Baseless adhesive sheet
A two-layer adhesive sheet with specific resin compositions ensures excellent handling, workability, and maintains adhesive strength at high temperatures, addressing the limitations of existing adhesive sheets in automobile brake applications.
Patent Information
- Application Number
- JP2022156268
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-09-29
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2042-09-29
AI Technical Summary
Existing adhesive sheets for bonding friction materials and metals in automobile brakes face issues with handling and workability due to tackiness, and they fail to maintain adhesive strength at high temperatures, particularly during the JIS-D4422 high-temperature test of 300°C.
A two-layer adhesive sheet structure is developed, comprising a non-tacky layer made of phenolic resin and alkyl acetalized polyvinyl alcohol resin, and a tacky layer made of resol type phenolic resin and acrylonitrile butadiene rubber, which maintains adhesive strength even at high temperatures.
The adhesive sheet exhibits excellent handling and workability with sustained adhesive strength up to 300°C, outperforming single-layer and supported sheets in tests like JIS-D4422 and JIS-D4419, and is effective in environments prone to rust.
Smart Images

Figure 0007564560000001 
Figure 0007564560000002 
Figure 0007564560000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an adhesive sheet used for bonding friction materials and metal, metal and metal, and metal and rubber in automobile brakes, and a method for producing the same. [Background technology]
[0002] Conventionally, brake disc pads were manufactured through a process in which a primer was applied to a metal plate, dried, and then an adhesive was applied to the friction material, and then dried. However, the primer and adhesive contained organic solvents, which had a significant impact on the human body in the working environment, and there were also problems with the uniformity of the amount of liquid applied, and ultimately with the quality of the product.
[0003] In recent years, adhesive sheets in which the adhesive has already been formed into a film have come into use; however, their tackiness makes them difficult to handle and difficult to apply, and the relationship between the properties of the adhesive and the material to be adhered means that sufficient adhesive strength is not always obtained.
[0004] For this reason, adhesive sheets have been developed that have different adhesive layers that are suitable for the characteristics of the adherend. In most layered adhesive sheets, the adhesive is impregnated into the support, and after drying, another adhesive is applied. Those that are bonded using layered adhesive sheets with a support have the disadvantage that the adhesive strength decreases, for example, in the high-temperature test at 300°C of JIS-D4422 due to residual solvent in the support. In addition, after the JIS-D4419 adhesive surface rust generation test for automobile disc brakes, no adhesive sheet had adhesive strength strong enough to cause material destruction of the friction material even in the high-temperature test at 300°C of JIS-D4422.
[0005] Also, adhesive sheets with a two-layer structure that do not have a support are known (Patent Documents 1 and 2), but these are not capable of withstanding the high temperature test of 300° C. according to JIS-D4422. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Jpn. Jpn. Published No. 51-25563 [Patent Document 2] JP 2010-77364 A Summary of the Invention [Problem to be solved by the invention]
[0007] The objective of the present invention is to provide a thermosetting adhesive sheet that is easy to handle and work with, and that does not lose its adhesive strength even at high temperatures of 300°C when used to join friction material and metal, metal and metal, and metal and rubber in automobile brakes, and a method for producing the same. [Means for solving the problem]
[0008] The present inventors have produced and tested adhesives of various compositions in order to develop a thermosetting adhesive sheet for bonding friction materials and metals, but have not been able to obtain a single-layer adhesive sheet that is satisfactory in terms of adhesive strength, handling, and workability. Therefore, they attempted to produce a two-layer adhesive sheet with different characteristics. In this case, from the viewpoint of workability, they produced and examined various adhesive sheets consisting of two layers, one with no adhesiveness on the surface and the other with adhesiveness on the surface. They found that among the two-layer adhesive sheets produced, one consisting of a combination of layers made of adhesives of specific compositions was excellent in handling, workability, and adhesive strength, and further, the adhesive strength did not decrease even at high temperatures, and thus the present invention was completed.
[0009] The present invention is a thermosetting adhesive sheet having a two-layer structure consisting of a layer having no adhesive surface and a layer having adhesive surface, and is based on the following technology.
[0010] (1) A thermosetting adhesive sheet having a two-layer structure without a support, in which one layer has a sticky surface and the other layer has a non-sticky surface, in which the non-sticky layer contains adhesive components made of phenolic resin and alkyl acetalized polyvinyl alcohol resin, and the sticky layer contains adhesive components made of resol-type phenolic resin and acrylonitrile butadiene rubber.
[0011] (2) The thermosetting adhesive sheet according to (1), wherein the adhesive component of the layer having no adhesiveness is 30 to 50 parts by weight of an alkyl acetalized polyvinyl alcohol resin per 100 parts by weight of a phenolic resin.
[0012] (3) A thermosetting adhesive sheet according to (1) or (2), wherein the adhesive component of the non-adhesive layer is a phenolic resin that is a resol type phenolic resin, and an alkyl acetalized polyvinyl alcohol resin that is a polyvinyl butyral resin.
[0013] (4) A thermosetting adhesive sheet according to any one of (1) to (3), wherein the adhesive component of the adhesive layer is 75 to 200 parts by weight of a resol type phenolic resin per 100 parts by weight of acrylonitrile butadiene rubber.
[0014] (5) A thermosetting adhesive sheet according to any one of (1) to (4), wherein the adhesive component of the adhesive layer is an acrylonitrile butadiene rubber which is a high molecular weight thermoplastic elastomer having an acrylonitrile content of 41% and a Mooney viscosity of 73, and the resol type phenolic resin is a mixture of an alkyl-modified phenolic resin and an epoxy-modified phenolic resin in a ratio of 1:1.
[0015] (6) The thermosetting adhesive sheet according to any one of (1) to (5), wherein the adhesive sheet has a thickness of 80 to 240 μm and a thickness ratio of the non-adhesive layer to the adhesive layer is 1:1 to 1:3.
[0016] (7) A method for producing an adhesive sheet according to any one of (1) to (6), comprising the steps of forming a non-adhesive layer with an adhesive whose adhesive components are a phenolic resin and an alkyl acetalized polyvinyl alcohol resin, and then forming a sticky layer with an adhesive whose adhesive components are a resol-type phenolic resin and an acrylonitrile butadiene rubber.
[0017] (8) A method for producing an adhesive sheet according to any one of (1) to (6), comprising the steps of forming a layer having adhesiveness with an adhesive whose adhesive components are a resol-type phenolic resin and an acrylonitrile butadiene rubber, and then forming a layer having no adhesiveness with an adhesive whose adhesive components are a phenolic resin and an alkylacetalized polyvinyl alcohol resin.
[0018] (9) A method for producing an adhesive sheet according to any one of (1) to (6), comprising the steps of forming a non-adhesive layer with an adhesive whose adhesive components are a phenolic resin and an alkyl acetalized polyvinyl alcohol resin, separately forming an adhesive layer with an adhesive whose adhesive components are a resol-type phenolic resin and an acrylonitrile butadiene rubber, and laminating the respective layers together. Effect of the Invention
[0019] The adhesive sheet of the present invention is a thermosetting adhesive sheet of a two-layer structure that does not have a support, has excellent adhesive strength that does not decrease even at high temperatures, and has excellent handling and workability because the surface of one layer is sticky and the surface of the other layer is non-sticky. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The thermosetting adhesive sheet of the present invention having a two-layer structure comprises a layer having no adhesive surface and a layer having adhesive surface.
[0021] <Layer without adhesiveness> The adhesive for the non-tacky layer (hereinafter referred to as "adhesive A") contains a phenol resin and an alkyl acetalized polyvinyl alcohol resin as components, and is used by dissolving it in a solvent.
[0022] As the phenolic resin, either a resol type phenolic resin or a novolac type phenolic resin can be used. The alkyl acetalized polyvinyl alcohol resin is a resin obtained by acetalizing polyvinyl alcohol with an aldehyde, and is not particularly limited, but is preferably a polyvinyl butyral resin obtained by acetalizing polyvinyl alcohol with butyral.
[0023] Any solvent can be used so long as it dissolves these resins, but a mixed solvent of methanol and methyl ethyl ketone is preferred in terms of solubility and ease of drying. In the adhesive component of the non-adhesive layer, 30 to 50 parts by weight of alkyl acetalized polyvinyl alcohol resin is used per 100 parts by weight of phenol resin.
[0024] <Layer having adhesiveness> The adhesive for the tacky layer (hereinafter referred to as "adhesive B") contains resol-type phenolic resin and acrylonitrile butadiene rubber as components, and is used by dissolving it in a solvent.
[0025] As the phenolic resin, a resol type phenolic resin is used. As the resol type phenolic resin, it is preferable to use an alkyl-modified resol type phenolic resin, an epoxy-modified resol type phenolic resin, or a mixture thereof.
[0026] There are many types of acrylonitrile butadiene rubber whose physical properties differ depending on the amount of bound acrylonitrile (AN) in the rubber and the Mooney viscosity (molecular weight), but those with a high AN content are used for compatibility with phenolic resins, and those with a high Mooney viscosity are used for mechanical strength. Any solvent that can dissolve these can be used, but a mixed solvent of methanol and methyl ethyl ketone is preferred in terms of solubility and ease of drying.
[0027] In the adhesive component of the adhesive layer, 75 to 200 parts by weight of resol type phenolic resin is used based on 100 parts by weight of acrylonitrile butadiene rubber.
[0028] Any solvent can be used so long as it dissolves these resins, but a mixed solvent of methanol and methyl ethyl ketone is preferred in terms of solubility and ease of drying. In addition, when the adhesive sheet is made into a sheet and then cured by heating, the phenol resin acts as a crosslinking agent, so that a crosslinking agent such as a sulfur-based, peroxide-based, or phenylene bisamide-based crosslinking agent may be further blended, although this is not particularly necessary.
[0029] <Method of manufacturing thermosetting adhesive sheet> An example of a method for producing a thermosetting adhesive sheet includes a production method comprising the following steps. (1) A process of applying a solution of adhesive A onto a release sheet and drying it to form a layer that does not have adhesive properties. (2) A process of applying a solution of adhesive B onto the resulting layer and drying it to form a sticky layer.
[0030] A layer having adhesive properties may be formed first, and then a layer having no adhesive properties may be formed. Alternatively, a layer having no adhesive properties formed on a release sheet and a layer having adhesive properties formed on a separate release sheet may be laminated together to form an adhesive sheet. EXAMPLES
[0031] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0032] An adhesive solution A having the composition shown in Table 1 was prepared for forming a layer having no tackiness.
[0033] [Table 1] *1: Product name: Resitop PGA-2400 (manufactured by Gun-ei Chemical Industry Co., Ltd.) *2: Product name: Resitop PL-4222 (manufactured by Gun-ei Chemical Industry Co., Ltd.) *3: Product name: Phenolite J-325 (manufactured by DIC) *4: Product name: BMK-2620 (manufactured by Aica Kogyo Co., Ltd.) *5: Product name: Polyvinyl butyral resin S-LEC B BH-3 (manufactured by Sekisui Chemical Co., Ltd.)
[0034] An adhesive solution B having the composition shown in Table 2 was prepared for forming a layer having adhesive properties.
[0035] [Table 2] *1: High nitrile acrylonitrile butadiene rubber, product name T-4103 (manufactured by JSR Corporation) *2: Product name: Thermal Granulation (manufactured by Asahi Carbon Co., Ltd.) *3: Product name: Zinca #20 (manufactured by Sakai Chemical Industry Co., Ltd.) *4: Alkyl-modified resol-type phenolic resin, product name Phenolite TD-2620 (manufactured by DIC Corporation) *5: Epoxy modified resol type phenolic resin, product name Phenolite 5592 (manufactured by DIC Corporation)
[0036] < Creating an adhesive sheet > On the release sheet, the A adhesive solution of A-5 in Table 1 was applied with an applicator (tabletop coater) so that the thickness after drying was 40 to 120 μm, and then it was placed in a hot air dryer at 80 ° C. and dried for 5 minutes to remove the solvent, forming a layer without adhesiveness. Similarly, the B adhesive solution of B-3 in Table 2 was applied with an applicator (tabletop coater) on the release sheet so that the thickness after drying was 40 to 120 μm, and the solvent was removed with a hot air dryer to form a layer with adhesiveness. Then, the two were laminated together using a rubber roller to produce the two-layer adhesive sheets described in Examples 1 to 9 in Table-3.
[0037] [Table 3] *1: 100% destruction of friction material
[0038] In addition, a PET nonwoven fabric was placed on the release sheet, and the B adhesive solution of B-3 in Table 2 was applied using a coater so that the thickness after drying would be 40 to 80 μm, and the solvent was removed in a dryer to form a layer having adhesive properties with a support. A separately formed layer having a thickness of 40 to 80 μm and no adhesive properties was attached to this, to produce a two-layer adhesive sheet having a support as described in Comparative Examples 1 to 3 in Table 4. Table 4 also lists examples in which the thicknesses of the A and B adhesive layers are the same.
[0039] [Table 4] *1: 100% destruction of friction material *2: 50% or more interface failure *3: Product name: Spunbond 90123WSO (12g) (manufactured by Unitika)
[0040] <Normal and hot adhesive strength tests> The test specimen used was a cold rolled steel plate (SPCC-SD) measuring 25 mm in width, 150 mm in length, and 1.6 mm in thickness. The overlapping area of the normal specimen was 10mm x 25mm, while that of the hot specimen was 25mm x 25mm, and the adhesive sheet was sandwiched between two SPCC plates and bonded together. Test pieces were obtained by curing at 200℃ for 30 minutes while applying a clamping pressure of 3MPa. After leaving the specimens at room temperature for 3 days, the room temperature shear adhesive strength was measured at 25℃ (±2℃), and the hot shear adhesive strength was measured at room temperature within 1 minute after holding the specimens at 300℃ (±10℃) for 5 minutes.
[0041] < JIS-D4422 test > Brake pads were prepared by sandwiching an adhesive sheet between a back plate (iron plate material / SAPH400) and friction material, and heating at 200°C for 30 minutes under a pressure of 3 MPa, and tests were conducted using these as samples. Note that the friction material used was semi-metallic (40 to 65 parts by weight of steel wool), which has a problem with rusting. In addition, the brake pads were subjected to a saltwater environment test in accordance with JIS-D4419 (test method for adhesive surface rust formation on automotive disc brake pads), and then a JIS-D4422 test was performed.
[0042] < Evaluation > Comparing Examples 1, 2, and 5 of the laminated sheet without a support in Table 4 with Comparative Examples 1, 2, and 3 having supports with the same thicknesses of the A and B adhesive layers, the JIS-D4422 test results are superior for the laminated sheet without a support, and in particular in an atmosphere where rust is likely to occur, the laminated sheet without a support breaks down the friction material, whereas the laminated sheet with a support breaks down at the interface. From this, it can be said that the two-layer adhesive sheet without a support of the present invention is suitable for bonding automotive brake pads where rust may occur.
[0043] <Reference example> In order to examine the effect of the adhesive sheet of the present invention being composed of two adhesive layers, adhesive sheets composed of a single layer of Adhesive A of A-5 in Table 1 and Adhesive B of B-3 in Table 3 were prepared as Reference Examples 1 to 3 and Reference Examples 4 to 6. These are shown in Table 5 together with examples of adhesive sheets with a two-layer structure having corresponding sheet thicknesses.
[0044] [Table 5]
[0045] The adhesive sheet consisting of a single layer of adhesive A and adhesive B was inferior in both hot shear adhesive strength and D4422 test results to the adhesive sheet consisting of a two-layer structure of adhesive A and adhesive B. It was confirmed that the adhesive strength was improved by using a two-layer structure adhesive sheet.
[0046] In addition, samples were prepared using liquid adhesives that are widely used in the manufacture of brake linings and brake pads, and normal and hot adhesive strength tests and JIS-D4422 tests were performed. The adhesives used and the test results are shown in Table 6 as Reference Examples 7 to 10, along with the results of some of the Examples.
[0047] [Table 6] *1: Epoxy modified phenolic resin, product name 110 (manufactured by Cemedine) *2: Nitrile rubber + phenolic resin, product name 680 (manufactured by Parker Asahi Co., Ltd.) *3: Phenol resin, product name PL-2239 (manufactured by Gun-ei Chemical Industry Co., Ltd.) *4: Nitrile rubber + phenolic resin, product name NT-752 (manufactured by No Tape Industrial Co., Ltd.) *5: Butyral + phenol resin, product name 687F (manufactured by Parker Asahi Co., Ltd.) *6: Epoxy modified phenolic resin, product name No. 2545 (manufactured by Cashew Co., Ltd.) *7: Nitrile rubber + phenolic resin, product name Y-900 (manufactured by Yokohama Rubber Co., Ltd.)
[0048] The reference examples did not exceed the examples in normal and hot shear strength, with some exceptions, and many of them caused interface failure in the JIS-D4422 test. Even in those that did not cause interface failure, the friction material did not show material failure in the JIS-D4422 test under conditions that would cause rust, and the results were not satisfactory. The adhesive sheet of the present invention is more effective than a liquid adhesive in terms of adhesive strength, as well as handling and workability. [Industrial Applicability]
[0049] According to the present invention, it is possible to provide a thermosetting adhesive sheet which is easy to handle and work with and which does not lose its adhesive strength even at high temperatures of 300°C when joining friction material and metal, metal and metal, and metal and rubber in automobile brakes, and which is of extremely high practical value. It can be widely used not only for bonding friction materials and metal materials in automobile brakes, but also as an adhesive sheet used in various fields where metal-to-metal and metal-to-rubber bonding is required.
Claims
1. A thermosetting adhesive sheet having a two-layer structure without a support, in which one layer has a sticky surface and the other layer has a non-sticky surface, the non-sticky layer having adhesive components which are a phenol resin and an alkyl acetalized polyvinyl alcohol resin, and the sticky layer having adhesive components which are a resol-type phenol resin and an acrylonitrile butadiene rubber.
2. 2. The thermosetting adhesive sheet according to claim 1, wherein the adhesive component of the layer having no adhesiveness contains 30 to 50 parts by weight of alkyl acetalized polyvinyl alcohol resin per 100 parts by weight of phenol resin.
3. 3. The thermosetting adhesive sheet according to claim 1, wherein the phenolic resin in the adhesive component of the layer having no adhesiveness is a resol type phenolic resin, and the alkyl acetalized polyvinyl alcohol resin is a polyvinyl butyral resin.
4. 2. The thermosetting adhesive sheet according to claim 1, wherein the adhesive component of said adhesive layer contains 75 to 200 parts by weight of resol type phenolic resin per 100 parts by weight of acrylonitrile butadiene rubber.
5. 5. The thermosetting adhesive sheet according to claim 1 or 4, wherein the acrylonitrile butadiene rubber in the adhesive component of the adhesive layer is a high molecular weight thermoplastic elastomer having an acrylonitrile content of 41% and a Mooney viscosity of 73, and the resol type phenolic resin is a mixture of an alkyl-modified phenolic resin and an epoxy-modified phenolic resin in a ratio of 1:
1.
6. 2. The thermosetting adhesive sheet according to claim 1, wherein the adhesive sheet has a thickness of 80 to 240 μm, and the thickness ratio of the non-adhesive layer to the adhesive layer is 1:1 to 1:
3.
7. A method for producing an adhesive sheet as described in claim 1, comprising the steps of forming a non-adhesive layer with an adhesive whose adhesive components are phenolic resin and alkyl acetalized polyvinyl alcohol resin, and then forming a sticky layer with an adhesive whose adhesive components are resol-type phenolic resin and acrylonitrile butadiene rubber.
8. A method for producing an adhesive sheet as described in claim 1, comprising the steps of forming a layer having adhesiveness with an adhesive whose adhesive components are a resol type phenolic resin and acrylonitrile butadiene rubber, and then forming a layer having no adhesiveness with an adhesive whose adhesive components are a phenolic resin and an alkyl acetalized polyvinyl alcohol resin.
9. A method for producing an adhesive sheet as described in claim 1, comprising the steps of forming a non-adhesive layer with an adhesive whose adhesive components are a phenolic resin and an alkyl acetalized polyvinyl alcohol resin, and separately forming an adhesive layer with an adhesive whose adhesive components are a resol type phenolic resin and an acrylonitrile butadiene rubber, and laminating the respective layers together.
Citation Information
Patent Citations
JP1968028608Y1
JP1973097463U
JP1976025563U
Adhesive for electroless plating
JP1988213676A
Adhesive tape for bonding electronic component
JP1990091177A