Welded joint
Patent Information
- Application Number
- PCT/JP2024/016972
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-08-10
- Filing Date
- 2024-05-07
- Publication Date
- 2025-02-13
Smart Images

Figure JP2024016972_13022025_PF_FP_ABST
Abstract
Description
Welded joints
[0001] The present invention relates to welded joints.
[0002] In recent years, efforts have been made to increase the strength of steel sheets used in various fields such as automobiles, home appliances, building materials, etc. For example, in the automobile field, the use of high-strength steel sheets has been increasing with the aim of reducing the weight of vehicle bodies to improve fuel efficiency.
[0003] In particular, in the automotive field, welded joints formed by spot welding zinc-based plated steel sheets are often used. When welding zinc-based plated steel sheets, particularly high-strength steel sheets, deterioration of weldability due to liquid metal embrittlement (LME) cracking can become a problem, as described in Patent Document 1, for example. LME cracking is thought to occur when the surface layer of the steel sheet transforms to austenite during welding, and molten zinc penetrates the grain boundaries, embrittling the steel sheet, and when tensile stress is applied to the steel sheet during welding.
[0004] In addition, Patent Document 2 discloses a steel sheet that suppresses LME cracking and improves weldability, and describes a steel sheet having a surface layer containing silicon oxide particles with a particle size of 20 nm or more at a rate of 3,000 to 6,000 particles / mm 2 The patent discloses a steel sheet having a suitable grain size distribution at a number density of 1000.degree.
[0005] International Publication No. WO 2019 / 116531 International Publication No. WO 2020 / 218575
[0006] An object of the present invention is to provide a welded joint that has good LME resistance during manufacturing.
[0007] Various studies have been conducted to improve LME resistance during the production of welded joints. In response to this, the present invention has discovered that it is preferable to concentrate B in the surface layer of the steel sheet that constitutes the welded joint. It has been discovered that in order to concentrate B in the surface layer of the steel sheet, it is effective to prevent external oxidation from progressing on the surface of the steel sheet during annealing, and to promote internal oxidation in which oxidation progresses toward the inside of the steel sheet in the surface layer of the steel sheet. The gist of the present invention is as follows.
[0008] [1] A welded joint comprising a plurality of overlapping steel plates, a nugget joining the plurality of steel plates, a spot weld having a pressure-welded portion and a heat-affected portion formed around the nugget, a non-heat-affected portion which is an area outside the heat-affected portion, and a separation portion formed around the pressure-welded portion, wherein at least one steel plate arranged outermost among the plurality of steel plates is a high-strength steel plate having a Vickers hardness of 240 Hv or more at the center of the plate thickness, and the chemical composition of the high-strength steel plate is, in mass %, C: 0.05 to 0.40%, Si: 0.7 to 3.0%, Mn: 0.1 to 5.0%, sol. Al: 0-2.0%, P: 0.0300% or less, S: 0.0300% or less, N: 0.0100% or less, B: 0.0005-0.0050%, Ti: 0.0010-0.1000%, Nb: 0-0.2000%, V: 0-0.15%, Cr: 0-2. 00%, Ni: 0-2.00%, Cu: 0-2.00%, Mo: 0-1.00%, W: 0-1.00%, Ca: 0-0.1000%, Mg: 0-0.100%, Zr: 0-0.100%, Hf: 0-0.100%, and REM: 0-0.100%. The balance is Fe and impurities, and at a position 50 μm outward from the end of the pressure weld, a high-ferrite layer having a ferrite phase area ratio of 90% or more is present with a thickness of 5 μm or more from the surface of the high-strength steel plate in the thickness direction of the high-strength steel plate, and at a position 50 μm outward from the end of the pressure weld, a B-enriched portion having a B intensity that is at least twice the B intensity at a depth of 50 μm determined by TOF-SIMS measurement is present with a thickness of 1.0 μm or more from the surface of the high-strength steel plate.
[0009] [2] The welded joint according to [1], wherein the high-strength steel plate has a Zn-containing plating layer formed on one or both sides of the high-strength steel plate.
[0010] [3] The welded joint according to [1] or [2], characterized in that in the non-heat-affected zone, the depth at which the emission intensity Bx at a depth x (μm) in a GDS measurement from the steel sheet surface in the thickness direction and the emission intensity B150 at a depth of 150 μm satisfy Bx / B150≧5...(1) is 1.5 μm or more.
[0011] [4] The welded joint according to [3], characterized in that in the non-heat-affected zone, in a GDS measurement from the steel sheet surface in the thickness direction, the maximum value Bmax of the B emission intensity in a range of 5 μm or less in depth and the emission intensity B150 at a depth of 150 μm satisfy Bmax / B150≧8...(2).
[0012] [5] The welded joint according to any one of [1] to [4], wherein the high ferrite layer has a thickness of 10 μm or more.
[0013] According to the present invention, it is possible to obtain a welded joint having good LME resistance during manufacturing.
[0014] 1 is an example of a microstructure photograph of a high ferrite layer in a surface layer portion of a steel plate constituting a welded joint of the present invention. 2 is an example of a TOF-SIMS measurement result of a B-enriched portion in a surface layer portion of a steel plate constituting a welded joint of the present invention. 3 is a diagram illustrating the position of a crack targeted in the LME resistance evaluation in the examples.
[0015] Hereinafter, an embodiment of the present invention will be described. The present invention is not limited to the following embodiment. First, an outline of the present embodiment for improving the LME resistance during the production of a welded joint will be described.
[0016] When plated steel sheets are spot welded, the coating melts and the surface layer of the steel sheet is heated, transforming the steel sheet structure to austenite. During this process, the hot-dip coating penetrates into the steel sheet structure along the austenite grain boundaries, embrittling the grain boundaries. Therefore, when stress is applied to the steel sheet, LME cracking is likely to occur at the grain boundaries. It is believed that LME is particularly likely to occur because tensile stress is applied to the steel sheet during welding. The inventors of the present invention came up with the idea of utilizing B (hereinafter also referred to as "boron" or "boron") as a method for improving LME resistance. Specifically, they came up with the idea of suppressing the penetration of molten zinc into the Fe grain boundaries and suppressing the occurrence of LME by segregating B at the Fe grain boundaries (austenite grain boundaries or ferrite grain boundaries) in the surface layer structure.
[0017] Generally, in boron-containing steel, a deboronization phenomenon is known in which the amount of boron near the surface decreases, particularly when heated to the austenite temperature range. As a result, in boron-containing steel, the boron concentration in the surface layer of the steel is generally lower than that in the center of the steel sheet. In this embodiment, when the steel sheet is annealed, internal oxidation, which tends to progress to grain boundaries in the surface layer of the steel sheet, is induced toward the interior of the steel sheet. This results in the formation of an internal oxidation layer in the surface layer of the steel sheet, making it possible to fix Si, which particularly deteriorates LME resistance, as an oxide in the internal oxidation layer. Furthermore, the oxide formed by internal oxidation captures boron that diffuses from the steel sheet to the surface layer upon heating, thereby suppressing the deboronization phenomenon. In this way, contrary to typical boron-containing steel, by forming a boron-enriched region in the surface layer of the steel, the combined effects of these factors improve LME resistance during the production of welded joints.
[0018] Normally, when a steel sheet is heated, such as during annealing, external oxidation occurs, in which oxides (scale) are formed on the surface of the steel sheet. This embodiment is based on the finding that imparting strain to the surface layer of the steel sheet in advance promotes oxygen diffusion into the material, and that annealing at an appropriate dew point can promote internal oxidation without promoting external oxidation.
[0019] This embodiment will be described in detail below.
[0020] <<Welded Joint>> The welded joint of this embodiment comprises a plurality of overlapping steel plates, a nugget joining the plurality of steel plates, a spot weld having a pressure-welded portion and a heat-affected portion formed around the nugget, a non-heat-affected portion which is an area outside the heat-affected portion, and a separation portion formed around the pressure-welded portion. Here, the "heat-affected portion" refers to a portion of the steel plate that has not melted and whose structure, metallurgical properties, mechanical properties, etc. have been changed by welding heat, and the "non-heat-affected portion" refers to a portion other than the heat-affected portion.
[0021] [High-strength steel plate] Among the plurality of steel plates, at least one steel plate located on the outermost side is a high-strength steel plate. An object of the present invention is to suppress LME cracking that occurs when spot welding high-strength steel plates. LME cracking occurs in high-strength steel plates. The welded joint of this embodiment is effective in suppressing LME cracking during the manufacture of a welded joint, and is particularly effective in suppressing cracking in the shoulder of a weld. Here, the high-strength steel plate refers to a steel plate having a Vickers hardness of 240 Hv or more at a position that is a non-heat-affected zone of the welded joint and at a half-depth position. Furthermore, the "shoulder" refers to the inclined portion of the edge of the depression formed by the electrode during spot welding.
[0022] The hardness of the steel plate is measured at a position in the non-heat-affected zone of the steel plate constituting the weld joint, at a position of 1 / 2 depth. The hardness measurement is performed in accordance with JIS Z 2244:2009. The measurement load is 200 gf. The Vickers hardness at the center of the plate thickness of the steel plate constituting the weld joint may be 260 Hv or more, 280 Hv or more, or 300 Hv or more.
[0023] In the welded joint of this embodiment, as long as at least one of the steel plates constituting the welded joint, the outermost one, is the high-strength steel plate described above, the other steel plates may be ordinary commercially available steel plates. Of course, all of the steel plates may be the high-strength steel plates described above. When manufacturing a welded joint, at least one of the surfaces that comes into contact with a welding electrode during spot welding is a high-strength steel plate described below.
[0024] [Chemical Composition of High-Strength Steel Plate] The chemical composition of the high-strength steel plate will be described below. Hereinafter, "%" regarding the chemical composition of the high-strength steel plate means "mass %." Furthermore, in the numerical range of the chemical composition, a numerical range expressed using "to" means a range that includes the numerical values written before and after "to" as the lower and upper limits.
[0025] (C: 0.05 to 0.40%) C (carbon) is an element that ensures the strength of steel. In order to obtain a hardness of 240 Hv or more, which is the target of this embodiment, the C content is set to 0.05% or more. In consideration of weldability, the C content is set to 0.40% or less. The C content may be 0.08% or more, 0.10% or more, or 0.15% or more. The C content may be 0.37% or less, 0.35% or less, or 0.30% or less.
[0026] (Si: 0.7 to 3.0%) Si (silicon) is an element that promotes decarburization and ferrite stabilization during the annealing process in the production of steel sheet, and also suppresses the deboronization phenomenon through internal oxidation. It is also an element that improves the corrosion resistance of steel. This results in the formation of a high ferrite layer and a B-enriched portion, which will be described later, in the surface layer of the steel sheet. To achieve this effect, the Si content is set to 0.7% or more. If the Si content is too high, Si is generally an element that reduces LME resistance during the production of welded joints. Therefore, the effect of the B distribution, which will be described later, is inhibited, and the effect of improving LME resistance during the production of welded joints is reduced. In consideration of this, the Si content is set to 3.0% or less. The Si content may be 0.8% or more, 0.9% or more, or 1.0% or more. The Si content may be 2.5% or less, 2.0% or less, or 1.5% or less.
[0027] It has been known in the past that adding Si to steel reduces LME resistance during the production of welded joints, but as a result of investigations by the present inventors, it has been found that, contrary to conventional knowledge, adding a large amount of Si improves LME resistance during the production of welded joints. This is thought to be because the inclusion of B and the production method described below cause the surface layer to have a structure mainly composed of ferrite, and B is concentrated in the surface layer and segregates at the Fe grain boundaries.
[0028] (Mn: 0.1 to 5.0%) Mn (manganese) is an element that is effective in improving the strength of steel by obtaining a hard structure. Also, like Si, it is an element that suppresses the deboronization phenomenon through internal oxidation. In order to obtain these effects, the lower limit of the Mn content is set to 0.1%. Furthermore, taking into consideration the deterioration of workability due to Mn segregation, the Mn content is set to 5.0% or less. The Mn content may be 0.5% or more, 1.0% or more, or 1.5% or more. The Mn content may be 4.5% or less, 4.0% or less, or 3.5% or less.
[0029] (Sol. Al: 0 to 2.0%) Aluminum (aluminum) is an element that dissolves in steel and promotes ferrite stabilization and decarburization, thereby improving LME resistance during the production of welded joints. Therefore, it may be contained as needed. Sol. Al refers to acid-soluble Al that is not in the form of oxides such as Al2O3 and is soluble in acid. It is determined as Al measured after subtracting the insoluble residue on the filter paper generated during the Al analysis process. The inclusion of sol. Al is not essential, and the lower limit of the sol. Al content is 0.0%. To obtain the desired effect, the sol. Al content may be 0.1% or more, 0.2% or more, or 0.3% or more. If the sol. Al content is too high, external oxidation progresses, forming oxides (scale) on the surface of the steel sheet, even after high-dew-point annealing, and LME resistance during the production of welded joints is reduced. Taking this into consideration, the sol. Al content is set to 2.0% or less. The Al content may be 1.5% or less, 1.2% or less, or 1.0% or less.
[0030] (P: 0.0300% or less) P (phosphorus) is an impurity generally contained in steel. If the P content exceeds 0.0300%, weldability may be reduced. Therefore, the P content is set to 0.0300% or less. The P content may be 0.0200% or less, 0.0100% or less, or 0.0050% or less. It is preferable that no P is contained, and the lower limit of the P content is 0. From the viewpoint of dephosphorization costs, the P content may be more than 0% or 0.0001% or more.
[0031] (S: 0.0300% or less) S (sulfur) is an impurity generally contained in steel. If the S content exceeds 0.0300%, weldability will decrease, and further, the amount of MnS precipitation will increase, which may decrease workability such as bendability. Therefore, the S content is set to 0.0300% or less. The S content may be 0.0100% or less, 0.0050% or less, or 0.0020% or less. It is preferable that no S is contained, and the lower limit of the S content is 0. From the viewpoint of desulfurization costs, the S content may be more than 0% or 0.0001% or more.
[0032] (N: 0.0100% or less) N (nitrogen) is an impurity generally contained in steel. If the N content exceeds 0.0100%, weldability may be reduced. Therefore, the N content is set to 0.0100% or less. The N content may be 0.0080% or less, 0.0050% or less, or 0.0030% or less. It is preferable that no N is contained, and the lower limit of the N content is 0. From the viewpoint of production costs, the N content may be more than 0% or 0.0010% or more.
[0033] (B: 0.0005 to 0.0050%) B (boron) is an element that improves hardenability and contributes to improving strength, and also segregates at grain boundaries to strengthen the grain boundaries and improve toughness. Furthermore, in the steel sheet of this embodiment, boron is concentrated in the surface layer of the steel sheet and segregates at the Fe grain boundaries. In order to achieve this effect, the B content is set to 0.0005% or more. From the viewpoint of toughness and weldability, the B content is set to 0.0050% or less. The B content may be 0.0006% or more, 0.0008% or more, or 0.0010% or more. The B content may be 0.0040% or less, 0.0030% or less, or 0.0020% or less.
[0034] Generally, the B concentration in the surface layer of steel is lower than that in the center of the steel sheet due to the deboronization phenomenon. In this embodiment, by using a manufacturing method described below, internal oxidation toward the inside of the steel sheet is promoted in the annealing process, B is taken in by oxides, the deboronization phenomenon is suppressed, and the concentration distribution described below is formed in the surface layer of the steel. It is believed that this B segregated at the Fe grain boundaries suppresses LME during the production of welded joints.
[0035] (Ti: 0.0010 to 0.1000%) Ti (titanium) is an element that precipitates as TiC during cooling of steel and contributes to improving strength. To achieve this effect, the Ti content is set to 0.0010% or more. Excessive Ti content may result in the formation of coarse TiN, which may impair toughness, so the Ti content is set to 0.1000% or less. The Ti content may be 0.0020% or more, 0.0030% or more, 0.0040% or more, 0.0080% or more, 0.0110% or more, or 0.0130% or more. The Ti content may be 0.0900% or less, 0.0800% or less, 0.0600% or less, 0.0500% or less, or 0.0400% or less.
[0036] (Nb: 0 to 0.2000%) Nb (niobium) is an element that contributes to improving strength by improving hardenability, so it may be contained as needed. Since it is not an essential element, the lower limit of the Nb content is 0. This effect can be obtained even with a small amount of Nb contained, but when Nb is contained, the Nb content may be 0.0001% or more, 0.0002% or more, 0.0003% or more, 0.0004% or more, or 0.0010% or more. From the viewpoint of ensuring toughness, the Nb content is set to 0.2000% or less. The Nb content may be 0.1500% or less, 0.1000% or less, 0.0600% or less, 0.0400% or less, 0.0200% or less, 0.0100% or less, 0.0050% or less, 0.0030% or less, or 0.0020% or less.
[0037] (V: 0 to 0.15%) V (vanadium) is an element that contributes to improving strength by improving hardenability, so it may be contained as needed. Since it is not an essential element, the lower limit of the V content is 0. This effect can be obtained even with a small amount of V, but when V is contained, the V content may be 0.001% or more, 0.002% or more, 0.003% or more, 0.005% or more, 0.006% or more, 0.008% or more, or 0.01% or more. From the viewpoint of ensuring toughness, the V content is set to 0.15% or less. The V content may be 0.14% or less, 0.13% or less, 0.12% or less, 0.10% or less, 0.08% or less, 0.05% or less, 0.04% or less, 0.03% or less, or 0.02% or less.
[0038] (Cr: 0 to 2.00%) Cr (chromium) is effective in improving the hardenability of steel and increasing its strength, and may be contained as needed. Since Cr is not an essential element, the lower limit of the Cr content is 0. This effect can be obtained even with a small amount of Cr, but when Cr is contained, the Cr content may be 0.001% or more, 0.01% or more, 0.05% or more, 0.07% or more, or 0.10% or more. Since excessive Cr content may form a large amount of Cr carbide, which may adversely impair hardenability, the Cr content is set to 2.00% or less. The Cr content may be 1.80% or less, 1.50% or less, 1.20% or less, 0.80% or less, 0.60% or less, 0.50% or less, 0.30% or less, or 0.20% or less.
[0039] (Ni: 0 to 2.00%) Ni (nickel) is effective in improving the hardenability of steel and increasing its strength, and may be contained as needed. Since it is not an essential element, the lower limit of the Ni content is 0. This effect can be obtained even with a small amount of Ni contained, but when Ni is contained, the Ni content may be 0.001% or more, 0.01% or more, 0.02% or more, 0.03% or more, 0.04% or more, or 0.05% or more. Since excessive addition of Ni increases costs, the Ni content is set to 2.00% or less. The Ni content may be 1.80% or less, 1.50% or less, 1.20% or less, 0.80% or less, 0.60% or less, 0.50% or less, 0.40% or less, 0.20% or less, or 0.15% or less.
[0040] (Cu: 0 to 2.00%) Cu (copper) is effective in improving the hardenability of steel and increasing its strength, so it may be contained as needed. Since it is not an essential element, the lower limit of the Cu content is 0. This effect can be obtained even with a small amount of Cu contained, but when contained, the Cu content may be 0.001% or more, 0.01% or more, 0.02% or more, 0.03% or more, 0.05% or more, or 0.07% or more. From the viewpoint of suppressing a decrease in toughness, cracking of the slab after casting, and a decrease in weldability, the Cu content is set to 2.00% or less. The Cu content may be 1.80% or less, 1.50% or less, 1.20% or less, 1.00% or less, 0.80% or less, 0.60% or less, 0.50% or less, 0.30% or less, 0.20% or less, or 0.15% or less.
[0041] (Mo: 0 to 1.00%) Mo (molybdenum) is effective in improving the hardenability of steel and increasing its strength, and may therefore be contained as needed. Since it is not an essential element, the lower limit of the Mo content is 0. This effect can be obtained even with a small amount of Mo contained, but when Mo is contained, the Mo content may be 0.001% or more, 0.01% or more, 0.02% or more, 0.03% or more, 0.05% or more, or 0.06% or more. From the viewpoint of suppressing a decrease in toughness, the Mo content is set to 1.00% or less. The Mo content may be 0.80% or less, 0.60% or less, 0.40% or less, 0.30% or less, 0.20% or less, or 0.15% or less.
[0042] (W: 0 to 1.00%) W (tungsten) is effective in improving the hardenability of steel and increasing its strength, and may therefore be contained as needed. Since it is not an essential element, the lower limit of the W content is 0. This effect can be obtained even with a small amount of W contained, but when W is contained, the W content may be 0.001% or more, 0.01% or more, 0.02% or more, or 0.03% or more. From the viewpoint of suppressing a decrease in toughness, the W content is set to 1.00% or less. The W content may be 0.80% or less, 0.60% or less, 0.40% or less, 0.30% or less, 0.20% or less, 0.15% or less, or 0.10% or less.
[0043] (Ca: 0 to 0.1000%) Ca (calcium) is an element that contributes to inclusion control, particularly to finely dispersing inclusions, and has the effect of increasing toughness, and therefore may be contained as needed. Since it is not an essential element, the lower limit of the Ca content is 0. This effect can be obtained even with a trace amount of Ca, but when Ca is contained, the Ca content may be 0.0001% or more, 0.0005% or more, 0.0010% or more, 0.0020% or more, 0.0040% or more, 0.0060% or more, or 0.0070% or more. If Ca is contained in excess, deterioration of surface properties may become apparent, so the Ca content is set to 0.1000% or less. The Ca content may be 0.0800% or less, 0.0600% or less, 0.0500% or less, 0.0400% or less, 0.0300% or less, or 0.0200% or less.
[0044] (Mg: 0 to 0.100%) Mg (magnesium) is an element that contributes to inclusion control, particularly to the fine dispersion of inclusions, and has the effect of increasing toughness, and therefore may be contained as needed. Since it is not an essential element, the lower limit of the Mg content is 0. This effect can be obtained even with a small amount of Mg contained, but when contained, the Mg content may be 0.0001% or more, 0.0005% or more, 0.001% or more, 0.002% or more, 0.004% or more, 0.008% or more, 0.010% or more, or 0.015% or more. Since excessive Mg content may cause noticeable deterioration in surface properties, the Mg content is set to 0.100% or less. The Mg content may be 0.090% or less, 0.080% or less, 0.070% or less, 0.050% or less, 0.040% or less, or 0.030% or less.
[0045] (Zr: 0 to 0.100%) Zr (zirconium) is an element that contributes to inclusion control, particularly to the fine dispersion of inclusions, and has the effect of increasing toughness, and therefore may be contained as needed. Since it is not an essential element, the lower limit of the Zr content is 0. Although this effect can be obtained even with a trace amount, the Zr content, when contained, may be 0.001% or more, 0.03% or more, 0.005% or more, 0.08% or more, or 0.010% or more. Since excessive Zr content may cause deterioration of surface properties to become apparent, the Zr content is set to 0.100% or less. The Zr content may be 0.090% or less, 0.080% or less, 0.060% or less, 0.050% or less, 0.040% or less, or 0.030% or less.
[0046] (Hf: 0 to 0.10%) Hf (hafnium) is an element that contributes to inclusion control, particularly to finely dispersing inclusions, and has the effect of increasing toughness, and therefore may be contained as needed. Since it is not an essential element, the lower limit of the Hf content is 0. This effect can be obtained even with a trace amount, but when contained, the Hf content may be 0.001% or more, 0.002% or more, or 0.005% or more. If Hf is contained in excess, deterioration of surface properties may become apparent, so the Hf content may be 0.10% or less, 0.08% or less, 0.06% or less, 0.05% or less, 0.04% or less, 0.03% or less, or 0.02% or less.
[0047] (REM: 0 to 0.100%) REM (rare earth element) is an element that contributes to inclusion control, particularly to the fine dispersion of inclusions, and has the effect of increasing toughness, and therefore may be contained as needed. Since it is not an essential element, the lower limit of the REM content is 0. Although this effect can be obtained even with a small amount of REM, when REM is contained, the REM content may be 0.0001% or more, 0.005% or more, or 0.001% or more. Since excessive REM content may cause deterioration of surface properties to become apparent, the REM content is set to 0.100% or less. The REM content may be 0.090% or less, 0.080% or less, 0.060% or less, 0.050% or less, 0.040% or less, 0.030% or less, 0.020% or less, 0.010% or less, or 0.005% or less. REM is an abbreviation for Rare Earth Metal, and refers to elements belonging to the lanthanide series. REM is usually added as misch metal.
[0048] (Remainder) In the steel plate constituting the welded joint according to this embodiment, the remainder other than the above chemical components is Fe and impurities. Here, the term "impurities" refers to components that are mixed in due to various factors in the manufacturing process, including raw materials such as ore and scrap, when industrially manufacturing the steel plate. The impurities do not adversely affect the LME resistance of the welded joint according to this embodiment during manufacturing, that is, they are contained in a range that achieves the LME resistance required for the steel plate according to this embodiment. Specific elements include, for example, O (oxygen). The content of O contained as an impurity may be, for example, 0.0500% or less, 0.0300% or less, 0.0200% or less, or 0.0100% or less. However, from the viewpoint of manufacturing costs, the content of O may be 0.00001% or more, 0.00005% or more, or 0.0001% or more.
[0049] (Method of Analyzing Chemical Components) The chemical components of steel sheets may be analyzed using an elemental analysis method known to those skilled in the art, for example, inductively coupled plasma mass spectrometry (ICP-MS). However, C and S may be measured using a combustion-infrared absorption method, and N may be measured using an inert gas fusion-thermal conductivity method. O may be measured using an inert gas fusion-infrared absorption method. These analyses may be performed on samples collected from the steel sheets according to JIS G0417:1999.
[0050] [High Ferrite Layer] In the high-strength steel plate constituting the welded joint of this embodiment, a high ferrite layer is present at a position 50 μm outward from the end of the pressure welded joint, with a thickness of 5 μm or more from the surface of the high-strength steel plate in the thickness direction of the high-strength steel plate. Here, the high ferrite layer refers to a structure in which the area ratio of the ferrite phase is 90% or more. In addition, the position 50 μm outward from the end of the pressure welded joint may be considered as the "heat-affected zone." The welded joint of this embodiment is characterized in that a high ferrite layer formed during steel plate manufacturing is present even in the heat-affected zone affected by the welding heat during the production of the welded joint.
[0051] Figure 1 shows an example of an SEM micrograph of the surface layer of a high-strength steel plate constituting a welded joint of this embodiment, located 50 µm outward from the end of the pressure weld. Figure 1 shows a cross section of the steel plate in the thickness direction, with the upper side being the steel plate surface. As shown in Figure 1, in the welded joint of this embodiment, a high-ferrite layer 1, in which the area ratio of the ferrite phase is 90% or more, is present on the surface side of the steel plate in the heat-affected zone caused by welding. The presence of a B-enriched portion, described below, in this layer improves LME resistance during the production of the welded joint.
[0052] Since the effect of improving LME resistance can be obtained when the thickness of the high ferrite layer is 5 μm or more, the upper limit of the thickness is not particularly limited. For example, it may be 100 μm or less, 80 μm or less, 60 μm or less, or 40 μm or less. From the viewpoint of LME resistance, the thickness of the high ferrite layer is preferably thicker, and is preferably 8 μm or more, more preferably 10 μm or more, 12 μm or more, 15 μm or more, 20 μm or more, or 25 μm or more.
[0053] The structure of the high ferrite layer other than ferrite is not limited, and may be, for example, one or more of martensite, bainite, and cementite.
[0054] The thickness of the high ferrite layer is determined by nital etching the thickness cross section of the steel sheet and observing it with an SEM at 1000x magnification, and distinguishing between ferrite and hard structures containing relatively large amounts of cementite, such as martensite and bainite, based on the structural morphology. The thickness of the high ferrite layer is determined by measuring five measurement ranges, each 500 μm apart in the direction perpendicular to the thickness direction, at intervals of 1000 μm, and averaging the measurements. Here, the area ratio of ferrite refers to the area ratio determined by observing the thickness cross section. Even if there are localized locations in the thickness direction where the area ratio of ferrite is less than 90%, this does not pose a problem as long as the area ratio of ferrite is 90% or more in the thickness cross section from the surface to a depth of 5 μm.
[0055] The ferrite area ratio is determined by cutting a cross section of the steel sheet in the thickness direction perpendicular to the rolling direction, mirror-polishing it, revealing the steel structure with nital solution, and capturing a secondary electron image using a field-emission scanning electron microscope. The observation position is within 500 μm from the surface of the sheet thickness or the interface between the coating layer and the steel sheet, and five equally spaced fields are observed. The fraction of each structure is calculated using the point-counting method for the obtained structure photograph. More specifically, a grid is first drawn with equal intervals on the structure photograph. Next, it is determined whether the structure at each grid point corresponds to tempered martensite, pearlite, ferrite, fresh martensite, retained austenite, or bainite. The fraction of each structure can be measured by determining the number of grid points corresponding to each structure and dividing by the total number of grid points. The greater the total number of grid points, the more accurately the area ratio can be determined. In this embodiment, the grid spacing is 2 μm × 2 μm, and the total number of grid points is 1,500.
[0056] The criteria for determining whether a material is tempered martensite, pearlite, ferrite, fresh martensite, retained austenite, or bainite are as follows: A region that has a substructure (lath boundaries, block boundaries) within the grains and where carbides are precipitated with multiple variants is determined to be tempered martensite; A region where cementite is precipitated in a lamellar form is determined to be pearlite; A region that has low brightness and no substructure is visible is determined to be ferrite; A region that has high brightness and where the substructure is not revealed by etching is determined to be fresh martensite or retained austenite; A region that does not fall into any of the above categories is determined to be bainite. Simply put, the area fraction of the ferrite phase can be determined by distinguishing between ferrite and other structures.
[0057] Ferrite is a structure that is less susceptible to LME than austenite, and the presence of a ferrite-rich layer in the surface layer of the steel sheet improves LME resistance during the production of welded joints. In this embodiment, the presence of a B-enriched portion, which will be described later, further improves LME resistance.
[0058] [B-enriched portion] In the high-strength steel plate constituting the welded joint of this embodiment, a B-enriched portion exists at a position 50 μm outward from the end of the pressure weld, with a thickness of 1.0 μm or more from the surface of the high-strength steel plate in the thickness direction of the high-strength steel plate. Here, the B-enriched portion refers to a portion where the B intensity determined by TOF-SIMS (Time-of-Flight Secondary Ion Mass Spectrometry) measurement is at least twice the B intensity at a depth of 50 μm determined by TOF-SIMS measurement. Figure 2 shows an example of measurement results using TOF-SIMS. Figure 2 shows the measurement results of cross section C of the overlapping portion of two steel plates in a welded joint, with the vertical direction being the thickness direction of the steel plate. The brighter the measurement results in Figure 2, the higher the B concentration. The dark area near the center is the gap between the two steel plates. The measurement results in Figure 2 show that the B concentration is high near the surface of the steel plate.
[0059] The analysis by TOF-SIMS was performed using a TOF-SIMS (manufactured by ION-TOF) as the device, and the primary ions were Bi32+ The measurement is performed under the conditions of a pressure voltage of 25 kV and a measurement area of 50 μm square. The measurement is performed by moving the field of view in the thickness direction of the high-strength steel sheet so as to measure the B-enriched portion on the surface of the high-strength steel sheet and a position 50 μm deep from the surface.
[0060] The thicker the B-enriched portion, the better from the viewpoint of LME resistance during the production of a welded joint. The thickness is preferably 2.0 μm or more, more preferably 3.0 μm or more, 4.0 μm or more, or even more preferably 5.0 μm or more.
[0061] In the welded joint of this embodiment, it is believed that B concentrated in the surface layer of the steel plate constituting the welded joint segregates at the Fe grain boundaries and inhibits the penetration of Zn, thereby suppressing LME during the production of the welded joint. Such a B distribution in the surface layer can be obtained by producing a steel plate from molten steel having the above-mentioned chemical composition by the production method described below.
[0062] [Plated layer] The high-strength steel sheet constituting the welded joint of this embodiment may have a Zn-containing plated layer on its surface. The plated layer may be formed on only one side of the high-strength steel sheet, or on both sides, or may be formed on only a part of the surface.
[0063] The plating layer is not particularly limited as long as it contains Zn, and examples include Zn-0.2%Al (GI), Zn-(0.3 to 1.5)%Al, Zn-4.5%Al, Zn-0.09%Al-10%Fe (GA), Zn-1.5%Al-1.5%Mg, Zn-11%Al-3%Mg-0.2%Si, Zn-11%Ni, Zn-15%Mg, Zn-20%Al-7%Mg, and Zn-30%Al-10%Mg.
[0064] The chemical composition of the plating layer can be determined by dissolving the plating layer in an acid solution to which an inhibitor that suppresses corrosion of the steel sheet has been added, and measuring the resulting solution by ICP (inductively coupled plasma) emission spectroscopy.
[0065] The thickness of the plating layer may be, for example, 3 to 50 μm. The coating weight of the plating layer is not particularly limited, but may be, for example, 10 to 170 g / m per side. 2In this embodiment, the coating weight of the plating layer is determined by dissolving the plating layer in an acid solution containing an inhibitor that suppresses corrosion of the steel sheet, and measuring the change in weight before and after the plating layer is removed by pickling. As the acid solution containing an inhibitor, for example, a 10% hydrochloric acid solution containing 0.06 mass % of an inhibitor (Ivit 710K, manufactured by Asahi Chemical Industry Co., Ltd.) may be used. After the plating layer is removed, the base steel sheet is washed with water and dried.
[0066] The thickness of the plating layer may be 5 μm or more, 7 μm or more, or 10 μm or more. The thickness of the plating layer may be 45 μm or less, 40 μm or less, 35 μm or less, or 30 μm or less. The coating weight of the plating layer is 15 g / m per side. 2 Above, 20g / m 2 Above, 25g / m 2 Above, 30g / m 2 The coating weight of the plating layer may be 160 g / m or more per side. 2 Below, 140g / m 2 Below, 120g / m 2 Below, 100g / m 2 It may be the following:
[0067] When a welded joint includes a general steel plate or the like that is not the high-strength steel plate described above, the steel plate that is not the high-strength steel plate may have the above-described plating layer.
[0068] The welded joint of this embodiment effectively improves LME resistance during manufacturing even when the steel sheets constituting the welded joint, particularly the outermost high-strength steel sheet, are not plated. LME cracking does not occur in the absence of molten zinc. However, for example, when a welding electrode spot-welded to a zinc-plated steel sheet is used to weld an unplated steel sheet, the plating adhering to the welding electrode may melt and transfer to the unplated steel sheet, resulting in LME cracking. Even in such a case, the welded joint of this embodiment effectively suppresses LME cracking during manufacturing because the B concentrated in the surface layer prevents the molten zinc from penetrating the Fe grain boundaries. Therefore, plating is not an essential component of the welded joint of this embodiment.
[0069] [B distribution in surface layer] In the welded joint of this embodiment, in the steel plate constituting the welded joint, particularly in the non-heat-affected zone of a high-strength steel plate, it is preferable that the depth satisfying the following formula (1) in a GDS (high-frequency glow discharge optical emission spectroscopy) measurement in the thickness direction of the steel plate is 1.5 μm or more from the surface of the steel plate.
[0070] Bx / B150≧5…(1)
[0071] In the above formula (1), Bx represents the luminescence intensity at a point at a depth x (μm) away from the interface between the steel sheet and the plating layer in the thickness direction of the steel sheet. Furthermore, B150 represents the luminescence intensity at a depth of 150 μm away from the interface between the steel sheet and the plating layer in the thickness direction of the steel sheet. In this embodiment, the "thickness direction" refers to a direction perpendicular to the interface between the steel sheet and the plating layer. A point away from the interface between the steel sheet and the plating layer in the thickness direction of the steel sheet refers to a point away from the interface between the steel sheet and the plating layer in the thickness direction of the steel sheet.
[0072] The left side of the above formula (1) represents the ratio of the B concentration at depth x to the B concentration at a depth of 150 μm. That is, Bx / B150≧5 means that the B concentration at depth x is 5 times or more the B concentration at a depth of 150 μm. The B concentration at a depth of 150 μm may be considered to be the B concentration at the center of the steel sheet thickness, and Bx / B150≧5 means that B is enriched at depth x. The expression "a depth of 1.5 μm or more from the surface of the steel sheet that satisfies formula (1)" means that formula (1) is satisfied in a range from the surface of the steel sheet to a depth of 1.5 μm or more in the thickness direction of the steel sheet, and that B is enriched in a range to a depth of 1.5 μm or more in the thickness direction of the steel sheet.
[0073] In this embodiment, the surface of the steel sheet and the interface between the steel sheet and the plating layer are defined as follows. First, the Fe content in the thickness direction of the plated steel sheet is measured by GDS measurement. The highest Fe content value is defined as the Fe content of the steel sheet. The point where the Fe content is 5% of the Fe content of this steel sheet is defined as the "surface of the steel sheet." When a plating layer is formed on the surface of the steel sheet, the interface between the steel sheet and the plating layer is considered to be the surface of the steel sheet and is used as the starting point for the depth of the GDS measurement. The "interface between the steel sheet and the plating layer" is defined as the point where the Fe content determined by GDS measurement is 93% of the Fe content of the steel sheet.
[0074] As described above, B is concentrated in the surface layer of the steel sheet, and thereby B segregates at the Fe grain boundaries in the surface layer structure, which prevents molten zinc from penetrating the Fe grain boundaries during spot welding and further prevents the occurrence of LME during the production of welded joints.
[0075] (GDS measurement method) For Bx and B150, a method is used in which the surface of the target steel sheet is placed in an Ar atmosphere by GDS, a voltage is applied to generate glow plasma, and the steel sheet surface is sputtered while being analyzed in the depth direction. Then, elements contained in the material are identified from the element-specific emission spectrum wavelengths emitted by excited atoms in the glow plasma, and the emission intensity of the identified elements is estimated.
[0076] The data in the depth direction can be estimated from the sputtering time. Specifically, by determining the relationship between the sputtering time and the sputtering depth in advance using a standard sample, the sputtering time can be converted into the sputtering depth. Therefore, the sputtering depth converted from the sputtering time can be defined as the depth from the surface of the material. The sputtering time is set so that the sputtering depth exceeds at least 150 μm.
[0077] The GDS measurement is performed five times in the thickness direction, and the average value is taken as the B concentration. The measurement conditions are as follows: Bx and B150 are the B concentrations corresponding to a depth of x (μm) and a depth of 150 μm, respectively.
[0078] Apparatus: High-frequency glow discharge optical emission analyzer (manufactured by LECO Japan LLC, model number "GDS850A" Ar gas pressure: 0.3 MPa Anode diameter: 4 mmφ RF output: 30 W Measurement time: 200 to 1500 seconds
[0079] In order to obtain the effect of suppressing the occurrence of LME, the depth at which Bx / B150≧5.0 is satisfied is preferably 1.5 μm or more. From the viewpoint of LME resistance, a larger Bx / B150 is more preferable, and it may be 1.6 μm or more, 1.8 μm or more, 2.0 μm or more, 2.5 μm or more, or 3.0 μm or more. Since Bx / B150 is the ratio of the B concentration at depth x to the B concentration at a depth of 150 μm, the depth at which Bx / B150≧5.0 is satisfied is less than 150 μm. Even if the depth at which Bx / B150≧5.0 is deep, LME resistance is not reduced, but the depth at which Bx / B150≧5.0 is satisfied may be 100.0 μm or less, 50.0 μm or less, 30.0 μm or less, 20.0 μm or less, or 10.0 μm or less.
[0080] In the welded joint of this embodiment, B concentrated in the surface layer of the steel plate constituting the welded joint segregates at the Fe grain boundaries. This is thought to suppress the penetration of molten zinc into the Fe grain boundaries during spot welding and to suppress LME during the production of the welded joint. Such a B distribution in the surface layer can be obtained by producing a steel plate from molten steel having the above-mentioned chemical composition using the production method described below.
[0081] <B Concentration in the Range up to a Depth of 5.0 μm> In the steel plate constituting the welded joint of this embodiment, it is preferable that the following formula (2) be further satisfied in the above-described GDS measurement.
[0082] Bmax / B150≧8…(2)
[0083] In the above formula (2), Bmax represents the maximum value of the emission intensity of B in the range from the surface of the steel sheet to a depth of 5.0 μm.
[0084] The left side of equation (2) represents the ratio of the maximum value of B emission intensity in the range from the surface of the steel sheet to a depth of 5.0 μm to the B concentration at a depth of 150 μm. That is, Bmax / B150≧8 means that the B concentration at the position where B is most concentrated in the range from the surface of the steel sheet to a depth of 5.0 μm is 8 times or more the B concentration at a depth of 150 μm. The B concentration at a depth of 150 μm can be regarded as the B concentration at the center of the steel sheet thickness, and Bmax / B150≧8 means that B is highly concentrated in the range from the surface of the steel sheet to a depth of 5.0 μm, i.e., in the vicinity of the surface.
[0085] From the viewpoint of LME resistance, the larger Bmax / B150 is the more preferable, and it is preferably 10 or more, more preferably 12 or more, 14 or more, or even more preferably 16 or more.
[0086] It is not essential for the steel sheet of this embodiment to satisfy formula (2), and good LME resistance can be obtained as long as formula (1) is satisfied, even if formula (2) is not satisfied. By making the B distribution in the surface layer such that formula (2) is satisfied, B that is more highly concentrated in the surface layer of the steel segregates at the Fe grain boundaries, preventing the penetration of molten zinc, and therefore, a greater effect of suppressing LME can be obtained.
[0087] [Thickness] The thickness of the steel plate constituting the welded joint of the present invention is not particularly limited. For example, it can be 0.6 to 3.2 mm. The thickness may be 0.8 mm or more, or 1.0 mm or more. The thickness may be 3.0 mm or less, 2.8 mm or less, 2.6 mm or less, 2.5 mm or less, 2.4 mm or less, 2.2 mm or less, 2.0 mm or less, or 1.8 mm or less.
[0088] <Method for Manufacturing Steel Plate> Next, a method for manufacturing the steel plate that constitutes the welded joint of this embodiment will be described.
[0089] The steel sheet that constitutes the welded joint according to this embodiment can be obtained by a manufacturing method including a casting step of casting molten steel with adjusted chemical composition to form a steel billet, a hot rolling step of hot rolling the steel billet to obtain a hot-rolled steel sheet, a coiling step of coiling the hot-rolled steel sheet, a pickling step of pickling the coiled hot-rolled steel sheet, a cold-rolling step of cold-rolling the pickled hot-rolled steel sheet to obtain a cold-rolled steel sheet, and an annealing step of annealing the cold-rolled steel sheet. Alternatively, the hot-rolled steel sheet may be pickled and then cold-rolled directly without being coiled after the hot rolling step.
[0090] [Casting Step] The conditions for the casting step are not particularly limited. For example, after melting in a blast furnace or an electric furnace, various secondary smelting processes may be carried out, and then casting may be carried out by a conventional method such as continuous casting or ingot casting.
[0091] [Hot Rolling Process] A hot-rolled steel plate can be obtained by hot-rolling the steel slab obtained by casting. The hot rolling process is carried out by reheating the cast steel slab directly or after cooling it once, followed by hot rolling. When reheating is carried out, the heating temperature of the steel slab may be, for example, 1100 to 1250°C. In the hot rolling process, rough rolling and finish rolling are usually carried out. The temperature and reduction ratio of each rolling step may be changed as appropriate depending on the desired metal structure and plate thickness. For example, the finishing temperature of finish rolling may be 900 to 1050°C, and the reduction ratio of finish rolling may be 10 to 50%.
[0092] [Coiling process] The hot-rolled steel sheet can be coiled at a predetermined temperature. The coiling temperature may be changed as appropriate depending on the desired metal structure, etc., and may be, for example, 500 to 800°C. The hot-rolled steel sheet may be subjected to a predetermined heat treatment by recoiling before or after coiling. Alternatively, the hot-rolled steel sheet may be pickled after the hot rolling process without being coiled, and then cold-rolled as described below.
[0093] [Pickling Process] The hot-rolled steel sheet is subjected to pickling. In the manufacturing method of the steel sheet constituting the welded joint of this embodiment, the unevenness of the steel sheet surface after pickling is controlled for the purpose of concentrating B in the surface layer of the steel sheet in the subsequent annealing process. Specifically, the unevenness is set to 1.5 μm or more in terms of Ra, which is the arithmetic mean height defined in JIS B0601:2013. This condition means that a certain degree of unevenness exists on the steel sheet surface. If the unevenness is small, the strain imparted to the surface layer of the steel sheet becomes small, so that internal oxidation does not progress even when annealing at a high dew point as described below, and the concentration of B in the surface layer of the steel sheet does not progress.
[0094] The larger the Ra of the unevenness, the better, and it is preferably 2.0 μm or more, more preferably 2.5 μm or more, 3.0 μm or more, and even more preferably 3.5 μm or more.
[0095] The unevenness of the steel sheet surface after pickling is determined as an arithmetic mean roughness Ra by randomly selecting 10 locations on the surface of the surface layer side, measuring the surface profile at each location with a contact surface roughness meter, and arithmetically averaging the surface roughnesses at those locations, in accordance with JIS B 0601:2013. It is not necessary to constantly measure the unevenness of the steel sheet surface after pickling, and once the pickling conditions under which the desired unevenness is formed have been determined, measurement of the unevenness may be omitted.
[0096] The surface roughness of the steel sheet varies depending on the pickling conditions, and therefore, the conditions may be adjusted appropriately to obtain the above-mentioned unevenness. For example, pickling may be performed using a 1 to 10 mass % hydrochloric acid solution at a temperature of 20 to 95°C for a pickling time of 30 to less than 200 seconds.
[0097] The surface of the steel sheet after pickling has such irregularities, and by rolling out these irregularities in the subsequent cold rolling process to impart strain to the surface layer of the steel, the concentration of B in the surface layer of the steel sheet is promoted in the subsequent annealing process.
[0098] [Cold Rolling Process] After subjecting the hot-rolled steel sheet to pickling or the like, the hot-rolled steel sheet can be cold-rolled to obtain a cold-rolled steel sheet. In the cold rolling process, the unevenness imparted in the above-mentioned pickling process is rolled and crushed, thereby imparting strain to the surface layer of the steel sheet. Therefore, the roll used for cold rolling preferably has a small surface roughness, and the surface roughness of the roll is preferably 1.0 μm or less in Ra. The surface roughness of the roll may be 0.8 μm or less, 0.6 μm or less, or 0.5 μm or less in Ra. The reduction ratio of the cold rolling may be appropriately changed depending on the desired metal structure and sheet thickness, and may be, for example, 20 to 80%. After the cold rolling process, the steel sheet may be cooled to room temperature, for example, by air cooling.
[0099] In the cold rolling process, the unevenness on the surface of the hot-rolled steel sheet is rolled out, imparting strain to the surface layer of the steel sheet, which promotes the concentration of B in the surface layer of the steel sheet in the subsequent annealing process.
[0100] [Annealing Step] After the cold rolling step, the obtained cold-rolled steel sheet is subjected to the following high dew-point annealing. In the method for producing a steel sheet and a galvannealed steel sheet according to the present embodiment, the annealing step prevents external oxidation from progressing on the surface of the steel sheet, but promotes internal oxidation in the surface layer of the steel sheet, i.e., oxidation progresses toward the inside of the steel sheet.
[0101] In the annealing step of this embodiment, the steel sheet having strain imparted to the surface layer by the above-described steps is held at a high dew point. Specifically, the holding temperature in the annealing step is 760 to 900°C to promote internal oxidation and B concentration, and the holding time at the holding temperature is 0 to 360 seconds. The holding temperature may be 770°C or higher, 780°C or higher, or 790°C or higher. The holding temperature may be 890°C or lower, 880°C or lower, or 870°C or lower. The holding time may be 10 seconds or higher, 30 seconds or higher, 50 seconds or higher, or 60 seconds or higher. The holding time may be 330 seconds or lower, 300 seconds or lower, 270 seconds or lower, 240 seconds or lower, or 200 seconds or lower.
[0102] The annealing atmosphere is preferably a non-oxidizing atmosphere, and can be, for example, N2-2 to 4 vol% H2. The oxygen concentration of the atmosphere is preferably 50 ppm or less, and may be 30 ppm or less, 20 ppm or less, or 10 ppm or less. By adopting these conditions, internal oxidation can proceed while suppressing oxidation of the coating surface. The rate of temperature rise to the holding temperature is not particularly limited. The rate of temperature rise may be, for example, 1 to 10°C / sec. If the rate of temperature rise is less than 1°C / sec, it may take too long to raise the temperature to the control temperature, which may result in thick oxide on the surface of the coating layer. On the other hand, if the rate of temperature rise is more than 10°C / sec, internal oxidation may not proceed sufficiently, and the strain imparted to the steel sheet surface layer may not be sufficiently released, resulting in insufficient boron concentration. From these perspectives, the rate of temperature rise may be 2°C / sec or more, 3°C / sec or more, or 4°C / sec or more. The temperature ramp rate may be 9°C / sec or less, 8°C / sec or less, or 7°C / sec or less.
[0103] In the annealing process of the method for manufacturing the steel sheet that constitutes the weld joint of this embodiment, the dew point of the atmosphere is changed in the first half and the second half of the temperature rise. Specifically, the dew point from room temperature to the controlled temperature is different from the dew point from the controlled temperature to the holding time.
[0104] The control temperature is a temperature at which the dew point is changed, and is set to 450 to 550° C. During the temperature rise from room temperature to the control temperature, the dew point of the annealing atmosphere is set to -40° C. or higher and -20° C. or lower. During the temperature rise from the control temperature to the holding temperature, the dew point of the annealing atmosphere is set to -20° C. or higher and 20° C. or lower.
[0105] If the control temperature is less than 450°C, the dew point increases at low temperatures, causing internal oxidation to proceed at low temperatures, releasing the strain imparted to the steel sheet surface layer, and preventing sufficient internal oxidation from occurring to suppress the deboronization phenomenon between the control temperature and the holding temperature.If the control temperature is more than 550°C, the strain imparted to the steel sheet surface layer is released before internal oxidation proceeds at high temperatures, preventing sufficient internal oxidation from occurring to suppress the deboronization phenomenon.
[0106] If the dew point during the temperature rise from room temperature to the control temperature is less than -40°C, external oxidation of Si and Mn may occur, and internal oxidation may not proceed between the control temperature and the holding temperature. If the dew point during the temperature rise from room temperature to the control temperature is more than -20°C, internal oxidation proceeds at a low temperature, and the strain imparted to the surface layer of the steel sheet is released. As a result, internal oxidation to suppress the deboronization phenomenon may not occur between the control temperature and the holding temperature.
[0107] Similarly, if the dew point between the control temperature and the holding temperature is −20° C. or lower, internal oxidation to suppress the deboronization may not proceed sufficiently. If the dew point between the control temperature and the holding temperature is higher than 20° C., external oxidation may proceed, and internal oxidation to suppress the deboronization may not proceed sufficiently.
[0108] Furthermore, the dew point during the temperature rise from the control temperature to the holding temperature is set to be 10° C. or more higher than the dew point during the temperature rise from room temperature to the control temperature. This allows internal oxidation to proceed, and the concentration of B to be promoted.
[0109] From the viewpoint of suitably concentrating B, the control temperature may be 460°C or higher, 470°C or higher, or 480°C or higher. The control temperature may be 540°C or lower, 530°C or lower, or 520°C or lower. From the viewpoint of suitably concentrating internal oxidation and B, the dew point during the temperature rise from room temperature to the control temperature may be -38°C or higher, -37°C or higher, or -35°C or higher. The dew point during the temperature rise from room temperature to the control temperature may be 18°C or lower, 17°C or lower, or 15°C or lower. The dew point from the control temperature to the holding temperature may be -18°C or higher, -17°C or higher, or -15°C or higher. The dew point from the control temperature to the holding temperature may be 18°C or lower, 17°C or lower, or 15°C or lower.
[0110] In a state in which strain is imparted to the surface layer of the steel sheet by the above-described method, by raising the dew point at a temperature equal to or higher than the control temperature in the annealing step, internal oxidation rapidly progresses in the surface layer of the steel sheet, and B is incorporated into the oxides formed inside the steel sheet, thereby concentrating B in the surface layer of the steel sheet and segregating B at the Fe grain boundaries, thereby obtaining the above-described B concentration distribution in the surface layer.
[0111] Annealing is performed under a tension of 1 to 20 MPa. Applying tension during annealing makes it possible to introduce strain into the steel sheet more effectively, and promotes B enrichment in the surface layer.
[0112] [Plating step] A plated steel sheet may be produced by a production method including a plating step using the steel sheet produced as described above. The plating step may be carried out according to a method known to those skilled in the art. The plating step may be carried out by, for example, a hot-dip plating method, an electroplating method, a vapor deposition plating method, a thermal spraying method, or a cold spraying method. Preferably, the plating step is carried out by a hot-dip plating method. The conditions for the plating step may be appropriately set taking into consideration the chemical composition, thickness, and coating weight of the desired plating layer, etc.
[0113] [Alloying Treatment Step] After the plating treatment step, a known alloying treatment may be performed to form an alloyed plating. The conditions for the alloying treatment step may be appropriately set in consideration of the chemical composition, thickness, coating weight, etc. of the desired plating layer.
[0114] [Spot welding process] A plurality of the above-described steel plates are stacked and spot welded to obtain a welded joint. The steel plates may be of the same type or may have different chemical compositions. As long as at least one steel plate arranged on the outermost side is the above-described high-strength steel plate, the other steel plates may be general commercially available steel plates.
[0115] The conditions for spot welding are not particularly limited. For example, spot welding can be performed using a dome radius type welding electrode with a tip diameter of 8 mm, with a pressure of 5.0 kN, a welding time of 1.2 seconds, and a current of 12 kA.
[0116] The welded joint according to the present invention is capable of suppressing LME cracking during manufacturing, and therefore can be suitably used in a wide range of fields such as automobiles, home appliances, building materials, etc. It is particularly preferable that it be used in the automobile field.
[0117] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. First, a method for manufacturing steel plates used to manufacture the welded joints in each example will be described.
[0118] Example No. 1 Molten steel was produced in a blast furnace and cast by continuous casting to obtain a slab having the chemical composition shown in No. 1 of Table 1. The obtained slab was heated to 1200°C and hot-rolled with a finish rolling ending temperature of 950°C and a finish rolling reduction of 30% to obtain a hot-rolled steel sheet. The obtained hot-rolled steel sheet was coiled at a coiling temperature of 650°C.
[0119] The coiled steel sheet was pickled for 40 seconds using a 5 mass % hydrochloric acid solution at 40° C. After pickling, the steel sheet was cold rolled at a reduction ratio of 50% to obtain a cold-rolled steel sheet. The thickness of the cold-rolled steel sheet was 1.6 mm.
[0120] Thereafter, annealing was performed in a furnace with an oxygen concentration of 20 ppm or less in an N2-4 vol% H2 gas atmosphere at a holding temperature of 800°C and a holding time of 0 seconds to prepare steel sheet samples. The temperature rise rate during annealing was 5.0°C / second. The dew point of the annealing atmosphere was set to a controlled temperature of 500°C, -20°C from room temperature to the controlled temperature, and -10°C from the controlled temperature to the holding temperature. The annealing was performed under a tension of 15 MPa. A holding time of 0 seconds means that the temperature was raised to 800°C and then immediately started to drop.
[0121] <Examples Nos. 2 to 32> Steel sheets were produced under the same conditions as in Example 1, except that the chemical compositions were as shown in Table 1, the annealing conditions were as shown in Table 2, and the coating type was as shown in Table 2. Regarding the coating type in Table 2, "a" indicates that the steel sheet was immersed in a 450°C hot-dip galvanizing bath (Zn-0.14% Al) for 3 seconds, then pulled out at 100 mm / s, and coated with 50 g / m2 of coating weight using N2 wiping gas. 2 "b" refers to hot-dip galvanizing in which the alloying treatment in "a" was omitted; and "c" refers to hot-dip galvanizing in which the plating bath in "a" was Zn-1.5%Al-1.5%Mg and the alloying treatment was omitted.
[0122] (Unevenness after pickling) When producing a steel sheet, the surface unevenness of the hot-rolled steel sheet after pickling was measured. The surface unevenness was measured in accordance with JIS B 0601:2013 by randomly selecting 10 locations on the surface of the surface layer side, measuring the surface profile at each location using a contact surface roughness meter, and calculating the arithmetic average of the surface roughnesses at those locations to obtain the arithmetic average roughness Ra. The surface unevenness of the hot-rolled steel sheet is shown in Table 2.
[0123]
[0124]
[0125] Two steel plates obtained in each example were overlapped and spot-welded using a dome radius type welding electrode with a tip diameter of 8 mm at an impact angle of 5°, a pressure of 5.0 kN, a welding time of 1.2 seconds, and a current of 12 kA to produce a welded joint, and the structure of the heat-affected zone and non-heat-affected zone, as well as the LME resistance during production, were evaluated.
[0126] (Hardness of Steel Plate) The hardness of the steel plate was measured in a non-heat-affected zone located at a distance of 5 mm or more from the outer end of the spot weld of the welded joint. The hardness of the steel plate was measured at a position half the depth of the steel plate in accordance with JIS Z 2244:2009. The measurement load was 200 gf. The hardness was evaluated as follows: A rating of A or higher was considered to be good hardness.
[0127] Rating AAA: 380Hv or more Rating AA: 300Hv or more, less than 380Hv Rating A: 240Hv or more, less than 300Hv Rating B: Less than 240Hv
[0128] (High Ferrite Layer) Samples were cut to 25 mm x 15 mm from a position 50 μm outward from the end of the pressure-welded portion of the welded joint, and subjected to nital etching. The T-section of each sample was observed with an SEM to measure the thickness of the high ferrite layer with a ferrite area ratio of 90% or more. The thickness was measured at five equally spaced points within a range of 500 μm in the T direction, and the average value was calculated. Here, the starting point of the "thickness" was the surface of the steel sheet for unplated steel sheets, and the starting point was the interface between the plating layer and the steel sheet for plated steel sheets, and was determined from the SEM image.
[0129] (B-enriched portion) A sample cut to 30 mm x 30 mm from a position 50 μm outward from the end of the pressure-welded portion of the welded joint was collected, and the thickness of the B-enriched portion was measured by TOF-SIMS measurement. The B-enriched portion was defined as a portion where the B intensity determined by TOF-SIMS measurement was at least twice the B intensity at a depth of 50 μm determined by TOF-SIMS measurement. The TOF-SIMS analysis was performed using a TOF-SIMS (manufactured by ION-TOF) as the apparatus, with primary ions: Bi3 2+ The measurement was performed under the conditions of a voltage of 25 kV and a measurement area of 50 μm square. The measurement was performed by moving the field of view in the thickness direction of the high-strength steel sheet so as to measure the B-enriched portion on the surface of the high-strength steel sheet and a position 50 μm deep from the surface.
[0130] (B Distribution in Steel Sheet Surface Layer in Non-Heat Affected Zone) The B distribution in the steel sheet surface layer in the non-heat affected zone was evaluated as follows.
[0131] GDS was performed using samples cut to a size of 50 mm x 50 mm from the non-heat-affected zone of each weld joint. GDS measurements were performed five times in the plate thickness direction, and the average value was taken as the B concentration. The measurement conditions were as follows: Bx and B150 are the B concentrations corresponding to a depth of x (μm) and a depth of 150 μm, respectively.
[0132] Apparatus: High-frequency glow discharge optical emission analyzer (manufactured by LECO Japan LLC, model number "GDS850A" Ar gas pressure: 0.3 MPa Anode diameter: 4 mmφ RF output: 30 W Measurement time: 200 to 1500 seconds
[0133] From the obtained Bx, the depth satisfying the formula (1): Bx / B150≧5.0 and the value of the left side of the formula (2): Bmax / B150 were obtained.
[0134] (LME resistance during production of welded joints) Two samples were cut to a size of 50 mm x 100 mm from each steel plate and galvannealed steel plate, and these two samples were spot welded using a dome radius welding electrode with a tip diameter of 8 mm at an impact angle of 5°, a pressure of 5.0 kN, a welding time of 1.2 seconds, and a current of 12 kA to produce welded joints. When producing welded joints using unplated steel plates, a welding electrode that had previously been used in spot welding steel plates that had been plated with zinc was used.
[0135] The evaluation of LME resistance during the manufacture of a welded joint will be described with reference to Figure 3. LME resistance was evaluated based on the length of an LME crack (shoulder crack 21) that occurred in the shoulder 14 of a weld 12 formed by spot welding two overlapping steel plates 11. The shoulder refers to the inclined portion of the edge of a depression 13 created by spot welding. The evaluation was performed based on the length of the shoulder crack 21 as follows: In this example, a rating of A or higher was determined to indicate excellent LME resistance during the manufacture of a welded joint.
[0136] Rating AAA: 0 μm Rating AA: More than 0 μm, less than 50 μm Rating A: 50 μm or more, less than 160 μm Rating B: 160 μm or more
[0137] The results of each evaluation are shown in Table 3.
[0138]
[0139] Nos. 1 to 22 are inventive examples, and it was confirmed that they had excellent LME resistance during the production of welded joints.
[0140] In No. 23, the Si content of the steel sheet was low. Therefore, decarburization and internal oxidation did not proceed sufficiently during the annealing process in the steel sheet production, resulting in a thin ferrite layer. In addition, the boron removal phenomenon could not be suppressed, and a B-enriched portion was not formed. As a result, the LME resistance during the production of the welded joint was poor.
[0141] In No. 24, the Si content of the steel plate was high. Therefore, even if a high ferrite layer and a B-enriched portion were formed, LME could not be suppressed. As a result, the LME resistance during the production of the welded joint was poor.
[0142] In No. 25, the dew point was low in the first half of the annealing process during steel sheet production. As a result, Si and Mn were externally oxidized, and internal oxidation did not progress in the second half of the annealing process, resulting in a thin ferrite layer and no B-enriched portion being formed. As a result, the LME resistance during weld joint production was poor.
[0143] In No. 26, the dew point was high in the first half of the annealing process during steel sheet production. As a result, internal oxidation progressed at a low temperature in the first half of the annealing process, the strain imparted to the surface layer of the steel sheet was released, and internal oxidation did not occur between the controlled temperature and the holding temperature. As a result, the boron removal phenomenon could not be suppressed, and the high ferrite layer and the B-enriched portion became thinner. As a result, the LME resistance during weld joint production was poor.
[0144] In No. 27, the dew point was low in the latter half of the annealing process during steel sheet production. As a result, internal oxidation to suppress the deboronization phenomenon did not progress sufficiently, and the high ferrite layer and B-enriched portion became thin. As a result, the LME resistance during weld joint production was poor.
[0145] In No. 28, the dew point was high in the latter half of the annealing process during steel plate production. As a result, external oxidation progressed, and internal oxidation to suppress the deboronization phenomenon did not progress sufficiently, resulting in a thin ferrite layer and no B-enriched portion being formed. As a result, the LME resistance during weld joint production was poor.
[0146] In No. 29, the control temperature was low. As a result, the dew point rose at low temperatures, internal oxidation progressed at low temperatures, the strain applied to the steel sheet surface layer was released, and sufficient internal oxidation to suppress the deboronization phenomenon did not occur between the control temperature and the holding temperature, resulting in thinning of the high ferrite layer and the B-enriched portion. As a result, the LME resistance during the production of welded joints was poor.
[0147] In No. 30, the controlled temperature was high. Therefore, the strain imparted to the surface layer of the steel sheet was released before internal oxidation progressed at high temperatures, and sufficient internal oxidation to suppress the deboronization phenomenon did not occur, resulting in a thin B-enriched portion. As a result, the LME resistance during weld joint production was poor.
[0148] In No. 31, the annealing temperature was low. As a result, internal oxidation and B enrichment did not progress sufficiently, the ferrite-rich layer became thin, and a B-enriched portion was not formed. As a result, the LME resistance during the production of the welded joint was poor.
[0149] In No. 32, the surface unevenness of the steel sheet after pickling during steel sheet production was small. Therefore, sufficient strain was not imparted to the surface layer of the steel sheet, and B did not concentrate in the surface layer of the steel sheet even after high dew-point annealing, resulting in a thin B-enriched portion. As a result, the LME resistance during weld joint production was poor.
[0150] REFERENCE SIGNS LIST 1 high ferrite layer 11 steel plate 12 welded portion 13 dent 14 shoulder portion 21 crack in shoulder portion
Claims
1. A welded joint comprising: a plurality of overlapping steel plates; a nugget joining the plurality of steel plates; a spot weld having a pressure weld portion and a heat-affected zone formed around the nugget; a non-heat-affected zone which is an area outside the heat-affected zone; and a separation portion formed around the pressure weld portion, wherein at least one of the plurality of steel plates arranged outermost is a high-strength steel plate having a Vickers hardness of 240 Hv or more at the center of the plate thickness, and the chemical composition of the high-strength steel plate is, in mass %, C: 0.05-0.40%, Si: 0.7-3.0%, Mn: 0.1-5.0%, sol. Al: 0-2.0%, P: 0.0300% or less, S: 0.0300% or less, N: 0.0100% or less, B: 0.0005-0.0050%, Ti: 0.0010-0.1000%, Nb: 0-0.2000%, V: 0-0.15%, Cr: 0-2.00%, Ni: 0-2.00%, Cu: 0-2.00%, Mo: 0-1.00%, W: 0-1.00%, Ca: 0-0.1000%, Mg: 0-0.100%, Zr: 0-0.100%, Hf: 0-0.100%, and REM: 0-0.100%. and the balance being Fe and impurities; a high ferrite layer having an area ratio of ferrite phase of 90% or more is present at a position 50 μm outward from an end of the pressure weld, with a thickness of 5 μm or more from the surface of the high strength steel plate in the thickness direction of the high strength steel plate; and a B-enriched portion having a B intensity two times or more the B intensity at a depth of 50 μm determined by TOF-SIMS measurement is present at a position 50 μm outward from the end of the pressure weld, with a thickness of 1.0 μm or more from the surface of the high strength steel plate.
2. The welded joint according to claim 1, characterized in that the high-strength steel plate has a Zn-containing plating layer formed on one or both sides of the high-strength steel plate.
3. The welded joint according to claim 1 or 2, characterized in that in the non-heat-affected zone, the depth at which the emission intensity Bx at a depth x (μm) in a GDS measurement from the steel plate surface in the thickness direction and the emission intensity B150 at a depth of 150 μm satisfy the following relationship: Bx / B150≧5 ... (1) is 1.5 μm or more.
4. The welded joint according to claim 3, characterized in that in the non-heat-affected zone, in a GDS measurement from the steel plate surface in the thickness direction, the maximum B emission intensity Bmax within a depth of 5 μm or less and the emission intensity B150 at a depth of 150 μm satisfy Bmax / B150≧8 ... (2).
5. A welded joint as described in claim 1 or 2, characterized in that the high ferrite layer has a thickness of 10 μm or more.
Citation Information
Patent Citations
Steel sheet, hot-dip zinc-coated steel sheet, and alloyed hot-dip zinc-coated steel sheet
WO2019116531A1
Steel sheet
WO2020218575A1
Method for manufacturing hot-dip zinc-coated high tensile strength steel sheet
JP2011231346A
High-strength hot-dip galvanized steel sheet with excellent surface quality and spot weldability, and its manufacturing method
JP2019504196A
Hot-dip galvanized steel plate with excellent coating adhesion and process for producing same
WO2014157155A1
Cited By
Steel plates and parts containing them
JP7897540B1
Steel plates and parts containing them
JP7897542B1