Method for evaluating carbonaceous materials for sintering and method for producing sintered ore

By evaluating carbonaceous materials using CO2 to measure the BET specific surface area within a specified range, the method addresses the challenge of inconsistent combustibility and NOx emissions, enhancing sintered ore production and reducing emissions effectively.

JP7564446B2Active Publication Date: 2024-10-09NIPPON STEEL CORPORATION
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021025943
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-22
Publication Date
2024-10-09
Estimated Expiration
2041-02-22

AI Technical Summary

Technical Problem

Existing methods for evaluating carbonaceous materials for sintering, such as char, fail to accurately measure the specific surface area of micropores, leading to inconsistent combustibility and NOx emissions, and there is a need for a method that can increase sintered ore production while reducing NOx emissions.

Method used

A method for evaluating carbonaceous materials using CO2 as the adsorbed gas to measure the BET specific surface area, ensuring the char has a specific surface area within the range of 200 to 450 m2/g, which is used as a solid fuel in the sintering process.

Benefits of technology

This method allows for increased production of sintered ore and reduced NOx emissions by maintaining an appropriate combustion state during the sintering process, balancing productivity and yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564446000001
    Figure 0007564446000001
  • Figure 0007564446000002
    Figure 0007564446000002
  • Figure 0007564446000003
    Figure 0007564446000003
Patent Text Reader

Abstract

To achieve increased production of sintered ore and small amounts of NOx emission in a sintering process using a new carbonaceous material for sintering.SOLUTION: The present invention discloses an evaluation method for carbonaceous materials for sintering, using a new carbonaceous material for sintering, and a sintered ore production method using the evaluation method. For char to be used as a carbonaceous material, its specific surface area is measured using CO2 as an adsorption gas, and its suitability as solid fuel is evaluated on the basis of the specific surface area.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for evaluating a carbonaceous material for sintering and a method for producing sintered ore. [Background technology]

[0002] In the sintering process, new raw materials for sintering are made up of iron ore (fine iron ore), miscellaneous iron-containing raw materials such as undersize powder, dust, and mill scale generated inside and outside the sintering plant, and slag-forming materials (auxiliary raw materials) such as limestone. The new raw materials are mixed with sintering carbon (agglomeration material), which is the fuel (solid fuel) for sintering (agglomerating) the sintered ore, and return ore to make a blended raw material. Return ore is sintered ore that does not meet the product particle size requirements, and is circulated in the sintering process to be sintered again.

[0003] In the currently commonly used sintering process using the Dwight Lloyd (DL) sintering machine, the pressure below the packed bed of the above-mentioned raw materials is negative, and air is drawn from above to below to combust the coagulants in the raw materials. The heat of combustion generated by the combustion of the coagulants is used to sinter the raw materials, producing agglomerated sintered ore. This sintered ore is used as the main raw material in the blast furnace. Conventionally, coke breeze has been mainly used as the coking material. Coke breeze is a specific particle size (e.g., particle size 0.5 to 3 mm) of coke produced and crushed in a coke oven that falls under the sieve. Compared to the granulated coke that is used in blast furnaces, the amount of coke breeze that falls under the sieve is small, and the amount of coke for sintered ore production is insufficient. For this reason, anthracite, which has a low volatile content, has also been used as a carbon material, but anthracite reserves are becoming depleted.

[0004] As an alternative fuel to coke powder and anthracite, it is possible to use coal (low-grade coal) such as lignite, subbituminous coal, and high-volatile bituminous coal as sintering materials. However, these coals have a high volatile matter content of 20 to 50%. If used as is, the volatile matter in the coal evaporates and gas containing volatile organic compounds (such as tar) is generated. The volatile organic compounds are not completely burned in the sintering bed and move in the exhaust gas and are discharged. Therefore, there is a risk that the exhaust gas blower will malfunction due to the adhesion of volatile organic compounds, and the exhaust gas discharged from the chimney to the outside of the sintering equipment will pollute the air (not meet the emission standards). Therefore, in order to use these coals as sintering materials, it is necessary to reduce the volatile matter content by performing a heat treatment (carbonization treatment) in advance to char them.

[0005] Here, since char generally has a high combustion rate, it is expected to have the effect of accelerating the sintering rate and increasing productivity in the sintered ore manufacturing process. On the other hand, it is also necessary to consider the effect of the increased sintering rate on the sinter yield.

[0006] In addition, in the sintered ore manufacturing process at steelworks, nitrogen oxides (NOx) are generated by the combustion of carbonaceous materials used as fuel and are discharged as exhaust gas. Reducing NOx emissions is an important issue in improving air pollution. Char generally has a large specific surface area per unit weight, so it is expected to be effective in reducing the amount of NOx generated.

[0007] As described above, char is expected to serve as an alternative fuel to coke breeze and anthracite in the sintered ore manufacturing process, but it is necessary to evaluate its impact on productivity and on nitrogen oxides (NOx) in the exhaust gas.

[0008] In the sintering process, the porosity and specific surface area of ​​the carbonaceous material are important factors related to the combustibility of the carbonaceous material itself and the permeability of the packed bed. There are various methods for measuring porosity, such as a method using a mercury porosimeter and a gas adsorption method that measures the amount of adsorbed gas. The range of pore sizes that can be measured varies depending on the measurement method.

[0009] Patent Document 1 describes the limitation of char by a parameter of a certain porosity as one of the indicators of suitable carbonaceous materials to be used as fuel for iron ore sintering. Here, a mercury porosimeter is used to measure the porosity, and the range of porosity is specified, on the assumption that pores of 0.1 microns or less are not a factor that determines combustibility.

[0010] Non-Patent Documents 1 and 2 report that when measuring the specific surface area of ​​a substance having micropores such as activated carbon using a gas adsorption method, N2 may result in an underestimate, and CO2 is more suitable as an adsorption gas. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] International Publication No. 2010 / 087468 [Non-patent literature]

[0012] [Non-Patent Document 1] Om P.Mahajan, Carbon,29(6),pp735-742,1991. [Non-Patent Document 2] D. Cazorla-Amoros, Langmuir,1996, 12, 2820-2824, 1996. Summary of the Invention [Problem to be solved by the invention]

[0013] The properties of char vary greatly depending on the raw materials, the mixing ratio of raw materials, the manufacturing method (manufacturing equipment), and manufacturing conditions (temperature, residence time, atmospheric gas, etc.).As a result, even if a part or all of the conventionally used sintering carbonaceous material (coke fines, anthracite) is replaced with char with the same particle size, calorific value, amount of fixed carbon in the carbonaceous material, etc. during the production of sintered ore, the combustibility in the sintering process changes greatly depending on the properties of the char used.

[0014] In the sintering process, as described above, porosity and specific surface area per unit weight are important as indicators of char properties. In Patent Document 1, pores of 0.1 microns or less are not a factor that determines combustibility, and porosity is specified based on the pore range measured by a mercury porosimeter. However, since pores of 0.1 microns or less are not considered, there are still issues to be addressed in the evaluation of char used in the sintering process. In addition, Non-Patent Documents 1 and 2 do not evaluate the specific surface area of ​​sintering carbonaceous materials using CO2 as the adsorbed gas, much less mention the relationship between the specific surface area and sintered ore productivity or NOx conversion rate.

[0015] The inventors have conventionally measured the specific surface area by N2 gas adsorption and evaluated char based on the measured value. However, it is difficult to measure extremely fine pores (micropores) using the N2 gas adsorption method, and there is a problem in that the specific surface area is underestimated.

[0016] This time, the inventors measured the specific surface area of ​​chars produced from lignite, subbituminous coal, and high volatile bituminous coal using a new CO2 gas adsorption method, and conducted sintering experiments using the produced chars. As a result, they discovered that it is possible to identify carbonaceous materials (chars) that can achieve both "increased sintered ore production" and "low NOx emissions" based on the specific surface area values ​​of chars measured using the CO2 gas adsorption method. Here, the CO2 gas adsorption method is a method for measuring the specific surface area using CO2 as the adsorption gas.

[0017] The object of the present invention is to provide a method for evaluating new carbonaceous materials for sintering that can increase sintered ore production and reduce NOx emissions, and a method for producing sintered ore, for use as a raw material for sintering. [Means for solving the problem]

[0018] The gist of the present invention is as follows. (1) A method for evaluating a carbonaceous material used in a sintered ore manufacturing process, comprising measuring the specific surface area of ​​char used as the carbonaceous material using CO2 as an adsorbed gas, and evaluating its suitability as a solid fuel based on the specific surface area. (2) In the evaluation of suitability, the specific surface area of ​​the char is 200 to 450 m 2 The method for evaluating a carbonaceous material for sintering according to (1), characterized in that when the carbonaceous material for sintering has a molecular weight within the range of 0.1 to 0.25, the carbonaceous material for sintering is evaluated as having suitability as a solid fuel. (3) A method for producing sintered ore, characterized in that the suitability of char to be used as the carbonaceous material is evaluated by the evaluation method for carbonaceous material for sintering described in (1) or (2), and char having a specific surface area within a predetermined range is used as solid fuel. Effect of the Invention

[0019] By using a simple and new evaluation method for carbonaceous materials for sintering and using carbonaceous materials that are evaluated as suitable as sintering raw materials (solid fuel), it is possible to achieve "increased sintered ore production" and "low NOx emissions" in the sintering manufacturing process. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] <Measurement of specific surface area of ​​carbonaceous material> Lignite, subbituminous coal, and bituminous coal contain high volatile matter. Char produced by heating (carbonizing) these coals has fine pores due to the evaporation of the high volatile matter. This tendency is particularly noticeable for char produced from coal with a Roga index of 10 or less. Char with fine pores can be produced by using low-fluidity coal with a Roga index of 10 or less as raw coal. Note that the fluidity of coal is a property resulting from the degree to which it breaks down into smaller molecules when heated, and low-fluidity coal is coal that is less likely to break down into smaller molecules when heated.

[0021] The specific surface area measurement method is a method for calculating the specific surface area of ​​a sample (total surface area of ​​a powder per unit mass) by gas adsorption. The specific surface area of ​​a sample is measured by physical adsorption of gas on a solid surface, and is calculated by determining the amount of adsorbed gas equivalent to a monolayer on the surface. Typically, the measurement is performed at the boiling point of liquid nitrogen, and the amount of adsorbed gas is measured by a dynamic flow method or a volumetric method. Based on the relationship between the gas adsorption amount and the relative pressure, the specific surface area (BET specific surface area) is calculated from the following BET equations (1) and (2).

[0022]

number

[0023]

number

[0024] Here, the elements in the above formula are as follows: P: Measurement pressure [Pa] P0: Saturated vapor pressure of the adsorbed gas [Pa] P / P0: Relative pressure of adsorbed gas [-] Q: Adsorption amount [mol / g] Qm: Monolayer adsorption amount [mol / g] C:BET parameters [-] S: Specific surface area [m 2 / g] s: Molecular occupied cross section [nm 2 ] (N2:0.162nm 2 ,CO2:0.210nm 2 ) K A :Avogadro constant [mol -1 ]

[0025] (N2 adsorption method - conventional technology) The inventors have conventionally used the N2 adsorption method to measure the specific surface area of ​​carbonaceous materials. Using a commercially available flow-type specific surface area measuring device, N2 was adsorbed as an adsorption gas at -196°C onto a carbonaceous material sample (0.25-0.5 mm) that had been pretreated (heated at 150°C for 4 hours while evacuating to a vacuum), and the amount of N2 adsorbed at a relative pressure of 0.3 was measured. Here, the relative pressure is P / P0 in the above formula (1).

[0026] (CO2 adsorption method - this invention) The present inventors considered that when measuring the specific surface area of ​​coal char having micropores, the specific surface area would be underestimated if N2 was used as the adsorption gas, and that CO2 would be more suitable. In the present invention, the carbonaceous material for sintering is evaluated based on the value of the BET specific surface area calculated based on the measurement value by the CO2 adsorption method. Also, the carbonaceous material for sintering whose BET specific surface area value measured and calculated by the CO2 adsorption method is within a predetermined range is used as the solid fuel.

[0027] By using the CO2 adsorption method, it is possible to express the extremely fine pores (micropores) of carbonaceous materials, which could not be measured by the conventional N2 adsorption method, as an index called specific surface area. By using char with a BET specific surface area measured by the CO2 adsorption method within an appropriate range as the carbonaceous material for sintering (fixed fuel), it is possible to maintain an appropriate combustion state in the sintering process, and it is possible to increase the production of sintered ore (increase in FFS, and maintain or slightly decrease the yield) and achieve low NOx emissions (low NOx conversion rate). In addition, char produced from coal with a Roga index of 10 or less has particularly many developed micropores. Therefore, it is preferable to use the CO2 adsorption method rather than the conventional N2 adsorption method to measure the BET specific surface area. The Roga index is calculated by the Roga test method specified in JIS-M8801.

[0028] The BET specific surface area measured by the CO2 adsorption method is medium (200 m 2 When char with a carbon content of 1000 ppm or less (0.1 ppm or less) is used as a carbonaceous material for sintering, it is possible to increase the production of sintered ore, but it is not possible to achieve low NOx emissions. In addition, the BET specific surface area measured by the CO2 adsorption method is high (450m 2 When char with a NOx content of 1000 ppm or more (0.1 ppm or more / g) is used as the carbonaceous material for sintering, low NOx emissions can be achieved, but the FFS increases excessively, resulting in a significant decrease in yield, and an increase in sinter production cannot be achieved. EXAMPLES

[0029] The inventors produced several chars of different qualities using low-grade coals such as lignite, subbituminous coal, and high-volatility bituminous coal as raw materials, and measured the specific surface area by the CO2 adsorption method according to the present invention. In addition, using the produced several chars, sintering tests were carried out using a pot test apparatus. The following examples are provided to illustrate the details of the embodiments of the present invention.

[0030] <Char production> (Char raw material) Table 1 shows the properties of the coal used as raw material in char production. Table 1 shows the proximate analysis values, elemental analysis values, and Roga index of the coal used as raw material. Coal A is lignite, coal B and C are subbituminous coal, and coals D to G are bituminous coal.

[0031] [Table 1]

[0032] (Char properties) Table 2 shows the properties of chars (A1 to A3, B to G) produced using coals A to G shown in Table 1 as raw materials, and the properties of conventional carbonaceous materials (coke breeze, anthracite) as reference examples. The leftmost column shows the correspondence with the experimental examples (see Table 5) described later. For chars A1 to A3, B, C, D, E, F, and G, char was produced by filling each carbonaceous raw material into a reactor and then heating the electric furnace outside the reactor to a predetermined pyrolysis temperature while circulating nitrogen gas. The pyrolysis temperature for the examples (chars A1, B to E) was 700°C, while the comparative examples (chars F, G, and A3) were pyrolyzed at a temperature exceeding 700°C. For char A2, char was produced by filling coal A into a reactor and then heating the electric furnace outside the reactor to a predetermined pyrolysis temperature while circulating a mixed gas (N2: 70%, CO2: 30%). The volatile matter content of all the produced chars was less than 10%. It is possible to use char with a volatile matter content of 10% or more at a lower production temperature. However, this is not preferable because, compared with conventional carbonaceous materials (coke powder, anthracite), the amount of volatile matter-derived components (tar components) that escape unburned into the exhaust gas from the sintering machine will be greater, which may have an adverse effect on the exhaust gas blower and exhaust gas purification equipment (dust collector, desulfurization equipment, etc.).

[0033] [Table 2]

[0034] The BET specific surface area (CO2) shown in Table 2 was measured using a commercially available constant volume adsorption measurement device (constant volume specific surface area measurement device) by adsorbing CO2 as the adsorption gas at 0°C on a carbonaceous material sample (0.25-0.5 mm) that had been pretreated (heated at 150°C for 4 hours while evacuating to a vacuum) at a relative pressure (ratio of adsorption equilibrium pressure to saturated vapor pressure) of 0.012 to 0.03 (in 0.002 increments). The rightmost column shows the BET specific surface area measured by the N2 adsorption method for reference.

[0035] <Sintering experiment> The sintering pot test was used to simulate the sintering process of a packed bed of raw materials in an actual machine, and the effects of improving productivity and reducing NOx in the sintering process were confirmed. (Ingredients for pot testing) Table 3 shows the raw material mix used as the base for the pot test (Reference Example 1 in Table 5). In the case of Reference Example 1 serving as a base, as shown in Table 3 (and Reference Example 1 in Table 5), the raw materials excluding return ore and carbonaceous material were taken as 100 mass%, and the blending ratios of return ore and carbonaceous material (coke fines in Table 2) were 15.0 mass% and 4.5 mass%, respectively, with the exception of these. In the cases of Reference Example 2, Examples 1 to 6, and Comparative Examples 1 to 3, as shown in the upper part of Table 5 (type of carbonaceous material and blending amount of carbonaceous material), one of the chars (A1 to A3, B to G) and anthracite shown in Table 2 was used as the carbonaceous material. In these cases, the blending amount of carbonaceous material was determined so that the amount of fixed carbon input of the char or anthracite used was the same as that of the base (Reference Example 1) using 4.5 mass% (excluding numbers) of coke powder.

[0036] [Table 3]

[0037] The particle size distribution of the carbonaceous materials used is shown in Table 4. The particle size distribution of the carbonaceous materials was the same for all experimental examples (Reference Examples 1 to 2, Examples 1 to 6, and Comparative Examples 1 to 3). After mixing these blended raw materials, they were granulated for a specified time (5 minutes) using a drum granulator with a target moisture content of 7.5 mass % to produce blended raw materials (sintered raw materials) for the pot sintering test.

[0038] [Table 4]

[0039] (Pot test firing conditions and evaluation) The raw materials were charged into a test pot with a diameter of 300 mm so that the layer thickness was 600 mm, and air was sucked downward at a pressure of 1530 kPa.

[0040] (Pot test evaluation items) For each case, the combustion rate, product yield, productivity, NOx emissions, and NOx conversion were evaluated. Here, NOx emissions are the amount of NOx (NO+NO2) contained in the exhaust gas from the start of ignition to the end of sintering (burn-through), expressed as nitrogen weight (oxygen not included). NOx conversion is the ratio, expressed as a percentage, of the amount of nitrogen detected as NOx in the exhaust gas to the amount of nitrogen contained in the carbonaceous material used as the raw material for the pot test.

[0041] (Pot test results) The results of the lower pan test are shown in Table 5. As a result of the pot test, when chars with BET specific surface areas within the appropriate range measured by the CO2 adsorption method (Char A1, A2, B, C, D, E) were used as carbonaceous materials (solid fuel), the sintered ore production rate was improved and NOx emissions were significantly reduced compared to the reference examples (coke breeze, anthracite). In the case of Comparative Example 1 (Char F) and Comparative Example 2 (Char G), which used char with a BET specific surface area below the lower limit of the appropriate range, the productivity of sintered ore was higher than that of the Reference Example, but the NOx emissions were at the same level as the Reference Example. This is because the coals (Coal F, Coal G) that are the raw materials for Char F and Char G have a Roga index greater than 10 and have greater caking properties (softening and melting properties) than the other coals used this time, which means that fewer pores are formed during char production (carbonization), and as a result, the BET specific surface area is below the appropriate range. Furthermore, in the case of Comparative Example 3 (Char A3), in which char whose BET specific surface area was equal to or greater than the upper limit of the appropriate range was used, the NOx emissions were significantly reduced compared to the Reference Example, but the sintered ore productivity was lower than that of the Reference Example.

[0042] [Table 5]

Claims

1. A method for evaluating a carbonaceous material used in a sintered ore manufacturing method, comprising: 2 A method for evaluating a carbonaceous material for sintering, comprising measuring a specific surface area using a carbonaceous material and evaluating its suitability as a solid fuel based on said specific surface area.

2. In the evaluation of suitability, the specific surface area of ​​the char is 200 to 450 m 2 2. The method for evaluating a carbonaceous material for sintering according to claim 1, wherein when the carbonaceous material for sintering has a molecular weight within the range of 0.1 to 0.5, the carbonaceous material is evaluated as having suitability as a solid fuel.

3. A method for producing sintered ore, comprising: evaluating the suitability of char to be used as the carbonaceous material by the evaluation method for carbonaceous material for sintering according to claim 1 or 2; and using, as a solid fuel, char having a specific surface area within a predetermined range.

Citation Information

Patent Citations

  • Process for producing setting material for manufacture of sintered ore

    JP2010254929A

  • Method for manufacturing carbon-containing nonfired agglomerated ore for blast furnace using coal-char

    JP2013213264A

  • Method for determining spontaneous ignition of char and method for determining spontaneous ignition of coal

    JP2019168273A

  • Method for manufacturing sintered ore by using low-quality coal

    KR1020160043606A

  • Carbonaceous material for sintering iron ore

    WO2010087468A1