Method for spot welding aluminum material and method for joining aluminum material
The two-stage pressurization and preheating process, combined with controlled energization and protrusions, addresses the issue of dust and quality in aluminum spot welding, resulting in stronger and more reliable aluminum material joints.
Patent Information
- Application Number
- JP2021025140
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-19
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2041-02-19
AI Technical Summary
Spot welding aluminum materials with adhesives often results in dust formation and compromised welding quality due to the challenges of applying optimal welding conditions and adhesive fluidity during the process.
A method involving a two-stage pressurization process with a lower initial pressurization step followed by a higher pressurization step, combined with a preheating step to manage adhesive viscosity and a controlled energization process to stabilize the welding, along with the use of protrusions to guide adhesive flow.
This method effectively suppresses dust generation and enhances the quality of aluminum material joints by ensuring stable adhesive removal and consistent welding conditions, improving joint strength and rigidity.
Smart Images

Figure 0007564013000004 
Figure 0007564013000005 
Figure 0007564013000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for spot welding aluminum materials and a method for joining aluminum materials. [Background technology]
[0002] In recent years, lightweight aluminum materials have been actively used instead of steel materials in the structures of vehicles such as automobiles. However, aluminum materials have lower electrical resistance and higher thermal conductivity than steel materials, so when spot welding aluminum materials, the welding current must be increased by about three times and the welding electrode pressure must be increased by about 1.5 times compared to steel materials. For this reason, it is difficult to apply the spot welding conditions for steel materials to spot welding of aluminum materials, and it is necessary to find new welding conditions that are optimal for aluminum materials. As an example of a method for spot welding aluminum material, Patent Document 1 discloses a technology in which the pressure applied to the welding electrode is changed in two stages and the welding current value is changed in two stages, from a large current to a small current, in accordance with this pressure.
[0003] Furthermore, in order to further improve the joint strength and rigidity of the above-mentioned structure, a weld bond method is disclosed in, for example, Patent Document 2, in which an adhesive is applied in advance to the welded parts of the plates to be joined and then the plates are spot welded together. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 3862640 [Patent Document 2] Japanese Patent Application Publication No. 5-285669 Summary of the Invention [Problem to be solved by the invention]
[0005] Such a weld bond method can further improve the joining strength between plate materials. However, when spot welding aluminum materials together using an adhesive, spatter is likely to occur, which may reduce the quality of the weld.
[0006] Therefore, an object of the present invention is to provide a spot welding method for aluminum materials and a joining method for aluminum materials that can suppress the generation of spatter during spot welding even when an adhesive is used in combination, and can produce high-quality joining. [Means for solving the problem]
[0007] The present invention comprises the following configurations. (1) a pressurizing step of sandwiching the aluminum materials, which have been stacked together with an uncured adhesive therebetween, between a pair of electrodes and applying pressure thereto; a main current application step of applying current between the electrodes while continuing pressure application by the electrodes; A spot welding method for aluminum materials comprising: The pressurizing step includes a first pressurizing step carried out before the main current passing step and a second pressurizing step carried out overlapping with the main current passing step, The pressure applied in the first pressurizing step is lower than the pressure applied in the second pressurizing step. How to spot weld aluminum materials. (2) providing a plurality of aluminum sheets; providing an adhesive between the aluminum materials; (1) A step of joining the aluminum materials together by the aluminum material spot welding method; A method for joining aluminum materials comprising the steps of: Effect of the Invention
[0008] According to the present invention, even when an adhesive is used in combination, the generation of dust during spot welding can be suppressed, and aluminum materials can be joined with high quality. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a schematic diagram showing the main components of a spot welder for welding aluminum materials. [Diagram 2] 2(A) and 2(B) are cross-sectional views that typically show how the adhesive between the first aluminum plate and the second aluminum plate spreads during the pressing step. [Diagram 3] FIG. 3 is a timing chart showing waveforms of the electrode pressure and welding current under a first welding condition. [Figure 4] FIG. 4 is a timing chart showing waveforms of the electrode pressure and welding current under the second welding condition. [Diagram 5] FIG. 5 is a timing chart showing waveforms of the electrode pressure and welding current under the third welding condition. [Figure 6] 6(A) to 6(D) are schematic cross-sectional views showing, in stages, how protrusions are formed on a first aluminum plate, an adhesive is applied to a second aluminum plate, and then the two aluminum plates are superimposed on each other. [Figure 7] FIG. 7 is a schematic cross-sectional view of the state in which the overlapping aluminum materials are sandwiched between a pair of electrodes and the pressure step is started. [Figure 8] FIG. 8 is a graph showing the results of summarizing the number of dust occurrences during the first squeeze period in Test Examples 2-1 to 2-6. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. <Spot welding machine> FIG. 1 is a schematic diagram showing the main components of a spot welder for welding aluminum materials.
[0011] The spot welder 11 sandwiches overlapping plate materials between a pair of electrodes 13, 15 and spot welds them by applying pressure in the plate thickness direction while passing current through them. The spot welder 11 includes the pair of electrodes 13, 15, a welding transformer unit 17 connected to the pair of electrodes 13, 15, a power supply unit 19, a control unit 21 that supplies welding power from the power supply unit 19 to the welding transformer unit 17, and an electrode drive unit 23 that moves the pair of electrodes 13, 15 relatively in the axial direction. The control unit 21 comprehensively controls the current value passed through the pair of electrodes 13, the current passing time, the axial pressure of the electrodes, the current passing timing, the pressure passing timing, and the like.
[0012] The spot welding machine 11 sandwiches at least two aluminum plates, a first aluminum plate 25 and a second aluminum plate 27, between a pair of electrodes 13, 15, overlapping each other with an adhesive, the details of which will be described later. Then, the electrode driving unit 23 moves the electrode 13 and the electrode 15 relative to each other, thereby pressing the first aluminum plate 25 and the second aluminum plate 27 in the plate thickness direction. By passing a current between the electrodes 13, 15 in this pressed state, a nugget N is formed between the first aluminum plate 25 and the second aluminum plate 27 sandwiched between the electrodes 13, 15 with the adhesive therebetween. In this way, an aluminum welded joint (joint) 29 in which the first aluminum plate 25 and the second aluminum plate 27 are integrated is obtained.
[0013] In the above example, the first aluminum plate 25 and the second aluminum plate 27 are joined to form the aluminum welded joint 29, but the present invention is not limited to this and three or more aluminum plates may be joined.
[0014] The pair of electrodes 13, 15 may be R-shaped or DR-shaped electrodes having a curved surface at the tip of the electrode. However, the type of the electrodes is not limited to this. The pair of electrodes 13, 15 each have a cooling unit therein. The cooling method of the cooling unit is not particularly limited, but in the illustrated configuration, a cooling pipe 33 is arranged in a recess 31 formed in each of the electrodes 13, 15, and a cooling medium such as water is supplied from the cooling pipe 33 into the recess 31 to cool the electrodes 13, 15.
[0015] <Aluminum material> The first aluminum plate 25 and the second aluminum plate 27 used here may be exemplified by heat-treated aluminum alloys. Specifically, 2000-series, 6000-series, and 7000-series aluminum alloys may be mentioned. The thickness of the first aluminum plate 25 and the second aluminum plate 27 is preferably 0.5 mm or more, more preferably 1.0 mm or more, or 2.0 mm or more, for use as structural members such as automobile frame members. When using other aluminum plates, it is preferable that the thickness and material of the aluminum plates are the same. The thicknesses of the aluminum plates may be the same or different from each other. The form of the aluminum material is not limited to rolled plates, and may be extruded, forged, or cast.
[0016] <Adhesive> An adhesive is provided between the plate materials including the first aluminum plate 25 and the second aluminum plate 27. For example, an epoxy resin can be used as the adhesive. The adhesive may be provided on the surface of the plate materials by coating, or may be provided by adhering a sheet-shaped adhesive sheet to the surface of the plate materials.
[0017] Hereinafter, a mode in which two plate materials, the first aluminum plate 25 and the second aluminum plate 27, are joined via an adhesive will be described, but the objects to be joined are not limited to this mode.
[0018] <Welding conditions> (First welding condition) The spot welding method for aluminum materials using the above-mentioned spot welding machine 11 includes a pressurizing step in which aluminum materials overlapping each other with uncured adhesive therebetween are sandwiched between a pair of electrodes together with the adhesive and pressurized, and a main current application step in which current is applied between the electrodes while continuing to apply pressure by the electrodes.
[0019] 2A and 2B are cross-sectional views that diagrammatically show how the adhesive between the first aluminum plate 25 and the second aluminum plate 27 spreads during the pressing process. As shown in FIG. 2(A), a first aluminum plate 25 and a second aluminum plate 27 are laminated together with an adhesive 35 provided between the opposing plate surfaces. Specifically, adhesive 35 is applied to a planned welding position on surface 27a of second aluminum plate 27 facing first aluminum plate 25. Adhesive 35 may be applied to surface 25a of first aluminum plate 25 facing second aluminum plate 27, or may be applied to each of surfaces 25a, 27a of first aluminum plate 25 and second aluminum plate 27 facing each other.
[0020] Then, the first aluminum plate 25 and the second aluminum plate 27, which are overlapped with each other, are inserted between a pair of electrodes 13, 15, and the intended welding positions of the first aluminum plate 25 and the second aluminum plate 27 are positioned at the pressure current application position Pa by the electrodes 13, 15 (the position of the electrode axis L).
[0021] 3 is a timing chart showing waveforms of the electrode pressure and welding current under the first welding condition. The pressure and welding current applied by electrodes 13, 15 are controlled by control unit 21 shown in FIG. The control unit 21 drives the electrode driving unit 23 to pressurize the first aluminum plate 25 and the second aluminum plate 27 sandwiched between the electrodes 13, 15 in the plate thickness direction by the electrodes 13, 15 at the pressurizing and current application position Pa. Then, the adhesive 35 spreads between the opposing surfaces 25a, 27a of the first aluminum plate 25 and the second aluminum plate 27 so as to be excluded from the position of the axis L of the electrodes 13, 15, as shown in FIG. 2(B).
[0022] As shown in Fig. 3, the pressing step of pressing the aluminum material with the electrodes 13 and 15 includes a first pressing step with a pressing force P1 and a second pressing step with a pressing force P2 greater than the pressing force P1. The first pressing step is performed for a period t P1 The second pressurizing step is carried out after the first pressurizing step, and is performed for a period t P2 The fluidity of the adhesive 35 is increased by setting the pressure P1 in the first pressurizing step lower than the pressure P2 in the second pressurizing step.
[0023] This current is applied from the start of the first pressurization step to the squeeze period t S Here, the current flow period starts when the upslope period t US After the welding current is gradually increased to a predetermined value I, the welding current I is maintained for a welding period t. The welding current is maintained for a period t of the second pressurizing step. P2 The second pressurization step is carried out within a period t S2 After the current is turned off, the hold period t HD During this period, the welding pressure P2 is maintained. Note that, depending on the welding conditions, this current flow may continue for an upslope period t US Alternatively, a single rectangular pulse current may be passed without providing the pulse width adjusting circuit 14.
[0024] According to the first welding condition described above, a first pressing step (first squeeze period t S1 ), the adhesive 35 gradually spreads from the pressurized and current-carrying position Pa toward its periphery, so that the thickness of the adhesive 35 at the pressurized and current-carrying position Pa is reliably reduced. Then, in the second pressurizing step after the first pressurizing step, the pressure applied to the adhesive 35 is increased to P2 (second squeeze period t S2 ). This makes it easier for the adhesive 35 remaining at the pressurized current-carrying position Pa in the first pressurizing step to be removed from the pressurized current-carrying position Pa. Thus, current flow is started in a state in which the adhesive 35 has been removed from the pressurized current-carrying position Pa, so that almost no adhesive 35 is present in the current-carrying path between the electrodes 13 and 15, and stable current flow is achieved.
[0025] In addition, this current application process is an upslope current application period t US By including the above, it is possible to prevent overshooting of the welding current, suppress the generation of spatter, and realize stable current flow. As a result, it is possible to suppress the generation of dust, stably form a nugget of an appropriate size, and improve the welding quality. In addition, the appropriate holding period t after the main current flow period is HD By providing the holding step, the effect of suppressing internal defects in the weld can be obtained.
[0026] When spot-welding an aluminum material via an adhesive 35 as shown in (B) of FIG. 2, even if a large pressing force is suddenly applied to the adhesive 35 to try to remove the adhesive 35 from the pressure-energization position Pa, the fluidity of the adhesive 35 is suppressed and it becomes difficult to remove. However, according to this method, the effect of removing the adhesive 35 from the pressure-energization position Pa is enhanced, thereby eliminating the factors that destabilize the energization path, such as the adhesive 35 intervening in the energization path and causing the electrical resistance to become non-uniform depending on the location.
[0027] And according to this method, since the adhesive 35 is provided between the first aluminum plate 25 and the second aluminum plate 27, the first aluminum plate 25 and the second aluminum plate 27 can be joined by the adhesive 35 around the welded portion where the nugget N shown in FIG. 1 is formed. Therefore, the combination of the joining at the spot-welded joint and the adhesion by the adhesive 35 enables a stronger joint. As a result, the peel resistance is enhanced, and the rigidity of the aluminum welded joint 29 can be further improved.
[0028] (Second welding condition) Next, the second welding condition will be described. FIG. 4 is a timing chart showing the waveforms of the pressing force and the welding current under the second welding condition. The second welding condition is the same as the first welding condition except that the first pressing step of the first welding condition shown in FIG. 3 described above is changed to a multi-stage pressing step in which the pressing force is increased step by step.
[0029] As shown in FIG. 4, the period t of the first pressing step P1 has a first squeeze period t in the first half when applying the pressing force P1a S1a and a first squeeze period t in the second half when applying the pressing force P1b S1b (however, P1a < P1b < P2). Also, the period from the start of the second pressing step until the welding current is energized is the second squeeze period t S2In the first pressurizing step, the number of stages for increasing the pressurizing force is exemplified as two stages here, but the number of stages is arbitrary. In addition, as long as it is possible to control the electrode driving unit 23 shown in FIG. 1, the pressurizing force may be increased continuously.
[0030] According to these welding conditions, the first pressurizing step is set to a lower pressurizing force than the second pressurizing step, and is gradually increased to a higher pressurizing force, thereby adjusting the removability of the adhesive 35 at the pressurized current application position Pa. For example, an optimal pressurizing pattern can be set according to the characteristic parameters of the adhesive 35, such as the viscosity and electrical conductivity, the welding execution conditions, and the like.
[0031] (Third welding condition) Next, the third welding condition will be described. FIG. 5 is a timing chart showing waveforms of the electrode pressure and welding current under the third welding condition. The third welding conditions are similar to the first welding conditions shown in FIG. 3 except that a preheat current application step is provided before the main current application step in the first welding conditions.
[0032] The preheat current application process is a process in which a welding current value Ip smaller than the welding current value I in the main current application process is applied. The preheat current application process has the effect of reducing the viscosity of the adhesive 35 before the main current application process and improving the fluidity of the adhesive 35.
[0033] The period of the preheat current application step is set so that at least a part of the period of the first pressurizing step is included in the period t PH is the first preheat period t which overlaps with the first pressurization step PH1 and a second preheat period t which overlaps with the second pressurizing step. PH2 and
[0034] According to these welding conditions, by providing a preheat current application step before the main current application step, the adhesive 35 is heated by the preheat current application and the viscosity is reduced. As a result, the adhesive 35 at the pressurized current application position Pa shown in FIG. 2B has improved fluidity and is easily removed from the pressurized current application position Pa. More specifically, the adhesive 35 is preheated in the first pressurizing step in which pressure is applied with a relatively low pressure P1 (first preheat period t PH1 ) The fluidity is further increased, and the expulsion from the pressurizing current applying position Pa is remarkably improved by the synergistic effect. In addition, since the preheating is continued even when the second pressurizing step in which the pressurizing force P2 is larger is reached (the second preheating period t PH2 ), the fluidity of the adhesive 35 continues to improve without decreasing, and the fluidity can be maintained even when the adhesive 35 is pressurized with a large pressurizing force P2. As a result, the adhesive 35 flows smoothly to the periphery and is reliably removed from the pressurized and energized position Pa.
[0035] In addition, after the preheat current application process, the upslope current application period t US By carrying out this current passing process including the above, more stable current passing can be achieved.
[0036] <Spot welding of aluminum material with protrusions> Next, a case will be described in which a protrusion is formed at a planned welding position of one of a pair of aluminum materials, the protrusion projecting toward the other aluminum material facing the one aluminum material. 6(A) to 6(D) are schematic cross-sectional views showing, in stages, how protrusions are formed on a first aluminum plate, an adhesive is applied to a second aluminum plate, and then the two aluminum plates are superimposed on each other.
[0037] (protrusion formation) 6(A), the first aluminum plate 25A is embossed to form protrusions. Specifically, an embossment E, which is a protrusion having a circular shape in plan view and bulges in the overlapping direction toward the second aluminum plate 27, is formed at a position to be welded on the first aluminum plate 25A by pressing or the like. When the embossment E is formed, the peripheral portion Es of the embossment E of the first aluminum plate 25 becomes harder than other portions due to work hardening.
[0038] The outer diameter (embossing diameter) φd of the facing surface 25a on the protruding side (second aluminum plate 27 side) of the embossing E is preferably 3√t to 7√t mm (t is plate thickness). The embossing height h from the facing surface 25a on the protruding side of the embossing E to the top Et of the embossing E is preferably t / 2 or less. In addition, the curvature radius r of the facing surface 25a on the protruding side of the embossing E is preferably smaller than the curvature radius of the tips of the electrodes 13, 15.
[0039] The emboss E is formed so that the emboss root diameter φdn on the surface 25b on the root side (opposite the protruding side of the first aluminum plate 25) is smaller than the tip diameter φde (region where the electrode tip has a constant radius of curvature) of the electrodes 13, 15. In other words, the electrodes 13, 15 used for welding have a tip diameter φde larger than the root diameter φn of the emboss E.
[0040] (Adhesive application) Furthermore, as shown in FIG. 6(B), an adhesive 35 is applied to a position to be welded on a surface 27a of the second aluminum plate 27 facing the first aluminum plate 21A.
[0041] (Placement process) Then, as shown in FIG. 6(C), the protruding side of the embossment E of the first aluminum plate 25A is faced toward the second aluminum plate 27, and the first aluminum plate 25A and the second aluminum plate 27 are overlapped with each other.
[0042] (Pressure application process, main current application process) The first aluminum plate 25A and the second aluminum plate 27 thus stacked on top of each other are inserted between the pair of electrodes 13, 15, as shown in Fig. 6(D). Then, the above-mentioned first pressurizing step is started, and then the second pressurizing step is started to carry out the main current passing step.
[0043] FIG. 7 is a schematic cross-sectional view of the state in which the overlapping aluminum materials are sandwiched between a pair of electrodes and the pressure step is started. As shown in FIG. 7, when the first aluminum plate 25A and the second aluminum plate 27 are pressed against each other, the center side of the embossment including the top Et (see FIG. 6D) of the embossment E is pressed in the opposite direction to the protruding direction (the direction of the arrow S) with the work-hardened peripheral edge Es as a fulcrum. As a result, the center side of the embossment E is recessed and the peripheral edge Es protrudes slightly in an annular shape toward the second aluminum plate 27. When the peripheral edge Es of the embossment E protruding in an annular shape comes into contact with the second aluminum plate 27, a gap space G that is slightly recessed toward the center side of the embossment E is formed on the surface of the first aluminum plate 25A. At this time, the adhesive 35 is pushed out from the center side of the embossment E toward the outer periphery, so that the adhesive 35 is no longer present in the gap space G.
[0044] While maintaining this pressurized state, a welding current is applied between the electrodes 13, 15. Then, the first aluminum plate 25A and the second aluminum plate 27 start to melt at the intended welding position between the electrodes 13, 15. At this time, the annular peripheral portion Es of the emboss E is pressed against the opposing surface 27a of the second aluminum plate 27, and a gap space G is formed on the center side of the emboss E, so that melting at the intended welding position starts from the peripheral portion Es of the emboss E and progresses toward the center of the emboss. As a result, the molten aluminum generated by the current is prevented from flowing out to the outer periphery side of the emboss E, and the gap space G is filled with molten aluminum.
[0045] When electricity is applied for a predetermined time, a nugget N is formed at the intended welding position, which has high circularity and an excellent penetration rate into the base materials, the first aluminum plate 25A, and the second aluminum plate 27. As a result, the first aluminum plate 25A and the second aluminum plate 27 are integrated with high strength, forming a high-quality aluminum welded joint.
[0046] In addition, the thickness of the nugget N is not excessive and the nugget N is not exposed on the surface of the aluminum plate, so that molten aluminum does not adhere to the surfaces of the electrodes 13, 15. Therefore, it is not necessary to frequently dress the electrodes 13, 15, and production efficiency can be improved.
[0047] When R-shaped or DR-shaped electrodes having curved end faces are used as the electrodes 13, 15, the tip faces of the electrodes 13, 15 are curved, so the effects of variations in the angles of the electrodes 13, 15 and uneven contact of the electrodes are suppressed compared to electrodes with flat tip shapes. This allows stable pressure to be applied to the first aluminum plate 25A and the second aluminum plate 27, and a nugget N with high circularity can be formed, achieving high-quality spot welding.
[0048] As the shape of the protrusions described above, an embossment that is easy to apply is exemplified, but the shape is not limited to this. For example, it is possible to adopt other forming methods as long as the protrusions can be formed, such as driving a protrusion member into the surface of the first aluminum material so that the protrusion member protrudes from the surface of the aluminum material. EXAMPLES
[0049] <Test Example 1> Two aluminum plates were prepared, an embossment was formed on one of the aluminum plates, an adhesive was applied to the other aluminum plate, and the two aluminum plates were overlapped and spot-welded so that the protruding side of the formed embossment faced the applied adhesive. The occurrence of spatter after spot welding in this case was confirmed. Here, five types of tests, Test Examples 1-1 to 1-5, were carried out with the same material and current conditions but different pressure conditions, to investigate the number of spatters that occurred.
[0050] (Aluminum plate) Upper plate Material: A6022 Plate thickness t: 1.0mm Emboss diameter φd: φ5mm Lower plate material: A6022 plate thickness t: 2.0mm (glue) Epoxy Resin (electrode) Type: Chromium copper, R-shaped electrode Tip curvature radius: 100mm Electrode diameter (original diameter) φde: 19mm (Welding conditions) Welding current value for this welding: I: 26kA Welding period t: 80 ms Upslope period t US :20ms
[0051] Table 1 shows the pressurizing conditions in Test Examples 1-1 to 1-5.
[0052] [Table 1]
[0053] Test Example 1-1 is the first pressurization step (t P1 ) is not provided, and the second pressurizing step (t P2 ) only during the second squeeze period t S2 600ms (squeeze period t S :600ms), retention period t HD This is a reference example where the delay is set to 400 ms. In Test Example 1-2, the period t P1 The second squeeze period t S2 is set to 100ms, and the squeeze period t S was set to 600 ms. In Test Example 1-3, the squeeze period t S The first squeeze period t in the first pressurization step is set to 600 ms. S1 was reduced from 500ms to 300ms. In Test Example 1-4, the pressure in the first pressurizing step of Test Example 1-2 was changed to a first-stage pressurizing force P1a of 1 kN (t S1a : 200ms), and the second pressure P1b is 2kN (t S1b : 200 ms), and the second squeeze period t S2 is set to 200ms, and the squeeze period t S was set to 600 ms. In the test example 1-5, the first pressurizing step was performed in two stages similar to the test example 1-4, and the period t S1a , the period t of the second stage pressure P1b S1b , the second squeeze period t S2 and the squeeze period tS has been extended to 1800ms.
[0054] The number of spatters generated when spot welding aluminum plates was performed under the conditions of each test example was examined. In the test example 1-1 in which the first pressurizing step was not performed, the number of dust particles generated reached eight. In Test Examples 1-2 and 1-3, in which the first pressurization step was performed in one stage, the number of spatters generated was three, less than half the number of spatters generated in Test Example 1-1, which did not have a first pressurization step, and spatter generation was suppressed. Also, in Test Examples 1-4 and 1-5, in which the first pressurization step was performed in two stages, the number of spatters generated was greater than in Test Examples 1-2 and 1-3, in which the first pressurization step was performed in one stage, but spatter generation was suppressed compared to Test Example 1-1. Among Test Examples 1-4 and 1-5, in which two-stage pressurization was performed, the number of spatters generated in the first pressurization step at the beginning of pressurization (period t S1a ) was set longer in Test Example 1-5, which tends to have a greater effect in suppressing dust generation.
[0055] <Test Example 2> Next, the pressure P1 of the first pressurizing step is set to 1 kN, and the squeeze period t S The number of dust particles generated was investigated when the temperature was changed. Table 2 shows the test conditions.
[0056] [Table 2]
[0057] In the test example 2-1, as shown in FIG. S1 500ms, the second squeeze period t S2 is 100ms, and the total squeeze period t S (=t S1 +t S2 As a result, the number of dust particles was reduced to three, which is less than half the number in the case of the above-mentioned Test Example 1-1.
[0058] In Test Example 2-2, the squeeze period t S The first squeeze period t S1 to 300 ms, and the second squeeze period t S2The time was extended to 300 ms. As a result, the number of dust particles was 3, which was the same as in Test Example 2-1.
[0059] In Test Example 2-3, the first squeeze period t S1 Reduce the squeeze period t from 500ms to 100ms. S The time was shortened from 600ms to 200ms. As a result, the number of dust particles increased to 5.
[0060] In Test Example 2-4, the first squeeze period t S1 The second squeeze period t S2 to 500ms, and the squeeze period t S As a result, the number of dust particles was 5, which was the same as in Test Example 2-3.
[0061] In Test Example 2-5, the first squeeze period t S1 is set to 1000 ms, and the second squeeze period t S2 is set to 100ms, and the squeeze period t S In the test example 2-6, the first squeeze period t in the test example 2-5 was extended to 1100 ms. S1 Extend the squeeze period t from 1000ms to 2000ms. S The results of Test Examples 2-5 and 2-6 showed that the number of dust particles was zero, and good results were obtained.
[0062] FIG. 8 shows the number of dust particles generated in Test Examples 2-1 to 2-6 during the first squeeze period t S1 1 is a graph showing the results of the above. According to FIG. 8, the first squeeze period t S1 It can be seen that the longer the time, the lower the number of dust particles.
[0063] If the distribution of the number of flash occurrences shown in Fig. 8 is linearly approximated, and the pressurization time at which the obtained approximation line Lp results in the number of flash occurrences being 0 is calculated to be approximately 950 ms. Therefore, if the period during which the pressurizing force P1 in the first pressurizing step is set to 1 kN is set to 1000 ms, the number of flash occurrences is likely to be 0. In this way, it was found that when there is a first pressurizing step in which pressurization is performed with a relatively low pressurizing force P1, the generation of flash occurrences can be suppressed by making the squeeze period at low pressurization sufficiently long.
[0064] <Test Example 3> Next, test examples in which the viscosity, one of the properties of the adhesive, was changed by preheating through electrical current to adjust the fluidity (removability) of the adhesive are shown below. Table 3 shows the test conditions for Test Examples 3-1 to 3-6.
[0065] (Welding conditions) Preheat period t PH Current value I P :8kA Welding period t: 80 ms
[0066] [Table 3]
[0067] In the test example 3-1, the welding current value I of the main welding shown in FIG. 5 was 25 kA, the pressure P1 of the first pressurizing step was 1 kN, the pressure P2 of the second pressurizing step was 3 kN, and the squeeze period t S 100ms, the first preheat period t PH1 400ms, the second preheat period t PH2 100ms, upslope period t US 20ms, retention period t HD The first preheat period t in Test Example 3-1 was set to 400 ms. As a result, the number of dust particles was two. PH1 The time was shortened from 400ms to 100ms. As a result, the number of dust particles was reduced to three.
[0068] In Test Example 3-3, the first preheat period t PH1is shortened from 400ms to 100ms, and the upslope period t US was extended from 20ms to 200ms. In Test Example 3-4, the upslope period t US In the test example 3-5, the upslope period t US was set to 60ms.
[0069] Test Examples 3-3, 3-4, and 3-5 are for the upslope period t US By extending the preheat period t, the welding quality became stable and the number of spatters was reduced to zero. PH If you provide an upslope period t US It is recommended to set this to 60 ms or more.
[0070] In Test Example 3-6, the welding current value I of the main welding in Test Example 3-5 was increased from 25 kA to 27 kA. Even in this case, the number of spatters generated remained at zero.
[0071] The present invention is not limited to the above-described embodiments, and the present invention also contemplates the mutual combination of the various components of the embodiments, as well as modifications and applications by those skilled in the art based on the description in the specification and well-known techniques, and these are included in the scope of protection sought.
[0072] As described above, the present specification discloses the following: (1) a pressurizing step of sandwiching the aluminum materials, which have been stacked together with an uncured adhesive therebetween, between a pair of electrodes and applying pressure thereto; a main current application step of applying current between the electrodes while continuing pressure application by the electrodes; A spot welding method for aluminum materials comprising: The pressurizing step includes a first pressurizing step carried out before the main current passing step and a second pressurizing step carried out overlapping with the main current passing step, The pressure applied in the first pressurizing step is lower than the pressure applied in the second pressurizing step. How to spot weld aluminum materials. According to this method for spot welding aluminum material, the first pressurizing step, which is carried out before the main current application step, is carried out at a lower pressure than the pressure applied in the second pressurizing step, thereby making it possible to suppress the generation of spatter compared to the case in which the first pressurizing step is not carried out.
[0073] (2) The spot welding method for aluminum materials according to (1), further comprising a preheat current application process, prior to the main current application process, of applying a current value smaller than the maximum welding current value of the main current application process. According to this method for spot welding aluminum materials, the adhesive is heated in the preheat current application step, and the viscosity of the adhesive is reduced, improving the dischargeability of the adhesive. In addition, even if the time of the first pressurizing step is shortened, the effect of suppressing spatter can be maintained, and the tact time of spot welding can be shortened.
[0074] (3) The spot welding method for aluminum materials according to (2), wherein the preheat current application process overlaps with at least a portion of the first pressurization process. According to this method for spot welding aluminum materials, the first pressurizing step, in which the pressure is relatively low, and the preheat current application step are overlapped, so that the heated adhesive can be smoothly caused to flow and be discharged.
[0075] (4) The spot welding method for aluminum materials according to (3), wherein an overlap period between the preheat current application step and the first pressurizing step is 100 ms or more and less than 400 ms. According to this method for spot welding aluminum materials, the viscosity of the adhesive can be effectively reduced and the flowability can be increased.
[0076] (5) The spot welding method for aluminum materials according to any one of (2) to (4), wherein the preheat current application step and the main current application step are carried out continuously. According to this method for spot welding aluminum materials, the adhesive heated in the preheat current application step can be spot welded without lowering its temperature, so that the high fluidity of the adhesive can be maintained.
[0077] (6) The spot welding method for aluminum materials according to (1), wherein a period of the first pressurizing step is 1000 ms or more and 2000 ms or less. According to this method for spot welding aluminum materials, the adhesive can be discharged reliably, thereby suppressing the generation of dust.
[0078] (7) The spot welding method for aluminum materials according to any one of (1) to (6), wherein the main current flow step includes an upslope current flow period. According to this method for spot welding aluminum materials, the welding quality can be stabilized by providing an upslope current application period.
[0079] (8) The spot welding method for aluminum materials according to any one of (1) to (7), wherein the first pressurizing step includes a multi-stage pressurizing step in which the pressurizing force is increased stepwise in two or more stages from the pressurizing force of the first pressurizing step to the pressurizing force of the second pressurizing step. According to this method for spot welding aluminum materials, the applied pressure in the first pressurizing step can be changed by simple control.
[0080] (9) The spot welding method for aluminum materials according to any one of (1) to (8), wherein the second pressurizing step includes a holding step of holding the pressure on the aluminum material after the main current passing step. According to this method for spot welding aluminum material, the effect of suppressing internal defects can be improved.
[0081] (10) A spot welding method for aluminum materials according to any one of (1) to (9), in which at least one of the aluminum materials has a protrusion at a planned welding position thereon, protruding toward another aluminum material facing the aluminum material. According to this method for spot welding aluminum material, the projection serves as a current path, and the adhesive spreads radially from the projection as the center, so that the adhesive can be reliably removed from the intended welding position.
[0082] (11) The spot welding method for aluminum materials according to (10), wherein the protrusion is an embossment having a circular shape in a plan view that bulges in the overlapping direction of the aluminum materials. According to this method for spot welding aluminum materials, protrusions can be formed by simple processing, and workability can be improved. That is, the embossment formed on the aluminum material is uniformly crushed by the electrodes, and the peripheral portion is work-hardened. The aluminum materials are overlapped at the intended welding positions with the bulging side of the embossment facing the other aluminum material, and the overlapped aluminum materials are sandwiched between the electrodes and pressurized. Then, the center side of the emboss is pressed and recessed, leaving the work-hardened peripheral portion of the embossment. When current is applied between the electrodes while continuing to apply pressure, melting begins at the intended welding position of the aluminum material placed between the electrodes. At this time, the peripheral portion of the emboss is pressed against the surface of the other aluminum material, and a gap is formed on the emboss center side, so that melting of the aluminum material at the intended welding position begins from the peripheral portion of the emboss and progresses toward the center of the emboss. For this reason, the molten aluminum generated by the current is not allowed to flow out to the outer periphery side of the emboss. In addition, since the gaps on the embossing center side are filled with molten aluminum, a nugget with high roundness and excellent penetration rate into the aluminum base material is formed. This results in a high-quality joint between aluminum materials. In addition, the nugget is prevented from becoming too thick and being exposed on the aluminum material surface, and molten aluminum does not adhere to the surface of the electrode. This eliminates the need to frequently dress the electrode, improving production efficiency.
[0083] (12) providing a plurality of aluminum sheets; providing an adhesive between the aluminum materials; A step of joining the aluminum materials together by the spot welding method for aluminum materials according to any one of (1) to (11); A method for joining aluminum materials comprising the steps of: According to this method for joining aluminum materials, it is possible to join aluminum materials together in a high-quality state in which dust generation is suppressed.
[0084] (13) The method for joining aluminum materials described in (12), further comprising a step of forming a protrusion at a planned welding position in at least one of the aluminum materials, the protrusion protruding in the overlapping direction toward the other aluminum material. According to this method for joining aluminum materials, by providing the aluminum plates with protrusions, the aluminum materials can be joined together more reliably.
[0085] (14) The method for joining aluminum materials according to (12) or (13), wherein the step of applying the adhesive is a step of applying the adhesive to each of a plurality of planned welding positions. According to this method for joining aluminum materials, adhesive can be easily applied even over a large area, improving workability.
[0086] (15) The method for joining aluminum materials according to (12) or (13), wherein the step of applying an adhesive is a step of sandwiching an adhesive sheet between the aluminum materials. According to this method for joining aluminum materials, adhesive of uniform thickness can be easily applied, improving workability. [Explanation of symbols]
[0087] 11 Spot welding machine 13,15 electrode 17 Welding transformer section 19 Power supply section 21 Control section 23 Electrode drive unit 25, 25A First aluminum plate (aluminum material) 27 Second aluminum plate (aluminum material) 29 Aluminum Welded Joints 31 Recess 33 Cooling pipe 35 Adhesive L axis Pa Pressurized current position P1, P2 pressure I, Ip Welding current value tHD Retention period t P1 Duration of the first pressurization step t P2 Duration of the second pressurization step t US Upslope Period t S Squeeze Period t S1 ,t S1a ,t S1b First squeeze period t S2 Second squeeze period t PH Preheat period t PH1 First preheat period t PH2 Second preheat period E Embossed (protrusion) G Gap space
Claims
1. a pressurizing step of sandwiching the aluminum materials, which have been stacked together with an uncured adhesive therebetween, between a pair of electrodes and applying pressure thereto; a main current application step of applying current between the electrodes while continuing pressure application by the electrodes; A spot welding method for aluminum materials comprising: The pressurizing step includes a first pressurizing step carried out before the main current passing step and a second pressurizing step carried out overlapping with the main current passing step, The pressure applied in the first pressurizing step is lower than the pressure applied in the second pressurizing step, a preheat current application process for applying a current at a value smaller than a maximum welding current value of the main current application process before the main current application process; The preheat current application process and the main current application process are carried out continuously. How to spot weld aluminum materials.
2. The preheat current application process overlaps with at least a portion of the first pressurization process. The spot welding method for aluminum materials according to claim 1.
3. The overlap period between the preheat current application step and the first pressurization step is 100 ms or more and less than 400 ms. The spot welding method for aluminum materials according to claim 2.
4. The period of the first pressurizing step is 1000 ms or more and 2000 ms or less. The spot welding method for aluminum materials according to claim 1.
5. The main current application step includes an upslope current application period. The spot welding method for aluminum materials according to any one of claims 1 to 4.
6. The first pressurizing step includes a multi-stage pressurizing step in which the pressurizing force is increased stepwise in two or more stages from the pressurizing force of the first pressurizing step to the pressurizing force of the second pressurizing step. The spot welding method for aluminum materials according to any one of claims 1 to 5.
7. The second pressurizing step includes a holding step of holding the pressure of the aluminum material after the main current passing step. The spot welding method for aluminum materials according to any one of claims 1 to 6.
8. At least one of the aluminum materials has a protrusion at a planned welding position thereof protruding toward another aluminum material facing the aluminum material; The spot welding method for aluminum materials according to any one of claims 1 to 7.
9. The protrusion is an embossment having a circular shape in a plan view that bulges in the overlapping direction of the aluminum materials. The spot welding method for aluminum materials according to claim 8.
10. providing a plurality of aluminum sheets; providing an adhesive between the aluminum materials; A step of joining the aluminum materials together by the spot welding method for aluminum materials according to any one of claims 1 to 9; Equipped with A method for joining aluminum materials.
11. The method further includes a step of forming a protrusion protruding in a direction toward the other aluminum material at a position to be welded in at least one of the aluminum materials, The method for joining aluminum materials according to claim 10.
12. The step of applying the adhesive is a step of applying the adhesive to each of a plurality of planned welding positions. The method for joining aluminum materials according to claim 10 or 11.
13. The step of applying the adhesive is a step of sandwiching an adhesive sheet between the aluminum materials. The method for joining aluminum materials according to claim 10 or 11.
14. A method for manufacturing a semiconductor device, comprising the steps of: preparing a plurality of aluminum sheets; providing an adhesive between the aluminum materials; a step of joining the aluminum materials to each other by a spot welding method; Equipped with The step of applying the adhesive is a step of applying the adhesive to each of a plurality of planned welding positions, The spot welding method for aluminum materials includes the steps of: a pressurizing step of sandwiching the aluminum materials, which have been stacked together with an uncured adhesive therebetween, between a pair of electrodes and applying pressure thereto; a main current application step of applying current between the electrodes while continuing pressure application by the electrodes; Equipped with The pressurizing step includes a first pressurizing step carried out before the main current passing step and a second pressurizing step carried out overlapping with the main current passing step, The pressure applied in the first pressurizing step is set to be lower than the pressure applied in the second pressurizing step. A method for joining aluminum materials.
15. The method further comprises the step of forming a protrusion at a planned welding position on at least one of the aluminum materials, the protrusion protruding in a direction of overlapping toward the other aluminum material. The method for joining aluminum materials according to claim 14.
Citation Information
Patent Citations
Denkyokunyorukanetsushikyosetsuho
JP1976060650A
Spot welding method for aluminum alloy sheets
JP1993000383A
Method for joining plate materials
JP1993285669A
Electrode for welding aluminum alloy material and welding method thereof
JP1997066371A
Aluminum material resistance spot welding method