Grain-oriented electrical steel sheet and method for manufacturing grain-oriented electrical steel sheet

By combining specific elements and controlled annealing processes, the method enhances magnetic flux density and film adhesion in grain-oriented electrical steel sheets, addressing the instability issues caused by Bi, Pb, In, and Te additions.

JP7564422B2Active Publication Date: 2024-10-09NIPPON STEEL CORPORATION
View PDF 19 Cites 0 Cited by

Patent Information

Application Number
JP2020073031
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-04-15
Publication Date
2024-10-09
Estimated Expiration
2040-04-15

AI Technical Summary

Technical Problem

Existing grain-oriented electrical steel sheets face challenges in achieving stable high magnetic flux density and film adhesion due to the addition of elements like Bi, Pb, In, and Te, which can lead to fine grains during secondary recrystallization, reducing hot ductility and varying magnetic properties.

Method used

A method involving the addition of specific combinations of Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt, and Hg, along with controlled annealing and coating compositions, to stabilize secondary recrystallization and enhance magnetic properties while improving film adhesion.

Benefits of technology

The method results in a grain-oriented electrical steel sheet with stable high magnetic flux density and excellent film adhesion, ensuring consistent performance and improved hot ductility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564422000001
    Figure 0007564422000001
  • Figure 0007564422000002
    Figure 0007564422000002
  • Figure 0007564422000003
    Figure 0007564422000003
Patent Text Reader

Abstract

To provide a method for producing an oriented electromagnetic steel sheet that can produce an oriented electromagnetic steel sheet having excellent magnetic properties on an industrial scale and in a stable manner.SOLUTION: An oriented electromagnetic steel sheet has: a base steel sheet containing, in mass%, Si: 2.5-4.5%, Mn: 0.04-0.20%, with the balance being Fe and inevitable impurities; and a coat predominantly composed of forsterite that is formed on the base steel sheet and contains at least two selected from the group consisting of Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt, and Hg in a total quantity of 0.02-0.50% (mass%), and at least one of Bi and Pb in a total quantity of 0.005% or less (mass%).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a grain-oriented electrical steel sheet having good magnetic properties and a method for stably producing the grain-oriented electrical steel sheet. [Background technology]

[0002] Grain-oriented electrical steel sheets contain about 2 to 5% Si and have grain orientation of {110} <001> This steel sheet has a high degree of grain orientation and is mainly used as the core material for stationary inductors in transformers, etc. The high degree of grain orientation is achieved by controlling a catastrophic grain growth phenomenon called secondary recrystallization.

[0003] As a method for controlling secondary recrystallization, there is a method in which a compound that functions as an inhibitor during secondary recrystallization is sufficiently dissolved before hot rolling, and then finely precipitated by hot rolling and subsequent annealing. In the method of Patent Document 1, MnS and AlN are used as inhibitors, and in the methods of Patent Documents 2 and 3, MnS and MnSe are used as inhibitors.

[0004] In addition, as a method for controlling secondary recrystallization, Patent Documents 4 and 5, for example, disclose a method in which a steel slab before hot rolling is heated to less than 1280°C, and then nitriding treatment after cold rolling is performed to form AlN, which is used as an inhibitor.

[0005] Grain-oriented electrical steel sheets with excellent magnetic properties have been developed based on the above-mentioned secondary recrystallization control. However, in recent years, momentum for energy conservation has increased, and further improvements in magnetic properties are required.

[0006] A typical index of the magnetic properties of grain-oriented electrical steel sheets is magnetic flux density. To increase magnetic flux density, the crystal grain orientation should be oriented in the {110} <001> It is necessary to accumulate the inhibitor in the orientation to a higher degree, and one method for achieving this is to use an auxiliary additive element that strengthens the inhibitor action. Patent documents 6 and 7 disclose a method using Bi, Patent document 8 discloses a method using Pb, and Patent documents 9 to 14 disclose that, in addition to using Te, auxiliary elements such as In, Ag, and Zn are effective.

[0007] Furthermore, Patent Document 15 discloses that Ag has the effect of suppressing the growth of primary grains in the secondary recrystallization process of electrical steel sheets and promoting secondary recrystallization. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Special Publication No. 40-015644 [Patent Document 2] Special Publication No. 51-013469 [Patent Document 3] Japanese Patent Application Publication No. 06-192735 [Patent Document 4] Special Publication No. 62-045285 [Patent Document 5] Japanese Patent Application Publication No. 02-077525 [Patent Document 6] Japanese Patent Application Publication No. 06-089805 [Patent Document 7] Japanese Patent Application Publication No. 08-269552 [Patent Document 8] JP 2017-186587 A [Patent Document 9] Japanese Patent Application Publication No. 06-184640 [Patent Document 10] Japanese Patent Application Publication No. 06-207220 [Patent Document 11] JP 2006-299297 A [Patent Document 12] JP 2008-196016 A [Patent Document 13] JP 2008-261013 A [Patent Document 14] JP 2009-235574 A [Patent Document 15] Special Publication No. 37-9305 Summary of the Invention [Problem to be solved by the invention]

[0009] The present inventors have investigated the composite addition of various elements with the aim of further improving the magnetic flux density of grain-oriented electrical steel sheets by utilizing inhibitor reinforcing elements such as Bi, Pb, In, and Te. As a result, they have noticed that even if Bi, Pb, In, Te, and the like are added to slabs for grain-oriented electrical steel sheets, the magnetic flux density of the final product may not be sufficiently improved. When the cause of this was investigated, it was found that when the improvement in properties is insufficient, fine grains are likely to occur in secondary recrystallization, and the variation in properties increases. It was also found that the addition of Bi, Pb, In, Te, and the like tends to reduce hot ductility, and may require trimming of the hot-rolled sheet edge, which tends to reduce productivity and yield. Further investigations have led to the development of a technology that improves hot ductility, suppresses the generation of fine grains in secondary recrystallization, and stably obtains high magnetic flux density in the final product by dividing the additive elements into several groups and containing an appropriate combination of elements classified into each group. Specifically, when Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt and Hg are added singly to a slab for grain-oriented electrical steel sheet containing Bi and / or Pb, the hot rollability is extremely poor, but when the required amounts of Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt and Hg are added in combination, the hot rollability can be improved and the generation of fine grains in secondary recrystallization can be suppressed, so that a high magnetic flux density can be stably obtained in the final product. However, the steel sheet obtained in this way may have insufficient coating adhesion under severe processing conditions, and there is room for further improvement in coating adhesion.

[0010] In view of the above-mentioned technical problems associated with the use of inhibitor reinforcing elements such as Bi, Pb, In, and Te, the present invention aims to solve these problems and provide a grain-oriented electrical steel sheet having good magnetic properties and coating adhesion, and a method for manufacturing the grain-oriented electrical steel sheet.

[0011] The present inventors have conducted extensive research into improving coating adhesion when inhibitor reinforcing elements such as Bi, Pb, In, and Te are utilized. As a result, it has been found that adding the required amounts of multiple types of Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt, and Hg to a slab for grain-oriented electrical steel sheet containing Bi and / or Pb improves hot rollability and provides a high and stable magnetic flux density in the final product, and further that controlling the amounts of Ca, Sr, Ba, Ce, Pr, Eu, and Gd added to the annealing separator that is applied and dried before final annealing ensures good coating adhesion.

[0012] The present invention has been made based on the above findings, and the gist of the present invention is as follows. [Means for solving the problem]

[0013] [1] In mass%, Si: 2.5 to 4.5%, C: 0.02 to 0.10%, acid-soluble Al: 0.01 to 0.05%, N: 0.003 to 0.02%, S+0.4·Se: 0.003 to 0.04%, Mn: 0.04 to 0.20%, the sum of one or more of Bi and Pb: 0.0005 to 0.05%, and further, the group consisting of Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt, and Hg. A slab containing 0.001 to 0.500% in total of at least two or more selected from the group consisting of Fe and impurities is heated to 1000 to 1450°C, hot-rolled to form a hot-rolled sheet, annealed, pickled, and then cold-rolled once or twice with annealing in between to form a cold-rolled sheet, and the cold-rolled sheet is subjected to decarburization annealing, and if necessary, nitriding treatment is performed during or after the annealing, and then An annealing separator containing magnesium oxide powder as a main component, The magnesium oxide powder of the annealing separator contains, as an impurity element, at least one element selected from the group consisting of Ca, Sr, Ba, Ce, Pr, Eu, and Gd in a total abundance ratio of 0.02 to 0.8% relative to the abundance of Mg in the magnesium oxide powder, The annealing separator further contains, in addition to the magnesium oxide powder, an additive containing at least one element selected from the group consisting of Ca, Sr, Ba, Ce, Pr, Eu, and Gd, such that the total amount of each element is 0.2 to 5.0% relative to the amount of Mg contained in the annealing separator, Further, an annealing separator in which the ratio of the total amount of Ca, Sr, Ba, Ce, Pr, Eu, and Gd as impurity elements in magnesium oxide powder in the annealing separator to the total amount of Ca, Sr, Ba, Ce, Pr, Eu, and Gd in the annealing separator is 0.02 to 0.66 is applied to the front and back surfaces of a steel sheet and dried, A method for producing a grain-oriented electrical steel sheet, comprising the steps of: [2] The method for producing a grain-oriented electrical steel sheet according to [1], wherein the slab contains at least one element selected from the group consisting of Te, In, Cd, Zn, and Ga in a total content of 0.0005% or more, and at least one element selected from the group consisting of Au, Ag, Pd, Pt, and Hg in a total content of 0.0005% or more. [3] A grain-oriented electrical steel sheet comprising: a base steel sheet containing, by mass%, 2.5-4.5% Si, 0.04-0.20% Mn, with the balance being Fe and unavoidable impurities; and a coating mainly composed of forsterite on a surface of the base steel sheet, the coating containing, by mass%, 0.02-0.50% in total of at least two elements selected from the group consisting of Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt, and Hg, 0.02-0.50% in total of at least one element selected from the group consisting of Ca, Sr, Ba, Ce, Pr, Eu, and Gd, and 0.005% or less in total of one or more elements of Bi and Pb. [4] On the surface of the base steel plate, [3] The grain-oriented electrical steel sheet according to [3], wherein a coating mainly composed of forsterite is present, which contains at least one selected from the group consisting of Te, In, Cd, Zn, and Ga in a total amount of 0.01% or more, and at least one selected from the group consisting of Au, Ag, Pd, Pt, and Hg in a total amount of 0.01% or more. [5] On the surface of the base steel plate, A grain-oriented electrical steel sheet as described in [3] or [4], comprising a coating mainly composed of forsterite, in which the difference between the depth in the sheet thickness direction of the element with the greatest content selected from the group consisting of Ca, Sr, Ba, Ce, Pr, Eu, and Gd and the depth in the sheet thickness direction of the element with the greatest content selected from the group consisting of S and Se is within ±1.5 μm. Effect of the Invention

[0014] According to the present invention, a grain-oriented electrical steel sheet having a stable high magnetic flux density, excellent coating adhesion and good hot rollability can be stably produced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] In the following description, all % in chemical composition means % by mass.

[0016] The present invention is characterized in that a slab for grain-oriented electrical steel sheet containing 0.0005 to 0.05% Bi and / or Pb as auxiliary elements reinforcing the inhibitor function is further made to contain 0.001 to 0.500% in total of at least two or more elements selected from the group consisting of Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt and Hg, and is produced by a predetermined production procedure described in detail later, whereby the annealing separator is controlled to have a predetermined chemical composition.

[0017] The final product, grain-oriented electrical steel sheet, is characterized in that a coating mainly composed of forsterite is formed on the surface of the base steel sheet, and contains at least two elements selected from the group consisting of Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt, and Hg in a total content of 0.02 to 0.50%, at least one element selected from the group consisting of Ca, Sr, Ba, Ce, Pr, Eu, and Gd in a total content of 0.02 to 0.50%, and at least one element and Pb in a total content of 0.005% or less.

[0018] (Slabs for grain oriented electrical steel sheets) First, the slab composition will be described. In this description, elements other than Bi, Pb, Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt and Hg are general matters and can be appropriately adjusted within known ranges.

[0019] Silicon is an important element that acts to increase electrical resistance and reduce iron loss. If added at less than 2.5%, the effect of reducing iron loss is not achieved. On the other hand, if added at more than 4.5%, the rolled material is prone to cracking during cold rolling, which may make rolling impossible. From the viewpoints of improving iron loss characteristics and avoiding cracking during rolling, a silicon content of 2.8 to 3.8% is preferable.

[0020] C is an element effective for improving strength and controlling crystal orientation, and is added in a required amount. Since decarburization occurs in the subsequent decarburization annealing process, the less C, the shorter the annealing time, which is preferable in terms of productivity, but if it is less than 0.02%, the crystal grains become coarse when the slab is heated, and the magnetic properties deteriorate. On the other hand, if it exceeds 0.10%, the decarburization annealing time becomes long, not only reducing productivity but also making decarburization insufficient. From the viewpoints of maintaining strength, controlling crystal orientation, and promoting decarburization, 0.04 to 0.08% is preferable.

[0021] Acid-soluble Al and N are the elements necessary to form AlN or (Al,Si)N, which act as inhibitors.

[0022] When the acid-soluble Al is less than 0.01% or the N is less than 0.003%, the amount of AlN or (Al, Si)N produced is small, and sufficient inhibitor function cannot be secured, and the desired secondary recrystallization does not occur. On the other hand, when the acid-soluble Al is more than 0.05% or the N is more than 0.02%, the secondary recrystallization temperature becomes too high due to the excess inhibitor, and secondary recrystallization failure occurs. In terms of securing an appropriate amount of inhibitor, the acid-soluble Al is preferably 0.02 to 0.035%, and the N is preferably 0.006 to 0.01%. As will be described later in relation to the manufacturing method, when a manufacturing method in which nitriding is performed during the manufacturing process to control the inhibitor effect is applied, the upper limit of N can be set lower, with the upper limit being 0.015%, and the preferred upper limit being 0.008%.

[0023] Mn is an element necessary to form inhibitors in manufacturing processes in which the slabs are heated at relatively high temperatures, utilizing Mn compounds (generally MnS or MnSe) as the primary inhibitors.

[0024] If the Mn content is less than 0.04%, the amount of Mn compounds produced is small, sufficient inhibitor function cannot be obtained, and the desired secondary recrystallization does not occur. On the other hand, if the Mn content exceeds 0.20%, the heating temperature for slab heating to dissolve the Mn compounds must be increased or the heating time must be extended, which increases the operational load. From the viewpoints of complete solution treatment and securing an appropriate amount of inhibitor, the Mn content is preferably 0.06 to 0.09%.

[0025] In addition, in a manufacturing method in which the inhibitor is reinforced with AlN formed by nitriding after hot rolling and the slab is heated at a relatively low temperature, there is a likelihood in the solution treatment state for ensuring the inhibitor function of the Mn compound, and some undissolved Mn is acceptable, so the preferable Mn range is 0.06 to 0.20%, and more preferably 0.08 to 0.15%.

[0026] S and Se are elements necessary to form inhibitors in manufacturing processes in which the slabs are heated at relatively high temperatures, utilizing Mn compounds (generally MnS or MnSe) as the primary inhibitors.

[0027] In this case, S and Se can be added alone or in combination, but the amount added can be specified as the total content, which is (S + 0.4 Se), and is added at 0.003 to 0.04%. Here, 0.4 in the formula is the atomic weight of S / atomic weight of Se, and is a coefficient that converts the effect of Se to the effect of S. If only MnS is used as an inhibitor of Mn compounds, this corresponds to S: 0.003 to 0.04%. Also, if only MnSe is used as an inhibitor of Mn compounds, this corresponds to Se: 0.0075 to 0.1%.

[0028] If (S+0.4·Se) is less than 0.003%, sufficient inhibitor function cannot be ensured, and the desired secondary recrystallization does not occur. On the other hand, if (S+0.4·Se) exceeds 0.04%, depending on the Mn content, it is necessary to increase the heating temperature or the heating time of the slab heating to solutionize the Mn compounds, which increases the operational load. In terms of ensuring the appropriate amount of inhibitor, (S+0.4·Se) is preferably 0.007 to 0.012%.

[0029] In addition, in a manufacturing method in which the inhibitor is reinforced with AlN formed by nitriding after hot rolling and the slab is heated at a relatively low temperature, the inhibitor function of the Mn compound does not need to be strong, so (S + 0.4 Se) can be 0.003 to 0.02%, and the preferable range is 0.003 to 0.010%.

[0030] The slab used in the manufacturing method of the present invention contains Bi and / or Pb as inhibitor reinforcing elements for increasing magnetic flux density. Hereinafter, in this specification, Bi and Pb may be collectively referred to as "B group elements". The B group elements may be contained alone or in combination, and in the present invention, the total content of the B group elements is defined, and the total of one or more of Bi and Pb is 0.0005 to 0.05%.

[0031] If the total content of B group elements is less than 0.0005%, the effect of improving magnetic flux density cannot be obtained. On the other hand, if the total content exceeds 0.05%, the effect of improving magnetic flux density is saturated and the hot ductility is reduced. To reliably obtain the effect of adding B group elements, it is preferable to add 0.001 to 0.002%.

[0032] In the slab of the present invention, in addition to the above-mentioned composition, two or more elements selected from the group consisting of Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt and Hg are contained in a total amount of 0.001 to 0.500%. Hereinafter, in this specification, Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt and Hg may be collectively referred to as "X group elements". The X group elements significantly increase the magnetic flux density when added simultaneously with the B group elements, but the inclusion of only one kind leads to a significant deterioration in hot ductility and destabilization of secondary recrystallization, which leads to a large variation in magnetic flux density. However, the addition of two or more kinds makes it possible to improve the hot ductility and suppress the variation in magnetic flux density by stabilizing the secondary recrystallization. When the content is less than 0.001%, the above-mentioned action does not appear. On the other hand, when the content exceeds 0.500%, not only the above-mentioned magnetic flux density improving effect is saturated, but also the hot ductility may be deteriorated. In addition, the cost of addition increases, so that it is not included in the present invention. The total content of two or more elements selected from the X group elements is preferably 0.002 to 0.240%, and more preferably 0.004 to 0.120%.

[0033] The mechanism by which the X group elements exert the above-mentioned action is not clear, but is thought to be as follows. The B group elements are generally elements that are difficult to dissolve in the αFe phase, which is the main phase of the structure of the steel sheet and slab of the present invention, and exert the effect of improving the magnetic flux density by strengthening the inhibitor. The inhibitor is further strengthened by adding the X group elements, which have a strong affinity with the B group elements, and it is expected that even higher magnetic flux density can be realized. On the other hand, the X group elements are also elements that tend to segregate alone to grain boundaries. For this reason, if added carelessly, it will reduce the hot ductility, make the secondary recrystallization unstable, and increase the variation in magnetic flux density. It is believed that by containing two or more types of X group elements rather than a single one, it is possible to suppress segregation to the grain boundaries, strongly exert the cooperative effect with the B group elements, and efficiently enjoy only the inhibitor strengthening function while avoiding the decrease in hot ductility.

[0034] In order to achieve the above-mentioned effect, it is preferable to classify the X-group elements into two groups, and to include at least one element from each of the group consisting of Te, In, Cd, Zn, and Ga, and the group consisting of Au, Ag, Pd, Pt, and Hg. Hereinafter, in this specification, Te, In, Cd, Zn, and Ga may be collectively referred to as "C-group elements", and Au, Ag, Pd, Pt, and Hg may be collectively referred to as "D-group elements". In the slab of the present invention, the above-mentioned effect is more significantly exhibited by satisfying the following: the total of at least one element selected from the C-group elements: 0.0005% or more, and the total of at least one element selected from the D-group elements: 0.0005% or more. (However, as mentioned above, the total of the X-group elements is 0.500% or less.) If either or both of the C-group elements and the D-group elements are less than 0.0005%, no significant effect can be obtained. For each of C and D, 0.001 to 0.120% is preferable, and 0.002 to 0.060% is more preferable. The total of C group elements and the total of D group elements do not need to be the same amount, but if the total content of X group elements is constant, the effect will be more remarkable if the contents are about the same. The same amount means that the amount of one group element is 0.5 to 1.5 times, more preferably 0.8 to 1.2 times, the amount of the other group element.

[0035] Although the mechanism is not clear, C-type elements have a high affinity with D-type elements, and the coexistence of both not only complicates the interactions, including with B-type elements, but also forms stable compounds with each type of element, which increases the effect of avoiding the retention of fine grains and the decrease in hot ductility during secondary recrystallization, and is thought to stabilize the inhibitor effect.

[0036] Furthermore, the slab of the present invention may contain one or more of other inhibitor constituent elements such as Cu, Sn, Sb, etc., within a known range. The total amount is generally 0.0005 to 0.5%.

[0037] The balance of the chemical composition of the slab is Fe and impurities. The impurities refer to elements that are mixed in from raw materials such as ores, scraps, or the manufacturing environment when the slab is industrially manufactured. In addition, this does not exclude the addition of known elements to replace Fe in the range that does not eliminate the effect of the present invention, in the expectation of a known effect.

[0038] (Grain-oriented electrical steel sheet) Next, grain-oriented electrical steel sheets will be described. In this description, elements other than Bi, Pb; Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt, and Hg; and Ca, Sr, Ba, Ce, Pr, Eu, and Gd are general matters and can be appropriately adjusted within known ranges.

[0039] The chemical composition of the base steel sheet of grain-oriented electrical steel sheet basically conforms to the composition of the raw material, the above-mentioned slab. However, in the general production of grain-oriented electrical steel sheet, some of the contained elements are discharged from the system by decarburization annealing and purification annealing during the manufacturing process, so the chemical composition of the raw material slab and the base steel sheet of the final product, grain-oriented electrical steel sheet, are clearly different. The following explanation is given with this in mind.

[0040] In addition, during the finish annealing in the manufacturing process of grain-oriented electrical steel sheet, a coating mainly composed of forsterite, generally called a "glass coating" or "primary coating", is formed on the surface of the base steel sheet. The grain-oriented electrical steel sheet of the present invention is characterized in that this coating contains an X group element, a B group element, and at least one element selected from the group consisting of Ca, Sr, Ba, Ce, Pr, Eu, and Gd.

[0041] First, the chemical composition of the base steel sheet will be described.

[0042] Silicon is an important element that acts to increase electrical resistance and reduce iron loss. If added at less than 2.5%, the effect of reducing iron loss is not achieved. On the other hand, if added at more than 4.5%, the rolled material is prone to cracking during cold rolling, which may make rolling impossible. From the viewpoints of improving iron loss characteristics and avoiding cracking during rolling, a silicon content of 2.8 to 3.8% is preferable.

[0043] Even if Mn is released from the system during the manufacturing process, it is an element that is added to the slab from the viewpoint of inhibitor control, but a not insignificant amount is contained in the final product. It is cost-prohibitive and difficult to perform purification annealing to a degree that results in a content of less than 0.04% in the final product. The upper limit is set at 0.20%, assuming that most of the Mn added to the slab remains in the final product.

[0044] C, acid-soluble Al, N, S and Se, which were essential elements in the slab composition, become optional elements in the product.

[0045] C is discharged from the system during decarburization annealing in the manufacturing process and is clearly reduced from the slab composition. It does not need to be contained in the final product, and since it can impair magnetic properties due to aging, it is basically an element that should be reduced, and zero is acceptable. Considering practical decarburization annealing capacity, it should be 0.005% or less. On the other hand, considering the cost of decarburization annealing, it is difficult to reduce it to less than 0.0001%.

[0046] As mentioned above, acid-soluble Al and N are elements that are used as inhibitors in the manufacturing process, but they do not need to be contained in the final product. A large proportion of these elements are discharged outside the system during purification annealing in the manufacturing process. Since Al reduces the saturation magnetic flux density and N causes magnetic aging, it is acceptable to have zero. Considering practical purification annealing capacity and cost, the acid-soluble Al: 0.0001-0.005%, N: 0.0001-0.005%.

[0047] As mentioned above, S and Se are also elements that are used as inhibitors in the manufacturing process, but they do not need to be contained in the final product and can be zero. A large proportion of these elements are discharged outside the system during purification annealing in the manufacturing process. Considering practical purification annealing capacity and costs, the limit for both S and Se is 0.0001 to 0.005%.

[0048] Attention should be paid to the B group elements and X group elements, which are essential elements in slabs. In a typical manufacturing method of grain-oriented electrical steel sheet involving purification annealing at high temperatures, these are almost completely removed from the base steel sheet, and it is very difficult to detect them in the chemical composition of the base steel sheet in the finished sheet. For this reason, in the present invention, the B group elements and X group elements are not specified as the chemical composition of the base steel sheet of the grain-oriented electrical steel sheet, but are specified in the chemical composition of the primary coating described below. However, the grain-oriented electrical steel sheet of the present invention does not exclude base steel sheets containing detectable amounts of B group elements and X group elements.

[0049] The balance of the chemical composition of the base steel sheet of the grain-oriented electrical steel sheet is Fe and impurities. The impurities refer to elements that are mixed in from raw materials such as ore, scrap, or the manufacturing environment when the base steel sheet is industrially manufactured. In addition, this does not exclude the addition of elements that exhibit known effects to replace Fe in the hope of achieving known effects, within the range that does not eliminate the effects of the present invention.

[0050] Next, the composition of the coating, which can be said to be the greatest feature of the grain-oriented electrical steel sheet of the present invention, will be described. The "coating" to be described here is a coating generally called a "glass coating" or "primary coating" as described above. The formation mechanism itself is well known in grain-oriented electrical steel sheets and is not special. In other words, the oxide layer that covers the steel sheet surface is mainly composed of oxides that are applied to the steel sheet surface as a so-called "annealing separator" before finish annealing and react with the base steel sheet during finish annealing. In this reaction process, various elements are discharged from the base steel sheet to the outside of the system, and at that time, they react with oxides caused by the annealing separator on the steel sheet surface and oxygen in the atmosphere. After finish annealing, some of them are naturally removed or removed by washing with water or light pickling, but some are fixed and held by the formation of a complex uneven interface with the base steel sheet surface. During the reaction, diffusion of elements from the base steel sheet to the final annealing atmosphere occurs, causing a large change in composition in the thickness direction, so that the chemical composition of the "primary coating" that is ultimately left attached to the surface of the base steel sheet is completely different from that of the annealing separator. Generally, it is mainly composed of forsterite, for example, forsterite (Mg2SiO4), spinel (MgAl2O4), or cordierite (Mg2Al4Si5O 16 ) and other composite oxides. In addition, relatively small amounts of sulfides of Mn and the like and nitrides of Ti and the like may be dispersed as metal compounds derived from the steel sheet and the annealing separator. Hereinafter, the coating mainly composed of forsterite that should contain an X group element in the present invention may be simply referred to as the "primary coating."

[0051] In the grain-oriented electrical steel sheet of the present invention, X-group elements discharged from the base steel sheet by purification annealing are incorporated into the primary coating, and the chemical composition of the primary coating of the product sheet appears as a characteristic. In the grain-oriented electrical steel sheet of the present invention, a coating containing at least two or more elements selected from the X-group elements in a total amount of 0.02 to 0.50% is formed on the surface of the base steel sheet. This results in a grain-oriented electrical steel sheet of the present invention having high magnetic flux density, little fluctuation in magnetic flux density, and stable properties. The content is preferably 0.03 to 0.40%, more preferably 0.05 to 0.30%.

[0052] Also, as explained in the slab composition, from the viewpoint of significantly exhibiting the effect of stabilizing high magnetic flux density, it is desirable that the above-mentioned primary coating specified in the grain-oriented electrical steel sheet of the present invention contains a combination of at least one each of the C group elements and the D group elements. In the above-mentioned primary coating, the above-mentioned effect is more significantly exhibited by satisfying the following: the total of at least one selected from the C group elements: 0.01% or more, and the total of at least one selected from the D group elements: 0.01% or more. (However, as mentioned above, the total of the X group elements is 0.50% or less.) If either or both of the C group elements and the D group elements are less than 0.01%, the effect cannot be obtained. For each of the C group and the D group, 0.02 to 0.20% is preferable, and 0.03 to 0.15% is more preferable. The total of the C group elements and the total of the D group elements do not need to be the same amount, but if the total content of the X group elements is constant, the effect will be more significant by making the contents approximately the same. The term "same degree" means that the amount of one type of element is 0.5 to 1.5 times, more preferably 0.8 to 1.2 times, the amount of the other type of element.

[0053] Furthermore, the primary coating may contain B group elements. However, B group elements are unlikely to remain in the primary coating that is fixed to the base steel sheet due to evaporation during purification annealing. This is believed to be due to the high vapor pressure of B group elements. For this reason, the content of B group elements in the analysis of the primary coating is often below the detection limit, i.e., zero, but they may be detected in small amounts. In this case, the detected amount is 0.005% or less in total of one or more B group elements, but this detection can be said to be evidence that B group elements were used as inhibitor reinforcing elements in the manufacturing process, and this is considered as one of the features of the present invention.

[0054] Furthermore, the primary coating contains at least one element selected from the group consisting of Ca, Sr, Ba, Ce, Pr, Eu, and Gd in a total amount of 0.02 to 0.50%. Hereinafter, in this specification, Ca, Sr, Ba, Ce, Pr, Eu, and Gd may be collectively referred to as "Y group elements". By containing the Y group elements in the primary coating in the above range, the coating adhesion of the grain-oriented electrical steel sheet is improved. The reason for this is not clear, but is thought to be as follows.

[0055] First, the reason why the coating adhesion is insufficient in steel sheets containing X group elements, which are the subject of the present invention, will be explained. As mentioned above, X group elements are elements that tend to segregate at grain boundaries, but such segregation also occurs at the interface between the steel sheet and the primary coating in the process of forming the primary coating on the steel sheet surface in the manufacturing process of grain-oriented electrical steel sheets. When the X group elements are concentrated as single elements at the interface and dissolve in the oxide layer, the melting point of the primary coating, which is an oxide, is significantly lowered. As a result, the interface unevenness disappears in the process of forming the primary coating, and the anchor effect due to the interface unevenness, which is generally the main factor in the adhesion between the base steel sheet and the coating, comes into play, and the adhesion is reduced.

[0056] In steel sheets in such a situation, the presence of Y group elements improves coating adhesion, and the reason for this is believed to be as follows. Y group elements have a stronger tendency to form more stable sulfides than MnS, preventing Mn from forming compounds as sulfides. As a result, Mn forms compounds with X group elements. Alternatively, Y group elements exist as compounds with X group elements. Therefore, even if X group elements segregate at the interface between the base steel sheet and the primary coating, they do not dissolve in the oxide layer, preventing the disappearance of interface irregularities and suppressing adverse effects on coating adhesion. If the content is 0.02% or less, the effect is not exerted, and if it is 0.50% or more, the irregularities at the interface between the coating and the base steel develop too much, deteriorating the magnetic properties. Here, in the case where sulfides are rendered most harmless (in other words, Y group elements form sulfides that are more stable than MnS, and Mn and X group elements form compounds, thereby suppressing the adverse effects of X group elements on coating adhesion), Y group elements are concentrated in the same region of sheet thickness depth as S and Se. If the difference between the depth of Y group elements and the depths of S and Se is ±1.5 μm or less, the Y group elements form sulfides that are difficult to decompose in the steel, and the effect of improving coating adhesion is fully exerted. When checking the above state, from the viewpoint of facilitating measurement, it may be confirmed that the difference between the depth in the sheet thickness direction of the element with the greatest content among the Y group elements (Ca, Sr, Ba, Ce, Pr, Eu, and Gd) and the depth in the sheet thickness direction of the element with the greatest content among the elements selected from the group consisting of S and Se is within a range of ±1.5 μm.

[0057] It should be noted here that the method of adding the Y group element is important. For example, it is possible to add the Y group element to the slab, which is the material, and then have the Y group element contained in the primary coating after the manufacturing process. However, since the steel sheet of the present invention is designed to reduce the hot ductility and improve the magnetic properties by making the X group element cooperate with the B group element as described above, it is not preferable for the X group element to form a compound with Mn or the Y group element in the entire steel material. For this reason, it is preferable to add the Y group element to the annealing separator so that the above-mentioned action occurs only in the region near the interface between the base steel sheet and the primary coating. This will be described later in relation to the manufacturing method.

[0058] The above-mentioned primary coating is formed on the surface of the base steel sheet. The present invention covers not only both sides of the base steel sheet, but also cases where the primary coating is formed on only one side. In addition, the entire surface does not need to be covered, and partial coverage is also covered by the present invention.

[0059] It should be noted that even if the primary coating is formed after the final annealing, it can be completely removed by subsequent treatment, for example, chemical treatment such as grinding or pickling. In other words, even if a grain-oriented electrical steel sheet is manufactured using the slab and manufacturing method of the present invention and enjoys the effects of the present invention, if the primary coating formed after the final annealing is completely removed, the grain-oriented electrical steel sheet will be outside the scope of the present invention. In this respect, the present invention as a grain-oriented electrical steel sheet is not fully prepared to exercise rights to a steel sheet that enjoys the effects of the present invention. However, looking at this from the other side, if the primary coating defined by the present invention is formed (remains) even on a part of the base steel sheet, it is also the basis for making it possible to judge that the steel sheet is within the scope of the present invention and enjoys the effects of the present invention.

[0060] (Manufacturing method) Next, the production method of the present invention will be described.

[0061] The present invention relates to a ferroelectric material containing 2.5 to 4.5% Si, 0.02 to 0.10% C, 0.01 to 0.05% acid-soluble Al, 0.003 to 0.02% N, 0.003 to 0.02% S+0.4·Se, 0.003 to 0.04% Mn, 0.04 to 0.20% Mn, and 0.0005 to 0.05% in total of at least one of Bi and Pb, and further, a mixture of at least two of Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt, and Hg. The method is characterized in that a slab containing 0.001 to 0.500% in total of Cu, with the balance being Fe and unavoidable impurities, is heated to 1000 to 1450°C, hot-rolled to form a hot-rolled sheet, annealed, and then pickled, followed by cold rolling once or twice with annealing in between to form a cold-rolled sheet, which is then subjected to decarburization annealing, and if necessary, nitriding treatment is performed during or after the annealing, followed by coating with a predetermined annealing separator and final annealing.

[0062] In this manufacturing method, the conditions are similar to known conditions and do not require special conditions, except that the slab contains B group elements and X group elements under specified conditions, and the annealing separator contains Y group elements under specified conditions. The following description will be given on this premise.

[0063] Slabs of the above chemistry can be produced by conventional melting and casting methods.

[0064] Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt and Hg are elements that are difficult to dissolve in Fe. However, for example, by adding each metal while stirring molten steel, it is possible to produce a slab containing Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt and Hg: 0.001 to 0.500%.

[0065] In order to dissolve the inhibitor constituent elements in the steel matrix, the cast slab is heated to 1000 to 1450°C. If a nitriding process is performed in a later step to introduce AlN (inhibitor), it is known that the heating temperature of the slab can be less than 1250°C.

[0066] The conditions in the steps following slab heating may be ordinary conditions.

[0067] The heated slab is hot-rolled to produce a hot-rolled sheet. The thickness of the hot-rolled sheet is not particularly limited, but is usually 1.8 to 3.5 mm in relation to the reduction ratio of the subsequent cold rolling. The hot-rolled sheet is usually annealed at 750 to 1200°C for 30 seconds to 10 minutes, pickled, and then cold-rolled.

[0068] Cold rolling is performed once, or twice with annealing in between. One cold rolling means performing cold rolling once or multiple times without annealing in between. In either cold rolling, the final reduction is preferably 80 to 95%.

[0069] When cold rolling is carried out in two steps with annealing in between, the annealing is preferably carried out at 750 to 1200° C. for 30 seconds to 10 minutes.

[0070] If cold rolling is performed once, the magnetic properties of the electrical steel sheet tend to be non-uniform in the width direction and length direction. If cold rolling is performed twice, the magnetic properties become uniform, but the magnetic flux density tends to decrease. The number of cold rolling steps is appropriately selected taking into consideration the desired magnetic properties and production costs.

[0071] After cold rolling, the cold-rolled sheet is subjected to decarburization annealing, which is usually performed at 800 to 900°C in a moist atmosphere containing hydrogen and nitrogen, to reduce the C content to 0.002% or less.

[0072] The heating rate in the decarburization annealing is preferably 80°C / s or more. This is because iron loss decreases at a heating rate of 80°C / s or more. There is no particular upper limit, but a rate of 200°C / s will be sufficient to achieve the desired effect.

[0073] When the slab is heated at less than 1250° C. and nitriding is performed during or after the decarburization annealing, the nitriding is performed in an atmosphere containing a gas having nitriding ability, such as ammonia.

[0074] After decarburization annealing or nitriding treatment, the steel sheet is coated with an annealing separator mainly composed of MgO, and then subjected to finish annealing. In the present invention, the annealing separator used in the finish annealing step contains magnesium oxide powder and additives. Magnesium oxide powder is the main component of the annealing separator, and the "main component" refers to a component that is contained in a certain substance (e.g., the annealing separator) at 50% or more, preferably 70% or more, and more preferably 80% or more. The amount of the annealing separator attached to the steel sheet is, for example, 2 g / m per side. 2 More than 10g / m 2 The amount of the annealing separator attached to the steel sheet is preferably 2 g / m or less. 2 If the amount of the annealing separator attached to the steel sheet is less than 10 g / m, the steel sheets will stick to each other during the final annealing, which is not preferable. 2 When the thickness exceeds 100 nm, the production cost increases, which is not preferable. The annealing separator may be applied by electrostatic application instead of by application of an aqueous slurry. The magnesium oxide powder is a powder whose main component is MgO and contains at least one metal (Y group element) selected from the group consisting of Ca, Sr, Ba, Ce, Pr, Eu, and Gd as an impurity, and the total content of the metals is in the range of 0.02 to 0.8% of the amount of Mg present in the magnesium oxide powder. less than On the other hand, if the content exceeds 0.8%, sulfides are formed at the interface between the steel sheet and the coating, accelerating the decomposition of the inhibitor, resulting in poor magnetic properties. The additives are compounds containing at least one Y group element, and the total amount of the additives is 0.2 to 5.0% relative to the amount of Mg present in the annealing separator. less than In this case, the coating adhesion improvement effect is not obtained, and the Super This would excessively promote the forsterite formation reaction, slowing down the decomposition of the inhibitor and resulting in the generation of fine grains, making it impossible to obtain stable magnetic properties. The ratio of the total amount of the Y group elements present in the magnesium oxide powder to the total amount of the Y group elements present in the entire annealing separator is 0.05 to 0.66. less than If the ratio is 0.66, the reaction of MgO is not sufficiently promoted, the decomposition of the inhibitor is slowed down, fine grains are generated, and the magnetic properties cannot be stably obtained. Super Otherwise, too much film will be formed, resulting in deterioration of the magnetic properties.

[0075] Finishing annealing is done on {110} <001> This is a process for secondary recrystallization of crystal grains in the oriented direction, and is an important process for increasing magnetic flux density. Usually, secondary recrystallization occurs in the process of heating to 1100-1200°C in a mixed atmosphere of nitrogen and hydrogen, and then the atmosphere is switched to a hydrogen atmosphere and annealing is performed at 1100-1200°C for about 20 hours. This annealing is generally called purification annealing, and it removes N, S, Se, etc. from the steel sheet to improve the magnetic properties.

[0076] From the viewpoints of stable progress of secondary recrystallization and improvement of magnetic flux density, the average heating rate in the final annealing is preferably slow, but from the viewpoint of productivity, it is preferably 3° C. / h or more, and more preferably 5 to 20° C. / h.

[0077] The rate of temperature rise up to 750° C. is not particularly limited, but is usually 15 to 100° C. / h, and from the viewpoint of productivity, a faster rate is more preferable.

[0078] After the finish annealing, a coating liquid containing, for example, aluminum phosphate and colloidal silica as main components is applied to the steel sheet and baked to form an insulating coating.

[0079] (Chemical composition measurement)

[0080] The composition of the base steel sheet is measured by immersing it in hot alkali or acid to remove the insulating coating and primary coating that form on the product steel sheet, and then using an appropriate analytical method such as ICP-MS or NDIR.

[0081] Furthermore, the components of the primary coating are determined by immersing the steel sheet in hot alkali to remove the insulating coating formed on the product steel sheet, or by electrolyzing the steel sheet with the primary coating in an acetylacetone-based electrolyte before the insulating coating is applied, extracting the primary coating as an electrolytic residue, and measuring it by XRF to measure the amounts of Bi, Pb, Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt, and Hg, as well as Ca, Sr, Ba, Ce, Pr, Eu, and Gd, in mass %, when the weight of the primary coating is taken as 100%.

[0082] (Measurement of the thickness depth position of a specific component) The position of concentration of a specific component in the coating of the base steel sheet is measured by immersing the sheet in hot alkali to remove the insulating coating formed on the product steel sheet, or by performing a GDS analysis on the steel sheet with the primary coating before the application of the insulating coating, and identifying the position of the highest luminescence intensity of the specific component element of interest. However, the area within 0.05 μm from the surface is excluded because it is the remains of the annealing separator or insulating coating that could not be removed by pickling, and the position of the highest luminescence intensity located more than 0.05 μm deep from the surface is adopted. EXAMPLES

[0083] Next, an embodiment of the present invention will be described, but the conditions in the embodiment are merely an example of conditions adopted to confirm the feasibility and effects of the present invention, and the present invention is not limited to this example of conditions. Various conditions can be adopted in the present invention as long as they do not deviate from the gist of the present invention and the object of the present invention is achieved. In the tables below, "-" denotes an element that is not intentionally added and indicates that no measurement was performed. It does not exclude the inclusion of the element at the level of unavoidable impurities. In addition, even if an element is intentionally added to a material, if the amount is below the detection limit due to purification during the manufacturing process, the value is indicated by "<".

[0084] Example 1 In a vacuum melting furnace, slabs were produced containing, by mass%, 0.09% C, 3.1% Si, 0.03% Al, 0.01% N, 0.03% S, 0.08% Mn, 0.2-0.3% Cu, Sn, Sb, and various amounts of added Bi, Pb, Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt, and Hg. The chemical composition is shown in Table 1. The slabs were hot-rolled at 1350°C for 1 hour to produce hot-rolled sheets with a thickness of 2.0 mm.

[0085] The hot-rolled sheet was annealed at 1080°C for 120 seconds, then pickled and cold-rolled to a thickness of 0.23 mm. The cold-rolled sheet was decarburized at 840°C for 110 seconds in a hydrogen-containing moist atmosphere at a heating rate of 300°C / s, and then coated with the annealing separator shown in Table 2 as a water slurry, followed by finish annealing at 1200°C for 20 hours.

[0086] After the final annealing, the steel sheet was washed with water and then sheared to a single sheet size for magnetic measurement. A coating solution containing aluminum phosphate and colloidal silica as main components was applied and baked to produce a grain-oriented electrical steel sheet with an insulating coating.

[0087] The magnetic flux density B8 of the produced grain-oriented electrical steel sheets was measured. B8 is the magnetic flux density at a magnetizing force of 800A / m, and was evaluated using a single sheet with a width of 60mm and a length of 300mm. Five single sheets were prepared for each soluble component, and B8 was measured. Of the five B8 measurements, the highest value was taken as B8max, and the lowest value was taken as B8min, with the difference between them being taken as ΔB8, which was used as an index showing the range of variation in magnetic properties.

[0088] The hot rollability was evaluated by visually observing the edge of the hot rolled sheet and classifying it into the following three levels according to the frequency of cracks. Good: When the edge of a hot-rolled sheet (widthwise end) is visually observed over a 1000 mm stretch in the rolling direction, the number of cracks measuring 20 mm or more in the widthwise direction is one or less. Acceptable: The edge (widthwise end) of a hot-rolled sheet is visually observed over a 1000mm stretch in the rolling direction, and there are two or more cracks with a length of 20mm or more in the widthwise direction. Crack: Breaking during hot rolling The cracks referred to here are those that occur on the edges of the steel plate and penetrate the plate thickness. The length of the crack in the plate width direction is the length in the plate width direction at the portion that penetrates the plate thickness.

[0089] The measurement results are shown in Table 3. When the slab contains one or more of the specified Bi and Pb, the index ΔB8 indicating the fluctuation range of the magnetic properties becomes smaller as the amount of Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt and Hg increases. In particular, samples 7 to 13, 15, 16, 19 and 20, which are added in a total of 0.001% or more by combining one or more elements from the group consisting of Te, In, Cd, Zn and Ga and the group consisting of Au, Ag, Pd, Pt and Hg, have ΔB8<0.04T, indicating that the effect of adding Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt and Hg is large. In addition, in the case of sample number 17, in which the amount of Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt and Hg in the slab exceeded 0.500%, and in the case of sample numbers 24, 25, 27 to 30, and 32 to 41, in which only one of Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt and Hg was added, the hot ductility was inferior.

[0090] The analysis results of the primary coating of each sample are shown in Table 4. When the slab contained two or more X group elements with a total content of 0.001-0.500%, the amounts of Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt, and Hg in the coating were within the range.

[0091] [Table 1]

[0092] [Table 2]

[0093] Here, the ratio R of the abundance of Y group elements as impurity elements in the magnesium oxide powder is Y , the ratio R' of the amount of additives present in the annealing separator Y The ratio is calculated as follows: The concentration (%) of Y group elements contained as impurities in magnesium oxide powder is W Y , the concentration (%) of impurity elements other than Y group elements is W X Then, the amount of Mg present per unit weight of the magnesium oxide powder is X Mg (mol / g) and the amount of Y present per unit weight of the magnesium oxide powder, X Y (mol / g) is X Mg =(100-W Y -W X ) / 100 / MgO molecular weight =(100-W Y -W X ) / 100 / (atomic weight of Mg + atomic weight of O) X Y =W Y / 100 / (Atomic weight of Y group elements) and The ratio R of the amount of Y group elements present to the amount of Mg present in the magnesium oxide powder Y (%)teeth, R Y =(X Y / X Mg )·100 It is. However, if the magnesium oxide powder contains two or more Y group elements as impurities, the same procedure as above is used to determine the X for each of the Y group elements. Y The sum of these values ​​is calculated as ΣX Y Using R Y =(ΣX Y / X Mg )·100 Let us assume that. In addition, the stoichiometric coefficient of the Y group element in the Y group element compound molecule added to the annealing separator prepared using the magnesium oxide powder as the main component is Z, and the addition ratio (%) of the Y group element compound to the magnesium oxide powder is A. Y Then, the amount of Y group element present in the additive in the annealing separator consisting of unit weight of magnesium oxide powder and additives added to unit weight of magnesium oxide powder is X' Y teeth, X' Y =(A Y / 100) Z / (Molecular weight of Y group element compound) and The ratio R' of the content of the Y group element in the additive to the amount of Mg present in the magnesium oxide in the annealing separator Y teeth, R' Y =(X' Y / X Mg )·100 It is. However, if the additive contains two or more types of Y group elements or two or more types of additives, the same procedure as above is used to determine X' for all Y group elements contained in all additives. Y The sum of these values ​​is calculated as ΣX'. Y Using R' Y =(ΣX' Y / X Mg )·100 It is. The ratio of the total amount of the Y group elements present in the magnesium oxide powder to the total amount of the Y group elements present in the annealing separator is: X Y / (X' Y +XY ) ={(X Y / X Mg )·100} / {(X' Y / X Mg )·100+(X Y / X Mg )·100}=R Y / (R' Y +R Y ) It is expressed as: [Table 3] [Table 4]

[0094] Example 2 In a vacuum melting furnace, slabs were produced containing, by mass%, C: 0.09%, Si: 3.1%, Al: 0.03%, N: 0.01%, S+0.4Se: 0.03%, Mn: 0.08%, Sn: 0.1 or 0.3%, Bi, Pb, and Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt, and Hg. The chemical composition is shown in Table 5. The slabs were hot-rolled at 1350°C for 1 hour to produce hot-rolled sheets with a thickness of 2.0 mm.

[0095] The hot-rolled sheet was annealed at 1080°C for 120 seconds, then pickled and cold-rolled to a thickness of 0.23 mm. The cold-rolled sheet was decarburized at 840°C for 110 seconds in a hydrogen-containing moist atmosphere at a heating rate of 300°C / s, and then coated with an annealing separator mainly composed of magnesium oxide powder shown in Table 6 as a water slurry, followed by finish annealing at 1200°C for 20 hours.

[0096] After the final annealing, the steel sheet was washed with water and then sheared to a single sheet size for magnetic measurement. A coating solution containing aluminum phosphate and colloidal silica as main components was applied and baked to produce a grain-oriented electrical steel sheet with an insulating coating.

[0097] The magnetic flux density B8 of the produced grain-oriented electrical steel sheets was measured. B8 is the magnetic flux density at a magnetizing force of 800A / m, and was evaluated using a single sheet with a width of 60mm and a length of 300mm. Five single sheets were prepared for each soluble component, and B8 was measured. Of the five B8 measurements, the highest value was taken as B8max, and the lowest value was taken as B8min, with the difference between them being taken as ΔB8, which was used as an index showing the range of variation in magnetic properties.

[0098] The hot rollability was evaluated by visually observing the edge of the hot rolled sheet and classifying it into the following three levels according to the frequency of cracks. Good: When the edge of a hot-rolled sheet (widthwise end) is visually observed over a 1000 mm stretch in the rolling direction, the number of cracks measuring 20 mm or more in the widthwise direction is one or less. Acceptable: The edge (widthwise end) of a hot-rolled sheet is visually observed over a 1000mm stretch in the rolling direction, and there are two or more cracks with a length of 20mm or more in the widthwise direction. Crack: Breaking during hot rolling The cracks referred to here are those that occur on the edges of the steel plate and penetrate the plate thickness. The length of the crack in the plate width direction is the length in the plate width direction at the portion that penetrates the plate thickness.

[0099] The measurement results are shown in Table 7. Samples 9 to 14, which were added in a total of 0.001% or more from the group consisting of Te, In, Cd, Zn, and Ga, and the group consisting of Au, Ag, Pd, Pt, and Hg, had ΔB8<0.04T, indicating that the effect of adding Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt, and Hg was large. In the case of samples 25 to 34, which were added with only one of Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt, and Hg, the hot ductility was inferior. In the case of samples 7, 8, 19, and 20, which used slurries 15 and 16, in which the ratio of the amount of Y group elements in the impurities in the magnesium oxide powder to the amount of Y group elements in the additives in the slurry components was outside the range, the rust resistance was inferior. In addition, in the case of samples 15 and 16 using slurries 11 and 12 in which the amounts of Y-group elements present in the magnesium oxide powder impurities were outside the range, the rust resistance was inferior. In the case of samples 17 and 18 using slurries 13 and 14 in which the amounts of Y-group elements present in the annealing separator additives were outside the range, the rust resistance was inferior.

[0100] The analysis results of the primary coating of each sample are shown in Table 8. When the slab contained two or more X group elements with a total content of 0.001-0.500%, the amounts of Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt, and Hg in the coating were within the range.

[0101] [Table 5] [Table 6]

[0102] [Table 7] [Table 8]

[0103] Example 3 In a vacuum melting furnace, slabs containing, by mass%, C: 0.09%, Si: 3.5%, Al: 0.03%, N: 0.01%, S + 0.4Se: 0.009%, Mn: 0.08%, Bi: 0.0030%, and two or more elements selected from Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt, and Hg were produced in a range of 0.001 to 0.05%. The chemical composition is shown in Table 9. The slabs were hot-rolled at 1150°C for 1 hour to produce hot-rolled sheets with a thickness of 2.0 mm.

[0104] The hot-rolled sheet was annealed at 1050°C for 120 seconds, then pickled and cold-rolled to a thickness of 0.23 mm. The cold-rolled sheet was decarburized at 850°C for 120 seconds in a hydrogen-containing moist atmosphere at a heating rate of 100°C / s, and then annealed at 750°C for 60 seconds in an ammonia-containing atmosphere to increase the nitrogen content in the steel.

[0105] The annealed cold-rolled sheet was mixed with pure water and stirred to prepare a water slurry, the water slurry being composed mainly of magnesium oxide powder containing 0.2% Ca as an impurity element, with 2.0% calcium sulfate hemihydrate added as an additive relative to the weight of the magnesium oxide powder, and 5.0% TiO2 added as an additive relative to the weight of the magnesium oxide powder. The water slurry was then applied to the front and back surfaces of the steel sheet and dried. At this time, the magnesium oxide powder contained Ca as an impurity element at an abundance ratio of 0.20% relative to the amount of Mg present in the magnesium oxide powder, The annealing separator contains an amount of Ca contained in additives other than the magnesium oxide powder in an amount of 0.56% relative to the amount of Mg contained in the magnesium oxide powder in the annealing separator, Furthermore, the ratio of Ca as an impurity element in the magnesium oxide powder in the annealing separator to the total amount of Ca in the annealing separator is 0.26. This was followed by a final annealing at 1200°C for 20 hours. After the final annealing, the steel sheets were washed with water and then sheared to a single sheet size for magnetic measurement. A coating solution containing aluminum phosphate and colloidal silica as main components was applied and baked to produce grain-oriented electrical steel sheets with an insulating coating.

[0106] The measurement results are shown in Table 10. The definitions or evaluations of B8max, B8min, ΔB8, and hot ductility are the same as those in Example 1. With an increase in the amount of Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt, and Hg, the index ΔB8 indicating the fluctuation range of the magnetic properties generally becomes smaller. In particular, samples 7 to 11, which are made by combining one or more elements from the group consisting of Te, In, Cd, Zn, and Ga and the group consisting of Au, Ag, Pd, Pt, and Hg, and adding a total of 0.001% or more, have ΔB8≦0.017T and good hot ductility, which shows that the effect of adding Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt, and Hg is large.

[0107] The analysis results of the primary coating of each sample are shown in Table 11. Samples 1 to 11, in which Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt and Hg were added to the slab in the range of 0.001 to 0.05%, showed that the effect of adding Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt and Hg was remarkable, and the amounts of Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt and Hg in the coating were within the range.

[0108] [Table 9]

[0109] [Table 10]

[0110] [Table 11] [Industrial Applicability]

[0111] According to the present invention, grain-oriented electrical steel sheets having good magnetic properties and good coating adhesion can be stably produced on an industrial scale, and therefore the present invention has great applicability in the electrical steel sheet manufacturing industry.

Claims

1. In mass%, Si: 2.5 to 4.5%, C: 0.02 to 0.10%, acid-soluble Al: 0.01 to 0.05%, N: 0.003 to 0.02%, S+0.4·Se: 0.003 to 0.04%, Mn: 0.04 to 0.20%, the total of one or more of Bi and Pb: 0.0005 to 0.05%, and further the group consisting of Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt, and Hg. A slab containing at least two or more selected from the above: 0.001 to 0.240% in total, with the balance being Fe and impurities, is heated to 1000 to 1450 ° C., hot-rolled to form a hot-rolled sheet, annealed, pickled, and then cold-rolled once or twice with annealing between them to form a cold-rolled sheet, and the cold-rolled sheet is subjected to decarburization annealing, and if necessary, nitriding treatment is performed during or after the annealing, and then An annealing separator containing magnesium oxide powder as a main component, The magnesium oxide powder of the annealing separator contains, as an impurity element, at least one element selected from the group consisting of Ca, Sr, Ba, Ce, Pr, Eu, and Gd in a total abundance ratio of 0.02 to 0.8% relative to the abundance of Mg in the magnesium oxide powder, The annealing separator further contains, in addition to the magnesium oxide powder, an additive containing at least one element selected from the group consisting of Ca, Sr, Ba, Ce, Pr, Eu, and Gd, such that the total amount of each element is in an abundance ratio of 0.2 to 5.0% relative to the amount of Mg contained in the annealing separator, Further, an annealing separator in which the ratio of the total amount of Ca, Sr, Ba, Ce, Pr, Eu, and Gd as impurity elements in the magnesium oxide powder in the annealing separator to the total amount of Ca, Sr, Ba, Ce, Pr, Eu, and Gd in the annealing separator is 0.02 to 0.66 is applied to the front and back surfaces of a steel sheet and dried, A method for producing a grain-oriented electrical steel sheet, comprising the steps of:

2. 2. The method for producing a grain-oriented electrical steel sheet according to claim 1, wherein the slab contains a total of at least one selected from the group consisting of Te, In, Cd, Zn, and Ga: 0.0005% or more, and a total of at least one selected from the group consisting of Au, Ag, Pd, Pt, and Hg: 0.0005% or more.

3. A grain-oriented electrical steel sheet comprising: a base steel sheet containing, by mass%, 2.5 to 4.5% Si, 0.04 to 0.20% Mn, with the balance being Fe and unavoidable impurities; and a coating mainly composed of forsterite, present on a surface of the base steel sheet, containing, by mass%, the following: a total of at least two or more elements selected from the group consisting of Te, In, Cd, Zn, Ga, Au, Ag, Pd, Pt, and Hg: 0.02 to 0.50%, a total of at least one or more elements selected from the group consisting of Ca, Sr, Ba, Ce, Pr, Eu, and Gd: 0.02 to 0.50%, and a total of one or more elements of Bi and Pb: 0.005% or less.

4. On the surface of the base steel plate, 4. The grain-oriented electrical steel sheet according to claim 3, further comprising a coating mainly composed of forsterite, which contains at least one element selected from the group consisting of Te, In, Cd, Zn, and Ga in a total amount of 0.01% or more, and at least one element selected from the group consisting of Au, Ag, Pd, Pt, and Hg in a total amount of 0.01% or more.

5. On the surface of the base steel plate, 5. The grain-oriented electrical steel sheet according to claim 3, wherein a coating mainly composed of forsterite is present, in which the difference between the depth in the sheet thickness direction of the element having the maximum content selected from the group consisting of Ca, Sr, Ba, Ce, Pr, Eu, and Gd and the depth in the sheet thickness direction of the element having the maximum content selected from the group consisting of S and Se is within a range of ±1.5 μm.

Citation Information

Patent Citations

  • JP1962-009305B

  • JP1965-015644B

  • hifunsaibutsushitsuofunsaisurutamenoshindomiru

    JP1976013469A

  • Video signal processing circuit

    JP1987045285A

  • Production of grain-oriented electrical steel sheet having excellent magnetic characteristic and film characteristic

    JP1990077525A