Al2O3·Cr2O3 phase is 10.0 to 50.0 μm.
[0030] The amount of the MnS phase in the slag is not particularly limited, but from the viewpoint of stably suppressing the elution of hexavalent chromium, it is preferably 0.01 to 2.00% by volume, and more preferably 0.01 to 1.50% by volume. The amount of the MgO·Al2O3·Cr2O3 phase in the slag is not particularly limited, but from the viewpoint of stably suppressing the elution of hexavalent chromium, it is preferably 0.01 to 20.00 volume %, more preferably 0.10 to 15.00 volume %, and even more preferably 1.00 to 12.00 volume %. The volume ratio of the MnS phase to the MgO·Al2O3·Cr2O3 phase (MnS phase / MgO·Al2O3·Cr2O3 phase) is preferably 0.004 or more, more preferably 0.005 or more. The upper limit of the volume ratio is not particularly limited, but is preferably 0.500, more preferably 0.100, and even more preferably 0.080.
[0031] In this specification, the amounts of the MnS phase and the MgO·Al2O3·Cr2O3 phase were estimated as the volume fraction (volume%) of each phase, calculated from the area ratio of each phase in the observation field of the SEM image of the slag cross section.
[0032] The stainless steel slag according to an embodiment of the present invention having the above-mentioned characteristics can be produced by a method including a step of controlling the composition of molten stainless steel so that the C concentration is 1.7 mass% or more, the Si concentration is 0.2 mass% or more, and X represented by formula (1) is 10.0 or less (hereinafter referred to as the "composition control step"), and a step of cooling the produced steelmaking slag so that the time during which the surface temperature is 500°C or higher is 10 hours or less (hereinafter referred to as the "cooling step"). X=Cr / (0.5×C+Si+Mn) (1) In the formula, Cr, C, Si, and Mn represent the contents (mass%) of the respective elements.
[0033] <Composition control process> The upper limit of the C concentration in the molten stainless steel is not particularly limited, but is preferably 5.0 mass %, and more preferably 4.5 mass %. The upper limit of the Si concentration in the molten stainless steel is not particularly limited, but is preferably 3.0 mass %, and more preferably 2.0 mass %. The respective concentrations of Cr and Mn in the molten stainless steel are not particularly limited as long as they are within the ranges where X represented by formula (1) falls within the above range. A typical Cr concentration in the molten stainless steel is 8.0 to 25.0 mass%. A typical Mn concentration in the molten stainless steel is 0.1 to 7.0 mass%. In addition to the above components, the molten stainless steel may contain components that are generally contained in stainless steels, such as Ni, Mo, and N, although these are not specifically mentioned because they have little effect on the effects of the present invention.
[0034] The method for controlling the composition of the molten stainless steel is not particularly limited, and can be carried out, for example, by adjusting the amounts of additives such as deoxidizers (Si, Al), deoxidizers / desulfurizers (CaO), refractory corrosion inhibitors (MgO), etc. Also, the types of raw materials may be selected and used so that the molten stainless steel has the above-mentioned composition.
[0035] The composition control process may be part of a melting process in which raw materials are melted to obtain molten stainless steel, or a refining process in which the molten stainless steel is refined. In the composition control process, the steelmaking slag formed above the molten stainless steel is separated from the molten stainless steel and discharged into a container (e.g., a slag pot).
[0036] <Cooling process> The steelmaking slag produced as described above is solidified in a cooling process to become stainless steel slag. In the cooling process, the steelmaking slag is cooled so that the time when the surface temperature is above 500°C is 10 hours or less. If the time when the surface temperature is above 500°C exceeds 10 hours, the MnS phase inside the slag coarsens and the number density of the MnS phase decreases. In addition, the MnS phase may separate into the CaSO4 phase or the MnO component in the slag, making it difficult to control the volume ratio of the MnS phase to the MgO·Al2O3·Cr2O3 phase within an appropriate range. As a result, when the stainless steel slag is crushed, there is not enough MnS phase near the MgO·Al2O3·Cr2O3 phase when it is exposed on the surface, and Cr is easily oxidized, so the effect of suppressing the elution of hexavalent chromium is not fully obtained. The cooling method is not particularly limited as long as it is a method that can satisfy the above cooling conditions, but it is preferable to use a method of cooling by spraying water onto a container in which the steelmaking slag has been discharged, a method of immersing the container together with the slag in a water tank, or a method of immersing only the slag in a water tank.
[0037] The stainless steel slag according to the embodiment of the present invention can suppress the elution of hexavalent chromium, and therefore can be used in various applications such as road materials, civil engineering materials, building materials, etc. Among these, the stainless steel slag is preferably used as a material to be buried in the ground.
[0038] A material for burial in soil according to an embodiment of the present invention includes the above-mentioned stainless steel slug. The stainless steel slag used as material for underground burial is preferably adjusted by crushing to a particle size of less than 40 mm. The content of the stainless steel slag in the material to be buried in the ground is not particularly limited, but is preferably 20 to 40 mass %.
[0039] The material to be buried in soil according to the embodiment of the present invention may further contain, in addition to the stainless steel slag, at least one selected from blast furnace slag, a solidification aid, an admixture, and an alkali irritant, if necessary. The content of blast furnace slag in the material to be buried in the earth is not particularly limited, but is preferably 40 to 60 mass %. The solidification aid is not particularly limited, but may be, for example, a silica-containing substance, a material having pozzolanic activity, gypsum, Portland cement, etc. The silica-containing substance and the material having pozzolanic activity may be, for example, coal ash, various cements (blast furnace cement, silica cement, fly ash cement, etc.). Among these, from the viewpoint of effective use of stainless steel slag, blast furnace cement and fly ash are preferred. The content of the solidification aid in the material to be buried in the ground is not particularly limited, but is preferably 10 to 30 mass%.
[0040] The admixture is not particularly limited, but examples thereof include dispersants containing cationic surfactants, anionic surfactants, nonionic surfactants, amphoteric surfactants, polymeric dispersants, etc. The amount of the admixture is not particularly limited, but is preferably 0.1 to 5 parts by mass per 100 parts by mass of the total of the stainless steel slag, blast furnace slag, and solidification aid. Examples of the alkaline stimulant include, but are not limited to, hydroxides, carbonates, sulfates, and chlorides of alkaline earth metals such as sodium hydroxide, calcium hydroxide, sodium carbonate, and calcium carbonate, or amines such as triethylamine, diethylamine, n-butylamine, p-dimethylaminoethanol, and triethanolamine, or quaternary ammonium salts such as ammonia, tetramethylammonium hydroxide, tetramethylammonium fluoride, tetra-n-butylammonium fluoride, and benzyltrimethylammonium fluoride. The amount of the alkaline stimulant is not particularly limited, but is preferably 0.1 to 5 parts by mass with respect to a total of 100 parts by mass of the stainless steel slag, blast furnace slag, and solidification aid. EXAMPLES
[0041] The present invention will be described in detail below with reference to examples, but the present invention should not be construed as being limited to these.
[0042] The raw materials for stainless steel were placed in an electric furnace and heated to produce molten stainless steel, after which the amounts of deoxidizers (Si, Al) and deoxidizer / desulfurizer (CaO) added were adjusted to control the composition as shown in Table 1.
[0043] [Table 1]
[0044] After melting, the steelmaking slag formed on the top of the molten stainless steel was separated from the molten stainless steel and discharged into an iron container (5 to 10 t). Next, the iron container was cooled by spraying water in the air so that the time during which the steelmaking slag had a surface temperature of 500°C or higher was the condition shown in Table 2, and stainless steel slag was obtained. The composition of the obtained stainless steel slag is shown in Table 2. The composition of the stainless steel slag was determined by fluorescent X-ray analysis. However, the F content was determined by ion electrode analysis. In the fluorescent X-ray analysis, the stainless steel slag was crushed in advance with a vibrating mill, and the obtained powder was pressed to prepare a powder briquette, which was used as a sample for fluorescent X-ray analysis. For the fluorescent X-ray analysis, a Shimadzu MXF-2100 (X-ray target: Rh) was used, and the output of the X-ray source was set to a tube voltage of 45 kV and a tube current of 60 mA. In addition, in the ion electrode analysis, the stainless steel slag was alkali-melted to prepare a solution, which was used as a sample for ion electrode analysis. For the ion electrode analysis, Orion Dual Star (registered trademark) manufactured by Thermo Scientific was used. In addition, in the composition of the stainless steel slag, the contents of CaO, SiO2, Fe, Ti, B, and P are the contents when the entire stainless steel slag is taken as 100%, and the contents of Cr2O3, Al2O3, MgO, Mn, S, and F are the contents when the total amount of Cr2O3, CaO, SiO2, Al2O3, MgO, Mn, S, and F is taken as 100 mass%.
[0045] [Table 2]
[0046] The stainless steel slag obtained above was cut, and the cut surface was dry-cut and then observed with an SEM. In the SEM observation, the presence or absence of undissolved CaO was confirmed, and the amount of MnS phase and MgO·Al2O3·Cr2O3 phase within the observation field was determined. The amount (volume %) of MnS phase and MgO·Al2O3·Cr2O3 phase was determined by the above method. The volume ratio of MnS phase / MgO·Al2O3·Cr2O3 phase was also calculated from the results. In addition, the circle equivalent diameters of 20 randomly selected MnS phase particles within a visual field of 1 mm x 1 mm or more obtained by SEM observation were measured, and the average value was taken as the average particle size of the MnS phase.
[0047] Next, the stainless steel slag obtained above was pulverized and a hexavalent chromium elution test was conducted. This test was conducted based on the elution test method in accordance with Environment Agency Notification No. 46, which is the inspection method for soil environmental standards. The grain size of the stainless steel slag used in the elution test was adjusted to 2 mm or less in accordance with Environment Agency Notification No. 46. If the amount of eluted hexavalent chromium is 0.05 mg / L or less, it can be considered as passing. The results of the above evaluations are shown in Table 3.
[0048] [Table 3]
[0049] As shown in Table 3, the stainless steel slags Nos. 1 to 10 (examples of the present invention) had a small amount of hexavalent chromium eluted. In contrast, the No. 11 stainless steel slag (comparison example) contained too much Cr2O3, resulting in a large amount of hexavalent chromium eluted. This is believed to be due to the formation of more MgO·Al2O3·Cr2O3 phase than MnS phase. The No. 12 stainless steel slag (comparison example) contained too much Al2O3, resulting in a large amount of hexavalent chromium eluted. This is believed to be due to the formation of more MgO·Al2O3·Cr2O3 phase than MnS phase. The No. 13 stainless steel slag (comparison example) had a large amount of hexavalent chromium eluted because the S content was too low. This is thought to be because the MnS phase was generated in smaller amounts than the MgO·Al2O3·Cr2O3 phase.
[0050] The stainless steel slag No. 14 (comparison example) had too little Mn content and too high basicity, resulting in a large amount of hexavalent chromium eluted. This is believed to be due to the formation of less MnS phase compared to the MgO·Al2O3·Cr2O3 phase. In the case of the stainless steel slag No. 15 (comparative example), the average particle size of the MnS phase was too large, resulting in a large amount of hexavalent chromium eluted. The MnS phase was coarsened because the cooling rate of the steelmaking slag was slow during the manufacturing process of the stainless steel slag, and the time during which the surface temperature was above 500°C was too long (15 hours). The amount of hexavalent chromium eluted was also large because the number density of the MnS phase was reduced due to the coarsening of the MnS phase, and there was not enough MnS phase near the MgO·Al2O3·Cr2O3 phase exposed during the slag crushing, making it easier for a reaction to occur in which Cr oxidizes and produces hexavalent chromium.
[0051] As can be seen from the above results, the present invention can provide a stainless steel slag capable of suppressing the elution of hexavalent chromium, a method for producing the same, and a material for burial in the ground. [Explanation of symbols]
[0052] 10 Phase containing CaO and SiO2 20 MnS phase 30 MgO·Al2O3·Cr2O3 phase
Claims
1. CaO and SiO 2 Contains a total of 50% by mass or more, Cr 2 O 3 , CaO, SiO 2 , Al 2 O 3 Cr, MgO, Mn, S and F when the total amount is 100 mass %. 2 O 3 0.2 to 8.0 mass% Al 2 O 3 is 2.0 to 15.0 mass%, MgO is 3.0 to 20.0 mass%, Mn is 0.10 to 5.00 mass%, S is 0.010 to 0.500 mass%, and F is 0.50 mass% or less, Basicity (CaO / SiO 2 ) is 0.8 to 1.5; A stainless steel slag having an average particle size of MnS phase of 25.0 μm or less.
2. The stainless steel slag according to claim 1, comprising at least one selected from Fe, Ti, B and P, the total amount of which is 5.00 mass% or less.
3. The MnS phase is 0.01 to 2.00 volume %, MgO.Al 2 O 3 Cr 2 O 3 phase is 0.01 to 20.00 vol. %, The MgO.Al 2 O 3 Cr 2 O 3 The MnS phase (MnS phase / MgO.Al 2 O 3 Cr 2 O 3 3. The stainless steel slag according to claim 1 or 2, wherein the volume ratio of the slag phase to the slag phase is 0.004 or more.
4. A method for producing stainless steel slag according to any one of claims 1 to 3, a step of controlling the composition of molten stainless steel by melting and refining raw materials so that the C concentration is 1.7 mass% or more, the Si concentration is 0.2 mass% or more, and X represented by formula (1) is 10.0 or less; a step of cooling the steelmaking slag generated on the upper part of the molten stainless steel so that the time during which the surface temperature of the steelmaking slag remains at 500° C. or higher is 10 hours or less when the steelmaking slag is separated from the molten stainless steel and cooled; A method for producing stainless steel slag comprising the steps of: X=Cr / (0.5×C+Si+Mn)... (1) In the formula, Cr, C, Si, and Mn represent the contents (mass%) of the respective elements.
5. A material for burial in soil, comprising the stainless steel slug according to any one of claims 1 to 3.
6. The material for burial in soil according to claim 5, further comprising at least one selected from the group consisting of blast furnace slag, a solidification aid, an admixture, and an alkali irritant.
Citation Information
Patent Citations
Method for modifying chromium oxide-containing slag
JP1994171993A
Reforming method of stainless steel slag
JP1996104553A
Treatment method for slag in refining chromium- containing steel
JP2003301215A
Method for controlling elution of hexavalent chromium from steel slug and material for land burial of the slug
JP2005254082A
Air and water granulation method and device for molten slag, and air and water granulated particle and its collecting device
JP2006170513A