Spherical boron nitride particles, filler for resin, resin composition, and method for producing spherical boron nitride particles
Spherical boron nitride particles with controlled surface conditions, produced via cavitation treatment, address the fluidity issues in resin compositions, ensuring high fluidity and low thixotropy, enhancing processing efficiency.
Patent Information
- Application Number
- JP2023541292
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-02-16
- Filing Date
- 2023-02-14
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2043-02-14
AI Technical Summary
Existing resin compositions suffer from decreased fluidity when inorganic fillers like boron nitride particles are added, leading to processing difficulties.
The production of spherical boron nitride particles with specific surface conditions, including a B 1s/O 1s ratio of 90 or less, achieved through cavitation treatment, enhances their dispersibility and reduces agglomeration, resulting in improved fluidity of resin compositions.
The spherical boron nitride particles provide resin compositions with excellent fluidity and low thixotropy, maintaining high fluidity across varying shear rates, even without additional homogenizer treatment.
Smart Images

Figure 0007564374000001
Abstract
Description
[Technical field]
[0001] The present invention relates to spherical boron nitride particles, a filler for resin, a resin composition, and a method for producing spherical boron nitride particles. [Background technology]
[0002] Hexagonal boron nitride (hereinafter referred to as "boron nitride") has lubricating properties, high thermal conductivity, and insulating properties, and is widely used as a solid lubricant, a release agent for molten gas and aluminum, and a filler for heat dissipating materials. As boron nitride particles that take advantage of the lubricity and high thermal conductivity that are characteristic of boron nitride, Patent Document 1 describes submicron, scale-shaped, highly pure, highly crystalline, spherical boron nitride microparticles with a small diameter-to-thickness ratio (aspect ratio), while Patent Document 2 describes submicron spherical boron nitride microparticles with high sphericality.
[0003] [Patent Document 1] International Publication No. 2015 / 122378 [Patent Document 2] International Publication No. 2015 / 122379 Summary of the Invention
[0004] In general, when an inorganic filler is blended with a resin, the fluidity of the resin composition tends to decrease. The present inventors have conducted extensive research into boron nitride microparticles that can achieve excellent fluidity even when blended with a resin. As a result, they have surprisingly found that spherical boron nitride particles having a specific surface condition can provide a resin composition with excellent fluidity.
[0005] An object of the present invention is to provide spherical boron nitride particles capable of giving a resin composition with excellent fluidity, a resin filler and resin composition containing the spherical boron nitride particles, and a method for producing the spherical boron nitride particles.
[0006] The present invention has the following aspects. [1] O measured by X-ray photoelectron spectroscopy 1s Semi-quantitative value calculated from peak intensity and B 1s Semi-quantitative value B calculated from peak intensity 1s / O 1s A spherical boron nitride particle having a ratio of 90 or less. [2] The spherical boron nitride particles according to [1], in which a mixture of 15 volume percent spherical boron nitride particles filled in an epoxy resin has a thixotropy index (TI value) of 2 or less, expressed as the ratio (η1 / η2) of the viscosity η1 measured at a shear rate of 1 (1 / s) to the viscosity η2 measured at a shear rate of 10 (1 / s), when the viscosity is measured at 25°C while changing the shear rate from 0.01 (1 / s) to 100 (1 / s). [3] Spherical boron nitride particles according to [1] or [2], in which a mixture of 15 volume percent spherical boron nitride particles filled in an epoxy resin has a thixotropy index (TI value) of 6 or less, expressed as the ratio (η1 / η2) of the viscosity η1 measured at a shear rate of 1 (1 / s) to the viscosity η2 measured at a shear rate of 10 (1 / s), when the viscosity is measured at 25°C while changing the shear rate from 100 (1 / s) to 0.01 (1 / s). [4] Spherical boron nitride particles according to any one of [1] to [3], having a volume-based cumulative diameter (D50) of 35 μm or less as evaluated by a laser diffraction scattering method without homogenization. [5] Spherical boron nitride particles according to any one of [1] to [4], having an average circularity of greater than 0.80. [6] O measured by X-ray photoelectron spectroscopy 1s The spherical boron nitride particles according to any one of [1] to [5], having a semi-quantitative value calculated from peak intensity of 0.6 or more. [7] A filler for resin, comprising the spherical boron nitride particles according to any one of [1] to [6]. [8] A resin composition comprising a resin and the spherical boron nitride particles according to any one of [1] to [6]. [9] A method for producing spherical boron nitride particles according to any one of [1] to [6], A manufacturing method comprising generating cavitation bubbles in a liquid containing raw spherical boron nitride particles and water.
[0007] According to the present invention, it is possible to provide spherical boron nitride particles, a resin filler and resin composition containing the spherical boron nitride particles, and a method for producing the spherical boron nitride particles, which can give a resin composition with excellent fluidity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] An embodiment of the present invention will be described in detail below. The present invention is not limited to the following embodiment, and can be carried out by making appropriate modifications within the scope that does not impair the effects of the present invention.
[0009] [Spherical boron nitride particles] The spherical boron nitride particles according to this embodiment have an O 1s Semi-quantitative value calculated from peak intensity and B 1s Semi-quantitative value B calculated from peak intensity 1s / O 1s Ratio (hereinafter simply referred to as "B 1s / O 1s The ratio (also called the "ratio") is 90 or less. O measured by X-ray photoelectron spectroscopy 1s Semi-quantitative value calculated from peak intensity and B 1s Semi-quantitative value B calculated from peak intensity 1s / O 1s By making the ratio 90 or less, the spherical boron nitride particles according to this embodiment can provide a resin composition with excellent fluidity when filled into a resin.
[0010] In this specification, "spherical" means that the particles are observed to have a circular or rounded grain shape when observed at 10,000 times magnification using a scanning electron microscope. 1s Semi-quantitative value calculated from peak intensity and B 1s Semi-quantitative value B calculated from peak intensity 1s / O 1sThe "ratio" is the ratio of the background to the B 1s and O 1s The semi-quantitative value was calculated from the peak intensity, and B 1s / O 1s It means a value obtained by calculating the ratio. In this specification, the "Shirley method" refers to a method for determining the shape of the background to be subtracted, assuming that the inelastically scattered electrons that cause the background are independent of energy and that the number of inelastically scattered electrons is proportional to the peak intensity. O measured by X-ray photoelectron spectroscopy 1s Semi-quantitative value calculated from peak intensity and B 1s Semi-quantitative value B calculated from peak intensity 1s / O 1s The spherical boron nitride particles having a ratio of 90 or less have a surface state that is excellent in dispersibility in water. Furthermore, surprisingly, such spherical boron nitride particles improve the flowability of a resin composition when mixed with a resin. The spherical boron nitride particles according to one embodiment have an O content measured by X-ray photoelectron spectroscopy. 1s Semi-quantitative value calculated from peak intensity and B 1s Semi-quantitative value B calculated from peak intensity 1s / O 1s It is preferred that the ratio be 85 or less, more preferably 85 or less, even more preferably 80 or less, even more preferably 75 or less, and especially preferably 70 or less. B 1s / O 1s The lower limit of the ratio is not particularly limited, but may be 10 or more, 15 or more, or 20 or more. B 1s / O 1s One method for making the ratio 90 or less is to subject the raw material spherical boron nitride particles to a cavitation treatment in a liquid containing water. The raw material spherical boron nitride particles have a tendency to aggregate, but when they are subjected to a cavitation treatment in a liquid containing water, the aggregates are broken down while maintaining the shape of the primary particles (spherical shape). Many hydroxyl groups are introduced onto the surfaces of the broken down primary particles, making it easy for B1s / O 1s The ratio can be reduced to 90 or less. B 1s / O 1s It is believed that re-agglomeration of the crushed spherical boron nitride particles in the resin can be suppressed by setting the ratio to 90 or less. Details of the cavitation treatment will be described later. By increasing the cavitation treatment time, B 1s / O 1s The ratio can be made smaller. By treating under conditions with a large number of cavitation bubbles or by extending the cavitation treatment time, the surface hydroxyl groups increase, and B 1s / O 1s The ratio can be reduced. Research by the present inventors has revealed that spherical boron nitride particles treated in this manner can enhance the fluidity of resin more than fine particles disintegrated by mechanical grinding.
[0011] The spherical boron nitride particles according to one embodiment have an O content measured by X-ray photoelectron spectroscopy. 1s The semi-quantitative value calculated from the peak intensity is preferably 0.6 or more, more preferably 0.65 or more, and even more preferably 0.7 or more. 1s The "semi-quantitative value calculated from peak intensity" is calculated by subtracting the background from the spectrum obtained by the Shirley method and 1s This is a semi-quantitative value calculated from the peak intensity. 1s The upper limit of the semi-quantitative value calculated from the peak intensity is not particularly limited, but may be 5.0 or less, 4.0 or less, 3.0 or less, or 2.0 or less. The spherical boron nitride particles according to one embodiment have a B measured by X-ray photoelectron spectroscopy. 1s The semi-quantitative value calculated from the peak intensity is preferably less than 48.4, more preferably 48.35 or less, and even more preferably 48.3 or less. 1sThe "semi-quantitative value calculated from peak intensity" is calculated by subtracting the background from the spectrum obtained using the Shirley method and 1s This is a semi-quantitative value calculated from the peak intensity.
[0012] The spherical boron nitride particles according to one embodiment have a thixotropy index (TI value, hereinafter referred to as the "TI value"), which is expressed by the ratio (η1 / η2) of the viscosity η1 measured when the shear rate is 1 (1 / s) to the viscosity η2 measured when the shear rate is 10 (1 / s), when the viscosity of a mixture of 15 volume % of spherical boron nitride particles filled in an epoxy resin is measured at 25°C while changing the shear rate from 0.01 (1 / s) to 100 (1 / s). (0.01-100) ") is preferably 2 or less, more preferably 1.8 or less, even more preferably 1.6 or less, even more preferably 1.4 or less, and particularly preferably 1.2 or less. The epoxy resin containing the spherical boron nitride particles according to one embodiment has the above-mentioned low thixotropy index (TI value), and therefore has excellent fluidity. TI value (0.01-100) The lower limit value is preferably closer to 1.
[0013] The spherical boron nitride particles according to one embodiment have a thixotropy index (TI value, hereinafter referred to as the "TI value") expressed by the ratio (η1 / η2) of the viscosity η1 measured when the shear rate is 1 (1 / s) to the viscosity η2 measured when the shear rate is 10 (1 / s), when the viscosity of a mixture of 15 volume % of spherical boron nitride particles filled in an epoxy resin is measured at 25°C while changing the shear rate from 100 (1 / s) to 0.01 (1 / s). (100-0.01) ") is preferably 6 or less, more preferably 5.6 or less, even more preferably 5.2 or less, even more preferably 4.8 or less, and particularly preferably 4.6 or less. The epoxy resin containing spherical boron nitride particles according to one embodiment has the above-mentioned low thixotropy index (TI value) in viscosity when the shear rate is changed from high shear to low shear, and therefore has excellent fluidity. TI value (100-0.01) The lower limit value is preferably closer to 1.
[0014] In this specification, the method for measuring the "thixotropy index (TI value)" is as follows. That is, 15% by volume of spherical boron nitride particles is filled into an epoxy resin by a known method to obtain a mixture (resin composition). The obtained mixture is measured at 25°C using a dynamic viscoelasticity measuring device. (1) The viscosity is measured by changing the shear rate from 0.01 (1 / s) to 100 (1 / s), or (2) by changing the shear rate from 100 (1 / s) to 0.01 (1 / s). The thixotropy index (TI value) is calculated as the ratio (η1 / η2) of the viscosity measured when the shear rate is 1 (1 / s) to the viscosity measured when the shear rate is 10 (1 / s). A mixture (resin composition) filled with spherical boron nitride particles according to one embodiment has a thixotropy index (TI value) close to 1 when the shear rate is changed from low shear to high shear, and when the shear rate is changed from high shear to low shear, meaning that it has excellent fluidity.
[0015] The spherical boron nitride particles according to one embodiment preferably have a volume-based cumulative size (D50) of 35 μm or less, more preferably 33 μm or less, even more preferably 32 μm or less, even more preferably 30 μm or less, and particularly preferably 28 μm or less, as evaluated by a laser diffraction scattering method without a specific dispersion treatment, such as a homogenizer treatment (i.e., without applying an external force). The lower limit of the volume-based cumulative size (D50) as evaluated by a laser diffraction scattering method without a homogenizer treatment (i.e., without applying an external force) is not particularly limited, but may be 5 μm or more, 10 μm or more, or 15 μm or more. In this specification, "volume-based cumulative (D50)" means a particle size at which the cumulative value corresponds to 50% in the volume-based cumulative particle size distribution measured by a laser diffraction scattering method (refractive index: 1.7). The cumulative particle size distribution is represented by a distribution curve with the particle size (μm) on the horizontal axis and the cumulative value (%) on the vertical axis. Despite not being homogenized, the spherical boron nitride particles according to one embodiment have a small volume-based cumulative size (D50) of 30 μm or less as evaluated by a laser diffraction scattering method. In other words, the spherical boron nitride particles according to one embodiment are characterized in that they are essentially smaller particles and have a higher proportion of primary particles than secondary particles, even without treatment such as homogenization. The spherical boron nitride particles according to one embodiment contribute to improving the fluidity of a mixture (resin composition) filled with the spherical boron nitride particles. B 1s / O 1s It is difficult for spherical boron nitride particles with a ratio exceeding 90 to achieve such a volume-based accumulation (D50). The spherical boron nitride particles according to the present embodiment can be made into smaller particles by further homogenizing. The spherical boron nitride particles according to one embodiment have a volume-based cumulative size (D50) evaluated by a laser diffraction scattering method after homogenizing in ethanol (conditions: 300 W, 90 sec) of 0.6 μm or less, more preferably 0.58 μm or less, and even more preferably 0.56 μm or less. The lower limit of the volume-based cumulative size (D50) evaluated by a laser diffraction scattering method after homogenizing (conditions: 300 W, 90 sec) is not particularly limited, but may be 0.1 μm or more, 0.2 μm or more, or 0.3 μm or more.
[0016] The spherical boron nitride particles according to one embodiment preferably have an average circularity of more than 0.70, more preferably 0.725 or more, even more preferably 0.75 or more, even more preferably 0.775 or more, and particularly preferably 0.80 or more. The upper limit of the average circularity is not particularly limited, but may be 1 or less, or 0.95 or less. In this specification, the "average circularity" refers to a value calculated as follows. The image of the boron nitride particle taken with a scanning electron microscope (SEM) (magnification: 10,000 times, image resolution: 1280 x 1024 pixels) is analyzed using image analysis software (e.g., MacView, manufactured by Mountec Co., Ltd.) to calculate the projected area (S) and perimeter (L) of the boron nitride particle. The projected area (S) and perimeter (L) are used to calculate the following formula: Circularity = 4πS / L 2 The circularity is calculated according to the following formula: The average circularity is defined as the average circularity obtained for 100 randomly selected boron nitride particles. The spherical boron nitride particles according to one embodiment are characterized by a high average circularity, which contributes to improving the flowability of a mixture (resin composition) filled with the spherical boron nitride particles according to one embodiment.
[0017] (Application) Spherical boron nitride particles can provide a resin composition with excellent fluidity, and therefore can be preferably used as a resin filler.
[0018] [Manufacturing method] The method for producing spherical boron nitride particles according to this embodiment includes generating cavitation bubbles in a liquid containing raw material spherical boron nitride particles and water.
[0019] (Raw material spherical boron nitride particles) The raw spherical boron nitride particles are preferably produced by the method described in Patent Document 2. That is, the raw material spherical boron nitride particles can be obtained by reacting ammonia with a borate ester having an ammonia / borate ester molar ratio of 1 to 10 in an inert gas stream at 750°C or higher for 30 seconds or less, followed by heat treatment in an atmosphere of ammonia gas or a mixed gas of ammonia gas and an inert gas at 1000 to 1600°C for 1 hour or more, and then calcining in an inert gas atmosphere at 1800 to 2200°C for 0.5 hours or more. An example of the borate ester is trimethyl borate.
[0020] The volume-based cumulative diameter (D50) of the raw spherical boron nitride particles evaluated by a laser diffraction scattering method (the method described in paragraph
[0037] , (Particle Size Distribution 2) below) may be 0.01 μm or more, 0.05 μm or more, 0.1 μm or more, 0.2 μm or more, 0.3 μm or more, or 0.4 μm or more, and from the viewpoint of improving the dielectric breakdown characteristics of the heat dissipation member, may be 1 μm or less, 0.9 μm or less, 0.8 μm or less, or 0.7 μm or less. It is preferably 0.01 to 1.0 μm, and more preferably 0.3 to 0.8 μm. The average circularity of the raw material spherical boron nitride particles is preferably 0.8 or more, and more preferably 0.87 or more. The method for measuring the volume-based cumulative diameter (D50) and the average circularity is as described above.
[0021] (Cavitation bubbles) In the method for producing spherical boron nitride particles according to this embodiment, the raw material spherical boron nitride particles are placed in a liquid containing water (preferably in water) to generate cavitation bubbles in the liquid. In this specification, the term "cavitation bubbles" refers to bubbles that are generated when a liquid vaporizes under low pressure. By generating cavitation bubbles in a liquid containing spherical boron nitride particles and water, the expansion and contraction forces caused by the pressure difference of the bubbles generated by cavitation break the secondary particles of the spherical boron nitride particles into primary particles, and at the same time, the surface condition of the particles changes, such as increasing the proportion of hydroxyl groups. The generation of cavitation bubbles can be performed using a commercially available device that generates cavitation bubbles by the foaming phenomenon in liquid caused by reduced pressure or ultrasonic waves. It is preferable to use a commercially available powder suction continuous dissolution and dispersion device, and it is particularly preferable to circulate the liquid for processing. The powder suction continuous dissolution and dispersion device generally has a mechanism for generating a flow rate by an agitator, and the rotation speed of the agitator is preferably 2000 to 10000 rpm, more preferably 4000 to 9000 rpm, even more preferably 4500 to 8000 rpm, even more preferably 5000 to 8000 rpm, and particularly preferably 6000 to 7200 rpm. The expansion and contraction forces caused by the pressure difference of the bubbles generated by cavitation break the secondary particles into primary particles, and at the same time, the surface condition of the particles changes, such as increasing the proportion of hydroxyl groups. In one embodiment, the process of generating cavitation bubbles is preferably performed 50 times or more, more preferably 100 times or more, and even more preferably 150 times or more, as the number of times of cavitation processing calculated from the rotation speed (rpm) of the stirring blade of the device and the discharge amount. 1s / O 1s The ratio can easily be kept below 90. O measured by X-ray photoelectron spectroscopy 1s Semi-quantitative value calculated from peak intensity and B 1s Semi-quantitative value B calculated from peak intensity 1s / O 1s Spherical boron nitride particles having a ratio of 90 or less are obtained.
[0022] In the method for producing spherical boron nitride particles according to this embodiment, the liquid used in the production may be a liquid consisting of only an organic solvent such as ethanol, or may be a mixed solution of water and an organic solvent. In the case of a mixed solution of water and an organic solvent, the water content in the mixed solution is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more, and it is particularly preferable that the mixed solution consists of water only.
[0023] The liquid used in the production preferably contains 5 to 30% by weight of spherical boron nitride particles, more preferably 5 to 20% by weight, even more preferably 5 to 15% by weight, even more preferably 5 to 10% by weight, and particularly preferably 8 to 10% by weight.
[0024] [Resin filler] The filler for resin according to this embodiment contains the spherical boron nitride particles. The spherical boron nitride particles are as described above. Resins to be filled with the resin filler according to this embodiment include epoxy resins, silicone resins, phenolic resins, melamine resins, urea resins, unsaturated polyesters, fluororesins, polyamides such as polyimide, polyamideimide and polyetherimide, polyesters such as polybutylene terephthalate and polyethylene terephthalate, polyphenylene ether, polyphenylene sulfide, wholly aromatic polyesters, polysulfones, liquid crystal polymers, polyethersulfones, polycarbonates, maleimide-modified resins, ABS resins, AAS (acrylonitrile-acrylic rubber-styrene) resins, AES (acrylonitrile-ethylene-propylene-diene rubber-styrene) resins, and the like. A resin containing one or more selected from these is preferable, and an epoxy resin is more preferable. The resin filler according to the present embodiment is added so that the content of the spherical boron nitride particles in the resin composition is preferably 5 to 80% by volume. When the resin filler is added so that the content of the spherical boron nitride particles in the resin composition is 5 to 30% by volume, more preferably 10 to 25% by volume, and even more preferably 15 to 20% by volume, a resin composition with higher fluidity is obtained. When the resin filler is added so that the content of the spherical boron nitride particles in the resin composition is 50 to 80% by volume, more preferably 60 to 80% by volume, and even more preferably 70 to 80% by volume, a resin composition with higher thermal conductivity is obtained. In one embodiment, the resin filler is added so that the content of the spherical boron nitride particles in the resin composition is more than 5% by volume and not more than 20% by volume.
[0025] [Resin composition] The resin composition according to this embodiment contains a resin and the spherical boron nitride particles described above. Examples of the resin include epoxy resin, silicone resin, phenol resin, melamine resin, urea resin, unsaturated polyester, fluororesin, polyamide such as polyimide, polyamideimide, polyetherimide, polyester such as polybutylene terephthalate, polyethylene terephthalate, polyphenylene ether, polyphenylene sulfide, wholly aromatic polyester, polysulfone, liquid crystal polymer, polyethersulfone, polycarbonate, maleimide-modified resin, ABS resin, AAS (acrylonitrile-acrylic rubber-styrene) resin, AES (acrylonitrile-ethylene-propylene-diene rubber-styrene) resin, and the like. It is preferable to include one or more selected from these, and it is more preferable to be an epoxy resin.
[0026] The content of the spherical boron nitride particles in the resin composition is 5 to 80% by volume. From the viewpoint of flowability, the content of the spherical boron nitride particles in the resin composition is preferably 5 to 30% by volume, more preferably 10 to 25% by volume, and even more preferably 15 to 20% by volume. In one embodiment, the content of the spherical boron nitride particles in the resin composition is more than 5% by volume and not more than 20% by volume. From the viewpoint of thermal conductivity, the content of the spherical boron nitride particles in the resin composition is 50 to 80% by volume, more preferably 60 to 80% by volume, and even more preferably 70 to 80% by volume. In one embodiment, the content of the spherical boron nitride particles in the resin composition is more than 70% by volume and not more than 80% by volume.
[0027] The resin composition may contain the following components and, if necessary, other additives. Examples of other additives include stress reducing agents such as rubber-like substances, such as silicone rubber, polysulfide rubber, acrylic rubber, butadiene rubber, styrene block copolymers, and saturated elastomers, various thermoplastic resins, and silicone resins, as well as epoxy resins and resins in which a part or all of a phenolic resin has been modified with aminosilicone, epoxysilicone, or alkoxysilicone, flame retardant assistants such as Sb2O3, Sb2O4, and Sb2O5, flame retardants such as halogenated epoxy resins and phosphorus compounds, and colorants such as carbon black, iron oxide, dyes, and pigments.
[0028] The resin composition can be produced by stirring, dissolving, mixing, and dispersing the above-mentioned materials in predetermined amounts. As an apparatus for mixing, stirring, dispersing, etc., a mortar and pestle machine equipped with a stirring and heating device, a three-roll mill, a ball mill, a planetary mixer, etc. can be used. These apparatuses may also be used in appropriate combination. EXAMPLES
[0029] The present invention will be described in more detail below with reference to examples, but the interpretation of the present invention is not limited to these examples.
[0030] The raw material spherical boron nitride particles were prepared by the following procedure. (1) A reaction tube (quartz tube) placed in a resistance heating furnace was heated to 1150°C. Nitrogen gas was passed through trimethyl borate and then introduced into the reaction tube, thereby introducing trimethyl borate into the reaction tube. Next, ammonia gas was directly introduced into the reaction tube. The molar ratio of the amount of ammonia introduced to the amount of trimethyl borate introduced (ammonia / trimethyl borate) was set to 1.8. Trimethyl borate and ammonia were reacted to obtain a precursor of boron nitride particles (white powder). (2) The obtained precursor of boron nitride particles was placed in a boron nitride crucible installed in a resistance heating furnace, and nitrogen gas and ammonia gas were introduced into the reaction tube at flow rates of 10 L / min and 15 L / min, respectively. The reaction tube was heated at 1500°C for 5 hours to obtain a second precursor. (3) The obtained second precursor was placed in a boron nitride crucible and heated in an induction heating furnace under a nitrogen atmosphere at 2000° C. for 5 hours to obtain spherical boron nitride particles. The volume-based cumulative diameter (D50) of the raw material spherical boron nitride particles evaluated by a laser diffraction scattering method was 0.62 μm, and the average circularity was 0.87.
[0031] [Examples 1 to 4, Comparative Example 1] Spherical boron nitride powder was mixed into 1000 cc of ion-exchanged water so that the concentration was 10% by weight. For Examples 1 to 4, the resulting aqueous solution was subjected to cavitation treatment using a powder suction continuous dissolution and dispersion device (manufactured by Nihon Spindle Co., Ltd., "Jet Paster", model number: JPSS) under the conditions shown in Table 1. For Comparative Example 1, no cavitation treatment was performed. In Table 1, "number of treatments" refers to the number of times the treatment solution passes through the agitator blade, calculated from the rotation speed (rpm) of the agitator blade of the powder suction, continuous dissolving and dispersing apparatus and the discharge amount per rotation. After the cavitation treatment, the liquid was filtered and dried to recover spherical boron nitride powder.
[0032] [measurement] The various physical properties described below were measured for the spherical boron nitride powders obtained in Examples 1 to 4 and Comparative Example 1. The results are shown in Table 1. (B 1s / O 1s ratio) The spherical boron nitride powders according to Examples 1 to 4 and Comparative Example 1 were measured using an X-ray photoelectron spectrometer (Thermo Corporation, "K-Alpha type X-ray photoelectron spectrometer", Al-X-ray source with monochromator, measurement area: 400 × 200 μm), and the spectrum was obtained by removing the background by the Shirley method, and B 1s and O 1s Calculate the semi-quantitative value from the peak intensity, B 1s / O 1s The ratio was calculated.
[0033] (Particle size distribution 1) 0.1 g of the spherical boron nitride particles according to Examples 1 to 4 and Comparative Example 1 was dispersed in 80 mL of ethanol, and the volumetric particle size distribution was measured using a laser diffraction scattering particle size distribution analyzer (manufactured by Beckman Coulter, Inc., product name: LS-13 320) without homogenizing. At this time, the refractive index of ethanol was set to 1.359, and the refractive index of the boron nitride powder was set to 1.7. From the frequency particle size distribution obtained, the median diameter D50 (μm) of the particles not homogenized was calculated.
[0034] (Particle size distribution 2) 0.01 g of the spherical boron nitride particles according to Examples 1 to 4 and Comparative Example 1 was dispersed in 80 mL of ethanol, and ultrasonic dispersion was performed for 1 minute and 30 seconds at an amplitude of 70 to 80% using an ultrasonic homogenizer (manufactured by Nippon Seiki Seisakusho, product name: US-300E was used), and then the volumetric particle size distribution was measured using a laser diffraction scattering particle size distribution measuring device (manufactured by Beckman Coulter, product name: LS-13 320 was used). From the obtained volumetric particle size distribution, the median diameter was calculated. This median diameter is the particle size at 50% of the cumulative value of the cumulative particle size distribution. At this time, the refractive index of ethanol was 1.359, and the refractive index of the boron nitride powder was 1.7. The results are shown in Table 1.
[0035] (Average circularity) The image of the boron nitride particle taken with a scanning electron microscope (SEM) (magnification: 10,000 times, image resolution: 1280 x 1024 pixels) is analyzed using image analysis software (e.g., MacView, manufactured by Mountec Co., Ltd.) to calculate the projected area (S) and perimeter (L) of the boron nitride particle. The projected area (S) and perimeter (L) are used to calculate the following formula: Circularity = 4πS / L 2 The circularity is calculated according to the following formula: The average circularity is defined as the average circularity obtained for 100 randomly selected boron nitride particles.
[0036] (Preparation of resin composition) The spherical boron nitride particles according to Examples 1 to 4 and Comparative Example 1 were blended with an epoxy resin as follows to prepare resin compositions. A dispersant (manufactured by BYK Japan, "DISPERBYK-111", 0.3 wt%), an SC material (manufactured by Tokyo Chemical Industry Co., Ltd., "3-glycidyloxypropyltrimethoxysilane", 1 wt%), and spherical boron nitride particles (15 wt%) according to Examples 1 to 4 and Comparative Example 1 were added to the epoxy resin, and the mixture was kneaded for 3 minutes at room temperature, at a revolution speed of 2000 rpm, and at a rotation speed of 800 rpm using a hybrid mixer (manufactured by Thinky, "Awatori Rentaro AR-250"). Then, the mixture was kneaded twice using a three-roll mill (manufactured by Imex, "BR-150VIII", gap: 10 μm, finishing roll rotation speed: 60 rpm) to obtain a resin composition.
[0037] (Thixotropy index (TI value)) For the obtained resin composition, the viscosity was measured at 25°C using a rheometer (Anton Paar, "MCR92") when (1) the shear rate was changed from 0.01 (1 / s) to 100 (1 / s) and (2) the shear rate was changed from 100 (1 / s) to 0.01 (1 / s). The thixotropy index (TI value) was calculated from the ratio (η1 / η2) of the viscosity η1 measured when the shear rate was 1 (1 / s) to the viscosity η2 measured when the shear rate was 10 (1 / s).
[0038] [Table 1]
[0039] As shown in Table 1, the resin compositions containing the spherical boron nitride particles according to Examples 1 to 4 have superior fluidity compared to the resin composition containing the spherical boron nitride particles according to Comparative Example 1. Surprisingly, not only when the shear rate is changed from low shear to high shear, but also when the shear rate is changed from high shear to low shear, the thixotropy index (TI value) is low, closer to 1, and has the property of high fluidity. [Industrial Applicability]
[0040] The spherical boron nitride particles of this embodiment can provide a resin composition with excellent fluidity, and therefore can be suitably used in resin fillers and resin compositions containing the spherical boron nitride particles, and have industrial applicability.
Claims
1. O measured by X-ray photoelectron spectroscopy 1s Semi-quantitative value calculated from peak intensity and B 1s Semi-quantitative value B calculated from peak intensity 1s / O 1s The ratio is 90 or less, Spherical boron nitride particles, in which a mixture of 15 volume % spherical boron nitride particles is filled into an epoxy resin, the viscosity of which is measured at 25°C while changing the shear rate from 0.01 (1 / s) to 100 (1 / s), and the thixotropy index (TI value) is expressed as the ratio (η1 / η2) of the viscosity η1 measured at a shear rate of 1 (1 / s) to the viscosity η2 measured at a shear rate of 10 (1 / s), of 2 or less.
2. O measured by X-ray photoelectron spectroscopy 1s Semi-quantitative value calculated from peak intensity and B 1s Semi-quantitative value B calculated from peak intensity 1s / O 1s The ratio is 90 or less, a mixture of an epoxy resin filled with 15 volume % spherical boron nitride particles, the viscosity of which is measured at 25°C while changing the shear rate from 0.01 (1 / s) to 100 (1 / s), the thixotropy index (TI value) represented by the ratio (η1 / η2) of the viscosity η1 measured at a shear rate of 1 (1 / s) to the viscosity η2 measured at a shear rate of 10 (1 / s) is 2 or less, Spherical boron nitride particles, in which a mixture of 15 volume % spherical boron nitride particles is filled into an epoxy resin, and the viscosity is measured at 25°C while changing the shear rate from 100 (1 / s) to 0.01 (1 / s), and the thixotropy index (TI value) is expressed as the ratio (η1 / η2) of the viscosity η1 measured when the shear rate is 1 (1 / s) to the viscosity η2 measured when the shear rate is 10 (1 / s), is 6 or less.
3. B 1s 3. The spherical boron nitride particles according to claim 1 or 2, having a semi-quantitative value calculated from peak intensity of less than 48.
4.
4. 3. The spherical boron nitride particles according to claim 1 or 2, which have a volume-based cumulative diameter (D50) of 35 μm or less as evaluated by a laser diffraction scattering method without homogenization treatment.
5. 3. Spherical boron nitride particles according to claim 1 or 2, having an average circularity of greater than 0.
80.
6. O measured by X-ray photoelectron spectroscopy 1s 3. The spherical boron nitride particles according to claim 1, wherein a semi-quantitative value calculated from peak intensity is 0.6 or more.
7. A filler for resin, comprising the spherical boron nitride particles according to claim 1 or 2.
8. A resin composition comprising a resin and the spherical boron nitride particles according to claim 1 or 2.
9. A method for producing the spherical boron nitride particles according to claim 1 or 2, A manufacturing method comprising generating cavitation bubbles in a liquid containing raw spherical boron nitride particles and water.
Citation Information
Patent Citations
Composition for forming heat-conducting material, heat-conducting material, heat-conducting sheet, and device with heat-conducting layer
WO2021059806A1
Boron nitride particles and method for producing same, and resin composition and receptor containing said boron nitride particles