Cementitious material for three-dimensional modeling for construction and method for three-dimensional modeling for construction

A cementitious material with specific components ensures rapid construction of large objects with enhanced strength and reduced dust, addressing inefficiencies in existing technologies.

JP7564187B2Active Publication Date: 2024-10-08DENKA CO LTD +1
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2022500477
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-02-13
Filing Date
2021-02-12
Publication Date
2024-10-08
Estimated Expiration
2041-02-12

AI Technical Summary

Technical Problem

Existing cementitious materials for three-dimensional modeling in construction lack sufficient short-term and long-term strength development, leading to inefficiencies in construction speed and finish quality, with issues such as dust generation and poor curing speed.

Method used

A cementitious material comprising specific ratios of cement, aggregate, lignin sulfonic acid dispersant, melamine sulfonic acid dispersant, Diutan gum, amorphous calcium aluminosilicate, gypsum, and short fibers, along with a setting retarder, to ensure fluidity, thixotropy, and rapid strength development.

Benefits of technology

The material enables rapid construction of large-sized shaped objects with excellent self-supporting properties and strength development, reducing dust generation and improving construction speed.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564187000009
    Figure 0007564187000009
  • Figure 0007564187000010
    Figure 0007564187000010
  • Figure 0007564187000011
    Figure 0007564187000011
Patent Text Reader

Abstract

The present invention employs a cementitious material for three-dimensional modeling for construction, said cementitious material containing: (A) cement; (B) aggregate; (C) a dispersant wherein the mass ratio of a lignin sulfonic acid-based dispersant (R) to a melamine sulfonic acid-based dispersant (M), namely R:M is 100:80-400; (D) a diutan gum which has an average molecular weight within the range of from 2,000,000 to 8,000,000, and 0.25% by mass aqueous solution of which has a viscosity of from 2,000 to 10,000 mPa·s; (E) a setting retarder; (F) an amorphous calcium aluminosilicate which contains from 10 to 25% by mass of SiO2 in terms of oxide; (G) gypsum; and (H) short fibers. The present invention is able to provide: a cementitious material for three-dimensional modeling for construction, said cementitious material enabling the achievement of excellent self-standing properties and excellent strength developability; and a three-dimensional modeling method for construction.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cementitious material for three-dimensional modeling for construction, which is mainly used in the fields of civil engineering, architecture, and factory products, and a method for three-dimensional modeling for construction using the same. [Background technology]

[0002] In recent years, three-dimensional modeling technology has been used in the manufacturing industry to create models and parts. The technologies can be classified into three categories: photolithography (a method of curing and laminating UV-curable resin one layer at a time), inkjet printing (a method of laminating by irradiating UV rays while spraying UV-curable resin from a printer head), powdered gypsum modeling (a method of spraying resin or glue from a printer head and solidifying powdered gypsum), powder sintering (a method of laminating by baking resin or metal powder with a laser), and fused deposition modeling (a method of laminating by ejecting thermoplastic resin melted by heat from a thin nozzle). The objects are mainly made of resin, gypsum, and metal, and the technology of creating large objects such as construction materials using cementitious materials has been studied more overseas than in Japan. In Europe, the United States, and China, automatic construction machines are already being used to manufacture large objects at the level of detached houses.

[0003] For example, as a three-dimensional modeling technique using cementitious materials, Patent Document 1 discloses a technique in which three-dimensional data created by a computer is cut at a predetermined thickness to create two-dimensional slice data, and mortar mixed with an accelerator is sprayed onto a bed (table) while controlling the movement of a spray nozzle in the vertical and horizontal directions based on the two-dimensional slice data, and the sprayed mortar is allowed to harden independently to form a solidified layer of a shape based on the two-dimensional slice data, and the solidified layer formation work is repeated to sequentially stack in the vertical direction to form a shape. Patent Document 2 describes a material for making a mold for producing castings using a 3D printer, and discloses a material made of cement, sand, and a water-soluble silicate as an accelerator. Patent Documents 3 and 4 disclose a method for producing prefabricated members using a 3D printer and a method for producing a concrete earthquake-resistant wall using a 3D printer. Patent Document 5 discloses a technique related to a nozzle that ejects a material for 3D printing. Patent Document 6 discloses a method for producing a cementitious hardened body, characterized in that the cementitious hardened body is molded and produced using a resin formwork produced using a three-dimensional modeling system.

[0004] On the other hand, as a cementitious material, a material using a lignin sulfonate-based dispersant and a melamine sulfonate-based dispersant in combination is already known as a grout composition or a high-strength concrete composition (Patent Documents 7 and 8). Also, a PC grout material is known as a material using a dispersant and a thickener in combination (Patent Document 9). Furthermore, as a material containing calcium aluminate containing SiO2, a cement admixture characterized by having 300 parts by weight or less of gypsum and 0.1 to 20 parts by weight of a setting regulator per 100 parts by weight of calcium aluminosilicate glass, and a cement composition in which the cement admixture is mixed with the cement (Patent Document 10), as well as a cement composition containing calcium aluminosilicate with a CaO / Al2O3 molar ratio of 2.0 to 3.5 and a SiO2 content of 10 to 25%, and one or more selected from latent hydraulic substances and pozzolanic substances (Patent Document 11), etc. are known.

[0005] Furthermore, a cementitious material for three-dimensional modeling for construction is known that contains cement, aggregate, a dispersant in which the mass ratio of a lignin sulfonate-based dispersant to a melamine sulfonate-based dispersant is R:M=100:80-400, a thickener, a setting retarder, amorphous calcium aluminosilicate containing 10-25% SiO2 in oxide equivalent, gypsum, and short fibers (Patent Document 12). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 10-235623 [Patent Document 2] U.S. Patent No. 8,211,226 [Patent Document 3] China Patent Publication No. 104308988 [Patent Document 4] China Patent Publication No. 104153493 [Patent Document 5] US Patent Application Publication No. 2014 / 0308381 [Patent Document 6] JP 2016-101737 A [Patent Document 7] JP 2008-247677 A [Patent Document 8] Special Publication No. 62-10949 [Patent Document 9] JP 2006-290694 A [Patent Document 10] Japanese Patent Application Publication No. 4-97932 [Patent Document 11] JP 2006-232603 A [Patent Document 12] JP 2018-140906 A Summary of the Invention [Problem to be solved by the invention]

[0007] Patent Document 1 is a technology in which dry mix mortar, which is a premix of cement and fine aggregate, and water containing an accelerator are sprayed while being mixed and stirred with a spray nozzle to harden the mortar by itself, and therefore there is a demand for further improving the finish of the shaped object and further reducing dust generation. Patent Document 2 uses a water-soluble silicate as an accelerator, which causes a problem that the hardening speed is slow and the strength expression may be poor. Patent Documents 3 and 4 relate to a technology for manufacturing components with a 3D printer, and there is no mention of the use of a specific material. Patent Document 5 relates to the shape of the nozzle of a 3D printer, and there is no mention of the use of a specific material. Patent Document 6 relates to a technology for manufacturing a cementitious hardened body by molding a resin mold with a 3D printer and filling the mold with a cementitious material, and there is a problem that the molded cementitious hardened body cannot be efficiently manufactured because the mold needs to be made. Although various cementitious materials are known, such as those described in Patent Documents 7 to 11, no cementitious material capable of solving the above problems is known. Furthermore, Patent Document 12 describes a cementitious material for three-dimensional modeling for construction, but does not describe short-term strength. The present invention can obtain a sufficient construction speed.

[0008] In view of the above problems, an object of the present invention is to provide a cementitious material for three-dimensional modeling for construction, which is excellent in self-supporting property and short-term and long-term strength development, and a method for three-dimensional modeling for construction. [Means for solving the problem]

[0009] As a result of various investigations conducted in order to solve the above problems, the present inventors have found that the above problems can be solved by using a cementitious material that combines aggregate, a dispersant containing a lignin sulfonate-based dispersant and a melamine sulfonate-based dispersant in a specific ratio, diutan gum having an average molecular weight in the range of 2 million to 8 million and a viscosity of a 0.25 mass% aqueous solution in the range of 2000 to 10000 mPa s, a setting retarder, amorphous calcium aluminosilicate containing SiO2 in a specific ratio, gypsum, and short fibers, and have thus completed the present invention. That is, the present invention provides (1) A cementitious material for three-dimensional modeling for construction, comprising: cement (A); aggregate (B); a dispersant (C) in which the mass ratio of a lignin sulfonate-based dispersant (R) to a melamine sulfonate-based dispersant (M) is R:M=100:80-400; diutan gum (D) having an average molecular weight in the range of 2 million to 8 million and a viscosity of a 0.25 mass% aqueous solution in the range of 2000 to 10000 mPa·s; a setting retarder (E); an amorphous calcium aluminosilicate (F) containing 10 to 25 mass% SiO2 in terms of oxide; gypsum (G); and short fibers (H); (2) The cementitious material for three-dimensional modeling for construction according to (1), wherein the amount of the dispersant (C) used is 0.2 to 3 parts by mass per 100 parts by mass of the cement (A). (3) The cementitious material for three-dimensional modeling for construction according to (1) or (2), wherein the amount of diutan gum (D) used is 0.03 to 1.0 part by mass per 100 parts by mass of cement (A). (4) The cementitious material for three-dimensional modeling for construction according to any one of (1) to (3), wherein the amount of the gypsum (G) used is 50 to 250 parts by mass per 100 parts by mass of the amorphous calcium aluminosilicate (F). (5) The cementitious material for three-dimensional modeling for construction according to any one of (1) to (4), wherein the total amount of the amorphous calcium aluminosilicate (F) and the gypsum (G) is 5 to 30 parts by mass relative to 100 parts by mass of the cement (A). (6) The cementitious material for three-dimensional modeling for construction according to any one of (1) to (5), wherein the aggregate (B) contains a balloon-type aggregate. (7) The cementitious material for three-dimensional modeling for construction according to any one of (1) to (6), wherein the setting retarder (E) contains an oxycarboxylic acid. (8) The cementitious material for three-dimensional modeling for construction according to any one of (1) to (7), wherein the short fibers (H) have an average fiber length of 5 to 15 mm. (9) The cementitious material for three-dimensional modeling for construction according to (8) above, wherein the short fibers (H) have an average fiber diameter of 100 to 250 μm and a number of fibers per 1 g of 5,000 or more. (10) A method for three-dimensional modeling for construction, comprising mixing any one of the cementitious materials for three-dimensional modeling for construction described above with water, pumping the resulting wet material with a pump, and stacking the wet material discharged from a nozzle while moving the nozzle to construct a modeled object; (11) A method for three-dimensional modeling for construction according to (10), wherein the pump is a rotary positive displacement uniaxial eccentric screw pump. Effect of the Invention

[0010] By using the cementitious material for three-dimensional modeling for construction and the method for three-dimensional modeling for construction of the present invention, it is possible to supply a constant amount of material and ensure a constant layering speed. In addition, since excellent self-supporting property and strength development are obtained, a large-sized model can be constructed in a short time. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a schematic diagram showing a 3D modeling experimental system. [Diagram 2] FIG. 2(a) is a schematic diagram of the spray nozzle as viewed from the side, and FIG. 2(b) is a schematic diagram of the spray nozzle as viewed from the discharge port side. [Diagram 3] FIG. 3 is a schematic diagram showing the cross-sectional shape of the three-dimensional object produced in Example 8. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] In the present invention, "three-dimensional modeling" refers to a technology for manufacturing molded bodies of any shape by directly layering a cross-sectional shape based on three-dimensional data without using dedicated tools such as molds. It is also called "additive modeling" or "rapid prototyping."

[0013] [Cementitious materials for three-dimensional modeling] The cementitious material for three-dimensional modeling of the present invention (hereinafter, may be simply referred to as "cementitious material") contains cement (A), aggregate (B), dispersant (C) in which the mass ratio of a lignin sulfonate-based dispersant (R) to a melamine sulfonate-based dispersant (M) is R:M=100:80-400, diutan gum (D) having an average molecular weight in the range of 2 million to 8 million and a viscosity of a 0.25 mass% aqueous solution in the range of 2000 to 20000 mPa s, a setting retarder (E), amorphous calcium aluminosilicate (F) containing 10 to 25 mass% SiO2 calculated as oxide, gypsum (G), and short fibers (H).

[0014] <Cement (A)> The cement (A) used in the present invention may be any of various Portland cements, such as ordinary, early strength, super early strength, low heat, and moderate heat, or any of various blended cements obtained by mixing these Portland cements with blast furnace slag, fly ash, or silica, or any of various blended cements having a Blaine specific surface area of ​​2000 cm 2 Examples include filler cements containing limestone powder or blast furnace slag powder with a specific surface area of ​​3000 cm2 or more, environmentally friendly cements (eco-cement) made from municipal waste incineration ash or sewage sludge incineration ash, and alumina cements used for refractory materials. One or more of these can be used. The Blaine specific surface area of ​​the cement is 3000 cm2. 2 / g or more is preferred.

[0015] <Aggregate (B)> The aggregate (B) used in the present invention is not particularly limited, and may be a commercially available aggregate derived from natural limestone, aggregate derived from siliceous material, or a heavy aggregate having a specific gravity of more than 3.0. In addition, for the purpose of improving self-supporting property, a part of the aggregate used may be a balloon-type aggregate. The balloon-type aggregate is generally called a lightweight aggregate, and examples thereof include fly ash balloons, shirasu balloons, and balloons obtained by firing and foaming obsidian in a kiln. The specific gravity of the lightweight aggregate is preferably 2.0 or less, more preferably 1.8 or less, and even more preferably 0.3 to 1.0. The maximum particle size of the aggregate (B) (including balloon-type aggregate) is preferably 10 mm or less, more preferably 5 mm or less, in consideration of pumpability. The amount of aggregate (B) used is preferably 50 to 300 parts by mass, more preferably 100 to 200 parts by mass, per 100 parts by mass of cement (A). If the amount used is too small, it tends to be difficult to ensure self-supporting properties, and if the amount used is too large, it becomes difficult to ensure appropriate softness, which may impair pumpability. When using a balloon-type aggregate, the amount of the aggregate (B) is preferably 25 parts by mass or less, more preferably 1 to 25 parts by mass, and even more preferably 3 to 15 parts by mass, per 100 parts by mass of the aggregate (B). If the amount is too large, the strength expression may decrease, or it may become difficult to ensure a suitable softness, which may cause a problem in pumpability. On the other hand, if the amount is too small, the effect of improving the self-supporting property may not be observed.

[0016] <Dispersant (C)> In the present invention, the dispersant (C) is a dispersant consisting of a lignin sulfonate-based dispersant (R) and a melamine sulfonate-based dispersant (M), and the lignin sulfonate-based dispersant (R) and the melamine sulfonate-based dispersant (M) are used in combination at a mass ratio of R:M=100:80-400. By using such a dispersant (C), the fluidity of the cementitious material kneaded with water can be ensured and the thixotropy can be improved. The ratio is more preferably R:M=100:100-250. If the blending ratio of the melamine sulfonate-based dispersant (M) is less than the lower limit, the amount of dispersant required to obtain the desired fluidity will increase, and the fluidity will change too much over time, which may hinder pumping. If the blending ratio of the melamine sulfonate-based dispersant (M) is more than the upper limit, setting will be delayed and the fluidity will change little over time, making it difficult to ensure self-supporting properties after pumping. The amount of the dispersant (C) used is preferably 0.2 to 3 parts by mass, more preferably 0.5 to 2 parts by mass, per 100 parts by mass of the cement (A). If the amount used is too small, it may be difficult to obtain sufficient fluidity, and if the amount used is too large, setting may be delayed, the change in fluidity over time may be small, and self-supporting properties may be lost.

[0017] <Diutan gum (D)> In the present invention, diutan gum (D) having an average molecular weight in the range of 2 million to 8 million and a viscosity of a 0.25% by mass aqueous solution in the range of 2000 to 10000 mPa s can be used. Here, the viscosity of a 0.25% by mass aqueous solution is a value measured at 25°C using a B-type viscometer at 3 rpm. Diutan gum is a natural polymeric polysaccharide whose constituent units are, for example, two glucose units, one glucuronic acid unit, and three rhamnose units. The average molecular weight is preferably a weight average molecular weight (hereinafter, the weight average molecular weight may be referred to as molecular weight). The weight average molecular weight is, for example, a value calculated in terms of standard polyethylene oxide measured by gel permeation chromatography (GPC) or size exclusion chromatography. Specifically, the weight average molecular weight can be determined by creating a calibration curve of a commercially available standard polyethylene oxide using a GPC system (SC-8010 manufactured by Tosoh Corporation) under the following conditions, using water as a solvent. Flow rate: 4.0ml / min Set temperature: 40℃ Column configuration: A Tosoh Corporation "TSKgel G5000PWXL" and a Tosoh Corporation "TSKgel G3000PWXL (Tosoh Corporation)" were connected in series in this order. Sample injection volume: 100 μl (sample concentration 1 mg / ml) Detector: RI detector The amount of diutan gum (D) used is preferably 0.03 to 1.0 part by mass, more preferably 0.05 to 0.5 part by mass, per 100 parts by mass of cement (A). If the amount used is too small, it may be difficult to impart sufficient thixotropy, whereas if the amount used is too large, pumpability and strength development may be impaired.

[0018] <Set retarder (E)> The retarder (E) used in the present invention may be any of those generally available commercially for cementitious materials. Examples of such retarders include inorganic retarders such as phosphates, silicofluorides, copper hydroxide, boric acid or its salts, zinc oxide, zinc chloride, and zinc carbonate, and one or more of these may be used in combination. In addition, examples of such retarders include organic retarders such as oxycarboxylic acids (citric acid, gluconic acid, malic acid, tartaric acid, glucoheptonic acid, oxymalonic acid, lactic acid, etc.) or their salts (hereinafter, oxycarboxylic acids and their salts may be collectively referred to as oxycarboxylic acids), and sugars, typified by sugar, and one or more of these may be used in combination. Furthermore, mixtures of inorganic compounds such as carbonates, bicarbonates, nitrates, hydroxides, and silicates with the above-mentioned oxycarboxylic acids or their salts may also be used. Among these, those containing oxycarboxylic acids are preferred, and one or more selected from the group consisting of oxycarboxylic acids alone or mixtures of oxycarboxylic acids and inorganic compounds are more preferred. The amount of the set retarder (E) used is preferably 0.05 to 0.7 parts by mass, more preferably 0.07 to 0.5 parts by mass, per 100 parts by mass of cement. If the amount used is too small, it may be difficult to ensure the pot life taking into account the mixing time and pumping time, and if the amount used is too large, the hardening time may be long and self-supporting properties may not be ensured.

[0019] <Amorphous calcium aluminosilicate (F)> The amorphous calcium aluminosilicate (F) containing 10-25 mass% of SiO2 in terms of oxide used in the present invention (hereinafter simply referred to as "calcium aluminosilicate") is a calcium aluminosilicate obtained by subjecting a mixture of CaO raw materials, Al2O3 raw materials, and SiO2 raw materials to a heat treatment such as firing in a kiln or melting in an electric furnace, etc., and is an amorphous calcium aluminosilicate with a SiO2 content of 10-25 mass%. Because it is amorphous, it has high reactivity. Here, from the viewpoint of reactivity, the term "amorphous" preferably refers to a vitrification rate of 70% or more, and more preferably refers to a vitrification rate of 90% or more. The vitrification rate is determined by measuring the main peak area S of the crystalline mineral by powder X-ray diffraction method beforehand for a sample before heating, heating at 1000°C for 2 hours, and then slowly cooling at a cooling rate of 1 to 10°C / min, and determining the main peak area S0 of the crystalline mineral after heating by powder X-ray diffraction method, and further using these S0 and S values ​​and the following formula to calculate the vitrification rate χ. Vitrification rate χ(%)=100×(1-S / S0) If the SiO2 content is less than 10% by mass, the hydration activity will be high, and the amount of set retarder required to adjust the hardening time will increase, which may affect thixotropy and self-supporting properties. If the SiO2 content exceeds 25% by mass, the hydration activity will be low, and it may not be possible to obtain an adequate hardening speed. The calcium aluminosilicate (F) preferably has a molar ratio of CaO to Al2O3 calculated as oxide, CaO / Al2O3, of 1.5 to 3.5, more preferably 1.7 to 2.0. As other components, alkali metals such as sodium, potassium, and lithium may be partially dissolved. The particle size of calcium aluminosilicate is 3000 cm in Blaine value. 2 If the Blaine value is too small, the strength development may decrease.

[0020] <Gypsum (G)> The gypsum (G) used in the present invention is a component that further improves strength when used in combination with the calcium aluminosilicate. Types of gypsum (G) include anhydrous gypsum, hemihydrate gypsum, and dihydrate gypsum, and gypsum produced as a by-product in factories or naturally occurring gypsum can be used. Among these, the use of anhydrous gypsum is preferred in terms of strength development. The grain size of gypsum (G) is 3000 cm in Blaine value. 2 If the Blaine value is too small, the effect of improving strength development may not be obtained. The ratio of gypsum (G) to the calcium aluminosilicate (F) is preferably 50 to 250 parts by mass, more preferably 100 to 200 parts by mass, per 100 parts by mass of the calcium aluminosilicate (F). If the ratio of gypsum (G) is too low, the effect of improving strength may not be obtained, and if the ratio of gypsum (G) is too high, the strength development may reach a plateau.

[0021] The total amount of the calcium aluminosilicate (F) and the gypsum (G) used is preferably 5 to 30 parts by mass, more preferably 10 to 20 parts by mass, per 100 parts by mass of the cement (A). If the amount used is too small, the strength enhancing effect may not be obtained, whereas if the amount used is too large, it may be difficult to ensure the pot life or the strength development may decrease.

[0022] <Short Fiber (H)> The short fibers (H) used in the present invention can be any commercially available short fibers for cement mixing. Examples include vinylon fibers, acrylic fibers, nylon fibers, steel fibers, glass fibers, polypropylene fibers, polyethylene fibers, polyester fibers, and basalt fibers, and it is also possible to use one or more of these fibers in combination. Among these, it is preferable to use one or more types selected from the group consisting of vinylon fibers, which have a wide variety of fiber diameters and lengths, and nylon fibers, which have excellent dispersibility. Considering that the short fibers (H) are premixed in advance, the average fiber length is preferably in the range of 5 to 15 mm. The average fiber diameter of the short fibers (H) is preferably 20 to 250 μm, more preferably 100 to 250 μm, from the viewpoint of three-dimensional modeling. Fibers with too small an average diameter may be difficult to obtain. On the other hand, fibers with too large an average fiber diameter may interfere with the pumpability of the wet material, and even if the wet material can be pumped, the temperature rise of the wet material due to pumping may be too large, and the hardening time may be excessively short, which may deteriorate the moldability or reduce the strength expression of the molded body. By making the average fiber diameter of the short fibers (H) 20 μm or more, particularly 100 μm or more, the frictional heat generated when pumping the wet material obtained by adding water to the cementitious material increases, and the temperature of the wet material discharged from the nozzle tip increases, thereby appropriately shortening the hardening time, thereby achieving a continuous higher layering. As the short fibers (H), those in the form of bundled fibers in which monofilaments are bundled together with a binder are preferred over those in the form of monofilaments, since a larger number of fibers can be mixed in. The number of short fibers (H) per 1 g is preferably 5,000 or more. If the number of fibers per 1 g is too small, the reinforcing effect and initial crack suppression effect of the short fibers (H) may not be exhibited. The number of short fibers (H) per 1 g is preferably 500,000 or less. The number of fibers per 1 g of short fibers (H) is calculated from the fineness (dtex, mass (g) per 10,000 m of monofilament) using the following formula. Number of fibers (pieces / g) = [1 / (fineness / 10,000(m))] / average fiber length (m / piece) The amount of the short fibers (H) used is preferably 0.1 to 1.0 part by mass, and more preferably 0.2 to 0.5 part by mass, per 100 parts by mass of the total of the cement (A) and aggregate (B). If the amount used is too small, the reinforcing effect may not be exhibited, and if the amount used is too large, pumping may be hindered.

[0023] <Other ingredients> In the present invention, it is possible to add various additives such as antifoaming agents, anti-rust agents, antifreeze agents, shrinkage reducing agents, inorganic minerals such as bentonite and sepiolite, anion exchangers such as hydrotalcite, polymer emulsions, etc., within the scope of not interfering with application and the performance of the hardened body. It is also possible to use inorganic powders with hydration activity such as blast furnace slag, silica fume, and fly ash, apart from those premixed with the cement.

[0024] <Water usage> The cementitious material of the present invention is mixed with water to prepare a wet material, which is then used for three-dimensional modeling. The amount of water used is preferably 13 to 20 parts by mass, more preferably 15 to 18 parts by mass, per 100 parts by mass of the cementitious material. If the amount used is too small, mixing may be difficult, and if the amount used is too large, the fluidity of the wet material may increase, decreasing its self-supporting ability.

[0025] [3D modeling method] The 3D modeling method of the present invention will be described below using the 3D modeling experimental system 1 shown in Fig. 1 as an example. Note that the 3D modeling experimental system 1 shown in Fig. 1 does not limit the 3D modeling method of the present invention. The 3D modeling method of the present invention can be classified into a mixing process of the cementitious material, a pumping process of the wet material obtained by mixing, and a 3D modeling process by controlled nozzle movement.

[0026] The method of mixing the cementitious material employed in the three-dimensional modeling method of the present invention is not particularly limited, and the material can be mixed using a commercially available mixer 10. Examples of the mixer include a pan-type mixer, a forced twin-shaft mixer, and a continuous mixing mixer pump that combines mixing and pressure pumping (a rotary positive displacement uniaxial eccentric screw pump).

[0027] The pump 20 for pumping the mixed wet material employed in the three-dimensional modeling method of the present invention is not particularly limited as long as it can pump the wet material without deteriorating its quality, but a rotary positive displacement uniaxial eccentric screw pump 20 is preferred. The rotary positive displacement uniaxial eccentric screw pump 20 is also called a mono pump or a snake pump, and compared to a squeeze pump, it is capable of pumping a fixed amount without pulsation during pumping, and the discharge amount can be adjusted by controlling the motor rotation speed. In addition, the rotary positive displacement uniaxial eccentric screw pump 20 is also preferred in that, due to its structure, it is considered that the temperature of the wet material being pumped is easily increased, and the hardening reaction of the wet material proceeds in a short time, improving the self-supporting stability and allowing the continuous stacking height to be increased. That is, the rotary volume type uniaxial eccentric screw pump 20 is equipped with a rotor corresponding to a male screw and a stator corresponding to a female screw. When the rotor is inserted into the stator, a sealed space called a cavity (for example, a space between the rotor and the stator) is formed in the gap, and the rotor rotates in the stator, generating a strong suction force, and the cavity moves to the discharge side, thereby continuously transferring the material. During transfer, for example, the rotor performs an eccentric rotation motion in which it rotates while revolving around the central axis of the stator. Then, when the material in the first cavity moves to the previous (discharge side) cavity by suction force, it is considered that it is heated by the frictional resistance with the stator surface. By utilizing such a heating phenomenon, it is possible to realize a three-dimensional modeling with excellent self-supporting stability while ensuring a pot life. For example, the rotary volume type uniaxial eccentric screw pump 20 is exemplified in paragraphs 0063 to 0064 of International Publication No. 2014 / 142239. The pressure-feeding pipe 30 can be a flexible hose with a pressure resistance of 2 to 4 MPa or a combination of metal pipes. The pipe diameter is preferably 20 to 50 mm in inner diameter, depending on the discharge rate. The length of the pressure-feeding pipe 30 is not particularly limited, but is preferably 20 m or less in consideration of pumpability.

[0028] A spray nozzle 40 is preferably provided at the discharge portion (the tip of the pressure-transfer pipe) of the wet material employed in the three-dimensional modeling method of the present invention. The diameter of the discharge port 41 (see FIG. 2) is not particularly limited, but may be appropriately set depending on the aggregate diameter used and the stacking width. For example, if the aggregate diameter is 5 mm or less and the stacking width is 50 mm or less, the inner diameter of the discharge port 41 is preferably 5 to 20 mm, more preferably 8 to 15 mm. The shape of the discharge port 41 is not particularly limited, but examples include a circle, an ellipse, a rectangle, a cross, and a star, and a brim may be provided around the discharge port for the purpose of providing smoothness to the surface of the discharged wet material. In these cases, the discharge port 41 is provided perpendicular to the bed 50, but in some cases, the discharge port 41 may be provided horizontally.

[0029] In the three-dimensional modeling method of the present invention, the control of the nozzle movement in the horizontal and vertical directions is preferably performed by fixing the spray nozzle 40 to a robot arm 60 or a gate-type plotter and controlling it by a computer. For example, a method is possible in which the three-dimensional data created by a computer is cut at a predetermined thickness to create two-dimensional slice data, and the spray nozzle 40 is moved in the horizontal direction, such as vertically, horizontally, or diagonally, based on the two-dimensional slice data while discharging the wet material from the spray nozzle 40 onto the bed 50, and the nozzle is moved in the vertical direction repeatedly to sequentially stack the wet material to form a three-dimensional modeled object (for example, a three-dimensional modeled object having a cross-sectional shape 70 shown in FIG. 3). When the spray nozzle 40 is fixed to the robot arm 60 or a gate-type plotter, a pulley 80 is preferably used to prevent the pressure feed pipe 30 from bending and becoming clogged. The moving speed of the spray nozzle 40 is not particularly limited and can be changed depending on the width of the wet material to be laminated. When the amount of wet material discharged is constant, a slower speed increases the width of the wet material to be laminated, and a faster speed decreases the width of the wet material to be laminated. EXAMPLES

[0030] The present invention will now be described in further detail with reference to examples. <Example 1> For 100 parts by mass of cement, 150 parts by mass of aggregate, 1.0 part by mass of dispersant with a mass ratio of lignin sulfonic acid dispersant (R) and melamine sulfonic acid dispersant (M) of R / M=100 / 200, diutan gum of the type and amount shown in Table 1, 0.25 parts by mass of retarder A, and 20 parts by mass of a mixture of 150 parts by mass of gypsum for 100 parts by mass of calcium aluminosilicate shown in Table 1 were mixed, and 0.2 parts by mass of short fiber A was mixed for a total of 100 parts by mass of cement and aggregate to prepare a cementitious material for three-dimensional modeling (hereinafter sometimes referred to as cementitious material). 17 parts by mass of water was added to 100 parts by mass of this prepared material, and the mixture was mixed with a pan-type mixer. The mini-slump (MS, immediately after mixing and 20 minutes after mixing), hardening time, and compressive strength of the obtained wet material were measured, and the MS reduction rate was calculated. The results are shown in Table 1.

[0031] (Materials used) <Cement (A)> Cement: Ordinary Portland cement (manufactured by Denka Co., Ltd., Blaine specific surface area 3400 cm 2 / g) <Aggregate (B)> Aggregate: Limestone aggregate (manufactured by Denka Co., Ltd., maximum particle size 1.2 mm, specific gravity 2.71) <Dispersant (C)> Lignin sulfonic acid dispersant (R): Nippon Paper Industries Co., Ltd., product name "Sanex P252" Melamine sulfonic acid dispersant (M): Made by Sika Japan Co., Ltd., product name "Sikament FF86 / 100" <Diutan gum (D)> Diutan gum A: Synthesized by aerobic fermentation of glucose using Alcaligenes microorganisms. Molecular weight: 4.1 million, viscosity of 0.25% by weight aqueous solution: 5600 mPa s Diutan gum B: Synthesized in the same way as diutan gum A, except for the fermentation time. Molecular weight: 2.2 million, viscosity of 0.25% by weight aqueous solution: 2300 mPa s Diutan gum C: Synthesized in the same way as diutan gum A, except for the fermentation time. Molecular weight: 5.3 million, viscosity of 0.25% by weight aqueous solution: 7500 mPa s Diutan gum D: Synthesized in the same way as diutan gum A, except for the fermentation time. Molecular weight 7.8 million, viscosity of 0.25% by weight aqueous solution 9600 mPa s Diutan gum E: Synthesized in the same way as diutan gum A, except for the fermentation time. Molecular weight 1.8 million, viscosity of 0.25% by weight aqueous solution 1800 mPa s <Thickening agents other than diutan gum> Thickener A: Cellulose ether type (manufactured by Shin-Etsu Chemical Co., Ltd., product name "hi90SH-30000" (viscosity of 2% by weight aqueous solution at 20°C is 30,000 mP·s)) <Set retarder (E)> Set retarder A: Citric acid (reagent grade 1) <Amorphous calcium aluminosilicate (F)> Calcium aluminosilicate A: Commercially available special grade reagents SiO, CaCO, and AlO were mixed in a specified ratio, heated and melted at approximately 2000°C using a high-frequency furnace, quenched in water, and pulverized to prepare a material (amorphous (in the following examples, amorphous refers to a glassification rate of 90% or more), SiO content 10.1%, CaO / AlO molar ratio 1.85, Blaine specific surface area 5900 cm). 2 / g) Calcium aluminosilicate B: Prepared in the same manner as calcium silicate A except for changing the mixing ratio of the reagents (amorphous, SiO2 content 14.9%, CaO / Al2O3 molar ratio 1.85, Blaine specific surface area 5800 cm 2 / g) Calcium aluminosilicate C: Prepared in the same manner as calcium silicate A except for changing the mixing ratio of the reagents (amorphous, SiO2 content 24.6%, CaO / Al2O3 molar ratio 1.85, Blaine specific surface area 5800 cm 2 / g) <Gypsum (G)> Gypsum: Natural anhydrous gypsum crushed product (Blaine specific surface area 5200 cm 2 / g) <Short Fiber (H)> Short fiber a: Vinylon fiber (average fiber length 12 mm, average fiber diameter 50 μm, number of fibers per 1 g 55,500)

[0032] (Test Method) All tests were carried out in an environment of 20°C. (1) Blaine specific surface area Measurements were performed in accordance with JIS R 5201-1997. (2) Maximum particle size The aggregate was sieved in accordance with JIS A 1102, and the size of the largest sieve opening that did not pass completely was taken as the maximum particle size. (3) Mini Slump (MS) It was based on JIS A 1171. Measurements were taken immediately after mixing and after 20 minutes. (4) MS reduction rate The mini-slump was calculated using the following formula from the mini-slump immediately after mixing and 20 minutes later. Slump reduction rate (%) = [Mini slump (immediately after mixing) - Mini slump (after 20 minutes)] / [Mini slump (immediately after mixing) x 100] (5)Curing time After mixing was completed, 2 kg of the wet material was packed into a plastic bag, and the time when it no longer dented when pressed with a finger was recorded as the hardening time. The finger pressing was performed at 5-minute intervals. (6) Compressive strength The mixed material was filled into a 4 x 4 x 16 cm triple formwork conforming to JIS R 5201, and measurements were taken at ages of 3 hours, 12 hours, 1 day, and 7 days. (7) Specific gravity of limestone aggregate Measured in accordance with JIS A 1109, and the bone dry density was taken as the specific gravity.

[0033] [Table 1]

[0034] As can be seen from Table 1, within the composition range of the diutan gum of the present invention, pumpability was not impaired and self-supporting properties were ensured after pumping. Furthermore, excellent values ​​were shown for both initial and long-term strength, allowing for excellent lamination and application speeds. On the other hand, when diutan gum or other thickeners outside the range of the present invention were used, although there were cases where an MS reduction rate sufficient to ensure self-supporting properties was shown, initial strength expression was poor and sufficient lamination and application speeds were not achieved.

[0035] <Example 2> A mixture of 150 parts by mass of aggregate, 0.1 parts by mass of diutan gum A, 0.25 parts by mass of retarder A, and 150 parts by mass of gypsum mixed with 100 parts by mass of calcium aluminosilicate B was mixed with 20 parts by mass per 100 parts by mass of cement, and 0.2 parts by mass of short fiber A was mixed with 100 parts by mass of cement and aggregate in total to prepare a cementitious material for three-dimensional modeling (hereinafter, sometimes referred to as cementitious material). 17 parts by mass of water was added to 100 parts by mass of this prepared material, and the mixture was mixed with a pan-type mixer. The mini-slump (MS, immediately after mixing and 20 minutes after mixing), hardening time, and compressive strength of the obtained wet material were measured, and the MS reduction rate was calculated. The results are shown in Table 2.

[0036] [Table 2]

[0037] As shown in Table 2, the combined use of the lignin sulfonate-based dispersant (R) and the melamine sulfonate-based dispersant (M) within the scope of the present invention did not impair pumpability and achieved a moderate slump reduction rate, ensuring self-support after pumping.

[0038] <Example 3> For 100 parts by mass of cement, 150 parts by mass of aggregate, 1.0 part by mass of dispersant with a mass ratio of lignin sulfonic acid dispersant (R) and melamine sulfonic acid dispersant (M) of R / M=100 / 200, 0.1 part by mass of diutan gum A, 0.25 part by mass of retarder A, and 20 parts by mass of a mixture with a ratio of calcium aluminosilicate B and gypsum shown in Table 3 were mixed, and 0.2 parts by mass of short fiber a was mixed with 100 parts by mass of cement and aggregate, to prepare a cementitious material for three-dimensional modeling. 17 parts by mass of water was added to 100 parts by mass of this prepared material, and the mixture was mixed with a pan-type mixer. The obtained wet material was measured for mini-slump (immediately after mixing and 20 minutes after mixing), hardening time, and compressive strength in the same manner as in Example 1, and the MS reduction rate was calculated. The results are shown in Table 3.

[0039] [Table 3]

[0040] It was found that by using 50 to 250 parts by mass of gypsum per 100 parts by mass of calcium aluminosilicate, an appropriate mini-slump reduction rate and hardening time for ensuring self-supporting properties can be obtained.

[0041] <Example 4> A mixture consisting of 150 parts by mass of aggregate, 1.0 part by mass of dispersant with a mass ratio of lignin sulfonic acid dispersant (R) and melamine sulfonic acid dispersant (M) of R / M=100 / 200, 0.1 part by mass of diutan gum A, 0.25 part by mass of retarder A, and 150 parts by mass of gypsum per 100 parts by mass of calcium aluminosilicate B was mixed in the amounts shown in Table 4, and 0.2 parts by mass of short fiber A was mixed with 100 parts by mass of cement and aggregate in total to prepare a cementitious material for three-dimensional modeling. 17 parts by mass of water was added to 100 parts by mass of this prepared material, and the mixture was mixed with a pan-type mixer. The obtained wet material was measured for mini-slump (immediately after mixing and 20 minutes after mixing), hardening time, and compressive strength in the same manner as in Example 1, and the MS reduction rate was calculated. The results are shown in Table 4.

[0042] [Table 4]

[0043] It was found that by using a combined amount of calcium aluminosilicate and gypsum of 5 to 30 parts by mass per 100 parts by mass of cement, an appropriate mini-slump reduction rate and hardening time for ensuring self-supporting properties can be obtained.

[0044] <Example 5> For 100 parts by mass of cement, 1.0 part by mass of aggregate and balloon aggregate shown in Table 5, 1.0 part by mass of dispersant with a mass ratio of lignin sulfonic acid dispersant (R) and melamine sulfonic acid dispersant (M) of R / M=100 / 200, 0.1 part by mass of diutan gum A, 0.25 part by mass of retarder A, and 20 parts by mass of a mixture consisting of 150 parts by mass of gypsum and 100 parts by mass of calcium aluminosilicate B were mixed, and 0.2 parts by mass of short fiber a was mixed with 100 parts by mass of cement and aggregate, to prepare a cementitious material for three-dimensional modeling. 17 parts by mass of water was added to 100 parts by mass of this prepared material, and the mixture was mixed with a pan-type mixer. For the obtained wet material, the mini-slump (immediately after mixing and 20 minutes after mixing), hardening time, and compressive strength were measured in the same manner as in Example 1, and the MS reduction rate was calculated. The results are shown in Table 5.

[0045] (Materials used) <Aggregate B> Aggregate: Limestone aggregate (manufactured by Denka Co., Ltd., maximum particle size 1.2 mm, specific gravity 2.71) Balloon aggregate: Tomoe Engineering Co., Ltd., product name "Senolite SA" (a granular product of fly ash balloons generated at thermal power plants, made in China, specific gravity 0.88, maximum particle size 150μm or less) (Materials used) (7) Specific gravity of balloon aggregate Measured according to JIS A 1134, and the bone dry density was used as the specific gravity.

[0046] [Table 5]

[0047] It was found that by using 50 to 300 parts by mass of aggregate per 100 parts by mass of cement, an appropriate mini-slump reduction rate and hardening time for ensuring self-supporting properties can be obtained. It was also found that the use of balloon-type aggregate increases the MS reduction rate and improves self-supporting properties.

[0048] <Example 6> For 100 parts by mass of cement, 150 parts by mass of aggregate, 1.0 part by mass of dispersant with a mass ratio of lignin sulfonic acid dispersant (R) and melamine sulfonic acid dispersant (M) of R / M=100 / 200, 0.1 part by mass of diutan gum A, retarders of the type and amount shown in Table 6, and 20 parts by mass of a mixture consisting of 150 parts by mass of gypsum and 100 parts by mass of calcium aluminosilicate B were mixed, and 0.2 parts by mass of short fiber a was mixed with 100 parts by mass of cement and aggregate to prepare a cementitious material for three-dimensional modeling. 17 parts by mass of water was added to 100 parts by mass of this prepared material, and the mixture was mixed with a pan-type mixer. For the obtained wet material, the mini-slump (immediately after mixing and 20 minutes after mixing), hardening time, and compressive strength were measured in the same manner as in Example 1, and the MS reduction rate was calculated. The results are shown in Table 6.

[0049] (Materials used) <Set retarder (E)> Set retarder A: Citric acid (reagent grade 1) Coagulation retarder B: Gluconic acid (reagent grade 1) Coagulation retarder C: Trisodium citrate (reagent grade 1)

[0050] [Table 6]

[0051] It was found that by using 0.05 to 0.7 parts by mass of a retarder containing hydroxycarboxylic acids per 100 parts by mass of cement, an appropriate reduction rate of mini-slump and hardening time for ensuring self-supporting properties can be obtained.

[0052] <Example 7> 100 parts by mass of cement, 150 parts by mass of aggregate, 1.0 part by mass of dispersant with a mass ratio of lignin sulfonic acid dispersant (R) and melamine sulfonic acid dispersant (M) of R / M=100 / 200, 0.1 parts by mass of diutan gum A, 0.25 parts by mass of retarder A, and 20 parts by mass of a mixture consisting of 150 parts by mass of gypsum and 100 parts by mass of calcium aluminosilicate B were mixed, and short fibers of the type and amount shown in Table 7 were mixed with 100 parts by mass of cement and aggregate to prepare a cementitious material for three-dimensional modeling. 17 parts by mass of water was added to 100 parts by mass of this prepared material, and the mixture was mixed with a pan-type mixer. The mini-slump (immediately after mixing and 20 minutes after mixing) and compressive strength of the obtained wet material were measured in the same manner as in Example 1, and the MS reduction rate was calculated. In addition, the initial crack width was measured by the following test method. The results are shown in Table 7.

[0053] (Materials used) <Short Fiber (H)> Short fiber a: Vinylon fiber (average fiber length 12 mm, average fiber diameter 50 μm, number of fibers per 1 g 55,500) Short fiber B: Nylon fiber (manufactured by Toray Amtex Co., Ltd., product name "Tough Binder" (average fiber length 10 mm, average fiber diameter 28 μm, number of fibers per 1 g 185,200)) Short fiber c: Nylon fiber (manufactured by Toray Amtex Co., Ltd., product name "Tough Binder" (average fiber length 5 mm, average fiber diameter 28 μm, number of fibers per 1 g 370,500)) Short fiber d: Vinylon fiber (manufactured by Kuraray Co., Ltd., product name "RECS100L" (average fiber length 12 mm, average fiber diameter 130 μm, number of fibers per 1 g 8,300))

[0054] (Test Method) Initial crack width: A formwork was set on a concrete slab (30 cm long x 30 cm wide x 6 cm thick), the wet material of the present invention was poured to a thickness of 2 cm, and the surface was finished with a trowel to prepare a test specimen. The test specimen was cured in an environment with a humidity of 60% by mass and a temperature of 5°C, and the crack width after 72 hours was measured. The crack width here refers to the width near the center of the length of any crack that occurred in the test specimen. If no cracks occurred after 72 hours, the width was recorded as 0.0 mm.

[0055] [Table 7]

[0056] It was found that by using 0.1 to 1.0 parts by mass of short fibers with an average fiber length of 5 to 15 mm per 100 parts by mass of cement and aggregate combined, an appropriate mini-slump reduction rate and hardening time can be obtained to ensure self-supporting properties, while also suppressing initial cracks.

[0057] <Example 8> A three-dimensional modeling experiment was actually carried out with the mixture of Experiment No. 1-22. The environmental temperature was 22°C. The system and conditions used are shown below. Also, a schematic diagram of the three-dimensional modeling experiment system is shown in FIG. 1, and a schematic diagram of the spray nozzle used is shown in FIG. 2. 30 kg of the cementitious material for three-dimensional modeling of Experiment No. 1-22 and 5.1 kg of water were added to the mixer 10 and mixed for 3 minutes to prepare a wet material. The obtained wet material was put into a rotary volumetric single-shaft eccentric screw pump 20 with a hopper, and the wet material was pumped through a flexible hose 30 and discharged from the discharge port 41 at the nozzle tip of the spray nozzle 40, thereby forming a three-dimensional model having a cross-sectional shape 70 shown in FIG. 3. That is, the three-dimensional model was formed by stacking the layers perpendicular to the cross-sectional shape 70. As a result, layers made of the cementitious material for three-dimensional modeling could be stacked in sequence, and a three-dimensional model with a vertical continuous stack height of 30 cm or more was obtained. In other words, continuous stacking up to a height of 30 cm or more was possible (see Figure 3).

[0058] <Example 9> Using the 3D modeling experimental system 1, 3D modeling experiments similar to those in Example 8 were carried out with the formulations of Experiments No. 1-9, No. 1-39, No. 7-17, and No. 7-18. The environmental temperature was 24°C. At that time, the temperature of the wet material immediately after kneading in the mixer, the temperature of the wet material pumped by the rotary volumetric uniaxial eccentric screw pump 20 and discharged from the discharge port 41 at the tip of the nozzle, the curing time, and the continuous stacking height were measured. The results are shown in Table 8.

[0059] (3D modeling experimental system) Mixer 10: Pan-type mixer (manufactured by Okasan Kiko Co., Ltd., product name "Damacut Mixer Type 2.8") Pump 20: Rotary positive displacement uniaxial eccentric screw pump (manufactured by PFT, product name "PFT BOLERO") Pressure hose 30: 4MPa pressure-resistant flexible hose (PFT, inner diameter 1 inch, pressure piping distance 10m) Spray nozzle 40: Homemade (see Figure 2), nozzle outlet diameter 18 mm (circular) Robot arm 60: A modified Yaskawa Electric robot arm (product name "MOTOMAN-MA2010") was used with a nozzle fixed to the tip of the arm.

[0060] (Modeling conditions) Cementitious material height per layer: 10mm Shape of the three-dimensional object: Truss shape (length 500 mm, width 1000 mm, layer width (thickness) approx. 30 mm) (see Figure 3) Wet material discharge volume: 0.25m 3 / hr, nozzle movement speed: 180mm / sec

[0061] (Test Method) Material temperature: measured with a digital thermometer Curing time: The material discharged from the nozzle tip was sampled and measured in the same manner as in Example 1. Continuous stacking height: Measure the height when stacking the model until it collapses.

[0062] [Table 8]

[0063] By using diutan gum within the range of the present invention, the early strength development was improved and the continuous stacking height was increased. On the other hand, when diutan gum outside the range of the present invention was used, the early strength development was poor, the laminated mortar could not withstand its own weight, and continuous stacking was not possible. [Industrial Applicability]

[0064] By using the cementitious material for three-dimensional modeling for construction and the method for three-dimensional modeling for construction of the present invention, a constant amount of material can be supplied, and a constant layering speed can be ensured. In addition, since excellent self-supporting properties and strength development (particularly initial strength development) can be obtained, a large shaped object can be constructed in a short time. Furthermore, the present invention is less likely to generate dust during molding. Therefore, the present invention can be suitably used for the manufacture of civil engineering and construction components. [Explanation of symbols]

[0065] 1. 3D modeling experiment system 10. Mixer 20 Pump (rotary positive displacement single-shaft eccentric screw pump) 30 Pressure pipe (flexible hose) 40 Spray nozzle 41 Discharge port 50 Beds 60 Robot Arm 70 Cross-sectional shape of a three-dimensional object 80 Pulley

Claims

1. Cement (A), aggregate (B), dispersant (C) in which the mass ratio of lignin sulfonate-based dispersant (R) to melamine sulfonate-based dispersant (M) is R:M=100:80-400, diutan gum (D) having an average molecular weight in the range of 2 million to 8 million and a viscosity of a 0.25 mass% aqueous solution in the range of 7500 to 10,000 mPa s, setting retarder (E), and SiO 2 A cementitious material for three-dimensional modeling for construction, comprising 10 to 25 mass% amorphous calcium aluminosilicate (F), gypsum (G), and short fibers (H).

2. 2. The cementitious material for three-dimensional modeling for construction according to claim 1, wherein the amount of the dispersant (C) used is 0.2 to 3 parts by mass per 100 parts by mass of the cement (A).

3. The cementitious material for three-dimensional modeling for construction according to claim 1 or 2, wherein the amount of diutan gum (D) used is 0.03 to 1.0 part by mass per 100 parts by mass of cement (A).

4. The cementitious material for three-dimensional modeling for construction according to any one of claims 1 to 3, wherein the amount of gypsum (G) used is 50 to 250 parts by mass relative to 100 parts by mass of the amorphous calcium aluminosilicate (F).

5. The total amount of the amorphous calcium aluminosilicate (F) and the gypsum (G) used is 5 to 30 parts by mass relative to 100 parts by mass of cement (A). The cementitious material for three-dimensional modeling for construction according to any one of claims 1 to 4.

6. The cementitious material for three-dimensional fabrication for construction according to any one of claims 1 to 5, wherein the aggregate (B) comprises a balloon-type aggregate.

7. The cementitious material for three-dimensional modeling for construction according to any one of claims 1 to 6, wherein the setting retarder (E) contains an oxycarboxylic acid.

8. The cementitious material for three-dimensional modeling for construction according to any one of claims 1 to 7, wherein the short fibers (H) have an average fiber length of 5 to 15 mm.

9. The cementitious material for three-dimensional modeling for construction according to claim 8, wherein the short fibers (H) have an average fiber diameter of 20 to 250 μm and a number of fibers per gram of 5,000 or more.

10. A method for three-dimensional modeling for construction, comprising mixing the cementitious material for three-dimensional modeling for construction according to any one of claims 1 to 9 with water, pumping the resulting wet material with a pump, and stacking the wet material discharged from a nozzle while moving the nozzle to construct a model.

11. The method for constructing a solid object according to claim 10, wherein the pump is a rotary positive displacement uniaxial eccentric screw pump.

Citation Information

Patent Citations

  • Concrete shear wall structure based on 3D printing and construction method of concrete shear wall structure

    CN104153493A

  • Method for producing precast concrete

    CN104308988A

  • Transmitting and receiving equipment

    JP1987010949A

  • Cement admixture and cement composition

    JP1992097932A

  • Solid forming method using cement-based material

    JP1998235623A